Pressure-sensitive adhesive composition, pressure-sensitive adhesive sheet, pressure-sensitive adhesive sheet with release film, laminate for image display device, image display device, and pressure-sensitive adhesive sheet for organic el display device
The adhesive composition for image display devices, using a (meth)acrylic polymer and a specific photoinitiator, addresses the challenge of curing with visible light and minimizing photodecomposition, achieving effective bonding and durability for organic EL displays by utilizing 405 nm wavelength active energy rays.
Patent Information
- Application Number
- PCT/JP2024/006782
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-02-26
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional adhesive sheets for image display devices, particularly organic EL display devices, face issues with deterioration due to ultraviolet rays and require adhesives that can cure with visible light to avoid interference from ultraviolet-absorbing components, while also minimizing photodecomposition products and ensuring efficient curing sensitivity.
A pressure-sensitive adhesive composition comprising a (meth)acrylic polymer and a photoinitiator with a radically polymerizable functional group and a radical generating group, which absorbs and reacts with active energy rays of 405 nm wavelength, facilitating curing while minimizing photodecomposition products and improving cohesive force.
The adhesive composition effectively cures with long-wavelength active energy rays, reducing photodecomposition products and enhancing the adhesive's durability and adhesion properties for organic EL display devices, ensuring efficient bonding and stability.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Pressure-sensitive adhesive composition, pressure-sensitive adhesive sheet, pressure-sensitive adhesive sheet with release film, laminate for image display device, image display device, and pressure-sensitive adhesive sheet for organic EL display device
[0001] The present invention relates to a pressure-sensitive adhesive composition, and a pressure-sensitive adhesive sheet, a pressure-sensitive adhesive sheet with a release film, a laminate for an image display device, an image display device, and a pressure-sensitive adhesive sheet for an organic EL display device, which use the same. This application claims priority based on Japanese Patent Application No. 2023-049998, filed in Japan on March 27, 2023, the contents of which are incorporated herein by reference.
[0002] In recent years, in order to improve the visibility of image display devices, the gap between an image display panel such as a liquid crystal display (LCD), a plasma display (PDP) or an electroluminescence display (ELD) and an optical component such as a protective panel or a touch panel component arranged on the front side (viewing side) of the image display panel has been filled with a resin such as an adhesive or glue to suppress reflection of incident light and outgoing light from the displayed image at the air layer interface.
[0003] For example, Patent Document 1 discloses a method for manufacturing a component laminate for an image display device, which has a configuration in which an image display device component is laminated on at least one side of a transparent double-sided adhesive sheet, in which an adhesive sheet that has been primarily crosslinked by ultraviolet light is attached to the image display device component, and then the adhesive sheet is irradiated with ultraviolet light through the image display device component to cause secondary curing.
[0004] Furthermore, Patent Document 2 discloses a pressure-sensitive adhesive sheet containing a (meth)acrylic copolymer having an ultraviolet-crosslinkable site, as a pressure-sensitive adhesive sheet useful for displays and touch panels.
[0005] Patent No. 4971529 Patent No. 6062740
[0006] Many pressure-sensitive adhesive sheets that form a crosslinked structure upon UV irradiation contain a photoinitiator that generates radicals upon UV irradiation. However, in recent years, from the perspectives of energy conservation and component protection, there has been an increasing demand for pressure-sensitive adhesive sheets that photocure with relatively low energy and high efficiency, i.e., pressure-sensitive adhesive sheets that cure with relatively long-wavelength energy rays (e.g., active energy rays with wavelengths longer than 380 nm), particularly visible light. Furthermore, in recent years, in response to the need for power-saving, lightweight, and thin image display devices, organic electroluminescence (EL) panels have been widely adopted as image display panels, replacing conventional liquid crystal panels. In image display devices such as organic EL display devices, UV rays can cause deterioration of components within the image display device. Therefore, there is a strong demand for pressure-sensitive adhesive sheets that cure with visible light to suppress such UV-induced deterioration. Furthermore, in pressure-sensitive adhesive sheets that are laminated to an adherend, such as an image display device component, and then irradiated with light through the component for secondary curing, there is a problem that the light required for curing the pressure-sensitive adhesive sheet does not reach the intervening component if the intervening component has UV absorption properties. Therefore, pressure-sensitive adhesive sheets used in such image display devices must be pressure-sensitive adhesive sheets that cure with visible light.
[0007] For this reason, photocurable adhesive sheets have been developed that use photoinitiators that absorb light in the long-wavelength ultraviolet or visible light range, such as α-aminoacetophenone-based or acylphosphine oxide-based photoinitiators. However, these cleavage-type photoinitiators are not environmentally friendly because they generate outgassing products such as benzaldehyde as photodecomposition products. On the other hand, hydrogen-abstraction-type photoinitiators such as thioxanthone-based and anthraquinone-based photoinitiators that do not produce photodecomposition products have absorption in the long-wavelength ultraviolet or visible light range, but they have poor hydrogen-abstraction ability compared to benzophenone-based photoinitiators that do not absorb light in the long-wavelength range, and therefore are unable to achieve sufficient curing sensitivity.
[0008] The present invention aims to provide a pressure-sensitive adhesive composition for bonding optical members that can be cured with energy rays on the relatively long wavelength side (for example, active energy rays with a wavelength longer than 380 nm, particularly active energy rays with a wavelength of 405 nm) and that produces few photodecomposition products, a pressure-sensitive adhesive sheet for bonding optical members, a pressure-sensitive adhesive sheet with a release film, and a laminate for an image display device, an image display device, and a pressure-sensitive adhesive sheet for an organic EL display device, using the same.
[0009] One embodiment of the present invention includes the following aspects. [1] A pressure-sensitive adhesive composition used for bonding optical members, comprising a (meth)acrylic polymer (A) and a photoinitiator (B), wherein the photoinitiator (B) is a compound having a radically polymerizable functional group having a carbon-carbon double bond and a radical generating group in its molecule, and the photoinitiator (b1) has a molar absorption coefficient at 405 nm of 30 (L / mol cm) or more. [2] The pressure-sensitive adhesive composition according to [1], wherein the photoinitiator (b1) comprises at least one selected from the group consisting of hydrogen abstraction photoinitiators having a structure in which the radical generating group is excited by irradiation with active energy rays to cause a hydrogen abstraction reaction to generate radicals, and intramolecular cleavage photoinitiators in which the radical generating group is excited by irradiation with active energy rays to cleave intramolecularly to generate radicals. [3] The pressure-sensitive adhesive composition according to [1] or [2], wherein the photoinitiator (b1) is a hydrogen abstraction photoinitiator, wherein the radical polymerizable functional group is a (meth)acryloyl group, and the radical generating group has a structure that generates radicals by causing a hydrogen abstraction reaction when excited by irradiation with active energy rays. [4] The pressure-sensitive adhesive composition according to any one of [1] to [3], wherein the radical generating group in the photoinitiator (b1) comprises at least one structure selected from the group consisting of a benzoin structure, a benzil ketal structure, an acylphosphine oxide structure, an α-aminoacetophenone structure, an α-hydroxyacetophenone structure, a benzophenone structure, a thioxanthone structure, an anthraquinone structure, a phenylglyoxylate structure, and an oxime ester structure. [5] The pressure-sensitive adhesive composition according to any one of [1] to [4], wherein the radical generating group in the photoinitiator (b1) has a thioxanthone structure. [6] The pressure-sensitive adhesive composition according to any one of [1] to [5], wherein the content of the photoinitiator (B) is 0.01 parts by mass or more relative to 100 parts by mass of the (meth)acrylic polymer (A). [7] The pressure-sensitive adhesive composition according to any one of [1] to [6], wherein the content of the photoinitiator (b1) in the photoinitiator (B) is 30% by mass or more relative to the total mass of the photoinitiator (B).[8] The pressure-sensitive adhesive composition according to any one of [1] to [7], wherein the (meth)acrylic polymer (A) comprises a structural unit derived from an alkyl (meth)acrylate (m1) having a linear or branched alkyl group with 3 to 30 carbon atoms in the alkyl group, and at least one structural unit selected from a structural unit derived from a hydroxyl group-containing monomer (a2) and a structural unit derived from a nitrogen-containing monomer (a3). [9] A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition according to any one of [1] to [8].
[10] The pressure-sensitive adhesive sheet according to [9], wherein the gel fraction (X0) is 20% or more.
[11] The pressure-sensitive adhesive sheet is active energy ray-curable, and the pressure-sensitive adhesive sheet is irradiated with active energy rays having a wavelength of 405 nm at an integrated light dose of 2000 to 4000 mJ / cm. 2
[12] The pressure-sensitive adhesive sheet according to any one of [9] to
[11] , wherein the gel fraction (X1) is 30% or more when irradiated at any irradiation dose within the range of
[10] to
[12] .
[13] The pressure-sensitive adhesive sheet according to any one of [9] to
[12] , wherein the difference (X1-X0) between the gel fraction (X1) and the gel fraction (X0) is 10% or more.
[14] A pressure-sensitive adhesive sheet with a release film, comprising the pressure-sensitive adhesive sheet according to any one of [9] to
[13] and a release film laminated together.
[15] A laminate for an image display device, comprising two optical members laminated together via the pressure-sensitive adhesive sheet according to any one of [9] to
[13] .
[16] An image display device comprising the laminate for an image display device according to
[15] .
[17] A pressure-sensitive adhesive sheet for an organic EL display device, comprising the pressure-sensitive adhesive sheet according to any one of [9] to
[13] .
[0010] The pressure-sensitive adhesive composition of the present invention can be cured with energy rays on the relatively long wavelength side (for example, energy rays with a wavelength longer than 380 nm, particularly active energy rays with a wavelength of 405 nm), and produces few photodecomposition products, making it suitable for use as a pressure-sensitive adhesive sheet used for bonding optical members, particularly a pressure-sensitive adhesive sheet for an organic EL display device.
[0011] An example of an embodiment of the present invention will be described in detail below. However, the present invention is not limited to the embodiment described below. In the present invention, the term "film" conceptually includes a sheet, a film, and a tape. Furthermore, when the term "panel" is used, such as an image display panel or a protective panel, it includes a plate, a sheet, and a film.
