Anion-modified cellulose nanofiber-containing powder
The anion-modified cellulose nanofiber powder, with controlled particle size and moisture content, addresses the handling and workability issues of anion-modified cellulose nanofibers by enhancing their redispersibility and water absorption, resulting in improved handling and packaging efficiency.
Patent Information
- Application Number
- PCT/JP2024/005690
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-22
- Filing Date
- 2024-02-19
- Publication Date
- 2024-10-03
AI Technical Summary
Cellulose nanofibers with anionic groups require high water content for stability, leading to increased costs in packaging, storage, and transportation, and their properties like viscosity are not fully restored after drying, resulting in poor handling and workability issues.
Anion-modified cellulose nanofiber powder with specific particle size, moisture content, and dispersion degree, characterized by an average fiber diameter of 3-500 nm, moisture content of 20% or less, average particle diameter of 45 μm or more, and dispersion degree of less than 25%, which improves handling and workability.
The powder exhibits excellent handling and workability, with reduced scattering and improved redispersibility, allowing for efficient use and packaging without sealing defects, and demonstrates good initial water absorption.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Anion-modified cellulose nanofiber-containing powder
[0001] The present invention relates to a powder containing anionically modified cellulose nanofibers.
[0002] It is known that introducing anionic groups such as carboxyl groups or carboxymethyl groups into cellulose molecular chains and mechanically processing (defibrating) them can convert them into cellulose nanofibers with nanoscale fiber diameters. Because cellulose nanofibers are light, strong, and biodegradable, their applications in a variety of fields are being explored.
[0003] Generally, cellulose nanofibers into which anionic groups have been introduced are produced in a stably dispersed state in water, and are usually used in the form of a cellulose nanofiber dispersion of a predetermined concentration for various purposes, such as industrial materials or additives for foods and cosmetics. To maintain the cellulose nanofiber state stably, water is required that is several tens of times the amount of cellulose nanofiber, but this high water content increases the costs of packaging, storage, transportation, etc. of the cellulose nanofiber, so the cellulose nanofiber is dried to produce a dried product, and when ready to use, water is added to redisperse it and used as a redispersion.
[0004] When an aqueous dispersion of cellulose nanofibers is dried to form a dry solid, hydrogen bonds are formed between the fine cellulose fibers. Therefore, even if water is added to this dry solid to redisperse it, the viscosity and other properties do not return to the same level as before drying, and drying methods are being investigated (Patent Document 1, etc.).
[0005] International Publication No. 2019 / 189318
[0006] Dried cellulose nanofibers are manufactured by subjecting cellulose nanofibers dispersed in water (wet state) to processes such as drying, pulverization, classification, and recovery. The cellulose nanofiber powder manufactured in this way is redispersed by adding water on the user's side and used as a redispersion for various applications. However, depending on the properties of the powder, dusting can occur during the process, making it difficult to handle and work with.
[0007] Therefore, an object of the present invention is to provide a powder containing anion-modified cellulose nanofibers that is easy to handle and work with.
[0008] As a result of extensive research into achieving this object, the present inventors have found that it is extremely effective to prepare a powder having a specific particle size and degree of dispersion, and have thus completed the present invention.
[0009] The present invention provides the following: (1) A powder containing anion-modified cellulose nanofibers having an average fiber diameter of 3 nm to 500 nm, the powder having a moisture content of 20 mass% or less, an average particle diameter of 45 μm or more, and a degree of dispersion of less than 25%. (2) The anion-modified cellulose nanofiber-containing powder according to (1), having an angle of repose of 40 to 49°. (3) The anion-modified cellulose nanofiber-containing powder according to (1), having a collapse angle of 15 to 24°. (4) The anion-modified cellulose nanofiber-containing powder according to (1), having a difference angle of 20 to 25°.
[0010] According to the present invention, it is possible to provide a powder containing anion-modified cellulose nanofibers that is easy to handle and work with.
[0011] The present invention will be described in detail below. In the present invention, "to" includes the end values. That is, "X to Y" includes the values X and Y at both ends.
[0012] (Anion-modified cellulose nanofiber-containing powder) The present invention is a powder containing anion-modified cellulose nanofibers (anion-modified CNF) having an average fiber diameter of 3 nm to 500 nm, a moisture content of 20 mass% or less, an average particle diameter of 45 μm or more, and a degree of dispersion of less than 25%.
[0013] (Moisture content) From the viewpoint of storage stability, the anion-modified CNF-containing powder of the present invention has a moisture content of 20% by mass or less, preferably 0 to 15% by mass, more preferably 0 to 10% by mass, and even more preferably 0 to 9.5% by mass. If the moisture content is higher than the upper limit, there is a problem of increased risk of spoilage. The powder may be dried to a moisture content of 0% (absolutely dry).
[0014] (Average particle size) From the viewpoint of ease of handling, the anion-modified CNF-containing powder of the present invention has a lower limit of the average particle size of 45 μm or more, preferably 50 μm or more, more preferably 60 μm or more, and an upper limit of 300 μm or less, preferably 250 μm or less, more preferably 150 μm or less. If the average particle size is too small, there is a problem that the powder is easily scattered and difficult to handle. Here, the average particle size (D50) is the particle size that includes 50% of the particle size distribution based on volume, calculated from the minimum value. The particle size distribution can be measured using a laser diffraction / scattering particle size distribution analyzer.
[0015] (Dispersibility) From the viewpoint of handleability and workability, the anion-modified CNF-containing powder of the present invention has a dispersibility of less than 25%, preferably less than 20%. The lower limit is preferably 8% or more. When the dispersibility is within the above range, the amount of scattering during the process is small, resulting in excellent handleability and workability. When the dispersibility is too high, the amount of scattering during the process increases, resulting in poor handleability. Furthermore, poor workability occurs, such as poor sealing during packaging. On the other hand, when the dispersibility is too low, the powder has low flowability and is prone to clogging. The dispersibility can be measured using a powder property tester.
[0016] (Angle of repose) From the viewpoint of handleability and workability, the anion-modified CNF-containing powder of the present invention preferably has an angle of repose of 40 to 49°, more preferably 42 to 48°. If the angle of repose is too large, deposition is likely to occur in the hopper, and if it is too small, the powder will not stop flowing from the feeder outlet, etc. The angle of repose can be measured using a powder property tester.
[0017] (Collapse angle) From the viewpoint of handleability and workability, the collapse angle of the anion-modified CNF-containing powder of the present invention is preferably 15 to 24°, more preferably 17 to 22°. If the collapse angle is too large, a large impact is required to collapse the volume of the powder, and if it is too small, the powder will not stop flowing from the outlet of the feeder, etc. The collapse angle can be measured using a powder property tester.
[0018] (Difference angle) From the viewpoint of handling and workability, the anion-modified CNF-containing powder of the present invention preferably has a difference angle of 20 to 25°, more preferably 21 to 25°. If the difference angle is too large beyond the above range, the powder tends to be highly jet-like and easily scatters, while if it is too small, a large force is required to discharge the powder, making it difficult to control the discharge amount. The difference angle can be calculated from the angle of repose and angle of collapse measured using a powder property tester using the following formula: Difference angle = angle of repose - angle of collapse
[0019] (Anion-modified cellulose nanofiber) In the present invention, anion-modified cellulose nanofiber (anion-modified CNF) is a fine fiber having an average fiber diameter (fiber width) of 3 to 500 nm and an aspect ratio of 100 or more, and can be obtained by defibrating anion-modified cellulose.
