Core-sheath composite fiber and nonwoven fabric formed therefrom

The core-sheath composite fiber with calcium carbonate in both the core and sheath components addresses the safety and sustainability concerns of titanium oxide in nonwoven fabrics by achieving comparable hiding properties and flexibility, reducing plastic volume, and minimizing processing issues.

WO2024202530A1PCT designated stage expired Publication Date: 2024-10-03TOYOBO MC CORP

Patent Information

Application Number
PCT/JP2024/003462
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-09-26
Filing Date
2024-02-02
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The use of titanium oxide in nonwoven fabrics for hygiene products raises safety concerns due to its carcinogenic classification and environmental sustainability issues, while alternative white pigments like zinc oxide are less safe and stable, making it difficult to achieve similar hiding properties and reduce plastic volume effectively.

Method used

A core-sheath composite fiber is developed using a polyester resin core and a polyolefin resin sheath with calcium carbonate added to both components, which improves the white hiding properties and flexibility of the fibers, reducing the need for titanium oxide and enhancing sustainability.

Benefits of technology

The solution maintains excellent white hiding properties and flexibility comparable to conventional fibers containing titanium oxide, while ensuring safety and environmental friendliness, reducing plastic volume and minimizing guide wear during processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024003462_03102024_PF_FP_ABST
    Figure JP2024003462_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a core-sheath composite fiber which is excellent in white fastness without using titanium oxide. This core-sheath composite fiber is composed of a core component containing a polyester-based resin and a sheath component containing a polyolefin-based resin having a melting point lower than the melting point of the polyester-based resin by 20°C or more. The core-sheath composite fiber is characterized in that: one or both of the core component and the sheath component contains, with respect to 100 mass% of each of the components, calcium carbonate at more than 1.0 mass% but not more than 30.0 mass%; the highest peak crystal melting temperature of the core component as measured by a differential scanning calorimeter is lower than 255°C; and the L value indicating the hue of the core-sheath composite fiber is 91 or more and the b value is 5.0 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Core-sheath composite fiber and nonwoven fabric formed therefrom

[0001] The present invention relates to a thermobondable conjugate fiber that maintains nonwoven fabric processability and is excellent in safety, hiding power, and sustainability, and to a nonwoven fabric formed therefrom, which is suitable for applications such as absorbent articles for sanitary materials, such as diapers, napkins, and pads, medical sanitary materials, daily living materials, general medical materials, bedding materials, filter materials, nursing care products, and pet products.

[0002] Some nonwoven fabrics used in hygiene products such as diapers and napkins are made by thermally bonding raw cotton with a core-sheath structure made of two resin components using the air-through method, and are required to have a white color that gives an impression of cleanliness and hiding properties to hide the color of blood and urine that has penetrated the fabric.

[0003] Titanium oxide is commonly incorporated into resins to improve the hiding power of the fibers that make up nonwoven fabrics, but titanium oxide will be classified as carcinogenic in Category 2 (inhalation) under the European CLP Regulation in October 2021, raising safety concerns, such as the requirement for specific warning and labeling on products containing more than 1% titanium oxide by mass.

[0004] Titanium dioxide has a high refractive index and is highly stable, making it widely used as a white pigment added to resins, accounting for 70% of the white raw materials currently in use. Other white pigments include zinc oxide, but they are less safe and stable than titanium dioxide, making them difficult to replace in hygiene and other applications. Furthermore, titanium dioxide is an underground resource (mineral resource), and is less sustainable than biological resources, which are environmentally friendly materials.

[0005] On the other hand, there have been many reported examples of incorporating inorganic particles other than titanium oxide and zinc oxide or talc into resins to improve the transparency and softness of fibers and nonwoven fabrics. However, because the refractive index of inorganic particles and talc is low and close to that of polyester resins, it has been thought that simply incorporating them into resins would not be able to achieve the same white color or hiding power as titanium oxide.

[0006] For example, in Patent Document 1, calcium carbonate is used to impart a soft feel and high rigidity to the nonwoven fabric, but the hiding power and color of the fiber are not considered.

[0007] Patent Document 2 describes that calcium carbonate improves mechanical hardness and thermal conductivity, and provides a multifilament fiber with increased opacity, but does not discuss opacity or color.

[0008] In Patent Document 3, inorganic particles are added to improve the anti-transparency (concealment) properties of a two-component core-sheath composite fiber, with the amount of inorganic particles added to the core being 0.10 to 10 mass % and the amount of inorganic particles added to the sheath being 0.050 to 1.0 mass %, and the functionality is achieved by including inorganic particles in both the core and the sheath, with titanium oxide being mainly used as the inorganic particles. One of the examples describes an example in which calcium carbonate is used in the core and aluminum oxide in the sheath, but no study is made on improving the anti-transparency properties by using calcium carbonate alone.

[0009] In Patent Document 4, recycled PET is used for the core of a recycled polyester sheath-core composite fiber, and 3 mass% or more of titanium oxide is added to improve the hue (L value, b value), but no other inorganic particles or talc are investigated. As shown in Patent Documents 3 and 4, titanium oxide is not suitable for use in plastic volume reduction, where the amount of resin is reduced by adding it at a high concentration.

[0010] JP 2020-90771 A JP 2019-112759 A JP 2021-55231 A JP 2006-328600 A

[0011] In light of the above, in order to overcome the drawbacks of titanium oxide, the conventionally used white pigment, such as its safety and sustainability, and its use in reducing the volume of plastics due to its high concentration addition, it is desirable to provide a fiber that can contribute to reducing the environmental load by adding other inorganic particles instead of titanium oxide, thereby reducing the amount of resin used without significantly affecting the quality of the fiber while maintaining the post-processability into nonwoven fabrics, etc. It is also desirable to provide a safe and sustainable fiber by using an inorganic substance that is expected to utilize biological resources, which are environmentally friendly materials. An object of the present invention is to provide a core-sheath composite fiber that has excellent white hiding power without using titanium oxide, and a nonwoven fabric formed therefrom.