[0012] In the present invention, when it is written as "x to y" (x and y are any numbers), unless otherwise specified, it means "x or more and y or less," and also includes the meaning of "preferably greater than x" or "preferably smaller than y." Furthermore, when it is written as "x or more" (x is any number), it also includes the meaning of "preferably greater than x" unless otherwise specified, and when it is written as "y or less" (y is any number), it also includes the meaning of "preferably smaller than y" unless otherwise specified. Furthermore, "x and / or y (x and y are any configurations)" means at least one of x and y, and can mean three possibilities: x only, y only, or x and y. Furthermore, in the present invention, "(meth)acrylic" means a comprehensive definition of acrylic and methacrylic, "(meth)acrylate" means a comprehensive definition of acrylate and methacrylate, and "(meth)acryloyl" means a comprehensive definition of acryloyl and methacryloyl. The term "(meth)acrylic polymer" refers to a copolymer having structural units derived from (meth)acrylic monomers. The (meth)acrylic polymer may further have structural units derived from monomers other than (meth)acrylic monomers (e.g., styrene).
[0013] <<Adhesive Composition>> The adhesive composition for bonding optical members according to the present invention (hereinafter referred to as "the adhesive composition") contains a (meth)acrylic polymer (A) and a photoinitiator (B), wherein the photoinitiator (B) is a compound having a radically polymerizable functional group having a carbon-carbon double bond and a radical-generating group in the molecule, and contains a photoinitiator (b1) having a molar absorption coefficient at 405 nm of 30 (L / mol cm) or more. Each component contained in the adhesive composition will be described in detail below.
[0014] <(Meth)acrylic polymer (A)> Examples of the (meth)acrylic polymer (A) contained in the present pressure-sensitive adhesive composition include a homopolymer of an alkyl(meth)acrylate, as well as a copolymer obtained by polymerizing a monomer component copolymerizable therewith. Among these, it is preferred that the (meth)acrylic polymer contains two or more copolymerization components, and at least one of the copolymerization components is an alkyl(meth)acrylate having an alkyl group with 3 to 30 carbon atoms.
[0015] More specifically, examples of the (meth)acrylic polymer (A) include copolymers of monomer components containing an alkyl(meth)acrylate having an alkyl group with 3 to 30 carbon atoms and one or more monomers copolymerizable therewith selected from (a1) a carboxy group-containing monomer, (a2) a hydroxy group-containing monomer, (a3) a nitrogen-containing monomer, (a4) an epoxy group-containing monomer, (a5) a vinyl monomer, (a6) an alkyl(meth)acrylate monomer having an alkyl group with 1 or 2 carbon atoms, (a7) an alicyclic monomer, and (a8) other copolymerizable monomers.
[0016] (1) Among the copolymerizable monomers (a1) to (a8), the following copolymerizable monomers (a1), (a2), and (a3) are particularly preferred. (2) Furthermore, it is particularly preferred to not include the copolymerizable monomer (a1) but include either the copolymerizable monomer (a2) or (a3). By including either the copolymerizable monomer (a2) or (a3), corrosion resistance, adhesion, and resistance to wet heat whitening can be achieved when the adherend contains a corrosive component such as a metal. Furthermore, it is particularly preferred to include both the copolymerizable monomers (a2) and (a3) in order to enhance cohesion. (3) Furthermore, among the copolymerizable monomers (a3), those having a tertiary nitrogen atom are preferred because they have the effect of sensitizing the hydrogen abstraction reaction described below, thereby enabling efficient crosslinking. (4) Among the above alkyl(meth)acrylates, alkyl(meth)acrylates having a tertiary carbon atom in the alkyl group are preferred. By using such alkyl (meth)acrylate, a hydrogen abstraction reaction is likely to occur upon light irradiation, and as a result, crosslinking can be easily and efficiently formed.
[0017] The alkyl(meth)acrylate is preferably a linear or branched alkyl(meth)acrylate having an alkyl group with 3 to 30 carbon atoms, and is represented by the following formula (m1) (hereinafter also referred to as polymerizable monomer (m1)): CH 2 = C(R 1 )-COO(R 2 )...Formula (m1) (In formula (m1), R 1 represents a hydrogen atom or a methyl group, R 2 represents a linear or branched alkyl group having 3 to 30 carbon atoms.
[0018] Examples of the alkyl(meth)acrylate represented by formula (m1) include linear alkyl(meth)acrylates such as n-propyl(meth)acrylate, i-propyl(meth)acrylate, n-butyl(meth)acrylate, n-pentyl(meth)acrylate, n-hexyl(meth)acrylate, n-heptyl(meth)acrylate, n-octyl(meth)acrylate, n-nonyl(meth)acrylate, n-decyl(meth)acrylate, undecyl(meth)acrylate, lauryl(meth)acrylate, n-tridecyl(meth)acrylate, n-tetradecyl(meth)acrylate, cetyl(meth)acrylate, stearyl(meth)acrylate, icosyl(meth)acrylate, heneicosyl(meth)acrylate, and behenyl(meth)acrylate; and sec-butyl Examples of branched alkyl (meth)acrylates include (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, isostearyl (meth)acrylate, isoicosyl (meth)acrylate, butyloctyl (meth)acrylate, isomyristyl (meth)acrylate, isocetyl (meth)acrylate, hexyldecyl (meth)acrylate, isostearyl (meth)acrylate, octyldecyl (meth)acrylate, octyldodecyl (meth)acrylate, and isobehenyl (meth)acrylate. These may be used alone or in combination of two or more.
[0019] Among these, linear alkyl(meth)acrylates are preferred from the viewpoint of obtaining flexibility. Furthermore, from the viewpoint of balancing adhesiveness and flexibility, alkyl(meth)acrylates having an alkyl group of 3 to 20 carbon atoms, more preferably 5 to 18, particularly 6 to 16, and even more particularly 7 to 14 carbon atoms are preferred, such as n-butyl(meth)acrylate, n-pentyl(meth)acrylate, n-hexyl(meth)acrylate, n-octyl(meth)acrylate, n-nonyl(meth)acrylate, decyl(meth)acrylate, and lauryl(meth)acrylate.
[0020] Among these, it is preferable to use a branched alkyl (meth)acrylate, since a hydrogen abstraction reaction, which will be described later, is likely to occur upon light irradiation, and as a result, a crosslinked structure can be efficiently formed. Among these, a branched alkyl (meth)acrylate having an alkyl group with 3 to 20 carbon atoms, more preferably 5 to 18, particularly 6 to 16, and even more particularly 7 to 14 carbon atoms is preferred, and for example, sec-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, and isodecyl (meth)acrylate are preferred.
[0021] The proportion of the alkyl (meth)acrylate-derived structural units relative to 100% by mass of all structural units constituting the (meth)acrylic polymer (A) is preferably 5% by mass or more and 95% by mass or less, more preferably 10% by mass or more and 90% by mass or less, even more preferably 15% by mass or more and 85% by mass or less, and particularly preferably 20% by mass or more and 80% by mass or less. If the proportion of the alkyl (meth)acrylate-derived structural units is above the lower limit, flexibility tends to be excellent, and conformability to unevenness tends to be excellent when the adherend has unevenness. If it is below the upper limit, the effects of the copolymerizable monomer described below are easily obtained, and adhesive strength and cohesive strength tend to be excellent. The lower and upper limits of the content of the alkyl (meth)acrylate-derived structural units can be arbitrarily combined.
[0022] Examples of the carboxy group-containing monomer (a1) include (meth)acrylic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxypropyl phthalic acid, 2-(meth)acryloyloxyethyl maleic acid, 2-(meth)acryloyloxypropyl maleic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxypropyl succinic acid, crotonic acid, fumaric acid, maleic acid, and itaconic acid. These may be used alone or in combination of two or more.
[0023] Examples of the hydroxyl group-containing monomer (a2) include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; caprolactone-modified hydroxy (meth)acrylates such as caprolactone-modified 2-hydroxyethyl (meth)acrylate; diethylene glycol (meth)acrylate; polyethylene glycol (meth)acrylate; polypropylene glycol (meth)acrylate; polytetramethylene glycol (meth)acrylate; polyoxyethylene poly(meth)acrylate; Examples of suitable monomers include (meth)acrylates having an oxyalkylene structure such as propylene glycol (meth)acrylate, primary hydroxyl group-containing (meth)acrylates such as 2-acryloyloxyethyl-2-hydroxyethyl phthalate, secondary hydroxyl group-containing (meth)acrylates such as 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 3-chloro-2-hydroxypropyl (meth)acrylate, tertiary hydroxyl group-containing (meth)acrylates such as 2,2-dimethyl 2-hydroxyethyl (meth)acrylate, and vinyl ethers such as 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, and 4-hydroxybutyl vinyl ether. These may be used alone or in combination of two or more. The hydroxyl group-containing monomer (a2) improves the adhesive strength of the pressure-sensitive adhesive sheet and can suppress whitening under heat and humidity. Furthermore, when the pressure-sensitive adhesive composition contains a thermal crosslinking agent, as described below, it serves as a crosslinking reaction site.
[0024] Among the hydroxyl group-containing monomers (a2), preferred are hydroxyl group-containing monomers having a hydroxyalkyl group having 1 to 10, more preferably 1 to 6, and even more preferably 2 to 4 carbon atoms, such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, and 4-hydroxybutyl vinyl ether, and particularly preferred are primary hydroxyl group-containing (meth)acrylates, such as 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate.
[0025] From the viewpoint of imparting adhesive strength and resistance to wet heat whitening, the content of the structural units derived from the hydroxyl group-containing monomer (a2) in the (meth)acrylic polymer (A) is preferably 3 to 30 mass%, more preferably 5 to 25 mass%, and particularly preferably 7 to 20 mass%, based on the total structural units of the (meth)acrylic polymer (A).
[0026] Examples of the nitrogen-containing monomer (a3) include amino group-containing monomers, amide group-containing monomers, isocyanate group-containing monomers, and (meth)acrylonitrile. The nitrogen-containing monomer (a3) improves the cohesive strength of the PSA sheet and can suppress whitening under wet heat. These monomers may be used alone or in combination of two or more. The nitrogen-containing monomer (a3) also has the effect of promoting the hydrogen abstraction reaction described below.
[0027] Examples of the amino group-containing monomer as the nitrogen-containing monomer include primary amino group-containing (meth)acrylates such as aminomethyl (meth)acrylate and aminoethyl (meth)acrylate; secondary amino group-containing (meth)acrylates such as t-butylaminoethyl (meth)acrylate and t-butylaminopropyl (meth)acrylate; tertiary amino group-containing (meth)acrylates such as ethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, diethylaminopropyl (meth)acrylate, and dimethylaminopropylacrylamide; and monomers such as N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, (meth)acryloylmorpholine, N-vinylacetamides, and N-vinylcaprolactam.
