Positive electrode sheet and preparation method therefor, electrode assembly, battery cell, battery, and electric apparatus
By forming a fluoride protective film on the positive electrode sheet of the lithium-ion battery, the problem of contact between the positive electrode material and air and electrolyte is solved, the stability and performance of the battery are improved, and the service life of the battery is extended.
Patent Information
- Application Number
- PCT/CN2023/117560
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2023-09-07
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium-ion batteries have problems with performance deterioration during cycling. This is mainly due to the deterioration of performance caused by the contact of the cathode material with air and the occurrence of interfacial side reactions with the electrolyte, resulting in reduced material stability.
A positive electrode plate including a current collector is used. The surface of the coating is provided with a fluoride protective film with a thickness of 1nm to 50nm. It is mainly composed of lithium fluoride and aluminum fluoride. The coating layer is formed through thin film deposition technology to reduce the interaction between the positive electrode material and the air. Opportunities for contact with the electrolyte to improve stability.
It effectively improves the stability of the cathode material and battery performance, reduces the polarization of lithium-ion batteries, and extends the cycle life and power performance of the battery.
Smart Images

Figure CN2023117560_03102024_PF_FP_ABST
Abstract
Description
Positive electrode sheet and preparation method thereof, electrode assembly, battery cell, battery and electrical device
[0001] Related applications
[0002] This application claims priority to Chinese patent application No. 202310312883.9 filed on March 28, 2023, the entire contents of which are incorporated by reference into this application. Technical Field
[0003] The present application relates to the field of battery technology, and in particular to a positive electrode sheet and a preparation method thereof, an electrode assembly, a battery cell, a battery, and an electrical device. Background Art
[0004] Lithium-ion batteries have become the most popular energy storage system due to their high operating potential, long life and environmental friendliness. They are now widely used in pure electric vehicles, hybrid electric vehicles, smart grids and other fields.
[0005] There is a problem of battery performance deterioration during the cycle of lithium-ion batteries.
[0006] Summary of the Invention
[0007] The main purpose of this application is to provide a positive electrode plate to improve the performance of the battery.
[0008] To achieve the above objectives, the present application proposes a positive electrode plate, which includes a current collector and a coating provided on at least one side of the current collector, wherein a protective film is provided on the surface of the coating, and the material of the protective film includes fluoride.
[0009] The positive electrode sheet of the present application includes a current collector and a coating disposed on at least one side of the current collector, the surface of the coating being provided with a protective film, the material of the protective film comprising a fluoride. Considering that the positive electrode material in the coating may deteriorate in performance when exposed to air, and that contact between the positive electrode material and the electrolyte may result in interfacial side reactions, in order to improve the performance of the positive electrode material, a protective film is provided on the surface of the coating to reduce the chance of contact between the positive electrode material and air, and to reduce the probability of interfacial reactions between the positive electrode material and the electrolyte, thereby improving the stability of the positive electrode material and thus improving the performance of the battery.
[0010] Optionally, the protective film has a thickness ranging from 1 nm to 50 nm, preferably from 5 nm to 20 nm.
[0011] In order to make the protective film effectively reduce the chance of contact between the electrolyte and the coating and ensure that lithium ions have a good migration rate, the thickness of the protective film ranges from 1 nm to 50 nm, preferably from 5 nm to 20 nm.
[0012] Optionally, the fluoride includes at least one of lithium fluoride and aluminum fluoride.
[0013] The fluoride includes at least one of lithium fluoride and aluminum fluoride. That is, the protective film may include both lithium fluoride and aluminum fluoride, or may be composed of lithium fluoride or aluminum fluoride independently. Of course, in some cases, other types of materials may be added to the protective film as needed. This application is not limited to this and the design can be based on the use requirements.
[0014] Optionally, the protective film includes a lithium fluoride protective film and an aluminum fluoride protective film, and the lithium fluoride protective film and the aluminum fluoride protective film are stacked on the surface of the coating;
[0015] And / or, the protective film includes a lithium fluoride protective film and an aluminum fluoride protective film, at least a portion of the surface of the coating is provided with the lithium fluoride protective film, and at least another portion of the surface of the coating is provided with the aluminum fluoride protective film.
[0016] The lithium fluoride protective film and the aluminum fluoride protective film are stacked on the surface of the coating, and the lithium fluoride protective film 30a and the aluminum fluoride protective film 30b are alternately arranged on the surface of the coating 20. For example, the lithium fluoride protective film 30a is arranged on the surface of the coating 20, and the aluminum fluoride protective film 30b is arranged on the side of the lithium fluoride protective film 30a away from the coating 20. Of course, the aluminum fluoride protective film 30b can also be arranged on the surface of the coating 20, and the lithium fluoride protective film 30a is arranged on the side of the aluminum fluoride protective film 30b away from the coating 20. The number of layers of the lithium fluoride protective film 30a and the aluminum fluoride protective film 30b is not specifically limited. For example, the lithium fluoride protective film 30a is two layers, and the aluminum fluoride protective film 30b is one layer. The aluminum fluoride protective film 30b is arranged between the two layers of lithium fluoride protective film 30a, and can be arranged according to needs.
[0017] At least a portion of the surface of the coating is provided with a lithium fluoride protective film, and at least another portion of the surface of the coating is provided with an aluminum fluoride protective film. The lithium fluoride protective film 30a is provided on at least a portion of the surface of the coating 20, and the aluminum fluoride protective film 30b is provided on at least another portion of the surface of the coating 20. It can be understood that the lithium fluoride protective film 30a and the aluminum fluoride protective film 30b can be provided side by side on one surface of the coating 20 without any specific limitation, and can be considered as needed.
[0018] Optionally, the coating layer includes a positive electrode material, a coating layer is formed on the surface of the positive electrode material, and the coating layer includes at least one of a sulfur-containing compound, a boron-containing compound, and a fluoride.
[0019] Positive electrode materials, such as ternary positive electrode materials, especially the higher the nickel content, the higher the residual lithium compounds present on the surface during the synthesis process. Such surface residual lithium can easily absorb carbon dioxide and water in the air, forming Li2CO3 and LiOH layers on the surface of the particles, which will have the following effects: it consumes the Li in the material and has no electrochemical activity, thus causing capacity decay; LiOH will react with polyvinylidene fluoride (PVDF), causing the slurry to gel, and the LiOH remaining on the electrode may also react with the electrolyte LiPF6, consuming the Li ions in the electrolyte and generating HF, which will further corrode the positive electrode material and alienate its surface; the dense Li2CO3 layer on the surface of the positive electrode particles will also hinder the diffusion of Li in the future, affecting the battery's electrical performance.
[0020] In order to solve the above problems, the residual lithium compounds are reduced or eliminated through chemical reactions, and an ion-conductive coating layer is formed on the surface of the positive electrode material to reduce battery polarization. The coating layer includes at least one of a sulfur-containing compound, a boron-containing compound, and a fluoride.
[0021] Optionally, the coating layer is lithium fluoride.
[0022] The lithium fluoride coating is obtained through a reaction with ammonium fluoride. By controlling the amount of ammonium fluoride added to the reaction, residual lithium can be completely removed. Furthermore, controlled operation steps can effectively remove reaction byproducts, thus avoiding the introduction of new impurities.
[0023] Furthermore, the ammonium fluoride can be added during the preparation of the coating slurry without adding any additional steps, thereby improving the preparation efficiency of the positive electrode sheet.
[0024] Optionally, the mass percentage of the lithium fluoride to the total mass of the positive electrode material is 0.01% to 5%, preferably 0.5% to 1.2%.
[0025] In the process of obtaining a lithium fluoride coating layer by reacting residual lithium with ammonium fluoride, the amount of ammonium fluoride to be added can be calculated based on the amount of residual lithium in the positive electrode material to completely react the residual lithium. In the obtained positive electrode material, the mass percentage of lithium fluoride to the total mass of the positive electrode material is 0.01% to 5%, preferably 0.5% to 1.2%.
[0026] Optionally, the general formula of the positive electrode material in the coating is Li x Ni y M 1-y O2, 0.9≤x≤1.15, 0.6≤y≤1, M is selected from one or more of Co, Mn, and Al;
[0027] And / or, the general formula of the positive electrode material in the coating is xLi2MnO3·(1-x)LiMO2, 0.1≤x≤0.9, and M is selected from one or more of Co, Mn, and Al.
[0028] The cathode material in the coating includes Li x Ni y M 1-y O2, 0.9≤x≤1.15, 0.6≤y≤1, M is selected from one or more of Co, Mn, and Al, and / or, including lithium-rich manganese-based positive electrode material xLi2MnO3·(1-x)LiMO2, 0.1≤x≤0.9, M is selected from one or more of Co, Mn, and Al.
[0029] The present application also provides a method for preparing a positive electrode sheet, comprising:
[0030] Prepare the positive electrode;
[0031] preparing fluoride precursors;
[0032] A protective film is formed on the coating surface of the positive electrode plate by thin film deposition technology.
[0033] In order to form a protective film on the coating surface of the positive electrode plate, the steps include preparing the positive electrode plate, preparing a fluoride precursor, and forming a protective film on the coating surface of the positive electrode plate by thin film deposition technology.
[0034] It is understandable that thin film deposition technology includes chemical vapor deposition and physical vapor deposition. This application does not limit which deposition technology is used to form a protective film on the coating surface, and it can be selected according to the experimental environment and actual needs.
[0035] Optionally, the thin film deposition technology includes an atomic layer deposition process.
