Fillet welding method, feeding control method, power supply, and fillet welding system
The fillet welding method addresses the robustness issues in feed control welding by alternating feed speeds and phase-based current control, enhancing penetration and bead width, and ensuring stable droplet transfer, thereby improving the quality of fillet welds despite misalignment and gaps.
Patent Information
- Application Number
- PCT/JP2024/005287
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-02-15
- Publication Date
- 2024-10-03
AI Technical Summary
Fillet welding methods, particularly feed control welding, face challenges with robustness due to misalignment and gaps between steel plates, leading to poor crosslinking properties and defective bead shapes, as conventional methods like MAG and pulsed MAG welding are insufficient in addressing these issues.
A fillet welding method that alternates feed speed between forward and reverse feed periods, with specific phase-based welding current settings to enhance penetration and bead width, and a power supply system that controls welding current according to wire position phases to maintain robustness.
The method achieves excellent robustness in fillet welding by optimizing penetration and bead width, reducing burn-through and spatter, and ensuring stable droplet transfer, even with significant deviations or gaps in the welding target position.
Smart Images

Figure JP2024005287_03102024_PF_FP_ABST
Abstract
Description
Fillet welding method, feed control method, power source, and fillet welding system
[0001] The present invention relates to a fillet welding method, a feed control method, a power source, and a fillet welding system.
[0002] Fillet welding is a construction method used in gas-shielded arc welding, and is applied in a variety of industries, including when overlapping thin steel plates (hereinafter also referred to as "lap fillet welding") and when welding steel plates orthogonally in a T-shape. In fillet welding, the welding target position can shift or gaps can occur between the steel plates due to factors such as the accuracy of the steel plate fixation, the accuracy of the steel plate workability, the accuracy of assembly, and distortion during welding. These target position shifts and the presence of gaps have traditionally led to problems such as poor bridging due to burn-through into the gap and poor bead shape.
[0003] In order to solve the above problems, for example, Patent Document 1 discloses a wire for MAG welding of thin steel plates containing, by mass%, C: 0.04 to 0.15%, Si: 0.75 to 1.00%, Mn: 1.00 to 2.00%, Cr: 0.35 to 0.80%, with the balance being Fe and unavoidable impurities.
[0004] Furthermore, Patent Document 2 discloses a gas-shielded arc welding method for thin steel plate having a plate thickness of 0.5 to 1.2 mm, using a wire having a wire diameter of 0.5 to 0.9 mm and containing, by mass, C: 0.02 to 0.10%, Si: 0.7 to 2.0%, Mn: 0.5 to 3.0%, P≦0.020%, S: 0.005 to 0.020%, with the balance being Fe and unavoidable impurities, and applying pulses with a peak current (Ip): 300 to 450 A and a base current (Ib): 20 to 100 A, wherein the relationship between the peak current (Ip) and the peak time (Tp) satisfies a predetermined formula (1).
[0005] Japanese Patent Publication No. 2012-170970 Japanese Patent Publication No. 2001-321946
[0006] As disclosed in Patent Documents 1 and 2, conventionally, MAG welding and pulse MAG welding have been used to widen the weld bead width. However, feed control welding, which has been increasingly adopted in recent years due to its advantages in welding workability, such as reduced spatter, has not yet solved the above problem. Feed control welding is a welding technique in which the welding wire feed speed is alternately switched between forward and reverse feed periods. Generally, feed control welding is based on a short-circuit transition that generates a short-circuit period and an arc period. Therefore, it is suitable for low-heat input welding. However, when the welding target position is misaligned or a gap occurs between the steel sheets, the penetration is shallow and the bead width does not increase, making it prone to poor bead shape and burn-through into the gap. In particular, the larger the misalignment of the welding target position or the gap, the more pronounced the problems of poor bead shape and bridging, and the less robust the welding is. Therefore, feed control welding, which has excellent welding workability, is desired to have robustness equal to or greater than that of conventional MAG welding and pulse MAG welding.
[0007] Therefore, an object of the present invention is to provide a fillet welding method, a feed control method, a power source, and a fillet welding system that can achieve excellent robustness even when a feed control welding method is applied to fillet welding.
[0008] The present invention has the following configuration: (1) A fillet welding method employing a feed control method for alternately switching a feed speed between a forward feed period and a reverse feed period, wherein, in the feed control method, when a wire position phase is set to 0° based on the position of the welding wire at the time of switching from the reverse feed period to the forward feed period, a period T in which the wire position phase is 90° to 180° is 90~180deg The average value of the welding current at 90~180deg_ave The set welding current value I set and during a period T when the wire position phase is between 180 degrees and 270 degrees. 180~270deg The average value of the welding current at 180~270deg_ave The set welding current value I set A fillet welding method characterized in that the welding distance is made smaller than
[0009] (2) A feed control method applied to a fillet welding method, which alternately switches the feed speed between a forward feed period and a reverse feed period, wherein, when a wire position phase based on the position of the welding wire at the time of switching from the reverse feed period to the forward feed period is set to 0°, a period T in which the wire position phase is 90° to 180° is 90~180deg The average value of the welding current at 90~180deg_ave The set welding current value I set and during a period T when the wire position phase is between 180 degrees and 270 degrees. 180~270deg The average value of the welding current at 180~270deg_ave The set welding current value I set The feed control method is characterized in that
[0010] (3) A power supply that is applied to a fillet welding method and has a function of performing feed control to alternately switch the feed speed between a forward feed period and a reverse feed period, wherein in the feed control method, when a wire position phase based on the position of the welding wire at the time of switching from the reverse feed period to the forward feed period is set to 0°, a period T in which the wire position phase is 90° to 180° is 90~180deg The average value of the welding current at 90~180deg_ave The set welding current value I set and during a period T when the wire position phase is between 180 degrees and 270 degrees. 180~270deg The average value of the welding current at 180~270deg_ave The set welding current value I set The power supply is characterized in that it is smaller than
[0011] (4) A fillet welding system employing a feed control method for alternately switching a feed speed between a forward feed period and a reverse feed period, wherein, in the feed control method, when a wire position phase based on the position of the welding wire at the time of switching from the reverse feed period to the forward feed period is set to 0°, a period T in which the wire position phase is 90° to 180° is 90~180deg The average value of the welding current at 90~180deg_ave The set welding current value I set and during a period T when the wire position phase is between 180 degrees and 270 degrees.180~270deg The average value of the welding current at 180~270deg_ave The set welding current value I set A fillet welding system characterized in that the welding distance is smaller than
[0012] According to the present invention, excellent robustness can be achieved even when a feed control welding method is applied to fillet welding.
[0013] FIG. 1 is a schematic diagram showing an example of the configuration of a welding system according to this embodiment. FIG. 2 is a block diagram showing a schematic configuration related to the control of a welding power source, a welding control device, and a servo amplifier according to this embodiment. FIG. 3 is a graph showing an example of the relationship between the wire feed speed, the wire tip position, and the current detection signal according to this embodiment. FIG. 4 is a diagram showing the compositions of two wires used in the examples. FIG. 5 is a diagram showing two welding methods used in the examples. FIG. 6 is a graph showing the welding current and feed speed when feed control method A is used as the welding method. FIG. 7 is a graph showing the welding current and feed speed when feed control method B is used as the welding method. FIG. 8 is a diagram showing the welding conditions and measured data when feed control method A, feed control method B, and pulsed MAG welding as a comparative example are used, respectively. FIG. 9A is a diagram showing the results of a target deviation test based on the welding conditions and measured data for Test No. 1. FIG. 9B is a diagram showing the results of a target deviation test based on the welding conditions and measured data for Test No. 2. FIG. 9C is a diagram showing the results of a target deviation test based on the welding conditions and measured data for Test No. 3. Fig. 9D is a diagram showing the results of the off-target test based on the welding conditions and actual measurement data for Test No. 3. Fig. 9E is a diagram showing the results of the off-target test based on the welding conditions and actual measurement data for Test No. 5.
[0014] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, embodiments of a fillet welding method, a feed control method, a power source, and a fillet welding system according to the present invention will be described in detail with reference to the accompanying drawings.
[0015] Hereinafter, embodiments of a gas-shielded arc welding method, control method, power supply, and welding system according to the present invention will be described in detail with reference to the drawings. Note that this embodiment is an example of a case where a welding robot is used, and the welding control method according to the present invention is not limited to the configuration of this embodiment. For example, an automatic welding device using a cart instead of a welding robot body may be applied, or a portable small welding robot may be applied.
[0016] The feed control method may be a type that alternates between a forward feed period and a reverse feed period, and performs welding based on a short-circuit transition mode that generates a short-circuit period and an arc period (hereinafter also referred to as a "short-circuit type feed control method"), or a type that alternates between a forward feed period and a reverse feed period, and performs welding based on a globule transition mode that suppresses the occurrence of a short-circuit period (hereinafter also referred to as a "short-circuit suppression type feed control method"). Although the welding method of the present invention is not particularly limited, the system configuration of the short-circuit suppression type feed control method will be described as an example in this embodiment. Furthermore, in this embodiment, lap fillet welding will be described as an example of fillet welding.
