Curable resin composition

The curable resin composition combines aliphatic bismaleimide and monomaleimide compounds with a polymerization initiator to achieve both low dielectric constants and high heat resistance, addressing the limitations of conventional compositions and meeting the demands of advanced communication systems.

WO2024202375A1PCT designated stage expired Publication Date: 2024-10-03SEKISUI CHEMICAL CO LTD

Patent Information

Application Number
PCT/JP2024/000016
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-01-04
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional curable resin compositions with bismaleimide compounds excel in low dielectric loss tangents but struggle to achieve both low dielectric constants and heat resistance, as reducing crosslinking points to lower dielectric constants compromises glass transition temperature and heat resistance.

Method used

A curable resin composition combining an aliphatic bismaleimide compound, an aliphatic monomaleimide compound, and a polymerization initiator, with specific molecular weight and carbon atom ranges, optionally including inorganic fillers and a polymer component, to achieve excellent dielectric properties and heat resistance after curing.

Benefits of technology

The composition effectively balances dielectric properties and heat resistance, with a dielectric constant of 2.60 or less and a glass transition temperature of 140°C or higher, suitable for high-frequency applications like 5G communication systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide a curable resin composition which, after being cured, exhibits excellent dielectric properties and heat resistance. The present invention is a curable resin composition containing an aliphatic bismaleimide compound, an aliphatic monomaleimide compound, and a polymerization initiator.
Need to check novelty before this filing date? Find Prior Art

Description

Curable resin composition

[0001] The present invention relates to a curable resin composition.

[0002] In recent years, the field of electronic devices has seen a demand for faster transmission and reception of larger volumes of data. The practical application of so-called fifth-generation mobile communication systems (5G) has also progressed, and this has led to an increase in the frequency of transmission signals. However, this increase in frequency has led to a problem of increased attenuation (transmission loss) of transmission signals. Therefore, curable resin compositions used as interlayer insulating materials for printed wiring boards, sealants for display elements, and the like, require dielectric properties such as low dielectric constant and low dielectric loss tangent. For example, Patent Documents 1 to 3 disclose resin compositions containing bismaleimide compounds each having a specific structure, as curable resin compositions with such excellent dielectric properties.

[0003] JP 2022-046517 A International Publication No. 2022 / 004211 JP 2017-071738 A

[0004] Conventional curable resin compositions containing bismaleimide compounds have excellent low dielectric loss tangents, but there has been a demand for a further reduction in the dielectric constant. While reducing the number of crosslinking points to suppress polarization is one way to lower the dielectric constant, reducing the number of crosslinking points poses problems such as a decrease in the glass transition temperature, resulting in a cured product with poor heat resistance. The present invention aims to provide a curable resin composition that has excellent dielectric properties and heat resistance after curing.

[0005] Disclosure 1 is a curable resin composition containing an aliphatic bismaleimide compound, an aliphatic monomaleimide compound, and a polymerization initiator. Disclosure 2 is the curable resin composition of Disclosure 1, wherein the content of the aliphatic bismaleimide compound is 10 parts by mass or more and 90 parts by mass or less per 100 parts by mass of the total of the aliphatic bismaleimide compound and the aliphatic monomaleimide compound. Disclosure 3 is the curable resin composition of Disclosure 1 or 2, wherein the aliphatic bismaleimide compound has a molecular weight of 880 or more and 5550 or less. Disclosure 4 is the curable resin composition of Disclosure 1, 2, or 3, wherein the aliphatic bismaleimide compound has a carbon number of 40 or more and 360 or less. Disclosure 5 is the curable resin composition of Disclosure 1, 2, 3, or 4, further containing an inorganic filler. Disclosure 6 is the curable resin composition of Disclosure 1, 2, 3, 4, or 5, further containing a polymer component. Disclosure 7 is the curable resin composition of Disclosure 6, wherein the polymer component is polyimide. The present invention is described in detail below.

[0006] The present inventors have found that by using a combination of an aliphatic bismaleimide compound, an aliphatic monomaleimide compound, and a polymerization initiator in a curable resin composition, it is possible to obtain a curable resin composition that is excellent in dielectric properties and heat resistance after curing, and have thereby completed the present invention.

