Resin composition and hot-melt adhesive composition
The resin composition, comprising polyolefin and acid-modified polyolefin resins, styrene-isobutylene-styrene block copolymer, adhesion promoter, and filler, addresses the challenge of achieving water vapor barrier and thermal shock resistance in low-pressure molding for electrical and electronic components, ensuring effective sealing and insulation.
Patent Information
- Application Number
- PCT/JP2024/003693
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-02-05
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional resin compositions used in low-pressure molding for electrical and electronic components lack sufficient water vapor barrier properties while maintaining resin fluidity and thermal shock resistance, leading to inadequate sealing and insulation.
A resin composition comprising a polyolefin resin, acid-modified polyolefin resin, styrene-isobutylene-styrene block copolymer, adhesion promoter, and filler, specifically formulated to achieve excellent water vapor barrier properties, adhesiveness, and thermal shock resistance, with optimized ratios and properties of each component to ensure effective sealing and insulation.
The resin composition provides excellent water vapor barrier properties, adhesiveness, and thermal shock resistance, making it suitable for high-performance sealing of electrical and electronic components, particularly in low-pressure molding applications.
Smart Images

Figure JP2024003693_03102024_PF_FP_ABST
Abstract
Description
Resin composition and hot melt adhesive composition
[0001] The present invention relates to a resin composition, and more particularly to a resin composition and a hot melt adhesive composition that are excellent in fluidity, water vapor barrier properties, adhesive properties, and thermal shock resistance.
[0002] Two-component curing epoxy resins and silicone resins have generally been used as insulating resins for sealing electrical and electronic components used in automobiles, electrical appliances, and other products. However, these require a long process time and there is a risk that the electrical and electronic components may be damaged due to shrinkage stress during curing. Therefore, in recent years, low-pressure molding using thermoplastic resins has become popular for sealing electrical and electronic components.
[0003]
[0003] From the viewpoints of electrical insulation, water resistance, durability, and melt viscosity, polyester resins are used as suitable materials for sealing resins for electrical and electronic components. However, in low-temperature, low-pressure molding to reduce damage to the electrical and electronic components, the adhesion between the electrical and electronic components and the sealing resin becomes insufficient, and the desired electrical insulation and waterproof properties are often not fully exhibited. Therefore, attempts to incorporate adhesion promoters having functional groups, etc., in order to improve adhesion have been actively investigated (e.g., Patent Document 1).
[0004] Japanese Patent Application Laid-Open No. 2004-210893
[0005] In recent years, electrical and electronic components are sometimes required to have high water vapor barrier properties in addition to the required physical properties described above, but when a thermoplastic resin containing an adhesion promoter as disclosed in Patent Document 1 is used, although the adhesiveness is improved, there is a problem in that the water vapor barrier properties are not ensured. Conventional techniques have not proposed an encapsulating resin composition that can achieve water vapor barrier properties while maintaining the fluidity, adhesiveness, and thermal shock resistance of resins that are particularly excellent in low-pressure molding.
[0006] The present invention has been made in view of the problems of the conventional art. That is, an object of the present invention is to provide a resin composition that has excellent water vapor barrier properties while maintaining the fluidity, adhesiveness, and thermal shock resistance of resins that are excellent in low-pressure molding.
[0007] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by the following means, and have arrived at the present invention. That is, the present invention has the following configurations. (1) A resin composition containing a polyolefin resin (A), an acid-modified polyolefin resin (B), a styrene-isobutylene-styrene block copolymer (C), an adhesion promoter (D), and a filler (E), wherein, when the total of the polyolefin resin (A), the acid-modified polyolefin resin (B), the styrene-isobutylene-styrene block copolymer (C), and the adhesion promoter (D) is taken as 100 parts by mass, the content of the styrene-isobutylene-styrene block copolymer (C) is 8 to 32 parts by mass, the content of the adhesion promoter (D) is 8 to 27 parts by mass, and the content of the filler (E) is 1 to 13 parts by mass, and the filler (E) is plate-shaped. (2) The resin composition according to (1), wherein the polyolefin resin (A) contains a polypropylene resin and further contains at least one of an ethylene-α-olefin copolymer and a propylene-α-olefin copolymer. (3) The resin composition according to (1) or (2), wherein the acid-modified polyolefin resin (B) has a melting point of 100°C or higher. (4) The resin composition according to any one of (1) to (3), wherein the styrene content of the styrene-isobutylene-styrene block copolymer (C) is 10 to 30% by weight. (5) The resin composition according to any one of (1) to (4), wherein the hydroxyl value of the tackifier (D) is 1 to 100 mgKOH / g. (6) The resin composition according to any one of (1) to (5), wherein, when the total of the polyolefin resin (A), the acid-modified polyolefin resin (B), the styrene-isobutylene-styrene block copolymer (C), and the tackifier (D) is 100 parts by mass, the content of the polyolefin resin (A) is 38 to 70 parts by mass and the content of the acid-modified polyolefin resin (B) is 1 to 22 parts by mass. (7) A hot melt adhesive composition containing the resin composition according to any one of (1) to (6).