[0017] 1 is a schematic diagram showing an example of the configuration of a welding system according to this embodiment. The welding system 50 includes a welding robot 110, a welding control device 120, a welding power source 140, a controller 150, a push motor 180 that feeds welding wire 100, a servo motor 170, a servo amplifier 160 that controls the servo motor 170, and a wire buffer 190. The push motor 180 feeds welding wire 100.
[0018] Welding power source 140 is connected to welding robot 110 via a positive power cable (not shown) so as to be able to energize welding wire 100, which is a consumable electrode, and is connected to workpiece (hereinafter also referred to as "base material") 200 via a negative power cable (not shown). This connection is for the case where welding is performed with reverse polarity; when welding with positive polarity is performed, the polarity of welding power source 140 can be reversed.
[0019] Furthermore, the welding power source 140 and the push motor 180 for feeding the welding wire 100 are connected by a signal line, and the feed speed of the welding wire can be controlled. In the feed control of this embodiment, the push motor 180 rotates only in the forward direction, and the servo motor 170, which will be described later, is switched between the forward and reverse directions.
[0020] The welding robot 110 is equipped with a welding torch 111 as an end effector. The welding torch 111 has a current-carrying mechanism, i.e., a welding tip, that applies current to the welding wire 100. When current is applied from the welding tip, the welding wire 100 generates an arc from its tip, and the generated heat welds the workpiece 200, which is the welding target. The welding tip is also generally referred to as a contact tip.
[0021] The welding torch 111 includes a shielding gas nozzle that ejects the shielding gas. While the shielding gas is not particularly limited, a gas composition that exhibits globular transition is preferable due to the characteristics of the control used in this embodiment. Specifically, it is preferable for the gas to contain at least one gas with a high potential gradient: carbon dioxide, nitrogen, hydrogen, or oxygen. From the perspective of versatility, in the case of a mixed gas with argon gas (hereinafter also referred to as "Ar gas"), a system containing at least 10% by volume of carbon dioxide is more preferable, a system containing 90% by volume or more of carbon dioxide is even more preferable, and carbon dioxide alone is even more preferable. The shielding gas is supplied from a shielding gas supply device (not shown).
[0022] Servo motor 170 is provided near welding torch 111. Servo amplifier 160 connected to servo motor 170 controls servo motor 170. In this embodiment, welding torch 111 is configured independent of servo motor 170, but a configuration in which servo motor 170 is provided inside welding torch 111 (also referred to as a servo torch) is also possible. Servo motor 170 switches between forward and reverse rotation directions based on a forward / reverse feed command to control feed. In addition, servo amplifier 160 enables high-speed calculation processing and has forward / reverse feed command generation unit 161, which will be described in detail later.
[0023] A wire buffer 190 is disposed between the push motor 180 and the servo motor 170. Because the push motor 180 only rotates forward and the servo motor 170 feeds in both forward and reverse directions, the feed directions of the push motor 180 and the servo motor 170 may differ, creating a situation in which a large load is likely to be placed on the wire within the feed path. To enable appropriate feed control even in such a feed system situation, a wire buffer is provided to suppress buckling of the wire.
[0024] The welding wire 100 used in this embodiment is not particularly limited. For example, either a solid wire containing no flux or a flux-cored wire containing flux may be used. The material of the welding wire 100 is also not limited. For example, the material may be mild steel, stainless steel, aluminum, or titanium, and the wire surface may be plated with Cu or the like. The diameter of the welding wire 100 is also not particularly limited. In this embodiment, the upper limit of the diameter is preferably 1.6 mm and the lower limit is preferably 0.8 mm. As such, the type and composition of the welding wire are not limited, but a wire composition that is particularly suitable for the welding method according to this embodiment will be described later.
[0025] In this embodiment, the specific configuration of workpiece 200 is not particularly important, and welding conditions such as joint shape, welding posture, and groove shape are also not particularly important. Welding control device 120 mainly controls the operation of welding robot 110. Therefore, welding control device 120 may also be referred to as a robot controller. Welding control device 120 holds teaching data that predefines the operation pattern, welding start position, welding end position, welding conditions, weaving operation, etc. of welding robot 110, and instructs welding robot 110 on these to control the operation of welding robot 110. Furthermore, welding control device 120 provides welding conditions such as welding current, welding voltage, and feed speed to welding power source 140 during welding operation in accordance with the teaching data.
[0026] As shown in FIG. 1, welding system 50 of this embodiment is configured such that welding control device 120 is independent from welding power source 140, but welding control device 120 may also be provided within welding power source 140.
[0027] Controller 150 is connected to welding control device 120, and creates or displays programs for operating welding robot 110, inputs teaching data, etc. Information input by the user to controller 150 is provided to welding control device 120. Controller 150 may also have a function for manually operating welding robot 110. Note that the connection between controller 150 and welding control device 120 may be wired or wireless.
[0028] In response to a command from welding control device 120, welding power source 140 supplies power to welding wire 100 and workpiece 200, thereby generating an arc between welding wire 100 and workpiece 200. In response to a command from welding control device 120, welding power source 140 outputs a control signal for push motor 180.
[0029] Next, the functional configuration of welding system 50 according to this embodiment will be described in detail with reference to Figures 2 and 3. Figure 2 is a block diagram showing a schematic configuration relating to the control of welding power source 140, welding control device 120, and servo amplifier 160 in this embodiment. Figure 3 is a graph illustrating an example of the relationship between the wire feed speed, wire tip position, and current detection signal in this embodiment.
[0030] Welding power source 140 is connected to welding control device 120 via digital communication, and welding control device 120 is connected to servo amplifier 160 via digital communication. That is, servo amplifier 160, welding control device 120, and welding power source 140 are digitally connected in a line configuration in this order. This can be interpreted as a state in which servo amplifier 160 and welding power source 140 are indirectly connected via digital communication. Note that servo amplifier 160, welding power source 140, and welding control device 120 may also be connected in a line configuration in this order. This can be interpreted as a state in which servo amplifier 160 and welding power source 140 are directly connected via digital communication.
[0031] In this embodiment, communication between welding power source 140 and welding control device 120 is performed via CAN (Controller Area Network), which is an industrial field network, and communication between welding control device 120 and servo amplifier 160 is performed via EtherCAT (Ethernet for Control Automation Technology) (registered trademark), which is also an industrial field network, but the communication network is not limited to these.
[0032] (Functional Configuration of the Welding Power Source) The control system 141 of the welding power source 140 is executed, for example, by the welding control device 120 or a computer (not shown) executing a program. The control system 141 of the welding power source 140 includes a current setting unit 36. In this embodiment, the current setting unit 36 has a function of setting various current values that define the welding current flowing through the welding wire 100 in accordance with processes such as arc start and welding determined by the welding sequence unit, and a function of setting the start and end times of each current control period. The current setting unit 36 has a target current setting unit 36A, a wire tip position conversion unit 36B, and a voltage setting unit 36C. The target current setting unit 36A has a function of setting the start and end times of each of the peak period Dap, fall period Ddwn, base period Db, and rise period Dup related to the current control. The wire tip position conversion unit 36B has a function of obtaining information on the tip position of the welding wire 100.
[0033] The various condition settings may be determined based on, for example, setting values input in advance by an operator, a waveform control table prepared in advance, a database of welding conditions, etc. The setting values, table, database, etc. may be stored in any of the components of welding system 50. The setting values, table, database, etc. may be stored in welding control device 120, welding power source 140, etc.
[0034] The various condition settings for the peak period Dp, fall period Ddwn, base period Db, and rise period Dup related to the current non-suppression period TIP (in this embodiment, the sum of the Dup and Dp periods) and the current suppression period TIB (in this embodiment, the sum of the Ddwn and Db periods) may be determined by the waveform control table linear calculation unit 37 based on a waveform control table prepared in advance. In this embodiment, the various condition settings refer to the setting of conditions such as current value, time, or phase.
[0035] In the case of the short-circuit suppression type feed control method applied in this embodiment shown in FIG. 3 , the welding current exhibits a pulse waveform that alternates between a current non-suppression period TIP and a current suppression period TIB based on the phase related to the wire tip position (hereinafter also referred to as the “wire position phase”). In this embodiment, the timing of the peak period Dap, the fall period Ddwn, the base period Db, and the rise period Dup are controlled based on the wire position phase of 0 to 360 degrees (0 to 2π), where 0 degrees is when the wire tip position is closest to the tip side and 180 degrees is when the wire tip position is closest to the base metal side. At least the welding current may be switched between a current suppression period TIB and a current non-suppression period TIP according to the feed speed phase, which will be described later.
[0036] Based on the set value of the average feed rate Favg in the welding condition information stored by the control system unit 141, the set current value Ip (hereinafter also referred to as the "peak current Ip") for the peak period Dap in the current non-suppression period TIP calculated by the waveform control table linear calculation unit 37 and the set current value Ib (hereinafter also referred to as the "base current Ib") for the base period Db in the current suppression period TIB are set in the current setting unit 36.
