Solar cell preparation method and solar cell

By preparing an intrinsic amorphous silicon layer on an untextured silicon substrate and texturing the surface of the doped layer, the problem of excessive size of the pyramid texture on the surface of the silicon substrate was solved, and the intrinsic amorphous silicon film and silicon were realized. Good contact with the substrate improves the efficiency of solar cells and cell performance.

WO2024199026A1PCT designated stage expired Publication Date: 2024-10-03TONGWEI SOLAR ENERGY (CHENGDU) CO LID

Patent Information

Application Number
PCT/CN2024/082610
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-20
Publication Date
2024-10-03

Smart Images

  • Figure CN2024082610_03102024_PF_FP_ABST
    Figure CN2024082610_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to a solar cell preparation method and a solar cell. The solar cell preparation method comprises: providing a silicon substrate (100) having non-textured surfaces; preparing intrinsic amorphous silicon layers on the two non-textured surfaces of the silicon substrate (100); respectively preparing an n-type microcrystalline doped layer and a p-type microcrystalline doped layer on the surfaces of the two intrinsic amorphous silicon layers; and texturing the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer.
Need to check novelty before this filing date? Find Prior Art

Description

Method for preparing solar cell, solar cell

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on March 24, 2023, with application number 202310304298.4 and invention name “Method for preparing solar cells, solar cells”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the technical field of solar cells, and in particular to a method for preparing a solar cell and a solar cell. Background Art

[0003] As the efficiency of solar cells continues to improve, the efficiency of the cell is mainly limited by the short-circuit current (Isc) loss in the doped amorphous silicon film layer. Doped microcrystalline silicon thin films have better carrier transport characteristics, lower parasitic absorption and better carrier selection interface, thereby improving the conversion efficiency of the cell. In the traditional process of growing microcrystalline thin films on a substrate, it is first necessary to perform texturing on the silicon matrix substrate, and then prepare an ultra-thin intrinsic amorphous silicon film to passivate the dangling bonds on the surface of the silicon matrix, so that the cell has a high open circuit voltage (Uoc) to improve efficiency. However, the size of the pyramid velvet surface generated by wet chemical reaction texturing on the silicon matrix surface is much larger than the thickness of the intrinsic amorphous silicon film, making it difficult for the intrinsic amorphous silicon film to fully contact the silicon matrix, forming defects on the surface of the intrinsic amorphous silicon film, which easily leads to direct contact between the doped microcrystalline silicon film and the silicon matrix, resulting in a decrease in the open circuit voltage (Uoc).

[0004] Summary of the Invention

[0005] Based on this, it is necessary to provide a method for preparing a solar cell and a solar cell. The method for preparing a solar cell can improve the contact effect between the intrinsic amorphous silicon film and the silicon substrate, reduce the risk of direct contact between the doped microcrystalline silicon film and the silicon substrate, and thus increase the open circuit voltage to improve the cell efficiency.

[0006] In a first aspect, the present application provides a method for preparing a solar cell, comprising:

[0007] Providing a silicon substrate with an untextured surface;

[0008] forming intrinsic amorphous silicon layers on both surfaces of the untextured silicon substrate;

[0009] forming an n-type microcrystalline doped layer and a p-type microcrystalline doped layer on the surfaces of the two intrinsic amorphous silicon layers respectively;

[0010] Texturing is performed on the surfaces of the n-type microcrystalline doping layer and the p-type microcrystalline doping layer.

[0011] In some embodiments, forming an n-type microcrystalline doped layer and a p-type microcrystalline doped layer on the surfaces of the two intrinsic amorphous silicon layers respectively includes:

[0012] forming an n-type amorphous doped sublayer and a p-type amorphous doped sublayer on the surfaces of the two intrinsic amorphous silicon layers respectively;

[0013] forming an n-type microcrystal growth sublayer on the n-type amorphous doped sublayer, and forming a p-type microcrystal growth sublayer on the p-type amorphous doped sublayer;

[0014] An n-type microcrystal doping sublayer is prepared on the n-type microcrystal growth sublayer, and a p-type microcrystal doping sublayer is prepared on the p-type microcrystal growth sublayer.

[0015] In some embodiments, texturing the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer includes:

[0016] The surfaces of the n-type microcrystalline doping layer and the p-type microcrystalline doping layer are textured at 60° C. to 65° C. using an alkali solution with a mass concentration of 0.8% to 1%.

[0017] In some embodiments, the thickness of the n-type microcrystalline doped sublayer is controlled to be 0.5 μm to 1 μm.

[0018] In some embodiments, the thickness of the p-type microcrystalline doped sublayer is controlled to be 0.5 μm to 1 μm.

[0019] In some embodiments, the pressure for preparing the n-type amorphous doped sublayer is 0.5 Torr to 0.57 Torr.

[0020] In some embodiments, the volume ratio of the gas used to prepare the n-type amorphous doped sublayer is SiH 4 :H 2 = 1:15-30.

[0021] In some embodiments, the ignition power for preparing the n-type amorphous doped sublayer is 200W to 800W.

[0022] In some embodiments, the pressure for preparing the p-type amorphous doped sublayer is 0.5 Torr to 0.57 Torr.

[0023] In some embodiments, the volume ratio of the gas used to prepare the p-type amorphous doped sublayer is SiH 4 :H 2 = 1:15-30.

[0024] In some embodiments, the ignition power for preparing the p-type amorphous doped sublayer is 200W to 800W.

[0025] In some embodiments, the pressure for forming the n-type microcrystalline growth sublayer on the n-type amorphous doped sublayer is 3 Torr to 5 Torr.

[0026] In some embodiments, the volume ratio of the gas used to prepare the n-type microcrystalline growth sublayer on the n-type amorphous doped sublayer is SiH 4 :H 2 = 1:150-200.

[0027] In some embodiments, the starting power for preparing the n-type microcrystalline growth sublayer on the n-type amorphous doped sublayer is 2000W to 3500W.

[0028] In some embodiments, the pressure for forming the p-type microcrystalline growth sublayer on the p-type amorphous doped sublayer is 3 Torr to 5 Torr.

[0029] In some embodiments, the volume ratio of the gas used to prepare the p-type microcrystalline growth sublayer on the p-type amorphous doped sublayer is SiH 4 :H 2 = 1:150-200.

[0030] In some embodiments, the starting power for preparing the p-type microcrystalline growth sublayer on the p-type amorphous doped sublayer is 2000W to 3500W.

[0031] In some embodiments, the pressure for forming the n-type microcrystalline doped sublayer on the n-type microcrystalline growth sublayer is 5 Torr to 8 Torr.

[0032] In some embodiments, the starting power for preparing the n-type microcrystal doped sublayer on the n-type microcrystal growth sublayer is 4000W to 7000W.

