Electrochemical device and electronic device
By designing a two-layer structure in the negative electrode sheet of the lithium-ion battery, using a combination of graphite and silicon-based materials to adjust the impedance ratio, the problem of capacity attenuation of lithium-ion batteries caused by silicon-based materials is solved, and a higher capacity retention rate is achieved. and cycle performance.
Patent Information
- Application Number
- PCT/CN2023/141698
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2023-12-25
- Publication Date
- 2024-10-03
AI Technical Summary
Silicon-based materials cause volume expansion and contraction of more than 300% during the lithium ion deintercalation process of lithium-ion batteries, leading to capacity fading problems in electrochemical devices.
Design an electrochemical device. The negative electrode plate includes a two-layer structure. The first layer is mainly composed of graphite, and the second layer is composed of graphite and silicon-based materials. The impedance ratio of the first layer to the second layer is 0.7 to 0.9. By adjusting the Si content, conductive agent content, binder type, coating formula and compaction density of the coating, it is ensured that the second layer of silicon-based material has a smaller magnification rate during the charge and discharge process and slows down the capacity fading rate.
Without basically losing the energy density of the electrochemical device, the capacity retention rate of the electrochemical device is improved, and the cycle performance of the lithium-ion battery is significantly improved.
Smart Images

Figure CN2023141698_03102024_PF_FP_ABST
Abstract
Description
Electrochemical devices and electronic devices
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application is based on the Chinese patent application with application number 202310303762.8, application date March 27, 2023, and name “Electrochemical Devices and Electronic Devices”, and claims the priority of the Chinese patent application. The entire content of the Chinese patent application is hereby introduced into this application as a reference. Technical Field
[0003] The present application relates to the field of electrochemical energy storage, and in particular to electrochemical devices and electronic devices. Background Art
[0004] With the development of electrochemical energy storage technology, the energy density and cycle performance of electrochemical devices (such as lithium-ion batteries) have been increasingly demanded. Using silicon-based materials as negative electrode active materials can significantly improve the energy density of electrochemical devices. However, silicon-based materials experience volume expansion and contraction exceeding 300% during lithium ion insertion and extraction, leading to capacity degradation and other issues. Therefore, further improvements in this area are desired.
[0005] Summary of the Invention
[0006] The present application provides an electrochemical device comprising a negative electrode sheet, the negative electrode sheet comprising a negative electrode current collector, a first layer, and a second layer, wherein the negative electrode current collector is positioned between the first and second layers. The first layer comprises a first negative electrode active material, and the second layer comprises a second negative electrode active material, wherein the first negative electrode active material comprises graphite, and the second negative electrode active material comprises graphite and a silicon-based material. The ratio of the impedance of the first layer to the impedance of the second layer is 0.7 to 0.9.
[0007] In some embodiments, the ratio of the capacity of the first layer to the capacity of the second layer is 0.6 to 1. In some embodiments, the ratio of the capacity of the first layer to the capacity of the second layer is 0.7 to 1. In some embodiments, the mass percentage of the silicon-based material in the second layer is 6% to 40%. In some embodiments, the mass percentage of the silicon-based material in the second layer is 12% to 20%. In some embodiments, the second layer further comprises a binder, and the mass percentage of the binder in the second layer is 1.4% to 5%. In some embodiments, the second layer further comprises carbon nanotubes, and the mass percentage of the carbon nanotubes in the second layer is 0.3% to 0.7%. In some embodiments, the second layer further comprises sodium carboxymethyl cellulose, and the mass percentage of the sodium carboxymethyl cellulose in the second layer is 0.3% to 0.7%. In some embodiments, the silicon-based material comprises at least one of silicon, silicon-carbon material, or silicon-oxygen material.
[0008] An embodiment of the present application further provides an electronic device comprising the above-mentioned electrochemical device.
