Method for producing wiring board
The method of using a photosensitive material layer on a thermosetting material layer in wiring board manufacturing addresses the challenge of achieving fine wiring and excellent insulation by maintaining the plasma mask as a primer layer, enhancing insulation and electrical properties while simplifying the process and preventing chemical damage.
Patent Information
- Application Number
- PCT/JP2024/005186
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-02-15
- Publication Date
- 2024-10-03
AI Technical Summary
Current methods for manufacturing wiring boards face challenges in achieving both fine wiring and excellent insulation and electrical properties, particularly due to difficulties in aligning via holes and trenches without damaging the insulating material layer, and the complexity of removing mask patterns during the plasma mask peeling process.
A method involving a photosensitive material layer applied on a thermosetting material layer, where the plasma mask remains as a primer layer after forming via holes or trenches, allowing for improved insulation and electrical properties without the need for mask pattern removal, and enabling finer wiring.
This approach results in wiring boards with enhanced insulation performance and electrical properties, preventing chemical damage to the insulating material layer and simplifying the manufacturing process by maintaining the plasma mask as a permanent film, thus allowing for finer circuitry.
Smart Images

Figure JP2024005186_03102024_PF_FP_ABST
Abstract
Description
Method for manufacturing a wiring board
[0001] The present invention relates to a method for manufacturing a wiring board and a semiconductor device.
[0002] In recent years, there has been a demand for thinner wiring boards and finer circuit wiring in wiring boards such as printed wiring boards, semiconductor package substrates, and wafer-level package substrates in order to reduce the size and increase the functionality of electronic devices. As a method for manufacturing a wiring board, for example, the method described in Patent Document 1 has been proposed.
[0003] Japanese Patent Application Laid-Open No. 2022-39763
[0004] In the method of manufacturing a wiring board, a via hole or a trench may be formed on an insulating layer (sometimes referred to as an "insulating material layer"). To form a via hole or a trench on an insulating layer, if the insulating layer is a photosensitive resin, the method involves patterning by exposure and development. If the insulating layer is a thermosetting resin, the method involves laser irradiation or plasma treatment or laser irradiation through a mask. Here, a "via hole" typically refers to a hole that penetrates an insulating layer. A "trench" typically refers to a groove that does not penetrate an insulating layer.
[0005] When the insulating layer is a cured product of a photosensitive material containing a photosensitive resin, photolithography can be utilized, which makes it easy to align the mask pattern and is advantageous for forming small diameter via holes or small diameter trenches. However, it has been difficult to improve the insulating performance and electrical characteristics while maintaining the resolution of the photosensitive material.
[0006] On the other hand, when the insulating layer is a cured product of a thermosetting material highly filled with an inorganic filler, the insulating layer can improve the insulating performance and electrical properties, but the surface irregularities caused by the inorganic filler make it difficult to form fine wiring.
[0007] To solve this problem, insulating materials have been proposed that have a smooth primer layer on the surface that is unfilled with inorganic fillers or contains only small amounts of inorganic fillers. However, this poses the problem of difficulty in accurately aligning the laser irradiation to the land when drilling small diameter vias, resulting in a large area occupied by the via hole or trench.
[0008] On the other hand, via holes and trenches can be formed in cured thermosetting materials, including thermosetting resins, using a peelable photoresist as a plasma mask, but the mask pattern must be removed and peeled off, which increases the number of steps and makes the process complicated. Furthermore, the thermosetting material is exposed to the stripping solution during the stripping process, which can cause damage to the solution.
[0009] An object of the present invention is to provide a method for manufacturing a wiring board that does not require removal of a mask pattern when forming a via hole or a trench, has an insulating material layer with excellent insulating performance and electrical properties, and is capable of fine wiring; and a semiconductor device.
[0010] As a result of extensive research to solve the above-mentioned problems, the present inventors have found that by leaving a mask containing a photosensitive material used in forming via holes or trenches in a thermosetting material as a residual film and leaving it as a primer layer (permanent film), it is possible to achieve excellent insulating performance and electrical properties and enable fine wiring, and have thereby completed the present invention.
[0011] That is, the present invention includes the following: [1] A method for manufacturing a wiring board, comprising: (1) preparing a substrate having a conductor circuit and, on the conductor circuit, an insulating material layer formed of a cured product of a thermosetting material, and forming a photosensitive material layer by either or both of applying and attaching a photosensitive material to the surface of the insulating material layer; (2) exposing and developing the photosensitive material layer to form a plasma mask having openings; (3) irradiating the insulating material layer with plasma through the plasma mask to form either or both of a via hole and a trench in the insulating material layer located at the openings in the plasma mask, and thinning the plasma mask; and (4) forming a conductor layer on the thinned plasma mask and on the surfaces of either or both of the via hole and the trench. [2] A method for manufacturing a wiring board according to [1], wherein step (4) comprises: (4-1) forming a plating seed layer on the thinned plasma mask and on the surfaces of either or both of the via hole and the trench; and (4-2) plating on the plating seed layer to form a conductor layer. [3] The method for manufacturing a wiring board according to [1] or [2], wherein the conductor layer includes either or both of a conductor wiring formed at a position other than the opening of the plasma mask and a conductor via layer formed in the opening of the plasma mask. [4] The method for manufacturing a wiring board according to [2], wherein the plating seed layer is formed by a dry plating method. [5] The method for manufacturing a wiring board according to any of [1] to [4], wherein the opening diameter of the via hole or trench is 20 μm or less. [6] The method for manufacturing a wiring board according to any of [1] to [5], wherein the thickness of the plasma mask after the step (3) is reduced is 0.1 μm or more and 20 μm or less. [7] The method for manufacturing a wiring board according to any of [1] to [6], wherein the wiring pitch of the conductor circuit is 0.2 μm or more and 10 μm or less. [8] The method for manufacturing a wiring board according to any of [1] to [7], wherein the arithmetic mean roughness (Ra) of the surface of the plasma mask after the step (3) is reduced is 100 nm or less. [9] The method for manufacturing a wiring board according to any one of [1] to [8], wherein the roughness (Sa) of the wall surface of the via hole or trench is 400 nm or less.
[10] The method for manufacturing a wiring board according to any one of [1] to [9], wherein the ratio (Ra / Sa) of the arithmetic mean roughness (Ra) of the surface of the reduced plasma mask to the roughness (Sa) of the wall surface of the via hole or trench after step (3) is 3 or less.
[11] The method for manufacturing a wiring board according to any one of [1] to
[10] , wherein the thickness of the photosensitive material layer is 1 μm or more and 100 μm or less.
[12] The method for manufacturing a wiring board according to any one of [1] to
[11] , wherein the thickness of the reduced plasma mask after step (3) is 0.7 or less, where the thickness of the plasma mask before plasma irradiation is 1.
[13] The method for manufacturing a wiring board according to any one of [1] to
[12] , wherein the absolute value of the difference between the linear thermal expansion coefficient of the cured product of the photosensitive material and the linear thermal expansion coefficient of the cured product of the insulating material in the range of 25°C to 150°C is 60 ppm / °C or less.
[14] The method for manufacturing a wiring board according to any one of [1] to
[13] , wherein the relationship T1 > T2 is satisfied when the thickness of the plasma mask after the step (2) is T1 and the thickness of the insulating material layer after the step (2) is T2.
[15] The method for manufacturing a wiring board according to any one of [1] to
[14] , wherein the relationship T3 < T4 is satisfied when the thickness of the plasma mask after the step (3) is T3 and the thickness of the insulating material layer after the step (3) is T4.
[16] The method for manufacturing a wiring board according to any one of [1] to
[15] , wherein the absolute value of the difference between the glass transition temperature of the photosensitive material contained in the plasma mask and the glass transition temperature of the thermosetting material is 100°C or less.
[17] The method for manufacturing a wiring board according to any one of [1] to
[16] , wherein the via taper angle of the via hole or trench is 65 degrees or more and 90 degrees or less.
[18] The method for manufacturing a wiring board according to any one of [1] to
[17] , wherein the via expansion ratio is 105% or more and 150% or less.
[19] The method for manufacturing a wiring board according to any one of [1] to
[18] , wherein the dielectric constant of the cured product of the photosensitive material and the dielectric constant of the cured product of the thermosetting material are both 3.5 or less.
[20] The method for manufacturing a wiring board according to any one of [1] to
[19] , wherein the breaking elongation of the cured product of the photosensitive material is 10% or more and is greater than the breaking elongation of the cured product of the thermosetting material.
[21] The method for manufacturing a wiring board according to any one of [1] to
[20] , wherein the etching rate in step (3) is 100 nm / min or more.
[22] The method for manufacturing a wiring board according to any one of [1] to
[21] , wherein the line (conductor layer width) / space (width between conductor layers) (L / S) of the conductor layer is 5 μm / 5 μm or less.
[23] The method for manufacturing a wiring board according to any one of [1] to
[22] , wherein the wiring board is a multilayer wiring board substrate including three or more conductor layers.
[24] The area of the wiring board is 2500 mm. 2The method for manufacturing a wiring board according to any one of [1] to
[23] , wherein the photosensitive material used in step (1) contains at least one resin selected from a resin developable with a developer and an epoxy resin.
[26] The method for manufacturing a wiring board according to
[25] , wherein the resin developable with a developer contains at least one resin selected from an alkali-soluble resin having a phenolic hydroxyl group in the molecule, a polyimide precursor, a polybenzoxazole precursor resin, and an acrylic resin.
[27] The method for manufacturing a wiring board according to any one of [1] to
[26] , wherein the photosensitive material used in step (1) contains an inorganic filler, and the content of the inorganic filler in the photosensitive material is 10% by mass or less, relative to 100% by mass of the non-volatile components of the photosensitive material.
[28] The method for manufacturing a wiring board according to any one of [1] to
[27] , wherein the thermosetting material contains an inorganic filler, and the content of the inorganic filler in the thermosetting material is 20% by mass or more relative to 100% by mass of the non-volatile components of the thermosetting material.
[29] The method for manufacturing a wiring board according to
[28] , wherein the content of the inorganic filler is 35% by mass or more and 90% by mass or less relative to 100% by mass of the non-volatile components of the thermosetting material.
[30] The method for manufacturing a wiring board according to any one of [1] to
[29] , wherein the photosensitive material used in step (1) contains an inorganic filler, and the inorganic filler in the photosensitive material has an average particle size of 0.2 μm or less, and the thermosetting material contains an inorganic filler, and the inorganic filler has an average particle size of 0.01 μm or more.
[31] The method for manufacturing a wiring board according to any one of [1] to
[30] , wherein the bulk of the insulating material layer and the reduced plasma mask after step (3) has a linear thermal expansion coefficient of 100 ppm / °C or less in the range of 25°C to 150°C.
[32] The method for manufacturing a wiring board according to any one of [1] to
[31] , wherein the photosensitive material used in step (1) is a solvent-developable negative photosensitive polyimide resin.
[33] The method for manufacturing a wiring board according to any one of [1] to
[32] , wherein step (1) includes at least one of applying a liquid photosensitive material and attaching a photosensitive material layer of a photosensitive resin sheet including a support and a photosensitive material layer formed of a photosensitive material provided on the support.
[34] The method for manufacturing a wiring board according to any one of [1] to
[33] , wherein the total thickness of the insulating material layer and the reduced plasma mask is 15 μm or less.
[35] The method for manufacturing a wiring board according to any one of [1] to
[34] , comprising the steps of attaching the thermosetting material layer of a thermosetting resin sheet including a support and a thermosetting material layer formed of a thermosetting material provided on the support to a conductor circuit and curing the thermosetting material layer to form an insulating material layer.
[36] (A) a step of preparing a substrate having a conductor circuit and an insulating material layer formed on the conductor circuit from a cured product of a thermosetting material, and forming a first photosensitive material layer by either or both of applying and attaching a first photosensitive material to the surface of the insulating material layer; (B) a step of exposing and developing the first photosensitive material layer to form a first plasma mask having an opening; (C) a step of irradiating the insulating material layer with plasma through the first plasma mask to form either or both of a via hole and a trench in the insulating material layer located at the opening of the plasma mask, and reducing the thickness of the plasma mask; (D) a step of applying and either or both of applying and attaching a second photosensitive material to cover the surface and the opening of the first plasma mask to form a second photosensitive material layer; (E) a step of exposing and developing the second photosensitive material layer to form a second plasma mask having an opening; A method for manufacturing a wiring board, comprising: (F) irradiating the first plasma mask and the insulating material layer with plasma through a second plasma mask to form either or both of a via hole and a trench in the insulating material layer; (G) forming a conductor layer on the surfaces of the first plasma mask and either or both of the via hole and the trench; and (H) scraping the surface of the conductor layer.
[37] A wiring board manufactured by the method for manufacturing a wiring board according to any one of [1] to
[36] .
[38] The wiring board according to
[37] , which is formed in this order with a conductor circuit, an insulating material layer, a plasma mask, and a conductor layer, and which has a via hole.
[39] The wiring board according to
[38] , which includes two or more conductor circuits, two or more insulating material layers, two or more plasma masks, two or more conductor layers, and two or more via holes.
[40] A semiconductor device containing a wiring board manufactured by the method for manufacturing a wiring board according to any one of [1] to
[36] .
[41] The semiconductor device according to
[40] , having a fan-out structure.
[42] The semiconductor device according to
[40] , having a chiplet structure.
[43] A semiconductor device having a semiconductor chip on a wiring board manufactured by the manufacturing method according to any one of [1] to
[36] .
[44] The semiconductor device according to any one of
[40] to
[43] , wherein the semiconductor chip is a mixed system of at least a logic die and a memory die.
[0012] According to the present invention, it is possible to provide a method for manufacturing a wiring board that does not require removal of a mask pattern when forming a via hole or a trench, has an insulating material layer with excellent insulating performance and electrical properties, and is capable of fine wiring; and a semiconductor device.
[0013] FIG. 1 is a schematic cross-sectional view showing an example of a substrate having an insulating material layer formed on an inner layer circuit board. FIG. 2 is a schematic cross-sectional view showing an example of a substrate having an insulating material layer formed on an inner layer circuit board, on which a photosensitive material layer has been formed. FIG. 3 is a schematic cross-sectional view showing an example of a plasma mask formed in the first embodiment. FIG. 4 is a schematic cross-sectional view showing an example of a process for forming trenches and via holes in the insulating material layer and etching the plasma mask in the first embodiment. FIG. 5 is a schematic cross-sectional view showing an example of a process for forming trenches and via holes in the insulating material layer in the first embodiment. FIG. 6 is a schematic cross-sectional view showing an example of a process for forming a plating seed layer on the surface of the reduced plasma mask and the insulating material layer in the first embodiment. FIG. 7 is a schematic cross-sectional view showing an example of a process for forming a patterned conductor layer by plating on the plating seed layer in the first embodiment. FIG. 8 is a schematic cross-sectional view showing an example of a process for forming a patterned conductor layer in the first embodiment. FIG. 9 is a schematic cross-sectional view showing another example of a process for forming a plasma mask in the first embodiment. FIG. 10 is a schematic cross-sectional view showing another example of the process of forming trenches and via holes in the insulating material layer and etching the plasma mask in the first embodiment. FIG. 11 is a schematic cross-sectional view showing another example of the process after trenches and via holes have been formed in the insulating material layer in the first embodiment. FIG. 12 is a schematic cross-sectional view showing an example of the process of forming a plating seed layer on the surface of the reduced plasma mask and the insulating material layer in the first embodiment. FIG. 13 is a schematic cross-sectional view showing another example of the process of forming a patterned conductor layer by plating on the plating seed layer in the first embodiment. FIG. 14 is a schematic cross-sectional view showing another example of the process of forming a patterned conductor layer in the first embodiment. FIG. 15 is a schematic cross-sectional view showing an example of the process of forming a first plasma mask in the second embodiment. FIG. 16 is a schematic cross-sectional view showing an example of the process of forming trenches in the insulating material layer and etching the first plasma mask in the second embodiment. FIG. 17 is a schematic cross-sectional view showing an example of the process of forming a second photosensitive material layer to cover the surface of the first plasma mask and the openings in the second embodiment.Fig. 18 is a schematic cross-sectional view showing an example of a state after a second plasma mask has been formed in the second embodiment. Fig. 19 is a schematic cross-sectional view showing an example of a state after a trench has been formed in the insulating material layer in the second embodiment. Fig. 20 is a schematic cross-sectional view showing an example of a state after a conductor layer has been formed in the second embodiment. Fig. 21 is a schematic cross-sectional view showing an example of a state after the surface of the conductor layer has been polished in the second embodiment.
[0014] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples described below, and can be implemented with any modifications within the scope of the claims of the present invention and their equivalents.
[0015] Before describing the method for manufacturing a wiring board of the present invention in detail, the thermosetting material, photosensitive material, thermosetting resin sheet, photosensitive resin sheet, and prepreg used in the method for manufacturing a wiring board of the present invention will be described.
[0016] [Thermosetting Material] A thermosetting material is typically used to form an insulating material layer by thermal curing, and the cured product may have sufficient hardness and insulating properties. Examples of such a thermosetting material include a composition containing a thermosetting resin. In addition to the thermosetting resin, the thermosetting material may further contain an inorganic filler, a curing accelerator, a thermoplastic resin, and other additives, as necessary.
[0017] The thermosetting material contains a thermosetting resin, and as the thermosetting resin, a conventionally known thermosetting resin used when forming an insulating material layer of a printed wiring board can be used.
[0018] Examples of thermosetting resins include epoxy resins, polyarylene ether resins, radically polymerizable resins, phenolic resins, naphthol resins, benzoxazine resins, active ester resins, cyanate ester resins, carbodiimide resins, amine resins, and acid anhydride resins. Thermosetting resins may be used singly or in combination of two or more in any ratio. Hereinafter, resins that can react with epoxy resins to harden thermosetting materials, such as phenolic resins, naphthol resins, benzoxazine resins, active ester resins, cyanate ester resins, carbodiimide resins, amine resins, and acid anhydride resins, may be collectively referred to as "curing agents." From the perspective of forming an insulating material layer, the thermosetting resin preferably contains an epoxy resin and a curing agent, and more preferably contains any of epoxy resins, active ester resins, phenolic resins, and cyanate ester resins. The epoxy resins and curing agents may be used singly or in combination of two or more.
[0019] Examples of epoxy resins as thermosetting resins include bixylenol-type epoxy resins, bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, bisphenol S-type epoxy resins, bisphenol AF-type epoxy resins, dicyclopentadiene-type epoxy resins, trisphenol-type epoxy resins, naphthol novolac-type epoxy resins, phenol novolac-type epoxy resins, tert-butyl-catechol-type epoxy resins, naphthalene-type epoxy resins, naphthol-type epoxy resins, anthracene-type epoxy resins, glycidylamine-type epoxy resins, glycidyl ester-type epoxy resins, cresol novolac-type epoxy resins, biphenyl-type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane-type epoxy resins, cyclohexane dimethanol-type epoxy resins, naphthylene ether-type epoxy resins, trimethylol-type epoxy resins, and tetraphenylethane-type epoxy resins.
[0020] The thermosetting material preferably contains an epoxy resin having two or more epoxy groups per molecule as a thermosetting resin. From the viewpoint of significantly achieving the desired effects of the present invention, the proportion of the epoxy resin having two or more epoxy groups per molecule is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more, relative to 100% by mass of the non-volatile components of the epoxy resin.
[0021] Epoxy resins include epoxy resins that are liquid at a temperature of 20° C. (hereinafter sometimes referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 20° C. (hereinafter sometimes referred to as "solid epoxy resins"). The thermosetting material may contain only liquid epoxy resins or only solid epoxy resins as the thermosetting resin, but from the viewpoint of significantly achieving the effects of the present invention, it is preferable to contain a combination of liquid epoxy resins and solid epoxy resins.
[0022] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.
[0023] Preferred liquid epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AF type epoxy resins, naphthalene type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, phenol novolac type epoxy resins, alicyclic epoxy resins having an ester skeleton, cyclohexane type epoxy resins, cyclohexanedimethanol type epoxy resins, glycidyl amine type epoxy resins, and epoxy resins having a butadiene structure, and more preferred are bisphenol A type epoxy resins and bisphenol F type epoxy resins.