[0007] The curable resin composition of the present invention contains an aliphatic bismaleimide compound. By using the aliphatic bismaleimide compound in combination with the aliphatic monomaleimide compound described below, the curable resin composition of the present invention will have excellent dielectric properties and heat resistance after curing. In this specification, the term "aliphatic" in the aliphatic bismaleimide compound and the aliphatic monomaleimide compound described below means that the structure directly bonded to the maleimide group is an aliphatic hydrocarbon.

[0008] The aliphatic bismaleimide compound has a molecular weight of preferably 880 (lower limit) and 5550 (upper limit). When the molecular weight of the aliphatic bismaleimide compound is within this range, the resulting curable resin composition exhibits superior effects of achieving both dielectric properties and heat resistance after curing. The aliphatic bismaleimide compound has a more preferred lower limit and 4000 (upper limit). In this specification, the "molecular weight" refers to the molecular weight calculated from the structural formula for compounds with specific molecular structures. However, for compounds with a wide distribution of polymerization degrees and compounds with unspecified modification sites, the "number average molecular weight" may be used. In this specification, the "number average molecular weight" refers to a value calculated in terms of polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran as a solvent. Examples of columns used when measuring the number average molecular weight calculated in terms of polystyrene by GPC include JAIGEL-2H-A (manufactured by Japan Analytical Industry Co., Ltd.).

[0009] The aliphatic bismaleimide compound preferably has a lower carbon number limit of 40 and a higher carbon number limit of 360. When the carbon number of the aliphatic bismaleimide compound is within this range, the resulting curable resin composition exhibits superior effects of achieving both dielectric properties and heat resistance after curing. A more preferred lower carbon number limit of the aliphatic bismaleimide compound is 44 and a more preferred upper carbon number limit is 350. The carbon number of the aliphatic bismaleimide compound also includes the number of carbon atoms contained in the maleimide group. Furthermore, in this specification, the "carbon number" refers to the carbon number determined from the structural formula for compounds with a specific molecular structure. However, for compounds with a wide distribution of polymerization degrees and compounds with unspecified modification sites, the "carbon number" refers to the carbon number of the compound corresponding to the position of the highest peak observed when determining the molecular weight using GPC by the above-described method. When multiple peaks with the highest peak heights are present, the carbon number is considered to correspond to the positions of all of those peaks. For example, when there are multiple peaks with the highest peak height, if any one of the peaks has a carbon number equal to or greater than the preferable lower limit, the number of carbon atoms in the aliphatic bismaleimide compound is deemed to be equal to or greater than the preferable lower limit, and the same applies to the preferable upper limit, the more preferable lower limit, and the more preferable upper limit.

[0010] Examples of the aliphatic bismaleimide compound include a compound represented by the following formula (1), a compound represented by the following formula (2), and a compound represented by the following formula (3). Among these, the compound represented by the following formula (1) and the compound represented by the following formula (2) are preferred. The compound represented by the following formula (1), the compound represented by the following formula (2), and the compound represented by the following formula (3) may all have a hydrogen atom substituted.

[0011]

[0012]

[0013] In formula (2), n is 1 or more and 10 or less.

[0014]

[0015] In formula (3), m is 1 or more and 10 or less.

[0016] The preferred lower limit of the content of the aliphatic bismaleimide compound is 10 parts by mass, and the preferred upper limit is 90 parts by mass, per 100 parts by mass of the total of the aliphatic bismaleimide compound and the aliphatic monomaleimide compound described below. When the content of the aliphatic bismaleimide compound is within this range, the resulting curable resin composition exhibits an excellent effect of achieving both dielectric properties and heat resistance after curing. The more preferred lower limit of the content of the aliphatic bismaleimide compound is 20 parts by mass, and the more preferred upper limit is 80 parts by mass. The even more preferred upper limit of the content of the aliphatic bismaleimide compound is 60 parts by weight.

[0017] The curable resin composition of the present invention contains an aliphatic monomaleimide compound. As described above, by using the aliphatic monomaleimide compound in combination with the aliphatic bismaleimide compound, the curable resin composition of the present invention exhibits excellent dielectric properties and heat resistance after curing.

[0018] The aliphatic monomaleimide compound has a molecular weight of preferably 139 or less and 270 or less. When the molecular weight of the aliphatic monomaleimide compound is within this range, the resulting curable resin composition exhibits an excellent effect of achieving both excellent dielectric properties and excellent heat resistance after curing.