[0033] In some embodiments, the pressure for forming the p-type microcrystalline doped sublayer on the p-type microcrystalline growth sublayer is 5 Torr to 8 Torr.

[0034] In some embodiments, the starting power for preparing the p-type microcrystal doped sublayer on the p-type microcrystal growth sublayer is 4000W to 7000W.

[0035] In some embodiments, before forming the intrinsic amorphous silicon layer on both surfaces of the untextured silicon substrate, the method further includes:

[0036] The untextured silicon substrate is subjected to rough polishing, pre-cleaning, polishing and passivation in sequence.

[0037] In some embodiments, the thicknesses of the two intrinsic amorphous silicon layers are controlled to be 5 nm to 10 nm respectively.

[0038] In a second aspect, the present application also provides a solar cell, comprising: an untextured silicon substrate, an intrinsic amorphous silicon layer respectively located on both surfaces of the untextured silicon substrate, an n-type microcrystalline doped layer and a p-type microcrystalline doped layer respectively located on the surfaces of the two intrinsic amorphous silicon layers away from the untextured silicon substrate, wherein the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer away from the untextured silicon substrate are both velvet surfaces.

[0039] In some embodiments, the n-type microcrystalline doped layer includes an n-type amorphous doped sublayer, an n-type microcrystalline growth sublayer and an n-type microcrystalline doped sublayer stacked in sequence, and the n-type amorphous doped sublayer is closer to the untextured silicon substrate than the n-type microcrystalline doped sublayer; the p-type microcrystalline doped layer includes a p-type amorphous doped sublayer, a p-type microcrystalline growth sublayer and a p-type microcrystalline doped sublayer stacked in sequence, and the p-type amorphous doped sublayer is closer to the untextured silicon substrate than the p-type microcrystalline doped sublayer.

[0040] In some embodiments, the thickness of the n-type microcrystalline doped sublayer is 0.5 μm to 1 μm.

[0041] In some embodiments, the thickness of the p-type microcrystalline doped sublayer is 0.5 μm to 1 μm.

[0042] In some embodiments, the textured surface has a plurality of pyramid structures, and the height of the pyramid structures is 0.5 μm to 1 μm.

[0043] The above-mentioned method for preparing solar cells does not perform texturing on the silicon substrate. Instead, an intrinsic amorphous silicon layer is prepared on the surface of the untextured silicon substrate. Then, an n-type microcrystalline doped layer and a p-type microcrystalline doped layer are respectively prepared on the surfaces of the two intrinsic amorphous silicon layers. Finally, the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer are texturized. Preparing the intrinsic amorphous silicon layer on the surface of the untextured silicon substrate can make the contact between the intrinsic amorphous silicon layer and the silicon substrate more complete. At the same time, texturing is performed on the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer to achieve a light trapping effect, thereby improving the light utilization rate of the battery. This method can achieve better contact between the intrinsic amorphous silicon film and the silicon matrix, reduce the risk of direct contact between the doped microcrystalline silicon film and the silicon matrix, and thus improve the conversion efficiency of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] FIG1 is a schematic diagram of a process for preparing a solar cell according to an embodiment of the present application;

[0045] FIG2 is a schematic diagram of the film structure of a solar cell provided in one embodiment of the present application.

[0046] Explanation of the reference numerals: 100, silicon substrate; 210, n-type intrinsic amorphous silicon layer; 220, p-type intrinsic amorphous silicon layer; 310, n-type microcrystal hatching sublayer; 320, p-type microcrystal hatching sublayer; 410, n-type microcrystal doping sublayer; 420, p-type microcrystal doping sublayer; 510, front transparent conductive oxide layer; 520, back transparent conductive oxide layer; 610, front electrode layer; 620, back electrode layer. DETAILED DESCRIPTION

[0047] To make the above-mentioned objects, features, and advantages of the present application more clearly understood, the specific embodiments of the present application are described in detail below with reference to the accompanying drawings. The following description sets forth many specific details to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the scope of the present application. Therefore, the present application is not limited to the specific embodiments disclosed below.

[0048] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application pertains. The terms used herein in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0049] 1 , an embodiment of the present application provides a method for preparing a solar cell, comprising:

[0050] S100: providing a silicon substrate with an untextured surface;

[0051] S200: forming an intrinsic amorphous silicon layer on both surfaces of the untextured silicon substrate;

[0052] S300: forming an n-type microcrystalline doped layer and a p-type microcrystalline doped layer on the surfaces of the two intrinsic amorphous silicon layers respectively;

[0053] S400: Texturing is performed on the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer. The above-mentioned method for preparing solar cells does not texturing the silicon substrate, but prepares an intrinsic amorphous silicon layer on the surface of the untextured silicon substrate, and then prepares an n-type microcrystalline doped layer and a p-type microcrystalline doped layer on the surfaces of the two intrinsic amorphous silicon layers, respectively. Finally, texturing is performed on the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer. Directly preparing the intrinsic amorphous silicon layer on the surface of the untextured silicon substrate can make the contact between the intrinsic amorphous silicon layer and the silicon substrate more complete. At the same time, texturing is performed on the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer to achieve a light trapping effect, thereby improving the light utilization rate of the cell. This method can achieve better contact between the intrinsic amorphous silicon film and the silicon matrix, reduce the risk of direct contact between the doped microcrystalline silicon film and the silicon matrix, and thus improve the conversion efficiency of the cell.

[0054] In one embodiment, the silicon substrate is an n-type single crystal silicon wafer.

[0055] In one embodiment, the intrinsic amorphous silicon layer is prepared by plasma chemical vapor deposition.

[0056] In one embodiment, a method for preparing a solar cell includes:

[0057] Providing a silicon substrate with an untextured surface;

[0058] Directly forming an intrinsic amorphous silicon layer on both surfaces of a silicon substrate that has not been textured;

[0059] forming an n-type microcrystalline doped layer and a p-type microcrystalline doped layer on the surfaces of the two intrinsic amorphous silicon layers respectively;

[0060] Texturing is performed on the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer.

[0061] In some embodiments, forming an n-type microcrystalline doped layer and a p-type microcrystalline doped layer on the surfaces of two intrinsic amorphous silicon layers includes: forming an n-type amorphous doped sublayer and a p-type amorphous doped sublayer on the surfaces of the two intrinsic amorphous silicon layers; forming an n-type microcrystalline growth sublayer on the n-type amorphous doped sublayer and a p-type microcrystalline growth sublayer on the p-type amorphous doped sublayer; forming an n-type microcrystalline doped sublayer on the n-type microcrystalline growth sublayer and a p-type microcrystalline doped sublayer on the p-type microcrystalline growth sublayer. First, an amorphous doped layer is formed on the intrinsic amorphous silicon layer. The amorphous doped layer can serve as an incubation layer for the microcrystalline film layer. Then, a microcrystalline growth layer is formed on the amorphous doped layer. By increasing the power, the growth of the film layer can be transformed from amorphous to microcrystalline. After the microcrystalline growth layer is formed, a thick microcrystalline doped layer is formed on the surface of the microcrystalline growth layer to provide conditions for texturing.