[0036] Thin film deposition technologies include chemical vapor deposition and physical vapor deposition. There is no restriction on the specific process to be selected. In order to make the prepared protective film more effective, the atomic layer deposition process is preferred. The atomic layer deposition process has better chemical ratio, strong stress control ability, smooth film surface, wide process window, and a wider range of precursor selection.
[0037] Optionally, the fluoride includes lithium fluoride and / or aluminum fluoride.
[0038] Fluoride can effectively reduce the oxidative activity of the positive electrode material surface, inhibit the oxidative decomposition of the electrolyte at the positive electrode, and promote the transport of lithium ions in the solid phase. A fluoride protective film is formed on the coating surface of the positive electrode sheet using thin film deposition technology by preparing a fluoride precursor. The fluoride precursor includes a lithium fluoride precursor and / or an aluminum fluoride precursor.
[0039] Optionally, the step of forming a coating layer on the coating surface of the positive electrode plate by an atomic layer deposition process includes:
[0040] Place the positive electrode sheet into the atomic layer deposition reaction chamber, evacuate the chamber, and set the deposition temperature to 200°C-250°C;
[0041] A suitable fluoride precursor is introduced into the reaction chamber to form a protective film on the surface of the coating. The vacuum is opened to remove the unreacted precursor, and the above steps are repeated to obtain a protective film of a preset thickness.
[0042] The material of the protective film includes fluoride. The type of fluoride is not specifically limited. The precursor can be selected according to the selected fluoride type. In the step of forming a coating layer on the coating surface of the positive electrode plate through the atomic layer deposition process, the process includes: placing the positive electrode plate into the atomic layer deposition reaction chamber, vacuuming, and setting the deposition temperature to 200°C-250°C; introducing a suitable fluoride precursor into the reaction chamber to form a protective film on the surface of the coating, opening the vacuum to remove the unreacted precursor, and repeating the above steps to obtain a protective film of a preset thickness.
[0043] Optionally, the step of introducing a suitable fluoride precursor into the reaction chamber to form a protective film on the surface of the coating, opening the vacuum to remove unreacted precursor, and repeating the above steps to obtain a protective film of a preset thickness includes:
[0044] A precursor of aluminum fluoride is introduced into the reaction chamber to form a protective film on the surface of the coating, and the vacuum is opened to remove unreacted precursor;
[0045] A lithium fluoride precursor is introduced into the reaction chamber to form a protective film on the surface of the coating, and the vacuum is opened to remove unreacted precursor;
[0046] Repeat the above steps to obtain a protective film of preset thickness.
[0047] The fluoride includes at least one of lithium fluoride and aluminum fluoride. In order to obtain a protective film of lithium fluoride and aluminum fluoride, a suitable fluoride precursor is introduced into a reaction chamber to form a protective film on the surface of the coating, the vacuum is opened to remove unreacted precursor, and the above steps are repeated to obtain a protective film of a preset thickness, which includes: introducing an aluminum fluoride precursor into the reaction chamber to form a protective film on the surface of the coating, opening the vacuum to remove unreacted precursor; introducing a lithium fluoride precursor into the reaction chamber to form a protective film on the surface of the coating, opening the vacuum to remove unreacted precursor; and repeating the above steps to obtain a protective film of a preset thickness.
[0048] Optionally, the step of introducing an aluminum fluoride precursor into the reaction chamber to form a protective film on the surface of the coating and opening the vacuum to remove unreacted precursor includes:
[0049] The reaction chamber is evacuated to reduce the pressure to 10 Pa or below;
[0050] Add AlCl3 gas into the reaction chamber and maintain for 10s-20s;
[0051] A purge gas is introduced into the reaction chamber, and the vacuum is opened to remove the unreacted AlCl3 gas;
[0052] The pressure in the reaction chamber is reduced to 10 Pa or below, and TiF4 gas is introduced into the reaction chamber and maintained for 10s-20s;
[0053] A purge gas is introduced into the reaction chamber, and the vacuum is opened to remove the unreacted TiF4 gas;
[0054] Repeat the above steps to obtain an aluminum fluoride protective film of a preset thickness.
[0055] The precursors of aluminum fluoride include AlCl3 and TiF4. In the step of preparing the aluminum fluoride protective film, the reaction chamber is evacuated and the pressure is reduced to 10Pa or below; AlCl3 gas is introduced into the reaction chamber and maintained for 10s-20s; purge gas is introduced into the reaction chamber, the vacuum is opened, and the unreacted AlCl3 gas is taken away; the pressure in the reaction chamber is reduced to 10Pa or below, TiF4 gas is introduced into the reaction chamber and maintained for 10s-20s; purge gas is introduced into the reaction chamber, the vacuum is opened, and the unreacted TiF4 gas is taken away; the above steps are repeated to obtain an aluminum fluoride protective film of a preset thickness.
[0056] It is understandable that AlCl 3 and TiF 4 are solid at room temperature. In order to obtain a gaseous precursor, a temperature that can vaporize the precursor is set to vaporize the solid to obtain a gaseous precursor.
[0057] It can be understood that the step of adding AlCl3 gas into the reaction chamber and maintaining it for 10s-20s is to introduce an appropriate amount of AlCl3 gas into the reaction chamber. The time for introducing the gas can be selected according to actual needs and is not specifically limited in this application.
[0058] Optionally, the step of introducing a lithium fluoride precursor into the reaction chamber to form a protective film on the surface of the coating and opening the vacuum to remove unreacted precursor includes:
[0059] The reaction chamber is evacuated to reduce the pressure to 10 Pa or below;
[0060] Alkyl lithium vapor is introduced into the reaction chamber and maintained for 10s-20s;
[0061] A purge gas is introduced into the reaction chamber, and the vacuum is opened to remove unreacted alkyl lithium vapor;
[0062] The pressure in the reaction chamber is reduced to 10 Pa or less, and TiF4 vapor is introduced into the reaction chamber for 10s-20s;
[0063] A purge gas is introduced into the reaction chamber, and the vacuum is opened to remove the unreacted TiF4 vapor;
[0064] Repeat the above steps to obtain a lithium fluoride protective film of a preset thickness.
[0065] The precursors of lithium fluoride include alkyl lithium and TiF4. In the step of preparing the lithium fluoride protective film, the reaction chamber is evacuated and the pressure is reduced to 10 Pa or below; alkyl lithium vapor is introduced into the reaction chamber and maintained for 10s-20s; purge gas is introduced into the reaction chamber, the vacuum is opened, and unreacted alkyl lithium vapor is taken away; the pressure in the reaction chamber is reduced to 10 Pa or below, TiF4 vapor is introduced into the reaction chamber and maintained for 10s-20s; purge gas is introduced into the reaction chamber, the vacuum is opened, and unreacted TiF4 vapor is taken away; and the above steps are repeated to obtain a lithium fluoride protective film of a preset thickness.
[0066] Optionally, the step of preparing the positive electrode sheet includes:
[0067] Mixing a positive electrode material with a reactive substance to react, thereby forming a coating layer on the surface of the positive electrode material;
[0068] The positive electrode material with the coating layer, the binder, and the conductive agent are mixed, and a solvent is added and stirred to obtain a positive electrode slurry;
[0069] Applying the positive electrode slurry to a current collector and drying it to obtain a positive electrode sheet;
[0070] Wherein, the reactive substance includes at least one of a sulfur compound and a boron compound.
[0071] Residual lithium on the surface of the positive electrode material will affect the performance of the battery. In order to remove the residual lithium, a reactive substance is used to react with the residual lithium. For example, sulfur compounds and boron compounds are mixed with the positive electrode material and reacted under certain conditions to form a coating layer on the surface of the positive electrode material; the positive electrode material with the coating layer, a binder, and a conductive agent are mixed, and a solvent is added and stirred to obtain a positive electrode slurry; the positive electrode slurry is coated on a current collector and dried to obtain a positive electrode sheet.
[0072] Optionally, the step of preparing the positive electrode sheet includes:
[0073] Mixing the positive electrode material, the binder, the conductive agent, and ammonium fluoride, adding a solvent and stirring to obtain a positive electrode slurry;
[0074] The positive electrode slurry is applied to a current collector and dried to obtain a positive electrode sheet.
[0075] Introducing ammonium fluoride during the slurry preparation process allows it to react with residual lithium on the surface of the positive electrode material to form a lithium fluoride coating. This can reduce the amount of residual alkali on the positive electrode material surface as needed, thereby reducing battery polarization. Compared to mixing sulfur compounds and boron compounds with the positive electrode material and reacting them under certain conditions to form a coating on the positive electrode material surface, the use of ammonium fluoride eliminates the need for additional steps. Ammonium fluoride can be added directly during the slurry preparation process, reducing process steps and improving the production efficiency of positive electrode sheets.
[0076] By converting residual lithium as a reactant into an effective lithium fluoride protective layer, the slurry gel condition is effectively improved, the residual lithium is removed, and a fast ion conductor coating layer is established, thereby improving the conductivity of the positive electrode sheet, reducing the polarization of the lithium-ion battery, and improving the power performance of the lithium-ion battery.
[0077] Optionally, the amount of ammonium fluoride added is in the range of 0.009% to 4.5% of the mass of the positive electrode material, preferably 0.45% to 1.1%.
[0078] During the process of removing residual lithium, the amount of ammonium fluoride to be added can be converted according to the amount of residual lithium. The amount of ammonium fluoride added accounts for 0.009% to 4.5% of the mass of the positive electrode material, preferably 0.45% to 1.1%.