[0020] (Cellulose Raw Material) Examples of cellulose raw materials for producing anion-modified cellulose include those derived from plant materials (e.g., wood, bamboo, hemp, jute, kenaf, agricultural waste, cloth, pulp (softwood unbleached kraft pulp (NUKP), softwood bleached kraft pulp (NBKP), hardwood unbleached kraft pulp (LUKP), hardwood bleached kraft pulp (LBKP), softwood unbleached sulfite pulp (NUSP), softwood bleached sulfite pulp (NBSP), thermomechanical pulp (TMP), recycled pulp, waste paper, etc.), animal materials (e.g., ascidians), algae, microorganisms (e.g., acetic acid bacteria (Acetobacter)), microbial products, etc., and any of these can be used. Cellulose fibers derived from plants or microorganisms are preferred, and plant-derived cellulose fibers are more preferred.
[0021] (Anionic Modification) In the present invention, anionic modification refers to the introduction of anionic groups into cellulose, specifically the introduction of anionic groups into the pyranose ring of cellulose by carboxylation (oxidation) or substitution reaction. In the present invention, the carboxylation (oxidation) reaction refers to a reaction in which the hydroxyl group of the pyranose ring is directly oxidized to a carboxy group. In addition, in the present invention, substitution reaction refers to a reaction in which anionic groups are introduced into the pyranose ring by a substitution reaction other than the carboxylation (oxidation).
[0022] Examples of anionic modification include carboxylation (oxidation), carboxymethylation, esterification, etc. Among these, carboxylation (oxidation), carboxymethylation, and phosphate esterification are more preferred, and carboxylation (oxidation) is particularly preferred.
[0023] (Carboxylation) In the present invention, when carboxylated (oxidized) cellulose is used as the anion-modified cellulose, the carboxylated cellulose (also called oxidized cellulose) can be obtained by carboxylating (oxidizing) the above-mentioned cellulose raw material by a known method. Although not particularly limited, during carboxylation, the amount of carboxy groups is preferably adjusted to 0.6 to 2.0 mmol / g, and more preferably 1.0 mmol / g to 2.0 mmol / g, relative to the bone dry mass of the anion-modified cellulose nanofiber.
[0024] An example of a carboxylation (oxidation) method is a method in which a cellulose raw material is oxidized in water using an oxidizing agent in the presence of an N-oxyl compound and a compound selected from the group consisting of bromides, iodides, or a mixture thereof. This oxidation reaction selectively oxidizes the primary hydroxyl group at the C6 position of the glucopyranose ring on the surface of the cellulose, leaving aldehyde groups and carboxy groups (—COOH) or carboxylate groups (—COO) on the surface. - The concentration of cellulose during the reaction is not particularly limited, but is preferably 5% by mass or less.
[0025] An N-oxyl compound refers to a compound capable of generating a nitroxy radical. Any compound can be used as the N-oxyl compound as long as it promotes the target oxidation reaction. Examples include 2,2,6,6-tetramethylpiperidine-1-oxyl radical (TEMPO) and its derivatives (e.g., 4-hydroxyTEMPO).
[0026] The amount of the N-oxyl compound used is not particularly limited, as long as it is a catalytic amount that can oxidize the raw material cellulose. For example, the amount is preferably 0.01 to 10 mmol, more preferably 0.01 to 1 mmol, and even more preferably 0.05 to 0.5 mmol, per 1 g of bone-dry cellulose. The amount is preferably about 0.1 to 4 mmol / L relative to the reaction system.
[0027] Bromides are compounds containing bromine, examples of which include alkali metal bromides that can dissociate and ionize in water. Iodides are compounds containing iodine, examples of which include alkali metal iodides. The amount of bromide or iodide used can be selected within a range that can promote the oxidation reaction. The total amount of bromide and iodide is, for example, preferably 0.1 to 100 mmol, more preferably 0.1 to 10 mmol, and even more preferably 0.5 to 5 mmol, per 1 g of bone-dry cellulose.
[0028] Known oxidizing agents can be used, such as halogens, hypohalous acids, halous acids, perhalogen acids or their salts, halogen oxides, and peroxides. Among these, sodium hypochlorite is preferred because it is inexpensive and has a low environmental impact. The appropriate amount of oxidizing agent used is, for example, preferably 0.5 to 500 mmol, more preferably 0.5 to 50 mmol, even more preferably 1 to 25 mmol, and most preferably 3 to 10 mmol, per 1 g of bone-dry cellulose. Furthermore, for example, 1 to 40 mol is preferred per 1 mol of the N-oxyl compound.
[0029] The cellulose oxidation process can proceed efficiently even under relatively mild conditions. Therefore, the reaction temperature is preferably 4 to 40°C, or may be room temperature, about 15 to 30°C. As the reaction proceeds, carboxyl groups are generated in the cellulose, resulting in a decrease in the pH of the reaction solution. To efficiently proceed with the oxidation reaction, it is preferable to add an alkaline solution such as an aqueous sodium hydroxide solution to maintain the pH of the reaction solution at about 8 to 12, preferably about 10 to 11. Water is preferred as the reaction medium because it is easy to handle and is less likely to cause side reactions.
[0030] The reaction time in the oxidation reaction can be appropriately set depending on the degree of progress of the oxidation, and is usually from 0.5 to 6 hours, for example, from about 0.5 to 4 hours.
[0031] The oxidation reaction may also be carried out in two stages. For example, the oxidized cellulose obtained by filtration after the completion of the first-stage reaction can be oxidized again under the same or different reaction conditions, thereby enabling efficient oxidation without reaction inhibition by sodium chloride produced as a by-product in the first-stage reaction.
[0032] Another example of a carboxylation (oxidation) method is a method in which cellulose raw materials are oxidized by contacting them with an ozone-containing gas. This oxidation reaction oxidizes at least the hydroxyl groups at positions 2 and 6 of the glucopyranose ring, and decomposes the cellulose chain. The ozone concentration in the ozone-containing gas is 50 to 250 g / m. 3 It is preferable that the density is 50 to 220 g / m 3 It is more preferable that the ozone addition amount relative to the cellulose raw material is preferably 0.1 to 30 parts by mass, and more preferably 5 to 30 parts by mass, based on 100 parts by mass of the solids content of the cellulose raw material. The ozone treatment temperature is preferably 0 to 50°C, and more preferably 20 to 50°C. The ozone treatment time is not particularly limited, but is approximately 1 to 360 minutes, and preferably approximately 30 to 360 minutes. When the ozone treatment conditions are within these ranges, excessive oxidation and decomposition of cellulose can be prevented, resulting in a good yield of oxidized cellulose. After the ozone treatment, a further oxidation treatment may be performed using an oxidizing agent. The oxidizing agent used in the further oxidation treatment is not particularly limited, but examples include chlorine-based compounds such as chlorine dioxide and sodium chlorite, oxygen, hydrogen peroxide, persulfuric acid, and peracetic acid. For example, the further oxidation treatment can be performed by dissolving these oxidizing agents in water or a polar organic solvent such as alcohol to prepare an oxidizing agent solution, and then immersing the cellulose raw material in the solution.
[0033] The amount of carboxy groups in the oxidized cellulose can be adjusted by controlling the reaction conditions, such as the amount of oxidizing agent added and the reaction time.
