Coating composition, coated article, and method for producing coated article

The coating composition, featuring a light interference scaly pigment with alternating layers, addresses the lack of angular color change in automotive paint films by providing a significant brightness and saturation shift, resulting in an achromatic appearance at normal angles and chromatic effects at highlights, enhancing design flexibility and visual appeal.

WO2024202274A1PCT designated stage expired Publication Date: 2024-10-03NIPPON PAINT AUTOMOTIVE COATINGS
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/044222
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2023-12-11
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing coating compositions for automotive paint films fail to provide a significant change in vividness and color appearance when viewed from different angles, lacking the desired design flexibility and originality.

Method used

A coating composition comprising a film-forming resin and a light interference scaly pigment, where the pigment has a specific structure with alternating layers of silicon dioxide or metal fluoride and metals, ensuring a significant change in brightness and saturation when viewed at various angles, creating an achromatic appearance at normal angles and chromatic effects at highlights.

Benefits of technology

The coating composition achieves a sharp change in brightness in the highlight region, appearing achromatic at normal angles but displaying chromatic colors as the viewing angle decreases, offering unprecedented design quality and visual interest.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023044222_03102024_PF_FP_ABST
    Figure JP2023044222_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This coating composition contains a coating film-forming resin and a pigment, and is configured such that: when incident light I45 falls incident at an angle of 45 degrees to the surface of a cured coating film of the coating composition, chroma C* -15 in the L*C*h color system, where the chroma is based on the spectral reflectance of reflected light R-15, which is reflected upon receipt of the incident light, at an angle of -15 degrees to normal reflected light, and chroma C* 15 in the L*C*h color system, where the chroma is based on the spectral reflectance of reflected light R15, which is reflected upon receipt of the incident light I45, at an angle of 15 degrees to normal reflected light, the relationships C* -15 > C* 15 > 10 and C* -15-C* 15 > 20 are satisfied; and chroma C* 45 in the L*C*h color system, where the chroma is based on the spectral reflectance of reflected light R45, which is reflected upon receipt of the incident light I45, at an angle of 45 degrees to normal reflected light, is 10 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Coating composition, coated article, and method for producing coated article

[0001] The present invention relates to coating compositions, coated articles, and methods for making coated articles.

[0002] In recent years, diversifying consumer preferences and the pursuit of originality have led to a wide variety of designs being required for coatings on automobiles and the like. Accordingly, various coating compositions have been developed. For example, Patent Document 1 discloses a coating composition that produces a coating film whose hue changes continuously as the observation angle changes from a face angle to a grazing angle, and that is achromatic at a face angle but chromatic at a grazing angle. Patent Document 2 discloses a coating composition that produces a coating film that is chromatic at a face angle but achromatic at a grazing angle.

[0003] JP 2010-209167 A JP 2012-046676 A

[0004] The present invention has a design different from that of Patent Documents 1 and 2, and aims to provide a coating composition that produces a coating film in which vividness changes significantly in the highlight region and which is observed as achromatic or a color close to achromatic in the face region.

[0005] In order to solve the above problems, the present invention provides the following aspects: [1] A coating composition comprising a film-forming resin and a pigment, wherein incident light I is incident at an angle of 45 degrees to the surface of a cured coating film of the coating composition. 45 The reflected light R received at an angle of −15 degrees with respect to the specular reflection light -15 L based on the spectral reflectance of * C * Chroma C in the h color system * -15 and the incident light I 45 The reflected light R received at an angle of 15 degrees to the specular reflected light 15 L based on the spectral reflectance of * C * Chroma C in the h color system * 15 But, C * -15 >C *15 >10, and C * -15 -C * 15 >20, and the incident light I 45 The reflected light R received at an angle of 45 degrees to the specular reflected light 45 L based on the spectral reflectance of * C * Chroma C in the h color system * 45 [2] The chroma C * -15 [3] The coating composition according to the above [1], wherein the chroma C is 50 or more. * 15 The coating composition according to the above [1] or [2], wherein the reflected light R -15 Lightness L based on the spectral reflectance * -15 and the reflected light R 15 Lightness L based on the spectral reflectance * 15 But, L * -15 -L * 15 [5] The coating composition according to any one of the above [1] to [3], which satisfies the relationship of ≧10. -15 The maximum spectral reflectance SR -15 and the reflected light R -15 Spectral reflectance SR -15 The reflected light R 15 Spectral reflectance SR 15 But, SR -15 -SR 15 [6] The coating composition according to any one of the above [1] to [4], wherein the reflected light R -15 Spectral reflectance SR -15 The wavelength W at which -15 and the reflected light R 15 Spectral reflectance SR 15 The wavelength W at which 15But, |W -15 -W 15 The coating composition according to any one of [1] to [5] above, which satisfies the relationship |≧40 (nm). [7] The coating composition according to any one of [1] to [6] above, wherein the pigment comprises an optically coherent scaly pigment, the optically coherent scaly pigment comprising: a scaly reflective substrate having a first surface and a second surface opposite to the first surface, a first layer comprising at least one element selected from the group consisting of silicon dioxide, aluminum oxide, and a metal fluoride, and a second layer comprising at least one element selected from the group consisting of chromium, aluminum, silver, nickel, palladium, platinum, titanium, vanadium, cobalt, iron, tin, tungsten, molybdenum, rhodium, niobium, copper, and gold, and wherein at least two of the first layers and the second layers are alternately arranged on each of the first surface and the second surface, with the first layer being the innermost layer. [8] A coated article comprising a substrate and a cured coating film of the coating composition described in any one of [1] to [7] above provided on the substrate. [9] A method for producing a coated article, comprising applying the coating composition described in any one of [1] to [7] above onto a substrate, and then curing the coating composition.

[0006] The coating composition of the present invention provides a coating film that exhibits a large change in vividness in the highlight area and is observed as achromatic or nearly so in the face area.

[0007] FIG. 1 is a diagram illustrating the angle of reflected light R -15 and R 15 1 is a graph showing a schematic example of a change in spectral reflectance.

[0008] [Paint Composition] The paint composition according to the present disclosure contains a film-forming resin and a pigment. The cured paint film of the paint composition according to the present disclosure exhibits a chromatic color and exhibits a significant change in vividness within the highlight region. That is, incident light I incident at an angle of 45 degrees to the surface of the cured paint film of the paint composition exhibits a chromatic color and a significant change in vividness within the highlight region. 45 The reflected light R received at an angle of −15 degrees with respect to the specular reflection light -15 L based on the spectral reflectance of* C * Chroma C in the h color system * -15 And, Light I 45 The reflected light R received at an angle of 15 degrees to the specular reflected light 15 L based on the spectral reflectance of * C * Chroma C in the h color system * 15 But, C * -15 >C * 15 >10, and C * -15 -C * 15 >20.

[0009] "C * -15 >C * 15 >10" is the reflected light R -15 and R 15 are all chromatic colors, and the reflected light R -15 The reflected light R 15 It indicates that the color is more saturated than "C * -15 -C * 15 >20" is the reflected light R -15 and reflected light R 15 This indicates that the difference in saturation between the two is greater than 20.

[0010] Furthermore, the cured coating film of the coating composition according to the present disclosure (hereinafter, sometimes simply referred to as "cured coating film") is observed as achromatic or a color close to achromatic in the face region. 45 The reflected light R received at an angle of 45 degrees to the specular reflected light 45 L based on the spectral reflectance of * C * Chroma C in the h color system * 45 The value is 10 or less.

[0011] The cured coating film is achromatic when viewed from its normal direction, but when the viewing angle is gradually reduced, that is, when the angle relative to the specularly reflected light is reduced from the normal direction of the coating film (in this case, a direction at 45 degrees to the specularly reflected light), a chromatic color suddenly appears when a certain angle is reached, providing an unprecedented design feature.

[0012] The highlight region refers to the range of -25 degrees or more and less than 25 degrees with respect to the specularly reflected light of light incident at an angle of 45 degrees. The shade region refers to the range of 75 degrees or more with respect to the specularly reflected light of light incident at an angle of 45 degrees. The face region is the range between the highlight and the shade (more than 25 degrees and less than 75 degrees with respect to the specularly reflected light). In this disclosure, the highlight region is observed as the region of -15 degrees to 15 degrees with respect to the specularly reflected light, which can also be called the super highlight region. In this disclosure, the face region is observed as a point at 45 degrees with respect to the specularly reflected light, which is equal to the normal direction of the cured coating film.

[0013] (Saturation C * -15 , C * 15 , C * 45 ) Saturation C * -15 is the incident light I incident at an angle of 45 degrees to the surface of the cured coating film. 45 The reflected light R received at an angle of −15 degrees with respect to the specular reflection light -15 L based on the spectral reflectance * C * saturation in the h color system. * 15 Similarly, incident light I is incident at an angle of 45 degrees to the surface of the cured coating film. 45 The reflected light R received at an angle of 15 degrees to the specular reflected light 15 L based on the spectral reflectance * C * saturation in the h color system. * 45 Similarly, incident light I is incident at an angle of 45 degrees to the surface of the cured coating film. 45 The reflected light R received at an angle of 45 degrees to the specular reflected light 45 L based on the spectral reflectance *C * h color system.