[0008] The resin composition of the present invention exhibits excellent resin fluidity, adhesiveness, and thermal shock resistance in low-pressure molding, and further has excellent water vapor barrier properties. Therefore, by using it as a sealing material for products that require high levels of waterproofing, it is possible to produce products that satisfy water vapor barrier properties. In particular, the resin composition of the present invention can be used as a hot melt adhesive, and is particularly suitable for sealing electrical and electronic components.
[0009] FIG. 1 shows a schematic diagram of a chart measured by a differential scanning calorimeter.
[0010] The present invention will be described in detail below.
[0011] <Polyolefin Resin (A)> The resin composition of the present invention contains a polyolefin resin (A). The inclusion of the polyolefin resin (A) can impart good water vapor barrier properties to the resin composition. While the polyolefin resin (A) used in the present invention is not particularly limited, polypropylene resin is preferred from the viewpoint of water vapor barrier properties. Furthermore, ethylene-α-olefin copolymers and propylene-α-olefin copolymers are preferred from the viewpoint of adhesion to metals and films. To achieve both high water vapor barrier properties and adhesive properties, polypropylene resins can also be used in combination with ethylene-α-olefin copolymers or propylene-α-olefin copolymers. Here, polypropylene resin refers to a so-called homopolypropylene composed primarily of propylene units, which does not contain copolymerized components such as α-olefins other than propylene, or if it does contain such components, it is contained in a very small amount, at most about 1 mol %. Furthermore, the polyolefin resin (A) does not fall under the category of the acid-modified polyolefin resin (B) described below, and refers to a resin that is not acid-modified.
[0012] When a polypropylene resin and an ethylene-α-olefin copolymer and / or a propylene-α-olefin copolymer (hereinafter collectively referred to as an olefin copolymer) are used in combination as the polyolefin resin (A), the blending ratio of polypropylene resin / olefin copolymer is preferably 20 / 80 to 80 / 20 by mass, more preferably 30 / 70 to 70 / 30, and even more preferably 40 / 60 to 60 / 40. By keeping the ratio within the above range, it is possible to achieve a high level of both water vapor barrier properties and adhesive properties.
[0013] The polyolefin resin (A) used in the present invention preferably has a melt mass-flow rate (hereinafter sometimes abbreviated as MFR) of 10 to 70 g / 10 min, measured according to JIS K 7210-1:2014 (test temperature 190°C, nominal load 2.16 kg). By setting the MFR at or above the lower limit, the resin maintains an appropriate level of fluidity, resulting in good moldability. Furthermore, by setting the MFR at or below the upper limit, the resin composition is prevented from becoming extremely soft due to a decrease in viscosity, resulting in good mechanical properties. When the polyolefin resin (A) contains multiple types of polyolefin resins, it is preferable that each of the polyolefin resins is within the above range.
[0014] When the resin composition of the present invention is used as a hot melt adhesive, rapid melting at 210 to 240°C is required for molding without causing thermal degradation of the resin as much as possible, so the upper limit of the melting point of the polyolefin resin (A) is desirably 210°C. Preferably, it is 200°C or lower, more preferably 190°C or lower. The lower limit is preferably 90°C or higher, more preferably 100°C or higher, even more preferably 110°C or higher, and particularly preferably 120°C or higher. It is preferable that the melting point be 5 to 10°C higher than the heat resistance temperature required for the relevant application. When the polyolefin resin (A) contains multiple types of polyolefin resins, it is preferable that each of the polyolefin resins is within the above range.
[0015] The content of polyolefin resin (A) in the resin composition of the present invention is preferably 38 parts by mass or more, more preferably 40 parts by mass or more, even more preferably 42 parts by mass or more, and particularly preferably 48 parts by mass or more, based on 100 parts by mass of the total of polyolefin resin (A), acid-modified polyolefin resin (B), styrene-isobutylene-styrene block copolymer (C), and adhesion promoter (D). It is also preferably 70 parts by mass or less, more preferably 68 parts by mass or less, and even more preferably 63 parts by mass or less. When the content ratio of polyolefin resin (A) is equal to or greater than the lower limit, the resin composition can be imparted with particularly good water vapor barrier properties. When the content ratio is equal to or less than the upper limit, the resin composition has good thermal shock resistance.
[0016] <Acid-Modified Polyolefin Resin (B)> The resin composition of the present invention contains an acid-modified polyolefin resin (B). The inclusion of the acid-modified polyolefin resin (B) can provide good dispersibility with the polyolefin resin (A), the styrene-isobutylene-styrene block copolymer (C), the adhesion promoter (D), and the filler (E), thereby imparting appropriate adhesiveness, thermal shock resistance, and water vapor barrier properties to the resin composition. The acid-modified polyolefin resin (B) is not particularly limited, and may be any resin having a polyolefin segment and a carboxylic acid segment. Examples include ethylene-unsaturated carboxylic acid copolymers such as ethylene-vinyl acetate-maleic anhydride terpolymer and ethylene-ethyl acrylate-maleic anhydride terpolymer, and unsaturated carboxylic acid-grafted polyolefin resins such as maleic anhydride-grafted polypropylene and maleic anhydride-grafted propylene-α-olefin copolymer. Among these, unsaturated carboxylic acid-grafted polyolefin resins are preferred, and it is more preferred that the unsaturated carboxylic acid used for graft modification is maleic anhydride.
