Shrink label

The shrink label design, with a heat-shrinkable base and water-based ink layer that maintains high initial contact angles and controlled decrease, addresses attachment issues on wet plastic containers by optimizing contact and friction, ensuring reliable attachment.

WO2024202382A1PCT designated stage expired Publication Date: 2024-10-03FUJI SEAL INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/000545
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-01-12
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Shrink labels with water-based ink layers face attachment issues on plastic containers, particularly when the surface is wet, due to slippage caused by low contact angles, leading to poor attachment and installation errors.

Method used

A shrink label design featuring a heat-shrinkable base material with a water-based ink layer that maintains a contact angle of 90° or more initially and decreases by 20% or less within 90 seconds, combined with a color ink layer, to enhance attachment by adjusting the ink composition and friction coefficients.

Benefits of technology

The solution effectively suppresses the occurrence of poor attachment to plastic containers by maintaining adequate contact and friction properties, ensuring reliable label placement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024000545_03102024_PF_FP_ABST
    Figure JP2024000545_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a shrink label that enables incidence of mis-fitting onto a plastic container to be controlled to a minimum. A shrink label (10) comprises: a heat-shrinkable base material (1); and an aqueous ink layer (3) over the base material (1). The contact angle of water droplets on the surface of the aqueous ink layer (3) one second after 2 μL of water has been dripped onto the surface of the aqueous ink layer (3) exceeds 90°. The rate of decrease in the contact angle of water droplets on the surface of the aqueous ink layer (3) from one second after to 90 seconds after 2 μL of water has been dripped is 20% or less of the contact angle of water droplets on the surface of the aqueous ink layer (3) one second after 2 μL of water has been dripped.
Need to check novelty before this filing date? Find Prior Art

Description

Shrink Label

[0001] The present disclosure relates to shrink labels.

[0002] In recent years, plastic containers such as polyethylene terephthalate (PET) bottles have come to be used for a variety of products. A shrink label having a printing layer for displaying product information and the like is generally attached to the body of the plastic container.

[0003] For example, Patent Document 1 describes a heat-shrinkable tubular label to be attached to the body of a container, in which a water-repellent overcoat layer printed with water-repellent ink is provided on the surface of the heat-shrinkable tubular label, and a water-repellent inner coat layer printed with water-repellent ink is provided on the back surface of the heat-shrinkable tubular label at least near the upper and lower ends, and the contact angle of the surface of the heat-shrinkable tubular label with pure water is 100° or more, and the contact angle of the surface of the back surface of the heat-shrinkable tubular label where the water-repellent inner coat layer is provided is 90° or more.

[0004] Japanese Patent Application Laid-Open No. 2020-203695

[0005] In recent years, with growing environmental awareness, there has been an increasing trend to use water-based inks, which use aqueous solvents, instead of oil-based inks, which use organic solvents, when printing shrink labels, in order to reduce the emission of VOCs (volatile organic compounds).

[0006] However, when the innermost surface of a shrink label made of a heat-shrinkable tubular film as described in Patent Document 1 contains an aqueous ink layer formed using an aqueous ink, the shrink label can sometimes be poorly attached to a plastic container. In particular, when the shrink label is attached to a plastic container surface that is wet with water, the shrink label loses its sliding properties relative to the plastic container, often resulting in poor attachment of the shrink label to the plastic container.

[0007] According to the embodiment disclosed herein, it is possible to provide a shrink label comprising a heat-shrinkable substrate and an aqueous ink layer on the substrate, in which the contact angle of a water droplet on the surface of the aqueous ink layer exceeds 90° one second after 2 μL of water is dropped onto the surface of the aqueous ink layer, and the rate of decrease in the contact angle of the water droplet on the surface of the aqueous ink layer from one second to 90 seconds after 2 μL of water is 20% or less of the contact angle of the water droplet on the surface of the aqueous ink layer one second after 2 μL of water is dropped.

[0008] According to the embodiments disclosed herein, it is possible to provide a shrink label that can prevent improper attachment to a plastic container.

[0009] FIG. 1 is a schematic cross-sectional view of an example of a shrink label according to an embodiment. FIG. 2 is a schematic perspective view of an example of a tubular shrink label according to an embodiment. FIG. 3 is a schematic perspective view showing an example of attaching the tubular shrink label shown in FIG. 2 to a plastic container. FIG. 4 is a schematic plan view of a test piece used for measuring the static and dynamic friction coefficients of a shrink label according to an embodiment. FIG. 5 is a schematic plan view of a mating material used for measuring the static and dynamic friction coefficients of a shrink label according to an embodiment. FIG. 6 is a schematic side view of a tensile tester used for measuring the static and dynamic friction coefficients of a shrink label according to an embodiment. FIG. 7 is a schematic plan view illustrating a method for measuring the static and dynamic friction coefficients of a shrink label according to an embodiment.

[0010] Hereinafter, embodiments will be described. In the drawings used to describe the embodiments, the same reference numerals denote the same or corresponding parts.