[0019] The aliphatic monomaleimide compound preferably has a lower limit of 7 carbon atoms and an upper limit of 16 carbon atoms. When the number of carbon atoms in the aliphatic monomaleimide compound is within this range, the resulting curable resin composition exhibits an excellent effect of achieving both dielectric properties and heat resistance after curing. The number of carbon atoms in the aliphatic monomaleimide compound includes the number of carbon atoms contained in the maleimide group.

[0020] Examples of the aliphatic monomaleimide compound include N-methylmaleimide, N-ethylmaleimide, N-propylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, N-hexylmaleimide, etc. Among these, N-alkylmaleimides having 7 to 16 carbon atoms are preferred.

[0021] The curable resin composition of the present invention may further contain a curable resin other than the aliphatic bismaleimide compound and the aliphatic monomaleimide compound, or may not contain such other curable resin.

[0022] Examples of the other curable resins include aromatic bismaleimide compounds, aromatic monomaleimide compounds, epoxy compounds, cyanate compounds, phenol compounds, imide compounds, silicone compounds, acrylic compounds, and fluorine compounds.

[0023] When the curable resin composition of the present invention contains the aromatic bismaleimide compound as the other curable resin, the upper limit of the amount of the aromatic bismaleimide compound per 100 parts by mass of all bismaleimide compounds is preferably 20 parts by mass, more preferably 10 parts by mass. From the viewpoint of achieving better dielectric properties after curing, it is preferable that the curable resin composition of the present invention does not contain the aromatic bismaleimide compound.

[0024] When the curable resin composition of the present invention contains the aromatic monomaleimide compound as the other curable resin, the upper limit of the content of the aromatic monomaleimide compound per 100 parts by mass of all the monomaleimide compounds is preferably 80 parts by mass, more preferably 50 parts by mass. From the viewpoint of achieving better dielectric properties after curing, it is preferable that the curable resin composition of the present invention does not contain the aromatic monomaleimide compound.

[0025] When the curable resin composition of the present invention contains the other curable resin, the preferred lower limit of the total content of the aliphatic bismaleimide compound and the aliphatic monomaleimide compound per 100 parts by mass of the entire curable resin containing the aliphatic bismaleimide compound and the aliphatic monomaleimide compound is 10 parts by mass, and the preferred upper limit is 90 parts by mass. When the total content of the aliphatic bismaleimide compound and the aliphatic monomaleimide compound is within the above range, the obtained curable resin composition exhibits an excellent effect of achieving both dielectric properties and heat resistance after curing. The more preferred lower limit of the total content of the aliphatic bismaleimide compound and the aliphatic monomaleimide compound is 20 parts by mass, and the more preferred upper limit is 80 parts by mass. The even more preferred lower limit of the total content of the aliphatic bismaleimide compound and the aliphatic monomaleimide compound is 60 parts by mass.

[0026] The curable resin composition of the present invention contains a polymerization initiator. Examples of the polymerization initiator include a thermal radical polymerization initiator and a photoradical polymerization initiator. Among these, a thermal radical polymerization initiator is preferred from the viewpoint of heat resistance.

[0027] Examples of the thermal radical polymerization initiator include organic peroxides, azo compounds, etc. Examples of the organic peroxides include 1,1-bis(t-hexylperoxy)-3,3,5-trimethylcyclohexane, t-hexylperoxypivalate, t-butylperoxypivalate, 2,5-dimethyl-2,5-bis(2-ethylhexanoylperoxy)hexane, t-hexylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, t-butylperoxyisobutyrate, t-butylperoxy-3,5,5-trimethylhexanoate, and t-butylperoxylaurate. Examples of the azo compound include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), etc. The thermal radical polymerization initiators may be used alone or in combination of two or more.