[0017] The melting point of the acid-modified polyolefin resin (B) used in the present invention is preferably 100° C. or higher, more preferably 110° C. or higher, and even more preferably 120° C. or higher. It is also preferably 160° C. or lower, more preferably 150° C. or lower. When the melting point of the acid-modified polyolefin resin (B) is the lower limit or higher, the resin composition has good heat resistance, and when the melting point is the upper limit or lower, the resin composition has good flowability during molding.
[0018] The content of the acid-modified polyolefin resin (B) in the resin composition of the present invention is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the total of the polyolefin resin (A), the acid-modified polyolefin resin (B), the styrene-isobutylene-styrene block copolymer (C), and the tackifier (D). It is also preferably 22 parts by mass or less, more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, and particularly preferably 10 parts by mass or less. When the content of the acid-modified polyolefin resin (B) is equal to or greater than the lower limit, dispersibility with the polyolefin resin (A), the styrene-isobutylene-styrene block copolymer (C), the tackifier (D), and the filler (E) is improved. When the content of the acid-modified polyolefin resin (B) is equal to or less than the upper limit, mechanical properties are improved.
[0019] <Styrene-Isobutylene-Styrene Block Copolymer (C)> The resin composition of the present invention contains a styrene-isobutylene-styrene block copolymer (C). By containing the styrene-isobutylene-styrene block copolymer (C), it is possible to impart appropriate thermal shock resistance to the resin composition. The styrene-isobutylene-styrene block copolymer (C) used in the present invention is not particularly limited, but a triblock structure is preferred from the viewpoints of water vapor barrier properties and thermal shock resistance.
[0020] The styrene content of the styrene-isobutylene-styrene block copolymer (C) used in the present invention is preferably 10% by weight or more, more preferably 13% by weight or more, and even more preferably 15% by weight or more. It is also preferably 30% by weight or less, more preferably 25% by weight or less, and even more preferably 20% by weight or less. When the styrene content of the styrene-isobutylene-styrene block copolymer (C) is equal to or greater than the above-mentioned lower limit, the heat resistance is improved. When the styrene content of the styrene-isobutylene-styrene block copolymer (C) is equal to or less than the above-mentioned upper limit, the flexibility is increased and the thermal shock resistance is improved.
[0021] The content of the styrene-isobutylene-styrene block copolymer (C) in the resin composition of the present invention must be 8 parts by mass or more, relative to 100 parts by mass of the total of the polyolefin resin (A), acid-modified polyolefin resin (B), styrene-isobutylene-styrene block copolymer (C), and adhesion promoter (D). It is preferably 10 parts by mass or more, more preferably 12 parts by mass or more, even more preferably 15 parts by mass or more, and particularly preferably 18 parts by mass or more. It must also be 32 parts by mass or less. It is preferably 30 parts by mass or less, more preferably 28 parts by mass or less, even more preferably 25 parts by mass or less, and particularly preferably 22 parts by mass or less. When the content ratio of the styrene-isobutylene-styrene block copolymer (C) is equal to or greater than the aforementioned lower limit, the thermal shock resistance is improved. When the content ratio of the styrene-isobutylene-styrene block copolymer (C) is equal to or less than the aforementioned upper limit, the fluidity of the resin is increased, resulting in improved moldability.
[0022] <Adhesion imparter (D)> The resin composition of the present invention contains an adhesion imparter (D). By containing the adhesion imparter (D), good adhesion can be imparted when the resin composition is used as a sealant, and the flowability of the resin composition can be appropriately improved. The adhesion imparter (D) used in the present invention is not particularly limited, and a phenolic compound, a xylene-modified phenolic resin, a terpene-modified phenolic resin, a hydrogenated terpene-modified phenolic resin obtained by hydrogenating a terpene-modified phenolic resin, or the like can be used. In particular, from the viewpoint of compatibility with the polyolefin resin (A), a xylene-modified phenolic resin or a terpene-modified phenolic resin is preferred.
[0023] The adhesion promoter (D) used in the present invention preferably has a hydroxyl group. When the adhesion promoter (D) has a hydroxyl group, it exhibits the effect of improving wettability to the substrate, improving adhesion to the substrate, and improving insulating properties. The hydroxyl value of the adhesion promoter (D) is preferably 1 mgKOH / g or more, more preferably 30 mgKOH / g or more, and even more preferably 50 mgKOH / g or more. Also, it is preferably 100 mgKOH / g or less, more preferably 90 mgKOH / g or less, even more preferably 80 mgKOH / g or less, and particularly preferably 70 mgKOH / g or less. When the hydroxyl value is below the upper limit, it is possible to appropriately maintain moisture permeability while improving adhesion.