[0024] Specific examples of liquid epoxy resins include "HP4032," "HP4032D," and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US," "jER828EL," "825," and "Epikote 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; and "630" and "630LSD" (glycidylamine type epoxy resins) manufactured by Mitsubishi Chemical Corporation. ); "ZX1059" (a mixture of bisphenol A epoxy resin and bisphenol F epoxy resin) manufactured by Nippon Steel Chemical & Material Corporation; "EX-721" (glycidyl ester epoxy resin) manufactured by Nagase ChemteX Corporation; "Celloxide 2021P" (alicyclic epoxy resin having an ester skeleton) manufactured by Daicel Corporation; "PB-3600" (epoxy resin having a butadiene structure) manufactured by Daicel Corporation; and "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane epoxy resin) manufactured by Nippon Steel Chemical & Material Corporation. These may be used alone or in combination of two or more.
[0025] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferred, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferred.
[0026] As the solid epoxy resin, bixylenol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, and tetraphenylethane type epoxy resin are preferred, and naphthalene type epoxy resin is more preferred.
[0027] As the solid epoxy resin, naphthalene-type tetrafunctional epoxy resin, cresol novolac-type epoxy resin, dicyclopentadiene-type epoxy resin, trisphenol-type epoxy resin, naphthol-type epoxy resin, biphenyl-type epoxy resin, naphthylene ether-type epoxy resin, anthracene-type epoxy resin, bisphenol A-type epoxy resin, and tetraphenylethane-type epoxy resin are preferred, and naphthalene-type tetrafunctional epoxy resin, naphthol-type epoxy resin, and biphenyl-type epoxy resin are more preferred. Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin), "HP-4700", "HP-4710" (naphthalene type tetrafunctional epoxy resin), "N-690" (cresol novolac type epoxy resin), "N-695" (cresol novolac type epoxy resin), "HP-7200", "HP-7200HH", "HP-7200H" (dicyclopentadiene type epoxy resin), "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", and "HP6000" (naphthylene ether type epoxy resin), manufactured by DIC Corporation; and "EPPN-502H" (trisphenol type epoxy resin), "NC7000L" (naphthol novolac type epoxy resin), "NC3000H", and "NC30 00," "NC3000L," and "NC3100" (biphenyl-type epoxy resins); "ESN475V" (naphthalene-type epoxy resin) and "ESN485" (naphthol novolac-type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H," "YL6121" (biphenyl-type epoxy resin), "YX4000HK" (bixylenol-type epoxy resin), and "YX8800" (anthracene-type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals Co., Ltd., and "YL7760" (bisphenol AF-type epoxy resin), "YL7800" (fluorene-type epoxy resin), "jER1010" (solid bisphenol A-type epoxy resin), and "jER1031S" (tetraphenylethane-type epoxy resin) manufactured by Mitsubishi Chemical Corporation. These may be used alone or in combination of two or more.
[0028] When a liquid epoxy resin and a solid epoxy resin are used in combination as the thermosetting resin, the ratio by mass of the liquid epoxy resin to the solid epoxy resin is preferably 1:0.1 to 1:20, more preferably 1:0.3 to 1:18, and particularly preferably 1:0.5 to 1:15. By ensuring that the ratio of the liquid epoxy resin to the solid epoxy resin is within this range, the desired effects of the present invention can be significantly achieved. Furthermore, when used in the form of a thermosetting resin sheet, appropriate adhesiveness is typically achieved. Furthermore, when used in the form of a thermosetting resin sheet, sufficient flexibility is typically achieved, improving handleability. Furthermore, a cured product with sufficient breaking strength can typically be obtained.
[0029] The epoxy equivalent of the epoxy resin used as the thermosetting resin is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., even more preferably 80 g / eq. to 2000 g / eq., and even more preferably 110 g / eq. to 1000 g / eq. By using this range, the cured product of the thermosetting material can have a sufficient crosslink density. The epoxy equivalent is the mass of the epoxy resin containing one equivalent of epoxy groups. This epoxy equivalent can be measured in accordance with JIS K7236.
[0030] From the viewpoint of significantly achieving the desired effects of the present invention, the weight average molecular weight (Mw) of the epoxy resin as the thermosetting resin is preferably 100 to 5000, more preferably 250 to 3000, and even more preferably 400 to 1500. The weight average molecular weight of the epoxy resin is a weight average molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC).
[0031] The content of the epoxy resin as the thermosetting resin is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, based on 100% by mass of the nonvolatile components in the thermosetting material, from the viewpoint of obtaining a cured product exhibiting good mechanical strength and insulation reliability. The upper limit of the epoxy resin content is preferably 60% by mass or less, more preferably 55% by mass or less, and particularly preferably 50% by mass or less, from the viewpoint of significantly obtaining the desired effects of the present invention.
[0032] Unless otherwise specified, the content of each component in the thermosetting material is a value when the non-volatile components in the thermosetting material are taken as 100 mass%, and the non-volatile components refer to all non-volatile components in the thermosetting material excluding the solvent.
[0033] From the viewpoint of obtaining the remarkable effects of the present invention, the content of the epoxy resin as the thermosetting resin is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less, when the resin component in the thermosetting material is taken as 100% by mass. The resin component refers to the non-volatile components in the thermosetting material excluding the inorganic filler.
[0034] The type of polyarylene ether resin as a thermosetting resin is not particularly limited as long as it has a polyarylene ether skeleton and exhibits crosslinkability through reaction of functional groups such as terminal hydroxy groups. Examples of polyarylene ether resins include polyphenylene ether resins and polynaphthylene ether resins, which may be homopolymers or copolymers. Examples of homopolymers of polyphenylene ether resins include 2,6-diC 1~3 Examples of the copolymer include those containing alkyl-1,4-phenylene ether units, and examples of the copolymer include 2,6-diC 1~3 Alkyl-1,4-phenylene ether unit with 2,3,6-tri C 1~3Examples of the polyarylene ether resin include graft, block, or random copolymers containing a combination of alkyl-1,4-phenylene ether units, etc. Examples of the polyarylene ether resin include "Noryl (registered trademark) SA90" manufactured by SABIC.
[0035] The number average molecular weight (Mn) of the polyarylene ether resin is preferably 200 to 5,000, more preferably 400 to 3,000, and even more preferably 600 to 2500. The Mn of the polyarylene ether resin can be measured by a GPC method as a polystyrene-equivalent value.
[0036] The type of radical polymerizable resin as a thermosetting resin is not particularly limited, as long as it has one or more (preferably two or more) radical polymerizable unsaturated groups in one molecule. Examples of the radical polymerizable resin include resins having one or more radical polymerizable unsaturated groups selected from maleimide groups, vinyl groups, allyl groups, styryl groups, vinylphenyl groups, acryloyl groups, methacryloyl groups, fumaroyl groups, and maleoyl groups. Among these, from the viewpoint of being able to produce a cured product that exhibits both good insulating properties and good heat resistance, it is preferable that the radical polymerizable resin contains one or more selected from maleimide resins, (meth)acrylic resins, and styryl resins.
[0037] The type of maleimide resin is not particularly limited as long as it has one or more (preferably two or more) maleimide groups (2,5-dihydro-2,5-dioxo-1H-pyrrol-1-yl groups) in one molecule. Examples of maleimide resins include maleimide resins containing an aliphatic skeleton (preferably an aliphatic skeleton containing a cyclic structure having 10 or more carbon atoms, more preferably an aliphatic skeleton having 36 carbon atoms derived from dimer diamine), such as "BMI-3000J," "BMI-5000," "BMI-1400," "BMI-1500," "BMI-1700," and "BMI-689" (all manufactured by Designer Molecules Inc.); maleimide resins containing an indane skeleton, as described in the Japan Institute of Invention and Innovation Disclosure Technical Bulletin No. 2020-500211; and maleimide resins containing an aromatic ring skeleton directly bonded to the nitrogen atom of the maleimide group, such as "MIR-3000-70MT" (manufactured by Nippon Kayaku Co., Ltd.), "BMI-4000," "BMI-1000" (manufactured by Daiwa Kasei Co., Ltd.), and "BMI-80" (manufactured by Keiai Kasei Co., Ltd.).
[0038] The (meth)acrylic resin may be of any type, and may be a monomer or oligomer, as long as it has one or more (preferably two or more) (meth)acryloyl groups in one molecule. Here, the term "(meth)acryloyl group" is a general term for acryloyl groups and methacryloyl groups. Examples of methacrylic resins include (meth)acrylate monomers, as well as (meth)acrylic resins such as "A-DOG" (manufactured by Shin-Nakamura Chemical Co., Ltd.), "DCP-A" (manufactured by Kyoeisha Chemical Co., Ltd.), "NPDGA," "FM-400," "R-687," "THE-330," "PET-30," and "DPHA" (all manufactured by Nippon Kayaku Co., Ltd.).
[0039] The styryl resin may be a monomer or an oligomer, and may be any styryl resin, as long as it contains one or more (preferably two or more) styryl or vinylphenyl groups per molecule. Examples of the styryl resin include "OPE-2St," "OPE-2St 1200," and "OPE-2St 2200" (all manufactured by Mitsubishi Gas Chemical Company, Inc.). Examples of the styryl resin include, in addition to styrene monomers, homopolymers of aromatic divinyl compounds such as divinylbenzene, 2,4-divinyltoluene, 2,6-divinylnaphthalene, 1,4-divinylnaphthalene, 4,4'-divinylbiphenyl, 1,2-bis(4-vinylphenyl)ethane, 2,2-bis(4-vinylphenyl)propane, and bis(4-vinylphenyl)ether, as well as copolymers of these aromatic divinyl compounds with aromatic monovinyl compounds such as styrene, vinyltoluene, ethylstyrene, and vinylnaphthalene.
[0040] As the activated ester resin used as the thermosetting resin, a resin having one or more activated ester groups per molecule can be used. Among these, preferred activated ester resins are those having two or more highly reactive ester groups per molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds. The active ester resin is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an activated ester resin obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an activated ester resin obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred.
[0041] Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid.
[0042] Examples of phenol compounds or naphthol compounds include hydroquinone, resorcinol, bisphenol A, bisphenol F, bisphenol S, phenolphthalene, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolak, etc. Here, "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one dicyclopentadiene molecule with two phenol molecules.
[0043] Specific preferred examples of the active ester resin include active ester resins containing a dicyclopentadiene-type diphenol structure, active ester resins containing a naphthalene structure, active ester resins containing an acetylated product of phenol novolac, and active ester resins containing a benzoylated product of phenol novolac. Among these, active ester resins containing a naphthalene structure and active ester resins containing a dicyclopentadiene-type diphenol structure are more preferred. The "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentylene-phenylene.
[0044] Commercially available activated ester resins include active ester resins containing a dicyclopentadiene-type diphenol structure such as "EXB9451", "EXB9460", "EXB9460S", "HPC-8000-65T", "HPC-8000H-65TM", and "EXB-8000L-65TM" (manufactured by DIC Corporation); and naphthalene-type activated ester resins containing a naphthalene structure such as "EXB9416-70BK", "EXB-8100L-65T", "EXB-8150L-65T", "EXB-8150-65T", "HPC-8150-60T", and "HPC-8150-62T" (manufactured by DIC Corporation), and "PC1300-02-65T" (manufactured by air). Examples of active ester resins that contain acetylated phenol novolac include "DC808" (manufactured by Mitsubishi Chemical Corporation); active ester resins that contain benzoated phenol novolac include "YLH1026" (manufactured by Mitsubishi Chemical Corporation); active ester resins that are acetylated phenol novolac include "DC808" (manufactured by Mitsubishi Chemical Corporation); active ester resins that are benzoated phenol novolac include "YLH1026" (manufactured by Mitsubishi Chemical Corporation), "YLH1030" (manufactured by Mitsubishi Chemical Corporation), and "YLH1048" (manufactured by Mitsubishi Chemical Corporation); and "EXB-8500-65T" (manufactured by DIC Corporation).
[0045] From the viewpoint of significantly obtaining the effects of the present invention, the content of the active ester resin as the thermosetting resin is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, relative to 100% by mass of the non-volatile components in the thermosetting material, and is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less.
[0046] From the viewpoint of significantly obtaining the effects of the present invention, the content of the active ester resin as the thermosetting resin is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, and is preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less, when the resin component in the thermosetting material is taken as 100% by mass.
[0047] The phenolic resin and naphtholic resin as the thermosetting resin are preferably those having a novolac structure from the viewpoints of heat resistance and water resistance, and are preferably nitrogen-containing phenolic resins, more preferably triazine skeleton-containing phenolic resins, from the viewpoint of adhesion to the conductor layer.
[0048] Specific examples of phenol-based resins and naphthol-based resins include "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Chemical Industry Co., Ltd.; "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd.; "SN170", "SN180", "SN190", "SN475", "SN485", "SN495", "SN-495V", "SN375", and "SN395" manufactured by Nippon Steel Chemical & Material Co., Ltd.; and "TD-2090", "LA-7052", "LA-7054", "LA-1356", "LA-3018-50P", and "EXB-9500" manufactured by DIC Corporation.
[0049] From the viewpoint of significantly obtaining the effects of the present invention, the content of the phenolic resin or naphtholic resin as the thermosetting resin is preferably 1% by mass or more, more preferably 1.5% by mass or more, and even more preferably 2% by mass or more, relative to 100% by mass of the non-volatile components in the thermosetting material, and is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less.
[0050] From the viewpoint of significantly obtaining the effects of the present invention, the content of the phenolic resin or naphtholic resin as the thermosetting resin is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, when the resin component in the thermosetting material is taken as 100% by mass, and is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less.
[0051] Examples of cyanate ester resins as thermosetting resins include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanatephenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanatephenyl-1-(methylethylidene))benzene, bis(4-cyanatephenyl)thioether, and bis(4-cyanatephenyl)ether; polyfunctional cyanate resins derived from phenol novolac, cresol novolac, etc.; and prepolymers in which these cyanate resins are partially triazine-converted. Specific examples of cyanate ester resins include "PT30," "PT30S," and "PT60" (phenol novolac type multifunctional cyanate ester resins), "ULL-950S" (multifunctional cyanate ester resin), "BA230," and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate is triazine-converted to form a trimer), all of which are manufactured by Arxada.
[0052] From the viewpoint of significantly obtaining the effects of the present invention, the content of the cyanate ester resin as the thermosetting resin is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, relative to 100% by mass of the non-volatile components in the thermosetting material, and is preferably 25% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less.
[0053] From the viewpoint of significantly obtaining the effects of the present invention, the content of the cyanate ester resin as the thermosetting resin is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, when the resin component in the thermosetting material is taken as 100% by mass, and is preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less.
[0054] Examples of benzoxazine-based resins, carbodiimide-based resins, and acid anhydride-based resins as thermosetting resins include those described in JP-A-2020-75977.
[0055] When the thermosetting resin contains an epoxy resin and a curing agent, the ratio of the amount of epoxy resin to all curing agents, expressed as the ratio of [total number of epoxy groups in the epoxy resin] to [total number of active groups in the curing agent], is preferably in the range of 1:0.01 to 1:5, more preferably 1:0.05 to 1:3, and even more preferably 1:0.1 to 1:2. Here, the "total number of epoxy groups in the epoxy resin" refers to the sum of all values obtained by dividing the mass of the non-volatile components of the epoxy resin present in the thermosetting material by the epoxy equivalent. Furthermore, the "total number of active groups in the curing agent" refers to the sum of all values obtained by dividing the mass of the non-volatile components of the curing agent present in the thermosetting material by the active group equivalent. By maintaining the ratio of epoxy resin to curing agent within this range, a cured product with excellent flexibility can be obtained.
[0056] From the viewpoint of significantly obtaining the effects of the present invention, the content of the curing agent as the thermosetting resin is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, relative to 100% by mass of the non-volatile components in the thermosetting material, and is preferably 40% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less.
[0057] From the viewpoint of significantly obtaining the effects of the present invention, the content of the curing agent as the thermosetting resin is preferably 5% by mass or more, more preferably 8% by mass or more, and even more preferably 10% by mass or more, and is preferably 60% by mass or less, more preferably 55% by mass or less, and even more preferably 50% by mass or less, when the resin component in the thermosetting material is taken as 100% by mass.
[0058] From the viewpoint of obtaining the effects of the present invention significantly, the content of the thermosetting resin is preferably 6% by mass or more, more preferably 13% by mass or more, and even more preferably 20% by mass or more, relative to 100% by mass of non-volatile components in the thermosetting material, and is preferably 65% by mass or less, more preferably 60% by mass or less, and even more preferably 55% by mass or less.
[0059] From the viewpoint of obtaining the effects of the present invention remarkably, the content of the thermosetting resin is preferably 15% by mass or more, more preferably 23% by mass or more, and even more preferably 30% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less, when the resin component in the thermosetting material is taken as 100% by mass, from the viewpoint of obtaining the effects of the present invention remarkably.
[0060] The thermosetting material preferably contains an inorganic filler. By including the inorganic filler in the thermosetting resin, the electrical properties of the insulating material layer can be improved. The inorganic filler may be used alone or in combination of two or more.
[0061] Inorganic compounds can be used as inorganic filler materials. Examples of inorganic filler materials include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium titanate zirconate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica and alumina are preferred, and silica is particularly preferred. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. Furthermore, spherical silica is preferred.
[0062] Commercially available inorganic fillers include, for example, "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", "YA010C", "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.; "UFP-30", "DAW-03", and "FB-105FD" manufactured by Denka Co., Ltd.; "Silfil NSS-3N", "Silfil NSS-4N", and "Silfil NSS-5N" manufactured by Tokuyama Corporation; "Cellphears" and "MGH-005" manufactured by Taiheiyo Cement Corporation; and "Sfereek" and "BA-1" manufactured by JGC Catalysts and Chemicals Co., Ltd.
[0063] The specific surface area of the inorganic filler is preferably 1 m 2 / g or more, more preferably 2m 2 / g or more, particularly preferably 3m 2 / g or more. There is no particular upper limit, but it is preferably 60 m 2 / g or less, 50m 2 / g or less or 40m 2 The specific surface area can be measured by a BET multipoint method using a fully automatic BET specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech Co., Ltd.) with nitrogen gas adsorbed onto the surface of the sample.
[0064] The average particle size of the inorganic filler is preferably 0.01 μm or more, more preferably 0.03 μm or more, particularly preferably 0.05 μm or more, and is preferably 5 μm or less, more preferably 2 μm or less, and even more preferably 1 μm or less.
[0065] The average particle size of the inorganic filler can be measured by a laser diffraction / scattering method based on Mie scattering theory. Specifically, a particle size distribution of the inorganic filler is created on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is used as the average particle size. A measurement sample can be prepared by weighing 100 mg of inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing the mixture ultrasonically for 10 minutes. The measurement sample is measured using a laser diffraction particle size distribution measuring device, with blue and red light source wavelengths used, using a flow cell system to measure the volume-based particle size distribution of the inorganic filler, and the average particle size can be calculated as the median diameter from the obtained particle size distribution. An example of a laser diffraction particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.
[0066] The inorganic filler is preferably treated with a surface treatment agent from the viewpoint of improving moisture resistance and dispersibility. Examples of the surface treatment agent include vinylsilane coupling agents, (meth)acrylic coupling agents, fluorine-containing silane coupling agents, aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, alkoxysilanes, organosilazane compounds, and titanate coupling agents. One type of surface treatment agent may be used alone, or two or more types may be used in any combination.
[0067] Commercially available surface treatment agents include, for example, Shin-Etsu Chemical Co., Ltd.'s "KBM1003" (vinyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM503" (3-methacryloxypropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), and Shin-Etsu Chemical Co., Ltd.'s "KBM1003" (vinyltriethoxysilane). Examples of suitable silane coupling agents include "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., "SZ-31" (hexamethyldisilazane) manufactured by Shin-Etsu Chemical Co., Ltd., "KBM103" (phenyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., "KBM-4803" (long-chain epoxy type silane coupling agent), and "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd.
[0068] The degree of surface treatment with the surface treatment agent is preferably within a predetermined range from the viewpoint of improving the dispersibility of the inorganic filler. Specifically, 100 parts by mass of the inorganic filler is preferably surface-treated with 0.2 to 5 parts by mass of the surface treatment agent, more preferably 0.2 to 3 parts by mass, and even more preferably 0.3 to 2 parts by mass.