[0028] Examples of the amide group-containing monomer include (meth)acrylamide; N-alkyl(meth)acrylamides such as N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-n-butyl(meth)acrylamide, diacetone(meth)acrylamide, and N,N'-methylenebis(meth)acrylamide; N,N-dialkyl(meth)acrylamides such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-ethylmethylacrylamide, and N,N-diallyl(meth)acrylamide; hydroxyalkyl(meth)acrylamides such as N-hydroxymethyl(meth)acrylamide and N-hydroxyethyl(meth)acrylamide; alkoxyalkyl(meth)acrylamides such as N-methoxymethyl(meth)acrylamide and N-(n-butoxymethyl)(meth)acrylamide; maleimide or a derivative thereof.
[0029] Examples of the isocyanate group-containing monomer include 2-(meth)acryloyloxyethyl isocyanate and alkylene oxide adducts thereof, etc. The isocyanate group may be protected with a blocking agent such as methyl ethyl ketone oxime, 3,5-dimethylpyrazole, 1,2,4-triazole, or diethyl malonate.
[0030] Among these, those having a tertiary nitrogen atom are preferred in terms of having a sensitizing effect on the hydrogen abstraction reaction described below, and as a result, being able to efficiently form a crosslinked structure. For example, tertiary amino group-containing (meth)acrylate, N,N-dialkyl(meth)acrylamide, N-vinylpyrrolidone, acryloylmorpholine, etc. are particularly preferred.
[0031] From the viewpoint of imparting cohesive strength and resistance to wet heat whitening, the content of the structural units derived from the nitrogen-containing monomer (a3) in the (meth)acrylic polymer (A) is preferably 0.1 to 15 mass%, more preferably 0.5 to 13 mass%, particularly preferably 1 to 10 mass%, and especially preferably 2 to 7 mass%, based on all structural units of the (meth)acrylic polymer (A).
[0032] Examples of the epoxy group-containing monomer (a4) include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate glycidyl ether. These may be used alone or in combination of two or more.
[0033] Examples of the vinyl monomer (a5) include compounds having a vinyl group in the molecule. Examples of such compounds include vinyl ester monomers such as vinyl acetate, vinyl propionate, vinyl laurate, and vinyl stearate, as well as aromatic vinyl monomers such as styrene, chlorostyrene, chloromethylstyrene, α-methylstyrene, and other substituted styrenes. These may be used alone or in combination of two or more. These may be used alone or in combination of two or more.
[0034] Examples of the alkyl (meth)acrylate monomer (a6) in which the alkyl group has 1 or 2 carbon atoms include methyl (meth)acrylate and ethyl (meth)acrylate. These may be used alone or in combination of two or more. From the viewpoint of imparting cohesive strength to the PSA sheet, the content of the structural units derived from the copolymerizable monomer (a6) in the (meth)acrylic polymer (A) is preferably 0.1 to 15 mass%, more preferably 0.5 to 13 mass%, particularly preferably 1 to 10 mass%, and especially preferably 2 to 7 mass%, relative to all structural units of the (meth)acrylic polymer (A).
[0035] Examples of the alicyclic monomer (a7) include cyclohexyl (meth)acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, and adamantyl (meth)acrylate. These may be used alone or in combination of two or more. From the viewpoint of imparting cohesive strength to the PSA sheet, the content of the structural units derived from the copolymerizable monomer (a7) in the (meth)acrylic polymer (A) is preferably 0.1 to 15% by mass, more preferably 0.5 to 13% by mass, particularly preferably 1 to 10% by mass, and especially preferably 2 to 7% by mass, relative to all structural units of the (meth)acrylic polymer (A).
[0036] Examples of the other copolymerizable monomer (a8) include (meth)acrylates having an alkoxyalkylene glycol skeleton, such as methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, butoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, butoxypolypropylene glycol (meth)acrylate, methoxypolytetramethylene glycol (meth)acrylate, butoxypolytetramethylene glycol (meth)acrylate, methoxypolyoxyethylene polyoxypropylene glycol (meth)acrylate, and butoxypolyoxyethylene polyoxypropylene glycol (meth)acrylate; phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenyldiethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, and phenoxypolyethylene glycol-polypropylene glycol-(meth)acrylate. aromatic (meth)acrylates such as acrylate and nonylphenol ethylene oxide adduct (meth)acrylate, 4-acryloyloxybenzophenone, 4-acryloyloxyethoxybenzophenone, 4-acryloyloxy-4'-methoxybenzophenone, 4-acryloyloxyethoxy-4'-methoxybenzophenone, 4-acryloyloxy-4'-bromobenzophenone, 4-acryloyloxyethoxy-4'-bromobenzophenone, 4-methacryloyloxybenzophenone, 4- Examples include (meth)acrylates having a benzophenone structure such as methacryloyloxyethoxybenzophenone, 4-methacryloyloxy-4'-methoxybenzophenone, 4-methacryloyloxyethoxy-4'-methoxybenzophenone, 4-methacryloyloxy-4'-bromobenzophenone, 4-methacryloyloxyethoxy-4'-bromobenzophenone, and mixtures thereof, heterocycle-containing (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate, and macromonomers. These can be used alone or in combination of two or more.
[0037] The content of the structural units derived from the copolymerizable monomer (a8) in the (meth)acrylic polymer (A) is preferably 1% by mass or more and 30% by mass or less, more preferably 3% by mass or more and 20% by mass or less, and even more preferably 5% by mass or more and 15% by mass or less, based on all structural units constituting the (meth)acrylic polymer (A). The lower and upper limits of the content can be combined in any manner.
[0038] The (meth)acrylic polymer (A) may have a photoactive moiety, such as a polymerizable carbon-carbon double bond group, introduced into its side chain, which can enhance the crosslinking efficiency of the pressure-sensitive adhesive composition and crosslink the pressure-sensitive adhesive composition in a shorter time, thereby increasing productivity.
[0039] Examples of a method for introducing a polymerizable carbon-carbon double bond group into the side chain of the (meth)acrylic polymer (A) include a method in which a copolymer containing the above-mentioned hydroxyl group-containing monomer (a2) or a functional group-containing ethylenically unsaturated monomer is prepared, and then a compound having a polymerizable carbon-carbon double bond group and a functional group reactive with the functional group is subjected to a condensation or addition reaction while maintaining the activity of the polymerizable carbon-carbon double bond group.
[0040] Examples of combinations of these functional groups include an epoxy group (glycidyl group) and a carboxy group, an amino group and a carboxy group, an amino group and an isocyanate group, an epoxy group (glycidyl group) and an amino group, a hydroxyl group and an epoxy group, and a hydroxyl group and an isocyanate group. Among these combinations of functional groups, a combination of a hydroxyl group and an isocyanate group is preferred because of the ease of reaction control. Among these, a combination in which the copolymer has a hydroxyl group and the compound has an isocyanate group is preferred.
[0041] Examples of the isocyanate compound having a polymerizable carbon-carbon double bond group include the above-mentioned 2-(meth)acryloyloxyethyl isocyanate and alkylene oxide adducts thereof.
[0042] From the viewpoint of improving adhesiveness and stress relaxation properties, the content of the compound having a functional group reactive with the functional group and a polymerizable carbon-carbon double bond group is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 1 part by mass or less, and particularly preferably 0.1 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic polymer (A). The lower limit is usually 0 parts by mass. Specifically, the content is preferably 0 parts by mass or more and 10 parts by mass or less, more preferably 0 parts by mass or more and 5 parts by mass or less, even more preferably 0 parts by mass or more and 1 part by mass or less, and particularly preferably 0 parts by mass or more and 0.1 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic polymer (A).
[0043] The weight-average molecular weight (Mw) of the (meth)acrylic polymer (A) is preferably 200,000 or more, more preferably 300,000 or more, and even more preferably 400,000 or more, from the viewpoint of obtaining a pressure-sensitive adhesive composition with high cohesive strength. Furthermore, from the viewpoint of ease of handling and uniform stirring, the upper limit of the weight-average molecular weight (Mw) of the (meth)acrylic polymer (A) is preferably 1.5 million or less, more preferably 1.2 million or less, even more preferably 1.1 million or less, and particularly preferably 1 million or less. Specifically, the weight-average molecular weight (Mw) of the (meth)acrylic polymer (A) is preferably 200,000 or more and 1.5 million or less, more preferably 300,000 or more and 1.2 million or less, even more preferably 400,000 or more and 1.1 million or less, and particularly preferably 400,000 or more and 1 million or less. The lower and upper limits of the weight-average molecular weight of the (meth)acrylic polymer (A) can be arbitrarily combined. The weight average molecular weight of the (meth)acrylic polymer (A) is a value calculated as a standard polystyrene as measured by gel permeation chromatography (GPC).
[0044] The method for producing the (meth)acrylic polymer (A) is not particularly limited. For example, a method of polymerizing a monomer mixture containing an alkyl(meth)acrylate having an alkyl group with 3 to 30 carbon atoms and one or more copolymerizable monomers selected from the group consisting of the copolymerizable monomers (a1) to (a8) used as needed can be used.
[0045] <Photoinitiator (B)> The pressure-sensitive adhesive composition contains, as the photoinitiator (B), a photoinitiator (b1), which is a compound having a radically polymerizable functional group having a carbon-carbon double bond and a radical-generating group in the molecule, and has a molar absorption coefficient at 405 nm of 30 (L / mol cm) or more. Here, the "radical-generating group" means a group that generates a radical that initiates a polymerization reaction when excited by active energy rays.
[0046] Photoinitiators are compounds that generate radicals when exposed to active energy rays. Photoinitiators are broadly classified into two types based on the radical generation mechanism. More specifically, they are broadly divided into cleavage-type photoinitiators, which can generate radicals by cleaving and decomposing the single bond of the initiator itself, and hydrogen abstraction-type photoinitiators, which can generate radicals by an excited initiator abstracting hydrogen from a hydrogen donor in the system.
[0047] Photoinitiators that are highly sensitive to long-wavelength light have primarily been α-aminoacetophenone-based and acylphosphine oxide-based photoinitiators. However, because these are cleavage-type photoinitiators, they generate photodecomposition products, such as benzaldehyde, and outgassing, so improvements have been strongly desired. Furthermore, hydrogen-abstraction photoinitiators such as thioxanthone and anthraquinone, which are traditionally known as photoinitiators sensitive to long-wavelength light, do not generate photodecomposition products. However, compared to those that do not absorb in the long-wavelength region, such as benzophenone-based photoinitiators, their hydrogen-abstraction ability is poor, making it impossible to achieve sufficient curing sensitivity, and therefore their use has been limited.