[0062] In one embodiment, the n-type amorphous doped sublayer is prepared by plasma chemical vapor deposition.

[0063] In one embodiment, the p-type amorphous doped sublayer is prepared by plasma chemical vapor deposition.

[0064] In one embodiment, the n-type microcrystalline growth sublayer is prepared by plasma chemical vapor deposition.

[0065] In one embodiment, the p-type microcrystalline growth sublayer is prepared by plasma chemical vapor deposition.

[0066] In one embodiment, the n-type microcrystalline doped sublayer is prepared by plasma chemical vapor deposition.

[0067] In one embodiment, the p-type microcrystalline doped sublayer is prepared by plasma chemical vapor deposition.

[0068] In some embodiments, texturing the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer includes:

[0069] The surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer are textured using an alkali solution having a mass concentration of 0.8% to 1% at 60° C. to 65° C. Optionally, the mass concentration of the alkali solution used for textured surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer is 0.8%, 0.81%, 0.82%, 0.83%, 0.84%, 0.85%, 0.86%, 0.87%, 0.88%, 0.89%, 0.9%, 0.91%, 0.92%, 0.93%, 0.94%, 0.95%, 0.96%, 0.97%, 0.98%, 0.99% or 1%. Optionally, the temperature for texturing the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer is 60°C, 60.5°C, 61°C, 61.5°C, 62°C, 62.5°C, 63°C, 63.5°C, 64°C, 64.5°C or 65°C.

[0070] In some embodiments, the thickness of the n-type microcrystalline doped sublayer is controlled to be 0.5 μm to 1 μm. Within this thickness range of the n-type microcrystalline doped sublayer, the subsequent texturing effect is better. Optionally, the thickness of the n-type microcrystalline doped sublayer is controlled to be 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.8 μm, 0.85 μm, 0.9 μm, 0.95 μm, or 1 μm.

[0071] In some embodiments, the thickness of the p-type microcrystalline doped sublayer is controlled to be 0.5 μm to 1 μm. Within this thickness range of the p-type microcrystalline doped sublayer, the subsequent texturing effect is better. Optionally, the thickness of the p-type microcrystalline doped sublayer is controlled to be 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.8 μm, 0.85 μm, 0.9 μm, 0.95 μm, or 1 μm.

[0072] In some embodiments, the pressure for preparing the n-type amorphous doped sublayer is 0.5 Torr to 0.57 Torr. At relatively low pressure, combined with a low silane-to-hydrogen volume ratio and low ignition power, an amorphous doped film layer can be deposited, which subsequently serves as an incubation layer for the microcrystalline film layer. Optionally, the pressure for preparing the n-type amorphous doped sublayer is 0.5 Torr, 0.51 Torr, 0.52 Torr, 0.53 Torr, 0.54 Torr, 0.55 Torr, 0.56 Torr, or 0.57 Torr.

[0073] In some embodiments, the volume ratio of the gas used to prepare the n-type amorphous doped sublayer is SiH4:H2=1:15-30. At a relatively low volume ratio of silane to hydrogen, combined with a low pressure and a low starting power, an amorphous doped film layer can be deposited, which subsequently serves as an incubation layer for the microcrystalline film layer. The volume ratio of the gas SiH4:H2 used to prepare the n-type amorphous doped sublayer is 1:15, 1:16, 1:17, 1:18, 1:19, 1:20, 1:21, 1:22, 1:23, 1:24, 1:25, 1:26, 1:27, 1:28, 1:29, or 1:30.

[0074] In some embodiments, the ignition power for forming the n-type amorphous doped sublayer is 200W to 800W. At relatively low ignition power, combined with low pressure and a low silane-to-hydrogen volume ratio, an amorphous doped film layer can be deposited, which subsequently serves as an incubation layer for the microcrystalline film layer. Optionally, the ignition power for forming the n-type amorphous doped sublayer is 200W, 250W, 300W, 350W, 400W, 450W, 500W, 550W, 600W, 650W, 700W, 750W, or 800W.

[0075] In some embodiments, the pressure for preparing the p-type amorphous doped sublayer is 0.5 Torr to 0.57 Torr. At relatively low pressures, combined with a low silane-to-hydrogen volume ratio and low ignition power, an amorphous doped film layer can be deposited, which subsequently serves as an incubation layer for the microcrystalline film layer. Optionally, the pressure for preparing the p-type amorphous doped sublayer is 0.5 Torr, 0.51 Torr, 0.52 Torr, 0.53 Torr, 0.54 Torr, 0.55 Torr, 0.56 Torr, or 0.57 Torr.

[0076] In some embodiments, the volume ratio of the gas used to prepare the p-type amorphous doped sublayer is SiH4:H2=1:15-30. At a relatively low volume ratio of silane to hydrogen, combined with a low pressure and a low ignition power, an amorphous doped film layer can be deposited, which subsequently serves as an incubation layer for the microcrystalline film layer. The volume ratio of the gas SiH4:H2 used to prepare the p-type amorphous doped sublayer is 1:15, 1:16, 1:17, 1:18, 1:19, 1:20, 1:21, 1:22, 1:23, 1:24, 1:25, 1:26, 1:27, 1:28, 1:29, or 1:30.

[0077] In some embodiments, the ignition power for forming the p-type amorphous doped sublayer is 200W to 800W. At relatively low ignition power, combined with low pressure and a low silane-to-hydrogen volume ratio, an amorphous doped film layer can be deposited, which subsequently serves as an incubation layer for the microcrystalline film layer. Optionally, the ignition power for forming the p-type amorphous doped sublayer is 200W, 250W, 300W, 350W, 400W, 450W, 500W, 550W, 600W, 650W, 700W, 750W, or 800W.

[0078] In some embodiments, the pressure for forming an n-type microcrystalline growth sublayer on an n-type amorphous doped sublayer is 3 Torr to 5 Torr. Increasing the pressure can transition the growth of the film layer from amorphous to microcrystalline. Within this pressure range, the growth of the microcrystalline film layer is better and the crystallization rate of the film layer is also higher. Optionally, the pressure for forming an n-type microcrystalline growth sublayer on an n-type amorphous doped sublayer is 3 Torr, 3.2 Torr, 3.4 Torr, 3.6 Torr, 3.8 Torr, 4 Torr, 4.2 Torr, 4.4 Torr, 4.6 Torr, 4.8 Torr, or 5 Torr.

