Electrolyte solution and battery

By adding fluorine-containing solvent A, sulfur compounds and nitrile substances to the electrolyte, a stable SEI film and complex layer are formed, which solves the problem of cycle stability and safety of the battery under high temperature conditions and achieves higher Capacity retention and safety performance.

WO2024199005A1PCT designated stage expired Publication Date: 2024-10-03ZHUHAI COSMX BATTERY CO LTD

Patent Information

Application Number
PCT/CN2024/082411
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing batteries have poor cycle stability under high temperature conditions. In particular, the increase in the gram capacity of the cathode material causes degumming of the aluminum-plastic film of the casing, causing safety accidents. Moreover, the existing oxide coating process is complex and costly, and the protection effect is poor.

Method used

An electrolyte is used, including electrolyte salt, carboxylic acid ester, carbonate, fluorine-containing solvent A, fluorine-containing solvent B, sulfur series compound and polynitrile compound. The thermal stability of the electrolyte is improved by fluorine-containing solvent A. The sulfur series The compound forms a stable SEI film, and nitriles complex the positive electrode metal ions to prevent oxidative decomposition and collapse.

Benefits of technology

The high-temperature cycle stability and safety of the battery are significantly improved. The capacity retention rate of lithium-ion batteries after 800 cycles at 45°C is over 80%, and the capacity retention rate after baking at 85°C for 8 hours is over 98%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2024082411-FTAPPB-I100001
    Figure PCTCN2024082411-FTAPPB-I100001
  • Figure PCTCN2024082411-FTAPPB-I100002
    Figure PCTCN2024082411-FTAPPB-I100002
  • Figure PCTCN2024082411-FTAPPB-I100003
    Figure PCTCN2024082411-FTAPPB-I100003
Patent Text Reader

Abstract

Provided in the present disclosure are an electrolyte solution and a battery comprising same. The electrolyte solution comprises an electrolyte salt, a carboxylic ester, a carbonic ester, a fluorine-containing solvent A, a fluorine-containing solvent B, a chalcogenide and a polynitrile compound, wherein the fluorine-containing solvent A improves the overall oxidation resistance of the electrolyte solution, and the introduction of the fluorine-containing solvent A solves the problem of poor high-temperature thermal stability of the fluorine-containing solvent B; moreover, the chalcogenide can form a film on a negative electrode and achieves protection on the negative electrode together with the fluorine-containing solvents; the polynitrile compound mainly achieves complexing protection on the surface of a positive electrode; and protection on the positive electrode and the negative electrode is achieved by means of the synergistic effect of these additives, such that the electrolyte solution is prevented from entering a material to cause damage.
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte and battery Technical Field

[0001] The present disclosure relates to the field of batteries, and in particular to an electrolyte and a battery containing the electrolyte. Background Art

[0002] With the improvement of people's living standards and the pursuit of a better life, higher requirements are being placed on battery safety and energy density. To improve battery energy density, further increasing the voltage of the cathode material is a common approach. However, as the limiting voltage of the cathode material continues to rise, the specific capacity of the cathode material gradually increases, which severely deteriorates the battery's high-temperature performance and makes long cycle life impossible to guarantee. Especially under high voltage, long-term charge and discharge cycles can cause the aluminum-plastic film of the outer casing to delaminate, ultimately leading to serious safety accidents.

[0003] Currently, cathode materials are typically modified with oxide coatings or by preparing cathode materials with different morphologies and structures. However, these processes are complex, costly, and offer poor protection. Therefore, developing a battery with improved safety and cycle stability is crucial.

[0004] Summary of the Invention

[0005] In view of this, the present disclosure provides an electrolyte and a battery containing the electrolyte. The electrolyte provided by the present disclosure can effectively improve the problem of SEI rupture and oxidation of the electrolyte, and at the same time can improve the high-temperature cycle stability of the battery.

[0006] To solve the above technical problems, the present disclosure adopts the following technical solutions:

[0007] In a first aspect, the present disclosure provides an electrolyte, comprising:

[0008] Electrolyte salt, carboxylic acid ester, carbonate ester, fluorinated solvent A, fluorinated solvent B, sulfur compound and polynitrile compound;

[0009] The structure of the fluorinated solvent A is shown in structural formula (1):

[0010] wherein R1, R2, R3, R4, R5 and R6 are each independently selected from any one of a hydrogen atom, a halogen, a C1-C20 alkyl group substituted or unsubstituted by halogen, a C1-C20 unsaturated olefin group substituted or unsubstituted by halogen, a C3-C20 cycloalkyl group substituted or unsubstituted by halogen, a phenyl group substituted or unsubstituted by halogen, a biphenyl group substituted or unsubstituted by halogen, a C6-C26 phenylalkyl group substituted or unsubstituted by halogen, and a C6-C26 condensed ring aromatic group substituted or unsubstituted by halogen, and at least one of R1, R2, R3, R4, R5 and R6 contains F;

[0011] The fluorinated solvent B comprises fluoroethylene carbonate;

[0012] The structure of the sulfur compound is shown in structural formula (2):

[0013] wherein X and Y are each independently selected from any one of -CH2-, -NH- and -O-, and R7 and R8 are each independently selected from any one of a hydrogen atom, a halogen, a hydrocarbon group and a halogen-containing hydrocarbon group;

[0014] The structure of the polynitrile compound is shown in structural formula (3):

[0015] Here, R9 is a group having 1 to 10 carbon atoms and having at least 4 substitution positions.

[0016] Furthermore, the amount of the fluorinated solvent A added is 0.1 wt% to 10 wt% of the total mass of the electrolyte; and / or the amount of the fluorinated solvent B added is 0.1 wt% to 10 wt% of the total mass of the electrolyte.

[0017] Furthermore, the amount of the fluorinated solvent A added is recorded as W1, the amount of the fluorinated solvent B added is recorded as W2, and the amounts of the fluorinated solvent A and the fluorinated solvent B added satisfy the following relationship:

[0018] 1≤W1 / W2≤2.

[0019] Furthermore, the fluorinated solvent A is selected from at least one of the substances represented by structural formula 1-1 to structural formula 1-43:

[0020] Furthermore, the carboxylate is selected from any two of propyl acetate, propyl propionate and propyl formate, the dielectric constant γ2 of the carboxylate satisfies 3F / m≤γ2≤5F / m, and the added amount of the carboxylate accounts for 35wt% to 55wt% of the total mass of the electrolyte; the carbonate is selected from any two of ethylene carbonate, propylene carbonate and butylene carbonate, and the added amount of the carbonate accounts for 5wt% to 35wt% of the total mass of the electrolyte.

[0021] Furthermore, the added amount of the sulfur compound accounts for 0.02 wt% to 6 wt% of the total mass of the electrolyte.

[0022] Furthermore, the sulfur-based compounds in the electrolyte are selected from any two of the sulfur-based compounds shown in structural formula (2).

[0023] Furthermore, the sulfur compound is selected from at least one of the substances represented by structural formula 2-1 to structural formula 2-9:

[0024] Furthermore, the addition amount of the polynitrile compound accounts for 0.02wt% to 12wt% of the total mass of the electrolyte; and / or the polynitrile compound is selected from at least one of the following compounds: 1,1,3,3-propanetetracarbonitrile, 1,2,2,3-tetracyanopropane, 1,2,4,5-tetracyanobenzene, 2,3,5,6-pyrazinetetracarbonitrile, 7,7,8,8-tetracyanoquinodimethane and tetracyanoethylene.