[0011] <Shrink Label> Figure 1 shows a schematic cross-sectional view of an example of a shrink label according to an embodiment. The shrink label 10 shown in Figure 1 comprises a substrate 1 and an aqueous ink layer 3 on the substrate 1. A color ink layer 2 is positioned between the substrate 1 and the aqueous ink layer 3.

[0012] <Heat-shrinkable substrate> The heat-shrinkable substrate 1 (hereinafter referred to as "substrate 1") is capable of supporting at least the water-based ink layer 3 and contains a resin that can shrink when heated. When the substrate 1 is immersed in hot water at 90°C for 10 seconds, the heat shrinkage rate of the substrate 1 in the main shrinkage direction is, for example, 30% or more, and preferably 50% or more.

[0013] The resin contained in the substrate 1 may be, for example, a thermoplastic resin. The resin contained in the substrate 1 may be, for example, a polyester (PET)-based resin, a polypropylene-based resin, a polystyrene (PS)-based resin, or a polyethylene-based resin. The substrate 1 may be, for example, composed of a single layer containing one or more of the above-mentioned resins, or may be composed of multiple layers in which multiple such single layers are laminated.

[0014] <Water-based ink layer> The water-based ink layer 3 is a layer formed by drying the water-based ink on the substrate 1. The water-based ink used to form the water-based ink layer 3 may be, for example, a water-based ink containing an aqueous solvent such as water or an alcohol aqueous solution, a resin, and a curing agent.

[0015] Examples of the resin contained in the aqueous ink used to form the aqueous ink layer 3 include acrylic resins, urethane resins, polyester resins, polyamide resins, cellulose resins, vinyl chloride resins, vinyl acetate resins, polyolefin resins (such as polyethylene resins or polybutadiene resins), isocyanate resins, rosin resins, polyvinyl alcohol resins (PVA resins), and imine resins, with acrylic resins being preferred. Furthermore, examples of the resin contained in the aqueous ink used to form the aqueous ink layer 3 include thermoplastic resins.

[0016] When an acrylic resin is used as the resin contained in the aqueous ink used to form the aqueous ink layer 3, for example, an aqueous acrylic ink containing an aqueous solvent, an acrylic resin, and a curing agent can be used as the aqueous acrylic ink used to form the aqueous ink layer 3. For example, a water-soluble aqueous acrylic ink in which an acrylic resin is dissolved in an aqueous solvent, or an emulsion-type aqueous acrylic ink in which an acrylic resin is dispersed in an aqueous solvent can be used as the aqueous acrylic ink.

[0017] The acrylic resin contained in the aqueous acrylic ink used to form the aqueous ink layer 3 may be, for example, a polymer composed of at least an acrylic monomer as a monomer component, and preferably an acrylic thermoplastic resin. The monomer components constituting the acrylic resin may include monomer components other than the acrylic monomer.

[0018] Examples of the acrylic monomer include alkyl (meth)acrylates having a linear or branched alkyl group, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, and dodecyl (meth)acrylate [preferably (meth)acrylic acid C 1-12 alkyl esters, etc.]; (meth)acrylic acid; carboxy group-containing (meth)acrylic acid esters such as carboxyethyl acrylate; hydroxy group-containing (meth)acrylic acid esters such as hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, diethylene glycol mono(meth)acrylate, and dipropylene glycol mono(meth)acrylate [preferably (meth)acrylic acid hydroxy C 1-8(meth)acrylic acid cycloalkyl esters such as cyclohexyl (meth)acrylate and isobornyl (meth)acrylate; (meth)acrylic acid amide derivatives such as N-methylol (meth)acrylamide, N-butoxymethyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, and N,N-diethyl (meth)acrylamide; and (meth)acrylic acid dialkylaminoalkyl esters such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dipropylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, and dipropylaminopropyl (meth)acrylate. The acrylic monomers may be used alone or in combination of two or more.

[0019] Examples of monomer components constituting the acrylic resin other than the acrylic monomer include carboxyl group-containing polymerizable unsaturated compounds or anhydrides thereof, such as crotonic acid, itaconic acid, fumaric acid, and maleic acid; styrene compounds, such as styrene, vinyl toluene, and α-methylstyrene; vinyl esters, such as vinyl acetate and vinyl propionate; vinyl halides, such as vinyl chloride; vinyl ethers, such as methyl vinyl ether; cyano group-containing vinyl compounds, such as (meth)acrylonitrile; ethylene or propylene.

[0020] The curing agent contained in the water-based ink used to form the water-based ink layer 3 can be, for example, a curing agent corresponding to the resin contained in the water-based ink layer 3. For example, if the resin contained in the water-based ink layer 3 has a hydroxyl group or an amino group, an isocyanate-based curing agent can be used as the curing agent. Furthermore, if the resin contained in the water-based ink layer 3 has an amino group or a carbonyl group, an epoxy-based curing agent can be used as the curing agent. Furthermore, if the resin contained in the water-based ink layer 3 has a carbonyl group, a carbodiimide-based curing agent, an aziridine-based curing agent, or a hydrazide-based curing agent can be used as the curing agent. The content of the curing agent can be, for example, 0.5% by weight or more and 15% by weight or less of the total water-based ink layer 3.