[0037] In the short-circuit suppression type feed control method of this embodiment, the welding current is basically controlled by two values: peak current Ip and base current Ib. Therefore, the start time of base period Db represents the time when base current Ib starts, i.e., base current start time. Furthermore, the end time of base period Db represents the time when base current Ib ends, i.e., base current end time. The start time of base period Db, the end time of base period Db, the duration (time) of fall period Ddwn, and the duration (time) of rise period Dup are calculated by waveform control table linear calculation unit 37. The start time of peak period Dap may be expressed as peak current start time, and the end time of peak period Dap may be expressed as peak current end time. As shown in FIG. 3 , the timing of the peak current end time is preferably determined by a set period d1 when the wire position phase is set to 0°, and the timing of the peak current start time is preferably determined by a set period d2 when the peak current end time is set. This setting period may be set by phase. For example, if d1 is set to 190° and d2 is set to 120°, the peak current ends when the wire position phase is 190° (d1) and starts when the wire position phase is 310° (d1 + d2).
[0038] Furthermore, the wire tip position converter 36B determines the wire tip position based on the phase synchronization signal and the phase delay correction amount signal from the servo amplifier 160. In this embodiment, the wire tip position may be expressed using an angle of 0 to 2π as the wire position phase, as described above, and the forward feed start position is defined as 0 as shown in FIG.
[0039] The phase delay correction amount signal is output from phase delay correction unit 38. Phase delay correction unit 38 has a database in which the error between the actual forward / reverse feed operation of servo motor 170 and the forward / reverse feed command of servo amplifier 160 is calculated in advance as a phase delay correction amount for each of various welding conditions. For example, if the various welding conditions are a wire forward / reverse frequency Tf, which is a frequency when the forward feed period and the reverse feed period are defined as one cycle, the phase delay correction amount is determined based on the database in accordance with the value of the wire forward / reverse frequency to be used, and is output from phase delay correction unit 38 as a phase delay correction amount signal.
[0040] The main power supply circuit of the welding power supply 140 is composed of a three-phase AC power supply (hereinafter also referred to as the “AC power supply”) 1, a primary side rectifier 2, a smoothing capacitor 3, a switching element 4, a transformer 5, a secondary side rectifier 6, and a reactor 7.
[0041] AC power input from AC power supply 1 is full-wave rectified by primary-side rectifier 2 and further smoothed by smoothing capacitor 3 to be converted into DC power. Next, the DC power is converted into high-frequency AC power by inverter control using switching element 4, and then converted into secondary-side power via transformer 5. The AC output of transformer 5 is full-wave rectified by secondary-side rectifier 6 and further smoothed by reactor 7. The output current of reactor 7 is provided to the welding tip as an output from the main power supply circuit, and is passed through welding wire 100, which serves as a consumable electrode.
[0042] The welding wire 100 is fed by the push motor 180 and the servo motor 170, generating an arc between the welding wire 100 and the base material 200. A forward feed period during which the tip of the welding wire 100 moves toward the base material 200 is referred to as a forward feed period TP. A reverse feed period during which the tip of the welding wire 100 moves in a direction opposite to the direction in which the base material 200 is located is referred to as a reverse feed period TN. In this embodiment, the servo motor 170 periodically feeds the welding wire 100, with the forward feed period TP and the reverse feed period TN combined forming one cycle. Note that the "tip of the welding wire" here generally refers to the tip of the wire when ignoring the presence of droplets hanging from the wire tip. In other words, the wire melted by the arc is considered to have immediately transferred to the base material.
[0043] The feeding of the welding wire 100 by the push motor 180 is controlled by a control signal from the push feeder control unit 39. The average value of the feeding speed is approximately the same as the melting speed. In this embodiment, the feeding of the welding wire 100 by the push motor 180 is also controlled by the welding power source 140.
[0044] The push feeder control unit 39 also performs control according to the state of the wire buffer 190. In this embodiment, the wire buffer 190 is provided with a wire slack portion (a gap into which the wire can escape if it becomes loose due to the influence of feeding between the motors) so that a large load is not applied to the wire in the feeding path between the push motor 180 and the servo motor 170, and an absolute encoder built into the wire buffer 190 detects the amount of wire slack in terms of a rotation angle. The detected value is converted into an analog signal by a serial-to-analog converter 191, and an electrical angle calculation unit calculates the electrical angle. The calculated electrical angle is input to an A / D input unit 40 of the welding power source.
[0045] A differential signal obtained by calculating the difference between the electrical angle from the A / D input unit 40 and a reference value of the electrical angle preset in the electrical angle adjustment unit 41 is input to the push feeder control unit 39. Based on this differential signal, the push feeder control unit 39 controls the push motor 180 to buffer an appropriate amount of wire, thereby performing interference control to prevent a large load from being placed on the feeding system. Note that, although the interference control described above is performed in this embodiment, it is not limited to this. Furthermore, although an absolute encoder built into the wire buffer 190 is used in this embodiment, it is not limited to this. For example, a rotation angle sensor may be used, in which case the serial-to-analog conversion unit 191 may not be provided.
[0046] A voltage setting signal Vap, which is a target value of the voltage to be applied between the base material 200 and the contact tip (not shown) and the current-carrying position of the welding wire 100, is given as a voltage command to the voltage setting unit 36C of the current setting unit 36. Based on the voltage setting signal Vap, the current setting unit 36 controls the welding current in each period, such as the peak period Dap, so that the length of the arc (hereinafter also referred to as "arc length") is constant.
[0047] The voltage detection signal Vo obtained by the voltage detection unit is an actual measurement value. In this embodiment, the voltage detection signal Vo passes through a low-pass filter LPF, passes through a separation detection unit 33, and is input to the current setting unit 36 as a separation detection signal DTR. Note that a voltage comparison unit may be provided to amplify the difference between the voltage setting signal Vap and the voltage detection signal Vo and output it to the current setting unit 36 as a voltage error amplified signal.
[0048] The current error amplifier 34 amplifies the difference between the current setting signal CCset given as a target value by the current setting unit 36 and the current detection signal Io detected by the current detection unit 31, and outputs the amplified current error signal Ed to the inverter drive unit 30. The inverter drive unit 30 corrects the drive signal Ec to the switching element 4 using the amplified current error signal Ed.
[0049] A detachment detection signal DTR, which is a signal for detecting detachment of a droplet from the tip of the welding wire 100, is also input to the current setting unit 36. The detachment detection signal DTR is output from the detachment detection unit 33. The detachment detection unit 33 monitors a change in the voltage detection signal Vo output by the voltage detection unit 32, and detects detachment of a droplet from the welding wire 100 from the change. Note that the detachment detection unit 33 is an example of a detection means.
[0050] The detachment detection unit 33 detects droplet detachment by, for example, comparing a value obtained by differentiating or second-order differentiating the voltage detection signal Vo passed through the LPF with a detection threshold value. The detection threshold value is pre-stored in a memory unit (not shown). The detachment detection unit 33 may also generate the detachment detection signal DTR based on a change in resistance value calculated from the voltage detection signal Vo and the current detection signal Io, which are actual measured values.
[0051] An average feed speed Favg of the welding wire 100 being fed is provided to waveform control table linear calculation unit 37. The average feed speed Favg is stored in advance in feed setting data unit 35. In this embodiment, feed setting data unit 35 is located within welding power source 140, but various pieces of information related to feed settings may be stored in welding control device 120, and the various pieces of information may be output from welding control device 120 to welding power source 140.
[0052] Based on the given average feed speed Favg, the waveform control table linear calculation unit 37 determines values of the peak current Ip, the base current Ib, the time t1 when the base current Ib starts, the time t2 when the base current Ib ends, and the like, and outputs these values to the current setting unit 36. Note that, since the values of the wire position phase, time, and cycle cyc can be converted into each other as described above, the set value of the base start phase, etc. may be converted into a value of time or cycle cyc, and the converted value may be output to the current setting unit 36.
[0053] 2, in this embodiment, the average feed speed Favg is input to the waveform control table linear calculation unit 37. However, a value related to the average feed speed Favg may be input as a set value to the waveform control table linear calculation unit 37, and the waveform control table linear calculation unit 37 may use the set value as the average feed speed Favg. For example, if a database of average feed speeds Favg and average current values that enable optimal welding for the average feed speed Favg is stored in a storage unit (not shown), the average current value may be used as the set value, and the set value may be used as the average feed speed Favg.
[0054] The feed setting data unit 35 may store set values such as the wire amplitude Wf, the wire forward / reverse frequency Sf, and the wire forward / reverse cycle Tf in addition to the average feed speed Favg. The wire amplitude Wf, the wire forward / reverse frequency Sf, and the wire forward / reverse cycle Tf may be determined based on the input average feed speed Favg. The feed setting data unit 35 may also store set values other than these as feed setting data. In this embodiment, the value of the wire amplitude Wf refers to the wave height Wh shown in FIG. 3. In other words, the set value of the wire amplitude Wf is set to be the same as the wave height Wh.
[0055] In this embodiment, a period in which the feed rate is higher than the average feed rate Favg is defined as a forward feed period, and a period in which the feed rate is lower than the average feed rate Favg is defined as a reverse feed period, resulting in feed in which forward and reverse feed periods alternate (hereinafter abbreviated as "amplitude feed"). The period in which the feed rate is lower than the average feed rate Favg refers to a feed rate lower than the average feed rate Favg, and includes a negative feed rate, i.e., a rate at which the wire tip moves in the opposite direction from the position of the base material 200. The wire amplitude Wf indicates the range of change relative to the average feed rate Favg, and the wire forward / reverse cycle Tf indicates the time period during which the wire amplitude changes, which is the repetition unit. The wire forward / reverse frequency Sf is the reciprocal of the wire forward / reverse cycle Tf.