[0014] Saturation C * -15 is greater than 10. This ensures that the cured coating appears chromatic in the highlight areas. * -15 It is desirable that saturation C is large because it tends to cause large changes in vividness. * -15 The chroma C may be 50 or more, 55 or more, 60 or more, 65 or more, or 70 or more. * -15 is 100 or less, may be 98 or less, or may be 95 or less.

[0015] Saturation C * 15 is greater than 10. On the other hand, from the same viewpoint as above, saturation C * 15 The smaller the value, the better. * 15 may be 40 or less, or may be 35 or less. * 15 may be 15 or more, or 20 or more.

[0016] C * -15 -C * 15 is greater than 20, may be 25 or greater, may be 30 or greater, or may be 35 or greater. * -15 -C * 15 may be 70 or less, may be 65 or less, or may be 60 or less.

[0017] Saturation C * -15 is 60 or more, and chroma C * 15 may be more than 10 and 40 or less.

[0018] Saturation C * 45 is 10 or less. At the point where it becomes closer to achromatic color, the saturation C * 45 The smaller the value, the better.* 45 may be 9 or less, may be 8 or less, or may be 5 or less.

[0019] (Lightness L * -15 , L * 15 ) Lightness L * -15 is the reflected light R -15 L based on the spectral reflectance of * C * Lightness in the h color system. * 15 Similarly, the reflected light R 15 L based on the spectral reflectance of * C * h color system.

[0020] Lightness L * -15 and lightness L * 15 That is, L * -15 -L * 15 ≧10. In this case, the cured coating film may change in brightness as well as saturation within the highlight region, thereby further improving the design properties.

[0021] L * -15 -L * 15 may be 15 or more, or may be 20 or more. * -15 -L * 15 may be 45 or less, or may be 40 or less.

[0022] Lightness L * -15 It is desirable that the value L is large because the change in lightness is likely to be large. * -15 The lightness L may be 35 or more, or may be 40 or more. * 15 When the lightness L is 35 or more, it is ensured that the cured coating film has a certain degree of brightness in the highlight area, and the design properties are further improved. *-15 may be 80 or less, or may be 75 or less.

[0023] Lightness L * 15 From the same viewpoint as above, it is desirable that the value is small. * 15 may be 50 or less, or may be 45 or less. * 15 may be 15 or more, or may be 20 or more.

[0024] (Spectral reflectance SR -15 , S.R. 15 ) Spectral reflectance SR -15 is the reflected light R in the wavelength range of 400 nm to 700 nm (visible light range). -15 The maximum spectral reflectance (%) of the 15 is the reflected light R -15 Spectral reflectance SR -15 The reflected light R 15 is the spectral reflectance of

[0025] Spectral reflectance SR -15 and spectral reflectance SR 15 What is SR? -15 -SR 15 ≧20(%). In this case, the cured coating film may also vary in brightness as well as saturation within the highlight region.

[0026] SR -15 -SR 15 may be 30% or more, or may be 35% or more. -15 -SR 15 may be 130% or less, or may be 120% or less.

[0027] SR -15 may be, for example, 50% or more, 60% or more, or 65% or more. -15 may be, for example, 180% or less, 170% or less, or 160% or less.

[0028] SR 15may be, for example, 10% or more, 20% or more, or 25% or more. 15 may be, for example, 80% or less, 70% or less, or 60% or less.

[0029] (Wavelength W -15 , W 15 ) Wavelength W -15 is the reflected light R at wavelengths from 400 nm to 700 nm. -15 Spectral reflectance SR -15 is the wavelength W at which the wavelength W is the maximum. 15 Similarly, in the wavelength range of 400 nm to 700 nm, the reflected light R 15 Spectral reflectance SR 15 is the wavelength W at which

[0030] Wavelength W -15 and wavelength W 15 That is, |W -15 Value - W 15 The relationship of the reflected light R -15 The peak wavelength of the spectral reflectance of the reflected light R 15 In this case, the hue of the cured coating film may change even within the highlight region.

[0031] |W -15 Value - W 15 The value | may be 43 nm or more, or may be 45 nm or more. -15 Value - W 15 The value | may be equal to or less than 80 nm, or may be equal to or less than 70 nm.

[0032] L * C * In the h color system, L * represents brightness, C * represents the saturation and h represents the hue angle. * C * In the h color system, saturation C * As the value of L increases, the vividness of the substance being measured increases, and as it decreases, the dullness increases. * C * In the h color system, lightness L *As the value of increases, the measured substance becomes brighter, and as the value decreases, the measured substance becomes darker.

[0033] L * C * h color system is CIE * a * b Color system (CIE1976L * a * b * It is calculated based on the CIE 1976L color space. * a * b * The color space can be determined in accordance with JIS Z 8781-4. * a * The RGB color system is defined by the International Commission on Illumination and is described in Section 4.2 of CIE Publication 15.2 (1986). * 15 and lightness L * 110 can be obtained using, for example, a multi-angle colorimeter (for example, BYK-mac i, product name, manufactured by BYK-Gardner).

[0034] FIG. 1 is a diagram illustrating the angle of reflected light. Incident light I is incident on the surface of a multi-layer coating film at an angle of 45 degrees. 45 The specular reflection of R 0 The incident light I 45 The reflected light received at an angle of -15 degrees to the specular reflected light of R -15 The reflected light R -15 From the spectral reflectance of * -15 , brightness L * -15 is calculated. 45 The specular reflection R 0 The reflected light received at an angle of 15 degrees to the 15 The incident light R 15 From the spectral reflectance of * 15 , brightness L * 15 is calculated. 45 The reflected light received at an angle of 45 degrees to the specular reflected light of R45 The reflected light R 45 From the spectral reflectance of * 45 is calculated.

[0035] FIG. 2 shows the reflected light R -15 and R 15 1 is a graph showing a schematic example of a change in the spectral reflectance of a reflected light R. In the graph, the horizontal axis represents wavelength and the vertical axis represents spectral reflectance. 15 The peak value (maximum value) of the spectral reflectance of the reflected light R -15 The peak value (maximum value) of the spectral reflectance of the reflected light R -15 The peak position is shifted to the longer wavelength side.

[0036] In the graph, reflected light R -15 The peak wavelength of the reflected light R is between 600 nm and 700 nm, and it is red in color. -15 The position of the peak wavelength is not limited to this and can be set to a desired wavelength range. The magnitude of the spectral reflectance at each wavelength is also not limited to this. In the wavelength range shown in the graph of Figure 2, there is only one peak for each reflected light, but there may be two or more peaks.

[0037] (Pigment) The coating composition may contain a light-interfering scale-like pigment as a pigment. This increases the change in vividness within the highlight region, and the chroma C * -15 Value and Saturation C * 15 The above relationship can be easily satisfied.

[0038] <<Light-Interfering Scaly Pigment>> The light-interfering scaly pigment (hereinafter sometimes simply referred to as "light-interfering pigment") comprises a scaly reflective substrate having a first surface and a second surface opposite the first surface, a first layer, and a second layer. At least two of the first layers and two of the second layers are alternately arranged on each of the first surface and the second surface, with the first layer being the innermost layer. That is, the light-interfering pigment has at least four layers on each of both surfaces of the scaly reflective substrate. Specifically, the light-interfering pigment has a configuration of second layer / first layer / second layer / first layer / reflective substrate / first layer / second layer / first layer / second layer. Six or more layers may be provided on each of the two surfaces of the reflective substrate.

[0039] The first layer contains at least one selected from the group consisting of silicon dioxide, aluminum oxide, and metal fluorides. Such a first layer is typically transparent and has a low refractive index, which allows for increased strength and thickness of the optical interference pigment without significantly affecting light transmittance.

[0040] The second layer contains at least one selected from the group consisting of chromium, aluminum, silver, nickel, palladium, platinum, titanium, vanadium, cobalt, iron, tin, tungsten, molybdenum, rhodium, niobium, copper, and gold. Such a second layer adjusts light transmittance to generate light interference.

[0041] By alternately disposing two or more first layers with low refractive index and two or more second layers that cause optical interference on each side of the reflective substrate, the coating thickness of the reflective substrate increases, and light reflected by the reflective substrate is more likely to be absorbed by these layers, which is thought to result in greater variations in vividness within the highlight areas of the cured coating film.

[0042] The term "scaly" refers to a shape in which the aspect ratio (average major axis of the pigment / average thickness of the pigment) exceeds 1.0. The aspect ratio of a scaly pigment is, for example, 20 or more and 300 or less. The aspect ratio of a scaly pigment may be 30 or more. The aspect ratio of a scaly pigment may be 200 or less.

[0043] The average thickness of the optical interference pigment is obtained by observing a cross section of a cured coating film containing the optical interference pigment using a transmission electron microscope (TEM) and averaging the thicknesses of 100 arbitrarily selected optical interference pigments.

[0044] The average thickness of the optical interference pigment is, for example, 0.01 μm or more and 1.2 μm or less. The average thickness of the optical interference pigment may be 0.04 μm or more. The average thickness of the optical interference pigment may be 1.1 μm or less.