[0021] For example, an aziridine-based, metal chelate-based, carbodiimide-based, or epoxy-based curing agent can be used as the curing agent when using an aqueous acrylic ink to form the aqueous ink layer 3. The content of the curing agent in the aqueous acrylic ink used to form the aqueous ink layer 3 is preferably 1% by weight or more and 10% by weight or less of the entire aqueous ink layer 3, from the viewpoint of preventing poor installation on a plastic container.

[0022] The water-based ink layer 3 may be a white ink layer, for example, by adding a white pigment to the water-based ink used to form the water-based ink layer 3. Titanium oxide, for example, can be used as the white pigment added to the water-based ink used to form the water-based ink layer 3. When titanium oxide is added to the water-based ink used to form the water-based ink layer 3, the titanium oxide may account for, for example, 50% by weight or more and 90% by weight or less of the total water-based ink layer 3.

[0023] The water-based ink layer 3 may be a transparent ink layer (medium), for example, by not including a coloring pigment in the water-based ink used to form the water-based ink layer 3. In this case, the water-based ink used to form the water-based ink layer 3 may contain 1% by weight or more and 15% by weight or less of a lubricant based on the entire water-based ink layer 3.

[0024] <Color Ink Layer> The color ink layer 2 is a layer formed by drying color inks printed on the substrate 1. The color ink layer 2 may contain, for example, different color pigments. By containing different color pigments, multiple color ink layers 2 of different colors can be provided in a predetermined region of the substrate 1. This allows for the provision of a single-layer color ink layer 2 region or a multi-layer color ink layer 2 region in which color ink layers 2 are stacked, allowing for the formation of predetermined designs or characters. The one or more color inks printed on the substrate 1 and used to form the color ink layer 2 can be, for example, aqueous color inks containing an aqueous solvent such as water or an alcohol aqueous solution (in the case of an emulsion, an aqueous dispersion medium may be used; the same applies hereinafter), a resin, an additive, a color pigment, etc. Resins that can be used to form the color ink layer 2 include, for example, acrylic resins, urethane resins, polyester resins, polyamide resins, cellulose resins, vinyl chloride resins, vinyl acetate resins, polyolefin resins (such as polyethylene resins or polybutadiene resins), isocyanate resins, rosin resins, polyvinyl alcohol resins (PVA resins), and imine resins. From the viewpoints of thermal shrinkage compliance and ink crack prevention, the one or more color inks used to form the color ink layer 2 preferably contain a thermoplastic resin as a resin component, more preferably an acrylic thermoplastic resin or a urethane thermoplastic resin, and even more preferably a urethane thermoplastic resin.

[0025] When a urethane-based resin is used as the resin contained in the aqueous ink used to form the aqueous ink layer 3, the urethane-based resin contained in the aqueous ink used to form the aqueous ink layer 3 may be, for example, a resin obtained by reacting a polyisocyanate compound with a polyol compound (i.e., a copolymer of a polyisocyanate compound and a polyol compound).

[0026] The polyisocyanate compound may be, for example, one or a mixture of two or more known aromatic, aliphatic, and alicyclic diisocyanates, such as tolylene diisocyanate, 4,4-diphenylmethane diisocyanate, 1,3-phenylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, 1,5-naphthalene diisocyanate, or isophorone diisocyanate.

[0027] Examples of polyol compounds that can be used include low-molecular-weight glycols such as ethylene glycol, diethylene glycol, 1,3-propanediol, propylene glycol (1,2-propanediol), butanediol (1,3-butanediol, 1,4-butanediol, etc.), 1,6-hexanediol, and cyclohexanedimethanol; polyether diols such as polyethylene glycol, polypropylene glycol, polytetramethylene glycol, and polytetramethylene glycol-polycaprolactone copolymer; polyester diols obtained from diols such as propylene glycol, butanediol, and hexanediol and dibasic acids such as adipic acid, sebacic acid, azelaic acid, isophthalic acid, terephthalic acid, and fumaric acid; and diols such as lactone diols such as polycaprolactone diol, polyvalerolactone diol, and lactone block copolymer diol.

[0028] <Effects of the Shrink Label> In the shrink label 10, (i) the contact angle of a water droplet on the surface of the water-based ink layer 3 one second after 2 μL of water is deposited on the surface of the water-based ink layer 3 exceeds 90°, and (ii) the rate of decrease in the contact angle of a water droplet on the surface of the water-based ink layer 3 one second after 90 seconds from one second after the 2 μL of water is no more than 20% of the contact angle of a water droplet on the surface of the water-based ink layer 3 one second after the 2 μL of water is deposited. This was achieved through extensive research by the inventors, who discovered that when the shrink label 10 satisfies the above conditions (i) and (ii), poor attachment of the shrink label 10 to a plastic container can be reduced.

