Depth filter

The depth filter configuration with a layered structure of nonwoven fabrics addresses the challenge of absolute filtration and gel removal for submicron particles, ensuring high collection efficiency and stability under high pressure, and maintaining excellent liquid permeability, suitable for semiconductor manufacturing.

WO2024202381A1PCT designated stage expired Publication Date: 2024-10-03JNC CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/000288
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-01-10
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current depth filters face challenges in achieving absolute filtration and gel removal for submicron-sized particles while maintaining excellent liquid permeability and stability under high pressure, leading to issues with filtration accuracy and productivity in electronic device manufacturing.

Method used

A depth filter configuration with an outer layer, pre-filtration layer, and microfiltration layer, where the outer layer is made of nonwoven fabric with a high melting point and low melting point resin, and the pre-filtration and microfiltration layers have specific fiber diameters and basis weights, ensuring continuous fiber diameter reduction and improved bonding for enhanced filtration performance.

Benefits of technology

The depth filter achieves high collection efficiency and stability under high pressure, maintaining excellent liquid permeability and preventing particle push-out, making it suitable for semiconductor manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided is a depth filter which has the absolute property of filtration and the removing performance of gel even for particles to be removed having a reduced particle diameter, and is excellent in liquid permeability. This depth filter comprises an outer layer, a pre-filtration layer, and a precision filtration layer arranged in this order with respect to the filtration direction. The outer layer is formed by winding an outer layer nonwoven fabric containing a high-melting-point resin and a low-melting-point resin multiply, the nonwoven fabrics to be wound are thermally bonded by the low-melting-point resin, and the average fiber diameter is continuously reduced with respect to the filtration direction. The precision filtration layer is a layer in which a nonwoven fabric for the precision filtration layer having an average fiber diameter of less than 300 nm is wound multiply. The pre-filtration layer is a layer in which a nonwoven fabric for the precision filtration layer having an average fiber diameter of 300 nm or more, a nonwoven fabric for a pre-filtration layer having an average fiber diameter of less than 1000 nm is wound multiply, and an average fiber diameter is constant or gradually decreases with respect to the filtration direction.
Need to check novelty before this filing date? Find Prior Art

Description

Depth Filter

[0001] The present invention relates to a depth filter for filtering fluids containing small particles.

[0002] In recent years, various electronic devices have been required to be more compact and perform better. This has led to a trend toward thinner and more multi-layered components. The presence of large particles in a given component's thickness can impair thickness uniformity, hindering the fabrication of high-resolution devices and directly leading to manufacturing problems. Therefore, depth filters are used to remove coarse particles from slurries prior to processing and molding. As components continue to become thinner, the size of what are considered coarse particles is shrinking to submicron sizes, creating an increasing demand for high-precision depth filters with high particle capture capabilities. Furthermore, recent evidence suggests that gels present in slurries may lead to defects during electronic device manufacturing, creating a need for gel capture capabilities.

[0003] Depth filters used in such fields have a thick filter medium, and by varying the fiber diameter or basis weight from upstream to downstream, they ensure filtration accuracy and liquid permeability for particulate-containing liquids with a relatively wide particle size distribution. Patent Document 1 discloses a depth filter that combines a pre-filtration layer configured so that the fiber diameter gradually narrows in the filtration direction with a microfiltration layer having a smaller fiber diameter than the pre-filtration layer. Such depth filters capture coarse particles on the outside and smaller particles and gels on the inside, thereby achieving high-accuracy filtration while relatively suppressing an increase in filtration pressure. However, the fiber diameter of the fibers constituting the microfiltration layer is not sufficiently thin, which presents a problem in that it cannot meet the recent needs for smaller and more stringent particle diameters for removal of particles.

[0004] On the other hand, Patent Document 2 discloses a depth filter including a pre-filtration layer and a microfiltration layer using ultrafine fibers. Attempts have been made to capture fine particles by thickening the nonwoven fabric layer made of such ultrafine fibers, but this tends to result in reduced liquid permeability and a high-pressure state. As a result, when the filtration volume of the filter increases and high filtration pressure is reached, a push-out phenomenon occurs in which captured particles or gels are easily pushed through the gaps between the fibers and leak downstream, resulting in a deterioration in filtration accuracy. In addition, careful filtration operations are required, which complicates filtration process management for operators. Furthermore, while the pressure applied to the filter can be reduced by reducing the liquid flow rate, this also results in a decrease in productivity. Furthermore, when filtering at a constant pressure, filters with higher pressure loss have a lower fluid throughput, so filters with lower pressure loss are preferable from the perspective of productivity.

[0005] On the other hand, high-precision filters using ultrafine fibers tend to have low water permeability. When passing an aqueous dispersion containing fine particles through such a high-precision depth filter, filtration is performed by wetting the filter material while removing the air contained in the filter material using pressure wetting. However, since many ultrafine fibers are hydrophobic, the filter material is difficult to wet, and high pressure or time is required to pass water through, which makes the preparation for filtration time-consuming and cumbersome for workers. Therefore, high-precision filters are desired to have handleability that allows smooth water passage.

[0006] Furthermore, filter media made of nonwoven fabrics made of melt-blown ultrafine fibers employ a depth filtration mechanism that captures fine particles through the thickness of the filter media, rather than surface filtration, which has high filtration accuracy like precision membranes with uniform pore sizes. Furthermore, fine particles that are not captured in the gaps between the filter media collide with the filter media and flow downstream, but the time it takes to leak varies. In recent years, strict control of coarse particles is required in the polishing process of semiconductor manufacturing, and it is preferable to be able to predict filter replacement in advance. In this situation, depth filters are also required to have absolute filtration accuracy, and ease of process control during filtration operations, such as ease of liquid flow and stable capture performance under high pressure, are also required.

[0007] Thus, there is a demand for a depth filter that is capable of high-precision filtration (absolute filtration) even for small particles to be removed, has gel removal performance, and is excellent in liquid permeability.

[0008] International Publication No. 1998 / 013123 Japanese Patent Application Laid-Open No. 2017-185422

[0009] In view of this situation, an object of the present invention is to provide a depth filter that has absolute filtration performance even for particles of reduced diameter that are the target of removal, gel removal performance, and excellent liquid permeability.

[0010] That is, the present invention has the following configurations: [1] A depth filter having an outer layer, a prefiltration layer, and a microfiltration layer arranged in this order in the filtration direction, wherein the outer layer is a layer formed by wrapping an outer layer nonwoven fabric containing a high-melting point resin and a low-melting point resin in multiple layers, the wrapped nonwoven fabrics being thermally bonded together by the low-melting point resin, and configured so that the average fiber diameter continuously decreases in the filtration direction, the microfiltration layer is a layer formed by wrapping a microfiltration layer nonwoven fabric in multiple layers, and the average fiber diameter of the fibers constituting the microfiltration layer nonwoven fabric is less than 300 nm, and the prefiltration layer is a layer formed by wrapping a prefiltration layer nonwoven fabric in multiple layers, and configured so that the average fiber diameter decreases uniformly or stepwise in the filtration direction, and the average fiber diameter of the fibers constituting the prefiltration layer nonwoven fabric is 300 nm or more and less than 1000 nm. [2] The depth filter according to [1], wherein the outer layer is a layer configured so that the average basis weight of the outer layer nonwoven fabric decreases continuously in the filtration direction. [3] The depth filter according to [1] or [2], wherein the average fiber diameter on the most upstream side of the outer layer is 5 to 50 μm and the average fiber diameter ratio between the most upstream side and the most downstream side is 5 or more. [4] The depth filter according to any one of [1] to [3], wherein the prefiltration layer contains polypropylene having a melt flow rate of 500 g / 10 min or more and a melting point of 160°C or more. [5] The depth filter according to [4], wherein the polypropylene is polypropylene polymerized with a metallocene catalyst. [6] The depth filter according to any one of [1] to [5], wherein the fibers constituting the microfiltration layer nonwoven fabric are polyamide resin. [7] The depth filter according to any one of [1] to [6], wherein the microfiltration layer is a layer formed by winding a laminate of at least one substrate and the microfiltration layer nonwoven fabric in multiple layers. [8] The depth filter according to [7], wherein the fibers constituting the substrate and the nonwoven fabric for the microfiltration layer are polyamide resins.

[0011] It is possible to provide a depth filter that has absolute filtration performance even for submicron-sized particles to be removed, gel removal performance, and excellent liquid permeability.

[0012] The depth filter of the present invention comprises an outer layer, a prefiltration layer, and a microfiltration layer arranged in this order in the filtration direction. The depth filter may also include a support layer downstream of the microfiltration layer.

[0013] (Outer Layer) In the present invention, the outer layer is the layer located most upstream in the filtration direction of the depth filter. The outer layer's main purpose is to prevent large aggregates and impurities from penetrating the prefiltration layer and microfiltration layer, protect the prefiltration layer, which is made of finer fibers than conventional fibers, and maintain the filter shape when high pressure is applied. The outer layer is a layer in which outer layer nonwoven fabrics containing a high-melting point resin and a low-melting point resin are wound in multiple layers, with the wound nonwoven fabrics thermally bonded by the low-melting point resin, and configured so that the average fiber diameter continuously decreases in the filtration direction.