[0045] The average major axis of the optical coherence pigment is synonymous with the average particle diameter D50. The average particle diameter D50 of the optical coherence pigment may be, for example, 10 μm or more and 100 μm or less. The lower limit of the average particle diameter D50 of the optical coherence pigment may be 15 μm, 20 μm, 25 μm, or 30 μm. The upper limit of the average particle diameter D50 of the optical coherence pigment may be 90 μm, 80 μm, 70 μm, or 60 μm.

[0046] The average particle diameter D50 of the optical coherence pigment can be determined by measuring the maximum lengths of 30 arbitrarily selected optical coherence pigment particles using a shape analysis laser microscope (for example, VK-X 250 manufactured by Keyence Corporation) and calculating the average value of these measurements.

[0047] The reflective substrate has a spectral reflectance of 5% or more and 100% or less in the wavelength range of 400 nm to 700 nm. The reflective substrate may be formed of a metal, a metal compound, an alloy, a nonmetal, or a combination thereof. In particular, the reflective substrate may be a metal, a metal compound, an alloy, or a combination thereof. Examples of metals and alloys include aluminum, copper, silver, gold, platinum, titanium, palladium, nickel, cobalt, niobium, chromium, tin, and alloys thereof, as well as combinations thereof. Examples of metal compounds include carbides, oxides, nitrides, sulfides, and combinations thereof of the above metals. In particular, the reflective substrate may be aluminum.

[0048] The thickness of the reflective substrate may be, for example, 5 nm or more and 1200 nm or less. The lower limit of the thickness of the reflective substrate may be 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 40 nm, 50 nm, 60 nm, or 70 nm. The upper limit of the thickness of the reflective substrate may be 1200 nm, 1100 nm, 1000 nm, 900 nm, 800 nm, 700 nm, 600 nm, or 500 nm.

[0049] The first layer has a refractive index of less than 1.65, for example. The first layer may particularly contain magnesium fluoride. The thickness of the first layer is appropriately set depending on the desired refractive index. The thickness of the first layer may be, for example, 100 nm or more and 1000 nm or less. The thickness of the first layer may be 500 nm or less, 300 nm or less, or 250 nm or less.

[0050] The second layer may be translucent or opaque. The second layer may contain chromium or nickel, particularly chromium. The metals may be present in the second layer as alloys, metal compounds, or mixtures with other materials, such as carbon, graphite, silicon, germanium, cermet, ferric oxide or other metal oxides, or dielectric matrices. Examples of alloys include Inconel (Ni—Cr—Fe), stainless steel, Hastelloy (Ni—Mo—Fe; Ni—Mo—Fe—Cr; Ni—Si—Cu), various titanium alloys, and cobalt-nickel alloys. Examples of mixtures include Ti / C, Ti / W, Ti / Nb, and Ti / Si. Examples of metal compounds include titanium silicide (TiSi2) and titanium boride (TiB2).

[0051] The thickness of the second layer is appropriately set depending on the desired optical coherence. The thickness of the second layer may be, for example, 1 nm or more and 50 nm or less. The thickness of the second layer may be 5 nm or more. The thickness of the second layer may be 10 nm or less.

[0052] In one embodiment, the optical interference pigment is Cr(second layer) / MgF 2 (1st layer) / Cr (2nd layer) / MgF 2 (1st layer) / Al (substrate) / MgF 2(1st layer) / Cr (2nd layer) / MgF 2 (first layer) / Cr (second layer).

[0053] The components contained in the multiple first layers may be the same or different. The thicknesses of the multiple first layers may be the same or different. The components contained in the multiple second layers may be the same or different. The thicknesses of the multiple second layers may be the same or different.

[0054] The optical interference pigment may be colored. The coloring material can be appropriately selected without any particular limitation as long as it does not impair the effect of the optical interference pigment.

[0055] As the optical interference pigment, commercially available products may be used, such as the Chromaflare (trademark) series from VIAVI Solutions.

[0056] The content of the optical coherence pigment, i.e., the mass ratio (PWC) of the optical coherence pigment to the solid content of the resin contained in the coating composition, is, for example, 1% by mass or more and 50% by mass or less. The PWC of the optical coherence pigment may be 5% by mass or more, or 8% by mass or more. The PWC of the optical coherence pigment may be 40% by mass or less, or 35% by mass or less. The solid content of the resin refers to the solid content of all resin components, such as the film-forming resin and curing agent described below.

[0057] <<Other Pigments>> The coating composition may contain a pigment other than the optical coherence pigment. Examples of the other pigment include color pigments, extender pigments, anti-rust pigments, optical coherence pigments other than the above optical coherence pigments, and luster pigments. The mass proportion (PWC) of the other pigment is not particularly limited as long as it is within a range that does not impair the effects of the coating composition according to the present disclosure. The mass proportion (PWC) of the other pigment may be 15% by mass or less, 13% by mass or less, or 10% by mass or less.

[0058] The color pigment may be inorganic or organic. The color pigment may be chromatic or achromatic. Examples of organic color pigments include azo chelate pigments, insoluble azo pigments, condensed azo pigments, diketopyrrolopyrrole pigments, phthalocyanine pigments, indigo pigments, perinone pigments, perylene pigments, dioxane pigments, quinacridone pigments, isoindolinone pigments, and metal complex pigments. Examples of inorganic color pigments include yellow lead, yellow iron oxide, red iron oxide, carbon black, and titanium dioxide. These may be used alone or in combination of two or more.

[0059] Examples of extender pigments include calcium carbonate, barium sulfate, clay, and talc, which may be used alone or in combination of two or more.

[0060] Examples of other light interference pigments and luster pigments include mica pigments such as interference mica, white mica, and colored mica; graphite pigments; glass flake pigments; and metal pigments such as aluminum, copper, zinc, iron, nickel, tin, aluminum oxide, chromium oxide, and alloys containing these. These pigments may be used alone or in combination of two or more. The other light interference pigments and luster pigments may be colored.

[0061] (Film-forming resin) Examples of film-forming resins include acrylic resins, acrylic silicone resins, polyester resins, polyurethane resins, epoxy resins, fluororesins, and silicone resins. These may be used alone or in combination of two or more. Among these, acrylic resins are preferred.

[0062] In the aqueous coating composition, these resins may be contained as an emulsion, a dispersion, or in a state dissolved in a solvent.

[0063] For example, the acrylic resin emulsion can be prepared by emulsion polymerization of α,β-ethylenically unsaturated monomers. Examples of the α,β-ethylenically unsaturated monomers include (meth)acrylic acid esters, α,β-ethylenically unsaturated monomers having an acid group, and α,β-ethylenically unsaturated monomers having a hydroxyl group. The monomers can be used alone or in combination of two or more.

[0064] Examples of (meth)acrylic acid esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, phenyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, dicyclopentadienyl (meth)acrylate, and dihydrodicyclopentadienyl (meth)acrylate. (Meth)acrylic acid esters refer to acrylic acid esters and methacrylic acid esters.

[0065] Examples of α,β-ethylenically unsaturated monomers having an acid group include acrylic acid, methacrylic acid, crotonic acid, 2-acryloyloxyethyl phthalic acid, 2-acryloyloxyethyl succinic acid, ω-carboxy-polycaprolactone mono(meth)acrylate, isocrotonic acid, α-hydro-ω-((1-oxo-2-propenyl)oxy)poly(oxy(1-oxo-1,6-hexanediyl)), maleic acid, fumaric acid, itaconic acid, 3-vinylsalicylic acid, 3-vinylacetylsalicylic acid, 2-acrylamido-2-methylpropanesulfonic acid, p-hydroxystyrene, and 2,4-dihydroxy-4′-vinylbenzophenone.

[0066] Examples of the α,β-ethylenically unsaturated monomer having a hydroxyl group include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, allyl alcohol, methallyl alcohol, and adducts of these with ε-caprolactone.

[0067] Other α,β-ethylenically unsaturated monomers may be used in combination. Examples of the other α,β-ethylenically unsaturated monomers include polymerizable amide compounds, polymerizable aromatic compounds, polymerizable nitriles, polymerizable alkylene oxide compounds, polyfunctional vinyl compounds, polymerizable amine compounds, α-olefins, dienes, polymerizable carbonyl compounds, polymerizable alkoxysilyl compounds, and other polymerizable compounds.

[0068] The emulsion polymerization method is not particularly limited. For example, an emulsifier is dissolved in an aqueous medium containing water or, if necessary, an organic solvent such as an alcohol or an ether (e.g., dipropylene glycol methyl ether, propylene glycol methyl ether, etc.), and an α,β-ethylenically unsaturated monomer and a polymerization initiator are added dropwise with heating and stirring. The α,β-ethylenically unsaturated monomer may be previously emulsified with an emulsifier.

[0069] Polymerization initiators and emulsifiers commonly used by those skilled in the art can be used. If necessary, a chain transfer agent such as a mercaptan (e.g., lauryl mercaptan) or α-methylstyrene dimer may be used to adjust the molecular weight. The reaction temperature, reaction time, and the like can be appropriately selected within ranges commonly used by those skilled in the art. The resulting acrylic resin emulsion is neutralized with a base, if necessary.