[0069] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of the inorganic filler is 0.02 mg / m 2 More than 0.1 mg / m 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of suppressing an increase in the melt viscosity of the resin varnish and the melt viscosity in the form of a sheet, it is more preferable that the amount of the resin varnish is 1 mg / m 2 Preferably, 0.8 mg / m or less 2 More preferably, 0.5 mg / m or less 2 The following is even more preferred:
[0070] The carbon amount per unit surface area of the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the carbon amount per unit surface area of the inorganic filler can be measured using a carbon analyzer. As the carbon analyzer, an "EMIA-320V" manufactured by Horiba, Ltd. or the like can be used.
[0071] The content of the inorganic filler is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 25% by mass or more, even more preferably 30% by mass or more, even more preferably 35% by mass or more, and particularly preferably 40% by mass or more, relative to 100% by mass of the non-volatile components in the thermosetting material, and is preferably 90% by mass or less, more preferably 87% by mass or less, and even more preferably 83% by mass or less.
[0072] The thermosetting material may contain a curing accelerator as needed. Examples of the curing accelerator include phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, guanidine-based curing accelerators, and metal-based curing accelerators. Among these, amine-based curing accelerators are preferred. One type of curing accelerator may be used alone, or two or more types may be used in combination.
[0073] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene, with 4-dimethylaminopyridine and 1,8-diazabicyclo(5,4,0)-undecene being preferred.
[0074] Other examples of the curing accelerator include those described in JP-A-2020-75977.
[0075] The content of the curing accelerator is preferably 0.001% by mass or more, more preferably 0.005% by mass or more, even more preferably 0.01% by mass or more, and is preferably 1.0% by mass or less, more preferably 0.5% by mass or less, even more preferably 0.3% by mass or less, relative to 100% by mass of the non-volatile components in the thermosetting material.
[0076] The content of the curing accelerator is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, and even more preferably 0.1% by mass or more, relative to 100% by mass of the resin component in the thermosetting material, and is preferably 5.0% by mass or less, more preferably 3.0% by mass or less, and even more preferably 1.0% by mass or less.
[0077] The thermosetting material may contain a thermoplastic resin as needed. Examples of the thermoplastic resin include phenoxy resin, polyvinyl acetal resin, polyolefin resin, polyimide resin, polyamideimide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polyetheretherketone resin, and polyester resin, with phenoxy resin being preferred. One type of thermoplastic resin may be used alone, or two or more types may be used in combination.
[0078] The weight average molecular weight of the thermoplastic resin in terms of polystyrene is preferably 8,000 or more, more preferably 10,000 or more, and even more preferably 20,000 or more. The upper limit is preferably 100,000 or less, more preferably 70,000 or less, even more preferably 60,000 or less, and particularly preferably 50,000 or less.
[0079] Examples of phenoxy resins include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group. One type of phenoxy resin may be used alone, or two or more types may be used in combination. Specific examples of phenoxy resins include "1256" and "4250" (both phenoxy resins containing a bisphenol A skeleton), "YX8100" (phenoxy resin containing a bisphenol S skeleton), and "YX6954" (phenoxy resin containing a bisphenol acetophenone skeleton), all manufactured by Mitsubishi Chemical Corporation. Other examples include "FX280" and "FX293" manufactured by Nippon Steel Chemical & Material Co., Ltd., and "YL7500BH30," "YX6954BH30," "YX7553," "YX7553BH30," "YL7769BH30," "YL6794," "YL7213," "YL7290," and "YL7482" manufactured by Mitsubishi Chemical Corporation.
[0080] Other examples of thermoplastic resins include those described in JP-A-2020-75977.
[0081] The content of the thermoplastic resin is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and even more preferably 0.5% by mass or more, based on 100% by mass of the nonvolatile components in the thermosetting material, and the upper limit is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less.
[0082] The content of the thermoplastic resin is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1.0% by mass or more, based on 100% by mass of the resin component in the thermosetting material, and the upper limit is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less.
[0083] The thermosetting material may further contain other additives in addition to the above-mentioned components. Examples of the other additives include polymerization initiators, organometallic compounds, colorants, polymerization inhibitors, leveling agents, thickeners, antifoaming agents, UV absorbers, adhesion improvers, adhesion promoters, antioxidants, fluorescent brighteners, surfactants, flame retardants, dispersants, stabilizers, photopolymerization initiation aids, and photosensitizers. One type of the other additives may be used alone, or two or more types may be used in combination.
[0084] The thermosetting material may contain a solvent as a volatile component. Examples of the solvent include ketones such as methyl ethyl ketone (MEK) and cyclohexanone; aromatic hydrocarbons such as xylene and tetramethylbenzene; glycol ethers such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, butyl cellosolve acetate, carbitol acetate, and ethyl diglycol acetate; aliphatic hydrocarbons such as octane and decane; petroleum-based solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha; and ether ester solvents such as propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, and methyl methoxypropionate. These may be used alone or in combination of two or more.
[0085] The thermosetting material may contain a solvent, but the amount thereof is preferably small. The amount of solvent contained in the thermosetting material is preferably 10% by mass or less, more preferably 8% by mass or less, and even more preferably 5% by mass or less, based on 100% by mass of the nonvolatile components in the thermosetting material.
[0086] The method for preparing the thermosetting material is not particularly limited, and examples thereof include a method in which the ingredients are mixed and dispersed, if necessary, together with a solvent, using a kneading device or a stirring device.
[0087] A cured product of a thermosetting material usually exhibits the characteristic of a high glass transition temperature (Tg). Therefore, when an insulating material layer is formed using this cured product, an insulating material layer with a high glass transition temperature can be obtained. The glass transition temperature of the cured product is preferably 130°C or higher, more preferably 140°C or higher, and even more preferably 150°C or higher. There is no particular upper limit, but it can be, for example, 400°C or lower. The glass transition temperature can be measured by the method described in the examples below.
[0088] A cured product of a thermosetting material typically exhibits the characteristic of a low coefficient of linear thermal expansion (CTE). Therefore, when an insulating material layer is formed using this cured product, an insulating material layer with a low coefficient of linear thermal expansion can be obtained. The coefficient of linear thermal expansion of the cured product is preferably 100 ppm / °C or less, more preferably 80 ppm / °C or less, and even more preferably 75 ppm / °C or less. The lower limit is not particularly limited, but can be, for example, 0.01 ppm / °C or more. The coefficient of linear thermal expansion can be measured by the method described in the examples below.
[0089] A cured product of a thermosetting material typically exhibits a high modulus of elasticity at 23°C. This allows for the production of an insulating material layer with excellent crack resistance. The modulus of elasticity of the cured product at 23°C is preferably 1.0 GPa or more, more preferably 1.5 GPa or more, and even more preferably 2.0 GPa or more. There is no particular upper limit, but it can be 50 GPa or less, for example. The modulus of elasticity can be measured by the method described in the examples below.
[0090] Cured products of thermosetting materials usually exhibit the characteristic of high elongation (elongation at break). Therefore, an insulating material layer with a high elongation at break can be obtained. The elongation at break of the cured product is preferably 0.5% or more, more preferably 1.0% or more, and particularly preferably 1.5% or more. There is no particular upper limit, and it can be, for example, 10% or less. Elongation can be measured according to the method described in the examples below.
[0091] A cured product of a thermosetting material usually exhibits the characteristic of a low dielectric loss tangent. Therefore, an insulating material layer with a low dielectric loss tangent can be obtained. The dielectric loss tangent of the cured product is preferably 0.03 or less, more preferably 0.02 or less, and even more preferably 0.01 or less. There is no particular restriction on the lower limit of the dielectric loss tangent, and it can be, for example, 0.0005 or more. The dielectric loss tangent can be measured by the method described in the examples below.
[0092] A cured product of a thermosetting material usually exhibits the characteristic of a low relative dielectric constant. Therefore, an insulating material layer with a low relative dielectric constant can be obtained. The dielectric constant of the cured product is preferably 5.0 or less, more preferably 4.0 or less, and even more preferably 3.5 or less. The lower limit is not particularly limited, but may be, for example, 0.0001 or more. The relative dielectric constant can be measured by the method described in the examples below.
[0093] [Photosensitive Material] The photosensitive material may be any material that can be used to form a plasma mask and has excellent resolution. The photosensitive material may be either a positive-type photosensitive material or a negative-type material. Examples of such photosensitive materials include compositions containing a resin that can be developed with a developer such as an alkaline aqueous solution. In addition to the resin that can be developed with a developer, the photosensitive material may further contain an epoxy resin, a crosslinking agent, a photopolymerization initiator, a photoacid generator, an adhesion aid, an organic filler, and other additives, as necessary.
[0094] The photosensitive material contains a resin that can be developed with a developer. Examples of the resin that can be developed with a developer include conventionally known resins used when forming solder resist layers on printed wiring boards. Examples of the resin that can be developed with a developer include alkali-soluble resins having a phenolic hydroxyl group in the molecule, polybenzoxazole precursor resins, polyimide precursors, p-hydroxystyrene / styrene copolymers, acrylic resins, and methacrylic resins. Of these, the resin that can be developed with a developer preferably contains one or more resins selected from alkali-soluble resins having a phenolic hydroxyl group in the molecule, polyimide precursors, polybenzoxazole precursor resins, and acrylic resins. The resin that can be developed with a developer may be used alone or in combination of two or more.
[0095] Examples of alkali-soluble resins having a phenolic hydroxyl group in the molecule include "TR4020G" manufactured by Asahi Organic Chemicals Co., Ltd.; AV Light series such as "TR4050G", "TR4080G", "TR5020G", "TR5050G", "TR6020G", "TR6050G", and "TR6080G" manufactured by Asahi Organic Chemicals Co., Ltd.; photoresist resin series manufactured by Sumitomo Bakelite Co., Ltd.; Resitop series manufactured by Gun-ei Chemical Industry Co., Ltd.; and "PR-30-40P", "PR-100L", "PR-100H", "PR-50", "PR-55", and "PR-56" manufactured by DIC Corporation. -1," "PR-56-2," "WR-101," "WR-102," "WR-103," "WR-104," and other Phenolite series; Lignite Corporation's "LF-100," "LF-110," "LF-120," "LF-200," "LF-400," and "LF-500"; Meiwa Kasei Co., Ltd.'s photoresist base resin series; Meiwa Kasei Co., Ltd.'s "MEHC-7851SS," "MEHC-78004S," "MEHC-7851-SS," "MEHC-7851-S," "MEHC-7851-M," "MEHC-7851-H," and "MEHC-7851-M" EHC-7800-4S” “MEHC-7800-SS” “MEHC-7800-S” “MEHC-7800-M” “MEH C-7800-H”, Nippon Kayaku Co., Ltd. “GPH-65”, “GPH-103”, “MEHC-7841-4S”; Honshu Kagaku Co., Ltd. “BisE” ", "BisP-TMC"; manufactured by Mitsui Chemicals Fine Co., Ltd. "BisA", "BisF", "BisP-M", "BisP-AP", "BisP-TMC"; sP-MIBK", "BisP-B", "Bis-Z", "BisP-CP", "o,o'-BPF", "BisP-IOTD", " BisP-IBTD”, “BisP-DED”, “BisP-BA”, “Bis-C”, “Bis26X-A”, “BisOPP- A", "BisOTBP-A", "BisOCHP-A", "BisOFP-A", "BisOC-Z", "BisOC-FL", " BisOC-CP”, “BisOCHP-Z”, “MethylenebisP-CR”, “TM-BPF”, “BisOC-F”, “Bis3M 6B-IBTD,” “BisOC-IST,” “BisP-IST,” “BisP-PRM,” and “BisP-LV.”
[0096] Examples of polybenzoxazole precursor resins, polyimide precursors, p-hydroxystyrene / styrene copolymers, and acrylic resins include those described in JP 2018-169547 A, JP 2018-169627 A, WO 2010 / 134207, WO 2014 / 069202, JP 2020-101813 A, WO 2018 / 232214, and the like.
[0097] Other examples of resins that can be developed with a developer include radical polymerizable resins, specific examples of which include resins having radical polymerizable unsaturated groups such as ethylenically unsaturated groups such as acrylic resins and methacrylic resins. Examples of resins having radical polymerizable unsaturated groups include those described in documents such as JP 2020-15859 A, JP 2020-52288 A, and JP 2018-169547 A.
[0098] The weight average molecular weight of the resin developable with the developer is preferably 100 or more, more preferably 150 or more, even more preferably 200 or more, and may be 300 or more, 500 or more, 700 or more, or 1000 or more. The upper limit is preferably 150,000 or less, more preferably 100,000 or less, even more preferably 50,000 or less, and may be 10,000 or less, 5,000 or less, 1,000 or less, 800 or less, or 500 or less.
[0099] The content of the resin developable with the developer is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 35% by mass or more, and is preferably 90% by mass or less, more preferably 85% by mass or less, and even more preferably 80% by mass or less, when the non-volatile components of the photosensitive material are taken as 100% by mass.
[0100] Unless otherwise specified, the content of each component in the photosensitive material is a value when the non-volatile components in the photosensitive material are taken as 100% by mass, and the non-volatile components refer to all non-volatile components in the photosensitive material excluding the solvent.
[0101] The photosensitive material may contain an epoxy resin. The epoxy resin is as described in the section on "Thermosetting Materials." The epoxy resin may be used alone or in combination of two or more types.
[0102] The photosensitive material may contain a crosslinking agent from the viewpoint of improving the strength of the cured product of the photosensitive material. The crosslinking agent may be used alone or in combination of two or more.
[0103] Examples of the crosslinking agent include compounds containing two or more alkoxymethyl groups in the molecule.
[0104] Examples of compounds containing two or more alkoxymethyl groups in the molecule include amino resins containing two or more alkoxymethyl groups in the molecule, and phenolic resins containing two or more alkoxymethyl groups in the molecule. Among these, amino resins containing two or more alkoxymethyl groups in the molecule are preferred because they have better photosensitivity. Examples of amino resins containing two or more alkoxymethyl groups in the molecule include melamine resins and urea resins, with melamine resins being preferred.
[0105] Specific examples of melamine resins include "MW-390," "MW-100LM," "MW-30HM," and "MX-750LM" manufactured by Sanwa Chemical Co., Ltd.; and the Cymel series manufactured by Allnex Japan Co., Ltd. Specific examples of urea resins include "MX-270," "MX-279," and "MX-280" manufactured by Sanwa Chemical Co., Ltd.; and the Cymel series manufactured by Allnex Japan Co., Ltd.
[0106] The content of the crosslinking agent is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, and is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less, based on 100% by mass of the non-volatile components of the photosensitive material.
[0107] The photosensitive material may contain a photopolymerization initiator. The photopolymerization initiator can promote the reaction of the resin that can be developed with a developer. The photopolymerization initiator may be used alone or in combination of two or more.
[0108] An example of the photopolymerization initiator is a photoacid generator. The photoacid generator can generate an acid when irradiated with actinic rays such as ultraviolet light. For example, the generated acid can promote the reaction of an alkali-soluble resin having a phenolic hydroxyl group in the molecule and a compound having two or more alkoxymethyl groups in the molecule.
[0109] The photoacid generator may be a compound capable of generating an acid upon irradiation with actinic rays, such as a halogen-containing compound, a diazoketone compound, a sulfone compound, a diazomethane compound, or a diazoquinone compound.
[0110] Examples of halogen-containing compounds that can be used as photoacid generators include haloalkyl group-containing hydrocarbon compounds, haloalkyl group-containing heterocyclic compounds, etc. Specific preferred examples of the halogen-containing compound include 2-[2-(furan-2-yl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine, 2-[2-(5-methylfuran-2-yl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine, 2-(methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-[2-(4-methoxyphenyl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine, 2-[2-(3,4-dimethoxyphenyl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine,
[0033] Examples of the halogen-containing compound include s-triazine derivatives such as [4-(4-chlorophenyl)ethenyl]-4,6-bis(trichloromethyl)-s-triazine, 1,10-dibromo-n-decane, 1,1-bis(4-chlorophenyl)-2,2,2-trichloroethane, phenyl-bis(trichloromethyl)-s-triazine, 4-methoxyphenyl-bis(trichloromethyl)-s-triazine, styryl-bis(trichloromethyl)-s-triazine, and naphthyl-bis(trichloromethyl)-s-triazine. Specific examples of the halogen-containing compound include "TFE-triazine," "TME-triazine," "MP-triazine," "MOP-triazine," and "dimethoxytriazine" (halogen-containing compound-based photoacid generators having a triazine skeleton), all manufactured by Sanwa Chemical Co., Ltd.
[0111] Examples of diazoketone compounds, sulfone compounds, and diazoquinone compounds are described in JP 2018-169627 A, WO 2010 / 134207 A, WO 2014 / 069202 A, JP 2020-101813 A, and WO 2018 / 232214 A.
[0112] Other examples of photopolymerization initiators include photoradical generators. When a radical polymerizable resin is used, the photoradical generator can effectively promote the reaction. Examples of photoradical generators include those described in documents such as JP 2020-15859 A, JP 2020-52288 A, and JP 2018-169627 A.
[0113] The content of the photopolymerization initiator is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more, and is preferably 3% by mass or less, more preferably 1.5% by mass or less, based on 100% by mass of the non-volatile components in the photosensitive material.
[0114] The photosensitive material may contain a thermal acid generator. The thermal acid generator can generate acid when the plasma mask is heated, thereby promoting the crosslinking reaction between the resin developable with a developer and the crosslinking agent. The thermal acid generator may be used alone or in combination of two or more types in any ratio.
[0115] Examples of the thermal acid generator include onium salt compounds, and examples of the onium salt compounds include those described in documents such as JP-A-2018-169627.
[0116] The content of the thermal acid generator is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more, and is preferably 3% by mass or less, more preferably 1.5% by mass or less, based on 100% by mass of the non-volatile components in the photosensitive material.
[0117] The photosensitive material may contain an adhesion aid. The adhesion aid may be a compound that improves the adhesion strength between the insulating material layer and the plasma mask. The adhesion aid may be used alone or in combination of two or more types in any ratio.
[0118] Examples of adhesion aids include γ-aminopropyldimethoxysilane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, 3-methacryloxypropyldimethoxymethylsilane, 3-methacryloxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, dimethoxymethyl-3-piperidinopropylsilane, diethoxy-3-glycidoxypropylmethylsilane, N-(3-diethoxymethylsilylpropyl)succinimide, N-[3-(triethoxysilyl)propyl]phthalamic acid, benzophenone-3,3'-bis(N-[3-triethoxysilyl]propylamide)-4,4'-dicarboxylic acid, benzene-1,4-bis(N-3-triethoxysilyl]propylamide)-2,5-Dicarboxylic acid, 3-(triethoxysilyl)propyl succinic anhydride, N-phenylaminopropyltrimethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, 3-(trialkoxysilyl)propylsuccinic anhydride, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, mercaptomethyltrimethoxysilane, mercaptomethylmethyldimethoxysilane, 3-mercaptopropyldiethoxymethoxysilane, 3-mercaptopropylethoxydimethoxysilane, 3-mercaptopropyltripropoxysilane, 3-mercaptopropyldiethoxypropoxysilane, 3-mercaptopropylethoxydipropoxysilane, 3-mercaptopropyldimethoxypropoxysilane, 3-mercaptopropylmethoxydipropoxysilane, 2-mercaptopropyl Examples of suitable silane coupling agents include triethyltrimethoxysilane, 2-mercaptoethyldiethoxymethoxysilane, 2-mercaptoethylethoxydimethoxysilane, 2-mercaptoethyltripropoxysilane, 2-mercaptoethyltrippropoxysilane, 2-mercaptoethylethoxydipropoxysilane, 2-mercaptoethyldimethoxypropoxysilane, 2-mercaptoethylmethoxydipropoxysilane, 4-mercaptobutyltrimethoxysilane, 4-mercaptobutyltriethoxysilane, 4-mercaptobutyltrippropoxysilane, N-(3-triethoxysilylpropyl)urea, N-(3-trimethoxysilylpropyl)urea, and compounds having an aminotriazine ring and an ethoxysilyl group; and aluminum-based adhesion promoters such as aluminum tris(ethylacetoacetate), aluminum tris(acetylacetonate), and ethylacetoacetate aluminum diisopropylate.