[0009] In the present application, the first negative electrode active material in the first layer of the negative electrode sheet includes graphite, and the second negative electrode active material in the second layer includes graphite and a silicon-based material. The ratio of the impedance of the first layer to the impedance of the second layer is 0.7 to 0.9, so that the second negative electrode active layer has a lower rate during the charge and discharge process, and can improve the capacity retention rate of the electrochemical device without substantially losing the energy density of the electrochemical device. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] FIG. 1 illustrates a cross-sectional view of a negative electrode sheet along a width direction according to some embodiments. DETAILED DESCRIPTION
[0011] The following embodiments may enable those skilled in the art to more fully understand the present application, but do not limit the present application in any way.
[0012] Some embodiments of the present application provide an electrochemical device, which includes a negative electrode plate. FIG1 shows a cross-sectional view of a negative electrode plate along the width direction according to some embodiments. In some embodiments, as shown in FIG1 , the negative electrode plate includes a negative electrode current collector 110, a first layer 111, and a second layer 112, and the negative electrode current collector 110 is located between the first layer 111 and the second layer 112. In some embodiments, the first layer 111 includes a first negative electrode active material, and the first negative electrode active material includes graphite and substantially does not include silicon-based materials. It should be understood that when the mass percentage of silicon-based materials in the first negative electrode active material is less than 0.2%, it can be considered that the first negative electrode active material substantially does not include silicon-based materials. By completely separating the silicon-based material from the graphite in the first layer 111, the ineffective pores between the graphite in the first layer 111 during the cycle are reduced, thereby reducing the overall expansion of the negative electrode plate.
[0013] In some embodiments, the second layer 112 includes a second negative electrode active material, which includes graphite and a silicon-based material. Therefore, the present application concentrates the silicon-based material on one side of the negative electrode current collector 110. Typically, the weight percentage of the silicon-based material in the layers on both sides of the negative electrode current collector is the same. In the present application, this is equivalent to replacing the silicon-based material on one side with an equal volume of graphite, and replacing the graphite on the other side with an equal volume of silicon-based material.
[0014] In some embodiments, the ratio of the impedance of the first layer 111 to the impedance of the second layer 112 is 0.7 to 0.9. In some embodiments, the impedance of the first layer 111 and the impedance of the second layer 112 can be adjusted by the Si content, conductive agent content, binder type, coating formula, coating quality, and compaction density of the corresponding coating. Since the impedance of the first layer 111 is less than the impedance of the second layer 112, the first layer 111 can be allowed to have a larger charge and discharge rate, and the second layer 112 can have a smaller charge and discharge rate. In this way, without changing the overall charge and discharge rate of the electrochemical device, reducing the charge and discharge rate of the second layer 112 containing silicon-based materials can slow down the capacity decay rate of the negative electrode and improve the capacity retention rate of the electrochemical device.
[0015] In some embodiments, the ratio of the capacity of the first layer 111 to the capacity of the second layer 112 is 0.6 to 1. In some embodiments, the capacity of the first layer 111 can be adjusted by coating quality, and the capacity of the second layer 112 can be adjusted by coating quality and / or Si content. By making the ratio of the capacity of the first layer 111 to the capacity of the second layer 112 0.6 to 1, the capacity retention rate of the electrochemical device can be improved.
[0016] In some embodiments, the ratio of the capacity of the first layer 111 to the capacity of the second layer 112 is 0.7 to 1. When the ratio of the capacity of the first layer 111 to the capacity of the second layer 112 is 0.7 to 1, the capacity retention rate of the electrochemical device is more significantly improved.
[0017] In some embodiments, the mass percentage of the silicon-based material in the second layer 112 is 6% to 40%, or the mass percentage of silicon in the second layer 112 is 4% to 20%. In some embodiments, because only silicon contributes to the capacity of the silicon-based material, when the mass percentage of the silicon-based material in the second layer 112 is less than 6%, the mass percentage of silicon is very small, and the energy density gain of the electrochemical device decreases significantly. When the mass percentage of the silicon-based material in the second layer 112 is greater than 40%, the mass percentage of silicon is high, and the cyclic expansion of the second layer 112 increases. In some embodiments, the mass percentage of the silicon-based material in the second layer 112 is 12% to 20%. When the mass percentage of the silicon-based material in the second layer 112 is 12% to 20%, or when the mass percentage of silicon in the second layer 112 is 4% to 10%, the capacity retention of the electrochemical device is more significantly improved.