[0028] Examples of the photoradical polymerization initiator include benzophenone compounds, acetophenone compounds, acylphosphine oxide compounds, titanocene compounds, oxime ester compounds, benzoin ether compounds, thioxanthone compounds, etc. Specific examples of the photoradical polymerization initiator include 1-hydroxycyclohexyl phenyl ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-(dimethylamino)-2-((4-methylphenyl)methyl)-1-(4-(4-morpholinyl)phenyl)-1-butanone, 2,2-dimethoxy-1,2-diphenylethan-1-one, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2-methyl-1-(4-methylthiophenyl) 2-morpholinopropan-1-one, 1-(4-(2-hydroxyethoxy)-phenyl)-2-hydroxy-2-methyl-1-propan-1-one, 1-(4-(phenylthio)phenyl)-1,2-octanedione 2-(O-benzoyloxime), 2-(acetoxyimino)-1-(4-(4-(2-hydroxyethoxy)phenylthio)phenyl)propan-1-one, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2,4-dimethylthioxanthen-9-one, and the like. The above photoradical polymerization initiators may be used alone or in combination of two or more.

[0029] The content of the polymerization initiator is preferably 0.5 parts by mass at the lower limit and 5 parts by mass at the upper limit, relative to 100 parts by mass of the total of the aliphatic bismaleimide compound and the aliphatic monomaleimide compound. By having the content of the polymerization initiator within this range, the resulting curable resin composition has better storage stability and curability. The lower limit of the content of the polymerization initiator is more preferably 1 part by mass, and the upper limit is more preferably 2 parts by mass.

[0030] The curable resin composition of the present invention may further contain an inorganic filler. By containing the inorganic filler, the resulting curable resin composition will have better dielectric properties after curing.

[0031] Examples of the inorganic filler include silica, alumina, boron nitride, magnesium oxide, and boehmite. Among these, silica is preferred. The inorganic fillers may be used alone or in combination of two or more.

[0032] The preferred lower limit of the average particle size of the inorganic filler is 0.2 μm, and the preferred upper limit is 5 μm. When the average particle size of the inorganic filler is within this range, the inorganic filler exhibits excellent dispersibility in the curable resin composition without impairing coating properties, etc. As a result, the resulting curable resin composition exhibits excellent dielectric properties after curing. The more preferred lower limit of the average particle size of the inorganic filler is 0.5 μm, and the more preferred upper limit is 2 μm. The average particle size of the inorganic filler can be measured by dispersing the inorganic filler in a solvent (water, organic solvent, etc.) using a particle size distribution analyzer. Examples of the particle size distribution analyzer include NICOMP 380ZLS (manufactured by PARTICLE SIZING SYSTEMS).

[0033] The content of the inorganic filler is preferably 150 parts by mass or less and 225 parts by mass or less, relative to 100 parts by mass of the total of the aliphatic bismaleimide compound and the aliphatic monomaleimide compound. When the content of the inorganic filler is 150 parts by mass or more, the resulting curable resin composition has better dielectric properties after curing. When the content of the inorganic filler is 225 parts by mass or less, the resulting curable resin composition has better coatability. The lower limit of the content of the inorganic filler is more preferably 187 parts by mass, and the upper limit is more preferably 210 parts by mass.

[0034] The curable resin composition of the present invention may contain an organic filler for the purposes of stress relaxation, toughness impartation, etc. Examples of the organic filler include silicone rubber particles, acrylic rubber particles, urethane rubber particles, polyamide particles, polyamideimide particles, polyimide particles, benzoguanamine particles, and core-shell particles thereof. Among these, polyamide particles, polyamideimide particles, and polyimide particles are preferred. The organic fillers may be used alone or in combination of two or more.

[0035] The curable resin composition of the present invention may further contain a polymer component, which serves as a film-forming component.

[0036] The number average molecular weight of the polymer component preferably has a lower limit of 3,000 and an upper limit of 100,000. When the number average molecular weight of the polymer component is within this range, the resulting curable resin composition has better flexibility and processability before curing and better heat resistance after curing. The number average molecular weight of the polymer component is more preferably 5,000 and an upper limit of 80,000.

[0037] Examples of the polymer component include polyimide, phenoxy resin, polyamide, polyamideimide, polymaleimide, cyanate resin, benzoxazine resin, acrylic resin, urethane resin, polyester, etc. Among these, from the viewpoint of heat resistance, polyimide, polyamide, polyamideimide, and polymaleimide are preferred, and polyimide is more preferred. The polymer component may be used alone or in combination of two or more types.