[0012] The sheath-core composite fiber of the present invention, which has achieved the above-mentioned object, has the following gist: The sheath-core composite fiber of the present invention is a sheath-core composite fiber composed of a core component containing a polyester-based resin and a sheath component containing a polyolefin-based resin having a melting point at least 20°C lower than the melting point of the polyester-based resin, characterized in that one or both of the core component and the sheath component contain calcium carbonate in an amount of more than 1.0% by mass and not more than 30.0% by mass, based on 100% by mass of each component, the maximum peak temperature of crystalline melting of the core component is lower than 255°C, and the L value, which indicates the hue of the sheath-core composite fiber, is 91 or more and the b value is 5.0 or less.

[0013] It is also preferable that the core component has a temperature-lowering crystallization peak temperature of 190°C to 220°C as measured by a differential scanning calorimeter.

[0014] It is preferable that the polyester resin contains polyethylene terephthalate, and the polyolefin resin contains polyethylene.

[0015] The content of the polyester resin is preferably 40% by mass or more of the total fiber.

[0016] The cross-sectional shape of the fibers may be concentric, eccentric or hollow.

[0017] The tensile strength measured in accordance with JIS L1013 8.5.1 is preferably 0.80 to 5.00 cN / dtex, and the elongation measured in accordance with JIS L1013 8.5.1 is preferably 30 to 200%.

[0018] The present invention also includes a nonwoven fabric formed from the core-sheath composite fiber.

[0019] According to the present invention, it is possible to provide a core-sheath composite fiber having excellent white hiding power without using titanium oxide, and a nonwoven fabric formed therefrom.

[0020] In other words, the core-sheath composite fiber of the present invention maintains the same hiding power, flexibility, bulkiness, and bulk recovery properties as conventional fibers to which a white pigment mainly made of titanium oxide has been added, while being excellent in safety and environmental sustainability, and it is possible to produce nonwoven fabrics that can reduce the environmental load by reducing the volume of plastic.

[0021] Furthermore, titanium oxide has a high Mohs hardness and causes metal abrasion, so fibers containing titanium oxide on the fiber surface wear the metal rollers of the processing machine, particularly during crimping, making sustained crimping difficult. In the present invention, by using calcium carbonate as the sheath component, it is possible to reduce guide wear and traveler wear during stretching, which have traditionally been problems with fibers containing titanium oxide on the fiber surface, and improve the white color hiding power of the fiber. Furthermore, in the present invention, the white color hiding power of the fiber can also be improved by using calcium carbonate as the core component. These factors make it possible to obtain a bicomponent composite fiber for nonwoven fabrics that combines the same white color, hiding power, and softness as conventional fibers containing titanium oxide, while also providing smoothness to the fiber surface.

[0022] Fig. 1 shows the results of differential scanning calorimetry of the calcium carbonate-containing polyester resin core component obtained in Comparative Example 3. Fig. 2 shows the results of differential scanning calorimetry of the calcium carbonate-containing polyester resin core component obtained in Example 1. Fig. 3 shows the results of differential scanning calorimetry of the calcium carbonate-containing polyester resin core component obtained in Example 5. Figs. 4(a) to (c) show the mechanism by which the whiteness (hiding ability) of a fiber is expressed by the polymer chain orientation contained in the unstretched resin, the presence or absence of calcium carbonate addition, and the polymer chain orientation contained in the resin due to stretching.

[0023] [Sheath-Core Composite Fiber] The sheath-core composite fiber of the present invention is a core composite fiber composed of a core component containing a polyester-based resin and a sheath component containing a polyolefin-based resin having a melting point at least 20°C lower than the melting point of the polyester-based resin, characterized in that one or both of the core and sheath components contain more than 1.0% by mass and not more than 30.0% by mass of calcium carbonate per 100% by mass of each component, the core component has a maximum crystal melting peak temperature of less than 255°C as measured by a differential scanning calorimeter, and the L value, which indicates the hue of the sheath-core composite fiber, is 91 or more and the b value is 5.0 or less. The fiber contains calcium carbonate in one or both of the core and sheath components, and by drawing this fiber, it is possible to increase the orientation of the polyester-based resin and increase the crystal size of the polyester-based resin in the presence of calcium carbonate, resulting in an improvement in the whiteness (hiding ability) of the sheath-core composite fiber.

[0024] The present invention encompasses (i) a sheath-core composite fiber in which only the core component contains calcium carbonate (first embodiment), (ii) a sheath-core composite fiber in which only the sheath component contains calcium carbonate (second embodiment), and (iii) a sheath-core composite fiber in which both the core component and the sheath component contain calcium carbonate (third embodiment). Hereinafter, unless explicitly stated as the first embodiment, the second embodiment, or the third embodiment, it is considered that all of these embodiments are referred to.

[0025] <Core Component> The core component contains a polyester resin.

[0026] The polyester resin may be any resin that exhibits the strength and low shrinkage required for the core component, and examples thereof include polyethylene terephthalate (melting point 255°C), polybutylene terephthalate (melting point 230°C), polytrimethylene terephthalate (melting point 230°C), polyethylene naphthalate (melting point 265°C), polybutylene naphthalate (melting point 243°C), polyhydroxyalkanoate (melting point approximately 180°C), polyhydroxybutyric acid (melting point 175°C), and polylactic acid (melting point 170 to 175°C).

[0027] Among these, from the viewpoints of strength and low shrinkage and of using a resin with a melting point 20°C or higher than that of the polyolefin resin used in the sheath component, the polyester resin preferably contains a polyester resin having a melting point of 200°C or higher (preferably 210°C or higher, more preferably 220°C or higher and 280°C or lower), more preferably polyethylene terephthalate (melting point 255°C), polybutylene terephthalate (melting point 230°C), polytrimethylene terephthalate (melting point 230°C), polyethylene naphthalate (melting point 265°C), or polybutylene naphthalate (melting point 243°C), even more preferably polyethylene terephthalate (melting point 255°C), polyethylene naphthalate (melting point 265°C), or polybutylene naphthalate (melting point 243°C), and particularly preferably polyethylene terephthalate (melting point 255°C). The polyester resin may be one type or two or more types.

