Preparation method for water-loss-resistant ionic conductive gelatin hydrogel
By adding sodium pyrrolidone carboxylate to gelatin hydrogel, the problems of easy water loss and poor ionic conductivity of gelatin hydrogel are solved, and the preparation of gelatin hydrogel with resistance to water loss and high conductivity is achieved, which satisfies long-term stable use. needs.
Patent Information
- Application Number
- PCT/CN2023/104863
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2023-06-30
- Publication Date
- 2024-10-03
Smart Images

Figure CN2023104863_03102024_PF_FP_ABST
Abstract
Description
Preparation method of anti-dehydration ion conductive gelatin hydrogel Technical Field
[0001] The invention relates to a method for preparing a hydrogel, belonging to the field of polymer preparation, and in particular to a method for preparing a water-loss-resistant ion-conductive gelatin hydrogel. Background Art
[0002] Hydrogels are polymers with a three-dimensional network structure and a large internal volume of water molecules. In recent years, they have gained widespread application in various fields due to their excellent flexibility, elasticity, and biocompatibility. Gelatin is a natural polymer extracted from animal connective tissues, such as skin, bone, and cartilage. It is primarily composed of collagen, a complex macromolecular polypeptide whose main component is a trimer composed of three helical collagen chains. Gelation is one of gelatin's key properties. When a hot aqueous gelatin solution cools, the gelatin undergoes a conformational transition within its molecular chains, causing it to gel, forming a gelatin hydrogel.
[0003] The gelling property of gelatin solutions, which undergoes phase transitions with temperature, makes them widely used. In many applications, gelatin hydrogels need to have ionic conductivity, and the current common method is to add inorganic salts such as potassium chloride or sodium chloride to the gelatin solution to enhance its ionic conductivity.
[0004] However, when gelatin hydrogel is exposed to air for a long time, it will inevitably lose water, causing it to mechanically harden while also blocking the transfer of ions in it, causing the gelatin hydrogel to lose its original mechanical properties and ionic conductivity, and unable to meet the needs of long-term stable use.
[0005] Therefore, preparing biocompatible gelatin hydrogels with both anti-water loss properties and ion conductivity is a major challenge currently. Summary of the Invention
[0006] To address the above problems, the present invention provides a simple and easy-to-implement method for preparing gelatin / sodium pyrrolidone carboxylate conductive hydrogel. The method is simple to operate, and the prepared hydrogel has elasticity, ductility, conductivity, and resistance to water loss, overcoming the characteristics of traditional hydrogels such as poor conductivity and easy water loss.
[0007] The technical solutions of the present invention are as follows:
[0008] Step 1: Place a certain amount of gelatin in a container and add deionized water, i.e., soak the gelatin in deionized water to allow the gelatin to swell for a period of time, then place the swollen gelatin in a water bath at a certain temperature and magnetically stir for a period of time to obtain a gelatin solution;
[0009] Step 2: adding sodium pyrrolidone carboxylate to the gelatin solution to obtain a gelatin-sodium pyrrolidone carboxylate mixed solution;
[0010] Step 3: Pour the gelatin-sodium pyrrolidone carboxylate mixed solution into a mold and cool it at a certain temperature for a period of time to obtain a gelatin-sodium pyrrolidone carboxylate hydrogel.
[0011] In step 1, the concentration of gelatin after adding deionized water is 15-20wt%, the gelatin immersion time is 30-60 min, the water bath temperature is 50-55°C, and the stirring time is 60-120 min.
[0012] In the step 2, a sodium pyrrolidone carboxylate solution is added to the gelatin solution, and then the solution is placed in a water bath at a certain temperature and magnetically stirred for a period of time to obtain a gelatin-sodium pyrrolidone carboxylate mixed solution.
[0013] In step 2, the concentration of sodium pyrrolidone carboxylate in the gelatin-sodium pyrrolidone carboxylate mixed solution is 0-40 wt%, the water bath temperature is 50-55°C, and the stirring time is 60-120 min.
[0014] In the step 3, the cooling temperature is 10-20° C., and the cooling time is 60-120 min.
[0015] The hydrogel of the present invention uses gelatin as a skeleton and water as a solvent. Sodium pyrrolidonecarboxylate is incorporated into the system as a substance to improve the gel's anti-water loss performance and provide ion conductivity, while also improving the mechanical properties of the hydrogel.
[0016] Sodium pyrrolidone carboxylate (PCA-Na) is a naturally occurring substance in the stratum corneum of the skin. It is an amino acid derivative and a natural moisturizing factor. Its molecular structure contains a pyrrolidone ring and a carboxylic acid functional group.