[0034] (Carboxymethylation) When carboxymethylated cellulose is used as the anion-modified cellulose in the present invention, the carboxymethylated cellulose may be obtained by carboxymethylating the above-mentioned cellulose raw material using a known method, or a commercially available product may be used. In either case, the carboxymethyl group substitution degree per anhydroglucose unit of the cellulose is preferably 0.01 to 0.50. An example of a method for producing such carboxymethylated cellulose is the following. Cellulose is used as the starting material, and 3 to 20 times by mass of water and / or a lower alcohol, specifically water, methanol, ethanol, N-propyl alcohol, isopropyl alcohol, N-butanol, isobutanol, tertiary butanol, etc., is used as a solvent, or a mixture of two or more of these. When a lower alcohol is mixed, the mixing ratio of the lower alcohol is 60 to 95% by mass. As the mercerizing agent, 0.5 to 20 times the molar amount of an alkali metal hydroxide, specifically sodium hydroxide or potassium hydroxide, is used per anhydroglucose residue of the starting material. The starting material, solvent, and mercerizing agent are mixed and subjected to mercerization treatment at a reaction temperature of 0 to 70°C, preferably 10 to 60°C, for a reaction time of 15 minutes to 8 hours, preferably 30 minutes to 7 hours. Thereafter, a carboxymethylating agent is added at 0.05 to 10.0 times the moles per glucose residue, and an etherification reaction is carried out at a reaction temperature of 30 to 90°C, preferably 40 to 80°C, for a reaction time of 30 minutes to 10 hours, preferably 1 hour to 4 hours.
[0035] (Crystallization degree of cellulose type I) The crystallinity of cellulose type I in carboxymethylated cellulose is preferably 50% or more, more preferably 60% or more. The crystallinity of cellulose type I in carboxymethylated cellulose can be controlled by the concentration of the mercerizing agent during production, the temperature during treatment, and the degree of carboxymethylation. Since high concentrations of alkali are used in mercerization and carboxymethylation, cellulose type I crystals are likely to be converted to type II crystals. However, the desired crystallinity can be maintained by, for example, adjusting the amount of alkali (mercerizing agent) used to adjust the degree of conversion. The upper limit of the crystallinity of cellulose type I is not particularly limited. In reality, it is thought that the upper limit is about 90%. The crystallinity of cellulose type I in carboxymethylated cellulose and the crystallinity of cellulose type I in carboxymethylated CNF obtained by defibrating it are usually the same.
[0036] In this specification, "carboxymethylated cellulose," a type of anion-modified cellulose used in preparing anion-modified CNF, refers to a material that maintains at least a portion of its fibrous shape when dispersed in water. Therefore, it is distinguished from carboxymethyl cellulose, a type of water-soluble polymer described below. When observing an aqueous dispersion of "carboxymethylated cellulose" with an electron microscope, fibrous material can be observed. On the other hand, when observing an aqueous dispersion of carboxymethyl cellulose, a type of water-soluble polymer, no fibrous material is observed. Furthermore, when "carboxymethylated cellulose" is measured by X-ray diffraction, peaks of cellulose type I crystals can be observed, but cellulose type I crystals are not observed in the water-soluble polymer carboxymethyl cellulose.
[0037] (Esterification) In the present invention, when esterified cellulose is used as the anion-modified cellulose, the esterified cellulose can be obtained by a method of mixing a powder or an aqueous solution of phosphoric acid compound A with the above-mentioned cellulose raw material, or a method of adding an aqueous solution of phosphoric acid compound A to a slurry of the cellulose raw material.
[0038] Examples of the phosphoric acid compound A include phosphoric acid, polyphosphoric acid, phosphorous acid, hypophosphorous acid, phosphonic acid, polyphosphonic acid, and esters thereof. These may be in the form of a salt. Among these, compounds having a phosphoric acid group are preferred because they are low cost, easy to handle, and can introduce phosphoric acid groups into the cellulose of the pulp fibers to improve defibration efficiency. Examples of compounds having a phosphoric acid group include phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, sodium phosphite, potassium phosphite, sodium hypophosphite, potassium hypophosphite, sodium pyrophosphate, sodium metaphosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, tripotassium phosphate, potassium pyrophosphate, potassium metaphosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, ammonium pyrophosphate, and ammonium metaphosphate. These compounds can be used alone or in combination of two or more. Among these, phosphoric acid, sodium salts of phosphoric acid, potassium salts of phosphoric acid, and ammonium salts of phosphoric acid are more preferred from the viewpoints of high efficiency of introducing phosphoric acid groups, ease of defibration in the defibration step described below, and ease of industrial application. Sodium dihydrogen phosphate and disodium hydrogen phosphate are particularly preferred. In addition, it is preferable to use the phosphoric acid compound A as an aqueous solution, since this increases the uniformity of the reaction and the efficiency of introducing the phosphoric acid group. The pH of the aqueous solution of phosphoric acid compound A is preferably 7 or less, since this increases the efficiency of introducing the phosphoric acid group, but from the viewpoint of suppressing hydrolysis of the pulp fiber, a pH of 3 to 7 is preferred.
[0039] The following method can be mentioned as an example of a method for producing phosphated cellulose. A phosphoric acid compound A is added to a dispersion of a cellulose raw material having a solids concentration of 0.1 to 10% by mass while stirring, to introduce phosphate groups into the cellulose. When the cellulose raw material is taken as 100 parts by mass, the amount of phosphoric acid compound A added is preferably 0.2 to 500 parts by mass, and more preferably 1 to 400 parts by mass, in terms of the amount of phosphorus element. If the proportion of phosphoric acid compound A is equal to or greater than the lower limit, the yield of fine cellulose fibers can be further improved. However, if the proportion exceeds the upper limit, the effect of improving the yield reaches a plateau, which is not preferable from a cost perspective.
[0040] In this case, in addition to the cellulose raw material and phosphoric acid compound A, a powder or aqueous solution of compound B may be mixed. Compound B is not particularly limited, but a basic nitrogen-containing compound is preferred. "Basic" here is defined as an aqueous solution exhibiting a pink to red color in the presence of a phenolphthalein indicator, or a pH of the aqueous solution greater than 7. The basic nitrogen-containing compound used in the present invention is not particularly limited as long as it achieves the effects of the present invention, but a compound having an amino group is preferred. Examples include, but are not limited to, urea, methylamine, ethylamine, trimethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine, pyridine, ethylenediamine, and hexamethylenediamine. Among these, urea is preferred due to its low cost and ease of handling. The amount of compound B added is preferably 2 to 1,000 parts by mass, more preferably 100 to 700 parts by mass, per 100 parts by mass of the solid content of the cellulose raw material. The reaction temperature is preferably 0 to 95°C, more preferably 30 to 90°C. The reaction time is not particularly limited, but is about 1 to 600 minutes, and more preferably 30 to 480 minutes. When the esterification reaction conditions are within these ranges, it is possible to prevent the cellulose from being excessively esterified and becoming more soluble, resulting in a good yield of phosphated cellulose. After dehydrating the resulting phosphated cellulose suspension, it is preferably heat-treated at 100 to 170°C in order to suppress cellulose hydrolysis. Furthermore, it is preferable to heat the suspension at 130°C or lower, preferably 110°C or lower, while it contains water, and then, after removing the water, to heat the suspension at 100 to 170°C.
[0041] The degree of phosphate substitution per glucose unit of the phosphate-esterified cellulose is preferably 0.001 to 0.40. Introducing phosphate group substituents into cellulose causes electrical repulsion between cellulose molecules. Therefore, cellulose with phosphate groups introduced therein can be easily defibrated. If the degree of phosphate substitution per glucose unit is less than 0.001, it cannot be sufficiently defibrated. On the other hand, if the degree of phosphate substitution per glucose unit is greater than 0.40, it may swell or dissolve, making it impossible to obtain fine cellulose fibers. To efficiently defibrate, the phosphate-esterified cellulose raw material obtained above is preferably washed by boiling and then washing with cold water. The modification by these esterifications is a modification by a substitution reaction. The degree of substitution in the esterified cellulose and the degree of substitution when the esterified cellulose is defibrated are usually the same.