[0038] The content of the polymer component is preferably 5 parts by mass or less and 20 parts by mass or less relative to 100 parts by mass of the total of the aliphatic bismaleimide compound and the aliphatic monomaleimide compound. When the content of the polymer component is within this range, the cured product of the obtained curable resin composition has better heat resistance. The lower limit of the content of the polymer component is more preferably 9 parts by mass or less and the upper limit is more preferably 15 parts by mass or less.

[0039] From the viewpoint of the flatness of the coating film, the curable resin composition of the present invention preferably further contains a leveling agent.

[0040] Examples of the leveling agent include silicone-based leveling agents, fluorine-based leveling agents, and acrylic-based leveling agents.

[0041] The content of the leveling agent is preferably 0.01 parts by mass at its lower limit and 0.5 parts by mass at its upper limit, relative to 100 parts by mass of the total of the aliphatic bismaleimide compound and the aliphatic monomaleimide compound. By using a leveling agent in this range, the resulting curable resin composition exhibits superior coatability and coating film flatness. The more preferred lower limit of the content of the leveling agent is 0.1 parts by mass.

[0042] The curable resin composition may contain a solvent from the viewpoint of coatability and the like. From the viewpoint of coatability, storage stability, and the like, the solvent preferably has a boiling point of less than 200°C. Examples of the solvent having a boiling point of less than 200°C include alcohol-based solvents, ketone-based solvents, ester-based solvents, hydrocarbon-based solvents, halogen-based solvents, ether-based solvents, and nitrogen-containing solvents. Examples of the alcohol-based solvents include methanol, ethanol, isopropyl alcohol, normal propyl alcohol, isobutyl alcohol, normal butyl alcohol, tertiary butyl alcohol, and 2-ethylhexanol. Examples of the ketone-based solvents include acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl propyl ketone, diisobutyl ketone, cyclohexanone, methylcyclohexanone, and diacetone alcohol. Examples of the ester-based solvents include methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, methoxybutyl acetate, amyl acetate, normal propyl acetate, isopropyl acetate, methyl lactate, ethyl lactate, and butyl lactate. Examples of the hydrocarbon solvents include benzene, toluene, xylene, normal hexane, isohexane, cyclohexane, methylcyclohexane, ethylcyclohexane, isooctane, normal decane, normal heptane, etc. Examples of the halogen-based solvents include dichloromethane, chloroform, trichloroethylene, etc. Examples of the ether-based solvents include diethyl ether, tetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, diisopropyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol monotertiary butyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether propionate, 3-methoxybutanol, 3-methoxy-3-methyl-1-butanol, diethylene glycol dimethyl ether, anisole, 4-methylanisole, etc.Examples of the nitrogen-containing solvent include acetonitrile, N,N-dimethylformamide, and N,N-dimethylacetamide. Among these, from the viewpoints of ease of handling and curing agent solubility, at least one solvent selected from the group consisting of ketone solvents having a boiling point of 60°C or higher but lower than 200°C, ester solvents having a boiling point of 60°C or higher but lower than 200°C, and ether solvents having a boiling point of 60°C or higher but lower than 200°C is preferred. Examples of such solvents include methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate, isobutyl acetate, 1,4-dioxane, 1,3-dioxolane, tetrahydrofuran, cyclohexanone, methylcyclohexanone, diethylene glycol dimethyl ether, and anisole. The solvents may be used alone or in combination of two or more. The "boiling point" refers to a value measured under conditions of 101 kPa or a value converted to 101 kPa using a boiling point conversion chart or the like.

[0043] The preferred lower limit of the content of the solvent in 100 parts by mass of the curable resin composition containing the solvent is 20 parts by mass, and the preferred upper limit is 90 parts by mass. When the content of the solvent is within this range, the resulting curable resin composition has better coatability, etc. The more preferred lower limit of the content of the solvent is 30 parts by mass, and the more preferred upper limit is 80 parts by mass.

[0044] The curable resin composition of the present invention may further contain additives such as a heat curing agent, a curing accelerator, a dispersant, a flame retardant, a coupling agent, a storage stabilizer, a bleeding inhibitor, and a fluxing agent.

[0045] Examples of a method for producing the curable resin composition of the present invention include a method of using a mixer to mix an aliphatic bismaleimide compound, an aliphatic monomaleimide compound, a polymerization initiator, a leveling agent, etc. Examples of the mixer include a homodisper, a universal mixer, a Banbury mixer, and a kneader.