[0018] In some embodiments, the silicon-based material includes at least one of silicon, silicon-oxygen material, silicon-carbon material, or silicon-oxygen-carbon material. In some embodiments, the negative electrode current collector 110 may be at least one of copper foil, nickel foil, or a carbon-based current collector. The first layer 111 and the second layer 112 may each include a conductive agent, a binder, and a thickener (e.g., sodium carboxymethyl cellulose). In some embodiments, the conductive agent in the first layer 111 and the second layer 112 may include at least one of conductive carbon black, Ketjen black, flake graphite, graphene, carbon nanotubes, or carbon fibers. In some embodiments, the binder in the first layer 111 and the second layer 112 may include at least one of carboxymethyl cellulose (CMC), polyacrylic acid, polyvinyl pyrrolidone, polyaniline, polyimide, polyamide-imide, polysiloxane, styrene-butadiene rubber, epoxy resin, polyester resin, polyurethane resin, or polyfluorene. In some embodiments, the mass percentage of the first negative electrode active material in the first layer is 97% to 98%. In some embodiments, the mass percentage of the second negative electrode active material in the second layer is 93.6% to 98%. In some embodiments, the mass ratio of the first negative electrode active material, thickener, and binder in the first layer 111 can be (97 to 98): (0.2 to 0.6): (1.8 to 2.4). In some embodiments, the mass ratio of the second negative electrode active material, conductive agent, binder, and thickener in the second layer 112 can be (93.6 to 98): (0.3 to 0.7): (1.4 to 5): (0.3 to 0.7). In some embodiments, the second layer 112 further includes a binder, and the mass percentage of the binder in the second layer 112 is 1.4% to 5%. In some embodiments, the second layer 112 further includes carbon nanotubes, and the mass percentage of the carbon nanotubes in the second layer 112 is 0.3% to 0.7%. In some embodiments, the second layer 112 further includes sodium carboxymethyl cellulose, and the mass percentage of the sodium carboxymethyl cellulose in the second layer 112 is 0.3% to 0.7%.
[0019] In some embodiments, the electrochemical device further includes a positive electrode sheet and a separator, wherein the positive electrode sheet and the negative electrode sheet are separated by the separator disposed therebetween.
[0020] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer, with the positive electrode active material layer being located on one or both sides of the positive electrode current collector. In some embodiments, the positive electrode current collector can be made of aluminum foil, although other common positive electrode current collectors in the art may also be used. In some embodiments, the positive electrode current collector can have a thickness of 1 μm to 50 μm.
[0021] In some embodiments, the positive electrode active material layer may include a positive electrode active material, a conductive agent, and a binder. In some embodiments, the positive electrode active material may include at least one of lithium cobaltate, lithium iron phosphate, lithium aluminate, lithium manganate, or lithium nickel cobalt manganate. In some embodiments, the conductive agent in the positive electrode active material layer may include at least one of conductive carbon black, lamellar graphite, graphene, or carbon nanotubes. In some embodiments, the binder in the positive electrode active material layer may include at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, a styrene-acrylate copolymer, a styrene-butadiene copolymer, a polyamide, a polyacrylonitrile, a polyacrylate, a polyacrylic acid, a polyacrylate, sodium carboxymethyl cellulose, polyvinyl acetate, polyvinylpyrrolidone, a polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, or polyhexafluoropropylene. In some embodiments, the mass ratio of the positive electrode active material, the conductive agent, and the binder in the positive electrode active material layer is (80-99): (0.1-10): (0.1-10), but this is only an example and any other suitable mass ratio may be used.
[0022] In some embodiments, the separator includes at least one of polyethylene, polypropylene, polyvinylidene fluoride, polyethylene terephthalate, polyimide, or aramid. For example, the polyethylene includes at least one selected from high-density polyethylene, low-density polyethylene, or ultra-high molecular weight polyethylene. Polyethylene and polypropylene are particularly effective in preventing short circuits and can improve battery stability through the shutdown effect. In some embodiments, the separator has a thickness ranging from approximately 3 μm to 20 μm.