[0024] The hydroxyl value can be measured, for example, by potentiometric titration as specified in JIS K 0070:1992.
[0025] The content of the tackifier (D) in the resin composition of the present invention must be 8 parts by mass or more, relative to 100 parts by mass of the total of the polyolefin resin (A), acid-modified polyolefin resin (B), styrene-isobutylene-styrene block copolymer (C), and tackifier (D). It is preferably 10 parts by mass or more, more preferably 13 parts by mass or more, and even more preferably 15 parts by mass or more. It must also be 27 parts by mass or less, and is preferably 25 parts by mass or less, more preferably 22 parts by mass or less, and even more preferably 20 parts by mass or less. When the content of the tackifier (D) is within the above range, particularly good adhesive properties can be exhibited. Furthermore, a decrease in adhesive properties due to a decrease in flexibility or embrittlement of the resin composition is suppressed.
[0026] <Filler (E)> The resin composition of the present invention contains a filler (E). The inclusion of the filler (E) can impart good water vapor barrier properties to the resin composition. The filler (E) used in the present invention is not particularly limited, and glass beads, calcium carbonate, kaolin, talc, glass fiber, carbon fiber, clay, etc. can be used. The filler (E) used in the present invention is plate-shaped. By making the filler (E) plate-shaped, the water vapor barrier properties are particularly improved. Here, "plate-shaped" refers to a plate-like shape in which the height of the filler is extremely small compared to its width and depth. The aspect ratio of the filler (E), i.e., the ratio of the minor axis to the major axis of the filler (E) (major axis / minor axis), is preferably 3 to 500. The aspect ratio of the filler (E) may be 5 or more, 10 or more, 20 or more, 50 or more, 100 or more, or 450 or less, 400 or less, 350 or less, 300 or less, or 200 or less. The aspect ratio of the filler (E) can be determined by a method such as automatic area measurement of an image obtained by observing the filler (E) with an electron microscope. If the aspect ratio of the filler (E) is too low, the water vapor barrier property will be reduced, and if the aspect ratio is too high, the dispersibility will be deteriorated and the mechanical properties may be reduced.
[0027] The content of the filler (E) in the resin composition of the present invention must be 1 part by mass or more, preferably 2 parts by mass or more, and more preferably 4 parts by mass or more, relative to 100 parts by mass of the total of the polyolefin resin (A), the acid-modified polyolefin resin (B), the styrene-isobutylene-styrene block copolymer (C), and the adhesion promoter (D). When the content of the filler (E) is equal to or greater than the lower limit, the water vapor barrier property is improved. Furthermore, the mechanical properties of the resin composition are improved, and the shear adhesive strength may be improved. Furthermore, the content of the filler (E) must be 13 parts by mass or less, preferably 10 parts by mass or less, and more preferably 8 parts by mass or less. When the content of the filler (E) is equal to or less than the upper limit, the adhesiveness is improved.
[0028] The particle size (D50) of the filler (D) in the resin composition of the present invention may be, for example, 1 to 50 μm. The particle size (D50) can be measured, for example, by laser diffraction or dynamic light scattering.
[0029] <Resin Composition> The resin composition of the present invention contains at least the polyolefin resin (A), the acid-modified polyolefin resin (B), the styrene-isobutylene-styrene block copolymer (C), the adhesion promoter (D), and the filler (E). If necessary, it may further contain various additives such as an antioxidant.
[0030] The resin composition of the present invention preferably has a melt viscosity of 5 to 1500 dPa·s at 240°C. The melt viscosity of the resin composition can be achieved by appropriately adjusting the types and blending ratios of the polyolefin resin (A), acid-modified polyolefin resin (B), styrene-isobutylene-styrene block copolymer (C), adhesion promoter (D), and filler (E). The melt viscosity at 240°C is a value measured as follows. That is, the resin composition is dried to a moisture content of 0.1% or less, and then heated to 240°C and stabilized using a flow tester (model CFT-500C) manufactured by Shimadzu Corporation. The resin composition is passed through a 10 mm thick die having a 1.0 mm hole diameter at a pressure of 98 N / cm. 2This is the measured viscosity when the resin composition is passed through at a pressure of 1500 dPa·s or less, preferably 1000 dPa·s or less. By using a resin composition having a melt viscosity of 1500 dPa·s or less, and preferably 1000 dPa·s or less, a product with excellent electrical insulation can be obtained at a relatively low injection pressure of 0.1 to 20 MPa without impairing its properties. Furthermore, from the viewpoint of the resin composition injection operation, a lower melt viscosity at 230°C is preferable, but considering the adhesiveness and cohesive strength of the resin composition, the lower limit is preferably 5 dPa·s or more, more preferably 10 dPa·s or more, more preferably 30 dPa·s or more, and most preferably 50 dPa·s or more.