[0056] The average feed rate Favg, wire amplitude Wf, wire forward / reverse frequency Sf, and wire forward / reverse cycle Tf stored in the feed setting data unit 35 are input from the digital communication unit 42 to the digital communication unit 122 of the welding control device 120. In this embodiment, the feed setting data is communicated via CAN communication.
[0057] The welding sequence unit processes each task in the order of idle, gas flow, arc start, welding in progress, and anti-stick based on the teaching data and on the gas ON and arc start signals output from welding control device 120. In the welding in progress task, control is performed primarily by current setting unit 36. In Figure 2, for convenience, the welding condition information held by welding control device 120 is also shown enclosed by a dashed line within welding power source 140.
[0058] (Functional Configuration of Welding Control Device) As described above, digital communication unit 122 of welding control device 120 receives, via CAN communication, feed setting data such as average feed rate Favg, wire amplitude Wf, wire forward / reverse frequency Sf, and wire forward / reverse cycle Tf from feed setting data unit 35 of welding power source 140. Welding control device 120 has digital communication unit 123 for outputting this feed setting data to digital communication unit 162 of servo amplifier 160. In this embodiment, digital communication unit 123 of welding control device 120 and digital communication unit 162 of servo amplifier 160 are connected via EtherCAT (registered trademark) communication.
[0059] In addition, welding control device 120 stores various welding condition information such as the timing of gas and arc start (welding ON), voltage, and average feed speed settings, and outputs signals for gas ON, arc start, voltage command, and feed command to welding power source 140 based on a program created to operate welding robot 110.
[0060] (Functional Configuration of Servo Amplifier) Feed setting data such as average feed speed Favg, wire amplitude Wf, wire forward / reverse frequency Sf, and wire forward / reverse cycle Tf are input to a digital communication unit 162 of the servo amplifier 160 via EtherCAT (registered trademark) communication. A forward / reverse feed command generation unit 161 of the servo amplifier 160 generates a feed command for forward feed or reverse feed based on the setting information input via digital communication, i.e., the feed setting data. More specifically, the forward / reverse feed command generation unit 161 of the servo amplifier 160 calculates an amplitude feed speed Ff from the wire amplitude Wf and the wire forward / reverse cycle Tf, and calculates a feed speed command signal Fw based on this amplitude feed speed Ff and the average feed speed Favg.
[0061] In this embodiment, the feeding speed command signal Fw is expressed by the following equation: Fw=Ff+Favg (Equation (A))
[0062] Furthermore, the forward / reverse feed command generation unit 161 may detect at which wire position phase of the amplitude feed the detachment occurred, based on the detachment detection signal DTR provided by the detachment detection unit 33. However, the feed speed command signal Fw expressed by equation (A) is generated only when the detachment of a droplet from the tip of the welding wire 100 is detected within an expected period. If the detachment of a droplet is not detected within the expected period, the forward / reverse feed command generation unit 161 may switch the feed speed command signal Fw to feed control at a constant speed. For example, the forward / reverse feed command generation unit 161 switches the feed speed command signal Fw to feeding at an average feed speed Favg. The switch from feeding at the average feed speed Favg to feed control expressed by equation (A) is determined depending on the timing at which the detachment of a droplet is detected.
[0063] The servo amplifier performs inverter control of the servo motor 170 based on the feed speed command signal Fw in a forward / reverse feed command generating unit 161. Furthermore, a synchronization signal generating unit 163 of the servo amplifier 160 outputs a phase synchronization signal to the welding power source 140. This phase synchronization signal is generated based on the feed speed command signal Fw.
[0064] Note that welding power source 140 and synchronization signal generating unit 163 of servo amplifier 160 may be connected at least via an analog input / output. In this case, a synchronization signal is input to welding power source 140 from servo amplifier 160 via the analog input / output. By transmitting feed setting data such as average feed rate Favg, wire amplitude Wf, wire forward / reverse frequency Sf, and wire forward / reverse cycle Tf via digital communication, while transmitting the synchronization signal via analog communication, digital communication and analog communication can be used efficiently depending on the application.
[0065] Here, the phase related to the feed speed command signal Fw (hereinafter also referred to as "feed speed phase") is 0° at the start of forward feed, 180° (π) at the end of forward feed and the start of reverse feed, and 360° (2π) at the end of reverse feed. In this embodiment, the phase synchronization signal is a feed speed phase synchronization signal and a wire position phase synchronization signal. The feed speed phase synchronization signal is ON during the forward feed period (position from 0 to π) and OFF during the reverse feed period (position from π to 2π). On the other hand, the wire position phase synchronization signal is ON during the period when the wire approaches the base material 200 side from the center position of the wave height when the wire is fed forward or backward (position from 0.5π to 1.5π), and OFF during the period when the wire approaches the tip side from the center position of the wire amplitude (position from 1.5π to 0.5π). Based on this phase synchronization signal and the aforementioned phase delay correction amount, the tip position of the welding wire 100, i.e., the wire position phase, is determined by the wire tip position converter 36B in the welding power source 140.
[0066] (Welding Method) Next, a welding method according to this embodiment will be described. The welding method according to this embodiment is based on the technical concept of locally increasing the arc pressure at a specific wire position phase in a wire feed control method, thereby expanding the molten pool and achieving penetration and a wide bead width.
[0067] In the feed control method, the wire tip is closest to the weld pool when switching from forward feed to reverse feed. As the wire tip approaches the weld pool, the arc length shortens, momentarily increasing the arc pressure on the weld pool. Therefore, the wire position phase that locally increases the arc pressure is before and after switching from forward feed to reverse feed, i.e., between 90° (0.5π) and 270° (1.5π). Further increasing the welding current during this period further enhances the weld pool expansion effect. However, such control can result in excessive weld pool expansion, which can lead to burn-through, molten metal sagging due to gravity, and poor crosslinking. Furthermore, the arc pressure pushing up the droplets increases even during the reverse feed period, which causes droplet detachment. This inhibits droplet detachment during the reverse feed period, destabilizing droplet transfer and potentially causing spatter. Therefore, in the welding method according to this embodiment, the welding current is significantly increased in a local range between 90° (0.5π) and 180° (1.5π) of the wire position phase to expand the molten pool and ensure penetration and a wide bead width, while the welding current is significantly decreased in the range between 180° (π) and 270° (1.5π) to provide a cooling period to prevent burn-through, dripping of the molten metal due to the influence of gravity, and failure of droplet detachment. This ensures robustness in fillet welding. The welding current between the above wire position phases will be described in detail below.
[0068] (Wire position phase period from 90° to 180°: Average current or more) The period from 90° to 180° of the wire position phase is the period for widening the penetration and bead width, and the average welding current I 90~180deg_ave is the average current value I ave The average welding current value I ave is the set welding current value I set In this embodiment, I ave ≒I set The average current value I 90~180deg_ave , the average current value I setBy setting the current value to the above, it is possible to widen the penetration and bead width in the wire feed control method. 90~180deg The average value of the welding current at 90~180deg_ave and the set welding current value I set (≒ average welding current I ave ) and (I 90~180deg_ave ) / (I set ) is preferably 1.10 or more.
[0069] (Wire position phase period from 180° to 270°: average current or less) The period from 180° to 270° of the wire position phase is a cooling period in which the welding current is significantly reduced. The average value I 180~270deg_ave is the average current value I ave The average welding current value I ave is the set welding current value I set In this embodiment, I ave ≒I set The average current value I 180~270deg_ave , the average current value I set By setting the current value below, burn-through, dripping of the molten part due to the influence of gravity, and failure of droplet separation can be prevented in the feed control method. 180~270deg The average value of the welding current at 180~270deg_ave and the set welding current value I set (≒ average welding current I ave ) and (I 180~270deg_ave ) / (I set ) is preferably 0.90 or less.
[0070] ((I 180~270deg_ave ) / (I 90~180deg_ave)≦0.50) As described above, by setting the average current or more during the wire position phase period from 90° to 180° and the average current or less during the wire position phase period from 180° to 270°, robustness in fillet welding can be ensured. This robustness is better the greater the difference between the average current during the wire position phase period from 90° to 180° and the average current during the wire position phase period from 180° to 270°. Specifically, during the period T when the welding wire position is from 90° to 180°, 90~180deg The average value of the welding current at 90~180deg_ave and the welding wire position is between 180° and 270° during the period T 180~270deg The average value of the welding current at 180~270deg_ave This is the ratio of (I 180~270deg_ave ) / (I 90~180deg_ave From the viewpoint of the stability of droplet transfer, the lower limit of this ratio should be set to 0.10 or more.
[0071] (Wire forward / reverse frequency: 50 to 150) The wire forward / reverse frequency is preferably in the range of 50 to 150. By setting the wire forward / reverse frequency to 150 or less, the period T 90~180deg The average value of the welding current at 90~180deg_ave and the period T when the wire position phase is 180° to 270°. 180~270deg The average value of the welding current at 180~270deg_ave On the other hand, by setting the value to 50 or more, the stability of the droplet transfer can be maintained.