[0070] The acrylic resin (acrylic resin emulsion) obtained by emulsion polymerization may have a number average molecular weight of 3,000 or more. The acrylic resin may have a hydroxyl value (solid content hydroxyl value) of 20 mg KOH / g or more and 180 mg KOH / g or less. The acrylic resin may have an acid value (solid content acid value) of 1 mg KOH / g or more and 80 mg KOH / g or less.

[0071] The number average molecular weight is determined by GPC using polystyrene as a standard. The acid value and hydroxyl value are calculated from the monomer composition used in the preparation based on the JIS standard.

[0072] The acrylic resin dispersion can be prepared, for example, by solution polymerizing the above-mentioned α,β-ethylenically unsaturated monomers and dispersing the resultant with a basic compound.

[0073] The water-soluble acrylic resin can be prepared, for example, by solution polymerizing the above-mentioned α,β-ethylenically unsaturated monomer and then solubilizing it in water using a basic compound.

[0074] The acrylic resin incorporated into the solvent-based coating composition can be prepared, for example, by solution polymerization of an α,β-ethylenically unsaturated monomer. The acrylic resin has a number average molecular weight of, for example, 1,000 or more and 20,000 or less. The acrylic resin may have an acid value (solid content acid value) of 1 mgKOH / g or more and 80 mgKOH / g or less. The acrylic resin may have a hydroxyl value (solid content hydroxyl value) of 101 mgKOH / g or more and 200 mgKOH / g or less.

[0075] Curing Agent The coating composition may contain a curing agent, which reacts with the film-forming resin to form a cured coating therewith.

[0076] Examples of curing agents include melamine resins, blocked isocyanate compounds, epoxy compounds, aziridine compounds, carbodiimide compounds, oxazoline compounds, and metal ions. These may be used alone or in combination of two or more. Among these, at least one of melamine resins and blocked isocyanate compounds may be used.

[0077] The melamine resin may be water-soluble or water-insoluble. The melamine resin has a structure in which hydrogen atoms or substituents (such as alkyl ether groups and methylol groups) are bonded to the periphery of a melamine nucleus (triazine nucleus) via three nitrogen atoms. The melamine resin is generally composed of a polynuclear compound in which multiple melamine nuclei are bonded to each other. The melamine resin may also be a mononuclear compound consisting of a single melamine nucleus.

[0078] Commercially available melamine resins may be used. Examples of commercially available melamine resins include the Cymel series (trade name) manufactured by Allnex, specifically Cymel 202, Cymel 204, Cymel 211, Cymel 232, Cymel 235, Cymel 236, Cymel 238, Cymel 250, Cymel 251, Cymel 254, Cymel 266, Cymel 267, Cymel 272, Cymel 285, Cymel 301, Cymel 303, Cymel 325, Cymel 327, Cymel 350, Cymel 370, Cymel 701, Cymel 703, and Cymel 1141; and the U-Ban (trade name) series manufactured by Mitsui Chemicals, Inc. These may be used alone or in combination of two or more.

[0079] The blocked isocyanate compound can be prepared by adding a blocking agent having an active hydrogen to a polyisocyanate such as trimethylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, or isophorone diisocyanate.

[0080] The content of the curing agent may be 10% by mass or more and 80% by mass or less of the resin solid content contained in the coating composition. The content of the curing agent may be 15% by mass or more. The content of the curing agent may be 60% by mass or less.

[0081] (Phosphate Group-Containing Organic Compound) The coating composition may further contain a phosphate group-containing organic compound, which facilitates improving the dispersibility of the optical interference pigment.

[0082] The content of the phosphate group-containing compound may be 0.1% by mass or more and 15% by mass or less of the total solid content of the coating composition. The content of the phosphate group-containing compound may be 1% by mass or more. The content of the phosphate group-containing compound may be 12% by mass or less.

[0083] The phosphate group-containing compound is a compound having a phosphate group (-P(=O)(OR) 2 (wherein each R is independently hydrogen or a hydrocarbon group) The phosphate group-containing compound is not particularly limited as long as it has such a structure. For example, the phosphate group-containing compound is at least one of an alkyl phosphate ester having an alkyl group having 4 to 30 carbon atoms and a phosphate group-containing polymer having a phosphate group value of 5 mgKOH / g or more and 300 mgKOH / g or less.

[0084] <Alkyl Phosphate Ester> The alkyl phosphate ester has an alkyl group having 4 to 30 carbon atoms. Examples of the alkyl phosphate ester include monoalkyl phosphate esters, dialkyl phosphate esters, and mixtures thereof. In the dialkyl phosphate ester, the two alkyl groups may be the same or different. The dialkyl phosphate ester preferably has the same two alkyl groups.

[0085] Examples of alkyl groups having 4 to 30 carbon atoms include butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, docosyl, tetracosyl, hexacosyl, and octacosyl. The alkyl group may be linear or branched.

[0086] Examples of alkyl phosphate esters include butyl acid phosphate (a mixture of monobutyl phosphate ester and dibutyl phosphate ester), 2-ethylhexyl acid phosphate (a mixture of mono-2-ethylhexyl phosphate ester and di-2-ethylhexyl phosphate ester), isodecyl acid phosphate (a mixture of monoisodecyl phosphate ester and diisodecyl phosphate ester), dilauryl acid phosphate, lauryl acid phosphate (a mixture of monolauryl phosphate ester and dilauryl phosphate ester), tridecyl acid phosphate (monotridecyl phosphate), Examples of suitable phosphates include monostearyl acid phosphate, distearyl acid phosphate, stearyl acid phosphate (a mixture of monostearyl phosphate and distearyl phosphate), isostearyl acid phosphate (a mixture of monoisostearyl phosphate and diisostearyl phosphate), oleyl acid phosphate (a mixture of monooleyl phosphate and dioleyl phosphate), and behenyl acid phosphate (a mixture of monobehenyl phosphate and dibehenyl phosphate).

[0087] <Phosphate Group-Containing Polymer> The phosphate group-containing polymer has a phosphate group value of 5 mgKOH / g or more and 300 mgKOH / g or less. The phosphate group value of the phosphate group-containing polymer may be 10 mgKOH / g or more, or 50 mgKOH / g or more. The phosphate group value of the phosphate group-containing polymer may be 250 mgKOH / g or less, or 150 mgKOH / g or less.

[0088] The phosphate value is calculated based on JIS K5601 2-1 Acid Value Measurement Method. Specifically, the acid value is the number of milligrams of potassium hydroxide (KOH) required to neutralize the free acid in 1 g of nonvolatile matter of the product.

[0089] The number average molecular weight of the phosphate group-containing polymer is, for example, 1,000 or more and 50,000 or less. The number average molecular weight of the phosphate group-containing polymer may be 3,000 or more, or 5,000 or more. The number average molecular weight of the phosphate group-containing polymer may be 30,000 or less, or 20,000 or less.

[0090] Examples of phosphate group-containing polymers include acrylic resins, polyester resins, polyether resins, and epoxy resins, each having a phosphate group value of 5 mgKOH / g or more and 300 mgKOH / g or less. These may be used alone or in combination of two or more. Among these, phosphate group-containing acrylic resins are particularly preferred. The phosphate group-containing acrylic resin can be obtained, for example, by polymerizing a phosphate group-containing α,β-ethylenically unsaturated monomer, or by copolymerizing this monomer with another α,β-ethylenically unsaturated monomer that does not contain a phosphate group. In particular, by using the above-mentioned light interference pigment in combination with a phosphate group-containing acrylic resin, the color vividness in the highlight region becomes more easily variable.

[0091] (Additives) The coating composition may contain additives commonly used by those skilled in the art, such as surface conditioners, viscosity control agents, thickeners, antioxidants, ultraviolet inhibitors, and antifoaming agents.

[0092] [Coated Article] The coated article according to the present disclosure comprises a substrate and the above-described cured coating film provided on the substrate. A coated article comprising the above-described cured coating film exhibits a significant change in vividness within the highlight region, and is observed as an achromatic or nearly so color in the face region. Therefore, when the coated article is viewed from the normal direction of the cured coating film, it appears achromatic. However, as the viewing angle is gradually reduced, a chromatic color suddenly emerges once the viewing angle exceeds a certain value, resulting in an unprecedented design.

[0093] - First embodiment In the first embodiment, the coated article comprises a substrate, the above-mentioned cured coating film (hereinafter sometimes referred to as the "base coating film") provided on the substrate, and a clear coating film provided on the base coating film.

[0094] (Substrate) Examples of the material of the substrate include metal, plastic, and foam. Among them, metal (particularly, casting) may be used, and metal that can be electrocoated may be used. Examples of such metals include iron, copper, aluminum, tin, zinc, etc., and alloys containing these metals.

[0095] The shape of the substrate is not particularly limited, and may be flat or three-dimensional. Specific examples of the substrate include automobile bodies and parts thereof, such as passenger cars, trucks, motorcycles, and buses.

[0096] The metal substrate may have been subjected to a chemical conversion treatment using a phosphate-based chemical conversion treatment agent, a zirconium-based chemical conversion treatment agent, or the like, and may have been subjected to electrodeposition coating. The electrodeposition coating composition may be either a cationic type or an anionic type. A cationic electrodeposition coating composition can form a coating film with excellent corrosion resistance.