[0028] The polyester resin may have a predetermined intrinsic viscosity, and the intrinsic viscosity (IV) of the polyester resin is preferably 0.3 to 2.0 dl / g, more preferably 0.5 to 1.5 dl / g, and even more preferably 0.55 to 0.80 dl / g. The intrinsic viscosity (IV) of the polyester resin can be determined by pulverizing and drying a sample, dissolving it in a 6 / 4 (mass ratio) mixed solvent of phenol and 1,1,2,2-tetrachloroethane, centrifuging the solution to remove inorganic particles and the like, and then measuring the IV at 30°C using an Ubbelohde viscometer.

[0029] The content of the polyester resin having a melting point of 200° C. or higher is preferably 80% by mass or higher, more preferably 90% by mass or higher, even more preferably 95% by mass or higher, still more preferably 97% by mass or higher, particularly preferably 99% by mass or higher, and most preferably 100% by mass, based on 100% by mass of the polyester resin. When the content of the polyester resin having a melting point of 200° C. or higher is within the above range, adding calcium carbonate and stretching the fiber promotes crystallization of the polyester resin, thereby increasing the whiteness of the fiber.

[0030] In the first and third embodiments, the content of the polyester resin is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, preferably less than 99% by mass, more preferably 98% by mass or less, even more preferably 97% by mass or less, and even more preferably 96% by mass or less, based on 100% by mass of the core component. If the content of the polyester resin is less than 70% by mass, the strength of the core may be reduced and the adhesion between the core and sheath may be reduced. If the content of the polyester resin is 99% by mass or more, crystallization of the polyester resin may not be promoted, and good whiteness may not be achieved. In the second embodiment, the content of the polyester resin is preferably 100% by mass based on 100% by mass of the core component.

[0031] From the viewpoint of core strength, the content of polyester resin is preferably 40% by mass or more of the total fiber, more preferably 45% by mass or more and 75% by mass or less, even more preferably 50% by mass or more and 70% by mass or less, and even more preferably 55% by mass or more and 65% by mass or less.

[0032] In the first and third embodiments, the calcium carbonate contained in the core component may be heavy calcium carbonate, light calcium carbonate, or a mixture thereof.

[0033] Heavy calcium carbonate may be obtained by crushing and classifying natural materials such as limestone, marble, calcite, and chalk, and is also called natural calcium carbonate. Light calcium carbonate may be obtained by precipitating crystals in a liquid through a chemical reaction (for example, by precipitating through the reaction of calcium hydroxide with carbon dioxide), and is also called synthetic calcium carbonate or precipitated calcium carbonate. Calcium carbonate may be surface-treated with a fatty acid, siloxane, resin, or the like. Examples of fatty acids include stearic acid, palmitic acid, myristic acid, and lauric acid, and may be used as a salt or ester of the fatty acid. Examples of resins include polyacrylate and polydiallyldimethylammonium chloride.

[0034] The calcium carbonate preferably has a predetermined average particle size d50 and top-cut particle size d90. The average particle size d50 means that 50% by mass of all particles have a particle size smaller than the indicated value, and the top-cut particle size d90 means that 90% by mass of all particles have a particle size smaller than the indicated value.

[0035] The average particle size d50 of calcium carbonate used in the core is preferably 0.02 to 3.0 μm, more preferably 0.35 to 1.75 μm, even more preferably 0.40 to 1.50 μm, and even more preferably 0.45 to 1.25 μm. The top-cut particle size d90 of calcium carbonate is preferably 5.0 μm or less, more preferably 4.0 μm or less, even more preferably 3.0 μm or less, even more preferably 2.0 μm or less, and particularly preferably 1.0 μm or less, and is preferably 0.3 μm or more or 0.5 μm or more.

[0036] In the first and third embodiments, the calcium carbonate content of the core component is preferably more than 1.0% by mass and not more than 30.0% by mass, more preferably 2.0% by mass or more and not more than 25.0% by mass, even more preferably 3.0% by mass or more and not more than 20.0% by mass, and even more preferably 4.0% by mass or more and not more than 15.0% by mass, based on 100% by mass of the core component. If the calcium carbonate content is 1.0% by mass or less, crystallization of the polyester resin may not be promoted, and the L value of the resulting fiber may be small. If the calcium carbonate content exceeds 30.0% by mass, the pressure rise rate of the filter used for spinning may increase, or adhesion at the interface between the core and sheath may decrease, resulting in fuzz and yarn breakage.

[0037] The core component may contain components other than the polyester resin and calcium carbonate as long as the effects of the present invention are achieved, and additives such as antioxidants, antistatic agents, antiblocking agents, pigments, heat stabilizers, ultraviolet absorbers, and lubricants may be added within limits that do not impair the effects of the present invention.

[0038] In the first and third embodiments, the content of the polyester resin and calcium carbonate in the core component is, based on 100% by mass of the core component, preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 97% by mass or more, still more preferably 99% by mass or more, and particularly preferably 100% by mass. The core component preferably does not substantially contain titanium oxide, and the content of titanium oxide in 100% by mass of the core component is more preferably 0.5% by mass or less, even more preferably 0.1% by mass or less, and still more preferably 0% by mass.