[0079] In some embodiments, the volume ratio of the gas used to form the n-type microcrystalline growth sublayer on the n-type amorphous doped sublayer is SiH4:H2=1:150 to 200. Alternatively, the volume ratio of the gas used to form the n-type microcrystalline growth sublayer on the n-type amorphous doped sublayer is 1:150, 1:155, 1:160, 1:156, 1:170, 1:175, 1:180, 1:185, 1:190, 1:195, or 1:200.

[0080] In some embodiments, the starting power for preparing an n-type microcrystalline growth sublayer on an n-type amorphous doped sublayer is 2000W to 3500W. After increasing the starting power, the growth of the film layer can be transformed from amorphous to microcrystalline growth at high power. Within the range of the starting power, the growth effect of the microcrystalline film layer is better and the crystallization rate of the film layer is also higher. Optionally, the starting power for preparing an n-type microcrystalline growth sublayer on an n-type amorphous doped sublayer is 2000W, 2100W, 2200W, 2300W, 2400W, 2500W, 2600W, 2700W, 2800W, 2900W, 3000W, 3100W, 3200W, 3300W, 3400W or 3500W.

[0081] In some embodiments, the pressure for forming a p-type microcrystalline growth sublayer on a p-type amorphous doped sublayer is 3 Torr to 5 Torr. Increasing the pressure can transition the growth of the film layer from amorphous to microcrystalline. Within this pressure range, the growth of the microcrystalline film layer is better and the crystallization rate of the film layer is also higher. Optionally, the pressure for forming a p-type microcrystalline growth sublayer on a p-type amorphous doped sublayer is 3 Torr, 3.2 Torr, 3.4 Torr, 3.6 Torr, 3.8 Torr, 4 Torr, 4.2 Torr, 4.4 Torr, 4.6 Torr, 4.8 Torr, or 5 Torr.

[0082] In some embodiments, the volume ratio of the gas used to form the p-type microcrystalline growth sublayer on the p-type amorphous doped sublayer is SiH4:H2=1:150 to 200. Alternatively, the volume ratio of the gas used to form the p-type microcrystalline growth sublayer on the p-type amorphous doped sublayer is SiH4:H2=1:150, 1:155, 1:160, 1:156, 1:170, 1:175, 1:180, 1:185, 1:190, 1:195, or 1:200.

[0083] In some embodiments, the starting power for preparing a p-type microcrystalline growth sublayer on a p-type amorphous doped sublayer is 2000W to 3500W. After increasing the starting power, the growth of the film layer can be transformed from amorphous to microcrystalline growth at high power. Within the range of the starting power, the growth effect of the microcrystalline film layer is better and the crystallization rate of the film layer is also higher. Optionally, the starting power for preparing a p-type microcrystalline growth sublayer on a p-type amorphous doped sublayer is 2000W, 2100W, 2200W, 2300W, 2400W, 2500W, 2600W, 2700W, 2800W, 2900W, 3000W, 3100W, 3200W, 3300W, 3400W or 3500W.

[0084] In some embodiments, the pressure for preparing an n-type microcrystalline doped sublayer on the n-type microcrystalline growth sublayer is 5Torr to 8Torr. After further increasing the preparation pressure, an n-type microcrystalline doped sublayer is prepared on the n-type microcrystalline growth sublayer. Under high pressure and high power, the growth effect of the n-type microcrystalline doped sublayer can be better, and the crystallization rate of the n-type microcrystalline doped sublayer is higher. The higher crystallization rate can ensure the anisotropy during the subsequent texturing on the surface of the high-thick microcrystalline doped layer, and the subsequent texturing effect is better. Optionally, the pressure for preparing the n-type microcrystalline doped sublayer on the n-type microcrystalline growth sublayer is 5Torr, 5.5Torr, 6Torr, 6.5Torr, 7Torr, 7.5Torr or 8Torr.

[0085] In some embodiments, the starting power for preparing an n-type microcrystalline doped sublayer on the n-type microcrystalline growth sublayer is 4000 W to 7000 W. Further increasing the starting power and preparing an n-type microcrystalline doped sublayer on the n-type microcrystalline growth sublayer, the high power and high pressure combined with the high intensity can achieve better growth of the n-type microcrystalline doped sublayer, resulting in a higher crystallization rate of the n-type microcrystalline doped sublayer. The higher crystallization rate can ensure anisotropy during subsequent texturing on the surface of the thick microcrystalline doped layer, resulting in better texturing results. Optionally, the ignition power for preparing the n-type microcrystal doped sublayer on the n-type microcrystal growth sublayer is 4000W, 4200W, 4400W, 4600W, 4800W, 5000W, 5200W, 5400W, 5600W, 5800W, 6000W, 6200W, 6400W, 6600W, 6800W or 7000W.

[0086] In some embodiments, the pressure for preparing a p-type microcrystalline doped sublayer on a p-type microcrystalline growth sublayer is 5Torr to 8Torr. After continuing to increase the preparation pressure, a p-type microcrystalline doped sublayer is prepared on the p-type microcrystalline growth sublayer. Under high pressure and high power, the growth effect of the p-type microcrystalline doped sublayer can be better, and the crystallization rate of the p-type microcrystalline doped sublayer is higher. The higher crystallization rate can ensure the anisotropy during the subsequent texturing on the surface of the high-thick microcrystalline doped layer, and the subsequent texturing effect is better. Optionally, the pressure for preparing a p-type microcrystalline doped sublayer on a p-type microcrystalline growth sublayer is 5Torr, 5.5Torr, 6Torr, 6.5Torr, 7Torr, 7.5Torr or 8Torr.

[0087] In some embodiments, the starting power for preparing a p-type microcrystalline doped sublayer on the p-type microcrystalline growth sublayer is 4000 W to 7000 W. Further increasing the starting power and preparing a p-type microcrystalline doped sublayer on the p-type microcrystalline growth sublayer under high pressure and high power can achieve better growth of the p-type microcrystalline doped sublayer and a higher crystallization rate of the p-type microcrystalline doped sublayer. The higher crystallization rate can ensure anisotropy during subsequent texturing on the surface of the thick microcrystalline doped layer, resulting in better texturing results. Optionally, the starting power for preparing the p-type microcrystal doped sublayer on the p-type microcrystal growth sublayer is 4000W, 4200W, 4400W, 4600W, 4800W, 5000W, 5200W, 5400W, 5600W, 5800W, 6000W, 6200W, 6400W, 6600W, 6800W or 7000W.

[0088] It is understood that, in some embodiments, texturing the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer is texturing the surfaces of the n-type microcrystalline doped sublayer and the p-type microcrystalline doped sublayer. Using alkaline solution for texturing can anisotropically etch the surfaces of the n-type microcrystalline doped sublayer and the p-type microcrystalline doped sublayer to form a pyramid-shaped microstructure to achieve a light trapping effect and improve the efficiency of the battery. Texturing at a lower concentration of alkaline solution and a lower temperature can reduce the difference in the texture formed on the surfaces of the n-type microcrystalline doped sublayer and the p-type microcrystalline doped sublayer, thereby forming a uniform texture.