[0048] Under these circumstances, the present inventors have conducted extensive research and found that by using a photoinitiator (b1) which is a compound having a radically polymerizable functional group having a carbon-carbon double bond and a radical generating group in the molecule and has a molar absorption coefficient at 405 nm of 30 (L / mol cm) or more, the curing reaction of the (meth)acrylic polymer (A) proceeds smoothly while suppressing the generation of decomposition products, and the (meth)acrylic polymer (A) is cured by energy rays on the long wavelength side, for example, energy rays with a wavelength of 405 nm, thereby completing the present invention.
[0049] The photoinitiator (b1) has a radically polymerizable functional group having a carbon-carbon double bond in the molecule. By having such a structure, the photoinitiator is incorporated into the polymerization structure after the photoreaction, making it possible to suppress the generation of decomposition products derived from the photoinitiator. This is also preferable in that it can suppress bleed-out of the photoinitiator and improve the cohesive strength of the pressure-sensitive adhesive sheet. Examples of the radically polymerizable functional group possessed by the photoinitiator (b1) include a (meth)acryloyl group and an allyl group. Of these, a (meth)acryloyl group is preferred due to its high reactivity, and an acryloyl group is more preferred. The number of radically polymerizable functional groups possessed by the photoinitiator (b1) may be one or two or more, but one is preferred.
[0050] The photoinitiator (b1) also has a radical generating group in its molecule. This allows it to be activated by active energy ray irradiation to generate radicals, which can serve as the starting point for the curing reaction. Examples of the radical generating group include groups derived from known photoradical generators, such as groups having a structure that is photocleaved by active energy ray irradiation, such as an acylphosphine oxide structure, an α-aminoacetophenone structure, or an α-hydroxyacetophenone structure; groups having a structure that is excited by active energy ray irradiation to generate radicals by causing a hydrogen abstraction reaction, such as a benzophenone structure, a thioxanthone structure, an anthraquinone structure, or a phenyl glyoxylate structure; and groups having an oxime ester structure. Among these, from the viewpoint of suppressing the generation of decomposition products, structures that are excited by active energy ray irradiation to cause a hydrogen abstraction reaction are preferred, and among these, groups having a thioxanthone structure are particularly preferred from the viewpoint of adjusting the molar extinction coefficient at 405 nm, as described below.
[0051] By having a group having a hydrogen abstraction structure as the radical generating group, the photoinitiator (b1) functions as a hydrogen abstraction photoinitiator. Conventional hydrogen abstraction photoinitiators, such as those having a benzophenone structure, a thioxanthone structure, an anthraquinone structure, or a phenyl glyoxylate structure, typically have low efficiency in abstracting hydrogen from a hydrogen donor under light in the long wavelength region, making it difficult for the curing reaction of the (meth)acrylic polymer (A) to proceed. However, it has been discovered that by using a photoinitiator that has, in addition to the hydrogen abstraction structure as the radical generating group, a radically polymerizable functional group having a carbon-carbon double bond in the molecule and has a molar absorption coefficient at 405 nm of 30 (L / mol cm) or more, the curing reaction of the (meth)acrylic polymer (A) proceeds smoothly, and the polymer is cured by energy rays on the long wavelength side, for example, energy rays with a wavelength of 405 nm. Hydrogen abstraction photoinitiators are preferred because they do not produce photodecomposition products like cleavage photoinitiators. Furthermore, hydrogen abstraction photoinitiators are also preferred in that they undergo a hydrogen abstraction reaction from the (meth)acrylic polymer (A) as well, leading to the incorporation of the (meth)acrylic polymer (A) into the crosslinked structure, thereby facilitating the formation of a crosslinked structure with many crosslinking points.Photoinitiators having a radically polymerizable functional group with a carbon-carbon double bond in the molecule are also preferred in that they bond with the carbon-carbon double bond of the (meth)acrylic polymer (A) or the polyfunctional (meth)acrylate (C) during the photocuring reaction and are incorporated into the crosslinked structure, thereby preventing bleed-out and migration of the photoinitiator.
[0052] The photoinitiator (b1) has a molar absorption coefficient at 405 nm of 30 (L / mol cm) or more, which means that it has excellent sensitivity to long-wavelength active energy rays. Therefore, the photoinitiator (b1) can be used to obtain the present pressure-sensitive adhesive composition that can be cured with relatively long-wavelength active energy rays (for example, active energy rays of 405 nm, which are longer than 380 nm). From this perspective, the molar absorption coefficient is preferably 40 (L / mol cm) or more, more preferably 50 (L / mol cm) or more, even more preferably 60 (L / mol cm) or more, and particularly preferably 70 (L / mol cm) or more. Note that the upper limit of the molar absorption coefficient is 1.0 × 10 in terms of internal (or deep) curability. 6 (L / mol cm) or less, and more preferably 5.0 × 10 5 (L / mol cm) or less, and more preferably 1.0 × 10 5 (L / mol cm) or less, and particularly preferably 5.0 × 10 4 (L / mol cm) or less. The lower and upper limits of the molar absorption coefficient can be combined arbitrarily. Specifically, the molar absorption coefficient is 40 (L / mol cm) or more and 1.0 × 10 6 (L / mol cm) or less, and more preferably 50 (L / mol cm) or more and 5.0 × 10 5 (L / mol cm) or less, and more preferably 60 (L / mol cm) or more and 1.0 × 10 5 (L / mol cm) or less, and particularly preferably 70 (L / mol cm) or more and 5.0 × 10 4 The molar absorption coefficient of the photoinitiator (b1) at 405 nm is calculated from the absorbance obtained by dissolving a predetermined concentration of the photoinitiator (b1) in chloroform or the like, measuring the absorbance at 405 nm using an ultraviolet-visible spectrophotometer, and using the following formula: A=εLc (A is absorbance, ε is the molar absorption coefficient (L / mol cm), c is the molar concentration of the photoinitiator (b1) (mol / L), and L is the optical path length (cm)).
[0053] Specific examples of the photoinitiator (b1) include 1-(meth)acryloyloxythioxanthone, 2-(meth)acryloyloxythioxanthone, 3-(meth)acryloyloxythioxanthone, 4-(meth)acryloyloxythioxanthone, 1-(2-(meth)acryloyloxyethoxy)thioxanthone, 2-(2-(meth)acryloyloxyethoxy)thioxanthone, 3-(2-(meth)acryloyloxyethoxy)thioxanthone, 4-(2-(meth)acryloyloxyethoxy)thioxanthone, 1-( 3-(meth)acryloyloxypropoxy)thioxanthone, 2-(3-(meth)acryloyloxypropoxy)thioxanthone, 3-(3-(meth)acryloyloxypropoxy)thioxanthone, 4-(3-(meth)acryloyloxypropoxy)thioxanthone, 1-(4-(meth)acryloyloxybutoxy)thioxanthone, 2-(4-(meth)acryloyloxybutoxy)thioxanthone, 3-(4-(meth)acryloyloxybutoxy)thioxanthone, 4-(4-(meth)acryloyloxybutoxy ) thioxanthone, thioxanthone-1-carboxylic acid 2-(2-(meth)acryloyloxyethoxy)-2-oxoethyl ester, thioxanthone-2-carboxylic acid 2-(2-(meth)acryloyloxyethoxy)-2-oxoethyl ester, thioxanthone-3-carboxylic acid 2-(2-(meth)acryloyloxyethoxy)-2-oxoethyl ester, thioxanthone-4-carboxylic acid 2-(2-(meth)acryloyloxyethoxy)-2-oxoethyl ester, thioxanthone-1-carboxylic acid 2-(3-(meth)acryloyloxyethoxy)-2-oxoethyl ester ) acryloyloxypropoxy)-2-oxoethyl ester, thioxanthone-2-carboxylic acid 2-(3-(meth)acryloyloxypropoxy)-2-oxoethyl ester, thioxanthone-3-carboxylic acid 2-(3-(meth)acryloyloxypropoxy)-2-oxoethyl ester, thioxanthone-4-carboxylic acid 2-(3-(meth)acryloyloxypropoxy)-2-oxoethyl ester, thioxanthone-1-carboxylic acid 2-(4-(meth)acryloyloxybutoxy)-2-oxoethyl ester,Thioxanthone-2-carboxylic acid 2-(4-(meth)acryloyloxybutoxy)-2-oxoethyl ester, thioxanthone-3-carboxylic acid 2-(4-(meth)acryloyloxybutoxy)-2-oxoethyl ester, thioxanthone-4-carboxylic acid 2-(4-(meth)acryloyloxybutoxy)-2-oxoethyl ester, thioxanthone-1-carboxylic acid 2-hydroxy-3-(2-(meth)acryloyloxyethoxy)propyl ester, thioxanthone-2-carboxylic acid 2-hydroxy-3-(2-(meth)acryloyloxyethoxy)propyl ester thioxanthone-3-carboxylic acid 2-hydroxy-3-(2-(meth)acryloyloxyethoxy)propyl ester, thioxanthone-4-carboxylic acid 2-hydroxy-3-(2-(meth)acryloyloxyethoxy)propyl ester, thioxanthone-1-carboxylic acid 2-hydroxy-3-(3-(meth)acryloyloxypropoxy)propyl ester, thioxanthone-2-carboxylic acid 2-hydroxy-3-(3-(meth)acryloyloxypropoxy)propyl ester, thioxanthone-3-carboxylic acid 2-hydroxy-3-(2-(meth)acryloyloxyethoxy)propyl ester, Xanthone-3-carboxylic acid 2-hydroxy-3-(3-(meth)acryloyloxypropoxy)propyl ester, thioxanthone-4-carboxylic acid 2-hydroxy-3-(3-(meth)acryloyloxypropoxy)propyl ester, thioxanthone-1-carboxylic acid 