[0072] (Wire amplitude: 3.3 to 6.3) The wire amplitude is preferably in the range of 3.3 to 6.3. By setting the wire amplitude to 3.3 or more, it is possible to maintain stable droplet transfer. On the other hand, by setting the wire amplitude to 6.3 or less, short circuits are prevented during the period when the wire position phase is between 90 degrees and 180 degrees, and the wire tip approaches the molten pool more closely, increasing the arc pressure and resulting in greater penetration and a wider bead width.
[0073] (Welding Wire) In the feed control method, when forward or reverse feed is performed, there are wire position phases in which the wire is fed at an excessively high feed rate and there are wire position phases in which the feed rate is zero, resulting in large speed fluctuations within one cycle in which forward and reverse feed are performed. This speed fluctuation is particularly noticeable in the short-circuit suppression type feed control. Specifically, in this embodiment, the wire feed reaches its maximum speed during forward feed when the wire position phase is 90 degrees, the feed rate is zero after about 180 degrees, and further reaches its maximum speed during reverse feed at 270 degrees, and the feed rate is zero just before 360 degrees. As described above, between 90° and 180° of wire position phase, strong arc pressure simultaneously pushes the weld pool and widens it. However, during this period, the feed rate drops from its maximum speed during forward feed to zero, and droplets formed at the wire tip are subject to inertial forces, making them prone to unintended droplet detachment and droplet oscillation. Unintended droplet detachment, such as during forward feed, can destabilize the timing of droplet transfer, potentially resulting in increased spatter and poor bead shape. Furthermore, droplet oscillation deflects the arc in response to the oscillating droplet movement. This causes the arc pressure to shift the position at which the weld pool is pushed into the weld pool, preventing concentration and preventing satisfactory penetration and bead width. Therefore, it is preferable to prevent droplet detachment and droplet oscillation, even when excessive inertial forces are applied.
[0074] Generally, to prevent unintended droplet detachment or droplet oscillation, welding wire can be designed to control the physical properties of the droplets during melting, such as by increasing the viscosity of the droplets. However, controlling the physical properties during melting limits the composition, which in turn limits the applicable wire composition. Therefore, in the welding method according to this embodiment, a welding wire that can prevent droplet detachment or droplet oscillation even when excessive inertial force is applied, without considering the physical properties of the droplets, is preferable. In contrast, the inventors have discovered that by using a welding wire suitable for the welding method according to this embodiment, which contains trace amounts of strong deoxidizing elements such as Ti, Al, Mg, and Zr and oxygen, droplet detachment and droplet oscillation can be prevented even when excessive inertial force is applied, without controlling the physical properties of the droplets through composition. This is because, when the welding wire is melted by the arc, strong deoxidizing elements such as Ti, Al, Mg, and Zr combine with oxygen in the wire, forming an oxide film of the strong deoxidizing elements on the droplet surface. This oxide film has a high interfacial tension with the surrounding gas and acts to reduce the surface area of the droplet itself, so at the initial droplet weight when the droplet begins to grow, the droplet is less likely to detach and oscillation is suppressed.
[0075] Here, the strong deoxidizing element contained in the wire naturally has a high affinity for oxygen, and an oxide film will not form on the droplet surface unless the element has a high melting point of its oxide. Therefore, the strong deoxidizing element added to the welding wire is preferably an element selected from Ti, Al, Mg, and Zr. Note that although there is no problem with the type of welding wire, a metal-based flux-cored wire may be used, but it is preferable to use a solid wire from the viewpoint of making it easier to control the amount of oxygen in the wire.
[0076] The form of the welding wire that is most suitable for the welding method according to this embodiment will be described in detail below. In the following description, the amount of each component in the wire is defined as the content relative to the total mass of the wire.
[0077] (C: 0.20 mass% or less (including 0 mass%)) C has a deoxidizing effect and is an element that has the effect of improving the mechanical performance of the weld metal. The C content can be adjusted appropriately depending on the strength of the application, and in the welding method according to this embodiment, C does not need to be contained if strength can be ensured with other elements. In other words, it can be 0 mass%. However, since C has a deoxidizing effect when contained, it is preferable to keep the content at 0.20 mass% or less in order to stably form an oxide film on the droplet surface. Furthermore, in applications such as lap fillet welding of 440 to 980 MPa class steel plates used in automotive suspension parts, it is more preferable to determine the content so that the MIX value, described below, falls within an appropriate range.
[0078] (Si: 1.00% by mass or less (including 0% by mass)) Si is a deoxidizer and a component that enhances the mechanical properties of the weld metal. The Si content can be adjusted appropriately depending on the strength of the application. In the welding method according to this embodiment, Si need not be present if strength can be ensured with other elements. In other words, 0% by mass is acceptable. However, the melting point of Si oxide is 1710°C, and if Si combines with oxygen to form oxide in the molten pool, it may remain in a molten state on the molten pool surface. Because molten oxide has very high viscosity, it inhibits deep penetration and bead width expansion between 90° and 180° of wire position phase. Furthermore, if Si oxide remains as slag on the weld bead, it will prevent the formation of an electrodeposition coating. Therefore, the lower the Si content, the better. 1.00% by mass or less is preferable, 0.50% by mass or less is more preferable, and 0.20% by mass or less is even more preferable. In particular, by limiting the Si content to 0.50 mass% or less, it is possible to suppress an increase in the viscosity of the molten pool, resulting in good robustness, and furthermore, the composition of the slag formed on the weld bead changes, resulting in a thin slag with good adhesion that can form an electrodeposition coating.In addition to reducing the Si content, it is even more preferable for lap fillet welding of 440 to 980 MPa class steel sheets used in automotive suspension parts if the MIX value, described below, is within the appropriate range.
[0079] (Mn: 1.30 to 2.40 mass%) Like Si, Mn is a deoxidizer and is a component that has the effect of improving the mechanical performance of the weld metal. The Mn content can be adjusted appropriately depending on the strength of the application. In the welding method according to this embodiment, Mn need not be contained if strength can be ensured with other elements. In other words, it can be 0 mass%. When the Si content is reduced as described above, the Mn content can be supplemented, and a content in the range of 1.30 to 2.40 mass% is preferable as a means of balancing mechanical performance without impairing the effects of this embodiment. Furthermore, in applications involving lap fillet welding of 440 to 980 MPa-class steel plates used in automotive suspension parts, it is more preferable to determine the content so that the MIX value, described below, falls within an appropriate range.
[0080] (P: 0.025% by mass (including 0% by mass)) P is an element related to the cracking tendency of the weld metal, and the lower the P content in the weld metal, the better the cracking resistance. Therefore, in the welding method according to this embodiment, it is not necessary to particularly include P. In other words, it may be 0% by mass. From the viewpoint of cracking resistance, the P content in the wire is preferably 0.025% by mass or less.
[0081] (S: 0.030% by mass (including 0% by mass)) S is a component that reduces the surface tension of the molten metal. The lower the surface tension, the more likely it is that droplet detachment is promoted. Therefore, in the present invention, in order to prevent droplet detachment between wire positions of 90 degrees and 180 degrees, it is preferable that the S content be 0.030% by mass or less. From the perspective of preventing droplet detachment, it is not particularly necessary to contain S (0% by mass is acceptable). However, an appropriate amount of S affects the physical properties of the molten pool surface and has the effect of improving the fit of the weld bead, so a content of 0.001% by mass is more preferable.
[0082] (Cu: 0.50 mass% or less (including 0 mass%)) Cu is a component that has the effect of enhancing the mechanical performance of the weld metal. The Cu content can be adjusted appropriately depending on the strength of the application. In the welding method according to this embodiment, Cu need not be contained if strength can be ensured with other elements. In other words, it can be 0 mass%. Furthermore, Cu may be added to the welding wire as a plating, and the total content in the wire and the plating amount is preferably 0.50 mass% or less. This is because keeping the Cu content at 0.50 mass% or less achieves a balance with other elements that enhance mechanical performance, and the weld metal does not have excessive strength. Furthermore, in applications such as lap fillet welding of 440 to 980 MPa class steel sheets used in automotive suspension parts, it is more preferable to determine the Cu content so that the MIX value, described below, falls within an appropriate range.
[0083] (Ni: 1.00 mass% or less (including 0 mass%)) Ni is a component that has the effect of enhancing the mechanical performance of the weld metal. The Ni content can be adjusted appropriately depending on the strength of the application, and in the welding method according to this embodiment, Ni need not be contained if strength can be ensured with other elements. In other words, 0 mass% is acceptable. By limiting the Ni content to 1.00 mass% or less, a balance is achieved with other elements that enhance mechanical performance, and the weld metal does not have excessive strength, so it is preferable to set the Ni content to 1.00 mass% or less. Furthermore, in applications such as lap fillet welding of 440 to 980 MPa class steel plates used in automotive suspension parts, it is more preferable to determine the content so that the MIX value, described below, falls within an appropriate range.
[0084] (Cr: 1.00 mass% or less (including 0 mass%)) Cr is a component that has the effect of enhancing the mechanical performance of the weld metal. The Cr content can be adjusted appropriately depending on the strength of the application, and in the welding method according to this embodiment, Cr need not be contained if strength can be ensured with other elements. In other words, it can be 0 mass%. By keeping the Cr content to 1.00 mass% or less, a balance is achieved with other elements that enhance mechanical performance, and the weld metal does not have excessive strength, so it is preferable to set the Cr content to 1.00 mass% or less. Furthermore, in applications such as lap fillet welding of 440 to 980 MPa class steel plates used in automotive suspension parts, it is more preferable to determine the content so that the MIX value, described below, falls within an appropriate range.