[0023] In some embodiments, the surface of the isolation membrane may further include a porous layer, disposed on at least one surface of the isolation membrane. The porous layer includes inorganic particles and a binder, wherein the inorganic particles are selected from at least one of aluminum oxide (Al2O3), silicon oxide (SiO2), magnesium oxide (MgO), titanium oxide (TiO2), hafnium dioxide (HfO2), tin oxide (SnO2), cerium dioxide (CeO2), nickel oxide (NiO), zinc oxide (ZnO), calcium oxide (CaO), zirconium oxide (ZrO2), yttrium oxide (Y2O3), silicon carbide (SiC), boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, or barium sulfate. In some embodiments, the pores of the isolation membrane have a diameter ranging from approximately 0.01 μm to 1 μm. The binder of the porous layer is selected from at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, sodium carboxymethyl cellulose, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, and polyhexafluoropropylene. The porous layer on the surface of the separator can improve the separator's heat resistance, oxidation resistance, and electrolyte wettability, and enhance the adhesion between the separator and the electrode.
[0024] In some embodiments, the electrochemical device includes a lithium ion battery, but the present application is not limited thereto. In some embodiments, the electrochemical device further includes an electrolyte, the electrolyte including at least one of a fluoroether, a fluoroethylene carbonate or an ether nitrile. In some embodiments, the electrolyte further includes a lithium salt, the lithium salt including lithium bis(fluorosulfonyl)imide and lithium hexafluorophosphate, the concentration of the lithium salt being 1 mol / L to 2 mol / L, and the mass ratio of lithium bis(fluorosulfonyl)imide and lithium hexafluorophosphate being 0.06 to 5. In some embodiments, the electrolyte may further include a non-aqueous solvent. The non-aqueous solvent may be a carbonate compound, a carboxylate compound, an ether compound, other organic solvents or a combination thereof.
[0025] The carbonate compound may be a linear carbonate compound, a cyclic carbonate compound, a fluorinated carbonate compound, or a combination thereof.
[0026] Examples of chain carbonate compounds are diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), methylethyl carbonate (MEC) and combinations thereof. Examples of cyclic carbonate compounds are ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylethylene carbonate (VEC) or combinations thereof. Examples of the fluorocarbonate compounds are fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate or combinations thereof.
[0027] Examples of the carboxylic acid ester compound are methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolide, valerolactone, mevalonolactone, caprolactone, methyl formate, or a combination thereof.
[0028] Examples of the ether compound are dibutyl ether, tetraglyme, diglyme, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, or a combination thereof.
[0029] Examples of other organic solvents are dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, trioctyl phosphate, and phosphoric acid esters or combinations thereof.
[0030] The embodiments of the present application also provide an electronic device including the above-mentioned electrochemical device. The electronic device of the embodiment of the present application is not particularly limited, and it can be any electronic device known in the prior art. In some embodiments, the electronic device may include, but is not limited to, a laptop computer, a pen-input computer, a mobile computer, an e-book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a drone, a lighting fixture, a toy, a game console, a clock, a power tool, a flashlight, a camera, a large household battery and a lithium ion capacitor, etc.
[0031] Some specific embodiments and comparative examples are listed below to better illustrate the present application, wherein a lithium-ion battery is used as an example.
[0032] Comparative Example 1
[0033] Preparation of the negative electrode sheet: Dissolve the negative electrode active material artificial graphite, the binder polyvinylidene fluoride, and sodium carboxymethyl cellulose in deionized water at a weight ratio of 97.5:2.1:0.44 to form a first slurry. Use 6μm thick copper foil as the negative electrode current collector and apply the first slurry to one side of the negative electrode current collector at a coating weight of 0.086mg / mm 2 , forming the first layer. Dissolve the negative electrode active materials artificial graphite, Si, binder polyacrylic acid, carbon nanotubes, and sodium carboxymethyl cellulose in deionized water at a weight ratio of 59.7:36:3.5:0.4:0.4 to form a second slurry. Apply the second slurry to the other side of the negative electrode current collector at a coating weight of 0.035.5 mg / mm 2 , forming the second layer. After drying, cold pressing and slitting, the negative electrode sheet is obtained.