[0042] Phosphate-esterified cellulose can be described as cellulose into which an anionic phosphorus oxoacid group or a substituent derived from a phosphorus oxoacid group (sometimes simply referred to as a "phosphorus oxoacid group") has been introduced. Here, the phosphorus oxoacid group is, for example, a divalent functional group obtained by removing a hydroxy group from phosphoric acid, specifically -PO 3 H 2 The substituent derived from the phosphorus oxo acid group includes salts of the phosphorus oxo acid group, phosphorus oxo acid ester groups, and other substituents. The substituent derived from the phosphorus oxo acid group may be contained in the cellulose nanofiber as a group in which a phosphate group is condensed (e.g., a pyrophosphate group). The phosphorus oxo acid group may also be, for example, a phosphorous acid group (phosphonic acid group), and the substituent derived from the phosphorus oxo acid group may be a salt of the phosphorous acid group, or the like.
[0043] The amount of phosphorus oxoacid groups, such as phosphate groups or phosphite groups, introduced into the phosphated cellulose is not particularly limited. During phosphate esterification, the amount of phosphorus oxoacid groups is preferably adjusted to 0.5 to 5 mmol / g, and more preferably 0.5 to 2.5 mmol / g, relative to the bone dry mass of the anion-modified cellulose nanofiber.
[0044] (Defibrillation) The device used to defibrate anionically modified cellulose is not particularly limited, and devices such as high-speed rotation, colloid mill, high-pressure, roll mill, and ultrasonic devices can be used. During defibration, it is preferable to apply a strong shear force to the aqueous dispersion of anionically modified cellulose. In particular, for efficient defibration, it is preferable to apply a pressure of 50 MPa or more to the aqueous dispersion and to use a wet high-pressure or ultra-high-pressure homogenizer capable of applying a strong shear force. The pressure is more preferably 100 MPa or more, and even more preferably 140 MPa or more. Furthermore, prior to the defibration and dispersion treatment using the high-pressure homogenizer, the aqueous dispersion may be subjected to a pretreatment, if necessary, using a known mixing, stirring, emulsifying, or dispersing device such as a high-speed shear mixer.
[0045] (Dispersant) From the viewpoint of improving redispersibility, the anion-modified cellulose nanofiber-containing powder of the present invention preferably contains a dispersant. Examples of dispersants include water-soluble polymers, surfactants, etc., and the use of a water-soluble polymer is preferred because it covers areas of low charge density on the surface of the anion-modified cellulose nanofiber, suppresses the formation of hydrogen bonds, and prevents aggregation of the cellulose nanofibers during drying.
[0046] (Water-Soluble Polymer) In the present invention, examples of water-soluble polymers include cellulose derivatives (carboxymethylcellulose, methylcellulose, hydroxypropylcellulose, ethylcellulose), xanthan gum, xyloglucan, dextrin, dextran, carrageenan, locust bean gum, alginic acid, alginates, pullulan, starch, potato starch, arrowroot flour, modified starch (cationized starch, phosphorylated starch, phosphate cross-linked starch, phosphate monoesterified phosphate cross-linked starch, hydroxypropyl starch, hydroxypropylated phosphate cross-linked starch, acetylated adipate cross-linked starch, acetylated phosphate cross-linked starch, acetylated oxidized starch, starch sodium octenylsuccinate, starch acetate, oxidized starch), corn starch, gum arabic, and gellan. Examples of the modified cellulose nanofibers include gum, polydextrose, pectin, chitin, water-soluble chitin, chitosan, casein, albumin, soy protein lysate, peptone, polyvinyl alcohol, polyacrylamide, sodium polyacrylate, polyvinylpyrrolidone, polyvinyl acetate, polyamino acids, polylactic acid, polymalic acid, polyglycerin, latex, rosin-based sizing agents, petroleum resin-based sizing agents, urea resin, melamine resin, epoxy resin, polyamide resin, polyamide-polyamine resin, polyethyleneimine, polyamine, vegetable gum, polyethylene oxide, hydrophilic crosslinked polymers, polyacrylates, starch-polyacrylic acid copolymers, tamarind gum, guar gum, and colloidal silica, as well as mixtures of one or more thereof. Among these, cellulose derivatives are preferred in terms of compatibility with anion-modified cellulose nanofibers, and carboxymethyl cellulose and its salts are particularly preferred. It is thought that water-soluble polymers such as carboxymethyl cellulose and its salts penetrate between the anion-modified cellulose nanofibers and increase the distance between the CNFs, thereby improving redispersibility.
[0047] When carboxymethyl cellulose or a salt thereof is used as the water-soluble polymer, it is preferable to use a carboxymethyl cellulose having a degree of carboxymethyl group substitution per anhydroglucose unit of 0.55 to 1.6, more preferably 0.55 to 1.1, and even more preferably 0.65 to 1.1. Furthermore, carboxymethyl cellulose with longer molecules (higher viscosity) is preferred because it is more effective at widening the distance between CNFs. The Brookfield viscosity of a 1% by mass aqueous solution of carboxymethyl cellulose at 25°C and 600 rpm is preferably 3 to 14,000 mPa s, more preferably 7 to 14,000 mPa s, and even more preferably 1,000 to 8,000 mPa s. Note that the "carboxymethyl cellulose or a salt thereof" referred to here as the water-soluble polymer is completely soluble in water, and is therefore distinguished from the carboxymethylated cellulose described above, the fibrous shape of which can be confirmed in water.
[0048] In the present invention, when a dispersant is contained in the anion-modified cellulose nanofiber-containing powder, the blending ratio of anion-modified CNF (bone dry solids) to dispersant is preferably 2:8 to 8:2, and more preferably 5:5 to 7:3, from the viewpoint of obtaining an improved effect on redispersibility. If the blending ratio of the dispersant is too much higher than the upper limit, problems such as reduced viscosity characteristics such as thixotropy, which are characteristic of anion-modified CNF, and reduced dispersion stability may occur. If the blending ratio of the dispersant is too much lower than the lower limit, sufficient redispersibility cannot be obtained.
[0049] (Method for producing powder) The method for producing the anion-modified CNF-containing powder of the present invention is not particularly limited. For example, there is a method in which an aqueous suspension containing anion-modified CNF and a dispersant blended as necessary is dehydrated and dried to obtain a dry solid, which is then pulverized using a pulverizer or the like, and the pulverized product is classified as necessary and recovered to obtain a powder; and a method in which the aqueous suspension is spray-dried to simultaneously dehydrate, dry, and powderize the resulting product, and the pulverized product is classified as necessary and recovered to obtain a powder.
[0050] Methods for dehydrating and drying aqueous suspensions containing anion-modified CNF may be conventionally known, such as spray drying, freeze drying, squeezing, air drying, hot air drying, and vacuum drying. Specific examples of drying apparatuses that can be used include the following: continuous tunnel dryers, band dryers, vertical dryers, vertical turbo dryers, multi-stage disk dryers, through-flow dryers, rotary dryers, flash dryers, spray dryer dryers, spray dryers, cylindrical dryers, drum dryers, reduced-pressure belt dryers, screw conveyor dryers, rotary dryers with heating tubes, vibration transport dryers, fluidized bed dryers, etc.; batch-type box dryers, through-flow dryers, vacuum box dryers, agitator dryers, shelf dryers, freeze dryers, etc., can be used alone or in combination of two or more. Among these, drum dryers and belt dryers are preferred, and from the viewpoint of energy efficiency, drum dryers, which directly and uniformly supply heat energy to the material to be dried, are even more preferred.