2-hydroxy-3-(4-(meth)acryloyloxybutoxy)propyl ester, thioxanthone-2-carboxylic acid 2-hydroxy-3-(4-(meth)acryloyloxybutoxy)propyl ester, thioxanthone-3-carboxylic acid 2-hydroxy-3- (4-(meth)acryloyloxybutoxy)propyl ester, thioxanthone-4-carboxylic acid 2-hydroxy-3-(4-(meth)acryloyloxybutoxy)propyl ester, 1-(2-hydroxy-3-(meth)acryloyloxypropoxy)thioxanthone, 2-(2-hydroxy-3-(meth)acryloyloxypropoxy)thioxanthone, 3-(2-hydroxy-3-(meth)acryloyloxypropoxy)thioxanthone, 4-(2-hydroxy-3-(meth)acryloyloxypropoxy)thioxanthone,Thioxanthone-1-carboxylic acid 2-hydroxy-3-(meth)acryloyloxypropyl ester, thioxanthone-2-carboxylic acid 2-hydroxy-3-(meth)acryloyloxypropyl ester, thioxanthone-3-carboxylic acid 2-hydroxy-3-(meth)acryloyloxypropyl ester, thioxanthone-4-carboxylic acid 2-hydroxy-3-(meth)acryloyloxypropyl ester, thioxanthone-1-carboxylic acid 2-(meth)acryloyloxyethyl ester, thioxanthone-2-carboxylic acid 2-(meth)acryloyloxypropyl ester ) acryloyloxyethyl ester, thioxanthone-3-carboxylic acid 2-(meth)acryloyloxyethyl ester, thioxanthone-4-carboxylic acid 2-(meth)acryloyloxyethyl ester, thioxanthone-1-carboxylic acid 3-(meth)acryloyloxypropyl ester, thioxanthone-2-carboxylic acid 3-(meth)acryloyloxypropyl ester, thioxanthone-3-carboxylic acid 3-(meth)acryloyloxypropyl ester, thioxanthone-4-carboxylic acid 3-(meth)acryloyloxypropyl ester thioxanthone-1-carboxylic acid 4-(meth)acryloyloxybutyl ester, thioxanthone-2-carboxylic acid 4-(meth)acryloyloxybutyl ester, thioxanthone-3-carboxylic acid 4-(meth)acryloyloxybutyl ester, thioxanthone-4-carboxylic acid 4-(meth)acryloyloxybutyl ester, 1-(3-(meth)acryloyloxy-1-oxopropoxy)thioxanthone, 2-(3-(meth)acryloyloxy-1-oxopropoxy)thioxanthone, 3-(3-(meth)acryloyl (oxy-1-oxopropoxy)thioxanthone, 4-(3-(meth)acryloyloxy-1-oxopropoxy)thioxanthone, 1-(4-(meth)acryloyloxy-1-oxobutoxy)thioxanthone, 2-(4-(meth)acryloyloxy-1-oxobutoxy)thioxanthone, 3-(4-(meth)acryloyloxy-1-oxobutoxy)thioxanthone, 4-(4-(meth)acryloyloxy-1-oxobutoxy)thioxanthone, 1-(5-(meth)acryloyloxy-1-oxopentoxy)thioxanthone,2-(5-(meth)acryloyloxy-1-oxopentoxy)thioxanthone, 3-(5-(meth)acryloyloxy-1-oxopentoxy)thioxanthone, 4-(5-(meth)acryloyloxy-1-oxopentoxy)thioxanthone, 1-[2-(2-(meth)acryloyloxyethoxy)-2-oxoethoxy]thioxanthone, 2-[2-(2-(meth)acryloyloxyethoxy)-2-oxoethoxy]thioxanthone, 3-[2-(2-(meth)acryloyloxyethoxy)-2-oxoethoxy]thioxanthone, 4-[2-(2-(meth)acryloyloxyethoxy)-2-oxoethoxy]thioxanthone, 1-[2-(3-(meth)acryloyloxypropoxy)-2-oxoethoxy]thioxanthone, 2-[2-(3-(meth)acryloyloxypropoxy)-2-oxoethoxy]thioxanthone, 3-[2-(3-(meth)acryloyloxypropoxy)-2-oxoethoxy]thioxanthone, 4-[2-(3-(meth)acryloyloxypropoxy)-2-oxoethoxy]thioxanthone, 1-[2-(4-(meth)acryloyloxy 2-[2-(4-(meth)acryloyloxybutoxy)-2-oxoethoxy]thioxanthone, 2-[2-(4-(meth)acryloyloxybutoxy)-2-oxoethoxy]thioxanthone, 3-[2-(4-(meth)acryloyloxybutoxy)-2-oxoethoxy]thioxanthone, 4-[2-(4-(meth)acryloyloxybutoxy)-2-oxoethoxy]thioxanthone, 1-[2-(2-hydroxy-3-(meth)acryloyloxypropoxy)-2-oxoethoxy]thioxanthone, 2-[2-(2-hydroxy-3-(meth)acryloyloxypropoxy) -2-oxoethoxy]thioxanthone, 3-[2-(2-hydroxy-3-(meth)acryloyloxypropoxy)-2-oxoethoxy]thioxanthone, 4-[2-(2-hydroxy-3-(meth)acryloyloxypropoxy)-2-oxoethoxy]thioxanthone, 1-[(2-(meth)acryloyloxyethoxy)carbonyloxy]thioxanthone, 2-[(2-(meth)acryloyloxyethoxy)carbonyloxy]thioxanthone, 3-[(2-(meth)acryloyloxyethoxy)carbonyloxy]thioxanthone,4-[(2-(meth)acryloyloxyethoxy)carbonyloxy]thioxanthone, 1-[(3-(meth)acryloyloxypropoxy)carbonyloxy]thioxanthone, 2-[(3-(meth)acryloyloxypropoxy)carbonyloxy]thioxanthone, 3-[(3-(meth)acryloyloxypropoxy)carbonyloxy]thioxanthone, 4-[(3-(meth)acryloyloxypropoxy)carbonyloxy]thioxanthone Examples of the photoinitiator (b1) include 1-[(4-(meth)acryloyloxybutoxy)carbonyloxy]thioxanthone, 1-[(4-(meth)acryloyloxybutoxy)carbonyloxy]thioxanthone, 2-[(4-(meth)acryloyloxybutoxy)carbonyloxy]thioxanthone, 3-[(4-(meth)acryloyloxybutoxy)carbonyloxy]thioxanthone, 4-[(4-(meth)acryloyloxybutoxy)carbonyloxy]thioxanthone, and derivatives thereof. One or more types of photoinitiator (b1) can be used in combination.
[0054] In the present invention, the content of the photoinitiator (B) is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, particularly preferably 0.08 parts by mass or more, and even more preferably 0.1 parts by mass or more, relative to 100 parts by mass of the (meth)acrylic polymer (A), and the upper limit is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, even more preferably 5 parts by mass or less, and especially preferably 3 parts by mass or less. When the content of the photoinitiator (B) is equal to or more than the lower limit, poor curing tends to be prevented, and when it is equal to or less than the upper limit, bleed-out of the photoinitiator (B) is suppressed and problems of embrittlement and coloration tend to be easily suppressed.
[0055] The content of the photoinitiator (b1) in the pressure-sensitive adhesive composition is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.2 parts by mass or more, per 100 parts by mass of the (meth)acrylic polymer (A). The upper limit is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, even more preferably 5 parts by mass or less, and particularly preferably 3 parts by mass or less. When the content of the photoinitiator (b1) is equal to or greater than the lower limit, poor curing tends to be prevented. When the content is equal to or less than the upper limit, bleed-out of the photoinitiator (b1) is suppressed and problems such as embrittlement and discoloration tend to be easily suppressed. Furthermore, when the content is equal to or greater than the upper limit, the residual concentration that is not completely consumed after light irradiation increases, which may cause product deterioration due to unintended curing reaction progression in environments exposed to harsh ultraviolet rays, for example. The lower and upper limits of the content of the photoinitiator (b1) can be arbitrarily combined. Specifically, the content of the photoinitiator (b1) in the present pressure-sensitive adhesive composition is preferably 0.05 parts by mass or more and 10 parts by mass or less, more preferably 0.1 parts by mass or more and 8 parts by mass or less, and even more preferably 0.2 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic polymer (A).
[0056] The pressure-sensitive adhesive composition may contain a photoinitiator (b2) other than the photoinitiator (b1) as the photoinitiator (B), as long as the effects of the present invention are not impaired. The photoinitiator (b2) is a compound that does not have a radically polymerizable functional group having a carbon-carbon double bond or that has a radical-generating group in the molecule, and has a molar absorption coefficient at 405 nm of not more than 30 (L / mol cm). The photoinitiator (b2) may be either a hydrogen abstraction type photoinitiator or a cleavage type photoinitiator, and may be used alone or in combination of both. Furthermore, one or more types of each may be used in combination.
[0057] Hydrogen abstraction photoinitiators are roughly classified into intermolecular hydrogen abstraction photoinitiators that abstract hydrogen from other molecules, and intramolecular hydrogen abstraction photoinitiators that also cause a hydrogen abstraction reaction within the same molecule. Examples of hydrogen abstraction photoinitiators as the photoinitiator (b2) include benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-phenylbenzophenone, 3,3'-dimethyl-4-methoxybenzophenone, methyl 2-benzoylbenzoate, 4-[(4-methylphenyl)thio]benzophenone, 4-acryloyloxybenzophenone, 4-acryloyloxyethoxybenzophenone, 4-acryloyloxy-4'-methoxybenzophenone, 4-acryloyloxyethoxy-4'-methoxybenzophenone, 4-acryloyloxy-4'-bromobenzophenone, and 4-acryloyloxyethoxy-4'-bromobenzophenone. Examples include intermolecular hydrogen abstraction photoinitiators such as benzophenone, 4-methacryloyloxybenzophenone, 4-methacryloyloxyethoxybenzophenone, 4-methacryloyloxy-4'-methoxybenzophenone, 4-methacryloyloxyethoxy-4'-methoxybenzophenone, 4-methacryloyloxy-4'-bromobenzophenone, and 4-methacryloyloxyethoxy-4'-bromobenzophenone; and intramolecular hydrogen abstraction photoinitiators such as methyl benzoylformate, oxyphenylacetic acid-2-(2-oxo-2-phenyl-acetoxy-ethoxy)ethyl ester, and oxyphenylacetic acid-2-(2-hydroxy-ethoxy)ethyl ester. Among these, 4-acryloyloxybenzophenone, 4-acryloyloxyethoxybenzophenone, 4-acryloyloxy-4'-methoxybenzophenone, 4-acryloyloxyethoxy-4'-methoxybenzophenone, etc., which have a radically polymerizable functional group having a carbon-carbon double bond in the molecule, are preferred in that they are incorporated into the polymerization structure after the photoreaction, thereby suppressing bleed-out of the photoinitiator and improving the cohesive strength of the pressure-sensitive adhesive sheet.Furthermore, intramolecular hydrogen abstraction photoinitiators such as methyl benzoylformate, oxyphenylacetic acid-2-(2-oxo-2-phenyl-acetoxy-ethoxy)ethyl ester, and oxyphenylacetic acid-2-(2-hydroxy-ethoxy)ethyl ester are preferred in that they not only act as hydrogen donors in the system but also themselves can serve as starting points for radical generation.