[0029] <Method for measuring the contact angle of a water droplet on the surface of the aqueous ink layer of a shrink label> The contact angle (°) of a water droplet on the surface of the aqueous ink layer 3 of the shrink label 10 is the average value of n5 contact angles measured using the following conditions and method in accordance with JIS K 6768. Measuring device: PCA-11 manufactured by Kyowa Interface Science Co., Ltd. Measurement method: Sessile drop method (sessile drop method) Analysis method: θ / 2 method Droplet volume: 2 μL Liquid: Distilled water

[0030] <Reduction in the Contact Angle of a Water Droplet on the Surface of the Water-Based Ink Layer of a Shrink Label> The reduction in the contact angle of a water droplet on the surface of the water-based ink layer 3 of a shrink label 10 between 1 second and 90 seconds after 2 μL of water is dropped is calculated using the following formula (I): Reduction in Contact Angle (%) = [1 - {(Contact angle (°) of a water droplet on the surface of the water-based ink layer 3 90 seconds after 2 μL of water is dropped) / (Contact angle (°) of a water droplet on the surface of the water-based ink layer 3 1 second after 2 μL of water is dropped)}] × 100 (I)

[0031] From the perspective of improving the ease with which the shrink label 10 can be attached to plastic containers, it is preferable that the rate of decrease in the contact angle of a water droplet on the surface of the water-based ink layer 3 of the shrink label 10 between 1 second and 10 seconds after 2 μL of water is dropped is 5% or less compared to the contact angle of the water droplet on the surface of the water-based ink layer 3 1 second after 2 μL of water is dropped; it is more preferable that the rate of decrease in the contact angle of a water droplet on the surface of the water-based ink layer 3 of the shrink label 10 between 1 second and 30 seconds after 2 μL of water is 10% or less compared to the contact angle of the water droplet on the surface of the water-based ink layer 3 1 second after 2 μL of water is dropped; and it is even more preferable that the rate of decrease in the contact angle of a water droplet on the surface of the water-based ink layer 3 of the shrink label 10 between 1 second and 60 seconds after 2 μL of water is 10% or less compared to the contact angle of the water droplet on the surface of the water-based ink layer 3 1 second after 2 μL of water is dropped.

[0032] The rate of decrease in the contact angle of a water droplet on the surface of the water-based ink layer 3 of the shrink label 10 between 1 second and 10 seconds after 2 μL of water is dropped is calculated using the following formula (II): Rate of decrease in contact angle (%) = [1 - {(contact angle (°) of the water droplet on the surface of the water-based ink layer 3 10 seconds after 2 μL of water is dropped) / (contact angle (°) of the water droplet on the surface of the water-based ink layer 3 1 second after 2 μL of water is dropped)}] × 100 (II)

[0033] The rate of decrease in the contact angle of a water droplet on the surface of the water-based ink layer 3 of the shrink label 10 between 1 second and 30 seconds after 2 μL of water is dropped is calculated using the following formula (III): Rate of decrease in contact angle (%) = [1 - {(contact angle (°) of the water droplet on the surface of the water-based ink layer 3 30 seconds after 2 μL of water is dropped) / (contact angle (°) of the water droplet on the surface of the water-based ink layer 3 1 second after 2 μL of water is dropped)}] × 100 (III)

[0034] The rate of decrease in the contact angle of a water droplet on the surface of the water-based ink layer 3 of the shrink label 10 between 1 second and 60 seconds after 2 μL of water is dropped is calculated using the following formula (IV): Rate of decrease in contact angle (%) = [1 - {(contact angle (°) of the water droplet on the surface of the water-based ink layer 3 60 seconds after 2 μL of water is dropped) / (contact angle (°) of the water droplet on the surface of the water-based ink layer 3 1 second after 2 μL of water is dropped)}] × 100 (IV).

[0035] <Label Manufacturing Method> The shrink label 10 shown in Figure 1 can be manufactured, for example, as follows. First, a step is carried out to form a color ink layer 2 on a substrate 1. This step can be carried out, for example, by printing the color inks used to form the color ink layer 2 on the surface of the substrate 1 by flexographic printing, gravure printing, or the like, and then drying the color inks.

[0036] Next, the step of forming the aqueous ink layer 3 on the color ink layer 2 is carried out. This step can be carried out, for example, by printing the aqueous ink used to form the aqueous ink layer 3 on the surface of the color ink layer 2 by flexographic printing, gravure printing, or the like, and then drying the aqueous ink. The aqueous ink layer 3 is formed by adjusting the aqueous ink so that at least (i) the contact angle of a water droplet on the surface of the aqueous ink layer 3 one second after 2 μL of water is dropped onto the surface of the aqueous ink layer 3 exceeds 90°, and (ii) the rate of decrease in the contact angle of a water droplet on the surface of the aqueous ink layer 3 from one second to 90 seconds after the 2 μL of water is 20% or less of the contact angle of a water droplet on the surface of the aqueous ink layer 3 one second after the 2 μL of water is dropped. The above steps make it possible to manufacture the shrink label 10.