[0051] The method for pulverizing the anion-modified CNF-containing dry solid to obtain a pulverized product is not particularly limited. For example, the pulverized product can be obtained by pulverizing the anion-modified CNF-containing dry solid with a pulverizer. Examples of pulverizers include cutting mills: mesh mill (manufactured by HORAI Co., Ltd.), Atoms (manufactured by Yamamoto Hyakuma Manufacturing Co., Ltd.), knife mill (manufactured by Parman Co., Ltd.), cutter mill (manufactured by Tokyo Atomizer Manufacturing Co., Ltd.), CS cutter (manufactured by Mitsui Mining Co., Ltd.), rotary cutter mill (manufactured by Nara Machinery Manufacturing Co., Ltd.), turbo cutter (manufactured by Freund Corporation), pulp crusher (manufactured by Zuiko Co., Ltd.), shredder (manufactured by Kobe Steel Pantech Co., Ltd.), hammer mills: jaw crusher (manufactured by Makino Corporation), etc. (manufactured by Makino Sangyo Co., Ltd.), hammer crusher (manufactured by Makino Sangyo Co., Ltd.), impact mill: Pulverizer (manufactured by Hosokawa Micron Corporation), Fine Impact Mill (manufactured by Hosokawa Micron Corporation), Super Micron Mill (manufactured by Hosokawa Micron Corporation), Inomizer (manufactured by Hosokawa Micron Corporation), Fine Mill (manufactured by Nippon Pneumatic Mfg. Co., Ltd.), CUM-type centrifugal mill (manufactured by Mitsui Mining Co., Ltd.), Exceed Mill (manufactured by Makino Sangyo Co., Ltd.), Ultraplex (manufactured by Makino Sangyo Co., Ltd.), Contraplex (manufactured by Makino Sangyo Co., Ltd.) Co., Ltd.), Coroplex (Makino Sangyo Co., Ltd.), Sample Mill (Seishin Co., Ltd.), Bantam Mill (Seishin Co., Ltd.), Atomizer (Seishin Co., Ltd.), Tornado Mill (Nikkiso Co., Ltd.), Nea Mill (Dalton Co., Ltd.), HT-type fine grinder (Horai Co., Ltd.), Free Grinding Mill (Nara Machinery Manufacturing Co., Ltd.), New Cosmomizer (Nara Machinery Manufacturing Co., Ltd.), Turbo Mill (Freund Corporation), Gather Mill (Nishimura Machinery Manufacturing Co., Ltd.), Super Powder Mill (Nishimura Machinery Manufacturing Co., Ltd.), Blade Mill (Nisshin Engineering Inc.), Super Rotor (Nisshin Engineering Inc.), Npa Crusher (Sansho Industry Co., Ltd.), Wheeley Grinding Mill (Sanki Manufacturing Co., Ltd.), Pulp Grinding Mill (Zuiko Co., Ltd.), Jacobson Fine Grinding Mill (Kobe Pantech Co., Ltd.), Universal Mill (Tokuju Kogyosho Co., Ltd.), Atomizer (Tokyo Atomizer Manufacturing Co., Ltd.), Mill Star Dam (Tokyo Atomizer Manufacturing Co., Ltd.),Airflow type mills: Stream Mill (manufactured by Nippon Coke Engineering Co., Ltd.), CGS type jet mill (manufactured by Mitsui Mining Co., Ltd.), Micron Jet (manufactured by Hosokawa Micron Corporation), Counter Jet Mill (manufactured by Hosokawa Micron Corporation), Cross Jet Mill (manufactured by Kurimoto Iron Works Co., Ltd.), Supersonic Jet Mill (manufactured by Nippon Pneumatic Mfg. Co., Ltd.), Current Jet (manufactured by Nisshin Engineering Inc.), Jet Mill (manufactured by Sansho Industry Co., Ltd.), Ebara Jet Micronizer (manufactured by Ebara Corporation), Ebara Triad Jet (manufactured by Ebara Corporation), Selenium Mirror (manufactured by Masuko Sangyo Co., Ltd.), New Micro Sic Examples include matte (manufactured by Masuno Manufacturing Co., Ltd.), Kryptron (manufactured by Kawasaki Heavy Industries, Ltd.), disc mills: vibrating disc mills (manufactured by Retsch), centri-cutter (manufactured by Nippon Coke Engineering Co., Ltd.), turbo disc mills (manufactured by Freund Turbo Corporation), mortar-type high-speed crushers (manufactured by Makino Sangyo Co., Ltd.), vertical roller mills: vertical roller mills (manufactured by Chinon Co., Ltd.), vertical roller mills (manufactured by Schaeffler Japan Co., Ltd.), roller mills (manufactured by Kotobuki Giken Kogyo Co., Ltd.), VX mills (manufactured by Kurimoto Iron Works Co., Ltd.), KVM-type vertical mills (manufactured by Earth Technica Co., Ltd.), and IS mills (manufactured by IHI Plant Engineering Co., Ltd.). The processing conditions for these mills cannot be uniformly determined because the principles of milling differ. However, for example, a method can be used in which processing conditions that affect the milling process, such as the screen diameter at the mill outlet and the rotation speed of the classification rotor, are adjusted, a calibration curve showing the relationship between processing conditions and particle size is created, and appropriate processing conditions are determined based on the calibration curve to achieve the desired average particle size.
[0052] The pulverized material containing anion-modified CNF may be classified as needed. When classification is performed, it can be performed using a classifier attached to or attached to a pulverizer.
[0053] The type of device used to collect the pulverized material containing anion-modified CNF and the granulated material obtained by spray drying is not particularly limited. Examples of the collection device include a cyclone and a bag filter.
[0054] The anion-modified CNF-containing powder may be classified after collection.
[0055] The anion-modified CNF-containing powder of the present invention has an average particle size of 45 μm or more and a degree of dispersion of less than 25%, so that it is less prone to dusting during processing, is easy to handle, and is easy to work with when performing redispersion work, etc. In addition, the anion-modified CNF-containing powder of the present invention has excellent initial water absorption.
[0056] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0057] (Average Fiber Diameter and Average Fiber Length of CNF) The powder was redispersed in water to prepare a suspension, which was then diluted. 200 randomly selected fibers were analyzed using an atomic force microscope (AFM) and the average was calculated. The aspect ratio was calculated using the following formula: Aspect ratio = Average fiber length / Average fiber diameter
[0058] (Carboxy group amount) The carboxy group amount was calculated using the following formula: 60 mL of a 0.5 mass% slurry (aqueous dispersion) of carboxylated cellulose was prepared, 0.1 M aqueous hydrochloric acid was added to adjust the pH to 2.5, 0.05 N aqueous sodium hydroxide was added dropwise, and the electrical conductivity was measured until the pH reached 11. The amount of carboxy groups was calculated using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of a weak acid, where the change in electrical conductivity was gradual: Carboxy group amount [mmol / g carboxylated cellulose] = a [mL] × 0.05 / mass of carboxylated cellulose [g].