[0089] In some embodiments, the alkali solution used for texturing the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer further includes an alcohol additive. The alcohol additive can reduce the intensity of the reaction during the texturing process, making the reaction milder and the texturing effect more uniform.

[0090] In some embodiments, the alkaline solution includes at least one of a NaOH solution and a KOH solution.

[0091] In some embodiments, after texturing the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer, the surface of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer is further treated with an HCl solution or an H2O2 solution. This treatment step can remove impurities such as metal ions and oil residues remaining due to exposure to air.

[0092] In some embodiments, after texturing the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer, the method further includes treating the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer with an HF solution. This treatment step can remove the surface oxide layer remaining due to exposure to air.

[0093] In some embodiments, before forming the intrinsic amorphous silicon layer on both surfaces of the untextured silicon substrate, the method further includes:

[0094] The untextured silicon substrate is subjected to rough polishing, pre-cleaning, polishing and passivation in sequence.

[0095] In some embodiments, the rough polishing includes soaking the surface of the silicon substrate in a strong alkaline solution. The rough polishing can corrode away the damage left by cutting on the surface of the silicon substrate and impurities such as metal residues.

[0096] In one embodiment, the rough polishing includes soaking the surface of the silicon substrate in a NaOH solution with a mass concentration of 5.19%.

[0097] In some embodiments, the pre-cleaning comprises cleaning the surface of the silicon substrate using a mixed solution of a strong base and hydrogen peroxide.

[0098] In one embodiment, the pre-cleaning includes cleaning the surface of the silicon substrate using a mixed solution of NaOH with a mass concentration of 1.12% and H2O2 with a mass concentration of 4.66%.

[0099] In some embodiments, polishing includes soaking the pre-cleaned silicon substrate in a hydrofluoric acid solution into which ozone is introduced, and then grinding and polishing the surface of the silicon substrate after soaking.

[0100] In one embodiment, the mass concentration of the hydrofluoric acid solution is 0.3%, and the concentration of ozone is 30 ppm.

[0101] In some embodiments, the passivation includes deoxidizing the surface of the silicon substrate using a hydrofluoric acid solution. Passivation not only deoxidizes the surface of the silicon substrate but also saturates dangling bonds on the surface of the silicon substrate with hydrogen, thereby achieving better passivation performance during the preparation of the intrinsic amorphous silicon layer on the silicon substrate.

[0102] In one embodiment, the mass concentration of hydrofluoric acid is 5.35%.

[0103] In some embodiments, the thickness of the two intrinsic amorphous silicon layers is 5 nm to 10 nm, respectively. Optionally, the thickness of the two intrinsic amorphous silicon layers is 5 nm, 5.5 nm, 6 nm, 6.5 nm, 7 nm, 7.5 nm, 8 nm, 8.5 nm, 9 nm, 9.5 nm, or 10 nm, respectively.

[0104] In some embodiments, after texturing the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer, the method further includes: preparing a transparent conductive oxide layer on the surfaces of the textured n-type microcrystalline doped layer and the p-type microcrystalline doped layer.

[0105] In some embodiments, the transparent conductive oxide layer is prepared by deposition.

[0106] In some embodiments, after forming a transparent conductive oxide layer on the surfaces of the texturized n-type microcrystalline doped layer and the p-type microcrystalline doped layer, the method further includes forming an electrode layer on the surface of the transparent conductive oxide layer.

[0107] In some embodiments, the electrode layer is prepared by screen printing.

[0108] In some embodiments, a method for preparing a solar cell includes:

[0109] (1) providing a silicon substrate having an untextured surface;

[0110] (2) rough polishing, pre-cleaning, polishing and passivation of the untextured silicon substrate in sequence;

[0111] (3) preparing an intrinsic amorphous silicon layer on both surfaces of an untextured silicon substrate;

[0112] (4) preparing an n-type microcrystalline doped layer and a p-type microcrystalline doped layer on the surfaces of the two intrinsic amorphous silicon layers;

[0113] (5) texturing the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer;

[0114] (6) treating the textured surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer with a mixed solution of HCl, H2O2, and HF solution in sequence;

[0115] (7) preparing a transparent conductive oxide layer on the textured surface of the treated n-type microcrystalline doped layer and the p-type microcrystalline doped layer;

[0116] (8) Preparing an electrode layer on the surface of the transparent conductive oxide layer.

[0117] In one embodiment, a method for preparing a solar cell includes the following steps:

[0118] (1) providing a silicon substrate having an untextured surface;

[0119] (2) rough polishing, pre-cleaning, polishing and passivation of the untextured silicon substrate in sequence;

[0120] (3) preparing an intrinsic amorphous silicon layer on both surfaces of an untextured silicon substrate;

[0121] (4) preparing an n-type amorphous doped sublayer and a p-type amorphous doped sublayer on the surfaces of the two intrinsic amorphous silicon layers;

[0122] (5) preparing an n-type microcrystal growth sublayer on the n-type amorphous doped sublayer, and preparing a p-type microcrystal growth sublayer on the p-type amorphous doped sublayer;

[0123] (6) preparing an n-type microcrystal doped sublayer on the n-type microcrystal growth sublayer, and preparing a p-type microcrystal doped sublayer on the p-type microcrystal growth sublayer;

[0124] (7) texturing the surfaces of the n-type microcrystal doped sublayer and the p-type microcrystal doped sublayer;

[0125] (8) treating the textured surfaces of the n-type microcrystalline doped sublayer and the p-type microcrystalline doped sublayer with a mixed solution of HCl, H2O2, and HF solution in sequence;

[0126] (9) preparing a transparent conductive oxide layer on the textured surface of the treated n-type microcrystalline doped sublayer and the p-type microcrystalline doped sublayer;

[0127] (10) Preparing an electrode layer on the surface of the transparent conductive oxide layer.