[0039] In the first to third embodiments, the core component (preferably a calcium carbonate-containing polyester resin or a calcium carbonate-free polyester resin) may have a predetermined maximum crystalline melting peak temperature measured with a differential scanning calorimeter. The maximum crystalline melting peak temperature of the core component is preferably less than 255°C, more preferably 243 to 254°C, even more preferably 244 to 253°C, and even more preferably 245 to 252°C. A maximum crystalline melting peak temperature within the above range is observed when the core component is stretched, regardless of the presence or absence of calcium carbonate, and promotes crystallization of the polyester resin, thereby increasing the whiteness of the fiber. When the core component is unstretched, the maximum crystalline melting peak temperature of the core component is 255°C or higher, which does not promote crystallization of the polyester resin and therefore does not increase the whiteness of the fiber. Note that as the calcium carbonate content of the core component increases within the above range, the maximum crystalline melting peak temperature tends to increase within the above temperature range. The differential scanning calorimeter may be, for example, a differential scanning calorimeter manufactured by TA Instruments. The crystal melting peak temperature is measured, for example, at a temperature increase rate of 10°C / min, and the temperature at which the measured melting endothermic curve gives an extreme value is defined as the crystal melting maximum peak temperature. The cooling crystallization peak temperature, which will be described later, is measured, for example, at a temperature decrease rate of 10°C / min, and the temperature at which the measured crystallization exothermic curve gives an extreme value is defined as the cooling crystallization peak temperature.

[0040] In the first to third embodiments, the core component may have a predetermined temperature-decreasing crystallization peak temperature measured with a differential scanning calorimeter, and the temperature-decreasing crystallization peak temperature of the core component is preferably 200° C. to 220° C., more preferably 202° C. to 218° C., even more preferably 204° C. to 216° C., and still more preferably 206° C. to 214° C. When the temperature-decreasing crystallization peak temperature is within the above range, unoriented fine crystals tend to be formed, accelerating the crystallization of the polyester resin.

[0041] <Sheath Component> The sheath component contains a polyolefin resin having a melting point that is 20° C. or more lower than the melting point of the polyester resin.

[0042] The polyolefin resin may be either a polyolefin homopolymer or a polyolefin copolymer. The carbon number of the olefin monomer constituting the polyolefin resin is, for example, 2 to 20, preferably 2 to 15, more preferably 2 to 10, and even more preferably 2 to 5. Examples of the olefin monomer include ethylene, propylene, butene, pentene, hexene, heptene, octene, nonene, and decene. Among these, the polyolefin resin has olefin monomers such as ethylene, propylene, butene, pentene, and hexene as the main structural unit (preferably 60 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, even more preferably 90 mol% or more, particularly preferably 95 mol% or more, and preferably 100 mol% or less or 99 mol% or less, of 100 mol% of all structural units).

[0043] Examples of polyolefin resins include polyethylenes such as low-density polyethylene (melting point 100°C to 115°C), high-density polyethylene (melting point 125°C to 137°C), and ultra-high molecular weight polyethylene (melting point 135°C to 140°C), polypropylene (melting point 165°C), polybutene-1 (melting point 126°C to 128°C), and 1,2-polybutadiene (melting point 71°C to 105°C).

[0044] When a polyolefin copolymer is used, a small amount of an α-olefin such as ethylene, propylene, butene, hexene, or octene may be copolymerized with the above-mentioned components as the copolymerization component.

[0045] Among these, the polyolefin resin preferably has a melting point of 180°C or lower (preferably 170°C or lower and 70°C or higher), more preferably contains polyethylene or polypropylene, and even more preferably contains polyethylene. The polyolefin resin may be one type or two or more types.

[0046] The polyolefin resin may have a predetermined melt flow rate (MFR) measured in accordance with JIS K 6922-2, and the melt flow rate (MFR) of the polyolefin resin is preferably 8 to 25 g / 10 min, more preferably 9 to 21 g / 10 min, under conditions of a load of 2.16 kg and a temperature of 190°C.

[0047] The polyolefin resin may have a predetermined density, and the low-density polyethylene has a density of 0.91 to 0.92 g / cm 3 , high density polyethylene has a density of 0.94 to 0.965 g / cm 3 , polypropylene has a density of 0.90 to 0.91 g / cm 3 It has.

[0048] The content of the polyolefin resin having a melting point of 180° C. or less is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, still more preferably 99% by mass or more, and particularly preferably 100% by mass, based on 100% by mass of the polyolefin resin. When the content of the polyolefin resin is within the above range, a nonwoven fabric having high adhesion between fibers by heat fusion can be produced.

[0049] In the second and third embodiments, the content of the polyolefin resin in 100% by mass of the sheath component is preferably 70% by mass or more, more preferably 75% by mass or more, even more preferably 80% by mass or more, still more preferably 85% by mass or more, and preferably 99% by mass or less, more preferably 98% by mass or less, even more preferably 97% by mass or less, and still more preferably 96% by mass or less. In the first embodiment, the content of the polyolefin resin in 100% by mass of the sheath component is preferably 100% by mass.

[0050] The content of the polyolefin resin in the entire fiber is preferably at least 20% by mass or more, more preferably 25% by mass or more and 55% by mass or less, even more preferably 30% by mass or more and 50% by mass or less, and even more preferably 35% by mass or more and 45% by mass or less.

[0051] In the second and third embodiments, the calcium carbonate contained in the shell component may be heavy calcium carbonate, light calcium carbonate, or a mixture thereof, similar to the calcium carbonate used in the core component.

[0052] Heavy calcium carbonate may be obtained by crushing and classifying natural materials such as limestone, marble, calcite, and chalk, and is also called natural calcium carbonate. Light calcium carbonate may be obtained by precipitating crystals in a liquid through a chemical reaction (for example, by precipitating through the reaction of calcium hydroxide with carbon dioxide), and is also called synthetic calcium carbonate or precipitated calcium carbonate. Calcium carbonate may be surface-treated with a fatty acid, siloxane, resin, or the like. Examples of fatty acids include stearic acid, palmitic acid, myristic acid, and lauric acid, and may be used as a salt or ester of the fatty acid. Examples of resins include polyacrylate and polydiallyldimethylammonium chloride.

[0053] The average particle size d50 of calcium carbonate used in the shell component is preferably 0.02 to 3.0 μm, more preferably 0.10 to 2.0 μm, and even more preferably 0.20 to 1.0 μm. The top cut particle size d90 of calcium carbonate used in the shell component is preferably 5.0 μm or less, more preferably 4.0 μm or less, even more preferably 3.0 μm or less, still more preferably 2.0 μm or less, particularly preferably 1.0 μm or less, and preferably 0.3 μm or more or 0.5 μm or more.