[0097] The metal substrate may have an electrodeposition coating film and an intermediate coating film formed thereon. The intermediate coating film is usually formed for the purpose of improving the adhesion and durability of the multi-layer coating film. The coating composition for the intermediate coating may contain, for example, a film-forming resin, a curing agent, a color pigment, and an extender pigment. Examples of the film-forming resin and curing agent include those contained in the coating composition according to the present disclosure.

[0098] (Base Coating Film) The base coating film is formed from the coating composition according to the present disclosure (hereinafter, may be referred to as "base coating composition"). The thickness of the base coating film may be 0.2 μm or more and 50 μm or less. The thickness of the base coating film may be 3 μm or more. The thickness of the base coating film may be 40 μm or less, 30 μm or less, or 20 μm or less.

[0099] (Clear Coating Film) The clear coating film protects the base coating film. The thickness of the clear coating film may be, for example, 10 μm or more and 80 μm or less. The thickness of the clear coating film may be 20 μm or more. The thickness of the clear coating film may be 60 μm or less.

[0100] The clear coating film is formed by a clear coating composition. The clear coating composition may be solvent-based, water-based, or powder-type. From the viewpoints of transparency, acid etching resistance, etc., the solvent-based clear coating composition may contain an acrylic resin and / or polyester resin as a film-forming resin and an amino resin and / or isocyanate as a curing agent. The solvent-based clear coating composition may also contain an acrylic resin and / or polyester resin having a carboxylic acid and / or an epoxy group.

[0101] The clear coating composition may contain the above-mentioned various pigments to the extent that the transparency and the effects of the coating composition according to the present disclosure are not impaired. The clear coating composition may contain various additives as needed. Examples of additives include ultraviolet absorbers, antioxidants, antifoaming agents, surface conditioners, and pinhole inhibitors.

[0102] Second Embodiment In the second embodiment, the coated article comprises a substrate, another cured coating film (hereinafter referred to as the "first base coating film") provided on the substrate, a cured coating film (hereinafter referred to as the "second base coating film") formed from the coating composition according to the present disclosure provided on the first base coating film, and a clear coating film provided on the second base coating film. The substrate and the clear coating film are the same as those in the first embodiment. The second base coating film is formed from the coating composition according to the present disclosure and is the same as the base coating film in the first embodiment. The first base coating film will be described below.

[0103] (First base coating film) The first base coating film is formed from a first base paint composition. The first base paint composition may contain a first film-forming resin and a pigment other than the above-mentioned optical coherence pigment.

[0104] The first film-forming resin may be the same as the film-forming resin used in the coating composition according to the present disclosure. The first film-forming resin may be the same or different. The pigment may be any pigment other than the above-mentioned optical interference pigment. The first base coating composition may also contain the same components as the coating composition according to the present disclosure.

[0105] The thickness of the first base coating film may be, for example, 0.2 μm or more and 20 μm or less, 5 μm or more, 15 μm or less, or 10 μm or less.

[0106] [Method for producing a coated article] A method for producing a coated article according to the present disclosure includes applying a coating composition according to the present disclosure to an object to be coated, followed by curing the coating composition, thereby obtaining the coated article.

[0107] The coated article according to the first embodiment, which further comprises a clear coating film, can be obtained by sequentially coating a substrate with the coating composition (base coating composition) according to the present disclosure and the clear coating composition, and then simultaneously curing both.

[0108] The coated article according to the second embodiment, which further comprises a first base coating film and a clear coating film, is obtained by sequentially coating the above-mentioned first base coating composition and the coating composition according to the present disclosure (second base coating composition) on the substrate, curing both simultaneously, and then coating and curing the clear coating composition.

[0109] The coated article according to the second embodiment may also be obtained by sequentially coating the above-mentioned first base coating composition, the coating composition according to the present disclosure (hereinafter sometimes referred to as the "second base coating composition"), and the clear coating composition, and then simultaneously curing them.

[0110] After application of the first base coating composition, preheating may be performed before application of the coating composition according to the present disclosure (second base coating composition). After application of the coating composition according to the present disclosure, preheating may be performed before application of the clear coating composition.

[0111] Examples of the coating method include air spray coating, airless spray coating, electrostatic spray coating, multi-stage coating (preferably two-stage coating) using air electrostatic spray coating, and coating that combines air electrostatic spray coating with a rotary atomizing electrostatic coater.

[0112] The curing of each coating composition is carried out, for example, at a heating temperature of 80° C. to 180° C. (preferably 100° C. to 160° C.) for a heating time of 5 to 60 minutes (preferably 10 to 30 minutes).

[0113] The present invention will be described in more detail with reference to the following examples, but is not limited thereto. In the examples, "parts" and "%" are by weight unless otherwise specified.

[0114] [Production Example 1] Production of acrylic resin emulsion (film-forming resin) 633 parts of deionized water was added to a reaction vessel, and the temperature was raised to 80°C while mixing and stirring in a nitrogen stream. Next, a monomer emulsion consisting of a first-stage monomer mixture of 75.65 parts by mass of styrene (ST), 178.96 parts by mass of methyl methacrylate (MMA), 75.94 parts by mass of n-butyl acrylate (BA), 64.45 parts by mass of 2-ethylhexyl acrylate (2-EHA), and 105.00 parts by mass of hydroxyethyl methacrylate (HEMA), 25.00 parts of Aqualon HS-10 (polyoxyethylene alkylpropenylphenyl ether sulfate, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), 25.00 parts of Adeka Reasoap NE-20 (α-[1-[(allyloxy)methyl]-2-(nonylphenoxy)ethyl]-ω-hydroxyoxyethylene, manufactured by Asahi Denka Co., Ltd.), and 400 parts of deionized water, and an initiator solution consisting of 1.2 parts of ammonium persulfate and 500 parts of deionized water were added dropwise to the reaction vessel in parallel over 1.5 hours. After the dropwise addition was completed, the mixture was aged at the same temperature for 1 hour.

[0115] Further, at 80°C, a second-stage monomer mixture of 53.65 parts by mass of styrene (ST), 178.96 parts by mass of methyl methacrylate (MMA), 75.94 parts by mass of n-butyl acrylate (BA), 64.45 parts by mass of 2-ethylhexyl acrylate (2-EHA), 105.00 parts by mass of hydroxyethyl methacrylate (HEMA), and 22 parts by mass of acrylic acid, a monomer emulsion of 10 parts of Aqualon HS-10 and 250 parts of deionized water, and an initiator solution of 3.0 parts of ammonium persulfate and 500 parts of deionized water were added dropwise to the reaction vessel in parallel over 1.5 hours. After completion of the dropwise addition, the mixture was aged at the same temperature for 2 hours.

[0116] The mixture was then cooled to 40°C and filtered through a 400 mesh filter, after which 100 parts of deionized water and 1.6 parts of dimethylaminoethanol were added to adjust the pH to 6.5, yielding an acrylic resin emulsion having an average particle size of 150 nm, a nonvolatile content of 35%, a solids acid value of 20 mgKOH / g, and a hydroxyl value of 100 mgKOH / g.

[0117] [Production Example 2] Production of phosphoric acid group-containing organic compound A 1-liter reaction vessel equipped with a stirrer, a temperature regulator, and a condenser was charged with 40 parts of ethoxypropanol, and 121.7 parts of a monomer solution consisting of 40 parts of a solution obtained by dissolving 20 parts of Phosmer PP (acid phosphooxyhexa(oxypropylene) monomethacrylate manufactured by Unichemical Co., Ltd.) in 4 parts of styrene, 35.96 parts of n-butyl acrylate, 18.45 parts of ethylhexyl methacrylate, 13.92 parts of 2-hydroxyethyl methacrylate, 7.67 parts of methacrylic acid, and 20 parts of ethoxypropanol, and 121.7 parts of a monomer solution consisting of 1.7 parts of azobisisobutyronitrile was added dropwise at 120°C over 3 hours, and stirring was continued for an additional 1 hour. The resulting phosphate group-containing organic compound had an acid value of 105 mgKOH / g, including a phosphate group value of 55 mgKOH / g, a hydroxyl group value of 60 mgKOH / g, a number average molecular weight of 6,000, and a nonvolatile content of 63%.

[0118] In the Examples herein, the number average molecular weight was measured using a GPC apparatus "HLC8220GPC" (trade name, manufactured by Tosoh Corporation) and four columns, "Shodex KF-606M" and "Shodex KF-603" (both trade names, manufactured by Showa Denko K.K.), under the conditions of a mobile phase of tetrahydrofuran, a measurement temperature of 40°C, a flow rate of 0.6 cc / min, and a detector of RI.

[0119] In the examples of this specification, the acid value and phosphate value of the phosphate group-containing organic compound were calculated based on the definition of acid value in JIS K5601 2-1 (the number of milligrams of potassium hydroxide (KOH) required to neutralize the free acid in 1 g of sample (non-volatile matter)). The hydroxyl value was calculated based on the definition of hydroxyl value in JIS K0070 (the number of milligrams of potassium hydroxide required to neutralize the acetic acid bonded to the hydroxyl group when 1 g of sample is acetylated).