[0085] (Mo: 1.00 mass% or less (including 0 mass%)) Mo is a component that has the effect of improving the mechanical performance of the weld metal. The Mo content can be adjusted appropriately depending on the strength of the application, and in the welding method according to this embodiment, Mo need not be contained if strength can be ensured with other elements. In other words, 0 mass% is acceptable. By keeping the Mo content at 1.00 mass% or less, a balance is achieved with other elements that improve mechanical performance, and the weld metal does not have excessive strength, so it is preferable to set the Mo content to 1.00 mass% or less. Furthermore, in applications where lap fillet welding of 440 to 980 MPa class steel plates is used in automotive suspension parts, it is more preferable to determine the content so that the MIX value, described below, falls within an appropriate range.
[0086] (V: 0.50 mass% or less (including 0 mass%)) V is a component that has the effect of enhancing the mechanical performance of the weld metal. The V content can be adjusted appropriately depending on the strength of the application, and in the welding method according to this embodiment, V need not be contained if strength can be ensured with other elements. In other words, it can be 0 mass%. By keeping the V content to 0.50 mass% or less, a balance is achieved with other elements that enhance mechanical performance, and the weld metal does not have excessive strength, so it is preferable to set the V content to 0.50 mass% or less. Furthermore, in applications such as lap fillet welding of 440 to 980 MPa class steel plates used in automotive suspension parts, it is more preferable to determine the content so that the MIX value, described below, falls within an appropriate range.
[0087] (B: 0.010% by mass or less (including 0% by mass)) B is a component that has the effect of enhancing the mechanical performance of the weld metal. The content of B can be adjusted appropriately depending on the strength of the application, and in the welding method according to this embodiment, B need not be contained if strength can be ensured with other elements. In other words, it may be 0% by mass. By keeping the B content to 0.010% by mass or less, a balance is achieved with other elements that enhance mechanical performance, and the weld metal does not have excessive strength, so it is preferable to set the B content to 0.010% by mass or less. Furthermore, in applications such as lap fillet welding of 440 to 980 MPa class steel plates used in automotive suspension parts, it is more preferable to determine the content so that the MIX value, described below, falls within an appropriate range.
[0088] (Total amount of Ti, Al, Mg, and Zr: 0.001 to 0.450 mass%) ((Ti + Al + Mg + Zr) / O: 0.5 to 150) Ti, Al, Mg, and Zr are strong deoxidizing elements that have a very high affinity with O (oxygen), and the melting points of these oxides are higher than the melting point of iron. When the welding wire contains at least one of Ti, Al, Mg, and Zr and O (oxygen), which will be described later, an oxide film forms on the surface of the droplets when they are formed at the tip of the welding wire. The formation of this oxide film makes it difficult for the shape of the droplets to change even if the feed rate changes locally depending on the wire position and an inertial force is applied to the droplets, thereby suppressing droplet oscillation and droplet detachment from unintended wire position phases. The total content of strong deoxidizing elements (Ti, Al, Mg, Zr) at which the above-mentioned effects are fully exhibited is preferably 0.001% by mass or more, more preferably 0.050% by mass or more, and even more preferably 0.150% by mass or more. Furthermore, if the contents of Ti, Al, Mg, and Zr are excessive, the amount of slag on the weld bead increases, and the slag composition also changes depending on the contents of Ti, Al, Mg, and Zr. Therefore, in applications for lap fillet welding of 440 to 980 MPa class steel sheets used in automobile suspension parts, from the viewpoints of bead appearance and electrodeposition paintability, the total content of Ti, Al, Mg, and Zr is preferably limited to 0.450% by mass or less, and more preferably 0.380% by mass or less. Furthermore, when droplets are formed at the tip of the welding wire, the relationship between Ti, Al, Mg, Zr and O (oxygen) suitable for forming an oxide film on the droplet surface is such that the value calculated from (Ti+Al+Mg+Zr / )O is preferably in the range of 0.5 to 150, and more preferably in the range of 0.5 to 75.0.
[0089] (O: 0.0010 to 0.0100 mass%) When O is contained together with the above-mentioned strong deoxidizing elements, an oxide film is formed on the surface of the droplets during droplet formation at the tip of the welding wire, thereby suppressing droplet oscillation and droplet detachment at unintended wire positions. In the welding method according to this embodiment, the O content effective for suppressing droplet oscillation and droplet detachment at unintended wire positions is preferably 0.0010 mass% or more, and more preferably 0.0015 mass% or more. Furthermore, if O is contained in excess in the wire, the amount of slag on the weld bead increases, which may affect the bead appearance. Therefore, the O content is preferably 0.0100 mass% or less, more preferably 0.0080 mass% or less, and even more preferably 0.0050 mass% or less.
[0090] (N: 0.0300% by mass or less) N is a component that has the effect of enhancing the mechanical performance of the weld metal. The N content can be adjusted appropriately depending on the strength of the application, and in the welding method according to this embodiment, N does not need to be contained if strength can be ensured by other elements. In other words, it can be 0% by mass. By limiting the N content to 0.0300% by mass or less, a balance is achieved with other elements that enhance mechanical performance, and the weld metal does not have excessive strength, so it is preferable to set the N content to 0.0300% by mass or less.
[0091] (0.35≦MIX value≦1.40) MIX value = C + Si / 24 + Mn / 6 + Ni / 40 + Cr / 5 + Mo / 4 + V / 4 + Cu / 13. When improving robustness by suppressing an increase in viscosity of the molten pool and improving electrodeposition coatability by controlling the slag composition, the Si content must be kept to 0.50 mass% or less. Therefore, the mechanical performance must be compensated for by the reduced Si content with other elements, but it is preferable to balance the other elements so that the MIX value falls within the range of 0.35 to 1.40.
[0092] (Ti: 0.030 to 0.250 mass%) (Al: 0.001 to 0.300 mass%) As the contained strong deoxidizing elements, Ti and Al are preferably selected. Oxides of Mg and Zr have melting points of 2500°C or higher, and their affinity with oxygen increases as the temperature decreases, so a thick oxide film forms over the entire droplet. As a result, a thick oxide film also forms on the upper part of the droplet, which is relatively cool, i.e., near the boundary between the droplet and the wire. This may hinder the formation of a necking at the droplet detachment position in the latter half of wire reverse feed (270°C to 360°C), preventing the droplet from detaching. On the other hand, oxides of Ti and Al have melting points of 2100°C or lower, and compared with Mg and Zr, the oxide film does not become thick, and an oxide film is less likely to form near the boundary between the droplet and the wire. Therefore, a necking occurs at the boundary between the wire and the droplet in the latter half of wire reverse feed, and the droplet detaches. Therefore, Ti and Al are preferably contained as strong deoxidizing elements, with the Ti content preferably being in the range of 0.030 to 0.250 mass%. The Al content is preferably in the range of 0.001 to 0.300 mass%, and more preferably in the range of 0.001 to 0.200 mass%. Furthermore, the Al content is more preferably greater than 0.10 mass%. Furthermore, the above effect is enhanced when the ratio of Ti to Al (Ti / Al) is 0.3 to 20. Furthermore, from the viewpoint of further improving electrodeposition coatability, when the Si content is limited to 0.5 mass% or less and the composition of the slag formed on the weld bead is controlled, the ratio of Ti to Al (Ti / Al) is even more preferably 0.4 to 13.0, and even more preferably 0.4 to 3.0.
[0093] In order to stably detach the wire due to inertial force during the latter half of reverse wire feeding, the maximum feed speed during reverse wire feeding is preferably 50 m / min or higher. On the other hand, in the welding method according to this embodiment, a high current is instantaneously applied during the latter half of forward wire feeding (90° to 180°) to increase the arc pressure on the molten pool, thereby achieving penetration and a wide bead width. Therefore, the maximum feed speed during forward wire feeding must necessarily be equal to or close to the maximum feed speed during reverse wire feeding. However, the higher the maximum speed on the forward wire feeding side, the greater the likelihood of droplet oscillation and detachment during the latter half of forward wire feeding (90° to 180°). In this embodiment, by containing the above-mentioned Al and Ti and controlling the oxide coating, droplet oscillation and detachment can be prevented during the latter half of forward wire feeding (90° to 180°) and droplet detachment can be promoted during the latter half of reverse wire feeding. Specifically, the distribution of strong deoxidizing elements is preferably (Ti + Al) / (Ti + Al + Mg + Zr) > 0.5, more preferably the value of (Ti + Al) / (Ti + Al + Mg + Zr) is 0.95 or more, and it is even more preferable that the contents of Mg and Zr are equal to or less than the contents of unavoidable impurities and that the alloy is composed only of Ti and Al.
[0094] (Balance: Fe and inevitable impurities) The balance of the wire preferably used in this embodiment is Fe and inevitable impurities. Examples of inevitable impurities include Nb, Li, Sn, Sb, Bi, and As. The content of each of these inevitable impurities is preferably 0.0100 mass% or less, and more preferably 0.0050 mass% or less, relative to the total mass of the wire. Furthermore, the total content of these inevitable impurities is preferably 0.0200 mass% or less, relative to the total mass of the wire.