[0079] Optionally, the step of mixing the positive electrode material, the binder, the conductive agent, and ammonium fluoride, adding a solvent and stirring to obtain a positive electrode slurry includes:
[0080] The positive electrode material, binder, conductive agent and ammonium fluoride are mixed for 5-60 minutes, and a solvent is added. The mixture is stirred at a speed of 300-2000 r / min for 30-3 hours, and the bubbles are removed and the air is evacuated to obtain a positive electrode slurry with a solid content of 60%-85%.
[0081] In order to fully mix ammonium fluoride and the positive electrode material in the process of preparing the slurry so as to achieve effective reaction, during the operation, the positive electrode material, binder, conductive agent and ammonium fluoride are mixed for 5min-60min, the solvent is added, and the mixture is stirred at a speed of 300r / min~2000r / min for 30min to 3h, and the bubbles are removed and the air is exhausted to obtain a positive electrode slurry with a solid content of 60%-85%.
[0082] Ammonium fluoride reacts with residual lithium, and the chemical reaction equations involved are as follows: 2NH4F+LiCO3→2LiF↓+(NH4)2CO3, NH4F+LiOH→LiF↓+NH3↑+H2O↑.
[0083] The by-products of the reaction are all volatile or decomposed substances. In order to facilitate the removal of by-products, degassing and exhaust are performed during the operation.
[0084] That is, a considerable amount of ammonium fluoride is used with residual lithium as the source, and the ammonium fluoride and the positive electrode material are fully contacted, mixed and reacted under the slurry stirring conditions. After the stirring is completed, part of the gas product is removed by exhausting the gas in the defoaming stage.
[0085] Optionally, the step of applying the positive electrode slurry to a current collector and drying to obtain a positive electrode sheet includes:
[0086] The positive electrode slurry is applied to a current collector and dried at a temperature of 100° C. to 170° C. to obtain a positive electrode sheet.
[0087] In order to effectively ensure the decomposition and removal of the reaction by-product (NH4)2CO3, the ammonium carbonate is decomposed and removed by adjusting the drying temperature during the drying process. The drying temperature is 100℃-170℃. Under this drying condition, the product (NH4)2CO3 decomposes and is discharged through the airway, which is conducive to the rapid decomposition and removal of (NH4)2CO3 and improves production efficiency.
[0088] Optionally, the ratio of the mass of residual lithium in the positive electrode material to the mass of the positive electrode material satisfies Li2CO3≥0.02%, and LiOH≥0.2%.
[0089] In order to prepare a coating layer with suitable coating quality so that the beneficial effects of the coating layer are obvious, the proportion of residual lithium in the positive electrode material to the positive electrode material mass satisfies Li2CO3≥0.02% and LiOH≥0.2%.
[0090] The present application also provides an electrode assembly, which includes the positive electrode sheet as described above, or includes a positive electrode sheet prepared by the method for preparing the positive electrode sheet as described above.
[0091] The present application also provides a battery cell, which includes the electrode assembly as described above.
[0092] The present application also provides a battery, which includes the battery cell as described above.
[0093] The present application also provides an electrical device, which includes the battery cell or the battery as described above.
[0094] The positive electrode sheet of the present application includes a current collector and a coating disposed on at least one side of the current collector, the surface of the coating being provided with a protective film, the material of the protective film comprising a fluoride. Considering that the positive electrode material in the coating may deteriorate in performance when exposed to air, and that contact between the positive electrode material and the electrolyte may result in interfacial side reactions, in order to improve the performance of the positive electrode material, a protective film is provided on the surface of the coating to reduce the chance of contact between the positive electrode material and air, and to reduce the probability of interfacial reactions between the positive electrode material and the electrolyte, thereby improving the stability of the positive electrode material and thus improving the performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0095] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.
[0096] FIG1 is a schematic structural diagram of a positive electrode sheet according to an embodiment of the present application;
[0097] FIG2 is a schematic structural diagram of a positive electrode sheet according to an embodiment of the present application;
[0098] FIG3 is a schematic structural diagram of a positive electrode sheet according to an embodiment of the present application;
[0099] FIG4 is a schematic flow chart of a method for preparing a positive electrode sheet according to an embodiment of the present application;
[0100] FIG5 is a schematic diagram of a battery cell according to an embodiment of the present application;
[0101] FIG6 is an exploded view of the battery cell according to one embodiment of the present application shown in FIG5 ;
[0102] FIG7 is a schematic diagram of a battery module according to an embodiment of the present application;
[0103] FIG8 is a schematic diagram of a battery pack according to an embodiment of the present application;
[0104] FIG9 is an exploded view of the battery pack according to one embodiment of the present application shown in FIG8 ;
[0105] FIG. 10 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.
[0106] Description of Figure Numbers:
[0107] The realization of the objectives, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0108] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
[0109] Below, the embodiments of the cathode electrode sheet, electrode assembly, battery cell, battery cell, battery and electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0110] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0111] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0112] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0113] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0114] The presence of impurities on the surface of the positive electrode material may reduce the performance of the positive electrode material.
[0115] For example, when preparing high-nickel ternary materials, there are structural stability issues during the synthesis process. Therefore, in order to synthesize in the form of stable oxides, excess Li / Me (alloying elements) conditions are usually designed to synthesize structurally stable positive electrode active materials. That is, in the process of preparing high-nickel ternary materials, the lithium salt is excessive in the mixed ternary precursor and lithium salt. The excess of lithium salt causes the excess part of the lithium salt to not participate in the reaction. As a result, this part of the lithium salt reacts with moisture and CO2 in the air to generate residual lithium (LiOH and Li2CO3). When manufacturing battery cells, the presence of residual lithium will cause many problems. For example, the residual lithium has poor ion conductivity. It is formed on the surface of the ternary material, which will hinder the transmission of lithium ions in the ternary material. In addition, Li2CO3 will react with the electrolyte to generate gas and heat, affecting the safety of the battery.
[0116] Applying cathode materials with residual lithium to the coating can degrade battery performance. For example, exposure to air can lead to performance degradation, and contact with the electrolyte can cause interfacial side reactions.
[0117] In order to solve the above problems, the present application provides a positive electrode plate, which includes a current collector and a coating provided on at least one side of the current collector, wherein a protective film is provided on the surface of the coating, and the material of the protective film includes fluoride.
[0118] A current collector is a structure or component that collects current. In lithium-ion batteries, this primarily refers to metal foil, such as copper or aluminum foil. The current collector serves as a substrate for the positive or negative active material, collecting the current generated by the active material and delivering high current output. Typically, aluminum foil is used as the positive current collector, while copper foil is used for the negative current collector.
[0119] The coating layer includes a positive electrode material, a binder, and a conductive agent. In the process of preparing the coating layer, the positive electrode material, the binder, the conductive agent and a solvent are mixed to prepare a slurry, and the prepared slurry is coated on the current collector to obtain the coating layer.
[0120] The positive electrode material can provide a lithium source and is used in batteries. During charging, lithium ions are released from the lattice of the positive electrode active material and inserted into the lattice of the negative electrode material after passing through the electrolyte; during discharging, lithium ions are released from the lattice of the negative electrode material and inserted into the lattice of the positive electrode material after passing through the electrolyte.
[0121] Binder refers to a material with adhesive properties that is used to bond different substances together.
[0122] Conductive agent is used to ensure that the electrode has good charge and discharge performance. A certain amount of conductive material is usually added during the production of the electrode. It collects microcurrents between the active materials and between the active materials and the current collector to reduce the contact resistance of the electrode and accelerate the movement rate of electrons. At the same time, it can also effectively increase the migration rate of lithium ions in the electrode material, thereby improving the charge and discharge efficiency of the electrode.
[0123] The protective film is a film structure provided on the surface of the coating. As shown in FIG1 , the positive electrode sheet 100 includes a current collector 10, a coating 20 provided on the current collector 10, and a protective film 30 provided on the surface of the coating 20. It is understood that the surface of the coating 20 refers to the surface of the coating exposed to the outside, for example, it can be the surface of the coating 20 facing away from the current collector, or it can be the surface located on the side of the coating 20. The protective film 30 can be provided on any surface of the coating 20, specifically according to the needs. For example, in one case, the protective film 30 is provided on each exposed surface of the coating to reduce the contact between the coating and the electrolyte.
[0124] Fluoride refers to a compound containing negatively charged fluorine.
[0125] Fluoride can effectively reduce the oxidation activity of the cathode material surface, inhibit the oxidative decomposition of the electrolyte at the cathode, and promote lithium ion transport in the solid phase. For example, fluoride can be lithium fluoride or aluminum fluoride, of which lithium fluoride is more beneficial for improving its air stability.
[0126] That is, in order to improve the performance of the coating, a protective film is set on the surface of the coating. The material of the protective film includes fluoride, which reduces the chance of contact between the positive electrode material in the coating and the air, and reduces the probability of interfacial reaction between the positive electrode material and the electrolyte, thereby improving the stability of the positive electrode material and thus improving the performance of the battery.
[0127] Moreover, lithium fluoride or aluminum fluoride are both ion conductors, which will not block the transmission of lithium ions and will not affect the infiltration.
[0128] In one embodiment, the thickness of the protection film ranges from 1 nm to 50 nm, preferably from 5 nm to 20 nm.
[0129] In order to make the protective film effectively reduce the chance of contact between the electrolyte and the coating and ensure that lithium ions have a good migration rate, the thickness of the protective film ranges from 1 nm to 50 nm, preferably from 5 nm to 20 nm.