[0120] [Production Example 3] Production of Water-Soluble Acrylic Resin 23.89 parts of tripropylene glycol methyl ether and 16.11 parts of propylene glycol methyl ether were added to a reaction vessel, and the mixture was heated to 105°C while being mixed and stirred in a nitrogen stream. Next, a monomer mixture containing 13.1 parts of methyl methacrylate, 68.4 parts of ethyl acrylate, 11.6 parts of 2-hydroxyethyl methacrylate, and 6.9 parts of methacrylic acid was prepared, and an initiator solution consisting of 100 parts of the monomer mixture, 10.0 parts of tripropylene glycol methyl ether, and 1 part of tert-butyl peroxy 2-ethylhexanoate was added dropwise to the reaction vessel in parallel over 3 hours. After completion of the dropwise addition, the mixture was aged at the same temperature for 0.5 hours.

[0121] Further, an initiator solution consisting of 5.0 parts of tripropylene glycol methyl ether and 0.3 parts of tertiary butyl peroxy 2-ethylhexanoate was added dropwise to the reaction vessel over 0.5 hours. After the completion of the addition, the mixture was aged at the same temperature for 2 hours.

[0122] Using a solvent remover, 16.1 parts of the solvent was distilled off under reduced pressure (70 torr) at 110°C, and then 204 parts of deionized water and 7.1 parts of dimethylaminoethanol were added to obtain a water-soluble acrylic resin solution. The resulting water-soluble acrylic resin solution had a nonvolatile content of 30%, a solids acid value of 40 mgKOH / g, a hydroxyl value of 50 mgKOH / g, and a viscosity of 140 poise (E-type viscometer, 1 rpm, 25°C).

[0123] Details of the pigments used in the examples and comparative examples are shown in Table 1.

[0124]

[0125] [Example 1] (1) Preparation of base coating composition (1-1) Preparation of color pigment dispersion 1 34.5 parts of the water-soluble acrylic resin solution obtained in Production Example 3, 10.4 parts of carbon black (color pigment), 18.6 parts of a pigment dispersant, 36.0 parts of ion-exchanged water, and 0.5 parts of an antifoaming agent were mixed using a stirrer such as a disperser. Next, the mixture was dispersed using a disperser filled with 0.05 mm zirconia beads as a medium at a volume filling rate of 70%, to obtain color pigment dispersion 1.

[0126] (1-2) Preparation of base coating composition 133.3 parts of acrylic resin emulsion of Production Example 1, 9.0 parts of dimethylaminoethanol, 35.6 parts of Cymel 370N (curing agent, solids content 87%), 13.5 parts of colored pigment dispersion 1, 10 parts by weight of light interference pigment per 100 parts by weight of resin solids, 5 parts of the phosphate group-containing organic compound of Production Example 2, 0.4 parts of lauryl acid phosphate, 50 parts of butyl cellosolve, 5.5 parts of Noigen EA-207D (surfactant, solids content 55%), 3 parts of linoleic acid were uniformly dispersed. After adding dimethylaminoethanol to adjust the pH to 8.1, it was diluted with deionized water to obtain an aqueous base coating composition with a resin solids concentration of 24.5% by weight.

[0127] (2) Formation of Multilayer Coating Films A zinc phosphate-treated, 0.8 mm thick, 30 cm long, and 40 cm wide dull steel plate was electrodeposited with the cationic electrodeposition coating composition "Power Top U-50" (manufactured by Nippon Paint Automotive Coatings) to a dry film thickness of 20 μm, and baked at 160°C for 30 minutes. The resulting coated plate was air-sprayed with the intermediate coating composition "OP-30P Middle Gray" (manufactured by Nippon Paint Automotive Coatings, polyester-melamine paint, pre-diluted to 25 seconds (measured at 20°C using a No. 4 Ford cup)) using an Anest Iwata air spray gun W-101-132G to a dry film thickness of 35 μm, and then baked and cured at 140°C for 30 minutes. In this way, a coated substrate having an electrodeposition coating film and an intermediate coating film was obtained.

[0128] The above aqueous base coating composition was spray-coated onto the substrate at a room temperature of 23°C and a humidity of 68% to a dry film thickness of 15 µm. After setting for 4 minutes, the coating was preheated at 80°C for 5 minutes.

[0129] The plate was allowed to cool to room temperature, and then a clear coating composition (Macflow-O-1810 (a solvent-based clear coating manufactured by Nippon Paint Automotive Coatings Co., Ltd.)) was spray-painted onto the plate to a dry film thickness of 35 μm, and the resulting coating was allowed to set for 7 minutes. The plate was then baked in a dryer at 140°C for 30 minutes, yielding a coated article having a multi-layer coating film consisting of a base coating film and a clear coating film.

[0130] Example 2 An aqueous base coating composition and a coated article were obtained in the same manner as in Example 1, except that Color Pigment Dispersion 1 was not blended.

[0131] [Comparative Example 1] (1) Preparation of base coating composition (1-1) Preparation of color pigment dispersion 2 76.8 parts of the water-soluble acrylic resin solution obtained in Production Example 3, 11.7 parts of perylene red (color pigment), 12.5 parts of anchor red (color pigment), 3.0 parts of carbon black (color pigment), 16.0 parts of titanium oxide (color pigment), 22.7 parts of pigment dispersant, 59.0 parts of ion-exchanged water, and 0.6 parts of antifoaming agent were mixed using a stirrer such as a disperser. Next, the mixture was dispersed using a disperser filled with 0.05 mm zirconia beads as a medium at a volume filling rate of 70%, to obtain color pigment dispersion 2.

[0132] (1-2) Preparation of base coating composition 143.3 parts of acrylic resin emulsion of Production Example 1, 1.4 parts of dimethylaminoethanol, 35.6 parts of Cymel 370N (curing agent, solids content 87%), 89.4 parts of colored pigment dispersion 2, 1.4 parts by weight of other light interference pigment 1 per 100 parts by weight of resin solids, 5 parts of the phosphate group-containing organic compound of Production Example 2, 0.4 parts of lauryl acid phosphate, 50 parts of butyl cellosolve, 5.5 parts of Noigen EA-207D (surfactant, solids content 55%), 3 parts of linoleic acid were uniformly dispersed. After adding dimethylaminoethanol to adjust the pH to 8.1, it was diluted with deionized water to prepare an aqueous base coating composition with a resin solids concentration of 24.5% by weight.

[0133] (2) Formation of Multi-Layer Coating Films Using the aqueous base coating composition prepared above, a coated article having a multi-layer coating film was obtained in the same manner as in Example 1.

[0134] [Comparative Example 2] (1) Preparation of base coating composition (1-1) Preparation of color pigment dispersion 3 59.8 parts of the water-soluble acrylic resin solution obtained in Production Example 3, 11.7 parts of perylene red (color pigment), 6.3 parts of carbon black (color pigment), 25.3 parts of pigment dispersant, 56.8 parts of ion-exchanged water, and 0.8 parts of antifoaming agent were mixed using a stirrer such as a disperser. Next, the mixture was dispersed using a disperser filled with 0.05 mm zirconia beads as a medium at a volume filling rate of 70%, to obtain color pigment dispersion 3.

[0135] (1-2) Preparation of base coating composition 143.3 parts of acrylic resin emulsion of Production Example 1, 1.4 parts of dimethylaminoethanol, 35.6 parts of Cymel 370N (curing agent, solids content 87%), 56.1 parts of colored pigment dispersion 3, 6.2 parts by weight of other light interference pigment 2 per 100 parts by weight of resin solids, 5 parts of the phosphate group-containing organic compound of Production Example 2, 0.4 parts of lauryl acid phosphate, 50 parts of butyl cellosolve, 5.5 parts of Noigen EA-207D (surfactant, solids content 55%), 3 parts of linoleic acid were uniformly dispersed. After adding dimethylaminoethanol to adjust the pH to 8.1, it was diluted with deionized water to prepare an aqueous base coating composition with a resin solids concentration of 24.5% by weight.

[0136] (2) Formation of Multi-Layer Coating Films Using the aqueous base coating composition prepared above, a coated article having a multi-layer coating film was obtained in the same manner as in Example 1.

[0137] [Comparative Example 3] (1) Preparation of base coating composition (1-1) Preparation of color pigment dispersion 4 74.1 parts of the water-soluble acrylic resin solution obtained in Production Example 3, 3.1 parts of perylene red (color pigment), 13.1 parts of anchor red (color pigment), 10.4 parts of carbon black (color pigment), 2.8 parts of titanium oxide (color pigment), 24.1 parts of pigment dispersant, 56.3 parts of ion-exchanged water, and 0.6 parts of defoamer were mixed using a stirrer such as a disperser. Next, the mixture was dispersed using a disperser filled with 0.05 mm zirconia beads as a medium at a volume filling rate of 70%, to obtain color pigment dispersion 4.