[0037] The shrink label 10 may be cylindrical, as shown in the schematic perspective view of FIG. 2 . The innermost layer of the cylindrical shrink label 10 may be composed of an aqueous ink layer 3, and the outermost layer may be composed of a substrate 1. In this case, as shown in the schematic perspective view of FIG. 3 , the cylindrical shrink label 10 can be attached to a plastic container 20 (e.g., a PET bottle container) so that the aqueous ink layer 3, which is the innermost layer of the cylindrical shrink label 10, contacts the surface of the plastic container 20 wet with water. The cylindrical shrink label 10 can be formed, for example, by forming the aqueous ink layer 3 on the color ink layer 2 as described above, overlapping both ends of the substrate 1 to form a cylindrical shape so that the aqueous ink layer 3 faces the inner peripheral surface of the cylindrical shrink label 10, and then bonding the overlapped regions of both ends of the substrate 1 with, for example, a solvent or adhesive. The outermost layer of the shrink label 10 may also include a printed layer (a surface medium layer or a matte varnish layer). The surface medium layer is provided, for example, to protect the shrink label 10. The matte varnish layer is provided, for example, to provide a matte finish.

[0038] <Dynamic Friction Coefficient of Water-Based Ink Layer Against Polyester Surface with 0.1 mL and 0.01 mL Water Droplets> From the perspective of improving the fit of the shrink label 10 to plastic containers, the dynamic friction coefficient of the water-based ink layer 3 of the shrink label 10 against a polyester surface with 0.1 mL of water droplets is preferably 1.0 or less, more preferably 0.6 or less, and even more preferably 0.1 to 0.5.

[0039] From the viewpoint of improving the fit of the shrink label 10 to plastic containers, the coefficient of dynamic friction of the aqueous ink layer 3 of the shrink label 10 against a polyester surface having a 0.01 mL water droplet thereon is preferably 2.5 or less, more preferably 2.0 or less, even more preferably less than 1.5, and particularly preferably 0.1 or more but less than 1.5.

[0040] <Static friction coefficient of water-based ink layer against polyester surface with 0.1 mL and 0.01 mL water droplets>

[0041] To prevent poor attachment of the shrink label 10 to a plastic container, the static friction coefficient of the water-based ink layer 3 of the shrink label 10 against a polyester surface having a 0.1 mL water droplet is preferably 0.6 or less, and more preferably 0.1 to 0.5. To prevent poor attachment of the shrink label 10 to a plastic container, the static friction coefficient of the water-based ink layer 3 of the shrink label 10 against a polyester surface having a 0.01 mL water droplet is preferably 0.6 or less, and more preferably 0.1 to 0.5.

[0042] <Dynamic friction coefficient of the water-based ink layer against the polyester surface in a dry state without water droplets (hereinafter referred to as "dry state")> From the perspective of preventing poor attachment of the shrink label 10 to a plastic container, the dynamic friction coefficient of the water-based ink layer 3 of the shrink label 10 against the polyester surface in a dry state is preferably 0.6 or less, and more preferably 0.1 or more and 0.5 or less.

[0043] <Static friction coefficient of the aqueous ink layer against the polyester surface when dry> From the perspective of preventing poor attachment of the shrink label 10 to a plastic container, the static friction coefficient of the aqueous ink layer 3 of the shrink label 10 against the polyester surface when dry is preferably 0.6 or less, and more preferably 0.1 or more and 0.5 or less.

[0044] <Measurement of static and dynamic friction coefficients> The methods for measuring the static and dynamic friction coefficients of the water-based ink layer 3 of the shrink label 10 against a polyester surface having a 0.1 mL water droplet, and the methods for measuring the static and dynamic friction coefficients of the water-based ink layer 3 of the shrink label 10 against a polyester surface having a 0.01 mL water droplet, are as follows.

[0045] First, a rectangular shrink label 10 is prepared as shown in the schematic plan view of Fig. 4. The rectangular shrink label 10 shown in Fig. 4 has a width of 100 mm in the machine direction (MD) and a width of 80 mm in the transverse direction (TD).

[0046] Also, a polyester film ("E5100" manufactured by Toyobo Co., Ltd., thickness 100 μm) having a rectangular untreated polyester surface 11 shown in the schematic plan view of Fig. 5 is prepared. The rectangular polyester film shown in Fig. 5 has a width of 300 mm in the MD direction and a width of 100 mm in the TD direction.

[0047] Next, a tensile tester 15 as shown in the schematic side view of FIG. 6 is prepared. The tensile tester 15 is a tensile tester (AGS-50G) manufactured by Shimadzu Corporation or a similar tensile tester capable of performing measurements. The tensile tester 15 includes a wire 12, a load cell 13, a horizontally installed test stand 14, and a pulley 16 located above the test stand 14. The test stand 14 is made of a non-magnetic metal to prevent the effects of static electricity. The pulley 16 can rotate smoothly and is installed at a height and position where the wire 12 and the surface of the test stand 14 are parallel.