[0014] Because the outer layer in the present invention contains a high-melting-point resin and a low-melting-point resin, even when heat-treated using a heating roll or the like to improve the pressure resistance of the depth filter, the entire nonwoven fabric is less likely to become film-like, thereby preventing a decrease in water permeability. Examples of such outer layer include nonwoven fabrics made of bicomponent fibers (composite fibers) composed of a high-melting-point resin and a low-melting-point resin, mixed-fiber nonwoven fabrics of single-component fibers (high-melting fibers) composed of a high-melting-point resin and a single-component fiber (low-melting fibers) composed of a low-melting-point resin, and mixed-fiber nonwoven fabrics of high-melting-point fibers and / or low-melting-point fibers and composite fibers. From the viewpoint of ease of production, mixed-fiber nonwoven fabrics of high-melting-point fibers and low-melting-point fibers are preferred. Furthermore, when composite fibers are used, their cross-sectional configuration is not particularly limited, and examples include concentric sheath-core, eccentric sheath-core, side-by-side, sea-island, and radial composite configurations.

[0015] The high-melting point resin or the low-melting point resin is not particularly limited, and a common thermoplastic resin can be used, such as polyamide, polyester, low-melting point copolymer polyester, polystyrene, polyurethane elastomer, polyester elastomer, high-density polyethylene, low-density polyethylene, linear low-density polyethylene, polypropylene, or copolymer polypropylene (for example, a binary or terpolymer mainly composed of propylene and ethylene, butene-1, 4-methylpentene-1, or the like). Combinations of high-melting point resins and low-melting point resins are not particularly limited, and examples include polypropylene / polyethylene, polypropylene / copolymer polypropylene, polyester / low-melting point copolymer polyester, and polyester / polyethylene. Among these, from the viewpoint of achieving strong bonding strength between fibers upon heat treatment and thus obtaining a high-strength outer layer, combinations of polypropylene / copolymer polypropylene, polypropylene / low-density polyethylene, or polypropylene / linear low-density polyethylene are preferred, and polypropylene / copolymer polypropylene are more preferred. In particular, when the combination of high-melting point resin and low-melting point resin is polypropylene / copolymer polypropylene, not only the bonding strength between low-melting point resins but also the bonding strength between high-melting point resin and low-melting point resin can be improved.

[0016] The difference in melting point between the high-melting point resin and the low-melting point resin in the outer layer nonwoven fabric is not particularly limited, but is preferably at least 10° C., more preferably at least 15° C., and even more preferably at least 30° C. If the difference in melting point is at least 10° C., the temperature range over which only the low-melting point resin softens or melts during heat treatment during depth filter molding becomes wider, and the depth filter of the present invention can be stably produced under a wide range of conditions.

[0017] The content of the low-melting-point resin in the outer layer nonwoven fabric is not particularly limited, but is preferably 10 to 90 wt %, more preferably 20 to 70 wt %, and even more preferably 30 to 50 wt %. If the content of the low-melting-point resin is 10 wt % or more, an outer layer with little fuzz and sufficient strength can be formed, and if it is 90 wt % or less, the low-melting-point resin is less likely to clog the interfiber voids upon heat treatment or the like, and a depth filter with excellent pressure resistance and liquid permeability can be obtained.

[0018] The outer layer in the present invention is configured so that the average fiber diameter continuously decreases in the filtration direction, enabling efficient filtration of slurries with a wide particle size distribution or high concentration / high viscosity slurries throughout the entire thickness. Furthermore, since the outer layer is configured so that the average fiber diameter continuously decreases in the filtration direction, the average fiber diameter on the most upstream side of the outer layer in the filtration direction is the maximum average fiber diameter, and the average fiber diameter on the most downstream side of the filtration direction is the minimum fiber diameter. Such an outer layer can be obtained by winding an outer layer nonwoven fabric in which the fiber diameter continuously changes.

[0019] In the present invention, the average fiber diameter at the most upstream side of the outer layer is not particularly limited, but is preferably 5 to 50 μm, more preferably 6 to 30 μm, and even more preferably 7 to 20 μm. An average fiber diameter at the most upstream side of 5 μm or more provides excellent pressure resistance, while an average fiber diameter of 50 μm or less can improve filtration performance for large aggregates and impurities. Furthermore, the average fiber diameter at the most downstream side of the outer layer is not particularly limited, but is preferably 0.3 to 5 μm, more preferably 0.5 to 3 μm, and even more preferably 0.7 to 2 μm. An average fiber diameter at the most downstream side of the outer layer of 0.3 μm or more prevents excessive pressure loss relative to the filtration accuracy, while an average fiber diameter of 5 μm or less can prevent coarse particles from penetrating the prefiltration layer and microfiltration layer.

[0020] In the present invention, the average fiber diameter ratio between the most upstream side and the most downstream side of the outer layer is not particularly limited, but is preferably 5 or more, more preferably 10 or more, and even more preferably 15 or more. If the average fiber diameter ratio between the most upstream side and the most downstream side is 5 times or more, an excellent balance between pressure resistance performance and coarse particle capture performance is achieved. On the other hand, the upper limit of the average fiber diameter ratio between the most upstream side and the most downstream side is not particularly limited, but in order to achieve a configuration in which the average fiber diameter changes continuously, it is practically 50 times or less.

[0021] The outer layer in the present invention is not particularly limited, but is preferably wound so that the average basis weight of the outer layer nonwoven fabric continuously decreases in the filtration direction. By continuously decreasing the average basis weight in this way, pressure loss is less likely to occur, the slurry flows smoothly, and the particles to be removed can be efficiently filtered in the thickness direction. Furthermore, the lower filtration pressure makes it less likely that push-out will occur, and as a result, high filtration accuracy can be easily maintained for a long period of time. When the outer layer is configured so that the average basis weight continuously decreases in the filtration direction, the average basis weight on the most upstream side of the outer layer in the filtration direction is the maximum average basis weight, and the average basis weight on the most downstream side of the filtration direction is the minimum average basis weight. The maximum average basis weight of the outer layer in the present invention is not particularly limited, but is preferably 10 to 100 g / m 2 It is preferable that the density is 20 to 80 g / m 2 More preferably, it is 30 to 60 g / m 2 It is more preferable that the maximum average basis weight of the outer layer nonwoven fabric is 10 g / m 2 If the thickness is 100 g / m or more, sufficient rigidity can be imparted to the outer layer. 2 If the minimum average basis weight of the outer layer nonwoven fabric is not more than 1000 g / m, the outer layer nonwoven fabric can be sufficiently heated to the inside during heat treatment, and the wound outer layer nonwoven fabrics can be bonded together by gentle heating and pressure. 2 It is preferable that the density is 3 to 30 g / m 2 More preferably, it is 5 to 20 g / m 2 It is more preferable that the minimum average basis weight of the outer layer is 1 g / m 2 If the tension is 40 g / m or more, the necessary tension can be applied in the subsequent winding process. 2 If the thickness is less than this, fly-out and the like are less likely to occur during the manufacturing process, and the uniformity of the outer layer nonwoven fabric can be improved.

[0022] The ratio of the maximum average basis weight to the minimum average basis weight in the outer layer nonwoven fabric is not particularly limited, but is preferably 1.2 or more, more preferably 1.5 or more, even more preferably 1.8 or more, and particularly preferably 2.0 or more. By setting the ratio of the maximum average basis weight to the minimum average basis weight in the above-mentioned range, the effects of the present invention can be more easily obtained.

[0023] In the outer layer of the present invention, the wound nonwoven fabrics are thermally bonded together with a low-melting-point resin, which makes it difficult for compaction due to an increase in filtration pressure to occur, maintaining water permeability, and enabling filtration under mild conditions for a relatively long period of time even if the amount of trapped particles increases over time, thereby preventing push-out. In the present invention, "bonding between nonwoven fabrics" means that the nonwoven fabrics are fixed to a degree that prevents them from unwinding when the depth filter is disassembled.

[0024] The outer layer nonwoven fabric can be produced by, but is not particularly limited to, the melt-blowing method. The melt-blowing method is a method in which molten thermoplastic resin extruded from spinning holes in the machine direction or length direction is blown onto a collection conveyor net or a rotating core material (hollow mandrel) by high-temperature, high-velocity gas blown from around the spinning holes to obtain an ultrafine fiber web. In this process, the average fiber diameter or average basis weight can be continuously changed by continuously changing the spinning conditions, such as the amount of resin discharged from the spinning holes (discharge rate), the blowing airflow ejection speed (or hot air pressure), or the collection conveyor net discharge speed. The blowing airflow used in the melt-blowing method is usually an inert gas such as air or nitrogen gas. The gas temperature is 200 to 500°C, and the pressure is 0.1 to 6.5 kgf / cm. 2 The range is generally used.

[0025] In the process of producing the outer layer nonwoven fabric, gradually decreasing the discharge rates of the high-melting point resin and the low-melting point resin and gradually increasing the hot air pressure can gradually make the fibers thinner and gradually decrease the average basis weight. Furthermore, simultaneously adjusting the discharge rates and the hot air pressure can increase the ratio of the maximum average fiber diameter to the minimum average fiber diameter and the ratio of the average basis weight in the outer layer. Furthermore, changing the number of spinning holes allocated to the low-melting point resin and the high-melting point resin, as well as changing the extrusion rate of each resin, can change the content of low-melting point fibers in the outer layer nonwoven fabric. Furthermore, spinning each resin at a different discharge rate per spinning hole can produce an outer layer nonwoven fabric in which fibers with different average fiber diameters are mixed.