[0059] (Degree of Carboxymethyl Substitution) The degree of carboxymethyl substitution was measured by the following method. Approximately 2.0 g of sample was weighed out and placed in a 300 mL Erlenmeyer flask with a stopper. 100 mL of a solution of 1000 mL of nitric acid methanol and 100 mL of special-grade concentrated nitric acid was added, and the mixture was shaken for 3 hours to convert the carboxymethylated cellulose CNF salt (CMC) into H-CMC (hydrogen-type carboxymethylated CNF). 1.5 to 2.0 g of the bone-dried H-CMC was weighed out and placed in a 300 mL Erlenmeyer flask with a stopper. The H-CMC was moistened with 15 mL of 80% methanol, 100 mL of 0.1 N NaOH was added, and the mixture was shaken at room temperature for 3 hours. Phenolphthalein was used as an indicator, and the 0.1 N-H 2 SO 4The excess NaOH was back-titrated with 0.05% NaOH, and the degree of carboxymethyl substitution (DS value) was calculated by the following formula: A = [(100 × F' - 0.1N - H 2 SO 4 (mL) × F × 0.1] / (bone dry mass (g) of H-CMC) Degree of carboxymethyl substitution = 0.162 × A / (1 - 0.058 × A) F': factor of 0.1N-NaOH F: factor of 0.1N-H 2 SO 4 Factor
[0060] The degree of carboxymethyl substitution in the CNF of carboxymethyl cellulose is usually the same as the degree of carboxymethyl substitution in the carboxymethyl cellulose before being converted into CNF.
[0061] (Crystallization degree of cellulose type I) The crystallinity of cellulose type I of carboxymethylated cellulose nanofibers was measured by the following method. A sample was placed in a glass cell and measured using an X-ray diffraction measurement device (LabX XRD-6000, manufactured by Shimadzu Corporation). The crystallinity was calculated using the method of Segal et al., and was calculated using the diffraction intensity of the 002 plane at 2θ = 22.6° and the diffraction intensity of the amorphous portion at 2θ = 18.5°, using the diffraction intensity from 2θ = 10° to 50° in the X-ray diffraction pattern as the baseline, using the following formula:
[0062] Xc = (I002c - Ia) / I002c × 100 Xc = Crystallinity (%) of cellulose type I I002c: 2θ = 22.6°, diffraction intensity of 002 plane Ia: 2θ = 18.5°, diffraction intensity of amorphous part
[0063] The proportion of type I crystals in carboxymethylated cellulose nanofibers is usually the same as that in the carboxymethyl cellulose before it is made into CNF.
[0064] (Amount of phosphorus oxoacid groups) The amount of phosphorus oxoacid groups (amount of phosphate groups or phosphite groups) was measured by the following method. First, ion-exchanged water was added to the target CNF to prepare a slurry with a solids concentration of 0.2 mass%. The obtained slurry was treated with an ion-exchange resin, and then titrated with an alkali to measure the amount of phosphorus oxoacid groups.
[0065] Treatment with ion exchange resin was carried out by adding 1 / 10 by volume of a strongly acidic ion exchange resin (Amberjet 1024; Organo Corporation, conditioned) to the above CNF-containing slurry, shaking for 1 hour, and then pouring it onto a mesh with 90 μm openings to separate the resin and slurry.
[0066] In addition, the alkali titration was performed by adding 10 μL of 0.1 N sodium hydroxide solution to the CNF-containing slurry after ion exchange resin treatment every 5 seconds while measuring the change in the pH value of the slurry. Nitrogen gas was bubbled into the slurry 15 minutes before the start of the titration. In this neutralization titration, two maximum points of increment (differential value of pH with respect to the amount of alkali added) were observed on the curve plotting the measured pH against the amount of alkali added. Of these, the maximum point of increment obtained first after starting the addition of alkali is called the first endpoint, and the maximum point of increment obtained next is called the second endpoint. The amount of alkali required from the start of the titration to the first endpoint is equal to the amount of first dissociated acid in the slurry used for titration. Furthermore, the amount of alkali required from the start of the titration to the second endpoint is equal to the total amount of dissociated acid in the slurry used for titration. The amount of alkali (mmol) required from the start of titration to the first endpoint was divided by the solid content (g) in the slurry to be titrated, and the value was taken as the amount of phosphorus oxo acid groups (mmol / g).
[0067] (Measurement of Moisture Content) The moisture content of the powder was calculated as the difference between the mass of the obtained powder after drying at 105° C. for 3 hours or more (bone dry mass) and the mass before drying.
[0068] (Average Particle Diameter) The average particle diameter (D50) of the powders used in the examples and comparative examples was determined from the particle diameter distribution based on the volume average particle diameter.
[0069] The particle size distribution was measured using a laser diffraction / scattering particle size distribution analyzer (Mastersizer 3000, manufactured by Spectris Co., Ltd.) under the condition of a particle refractive index of 1.5. The measurement was performed by directly putting the dry powder sample into the device.
[0070] (Dispersibility) The dispersibility of the powders obtained in the examples and comparative examples was measured using a powder tester (Powder Tester PT-X, manufactured by Hosokawa Micron Corporation). Specifically, when 10 g of a sample was placed in the dispersion unit of the PT-X and dropped, the dispersibility was calculated from the amount of powder that fell onto a watch glass using the following formula: Dispersibility (%) = (10 (g) - amount of powder that fell onto the watch glass (g)) / 10 (g).
[0071] (Angle of Repose) The angle of repose of the powders obtained in the Examples and Comparative Examples was determined as the value of the angle of repose (angle of elevation) when the powder was dropped and deposited from the hole of a funnel onto a horizontal plate of a certain area until it took on a certain shape using a powder property testing device (Powder Tester PT-X model, manufactured by Hosokawa Micron Corporation) to form conical granules.
[0072] (Collapse Angle) The collapse angle of the powders obtained in the Examples and Comparative Examples was measured using a powder property tester (Powder Tester PT-X, manufactured by Hosokawa Micron Corporation) by dropping and depositing the powder from the holes of a funnel onto a horizontal plate of a certain area until a certain shape was achieved, forming conical granules. Next, a weight of a certain weight placed on the same base as the horizontal plate was dropped to apply a certain impact to the powder, and after some of the powder naturally flowed and fell off the horizontal plate, the angle of elevation of the remaining conical granules from a point on the outer periphery of the base to the apex of the cone was taken as the collapse angle.
[0073] (Difference Angle) Using the angle of repose and angle of collapse measured above, the difference angle was calculated according to the following formula: Difference Angle = Angle of Repose - Angle of Collapse
[0074] (Workability during packaging) The workability during packaging was checked for the powders obtained in the Examples and Comparative Examples. The sample powder was placed in a polyethylene bag to fill 70% of the bag and sealed, and the adhesive seal area was visually inspected and evaluated according to the following criteria. A: Little powder scattering, no powder adhering to the adhesive seal area, and almost no deterioration in sealing ability B: Some powder scattering and adhesion to the adhesive seal area, resulting in a slight deterioration in sealing ability C: Much powder scattering, much powder adhering to the adhesive seal area, resulting in a significant deterioration in sealing ability
[0075] (Evaluation of Initial Water Absorbency) The water absorbency (initial water absorbency) of the powders obtained in the Examples and Comparative Examples was evaluated in a short time. 0.1 g of a specimen was placed flat on a rectangular glass plate. 1 mL of pure water was then dropped evenly onto the specimen using a dropper, and the water absorbency immediately afterwards was evaluated according to the following criteria: A: Immediately after dropping, water absorption into the powder occurred, and a gel layer was formed all over. B: Immediately after dropping, water absorption into the powder was slow, and a gel layer was formed in some areas, but the remaining pure water separated into droplets on the powder. C: Immediately after dropping, water absorption into the powder was slow, and most of the pure water separated into droplets on the powder.
[0076] (Production Example 1) (Production of Carboxylated CNF1) 500 g (bone dry) of bleached, unbeaten kraft pulp derived from softwood (brightness 85%) was added to 20 L of an aqueous solution containing TEMPO (Sigma-Aldrich) (0.025 mmol / g relative to the cellulose raw material) and sodium bromide (1 mmol / g relative to the cellulose raw material), and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system to a concentration of 5.2 mmol / g, initiating the oxidation reaction. During the reaction, the pH of the system decreased, but 3 M aqueous sodium hydroxide was gradually added to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. The reaction mixture was filtered through a glass filter to separate the pulp, which was then thoroughly washed with water to obtain oxidized pulp (carboxylated cellulose). The pulp yield at this time was 90%, the time required for the oxidation reaction was 100 minutes, and the amount of carboxyl groups was 1.4 mmol / g.