[0025] Furthermore, the electrolyte salt includes at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium bis(trifluoromethylsulfonyl)imide, lithium difluorobis(oxalatophosphate), lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium hexafluoroantimonate, lithium hexafluoroarsenate, lithium bis(pentafluoroethylsulfonyl)imide, lithium tris(trifluoromethylsulfonyl)methyllithium or lithium bis(trifluoromethylsulfonyl)imide.

[0026] In a second aspect, the present disclosure provides a battery comprising the electrolyte as described above.

[0027] The beneficial effects of the above technical solution disclosed in the present invention are as follows:

[0028] The present disclosure provides an electrolyte solution, which includes: an electrolyte salt, a carboxylate, a carbonate, a fluorine-containing solvent A, a fluorine-containing solvent B, a sulfur-based compound, and a polynitrile compound.

[0029] The electrolyte provided in the present disclosure has at least the following advantages:

[0030] (1) Fluorinated solvent B in the electrolyte can participate in the formation of SEI film in the formation stage, thus playing a role in protecting the electrode. However, fluorinated solvent B has the problem of poor thermal stability in the later cycle at high temperature. Fluorinated solvent A is a fluorinated solvent with oxidation resistance and high thermal stability. Under the premise of meeting the requirements of interfacial film formation, it can improve the overall thermal stability of the fluorinated solvent in the electrolyte, thereby improving the high-temperature thermal stability of the battery.

[0031] (2) In the electrolyte provided by the present disclosure, in addition to carbonate, carboxylic acid ester is also included. Compared with carbonate solvent, carboxylic acid ester can increase the Li + The transmission speed significantly improves the dynamic performance of the electrolyte;

[0032] (3) Sulfur compounds: Sulfur compounds can form lithium alkylsulfonate RSO3Li, which increases the ionic conductivity of the SEI film. It not only stabilizes the SEI film of the negative electrode, but also prevents the collapse of the SEI film and CEI film during high-temperature storage by forming a stable film in the form of Li2SO3 on the positive electrode.

[0033] (4) Nitriles in the electrolyte can effectively complex the metal ions of the positive electrode and inhibit the oxidative decomposition of the electrolyte and the dissolution of metal ions, thereby effectively improving the high-temperature cycle performance of the battery.

[0034] In summary, fluorinated solvent A improves the overall oxidation resistance of the electrolyte, and the introduction of fluorinated solvent A solves the problem of poor high-temperature thermal stability of fluorinated solvent B. At the same time, the sulfur compound can form a film on the negative electrode, forming a protective layer on the negative electrode together with the fluorinated solvent. The nitrile compound contained mainly forms a complex protection on the surface of the positive electrode. Through the synergistic effect of these additives, protection is formed on the positive and negative electrodes, preventing the electrolyte from entering the interior of the material and causing damage. The lithium-ion battery provided in this disclosure has a capacity retention rate of over 80% after 800 cycles at 45°C, and a capacity retention rate of over 98% after baking at 85°C for 8 hours. DETAILED DESCRIPTION

[0035] In order to further understand the present disclosure, preferred embodiments of the present disclosure are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present disclosure, rather than limiting the present disclosure.

[0036] In a first aspect, the present disclosure provides an electrolyte solution, comprising: an electrolyte salt, a carboxylate, a carbonate, a fluorine-containing solvent A, a fluorine-containing solvent B, a sulfur-based compound, and a polynitrile compound.

[0037] Wherein, the structure of the fluorinated solvent A is shown in structural formula (1):

[0038] Wherein, R1, R2, R3, R4, R5 and R6 are each independently selected from any one of a hydrogen atom, a halogen, a C1-C20 alkyl group substituted or unsubstituted by halogen, a C1-C20 unsaturated olefin group substituted or unsubstituted by halogen, a C3-C20 cycloalkyl group substituted or unsubstituted by halogen, a phenyl group substituted or unsubstituted by halogen, a biphenyl group substituted or unsubstituted by halogen, a C6-C26 phenylalkyl group substituted or unsubstituted by halogen, and a C6-C26 condensed ring aromatic group substituted or unsubstituted by halogen, and at least one of R1, R2, R3, R4, R5 and R6 contains F; and the fluorine-containing solvent B comprises fluoroethylene carbonate.

[0039] In some embodiments of the present disclosure, when R1, R2, R3, R4, R5 and R6 are substituted by halogen atoms, the substituted halogen atoms may be: F, Cl, I, etc.

[0040] Specifically, when R1, R2, R3, R4, R5 and R6 are each independently selected from a C1-C20 alkyl group (i.e., an alkyl group with 1 to 20 carbon atoms) substituted or unsubstituted by halogen, the specific type of the alkyl group is not limited and can be selected according to actual needs, for example, both chain (halogenated) alkyl groups and (halogenated) cyclic alkyl groups are possible, where chain alkyl groups include straight-chain alkyl groups and branched-chain alkyl groups. In addition, the cyclic alkyl group may have a substituent or may not have a substituent. Specific examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, cyclopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, cyclobutyl, n-pentyl, isopentyl, tert-pentyl, neopentyl, cyclopentyl, 2,2-dimethylpropyl, 1-ethylpropyl, 1-methylbutyl, 2-methylbutyl, n-hexyl, isohexyl, 2-hexyl, 3-hexyl, cyclohexyl, 2-methylpentyl, 3-methylpentyl, 1,1,2-trimethylpropyl, 3,3-dimethylbutyl, n-heptyl, 2-heptyl, 3-heptyl, 2-methylhexyl, 3-methylhexyl, 4-methylhexyl, isoheptyl, cycloheptyl, n-octyl, cyclooctyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, and eicosyl.

[0041] In some embodiments of the present disclosure, the amount of the fluorinated solvent A added is 0.1 wt% to 10 wt% of the total mass of the electrolyte, for example, 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 1 wt%, 1.2 wt%, 1.3 wt%, 1.5 wt%, 1.6 wt%, 1.8 wt%, 2 wt%, 2.2 wt%, 2.4 wt%, 2.5 wt%, 2.6 wt%, 2.8 wt%, 3 wt%, 3.3 wt%, 3.5 wt%, 3.8 wt%, 4 wt%, 4.2 wt%, 4.5 wt%, 4.8 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt% or 10 wt%.

[0042] In some embodiments of the present disclosure, the added amount of the fluorine-containing solvent A accounts for 6 wt % to 9 wt % of the total mass of the electrolyte.

[0043] In some embodiments of the present disclosure, the added amount of the fluorine-containing solvent A accounts for 8 wt % to 9 wt % of the total mass of the electrolyte.

[0044] In some embodiments of the present disclosure, the amount of the fluorinated solvent B added is 0.1 wt% to 10 wt% of the total mass of the electrolyte, for example, 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 1 wt%, 1.2 wt%, 1.3 wt%, 1.5 wt%, 1.6 wt%, 1.8 wt%, 2 wt%, 2.2 wt%, 2.4 wt%, 2.5 wt%, 2.6 wt%, 2.8 wt%, 3 wt%, 3.3 wt%, 3.5 wt%, 3.8 wt%, 4 wt%, 4.2 wt%, 4.5 wt%, 4.8 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt% or 10 wt%.

[0045] Preferably, the fluorinated solvent A is selected from at least one of the substances represented by structural formula 1-1 to structural formula 1-43:

[0046] In some embodiments of the present disclosure, the addition amount of the fluorinated solvent A is recorded as W1, and the addition amount of the fluorinated solvent B is recorded as W2. The addition amounts of the fluorinated solvent A and the fluorinated solvent B satisfy the following relationship: 1≤W1 / W2≤2 (for example, W1 / W2 is equal to 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 2).