[0128] In one embodiment, the method for preparing a solar cell comprises the following steps:

[0129] (1) providing a silicon substrate having an untextured surface;

[0130] (2) rough polishing, pre-cleaning, polishing and passivation of the untextured silicon substrate in sequence;

[0131] (3) preparing an intrinsic amorphous silicon layer on both surfaces of an untextured silicon substrate;

[0132] (4) preparing an n-type amorphous doped sublayer and a p-type amorphous doped sublayer on the surfaces of the two intrinsic amorphous silicon layers;

[0133] (5) preparing an n-type microcrystal growth sublayer on the n-type amorphous doped sublayer, and preparing a p-type microcrystal growth sublayer on the p-type amorphous doped sublayer;

[0134] (6) preparing an n-type microcrystal doped sublayer on the n-type microcrystal growth sublayer, and preparing a p-type microcrystal doped sublayer on the p-type microcrystal growth sublayer;

[0135] (7) texturing the surfaces of the n-type microcrystal doped sublayer and the p-type microcrystal doped sublayer;

[0136] (8) treating the textured surfaces of the n-type microcrystalline doped sublayer and the p-type microcrystalline doped sublayer with a mixed solution of HCl, H2O2, and HF solution in sequence;

[0137] (9) preparing a transparent conductive oxide layer on the textured surface of the treated n-type microcrystalline doped sublayer and the p-type microcrystalline doped sublayer;

[0138] (10) Preparing an electrode layer on the surface of the transparent conductive oxide layer.

[0139] 2 , another embodiment of the present application provides a solar cell, comprising: an untextured silicon substrate, an intrinsic amorphous silicon layer respectively located on both surfaces of the untextured silicon substrate, an n-type microcrystalline doped layer and a p-type microcrystalline doped layer respectively located on the surfaces of the two intrinsic amorphous silicon layers away from the untextured silicon substrate, wherein the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer away from the untextured silicon substrate are both velvet surfaces.

[0140] In some embodiments, the n-type microcrystalline doped layer includes an n-type amorphous doped sublayer, an n-type microcrystalline growth sublayer and an n-type microcrystalline doped sublayer stacked in sequence, and the n-type amorphous doped sublayer is closer to the untextured silicon substrate than the n-type microcrystalline doped sublayer; the p-type microcrystalline doped layer includes a p-type amorphous doped sublayer, a p-type microcrystalline growth sublayer and a p-type microcrystalline doped sublayer stacked in sequence, and the p-type amorphous doped sublayer is closer to the untextured silicon substrate than the p-type microcrystalline doped sublayer.

[0141] In some embodiments, the thickness of the n-type microcrystalline doped sublayer is 0.5 μm to 1 μm. Alternatively, the thickness of the n-type microcrystalline doped sublayer is 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.8 μm, 0.85 μm, 0.9 μm or 1 μm.

[0142] In some embodiments, the thickness of the p-type microcrystalline doped sublayer is 0.5 μm to 1 μm. Alternatively, the thickness of the p-type microcrystalline doped sublayer is 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.8 μm, 0.85 μm, 0.9 μm or 1 μm.

[0143] In some embodiments, the textured surface has a plurality of pyramid structures, each having a height of 0.5 μm to 1 μm. Within this range of pyramid structure heights, the light trapping effect is better. Optionally, the pyramid structure height is 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.8 μm, 0.85 μm, 0.9 μm, or 1 μm.

[0144] In some embodiments, a transparent conductive oxide layer is further disposed on the surface of the n-type microcrystalline doped layer and the surface of the p-type microcrystalline doped layer away from the substrate.

[0145] In some embodiments, an electrode layer is disposed on the surface of the transparent conductive oxide layer.

[0146] The following is a specific implementation method

[0147] Example 1

[0148] The structure of solar cells:

[0149] Referring again to FIG2 , the solar cell includes: an untextured silicon substrate 100, the silicon substrate 100 including a front side and a back side, the front side of the silicon substrate 100 is sequentially stacked with an n-type intrinsic amorphous silicon layer 210, an n-type microcrystal hatching sublayer 310, an n-type microcrystal doping sublayer 410, a front transparent conductive oxide layer 510 and a front electrode layer 610, wherein the n-type intrinsic amorphous silicon layer 210 is closer to the silicon substrate 100 than the front electrode layer 610, the n-type microcrystal hatching sublayer 310 includes a stacked n-type amorphous doping sublayer and an n-type microcrystal growth sublayer, and the n-type amorphous doping sublayer is closer to the n-type The microcrystal growth sublayer is closer to the n-type intrinsic amorphous silicon layer 210; the back side of the substrate is sequentially stacked with a p-type intrinsic amorphous silicon layer 220, a p-type microcrystal incubation sublayer 320, a p-type microcrystal doped sublayer 420, a back transparent conductive oxide layer 520 and a back electrode layer 620, wherein the p-type intrinsic amorphous silicon layer 220 is closer to the silicon substrate 100 than the back electrode layer 620, and the p-type microcrystal incubation sublayer 320 includes a stacked p-type amorphous doped sublayer and a p-type microcrystal growth sublayer, and the p-type amorphous doped sublayer is closer to the p-type intrinsic amorphous silicon layer 220 than the p-type microcrystal growth sublayer.

[0150] Preparation method of solar cell:

[0151] (1) Provide an n-type single crystal silicon wafer whose surface is not textured.

[0152] (2) The surface of the untextured n-type single crystal silicon wafer is subjected to rough polishing, pre-cleaning, polishing and passivation in sequence; the rough polishing is to soak the surface of the silicon substrate 100 in a NaOH solution with a mass concentration of 5.19%, the pre-cleaning is to clean the surface of the silicon substrate 100 with a mixed solution of NaOH with a mass concentration of 1.12% and H2O2 with a mass concentration of 4.66%, the polishing is to soak the pre-cleaned silicon substrate 100 in a hydrofluoric acid solution into which ozone is introduced, the mass concentration of the hydrofluoric acid solution is 0.3%, and the concentration of ozone is 30ppm, and then the surface of the silicon substrate 100 is ground and polished after soaking, and the passivation is to deoxidize the surface of the silicon substrate 100 with a hydrofluoric acid solution with a mass concentration of 5.35%.

[0153] (3) A front intrinsic amorphous silicon layer is prepared on the front side of an untextured n-type single crystal silicon wafer by plasma chemical vapor deposition, and a back intrinsic amorphous silicon layer is prepared on the back side of an untextured n-type single crystal silicon wafer by plasma chemical vapor deposition. The thickness of the front intrinsic amorphous silicon layer and the back intrinsic amorphous silicon layer are both 5nm to 10nm.

[0154] (4) An n-type amorphous doped sublayer is prepared on the surface of the front intrinsic amorphous silicon layer by plasma chemical vapor deposition, and a p-type amorphous doped sublayer is prepared on the surface of the back intrinsic amorphous silicon layer by plasma chemical vapor deposition. The pressure of the plasma chemical vapor deposition is 0.5 Torr to 0.57 Torr, the volume ratio of the deposition gas of the plasma chemical vapor deposition is SiH4:H2=1:15~30, and the starting power of the plasma chemical vapor deposition is 200W~800W.

[0155] (5) Changing the preparation parameters, preparing an n-type microcrystalline growth sublayer on the surface of the n-type amorphous doped sublayer by plasma chemical vapor deposition, and preparing a p-type microcrystalline growth sublayer on the surface of the p-type amorphous doped sublayer by plasma chemical vapor deposition, the pressure of the plasma chemical vapor deposition is 3 Torr to 5 Torr, the volume ratio of the deposition gas of the plasma chemical vapor deposition is SiH4:H2=1:150~200, and the starting power of the plasma chemical vapor deposition is 2000W~3500W.