[0026] (Prefiltration Layer) The prefiltration layer in the present invention is a layer located intermediate between the outer layer and the microfiltration layer in the filtration direction, and is a layer whose main purpose is to capture microparticles that could not be captured by the outer layer. By capturing a certain amount of microparticles in the prefiltration layer, the filtration load on the microfiltration layer can be reduced. The prefiltration layer is a layer in which a prefiltration layer nonwoven fabric having an average fiber diameter of 300 nm or more and less than 1000 nm is wound in multiple layers, and is configured so that the average fiber diameter decreases constantly or stepwise in the filtration direction, i.e., the average fiber diameter decreases continuously.

[0027] The nonwoven fabric for the prefiltration layer in the present invention is characterized by an average fiber diameter of 300 nm or more and less than 1000 nm. It has been discovered that the depth filter of the present invention can significantly improve the absoluteness of filtration, gel removal performance, liquid permeability, and stability of capture performance under high pressure by using a prefiltration layer with a smaller average fiber diameter than conventional filters. An average fiber diameter of 300 nm or more can sufficiently maintain liquid permeability, while an average fiber diameter of less than 1000 nm can capture submicron-sized particles to a certain extent in the prefiltration layer, thereby achieving the absoluteness of filtration, gel removal performance, and stability of capture performance under high pressure. From this perspective, the average fiber diameter for the prefiltration layer is preferably 300 nm or more and less than 800 nm, and more preferably 300 nm or more and less than 700 nm.

[0028] The prefiltration layer in the present invention is a layer in which a prefiltration layer nonwoven fabric is wound in multiple layers, and is configured so that the average fiber diameter is constant or gradually decreases in the filtration direction. Note that a state in which the average fiber diameter gradually decreases in the filtration direction is distinguished from a state in which the average fiber diameter continuously decreases in the filtration direction, as in the outer layer. Specifically, an example of a prefiltration layer is one in which a prefiltration layer nonwoven fabric having an average fiber diameter of 700 nm or more and less than 1000 nm is wound in multiple layers, and a prefiltration layer nonwoven fabric having an average fiber diameter of 300 nm or more and less than 700 nm is wound in multiple layers downstream of the prefiltration layer nonwoven fabric.

[0029] The nonwoven fabric for the pre-filtration layer is not particularly limited, and may be composed of a single component or multiple components (such as composite fibers or mixed fibers), and may be made of the thermoplastic resins exemplified for the nonwoven fabric for the outer layer, or combinations thereof.

[0030] The nonwoven fabric for the prefiltration layer is not particularly limited, but preferably contains polypropylene having a melt flow rate of 500 g / 10 min or more and a melting point of 160° C. or more. By containing such polypropylene, it becomes easier to obtain a nonwoven fabric having excellent heat resistance and solvent resistance and an average fiber diameter of 300 nm or more and less than 1000 nm. From this perspective, it is more preferable that the polypropylene has a melt flow rate of 600 g / 10 min or more and a melting point of 160° C. or more. Furthermore, if the polypropylene is polypropylene polymerized using a metallocene catalyst, it is preferable because it has a narrow molecular weight distribution, therefore has little variation in average fiber diameter, good spinnability, and excellent processability. Furthermore, when the nonwoven fabric for the prefiltration layer is composed of a high-melting point resin and a low-melting point resin, the high-melting point resin can be polypropylene having a melt flow rate of 500 g / 10 min or more and a melting point of 160°C or more, and the low-melting point resin can be copolymerized polypropylene having a melting point of 150°C or less. This allows the copolymerized polypropylene to fuse together during molding of the depth filter, thereby improving the strength of the prefiltration layer.

[0031] The prefiltration layer nonwoven fabric is not particularly limited, and may be a laminate of multiple filtration layer nonwoven fabrics with different fiber diameters or components. For example, a first prefiltration layer nonwoven fabric having an average fiber diameter of 700 nm or more and less than 1000 nm and a second prefiltration layer nonwoven fabric having an average fiber diameter of 300 nm or more and less than 700 nm may be laminated to form a multi-wound prefiltration layer. Alternatively, a multi-wound prefiltration layer may be formed by laminating a polypropylene / copolymer polypropylene mixed fiber nonwoven fabric having an average fiber diameter of 700 nm or more and less than 1000 nm (first prefiltration layer nonwoven fabric) and a single-component polypropylene nonwoven fabric having an average fiber diameter of 300 nm or more and less than 700 nm (second prefiltration layer nonwoven fabric). Furthermore, a multi-wound prefiltration layer may be formed by laminating multiple first prefiltration layer nonwoven fabrics and multiple second prefiltration layer nonwoven fabrics in a multilayer structure. When multiple layers are laminated, the first pre-filtration layer nonwoven fabric and the second pre-filtration layer nonwoven fabric may be laminated alternately. The number of layers is not particularly limited, and any number of layers may be laminated as long as it does not interfere with the formation of the depth filter. However, a range of 1 to 10 layers provides an excellent balance between the functionality of the pre-filtration layer and workability during production.

[0032] The pre-filtration layer is not particularly limited, and may or may not be bonded between the wound nonwoven fabrics. However, it is preferable that the wound nonwoven fabrics are bonded between them. For example, by using a pre-filtration layer nonwoven fabric containing a high-melting point resin and a low-melting point resin, and heating it to a temperature above the melting point of the low-melting point resin but below the melting point of the high-melting point resin and winding it under a certain pressure, the wound nonwoven fabrics can be bonded by the low-melting point resin, and a depth filter with excellent pressure resistance can be obtained. On the other hand, by using a single-component pre-filtration layer nonwoven fabric and winding it under temperature and pressure conditions that do not completely melt but slightly soften it, the wound nonwoven fabrics can be fixed to a degree that does not easily peel off due to the anchor effect, and a depth filter with excellent water permeability can be obtained. Note that the state in which the wound nonwoven fabrics are fixed to a degree that does not easily peel off due to the anchor effect is also included in the state in which the wound nonwoven fabrics are bonded together.

[0033] The prefiltration layer is not particularly limited, and may be a laminate of a base sheet other than the prefiltration layer nonwoven fabric and the prefiltration layer nonwoven fabric wound in multiple layers. Examples of base sheets other than the prefiltration layer nonwoven fabric include nonwoven fabrics having an average fiber diameter of 1 to 1000 μm (spunbond nonwoven fabrics, meltblown nonwoven fabrics, through-air nonwoven fabrics, airlaid nonwoven fabrics, spunlace nonwoven fabrics, wet-laid nonwoven fabrics, etc.), woven and knitted fabrics, nets, etc. The base sheet other than the prefiltration layer nonwoven fabric can be made of the thermoplastic resin exemplified for the outer layer nonwoven fabric. Such a prefiltration layer can be formed simultaneously with the outer layer by, for example, using a nonwoven fabric in which the outer layer nonwoven fabric (region in which the average fiber diameter changes continuously) and the base sheet (region in which the average fiber diameter is constant) are connected, and winding the nonwoven fabric around a core material or the like while inserting the prefiltration layer nonwoven fabric onto the base sheet region.

[0034] The nonwoven fabric for the pre-filtration layer can be produced by the melt-blowing method described above, although it is not particularly limited thereto. However, unlike the method for producing the nonwoven fabric for the outer layer, the pre-filtration layer can be produced under constant conditions or by gradually changing the conditions without gradually changing the discharge rate or hot air pressure.

[0035] (Microfiltration Layer) The microfiltration layer in the present invention is a layer located downstream of the prefiltration layer described above in the filtration direction, and its main purpose is to capture fine particles and gels that could not be captured by the prefiltration layer. The microfiltration layer is a layer in which a nonwoven fabric for a prefiltration layer having an average fiber diameter of less than 300 nm is wound multiple times.

[0036] The nonwoven fabric for the microfiltration layer in the present invention is characterized in that the average fiber diameter is less than 300 nm. If the average fiber diameter of the nonwoven fabric for the microfiltration layer is less than 300 nm, it can capture fine particles and gels with an excellent balance between collection efficiency and liquid passage resistance, and from this viewpoint, it is preferably 250 nm or less, and more preferably 200 nm or less. Furthermore, the lower limit of the average fiber diameter of the nonwoven fabric for the microfiltration layer is not particularly limited, but in consideration of practical strength, productivity, etc., it is preferably 50 nm or more, and more preferably 100 nm or more.

[0037] The CV value of the fiber diameter of the fibers constituting the nonwoven fabric for the microfiltration layer is not particularly limited, but is preferably 0.3 or less, more preferably 0.2 or less. If the CV value of the fiber diameter is 0.3 or less, the average pore size of the nonwoven fabric for the microfiltration layer becomes small, and the capturing performance of fine particles and gel can be improved. Furthermore, the lower limit of the CV value of the fiber diameter is not particularly limited, but in reality it is 0.01 or more.

[0038] The resin constituting the prefiltration layer in the present invention is not particularly limited, and examples thereof include polyamide resins such as nylon 4, nylon 6, nylon 11, nylon 12, nylon 66, nylon 610, polyparaphenylene terephthalamide, polymetaxylylene adipamide, and polyhexamethylene terephthalamide, fluorine-based resins such as polyvinylidene fluoride and polyvinylidene fluoride-hexafluoropropylene copolymer, acrylic resins such as polyacrylonitrile, polyacrylonitrile-methacrylate copolymer, and polymethyl methacrylate, polyolefin resins such as polyethylene and polypropylene, polyester resins such as polylactic acid and polyethylene terephthalate, polyimide, polyvinyl alcohol, polyethylene oxide, polyethyleneimine, polysulfone, polyethersulfone, cellulose derivatives, and mixtures thereof. Among these, from the viewpoints of water permeability and chemical resistance, polyamide resins are preferred, and nylon 6 or nylon 6,6 is more preferred.