[0017] PCA-Na has very strong hygroscopicity and can absorb hundreds of times its own weight in water, so it has excellent moisturizing function. By adding PCA-Na as a liquid with good biocompatibility, the gel can form a large number of hydrogen bonds with the water molecules in the gelatin hydrogel, thereby slowing down the volatilization of water molecules in the hydrogel and playing a moisturizing role for the gelatin hydrogel. In addition, the carboxylic acid functional groups in PCA-Na can form ionic crosslinks with the amino groups on the gelatin molecular chain, and the electrostatic interaction between the two can greatly enhance the mechanical strength of the gelatin hydrogel. In addition, the sodium ions in the PCA-Na molecules can move freely in the hydrogel network, giving the hydrogel excellent ionic conductivity.
[0018] Therefore, the preparation method proposed in the present invention improves the shortcomings of gelatin hydrogel such as easy water loss, poor mechanical properties and poor ion conductivity, and can prepare gelatin hydrogel that is resistant to water loss and ion conductive.
[0019] The beneficial effects of the present invention are:
[0020] (1) The introduction of PCA-Na can form strong hydrogen bonds with water molecules to achieve a moisturizing effect, and at the same time can also improve the mechanical strength and ionic conductivity of gelatin hydrogel.
[0021] (2) The preparation method of the present invention is simple, inexpensive, highly practical, and easy to promote. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 shows the stress-strain diagram of hydrogels with different PCA-Na contents, where 0%-40 wt% represents the PCA-Na content in the system.
[0023] Figure 2 shows the change curve of the composite viscosity of hydrogels with different PCA-Na contents as a function of temperature, where 0%-40% represents the PCA-Na content in the system.
[0024] Figure 3 shows the conductivity of hydrogels with different PCA-Na contents.
[0025] Figure 4 shows the water retention of hydrogels with different PCA-Na contents, where 0%-40% represents the PCA-Na content in the system. DETAILED DESCRIPTION
[0026] The present invention will be further described below with reference to the accompanying drawings and specific implementations.
[0027] The embodiments of the present invention are as follows: Example 1
[0028] 0.4 g of gelatin was added to 1.88 mL of deionized water, soaked for 1 hour, and then stirred at 50°C for 2 hours to form a uniform gelatin solution; 0.12 g of sodium pyrrolidonecarboxylate (PCA-Na) was added to the uniform gelatin solution, and then stirred at 50°C for 2 hours to form a gelatin-sodium pyrrolidonecarboxylate mixed solution; the gelatin-sodium pyrrolidonecarboxylate mixed solution was poured into a mold and cooled at 20°C for 1 hour to obtain the water loss-resistant ion conductive gelatin hydrogel. Example 2
[0029] 0.4 g of gelatin was added to 1.76 mL of deionized water, soaked for 1 h, and then stirred at 50°C for 2 h to form a uniform gelatin solution; 0.24 g of sodium pyrrolidonecarboxylate (PCA-Na) was added to the uniform gelatin solution, and then stirred at 50°C for 2 h to form a gelatin-sodium pyrrolidonecarboxylate mixed solution; the gelatin-sodium pyrrolidonecarboxylate mixed solution was poured into a mold and cooled at 20°C for 1 h to obtain a water-loss-resistant ion-conductive gelatin hydrogel. Example 3
[0030] 0.4 g of gelatin was added to 1.52 mL of deionized water, soaked for 1 h, and then stirred at 50°C for 2 h to form a uniform gelatin solution; 0.48 g of sodium pyrrolidonecarboxylate (PCA-Na) was added to the uniform gelatin solution and then stirred at 50°C for 2 h to form a gelatin-sodium pyrrolidonecarboxylate mixed solution; the gelatin-sodium pyrrolidonecarboxylate mixed solution was poured into a mold and cooled at 20°C for 1 h to obtain a water-loss-resistant ion-conductive gelatin hydrogel. Example 4
[0031] 0.4 g of gelatin was added to 1.28 mL of deionized water, soaked for 1 h, and then stirred at 50°C for 2 h to form a uniform gelatin solution; 0.72 g of sodium pyrrolidonecarboxylate (PCA-Na) was added to the uniform gelatin solution and then stirred at 50°C for 2 h to form a gelatin-sodium pyrrolidonecarboxylate mixed solution; the gelatin-sodium pyrrolidonecarboxylate mixed solution was poured into a mold and cooled at 20°C for 1 h to obtain a water-loss-resistant ion-conductive gelatin hydrogel. Example 5
[0032] 0.4 g of gelatin was added to 1.04 mL of deionized water, soaked for 1 h, and then stirred at 50°C for 2 h to form a uniform gelatin solution; 0.96 g of sodium pyrrolidonecarboxylate (PCA-Na) was added to the uniform gelatin solution and then stirred at 50°C for 2 h to form a gelatin-sodium pyrrolidonecarboxylate mixed solution; the gelatin-sodium pyrrolidonecarboxylate mixed solution was poured into a mold and cooled at 20°C for 1 h to obtain a water-loss-resistant ion-conductive gelatin hydrogel.