[0047] The present disclosure provides an electrolyte, which includes: electrolyte salt, carboxylic acid ester, carbonate, fluorine-containing solvent A and fluorine-containing solvent B. Among them, the fluorine-containing solvent B in the electrolyte can participate well in the formation of SEI film in the formation stage, thereby playing a role in protecting the electrode. However, the fluorine-containing solvent B has the problem of poor thermal stability in the late high-temperature cycle, because the F in the fluorine-containing solvent B is easy to fall off at high temperature. Fluorine-containing solvent A is a fluorinated solvent with oxidation resistance and high thermal stability. In fluorine-containing solvent A, the electron affinity of fluorine atoms is large, which will attract the electrons of neighboring carbon atoms, resulting in changes in chemical shift, and the structure is not easy to fall off compared with fluorine-containing solvent B. Under the premise of meeting the interface film formation, the overall thermal stability of the fluorine-containing solvent in the electrolyte can be improved, thereby improving the high-temperature thermal stability of the battery. The inventors found that when the addition amount of the fluorine-containing solvent A and the fluorine-containing solvent B satisfies the following relationship: 1≤W1 / W2≤2, it can effectively improve the overall thermal stability of the fluorine-containing solvent in the electrolyte, and at the same time it can also participate well in the formation of SEI film.

[0048] In some embodiments of the present disclosure, the carbonate is selected from any two of ethylene carbonate, propylene carbonate and butylene carbonate, and the amount of the carbonate added accounts for 5wt% to 35wt% (for example, 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt% or 35wt%) of the total mass of the electrolyte. In the present disclosure, the dielectric constant γ1 after the two carbonates are mixed is controlled to be: 55F / m≤γ1≤105F / m (for example, 55F / m, 60F / m, 65F / m, 70F / m, 75F / m, 80F / m, 85F / m, 90F / m, 95F / m, 100F / m or 105F / m). At the same time, when the carbonates are selected from ethylene carbonate and propylene carbonate, the ratio of the amount of ethylene carbonate added to the amount of propylene carbonate added is ≤1 / 2. When the carbonate is selected from ethylene carbonate and butylene carbonate, the ratio of the amount of ethylene carbonate added to the amount of butylene carbonate added is ≤ 1 / 2. When the carbonate is selected from propylene carbonate and butylene carbonate, the ratio of the amount of propylene carbonate added to the amount of butylene carbonate added is ≤ 1 / 2.

[0049] When the dielectric constant of the carbonate after full mixing meets the above γ1, a protective SEI film can be formed to inhibit the continuous decomposition of the electrolyte during the lithium insertion and extraction process of the electrode. The self-discharge phenomenon in the lithium insertion state is suppressed to a certain extent, and the cycle stability is significantly improved.

[0050] In the present disclosure, the dielectric constant of the carbonate can be measured by conventional methods in the art, such as the electrostatic capacitance method.

[0051] Ethylene carbonate is a cyclic carbonate with poor thermal stability at high temperatures and prone to ring-opening decomposition. Propylene carbonate, due to the addition of a methyl group to its ring structure, is more resistant to oxidation, and butylene carbonate is even more resistant to oxidation. The present disclosure found that when the addition amounts of the two carbonates satisfy the above relationship, the battery's electrical performance shows significant improvements in high-temperature storage and cycling.

[0052] In some embodiments of the present disclosure, the carboxylate is selected from any two of propyl acetate, propyl propionate and propyl formate, the dielectric constant γ2 of the carboxylate satisfies 3F / m≤γ2≤5F / m (for example, 3F / m, 3.5F / m, 4F / m, 4.5F / m or 5F / m), and the amount of the carboxylate added accounts for 35wt% to 55wt% of the total mass of the electrolyte (for example, 35wt%, 40wt%, 45wt%, 50wt% or 55wt%). In the electrolyte provided by the present disclosure, in addition to carbonate, carboxylate is also included. Compared with carbonate solvents, carboxylate can increase the Li + The transmission speed is improved, which significantly improves the dynamic performance of the electrolyte.

[0053] In the present disclosure, the dielectric constant of the carboxylic acid ester can be measured by conventional methods in the art, such as an electrostatic capacitance method.

[0054] In the electrolyte provided by the present disclosure, the electrolyte further comprises: a sulfur compound, the structure of which is shown in structural formula (2):

[0055] Wherein, X and Y are each independently selected from any one of -CH2-, -NH- and -O-, and R7 and R8 are each independently selected from any one of a hydrogen atom, a halogen, a hydrocarbon group and a halogen-containing hydrocarbon group.

[0056] According to other embodiments of the present disclosure, the amount of the sulfur compound added is 0.02 wt% to 6 wt% of the total mass of the electrolyte, for example, 0.02 wt%, 0.05 wt%, 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 1 wt%, 1.2 wt%, 1.3 wt%, 1.5 wt%, 1.6 wt%, 1.8 wt%, 2 wt%, 2.2 wt%, 2.4 wt%, 2.5 wt%, 2.6 wt%, 2.8 wt%, 3 wt%, 3.3 wt%, 3.5 wt%, 3.8 wt%, 4 wt%, 4.2 wt%, 4.5 wt%, 4.8 wt%, 5 wt% or 6 wt%.

[0057] The inventors of the present disclosure have discovered that when the amount of sulfur-based compounds added to the electrolyte is within a specific range, the ionic conductivity of the SEI film can be further increased, and the SEI film can be stabilized.

[0058] According to other embodiments of the present disclosure, the sulfur-based compound is selected from at least one of the substances represented by Structural Formulas 2-1 to 2-9:

[0059] According to other embodiments of the present disclosure, the sulfur-based compounds in the electrolyte are selected from any two of the sulfur-based compounds shown in structural formula (2).

[0060] According to other embodiments of the present disclosure, the sulfur-based compounds in the electrolyte are selected from any two of the sulfur-based compounds shown in structural formula (2), and the addition amounts of the two sulfur-based compounds are the same.

[0061] The electrolyte provided by the present disclosure also includes a sulfur-based compound, which can form lithium alkylsulfonate RSO3Li, thereby increasing the ionic conductivity of the SEI film. It not only has the effect of stabilizing the SEI film of the Si negative electrode, but also can prevent the collapse of the SEI film and CEI film during high-temperature storage by forming a stable film in the form of Li2SO3 on the positive electrode.

[0062] In the electrolyte provided by the present disclosure, the electrolyte further comprises a polynitrile compound, the structure of the polynitrile compound is shown in structural formula (3):

[0063] Here, R9 is a group having 1 to 10 carbon atoms and having at least 4 substitution positions.

[0064] According to some other embodiments of the present disclosure, the added amount of the polynitrile compound accounts for 0.02 wt % to 12 wt % of the total mass of the electrolyte. For example, 0.02wt%, 0.05wt%, 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 1.2wt%, 1.3wt%, 1.5wt%, 1.6wt%, 1.8wt%, 2wt%, 2.2wt%, 2.4wt%, 2.5wt%, 2.6wt%, 2.8wt%, 3wt%, 3.3wt%, 3.5wt%, 3.8wt%, 4wt%, 4.2wt%, 4.5wt%, 4.8wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt% or 12wt%.

[0065] Preferably, the added amount of the polynitrile compound accounts for 0.5 wt% to 8 wt% of the total mass of the electrolyte.