[0039] The basis weight of the nonwoven fabric for the microfiltration layer is not particularly limited, but is preferably 0.1 to 15 g / m 2 It is preferable that the density is 0.1 to 10 g / m 2 More preferably, it is 0.1 to 5.0 g / m 2 More preferably, it is 0.2 to 4.0 g / m 2 It is particularly preferable that the density is 0.5 to 3.0 g / m 2 It is most preferable that the basis weight of the nonwoven fabric for the microfiltration layer is 0.1 g / m 2 If the density is 15.0 g / m or more, the capturing performance of fine particles and gel can be improved. 2 If it is below this value, the filtration pressure will not become too high, and compaction and push-out will be less likely to occur.

[0040] The microfiltration layer is not particularly limited, but may be a laminate (microfiltration layer laminate) of at least one substrate and a microfiltration layer nonwoven fabric wound in multiple layers. The microfiltration layer nonwoven fabric has low strength and rigidity by itself and may wrinkle or break due to tension when formed into a depth filter. However, laminating it with a substrate makes it easier to form a depth filter. Examples of substrates include nonwoven fabrics having an average fiber diameter of 300 nm to 1000 μm (spunbond nonwoven fabrics, meltblown nonwoven fabrics, electrospun nonwoven fabrics, through-air nonwoven fabrics, airlaid nonwoven fabrics, spunlace nonwoven fabrics, wet-laid nonwoven fabrics, etc.), woven and knitted fabrics, nets, etc. In addition, nonwoven fabrics for the outer layer and nonwoven fabrics for the pre-filtration layer can also be used as the substrate. The substrate can be made of the thermoplastic resin exemplified for the outer layer nonwoven fabric, but a spunbonded or meltblown nonwoven fabric made of polyamide or polypropylene, or a through-air nonwoven fabric or composite spunbonded nonwoven fabric using composite fibers made of polyethylene / polypropylene or polyethylene / polyester is preferred from the viewpoints of imparting strength to the microfiltration layer nonwoven fabric and processability. In particular, when the microfiltration layer nonwoven fabric is made of polyamide, it is preferable to use a substrate made of polyamide. Furthermore, when a prefiltration layer nonwoven fabric is used as the substrate, it is preferable that the microfiltration layer nonwoven fabric be arranged adjacent to the prefiltration layer nonwoven fabric on the downstream side in the filtration direction from the viewpoint of microparticle capture performance.

[0041] The nonwoven fabric for the microfiltration layer can be produced by, but is not particularly limited to, electrospinning, which not only makes it possible to form fibers from a wide range of materials but also makes it possible to make the average fiber diameter of the fibers constituting the nonwoven fabric for the microfiltration layer small and uniform.

[0042] The electrostatic spinning method is a method in which a spinning solution is discharged and an electric field is applied to the discharged spinning solution to form fibers with a very small fiber diameter on a collector. Examples of the electrostatic spinning method include a method in which a spinning solution is extruded from a nozzle and an electric field is applied to the spinning solution, a method in which a spinning solution is foamed and an electric field is applied to the spinning solution, and a method in which a spinning solution is introduced onto the surface of a cylindrical electrode and an electric field is applied to the spinning solution.

[0043] The spinning solution is not particularly limited as long as it has spinnability. For example, a solution in which the above-mentioned resin is dispersed in a solvent, a solution in which the resin is dissolved in a solvent, or a solution in which the resin is melted by heat or laser irradiation can be used. From the viewpoint of fineness and uniformity of the fibers, however, it is preferable to use a solution in which the resin is dissolved in a solvent.

[0044] The solvent used in the spinning solution is not particularly limited, and examples thereof include water, methanol, ethanol, propanol, acetone, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylpropionamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, triethyl phosphate, propylene glycol monomethyl ether, diethylene glycol ethyl methyl ether, toluene, xylene, pyridine, formic acid, acetic acid, tetrahydrofuran, dichloromethane, chloroform, 1,1,1,3,3,3-hexafluoroisopropanol, and mixtures thereof.

[0045] The resin concentration in the spinning solution is not particularly limited, but can be 1 to 50 wt %. Furthermore, to improve the stability and spinnability of electrospinning, the spinning solution may contain 0.001 to 5 wt % of a surfactant. Furthermore, additives such as antibacterial agents, deodorants, antistatic agents, conductive materials, fluorescent materials, smoothing agents, hydrophilic agents, water repellents, hydrophilic and oil repellents, antioxidants, weather resistance agents, and charge stabilizers may be added within a range that does not significantly impair the effects of the present invention.

[0046] The applied voltage is not particularly limited as long as it is within a range that allows fibers to be formed and stable spinning is possible, and examples thereof include 5 to 100 kV. The distance between the nozzle and the collector is also not particularly limited as long as it is within a range that allows sufficient solvent volatilization, and examples thereof include 5 to 100 cm. The discharge rate of the spinning solution can be appropriately adjusted taking into consideration the average fiber diameter, CV value, productivity, etc. of the resulting fibers, and examples thereof include 0.1 to 50 ml / hr. The material of the collector is not particularly limited as long as it can collect electrospun fibers, but conductive materials such as metals are preferably used. The shape of the collector is not particularly limited, and examples thereof include a flat plate, a shaft, or a conveyor-shaped collector. A flat plate-shaped collector can produce a sheet-shaped laminate, and a shaft-shaped collector can produce a tubular laminate. A conveyor-shaped collector can continuously produce a sheet-shaped laminate.

[0047] When a laminate for a microfiltration layer is used, it is preferable to produce the nonwoven fabric for the microfiltration layer by directly electrospinning the substrate while conveying the substrate on a conveyor. By producing in this manner, the adhesion between the substrate and the nonwoven fabric for the microfiltration layer is improved, making it easier to form a depth filter. In particular, by making the substrate and the nonwoven fabric for the microfiltration layer from the same resin, it is possible to further improve the adhesion. Among them, from the viewpoints of water permeability, chemical resistance, ease of availability, etc., it is preferable that the substrate and the nonwoven fabric for the microfiltration layer are made of a polyamide-based resin.

[0048] (Support Layer) The depth filter of the present invention may have a support layer downstream of the microfiltration layer in the filtration direction, although this support layer is not particularly limited. The support layer is provided to maintain the shape of the prefiltration layer and microfiltration layer and to prevent the filter material from falling off the microfiltration layer. Examples of the support layer include a resin core material having open holes, as well as a layer formed by winding a nonwoven fabric, a woven fabric, or a net. The nonwoven fabric constituting the support layer (nonwoven fabric for the support layer) may be the same as the nonwoven fabric for the outer layer, or a stronger nonwoven fabric such as a spunbond nonwoven fabric may be used.

[0049] The nonwoven fabric for the support layer can be produced by the melt-blowing method described above, although it is not particularly limited thereto. The discharge rate and hot air pressure may be gradually changed, or the fabric may be produced under constant conditions or by gradually changing the conditions. From the viewpoint of efficient continuous production of depth filters, it is particularly preferable to gradually change the discharge rate and hot air pressure to form a support layer in which the average fiber diameter and / or average basis weight increases continuously in the filtration direction.

[0050] (Depth Filter) The depth filter of the present invention comprises the outer layer, prefiltration layer, and microfiltration layer arranged in this order in the filtration direction, and a support layer is arranged downstream of the microfiltration layer as needed. Layers other than those described above may be formed upstream of the outer layer, between the layers, and downstream of the support layer.

[0051] In the depth filter of the present invention, although not particularly limited, the outer layer and the prefiltration layer are preferably bonded to each other. Also, although not particularly limited, the prefiltration layer and the microfiltration layer are preferably bonded to each other. Such adhesion between the layers can suppress compaction of the depth filter.

[0052] The depth filter of the present invention can be obtained by winding and fixing the above-mentioned outer layer nonwoven fabric, prefiltration layer nonwoven fabric, and microfiltration layer nonwoven fabric around a core material. In particular, when winding the outer layer nonwoven fabric, it is preferable to wind it while heating it with a through-air heat treatment or a far-infrared heater, etc., in order to melt the low-melting point resin. The depth filter can be formed by winding each nonwoven fabric sequentially, or it can be continuously formed by inserting each nonwoven fabric while winding the base sheet.

[0053] The diameter and thickness of the depth filter of the present invention can be appropriately set depending on the desired performance and the properties of the filtrate. For example, in the case of a depth filter used for slurry filtration in the production process of CMP slurry, the inner diameter is preferably about 23 to 100 mm. By setting the inner diameter to 23 mm or more, a sufficient amount of liquid can be ensured to flow to the inner wall side. By setting the inner diameter to 100 mm or less, the depth filter can be made compact. Furthermore, the thickness (= (outer diameter - inner diameter) ÷ 2) is preferably 10 to 30 mm. By setting the thickness to 10 mm or more, a sufficient change ratio between the average fiber diameter and the average basis weight can be achieved. By setting the thickness to 30 mm or less, a depth filter with excellent liquid permeability can be obtained.

[0054] The depth filter produced as described above can be cut to an appropriate size and end caps attached to both ends to form a cylindrical depth filter, or can be enclosed in a small capsule for use.