[0033] Comparative Example 1:
[0034] 0.4 g of gelatin was added to 2 mL of deionized water, soaked for 1 h, and then stirred at 50°C for 2 h to form a uniform gelatin solution; the gelatin solution was poured into a mold and cooled at 20°C for 1 h to obtain a gelatin hydrogel.
[0035] The above-mentioned Examples 1-5 and Comparative Document 1 were tested in many aspects to obtain results in stress-strain, complex viscosity, conductivity, water retention, etc., as shown in Figures 1-4.
[0036] In each figure, 0% PCA-Na refers to Comparative Example 1, and the mass content of PCA-Na in Examples 1-5 increases successively to 5%, 10%, 20%, 30%, and 40%, respectively.
[0037] The stress-strain results obtained after testing of the above-mentioned Examples 1-5 and Comparative Document 1 are shown in FIG1 . It can be seen from the figure that as the content of PCA-Na increases, the Young's modulus of the hydrogel increases.
[0038] The results of the changes in complex viscosity with temperature obtained by testing the above Examples 1-5 and Comparative Document 1 are shown in Figure 2. It can be seen from the figure that as the PCA-Na content increases, the viscosity of the hydrogel increases.
[0039] The conductivity results obtained after testing of the above Examples 1-5 and Comparative Document 1 are shown in FIG3 . It can be seen from the figure that as the PCA-Na content increases, the conductivity of the hydrogel increases.
[0040] The water retention results obtained through testing of the above Examples 1-5 and Comparative Document 1 are shown in FIG4 . It can be seen from the figure that as the PCA-Na content increases, the water retention of the hydrogel increases.
[0041] From this implementation, it can be seen that the present invention can improve the anti-water loss performance of the gel by adding sodium pyrrolidonecarboxylate, and the substance providing ion conductivity is incorporated into the system to improve the mechanical properties of the hydrogel.
[0042] It should be noted that the above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art will be able to modify the technical solutions described in the aforementioned embodiments or replace parts thereof with equivalents. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present invention shall be included within the scope of protection of the present invention.
Claims
1. A method for preparing a water-depletion-resistant ion-conductive gelatin hydrogel, Features: The method steps and conditions are as follows: Step 1, adding a certain amount of gelatin to deionized water, that is, soaking the gelatin in deionized water to allow the gelatin to swell for a period of time, and then placing the swollen gelatin in a water bath at a certain temperature and magnetically stirring for a period of time to obtain a gelatin solution; Step 2, adding sodium pyrrolidone carboxylate to the gelatin solution to obtain a gelatin-sodium pyrrolidone carboxylate mixed solution; Step 3: Pour the gelatin-sodium pyrrolidone carboxylate mixed solution into a mold and cool it at a certain temperature for a period of time to obtain a gelatin-sodium pyrrolidone carboxylate hydrogel.
2. A method for preparing a dehydration-resistant ion-conductive gelatin hydrogel according to claim 1, Features: In the step 1, the concentration of gelatin after adding deionized water is 15-20wt%, the immersion time of gelatin is 30-60 min, the water bath temperature is 50-55°C, and the stirring time is 60-120 min.
3. The method for preparing the water-dehydration-resistant ion-conductive gelatin hydrogel according to claim 1, Features: In the step 2, a sodium pyrrolidone carboxylate solution is added to the gelatin solution, and then the solution is placed in a water bath at a certain temperature and magnetically stirred for a period of time to obtain a gelatin-sodium pyrrolidone carboxylate mixed solution.
4. The method for preparing the water-dehydration-resistant ion-conductive gelatin hydrogel according to claim 3, Features: In the step 2, the concentration of sodium pyrrolidone carboxylate in the gelatin-sodium pyrrolidone carboxylate mixed solution is 0-40 wt%, the water bath temperature is 50-55°C, and the stirring time is 60-120 min.
5. The method for preparing a dehydration-resistant ion-conductive gelatin hydrogel according to claim 1, Features: In the step 3, the cooling temperature is 10-20° C. and the cooling time is 60-120 min.
Citation Information
Patent Citations
Carbamido pyrimidone modified gelatin injectable self-healing hydrogel and preparation method thereof
CN107043465A
Preparation method for gelatin high-strength high-strength hydrogel
CN110078945A
Medical conductive gel and preparation method thereof
CN110655663A
Hydrogel and preparation method thereof
CN115703888A
Preparation method of anti-dehydration ionic conductive gelatin hydrogel
CN116284863A
Cited By
Wide-temperature-range hydrogel for battery thermal management as well as preparation method and application of wide-temperature-range hydrogel
CN121064499A