[0095] The present embodiment will be described in more detail below with reference to examples, but the present invention is not limited to these examples, and modifications can be made within the scope of the spirit of the present invention, and all such modifications are included in the technical scope of the present invention.
[0096] (Welding Wire) Figure 4 is a diagram showing the compositions of two wires used in the examples. In the examples, two types of wire, Wire A and Wire B, were used. The components contained in each wire are as shown in Figure 4. Note that all values in Figure 4 indicate mass %. The remainder other than the wire components shown in Figure 4 is Fe and unavoidable impurities.
[0097] (Welding Control Method) Fig. 5 is a diagram showing two welding methods used in the examples. In the examples, two types of welding methods were used: Feed Control Method A and Feed Control Method B. Note that general pulsed MAG welding was used as a comparative example.
[0098] The feed control method A is a short-circuit suppression method, with a wire frequency of 70 Hz and a wave height of 5 mm (amplitude ±2.5 mm). The current control switching timing is fixed at the wire position. The wire position for peak current switching is 157 degrees, and the wire position for base current switching is 350 degrees (see Figure 6).
[0099] The feed control method B is a short-circuit type method. The wire frequency varies according to the short-circuit period. The wire amplitude also varies. The timing for switching the current control is when a short circuit is detected.
[0100] (Welding conditions) The welding conditions were set as follows: Steel plate: 200 mm long x 50 mm wide x 2.3 mm thick, SPH440 steel plate Welding position: horizontal lap fillet welding Shielding gas: 100% by volume CO 2 Gas: 80% Ar by volume + 20% CO by volume 2 Gas ・Average current: 200-250A ・Average voltage: 19-27V ・Wire feed rate: 7.0m / min ・Welding speed: 100cm / min ・Welding length: 150mm
[0101] (Evaluation Results) Fig. 6 is a graph of the welding current and the feed speed when feed control method A was used as the welding method. Fig. 7 is a graph of the welding current and the feed speed when feed control method B was used as the welding method. In both graphs, the horizontal axis represents the wire position phase. The vertical axis represents the welding current in amperes (A) and the feed speed in meters per minute (mpm).
[0102] Fig. 8 shows welding conditions and actual measurement data when feed control method A, feed control method B, and pulsed MAG welding as a comparative example are used, respectively. Figs. 9A to 9E show the results of a target deviation test based on the welding conditions and actual measurement data shown in Fig. 8.
[0103] First, the welding conditions will be explained. Test Nos. 1 and 2 used feed control method A. Test Nos. 3 and 4 used feed control method B. Test No. 5 used pulsed MAG welding. Regarding the type of wire, Test No. 2 used Wire B, and Test Nos. 1, 3-5 used Wire A. The shielding gas was 100% by volume CO for Test Nos. 1-3. 2 Gas (CO 2 ) for test number 4-5, 80 vol% Ar + 20 vol% CO 2 Gas (Ar—CO in FIG. 8 and the following) 2 The welding speed was 100 cm / min in all tests, and the feed rate was 7 m / min in all tests.
[0104] Next, the actual measurement data will be described. For each test number, the average current and average voltage values are shown in Figure 8. For test numbers 1 to 4, the average current over a predetermined period and the average voltage over a predetermined period are shown in Figure 8. Furthermore, for test numbers 1 to 4, the ratio of the average current was also calculated based on the above-mentioned actual measurement values, and is shown in Figure 8.
[0105] As shown in Figures 9A to 9E, trials were conducted for each test number using multiple target positions. The test results show the gap width and target position (amount of deviation from the target position) at that time, as well as whether the welding result was good (good welding results are indicated by a circle in Figures 9A to 9E) or poor (poor welding results are indicated by a cross in Figures 9A to 9E). The target position (amount of deviation from the target position) is the amount of deviation when the axis is perpendicular to the weld line, with a value of 0 representing the correct target position. Negative values (-1 to -5) indicate a deviation in the direction of the upper plate, and positive values (1 to 5) indicate a deviation in the opposite direction.
[0106] Furthermore, the test results, indicated by circles (○) and crosses (×), were plotted on a target deviation tolerance graph. The horizontal axis of the target deviation tolerance graph represents the target position (mm), and the vertical axis represents the gap width (mm). The allowable range is indicated by a dashed line on the target deviation tolerance graph. The allowable range is indicated as a rectangle that falls within the region formed by connecting the plotted points where the test results are marked ○. The larger the area of this dashed region, the higher the robustness. This is because, as described above, the greater the deviation in the welding target position or the gap, the more pronounced the problems of poor bead shape and bridging become. However, within the dashed region, there is a high probability of obtaining good welding results, and a large area of the dashed region indicates that good welding results can be obtained even if the target position is deviated significantly or the gap width is larger.
[0107] 9A to 9E, it can be seen that the area of the dashed line region is larger and more robust in the case of feed control method A than in the case of feed control method B. It can also be seen that when the same feed control method A is used, the area of the dashed line region is larger and more robust when wire A is used than when wire B is used.
[0108] The present invention is not limited to the above-described embodiments, and the present invention also contemplates the mutual combination of the various components of the embodiments, as well as modifications and applications by those skilled in the art based on the description in the specification and well-known techniques, and these modifications and applications are included in the scope of protection sought.
[0109] As described above, the present specification discloses the following:
[0110] (1) A fillet welding method employing a feed control method for alternately switching a feed speed between a forward feed period and a reverse feed period, wherein, in the feed control method, when a wire position phase based on the position of the welding wire at the time of switching from the reverse feed period to the forward feed period is set to 0°, a period T in which the wire position phase is 90° to 180° is 90~180deg The average value of the welding current at 90~180deg_ave The set welding current value I set and during a period T when the wire position phase is between 180 degrees and 270 degrees. 180~270deg The average value of the welding current at 180~270deg_ave The set welding current value I set According to this fillet welding method, excellent robustness can be achieved even when a feed control welding method is applied.
[0111] (2) The fillet welding method according to (1), wherein the wire feed control method sets a wire frequency to a predetermined value when a forward feed period and a reverse feed period are defined as one cycle, and switches at least the welding current between a current suppression period and a current non-suppression period according to the wire position phase or the wire feed speed phase. This fillet welding method can achieve excellent robustness even in the case of a short-circuit suppression type feed control method.
[0112] (3) A period T in which the wire position phase is 90 degrees to 180 degrees 90~180deg The average value of the welding current at 90~180deg_ave and the set welding current value I set is the ratio of (I 90~180deg_ave ) / (I set ) is 1.10 or more. This fillet welding method can further increase the penetration and bead width.
[0113] (4) A period T in which the wire position phase is 180 degrees to 270 degrees 180~270deg The average value of the welding current at 180~270deg_aveand the set welding current value I set is the ratio of (I 180~270deg_ave ) / (I set ) is 0.90 or less. This fillet welding method can further increase the penetration and bead width.
[0114] (5) A period T in which the wire position phase is 90 degrees to 180 degrees 90~180deg The average value of the welding current at 90~180deg_ave and the period T in which the wire position phase is 180° to 270° 180~270deg The average value of the welding current at 180~270deg_ave is the ratio of (I 180~270deg_ave ) / (I 90~180deg_ave ) is 0.5 or less. This fillet welding method can ensure high robustness.
[0115] (6) The fillet welding method according to any one of (1) to (5), characterized in that the welding wire contains, relative to the total mass of the welding wire, O: 0.0010 to 0.0100 mass%, further contains at least one of Ti, Al, Mg, and Zr, and the total amount of Ti, Al, Mg, and Zr is 0.001 to 0.450 mass%. According to this fillet welding method, when droplets are formed at the tip of the welding wire, an oxide film is formed on the surface of the droplets, which causes the feed rate to change locally depending on the wire position, making it difficult for the droplets to change shape even if an inertial force is applied to the droplets, thereby suppressing fluctuation of the droplets and droplet detachment from unintended wire positions.
[0116] (7) The fillet welding method according to (6), characterized in that the Si content of the welding wire is 0.50 mass% or less based on the total mass of the welding wire, and the value of C + Si / 24 + Mn / 6 + Ni / 40 + Cr / 5 + Mo / 4 + V / 4 + Cu / 13 is 0.35 to 1.40. According to this fillet welding method, by limiting the Si content to 0.50 mass% or less, an increase in the viscosity of the molten pool can be suppressed, resulting in good robustness. Furthermore, the composition of the slag formed on the weld bead changes, resulting in a thin slag with good adhesion that can form an electrodeposition coating. Furthermore, while the reduced Si content requires the use of other elements to compensate for the mechanical performance, the MIX value within the above-mentioned range allows for a balance of the other elements.
[0117] (8) The fillet welding method according to (7), characterized in that the welding wire contains, relative to the total mass of the wire, Ti: 0.030 to 0.250 mass% and Al: 0.001 to 0.300 mass%, with a Ti / Al ratio of 0.3 to 20. According to this fillet welding method, the melting points of oxides of Ti and Al are 2100°C or less, and compared with Mg and Zr, the oxide film is not thick and is less likely to form near the boundary between the droplet and the wire. Therefore, in the latter half of reverse wire feeding, a constriction occurs at the boundary between the wire and the droplet, causing the droplet to detach. This effect is promoted by the Ti / Al ratio being 0.3 to 20.