[0119] The content of the adhesion aid is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, even more preferably 0.1% by mass or more, relative to 100% by mass of the non-volatile components of the photosensitive material, and is preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 1% by mass or less.
[0120] The photosensitive material may contain an organic filler. Examples of organic fillers include urethane particles, rubber particles, polyamide particles, and silicone particles. Of these, urethane particles are preferred. Examples of urethane particles include "MM-101SW," "MM-101SWA," "MM-101SM," "MM-101SMA," and "MM-110SMA" manufactured by Negami Chemical Industrial Co., Ltd. One type of organic filler may be used alone, or two or more types may be used in combination at any ratio.
[0121] The average particle size of the organic filler is preferably 0.005 μm or more, more preferably 0.2 μm or more, and preferably 1 μm or less, more preferably 0.6 μm or less. The average particle size of the organic filler can be measured using dynamic light scattering. Specifically, the average particle size of the organic filler can be measured by uniformly dispersing the organic filler in an appropriate organic solvent using ultrasonic waves, creating a particle size distribution of the organic filler on a mass basis using a concentrated particle size analyzer (FPAR-1000; manufactured by Otsuka Electronics Co., Ltd.), and taking the median diameter as the average particle size.
[0122] The content of the organic filler is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, and is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less, assuming that the non-volatile components of the photosensitive material are 100% by mass.
[0123] The photosensitive material may or may not contain an inorganic filler. When the photosensitive material contains an inorganic filler, the content of the inorganic filler may be less than the lower limit of the range of the content of the inorganic filler in the thermosetting material, for example, 10% by mass or less relative to 100% by mass of the nonvolatile components of the photosensitive material. The content of the inorganic filler in the photosensitive material is usually preferably within the range of the content of the inorganic filler in the thermosetting material.
[0124] When the photosensitive material contains an inorganic filler, the average particle size of the inorganic filler is preferably 0.2 μm or less, more preferably 0.15 μm or less, even more preferably 0.1 μm or less, and preferably 0.01 μm or more, more preferably 0.03 μm or more, particularly preferably 0.05 μm or more.
[0125] The photosensitive material may further contain other additives in addition to the components described above. Examples of the other additives include a polymerization inhibitor, an antifoaming agent, a surfactant, a thermoplastic resin, a colorant, a thickener, an antifoaming agent, and a flame retardant. The photosensitive material may also contain components that can be contained in the thermosetting material described above. The other additives may be used alone or in combination of two or more.
[0126] The photosensitive material may contain a solvent as a volatile component, which is the same as the solvent that may be contained in the thermosetting material.
[0127] The photosensitive material may contain a solvent, but the amount thereof is preferably small. The amount of solvent contained in the photosensitive material is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less, based on 100% by mass of the nonvolatile components in the photosensitive material.
[0128] The method for preparing the photosensitive material is not particularly limited, and examples thereof include a method in which the ingredients are kneaded and dispersed, if necessary, together with a solvent, using a kneading or stirring device. A preferred embodiment of the photosensitive material is a negative-type photosensitive material that contains a polyimide precursor and can be developed with a solvent, i.e., a solvent-developable negative-type photosensitive polyimide resin. The photosensitive material is preferably in a liquid state.
[0129] The photosensitive material may be a commercially available product, such as "SU-8 3010" manufactured by Nippon Kayaku Co., Ltd.
[0130] A cured product of a photosensitive material usually exhibits the characteristic of a high glass transition temperature (Tg). Therefore, when a plasma mask is formed using this cured product, a plasma mask with a high glass transition temperature can be obtained. The glass transition temperature of the cured product is preferably 130°C or higher, more preferably 140°C or higher, and even more preferably 150°C or higher. The upper limit is not particularly limited, but can be, for example, 400°C or lower. The glass transition temperature can be measured by the method described in the examples below.
[0131] A cured product of a photosensitive material typically exhibits the characteristic of a low coefficient of linear thermal expansion (CTE). Therefore, when a plasma mask is formed using this cured product, a plasma mask with a low coefficient of linear thermal expansion can be obtained. The coefficient of linear thermal expansion of the cured product is preferably 100 ppm / °C or less, more preferably 80 ppm / °C or less, and even more preferably 75 ppm / °C or less. The lower limit is not particularly limited, but can be, for example, 0.01 ppm / °C or more. The coefficient of linear thermal expansion can be measured by the method described in the examples below.
[0132] The cured product of the photosensitive material typically exhibits a high modulus of elasticity at 23°C. This allows for the production of a plasma mask with excellent crack resistance. The modulus of elasticity of the cured product at 23°C is preferably 1.0 GPa or more, more preferably 1.5 GPa or more, and even more preferably 2.0 GPa or more. There is no particular upper limit, but it can be 50 GPa or less, for example. The modulus of elasticity can be measured by the method described in the examples below.
[0133] A cured product of a photosensitive material usually exhibits the characteristic of large elongation (elongation at break). Therefore, a plasma mask with a large elongation at break can be obtained. The elongation at break of the cured product is preferably 10% or more, more preferably 20% or more, and particularly preferably 30% or more. There is no particular upper limit, and it can be, for example, 80% or less, 70% or less, or 60% or less. The elongation can be measured according to the method described in the examples below.
[0134] In the present invention, it is preferable that the breaking elongation of the cured product of the photosensitive material is greater than the breaking elongation of the cured product of the thermosetting material.
[0135] A cured product of a photosensitive material usually exhibits the characteristic of a low dielectric loss tangent. Therefore, a plasma mask with a low dielectric loss tangent can be obtained. The dielectric loss tangent of the cured product is preferably 0.05 or less, more preferably 0.04 or less, and even more preferably 0.03 or less. There is no particular restriction on the lower limit of the dielectric loss tangent, and it can be, for example, 0.0005 or more. The dielectric loss tangent can be measured by the method described in the examples below.
[0136] A cured product of a photosensitive material usually exhibits the characteristic of a low dielectric constant. Therefore, a plasma mask with a low dielectric constant can be obtained. The dielectric constant of the cured product is preferably 5.0 or less, more preferably 4.0 or less, and even more preferably 3.5 or less. The lower limit is not particularly limited, but may be, for example, 0.0001 or more. The dielectric constant can be measured by the method described in the examples below. In the present invention, it is preferable that the dielectric constant of the cured product of the photosensitive material and the dielectric constant of the cured product of the thermosetting material are both 3.5 or less.
[0137] [Thermosetting resin sheet and photosensitive resin sheet] The thermosetting resin sheet includes a support and a thermosetting material layer formed of a thermosetting material provided on the support. The thermosetting material is as described in the [Thermosetting material] section.
[0138] The photosensitive resin sheet includes a support and a photosensitive material layer formed of a photosensitive material provided on the support. The photosensitive material is as described in the [Photosensitive Material] section.
[0139] Hereinafter, the thermosetting material layer and the photosensitive material layer may be collectively referred to as "material layer", and the thermosetting resin sheet and the photosensitive resin sheet may be collectively referred to as "resin sheet".
[0140] The thickness of the thermosetting material layer is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 40 μm or less, 30 μm or less, or 20 μm or less, from the viewpoints of thinning the printed wiring board and providing a cured product with excellent insulating properties even when the cured product of the thermosetting material layer is thin. The lower limit of the thickness of the thermosetting material layer is not particularly limited, but can usually be 1 μm or more, 3 μm or more, etc.
[0141] The thickness of the photosensitive material layer is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 40 μm or less, from the viewpoint of significantly obtaining the effects of the present invention. The lower limit of the thickness of the photosensitive material layer is preferably 1 μm or more, more preferably 3 μm or more, and even more preferably 5 μm or more, from the viewpoint of leaving a film as a plasma mask on the insulating material layer.
[0142] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.
[0143] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, with inexpensive polyethylene terephthalate being particularly preferred.
[0144] When a metal foil is used as the support, examples of the metal foil include copper foil and aluminum foil, with copper foil being preferred. The copper foil may be a foil made of a single metal, such as copper, or a foil made of an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.).
[0145] The surface of the support that is to be bonded to the material layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.
[0146] The support may also be a support with a release layer, which has a release layer on the surface that bonds with the material layer. Examples of the release agent used in the release layer of the support with a release layer include one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. Commercially available products may be used as the support with a release layer, including, for example, PET films having a release layer primarily composed of an alkyd resin-based release agent, such as "SK-1," "AL-5," and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Uni-Peel" manufactured by Unitika Limited; and "U2-NR1" manufactured by DuPont Films.
[0147] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the thickness of the entire support with a release layer is in the above range.
[0148] In one embodiment, the resin sheet may further include other layers as necessary. Examples of such other layers include a protective film conforming to the support and provided on the surface of the material layer that is not bonded to the support (i.e., the surface opposite the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, it is possible to prevent the adhesion of dust and the like to the surface of the material layer and scratches.
[0149] The resin sheet can be produced, for example, by preparing a resin varnish by dissolving a thermosetting material or a photosensitive material in an organic solvent, applying the resin varnish to a support using a die coater or the like, and then drying the applied resin varnish to form a material layer. The solvent may be any of those described above.
[0150] Drying may be carried out by known methods such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is carried out so that the content of organic solvent in the material layer becomes 10% by mass or less, preferably 5% by mass or less. Although this varies depending on the boiling point of the organic solvent in the resin varnish, for example, when a resin varnish containing 30% by mass to 60% by mass of organic solvent is used, the material layer can be formed by drying at 50°C to 150°C for 3 to 10 minutes.
[0151] The resin sheet can be stored in a rolled state. When the resin sheet has a protective film, it can be used by peeling off the protective film.
[0152] [Prepreg] The prepreg is formed by impregnating a sheet-like fiber substrate with the above-mentioned thermosetting material.
[0153] The sheet-like fiber substrate used for the prepreg can be, for example, a commonly used prepreg substrate such as glass cloth, aramid nonwoven fabric, or liquid crystal polymer nonwoven fabric. From the viewpoint of thinning the wiring board, the thickness of the sheet-like fiber substrate is preferably 50 μm or less, more preferably 40 μm or less, even more preferably 30 μm or less, and particularly preferably 20 μm or less. The lower limit of the thickness of the sheet-like fiber substrate is not particularly limited, and is usually 10 μm or more. The thickness of the prepreg can be in the same range as the above-mentioned sheet-like fiber substrate.
[0154] The prepreg can be produced by a method such as a hot melt method or a solvent method.
[0155] [Method for Manufacturing a Wiring Board] A first embodiment of the method for manufacturing a wiring board of the present invention includes the steps of: (1) preparing a substrate having a conductor circuit and, on the conductor circuit, an insulating material layer formed of a cured product of a thermosetting material, and forming the photosensitive material layer by applying and / or attaching a photosensitive material to the surface of the insulating material layer; (2) exposing and developing the photosensitive material layer to form a plasma mask having openings; (3) irradiating the insulating material layer with plasma through the plasma mask to form either or both of a via hole and a trench in the insulating material layer located at the openings in the plasma mask, and thinning the plasma mask; and (4) forming a conductor layer on the surfaces of the thinned plasma mask and either or both of the via hole and the trench.
[0156] As mentioned above, conventionally, via holes or trenches are formed in an insulating material layer by forming a mask such as a dry film or metal foil on the insulating material layer, patterning the mask to form a mask pattern, and then performing plasma or laser treatment through the mask pattern to peel or remove the mask pattern. The wiring board manufacturing method of the present invention leaves a plasma mask corresponding to the conventional mask pattern as a primer layer (permanent film), eliminating the need to remove the mask pattern as in the past. In the present invention, the plasma mask is left intact, preventing chemical damage to the insulating material layer by a stripper used to remove the mask pattern. As a result, the insulating material layer has excellent insulating properties and electrical properties, and can improve its insulating performance after HAST testing. In particular, since cured products of thermosetting materials tend to have better insulating properties and electrical properties than cured products of photosensitive materials, combining an insulating material layer formed from a cured product of a thermosetting material with a plasma mask formed from a cured product of a photosensitive material can effectively improve insulating properties and electrical properties. Furthermore, since the photosensitive material layer is formed on the insulating material layer, the mask pattern can be easily aligned, making it possible to form small diameter via holes or small diameter trenches.
[0157] <Step (1)> In step (1), a substrate is prepared in which an insulating material layer is formed on an inner layer circuit board on which conductor circuits are formed, and a photosensitive material is applied and / or attached (laminated) to the insulating material layer of the substrate to form a photosensitive material layer. In step (1), as shown in an example in Figure 1, a substrate 10 is prepared in which an insulating material layer 11 is formed on the conductor circuits of an inner layer circuit board 12 on which conductor circuits (not shown) are formed. The insulating material layer 11 contains a cured product of a thermosetting material, from the viewpoint of significantly achieving the effects of the present invention.
[0158] The step (1) may include a step (1-1) of preparing an inner layer circuit board on which a conductor circuit is formed. The inner layer circuit board on which a conductor circuit is formed typically includes a support substrate and a metal layer provided on the surface of the support substrate. The metal layer is typically exposed on the surface of the inner layer circuit board and functions as a conductor circuit.
[0159] Examples of materials for the support substrate include a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, a thermosetting polyphenylene ether substrate, etc. Examples of materials for the metal layer include copper foil, copper foil with a carrier, and materials for the conductor layer described below, with copper foil being preferred.
[0160] The conductor circuit can be formed by the same method as that for forming the conductor layer in step (4) described below.
[0161] When the conductor circuit is a patterned conductor circuit, the line (conductor layer width) / space (width between conductor layers) (L / S) of the conductor circuit, i.e., the wiring pitch of the conductor circuit, is preferably 5 μm / 5 μm or less (i.e., wiring pitch of 10 μm or less), more preferably 4 μm / 4 μm or less (wiring pitch of 8 μm or less), and even more preferably 3 μm / 3 μm or less (wiring pitch of 6 μm or less) from the viewpoint of fine wiring. The lower limit of the line / space ratio of the conductor circuit is preferably 0.1 μm / 0.1 μm or more (wiring pitch of 0.2 μm or more), more preferably 0.5 μm / 0.5 μm or more (wiring pitch of 1 μm or more), and even more preferably 1 μm / 1 μm or more (wiring pitch of 2 μm or more). The wiring pitch does not need to be uniform throughout the entire conductor circuit.
[0162] The step (1) may include a step (1-2) of forming a thermosetting material layer on the conductor circuit of the inner layer circuit board and thermally curing the thermosetting material layer to form an insulating material layer. Examples of methods for forming the insulating material layer include a method of applying a thermosetting material directly to the conductor circuit of the inner layer circuit board to form a thermosetting material layer and then thermally curing the layer to form an insulating material layer; a method of attaching (laminating) a thermosetting resin sheet to the conductor circuit of the inner layer circuit board and thermally curing the thermosetting material layer to form an insulating material layer; and a method of laminating a prepreg on the conductor circuit of the inner layer circuit board and thermally curing the prepreg to form an insulating material layer. Among these, from the viewpoint of achieving the most significant effects of the present invention, the step (1-2) is preferably a step of laminating a thermosetting material layer of a thermosetting resin sheet on the conductor circuit of the inner layer circuit board and thermally curing the thermosetting material layer to form an insulating material layer. The thermosetting material, the thermosetting resin sheet, and the prepreg are as described above. The insulating material layer may be a single layer or a laminate of multiple layers.
[0163] The lamination of the inner layer circuit board and the thermosetting resin sheet can be carried out, for example, by thermocompression bonding the thermosetting resin sheet to the inner layer circuit board from the support side. Examples of a member for thermocompression bonding the thermosetting resin sheet to the inner layer circuit board (hereinafter also referred to as a "thermocompression bonding member") include a heated metal plate (such as a SUS panel) or a metal roll (such as a SUS roll). Note that rather than pressing the thermocompression bonding member directly onto the thermosetting resin sheet, it is preferable to press it via an elastic material such as heat-resistant rubber so that the thermosetting resin sheet can sufficiently conform to the surface irregularities of the inner layer circuit board.
[0164] The lamination of the inner layer circuit board and the thermosetting resin sheet may be carried out by a vacuum lamination method. In the vacuum lamination method, the thermocompression bonding temperature is preferably in the range of 60°C to 160°C, more preferably 80°C to 140°C, the thermocompression bonding pressure is preferably in the range of 0.098 MPa to 1.77 MPa, more preferably 0.29 MPa to 1.47 MPa, and the thermocompression bonding time is preferably in the range of 20 seconds to 400 seconds, more preferably 30 seconds to 300 seconds. The lamination is preferably carried out under reduced pressure conditions of 26.7 hPa or less.
[0165] The lamination can be performed using a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch-type vacuum pressure laminator.
[0166] After lamination, the laminated thermosetting resin sheets may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. Note that the lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.
[0167] The support may be removed after laminating the thermosetting resin sheet and before thermal curing, or after thermal curing the thermosetting material layer, or before forming the photosensitive material layer on the insulating material layer.
[0168] After laminating the thermosetting resin sheet on the inner layer circuit board, the thermosetting material layer is thermally cured to form an insulating material layer. The thermal curing conditions for the thermosetting material layer are not particularly limited, and conditions typically employed for forming insulating material layers for printed wiring boards may be used.
[0169] For example, although the heat curing conditions for the thermosetting material layer vary depending on the type of thermosetting material, the curing temperature is preferably 120° C. to 240° C., more preferably 150° C. to 220° C., and even more preferably 170° C. to 210° C. The curing time is preferably 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and even more preferably 15 minutes to 100 minutes.
[0170] Before thermally curing the thermosetting material layer, the thermosetting material layer may be preheated at a temperature lower than the curing temperature. For example, prior to thermally curing the thermosetting material layer, the thermosetting material layer may be preheated at a temperature of 50°C or higher and lower than 120°C (preferably 60°C or higher and 115°C or lower, more preferably 70°C or higher and 110°C or lower) for 5 minutes or longer (preferably 5 to 150 minutes, more preferably 15 to 120 minutes, and even more preferably 15 to 100 minutes).
[0171] The thickness of the insulating material layer is preferably 100 μm or less, more preferably 50 μm or less, further preferably 40 μm or less, 30 μm or less, or 20 μm or less, and is preferably 1 μm or more, more preferably 3 μm or more.
[0172] When an insulating material layer is formed by applying a thermosetting material directly onto the conductor circuit of an inner layer circuit board, the conditions for forming the insulating material layer are the same as those for forming an insulating material layer using a thermosetting resin sheet. Examples of methods for applying the thermosetting material include wire bar coating, reverse coating, gravure coating, die coating, blade coating, dip coating, air knife coating, curtain coating, and roller coating. When an insulating material layer is formed using a prepreg, the conditions for forming the insulating material layer are the same as those for forming an insulating material layer using a thermosetting resin sheet.
[0173] As shown in FIG. 2 as an example, step (1) includes step (1-3) of forming a photosensitive material layer 20 by applying and / or attaching a photosensitive material to the surface of the insulating material layer 11. Details of the photosensitive material layer 20 include a method of forming a photosensitive material layer by applying a photosensitive material directly to the surface of the insulating material layer, and a method of attaching (laminating) a photosensitive resin sheet having a photosensitive material layer on the surface of the insulating material layer. The photosensitive material and the photosensitive resin sheet are as described above. The photosensitive material layer may be a single layer, or multiple layers may be laminated.
[0174] The absolute value of the difference between the linear thermal expansion coefficient of the cured product of the photosensitive material (plasma mask) and the linear thermal expansion coefficient of the cured product of the thermosetting material (insulating material layer) is preferably 60 ppm / °C or less, more preferably 55 ppm / °C or less, and even more preferably 50 ppm / °C or less, and although there is no particular lower limit, it is preferably 0 ppm / °C or more, more preferably 0.5 ppm / °C or more, and even more preferably 1 ppm / °C or more. By selecting a photosensitive material (or a photosensitive material layer when the photosensitive material layer 20 is formed from a photosensitive resin sheet) so that the absolute value of the difference in the linear thermal expansion coefficient of the cured product of the photosensitive material falls within this range, the effects of the present invention can be significantly achieved.