[0034] Positive electrode sheet preparation: The positive electrode active material, lithium cobalt oxide, the conductive agent, and the binder, polyvinylidene fluoride (PVDF), were dissolved in an N-methylpyrrolidone (NMP) solution at a weight ratio of 97.6:1.1:1.3 to form a positive electrode slurry. An 8μm-thick aluminum foil was used as the positive electrode current collector. The positive electrode slurry was coated on both sides of the positive electrode current collector to a thickness of 50μm. After drying, cold pressing, and slitting, the positive electrode sheets were obtained.
[0035] Preparation of the isolation membrane: The isolation membrane substrate is 8 μm thick polyethylene (PE), and a 2 μm alumina ceramic layer is coated on both sides of the isolation membrane substrate. Finally, 2.5 mg of the binder polyvinylidene fluoride (PVDF) is coated on both sides of the ceramic layer and dried.
[0036] Preparation of electrolyte: In an environment with a water content of less than 10 ppm, lithium hexafluorophosphate and a non-aqueous organic solvent (ethylene carbonate (EC): propylene carbonate (PC): polypropylene (PP): diethyl carbonate (DEC) = 1:1:1:1, mass percentage) are prepared into an electrolyte with a lithium salt concentration of 1.15 mol / L.
[0037] Preparation of a lithium-ion battery: The positive electrode sheet, separator, and negative electrode sheet are stacked in sequence, with the separator positioned between the positive and negative electrodes to provide insulation. The electrodes are then wound to form an electrode assembly. The electrode assembly is then placed in an aluminum-plastic film package. After dehydration at 80°C, the electrolyte is injected and the battery is packaged. The battery undergoes a series of processes, including formation, degassing, and shaping, to produce a lithium-ion battery.
[0038] The difference between Comparative Example 2 and Examples 1 to 11 lies in the preparation of the negative electrode sheet, specifically, the parameters of the first layer and the second layer are different, see Table 1 and Table 2 for details.
[0039] In addition, in this application, the following method is used to measure the corresponding parameters, and the effective area of the single-layer laminated battery used in this application is 49.5*42mm 2 .
[0040] 1) The battery was discharged to 3.0 V, and the positive and negative electrodes were disassembled and soaked in dimethyl carbonate (DMC) solution for 15 min and then dried for later use;
[0041] 2) In a dry inert gas environment in a glove box, punch out the positive and negative electrode sheets from 1), match the positive and negative electrodes, and add a separator to form a single-layer laminate battery. Encapsulate and inject liquid with a pressure fixture to maintain interfacial contact. Charge at a constant current of 0.7C to the charge cutoff voltage, then charge at a constant voltage until the battery reaches a full charge state. Discharge at a DC current of 0.2C to 3.0V to obtain the capacity of the single-layer laminate battery. Then, calculate the capacity per unit area of the negative electrode sheet (capacity per unit area of the negative electrode sheet = capacity of the single-layer laminate battery / effective area of the single-layer laminate battery). Then, calculate the capacity of one side of the negative electrode sheet based on the active coating area of the negative electrode sheet. Repeat the above method to obtain the capacity of the other side.
[0042] 3) Using the single-layer laminated battery in 2), the AC impedance method can be used to test Rs+Rct (Rs refers to ohmic impedance, Rct refers to electrochemical transfer impedance). Due to the influence of other conditions such as the area of the single-layer laminated battery manufactured and the manufacturing process, the absolute value of Rs+Rct may vary, but the ratio of Rs+Rct on both sides of the electrode can be used as the basis for shunting on both sides of the electrode.
[0043] 4) Capacity retention after 500 cycles = capacity after 500 cycles / fresh battery capacity. The capacity test conditions are: constant current charging at 0.7C to 4.5V, constant voltage charging to 0.02C, and then DC discharge at 0.2C to 3.0V as one cycle at 25°C, for a total of 500 cycles.