[0054] In the second and third embodiments, the calcium carbonate content of the sheath component is preferably more than 1.0% by mass and not more than 30.0% by mass, more preferably 2.0% by mass or more and not more than 25.0% by mass, even more preferably 3.0% by mass or more and not more than 20.0% by mass, and even more preferably 4.0% by mass or more and not more than 15.0% by mass, based on 100% by mass of the sheath component. If the calcium carbonate content is 1.0% by mass or less, crystallization of the polyolefin resin may not be promoted, and the L value of the resulting fiber may be small. If the calcium carbonate content exceeds 30.0% by mass, the pressure increase rate of the filter used for spinning may increase, or adhesion at the interface between the core and sheath may decrease, resulting in fuzz and yarn breakage.

[0055] The calcium carbonate used in the core component and the calcium carbonate used in the sheath component may be the same or different.

[0056] The sheath component may contain components other than the polyolefin resin and calcium carbonate as long as the effects of the present invention are achieved, and additives such as antioxidants, antistatic agents, antiblocking agents, pigments, heat stabilizers, ultraviolet absorbers, and lubricants may be added within limits that do not impair the effects of the present invention.

[0057] In the second and third embodiments, the content of the polyolefin resin and calcium carbonate in the shell component is preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 97% by mass or more, still more preferably 99% by mass or more, and particularly preferably 100% by mass, based on 100% by mass of the shell component. The shell component preferably does not substantially contain titanium oxide, and the content of titanium oxide in the shell component is more preferably 0.5% by mass or less, even more preferably 0.1% by mass or less, and still more preferably 0% by mass, based on 100% by mass of the shell component.

[0058] The calcium carbonate content is preferably 1 to 25 mass%, more preferably 1.5 to 20 mass%, and even more preferably 2.0 to 15 mass%, based on 100 mass% of the sheath-core composite fiber. When the calcium carbonate content in the sheath-core composite fiber is within the above range, volume reduction of the polyester resin or polyolefin resin is promoted, and when the fiber is drawn, the whiteness of the sheath-core composite fiber is improved.

[0059] In the core-sheath composite fiber of the present invention, the mass ratio of the core component to the sheath component is preferably less than 7.0, more preferably 5.0 or less, even more preferably 4.0 or less, still more preferably 3.0 or less, particularly preferably 2.0 or less, and is preferably 0.2 or more or 0.3 or more. By setting the mass ratio of the core component to the sheath component within the above range, the strength and elongation of the fiber can be made appropriate for nonwoven fabrics.

[0060] The polyester resin, polyolefin resin, and both of them used in the present invention may contain more than 1.0% by mass of calcium carbonate (based on the mass of each resin). Calcium carbonate is added to improve the fiber hiding ability, i.e., whiteness, by controlling the size of the crystals formed by the resin. If the amount is 1.0% by mass or less, the improvement in whiteness when made into a nonwoven fabric will be insufficient.

[0061] The single filament fineness of the core-sheath composite fiber is preferably 0.1 to 8.0 dtex, more preferably 0.2 to 4.8 dtex, even more preferably 0.5 to 4.6 dtex, still more preferably 1.0 to 4.4 dtex, and particularly preferably 1.5 to 4.2 dtex. The single filament fineness of the core-sheath composite fiber can be measured in accordance with JIS L-1095 9.4.1.

[0062] The cross-sectional shape of the core-sheath composite fiber is preferably a concentric cross-section, an eccentric cross-section, or a hollow cross-section, and more preferably a concentric cross-section. A concentric cross-section means that the center of gravity of the core and the center of gravity of the sheath are the same, an eccentric cross-section means that the center of gravity of the core and the center of gravity of the sheath are not the same, and a hollow cross-section means that the core has a core and a sheath, but the core has a hollow structure.

[0063] The sheath-core composite fiber of the present invention has a predetermined L value and b value according to the Hunter color difference formula, which indicate an appropriate whiteness for appearance quality. That is, the L value, which indicates the hue of the sheath-core composite fiber, is 91 or more, and the b value is 5.0 or less. The L value is preferably 91.5 or more, more preferably 92 or more, even more preferably 92.5 or more, and still more preferably 93 or more, and preferably 99 or less or 98 or less. An L value of less than 91 is not suitable for use as a nonwoven fabric for sanitary materials.

[0064] The b value is preferably 4.5 or less, more preferably 4.0 or less, even more preferably 3.5 or less, even more preferably 3.0 or less, particularly preferably 2.5 or less, and most preferably 2.0 or less. If the b value exceeds 5.0, the color tone will be yellowish and the nonwoven fabric will not be suitable for use as a sanitary material. The L value and b value can be measured, for example, using a sample in which the core-sheath composite fiber is wrapped around a black backing so that the color of the backing is not visible to the naked eye, using a color difference meter (for example, a MINOLTA CM-3700d spectrophotometer).

[0065] The sheath-core composite fiber of the present invention may have a predetermined strength and elongation. The strength of the fiber, as measured in accordance with JIS L1013 8.5.1, is preferably 0.80 to 5.00 cN / dtex, more preferably 0.85 to 4.80 cN / dtex, even more preferably 0.90 to 4.60 cN / dtex, still more preferably 0.95 to 4.40 cN / dtex, and particularly preferably 1.00 to 4.20 cN / dtex.

[0066] The elongation of the fiber, as measured in accordance with JIS L1013 8.5.1, is preferably 30 to 200%, more preferably 35 to 190%, even more preferably 40 to 180%, still more preferably 45 to 170%, and particularly preferably 50 to 160%. The sheath-core composite fiber of the present invention has an elongation that is equal to or greater than that of general fibers.