[0130] In the above-mentioned 1nm to 50nm, the values include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 1nm, 3nm, 5nm, 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, etc.
[0131] In the above-mentioned 5nm to 20nm, the values include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 5nm, 10nm, 15nm, 20nm, 25nm, 30nm, etc.
[0132] In one embodiment, the fluoride includes at least one of lithium fluoride and aluminum fluoride.
[0133] The fluoride includes at least one of lithium fluoride and aluminum fluoride. That is, the protective film may include both lithium fluoride and aluminum fluoride, or may be composed of lithium fluoride or aluminum fluoride independently. Of course, in some cases, other types of materials may be added to the protective film as needed. This application is not limited to this and the design can be based on the use requirements.
[0134] Lithium fluoride, an inorganic substance with the chemical formula LiF, is an alkali metal halide. It is a white crystal at room temperature and is insoluble in water.
[0135] Aluminum fluoride, an inorganic substance with the chemical formula AlF3, is insoluble in water, acid, and alkali. It is very stable.
[0136] Lithium fluoride and aluminum fluoride are ion-conducting substances that are conducive to the transmission of lithium ions. For example, lithium fluoride is an electronic insulator with an ion conductivity of about 10 -13 Scm -1 -10 -14 Scm -1 .
[0137] The specific type of fluoride in this application is not limited, as long as it can be set on the surface of the coating, reduce the chance of contact between the positive electrode material in the coating and the air, and reduce the probability of interfacial reaction between the positive electrode material and the electrolyte.
[0138] In one embodiment, the protective film includes a lithium fluoride protective film and an aluminum fluoride protective film, and the lithium fluoride protective film and the aluminum fluoride protective film are stacked on the surface of the coating; and / or, the protective film includes a lithium fluoride protective film and an aluminum fluoride protective film, at least a portion of the surface of the coating is provided with the lithium fluoride protective film, and at least another portion of the surface of the coating is provided with the aluminum fluoride protective film.
[0139] The lithium fluoride protective film and the aluminum fluoride protective film are stacked on the surface of the coating. As shown in Figure 3, the lithium fluoride protective film 30a and the aluminum fluoride protective film 30b are alternately arranged on the surface of the coating 20. For example, the lithium fluoride protective film 30a is arranged on the surface of the coating 20, and the aluminum fluoride protective film 30b is arranged on the side of the lithium fluoride protective film 30a away from the coating 20. Of course, the aluminum fluoride protective film 30b can also be arranged on the surface of the coating 20, and the lithium fluoride protective film 30a is arranged on the side of the aluminum fluoride protective film 30b away from the coating 20. The number of layers of the lithium fluoride protective film 30a and the aluminum fluoride protective film 30b is not specifically limited. For example, the lithium fluoride protective film 30a is two layers, and the aluminum fluoride protective film 30b is one layer. The aluminum fluoride protective film 30b is arranged between the two layers of lithium fluoride protective film 30a, which can be arranged according to needs.
[0140] At least a portion of the surface of the coating is provided with a lithium fluoride protective film, and at least another portion of the surface of the coating is provided with an aluminum fluoride protective film. As shown in FIG2 , at least a portion of the surface of the coating 20 is provided with a lithium fluoride protective film 30a, and at least another portion of the surface of the coating 20 is provided with an aluminum fluoride protective film 30b. It can be understood that the lithium fluoride protective film 30a and the aluminum fluoride protective film 30b can be provided side by side on one surface of the coating 20 without any specific limitation, and can be considered as needed.
[0141] The protective film includes a lithium fluoride protective film and an aluminum fluoride protective film, that is, the protective film includes both lithium fluoride and aluminum fluoride protective films. The thickness ratio of the lithium fluoride and aluminum fluoride protective films is not limited and can be set according to needs. For example, the film thickness of lithium fluoride and aluminum fluoride can be 1:1. Both lithium fluoride and aluminum fluoride can effectively reduce the oxidation activity on the surface of the positive electrode material, inhibit the oxidative decomposition of the electrolyte at the positive electrode, and promote the lithium ion transport in the solid phase. Among them, lithium fluoride is more beneficial for improving its air stability. When the coating is sensitive to air, the thickness of lithium fluoride can be increased.
[0142] In one embodiment, the coating layer includes a positive electrode material, a coating layer is formed on the surface of the positive electrode material, and the coating layer includes at least one of a sulfur-containing compound, a boron-containing compound, and a fluoride.
[0143] Sulfur-containing compounds, which can react with residual lithium, can be, for example, K2S2O3 or Na2S2O3.
[0144] Boron-containing compound, the boron-containing compound can react with residual lithium, for example, it can be B2O3.
[0145] Positive electrode materials, such as ternary positive electrode materials, especially the higher the nickel content, the higher the residual lithium compounds present on the surface during the synthesis process. Such surface residual lithium can easily absorb carbon dioxide and water in the air, forming Li2CO3 and LiOH layers on the surface of the particles, which will have the following effects: it consumes the Li in the material and has no electrochemical activity, thus causing capacity decay; LiOH will react with polyvinylidene fluoride (PVDF), causing the slurry to gel, and the LiOH remaining on the electrode may also react with the electrolyte LiPF6, consuming the Li ions in the electrolyte and generating HF, which will further corrode the positive electrode material and alienate its surface; the dense Li2CO3 layer on the surface of the positive electrode particles will also hinder the diffusion of Li in the future, affecting the battery's electrical performance.
[0146] In order to solve the above problems, the residual lithium compounds are reduced or eliminated through chemical reactions, and an ion-conductive coating layer is formed on the surface of the positive electrode material to reduce battery polarization. The coating layer includes at least one of sulfur-containing compounds, boron-containing compounds, and fluorides.
[0147] It is understood that the residual lithium compounds in the positive electrode material can be reacted with sulfur-containing compounds, boron-containing compounds, ammonium fluoride and the like. For example, the sulfur-containing compounds are used to react with the residual lithium (LiOH and Li2CO3) to reduce the content of residual lithium and increase the ion-conducting substances. The sulfur compounds include K2S x O y or Na2S x O y (x=1-8, y=1-8), for example, it can be K2S2O3, Na2S2O3, and its reaction formula is nLiOH+nK2S x O y ->nLi2S+nLi2SO x +nH2O (n=integer); nLi2CO3 + nK2S x O y ->nK2CO3+nLi2S x O y (n = integer); nLiOH + nNa2S x O y ->nLi2S+nLi2SO x +nH2O (n=integer); nLi2CO3 + nNa2S x O y ->nNa2CO3+nLi2S x O y (n=integer).
[0148] Boron-containing compounds are used to react with residual lithium (LiOH and Li2CO3) to reduce the residual lithium content and increase ion-conducting substances. Boron compounds include H3BO3 or B2O3, and the reaction formula is nLiOH+nB2O3->nLi3BO3+nH2O (n=integer); nLi2CO3+nB2O3->nLi3BO3+nCO2 (n=integer).
[0149] Ammonium fluoride is used to react with residual lithium (LiOH and Li2CO3), reducing or eliminating residual lithium and increasing ion-conducting substances, 2NH4F+Li2CO3->2LiF↓+(NH4)2CO3, NH4F+LiOH->LiF↓+NH3↑+H2O↑.
[0150] Considering that although the ternary material is modified and coated during the material production process, the basic residual lithium characterization at the material level shows that there is still a certain amount of residual lithium present, then these residual lithium will still be exposed to the air during the subsequent preparation of the battery. Such reactions will continue to exist and the impact on performance will continue to exist. This application introduces two protection steps in the preparation of the positive electrode sheet to achieve the ultimate all-round protection of the positive electrode sheet.
[0151] The first step is to form a coating layer on the surface of the positive electrode material, and the second step is to use the atomic layer deposition process to build a protective film on the surface of the positive electrode.
[0152] It is understandable that the coating layer depends on the distribution of residual lithium on the surface of the original ternary material. If there is no residual lithium in this area, the protective film cannot be formed through chemical reaction. Therefore, a double protection process is adopted. The second protective film can effectively protect the positive electrode material that is not coated with the coating layer, and effectively inhibit the performance degradation caused by the contact of the positive electrode surface with the air in the subsequent process. It can also reduce the probability of interfacial side reactions between the positive electrode and the electrolyte. The composite protective layer constructed by the two processes can further protect the structural stability of the positive electrode material during deep lithium deintercalation.
[0153] It is understandable that the second step is to use the atomic layer deposition process to construct a nano-scale protective film on the surface of the positive electrode, which can not only achieve a dense and uniform film layer, but also will not affect the energy density due to the thickness like traditional gravure coating.
[0154] In one embodiment, the coating layer is lithium fluoride.
[0155] The lithium fluoride coating is obtained through a reaction with ammonium fluoride. By controlling the amount of ammonium fluoride added to the reaction, residual lithium can be completely removed. Furthermore, controlled operation steps can effectively remove reaction byproducts, thus avoiding the introduction of new impurities.
[0156] Furthermore, the ammonium fluoride can be added during the preparation of the coating slurry without adding any additional steps, thereby improving the preparation efficiency of the positive electrode sheet.
[0157] In one embodiment, the mass percentage of lithium fluoride to the total mass of the positive electrode material is 0.01% to 5%, preferably 0.5% to 1.2%.
[0158] The total mass of the positive electrode material is the sum of the mass of the positive electrode material and the mass of lithium fluoride. For example, the mass of lithium fluoride is m1 and the mass of the positive electrode material is m2. The mass percentage of lithium fluoride to the total mass of the positive electrode material is calculated as m1 / (m1+m2)×100%.