[0066] According to some other embodiments of the present disclosure, the polynitrile compound is at least one selected from the group consisting of 1,1,3,3-propanetetracarbonitrile, 1,2,2,3-tetracyanopropane, 1,2,4,5-tetracyanobenzene, 2,3,5,6-pyrazinetetracarbonitrile, 7,7,8,8-tetracyanoquinodimethane, and tetracyanoethylene.

[0067] The electrolyte provided by the present disclosure further includes a polynitrile compound, which can effectively complex the metal ions of the positive electrode and inhibit the oxidative decomposition of the electrolyte and the dissolution of the metal ions, thereby effectively improving the high-temperature cycle performance of the battery.

[0068] According to other embodiments of the present disclosure, the electrolyte salt includes at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium bis(trifluoromethylsulfonyl)imide, lithium difluorobis(oxalatophosphate), lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium hexafluoroantimonate, lithium hexafluoroarsenate, lithium bis(pentafluoroethylsulfonyl)imide, tris(trifluoromethylsulfonyl)methyllithium, or lithium bis(trifluoromethylsulfonyl)imide.

[0069] In the present disclosure, the electrolyte salt is preferably a lithium salt.

[0070] In a second aspect, the present disclosure provides a battery comprising the electrolyte as described above.

[0071] According to other embodiments of the present disclosure, the battery includes: the electrolyte as described above, a positive electrode sheet containing a positive electrode active material, a negative electrode sheet containing a negative electrode active material, and a separator.

[0072] According to some other embodiments of the present disclosure, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer coated on one or both sides of the positive electrode current collector, and the positive electrode active material layer includes the positive electrode active material, a positive electrode conductor and a positive electrode binder.

[0073] According to some other embodiments of the present disclosure, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer coated on one or both sides of the negative electrode current collector, and the negative electrode active material layer includes the negative electrode active material, a negative electrode conductor and a negative electrode binder.

[0074] According to other embodiments of the present disclosure, the mass percentages of the components in the positive electrode active material layer are: 80 wt%-99.8 wt% of the positive electrode active material, 0.1 wt%-10 wt% of the positive electrode conductive agent, and 0.1 wt%-10 wt% of the positive electrode binder. Preferably, the mass percentages of the components in the positive electrode active material layer are: 90 wt%-99.6 wt% of the positive electrode active material, 0.2 wt%-5 wt% of the positive electrode conductive agent, and 0.2 wt%-5 wt% of the positive electrode binder.

[0075] According to other embodiments of the present disclosure, the mass percentages of the components in the negative electrode active material layer are: 80 wt%-99.8 wt% of the negative electrode active material, 0.1 wt%-10 wt% of the negative electrode conductive agent, and 0.1 wt%-10 wt% of the negative electrode binder. Preferably, the mass percentages of the components in the negative electrode active material layer are: 90 wt%-99.6 wt% of the negative electrode active material, 0.2 wt%-5 wt% of the negative electrode conductive agent, and 0.2 wt%-5 wt% of the negative electrode binder.

[0076] According to other embodiments of the present disclosure, the positive electrode conductive agent and the negative electrode conductive agent are each independently selected from at least one of conductive carbon black, acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotubes, metal powder and carbon fiber.

[0077] According to other embodiments of the present disclosure, the positive electrode binder and the negative electrode binder are each independently selected from at least one of sodium carboxymethyl cellulose, styrene-butadiene latex, polytetrafluoroethylene, and polyethylene oxide.

[0078] According to other embodiments of the present disclosure, the positive electrode active material includes at least one of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate and transition metal lithium oxide. The chemical formula of the transition metal lithium oxide is Li 1+x Ni y Co z M (1-y-z) O2, wherein -0.1≤x≤1; 0≤y≤1, 0≤z≤1, and 0≤y+z≤1; and M is at least one of Mg, Zn, Ga, Ba, Al, Fe, Cr, Sn, V, Mn, Sc, Ti, Nb, Mo, and Zr. The negative electrode active material includes at least one of artificial graphite, natural graphite, mesocarbon microbeads, hard carbon, soft carbon, silicon-carbon / graphite, and silicon-oxygen / graphite.

[0079] The present disclosure is further illustrated below through some specific embodiments.

[0080] Group A of Examples is used to illustrate the electrolytes of the present disclosure.

[0081] Example A1 Preparation of electrolyte

[0082] 1.1 The electrolyte includes the following components:

[0083] Carbonates: ethylene carbonate, 4 wt% and propylene carbonate, 8 wt%, totaling 12 wt%;

[0084] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 39 wt%, totaling 51 wt%;

[0085] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0086] Fluorinated solvent A: structural formula 1-14, 8 wt%;

[0087] Fluorinated solvent B: fluoroethylene carbonate, 6 wt %;

[0088] Sulfur compounds: structural formula 2-4, 3 wt% and structural formula 2-7, 3 wt%, totaling 6 wt%;

[0089] Polynitrile compound: 1,2,2,3-tetracyanopropane, 4 wt%;

[0090] Among them, W1 / W2 is 1.33.

[0091] 1.2 Preparation Method: First, add and mix the carbonate and carboxylate according to the ratio. After mixing, add the electrolyte salt, mix thoroughly, and shake well. After cooling to room temperature, add the other components. Finally, shake evenly again for 10 minutes until the electrolyte solution is clear and free of solids and suspension. Specifically, after adding the electrolyte salt, add the fluorinated solvent A, fluorinated solvent B, and sulfur compound, and finally add the polynitrile compound.

[0092] Example A2 Preparation of electrolyte

[0093] 1.1 The electrolyte includes the following components:

[0094] In this embodiment, the polynitrile compound is 1,2,4,5-tetracyanobenzene, 4 wt%

[0095] The remaining components and the contents of each component are the same as those in Example 1;

[0096] Among them, W1 / W2 is 1.33.

[0097] 1.2 Preparation method: same as Example 1.

[0098] Example A3 Preparation of electrolyte

[0099] 1.1 The electrolyte includes the following components:

[0100] Carbonates: ethylene carbonate, 4 wt% and propylene carbonate, 8 wt%, totaling 12 wt%;

[0101] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 40 wt%, totaling 52 wt%;

[0102] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0103] Fluorinated solvent A: structural formula 1-34, 8 wt%;

[0104] Fluorinated solvent B: fluoroethylene carbonate, 6 wt %;

[0105] Sulfur compounds: structural formula 2-3, 3 wt% and structural formula 2-5, 3 wt%, totaling 6 wt%;

[0106] Polynitrile compound: 1,1,3,3-propanetetracarbonitrile, 3 wt%;

[0107] Among them, W1 / W2 is 1.33.

[0108] 1.2 Preparation method: same as Example 1.

[0109] Example A4 Preparation of electrolyte

[0110] 1.1 The electrolyte includes the following components:

[0111] Carbonates: ethylene carbonate, 4 wt% and propylene carbonate, 8 wt%, totaling 12 wt%;

[0112] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 39 wt%, totaling 51 wt%;

[0113] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0114] Fluorinated solvent A: structural formula 1-41, 8 wt%;

[0115] Fluorinated solvent B: fluoroethylene carbonate, 6 wt %;

[0116] Sulfur compounds: structural formula 2-6, 3 wt% and structural formula 2-8, 3 wt%, totaling 6 wt%;

[0117] Polynitrile compound: 1,2,2,3-tetracyanopropane, 4 wt%;

[0118] Among them, W1 / W2 is 1.33.

[0119] 1.2 Preparation method: same as Example 1.