[0055] The above manufacturing method is only an outline, and in addition to the above steps, known steps such as heat treatment, cooling, chemical treatment, molding, and washing can be carried out as necessary.

[0056] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. The measurement methods or definitions of the physical properties shown in the examples are as follows.

[0057] <Average fiber diameter of fibers constituting each nonwoven fabric> The lengths (diameters) of 100 fibers in the direction perpendicular to the longitudinal direction were measured from the cross section of the filter photographed with an electron microscope, and the arithmetic mean value was taken as the average fiber diameter. This measurement was performed using image processing software "Scion Image" (product name) from Scion Corporation.

[0058] <Average basis weight of each nonwoven fabric> The nonwoven fabric obtained by spinning was cut into a circle of 100 cm 2 The measurement sample was cut into 3 pieces, and three pieces were taken in the width direction (left side, center, right side). The weight of each piece was measured, and the weight per unit area (g / m 2 ) was calculated and the arithmetic mean value was taken as the basis weight.

[0059] <Melt flow rate (MFR) of resin> The MFR was measured in accordance with the method of JIS K 7210-1:2014 using a standard die at a temperature of 230°C and a load of 2.16 kg.

[0060] <Melting Point of Resin> Using a differential scanning calorimeter (DSC8500) manufactured by PerkinElmer Japan, the temperature corresponding to the peak on the melting absorption curve obtained when the thermoplastic resin was heated at a rate of 10°C / min was taken as the melting point of the resin.

[0061] <Water flow performance> Water was passed through the filter housing without a filter attached, and the relationship between the amount of water passing and the pressure loss before and after the housing was determined, and this value was taken as the piping resistance. Next, the filter was attached to the housing as a test sample and water was passed through (maximum pressure 0.28 MPa), and the amount of water passing through and the pressure loss before and after the housing were determined, and this value was taken as the provisional pressure loss. The value obtained by subtracting the piping resistance from the provisional pressure loss was taken as the true differential pressure of the test sample. Water was passed through at flow rates of 10 L / min, 15 L / min, and 20 L / min. Note that if water could not pass through, it was marked as x.

[0062] <Filtration Performance> The collection efficiency and differential pressure were measured over time using the following test powder and method. Nippon Shokubai's spherical silica (Seahorstar KE-S30 (average particle size 300 nm)) was used as the test powder. 3 g of spherical silica and 3 mL of a 0.2% aqueous solution of sodium hexametaphosphate were added to a magnetic mortar and mixed with a pestle. The spherical silica prepared above was then added to a 250 mL standard container of a Kurabo Mazerustar planetary mixer / stirring / deaerating device. A 0.2% aqueous solution of sodium hexametaphosphate was then added until the total weight reached 250 g, and the mixture was stirred for 20 minutes. 250 g of the spherical silica dispersion was transferred to a 3 L flask, and ultrapure water was added to a total volume of 3 L to prepare a spherical silica dispersion. The filter was then attached to a filtration tester, and water was circulated at a rate of 10 L / min for 30 minutes. Thereafter, 30 L of pure water was placed in the tank of the filtration tester, and while stirring with a stirring blade, 3 L of spherical silica dispersion was continuously pumped into the 30 L tank at a rate of 100 mL / min, and the liquid was passed through the filtration tester equipped with a filter at a rate of 10 L / min. The liquid was passed through and the spherical silica dispersion was added until the differential pressure between the inlet pressure and the outlet pressure reached 300 kPa. Just before the 3 L of spherical silica dispersion was completely drained, 3 L of new spherical silica dispersion was added, and filtration was continued. During this time, fluid was collected from the inlet and outlet sides of the filter at any time, and this was used as a sample. The collected sample was used to measure the number of particles before and after the filter using an Accusizer 780APS (manufactured by PSS Japan Co., Ltd.), and the collection efficiency was calculated using the following formula. Filtration efficiency (%) = (1 - number of particles after passing through the filter / number of particles before passing through the filter) x 100. The collection efficiency was calculated from the measured value for a particle diameter of 0.57 µm. Note that, since the filtration performance evaluation was performed after the water permeability performance evaluation, the collection efficiency of filters that could not pass water was marked x.

[0063] <Gel Capture Performance> 1 L of ultrapure water in a beaker was heated in a water bath set to 95°C, and 5 g of methylcellulose 25 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added little by little and stirred for 10 minutes. The mixture was then allowed to cool in an oven set to 28°C and allowed to stand for at least 12 hours. Next, a gel dispersion was prepared by ultrasonically stirring the gel precipitated at the bottom of the beaker. A 3 cm long filter with end caps welded to both ends was attached to a filtration tester, and water was passed through it at a maximum pressure of 280 kPa. The gel dispersion prepared by the above method was pumped through the filter at a rate of 100 mL / min, and filtered in one pass until 1 L of the prepared gel dispersion was used. The gel dispersion was collected before and after passing through the filter, and the number of particles before and after the filter was measured using an Accusizer 780APS (manufactured by PSS Japan Co., Ltd.). The collection efficiency was calculated using the following formula. Ultrapure water at 18°C ​​was used for the measurements. Collection efficiency (%) = (1 - number of particles after passing through the filter / number of particles before passing through the filter) x 100. The collection efficiency of a filter through which water could not pass was marked x.

[0064] [Example 1] <Production of Laminate 1 for Microfiltration Layer> Nylon 6 resin (product name: A1030BRT) manufactured by Unitika was dissolved at a concentration of 15 wt% in a cosolvent of formic acid and acetic acid (30 / 70 (w / w)) to prepare an electrospinning solution. The obtained spinning solution was electrospun using a multi-hole spinneret having 12 nozzle holes with an inner diameter of 0.3 mm under the conditions of a solution supply rate of 1.0 mL / h to each nozzle hole, an applied voltage of 50.0 kV, and a spinning distance of 15.0 cm. On the collector electrode, a nylon spunbond nonwoven fabric (product name: ELTAS Nylon (N05050), average fiber diameter: 15.60 μm, basis weight: 50 g / m) manufactured by Asahi Kasei was placed. 2 ) was placed as a substrate, and the electrospun nonwoven fabric for the microfiltration layer was placed on the substrate at a density of 2.5 g / m 2 The nonwoven fabric for the microfiltration layer had an average fiber diameter of 270 nm and a CV value of the fiber diameter of 0.12.

[0065] <Production of nonwoven fabric 1 having a continuous fiber diameter gradient> As the high-melting-point resin, polypropylene polymerized by a metallocene catalyst (MF650Y, manufactured by PolyMirae Co., Ltd., MFR: 1500 g / 10 min, melting point: 165°C) was used, and as the low-melting-point resin, copolymer polypropylene (SOW0279, manufactured by Japan Polypropylene Corporation, MFR: 60 g / 10 min, melting point: 140°C) was used. A melt-blown spinneret with a total of 501 holes was used, in which spinning holes for discharging high-melting-point resin and spinning holes for discharging low-melting-point resin, each with a hole diameter of 0.2 mm, were arranged alternately in a row. At a spinning temperature of 370°C, a high-melting-point resin and a low-melting-point resin (weight ratio 5:5) were extruded while the extrusion rate was continuously changed from 234 g / min to 40 g / min, and the hot air pressure at a temperature of 400°C was continuously changed from 11.8 kPa to 31.7 kPa, and then the extrusion was continued while the extrusion rate was continuously changed from 40 g / min to 234 g / min, and the hot air pressure at a temperature of 400°C was continuously changed from 31.7 kPa to 11.8 kPa, and the extrusion was spun by blowing the extrusion onto a conveyor net equipped with a suction device and winding it up on a paper tube roll at 9 m / min, to obtain a nonwoven fabric 1 having a continuous fiber diameter gradient. The obtained nonwoven fabric 1 had an average fiber diameter that continuously changed from 11.57 μm to 0.61 μm and an average basis weight of 47.7 g / m. 2 to 14.7 g / m 2 and a portion (corresponding to the outer layer nonwoven fabric) in which the average fiber diameter is 0.61 μm and the average basis weight is 14.7 g / m. 2 and a portion in which the average fiber diameter continuously changes from 0.61 μm to 11.57 μm and the average basis weight is 14.7 g / m 2 to 47.7 g / m 2 The nonwoven fabric was composed of a portion (corresponding to the nonwoven fabric for the support layer) in which the thickness of the nonwoven fabric changed continuously.

[0066] <Production of Depth Filter> A nonwoven fabric 1 having a continuous fiber diameter gradient was heated in a through-air processing machine under conditions of a conveyor speed of 8.5 m / min and a set temperature of 131°C, and immediately thereafter wound around a core material with an outer diameter of 30 mm to obtain a cylindrical molded article. At this time, a 0.8 m long microfiltration layer laminate 1 was inserted at the most downstream position of the prefiltration layer nonwoven fabric portion. The obtained cylindrical molded article had, from the outside, an outer layer, a prefiltration layer, a microfiltration layer, and a support layer in that order. In the outer layer, the nonwoven fabric on the most upstream side in the filtration direction had an average fiber diameter of 11.57 μm and an average basis weight of 47.7 g / m 2 The average fiber diameter of the nonwoven fabric on the most downstream side is 0.61 μm and the average basis weight is 14.7 g / m 2 The pre-filtration layer had an average fiber diameter of 0.61 μm and an average basis weight of 14.7 g / m 2 The microfiltration layer is a layer in which a laminate of a melt-blown nonwoven fabric (corresponding to the substrate) having an average fiber diameter of 1.37 μm and a microfiltration layer laminate 1 is wound around the support layer. The average fiber diameter of the support layer increases continuously from 0.61 μm to 11.57 μm in the filtration direction, and the average basis weight is 14.7 g / m. 2 to 47.7 g / m 2 The thickness of the layer increased continuously. The obtained cylindrical molding was allowed to cool at room temperature, removed from the core material, and both ends were cut to obtain a depth filter with a total length of 245 mm, an outer diameter of 68 mm, and an inner diameter of 30 mm. The nonwoven fabric for the outer layer and the nonwoven fabric for the pre-filtration layer were bonded between the wound nonwoven fabrics, and the outer layer and the pre-filtration layer were bonded to each other. The ends of the depth filter were then sealed with flat gaskets (polyethylene foam with a foaming ratio of 3 times and a thickness of 3 mm, cut into doughnut shapes), resulting in a total length of 250 mm. The flat gasket and the cylindrical molding were thermally bonded to form an integrated unit.