[0159] In the process of obtaining a lithium fluoride coating layer by reacting residual lithium with ammonium fluoride, the amount of ammonium fluoride to be added can be calculated based on the amount of residual lithium in the positive electrode material to completely react the residual lithium. In the obtained positive electrode material, the mass percentage of lithium fluoride to the total mass of the positive electrode material is 0.01% to 5%, preferably 0.5% to 1.2%.
[0160] In the above-mentioned 0.01% to 5%, the values include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 0.01%, 0.05%, 0.1%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc.
[0161] In the above 0.5% to 1.2%, the values include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 0.5%, 0.7%, 0.9%, 1%, 1.2%, etc.
[0162] In one embodiment, the positive electrode material in the coating has the general formula Li x Ni y M 1-y O2, 0.9≤x≤1.15, 0.6≤y≤1, M is selected from one or more of Co, Mn, and Al; and / or, the general formula of the positive electrode material in the coating is xLi2MnO3·(1-x)LiMO2, 0.1≤x≤0.9, M is selected from one or more of Co, Mn, and Al.
[0163] The cathode material in the coating includes Li x Ni y M 1-yO2, 0.9≤x≤1.15, 0.6≤y≤1, M is selected from one or more of Co, Mn, and Al, and / or, including lithium-rich manganese-based positive electrode material xLi2MnO3·(1-x)LiMO2, 0.1≤x≤0.9, M is selected from one or more of Co, Mn, and Al.
[0164] In one embodiment, the present application also provides a method for preparing a positive electrode plate, comprising: preparing a positive electrode plate; preparing a fluoride precursor; and forming a protective film on the coating surface of the positive electrode plate by thin film deposition technology.
[0165] Thin film deposition technology, including chemical vapor deposition and physical vapor deposition.
[0166] Chemical vapor deposition (CVD) is a chemical process that uses one or more vapor-phase compounds or elements containing the thin film elements to chemically react on a substrate surface to form a thin film. Examples include atomic layer deposition (ALD).
[0167] Physical vapor deposition (PVD) refers to a technique that uses physical methods to vaporize the surface of a material source (solid or liquid) into gaseous atoms or molecules, or partially ionize them into ions, under vacuum conditions. This technique then deposits a thin film with specific functionalities on the surface of a substrate through a low-pressure gas (or plasma) process. Examples include vacuum evaporation, sputtering, arc plasma coating, ion plating, and molecular beam epitaxy.
[0168] In order to form a protective film on the coating surface of the positive electrode plate, the steps include preparing the positive electrode plate, preparing a fluoride precursor, and forming a protective film on the coating surface of the positive electrode plate by thin film deposition technology.
[0169] In one embodiment, the thin film deposition technique includes an atomic layer deposition process.
[0170] Atomic layer deposition (ALD) is a method (technology) for forming deposited films by alternately pulses of vapor-phase precursors into a reactor, where they chemically adsorb and react on a substrate. When the precursors reach the substrate surface, they chemically adsorb and react. The ALD reactor is purged with an inert gas between precursor pulses.
[0171] In order to make the prepared protective film better, the atomic layer deposition process is preferred. The atomic layer deposition process has better chemical ratio, strong stress control ability, smooth film surface, wide process window range, and wider range of precursor selection.
[0172] For example, in one embodiment, in order to form a protective film on the positive electrode plate, the positive electrode plate is prepared, and a protective film is formed on the coating surface using an atomic layer deposition process. A nano-scale protective film is constructed on the coating surface using an atomic layer deposition process, which can achieve a dense and uniform film layer without affecting the energy density due to the thickness like traditional gravure coating.
[0173] In one embodiment, the fluoride includes lithium fluoride and / or aluminum fluoride.
[0174] Fluoride can effectively reduce the oxidative activity of the positive electrode material surface, inhibit the oxidative decomposition of the electrolyte at the positive electrode, and promote the transport of lithium ions in the solid phase. A fluoride protective film is formed on the coating surface of the positive electrode sheet using thin film deposition technology by preparing a fluoride precursor. The fluoride precursor includes a lithium fluoride precursor and / or an aluminum fluoride precursor.
[0175] In one embodiment, the step of forming a coating layer on the coating surface of the positive electrode plate through an atomic layer deposition process includes: placing the positive electrode plate into an atomic layer deposition reaction chamber, evacuating the chamber, and setting the deposition temperature to 200°C-250°C; introducing a suitable fluoride precursor into the reaction chamber to form a protective film on the surface of the coating, opening the vacuum to remove unreacted precursors, and repeating the above steps to obtain a protective film of a preset thickness.
[0176] The material of the protective film includes fluoride. The type of fluoride is not specifically limited. The precursor can be selected according to the selected fluoride type. The step of forming a coating layer on the coating surface of the positive electrode plate through the atomic layer deposition process includes: placing the positive electrode plate into the atomic layer deposition reaction chamber, vacuuming, and setting the deposition temperature to 200℃-250℃; introducing a suitable fluoride precursor into the reaction chamber to form a protective film on the surface of the coating, opening the vacuum to remove the unreacted precursor, and repeating the above steps to obtain a protective film of a preset thickness.
[0177] During the preparation of the protective film, it is necessary to maintain a vacuum environment to prevent active substances in the air from participating in the reaction during the film formation process and affecting the quality of the film layer. Therefore, the positive electrode plate needs to be placed in the reaction chamber and vacuumed so that the protective film can be prepared in a vacuum environment.
[0178] In the above-mentioned 200℃-250℃, the values include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 200℃, 210℃, 220℃, 230℃, 240℃, 250℃, etc.
[0179] In one embodiment, the steps of introducing a suitable fluoride precursor into the reaction chamber to form a protective film on the surface of the coating, opening the vacuum to remove unreacted precursor, and repeating the above steps to obtain a protective film of a preset thickness include: introducing an aluminum fluoride precursor into the reaction chamber to form a protective film on the surface of the coating, opening the vacuum to remove unreacted precursor; introducing a lithium fluoride precursor into the reaction chamber to form a protective film on the surface of the coating, opening the vacuum to remove unreacted precursor; and repeating the above steps to obtain a protective film of a preset thickness.
[0180] The fluoride includes at least one of lithium fluoride and aluminum fluoride. In order to obtain a protective film of lithium fluoride and aluminum fluoride, a suitable fluoride precursor is introduced into a reaction chamber to form a protective film on the surface of the coating, the vacuum is opened to remove unreacted precursors, and the above steps are repeated to obtain a protective film of a preset thickness, which includes: introducing an aluminum fluoride precursor into the reaction chamber to form a protective film on the surface of the coating, opening the vacuum to remove unreacted precursors; introducing a lithium fluoride precursor into the reaction chamber to form a protective film on the surface of the coating, opening the vacuum to remove unreacted precursors; and repeating the above steps to obtain a protective film of a preset thickness.
[0181] In one embodiment, the steps of introducing an aluminum fluoride precursor into a reaction chamber, forming a protective film on the surface of the coating, and opening the vacuum to remove unreacted precursor include: evacuating the reaction chamber to reduce the pressure to 10Pa or below; introducing AlCl3 gas into the reaction chamber and maintaining it for 10s-20s; introducing purge gas into the reaction chamber, opening the vacuum, and removing unreacted AlCl3 gas; reducing the pressure in the reaction chamber to 10Pa or below, introducing TiF4 gas into the reaction chamber and maintaining it for 10s-20s; introducing purge gas into the reaction chamber, opening the vacuum, and removing unreacted TiF4 gas; repeating the above steps to obtain an aluminum fluoride protective film of a preset thickness.
[0182] The precursors of aluminum fluoride include AlCl3 and TiF4. In the step of preparing the aluminum fluoride protective film, the reaction chamber is evacuated and the pressure is reduced to 10Pa or below; AlCl3 gas is introduced into the reaction chamber and maintained for 10s-20s; purge gas is introduced into the reaction chamber, the vacuum is opened, and the unreacted AlCl3 gas is taken away; the pressure in the reaction chamber is reduced to 10Pa or below, TiF4 gas is introduced into the reaction chamber and maintained for 10s-20s; purge gas is introduced into the reaction chamber, the vacuum is opened, and the unreacted TiF4 gas is taken away; the above steps are repeated to obtain an aluminum fluoride protective film of a preset thickness.
[0183] It is understandable that AlCl 3 and TiF 4 are solid at room temperature. In order to obtain a gaseous precursor, a temperature that can vaporize the precursor is set to vaporize the solid to obtain a gaseous precursor.
[0184] It can be understood that the step of adding AlCl3 gas into the reaction chamber and maintaining it for 10s-20s is to introduce an appropriate amount of AlCl3 gas into the reaction chamber. The time for introducing the gas can be selected according to actual needs and is not specifically limited in this application.
[0185] The purpose of introducing a purge gas into the reaction chamber is to remove other unreacted gases or impurities. The purge gas is an inert gas, such as argon.
[0186] In one embodiment, the steps of introducing a lithium fluoride precursor into a reaction chamber, forming a protective film on the surface of the coating, and opening the vacuum to remove unreacted precursor include: evacuating the reaction chamber to reduce the pressure to 10Pa or below; introducing alkyl lithium vapor into the reaction chamber and maintaining it for 10s-20s; introducing purge gas into the reaction chamber, opening the vacuum, and removing unreacted alkyl lithium vapor; reducing the pressure in the reaction chamber to 10Pa or below, introducing TiF4 vapor into the reaction chamber and maintaining it for 10s-20s; introducing purge gas into the reaction chamber and opening the vacuum to remove unreacted TiF4 vapor; repeating the above steps to obtain a lithium fluoride protective film of a preset thickness.