[0058] Furthermore, a cleavage-type photoinitiator may also be used as the photoinitiator (b2) to the extent that photodecomposition products do not affect the quality. Cleavage-type photoinitiators are preferred because they have high photosensitivity. Examples of the cleavage-type photopolymerization initiator include 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)benzyl]phenyl}- 2-Methyl-propan-1-one, oligo(2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)propanone), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butan Tanone, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, (2,4,6-trimethylbenzoyl)ethoxyphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)2,4,4-trimethylpentylphosphine oxide, 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-(O-benzoyloxime), 1 1-[4-[[4-(2-hydroxyethoxy)phenyl]thio]phenyl]-1,2-propanedione 2-(O-acetyloxime), 1-[1-(4-benzoylphenyl)-1H-indol-3-yl]-1,2-octanedione 2-(O-acetyloxime), and derivatives thereof.
[0059] The content of the photoinitiator (b2) in the pressure-sensitive adhesive composition is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, even more preferably 3 parts by mass or less, and particularly preferably 2 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic polymer (A). The lower limit is usually 0 parts by mass. Specifically, the content of the photoinitiator (b2) in the pressure-sensitive adhesive composition is preferably 0 parts by mass or more and 5 parts by mass or less, more preferably 0.1 parts by mass or more and 4 parts by mass or less, even more preferably 0.5 parts by mass or more and 3 parts by mass or less, and particularly preferably 1 part by mass or more and 2 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic polymer (A).
[0060] In the present invention, from the viewpoint of obtaining the effects of the present invention, the content of the photoinitiator (b1) in the photoinitiator (B) is preferably 30% by mass or more, more preferably 50% by mass or more, and even more preferably 70% by mass or more, based on the total mass of the photoinitiator (B). Furthermore, it is preferable that the entire amount of the photoinitiator (B) is the photoinitiator (b1).
[0061] <Polyfunctional (meth)acrylate (C)> From the viewpoint of promoting the crosslinking reaction, the present pressure-sensitive adhesive composition preferably contains a polyfunctional (meth)acrylate (C). This allows the present pressure-sensitive adhesive composition to quickly form a crosslinked structure, for example, even with the same light irradiation dose. Furthermore, when a crosslinked structure is formed in a pressure-sensitive adhesive sheet using the present pressure-sensitive adhesive composition, adhesive extrusion during storage or when wound into a roll can be prevented, and good adhesiveness and cohesive strength can be obtained. However, if the acrylic polymer (A) undergoes a hydrogen abstraction reaction due to the action of the photoinitiator (B) or the like, and a sufficient crosslinked structure can be formed at least within the acrylic polymer (A) and between the acrylic polymers (A), the polyfunctional (meth)acrylate (C) does not necessarily need to be contained.
[0062] Examples of the polyfunctional (meth)acrylate (C) include (meth)acrylic monomers and (meth)acrylic oligomers having two or more functional groups, which may be used alone or in combination of two or more.
[0063] Examples of the (meth)acrylic monomer having two or more functional groups include pentanediol di(meth)acrylate, hexadiol di(meth)acrylate, heptanediol di(meth)acrylate, octanediol di(meth)acrylate, nonanediol di(meth)acrylate, decanediol di(meth)acrylate, undecanediol di(meth)acrylate, dodecanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, glycerin di(meth)acrylate, neopentyl glycol di(meth)acrylate, glycerin glycidyl ether di(meth)acrylate, tricyclodecane dimethacrylate, tricyclodecane dimethanol di(meth)acrylate, bisphenol A polyethoxy di(meth)acrylate, bisphenol A polypropoxy di(meth)acrylate, bisphenol F polyethoxy di(meth)acrylate, ethylene glycol di(meth)acrylate tri(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane trioxyethyl (meth)acrylate, ε-caprolactone-modified tris(2-hydroxyethyl) isocyanurate tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propoxylated pentaerythritol tri(meth)acrylate, ethoxylated pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, propoxylated pentaerythritol tri(meth)acrylate Pentaerythritol tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, tris(acryloxyethyl)isocyanurate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate , tripentaerythritol hexa(meth)acrylate, tripentaerythritol penta(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, di(meth)acrylate of hydroxypivalic acid neopentyl glycol ε-caprolactone adduct, trimethylolpropane tri(meth)acrylate, trimethylolpropane polyethoxytri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, etc.
[0064] Examples of polyfunctional (meth)acrylic oligomers include polyester (meth)acrylate oligomers, epoxy (meth)acrylate oligomers, urethane (meth)acrylate oligomers, polyether (meth)acrylate oligomers, etc. Among these, (meth)acrylate monomers and oligomers having a glycol structure are preferred from the viewpoint of imparting appropriate flexibility to the cured product.
[0065] The content of the polyfunctional (meth)acrylate (C) in the present pressure-sensitive adhesive composition is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, per 100 parts by mass of the (meth)acrylic polymer (A), from the viewpoint of imparting shape stability to the pressure-sensitive adhesive sheet and durability when formed into a laminate for an image display device. Furthermore, the upper limit is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, even more preferably 12 parts by mass or less, and particularly preferably 10 parts by mass or less, from the viewpoint of maintaining the flexibility of the pressure-sensitive adhesive sheet. The lower and upper limits of the content of the polyfunctional (meth)acrylate (C) can be arbitrarily combined. The content of the polyfunctional (meth)acrylate (C) in the present pressure-sensitive adhesive composition is preferably 0.1 parts by mass or more and 20 parts by mass or less, more preferably 0.5 parts by mass or more and 15 parts by mass or less, even more preferably 1 part by mass or more and 12 parts by mass or less, and particularly preferably 1 part by mass or more and 10 parts by mass or less, per 100 parts by mass of the (meth)acrylic polymer (A).
[0066] In addition to the polyfunctional (meth)acrylate (C), a thermal crosslinking agent can be used in combination to further improve the crosslinking density and thereby enhance long-term reliability. Examples of such thermal crosslinking agents include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, aziridine-based crosslinking agents, melamine-based crosslinking agents, aldehyde-based crosslinking agents, amine-based crosslinking agents, and metal chelate-based crosslinking agents. Among these, it is preferable to use an isocyanate-based crosslinking agent because of its excellent reactivity with the (meth)acrylic polymer (A).
[0067] <Other Components> The present pressure-sensitive adhesive composition may contain, as needed, various additives such as silane coupling agents, plasticizers, tackifying resins, antioxidants, light stabilizers, metal deactivators, antiaging agents, moisture absorbers, rust inhibitors, UV absorbers, and inorganic particles as "other components," as long as the effects of the present invention are not impaired. Furthermore, the present pressure-sensitive adhesive composition may contain, as needed, reaction catalysts such as tertiary amine compounds, quaternary ammonium compounds, and tin laurate compounds. These may be used alone or in combination of two or more.
[0068] [Silane coupling agent] Silane coupling agent is an organosilicon compound that contains one or more reactive functional groups and one or more alkoxy groups bonded to silicon atoms in its structure.The reactive functional groups include, for example, epoxy groups, (meth)acryloyl groups, mercapto groups, hydroxyl groups, carboxy groups, amino groups, amide groups, and isocyanate groups.Among these, epoxy groups and mercapto groups are preferred from the viewpoint of balance of durability.
[0069] The alkoxy group bonded to the silicon atom preferably contains an alkoxy group having 1 to 8 carbon atoms, from the viewpoint of durability and storage stability, and is particularly preferably a methoxy group or an ethoxy group. The silane coupling agent may also contain an organic substituent other than the reactive functional group and the alkoxy group bonded to the silicon atom, such as an alkyl group or a phenyl group.
[0070] Examples of the silane coupling agent used in the present invention include monomeric epoxy group-containing silane coupling agents, which are silane compounds such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; and silane coupling agents in which a part of the silane compounds is hydrolyzed and condensed, or in which the silane compounds are combined with methyltriethoxysilane, ethyltriethoxysilane, and the like. oligomeric epoxy group-containing silane coupling agents which are silane compounds obtained by co-condensation of alkyl group-containing silane compounds such as silane, methyltrimethoxysilane, and ethyltrimethoxysilane; monomeric mercapto group-containing silane coupling agents which are silane compounds such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, γ-mercaptopropyldimethoxymethylsilane, and 3-mercaptopropylmethyldimethoxysilane; and silane coupling agents which are silane compounds obtained by hydrolysis and condensation polymerization of a part of the silane compounds, or silane compounds obtained by hydrolysis and condensation polymerization of the silane compounds. and an alkyl group-containing silane compound such as methyltriethoxysilane, ethyltriethoxysilane, methyltrimethoxysilane, or ethyltrimethoxysilane, which is a silane compound obtained by co-condensation of the silane compound with an alkyl group-containing silane compound such as methyltriethoxysilane, ethyltriethoxysilane, methyltrimethoxysilane, or ethyltrimethoxysilane; (meth)acryloyl group-containing silane compounds such as 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, or 3-acryloxypropyltrimethoxysilane; Coupling agents: amino group-containing silane coupling agents such as N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, and N-phenyl-3-aminopropyltrimethoxysilane; isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane;Examples of suitable silane coupling agents include vinyl group-containing silane coupling agents such as vinyltrimethoxysilane and vinyltriethoxysilane. These may be used alone or in combination of two or more.
[0071] Among these, epoxy group-containing silane coupling agents and mercapto group-containing silane coupling agents are preferably used because of their excellent durability, and among these, epoxy group-containing silane coupling agents are particularly preferred.
[0072] The content of the silane coupling agent in the pressure-sensitive adhesive composition is preferably 0.005 to 10 parts by mass, more preferably 0.01 to 5 parts by mass, and particularly preferably 0.05 to 1 part by mass, per 100 parts by mass of the (meth)acrylic polymer (A). When the content is equal to or greater than the lower limit, durability tends to be improved, whereas when the content is equal to or less than the upper limit, durability tends to be improved.
[0073] [Plasticizer] The present pressure-sensitive adhesive composition may contain a plasticizer in order to impart flexibility to the pressure-sensitive adhesive sheet.
[0074] Examples of the plasticizer include, but are not limited to, polyisobutylene, polyisoprene, polybutadiene, amorphous polyolefins and their copolymers, silicone, polyacrylate, oligomeric polyurethane, ethylene-propylene copolymer, and any combination or mixture thereof. Among these, polyisobutylene is preferred as the plasticizer. Examples of polyisobutylene plasticizers that can be used herein include those commercially available from BASF under the trade name OPPANOL, particularly those selected from the OPPANOL B series.
[0075] From the viewpoint of environmental protection, the smaller the volatile organic compound (VOC) value of the plasticizer used, the better. When measured by thermogravimetric analysis, the VOC value is preferably less than 1000 ppm, more preferably less than 800 ppm, even more preferably less than 600 ppm, and most preferably less than 400 ppm.