[0067] [Method for Preparing Sheath-Core Composite Fiber] The sheath-core composite fiber of the present invention preferably includes at least the steps of melt-spinning a core-sheath fiber using a polyester resin as the core component, a polyolefin resin as the sheath component, and calcium carbonate as one or both of the core and sheath components to prepare an undrawn yarn, and drawing the undrawn yarn under heating conditions. The polyester resin, polyolefin resin, calcium carbonate, and amounts thereof used are as described above.

[0068] Calcium carbonate may be dispersed by adding and stirring a predetermined amount during or immediately after the polymerization of the resin, and then chipping the mixture while extruding it with an extruder, or by spinning the resin in a molten state. Examples of methods for uniformly dispersing calcium carbonate in a resin include a circulation dispersion method and a masterbatch method. The circulation dispersion method may be a method in which a predetermined amount of calcium carbonate is added immediately after the polymerization of the resin, and the resin melt is circulated to disperse the calcium carbonate. The masterbatch method may be a method in which a predetermined amount of calcium carbonate is previously wetted with water, a solvent, or the like, and mixed with a predetermined resin in a pressure kneader, and the calcium carbonate is dispersed while separating the water and solvent.

[0069] <Melt Spinning Step> Preferably, the polyester resin and the polyolefin resin are melted while incorporating calcium carbonate into one or both of them, and the molten resin is extruded from a core-sheath spinneret through a spinning pack. The extrusion nozzle preferably has 10 to 1,000 holes, more preferably 50 to 800 holes, even more preferably 100 to 600 holes, and even more preferably 200 to 400 holes, and the resin is spun at a spinning temperature 10 to 30°C higher than the melting point of the polyester resin. The spun yarn is then cooled by blowing air at a temperature of 10 to 25°C, preferably at a flow rate of 50 to 100 m / min, and a spinning oil is applied. The undrawn yarn may then be collected in a container (e.g., a can) preferably at a take-up speed of 1,000 to 1,500 m / min.

[0070] <Drawing Step> The obtained undrawn yarn is drawn using a liquid phase or a gas phase, preferably at a temperature of 60°C to 130°C, at a draw ratio of preferably 1.5 to 6.0 times, more preferably 1.5 to 5.0 times, even more preferably 1.5 to 4.0 times, and even more preferably 1.5 to 3.0 times. In particular, from the viewpoint of further increasing the L value and further decreasing the maximum crystalline melting peak temperature, the undrawn yarn is drawn at a draw ratio of preferably 1.55 to 3.0 times, more preferably 1.60 to 2.9 times, and even more preferably 1.70 to 2.8 times. Drawing may be performed in one stage or two or more stages. In the case of two-stage drawing, the first stage of drawing is preferably performed at a temperature of 60 to 90°C (preferably 60 to 80°C) and a draw ratio of 2.0 to 4.0 times (preferably 3.6 times or less, more preferably 3.2 times or less). The second stage stretching is preferably carried out at a temperature of 90 to 130° C. (preferably 100 to 120° C.) and at a stretching ratio of 0.8 to 1.2 times (preferably 0.9 to 1.1 times), for example.

[0071] The method for producing a core-sheath composite fiber of the present invention may include, in addition to the above steps, a crimping step, a post-heat treatment step, and a cutting step. The crimping step may involve crimping using a crimper such as a stuffer box crimper. The post-heat treatment step may involve treating the resulting fiber at a temperature of 90 to 140°C (preferably 100 to 130°C) without applying tension to the fiber.

[0072] When the core-sheath composite fibers are cut into short fibers, the average length of the short fibers is preferably 30 to 80 mm, more preferably 31 to 70 mm, and even more preferably 32 to 60 mm.

[0073] The core-sheath composite fiber may be surface-treated with an oil agent that exhibits hydrophilicity or water repellency, and may be treated with the oil agent in any step after cutting, drying, or the like.

[0074] Adding calcium carbonate to a polyester resin and then performing drawing and crystallization treatments controls the crystalline structure of the drawn yarn, resulting in a core-sheath composite fiber that combines whiteness (white color, opacity, and anti-transparency) with the mechanical properties required for raw cotton for nonwoven fabrics. The mechanism by which whiteness is improved in the first and third embodiments of the present invention is shown in Figures 4(a) to 4(c). As shown in Figure 4(a), the polymer chains contained in the undrawn polyester resin are randomly oriented. As shown in Figure 4(b), in the absence of inorganic particles such as calcium carbonate, unoriented crystals (e.g., spherulites) grow during the process of neck deformation caused by drawing an undrawn yarn, acting as a factor inhibiting the orientation of the polymer chains contained in the polyester resin. In contrast, as shown in Figure 4(c), adding inorganic particles such as calcium carbonate acts as a nucleating agent for the PET resin, thereby reducing the crystal size of unoriented crystals formed in the system (the nucleating agent effect promotes crystallization as unoriented, small crystals). This allows for the application of linear and uniform stress to the undrawn yarn compared to systems without calcium carbonate, which promotes oriented crystallization and allows for the production of drawn yarn with crystal sizes that diffuse visible light (larger crystal sizes result in higher visible light diffusion and higher whiteness). The phenomenon of calcium carbonate acting as a nucleating agent for PET can be inferred from the temperature-reducing crystallization peak temperature in differential scanning calorimetry (DSC) (Figures 2 and 3). As the calcium carbonate concentration increases, the temperature-reducing crystallization peak temperature appears on the higher side, suggesting that the nucleating agent effect promotes the formation of unoriented, fine crystals.