[0120] Example A5 Preparation of electrolyte

[0121] 1.1 The electrolyte includes the following components:

[0122] Carbonates: ethylene carbonate, 4 wt% and propylene carbonate, 8 wt%, totaling 12 wt%;

[0123] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 40 wt%, totaling 52 wt%;

[0124] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0125] Fluorinated solvent A: structural formula 1-43, 8 wt%;

[0126] Fluorinated solvent B: fluoroethylene carbonate, 6 wt %;

[0127] Sulfur compounds: structural formula 2-4, 3 wt% and structural formula 2-6, 3 wt%, totaling 6 wt%;

[0128] Polynitrile compound: tetracyanoethylene, 3 wt%;

[0129] Among them, W1 / W2 is 1.33.

[0130] 1.2 Preparation method: same as Example 1.

[0131] Example A6 Preparation of Electrolyte

[0132] 1.1 The electrolyte includes the following components:

[0133] Carbonates: ethylene carbonate, 2 wt% and propylene carbonate, 4 wt%, totaling 6 wt%;

[0134] Carboxylate: propyl acetate, 14 wt% and propyl propionate, 43 wt%, totaling 57 wt%;

[0135] The remaining components and the contents of each component are the same as those in Example 1;

[0136] Among them, W1 / W2 is 1.33.

[0137] 1.2 Preparation method: same as Example 1.

[0138] Example A7 Preparation of Electrolyte

[0139] 1.1 The electrolyte includes the following components:

[0140] Carbonates: ethylene carbonate, 0.5 wt% and propylene carbonate, 5.5 wt%, totaling 6 wt%;

[0141] Carboxylate: propyl acetate, 14 wt% and propyl propionate, 43 wt%, totaling 57 wt%;

[0142] The remaining components and the contents of each component are the same as those in Example 1;

[0143] Among them, W1 / W2 is 1.33.

[0144] 1.2 Preparation method: same as Example 1.

[0145] Example A8 Preparation of Electrolyte

[0146] 1.1 The electrolyte includes the following components:

[0147] Carbonates: ethylene carbonate, 2 wt% and propylene carbonate, 4 wt%, totaling 6 wt%;

[0148] Carboxylate: propyl acetate, 16 wt% and propyl propionate, 50 wt%, totaling 66 wt%;

[0149] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0150] Fluorinated solvent A: structural formula 1-14, 4 wt%;

[0151] Fluorinated solvent B: fluoroethylene carbonate, 3 wt%;

[0152] Sulfur compounds: structural formula 2-4, 2 wt% and structural formula 2-7, 2 wt%, totaling 4 wt%;

[0153] Polynitrile compound: 1,2,2,3-tetracyanopropane, 4 wt%;

[0154] Among them, W1 / W2 is 1.33.

[0155] 1.2 Preparation method: same as Example 1.

[0156] Example A9 Preparation of electrolyte

[0157] 1.1 The electrolyte includes the following components:

[0158] Carbonates: ethylene carbonate, 8 wt% and propylene carbonate, 4 wt%, totaling 12 wt%;

[0159] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 39 wt%, totaling 51 wt%;

[0160] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0161] Fluorinated solvent A: structural formula 1-14, 8 wt%;

[0162] Fluorinated solvent B: fluoroethylene carbonate, 6 wt %;

[0163] Sulfur compounds: structural formula 2-4, 3 wt% and structural formula 2-7, 3 wt%, totaling 6 wt%;

[0164] Polynitrile compound: 1,2,2,3-tetracyanopropane, 4 wt%;

[0165] Among them, W1 / W2 is 1.33.

[0166] 1.2 Preparation method: same as Example 1.

[0167] Example A10 Preparation of electrolyte

[0168] 1.1 The electrolyte includes the following components:

[0169] Carbonates: ethylene carbonate, 4 wt% and propylene carbonate, 8 wt%, totaling 12 wt%;

[0170] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 39 wt%, totaling 51 wt%;

[0171] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0172] Fluorinated solvent A: structural formula 1-14, 6 wt%;

[0173] Fluorinated solvent B: fluoroethylene carbonate, 8 wt%;

[0174] Sulfur compounds: structural formula 2-4, 3 wt% and structural formula 2-7, 3 wt%, totaling 6 wt%;

[0175] Polynitrile compound: 1,2,2,3-tetracyanopropane, 4 wt%;

[0176] Among them, W1 / W2 is 0.75.

[0177] 1.2 Preparation method: same as Example 1.

[0178] Example A11 Preparation of electrolyte

[0179] 1.1 The electrolyte includes the following components:

[0180] Carbonate: ethylene carbonate, 4 wt% and propylene carbonate 8 wt%, totaling 12 wt%;

[0181] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 40 wt%, totaling 52 wt%;

[0182] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0183] Fluorinated solvent A: structural formula 1-14, 8 wt%;

[0184] Fluorinated solvent B: fluoroethylene carbonate, 6 wt %;

[0185] Sulfur compounds: structural formula 2-4, 4 wt% and structural formula 2-7, 2 wt%, totaling 6 wt%;

[0186] Polynitrile compound: 1,2,2,3-tetracyanopropane, 3 wt%;

[0187] Among them, W1 / W2 is 1.33.

[0188] 1.2 Preparation method: same as Example 1.

[0189] Example A12 Preparation of Electrolyte

[0190] This group of examples was carried out with reference to Example A1, except that the content of the fluorinated solvent A was changed to verify the effect of the change in the content of the fluorinated solvent A. Specifically:

[0191] In embodiment A12a, the electrolyte comprises the following components:

[0192] Carbonates: ethylene carbonate, 4 wt% and propylene carbonate, 8 wt%, totaling 12 wt%;

[0193] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 46 wt%, totaling 58 wt%;

[0194] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0195] Fluorinated solvent A: structural formula 1-14, 1 wt%;

[0196] Fluorinated solvent B: fluoroethylene carbonate, 6 wt %;

[0197] Sulfur compounds: structural formula 2-4, 3 wt% and structural formula 2-7, 3 wt%, totaling 6 wt%;

[0198] Polynitrile compound: 1,2,2,3-tetracyanopropane, 4 wt%;

[0199] Among them, W1 / W2 is 0.17.

[0200] In embodiment A12b, the electrolyte comprises the following components:

[0201] Carbonates: ethylene carbonate, 4 wt% and propylene carbonate, 8 wt%, totaling 12 wt%;

[0202] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 45 wt%, totaling 57 wt%;

[0203] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0204] Fluorinated solvent A: structural formula 1-14, 2 wt%;

[0205] Fluorinated solvent B: fluoroethylene carbonate, 6 wt %;

[0206] Sulfur compounds: structural formula 2-4, 3 wt% and structural formula 2-7, 3 wt%, totaling 6 wt%;

[0207] Polynitrile compound: 1,2,2,3-tetracyanopropane, 4 wt%;

[0208] Among them, W1 / W2 is 0.33.

[0209] In Example A12c, the electrolyte includes the following components:

[0210] Carbonates: ethylene carbonate, 4 wt% and propylene carbonate, 8 wt%, totaling 12 wt%;

[0211] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 41 wt%, totaling 53 wt%;

[0212] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0213] Fluorinated solvent A: structural formula 1-14, 6 wt%;

[0214] Fluorinated solvent B: fluoroethylene carbonate, 6 wt %;

[0215] Sulfur compounds: structural formula 2-4, 3 wt% and structural formula 2-7, 3 wt%, totaling 6 wt%;

[0216] Polynitrile compound: 1,2,2,3-tetracyanopropane, 4 wt%;

[0217] Among them, W1 / W2 is 1.