[0048] Next, as shown in Figure 7, the polyester film is placed on a test stand 14 without wrinkles, with the polyester surface 11 facing upward. Next, a 0.1 mL or 0.01 mL droplet of tap water is placed on the polyester surface 11. The droplet is placed at a single location on the polyester surface 11 that corresponds to the center of the shrink label 10 that will be placed on the polyester surface 11.

[0049] Next, a weight 17 is prepared, having a square base measuring 63 mm x 63 mm and a mass of 200 g ± 2 g (1.96 N ± 0.02 N). The top surface of the substrate 1 of the shrink label 10 is attached to the bottom surface of the weight 17 so as to prevent wrinkles from forming in the shrink label 10. The shrink label 10 is attached so that the center of the bottom surface of the weight 17 is aligned with the center of the top surface of the substrate 1 of the shrink label 10.

[0050] Next, the shrink label 10 is attached to one end of the wire 12 connected to the load cell 13. The wire 12 is not taut, but is left with a little slack.

[0051] Next, the shrink label 10 attached to the bottom surface of the weight 17 is gently placed so that the water droplet on the polyester surface 11 contacts the center of the surface of the water-based ink layer 3 of the shrink label 10 and so that the surface of the water-based ink layer 3 is parallel to the surface of the test bench 14.

[0052] Next, as shown in FIG. 7 , the load cell 13 pulls the wire 12 via the pulley 16 in the direction of arrow 18, parallel to the surface of the test table 14, at a speed of 100 mm / min for a distance of 85 mm, thereby measuring the static and kinetic frictional forces of the water-based ink layer 3 against the polyester surface having a 0.1 mL or 0.01 mL water droplet. Here, the kinetic frictional force of the outer layer against the polyester surface having a 0.1 mL or 0.01 mL water droplet is taken as the average value over a distance of 10 mm to 85 mm. The static and kinetic frictional forces are then calculated from the measured static and kinetic frictional forces, respectively. The measurement conditions for the static and kinetic frictional forces are based on JIS K 7125:1999. The temperature and humidity for measuring the static friction force and dynamic friction force are based on JIS K 7100 standard temperature condition class 2 (temperature: 23±2° C., relative humidity: 50±10%).

[0053] The static and dynamic friction coefficients of the water-based ink layer 3 of the shrink label 10 against the polyester surface in the dry state were measured in the same manner as above, except that no water droplets were dropped onto the polyester surface 11.

[0054] <Preparation of Shrink Label for Experimental Example 1> For the shrink label for Experimental Example 1, a shrink label 10 having the cross-sectional configuration shown in Figure 1 was prepared. First, a substrate 1 was made of a 40 μm-thick multilayer shrink film (surface layer: PET-based resin / center layer: PS-based resin / back layer: PET-based resin, manufactured by Gunze Co., Ltd.). A water-based flexographic ink (Hydric FCF series) containing a urethane thermoplastic resin containing a colored pigment, manufactured by Dainichiseika Chemicals, was printed on one surface of the substrate and dried twice to form a color ink layer 2 (0.6 μm thick) by flexographic printing. Next, a water-based acrylic white ink for forming water-based ink layer 3, containing an aqueous solvent, an acrylic thermoplastic resin, an aziridine curing agent, and a white color pigment, was flexographically printed on the color ink layer 2 and then dried to form a water-based ink layer 3 consisting of a white water-based acrylic ink layer. The shrink label 10 for Experimental Example 1 was prepared using the above process. In Experimental Example 1, the content of the aziridine-based curing agent in the water-based acrylic white ink used to form the water-based ink layer 3 was 2% by weight of the entire water-based ink layer 3 after the water-based acrylic white ink for forming the water-based ink layer 3 was dried.

[0055] <Preparation of Shrink Label of Experimental Example 2> The shrink label 10 of Experimental Example 2 was prepared using the same method and conditions as the shrink label 10 of Experimental Example 1, except that a different type of water-based acrylic white ink (containing a larger amount of white color pigment than in Experimental Example 1) was used to form the water-based ink layer 3 of the shrink label 10 of Experimental Example 1. The water-based acrylic white ink used to form the water-based ink layer 3 of the shrink label 10 of Experimental Example 2 contained an aqueous solvent, an acrylic thermoplastic resin, an aziridine-based curing agent, and a white color pigment, and the content of the aziridine-based curing agent was 2 wt % of the total water-based ink layer 3 after the water-based acrylic white ink used to form the water-based ink layer 3 had dried.