[0175] The absolute value of the difference between the glass transition temperature (Tg) of the photosensitive material that can be contained in the plasma mask and the glass transition temperature (Tg) of the thermosetting material that can be contained in the insulating material layer is preferably 100° C. or less, more preferably 90° C. or less, and even more preferably 80° C. or less, and although there is no particular lower limit, it is preferably 0° C. or more, more preferably 0.5° C. or more, and even more preferably 1° C. or more. By selecting a photosensitive material (or a photosensitive material layer when the photosensitive material layer 20 is formed from a photosensitive resin sheet) so that the absolute value of the difference in glass transition temperature of the cured product of the photosensitive material falls within this range, it becomes possible to obtain the effects of the present invention significantly.
[0176] The linear thermal expansion coefficient of the bulk laminated with the cured photosensitive material (plasma mask) and the cured thermosetting material (insulating material layer) is preferably 100 ppm / °C or less, more preferably 50 ppm / °C or less, and even more preferably 45 ppm / °C or less. There is no particular lower limit, but it may be 1 ppm / °C or more, 10 ppm / °C or more, etc. By selecting the photosensitive material (the photosensitive material layer when the photosensitive material layer 20 is formed from a photosensitive resin sheet) and the thermosetting material (the thermosetting material layer when the insulating material layer is formed from a thermosetting resin sheet) so that the linear thermal expansion coefficient of the bulk falls within this range, the effects of the present invention can be significantly achieved.
[0177] The lamination conditions for the insulating material layer and the photosensitive resin sheet may be the same as the lamination conditions for the inner layer circuit board and the thermosetting resin sheet.
[0178] When forming a photosensitive material layer by applying a photosensitive material directly onto the surface of an insulating material layer, the application method of the photosensitive material may be the same as the application method when applying a thermosetting material directly onto the conductor circuit of an inner layer circuit board. In this case, the photosensitive material is preferably in liquid form.
[0179] The thickness of the photosensitive material layer is the same as the thickness of the photosensitive material layer in the photosensitive resin sheet.
[0180] <Step (2)> In step (2), as shown in an example in Fig. 3, the photosensitive material layer 20 is irradiated with active energy rays, exposed, and developed to form a plasma mask 21 having openings 211. In detail, the exposure is performed by irradiating the surface of the photosensitive material layer with active energy rays through a photomask not shown in Fig. 3, thereby curing the photosensitive material layer. In step (2), as shown in an example in Fig. 9, a plasma mask 21 having a plurality of openings 211 may be formed.
[0181] Examples of the active energy ray include ultraviolet light, visible light, electron beams, and X-rays, with ultraviolet light being preferred. The dose and duration of ultraviolet light irradiation can be appropriately set depending on the photosensitive material layer. Examples of the exposure method include a contact exposure method in which a mask pattern is brought into close contact with the photosensitive material layer and exposed, and a non-contact exposure method in which a mask pattern is not brought into close contact with the photosensitive material layer and exposed using parallel light.
[0182] After exposure, development is performed to remove the exposed or unexposed portions of the photosensitive material layer to form a plasma mask. Development may be performed by either wet development or dry development. Examples of development methods include dipping, puddling, spraying, brushing, and scraping.
[0183] In step (2), if necessary, a descum treatment may be carried out by plasma treatment after development to remove residues such as deposits remaining on the surface of the plasma mask.
[0184] From the viewpoint of obtaining the effects of the present invention significantly, the thickness of the plasma mask is preferably 0.1 μm or more, more preferably 0.3 μm or more, even more preferably 0.5 μm or more, and is preferably 20 μm or less, more preferably 10 μm or less, even more preferably 5 μm or less.
[0185] When the thickness of the plasma mask after the completion of step (2) is T1 (μm) and the thickness of the insulating material layer after the completion of step (2) is T2 (μm), it is preferable to satisfy the relationship T1 > T2 from the viewpoint of significantly obtaining the effects of the present invention.
[0186] 4, in step (3), plasma is irradiated from above insulating material layer 11 through plasma mask 21 to form either or both of via holes 30 and trenches (not shown) in insulating material layer 11 located at openings 211 in plasma mask 21, and simultaneously etch the plasma mask 21 to reduce the thickness of plasma mask 21. As shown in an example in Fig. 5, after step (3) is completed, plasma mask 21 is etched and reduced in thickness by the plasma irradiation, but remains as a primer layer (permanent film) on insulating material layer 11.
[0187] The thickness of the plasma mask after plasma irradiation, i.e., the thickness of the reduced plasma mask after step (3), is preferably 0.01 or more, more preferably 0.05 or more, even more preferably 0.1 or more, or 0.15 or more, relative to the thickness of the plasma mask before plasma irradiation, which is taken as 1, from the viewpoint of significantly obtaining the effects of the present invention. It is preferably 0.7 or less, more preferably 0.6 or less, and even more preferably 0.5 or less. In conventional wiring board manufacturing methods, the mask is removed or peeled off after the via hole or trench is formed, so the thickness of the mask after plasma treatment is at most 0.05, relative to the thickness of the mask before plasma treatment, which is taken as 1.
[0188] From the viewpoint of significantly obtaining the effects of the present invention, the thickness of the reduced plasma mask after step (3) is preferably 0.1 μm or more, more preferably 0.3 μm or more, even more preferably 0.5 μm or more, and preferably 20 μm or less, more preferably 10 μm or less, even more preferably 5 μm or less.
[0189] From the viewpoint of significantly obtaining the effects of the present invention, the total thickness of the reduced plasma mask and the insulating material layer after step (3) is preferably 20 μm or less, more preferably 15 μm or less, even more preferably 13 μm or less, and is preferably 1 μm or more, more preferably 3 μm or more, even more preferably 5 μm or more.
[0190] The plasma treatment in step (3) involves treating the surfaces of the insulating material layer and the plasma mask located at the opening with plasma generated by introducing a gas into a plasma generator, thereby forming a via hole or a trench in the surface of the insulating material layer located at the opening, and reducing the thickness of the plasma mask by etching. The method for generating plasma is not particularly limited, and examples include microwave plasma generated by microwaves, high-frequency plasma using high frequency waves, atmospheric pressure plasma generated under atmospheric pressure, and atmospheric pressure plasma generated in a vacuum, with atmospheric pressure plasma generated in a vacuum being preferred.
[0191] The plasma used in step (3) is preferably RF plasma excited by high frequency waves.
[0192] Examples of gases that can be turned into plasma include Ar and O. 2 , C.F. 4 and SF 6 and O 2 and CF 4 A mixed gas containing the following is more preferred.
[0193] O 2 and CF 4 Mixing ratio of mixed gas containing (CF 4 / O 2 The ratio of the ionic liquid to the conductive layer (unit: sccm) is preferably 99 / 1 to 1 / 99, more preferably 90 / 10 to 30 / 70, and even more preferably 90 / 10 to 70 / 30, from the viewpoint of making the thickness of the conductive layer formed in the via hole or trench uniform.
[0194] The plasma irradiation time in the plasma treatment is not particularly limited, but is preferably 1 minute or more, more preferably 2 minutes or more, and even more preferably 3 minutes or more. The upper limit is not particularly limited, but is preferably 120 minutes or less, more preferably 100 minutes or less, and even more preferably 60 minutes or less.
[0195] In the present invention, via holes or trenches are formed in the insulating material layer located at the openings of the plasma mask by plasma treatment, so that the opening diameter of the via holes or trenches can be made small. The opening diameter is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less. The lower limit is not particularly limited, but may be 1 μm or more.
[0196] From the viewpoint of obtaining the remarkable effect of the present invention, the etching rate by plasma irradiation is preferably 100 nm / min or more, more preferably 110 nm / min or more, and even more preferably 120 nm / min or more. There is no particular upper limit, but it is preferably 2000 nm / min or less, more preferably 1500 nm / min or less, and even more preferably 1000 nm / min or less.
[0197] In the present invention, since the via hole or trench is formed by plasma treatment, the via taper angle of the via hole or trench can be made to be approximately 90 degrees. The via taper angle is preferably 65 degrees or more, more preferably 70 degrees or more, and even more preferably 72 degrees or more. There is no particular upper limit, but it is preferably 90 degrees or less, more preferably 88 degrees or less, and even more preferably 85 degrees or less. The via taper angle refers to the angle between the wall surface of the via hole or trench and the via bottom.
[0198] The arithmetic mean roughness (Ra) of the plasma mask surface after the plasma treatment, from the viewpoint of obtaining the effects of the present invention remarkably, is preferably 100 nm or less, more preferably 80 nm or less, and even more preferably 60 nm or less. There is no particular lower limit, but it may be 1 nm or more, 10 nm or more, etc. The arithmetic mean roughness can be measured by the method described in the examples below.
[0199] From the viewpoint of obtaining a significant effect of the present invention, the roughness (Sa) of the wall surface of the via hole or trench after plasma treatment is preferably 400 nm or less, more preferably 350 nm or less, and even more preferably 300 nm or less. There is no particular lower limit, but it can be 110 nm or more, 150 nm or more, etc. The roughness (Sa) represents the arithmetic mean height specified in ISO 25178 and can be measured by the method described in the examples below.
[0200] From the viewpoint of significantly obtaining the effects of the present invention, the ratio (Ra / Sa) of the arithmetic mean roughness (Ra) of the surface of the reduced plasma mask after plasma treatment to the roughness (Sa) of the wall surface of the via hole or trench after plasma treatment is preferably 3 or less, more preferably 2 or less, even more preferably 1 or less, or 0.5 or less, and is preferably 0.01 or more, more preferably 0.05 or more, and even more preferably 0.1 or more.
[0201] From the viewpoint of obtaining a significant effect of the present invention, the via expansion ratio is preferably 150% or less, more preferably 145% or less, even more preferably 140% or less, and preferably 100% or more, even more preferably 105% or more, and even more preferably 110% or more. The via expansion ratio is expressed as a ratio of the diameter of the boundary between the plasma mask and the insulating material layer in the via hole or trench after the completion of step (3), with the diameter of the bottom of the plasma mask pattern after the completion of step (2) being 100%. A ratio exceeding 100% means that the diameter has expanded, while a ratio less than 100% means that the diameter has contracted. In the present invention, even if plasma treatment is performed in step (3), the diameter of the bottom of the plasma mask pattern is prevented from becoming too large, thereby enabling fine wiring. The via expansion ratio can be measured by the method described in the Examples below.
[0202] When the thickness of the reduced plasma mask after the completion of step (3) is T3 (μm) and the thickness of the insulating material layer after the completion of step (3) is T4 (μm), it is preferable to satisfy the relationship T3 < T4 from the viewpoint of obtaining the effects of the present invention significantly.
[0203] <Step (4)> Step (4) is a step of forming a conductor layer on the surface of the reduced plasma mask and on either or both of the via hole and trench exposed through the opening in the plasma mask. Details of the conductor layer include either or both of a conductor wiring formed at a position other than the opening in the plasma mask and a conductor via layer formed in the opening in the plasma mask. The conductor material used for the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin, and indium. The conductor layer may be a single metal layer or an alloy layer. Examples of alloy layers include layers formed from an alloy of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy, and copper-titanium alloy). Among these, from the viewpoints of versatility in forming the conductor layer, cost, ease of patterning, etc., a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy, a copper-nickel alloy, or a copper-titanium alloy is preferred, and a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy is more preferred.
[0204] The conductor layer may have a single layer structure or a multi-layer structure in which two or more single metal layers or alloy layers made of different types of metals or alloys are stacked. When the conductor layer has a multi-layer structure, the layer in contact with either the via hole or the trench is preferably a single metal layer of chromium, zinc, or titanium, or an alloy layer of a nickel-chromium alloy.
[0205] The thickness of the conductor layer depends on the desired design of the printed wiring board, but is generally 3 μm to 35 μm, preferably 5 μm to 30 μm.
[0206] The conductor layer can be formed by any suitable conventional method such as plating, sputtering, vapor deposition, etc., and is preferably formed by plating. In one suitable embodiment, for example, a patterned conductor layer having a desired wiring pattern is formed by plating the surface of a plasma mask that has been thinned by a conventional technique such as a semi-additive method or a full-additive method, and one or both of the via hole and the trench.
[0207] Step (4) may include, as an example shown in FIG. 6 , a step (4-1) of forming a plating seed layer 41 on the surface of the reduced plasma mask 21 and on the surface of either or both of the via hole 30 and the trench (not shown). The plating seed layer may be formed by dry plating or wet plating. Examples of dry plating include physical vapor deposition (PVD) methods such as sputtering, ion plating, and vacuum deposition, and chemical vapor deposition (CVD) methods such as thermal CVD and plasma CVD. Examples of wet plating include electroless plating. In step (4-1), the plating seed layer is preferably formed by dry plating, and more preferably by sputtering from the viewpoint of achieving fine wiring.
[0208] When forming a conductive layer by sputtering, typically, a conductive seed layer is first formed by sputtering on the surface of the reduced plasma mask and on the surface of either or both of the via hole and trench, and then a conductive sputter layer is formed on the conductive seed layer by sputtering. Before forming the conductive seed layer by sputtering, the surface of the reduced plasma mask and the surface of either or both of the via hole and trench may be cleaned by reverse sputtering. Furthermore, if a trench is present, an optional diffusion prevention layer may be provided to improve insulation reliability. Various gases can be used for the reverse sputtering, among which Ar, O 2 , N 2 When the seed layer is made of Cu or a Cu alloy, Ar or O is preferable. 2 Or Ar, O 2 Mixture gas, Ar or N when the seed layer is Ti2 Or Ar, N 2 Mixture gas, Ar or O if the seed layer is Cr or Cr alloy (such as nichrome) 2 Or Ar, O 2 A mixed gas is preferred. Sputtering can be performed using various sputtering devices such as magnetron sputtering and mirror tron sputtering. Examples of metals that form the conductive seed layer include Cr, Ni, Ti, nichrome, etc. Cr and Ti are particularly preferred. The thickness of the conductive seed layer is usually preferably 5 nm or more, more preferably 10 nm or more, and is preferably formed to be 1000 nm or less, more preferably 500 nm or less. Examples of metals that form the conductive sputter layer include Cu, Pt, Au, Pd, etc. Cu is particularly preferred. The thickness of the conductive sputter layer is usually preferably 50 nm or more, more preferably 100 nm or more, and is preferably formed to be 3000 nm or less, more preferably 1000 nm or less.
[0209] When forming the conductive seed layer, the surface roughness (Ra value) formed on the surface of the reduced plasma mask and on the surface of either or both of the via hole and the trench is preferably 150 nm or less, more preferably in the range of 10 to 150 nm, and even more preferably 10 to 120 nm, measured after removing the conductive seed layer by etching.
[0210] After forming a plating seed layer 41 by sputtering, the method may further include a step (4-2) of plating on the plating seed layer 41 to form a conductor layer, as shown in an example in FIG. 7. Specifically, after forming the plating seed layer, a mask pattern (not shown) is formed to expose a portion of the plating seed layer. The mask pattern can be formed, for example, by bonding a dry film to the plating seed layer and then performing exposure, development, and cleaning under predetermined conditions. In the case of trench-filled wiring, wiring can be formed by filling the trench with plating and then polishing the resulting material using a polishing process such as CMP.
[0211] The dry film may be a photosensitive dry film made of a photoresist composition. Examples of such dry films include dry films made of novolac resin, acrylic resin, etc. Commercially available dry films may be used, such as "Photec RY-5115" manufactured by Resonac Corporation and "ALPHO 20A263" manufactured by Nikko Materials Co., Ltd.
[0212] Next, an electrolytic plating layer 42 is formed by electrolytic plating on the exposed plating seed layer 41. When either or both of a via hole and a trench are present, the electrolytic plating layer 42 may be formed on the exposed plating seed layer 41 by electrolytic plating, and either or both of the via hole and the trench may be filled by electrolytic plating to form a filled via.
[0213] After forming the electrolytic plating layer 42, as shown in an example in Fig. 8, the mask pattern (not shown) is removed, and the unnecessary plating seed layer 41 is removed by an etching process such as flash etching, to form the conductor layer 40. After removing the mask pattern, an annealing process may be performed as needed. In Fig. 8, the conductor layer 40 is a patterned conductor layer, but it may also be an unpatterned conductor layer.
[0214] The mask pattern can be removed using an alkaline remover such as a sodium hydroxide solution.
[0215] The annealing treatment can be carried out, for example, by heating the inner layer substrate at 150 to 200° C. for 20 to 90 minutes.
[0216] Flash etching is usually performed using an etchant such as an etching solution. For example, when the material of the patterned conductor layer is copper, examples of the etching solution include an etching solution containing hydrogen peroxide as a main component (hydrogen peroxide-based etching solution), an acidic etching solution, and an alkaline etching solution.
[0217] From the viewpoint of significantly obtaining the effects of the present invention, the temperature of the etching solution is preferably 5°C or higher, more preferably 10°C or higher, and even more preferably 15°C or higher, and is preferably 60°C or lower, more preferably 50°C or lower, and even more preferably 40°C or lower.
[0218] From the viewpoint of thinning, the thickness of the conductor layer is preferably 30 μm or less, more preferably 20 μm or less, and even more preferably 10 μm or less. The lower limit is preferably 1 μm or more, more preferably 2 μm or more, and even more preferably 3 μm or more.
[0219] When the conductor layer is a patterned conductor layer, the line width of the patterned conductor layer (conductor layer width) is preferably 5 μm or less, more preferably 4 μm, and even more preferably 3 μm from the viewpoint of fine wiring. The lower limit of the line width of the conductor layer is not particularly limited, but is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1 μm or more.
[0220] When the conductor layer is a patterned conductor layer, the space between the patterned conductor layers (the width between the conductor layers) is preferably 5 μm or less, more preferably 4 μm, and even more preferably 3 μm, from the viewpoint of achieving fine wiring. The lower limit of the line of the conductor layer is not particularly limited, but is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1 μm or more.
[0221] When the conductor layer is a patterned conductor layer, the line (conductor layer width) / space (width between conductor layers) (L / S) of the patterned conductor layer is, from the viewpoint of fine wiring, preferably 5 μm / 5 μm or less (i.e., a pattern with a wiring pitch of 10 μm or less), more preferably 4 μm / 4 μm or less (a pattern with a wiring pitch of 8 μm or less), and even more preferably 3 μm / 3 μm or less (a pattern with a wiring pitch of 6 μm or less). The lower limit of the line / space ratio of the conductor layer is preferably 0.1 μm / 0.1 μm or more (a pattern with a wiring pitch of 0.2 μm or more), more preferably 0.5 μm / 0.5 μm or more (a pattern with a wiring pitch of 1 μm or more), and even more preferably 1 μm / 1 μm or more (a pattern with a wiring pitch of 2 μm or more). The wiring pitch does not need to be the same throughout the conductor layer.
[0222] When manufacturing a wiring board, steps (1) to (4) may be repeated as necessary to form a multilayer wiring board.
[0223] The wiring board obtained by the wiring board manufacturing method of the first embodiment is preferably formed in the order of a conductor circuit, an insulating material layer, a plasma mask, and a conductor layer, as shown in an example in FIG. 8 , and has via holes, and more preferably includes two or more of each of the conductor circuit, insulating material layer, plasma mask, conductor layer, and via hole.
[0224] In the first embodiment, for convenience of explanation, an embodiment having only the via hole 30 has been described with reference to FIGS. 4 to 8 . However, the first embodiment may have both the via hole 30 and the trench 31, or may have only the trench. Specifically, as shown in an example in FIG. 10 , plasma is irradiated from above the insulating material layer 11 through a plasma mask 21 to form either or both of the via hole 30 and the trench 31 in the insulating material layer 11 located at the opening 211 of the plasma mask 21. At the same time, the plasma mask 21 is etched to reduce the thickness of the plasma mask 21. As shown in an example in FIG. 11 , the plasma mask 21 is left on the insulating material layer 11 as a primer layer (permanent film). Then, as shown in an example in FIG. 12 , a plating seed layer 41 is formed on the reduced surface of the plasma mask 21 and on the surfaces of either or both of the via hole 30 and the trench 31. As shown in an example in FIG. 13 , plating is then performed on the plating seed layer 41. As shown in an example in FIG. 14, the unnecessary plating seed layer 41 is removed by etching such as flash etching to form the conductor layer 40.