[0138] (1-2) Preparation of base coating composition 143.3 parts of acrylic resin emulsion of Production Example 1, 1.4 parts of dimethylaminoethanol, 35.6 parts of Cymel 370N (curing agent, solids content 87%), 16.7 parts of colored pigment dispersion 4, 6.6 parts by weight of other light interference pigment 3 per 100 parts by weight of resin solids, 5 parts of the phosphate group-containing organic compound of Production Example 2, 0.4 parts of lauryl acid phosphate, 50 parts of butyl cellosolve, 5.5 parts of Noigen EA-207D (surfactant, solids content 55%), 3 parts of linoleic acid were uniformly dispersed. After adding dimethylaminoethanol to adjust the pH to 8.1, it was diluted with deionized water to prepare an aqueous base coating composition with a resin solids concentration of 24.5% by weight.

[0139] (2) Formation of Multi-Layer Coating Films Using the aqueous base coating composition prepared above, a coated article having a multi-layer coating film was obtained in the same manner as in Example 1.

[0140] [Comparative Example 4] (1) Preparation of base coating composition (1-1) Preparation of color pigment dispersion 5 34.5 parts of the water-soluble acrylic resin solution obtained in Production Example 3, 10.4 parts of carbon black (color pigment), 18.6 parts of pigment dispersant, 36.0 parts of ion-exchanged water, and 0.5 parts of antifoaming agent were mixed using a stirrer such as a disperser. Next, the mixture was dispersed using a disperser filled with 0.05 mm zirconia beads as a medium at a volume filling rate of 70%, to obtain color pigment dispersion 5.

[0141] (1-2) Preparation of base coating composition 133.3 parts of the acrylic resin emulsion of Production Example 1, 9.0 parts of dimethylaminoethanol, 35.6 parts of Cymel 370N (curing agent, solids content 87%), 43.2 parts of colored pigment dispersion 5, 0.8 parts by weight of other light interference pigment 3 per 100 parts by weight of resin solids, 3.1 parts by weight of other light interference pigment 4 per 100 parts by weight of resin solids, 5 parts of the phosphate group-containing organic compound of Production Example 2, 0.4 parts of lauryl acid phosphate, 50 parts of butyl cellosolve, 5.5 parts of Noigen EA-207D (surfactant, solids content 55%), and 3 parts of linoleic acid were uniformly dispersed. After adjusting the pH to 8.1 by adding dimethylaminoethanol, the mixture was diluted with deionized water to prepare an aqueous base coating composition with a resin solids concentration of 24.5% by weight.

[0142] (2) Formation of Multi-Layer Coating Films Using the aqueous base coating composition prepared above, a coated article having a multi-layer coating film was obtained in the same manner as in Example 1.

[0143] [Example 3] (1) Preparation of the first base coating composition (1-1) Preparation of color pigment dispersion 6 78.3 parts of the water-soluble acrylic resin solution obtained in Production Example 3, 11.5 parts of perylene red (color pigment), 10.4 parts of carbon black (color pigment), 2.0 parts of Hoster Palm Violet (color pigment), 1.4 parts of Shannin Blue (color pigment), 34.3 parts of DISPEX ULTRA PA 4550 as a pigment dispersant, 81.3 parts of ion-exchanged water, and 1.1 parts of BYK-011 as an antifoaming agent were mixed with a stirrer such as a disperser. Then, the mixture was dispersed in a disperser filled with 0.05 mm zirconia beads as a medium at a volume filling rate of 70%, to obtain a color pigment dispersion 6.

[0144] (1-2) Preparation of the first base coating composition 122.1 parts of the acrylic resin emulsion of Production Example 1, 2.0 parts of dimethylaminoethanol, Cymel 370N (curing agent, solids content 87%) 35.6 parts, colored pigment dispersion 6 102.0 parts, paste containing a non-optical interference bright pigment (active ingredient 60%) 2.1 parts per 100 parts by weight of resin solids, 5 parts of the phosphate group-containing organic compound of Production Example 2, lauryl acid phosphate 0.4 parts, butyl cellosolve 50 parts, Noigen EA-207D (surfactant, solids content 55%) 5.5 parts, 3 parts of linoleic acid were uniformly dispersed. After adjusting the pH to 8.1 by adding dimethylaminoethanol, it was diluted with deionized water to prepare a first base coating composition with a resin solids concentration of 19.9% ​​by weight.

[0145] (2) Preparation of the second base coating composition 143.3 parts of the acrylic resin emulsion of Production Example 1, 1.4 parts of dimethylaminoethanol, 35.6 parts of Cymel 370N (curing agent, solids content 87%), 30 parts by weight of light interference pigment per 100 parts by weight of resin solids, 5 parts of the phosphate group-containing organic compound of Production Example 2, 0.4 parts of lauryl acid phosphate, 50 parts of butyl cellosolve, 5.5 parts of Noigen EA-207D (surfactant, solids content 55%), 3 parts of linoleic acid were uniformly dispersed. After adding dimethylaminoethanol to adjust the pH to 8.1, it was diluted with deionized water to prepare an aqueous second base coating composition with a resin solids concentration of 11.0% by weight.

[0146] (3) Formation of Multilayer Coating Films In the same manner as in Example 1, a coated article having an electrodeposition coating film and an intermediate coating film was obtained.

[0147] The first base coating composition prepared above was spray-coated onto the substrate at a room temperature of 23°C and a humidity of 68% to a dry film thickness of 8 µm. After setting for 4 minutes, the coating was preheated at 80°C for 5 minutes.

[0148] Subsequently, the aqueous second base coating composition prepared above was spray-coated wet-on-wet at a room temperature of 23°C and a humidity of 68% to a dry film thickness of 4 µm. After setting for 4 minutes, the coating was preheated at 80°C for 5 minutes.

[0149] After the mounting board was allowed to cool to room temperature, the clear coating composition was air spray painted on in the same manner as in Example 1 to obtain a painted article having a multi-layer coating film consisting of a first base coating film, a second base coating film and a clear coating film.

[0150] Example 4 A multi-layer coating film was formed in the same manner as in Example 3, except that the second aqueous base coating composition prepared below was used.

[0151] (2) Preparation of second base coating composition (2-1) Preparation of color pigment dispersion 7 38.9 parts of the water-soluble acrylic resin solution obtained in Production Example 3, 11.7 parts of perylene red (color pigment), 14.0 parts of pigment dispersant, 34.9 parts of ion-exchanged water, and 0.5 parts of antifoaming agent were mixed using a stirrer such as a disperser. Next, the mixture was dispersed using a disperser filled with 0.05 mm zirconia beads as a medium at a volume filling rate of 70%, to obtain color pigment dispersion 7.

[0152] (2-2) Preparation of the second base coating composition 143.3 parts of the acrylic resin emulsion of Production Example 1, 1.4 parts of dimethylaminoethanol, 35.6 parts of Cymel 370N (curing agent, solids content 87%), 8.5 parts of colored pigment dispersion 7, 29.5 parts by weight of light interference pigment per 100 parts by weight of resin solids, 5 parts of the phosphate group-containing organic compound of Production Example 2, 0.4 parts of lauryl acid phosphate, 50 parts of butyl cellosolve, 5.5 parts of Noigen EA-207D (surfactant, solids content 55%), 3 parts of linoleic acid were uniformly dispersed. After adjusting the pH to 8.1 by adding dimethylaminoethanol, it was diluted with deionized water to prepare an aqueous second base coating composition with a resin solids concentration of 11.0% by weight.

[0153] [Comparative Example 5] (1) Preparation of first base coating composition (1-1) Preparation of color pigment dispersion 8 72.6 parts of the water-soluble acrylic resin solution obtained in Production Example 3, 11.5 parts of perylene red (color pigment), 10.4 parts of carbon black (color pigment), 32.3 parts of pigment dispersant, 70.2 parts of ion-exchanged water, and 1.0 part of antifoaming agent were mixed using a stirrer such as a disperser. Next, the mixture was dispersed using a disperser filled with 0.05 mm zirconia beads as a medium at a volume filling rate of 70%, to obtain color pigment dispersion 8.

[0154] (1-2) Preparation of the first base coating composition 122.1 parts of the acrylic resin emulsion of Production Example 1, 2.0 parts of dimethylaminoethanol, Cymel 370N (curing agent, solids content 87%) 35.6 parts, colored pigment dispersion 8 95.8 parts, paste containing a non-optical interference bright pigment (active ingredient 60%) 2.1 parts per 100 parts by weight of resin solids, 5 parts of the phosphate group-containing organic compound of Production Example 2, lauryl acid phosphate 0.4 parts, butyl cellosolve 50 parts, Noigen EA-207D (surfactant, solids content 55%) 5.5 parts, 3 parts of linoleic acid were uniformly dispersed. After adjusting the pH to 8.1 by adding dimethylaminoethanol, it was diluted with deionized water to prepare a first base coating composition with a resin solids concentration of 19.9% ​​by weight.

[0155] (2) Preparation of second base coating composition (2-1) Preparation of color pigment dispersion 9 94.2 parts of the water-soluble acrylic resin solution obtained in Production Example 3, 10.1 parts of perylene red (color pigment), 24.4 parts of anchor red (color pigment), 1.9 parts of carbon black (color pigment), 18.0 parts of pigment dispersant, 55.9 parts of ion-exchanged water, and 0.5 parts of defoamer were mixed with a stirrer such as a disperser. Next, the mixture was dispersed in a disperser filled with 0.05 mm zirconia beads as a medium at a volume filling rate of 70%, to obtain color pigment dispersion 9.