[0031] The resin composition of the present invention may further contain an antioxidant. The antioxidant used in the present invention is not particularly limited as long as it can prevent oxidation of the polyolefin resin (A), and hindered phenol-based antioxidants, phosphorus-based antioxidants, thioether-based antioxidants, etc. can be used. For example, hindered phenol-based antioxidants include 1,3,5-tris(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, 1,1,3-tri(4-hydroxy-2-methyl-5-t-butylphenyl)butane, 1,1-bis(3-t-butyl-6-methyl-4-hydroxyphenyl)butane, 3,5-bis(1,1-dimethylethyl)-4-hydroxy-benzenepropanoic acid, pentaerythrityl tetraki ...1,1-bis(1,1-dimethylethyl)-4-hydroxy-benzenepropanoic acid, and pentaerythrityl tetrakis(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate. hydroxyphenyl)propionate, 3-(1,1-dimethylethyl)-4-hydroxy-5-methyl-benzenepropanoic acid, 3,9-bis[1,1-dimethyl-2-[(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, 1,3,5-trimethyl-2,4,6-tris(3',5'-di-t-butyl-4'-hydroxybenzyl)benzene, as phosphorus-based compounds, 3,9- Bis(p-nonylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 3,9-bis(octadecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, tri(mononylphenyl)phosphite, triphenoxyphosphine, isodecyl phosphite, isodecylphenyl phosphite, diphenyl 2-ethylhexyl phosphite, dinonylphenylbis(nonyl phenyl) ester phosphorus acid, 1,1,3-tris(2-methyl-4-ditridecylphosphite-5-t-butylphenyl)butane, tris(2,4-di-t-butylphenyl)phosphite, pentaerythritol bis(2,4-di-t-butylphenyl phosphite), 2,2'-methylenebis(4,6-di-t-butylphenyl)2-ethylhexyl phosphite, bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite, thioether-based 4,Examples include 4'-thiobis[2-t-butyl-5-methylphenol]bis[3-(dodecylthio)propionate], thiobis[2-(1,1-dimethylethyl)-5-methyl-4,1-phenylene]bis[3-(tetradecylthio)propionate], pentaerythritol tetrakis(3-n-dodecylthiopropionate), and bis(tridecyl)thiodipropionate, which can be used alone or in combination.
[0032] The content of the antioxidant is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.3 parts by mass or more, per 100 parts by mass of the total of the polyolefin resin (A), acid-modified polyolefin resin (B), styrene-isobutylene-styrene block copolymer (C), and adhesion promoter (D). If the content is too low, it may have an adverse effect on long-term durability at high temperatures. It is also preferably 5 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 1 part by mass or less. If the content is too high, it may have an adverse effect on adhesion, etc.
[0033] The resin composition of the present invention may also contain other resins, such as polyamides, polycarbonates, acrylics, and ethylene vinyl acetates, that do not fall under any of the polyolefin resin (A), acid-modified polyolefin resin (B), styrene-isobutylene-styrene block copolymer (C), adhesion promoter (D), and filler (E), as long as the effects of the present invention are not impaired. The inclusion of these components may improve adhesion, flexibility, durability, and other properties. In this case, the polyolefin resin (A) is preferably contained in an amount of 30 to 70 wt %, more preferably 40 to 60 wt %, based on the total resin composition of the present invention. If the content of polyolefin resin (A) is too low, the excellent water vapor barrier properties and durability inherent to the polyolefin resin (A) tend to be reduced, while if the content is too high, flexibility and adhesion tend to be reduced.
[0034] Furthermore, when weather resistance is required for the resin composition of the present invention, it is preferable to add a light stabilizer, such as a benzotriazole-based light stabilizer, a benzophenone-based light stabilizer, a hindered amine-based light stabilizer, a nickel-based light stabilizer, or a benzoate-based light stabilizer. Examples of the benzotriazole light stabilizer include 2-(3,5-di-tert-amyl-2'hydroxyphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2H-benzotriazol-2-yl)-p-cresol, 2-(2'-hydroxy-5'-methylphenyl)-benzotriazole, 2,4-di-tert-butyl-6-(5-chlorobenzotriazol-2-yl)phenol, and 2-[2-hydroxy-3,5-di(1,1-dimethylbenzyl)]-2H-benzotriazole. Examples of the benzophenone-based light stabilizer include 2-hydroxy-4-(octyloxy)benzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-benzophenone-5-sulfonic acid, 2-hydroxy-4-n-dodecyloxybenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2-2'-dihydroxy-4-methoxybenzophenone, and 2,2'-dihydroxy-4,4'-dimethoxybenzophenone.Examples of the hindered amine light stabilizer include bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate, dimethyl succinate / 1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine polycondensate, poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl) imino}hexamethylene(2,2,6,6-tetramethyl-4-piperidyl)imino}], 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-s-triazine-2,4,6(1H,3H,5H)trione, tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-s-triazine-2,4,6-(1H,3H,5H)trione, etc. Examples of nickel-based light stabilizers include [2,2'-thio-bis(4-tert-octylphenolate)]-2-ethylhexylamine-nickel-(II), nickel dibutyldithiocarbamate, and [2',2'-thio-bis(4-tert-octylphenolate)]-n-butylamine-nickel. Benzoate-based light stabilizers include 2,4-di-t-butylphenyl-3,5'-di-tert-butyl-4'-hydroxybenzoate. These light stabilizers can be used alone or in combination. When added, the amount added is preferably 0.1% by mass or more and 5% by mass or less of the entire resin composition. If it is less than 0.1% by mass, the weather resistance effect may be poor. If it exceeds 5% by mass, it may have a negative effect on adhesion, etc.