[0056] Preparation of Shrink Label of Experimental Example 3 First, a color ink layer 2 (0.6 μm thick) was formed by gravure printing on one surface of a substrate 1 made of a 40 μm-thick multilayer shrink film (surface layer: PET resin / center layer: PS resin / back layer: PET resin, manufactured by Gunze Ltd.). A water-based gravure ink containing a colored pigment and an acrylic thermoplastic resin was printed and dried twice. Next, a water-based acrylic white ink different from the water-based acrylic white ink used to form the water-based ink layer 3 of the shrink label 10 of Experimental Example 1 was gravure-printed on the color ink layer 2 and then dried, forming a water-based ink layer 3 consisting of a white water-based acrylic ink layer. The shrink label 10 of Experimental Example 3 was prepared using the above process. The water-based acrylic white ink used to form the water-based ink layer 3 of the shrink label 10 of Experimental Example 3 contained an aqueous solvent, an acrylic thermoplastic resin, a metal chelate curing agent, and a white coloring pigment, and the content of the metal chelate curing agent was 3 wt % of the entire water-based ink layer 3 after the water-based acrylic white ink used to form the water-based ink layer 3 had dried.

[0057] <Preparation of Shrink Label of Experimental Example 4> The shrink label 10 of Experimental Example 4 was prepared in the same manner and under the same conditions as the shrink label 10 of Experimental Example 1, except that a water-based acrylic clear ink was used instead of the water-based acrylic white ink used to form the water-based ink layer 3 of the shrink label 10 of Experimental Example 1. The water-based acrylic clear ink used to form the water-based ink layer 3 of the shrink label 10 of Experimental Example 4 contained an aqueous solvent, an acrylic thermoplastic resin, and an epoxy-based curing agent, but was transparent because it did not contain a coloring pigment, and the content of the epoxy-based curing agent was 6 wt % of the entire water-based ink layer 3 after the water-based acrylic clear ink used to form the water-based ink layer 3 had dried.

[0058] <Preparation of Shrink Label of Experimental Example 5> The shrink label 10 of Experimental Example 5 was prepared in the same manner and under the same conditions as the shrink label 10 of Experimental Example 1, except that a water-based urethane white ink containing an aqueous solvent, a urethane-based thermoplastic resin, an isocyanate-based curing agent, and a white coloring pigment was used instead of the water-based acrylic white ink used to form the water-based ink layer 3 of the shrink label 10 of Experimental Example 1. The content of the isocyanate-based curing agent in the water-based urethane white ink used to form the water-based ink layer 3 of the shrink label 10 of Experimental Example 5 was 5 wt % of the total water-based ink layer 3 after the water-based urethane white ink used to form the water-based ink layer 3 had dried.

[0059] <Preparation of Shrink Label of Experimental Example 6> The shrink label 10 of Experimental Example 6 was prepared using the same method and conditions as the shrink label 10 of Experimental Example 5, except that a clear aqueous urethane ink was used instead of the white aqueous urethane ink used to form the water-based ink layer 3 of the shrink label 10 of Experimental Example 5. The clear aqueous urethane ink used to form the water-based ink layer 3 of the shrink label 10 of Experimental Example 6 contained an aqueous solvent, a urethane-based thermoplastic resin, and an isocyanate-based curing agent, but was transparent because it contained no coloring pigment, and the content of the isocyanate-based curing agent was 6 wt % of the total water-based ink layer 3 after the clear aqueous urethane ink used to form the water-based ink layer 3 had dried.

[0060] <Measurement of Contact Angle (°) of Shrink Labels of Experimental Examples 1 to 6> Using the method described above in the section "<Method for Measuring the Contact Angle of a Water Droplet on the Surface of the Water-Based Ink Layer of a Shrink Label>," 2 μL of water was dropped onto the surface of the water-based ink layer 3 of the shrink labels 10 of Experimental Examples 1 to 6. The contact angle (°) of the water droplet on the surface of the water-based ink layer 3 was measured 1 second, 10 seconds, 30 seconds, 60 seconds, and 90 seconds later. The results are shown in Table 1.

[0061] Calculation of the Percentage Reduction in Contact Angle for Shrink Labels of Experimental Examples 1 to 6 Using the contact angle (°) of the water droplet on the surface of the water-based ink layer 3 1 second, 10 seconds, 30 seconds, 60 seconds, and 90 seconds after 2 μL of water was dropped onto the surface of the water-based ink layer 3 of the shrink labels 10 of Experimental Examples 1 to 6 shown in Table 1, the percentage reduction in the contact angle of the water droplet on the surface of the water-based ink layer 3 1 second, 10 seconds, 30 seconds, 60 seconds, and 90 seconds after 2 μL of water was dropped onto the surface of the water-based ink layer 3 of the shrink labels 10 of Experimental Examples 1 to 6 was calculated using the method described above in the "Percentage Reduction in Contact Angle of the Water Droplet on the Surface of the Water-Based Ink Layer of Shrink Label" section. The results are shown in Table 1.