[0118] (9) The fillet welding method according to (6), characterized in that the feed rate during reverse feed when the wire position phase is 270° is 50 m / min or more, and the value of the formula (Ti + Al) / (Ti + Al + Mg + Zr) obtained by the contents of Ti, Al, Mg, and Zr contained in the welding wire is 0.5 or more. According to this fillet welding method, by setting the maximum feed rate during reverse feed to 50 m / min or more, the wire can be stably detached by inertial force in the latter half of reverse feed. Furthermore, by containing Al and Ti and controlling the oxide coating, it is possible to prevent droplet oscillation and detachment in the latter half of forward feed (90 to 180°) and promote detachment in the latter half of reverse feed.
[0119] (10) A feed control method applied to a fillet welding method, which alternately switches a feed speed between a forward feed period and a reverse feed period, wherein, when a wire position phase based on the position of the welding wire at the time of switching from the reverse feed period to the forward feed period is set to 0°, a period T in which the wire position phase is 90° to 180° is 90~180deg The average value of the welding current at 90~180deg_ave The set welding current value I set and during a period T when the wire position phase is between 180 degrees and 270 degrees. 180~270deg The average value of the welding current at 180~270deg_ave The set welding current value I set According to this feed control method, excellent robustness can be achieved even when it is applied to fillet welding.
[0120] (11) A power supply that is applied to a fillet welding method and has a function of performing feed control to alternately switch a feed speed between a forward feed period and a reverse feed period, wherein in the feed control, when a wire position phase based on the position of the welding wire at the time of switching from the reverse feed period to the forward feed period is set to 0 deg, a period T in which the wire position phase is 90 deg to 180 deg is 90~180deg The average value of the welding current at 90~180deg_ave The set welding current value I set and during a period T when the wire position phase is between 180 degrees and 270 degrees. 180~270deg The average value of the welding current at 180~270deg_ave The set welding current value I set This power supply can achieve excellent robustness even when a feed control welding method in which the power supply controls the feed is applied to fillet welding.
[0121] (12) A fillet welding system employing a feed control method for alternately switching a feed speed between a forward feed period and a reverse feed period, wherein, in the feed control method, when a wire position phase based on a position of the welding wire at the time of switching from the reverse feed period to the forward feed period is set to 0°, a period T in which the wire position phase is 90° to 180° is 90~180deg The average value of the welding current at 90~180deg_ave is the set welding current value I set and during a period T when the wire position phase is between 180 degrees and 270 degrees. 180~270deg The average value of the welding current at 180~270deg_ave is the set welding current value I set According to this fillet welding system, excellent robustness can be achieved even when a feed control welding method is applied.
[0122] Although various embodiments have been described above, it goes without saying that the present invention is not limited to such examples. It is clear that a person skilled in the art can conceive of various modifications or alterations within the scope of the claims, and it is understood that these also naturally fall within the technical scope of the present invention. Furthermore, the components of the above embodiments may be combined in any manner as long as they do not deviate from the spirit of the invention.
[0123] This application is based on a Japanese patent application (Patent Application No. 2023-059087) filed on March 31, 2023, the contents of which are incorporated herein by reference.
[0124] REFERENCE SIGNS LIST 1 AC power supply 2 Primary side rectifier 3 Smoothing capacitor 4 Switching element 5 Transformer 6 Secondary side rectifier 7 Reactor 30 Inverter drive unit 31 Current detection unit 32 Voltage detection unit 33 Separation detection unit 34 Current error amplification unit 35 Feed setting data unit 36 Current setting unit 36A Target current setting unit 36B Wire tip position conversion unit 36C Voltage setting unit 37 Waveform control table linear calculation unit 38 Phase delay correction unit 39 Push feeder control unit 40 A / D input unit 41 Electrical angle adjustment unit 42 Digital communication unit 50 Welding system 100 Welding wire 110 Welding robot 111 Welding torch 120 Welding control device 122 Digital communication unit 123 Digital communication unit 140 Welding power source 141 Control system unit 150 Controller 160 Servo amplifier 161 Forward / reverse feed command generating section 162 Digital communication section 163 Synchronization signal generating section 170 Servo motor 180 Push motor 190 Wire buffer 191 Serial-to-analog conversion section 200 Work
Claims
1. A fillet welding method using a feed control method that alternately switches the feed speed between a forward feed period and a reverse feed period, wherein, in the feed control method, when a wire position phase based on the position of the welding wire at the time of switching from the reverse feed period to the forward feed period is set to 0 deg, 90~180deg The average value of the welding current in 90~180deg_ave The set welding current value I set and the wire position phase is in a period T 180~270deg The average value of the welding current in 180~270deg_ave The set welding current value I set The fillet welding method according to claim 1, wherein the welding distance is smaller than or equal to the welding distance.
2. The fillet welding method according to claim 1, characterized in that the wire feed control method sets a wire frequency at a predetermined value when a forward feed period and a reverse feed period form one cycle, and switches at least the welding current between a current suppression period and a current non-suppression period according to the wire position phase or the wire feed speed phase.
3. The period T during which the wire position phase is 90 deg to 180 deg 90~180deg The average value of the welding current in 90~180deg_ave and the set welding current value I set is the ratio of (I 90~180deg_ave ) / (I set 2. The fillet welding method according to claim 1, wherein the ratio of the welded joint strength to the welded joint strength is 1.10 or more.
4. The period T during which the wire position phase is 180 deg to 270 deg 180~270deg The average value of the welding current in 180~270deg_ave and the set welding current value I set is the ratio of (I 180~270deg_ave ) / (I set 2. The fillet welding method according to claim 1, wherein the difference between the welded joint and the welded joint is 0.90 or less.
5. The period T during which the wire position phase is 90 deg to 180 deg 90~180deg The average value of the welding current in 90~180deg_ave and a period T in which the wire position phase is 180 deg to 270 deg. 180~270deg The average value of the welding current in 180~270deg_ave is the ratio of (I 180~270deg_ave ) / (I 90~180deg_ave 2. The fillet welding method according to claim 1, wherein the difference between the welded joint and the welded joint is 0.5 or less.
6. A fillet welding method according to any one of claims 1 to 5, characterized in that the welding wire contains, relative to the total mass of the welding wire, O: 0.0010 to 0.0100 mass%, further contains at least one of Ti, Al, Mg, and Zr, and contains Ti, Al, Mg, and Zr in a total amount of 0.001 to 0.450 mass%.
7. The fillet welding method according to claim 6, characterized in that the Si content of the welding wire is 0.50 mass% or less with respect to the total mass of the welding wire, and the value of C+Si / 24+Mn / 6+Ni / 40+Cr / 5+Mo / 4+V / 4+Cu / 13 is 0.35 to 1.
40.
8. The fillet welding method according to claim 7, characterized in that the welding wire contains, relative to a total mass of the welding wire, Ti: 0.030 to 0.250 mass % and Al: 0.001 to 0.300 mass %, and the Ti / Al ratio is 0.3 to 20.
9. A fillet welding method according to claim 6, characterized in that: the feed speed during reverse feed when the wire position phase is 270 deg is 50 m / min or more; and the value of the formula (Ti + Al) / (Ti + Al + Mg + Zr) obtained by the contents of Ti, Al, Mg and Zr contained in the welding wire is 0.5 or more.
10. A feed control method for a fillet welding method, which alternately switches the feed speed between a forward feed period and a reverse feed period, wherein, when a wire position phase based on the position of the welding wire at the time of switching from the reverse feed period to the forward feed period is set to 0 deg, 90~180deg The average value of the welding current in 90~180deg_ave The set welding current value I set and the wire position phase is in a period T 180~270deg The average value of the welding current in 180~270deg_ave The set welding current value I set The feed control method according to claim 1, wherein the feed control amount is smaller than the feed control amount.
11. A power source that is applied to a fillet welding method and has a function of performing feed control to alternately switch the feed speed between a forward feed period and a reverse feed period, wherein in the feed control, when a wire position phase based on the position of the welding wire at the time of switching from the reverse feed period to the forward feed period is set to 0 deg, during a period T when the wire position phase is 90 deg to 180 deg, 90~180deg The average value of the welding current in 90~180deg_ave The set welding current value I set and the wire position phase is in a period T 180~270deg The average value of the welding current in 180~270deg_ave The set welding current value I set The power supply is characterized in that it is smaller than 12. A fillet welding system to which a feed control method is applied in which a feed speed is alternately switched between a forward feed period and a reverse feed period, wherein in the feed control method, when a wire position phase based on the position of the welding wire at the time of switching from the reverse feed period to the forward feed period is set to 0 deg, 90~180deg The average value of the welding current in 90~180deg_ave The set welding current value I set and the wire position phase is in a period T 180~270deg The average value of the welding current in 180~270deg_ave The set welding current value I set The fillet welding system according to claim 1, wherein the fillet welding distance is less than or equal to the distance between the fillet welding points.
Citation Information
Patent Citations
Gas shielded arc welding method for steel sheet
JP2001321946A
Wire for MAG welding of thin steel plate
JP2012170970A
Wiring sheet
JP2023059087A
Fillet welded joint, and gas shielded arc welding method
JP2012011429A
Heat exchanger and method for producing the same
JP2014163587A
Cited By
Arc welding method
WO2026211998A1
Arc welding method
WO2026211999A1
Arc welding method
WO2026212001A1