[0218] In embodiment A12d, the electrolyte comprises the following components:

[0219] Carbonates: ethylene carbonate, 4 wt% and propylene carbonate, 8 wt%, totaling 12 wt%;

[0220] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 38 wt%, totaling 50 wt%;

[0221] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0222] Fluorinated solvent A: structural formula 1-14, 9 wt%;

[0223] Fluorinated solvent B: fluoroethylene carbonate, 6 wt %;

[0224] Sulfur compounds: structural formula 2-4, 3 wt% and structural formula 2-7, 3 wt%, totaling 6 wt%;

[0225] Polynitrile compound: 1,2,2,3-tetracyanopropane, 4 wt%;

[0226] Among them, W1 / W2 is 1.5.

[0227] Example A13 Preparation of Electrolyte

[0228] This group of examples was carried out with reference to Example A1, except that the fluorinated solvent A was changed to verify the effects of the change in the fluorinated solvent A. Specifically:

[0229] In embodiment A13a, the electrolyte comprises the following components:

[0230] Carbonates: ethylene carbonate, 4 wt% and propylene carbonate, 8 wt%, totaling 12 wt%;

[0231] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 39 wt%, totaling 51 wt%;

[0232] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0233] Fluorinated solvent A: structural formula 1-15, 8 wt%;

[0234] Fluorinated solvent B: fluoroethylene carbonate, 6 wt %;

[0235] Sulfur compounds: structural formula 2-4, 3 wt% and structural formula 2-7, 3 wt%, totaling 6 wt%;

[0236] Polynitrile compound: 1,2,2,3-tetracyanopropane, 4 wt%;

[0237] Among them, W1 / W2 is 1.33.

[0238] In embodiment A13b, the electrolyte comprises the following components:

[0239] Carbonates: ethylene carbonate, 4 wt% and propylene carbonate, 8 wt%, totaling 12 wt%;

[0240] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 39 wt%, totaling 51 wt%;

[0241] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0242] Fluorinated solvent A: structural formula 1-7, 8 wt%;

[0243] Fluorinated solvent B: fluoroethylene carbonate, 6 wt %;

[0244] Sulfur compounds: structural formula 2-4, 3 wt% and structural formula 2-7, 3 wt%, totaling 6 wt%;

[0245] Polynitrile compound: 1,2,2,3-tetracyanopropane, 4 wt%;

[0246] Among them, W1 / W2 is 1.33.

[0247] In Example A13c, the electrolyte comprises the following components:

[0248] Carbonates: ethylene carbonate, 4 wt% and propylene carbonate, 8 wt%, totaling 12 wt%;

[0249] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 39 wt%, totaling 51 wt%;

[0250] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0251] Fluorinated solvent A: structural formula 1-6, 8 wt%;

[0252] Fluorinated solvent B: fluoroethylene carbonate, 6 wt %;

[0253] Sulfur compounds: structural formula 2-4, 3 wt% and structural formula 2-7, 3 wt%, totaling 6 wt%;

[0254] Polynitrile compound: 1,2,2,3-tetracyanopropane, 4 wt%;

[0255] Among them, W1 / W2 is 1.33.

[0256] Example A14 Preparation of Electrolyte

[0257] This group of examples was carried out with reference to Example A1, except that the content of fluorinated solvent A and / or fluorinated solvent B was changed to verify the effect of the change in W1 / W2. Specifically:

[0258] In embodiment A14a, the electrolyte comprises the following components:

[0259] Carbonates: ethylene carbonate, 4 wt% and propylene carbonate, 8 wt%, totaling 12 wt%;

[0260] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 41 wt%, totaling 53 wt%;

[0261] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0262] Fluorinated solvent A: structural formula 1-14, 6 wt%;

[0263] Fluorinated solvent B: fluoroethylene carbonate, 6 wt %;

[0264] Sulfur compounds: structural formula 2-4, 3 wt% and structural formula 2-7, 3 wt%, totaling 6 wt%;

[0265] Polynitrile compound: 1,2,2,3-tetracyanopropane, 4 wt%;

[0266] Among them, W1 / W2 is 1.

[0267] In embodiment A14b, the electrolyte comprises the following components:

[0268] Carbonates: ethylene carbonate, 4 wt% and propylene carbonate, 8 wt%, totaling 12 wt%;

[0269] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 41 wt%, totaling 53 wt%;

[0270] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0271] Fluorinated solvent A: structural formula 1-14, 8 wt%;

[0272] Fluorinated solvent B: fluoroethylene carbonate, 4 wt%;

[0273] Sulfur compounds: structural formula 2-4, 3 wt% and structural formula 2-7, 3 wt%, totaling 6 wt%;

[0274] Polynitrile compound: 1,2,2,3-tetracyanopropane, 4 wt%;

[0275] Among them, W1 / W2 is 2.

[0276] In Example A14c, the electrolyte includes the following components:

[0277] Carbonates: ethylene carbonate, 4 wt% and propylene carbonate, 8 wt%, totaling 12 wt%;

[0278] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 51 wt%, totaling 63 wt%;

[0279] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0280] Fluorinated solvent A: structural formula 1-14, 1 wt%;

[0281] Fluorinated solvent B: fluoroethylene carbonate, 1 wt%;

[0282] Sulfur compounds: structural formula 2-4, 3 wt% and structural formula 2-7, 3 wt%, totaling 6 wt%;

[0283] Polynitrile compound: 1,2,2,3-tetracyanopropane, 4 wt%;

[0284] Among them, W1 / W2 is 1.

[0285] The electrolytes in Examples A1-A14 satisfy the following conditions: 55 F / m≤γ1≤105 F / m and 3 F / m≤γ2≤5 F / m.

[0286] Preparation of Comparative Example A1 Electrolyte

[0287] 1.1 The electrolyte includes the following components:

[0288] Carbonates: ethylene carbonate, 4 wt% and propylene carbonate, 8 wt%, totaling 12 wt%;

[0289] Carboxylate: propyl acetate, 12 wt% and propyl propionate, 55 wt%, totaling 67 wt%;

[0290] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0291] Fluorinated solvent B: fluoroethylene carbonate, 8 wt %.

[0292] 1.2 Preparation method:

[0293] First, add and mix the carbonate and carboxylate according to the ratio. After mixing, add the electrolyte salt, mix thoroughly and shake well. After cooling to room temperature, add other components and finally shake evenly again for 10 minutes until the electrolyte is clear and free of solids and suspensions.

[0294] Preparation of Comparative Example A2 Electrolyte

[0295] 1.1 The electrolyte includes the following components (based on 100% of the total mass of the electrolyte):

[0296] Carbonates: ethylene carbonate, 5 wt% and propylene carbonate, 10 wt%, totaling 15 wt%;

[0297] Carboxylate: propyl acetate, 14 wt% and propyl propionate, 40 wt%, totaling 54 wt%;

[0298] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0299] Fluorinated solvent A: structural formula 1-14, 10 wt%;

[0300] Fluorinated solvent B: fluoroethylene carbonate, 8 wt %.

[0301] 1.2 Preparation method:

[0302] First, add and mix the carbonate and carboxylate according to the ratio. After mixing, add the electrolyte salt, mix thoroughly and shake well. After cooling to room temperature, add other components and finally shake evenly again for 10 minutes until the electrolyte is clear and free of solids and suspensions.