[0187] The precursors of lithium fluoride include alkyl lithium and TiF4. In the step of preparing the lithium fluoride protective film, the reaction chamber is evacuated and the pressure is reduced to 10 Pa or below; alkyl lithium vapor is introduced into the reaction chamber and maintained for 10s-20s; purge gas is introduced into the reaction chamber, the vacuum is opened, and unreacted alkyl lithium vapor is taken away; the pressure in the reaction chamber is reduced to 10 Pa or below, TiF4 vapor is introduced into the reaction chamber and maintained for 10s-20s; purge gas is introduced into the reaction chamber, the vacuum is opened, and unreacted TiF4 vapor is taken away; and the above steps are repeated to obtain a lithium fluoride protective film of a preset thickness.
[0188] Alkyl lithium can be lithium tert-butoxide, butyl lithium, phenyl lithium, etc. For example, lithium tert-butoxide and TiF4 are solid at room temperature. In order to obtain a gaseous precursor, a temperature that can vaporize the precursor is set to vaporize the solid to obtain a gaseous precursor.
[0189] In one embodiment, the steps of preparing a positive electrode plate include: mixing a positive electrode material with a reactive substance to react, thereby forming a coating layer on the surface of the positive electrode material; mixing the positive electrode material with the coating layer, a binder, and a conductive agent, adding a solvent and stirring to obtain a positive electrode slurry; applying the positive electrode slurry to a current collector, and drying to obtain a positive electrode plate; wherein the reactive substance includes at least one of a sulfur compound and a boron compound.
[0190] For example, sulfur compounds and boron compounds are mixed with positive electrode materials and reacted under certain conditions to form a coating layer on the surface of the positive electrode material; the positive electrode material with the coating layer, a binder, and a conductive agent are mixed, and a solvent is added and stirred to obtain a positive electrode slurry; the positive electrode slurry is coated on a current collector and dried to obtain a positive electrode sheet.
[0191] In one embodiment, the step of preparing the positive electrode sheet includes: mixing the positive electrode material, the binder, the conductive agent, and ammonium fluoride, adding a solvent and stirring to obtain a positive electrode slurry; applying the positive electrode slurry to a current collector, and drying to obtain a positive electrode sheet.
[0192] Introducing ammonium fluoride during the slurry preparation process allows it to react with residual lithium on the surface of the positive electrode material to form a lithium fluoride coating. This can reduce the amount of residual alkali on the positive electrode material surface as needed, thereby reducing battery polarization. Compared to mixing sulfur compounds and boron compounds with the positive electrode material and reacting them under certain conditions to form a coating on the positive electrode material surface, the use of ammonium fluoride eliminates the need for additional steps. Ammonium fluoride can be added directly during the slurry preparation process, reducing process steps and improving the production efficiency of positive electrode sheets.
[0193] By converting residual lithium as a reactant into an effective lithium fluoride protective layer, the slurry gel condition is effectively improved, the residual lithium is removed, and a fast ion conductor coating layer is established, thereby improving the conductivity of the positive electrode sheet, reducing the polarization of the lithium-ion battery, and improving the power performance of the lithium-ion battery.
[0194] In one embodiment, the amount of ammonium fluoride added ranges from 0.009% to 4.5% by mass of the positive electrode material, and preferably from 0.45% to 1.1%.
[0195] For example, the added mass of ammonium fluoride is M1, and the mass of the positive electrode material is M2. Then, the calculation formula for the added amount of ammonium fluoride to the mass of the positive electrode material is M1 / M2×100%.
[0196] The amount of residual lithium in the positive electrode material can be measured by hydrochloric acid titration, and the amount of ammonium fluoride required can be calculated based on the measured amount of residual lithium. The amount of ammonium fluoride added ranges from 0.009% to 4.5% of the mass of the positive electrode material, preferably from 0.45% to 1.1%.
[0197] In the above-mentioned 0.009% to 4.5%, the values include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 0.009%, 0.01%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4.5%, etc.
[0198] In the above-mentioned 0.45% to 1.1%, the values include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 0.45%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, 1.0%, 1.1%, etc.
[0199] In one embodiment, the step of mixing the positive electrode material, the binder, the conductive agent, and ammonium fluoride, adding a solvent and stirring to obtain a positive electrode slurry includes: mixing the positive electrode material, the binder, the conductive agent, and ammonium fluoride for 5 minutes to 60 minutes, adding the solvent, stirring at a speed of 300 r / min to 2000 r / min for 30 minutes to 3 hours, removing bubbles and exhausting air to obtain a positive electrode slurry with a solid content of 60% to 85%.
[0200] In order to fully mix ammonium fluoride and the positive electrode material in the process of preparing the slurry so as to achieve effective reaction, during the operation, the positive electrode material, binder, conductive agent and ammonium fluoride are mixed for 5min-60min, the solvent is added, and the mixture is stirred at a speed of 300r / min~2000r / min for 30min to 3h, and the bubbles are removed and the air is exhausted to obtain a positive electrode slurry with a solid content of 60%-85%.
[0201] Ammonium fluoride reacts with residual lithium, and the chemical reaction equations involved are as follows: 2NH4F+LiCO3→2LiF↓+(NH4)2CO3, NH4F+LiOH→LiF↓+NH3↑+H2O↑.
[0202] The by-products of the reaction are all volatile or decomposed substances. In order to facilitate the removal of by-products, degassing and exhaust are performed during the operation.
[0203] That is, a considerable amount of ammonium fluoride is used with residual lithium as the source, and the ammonium fluoride and the positive electrode material are fully contacted, mixed and reacted under the slurry stirring conditions. After the stirring is completed, part of the gas product is removed by exhausting the gas in the defoaming stage.
[0204] In one embodiment, the step of applying the positive electrode slurry to the current collector and drying to obtain the positive electrode sheet includes: applying the positive electrode slurry to the current collector and drying at a temperature of 100° C.-170° C. to obtain the positive electrode sheet.
[0205] In order to effectively ensure the decomposition and removal of the reaction by-product (NH4)2CO3, the ammonium carbonate is decomposed and removed by adjusting the drying temperature during the drying process. The drying temperature is 100℃-170℃. Under this drying condition, the product (NH4)2CO3 decomposes and is discharged through the airway, which is conducive to the rapid decomposition and removal of (NH4)2CO3 and improves production efficiency.
[0206] In one embodiment, the mass of residual lithium in the positive electrode material accounts for the mass of the positive electrode material and satisfies Li2CO3≥0.02% and LiOH≥0.2%.
[0207] In order to prepare a coating layer with suitable coating quality so that the beneficial effects of the coating layer are obvious, the proportion of residual lithium in the positive electrode material to the positive electrode material mass satisfies Li2CO3≥0.02% and LiOH≥0.2%.
[0208] A full range of protective films are formed on the surface of the positive electrode material and the surface and depth of the positive electrode sheet. The technical effects of the protective film are as follows:
[0209] The present application converts residual lithium as a reactant into an effective coating layer, effectively improving the slurry gel condition, removing residual lithium, establishing a fast ion conductor coating layer, improving the conductivity of the positive electrode plate, reducing the polarization of the lithium-ion battery, and improving the power performance of the lithium-ion battery; and on the basis of the coating layer, adding a lithium fluoride and / or aluminum protective film to protect the positive electrode from interfacial side reactions with the electrolyte. The composite protective layer constructed by the two processes can further protect the structural stability and surface stability of the positive electrode material during deep lithium deintercalation, which is beneficial to improving the battery life.
[0210] In one embodiment, the present application further provides an electrode assembly, which includes the positive electrode plate as described above, or includes a positive electrode plate produced by the method for producing the positive electrode plate as described above.
[0211] Since the positive electrode plate adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.
[0212] In one embodiment, the present application further provides a battery cell, which includes the electrode assembly as described above.
[0213] Since the electrode assembly adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.
[0214] In one embodiment, the present application further provides a battery, which includes the battery cell as described above.
[0215] Since the battery cell adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described in detail here.
[0216] In one embodiment, the present application further provides an electrical device, which includes the battery cell or battery as described above.
[0217] Since the battery cell or battery adopts all the technical solutions of all the above embodiments, it at least has all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.
[0218] In addition, the battery (battery cell, battery module, battery pack) and the electric device of the present application will be described below with reference to the drawings as appropriate.
[0219] In one embodiment of the present application, a secondary battery is provided.
[0220] Typically, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the battery's charge and discharge process, active ions are embedded in and released from the positive and negative electrodes. The electrolyte conducts ions between the positive and negative electrodes. The separator is located between the positive and negative electrodes, primarily preventing a short circuit between the positive and negative electrodes while allowing ions to pass through. The separator is the separator described above in this application.
[0221] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector.
[0222] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.
[0223] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0224] In some embodiments, when the secondary battery is a lithium-ion battery, the positive electrode active material may adopt the positive electrode active material for lithium-ion batteries known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as battery positive electrode active materials may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.
[0225] The battery's charge and discharge processes involve the intercalation and deintercalation of lithium, leading to different molar Li contents at different discharge states. The molar Li contents listed in this application for cathode materials refer to the initial state of the material, i.e., the state before addition of the materials. When the cathode material is used in a battery system, the molar Li content will change after charge and discharge cycles.
[0226] In the list of positive electrode materials in this application, the molar content of O is only a theoretical value. Lattice oxygen release will cause the molar content of oxygen to change, and the actual molar content of O will fluctuate.