[0077] The oxidized pulp obtained in the above process was adjusted to 1.0% (w / v) with water and treated three times with an ultra-high pressure homogenizer (20°C, 150 MPa) to obtain a dispersion of carboxylated CNF1. The obtained fibers had an average fiber diameter of 4 nm and an aspect ratio of 220.
[0078] (Production Example 2) (Production of Carboxylated CNF2) 500 g (bone-dry) of bleached softwood-derived dissolving kraft pulp (DKP manufactured by Buckeye) was added to 50 L of an aqueous solution containing 7.8 g (0.05 mol) of TEMPO (Sigma-Aldrich) and 75.5 g (0.74 mol) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. 1.6 L of a 2 M aqueous sodium hypochlorite solution was added to the reaction system, and then the oxidation reaction was initiated (oxidation treatment). During the reaction, the pH in the system decreased, but was adjusted to pH 10 by successive addition of a 3 M aqueous sodium hydroxide solution. After reacting for 2 hours, the mixture was filtered through a glass filter and thoroughly washed with water to obtain carboxylated cellulose. A 5.0% (w / v) carboxylated cellulose slurry was prepared using water. Hydrogen peroxide was added to the slurry at 2% (w / w) relative to the carboxylated cellulose, and the pH was adjusted to 11.3 with 3M sodium hydroxide. The slurry was then hydrolyzed at 80°C for 2 hours. The resulting slurry was adjusted to 5.0% (w / v) with water and subjected to five cycles in an ultra-high-pressure homogenizer (20°C, 140 MPa) to obtain a dispersion of carboxylated CNF2. The resulting carboxylated CNF2 had a carboxyl group content of 1.7 mmol / g, an average fiber diameter of 3 nm, and an aspect ratio of 117.
[0079] (Production Example 3) (Production of Carboxymethylated CNF) 500 parts of isopropanol (IPA) and a solution of 15 parts of sodium hydroxide dissolved in 200 parts of water were added to a 5 L twin-screw kneader adjusted to 100 rpm, and 100 parts of hardwood pulp (LBKP, manufactured by Nippon Paper Industries Co., Ltd.) was added (based on the dry mass of the pulp dried at 100°C for 60 minutes). The mixture was stirred and mixed at 30°C for 90 minutes to prepare mercerized cellulose. 19 parts of sodium monochloroacetate dissolved in 20 parts of 90% IPA was added with further stirring, and the mixture was stirred at 30°C for 30 minutes. After stirring, the mixture was heated to 70°C and subjected to a carboxymethylation reaction at 70°C for 90 minutes. After the reaction was completed, the mixture was neutralized, washed with 65% aqueous methanol, deliquored, dried, and pulverized to obtain a sodium salt of carboxymethylated cellulose with a carboxymethyl substitution degree of 0.18 and a crystallinity of cellulose type I of 64%. The methods for measuring the degree of carboxymethyl substitution and the crystallinity of cellulose type I are as described above.
[0080] The sodium salt of carboxymethyl cellulose obtained in the above process was adjusted to 1.0% (w / v) with water and treated three times with an ultra-high pressure homogenizer (20°C, 150 MPa) to obtain a dispersion of carboxymethylated CNF. The obtained carboxymethylated CNF had an average fiber diameter of 8 nm and an aspect ratio of 60.
[0081] (Production Example 4) (Production of phosphorylated CNF) Bleached unbeaten kraft pulp derived from coniferous trees (brightness 85%, basis weight 245 g / m 2 A phosphorus oxo-oxidation treatment was carried out on the raw pulp (sheet form) as follows. First, a mixed aqueous solution of ammonium dihydrogen phosphate and urea was added to 100 parts by mass (bone dry) of the raw pulp to adjust the total weight to 45 parts by mass of ammonium dihydrogen phosphate, 120 parts by mass of urea, and 150 parts by mass of water, to obtain a chemical-impregnated pulp. The resulting chemical-impregnated pulp was then heated in a hot air dryer at 165°C for 250 seconds to introduce phosphate groups into the cellulose in the pulp, thereby obtaining a phosphorylated pulp. 100 g of the resulting phosphorylated pulp (bone dry) was mixed with 10 L of ion-exchanged water to obtain a pulp dispersion. The pulp was stirred to uniformly disperse, and then repeatedly filtered and dehydrated for washing. The washing endpoint was reached when the electrical conductivity of the filtrate reached 100 μS / cm or less. The washed phosphorylated pulp was then diluted with 10 L of ion-exchanged water, and a 1 N aqueous sodium hydroxide solution was added little by little while stirring to obtain a phosphorylated pulp slurry with a pH of 12 to 13. The phosphorylated pulp slurry was dewatered and washed to obtain neutralized phosphorylated pulp.
[0082] The obtained phosphorylated pulp was subjected to infrared absorption spectroscopy using FT-IR. -1 The absorption due to P=O of the phosphate group was observed around the 2θ=14° to 17° angle and the 2θ=22° to 23° angle.
[0083] The phosphorylated pulp obtained in the above process was adjusted to 1.0% (w / v) with water and treated three times with an ultra-high pressure homogenizer (20°C, 150 MPa) to obtain a phosphorylated CNF dispersion. The obtained fibers had an average fiber diameter of 4 nm and an aspect ratio of 200.
[0084] X-ray diffraction confirmed that the obtained CNF maintained cellulose type I crystal structure. The amount of phosphate groups (amount of first dissociated acid) was 1.45 mmol / g. The total amount of dissociated acid was 2.45 mmol / g.
[0085] Example 1 (Production of Dried Product) Carboxylated CNF1 (carboxyl group amount: 1.4 mmol / g, average fiber diameter: 4 nm, aspect ratio: 220) obtained in Production Example 1 was used as anion-modified CNF. Carboxymethyl cellulose (product name: F350HC-4, viscosity (1%, 25°C) approximately 3000 mPa·s, degree of carboxymethyl substitution approximately 0.9) was added to a 0.7% by mass aqueous suspension of carboxylated CNF1 in an amount of 40% by mass relative to the anion-modified CNF (i.e., so that the solid content of carboxymethyl cellulose was 40 parts by mass per 100 parts by mass of the solid content of the anion-modified CNF), and the mixture was stirred for 60 minutes with a TK Homomixer (12,000 rpm) to prepare an aqueous dispersion containing anion-modified CNF. The pH of this dispersion was approximately 7 to 8. This aqueous dispersion was added with 5% aqueous sodium hydroxide solution to adjust the pH to 9, and then coated on the drum surface of a drum dryer D0405 (manufactured by Katsuragi Kogyo Co., Ltd.) to form a thin film with a thickness of approximately 100 to 200 μm.The film was dried at a drum surface temperature of 80°C, an internal pressure of the dryer of 2 kPa, and a drum rotation speed of 2 rpm, yielding a dried body containing anion-modified CNF with a moisture content of 5% by mass.
[0086] (Production of powder) The dried body containing CNF obtained as described above was pulverized using a hammer mill (Hammer Mill TAP-3, manufactured by Tokyo Atomizer Co., Ltd.) to obtain a pulverized product. The particle size of the obtained pulverized product was adjusted by adjusting the screen diameter at the outlet of the pulverizer. The pulverized product after particle size adjustment was recovered using a cyclone to obtain a powder containing anion-modified CNF. The moisture content of the obtained powder was 8% by mass.