[0062] <Measurement of static and dynamic friction coefficients of shrink labels of Experimental Examples 1 to 6> Using the method described above in the section "<Measurement of static and dynamic friction coefficients>," the static and dynamic friction coefficients of the water-based ink layer 3 against the polyester surface of the shrink labels 10 of Experimental Examples 1 to 6 with a 0.1 mL water droplet, and the static and dynamic friction coefficients of the water-based ink layer 3 against the polyester surface with a 0.01 mL water droplet were measured. The results are shown in Table 1. Furthermore, the static and dynamic friction coefficients of the shrink labels of Experimental Examples 1 to 6 in their dry state were measured using the same method and under the same conditions as described above in the section "<Measurement of static and dynamic friction coefficients>," except that no water droplets were applied. The results are shown in Table 1.

[0063] <Method for Evaluating the Label Attachment Suitability of Shrink Labels of Experimental Examples 1 to 6> Using an LSA9000 series application machine manufactured by Fuji Astec Co., Ltd., the label attachment suitability of each of the shrink labels 10 of Experimental Examples 1 to 6 was evaluated according to the following evaluation criteria. The results are shown in Table 1. The label attachment suitability was evaluated by continuously attaching the labels to 500 PET bottle containers, and the surfaces of the PET bottle containers were wetted with water droplets during attachment. Experimental Examples 1 to 4 are working examples, and Experimental Examples 5 and 6 are comparative examples.

[0064] <Evaluation criteria for label attachment suitability> A: Label misalignment failure rate of 1.5% or less B: Label misalignment failure rate of 1.6% to 3.0% C: Label misalignment failure rate of 3.1% or more

[0065] When the evaluation standard for label attachment suitability was B or higher, it was evaluated that the occurrence of poor attachment of shrink labels to PET bottle containers was suppressed.

[0066]

[0067] As shown in Table 1, the shrink labels 10 of Experimental Examples 1 to 4, in which (i) the contact angle of the water droplet on the surface of the water-based ink layer 3 was greater than 90° 1 second after 2 μL of water was dropped onto the surface of the water-based ink layer 3, and (ii) the rate of decrease in the contact angle of the water droplet on the surface of the water-based ink layer 3 from 1 second to 90 seconds after 2 μL of water was 20% or less of the contact angle of the water droplet on the surface of the water-based ink layer 3 1 second after 2 μL of water was dropped, tended to be rated higher in label attachment suitability than the shrink labels 10 of Experimental Examples 5 and 6, which did not satisfy both of the above conditions (i) and (ii).

[0068] Furthermore, as shown in Table 1, the shrink labels 10 of Experimental Examples 1 to 4, which satisfied both the above conditions (i) and (ii) and in which the dynamic friction coefficient of the aqueous ink layer 3 of the shrink label 10 against a polyester surface having a 0.01 mL water droplet was within the range of 0.1 or more and less than 1.5, tended to be rated higher in label attachment suitability than the shrink labels 10 of Experimental Examples 5 and 6, which did not satisfy both the above conditions (i) and (ii) and in which the dynamic friction coefficient of the aqueous ink layer 3 of the shrink label 10 against a polyester surface having a 0.01 mL water droplet was outside the range of 0.1 or more and less than 1.5.

[0069] Although the embodiments and experimental examples have been described above, it is also planned from the beginning that the configurations of the above-described embodiments and experimental examples may be appropriately combined.

[0070] The embodiments and experimental examples disclosed herein should be considered to be illustrative in all respects and not restrictive. The scope of the present invention is defined by the claims, not by the above description, and is intended to include all modifications within the meaning and scope of the claims.

[0071] 1 substrate, 2 color ink layer, 3 water-based ink layer, 10 shrink label, 11 polyester surface, 12 wire, 13 load cell, 14 test stand, 15 tensile tester, 16 pulley, 17 weight, 18 arrow, 20 plastic container.

Claims

1. A shrink label comprising: a heat-shrinkable substrate; and an aqueous ink layer on said substrate, wherein one second after 2 μL of water is dropped onto the surface of said aqueous ink layer, the contact angle of a water droplet on the surface of said aqueous ink layer exceeds 90°, and the rate of decrease in the contact angle of the water droplet on the surface of said aqueous ink layer from one second to 90 seconds after said 2 μL of water is 20% or less of the contact angle of the water droplet on the surface of said aqueous ink layer one second after said 2 μL of water is dropped.

2. A shrink label as described in claim 1, wherein the dynamic friction coefficient of the water-based ink layer against a polyester surface having a 0.1 mL water droplet is 1.0 or less, and the dynamic friction coefficient of the water-based ink layer against a polyester surface having a 0.01 mL water droplet is less than 1.

5.

3. The shrink label according to claim 1, wherein the shrink label is cylindrical and the inner peripheral surface of the shrink label includes the water-based ink layer.

4. The shrink label according to claim 1, wherein the water-based ink layer contains at least one hardener selected from the group consisting of aziridine-based hardeners, metal chelate-based hardeners, epoxy-based hardeners, and carbodiimide-based hardeners, and an acrylic thermoplastic resin.

Citation Information

Patent Citations

  • Topcoat composition for plastic label

    JP2002311832A

  • Shrink label

    WO2023188581A1