[0156] (6) Changing the pressure and starting power of plasma chemical vapor deposition, an n-type microcrystal doped sublayer 410 is prepared on the surface of the n-type microcrystal growth sublayer by plasma chemical vapor deposition, and a p-type microcrystal doped sublayer 420 is prepared on the surface of the p-type microcrystal growth sublayer by plasma chemical vapor deposition. The thickness of the n-type microcrystal doped sublayer 410 and the p-type microcrystal doped sublayer 420 are both 0.5 μm to 1 μm. The pressure of plasma chemical vapor deposition is 5 Torr to 8 Torr, and the starting power of plasma chemical vapor deposition is 4000 W to 7000 W.

[0157] (7) After using an alkali solution with a mass concentration of 0.8% to 1% mixed with an alcohol additive, the surfaces of the n-type microcrystalline doped sublayer 410 and the p-type microcrystalline doped sublayer 420 are textured at 60° C. to 65° C.

[0158] (8) After texturing, the surfaces of the n-type microcrystalline doped sublayer 410 and the p-type microcrystalline doped sublayer 420 are treated in sequence using a mixed solution of HCl, H2O2, and an HF solution.

[0159] (9) A front transparent conductive oxide layer 510 is formed on the surface of the treated n-type microcrystalline doped sublayer 410 , and a back transparent conductive oxide layer 520 is formed on the surface of the p-type microcrystalline doped sublayer 420 .

[0160] (10) A front electrode layer 610 is formed on the surface of the front transparent conductive oxide layer 510 , and a back electrode layer 620 is formed on the surface of the back transparent conductive oxide layer 520 .

[0161] The contact between the intrinsic amorphous layer and the substrate in the solar cell prepared in this embodiment is good, the crystallization rate of the n-type microcrystalline doped sublayer 410 and the p-type microcrystalline doped sublayer 420 is high, and the uniformity of the texturing on the surface of the n-type microcrystalline doped sublayer 410 and the p-type microcrystalline doped sublayer 420 is good, and the efficiency of the battery is high.

[0162] Comparative Example 1

[0163] Preparation method of solar cell:

[0164] (1) An n-type single crystal silicon wafer is provided, and the surface of the n-type single crystal silicon wafer is subjected to rough polishing, pre-cleaning, polishing and passivation in sequence; the rough polishing comprises soaking the surface of the n-type single crystal silicon wafer in a NaOH solution with a mass concentration of 5.19%, the pre-cleaning comprises cleaning the surface of the n-type single crystal silicon wafer with a mixed solution of NaOH with a mass concentration of 1.12% and H2O2 with a mass concentration of 4.66%, the polishing comprises soaking the pre-cleaned n-type single crystal silicon wafer in a hydrofluoric acid solution into which ozone is introduced, wherein the mass concentration of the hydrofluoric acid solution is 0.3% and the concentration of ozone is 30 ppm, and then the surface of the n-type single crystal silicon wafer is ground and polished after soaking, and the passivation comprises deoxidizing the surface of the n-type single crystal silicon wafer using a hydrofluoric acid solution with a mass concentration of 5.35%.

[0165] (2) Using an alkali solution with a mass concentration of 1.51% mixed with an alcohol additive, the surface of the deoxidized n-type single crystal silicon wafer is textured at 80° C. to 85° C.

[0166] (3) A front intrinsic amorphous silicon layer is prepared on the front side of the n-type single crystal silicon wafer after texturing by plasma chemical vapor deposition, and a back intrinsic amorphous silicon layer is prepared on the back side of the n-type single crystal silicon wafer after texturing by plasma chemical vapor deposition. The thickness of the front intrinsic amorphous silicon layer and the back intrinsic amorphous silicon layer are both 5nm to 10nm.

[0167] (4) An n-type amorphous doped sublayer is prepared on the surface of the front intrinsic amorphous silicon layer by plasma chemical vapor deposition, and a p-type amorphous doped sublayer is prepared on the surface of the back intrinsic amorphous silicon layer by plasma chemical vapor deposition. The pressure of the plasma chemical vapor deposition is 0.5 Torr to 0.57 Torr, the volume ratio of the deposition gas of the plasma chemical vapor deposition is SiH4:H2=1:15~30, and the starting power of the plasma chemical vapor deposition is 200W~800W.

[0168] (5) Changing the preparation parameters, preparing an n-type microcrystalline growth sublayer on the surface of the n-type amorphous doped sublayer by plasma chemical vapor deposition, and preparing a p-type microcrystalline growth sublayer on the surface of the p-type amorphous doped sublayer by plasma chemical vapor deposition, the pressure of the plasma chemical vapor deposition is 3 Torr to 5 Torr, the volume ratio of the deposition gas of the plasma chemical vapor deposition is SiH4:H2=1:150~200, and the starting power of the plasma chemical vapor deposition is 2000W~3500W.

[0169] (6) A front transparent conductive oxide layer is formed on the surface of the n-type microcrystal growth sublayer, and a back transparent conductive oxide layer is formed on the surface of the p-type microcrystal growth sublayer.

[0170] (7) A front electrode layer is formed on the surface of the front transparent conductive oxide layer, and a back electrode layer is formed on the surface of the back transparent conductive oxide layer.

[0171] The electrical properties of the solar cells prepared in Example 1 and the comparative example are compared, as shown in Table 1 below:

[0172] Table 1

[0173] It can be seen that the solar cell prepared in Example 1 has a higher E than the solar cell prepared by conventional texturing on silicon substrate. ta Improved by nearly 0.7%, R s The V of the solar cell prepared in Example 1 is slightly larger, which is due to the larger thickness of the n-type microcrystalline doped sublayer and the p-type microcrystalline doped sublayer. oc , I sc and FF have been improved to achieve E ta improvement.

[0174] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

Claims

1. A method for preparing a solar cell, comprising: Providing a silicon substrate with a surface that is not textured; Preparing intrinsic amorphous silicon layers on both surfaces of the untextured silicon substrate; Forming an n-type microcrystalline doped layer and a p-type microcrystalline doped layer on the surfaces of the two intrinsic amorphous silicon layers respectively; Texturing is performed on the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer.

2. The method for preparing a solar cell according to claim 1, wherein: The step of preparing an n-type microcrystalline doped layer and a p-type microcrystalline doped layer on the surfaces of the two intrinsic amorphous silicon layers comprises: Preparing an n-type amorphous doped sublayer and a p-type amorphous doped sublayer on the surfaces of the two intrinsic amorphous silicon layers respectively; Preparing an n-type microcrystalline growth sublayer on the n-type amorphous doped sublayer, and preparing a p-type microcrystalline growth sublayer on the p-type amorphous doped sublayer; An n-type microcrystal doping sublayer is prepared on the n-type microcrystal growth sublayer, and a p-type microcrystal doping sublayer is prepared on the p-type microcrystal growth sublayer.