[0227] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.
[0228] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0229] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0230] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0231] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0232] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0233] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0234] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0235] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0236] In some embodiments, the negative electrode film layer may optionally further include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0237] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0238] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. This application has no specific restrictions on the type of electrolyte, and it can be selected according to needs.
[0239] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.
[0240] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0241] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0242] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0243] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0244] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0245] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.
[0246] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0247] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0248] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG5 shows a battery cell 5 having a square structure as an example.
[0249] In some embodiments, referring to Figure 6, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the diaphragm can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0250] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.
[0251] FIG7 shows an example battery module 4. Referring to FIG7 , within the battery module 4, multiple battery cells 5 may be arranged sequentially along the length of the battery module 4. Of course, they may also be arranged in any other manner. Furthermore, the multiple battery cells 5 may be secured together using fasteners.
[0252] Optionally, the battery module 4 may further include a housing having an accommodation space, and the plurality of battery cells 5 are accommodated in the accommodation space.
[0253] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.
[0254] Figures 8 and 9 illustrate an example battery pack 1. Referring to Figures 8 and 9 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be positioned over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0255] In addition, the present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.
[0256] As an electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.
[0257] Figure 10 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.
[0258] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.
[0259] Example
[0260] Example 1
[0261] Cathode slurry preparation
[0262] The positive electrode material LiNi 0.8 Co 0.1 Mn 0.1 O2, binder PVDF, and conductive agent carbon black are mixed in a ratio of 90:5:5, and the corresponding ammonium fluoride is added according to the residual lithium amount (the percentage of residual alkali in the positive electrode material is 0.2%, and the mass of the added ammonium fluoride accounts for 0.18% of the mass of the positive electrode material). After dry mixing for 15 minutes, NMP is added and stirred at a high speed of 1000 rpm for 120 minutes, and then defoamed and exhausted to finally obtain a uniform positive electrode slurry with a solid content of 70%.
[0263] Positive electrode preparation
[0264] The above-mentioned positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, and the oven temperature is set to 130°C to dry the electrode; then an aluminum fluoride thin film layer is deposited on the positive electrode using an atomic layer deposition device. Precursor A is ground TiF4, precursor B is AlCl3, and the deposition temperature is 250°C. The positive electrode piece is placed in the atomic layer deposition ALD reaction chamber, and the deposition parameters and deposition process are as follows: 1) Vacuum the reaction chamber and wait until the pressure drops below 10Pa; 2) Open the valve of precursor A, put AlCl3 vapor into the reaction chamber, and maintain it for 15 seconds. The temperature of the generated vapor is 120°C; 3) Argon is introduced into the reaction chamber for 120 seconds, and then the vacuum is opened to take away the unreacted precursor A; 4) Wait until the pressure in the reaction chamber drops to 10Pa, open the valve of precursor B, put TiF4 vapor into the reaction chamber, and maintain it for 15 seconds. The temperature of the generated vapor is 120°C; 5) Argon is introduced into the reaction chamber for 100 seconds, and then the vacuum is opened to take away the unreacted precursor B; from 1) to 5) is a complete cycle process, and the above cycle is repeated to obtain a protective film with a thickness of about 10nm; the electrode piece treated with the protective film is subjected to cold pressing, slitting and other processes to obtain an assembleable positive electrode piece.
[0265] Preparation of battery components and finished products
[0266] The negative electrode material graphite, conductive agent acetylene black, binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC) are thoroughly stirred and mixed in a deionized water solvent system in a mass ratio of 90:5:2:2:1, and then coated on the negative electrode current collector copper foil. After drying, the negative electrode sheet is obtained by cold pressing, slitting and other processes; a PE porous polymer membrane treated with alumina ceramic is used as an isolation membrane; the electrolyte is a 1 mol / L LiPF6 solution, and the organic solvent is ethylene carbonate (EC), diethyl carbonate (DEC), and dimethyl carbonate (DMC) in a volume ratio of 5:2:3, and film-forming additives are appropriately added to obtain the required electrolyte; the positive electrode sheet, isolation membrane, and negative electrode sheet are assembled in a dry room environment with a humidity of less than 2%, and then baked and dried, and then injected with the corresponding electrolyte and packaged. A soft-pack battery with a capacity of 2.8Ah is prepared through a formation test, and the electrical performance test is carried out.
[0267] Example 2
[0268] Cathode slurry preparation
[0269] The positive electrode material LiNi 0.8 Co 0.1 Mn 0.1 O2, binder PVDF, and conductive agent carbon black are mixed in a ratio of 90:5:5, and the corresponding ammonium fluoride is added according to the residual lithium amount. After dry mixing for 15 minutes, NMP is added and stirred at a high speed of 1000 rpm for 120 minutes, and then defoamed and exhausted to finally obtain a uniform positive electrode slurry with a solid content of 70%.
[0270] Positive electrode preparation
[0271] The above-mentioned positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, and the oven temperature is set to 130°C to dry the electrode; then, an atomic layer deposition device is used to deposit an aluminum fluoride protective film and a lithium fluoride protective film on the positive electrode, wherein the aluminum fluoride film precursor A is ground TiF4, the precursor B is AlCl3, the lithium fluoride film precursor A is lithium tert-butoxide, the precursor B is TiF4, and the deposition temperature is 250°C. The positive electrode is placed in the atomic layer deposition (ALD) reaction chamber. The deposition parameters and deposition process of the aluminum fluoride composite film are as follows: 1) Vacuum the reaction chamber until the pressure drops below 10 Pa; 2) Open the valve of precursor A, add AlCl3 vapor into the reaction chamber, and maintain it for 15 seconds. The temperature of the generated vapor is 120°C; 3) Argon is introduced into the reaction chamber for 120 seconds, and then the vacuum is opened to remove the unreacted precursor A; 4) When the pressure in the reaction chamber drops to 10 Pa, open the valve of precursor B, add TiF4 into the reaction chamber, and maintain it for 15 seconds. The temperature of the generated vapor is 120°C; 5) Argon is introduced into the reaction chamber for 120 seconds, and then the vacuum is opened to remove the unreacted precursor B; 1)-5) is a complete aluminum fluoride deposition cycle. The deposition parameters and process for the lithium fluoride composite film are as follows: 1) Evacuate the reaction chamber until the pressure drops below 10 Pa; 2) Open the valve for precursor A and introduce lithium tert-butoxide vapor into the reaction chamber, maintaining the pressure for 15 seconds. The generated vapor temperature is 165°C. 3) Argon is introduced into the reaction chamber for 120 seconds, and then the vacuum is released to remove any unreacted precursor A. 4) After the pressure in the reaction chamber drops to 10 Pa, open the valve for precursor B and introduce TiF4 vapor into the reaction chamber, maintaining the pressure for 15 seconds. The generated vapor temperature is 120°C. 5) Argon is introduced into the reaction chamber for 120 seconds, and then the vacuum is released to remove any unreacted precursor B. The steps from 1) to 5) constitute a complete lithium fluoride deposition cycle. A protective film approximately 10 nm thick is obtained by alternating the deposition of LiF and AlF3 in a 1:1 ratio. The electrode, treated with the protective film, undergoes cold pressing and slitting to obtain an assembled positive electrode.
[0272] Preparation of battery components and finished products is the same as in step 1
[0273] Example 3
[0274] On the basis of Example 2, the number of deposition cycles was adjusted to obtain a protective film with a thickness of 20 nm.
[0275] Example 4
[0276] Cathode slurry preparation
[0277] The positive electrode material LiNi 0.8 Co0.1 Mn 0.1 O2, binder PVDF, and conductive agent carbon black were dry-mixed in a ratio of 90:5:5 for 15 minutes, and then NMP was added and stirred at a high speed of 1000 rpm for 120 minutes, and then defoamed to finally obtain a uniform positive electrode slurry with a solid content of 70%.
[0278] The positive electrode sheet was prepared in the same manner as in Example 2.
[0279] Preparation of battery components and finished products is the same as in step 1
[0280] Example 5-Example 9
[0281] On the basis of Example 1, the number of deposition cycles was adjusted to obtain protective films of different thicknesses.
[0282] Comparative Example 1
[0283] Cathode slurry preparation
[0284] The positive electrode material LiNi 0.8 Co 0.1 Mn 0.1 O2, binder PVDF, and conductive agent carbon black were dry-mixed in a ratio of 90:5:5 for 15 minutes, and then NMP was added and stirred at a high speed of 1000 rpm for 120 minutes, and then defoamed to finally obtain a uniform positive electrode slurry with a solid content of 70%.
[0285] Positive electrode preparation
[0286] The positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil and dried.
[0287] Preparation of battery components and finished products is the same as in step 1
[0288] Comparative Example 2
[0289] Cathode slurry preparation
[0290] The preparation method of the positive electrode slurry is the same as that in Example 1.
[0291] Positive electrode preparation
[0292] The positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil and dried.
[0293] Preparation of battery components and finished products is the same as in step 1
[0294] The prepared batteries were tested using the following method:
[0295] 1. Slurry static test
[0296] The prepared positive electrode slurry was placed in an environment with a temperature of 25° C. and a humidity of 40% for 24 h, and the surface state of the positive electrode slurry was observed.
[0297] 2. Gas production test
[0298] The fully charged lithium-ion battery was placed in a 70°C constant temperature box. After 30 days, its volume was measured by the discharge method and converted into mL / Ah.