[0046] The curable resin composition of the present invention can be applied to a substrate film and dried to obtain a curable resin composition film made of the curable resin composition of the present invention, and the curable resin composition film can be cured to obtain a cured product.

[0047] The curable resin composition of the present invention can be cured by heating at 190°C for 1 hour or by irradiating ultraviolet light having a wavelength of 365 nm at 3000 mJ / cm using an LED UV lamp. 2 When the composition is cured by irradiation, irradiation with light, or both, the reaction rate derived from the calorific value measured by differential scanning calorimetry of the curable resin composition before curing and the cured product of the curable resin composition is preferably 85% or more. A reaction rate of 85% or more makes the curable resin composition of the present invention more suitable for use as an adhesive, sealant, interlayer insulating material, etc. A preferred lower limit of the reaction rate is 87%. A higher reaction rate is preferable, with 100% being most preferred. The differential scanning calorimetry is performed using a differential scanning calorimeter in a temperature range of 25°C to 300°C at a heating rate of 10°C / min. An example of the differential scanning calorimeter is a DSC200 (manufactured by Hitachi High-Tech Science Corporation).

[0048] The curable resin composition of the present invention preferably has an upper limit of the dielectric constant at 23°C after curing of 2.60. Since the dielectric constant at 23°C after curing is 2.60 or less, the curable resin composition of the present invention can be suitably used as an interlayer insulating material for multilayer printed wiring boards, etc. A more preferred upper limit of the dielectric constant at 23°C after curing is 2.50. There is no particular preferred lower limit for the dielectric constant after curing, but the substantial lower limit is 2.40. The dielectric constant and the dielectric loss tangent described below are values ​​measured under 1.0 GHz conditions using a dielectric constant measuring device and a network analyzer. The cured product for measuring the dielectric constant and the dielectric loss tangent described below can be obtained by curing a film of the curable resin composition having a thickness of 40 to 200 μm. For curing, a method of heating at 190°C for 1 hour is used in the case of a thermosetting curable resin composition, and a method of curing a photocurable curable resin composition by irradiating the composition with ultraviolet light having a wavelength of 365 nm at 3000 mJ / cm. 2 In the case of a photo-thermosetting curable resin composition, a combination of these two methods is used.

[0049] The curable resin composition of the present invention preferably has a dielectric loss tangent at 23°C after curing of less than 0.0030. Since the dielectric loss tangent at 23°C after curing is less than 0.0030, the curable resin composition of the present invention can be suitably used as an interlayer insulating material for multilayer printed wiring boards, etc. It is more preferable that the dielectric loss tangent at 23°C after curing is 0.0025 or less. There is no particular preferred lower limit for the dielectric loss tangent after curing, but the substantial lower limit is 0.0023.

[0050] The curable resin composition of the present invention has a preferred lower limit of the glass transition temperature after curing of 140°C. Since the cured glass transition temperature is 140°C or higher, the curable resin composition of the present invention can be suitably used in applications requiring heat resistance. A more preferred lower limit of the glass transition temperature after curing is 150°C. There is no particular preferred upper limit for the glass transition temperature after curing, but the practical upper limit is 200°C. In this specification, the "glass transition temperature" refers to the temperature at which a maximum due to micro-Brownian motion appears among the maximums of the loss tangent (tan δ) obtained by dynamic viscoelasticity measurement. The glass transition temperature can be measured by a conventionally known method using a dynamic viscoelasticity measuring device or the like. The cured product for measuring the glass transition temperature and the 5% weight loss temperature described below can be obtained by coating the curable resin composition on a substrate PET film to a thickness of 100 μm after drying, drying, and then curing. As a curing method, in the case of a thermosetting curable resin composition, a method of heating at 190°C for 1 hour is used, and in the case of a photocurable curable resin composition, a method of irradiating ultraviolet light with a wavelength of 365 nm at 3000 mJ / cm 2 In the case of a photo-thermosetting curable resin composition, a combination of these two methods is used.

[0051] The curable resin composition of the present invention preferably has a 5% weight loss temperature after curing that exceeds 390°C. By having a 5% weight loss temperature after curing that exceeds 390°C, the curable resin composition of the present invention can be suitably used in applications that particularly require heat resistance. The 5% weight loss temperature after curing of the curable resin composition of the present invention is more preferably greater than 400°C. Furthermore, there is no particular preferred upper limit to the 5% weight loss temperature after curing of the curable resin composition of the present invention, but the substantial upper limit is 405°C.