[0225] A second embodiment of the method for manufacturing a wiring board of the present invention includes the steps of: (A) preparing a substrate having a conductor circuit and an insulating material layer formed on the conductor circuit from a cured product of a thermosetting material, and forming the first photosensitive material layer by either or both of applying and attaching a first photosensitive material to the surface of the insulating material layer; (B) exposing and developing the first photosensitive material layer to form a first plasma mask having openings; (C) irradiating the insulating material layer with plasma through the first plasma mask to form either or both of a via hole and a trench in the insulating material layer located at the openings in the plasma mask, and reducing the thickness of the plasma mask; (D) applying and either or both of applying and attaching a second photosensitive material to cover the surface and openings of the first plasma mask to form a second photosensitive material layer; (E) exposing and developing the second photosensitive material layer to form a second plasma mask having openings; (F) irradiating the first plasma mask and the insulating material layer with plasma through the second plasma mask to form either or both of a via hole and a trench in the insulating material layer; (G) forming a conductor layer on the surfaces of the first plasma mask and either or both of the via hole and the trench; and (H) scraping the surface of the conductor layer.
[0226] In the second embodiment, the first plasma mask is left intact, thereby preventing chemical damage to the insulating material layer caused by a stripping solution or the like used to remove the mask pattern. As a result, the insulating material layer has excellent insulating performance and electrical properties, and the insulating performance after the HAST test can be improved. In particular, since a cured product of a thermosetting material tends to have better insulating performance and electrical properties than a cured product of a photosensitive material, the combination of an insulating material layer formed of a cured product of a thermosetting material and a first plasma mask formed of a cured product of a photosensitive material can effectively improve the insulating performance and electrical properties. Furthermore, since the photosensitive material layer is formed on the insulating material layer, the alignment of the mask pattern is facilitated, making it possible to form small-diameter via holes or small-diameter trenches.
[0227] <Step (A)> Step (A) is the same as step (1) in the first embodiment. The first photosensitive material is the same as the photosensitive material in the first embodiment.
[0228] <Step (B)> In step (B), as shown in an example in Fig. 15 , the first photosensitive material layer 22 is irradiated with active energy rays, exposed, and developed to form a first plasma mask having openings 212. In detail, the surface of the first photosensitive material layer 22 is irradiated with active energy rays through a photomask not shown in Fig. 15 to cure the first photosensitive material layer 22.
[0229] The exposure and development methods for the first photosensitive material layer are the same as those in step (B) of the first embodiment, and the thickness of the first plasma mask is the same as that of the plasma mask in step (B) of the first embodiment.
[0230] When the thickness of the first plasma mask after the completion of step (B) is T1A (μm) and the thickness of the insulating material layer after the completion of step (B) is T2A (μm), it is preferable to satisfy the relationship T1A > T2A from the viewpoint of significantly obtaining the effects of the present invention.
[0231] 16 , in step (C), plasma is irradiated from above the insulating material layer 11 through the first plasma mask 24 to form either or both of a via hole (not shown) and a trench 31 in the insulating material layer 11 located at the opening 212 of the first plasma mask 24, and simultaneously, the first plasma mask 24 is etched to reduce the thickness of the first plasma mask 24. Step (C) can be performed in the same manner as step (3) of the first embodiment.
[0232] 17 , a second photosensitive material is applied and / or attached to the surface of the first plasma mask 24 and the openings 212 to form a second photosensitive material layer 23. The application and attachment of the second photosensitive material are the same as in step (1) in the first embodiment. The second photosensitive material may be the same as or different from the first photosensitive material.
[0233] <Step (E)> In step (E), as shown in an example in Fig. 18 , the second photosensitive material layer 23 is irradiated with active energy rays, exposed, and developed to form a second plasma mask 25 having openings 212 and a predetermined pattern. In detail, the surface of the second photosensitive material layer is irradiated with active energy rays through a photomask not shown in Fig. 18 to harden the second photosensitive material layer.
[0234] The exposure and development methods for the second photosensitive material layer are the same as those in step (B) of the first embodiment, and the thickness of the second plasma mask is the same as that of the plasma mask in step (B) of the first embodiment.
[0235] 19 , in step (F), plasma is irradiated onto the first plasma mask 24 and the insulating material layer 11 through the second plasma mask to form either a via hole (not shown) or a trench 31, or both, in the insulating material layer 11. In this step, etching of the first plasma mask 24 may be performed at the same time to further reduce the thickness of the first plasma mask 24. In step (F), the second plasma mask may be completely removed by plasma etching, or may remain.
[0236] The plasma treatment is the same as the plasma treatment in step (3) of the first embodiment.
[0237] Furthermore, from the viewpoint of significantly obtaining the effects of the present invention, the thickness of the first plasma mask after the completion of step (F) is preferably 0.01 or more, more preferably 0.05 or more, even more preferably 0.1 or more, or 0.15 or more, where the thickness of the plasma mask before plasma irradiation is taken as 1. It is preferably 0.7 or less, more preferably 0.6 or less, and even more preferably 0.5 or less. In conventional wiring board manufacturing methods, the mask is removed or peeled off after the via hole or trench is formed, so the thickness of the mask after plasma treatment is at most 0.05, where the thickness of the mask before plasma treatment is taken as 1.
[0238] The thickness of the first plasma mask after the step (F) is the same as or reduced from the thickness of the plasma mask after the step (3) of the first embodiment.
[0239] <Step (G)> In step (G), as shown in an example in FIG. 20 , a conductor layer 40 is formed on the surfaces of the first plasma mask 24 and either or both of the via hole and trench 31. The formation of the conductor layer is the same as the formation of the conductor layer in step (4) of the first embodiment. Performing step (G) may include a step (G-1) of forming a plating seed layer 41 on the surface of the first plasma mask 24 and either or both of the via hole (not shown) and trench 31. The plating seed layer is the same as the plating seed layer in step (4) of the first embodiment. Alternatively, a barrier metal layer may be formed instead of the plating seed layer.
[0240] After forming the plating seed layer, the method may further include a step (G-2) of performing electrolytic plating on the plating seed layer 41 and filling either or both of the via holes and trenches by electrolytic plating to form filled vias. In detail, an electrolytic plated layer 42 is formed by electrolytic plating on the exposed plating seed layer 41. For either or both of the via holes and trenches, an electrolytic plated layer 42 is formed on the exposed plating seed layer 41 by electrolytic plating, and either or both of the via holes and trenches are filled by electrolytic plating to form filled vias. The electrolytic plating is the same as the formation of the electrolytic plated layer in step (4) of the first embodiment.
[0241] <Step (H)> In step (H), the surface of the conductor layer is scraped, that is, the surface of the conductor layer 40 is polished so that the first plasma mask 24 is exposed, as shown in an example in FIG. 21 . As the polishing method, any method capable of polishing the surface of the conductor layer can be used. Examples of such polishing methods include CMP (chemical mechanical polishing), buff polishing, belt polishing, etc. Among these, CMP is preferred.
[0242] After the step (H), a barrier metal layer may be formed on the surface of the conductor layer, if necessary. In manufacturing a wiring board, the steps (A) to (H) may be repeated, if necessary, to form a multilayer wiring board.
[0243] The area of the wiring board is preferably 2500 mm 2 More preferably, 3000 mm 2 More preferably, 3500 mm 2 There is no particular upper limit, but it is 10,000 mm 2 It could be as follows:
[0244] The wiring board obtained by the manufacturing method of the present invention may be a multilayer wiring board having a plurality of laminated conductor layers, preferably three or more conductor layers.
[0245] [Semiconductor Device] The semiconductor device of the present invention includes a wiring board obtained by the manufacturing method of the present invention. Examples of the semiconductor device include various semiconductor devices used in electrical appliances (e.g., computers, mobile phones, digital cameras, televisions, etc.) and vehicles (e.g., motorcycles, automobiles, trains, ships, aircraft, etc.).
[0246] The semiconductor device of the present invention may have a fan-out structure or a chiplet structure. The semiconductor device of the present invention has a semiconductor chip on a wiring board obtained by the manufacturing method of the present invention, and the semiconductor chip is preferably a mixed system of at least a logic die and a memory die.
[0247] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the following examples. In the following description, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified. Furthermore, the operations described below were carried out in an environment of normal temperature and pressure, unless otherwise specified.
[0248] Inorganic fillers 1 and 2 are as follows: Inorganic filler 1: spherical silica (manufactured by Denka Co., Ltd., "UFP-30", average particle size 0.078 μm, specific surface area 30.7 m) 2 / g) surface-treated with N-phenyl-3-aminopropyltrimethoxysilane (KBM573, manufactured by Shin-Etsu Chemical Co., Ltd.). Inorganic filler 2: spherical silica ("SO-C2", manufactured by Admatechs Co., Ltd., average particle size: 0.5 μm, specific surface area: 5.8 m 2 / g) was surface-treated with N-phenyl-8-aminooctyltrimethoxysilane (KBM6803, manufactured by Shin-Etsu Chemical Co., Ltd.).
[0249] <Preparation of Thermosetting Material 1> A mixture of 6 parts of bixylenol-type epoxy resin ("YX4000HK" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: approximately 185 g / eq.), 5 parts of naphthalene-type epoxy resin ("ESN475V" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., epoxy equivalent weight: approximately 332 g / eq.), 15 parts of bisphenol AF-type epoxy resin ("YL7760" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: approximately 238 g / eq.), 15 parts of naphthylene ether-type epoxy resin ("HP6000L" manufactured by DIC Corporation, epoxy equivalent weight: approximately 100 g / eq.), and 10 parts of bisphenol AF-type epoxy resin ("YL7760" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: approximately 238 g / eq.). 2 parts of a cyclohexane-type epoxy resin ("ZX1658GS" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: approximately 135 g / eq.), 2 parts of a cyclohexane-type epoxy resin ("YX7800BH30" manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of cyclohexanone:methyl ethyl ketone (MEK) with a solids content of 30 mass%, Mw=20,000) were heated and dissolved with stirring in a mixed solvent of 20 parts of solvent naphtha and 10 parts of cyclohexanone. After cooling to room temperature, 20 parts of a prepolymer in which part or all of bisphenol A dicyanate had been triazinized to form a trimer ("BA230S" manufactured by Arxada, cyanate equivalent: 232 g / eq.) and 0.05 parts of an amine-based curing accelerator (4-dimethylaminopyridine (DMAP)) were mixed therein, and the mixture was uniformly dispersed using a high-speed rotary mixer. The mixture was then filtered through a cartridge filter ("SHP020" manufactured by ROKITECHNO) to prepare thermosetting material 1.
[0250] <Preparation of Thermosetting Material 2> A mixture of 6 parts of bixylenol-type epoxy resin ("YX4000HK" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: approximately 185 g / eq.), 5 parts of naphthalene-type epoxy resin ("ESN475V" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., epoxy equivalent weight: approximately 332 g / eq.), 15 parts of bisphenol AF-type epoxy resin ("YL7760" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: approximately 238 g / eq.), 15 parts of naphthylene ether-type epoxy resin ("HP6000L" manufactured by DIC Corporation, epoxy equivalent weight: approximately 100 g / eq.), and 10 parts of bisphenol AF-type epoxy resin ("YL7760" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: approximately 238 g / eq.). 2 parts of a cyclohexane-type epoxy resin ("ZX1658GS" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: approximately 135 g / eq.), and 2 parts of a phenoxy resin ("YL7500BH30" manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of cyclohexanone:methyl ethyl ketone (MEK) with a solids content of 30 mass%, Mw=44,000) were heated and dissolved with stirring in a mixed solvent of 20 parts solvent naphtha and 10 parts cyclohexanone. After cooling to room temperature, 4 parts of a triazine skeleton-containing cresol novolac curing agent ("LA-3018-50P" manufactured by DIC Corporation, hydroxyl group equivalent of approximately 151 g / eq., 2-methoxypropanol solution with a solids content of 50%), 6 parts of an active ester curing agent ("HP-B-8151-62T" manufactured by DIC Corporation, active group equivalent of 238 g / eq., toluene solution with a solids content of 62%), 30 parts of inorganic filler 1, and 0.05 parts of an amine curing accelerator (4-dimethylaminopyridine (DMAP)) were mixed therein and dispersed uniformly using a high-speed rotary mixer. The mixture was then filtered using a cartridge filter ("SHP020" manufactured by ROKITECHNO Corporation) to prepare thermosetting material 2.
[0251] <Preparation of Thermosetting Material 3> A mixture of 6 parts of bixylenol-type epoxy resin ("YX4000HK" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: approximately 185 g / eq.), 5 parts of naphthalene-type epoxy resin ("ESN475V" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., epoxy equivalent weight: approximately 332 g / eq.), 15 parts of bisphenol AF-type epoxy resin ("YL7760" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: approximately 238 g / eq.), 15 parts of naphthylene ether-type epoxy resin ("HP6000L" manufactured by DIC Corporation, epoxy equivalent weight: approximately 100 g / eq.), and 10 parts of bisphenol AF-type epoxy resin ("YL7760" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: approximately 238 g / eq.). Two parts of a cyclohexane-type epoxy resin ("ZX1658GS" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: approximately 135 g / eq.), and two parts of a phenoxy resin ("YL7500BH30" manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of cyclohexanone:methyl ethyl ketone (MEK) with a solids content of 30 mass%, Mw=44,000) were heated and dissolved with stirring in a mixed solvent of 20 parts solvent naphtha and 10 parts cyclohexanone. After cooling to room temperature, 4 parts of a triazine skeleton-containing cresol novolac curing agent ("LA-3018-50P" manufactured by DIC Corporation, hydroxyl group equivalent of approximately 151 g / eq., 2-methoxypropanol solution with a solids content of 50%), 6 parts of an active ester curing agent ("HP-B-8151-62T" manufactured by DIC Corporation, active group equivalent of 238 g / eq., toluene solution with a solids content of 62%), 60 parts of inorganic filler 1, and 0.05 parts of an amine curing accelerator (4-dimethylaminopyridine (DMAP)) were mixed therein and dispersed uniformly using a high-speed rotary mixer. The mixture was then filtered using a cartridge filter ("SHP020" manufactured by ROKITECHNO Corporation) to prepare thermosetting material 3.
[0252] <Preparation of Thermosetting Material 4> A mixture of 6 parts of bixylenol-type epoxy resin ("YX4000HK" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: approximately 185 g / eq.), 5 parts of naphthalene-type epoxy resin ("ESN475V" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., epoxy equivalent weight: approximately 332 g / eq.), 15 parts of bisphenol AF-type epoxy resin ("YL7760" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: approximately 238 g / eq.), 15 parts of naphthylene ether-type epoxy resin ("HP6000L" manufactured by DIC Corporation, epoxy equivalent weight: approximately 100 g / eq.), and 10 parts of bisphenol AF-type epoxy resin ("YL7760" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: approximately 238 g / eq.). Two parts of a cyclohexane-type epoxy resin ("ZX1658GS" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight: approximately 135 g / eq.), and two parts of a phenoxy resin ("YL7500BH30" manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of cyclohexanone:methyl ethyl ketone (MEK) with a solids content of 30 mass%, Mw=44,000) were heated and dissolved with stirring in a mixed solvent of 20 parts solvent naphtha and 10 parts cyclohexanone. After cooling to room temperature, 4 parts of a triazine skeleton-containing cresol novolac curing agent ("LA-3018-50P" manufactured by DIC Corporation, hydroxyl group equivalent of approximately 151 g / eq., 2-methoxypropanol solution with a solids content of 50%), 6 parts of an active ester curing agent ("HP-B-8151-62T" manufactured by DIC Corporation, active group equivalent of 238 g / eq., toluene solution with a solids content of 62%), solvent IP150 (manufactured by Idemitsu Kosan Co., Ltd.), 150 parts of inorganic filler 2, and 0.05 parts of an amine curing accelerator (4-dimethylaminopyridine (DMAP)) were mixed therein and dispersed uniformly using a high-speed rotary mixer. The mixture was then filtered using a cartridge filter ("SHP050" manufactured by ROKITECHNO Co., Ltd.) to prepare thermosetting material 4.
[0253] The components used in preparing Thermosetting Materials 1 to 4 and their amounts are shown in the table below. *In the table, the content of the curing agent represents the content of the curing agent when the resin component in the thermosetting material is taken as 100% by mass, and the contents of the cyanate ester resin, active ester resin, phenolic resin, and inorganic filler represent the content when the non-volatile component in the thermosetting material is taken as 100% by mass.
[0254] <Preparation of Thermosetting Resin Sheet 1> A PET film (Toray Industries, Inc., "Lumirror R80," 38 μm thick, softening point 130°C, "release PET") that had been release-treated with an alkyd resin-based release agent (Lintec Corporation, "AL-5") was prepared as a support. Thermosetting material 1 was uniformly applied to the release agent on the support using a die coater so that the thermosetting material layer would be 5 μm thick after drying, and the film was dried at 70°C to 95°C for 2 minutes to obtain a thermosetting material layer on the release PET. Next, a roughened surface of a polypropylene film (Oji F-Tex Co., Ltd., "Alphan MA-411," 15 μm thick) was laminated as a protective film on the side of the resin sheet not bonded to the support, so as to be bonded to the thermosetting material layer. This yielded a thermosetting resin sheet for forming an insulating material layer 1 consisting, in this order, of release PET (support), a thermosetting material layer, and a protective film.
[0255] <Preparation of Thermosetting Resin Sheet 2> In the preparation of the thermosetting resin sheet 1, the thermosetting material 1 was changed to the thermosetting material 2. Except for the above, the thermosetting resin sheet 2 was prepared in the same manner as the preparation of the thermosetting resin sheet 1.
[0256] <Preparation of Thermosetting Resin Sheet 3> In the preparation of the thermosetting resin sheet 1, the thermosetting material 1 was changed to the thermosetting material 3. Except for the above, the thermosetting resin sheet 3 was prepared in the same manner as the preparation of the thermosetting resin sheet 1.
[0257] <Preparation of Thermosetting Resin Sheet 4> In the preparation of the thermosetting resin sheet 1, the thermosetting material 1 was changed to the thermosetting material 4. Except for the above, the thermosetting resin sheet 4 was prepared in the same manner as the preparation of the thermosetting resin sheet 1.
[0258] <Preparation of Photosensitive Material 1> A negative photosensitive material 1 was obtained by mixing 10 parts by mass of an alkali-soluble resin ("TR4020G" manufactured by Asahi Organic Chemicals Co., Ltd.), 5 parts by mass of an alkali-soluble resin ("MEHC-7851SS" manufactured by Meiwa Chemical Industry Co., Ltd.), 5 parts by mass of an alkali-soluble resin ("BisE" manufactured by Honshu Chemical Co., Ltd.), 5 parts by mass of a compound containing at least two alkoxymethyl groups in the molecule ("MW-390" manufactured by Sanwa Chemical Co., Ltd.), 0.05 parts by mass of a photoacid generator ("MP-triazine" manufactured by Sanwa Chemical Co., Ltd.), 2 parts by mass of an organic filler ("MM-101SM" manufactured by Negami Chemical Industrial Co., Ltd.), and 12 parts by mass of MEK (manufactured by Junsei Chemical Co., Ltd.).
[0259] <Preparation of Photosensitive Material 2> (Synthesis of Polybenzoxazole Precursor Resin) 443.2 g (0.90 mol) of a dicarboxylic acid derivative obtained by reacting 1 mol of diphenylether-4,4'-dicarboxylic acid with 2 mol of 1-hydroxybenzotriazole and 366.3 g (1.00 mol) of hexafluoro-2,2-bis(3-amino-4-hydroxyphenyl)propane were placed in a four-neck separable flask equipped with a thermometer, a stirrer, a raw material inlet, and a dry nitrogen gas inlet tube, and 3,000 g of N-methyl-2-pyrrolidone was added and dissolved. The mixture was then reacted for 16 hours at 75°C using an oil bath.