[0087] (Example 2) A pulverized product was obtained in the same manner as in Example 1, except that the dried product containing CNF obtained in Example 1 was pulverized using an impact mill (Pulverizer, manufactured by Hosokawa Micron Corporation) instead of a hammer mill. The particle size of the obtained pulverized product was adjusted by adjusting the rotation speed of the classification rotor. The pulverized product after particle size adjustment was recovered using a cyclone, and a powder containing anion-modified CNF was obtained. The moisture content of the obtained powder was 10% by mass.
[0088] (Example 3) A pulverized product was obtained in the same manner as in Example 1, except that the dried body containing CNF obtained in Example 1 was pulverized using a disk mill (Centri-cutter, manufactured by Nippon Coke Engineering Co., Ltd.) instead of a hammer mill. The pulverized product obtained was collected using a cyclone to obtain an anion-modified CNF-containing powder. The moisture content of the obtained powder was 9.7% by mass.
[0089] (Example 4) A pulverized product was obtained in the same manner as in Example 1, except that the dried body containing CNF obtained in Example 1 was pulverized using an impact mill (Atomizer, manufactured by Tokyo Atomizer Mfg. Co., Ltd.) instead of a hammer mill. The particle size of the pulverized product obtained was adjusted and collected in the same manner as in Example 1, yielding a powder containing anion-modified CNF. The moisture content of the obtained powder was 9.3% by mass.
[0090] (Example 5) A pulverized product was obtained in the same manner as in Example 1, except that the dried product containing CNF obtained in Example 1 was pulverized using a Turbo Mill (manufactured by Freund Corporation) as the pulverizer. The particle size of the obtained pulverized product was adjusted by adjusting the gap between the rotor and the liner. The pulverized product after particle size adjustment was collected using a cyclone, and a powder containing anion-modified CNF was obtained. The moisture content of the obtained powder was 7.8% by mass.
[0091] Example 6 Production of Dried Product Carboxymethylated CNF (degree of carboxymethyl substitution: 0.18, average fiber diameter: 8 nm, aspect ratio: 60) obtained in Production Example 3 was used as anion-modified CNF. Carboxymethyl cellulose (manufactured by Nippon Paper Industries Co., Ltd., product name: F350HC-4, viscosity (1% by mass, 25°C, 60 rpm) approximately 3000 mPa s, degree of carboxymethyl substitution approximately 0.90) was added to a 0.7% by mass aqueous suspension of carboxymethylated CNF in an amount of 40% by mass relative to the carboxymethylated CNF (i.e., so that the solid content of carboxymethyl cellulose was 40 parts by mass per 100 parts by mass of the solid content of carboxymethylated CNF), and the mixture was stirred for 60 minutes with a TK Homomixer (12,000 rpm) to prepare an aqueous dispersion containing carboxymethylated CNF as anion-modified CNF. To this aqueous dispersion, 5% by mass of aqueous sodium hydroxide solution was added to adjust the pH to 9, and then the dispersion was applied to the drum surface of a drum dryer D0405 (manufactured by Katsuragi Kogyo Co., Ltd.) and dried for 1 minute at 140° C. The resulting dried product was scraped off to obtain a dried body containing anion-modified CNF.
[0092] (Production of powder) The dried body containing CNF obtained as described above was pulverized in the same manner as in Example 2 to obtain a pulverized product. The particle size of the obtained pulverized product was adjusted by adjusting the rotation speed of the classifying rotor. The pulverized product after particle size adjustment was collected using a cyclone to obtain a powder containing anion-modified CNF. The moisture content of the obtained powder was 8.2% by mass.
[0093] (Example 7) A dried body containing anion-modified CNF was produced in the same manner as in Example 2, except that the phosphorylated CNF obtained in Production Example 4 (phosphate group amount: 1.45 mmol / g, average fiber diameter: 4 nm, aspect ratio: 200) was used as the anion-modified CNF. This dried body was pulverized in the same manner as in Example 2 to obtain a pulverized product. The particle size of the obtained pulverized product was adjusted by adjusting the rotation speed of the classifying rotor. The pulverized product after particle size adjustment was recovered using a cyclone to obtain a powder containing phosphorylated CNF. The moisture content of the obtained powder was 8.5% by mass.
[0094] (Comparative Example 1) (Production of dried body) A 5.0 mass% aqueous suspension (pH 7.5) of carboxylated CNF2 (carboxy group amount: 1.7 mmol / g, average fiber diameter: 3 nm, aspect ratio: 117) obtained in Production Example 2 was prepared as anion-modified CNF, and dried using a two-fluid nozzle spray dryer (Okawahara Chemical Engineering Co., Ltd., OUDT-25) at an inlet temperature of 160°C, an outlet temperature of 70°C, a drying air flow rate of 80 kg / h, and a liquid feed rate of 54.2 kg / h to obtain a powdery CNF dried body.
[0095] The resulting dried product was collected using a cyclone to obtain anion-modified CNF powder, which had a moisture content of 4.4% by mass.
[0096]
[0097] As can be seen from Table 1, the powders containing anion-modified cellulose nanofibers with fiber diameters of 3 to 500 nm of Examples 1 to 7, which had a moisture content of 20% by mass or less, an average particle diameter of 45 μm or more, and a degree of dispersion of less than 25%, suppressed scattering during processing and exhibited excellent handleability. Furthermore, they also exhibited excellent workability during packaging. They also exhibited good initial water absorption. This indicates that, for example, when the powder is added to a tank filled with water and redispersed, the powder does not float to the water surface and is easily suspended in water, suggesting excellent dispersion and homogenization in water by stirring. On the other hand, the anion-modified cellulose nanofiber powder of Comparative Example 1, which had a small average particle diameter, had a degree of dispersion outside the above range, making it difficult to suppress scattering during processing and exhibiting poor handleability. Furthermore, they exhibited poor workability during packaging, raising concerns about poor sealing during packaging. Furthermore, the initial water absorption was slow, and the water and powder separated, resulting in poor compatibility. Typically, cellulose nanofiber powders are adjusted in various ways to ensure the redispersibility of the cellulose nanofibers when redispersed in a solvent. Therefore, the adhesive force between cellulose nanofiber powders is weaker than that of ordinary cellulose-based powders, which raises concerns that the powders may be more prone to scattering and have poorer workability than ordinary cellulose-based powders. The anion-modified cellulose nanofiber-containing powder of the present invention is the first to demonstrate that even cellulose nanofibers adjusted to have good redispersibility can be used to obtain a cellulose nanofiber powder with excellent workability and reduced scattering by adjusting the moisture content, average particle size, and dispersibility to an appropriate balance.
Claims
1. A powder containing anion-modified cellulose nanofibers having an average fiber diameter of 3 nm to 500 nm, a moisture content of 20 mass% or less, an average particle diameter of 45 μm or more, and a degree of dispersion of less than 25%.
2. The powder containing anion-modified cellulose nanofibers according to claim 1, having an angle of repose of 40 to 49°.
3. The powder containing anion-modified cellulose nanofibers according to claim 1, having a collapse angle of 15 to 24°.
4. The anionically modified cellulose nanofiber-containing powder according to claim 1, wherein the difference angle is 20 to 25°.
Citation Information
Patent Citations
Method for producing cellulose nanofiber dry solid
WO2019189318A1
Cellulose powder
JP2018016818A
Dried cellulose fiber and method for producing the same, and method for producing resin composite
JP2021169577A
Method for producing dried cellulose fiber and method for producing resin composite
JP2021169578A
Dried cellulose fiber and method for producing the same, and method for producing resin composite
JP2021169579A