[0052] The curable resin composition of the present invention can be used in a wide range of applications. For example, it can be used as an adhesive for printed wiring boards, an adhesive for coverlays of flexible printed circuit boards, copper-clad laminates, adhesives for semiconductor bonding, interlayer insulating materials, prepregs, sealants for LEDs, adhesives for structural materials, sealants for display elements, etc. In particular, the curable resin composition of the present invention can be suitably used as an interlayer insulating material or a sealant for organic EL display elements, which require these properties, because the cured product has a low dielectric constant, a low dielectric dissipation factor, excellent dielectric properties, and excellent heat resistance.

[0053] According to the present invention, it is possible to provide a curable resin composition that has excellent dielectric properties and heat resistance after curing.

[0054] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0055] (Preparation of Polyimide Resin Solution) 54.6 parts by mass of 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride (manufactured by Tokyo Chemical Industry Co., Ltd.) and 200 parts by mass of cyclohexanone were charged into a reaction vessel equipped with a stirrer, a water divider, and a nitrogen gas inlet tube and dissolved. To the resulting solution, a mixed solution of 56.1 parts by mass of Priamine 1074 (manufactured by Croda) which is a dimer diamine and 55.0 parts by mass of cyclohexanone was added dropwise, and then an imidization reaction was carried out at 150 ° C. for 8 hours to obtain a polyimide resin solution. The solids concentration of the obtained polyimide resin solution was 30% by mass, and the number average molecular weight of the polyimide resin was 25,000.

[0056] (Examples 1 to 11, Comparative Examples 1 to 5) Each material was stirred and mixed using a disper according to the compounding ratios shown in Tables 1 and 2 to prepare each of the curable resin compositions of Examples 1 to 11 and Comparative Examples 1 to 5.

[0057] <Evaluation> The curable resin compositions obtained in the examples and comparative examples were evaluated as follows. The results are shown in Tables 1 and 2.

[0058] (Dielectric Properties) Each of the obtained curable resin compositions was coated on a substrate PET film and dried to obtain an uncured laminate film having a substrate PET film and a 40 μm thick curable resin composition layer on the substrate PET film. The obtained uncured laminate film was cut into a size of 2 mm wide and 80 mm long. The substrate PET film was peeled from the curable resin composition layer of the cut uncured laminate film, and five curable resin composition layers were stacked using a laminator to obtain a laminate with a thickness of approximately 200 μm. The obtained laminate was cured to obtain a cured product. The laminates using the curable resin compositions obtained in Examples 1 to 10 and Comparative Examples 1 to 5 were heated at 190°C for 1 hour to be cured. The laminate using the curable resin composition obtained in Example 11 was cured by irradiating 3000 mJ / cm of ultraviolet light with a wavelength of 365 nm using an LED UV lamp. 2 The cured product was cured by irradiating the cured product with light. The dielectric constant and dielectric loss tangent of the resulting cured product were measured by the cavity resonance method at 23°C and a frequency of 1.0 GHz using a cavity resonance perturbation dielectric constant measuring device CP521 (manufactured by Kanto Electronics Application Development Co., Ltd.) and a network analyzer N5224A PNA (manufactured by Keysight Technologies). The dielectric properties (dielectric constant) were evaluated according to the following criteria: ◎: When the dielectric constant was 2.50 or less ○: When the dielectric constant was more than 2.50 and less than 2.60 △: When the dielectric constant was more than 2.60 and less than 3.00 ×: When the dielectric constant was 3.00 or more The dielectric properties (dielectric loss tangent) were also evaluated according to the following criteria. ◎: When the dielectric dissipation factor was 0.0025 or less. ○: When the dielectric dissipation factor was more than 0.0025 and less than 0.0030. △: When the dielectric dissipation factor was 0.0030 or more and less than 0.0040. ×: When the dielectric dissipation factor was 0.0040 or more.