[0067] [Example 2] <Production of laminate 2 for microfiltration layer> A polypropylene melt-blown nonwoven fabric (product name: nano2, average fiber diameter: 600 nm, basis weight: 10 g / m) manufactured by Mitsui Chemicals was used as the substrate. 2 ) was used, and the basis weight of the nonwoven fabric for the microfiltration layer was set to 0.8 g / m 2A laminate 2 for a microfiltration layer was produced in the same manner as in Example 1, except that the nonwoven fabric for the microfiltration layer was changed to 1. The obtained laminate 2 for a microfiltration layer had good formation, with no peeling or wrinkling of the nonwoven fabric for the microfiltration layer being observed. The nonwoven fabric for the microfiltration layer had an average fiber diameter of 270 nm and a CV value of the fiber diameter of 0.12.

[0068] <Preparation of Nonwoven Fabric 2 for Pre-filtration Layer> A polypropylene melt-blown nonwoven fabric (product name: nano2; average fiber diameter: 600 nm, average basis weight: 10 g / m) manufactured by Mitsui Chemicals was used. 2 ) was used as a laminate of six layers.

[0069] <Production of Nonwoven Fabric 2 Having Continuous Fiber Diameter Gradient> Polypropylene (SA08A, manufactured by Japan Polypropylene Corporation, MFR: 80 g / 10 min, melting point: 165°C) was used as the high-melting-point resin, and copolymer polypropylene (SOW0279, manufactured by Japan Polypropylene Corporation, MFR: 60 g / 10 min, melting point: 140°C) was used as the low-melting-point resin. Using the same melt-blowing spinneret as in Example 1, a high-melting-point resin and a low-melting-point resin (weight ratio 5:5) were extruded at a spinning temperature of 360°C while the extrusion rate was continuously changed from 120 g / min to 20 g / min, and the hot air pressure at a temperature of 400°C was continuously changed from 10 kPa to 99 kPa, and then the extrusion was continued while the extrusion rate was continuously changed from 20 g / min to 120 g / min, and the hot air pressure at a temperature of 400°C was continuously changed from 99 kPa to 10 kPa, and the extrusion was spun by blowing the extruded material onto a conveyor net equipped with a suction device and winding it up on a paper tube roll at 9 m / min, thereby obtaining a nonwoven fabric 2 having a continuous fiber diameter gradient. The obtained nonwoven fabric 2 had an average fiber diameter that continuously changed from 24 μm to 1.37 μm and an average basis weight of 47.7 g / m. 2 to 10.7 g / m 2 and a portion (corresponding to the outer layer nonwoven fabric) in which the average fiber diameter is 1.37 μm and the average basis weight is 14.7 g / m. 2 The average fiber diameter continuously changes from 1.37 μm to 24 μm, and the average basis weight is 10.7 g / m 2 to 47.7 g / m 2The nonwoven fabric was composed of a portion (corresponding to the nonwoven fabric for the support layer) in which the thickness of the nonwoven fabric changed continuously.

[0070] <Production of Depth Filter> Nonwoven fabric 2 having a continuous fiber diameter gradient was heated in a through-air processing machine at a conveyor speed of 8.5 m / min and a set temperature of 131°C, and immediately thereafter wound around a core material with an outer diameter of 30 mm to obtain a cylindrical molded article. At this time, the portion of nonwoven fabric 2 corresponding to the base sheet (average fiber diameter of 1.37 μm, average basis weight of 14.7 g / m) was 2 A 2.4 m long laminate 2 for a microfiltration layer and a 0.8 m long nonwoven fabric 2 for a prefiltration layer were inserted in this order into the cylindrical molded article (a certain portion of the outer layer). The obtained cylindrical molded article had, from the outside, an outer layer, a prefiltration layer, a microfiltration layer, and a support layer, in that order. In the outer layer, the nonwoven fabric on the most upstream side in the filtration direction had an average fiber diameter of 24 μm and an average basis weight of 47.7 g / m 2 The average fiber diameter of the nonwoven fabric on the most downstream side is 1.37 μm and the average basis weight is 10.7 g / m 2 The prefiltration layer was a layer in which a laminate of a melt-blown nonwoven fabric (corresponding to the base sheet) having an average fiber diameter of 1.37 μm and a nonwoven fabric 2 for the prefiltration layer was wound, the microfiltration layer was a layer in which a laminate of a melt-blown nonwoven fabric (corresponding to the substrate) having an average fiber diameter of 1.37 μm and a laminate 2 for the microfiltration layer was wound, and the support layer had an average fiber diameter that continuously increased from 1.37 μm to 24 μm in the filtration direction and an average basis weight of 10.7 g / m 2 to 47.7 g / m 2 The thickness of the outer layer nonwoven fabric and the thickness of the pre-filtration layer nonwoven fabric were continuously increased. A depth filter was then produced in the same manner as in Example 1. The outer layer nonwoven fabric and the pre-filtration layer nonwoven fabric were bonded together between the wound nonwoven fabrics, and the outer layer and the pre-filtration layer were also bonded together.

[0071] [Example 3] <Production of laminate 3 for microfiltration layer> A nylon meltblown nonwoven fabric (product name: N050F-00F, average fiber diameter: 4.59 μm, basis weight: 50 g / m) manufactured by Tapyrus was used as the substrate. 2 ) was used, and the basis weight of the nonwoven fabric for the microfiltration layer was 3.0 g / m 2Except for this, a laminate 3 for a microfiltration layer was produced in the same manner as in Example 1. The obtained laminate 3 for a microfiltration layer showed no peeling or wrinkling of the nonwoven fabric for the microfiltration layer and had good formation. The nonwoven fabric for the microfiltration layer had an average fiber diameter of 270 nm and a CV value of the fiber diameter of 0.12.

[0072] <Preparation of Nonwoven Fabric 3 for Pre-filtration Layer> A polypropylene melt-blown nonwoven fabric (product name: nano2; average fiber diameter: 600 nm, average basis weight: 10 g / m) manufactured by Mitsui Chemicals was used. 2 ) was used as a laminate of six layers.

[0073] <Production of Nonwoven Fabric 3 with Continuous Fiber Diameter Gradient> Nonwoven fabric 3 with continuous fiber diameter gradient was produced in the same manner as in Example 1, except that spinning was performed while continuously changing the hot air pressure from 10.2 kPa to 34.5 kPa at a temperature of 400°C. The obtained nonwoven fabric 3 had an average fiber diameter that continuously changed from 9.15 μm to 0.63 μm and an average basis weight of 54.0 g / m 2 to 16.8 g / m 2 and a portion (corresponding to the outer layer nonwoven fabric) in which the average fiber diameter is 0.63 μm and the average basis weight is 16.8 g / m. 2 and a portion in which the average fiber diameter continuously changes from 0.63 μm to 9.15 μm and the average basis weight is 16.8 g / m. 2 to 54.0 g / m 2 The nonwoven fabric was composed of a portion (corresponding to the nonwoven fabric for the support layer) in which the thickness of the nonwoven fabric changed continuously.

[0074] <Production of Depth Filter> A nonwoven fabric 3 having a continuous fiber diameter gradient was heated in a through-air processing machine under conditions of a conveyor speed of 8.5 m / min and a set temperature of 131°C, and immediately thereafter wound around a core material with an outer diameter of 30 mm to obtain a cylindrical molded article. At this time, a 0.8 m long microfiltration layer laminate 3 was inserted at the most downstream position of the prefiltration layer nonwoven fabric portion, and then a 0.6 m long prefiltration layer nonwoven fabric 3 was inserted in this order. The obtained cylindrical molded article had, from the outside, an outer layer, a prefiltration layer, a microfiltration layer, and a support layer, in that order. In the outer layer, the nonwoven fabric most upstream in the filtration direction had an average fiber diameter of 9.15 μm and an average basis weight of 54.0 g / m 2The average fiber diameter of the nonwoven fabric on the most downstream side is 0.63 μm and the average basis weight is 16.8 g / m 2 The prefiltration layer was a layer formed by winding a laminate of a melt-blown nonwoven fabric (corresponding to the first prefiltration layer nonwoven fabric) having an average fiber diameter of 0.63 μm and a prefiltration layer nonwoven fabric 2 (corresponding to the second prefiltration layer nonwoven fabric), the microfiltration layer was a layer formed by winding a laminate of a melt-blown nonwoven fabric (corresponding to the substrate) having an average fiber diameter of 0.63 μm and a microfiltration layer laminate 3, and the support layer had an average fiber diameter that continuously increased from 0.63 μm to 9.15 μm in the filtration direction and an average basis weight of 16.8 g / m 2 to 54.0 g / m 2 The thickness of the layers increased continuously. Except for this, a depth filter was produced in the same manner as in Example 1. The outer layer nonwoven fabric and the prefiltration layer nonwoven fabric were bonded between the wound nonwoven fabrics, and the outer layer and the prefiltration layer were bonded to each other.