3. The method for preparing a solar cell according to any one of claims 1 to 2, wherein: The texturing on the surface of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer comprises: The surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer are textured at 60° C. to 65° C. using an alkali solution with a mass concentration of 0.8% to 1%.

4. The method for preparing a solar cell according to any one of claims 2 to 3, wherein: The thickness of the n-type microcrystalline doped sublayer is controlled to be 0.5 μm to 1 μm.

5. The method for preparing a solar cell according to any one of claims 2 to 4, wherein: The thickness of the p-type microcrystalline doped sublayer is controlled to be 0.5 μm to 1 μm.

6. The method for preparing a solar cell according to any one of claims 2 to 5, wherein: The pressure for preparing the n-type amorphous doped sublayer is 0.5 Torr to 0.57 Torr.

7. The method for preparing a solar cell according to any one of claims 2 to 6, wherein: The volume ratio of the gas used to prepare the n-type amorphous doped sublayer is SiH4:H2=1:15-30.

8. The method for preparing a solar cell according to any one of claims 2 to 7, wherein: The starting power for preparing the n-type amorphous doped sublayer is 200W to 800W.

9. The method for preparing a solar cell according to any one of claims 2 to 8, wherein: The pressure for preparing the p-type amorphous doped sublayer is 0.5 Torr to 0.57 Torr.

10. The method for preparing a solar cell according to any one of claims 2 to 9, wherein: The volume ratio of the gas used to prepare the p-type amorphous doped sublayer is SiH4:H2=1:15-30.

11. The method for preparing a solar cell according to any one of claims 2 to 10, wherein: The starting power for preparing the p-type amorphous doped sublayer is 200W to 800W.

12. The method for preparing a solar cell according to any one of claims 2 to 11, wherein: The pressure for preparing the n-type microcrystalline growth sublayer on the n-type amorphous doped sublayer is 3 Torr-5 Torr.

13. The method for preparing a solar cell according to any one of claims 2 to 12, wherein: The volume ratio of the gas used to prepare the n-type microcrystalline growth sublayer on the n-type amorphous doped sublayer is SiH4:H2=1:150-200.

14. The method for preparing a solar cell according to any one of claims 2 to 13, wherein: The starting power for preparing the n-type microcrystalline growth sublayer on the n-type amorphous doped sublayer is 2000W-3500W.

15. The method for preparing a solar cell according to any one of claims 2 to 14, wherein: The pressure for preparing the p-type microcrystalline growth sublayer on the p-type amorphous doped sublayer is 3 Torr-5 Torr.

16. The method for preparing a solar cell according to any one of claims 2 to 15, wherein: The volume ratio of the gas used to prepare the p-type microcrystalline growth sublayer on the p-type amorphous doped sublayer is SiH4:H2=1:150-200.

17. The method for preparing a solar cell according to any one of claims 2 to 16, wherein: The starting power for preparing the p-type microcrystalline growth sublayer on the p-type amorphous doped sublayer is 2000W to 3500W.

18. The method for preparing a solar cell according to any one of claims 2 to 17, wherein: The pressure for preparing the n-type microcrystal doping sublayer on the n-type microcrystal growth sublayer is 5 Torr-8 Torr.

19. The method for preparing a solar cell according to any one of claims 2 to 18, wherein: The starting power for preparing the n-type microcrystal doping sublayer on the n-type microcrystal growth sublayer is 4000W to 7000W.

20. The method for preparing a solar cell according to any one of claims 2 to 19, wherein: The pressure for preparing the p-type microcrystalline doped sublayer on the p-type microcrystalline growth sublayer is 5 Torr-8 Torr.

21. The method for preparing a solar cell according to any one of claims 2 to 20, wherein: The starting power for preparing the p-type microcrystal doping sublayer on the p-type microcrystal growth sublayer is 4000W to 7000W.

22. The method for preparing a solar cell according to any one of claims 1 to 21, wherein: Before the intrinsic amorphous silicon layer is prepared on both surfaces of the untextured silicon substrate, the method further comprises: The untextured silicon substrate is subjected to rough polishing, pre-cleaning, polishing and passivation in sequence.

23. The method for preparing a solar cell according to any one of claims 1 to 22, wherein: The thicknesses of the two intrinsic amorphous silicon layers are controlled to be 5nm-10nm respectively.

24. A solar cell comprising: An untextured silicon substrate, an intrinsic amorphous silicon layer respectively located on two surfaces of the untextured silicon substrate, an n-type microcrystalline doped layer and a p-type microcrystalline doped layer respectively located on the surfaces of the two intrinsic amorphous silicon layers away from the untextured silicon substrate, and the surfaces of the n-type microcrystalline doped layer and the p-type microcrystalline doped layer away from the untextured silicon substrate are both velvet surfaces.

25. The solar cell according to claim 24, wherein: The n-type microcrystalline doped layer includes an n-type amorphous doped sublayer, an n-type microcrystalline growth sublayer and an n-type microcrystalline doped sublayer which are stacked in sequence, and the n-type amorphous doped sublayer is closer to the un-textured silicon substrate than the n-type microcrystalline doped sublayer; the p-type microcrystalline doped layer includes a p-type amorphous doped sublayer, a p-type microcrystalline growth sublayer and a p-type microcrystalline doped sublayer which are stacked in sequence, and the p-type amorphous doped sublayer is closer to the un-textured silicon substrate than the p-type microcrystalline doped sublayer.

26. The solar cell according to claim 25, wherein: The thickness of the n-type microcrystalline doped sublayer is 0.5 μm to 1 μm.

27. The solar cell according to any one of claims 25 to 26, wherein: The thickness of the p-type microcrystalline doped sublayer is 0.5 μm to 1 μm.

28. The solar cell according to any one of claims 24 to 27, wherein: The velvet surface has a plurality of pyramid structures, and the height of the pyramid structures is 0.5 μm to 1 μm.

Citation Information

Patent Citations

  • Preparation method of double-sided passivated crystalline silicon solar cell

    CN101937944A

  • Heterojunction solar cell and preparation method thereof

    CN115566094A

  • Silicon heterojunction battery and preparation method thereof

    CN115799402A

  • Preparation method of solar cell and solar cell

    CN116093208A

  • Ultra thin hit solar cell and fabricating method of the same

    US20150287868A1

Cited By

  • Silicon wafer for solar cell, texturing method of silicon wafer, photoelectric device and photovoltaic system

    CN119815975A