[0303] Preparation of Comparative Example A3 Electrolyte

[0304] 1.1 The electrolyte includes the following components:

[0305] In this embodiment, the fluorinated solvent A has the structural formula 1-34; the remaining components and the contents of each component are the same as those in Comparative Example 2.

[0306] 1.2 Preparation method: same as Comparative Example 2.

[0307] Preparation of Comparative Example A4 Electrolyte

[0308] 1.1 The electrolyte includes the following components:

[0309] In this embodiment, the fluorinated solvent A has the structural formula 1-41; the remaining components and the contents of each component are the same as those in Comparative Example 2.

[0310] 1.2 Preparation method: same as Comparative Example 2.

[0311] Preparation of Comparative Example A5 Electrolyte

[0312] 1.1 The electrolyte includes the following components:

[0313] In this embodiment, the fluorinated solvent A has the structural formula 1-42; the remaining components and the contents of each component are the same as those in Comparative Example 2.

[0314] 1.2 Preparation method: same as Comparative Example 2.

[0315] Preparation of Comparative Example A6 Electrolyte

[0316] 1.1 The electrolyte includes the following components:

[0317] In this embodiment, the fluorinated solvent A has the structural formula 1-43; the remaining components and the contents of each component are the same as those in Comparative Example 2.

[0318] 1.2 Preparation method: same as Comparative Example 2.

[0319] Preparation of Comparative Example A7 Electrolyte

[0320] 1.1 The electrolyte includes the following components:

[0321] In this embodiment, the fluorinated solvent A has the structural formula 1-40; the remaining components and the contents of each component are the same as those in Comparative Example 2.

[0322] 1.2 Preparation method: same as Comparative Example 2.

[0323] Preparation of Comparative Example A8 Electrolyte

[0324] 1.1 The electrolyte includes the following components:

[0325] Carbonates: ethylene carbonate, 5 wt% and propylene carbonate, 10 wt%, totaling 15 wt%;

[0326] Carboxylate: propyl acetate, 13 wt% and propyl propionate, 39 wt%, totaling 52 wt%;

[0327] Electrolyte salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0328] Fluorinated solvent A: structural formula 1-14, 8 wt%;

[0329] Fluorinated solvent B: fluoroethylene carbonate, 6 wt %;

[0330] Sulfur compound: structural formula 2-4, 6 wt%.

[0331] 1.2 Preparation method: The same as Comparative Example 2, that is, after adding the electrolyte salt, the fluorinated solvent A, the fluorinated solvent B and the sulfur compound are added together.

[0332] Preparation of Comparative Example A9 Electrolyte

[0333] 1.1 The electrolyte includes the following components:

[0334] In this embodiment, the sulfur compounds include structural formula 2-4, 3 wt% and structural formula 2-7, 3 wt%, for a total of 6 wt%;

[0335] The remaining components and the contents of each component are the same as those in Comparative Example 8.

[0336] 1.2 Preparation method: same as Comparative Example 8.

[0337] Group B of Examples is used to illustrate the batteries of the present disclosure.

[0338] Example B Preparation of lithium ion battery

[0339] 1) Preparation of positive electrode sheet

[0340] The positive electrode active materials lithium cobalt oxide (LiCoO2), polyvinylidene fluoride (PVDF), SP (superP) and carbon nanotubes (CNT) are mixed in a mass ratio of 96:2:1.5:0.5, N-methylpyrrolidone (NMP) is added, and the mixture is stirred under the action of a vacuum mixer until the mixed system becomes a positive electrode active slurry with uniform fluidity; the positive electrode active slurry is evenly coated on both surfaces of an aluminum foil; the coated aluminum foil is dried, and then rolled and cut to obtain the desired positive electrode sheet.

[0341] 2) Negative electrode preparation

[0342] The negative electrode active materials artificial graphite, sodium carboxymethyl cellulose (CMC-Na), styrene-butadiene rubber, conductive carbon black (SP) and single-walled carbon nanotubes (SWCNTs) were mixed in a mass ratio of 94.5:2.5:1.5:1:0.5, deionized water was added, and a negative electrode active slurry was obtained under the action of a vacuum mixer; the negative electrode active slurry was evenly coated on both surfaces of the copper foil; the coated copper foil was dried at room temperature, then transferred to an 80°C oven for drying for 10 hours, and then cold pressed and slit to obtain the negative electrode sheet.

[0343] 3) The positive electrode sheet, negative electrode sheet, and separator prepared above were stacked in the order of positive electrode sheet, separator, and negative electrode sheet, and then wound to obtain a battery cell; the battery cell was placed in an outer packaging aluminum foil, and the electrolyte prepared in Example A was injected into the outer packaging. After vacuum packaging, static standing, formation, shaping, and sorting, different lithium-ion batteries were obtained. The battery disclosed herein has a charge and discharge range of 3.0-4.5V.

[0344] Note: Example B1 uses the electrolyte prepared in Example A1, Example B2 uses the electrolyte prepared in Example A2, and so on.

[0345] The components and their contents in Example A and Comparative Example A are shown in Table 1.

[0346] Comparative Example B group was carried out with reference to Implementation Group B, except that the electrolyte was replaced with the electrolyte prepared in Comparative Example A group of the same mass.

[0347] Performance Testing

[0348] 1) 45℃ cycle performance test

[0349] The lithium-ion batteries prepared in Example Group B and Comparative Example Group B were each subjected to 1000 charge-discharge cycles at 45°C at a rate of 1C within the charge-discharge cutoff voltage range. The discharge capacity in the first cycle was calculated as x1 mAh, and the discharge capacity in the Nth cycle was calculated as y1 mAh. The capacity in the Nth cycle was divided by the capacity in the first cycle to obtain the cycle capacity retention ratio in the Nth cycle, R1 = y1 / x1. The test results are shown in Table 2.

[0350] 2) 85℃ high temperature storage test

[0351] After discharging to capacity, the batteries were allowed to rest for 10 minutes. They were then discharged at 0.2C to 3V, left to rest for 10 minutes, and then fully charged at 0.5C, with the charge cutoff at 0.05C, and left to rest for 10 minutes. The fully charged batteries were tested for voltage, internal resistance, and thickness at 25±5°C. After the fully charged batteries were placed in an 85°C oven for 8 hours, the hot batteries were removed and tested for voltage, internal resistance, and thickness. Capacity retention and recovery tests were also performed. The test results are shown in Table 2.

[0352] Table 1

[0353] Table 1

[0354] In Table 1, EC is ethylene carbonate, PC is propylene carbonate, EP is propyl acetate, and PP is propyl propionate.

[0355] Table 2

[0356] It can be seen from the data in Table 2 that the high-temperature cycle performance of the battery is greatly improved when the fluorinated solvent A is added to the electrolyte compared with the comparative example 1 in which the fluorinated solvent A is not added. Furthermore, after adding sulfur compounds and polynitrile compounds to the electrolyte, the high-temperature cycle performance of the battery is further improved. Specifically, the fluorinated solvent A improves the overall oxidation resistance of the electrolyte, and the introduction of the fluorinated solvent A solves the problem of poor high-temperature thermal stability of the fluorinated solvent B; at the same time, the sulfur compound can form a film at the negative electrode and form protection at the negative electrode together with the fluorinated solvent; the nitrile compound contained mainly forms a complex protection on the surface of the positive electrode, and through the synergistic effect between these additives, protection is formed at the positive and negative electrodes, preventing the electrolyte from entering the interior of the material and causing damage. It can be seen from the data in Table 2 that the capacity retention rate of the lithium-ion batteries in Examples B1-B5 after 800 cycles at 45°C is above 80%, and the capacity retention rate after baking at 85°C for 8 hours is above 98%. More specifically, the data in Table 2 shows that the improvement in high-temperature performance is most pronounced when the combined amount of ethylene carbonate and propylene carbonate in the electrolyte is between 5wt% and 35wt%, and when the ratio of ethylene carbonate to propylene carbonate is between 0 and 1 / 2. The improvement in high-temperature performance is most pronounced when the ratio of fluorinated solvent A to fluorinated solvent B is between 1 and 2, and when two sulfur-based compounds are used in equal amounts.