[0035] <Hot Melt Adhesive Composition> The resin composition of the present invention can be used as a hot melt adhesive composition. As a hot melt adhesive composition, it can be suitably used, for example, as a sealant for electrical and electronic components. As a specific example of a method of use, the resin composition of the present invention can be injected into a mold in which a product to be waterproofed is set, thereby obtaining a molded product that seals the product. More specifically, when a screw-type hot melt molding applicator is used, the composition is heated and melted at approximately 180 to 250°C, and injected into a mold through an injection nozzle. After a certain cooling time, the molded product can be removed from the mold to obtain the molded product.
[0036] The type of hot melt molding applicator is not particularly limited, but examples include a vertical extrusion molding machine IMC-18F9 manufactured by Imoto Manufacturing Co., Ltd., and a hybrid small vertical injection molding machine STX20 or THX5S1VN manufactured by Nissei Plastic Industrial Co., Ltd.
[0037] In order to explain the present invention in more detail, examples and comparative examples are given below, but the present invention is not limited to these examples. The measured values described in the examples and comparative examples were measured by the following methods.
[0038] <Measurement of Melting Point> Using a differential scanning calorimeter "DSC220" manufactured by Seiko Instruments Inc., 5 mg of a measurement sample (polyolefin resin (A) or acid-modified polyolefin resin (B)) was placed in an aluminum pan, the pan was sealed with a lid, and the pan was heated to 230°C at a heating rate of 20°C / min to melt. Next, the pan was cooled to -130°C at a heating rate of 20°C / min using liquid nitrogen, held for 5 minutes, and then measured from -130°C to 230°C at a heating rate of 20°C / min. The minimum point of the endothermic peak in the obtained curve as shown in Figure 1 (marked with an x in the figure) was taken as the melting point (Tm).
[0039] <Hydroxyl Value> The hydroxyl value of the adhesion promoter (D) was measured by the potentiometric titration method specified in JIS K 0070:1992.
[0040] <Melt Viscosity> Using a Shimadzu flow tester (CFT-500C type), the cylinder at the center of the heater set to 240°C was filled with compounded raw materials or resin compositions dried to a moisture content of 0.1% or less. One minute after filling, a load was applied to the sample via the plunger, and the molten sample was extruded from a die (hole diameter: 1.0 mm, thickness: 10 mm) at the bottom of the cylinder at a pressure of 98 N / cm2. The plunger's descent distance and descent time were recorded, and the melt viscosity was calculated. From the melt viscosity value, the melting characteristics (fluidity) were evaluated according to the following evaluation criteria. Evaluation criteria: ◯: Melt viscosity @ 240°C 5 dPa·s or more and less than 1000 dPa·s △: Melt viscosity @ 240°C 1000 dPa·s or more and less than 1500 dPa·s ×: Melt viscosity @ 240°C 1500 dPa·s or more
[0041] <Water Vapor Barrier Property> A film having a thickness of approximately 120 μm was produced from the resin composition by heat pressing using a heat press machine (SA-303 manufactured by Tester Sangyo Co., Ltd.). The heat pressing conditions were a temperature of 200°C, a press pressure of 10 MPa, and a press time of 30 seconds. Test specimens based on JIS Z0208:1976 were cut out from the heat-pressed film using a cutter. The film was then set in a jig specified in JIS Z0208:1976 and allowed to stand for a total of 96 hours in an environment of 25°C and 90% relative humidity (RH). The sample was removed 24 hours, 48 hours, 72 hours, and 96 hours after the start of the test, and the weight was measured. The moisture permeability (water vapor barrier property) was calculated from the weight of water absorbed by calcium chloride every 24 hours between (1) 24 hours and 48 hours, (2) 48 hours and 72 hours, and (3) 72 hours and 96 hours, and the average of the three moisture permeability values was taken as the moisture permeability. The moisture permeability was calculated using the following formula. The moisture permeability area refers to the area of the film made from the resin composition. Moisture permeability (g / (m 2 24h)) = (240 × m) / (t × s) m: Sum of the increased mass (mg) in the last two weighing intervals in the test t: Time between the last two weighing intervals in the test = 24h s: Moisture permeability area (cm 2 ) Evaluation criteria ◎: Moisture permeability 0.5 (g / (m 2 Less than 24h) ◯: Moisture permeability 0.5 (g / (m 2 ・24h)) or more 1.0(g / (m 2 Less than 24h) △: Moisture permeability 1.0 (g / (m 2 ・24h)) or more 1.5(g / (m 2 Less than 24h) ×: Moisture permeability 1.5 (g / (m 2 ・24 hours or more
[0042] <Adhesion Test (T-Peel Adhesion Strength)> Method for Preparing T-Peel Adhesion Test Pieces A substrate (aluminum substrate: A5052 (thickness: 0.1 mm)) was cut to a size of 40 mm x 25 mm, and the surface was wiped with acetone to remove oil. Next, a film approximately 200 μm thick was produced from the resin composition by heat pressing using a heat press machine (SA-303 manufactured by Tester Sangyo Co., Ltd.). The heat pressing conditions were a temperature of 200°C, a press pressure of 6 MPa, and a press time of 10 seconds. A piece of 20 mm x 25 mm was cut from the heat-pressed film, two of which were stacked, sandwiched between pre-cut aluminum substrates, and heat-sealed using a heat seal tester (TP-701-B manufactured by Tester Sangyo Co., Ltd.). The heat sealing conditions were a temperature of 220°C, a pressure of 0.4 MPa, and a press time of 30 seconds, yielding a T-peel adhesion test piece in which a film made of the resin composition was sandwiched between aluminum substrates.