[0260] Next, 32.8 g (0.20 mol) of 5-norbornene-2,3-dicarboxylic anhydride dissolved in 100 parts by mass of N-methyl-2-pyrrolidone was added, and the mixture was stirred for an additional 3 hours to complete the reaction. The reaction mixture was filtered, and then poured into a 3:1 water / isopropanol solution. The precipitate was collected by filtration, thoroughly washed with water, and then dried under vacuum to obtain the target polybenzoxazole precursor resin (A-1), which was a polybenzoxazole precursor resin in which general formula (5-4) and general formula (5-5) were randomly copolymerized and had a number average molecular weight of 12,000.
[0261] (Synthesis of Photosensitive Diazoquinone Compound) 12.74 g (0.030 mol) of a phenolic compound represented by the following formula (1) and 7.59 g (0.075 mol) of triethylamine were placed in a four-neck separable flask equipped with a thermometer, a stirrer, a raw material inlet, and a dry nitrogen gas inlet tube, and 103 g of acetone was added to dissolve the compound. After cooling the reaction solution to below 10°C, 20.15 g (0.075 mol) of 1,2-naphthoquinone-2-diazide-5-sulfonyl chloride was gradually added dropwise together with 100 g of acetone so that the temperature did not exceed 10°C. The reaction mixture was then stirred at below 10°C for 5 minutes, and then stirred at room temperature for 5 hours to terminate the reaction. The reaction mixture was filtered and then poured into a solution of water / methanol = 3 / 1 (volume ratio). The precipitate was collected by filtration, thoroughly washed with water, and then dried under vacuum to obtain a photosensitive diazoquinone compound represented by the following formula (2). In formula (2), Q represents a hydrogen atom or a group represented by formula (3), and 83% of all Qs are groups represented by formula (3). * in formula (3) represents a bond.
[0262] (Preparation of Photosensitive Material 2) 100 g of the synthesized polybenzoxazole precursor resin (A-1), 19 g of the photosensitive diazoquinone compound represented by formula (2), 4 g of the hindered phenolic antioxidant represented by formula (5), 10 g of the phenolic compound represented by formula (4), and 8 g of 3-methacryloxypropyltrimethoxysilane were dissolved in 200 g of γ-butyrolactone, and then filtered through a 0.2 μm Teflon (registered trademark) filter to obtain a positive-type photosensitive material 2.
[0263] <Preparation of Photosensitive Material 3> (Synthesis of Polymer A) 155.1 g of 4,4'-oxydiphthalic dianhydride (ODPA) was placed in a 2 L separable flask, 131.2 g of 2-hydroxyethyl methacrylate (HEMA) and 400 mL of γ-butyrolactone were added, and the mixture was stirred at room temperature. 81.5 g of pyridine was added with stirring to obtain a reaction mixture. After the heat generation due to the reaction had ceased, the mixture was allowed to cool to room temperature and left to stand for 16 hours.
[0264] Next, under ice cooling, a solution of 206.3 g of dicyclohexylcarbodiimide (DCC) dissolved in 180 mL of γ-butyrolactone was added to the reaction mixture over 40 minutes with stirring. Subsequently, a suspension of 45.1 g of 4,4'-diaminodiphenyl ether (DADPE) in 350 mL of γ-butyrolactone was added over 60 minutes with stirring. After further stirring at room temperature for 2 hours, 30 mL of ethyl alcohol was added and stirred for 1 hour, and then 400 mL of γ-butyrolactone was added. The precipitate that formed in the reaction mixture was removed by filtration to obtain a reaction solution.
[0265] The resulting reaction solution was added to 3 L of ethyl alcohol to produce a precipitate consisting of a crude polymer. The produced crude polymer was filtered off and dissolved in 1.5 L of γ-butyrolactone to obtain a crude polymer solution. The obtained crude polymer solution was added dropwise to 28 L of water to precipitate the polymer, and the resulting precipitate was filtered off and then vacuum dried to obtain a powdery polymer (Polymer A).
[0266] (Preparation of Photosensitive Material 3) 100 g of Polymer A was dissolved in a mixed solvent consisting of 80 g of N-methyl-2-pyrrolidone and 20 g of ethyl lactate together with 4 g of a photopolymerization initiator (1-[4-(Phenylthio)phenyl]-3-cyclopentylpropane-1,2-dione-2-(o-benzoyloxime)) and 4 g of tetraethylene glycol dimethacrylate. The viscosity of the resulting solution was adjusted to about 35 poise by further adding a small amount of the mixed solvent, and a negative-type Photosensitive Material 3 was obtained.
[0267] <Preparation of Photosensitive Material 4> (Synthesis of p-hydroxystyrene / styrene copolymer A1) A total of 100 parts by weight of p-t-butoxystyrene and styrene were prepared in a molar ratio of 85:15. These were dissolved in 150 parts by weight of propylene glycol monomethyl ether. Under a nitrogen atmosphere, the reaction temperature was maintained at 70°C, and polymerization was carried out using 4 parts by weight of azobisisobutyronitrile, with stirring at a rotation speed of approximately 160 rpm for 10 hours. Sulfuric acid was then added to the reaction solution, and the reaction temperature was maintained at 90°C for 10 hours to deprotect the p-t-butoxystyrene and convert it to hydroxystyrene. Ethyl acetate was added to the resulting copolymer, and the mixture was washed with water five times. The ethyl acetate phase was separated and the solvent was removed to obtain p-hydroxystyrene / styrene copolymer A1 (hereinafter, p-hydroxystyrene / styrene copolymer A1 may be referred to as "A1").
[0268] (Preparation of Photoacid Generator and Crosslinker) 1-naphthoquinone-2-diazide-5-sulfonic acid ester of 1,1-bis(4-hydroxyphenyl)-1-[4-{1-(4-hydroxyphenyl)-1-methylethyl}phenyl]ethane (esterification rate approximately 90%, manufactured by AZ Electronic Materials, "TPPA528") was prepared as a photoacid generator (hereinafter, this photoacid generator may be referred to as "B1"). Hexakis(methoxymethyl)melamine (manufactured by Sanwa Chemical Co., Ltd., "Nikarac MW-30HM") was prepared as a crosslinker (hereinafter, this crosslinker may be referred to as "C1").
[0269] (Synthesis of Acrylic Resin D1) 55 g of ethyl lactate was weighed into a 100 ml three-neck flask equipped with a stirrer, a nitrogen inlet tube, and a thermometer, and separately weighed polymerizable monomers (34.7 g of n-butyl acrylate (BA), 2.2 g of lauryl acrylate (LA), 3.9 g of acrylic acid (AA), 2.6 g of hydroxybutyl acrylate (HBA), and 1.7 g of 1,2,2,6,6-pentamethylpiperidin-4-yl methacrylate (manufactured by Resonac Corporation, "FA-711MM") and 0.29 g of azobisisobutyronitrile (AIBN) were added. While stirring at a rotation speed of 160 rpm, nitrogen gas was passed through at a flow rate of 400 ml / min for 30 minutes to remove dissolved oxygen. The nitrogen gas flow was then stopped, the flask was sealed, and the temperature was raised to 65°C in a thermostatic water bath in about 25 minutes. The same temperature was maintained for 10 hours to carry out a polymerization reaction, yielding acrylic resin D1 (hereinafter, acrylic resin D1 may be referred to as "D1"). The polymerization rate at this time was 99%. The weight-average molecular weight of this D1 was about 22,000. The molar ratio of the polymerizable monomers in D1 was as follows: BA / LA / AA / HBA / FA711MM = 75.5 / 2.5 / 15 / 5 / 2 (mol%).
[0270] (Preparation of Photosensitive Material 4) 80 parts of A1, 20 parts of B1, 5 parts of C1, 20 parts of D1, 120 parts of ethyl lactate as a solvent, and 2 parts of a 50% methanol solution of urea propyl triethoxysilane as a coupling agent were blended, and the mixture was pressure-filtered using a Teflon (registered trademark) filter with 3 μm pores to prepare Photosensitive Material 4.
[0271] (Preparation of Photosensitive Material 5) As the photosensitive material 5, an epoxy resin photosensitive material SU-8 3010 (manufactured by Nippon Kayaku Co., Ltd.) was used.
[0272] <Preparation of Photosensitive Resin Sheet A> A PET film ("Lumirror T60" manufactured by Toray Industries, Inc., thickness 38 μm) was prepared as a support. Photosensitive material 1 was uniformly applied to the PET film using a die coater so that the thickness of the photosensitive material layer after drying would be 10 μm, and the PET film was dried at 80° C. to 110° C. for 6 minutes to obtain a photosensitive resin sheet A having a photosensitive material layer on a release PET film.
[0273] [Example 1] <Preparation of Evaluation Substrate> (1) Preparation of Silicon Wafer A silicon wafer (copper foil thickness: 1 μm, substrate thickness: 0.8 mm, size: 8 inches) having a copper layer laminated on one side was prepared as a substrate, and was placed in an oven at 130° C. and dried for 30 minutes.
[0274] (2) Lamination of thermosetting resin sheet The protective film on the thermosetting resin sheet 1 was peeled off, and the thermosetting material layer was laminated onto one side of the wafer using a batch-type vacuum pressure laminator (Nikko Materials Co., Ltd., two-stage build-up laminator, CVP700) so that the thermosetting material layer was in contact with the silicon wafer. Lamination was performed by reducing the pressure to 13 hPa or less for 30 seconds, and then pressing at 130 ° C and a pressure of 0.74 MPa for 45 seconds. Next, a heat press was performed at 120 ° C and a pressure of 0.5 MPa for 75 seconds.
[0275] (3) Thermal curing of the thermosetting material layer The silicon wafer laminated with the thermosetting resin sheet 1 was placed in an oven at 100°C for 30 minutes, then transferred to an oven at 180°C for 30 minutes to thermally cure the thermosetting material layer, forming an insulating material layer, and the support was peeled off. This yielded a substrate A on which an insulating material layer with a thickness of 5 μm was formed.
[0276] (4) Lamination of Photosensitive Resin Sheet A Photosensitive resin sheet A was laminated on the insulating material layer of substrate A. Specifically, using a batch-type vacuum pressure laminator (Nikko Materials Co., Ltd., two-stage build-up laminator, CVP700), lamination was performed so that the substrate A and the photosensitive material layer of photosensitive resin sheet A were in contact. Lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing at 80 ° C and a pressure of 0.74 MPa for 45 seconds. Next, a heat press was performed at 80 ° C and a pressure of 0.5 MPa for 75 seconds.
[0277] (5) Patterning of the Photosensitive Material Layer After laminating the photosensitive resin sheet A, the substrate A was baked at 80°C for 30 seconds and exposed for 1800 msec using a UX-2240 manufactured by Ushio Inc. After exposure, the substrate A was baked at 75°C for 180 seconds and then developed using a 2.38% TMAH solution under puddle conditions of 30 seconds x 2 times. The developed pattern was subjected to descum treatment using a SAMCO plasma device (O 2 (Flow rate: 50 sccm, RF power: 500 W, process pressure: 12 Pa, processing time: 1 minute). Then, 5000 mJ / cm 2 The mask was post-baked at an exposure dose of 100°C for 30 minutes, then left for 30 minutes, and then heated at 190°C for 60 minutes, followed by cooling to 50°C over 30 minutes or more.
[0278] (6) Formation of via holes and plasma dry etching of plasma mask Plasma dry etching equipment (PlasmaPro100 manufactured by Oxford Instruments), CF 4 / O 2 The plasma mask obtained in (5) was subjected to plasma treatment using a mixture of 80:20 (sccm) of HCl and HCl, a degree of vacuum of 50 mTorr, an RF power of 120 W, and an ICP power of 100 W, to form via holes in the insulating material layer. This plasma treatment was carried out to such an extent that the plasma mask was not completely removed but remained on the insulating material layer.
[0279] (7) Measurement of arithmetic mean roughness (Ra) The arithmetic mean roughness (Ra) of the surface of the plasma mask after via hole formation was measured using a non-contact surface roughness meter (WYKO NT3300 manufactured by Veeco Instruments, Inc.) The measurement was performed in VSI mode with a 50x magnification lens and a measurement range of 121 μm × 92 μm.
[0280] (8) Measurement of wall roughness (Sa) of via holes After forming via holes in the insulating material layer, the mask pattern was polished to expose a cross section, and the wall roughness of the via holes was measured using a laser microscope (Keyence Corporation, "VK-X3000").
[0281] (9) Measurement of Via Taper Angle and Via Expansion Ratio The cross sections before and after the via hole formation were observed using a Hitachi High-Tech FIB-SEM (Ethos NX5000) to measure the via taper angle and via expansion ratio.
[0282] (10) Formation of Conductive Layer After via hole formation, the plasma mask surface was sputtered using a sputtering device (Canon Anelva's "E-400S") to form a 10 nm thick titanium layer, followed by a 100 nm thick copper layer. After annealing by heating at 150°C for 30 minutes, an etching resist was formed according to the semi-additive method, and a comb-shaped pattern with L / S = 1 / 1 μm (line width 1 mm) was formed by exposure and development. Then, copper sulfate electroplating was performed to form a 2 μm thick conductor layer. After forming the conductor pattern, the substrate was annealed by heating at 200°C for 60 minutes. The resulting substrate is referred to as "Substrate B."
[0283] <Evaluation of Fine Wiring (Appearance Evaluation)> The comb-tooth wiring of Substrate B was observed using a microscope (Keyence Corporation's "VHX-7000") and evaluated according to the following criteria. Here, "wire skip" means that the conductor layer was not formed in the intended position and the comb-tooth pattern of the conductor layer was interrupted midway. ◯: No wire skip was observed in the comb-tooth pattern. ×: Wire skip was observed in the comb-tooth pattern.
[0284] <Evaluation of Insulation Properties After HAST Test> The comb-tooth pattern of substrate B was embedded in a thermosetting material layer of thermosetting resin sheet 1 and cured. Specifically, the protective film of the thermosetting resin sheet was peeled off, and the thermosetting material layer was laminated to contact the conductor layer of substrate B using a batch-type vacuum pressure laminator (Nikko Materials Co., Ltd., two-stage build-up laminator, CVP700). Lamination was performed by reducing the pressure to 13 hPa or less for 30 seconds, and then pressing at 130 ° C and a pressure of 0.74 MPa for 45 seconds. Next, a heat press was performed at 120 ° C and a pressure of 0.5 MPa for 75 seconds. After lamination, substrate B was heated at 180 ° C for 90 minutes to cure the thermosetting material layer, and the electrode portion connected to the comb-tooth pattern was exposed. A voltage of 1.0 V was applied, and a test was performed at 130 ° C, 85 RH, %RH for 200 h. The insulation properties were confirmed according to the following criteria. ○: Resistance value is 10 6 Resistance exceeds 10Ω. 6 Ω or less.
[0285] <Measurement of bulk linear thermal expansion coefficient (bulk CTE)> The bulk linear thermal expansion coefficient was calculated using the following formula: Bulk linear thermal expansion coefficient = Linear thermal expansion coefficient of reduced plasma mask × (thickness of reduced plasma mask / thickness of reduced plasma mask + thickness of insulating material layer) + Linear thermal expansion coefficient of insulating material layer × (thickness of insulating material layer / thickness of reduced plasma mask + thickness of insulating material layer).
[0286] Example 2 In Example 1, the thermosetting resin sheet 1 was changed to the thermosetting resin sheet 2. Except for the above, a substrate A was produced in the same manner as in Example 1 and evaluated.
[0287] Example 3 In Example 1, the thermosetting resin sheet 1 was changed to the thermosetting resin sheet 3. Except for the above, a substrate A was produced in the same manner as in Example 1 and evaluated.
[0288] Example 4 In Example 1, the thermosetting resin sheet 1 was changed to the thermosetting resin sheet 4. Except for the above, a substrate A was produced in the same manner as in Example 1 and evaluated.
[0289] [Example 5] In Example 2, (4) Lamination of photosensitive resin sheet A was changed to the following (4-1) Formation of a coating film of photosensitive material 2, and (5) Patterning of the photosensitive material layer was changed to (5-1) Patterning of a coating film of photosensitive material 2. Except for the above, substrate A was produced in the same manner as in Example 2 and evaluated.
[0290] (4-1) Formation of a Coating Film of Photosensitive Material 2 Photosensitive material 2 was applied onto a silicon wafer using a spin coater, and then pre-baked on a hot plate at 120° C. for 4 minutes to obtain a coating film with a thickness of approximately 10 μm.
[0291] (5-1) Patterning of the coating film of the photosensitive material 2 The coating film was exposed to light at an exposure dose of 280 mJ / cm using an i-line stepper (Nikon Corporation "4425i"). 2 Next, puddle development was performed using a 2.38% aqueous solution of tetramethylammonium hydroxide, adjusting the development time so that the difference in film thickness in the unexposed area after pre-baking and after development was 1 μm. Thereafter, the film was rinsed with pure water for 10 seconds to form a pattern, thereby obtaining a plasma mask.
[0292] [Example 6] In Example 2, (4) Lamination of photosensitive resin sheet A was changed to the following (4-2) Formation of a coating film of photosensitive material 3, and (5) Patterning of the photosensitive material layer was changed to (5-2) Patterning of a coating film of photosensitive material 3. Except for the above, substrate A was produced in the same manner as in Example 2 and evaluated.
[0293] (4-2) Formation of a Coating Film of Photosensitive Material 3 Photosensitive material 3 was applied onto a silicon wafer using a spin coater and then dried to obtain a coating film with a thickness of 10 μm.
[0294] (5-2) Patterning of the coating film of the photosensitive material 3 The coating film was exposed to light at an exposure dose of 500 mJ / cm using a ghi stepper (Prisma-ghi, manufactured by Ultratech). 2The coating film was then spray-developed using cyclopentanone in a developing machine (D-SPIN636, manufactured by Dainippon Screen Mfg. Co., Ltd.). The unexposed areas were then rinsed with propylene glycol methyl ether acetate to develop and remove the unexposed areas, thereby forming a pattern in the coating film. The coating film pattern was cured in a temperature-programmable curing oven (VF-2000, manufactured by Koyo Lindberg Co., Ltd.) at 200°C for 2 hours under a nitrogen atmosphere, thereby obtaining a cured pattern (plasma mask) with a thickness of approximately 9 μm.
[0295] [Example 7] In Example 2, (4) Lamination of photosensitive resin sheet A was changed to (4-3) Formation of a coating film of photosensitive material 4 below, and (5) Patterning of the photosensitive material layer was changed to (5-3) Patterning of a coating film of photosensitive material 4. Except for the above, substrate A was produced in the same manner as in Example 2 and evaluated.
[0296] (4-3) Formation of a Coating Film of Photosensitive Material 4 Photosensitive material 4 was spin-coated onto a silicon wafer substrate and heated at 120° C. for 4 minutes to form a coating film with a thickness of 10 μm.
[0297] (5-3) Patterning of the coating film of the photosensitive material 4 The coating film was exposed to i-line (365 nm) using an i-line stepper (Canon, "FPA-3000iW"). The exposure dose was 460 mJ / cm. 2 After exposure, the pattern was developed using a 2.38% aqueous solution of tetramethylammonium hydroxide (TMAH). The pattern was then heat-treated in nitrogen at 200°C (heat-up time: 1.5 hours) for 2 hours using a vertical diffusion furnace (Koyo Thermo Systems Co., Ltd., "μ-TF") to obtain a plasma mask.
[0298] [Example 8] In Example 2, (4) Lamination of photosensitive resin sheet A was changed to (4-4) Formation of a coating film of photosensitive material 5, and (5) Patterning of the photosensitive material layer was changed to (5-4) Patterning of a coating film of photosensitive material 5. Except for the above, substrate A was produced in the same manner as in Example 2 and evaluated.
[0299] (4-4) Formation of a Coating Film of Photosensitive Material 5 Photosensitive material 5 was spin-coated onto a silicon wafer substrate and heated at 95° C. for 10 minutes to form a coating film with a thickness of 10 μm.
[0300] (5-4) Patterning of the coating film of the photosensitive material 5 The coating film was exposed to i-line (365 nm) using an i-line stepper (Canon, "FPA-3000iW"). The exposure dose was 200 mJ / cm. 2 After exposure, the pattern was baked at 95°C for 5 minutes. Next, it was developed using SU-8 Developer (manufactured by Nippon Kayaku Co., Ltd.). Thereafter, the pattern was heat-treated in nitrogen at a temperature of 200°C (heat-up time: 1.5 hours) for 2 hours using a vertical diffusion furnace (manufactured by Koyo Thermo Systems Co., Ltd., "μ-TF") to obtain a plasma mask.