[0044] 5) Charge the lithium-ion battery at a constant current rate of 0.2C to 4.45V, then charge it at a constant voltage rate of 0.02C to fully charge the lithium-ion battery. Next, discharge it at a constant current rate of 0.2C until the voltage drops to 3.0V. Record the total capacity released during the discharge as C and the voltage platform as U. Measure the actual thickness, length, and width of the lithium-ion battery, and calculate the actual volume V of the lithium-ion battery. Energy density = C*U / V.
[0045] Tables 1 and 2 show various parameters and evaluation results of Examples 1 to 11 and Comparative Examples 1 to 4.
[0046] Table 1
[0047] Table 2
[0048] Comparison of Examples 1 to 3 and Comparative Examples 1 to 2 shows that when the ratio of the impedance of the first layer to the impedance of the second layer is between 0.7 and 0.9, the energy density loss of the lithium-ion battery is minimal, and the capacity retention of the lithium-ion battery is significantly improved. Furthermore, as the silicon mass content of the second layer decreases, the capacity retention of the lithium-ion battery shows a trend of first increasing and then decreasing.
[0049] By comparing Examples 4 to 6, it can be seen that as the content of the conductive agent in the second layer increases, the impedance of the second layer tends to decrease, and the capacity retention rate of the lithium-ion battery tends to decrease.
[0050] By comparing Examples 7 to 11, it can be seen that as the ratio of the capacity of the first layer to the capacity of the second layer increases, the energy density of the lithium-ion battery tends to decrease, and the capacity retention rate of the lithium-ion battery tends to first increase and then decrease.
[0051] The above description is merely a preferred embodiment of the present application and an illustration of the technical principles employed. Those skilled in the art should understand that the scope of disclosure in this application is not limited to technical solutions formed by a specific combination of the above-mentioned technical features, but also encompasses other technical solutions formed by any combination of the above-mentioned technical features or their equivalents. For example, a technical solution formed by replacing the above-mentioned features with technical features with similar functions disclosed in this application.
Claims
1. An electrochemical device comprising: A negative electrode plate, the negative electrode plate comprising a negative electrode current collector, a first layer and a second layer, the negative electrode current collector being located between the first layer and the second layer; The first layer includes a first negative electrode active material, the second layer includes a second negative electrode active material, the first negative electrode active material includes graphite, the second negative electrode active material includes graphite and a silicon-based material, and a ratio of an impedance of the first layer to an impedance of the second layer is 0.7 to 0.
9.
2. The electrochemical device according to claim 1, wherein: A ratio of the capacity of the first layer to the capacity of the second layer is 0.6 to 1.
3. The electrochemical device according to claim 1, wherein A ratio of the capacity of the first layer to the capacity of the second layer is 0.7 to 1.
4. The electrochemical device according to claim 1, wherein The mass percentage of the silicon-based material in the second layer is 6% to 40%.
5. The electrochemical device according to claim 1, wherein The mass percentage of the silicon-based material in the second layer is 12% to 20%.
6. The electrochemical device according to claim 4, wherein: The mass percentage of silicon in the second layer is 4% to 20%.
7. The electrochemical device according to claim 5, wherein: The mass percentage of silicon in the second layer is 4% to 10%.
8. The electrochemical device according to claim 4, wherein: The second layer further includes a binder, and the mass percentage of the binder in the second layer is 1.4% to 5%.
9. The electrochemical device according to claim 4, wherein: The second layer further comprises carbon nanotubes, and the mass percentage of the carbon nanotubes in the second layer is 0.3% to 0.7%.
10. The electrochemical device according to claim 4, wherein: The second layer further comprises sodium carboxymethyl cellulose, and the mass percentage of the sodium carboxymethyl cellulose in the second layer is 0.3% to 0.7%.
11. The electrochemical device according to claim 1, wherein The silicon-based material includes at least one of silicon, silicon-carbon material or silicon-oxygen material.
12. An electronic device comprising the electrochemical device according to any one of claims 1 to 11.
Citation Information
Patent Citations
Secondary battery and electric device
CN115832185A
Electrochemical device and electronic device
CN116314608A
Cylindrical lithium ion battery
JP2001155776A
Electrode assembly, secondary battery, battery module, battery pack, and electric apparatus
WO2023060494A1
KR20210039599A