[0043] T-peel adhesive strength test method: The T-peel adhesive strength test piece was clamped with an autograph (AG-IS manufactured by Shimadzu Corporation) by chucking the aluminum substrate, and the film layer made of the resin composition was peeled off by T-peel in a 25°C or 90°C environment, and the T-peel adhesive strength was measured. The pulling speed was 300 mm / min. Evaluation criteria: ○: T-peel adhesive strength of 70 N / 25 mm or more; △: T-peel adhesive strength of 40 N / 25 mm or more but less than 70 N / 25 mm; ×: T-peel adhesive strength of less than 40 N / 25 mm
[0044] <Thermal Shock Resistance Test> Method for Preparing a Thermal Shock Resistance Test Sample A substrate (aluminum substrate: A5052 (40 mm x 30 mm x 5 mm thick)) was machined to 30 mm x 1 mm x 1 mm, and the machined portion was blasted to an Rz (surface roughness) of approximately 5 μm. The surface was wiped with acetone to remove oil. Next, the substrate was set in a predetermined mold, and a resin composition was injection molded and filled into the machined portion using an injection molding machine (Nissei Plastic Industrial Co., Ltd., hybrid small vertical injection molding machine THX5S1VN). The injection molding conditions were a temperature of 240 ° C, a mold temperature of 80 ° C, an injection speed of 30 mm / s, a holding pressure of 50 MPa, an injection time of 10 seconds, a holding pressure time of 20 seconds, and a press time of 10 seconds. A thermal shock resistance test sample was obtained in which the resin composition was adhered to the machined aluminum substrate portion.
[0045] Thermal Shock Resistance Test Method The thermal shock resistance test sample was subjected to a thermal shock test in a thermal shock test chamber (TSE-11 manufactured by Espec Corporation) under an environment of -45°C and 95°C (1 cycle: -45°C for 9 minutes, 95°C for 10 minutes), and the test was carried out up to 2000 cycles. Evaluation criteria: ○: No cracking or peeling of the resin composition from the aluminum substrate after 2000 cycles; ×: Cracking or peeling of the resin composition from the aluminum substrate after 2000 cycles.
[0046] Examples 1 to 9, Comparative Examples 1 to 8 Resin compositions 1 to 17 were obtained by melt-kneading polyolefin resin (A), acid-modified polyolefin resin (B), styrene-isobutylene-styrene block copolymer (C) (styrene-ethylene-butylene-styrene block copolymer for resin composition 17), adhesion promoter (D), and filler (E) in the proportions shown in Table 1 using a twin-screw extruder at a die temperature of 160°C to 220°C. The melt viscosity, water vapor barrier property, T-peel adhesive strength, and thermal shock resistance of the resin compositions were evaluated using the methods described separately. The evaluation results are shown in Table 1 below.