[0075] [Example 4] <Production of laminate 4 for microfiltration layer> A polypropylene melt-blown nonwoven fabric (product name: nano2, average fiber diameter: 600 nm, basis weight: 10 g / m) manufactured by Mitsui Chemicals was used as the substrate. 2 ) was used, and the basis weight of the nonwoven fabric for the microfiltration layer was set to 2.7 g / m 2 Except for this, a laminate 4 for a microfiltration layer was produced in the same manner as in Example 1. The obtained laminate 4 for a microfiltration layer showed no peeling or wrinkling of the nonwoven fabric for the microfiltration layer and had good formation. The nonwoven fabric for the microfiltration layer had an average fiber diameter of 270 nm and a CV value of the fiber diameter of 0.12.

[0076] <Production of Nonwoven Fabric 4 Having Continuous Fiber Diameter Gradient> MF650X (manufactured by PolyMirae Co., Ltd., MFR: 1200 g / 10 min, melting point: 165°C) was used as the high-melting-point resin, and SOW0279 (manufactured by Japan Polypropylene Corporation, MFR: 60 g / 10 min, melting point: 140°C) was used as the low-melting-point resin. Using the same melt-blowing spinneret as in Example 1, a high-melting point resin and a low-melting point resin (weight ratio 5:5) were extruded at a spinning temperature of 360°C while continuously changing the discharge rate from 233 g / min to 42 g / min, and the hot air pressure at a temperature of 400°C was continuously changed from 13.9 kPa to 32.1 kPa. After maintaining these conditions for a while, the extrusion was continued while continuously changing the discharge rate from 42 g / min to 233 g / min, and the hot air pressure at a temperature of 400°C was continuously changed from 32.1 kPa to 13.9 kPa to perform spinning. The resulting mixture was blown onto a conveyor net equipped with a suction device and taken up around a paper tube roll at 9 m / min, thereby obtaining nonwoven fabric 4 having a continuous fiber diameter gradient. The obtained nonwoven fabric 4 had an average fiber diameter that continuously changed from 13.6 μm to 0.71 μm and an average basis weight of 47.7 g / m 2 to 14.2 g / m 2 and a portion (corresponding to the outer layer nonwoven fabric) in which the average fiber diameter is 0.71 μm and the average basis weight is 9.9 g / m. 2 and a portion in which the average fiber diameter continuously changes from 0.71 μm to 13.6 μm and the average basis weight is 14.2 g / m. 2 to 47.7 g / m 2 The nonwoven fabric was composed of a portion (corresponding to the nonwoven fabric for the support layer) in which the thickness of the nonwoven fabric changed continuously.

[0077] <Production of Depth Filter> A cylindrical molded article was obtained in the same manner as in Example 3, except that nonwoven fabric 4 was used instead of nonwoven fabric 3, and laminate for a microfiltration layer 4 was used instead of laminate for a microfiltration layer 3. The obtained cylindrical molded article had, from the outside, an outer layer, a prefiltration layer, a microfiltration layer, and a support layer in that order, and in the outer layer, the nonwoven fabric on the most upstream side in the filtration direction had an average fiber diameter of 13.6 μm and an average basis weight of 47.7 g / m 2 The average fiber diameter of the nonwoven fabric on the most downstream side is 0.71 μm and the average basis weight is 14.2 g / m2 The prefiltration layer was a layer formed by winding a laminate of a melt-blown nonwoven fabric (corresponding to the first prefiltration layer nonwoven fabric) having an average fiber diameter of 0.71 μm and a prefiltration layer nonwoven fabric 2 (corresponding to the second prefiltration layer nonwoven fabric), the microfiltration layer was a layer formed by winding a laminate of a melt-blown nonwoven fabric (corresponding to the substrate) having an average fiber diameter of 0.71 μm and a microfiltration layer laminate 4, and the support layer had an average fiber diameter that continuously increased from 0.71 μm to 13.6 μm in the filtration direction and an average basis weight of 14.2 g / m 2 to 47.7 g / m 2 The thickness of the layers increased continuously. Except for this, a depth filter was produced in the same manner as in Example 1. The outer layer nonwoven fabric and the prefiltration layer nonwoven fabric were bonded between the wound nonwoven fabrics, and the outer layer and the prefiltration layer were bonded to each other.

[0078] [Example 5] <Production of laminate 5 for microfiltration layer> A polypropylene melt-blown nonwoven fabric (product name: nano2, average fiber diameter: 600 nm, basis weight: 10 g / m) manufactured by Mitsui Chemicals was used as the substrate. 2 ) was used, and the basis weight of the nonwoven fabric for the microfiltration layer was set to 2.6 g / m 2 Except for this, a laminate 5 for a microfiltration layer was produced in the same manner as in Example 1. The obtained laminate 5 for a microfiltration layer showed no peeling or wrinkling of the nonwoven fabric for the microfiltration layer and had good formation. The nonwoven fabric for the microfiltration layer had an average fiber diameter of 270 nm and a CV value of the fiber diameter of 0.12.

[0079] <Production of Nonwoven Fabric 5 Having Continuous Fiber Diameter Gradient> MF650Z (manufactured by PolyMirae Co., Ltd., MFR: 2300 g / 10 min, melting point: 165°C) was used as the high-melting-point resin, and SOW0279 (manufactured by Japan Polypropylene Corporation, MFR: 60 g / 10 min, melting point: 140°C) was used as the low-melting-point resin. Using the same melt-blown spinneret as in Example 1, a high-melting point resin and a low-melting point resin (weight ratio 5:5) were extruded at a spinning temperature of 360°C while continuously changing the discharge rate from 236 g / min to 41 g / min, and the hot air pressure at a temperature of 400°C was continuously changed from 11.9 kPa to 32.3 kPa. After maintaining constant conditions for a while, the extrusion was continued while continuously changing the discharge rate from 41 g / min to 236 g / min, and the hot air pressure at a temperature of 400°C was continuously changed from 11.9 kPa to 32.3 kPa to perform spinning, and the resulting mixture was blown onto a conveyor net equipped with a suction device and taken up around a paper tube roll at 9 m / min to obtain nonwoven fabric 5 having a continuous fiber diameter gradient. The obtained nonwoven fabric 5 has an average fiber diameter that continuously changes from 8.8 μm to 0.64 μm and an average basis weight of 54.7 g / m 2 to 17.3 g / m 2 and a portion (corresponding to the outer layer nonwoven fabric) in which the average fiber diameter is 0.64 μm and the average basis weight is 17.3 g / m. 2 and a portion in which the average fiber diameter continuously changes from 0.64 μm to 8.8 μm and the average basis weight is 17.3 g / m. 2 to 54.7 g / m 2 The nonwoven fabric was composed of a portion (corresponding to the nonwoven fabric for the support layer) in which the thickness of the nonwoven fabric changed continuously.

[0080] <Production of Depth Filter> A cylindrical molded article was obtained in the same manner as in Example 4, except that nonwoven fabric 5 was used instead of nonwoven fabric 4, and laminate for a microfiltration layer 5 was used instead of laminate for a microfiltration layer 4. The obtained cylindrical molded article had, from the outside, an outer layer, a prefiltration layer, a microfiltration layer, and a support layer in that order, and in the outer layer, the nonwoven fabric on the most upstream side in the filtration direction had an average fiber diameter of 8.8 μm and an average basis weight of 54.7 g / m 2 The average fiber diameter of the nonwoven fabric on the most downstream side is 0.64 μm and the average basis weight is 17.3 g / m2 The prefiltration layer was a layer formed by winding a laminate of a melt-blown nonwoven fabric (corresponding to the first prefiltration layer nonwoven fabric) having an average fiber diameter of 0.64 μm and a prefiltration layer nonwoven fabric 2 (corresponding to the second prefiltration layer nonwoven fabric), the microfiltration layer was a layer formed by winding a laminate of a melt-blown nonwoven fabric (corresponding to the substrate) having an average fiber diameter of 0.64 μm and a microfiltration layer laminate 5, and the support layer had an average fiber diameter that continuously increased from 0.64 μm to 8.8 μm in the filtration direction and an average basis weight of 17.3 g / m 2 to 54.7 g / m 2 The thickness of the layers increased continuously. Except for this, a depth filter was produced in the same manner as in Example 1. The outer layer nonwoven fabric and the prefiltration layer nonwoven fabric were bonded between the wound nonwoven fabrics, and the outer layer and the prefiltration layer were bonded to each other.