[0076] The content of the plasticizer in the present pressure-sensitive adhesive composition is not particularly limited, and is preferably 0.1 to 20 parts by mass, and more preferably 0.5 to 15 parts by mass, per 100 parts by mass of the (meth)acrylic polymer (A).
[0077] [Tackifier] The present PSA composition may contain a tackifier to improve the adhesive strength of the PSA sheet. Examples of tackifiers include terpene resins such as polyterpenes (e.g., α-pinene resins, β-pinene resins, and limonene resins) and aromatic-modified polyterpene resins (e.g., phenol-modified polyterpene resins), coumaran-indene resins, petroleum-based resins such as C5 hydrocarbon resins, C9 hydrocarbon resins, C5 / C9 hydrocarbon resins, and dicyclopentadiene resins, and rosins such as modified rosin, hydrogenated rosin, polymerized rosin, and rosin esters.
[0078] The content of the tackifier in the present pressure-sensitive adhesive composition is not particularly limited, and is preferably 0.1 to 20 parts by mass, and more preferably 0.5 to 15 parts by mass, per 100 parts by mass of the (meth)acrylic polymer (A).
[0079] [Rust inhibitor] The present pressure-sensitive adhesive composition may contain a rust inhibitor to prevent corrosion when the adherend contains a corrosive portion such as metal wiring. Examples of rust inhibitors include triazoles and benzotriazoles. The content of the rust inhibitor in the present pressure-sensitive adhesive composition is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 3 parts by mass, per 100 parts by mass of the (meth)acrylic polymer (A).
[0080] [Ultraviolet absorber] The present pressure-sensitive adhesive composition may contain an ultraviolet absorber. By including an ultraviolet absorber, deterioration of the pressure-sensitive adhesive sheet itself and the adherend due to ultraviolet light can be suppressed. When the present pressure-sensitive adhesive composition contains an ultraviolet absorber, it is preferable to photocure the composition by using light having a wavelength other than the absorption wavelength of the ultraviolet absorber.
[0081] Examples of the ultraviolet absorber include benzophenone-based ultraviolet absorbers, benzotriazole-based ultraviolet absorbers, triazine-based ultraviolet absorbers, salicylic acid-based ultraviolet absorbers, cyanoacrylate-based ultraviolet absorbers, etc. These ultraviolet absorbers can be used alone or in combination of two or more.
[0082] Examples of the benzophenone-based ultraviolet absorbers include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, 2-hydroxy-4-methoxy-5-sulfoxybenzophenone, 2-hydroxy-4-methoxy-5-sulfoxytrihydridolate benzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxy-5-sodium sulfoxybenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2-hydroxy-4-n-dodecyloxybenzophenone, and 2-hydroxy-4-methoxy-2'-carboxybenzophenone.
[0083] Examples of the benzotriazole-based ultraviolet absorbers include 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-dicumylphenyl)phenylbenzotriazole, 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol], 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-tert-amylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-4-octoxyphenyl)benzotriazole, 2,2'-methylenebis(4-cumyl-6-benzotriazolephenyl), 2,2'-p-phenylenebis(1,3-benzoxazin-4-one, 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimidomethyl)-5-methylphenyl]benzotriazole, and the like.
[0084] Examples of the triazine-based ultraviolet absorber include 2-(2-hydroxy-4-methoxyphenyl)-4,6-diphenyl-1,3,5-triazine, 2-(2-hydroxy-4-ethoxyphenyl)-4,6-diphenyl-1,3,5-triazine, 2-(2-hydroxy-4-propoxyphenyl)-4,6-diphenyl-1,3,5-triazine, 2-(2-hydroxy-4-butoxyphenyl)-4,6-diphenyl-1,3,5-triazine, and 2-(2-hydroxy-4-hexyloxyphenyl)-4,6-diphenyl-1,3,5-triazine. Triazine, 2-(2-hydroxy-4-octyloxyphenyl)-4,6-diphenyl-1,3,5-triazine, 2-(2-hydroxy-4-dodecyloxyphenyl)-4,6-diphenyl-1,3,5-triazine, 2-(2-hydroxy-4-benzyloxyphenyl)-4,6-diphenyl-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-dibutoxyphenyl)-1,3-5-triazine, 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1 ,3,5-triazine, 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4- [(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis(2,4-dimethylphenyl)-6-[2-hydroxy-4-(3-octyloxy-2-hydroxypropyloxy)-5-α-cumylphenyl]-s-triazine, 2,4-bis(2,4-dimethylphenyl)-6-[2-hydroxy-4-(3-nonyloxy-2-hydroxypropyloxy)-5-α-cumylphenyl]-s-triazine 2,4-bis(2,Examples include 2-(2-hydroxy-4-(3-decyloxy-2-hydroxypropyloxy)-5-α-cumylphenyl)-s-triazine, 2-(2-hydroxy-4-acryloyloxyethoxyphenyl)-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, etc.
[0085] Examples of the salicylic acid-based ultraviolet absorbers include phenyl salicylate, p-tert-butylphenyl salicylate, and p-octylphenyl salicylate.
[0086] Examples of the cyanoacrylate ultraviolet absorber include 2-ethylhexyl-2-cyano-3,3'-diphenylacrylate and ethyl-2-cyano-3,3'-diphenylacrylate.
[0087] Among these, from the viewpoint of effectively suppressing ultraviolet degradation of the PSA sheet itself and the adherend, benzophenone-based ultraviolet absorbers, benzotriazole-based ultraviolet absorbers, and triazine-based ultraviolet absorbers are preferred, and among these, triazine-based ultraviolet absorbers containing a triazine structure are more preferred from the viewpoint of excellent heat resistance.
[0088] From the viewpoint of improving light resistance reliability, the content of the ultraviolet absorber in the pressure-sensitive adhesive composition is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1.5 parts by mass or more, particularly preferably 3 parts by mass or more, and most preferably 5 parts by mass or more, per 100 parts by mass of the (meth)acrylic polymer (A). On the other hand, from the viewpoint of suppressing bleed-out and improving yellowing resistance, the content of the ultraviolet absorber is preferably 15 parts by mass or less, more preferably 12 parts by mass or less, even more preferably 10 parts by mass or less, particularly preferably 8 parts by mass or less, and most preferably 7 parts by mass or less, per 100 parts by mass of the (meth)acrylic polymer (A).
[0089] The method for preparing the present pressure-sensitive adhesive composition is not particularly limited. For example, the present pressure-sensitive adhesive composition is prepared by mixing predetermined amounts of the (meth)acrylic polymer (A) and the photoinitiator (b1), and, if necessary, other components such as the photoinitiator (b2), the polyfunctional (meth)acrylate (C), and the silane coupling agent. The pressure-sensitive adhesive composition thus obtained is suitable for use in pressure-sensitive adhesive sheets, particularly pressure-sensitive adhesive sheets used for bonding optical components.
[0090] The present PSA composition may be in a syrup form. In this case, the syrup component may be composed of an acrylic polymer and a monomer component. In one example, such a syrup component may be formed by so-called partial polymerization, or may be prepared by adding a monomer to a polymer in which the monomers constituting the (meth)acrylic polymer (A) are completely or partially polymerized. That is, when a specific monomer composition is partially polymerized, some of the monomers polymerize to form oligomers or polymers, while some of the monomers remain, thereby forming the syrup component. In another example, a syrup can be formed by adding a monomer component to a partially or completely polymerized polymer. Therefore, the monomer units constituting the (meth)acrylic polymer (A) in this specification may refer to monomers present in the acrylic polymer component in the form of oligomers or polymers, or monomers contained in the syrup component before polymerization.
[0091] <<Adhesive Sheet>> The adhesive sheet for laminating optical members of the present invention (hereinafter also referred to as "the present adhesive sheet") is an adhesive sheet having an adhesive layer formed from the present adhesive composition. The present adhesive sheet is particularly useful as an adhesive sheet for organic EL display devices. The present adhesive sheet may be a single-layer sheet consisting only of an adhesive layer formed from the present adhesive composition (hereinafter also referred to as "the present adhesive layer"), or a multilayer sheet in which multiple present adhesive layers are laminated.
[0092] <Physical Properties of the Present Pressure-Sensitive Adhesive Sheet> The present pressure-sensitive adhesive sheet can have the following physical properties.
[0093] [Gel Fraction (X0)] The gel fraction (X0) of the present pressure-sensitive adhesive sheet is preferably 20% or more. If the gel fraction of the present pressure-sensitive adhesive sheet is equal to or greater than the lower limit, the shape is easily maintained. From this viewpoint, the gel fraction (X0) is more preferably 25% or more, even more preferably 30% or more, and particularly preferably 35% or more. Furthermore, from the viewpoint of obtaining flexibility, the gel fraction (X0) of the present pressure-sensitive adhesive sheet is preferably 70% or less, more preferably 60% or less, even more preferably 55% or less, and particularly preferably 50% or less. The lower and upper limits of the gel fraction (X0) can be arbitrarily combined. Specifically, the gel fraction (X0) of the present pressure-sensitive adhesive sheet is preferably 20% or more and 70% or less, more preferably 25% or more and 60% or less, even more preferably 30% or more and 55% or less, and particularly preferably 35% or more and 50% or less. The gel fraction (X0) is an index of the degree of crosslinking (degree of curing), and can be measured under the measurement conditions described in the examples below.
[0094] The present pressure-sensitive adhesive sheet is preferably active energy ray-curable. However, "the pressure-sensitive adhesive sheet is active energy ray-curable" means that the pressure-sensitive adhesive sheet has the property of being curable by active energy rays, in other words, that the pressure-sensitive adhesive sheet has room to be cured by active energy rays.
[0095] The present pressure-sensitive adhesive sheet may be one in which the pressure-sensitive adhesive composition has been cured to a state in which there is still room for it to be cured by active energy rays (hereinafter also referred to as "primary curing"), or one in which the pressure-sensitive adhesive composition has been crosslinked (primary curing) with a thermal crosslinking agent and is therefore curable by active energy rays. The pressure-sensitive adhesive sheet in the primary cured state can be cured (hereinafter also referred to as "secondary curing") by irradiating it with active energy rays before or after being attached to an adherend. Note that when the present pressure-sensitive adhesive sheet is active energy ray-curable, the "gel fraction X0" refers to the gel fraction of the pressure-sensitive adhesive sheet in the primary cured state.
[0096] When the pressure-sensitive adhesive sheet is primarily cured, the primary curing may be by heat or by active energy rays, but from the viewpoint of easily controlling the gel fraction (X0) within a predetermined range, a pressure-sensitive adhesive sheet that has been primarily cured by irradiation with active energy rays is preferred.