[0301] Comparative Example 1 In Example 2, (3) thermal curing of the thermosetting material layer, (4) lamination of the photosensitive resin sheet A, and (5) patterning of the photosensitive material layer were changed to the following steps: A substrate B was produced and evaluated in the same manner as in Example 2 except for the above points.
[0302] After laminating the thermosetting resin sheet 2, the support was peeled off, and copper foil ("MT-EX" manufactured by Mitsui Mining & Smelting Co., Ltd.) was laminated onto the thermosetting material layer by reducing the pressure for 30 seconds to 13 hPa or less, pressing the foil at 130°C and a pressure of 0.74 MPa for 45 seconds, and then hot pressing the foil at 120°C and a pressure of 0.5 MPa for 75 seconds.
[0303] The silicon wafer laminated with copper foil was placed in an oven at 100° C. for 30 minutes, then transferred to an oven at 180° C. for 30 minutes, whereby the thermosetting material layer was thermally cured to form an insulating material layer.
[0304] After peeling off the copper foil carrier support, a photosensitive film ("RY5115" manufactured by Showa Denko Materials) was attached using a laminating device ("V-160" manufactured by Nikko Materials Co., Ltd.) and exposed to light at 125 mJ using a UX-2240 manufactured by Ushio Inc. The photosensitive film was developed using an EF-105A manufactured by Mitsubishi Gas Chemical Company, Inc. that had been diluted 5 times with pure water, to obtain a φ7 μm mask pattern.
[0305] This mask was then treated with an adjusted etching solution (JCU Corporation, "SACII-710W3C", approximately 1020 mL of Millipore water, CuSO 4 ・5H 2 O 36g, 75% concentration H 2 SO 4 80 mL, SACII 24 mL, 35% H 2 O 2 After dissolving the copper foil in 60 mL of a stripper (manufactured by Mitsubishi Gas Chemical Company, Inc., "R-100S"), 97 mL of a stripper (manufactured by Mitsubishi Gas Chemical Company, Inc., "R-101"), and 923 mL of Millipore water, the mask pattern was stripped off to obtain a Cu mask pattern with a diameter of 12 μm.
[0306] In Comparative Example 1, an attempt was made to form via holes and a conductor layer using a Cu mask pattern, but the surface was highly rough, making etching difficult to perform when forming a plating seed layer, and therefore it was not possible to form a conductor layer having a wiring pattern of L / S = 1 / 1 μm.
[0307] Comparative Example 2 In Example 2, (4) lamination of photosensitive resin sheet A, (5) patterning of photosensitive material layer, and (6) formation of via holes were changed to the following steps: A substrate B was produced and evaluated in the same manner as in Example 2 except for the above points.
[0308] After the thermosetting material layer of the thermosetting resin sheet 2 was cured, a photosensitive film ("RY5115" manufactured by Showa Denko Materials) was attached using a laminating device ("V-160" manufactured by Nikko Materials Co., Ltd.) and exposed to light at 125 mJ using a UX-2240 manufactured by Ushio Inc. The photosensitive film was developed using an EF-105A manufactured by Mitsubishi Gas Chemical Company, Inc. that had been diluted 5 times with pure water, to obtain a φ7 μm mask pattern.
[0309] Plasma dry etching equipment (PlasmaPro100 manufactured by Oxford Instruments), CF 4 / O 2A plasma treatment was performed on the mask pattern using a mixture of 80:20 (sccm), vacuum level: 50 mTorr, RF power: 120 W, and ICP power: 100 W, to form via holes in the insulating material layer. The mask pattern was then stripped using a stripper (Mitsubishi Gas Chemical Company, Inc., "R-100S"). It was confirmed that chemical damage had occurred in the areas of the insulating material layer that had come into contact with the stripper when the mask pattern was stripped.
[0310] Comparative Example 3 In Example 2, (4) lamination of photosensitive resin sheet A, (5) patterning of photosensitive material layer, and (6) formation of via holes were changed to the following steps: A substrate B was produced and evaluated in the same manner as in Example 2 except for the above points.
[0311] An opening was made from above the insulating material layer of the substrate A using a UV laser (LUK-2K21 (Viamechanics)), and a wet desmear treatment was carried out.
[0312] Thereafter, a plating seed layer was formed by electroless plating, and an attempt was made to form a conductor layer having a wiring pattern of L / S = 1 / 1 μm. However, since the arithmetic mean roughness (Ra) of the surface of the insulating material layer was high, the non-uniformity of the electroless plating resulted in poor wiring formation and the formation of a conductor layer was not possible.
[0313] Comparative Example 4 In Example 1, (2) laminating the thermosetting resin sheet, (3) thermal curing of the thermosetting material layer, (4) laminating the photosensitive resin sheet A, (5) patterning the photosensitive material layer, and (6) forming the via holes were changed to the following steps: A substrate B was produced and evaluated in the same manner as in Example 1 except for the above points.
[0314] The protective film of the photosensitive resin sheet A was peeled off, and the photosensitive material layer was laminated onto one side of the wafer using a batch-type vacuum pressure laminator (Nikko Materials Co., Ltd., two-stage build-up laminator, CVP700) so that the photosensitive material layer was in contact with the silicon wafer. Lamination was performed by reducing the pressure to 13 hPa or less for 30 seconds, and then pressing at 130 ° C and a pressure of 0.74 MPa for 45 seconds. Next, a heat press was performed at 120 ° C and a pressure of 0.5 MPa for 75 seconds.
[0315] After laminating the photosensitive resin sheet A, the substrate A was baked at 80°C for 30 seconds and exposed for 1800 msec using a UX-2240 manufactured by Ushio Inc. After the exposure, the substrate A was baked at 75°C for 180 seconds and then developed with a 2.38% TMAH solution under puddle conditions of 30 seconds x 2 times. The developed pattern was subjected to descum treatment using a plasma device manufactured by SAMCO Corporation (O 2 (Flow rate: 50 sccm, RF power: 500 W, process pressure: 12 Pa, processing time: 1 minute). Then, 5000 mJ / cm 2 Post-baking was carried out at the exposure dose, and finally post-curing was carried out to obtain an insulating material layer having via holes.
[0316] Comparative Example 5 In Comparative Example 1, the thermosetting resin sheet 2 was changed to the thermosetting resin sheet 1. Except for the above, the same procedures as in Comparative Example 1 were carried out to produce and evaluate a substrate B.
[0317] In Comparative Example 5, an attempt was made to form via holes and a conductor layer using a Cu mask pattern, but the surface roughness of the cured thermosetting material was high, making etching difficult to perform when forming a plating seed layer, and therefore a conductor layer having a wiring pattern of L / S = 1 / 1 μm could not be formed.
[0318] Comparative Example 6 In Comparative Example 2, the thermosetting resin sheet 2 was changed to the thermosetting resin sheet 1. Except for the above, a substrate B was produced and evaluated in the same manner as in Comparative Example 2.
[0319] Comparative Example 7 In Comparative Example 3, thermosetting resin sheet 2 was changed to thermosetting resin sheet 1. Except for the above, substrate B was produced and evaluated in the same manner as in Comparative Example 3. In Comparative Example 7, a plating seed layer was formed by electroless plating, and an attempt was made to form a conductor layer having a wiring pattern of L / S = 1 / 1 μm. However, since the arithmetic mean roughness (Ra) of the surface of the insulating material layer was high, the electroless plating was non-uniform, and wiring formation was poor, making it impossible to form a wiring.
[0320]
[0321] <Preparation of cured product samples> Photosensitive materials 1 to 5 were each coated onto release PET using a blade to a film thickness of 140 μm. The solution on the release PET was heated at 80°C for 20 minutes using a heater to form a photosensitive resin sheet having a photosensitive material layer. The photosensitive material layer was peeled from the release PET, and the photosensitive material layer was attached to a metal frame with heat-resistant tape. Curing was then carried out for an additional 120 minutes at 200°C (only the photosensitive resin sheet using photosensitive material 2 was cured at 230°C for 120 minutes) to prepare a cured product sample. For photosensitive material 1, 3000 mJ / cm 2 After exposure under the conditions of , an additional thermal cure was carried out.
[0322] Each of the thermosetting materials 1 to 4 was uniformly applied to a polyimide film using a die coater so that the thickness of the thermosetting material layer after drying was 20 μm, and the coating was dried for 2 minutes at 70 to 95° C. to prepare a resin sheet having a thermosetting material layer on a polyimide film. The resin sheet was then cured for 120 minutes at 200° C., after which the polyimide film was peeled off to obtain a cured product sample.
[0323] <Measurement of Glass Transition Temperature and Linear Thermal Expansion Coefficient> The cured product sample obtained above was cut into a length of 20 mm and a width of 6 mm to obtain a cured product for evaluation. A first TMA curve was obtained for this cured product for evaluation using a thermomechanical analyzer (TMA) manufactured by Rigaku Corporation, with the temperature rising from 25°C to 250°C at a temperature rise rate of 5°C / min using the tensile load method. Thereafter, the same measurement was performed on the same cured product for evaluation, with the temperature rising from 25°C to 250°C at a temperature rise rate of 5°C / min using the tensile load method to obtain a second TMA curve. The glass transition temperature Tg (°C) and linear thermal expansion coefficient (CTE: (ppm / °C)) were determined from the TMA curve obtained the second time.
[0324] <Measurement of dielectric loss tangent and dielectric constant> The cured product sample obtained above was cut into test pieces with an actual width of 2 mm and a length of 80 mm. Measurements were performed on three test pieces using an "HP8362B" manufactured by Agilent Technologies Inc. by the cavity resonance perturbation method at a measurement frequency of 5.8 GHz and a measurement temperature of 23°C, and the average values were calculated as the dielectric loss tangent and dielectric constant.
[0325] <Evaluation of Elastic Modulus and Elongation at Break> For the thermosetting material, a cured sample was cut into a No. 1 dumbbell shape to obtain a test piece. For the photosensitive material, a No. 1 dumbbell shape was obtained by exposure and development, and the photosensitive material layer was attached to a metal frame with heat-resistant tape. An additional 120 minutes of curing was carried out at 200°C (only the photosensitive resin sheet using Photosensitive Material 2 was cured at 230°C for 120 minutes) to prepare a test piece. For Photosensitive Material 1, 3000 mJ / cm 2 After exposure under the conditions of
[0045] , additional heat curing was carried out. The obtained test specimens were subjected to tensile strength measurement using an Orientec tensile testing machine "RTC-1250A", and the elastic modulus and elongation at break at 23°C were measured. The measurement was carried out in accordance with JIS K7127. The measurement was carried out 10 times (n=10), and the average value of the top three elongation points was calculated.
[0326]
[0327] REFERENCE SIGNS LIST 10 Substrate 11 Insulating material layer 12 Inner layer circuit board 20 Photosensitive material layer 21 Plasma mask (permanent film) 22 First photosensitive material layer 23 Second photosensitive material layer 24 First plasma mask (permanent film) 25 Second plasma mask 211 Opening 212 Opening 30 Via hole 31 Trench 40 Patterned conductor layer 41 Plating seed layer 42 Electrolytic plating layer
Claims
1. A method for manufacturing a wiring board, comprising the steps of: (1) preparing a substrate having a conductor circuit and, on the conductor circuit, an insulating material layer formed of a cured product of a thermosetting material, and forming a photosensitive material layer by either or both of applying and attaching a photosensitive material to the surface of the insulating material layer; (2) exposing and developing the photosensitive material layer to form a plasma mask having openings; (3) irradiating the insulating material layer with plasma through the plasma mask to form either or both of a via hole and a trench in the insulating material layer located at the openings of the plasma mask, and thinning the plasma mask; and (4) forming a conductor layer on the surfaces of the thinned plasma mask and either or both of the via hole and the trench.
2. The method for producing a wiring board according to claim 1, wherein step (4) comprises: (4-1) forming a plating seed layer on the surfaces of the reduced plasma mask and either or both of the via hole and the trench; and (4-2) plating the plating seed layer to form a conductor layer.
3. A method for manufacturing a wiring board as described in claim 1, wherein the conductor layer includes either or both of conductor wiring formed in positions other than the openings in the plasma mask and a conductor via layer formed in the openings in the plasma mask.
4. The method for producing a wiring board according to claim 2, wherein the plating seed layer is formed by a dry plating method.
5. The method for manufacturing a wiring board according to claim 1, wherein the opening diameter of the via hole or trench is 20 μm or less.
6. The method for producing a wiring board according to claim 1, wherein the thickness of the reduced plasma mask after step (3) is 0.1 μm or more and 20 μm or less.
7. The method for producing a wiring board according to claim 1, wherein the wiring pitch of the conductor circuits is 0.2 μm or more and 10 μm or less.
8. The method for producing a wiring board according to claim 1, wherein the arithmetic mean roughness (Ra) of the surface of the reduced plasma mask after step (3) is 100 nm or less.
9. The method for manufacturing a wiring board according to claim 1, wherein the wall surface roughness (Sa) of the via hole or trench is 400 nm or less.
10. The method for manufacturing a wiring board according to claim 1, wherein the ratio (Ra / Sa) of the arithmetic mean roughness (Ra) of the reduced plasma mask surface after step (3) and the roughness (Sa) of the wall surface of the via hole or trench is 3 or less.
11. The method for producing a wiring board according to claim 1, wherein the thickness of the photosensitive material layer is from 1 μm to 100 μm.
12. The method for producing a wiring board according to claim 1, wherein the thickness of the reduced plasma mask after step (3) is 0.7 or less, assuming that the thickness of the plasma mask before plasma exposure is 1.
13. The method for manufacturing a wiring board according to claim 1, wherein the absolute value of the difference between the linear thermal expansion coefficient of the cured photosensitive material and the linear thermal expansion coefficient of the cured insulating material in the range of 25°C to 150°C is 60 ppm / °C or less.
14. The method for manufacturing a wiring board according to claim 1, wherein when the thickness of the reduced plasma mask after step (2) is T1 and the thickness of the insulating material layer after step (2) is T2, the relationship T1 > T2 is satisfied.
15. The method for manufacturing a wiring board according to claim 1, wherein when the thickness of the reduced plasma mask after step (3) is T3 and the thickness of the insulating material layer after step (3) is T4, the relationship T3 < T4 is satisfied.
16. The method for manufacturing a wiring board according to claim 1, wherein the absolute value of the difference between the glass transition temperature of the photosensitive material contained in the plasma mask and the glass transition temperature of the thermosetting material is 100° C. or less.
17. The method for manufacturing a wiring board according to claim 1, wherein the via taper angle of the via hole or trench is 65 degrees or more and 90 degrees or less.
18. The method for manufacturing a wiring board according to claim 1, wherein the via expansion rate is 105% or more and 150% or less.
19. The method for producing a wiring board according to claim 1, wherein the relative dielectric constant of the cured product of the photosensitive material and the relative dielectric constant of the cured product of the thermosetting material are both 3.5 or less.
20. A method for manufacturing a wiring board as described in claim 1, wherein the breaking elongation of the cured product of the photosensitive material is 10% or more, and the breaking elongation of the cured product of the photosensitive material is greater than the breaking elongation of the cured product of the thermosetting material.
21. The method for producing a wiring board according to claim 1, wherein the etching rate in step (3) is 100 nm / min or more.
22. The method for producing a wiring board according to claim 1, wherein the line (conductor layer width) / space (width between conductor layers) (L / S) of the conductor layer is 5 μm / 5 μm or less.
23. The method for producing a wiring board according to claim 1, which is a multilayer wiring board substrate containing three or more conductor layers.
24. The area of the wiring board is 2500 mm 2 The method for producing a wiring board according to claim 1 .
25. The method for producing a wiring board according to claim 1, wherein the photosensitive material used in step (1) contains at least one type selected from a resin developable with a developer and an epoxy resin.
26. The method for producing a wiring board according to claim 25, wherein the resin developable with a developer contains at least one type selected from the group consisting of an alkali-soluble resin having a phenolic hydroxyl group in the molecule, a polyimide precursor, a polybenzoxazole precursor resin, and an acrylic resin.
27. A method for manufacturing a wiring board as described in claim 1, wherein the photosensitive material used in step (1) contains an inorganic filler, and the content of the inorganic filler in the photosensitive material is 10 mass % or less relative to 100 mass % of the non-volatile components of the photosensitive material.
28. A method for manufacturing a wiring board as described in claim 1, wherein the thermosetting material contains an inorganic filler, and the content of the inorganic filler in the thermosetting material is 20 mass % or more relative to 100 mass % of the non-volatile components of the thermosetting material.
29. The method for producing a wiring board according to claim 28, wherein the content of the inorganic filler is 35% by mass or more and 90% by mass or less, based on 100% by mass of the non-volatile components of the thermosetting material.
30. A method for manufacturing a wiring board as described in claim 1, wherein the photosensitive material used in step (1) contains an inorganic filler, the average particle size of the inorganic filler in the photosensitive material being 0.2 μm or less, and the thermosetting material contains an inorganic filler, the average particle size of the inorganic filler being 0.01 μm or more.
31. The method for producing a wiring board according to claim 1, wherein the bulk of the reduced plasma mask after step (3) and the insulating material layer has a linear thermal expansion coefficient of 100 ppm / °C or less in the range of 25°C to 150°C.
32. The method for producing a wiring board according to claim 1, wherein the photosensitive material used in step (1) is a solvent-developable negative photosensitive polyimide resin.
33. A method for manufacturing a wiring board as described in claim 1, wherein step (1) includes at least one of applying a liquid photosensitive material and attaching a photosensitive material layer of a photosensitive resin sheet including a support and a photosensitive material layer formed of a photosensitive material provided on the support.
34. The method for producing a wiring board according to claim 1, wherein the total thickness of the insulating material layer and the reduced plasma mask is 15 μm or less.
35. A method for manufacturing a wiring board according to claim 1, comprising the steps of attaching a thermosetting resin sheet including a support and a thermosetting material layer formed of a thermosetting material provided on the support to a conductor circuit, and curing the thermosetting material layer to form an insulating material layer.
36. (A) preparing a substrate having a conductor circuit and an insulating material layer formed on the conductor circuit from a cured product of a thermosetting material, and forming a first photosensitive material layer by either or both of applying and attaching a first photosensitive material to the surface of the insulating material layer; (B) exposing and developing the first photosensitive material layer to form a first plasma mask having an opening; (C) irradiating the insulating material layer with plasma through the first plasma mask to form either or both of a via hole and a trench in the insulating material layer located at the opening of the plasma mask, and reducing the thickness of the plasma mask; (D) applying and either or both of applying and attaching a second photosensitive material to cover the surface and opening of the first plasma mask to form a second photosensitive material layer; (E) exposing and developing the second photosensitive material layer to form a second plasma mask having an opening. (F) irradiating the first plasma mask and the insulating material layer with plasma through a second plasma mask to form either or both of a via hole and a trench in the insulating material layer; (G) forming a conductor layer on surfaces of the first plasma mask and either or both of the via hole and the trench; and (H) scraping the surface of the conductor layer.
37. A wiring board manufactured by the method for manufacturing a wiring board according to any one of claims 1 to 36.
38. The wiring board according to claim 37, which is formed in the following order: a conductor circuit, an insulating material layer, a plasma mask, and a conductor layer, and which has a via hole.
39. The wiring board of claim 38, comprising two or more of each of a conductor circuit, an insulating material layer, a plasma mask, a conductor layer, and a via hole.
40. A semiconductor device including a wiring board manufactured by the method for manufacturing a wiring board according to any one of claims 1 to 36.
41. The semiconductor device according to claim 40, having a fan-out structure.
42. The semiconductor device of claim 40 having a chiplet structure.
43. A semiconductor device having a semiconductor chip on a wiring board manufactured by the manufacturing method according to any one of claims 1 to 36.
44. The semiconductor device according to claim 40, wherein the semiconductor chip is a mixed system of at least a logic die and a memory die.
Citation Information
Patent Citations
Semiconductor device and manufacture thereof
JP1999274121A
Method for working insulating material and resist material used for worked insulating material by the method
JP2000054164A
Method for manufacturing printed wiring board
JP2022039763A