[0299] 3. Cycle test
[0300] The charge and discharge test was carried out for 300 cycles at 1C / 1C 2.8-4.25V voltage range at a temperature of 45°C, and the capacity retention rate was recorded.
[0301] Table 1 Experimental data list
[0302] It can be seen from the above table that: this application can effectively improve the slurry gel condition by adding additives to remove residual lithium when stirring the positive electrode material, and can effectively improve the specific capacity of the battery through the protective film, reduce the high-temperature gas production level, and improve the high-temperature cycle life of the battery. This is because while the composite protective film purifies the residual lithium, its product and the composite protective film have ion transmission properties, which can improve the ion transmission performance of the positive electrode material surface. At the same time, the protective film can effectively protect the surface of the positive electrode material under high-temperature degradation conditions, inhibit the oxidation of the active substance to the electrolyte and the side reaction process, maintain the structural stability and surface stability of the positive electrode material, and significantly improve the cycle life and gas production level of the battery.
[0303] The above is only a preferred embodiment of the present application and does not limit the patent scope of the present application. All equivalent structural transformations made based on the contents of the present application specification and drawings, or direct / indirect application in other related technical fields, are included in the patent protection scope of the present application.
Claims
1. A positive electrode sheet, wherein: The positive electrode plate includes a current collector and a coating disposed on at least one side of the current collector. A protective film is disposed on the surface of the coating. The material of the protective film includes fluoride.
2. The positive electrode sheet according to claim 1, wherein: The thickness of the protective film ranges from 1 nm to 50 nm, preferably from 5 nm to 20 nm.
3. The positive electrode sheet according to claim 1 or 2, wherein: The fluoride includes at least one of lithium fluoride and aluminum fluoride.
4. The positive electrode sheet according to any one of claims 1 to 3, wherein: The protective film comprises a lithium fluoride protective film and an aluminum fluoride protective film, and the lithium fluoride protective film and the aluminum fluoride protective film are stacked on the surface of the coating; And / or, the protective film includes a lithium fluoride protective film and an aluminum fluoride protective film, at least a portion of the surface of the coating is provided with the lithium fluoride protective film, and at least another portion of the surface of the coating is provided with the aluminum fluoride protective film.
5. The positive electrode sheet according to any one of claims 1 to 4, wherein: The coating layer includes a positive electrode material, a coating layer is formed on the surface of the positive electrode material, and the coating layer includes at least one of a sulfur-containing compound, a boron-containing compound, and a fluoride.
6. The positive electrode sheet according to claim 5, wherein: The coating layer is lithium fluoride.
7. The positive electrode sheet according to claim 6, wherein: The mass percentage of the lithium fluoride to the total mass of the positive electrode material is 0.01% to 5%, preferably 0.5% to 1.2%.
8. The positive electrode sheet according to any one of claims 1 to 7, wherein: The general formula of the positive electrode material in the coating is Li x Ni y M 1-y O2, 0.9≤x≤1.15, 0.6≤y≤1, M is selected from one or more of Co, Mn, and Al; And / or, the general formula of the positive electrode material in the coating is xLi2MnO3·(1-x)LiMO2, 0.1≤x≤0.9, and M is selected from one or more of Co, Mn, and Al.
9. A method for preparing a positive electrode sheet according to any one of claims 1 to 8, wherein: include: Prepare the positive electrode; preparing fluoride precursors; A protective film is formed on the coating surface of the positive electrode plate by thin film deposition technology.
10. The method for preparing a positive electrode sheet according to claim 9, wherein: The thin film deposition technology includes an atomic layer deposition process.
11. The method for preparing a positive electrode sheet according to claim 9 or 10, wherein: The fluoride includes lithium fluoride and / or aluminum fluoride.
12. The method for preparing a positive electrode sheet according to claim 10 or 11, wherein: The step of forming a coating layer on the coating surface of the positive electrode plate by an atomic layer deposition process includes: The positive electrode sheet is placed in an atomic layer deposition reaction chamber, vacuumed, and the deposition temperature is set to 200° C.-250° C.; A suitable fluoride precursor is introduced into the reaction chamber to form a protective film on the surface of the coating, and the vacuum is opened to remove the unreacted precursor. The above steps are repeated to obtain a protective film of a preset thickness.
13. The method for preparing a positive electrode sheet according to claim 12, wherein: The step of introducing a suitable fluoride precursor into the reaction chamber to form a protective film on the surface of the coating, opening the vacuum to remove the unreacted precursor, and repeating the above steps to obtain a protective film of a preset thickness includes: A precursor of aluminum fluoride is introduced into the reaction chamber to form a protective film on the surface of the coating, and the vacuum is opened to remove the unreacted precursor; A lithium fluoride precursor is introduced into the reaction chamber to form a protective film on the surface of the coating, and the vacuum is opened to remove the unreacted precursor; Repeat the above steps to obtain a protective film of a preset thickness.
14. The method for preparing a positive electrode sheet according to claim 13, wherein: The step of introducing an aluminum fluoride precursor into the reaction chamber to form a protective film on the surface of the coating and opening the vacuum to remove the unreacted precursor comprises: The reaction chamber is evacuated to reduce the pressure to 10Pa or less; Add AlCl3 gas into the reaction chamber and maintain for 10s-20s; Introduce purge gas into the reaction chamber, open the vacuum, and take away the unreacted AlCl3 gas; The pressure in the reaction chamber is reduced to 10 Pa or less, and TiF4 gas is introduced into the reaction chamber for 10s-20s; A purge gas is introduced into the reaction chamber, and the vacuum is opened to remove the unreacted TiF4 gas; Repeat the above steps to obtain an aluminum fluoride protective film of a preset thickness.
15. The method for preparing a positive electrode sheet according to claim 13 or 14, wherein: The steps of introducing a lithium fluoride precursor into the reaction chamber, forming a protective film on the surface of the coating, and opening the vacuum to remove the unreacted precursor include: The reaction chamber is evacuated to reduce the pressure to 10Pa or less; Alkyl lithium vapor is introduced into the reaction chamber and maintained for 10s-20s; Introducing purge gas into the reaction chamber, opening the vacuum, and taking away unreacted alkyl lithium vapor; The pressure in the reaction chamber is reduced to 10 Pa or less, and TiF4 vapor is introduced into the reaction chamber for 10s-20s; A purge gas is introduced into the reaction chamber, and the vacuum is opened to remove the unreacted TiF4 vapor; Repeat the above steps to obtain a lithium fluoride protective film with a preset thickness.
16. The method for preparing a positive electrode sheet according to any one of claims 9 to 15, wherein: The steps of preparing the positive electrode include: Mixing the positive electrode material with the reactive substance to form a coating layer on the surface of the positive electrode material; The positive electrode material with the coating layer, the binder, and the conductive agent are mixed, and a solvent is added and stirred to obtain a positive electrode slurry; Applying the positive electrode slurry to a current collector and drying it to obtain a positive electrode sheet; Wherein, the reactive substance includes at least one of a sulfur compound and a boron compound.
17. The method for preparing a positive electrode sheet according to any one of claims 9 to 15, wherein: The steps of preparing the positive electrode include: The positive electrode material, the binder, the conductive agent and the ammonium fluoride are mixed, and the solvent is added and stirred to obtain a positive electrode slurry; The positive electrode slurry is coated on a current collector and dried to obtain a positive electrode sheet.
18. The method for preparing a positive electrode sheet according to claim 17, wherein: The amount of ammonium fluoride added is in the range of 0.009% to 4.5% of the mass of the positive electrode material, preferably 0.45% to 1.1%.
19. The method for preparing a positive electrode sheet according to any one of claims 17 or 18, wherein: The step of mixing the positive electrode material, the binder, the conductive agent and the ammonium fluoride, adding the solvent and stirring to obtain the positive electrode slurry comprises: The positive electrode material, binder, conductive agent and ammonium fluoride are mixed for 5-60 minutes, and a solvent is added. The mixture is stirred at a speed of 300-2000 r / min for 30-3 hours, and bubbles are removed and air is evacuated to obtain a positive electrode slurry with a solid content of 60%-85%.
20. The method for preparing a positive electrode sheet according to any one of claims 17 to 19, wherein: The step of applying the positive electrode slurry to the current collector and drying to obtain the positive electrode sheet includes: The positive electrode slurry is coated on a current collector and dried at a temperature of 100° C. to 170° C. to obtain a positive electrode sheet.
21. The method for preparing a positive electrode sheet according to any one of claims 16 to 20, wherein: The mass of residual lithium in the positive electrode material accounts for the mass of the positive electrode material in a ratio of Li2CO3≥0.02% and LiOH≥0.2%.
22. An electrode assembly, wherein: The electrode assembly includes the positive electrode sheet according to any one of claims 1 to 8, or includes a positive electrode sheet prepared by the method for preparing a positive electrode sheet according to any one of claims 9 to 21.
23. A battery cell, wherein: The battery cell includes the electrode assembly as claimed in claim 22 .
24. A battery, wherein: The battery comprises the battery cell as claimed in claim 23.
25. An electrical device, wherein: The electrical device comprises the battery cell as claimed in claim 23 or the battery as claimed in claim 24.
Citation Information
Patent Citations
Layered lithium-rich anode material clad by metal fluoride, and preparation method thereof
CN102496722A
Fluoride stabilizing layer of lithium-sulfur battery, preparation method and lithium-sulfur battery
CN110718692A
Positive pole piece and lithium ion battery by using same
CN110970613A
Method for manufacturing anodes for lithium-ion batteries
CN112055903A
Positive electrode, method for preparing the same and electrochemical device
US20190207202A1