[0357] Unless otherwise defined, the technical or scientific terms used in this disclosure shall have the ordinary meanings understood by persons having ordinary skills in the field to which this disclosure belongs. The words "first", "second" and similar terms used in this disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. The words "connected" or "connected" and similar terms are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the object being described changes, the relative positional relationship also changes accordingly.

[0358] The above is a preferred embodiment of the present disclosure. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles described in the present disclosure. These improvements and modifications should also be regarded as the scope of protection of the present disclosure.

Claims

1. An electrolyte, characterized in that: The electrolyte comprises: Electrolyte salt, carboxylic acid ester, carbonate ester, fluorine-containing solvent A, fluorine-containing solvent B, sulfur compound and polynitrile compound; Wherein, the structure of the fluorinated solvent A is shown in structural formula (1): wherein R1, R2, R3, R4, R5 and R6 are independently selected from any one of a hydrogen atom, a halogen, a C1-C20 alkyl group substituted or unsubstituted by halogen, a C1-C20 unsaturated olefin group substituted or unsubstituted by halogen, a C3-C20 cycloalkyl group substituted or unsubstituted by halogen, a phenyl group substituted or unsubstituted by halogen, a biphenyl group substituted or unsubstituted by halogen, a C6-C26 phenylalkyl group substituted or unsubstituted by halogen, and a C6-C26 condensed aromatic hydrocarbon group substituted or unsubstituted by halogen, and at least one of R1, R2, R3, R4, R5 and R6 contains F; The fluorinated solvent B comprises fluoroethylene carbonate; The structure of the sulfur compound is shown in structural formula (2): Wherein, X and Y are each independently selected from any one of -CH2-, -NH- and -O-, and R7 and R8 are each independently selected from any one of a hydrogen atom, a halogen, a hydrocarbon group and a halogen-containing hydrocarbon group; The structure of the polynitrile compound is shown in structural formula (3): Here, R9 is a group having 1 to 10 carbon atoms and having at least 4 substitution positions.

2. The electrolyte according to claim 1, characterized in that The amount of the fluorinated solvent A added is 0.1wt% to 10wt% of the total mass of the electrolyte; Preferably, the amount of the fluorinated solvent A added is 8wt% to 9wt% of the total mass of the electrolyte; and / or, The amount of the fluorinated solvent B added is 0.1 wt% to 10 wt% of the total mass of the electrolyte.

3. The electrolyte according to claim 1 or 2, characterized in that The amount of the fluorinated solvent A added is recorded as W1, the amount of the fluorinated solvent B added is recorded as W2, and the amounts of the fluorinated solvent A and the fluorinated solvent B added satisfy the following relationship: 1≤W1 / W2≤2.

4. The electrolyte according to any one of claims 1 to 3, characterized in that The fluorinated solvent A is selected from at least one of the substances represented by structural formula 1-1 to structural formula 1-43:

5. The electrolyte according to any one of claims 1 to 4, characterized in that The carboxylic acid ester is selected from any two of propyl acetate, propyl propionate and propyl formate; and / or, The dielectric constant γ2 of the carboxylate satisfies 3F / m≤γ2≤5F / m; and / or, The added amount of the carboxylic acid ester accounts for 35 wt% to 55 wt% of the total mass of the electrolyte.

6. The electrolyte according to any one of claims 1 to 5, characterized in that The carbonate is selected from any two of ethylene carbonate, propylene carbonate and butylene carbonate; and / or, The amount of carbonate added is 5wt% to 35wt% of the total mass of the electrolyte; and / or, The dielectric constant γ1 of the carbonate satisfies 55 F / m≤γ1≤105 F / m.

7. The electrolyte according to claim 6, characterized in that The carbonate is ethylene carbonate and propylene carbonate, and the ratio of the amount of ethylene carbonate added to the amount of propylene carbonate added is ≤ 1 / 2; and / or, The carbonate is ethylene carbonate and butylene carbonate, and the ratio of the amount of ethylene carbonate added to the amount of butylene carbonate added is ≤ 1 / 2; and / or, The carbonates are propylene carbonate and butylene carbonate, and the ratio of the added amount of propylene carbonate to the added amount of butylene carbonate is ≤1 / 2.

8. The electrolyte according to any one of claims 1 to 7, characterized in that The added amount of the sulfur compound accounts for 0.02wt% to 6wt% of the total mass of the electrolyte.

9. The electrolyte according to any one of claims 1 to 8, characterized in that The sulfur compound in the electrolyte is selected from any two of the sulfur compounds shown in structural formula (2); Preferably, the addition amounts of any two sulfur-based compounds are the same.

10. The electrolyte according to any one of claims 1 to 9, characterized in that The sulfur compound is selected from at least one of the substances represented by structural formula 2-1 to structural formula 2-9:

11. The electrolyte according to any one of claims 1 to 10, characterized in that The addition amount of the polynitrile compound accounts for 0.02wt% to 12wt% of the total mass of the electrolyte; Preferably, the added amount of the polynitrile compound accounts for 0.5wt% to 8wt% of the total mass of the electrolyte.

12. The electrolyte according to any one of claims 1 to 11, characterized in that The polynitrile compound is selected from at least one of the following compounds: 1,1,3,3-propanetetracarbonitrile, 1,2,2,3-tetracyanopropane, 1,2,4,5-tetracyanobenzene, 2,3,5,6-pyrazinetetranitrile, 7,7,8,8-tetracyanoquinodimethane and tetracyanoethylene.

13. The electrolyte according to any one of claims 1 to 12, characterized in that The electrolyte salt includes at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium bis(trifluoromethylsulfonyl)imide, lithium difluorobis(oxalatophosphate), lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium hexafluoroantimonate, lithium hexafluoroarsenate, lithium bis(pentafluoroethylsulfonyl)imide, tris(trifluoromethylsulfonyl)methyllithium or lithium bis(trifluoromethylsulfonyl)imide.

14. A battery, characterized in that: The battery comprises the electrolyte according to any one of claims 1 to 13.

15. The battery according to claim 14, characterized in that The battery also includes a positive electrode sheet, a negative electrode sheet and a separator; the positive electrode sheet includes a positive electrode collector and a positive electrode active material layer coated on one side or both sides of the positive electrode collector; the negative electrode sheet includes a negative electrode collector and a negative electrode active material layer coated on one side or both sides of the negative electrode collector.

Citation Information

Patent Citations

  • Electrolyte, secondary battery comprising same, and electronic device

    CN111435759A

  • Non-aqueous electrolyte with polynitrile compounds and lithium ion battery

    CN113140797A

  • Organic electrolyte and lithium ion secondary battery containing same

    CN115528309A

  • Electrolyte and battery containing same

    CN116154303A

  • Nonaqueous electrolyte and lithium ion secondary battery comprising the same

    JP2018200893A

Cited By

  • Secondary battery

    CN119674235A

  • Lithium ion battery electrolyte, lithium ion battery, preparation method and application

    CN120165052A