[0075] The phenomenon in which the crystal size of drawn yarns increases depending on the drawing and crystallization conditions in systems containing calcium carbonate can be inferred from the results of differential scanning calorimetry (DSC). In the DSC curve (FIG. 1) of Comparative Example 3, which was not drawn after calcium carbonate was added, the PET-derived crystalline melting curve appears as a single broad absorption curve with a peak near 255°C. This is a crystalline melting curve derived from unoriented crystals (spherulites) without orientation of the polymer chains contained in the polyester-based resin. In contrast, the DSC curve (FIG. 2) of Example 1 shows a broad absorption curve with a peak near 255°C, as well as another absorption curve with a maximum peak temperature near 250°C. This is a crystalline melting curve resulting from drawing and derived from crystals with orientation of the polymer chains contained in the polyester-based resin. As the draw ratio is increased to near the break region, the broad absorption curve with a peak near 255°C attenuates, and the peak near 255°C is no longer observed (only an absorption curve with a maximum peak temperature near 250°C remains). Drawn yarn in this state has excellent whiteness, but its elongation is significantly reduced, making it unsuitable for nonwoven fabric applications. Therefore, in order to obtain drawn yarn that combines excellent whiteness and mechanical properties, it is important that the maximum peak crystalline melting temperature of the drawn yarn is measured at a temperature lower than 255°C.

[0076] Increasing the calcium carbonate concentration can promote the formation of oriented crystals, thereby improving whiteness. In the DSC curve of Example 1 (FIG. 2), the maximum peak crystal melting temperature of oriented crystals (crystals with high visible light diffusion) is measured at 250°C, whereas in Example 5 (FIG. 3), where a higher calcium carbonate concentration is added, the maximum peak crystal melting temperature of oriented crystals is measured at 252°C. The shift of the crystal melting peak to the higher temperature side suggests that the crystal size of oriented crystals increases as the calcium carbonate concentration increases.

[0077] The sheath-core composite fibers of the present invention may be long fibers (filaments), short fibers (staples), or a combination thereof.

[0078] The present invention includes a nonwoven fabric formed from core-sheath composite fibers. The nonwoven fabric is preferably formed by a conventionally known fleece forming or fleece bonding method. The fleece can be formed by a dry method, a wet method, a spunbonding method, a meltflow method, or the like, and the fleece can be bonded by a thermal bond method, a chemical bond method, a needle punch method, a spunlace method, a stitch bond method, a steam jet method, or the like. The fleece forming or fleece bonding method may be selected from the above methods depending on the desired nonwoven fabric.

[0079] This application claims the benefit of priority based on Japanese Patent Application No. 2023-058130 filed on March 31, 2023, and Japanese Patent Application No. 2023-162951 filed on September 26, 2023. The entire contents of the specifications of Japanese Patent Application No. 2023-058130 filed on March 31, 2023, and Japanese Patent Application No. 2023-162951 filed on September 26, 2023 are incorporated herein by reference.

[0080] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples, and it is possible to carry out the invention with appropriate modifications within the scope of the above and below-described aims, and all such modifications are included within the technical scope of the present invention. In the following, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass." The sample size is based on the size described below, but when the sample was insufficient, measurements were carried out using the largest possible sample size.

[0081] (1) Materials The core of the bicomponent core-sheath composite fiber was polyethylene terephthalate (PET) with an intrinsic viscosity IV of 0.63 dl / g, and the sheath was high-density polyethylene (HDPE) with an MFR of 20 g / 10 min (load 2.16 kg, temperature 190°C). Calcium carbonate KRS1 manufactured by Maruo Calcium Co., Ltd. was used for the PET core component, and YM10 manufactured by Maruo Calcium Co., Ltd. was used for the PE sheath component.

[0082] (2) Color Tone Measurement The L value and b value were measured using a MINOLTA CM-3700d color difference meter with settings that excluded reflected light. The L value and b value in the present invention were measured using samples in which the obtained fibers were wound on a black backing and visually confirmed that the color of the backing did not show through. The L value is an index of the whiteness of the color, and the b value is an index of the yellowness of the color. If the L value is less than 85 or the b value exceeds 5.0, when used as a nonwoven fabric, the appearance of the color tone will be poor and the quality will be poor, with insufficient hiding power. Although anti-see-through properties can be obtained even with an L value of 90 or less, an L value of 91 or more is desirable for nonwoven fabrics used as sanitary materials.

[0083] (3) Differential Scanning Calorimetry Measurement The crystal melting peak temperature was measured at a heating rate of 10°C / min using a differential scanning calorimeter manufactured by TA Instruments. The temperature at the extreme value of the measured melting absorption curve was taken as the crystal melting peak. The cooling crystallization peak temperature was measured at a cooling rate of 10°C / min.

[0084] (4) Fineness, Single Yarn Fineness Measured by the method described in JIS L-1095 9.4.1. The single yarn fineness was calculated by dividing the fineness by the number of filaments.

[0085] (5) Maximum stress (also called tensile strength, shown as "strength" in Table 1) and maximum elongation (also called "elongation") were measured in accordance with JIS L1013 8.5.1. The stress at the maximum load was taken as the maximum stress, and the elongation at the maximum load was taken as the maximum elongation.

[0086] Example 1: Polyethylene terephthalate (PET) was dried using conventional methods as a polyester-based resin, and then adjusted to a calcium carbonate content of 4.0% by mass together with PET. This was then fed separately to a bicomponent fiber spinning machine along with a separately prepared polyolefin-based resin, high-density polyethylene (HDPE). The resulting mixture was melt-extruded at 285°C using an extruder attached to the bicomponent fiber spinning machine, and bicomponent spun using a spinneret with multiple holes to form a core-sheath structure in which the two components were concentrically spun in a 40 / 60 (sheath / core) mass ratio, with PET positioned on the core side and HDPE positioned on the sheath side. The spun yarn was cooled by airflow, oiled using an oiling guide, and bundled using a bundle guide. It was then pulled by a roller at a spinning speed of 1240 m / min and wound on a winder. The resulting fiber (undrawn yarn) had a single yarn fineness of 5.0 dtex. Next, this was drawn in a drawing device at a speed of 40 m / min at a drawing temperature of 70° C. to a draw ratio of 2.4, and then drawn 0.95 times at a drawing temperature of 110° C., and heat-set at 120° C. These spinning and drawing steps yielded a core-sheath composite fiber with a single filament fineness of 2.2 dtex, in which PET was arranged on the core side and HDPE was arranged on the sheath side concentrically in a mass ratio of 40 / 60 (sheath / core).