[0156] (2-2) Preparation of the second base coating composition 143.3 parts of the acrylic resin emulsion of Production Example 1, 1.4 parts of dimethylaminoethanol, Cymel 370N (curing agent, solids content 87%) 35.6 parts, colored pigment dispersion 9 37.2 parts, other light interference pigment 2 15 parts by weight per 100 parts by weight of resin solids, 5 parts of the phosphate group-containing organic compound of Production Example 2, lauryl acid phosphate 0.4 parts, butyl cellosolve 50 parts, Noigen EA-207D (surfactant, solids content 55%) 5.5 parts, 3 parts of linoleic acid were uniformly dispersed. After adjusting the pH to 8.1 by adding dimethylaminoethanol, it was diluted with deionized water to prepare an aqueous second base coating composition with a resin solids concentration of 11.0% by weight.

[0157] (3) Formation of Multi-Layer Coating Films Multi-layer coating films were formed in the same manner as in Example 3, except that the first and second base coating compositions described above were used.

[0158] [Evaluation] The multilayer coating films obtained in the Examples and Comparative Examples were evaluated as follows. The evaluation results are shown in the table below. (1) Spectral reflectance, lightness and saturation Using a spectrophotometer "BYK-mac i" manufactured by BYK-Gardner, the spectral reflectance, lightness and saturation were measured by measuring the spectral reflectance, lightness and saturation of the coated article at an angle of 45 degrees from the clear coating side. 45 The spectral reflectance, L, is the reflectance when light is received at angles of -15 degrees, 15 degrees, and 45 degrees relative to the specular reflection light. * C * The saturation and brightness in the h color system were obtained. The average value of five different samples was used as the saturation C * -15 , C * 15 , C * 45 , brightness L * -15 , L * 15 It was decided.

[0159] (2) Appearance of Coating Film The multilayer coating films obtained in the Examples and Comparative Examples were observed from an incident angle of 45° and an acceptance angle of about −15°, and then the multilayer coating film was moved so that the acceptance angle increased, and visual observation was performed, and the appearance was evaluated based on the following criteria.

[0160] Evaluation criteria A: At a light receiving angle of around -15°, vividness is perceived, but as the light receiving angle is increased, the saturation is perceived less and the change in saturation is clearly recognized. B: At a light receiving angle of around -15°, vividness is perceived to a certain extent, but as the light receiving angle is increased, a decrease in saturation is perceived to a certain extent. C: No change in saturation is perceived when the light receiving angle is increased from -15°.

[0161]

[0162]

[0163] For all of the coating films of the Examples, the vividness changed significantly in the highlight region, and the color was perceived as almost achromatic in the face region. For the coating films of Comparative Examples 1 and 5, as the light-receiving angle was increased from -15°, some change in saturation was perceived in the highlight region, but the change was small, and the color was not perceived as achromatic in the face region. For the coating films of Comparative Examples 2 to 4, almost no change in saturation was perceived in the highlight region.

[0164] The present disclosure includes the following aspects: [1] A coating composition comprising a film-forming resin and a pigment, wherein incident light I is incident at an angle of 45 degrees to the surface of a cured coating film of the coating composition. 45 The reflected light R received at an angle of −15 degrees with respect to the specular reflection light -15 L based on the spectral reflectance of * C * Chroma C in the h color system * -15 and the incident light I 45 The reflected light R received at an angle of 15 degrees to the specular reflected light 15 L based on the spectral reflectance of * C * Chroma C in the h color system * 15 But, C * -15 >C * 15 >10, and C * -15 -C * 15 >20, and the incident light I 45 The reflected light R received at an angle of 45 degrees to the specular reflected light 45 L based on the spectral reflectance of * C * Chroma C in the h color system * 45 [2] The chroma C * -15 The coating composition according to the above [1], wherein the chroma C is 50 or more. * 15 The coating composition according to the above [1] or [2], wherein the reflected light R -15Lightness L based on the spectral reflectance * -15 and the reflected light R 15 Lightness L based on the spectral reflectance * 15 But, L * -15 -L * 15 [5] The coating composition according to any one of [1] to [3] above, which satisfies the relationship of ≧10. -15 The maximum spectral reflectance SR -15 and the reflected light R -15 Spectral reflectance SR -15 The reflected light R 15 Spectral reflectance SR 15 But, SR -15 -SR 15 [6] The coating composition according to any one of [1] to [4] above, wherein the reflected light R -15 Spectral reflectance SR -15 The wavelength W at which -15 and the reflected light R 15 Spectral reflectance SR 15 The wavelength W at which 15 But, |W -15 -W 15[7] The coating composition of any of [1] to [5] above, wherein the coating composition satisfies the relationship |≧40 (nm). [7] The coating composition of any of [1] to [6] above, wherein the pigment comprises an optically coherent scaly pigment comprising: a scaly reflective substrate having a first surface and a second surface opposite to the first surface, a first layer comprising at least one element selected from the group consisting of silicon dioxide, aluminum oxide, and a metal fluoride, and a second layer comprising at least one element selected from the group consisting of chromium, aluminum, silver, nickel, palladium, platinum, titanium, vanadium, cobalt, iron, tin, tungsten, molybdenum, rhodium, niobium, copper, and gold, and wherein at least two of the first layers and the second layers are alternately arranged on each of the first surface and the second surface, with the first layer being the innermost layer. [8] A coated article comprising a substrate and a cured coating film of the coating composition of any one of [1] to [7] above provided on the substrate. [9] A method for producing a coated article, comprising applying the coating composition of any one of [1] to [7] above onto the substrate, and then curing the composition.

[0165] The coated article of the present invention is particularly suitable as the outer panel of an automobile body.

[0166] This application claims priority based on Japanese Patent Application No. 2023-051982, filed on March 28, 2023, the entire contents of which are incorporated herein by reference.

Claims

1. A coating composition containing a film-forming resin and a pigment, wherein incident light I is incident at an angle of 45 degrees on the surface of a cured coating of the coating composition. 45 The reflected light R received at an angle of -15 degrees to the regular reflected light -15 Based on the spectral reflectance of * C * Saturation C in the h color system * -15 and the incident light I 45 The reflected light R received at an angle of 15 degrees to the regular reflected light 15 Based on the spectral reflectance of * C * Saturation C in the h color system * 15 But, C * -15 >C * 15 >10, and C * -15 -C * 15 >20, and the incident light I 45 The reflected light R received at an angle of 45 degrees to the regular reflected light 45 Based on the spectral reflectance of * C * Saturation C in the h color system * 45 is 10 or less.

2. Saturation C * -15 The coating composition according to claim 1, wherein the Mn is 50 or more.

3. Saturation C * 15 The coating composition according to claim 1 or 2, wherein the viscosity is more than 10 and not more than 40.

4. The reflected light R -15 Lightness L based on the spectral reflectance * -15 and the reflected light R 15 Lightness L based on the spectral reflectance * 15 But, L * -15 -L * 15 The coating composition according to any one of claims 1 to 3, which satisfies the relationship: ≧10.

5. In the wavelength range of 400 nm to 700 nm, the reflected light R -15 The maximum spectral reflectance SR -15 and the reflected light R -15 Spectral reflectance SR -15 The reflected light R 15 Spectral reflectance SR 15 But, SR -15 -SR 15 The coating composition according to any one of claims 1 to 4, which satisfies the relationship: ≧20(%).

6. In the wavelength range of 400 nm to 700 nm, the reflected light R -15 Spectral reflectance SR -15 The wavelength W at which -15 and the reflected light R 15 Spectral reflectance SR 15 The wavelength W at which 15 And, |W -15 -W 15 The coating composition according to any one of claims 1 to 5, which satisfies the relationship: |≧40 (nm).

7. A coating composition according to any one of claims 1 to 6, wherein the pigment comprises an optically coherent scaly pigment comprising: a scaly reflective substrate having a first surface and a second surface opposite to the first surface; a first layer comprising at least one element selected from the group consisting of silicon dioxide, aluminum oxide and metal fluorides; and a second layer comprising at least one element selected from the group consisting of chromium, aluminum, silver, nickel, palladium, platinum, titanium, vanadium, cobalt, iron, tin, tungsten, molybdenum, rhodium, niobium, copper and gold, and wherein at least two of the first layers and the second layers are alternately arranged on each of the first surface and the second surface, with the first layer as the innermost layer.

8. A coated article comprising: a substrate; and a cured coating film of the coating composition according to any one of claims 1 to 7 provided on the substrate.

9. A method for producing a coated article, comprising applying the coating composition according to any one of claims 1 to 7 onto an object to be coated, and then curing the composition.

Citation Information

Patent Citations

  • Paint composition, method for forming coating film using the same and coating film

    JP2010209167A

  • Coating composition, method for forming coating film using the same, and coating film

    JP2012046676A

  • A small interface for managing alerts

    JP2023051982A

  • Coating film forming method and base material having coating film by coating film forming method

    JP2002224618A

  • Method of forming multilayer coating film

    JP2011131186A