[0047]
[0048] The polyolefin resin, acid-modified polyolefin resin, styrene-isobutylene-styrene block copolymer, adhesion promoter, and filler used in Table 1 are as follows: Polyolefin resin (A-1): J107G, manufactured by Prime Polymer Co., Ltd., homopolypropylene resin, melting point: 165°C, density: 0.90 g / cm 3 Polyolefin resin (A-2): EUL731, manufactured by Sumitomo Chemical Co., Ltd., ethylene-α-olefin copolymer, melting point: 113 to 117°C, density: 0.90 g / cm 3 Polyolefin resin (A-3): Tafmer PN-20300, manufactured by Mitsui Chemicals, Inc., propylene-α-olefin copolymer, melting point: 160°C, density: 0.87 g / cm 3 Acid-modified polyolefin resin (B-1): PMA H1100P, manufactured by Toyobo Co., Ltd., maleic anhydride graft-modified polypropylene resin, melting point: 147 ° C., molecular weight Mw: 74,000 Styrene-isobutylene-styrene block copolymer (C-1): SIBSTAR 062T, manufactured by Kaneka Corporation, styrene-isobutylene-styrene block copolymer, styrene content: 23 wt%, MFR: 10 g / 10 min (230 ° C, 2.16 kg), density: 0.95 g / cm 3 Styrene-isobutylene-styrene block copolymer (C-2): SIBSTAR 102T, manufactured by Kaneka Corporation, styrene-isobutylene-styrene block copolymer, styrene content: 15 wt%, MFR: 0.6 g / 10 min (230 ° C, 2.16 kg), density: 0.94 g / cm 3Adhesion promoter (D-1): YS Polystar T160, manufactured by Yasuhara Chemical Co., Ltd., terpene-modified phenolic resin, hydroxyl value: 60 mg KOH / g Adhesion promoter (D-2): YS Polystar G150, manufactured by Yasuhara Chemical Co., Ltd., terpene-modified phenolic resin, hydroxyl value: 140 mg KOH / g Filler (E-1): K-1, manufactured by Nippon Talc Co., Ltd., talc, plate-like, particle size (D50): 8.0 μm, aspect ratio: 3 to 10 Filler (E-2): I. 44P, manufactured by Volclay Japan Co., Ltd., montmorillonite, plate-like, size: 14-18 μm, aspect ratio: 100 to 500 Filler (E-3): UBS-0005E, manufactured by Unitika Ltd., glass beads, spherical, particle size: up to 5 μm, aspect ratio: 1 Styrene-ethylene-butylene-styrene block copolymer (F-1): Tuftec H1043, manufactured by Asahi Kasei Corporation, styrene-ethylene-butylene-styrene block copolymer, styrene content: 67 wt%, MFR: 2.0 g / 10 min (230 ° C, 2.16 kg), density: 0.97 g / cm 3
[0049] As is clear from Table 1, the resin compositions of Examples 1 to 9 all exhibited excellent results in terms of melt viscosity (fluidity), moisture permeability (water vapor barrier property), T-peel adhesive strength (adhesion), and thermal shock resistance. On the other hand, Comparative Example 1 did not contain a filler and therefore exhibited poor water vapor barrier property. Comparative Example 2 contained a large amount of filler, resulting in a high melt viscosity and poor adhesion and thermal shock resistance. Comparative Example 3 contained spherical fillers and therefore exhibited poor water vapor barrier property. Comparative Example 4 contained a small amount of tackifier, resulting in an increased melt viscosity and poor adhesion. Comparative Example 5 contained too much tackifier, which actually reduced adhesion. Comparative Example 6 did not contain a styrene-isobutylene-styrene block copolymer and therefore exhibited poor thermal shock resistance. Comparative Example 7 contained a large amount of styrene-isobutylene-styrene block copolymer and therefore exhibited poor adhesion. Comparative Example 8 used a styrene-ethylene-butylene-styrene block copolymer instead of the styrene-isobutylene-styrene block copolymer and therefore exhibited poor moisture permeability and adhesion.
[0050] The resin composition of the present invention has a low melt viscosity when molded into products, excellent adhesion to aluminum substrates, and excellent water vapor barrier properties and thermal shock resistance, and is therefore useful as a hot melt adhesive composition for waterproofing purposes.
Claims
1. A resin composition comprising a polyolefin resin (A), an acid-modified polyolefin resin (B), a styrene-isobutylene-styrene block copolymer (C), an adhesion promoter (D) and a filler (E), wherein, when the total amount of the polyolefin resin (A), the acid-modified polyolefin resin (B), the styrene-isobutylene-styrene block copolymer (C), and the adhesion promoter (D) is 100 parts by mass, the content of the styrene-isobutylene-styrene block copolymer (C) is 8 to 32 parts by mass, the content of the adhesion promoter (D) is 8 to 27 parts by mass, and the content of the filler (E) is 1 to 13 parts by mass, and the filler (E) is in a plate shape.
2. The resin composition according to claim 1, wherein the polyolefin resin (A) comprises a polypropylene resin and further comprises at least one of an ethylene-α-olefin copolymer and a propylene-α-olefin copolymer.
3. The resin composition according to claim 1, wherein the acid-modified polyolefin resin (B) has a melting point of 100° C. or higher.
4. The resin composition according to claim 1, wherein the styrene content of the styrene-isobutylene-styrene block copolymer (C) is 10 to 30% by weight.
5. The resin composition according to claim 1, wherein the adhesion promoter (D) has a hydroxyl value of 1 to 100 mgKOH / g.
6. The resin composition according to claim 1, wherein the content of the polyolefin resin (A) is 38 to 70 parts by mass, and the content of the acid-modified polyolefin resin (B) is 1 to 22 parts by mass, when the total of the polyolefin resin (A), the acid-modified polyolefin resin (B), the styrene-isobutylene-styrene block copolymer (C) and the adhesion promoter (D) is 100 parts by mass.
7. A hot melt adhesive composition containing the resin composition according to any one of claims 1 to 6.
Citation Information
Patent Citations
Molding resin composition
JP2004210893A
Preparation process of high polymer material for automotive trim product
CN103554692A
Polypropylene resin composition
JP2019099807A
Hot melt adhesive
WO2022181690A1
Cited By
Resin composition and hot-melt adhesive composition
WO2026070646A1