[0087] [Example 2] The same procedure as in Example 1 was carried out, except that an undrawn yarn was obtained by the method of Example 1 and then the single yarn fineness was adjusted to 2.8 dtex by the draw ratio.

[0088] Example 3 The same procedure as in Example 1 was carried out, except that an undrawn yarn was obtained by the method of Example 1 and then the single yarn fineness was adjusted to 3.3 dtex by the draw ratio.

[0089] Example 4 The same procedure as in Example 1 was carried out, except that the calcium carbonate content of the PET in Example 1 was changed to 8.0% by mass.

[0090] Example 5 The same procedure as in Example 1 was carried out, except that the calcium carbonate content of the PET in Example 1 was changed to 15.0% by mass.

[0091] Example 6: PET containing 10% by mass of calcium carbonate and HDPE containing 10% by mass of calcium carbonate were melt-extruded at 285°C using an extruder attached to a composite fiber spinning machine. Using a spinneret with multiple holes, the two components were concentrically spun in a 40 / 60 (sheath / core) mass ratio to form a core-sheath structure with PET on the core side and HDPE on the sheath side. The spun yarn was cooled by airflow, oiled using an oiling guide, and focused using a focusing guide. It was then pulled by a roller at a spinning speed of 1240 m / min and spun down into a can. The resulting undrawn yarn was drawn 2.7 times in a drawing device at a drawing temperature of 70°C, mechanically crimped, and heat-set at 120°C without tension. The resultant yarn was then cut to obtain staple fibers (short fibers) with a single yarn fineness of 2.4 dtex.

[0092] Example 7 Polyethylene terephthalate (PET) was dried as a polyester resin by conventional methods. Separately, high-density polyethylene (HDPE) was prepared as a polyolefin resin. The calcium carbonate content of HDPE and the HDPE was adjusted to 5.0% by mass, and each was fed into a conjugate fiber spinning machine. The resulting mixture was melt-extruded at 285°C using an extruder attached to the conjugate fiber spinning machine. Using a spinneret with multiple holes, conjugate spinning was performed to form a core-sheath structure in which the two components were concentrically spun in a 40 / 60 (sheath / core) mass ratio, with PET positioned on the core side and HDPE positioned on the sheath side. The spun yarn was cooled by airflow, oiled using an oiling guide, and converged using a converging guide. It was then pulled by a roller at a spinning speed of 1240 m / min and wound on a winder. The resulting fiber (undrawn yarn) had a single yarn fineness of 5.0 dtex. Next, this was drawn 2.4 times in a drawing device at a speed of 40 m / min and a drawing temperature of 70° C., and then drawn 0.95 times at a drawing temperature of 110° C., and heat set at 120° C. These spinning and drawing steps yielded a core-sheath composite fiber with a single filament fineness of 2.3 dtex, in which PET was arranged on the core side and HDPE was arranged on the sheath side concentrically in a mass ratio of 40 / 60 (sheath / core).

[0093] Example 8 The same procedure as in Example 7 was carried out, except that the calcium carbonate content of the HDPE in Example 7 was changed to 20.0 mass %.

[0094] Comparative Example 1 The same procedure as in Example 1 was carried out, except that the calcium carbonate content was changed to 1.0 mass % and the stretching and heat treatment were not carried out.

[0095] Comparative Example 2 The same procedure as in Example 1 was carried out, except that the calcium carbonate content was changed to 1.0 mass %.

[0096] Comparative Example 3 The same procedure as in Example 1 was carried out, except that the stretching and heat treatment were not carried out.

[0097] Comparative Example 4 The same procedure as in Example 7 was carried out except that the stretching and heat treatment were not carried out.

[0098]

[0099] The core-sheath composite fiber of the present invention can be suitably used for applications such as absorbent articles for sanitary materials such as diapers, napkins, and pads, medical and sanitary materials, daily living materials, general medical materials, bedding materials, filter materials, nursing care products, and pet products.

Claims

1. A sheath-core composite fiber composed of a core component containing a polyester-based resin and a sheath component containing a polyolefin-based resin having a melting point 20°C or more lower than the melting point of the polyester-based resin, wherein one or both of the core component and the sheath component contain calcium carbonate in an amount of more than 1.0% by mass and not more than 30.0% by mass per 100% by mass of each component, the maximum crystal melting peak temperature of the core component measured with a differential scanning calorimeter is lower than 255°C, and the L value indicating the hue of the core-sheath composite fiber is 91 or more and the b value is 5.0 or less.

2. The core-sheath composite fiber according to claim 1, wherein the core component has a temperature-lowering crystallization peak temperature of 190°C to 220°C as measured by a differential scanning calorimeter.

3. The core-sheath composite fiber according to claim 1 or 2, wherein the polyester resin contains polyethylene terephthalate and the polyolefin resin contains polyethylene.

4. A core-sheath composite fiber according to claim 1 or 2, in which the content of the polyester resin in the entire fiber is 40 mass% or more.

5. The core-sheath composite fiber according to claim 1 or 2, wherein the cross-sectional shape of the fiber is concentric, eccentric or hollow.

6. The core-sheath composite fiber according to claim 1 or 2, having a tensile strength of 0.80 to 5.00 cN / dtex as measured in accordance with JIS L1013 8.5.

1.

7. The core-sheath composite fiber according to claim 1 or 2, which has an elongation of 30 to 200% as measured in accordance with JIS L1013 8.5.

1.

8. A nonwoven fabric formed from the core-sheath composite fiber according to claim 1 or 2.

Citation Information

Patent Citations

  • Recycled polyester conjugate fiber

    JP2006328600A

  • Multifilament polyester fiber

    JP2019112759A

  • CaCO3 IN POLYESTER FOR NONWOVEN FABRICS AND FIBERS

    JP2020090771A

  • Eccentric core-sheath composite fibers

    JP2021055231A

  • Game machine

    JP2023058130A

Cited By

  • Polyester fiber and nonwoven fabric formed therefrom

    WO2025070344A1