[0081] Comparative Example 1 Production of Nonwoven Fabric 6 Having a Continuous Fiber Diameter Gradient Using the same resin and melt-blowing spinneret as in Example 2, a high-melting point resin and a low-melting point resin (weight ratio 5:5) were extruded at a spinning temperature of 360°C while the output rate was continuously changed from 120 g / min to 20 g / min, and the hot air pressure at a temperature of 400°C was continuously changed from 10 kPa to 99 kPa. Immediately after that, the extrusion was continued while the output rate was continuously changed from 20 g / min to 120 g / min, and the hot air pressure at a temperature of 400°C was continuously changed from 99 kPa to 10 kPa, thereby spinning the extruded material. The extruded material was then blown onto a conveyor net equipped with a suction device and taken up around a paper tube roll at 9 m / min, thereby obtaining nonwoven fabric 6 having a continuous fiber diameter gradient. The obtained nonwoven fabric 6 has an average fiber diameter that continuously changes from 24 μm to 1.37 μm and an average basis weight of 47.7 g / m 2 to 10.7 g / m 2 and a portion in which the average fiber diameter continuously changes from 1.37 μm to 24 μm and the average basis weight is 10.7 g / m. 2 to 47.7 g / m 2 The nonwoven fabric was composed of a portion (corresponding to the nonwoven fabric for the support layer) in which the thickness changed continuously, and there was no portion corresponding to the nonwoven fabric for the pre-filtration layer.

[0082] <Production of Depth Filter> A nonwoven fabric 6 having a continuous fiber diameter gradient was heated in a through-air processing machine at a conveyor speed of 8.5 m / min and a set temperature of 131°C, and immediately thereafter wound around a core material having an outer diameter of 30 mm to obtain a cylindrical molded article. The obtained cylindrical molded article had, from the outside, an outer layer and a support layer in that order. In the outer layer, the nonwoven fabric on the most upstream side in the filtration direction had an average fiber diameter of 24 μm and an average basis weight of 47.7 g / m 2 The average fiber diameter of the nonwoven fabric on the most downstream side is 1.37 μm and the average basis weight is 10.7 g / m 2 In addition, the support layer had an average fiber diameter that continuously increased from 1.37 μm to 24 μm in the filtration direction, and an average basis weight of 10.7 g / m 2 to 47.7 g / m 2 The thickness of the layer was increased continuously. Then, in the same manner as in Example 1, a depth filter was prepared.

[0083] [Comparative Example 2] <Production of Laminate 6 for Microfiltration Layer> A polyvinylidene fluoride copolymer resin (product name: Kynar 3120-50) manufactured by Arkema was dissolved at a concentration of 18 wt% in a cosolvent of N,N-dimethylformamide and acetone (60 / 40 (w / w)) to prepare an electrospinning solution. The obtained spinning solution was electrospun using a multi-hole spinneret having eight nozzle holes with an inner diameter of 0.3 mm under the conditions of a solution supply rate of 3.0 mL / h to each nozzle hole, an applied voltage of 45.0 kV, and a spinning distance of 12.5 cm. On the collector electrode, a through-air nonwoven fabric (basis weight: 40 g / m) made of 3 dtex / f heat-fusible composite fiber (sheath / core = high-density polyethylene / polypropylene, sheath / core ratio 50 / 50% by volume) was placed. 2 ) was placed as a substrate, and the electrospun nonwoven fabric for the microfiltration layer was placed on the substrate at a density of 1.5 g / m 2 The nonwoven fabric for the microfiltration layer had an average fiber diameter of 230 nm and a CV value of the fiber diameter of 0.49.

[0084] <Production of Nonwoven Fabric 7> Using the same resin and melt-blowing spinneret as in Example 2, a high-melting point resin and a low-melting point resin (weight ratio 5:5) were extruded at a spinning temperature of 340°C at a discharge rate of 240 g / min while maintaining a constant hot air pressure of 400°C at 30.7 kPa to perform spinning, which was then blown onto a conveyor net equipped with a suction device and taken up on a paper tube roll at 9 m / min to obtain nonwoven fabric 7. The obtained nonwoven fabric 7 did not have a fiber diameter gradient or basis weight gradient, and had an average fiber diameter of 5 μm and an average basis weight of 25 g / m 2 It was.

[0085] <Production of Depth Filter> Nonwoven fabric 7 was heated in a through-air processing machine under conditions of a conveyor speed of 8.5 m / min and a set temperature of 131 ° C., and immediately thereafter wound around a core material with an outer diameter of 30 mm to obtain a cylindrical molded product. At this time, a 0.8 m long microfiltration layer laminate 6 was inserted during winding, and even after insertion, the nonwoven fabric 7 was continued to be wound. The obtained cylindrical molded product had, from the outside, a layer wound with nonwoven fabric 7, a layer wound with a laminate of nonwoven fabric 7 and nonwoven fabric 6 for microfiltration layer, and a layer wound with nonwoven fabric 7, in that order. Next, a depth filter was produced in the same manner as in Example 1.

[0086] [Comparative Example 3] <Production of laminate 7 for microfiltration layer> The basis weight of the nonwoven fabric for the microfiltration layer was 3.0 g / m 2 Except for this, laminate 7 for a microfiltration layer was produced in the same manner as in Comparative Example 1. The obtained laminate 7 for a microfiltration layer had good formation, with no peeling or wrinkling of the nonwoven fabric for the microfiltration layer being observed. The nonwoven fabric for the microfiltration layer had an average fiber diameter of 230 nm and a CV value of the fiber diameter of 0.49.

[0087] <Production of Depth Filter> A depth filter was obtained in the same manner as in Comparative Example 2, except that the laminate 7 for a microfiltration layer was used instead of the laminate 6 for a microfiltration layer.

[0088] Comparative Example 4 A Profile Nano manufactured by Nippon Pall was used.

[0089] The results of the water permeability, filtration performance, and gel capture performance of Examples 1 to 5 and Comparative Examples 1 to 4 are shown in Tables 1, 2, and 3, respectively.

[0090]

[0091]

[0092]

[0093] These results demonstrate that the depth filter of the present invention has a very high collection efficiency and is stable even under high pressure. Furthermore, it exhibited high capture performance even for gels that are difficult to capture. On the other hand, Comparative Example 1 did not have layers corresponding to the prefiltration layer and microfiltration layer, resulting in low collection efficiency. Comparative Example 2 had a high collection efficiency, but its collection efficiency rapidly decreased under high pressure. This is believed to be due to the lack of a continuous fiber diameter gradient upstream of the microfiltration layer, which weakens the strength of the filter itself, or to silica particles being concentrated in the microfiltration layer and pushed out by high pressure. In Comparative Example 3, attempts to wet the filter under high pressure were made, but no water could pass through. This is believed to be due to the dense pore structure of the hydrophobic polyvinylidene fluoride copolymer resin. The fact that the depth filter does not wet with water under high pressure is expected to make it difficult to use in practical manufacturing processes. Comparative Example 4 had a very high collection efficiency, but silica microparticles leaked under high pressure. This phenomenon is something that should be avoided in the polishing process of semiconductor materials, where reliable filtration is required. In contrast, the depth filters of Examples 1 to 5 can maintain a stable, high collection efficiency even under high pressure, making them ideal for various filtration situations, particularly processes where filtration reliability is important, such as semiconductor polishing processes. Furthermore, despite their high collection efficiency, they also have excellent water permeability, making them easy to handle for manufacturers.

[0094] The depth filter of the present invention has absolute filtration performance and gel removal performance even for small particles to be removed, excellent liquid permeability, and excellent stability of capture performance under high pressure, and therefore can be suitably used in applications such as the production process of CMP slurry and the production process of multilayer ceramic capacitors.

Claims

1. A depth filter having an outer layer, a pre-filtration layer, and a microfiltration layer arranged in this order in the filtration direction, wherein the outer layer is a layer in which an outer layer nonwoven fabric containing a high melting point resin and a low melting point resin is wound in multiple layers, the wound nonwoven fabrics are thermally bonded with the low melting point resin, and the average fiber diameter is continuously reduced in the filtration direction, the microfiltration layer is a layer in which a microfiltration layer nonwoven fabric is wound in multiple layers, and the average fiber diameter of the fibers constituting the microfiltration layer nonwoven fabric is less than 300 nm, and the pre-filtration layer is a layer in which a pre-filtration layer nonwoven fabric is wound in multiple layers, and the average fiber diameter is constant or gradually reduced in the filtration direction, and the average fiber diameter of the fibers constituting the pre-filtration layer nonwoven fabric is 300 nm or more and less than 1000 nm.

2. The depth filter according to claim 1, wherein the outer layer is a layer configured so that the average basis weight of the outer layer nonwoven fabric continuously decreases in the filtration direction.

3. A depth filter according to claim 1 or 2, wherein the average fiber diameter on the most upstream side of the outer layer is 5 to 50 μm, and the ratio of the average fiber diameters on the most upstream side to the most downstream side is 5 or more.

4. The depth filter of claim 1 or 2, wherein the prefiltration layer comprises polypropylene having a melt flow rate of 500 g / 10 min or more and a melting point of 160° C. or more.

5. The depth filter of claim 4, wherein the polypropylene is a metallocene-catalyzed polypropylene.

6. The depth filter according to claim 1 or 2, wherein the fibers constituting the nonwoven fabric for the microfiltration layer are made of a polyamide resin.

7. A depth filter according to claim 1 or 2, wherein the microfiltration layer is a layer in which a laminate of at least one substrate and the nonwoven fabric for the microfiltration layer is wound in multiple layers.

8. The depth filter according to claim 7, wherein the fibers constituting the substrate and the nonwoven fabric for the microfiltration layer are made of a polyamide resin.

Citation Information

Patent Citations

  • High-precision filter

    WO1998013123A1

  • Blended ultra-fine fiber good and its production

    JP1995082649A

  • Depth type filter

    JP1999156125A

  • Nonwoven fabric and filtering material used for air filter which uses the same