[0059] (Heat resistance) Each of the obtained curable resin compositions was coated on a substrate PET film so that the thickness after drying was 100 μm, dried, and then cured. The curable resin compositions obtained in Examples 1 to 10 and Comparative Examples 1 to 5 were cured by heating at 190° C. for 1 hour. The curable resin composition obtained in Example 11 was cured by irradiating ultraviolet light of 365 nm wavelength at 3000 mJ / cm using an LED UV lamp. 2The cured product was cured by irradiating the cured product with light. Dynamic viscoelasticity measurements were performed on the resulting cured product using a dynamic viscoelasticity measuring device (IT Measurement & Control Co., Ltd., "DVA-200") under conditions of a grip width of 24 mm, a heating rate of 10°C / min, and a frequency of 10 Hz, over a range of 25°C to 250°C. The temperature at which the loss tangent (tan δ) reached its maximum was determined as the glass transition temperature. Heat resistance (glass transition temperature) was evaluated according to the following criteria: ⊚: Glass transition temperature was 190°C or higher; ∘: Glass transition temperature was 140°C or higher but less than 190°C; Δ: Glass transition temperature was 100°C or higher but less than 140°C; ×: Glass transition temperature was less than 100°C. Furthermore, thermogravimetric measurements were performed on the resulting cured product using a thermogravimetric measuring device (Hitachi High-Tech Science Corporation, "TG / DTA6200") at a heating rate of 10°C / min from 30°C to 500°C, and the 5% weight loss temperature was determined. Heat resistance (5% weight loss temperature) was evaluated according to the following criteria: ◎: 5% weight loss temperature exceeded 400°C ○: 5% weight loss temperature exceeded 390°C and was 400°C or less △: 5% weight loss temperature exceeded 380°C and was 390°C or less ×: 5% weight loss temperature was 380°C or less

[0060] (Reactivity) Each of the obtained curable resin compositions was coated on a substrate PET film and dried to obtain an uncured laminate film having a substrate PET film and a 40 μm thick curable resin composition layer on the substrate PET film. The obtained uncured laminate film was cut into a size of 2 mm wide and 80 mm long. Next, the curable resin composition layer of the obtained laminate was cured to obtain a cured product. The laminates using the curable resin compositions obtained in Examples 1 to 10 and Comparative Examples 1 to 5 were heated at 190°C for 1 hour to be cured. The laminate using the curable resin composition obtained in Example 11 was cured by irradiating the curable resin composition with 365 nm ultraviolet light at 3000 mJ / cm using an LED UV lamp. 2The curable resin composition before curing and the resulting cured product were subjected to differential scanning calorimetry using a differential scanning calorimeter (manufactured by Hitachi High-Tech Science Corporation, "DSC200") in a temperature range of 25°C to 300°C at a heating rate of 10°C / min to measure the calorific value, and the reaction rate was calculated.

[0061]

[0062]

[0063] According to the present invention, it is possible to provide a curable resin composition that has excellent dielectric properties and heat resistance after curing.

Claims

1. A curable resin composition comprising an aliphatic bismaleimide compound, an aliphatic monomaleimide compound, and a polymerization initiator.

2. The curable resin composition according to claim 1, wherein the content of the aliphatic bismaleimide compound is 10 parts by mass or more and 90 parts by mass or less per 100 parts by mass of the total of the aliphatic bismaleimide compound and the aliphatic monomaleimide compound.

3. The curable resin composition according to claim 1 or 2, wherein the aliphatic bismaleimide compound has a molecular weight of 880 or more and 5,550 or less.

4. The curable resin composition according to claim 1, 2 or 3, wherein the aliphatic bismaleimide compound has 40 or more and 360 or less carbon atoms.

5. The curable resin composition according to claim 1, 2, 3 or 4, further comprising an inorganic filler.

6. The curable resin composition according to claim 1, 2, 3, 4 or 5, further comprising a polymer component.

7. The curable resin composition according to claim 6, wherein the polymer component is a polyimide.

Citation Information

Patent Citations

  • Curable resin composition

    JP1983136637A

  • Anisotropic conductive adhesive and printed wiring board using the same

    JP2015193725A

  • Thermosetting resin composition

    JP2020045446A

  • Photocurable ink jet ink

    WO2012172816A1

  • Thermosetting resin composition, prepreg and cured product thereof

    WO2017170844A1

Cited By

  • Bismaleimide compounds, curable compositions, and cured products

    JP2026145044A