[0097] The active energy rays used for the primary curing are preferably active energy rays with a wavelength longer than 380 nm, and particularly preferably active energy rays with a wavelength longer than 400 nm. When the pressure-sensitive adhesive sheet is primarily cured with active energy rays, for example, the cumulative dose at 405 nm is 10 to 4000 mJ / cm. 2 In the case of such active energy ray irradiation, a preferred dose is 50 mJ / cm. 2 More than 3500mJ / cm 2 or less, more preferably 100 mJ / cm 2 More than 3000mJ / cm 2 Below 200 mJ / cm, particularly preferably 2 More than 2500mJ / cm 2 More preferably, 300 mJ / cm or less 2 More than 2000mJ / cm 2 When the irradiation amount is within the above range, it is preferable because the degree of cure tends to be adjustable while leaving room for cure. Note that when the active energy rays are irradiated from both sides, the active energy ray irradiation amount is the sum of the integrated energy on one side and the integrated energy on the other side.
[0098] [Gel fraction (X1)] When the pressure-sensitive adhesive sheet is active energy ray-curable, the pressure-sensitive adhesive sheet is irradiated with active energy rays having a wavelength of 405 nm in an integrated light amount of 2000 to 4000 mJ / cm 2The gel fraction (X1) (after secondary curing) when irradiated with any irradiation amount within this range is preferably 30% or more, more preferably 40% or more, even more preferably 50% or more, and particularly preferably 60% or more. Specifically, the gel fraction (X1) is preferably 30% or more and 100% or less, more preferably 40% or more and 90% or less, even more preferably 50% or more and 80% or less, and particularly preferably 60% or more and 70% or less. When the gel fraction (X1) after secondary curing is 30% or more, a laminate for an image display device using this pressure-sensitive adhesive sheet will have excellent durability.
[0099] Furthermore, the difference (X1-X0) between the gel fraction (X1) after the secondary curing and the gel fraction (X0) before irradiation with active energy rays (before the secondary curing), i.e., in the primary curing state, is preferably 10% or more, more preferably 15% or more, and even more preferably 20% or more. Specifically, the difference (X1-X0) is preferably 10% or more and 50% or less, more preferably 15% or more and 45% or less, and even more preferably 20% or more and 40% or less. By having the difference (X1-X0) of 10% or more, it is possible to achieve both high levels of adhesion to components of an image display device when the pressure-sensitive adhesive sheet is laminated to the component, and high levels of durability of the laminate for an image display device after lamination. The gel fraction (X1) can be measured by the method described in the Examples below.
[0100] [Adhesive Strength] When the pressure-sensitive adhesive sheet is active energy ray-curable, the pressure-sensitive adhesive sheet is laminated to soda lime glass, and then exposed to active energy rays having a wavelength of 405 nm in an integrated light amount of 2000 to 4000 mJ / cm 2When irradiated with any irradiation amount within this range, the adhesive strength to soda lime glass at a peel angle of 180° and a peel speed of 60 mm / min is preferably 5.0 N / cm or more, more preferably 6.0 N / cm or more, and even more preferably 7.0 N / cm or more. Specifically, the adhesive strength is preferably 5.0 N / cm or more and 10.0 N / cm or less, more preferably 6.0 N / cm or more and 9.0 N / cm or less, and even more preferably 7.0 N / cm or more and 8.0 N / cm or less. An adhesive strength of 5.0 N / cm or more makes a laminate for an image display device using this adhesive sheet excellent in durability.
[0101] In measuring the adhesive strength, the peeling mode when peeling the adhesive sheet from the component sheet is preferably interfacial peeling. Many of the image display device components used in image display devices are expensive, and if a failure occurs during the component lamination process, reworkability is required to allow the sheet to be peeled off without leaving any adhesive residue. Specifically, it is necessary to prevent the adhesive sheet from remaining on the surface of the component when peeling the image display device components, a so-called "sad separation." Interfacial peeling results in an adhesive sheet with excellent reworkability that does not contaminate the product. The peeling mode of the adhesive sheet can be determined, for example, by visually observing the adherend after the adhesive strength measurement test and checking for the presence or absence of adhesive residue. More specifically, the presence of adhesive residue that can be visually confirmed can be determined to be cohesive failure.
[0102] [Chromaticity] The chromaticity (b*) of the present pressure-sensitive adhesive sheet is preferably 4.0 or less, more preferably 3.0 or less, even more preferably 2.5 or less, particularly preferably 2.0 or less, even more preferably 1.5 or less, and most preferably 1.0 or less. Specifically, the chromaticity (b*) is preferably 0 to 4.0, more preferably 0 to 3.0, even more preferably 0.1 to 2.5, particularly preferably 0.3 to 2.0, even more preferably 0.5 to 1.5, and most preferably 0.8 to 1.0.
[0103] This pressure-sensitive adhesive sheet has transparency when observed with the naked eye, and transparency indicates that each component is uniformly dissolved in the sheet. The transparency of this pressure-sensitive adhesive sheet allows for an excellent appearance to be obtained without impairing the visibility of the image display surface. Specifically, transparency when observed with the naked eye means that the pressure-sensitive adhesive sheet has a total light transmittance of 50% or more as measured in accordance with JIS K7361-1 (ISO-13468-1) and a haze value of 10% or less as measured in accordance with JIS K7136 (ISO-14782).
[0104] [Total Light Transmittance, Haze] The total light transmittance of the present pressure-sensitive adhesive sheet, measured in accordance with JIS K7361-1 (ISO-13468-1), is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. Specifically, the total light transmittance is preferably 80% or more and 100% or less, more preferably 85% or more and 100% or less, and even more preferably 90% or more and 100% or less. When the total light transmittance of the present pressure-sensitive adhesive sheet is equal to or greater than the lower limit, it can be suitably used as a pressure-sensitive adhesive sheet for image display devices.
[0105] The haze of the pressure-sensitive adhesive sheet, measured in accordance with JIS K7136 (ISO-14782), is preferably 1.0% or less, more preferably 0.8% or less, and even more preferably 0.5% or less. Specifically, the haze is preferably 0% or more and 1.0% or less, more preferably 0% or more and 0.8% or less, and even more preferably 0% or more and 0.5% or less. When the haze of the pressure-sensitive adhesive sheet is 1.0% or less, it can be suitably used as a pressure-sensitive adhesive sheet for image display devices. The haze can be measured with a haze meter. In order to keep the haze of the pressure-sensitive adhesive sheet within the above range, it is preferable that the pressure-sensitive adhesive sheet does not contain particles such as organic particles.
[0106] <Thickness> The thickness of the present pressure-sensitive adhesive sheet is not particularly limited, but a thickness of 10 μm or more provides good handleability, and a thickness of 1000 μm or less can contribute to the thinning of the present pressure-sensitive adhesive sheet. From this perspective, the thickness of the present pressure-sensitive adhesive sheet is preferably 10 μm or more, more preferably 15 μm or more, even more preferably 20 μm or more, and particularly preferably 25 μm or more. On the other hand, the upper limit is preferably 1000 μm or less, more preferably 500 μm or less, even more preferably 400 μm or less, particularly preferably 300 μm or less, and especially preferably 250 μm or less. Specifically, the thickness of the pressure-sensitive adhesive sheet is preferably 10 μm or more and 1000 μm or less, more preferably 15 μm or more and 500 μm or less, even more preferably 20 μm or more and 300 μm or less, and particularly preferably 25 μm or more and 250 μm or less.
[0107] <Method for producing the present pressure-sensitive adhesive sheet> Next, a method for producing the present pressure-sensitive adhesive sheet will be described. However, the following description is an example of a method for producing the present pressure-sensitive adhesive sheet, and the present pressure-sensitive adhesive sheet is not limited to sheets produced by this method.
[0108] The present pressure-sensitive adhesive sheet may be produced, for example, by preparing the present pressure-sensitive adhesive composition, molding the present pressure-sensitive adhesive composition into a sheet, curing the composition by crosslinking, i.e., polymerization, and then processing the composition appropriately as necessary. Alternatively, the present pressure-sensitive adhesive sheet may be produced by preparing the present pressure-sensitive adhesive composition, coating it onto a component for an image display device, and curing the pressure-sensitive adhesive composition.
[0109] When preparing the present pressure-sensitive adhesive composition, the raw materials may be mixed using a propeller-type agitator or kneader (for example, a single-screw extruder, a twin-screw extruder, a planetary mixer, a twin-screw mixer, a pressure kneader, etc.). When mixing various raw materials, various additives such as silane coupling agents and antioxidants may be blended together with the resin in advance and then supplied to the agitator or kneader, or all materials may be melt-mixed in advance and then supplied, or a masterbatch in which only the additives are concentrated in the resin may be prepared in advance and then supplied.
[0110] The pressure-sensitive adhesive composition can be formed into a sheet by any known method, such as wet lamination, dry lamination, extrusion casting using a T-die, extrusion lamination, calendaring, inflation, injection molding, and liquid injection curing. Of these, when producing a sheet, wet lamination, extrusion casting, and extrusion lamination are preferred.
[0111] The present pressure-sensitive adhesive composition can be cured by irradiation with active energy rays, and the present pressure-sensitive adhesive sheet can be produced by irradiating a molded product of the present pressure-sensitive adhesive composition, for example, a sheet, with active energy rays. In addition to irradiation with active energy rays, further curing can be achieved by heating.
[0112] The irradiation energy, irradiation time, irradiation method, etc. of the active energy ray are not particularly limited as long as they can activate the photopolymerization initiator and polymerize the monomer component.
[0113] Examples of the active energy rays in the active energy ray irradiation include light rays such as far ultraviolet rays, ultraviolet rays, near ultraviolet rays, infrared rays, and visible light rays, as well as ionizing radiation such as X-rays, α-rays, β-rays, γ-rays, electron beams, proton beams, and neutron beams. Among these, ultraviolet rays or visible light rays are preferred from the viewpoints of suppressing damage to components of the image display device and facilitating reaction control. Furthermore, curing by ultraviolet irradiation or visible light irradiation is advantageous from the viewpoints of curing speed, ease of availability of irradiation equipment, cost, and the like. Among these, curing by visible light rays, for example, active energy rays of 405 nm, is preferred from the viewpoint of preventing curing inhibition by ultraviolet absorbers.
[0114] Examples of light sources for active energy ray irradiation include high-pressure mercury lamps, ultra-high-pressure mercury lamps, low-pressure mercury lamps, carbon arc lamps, metal halide lamps, xenon lamps, chemical lamps, electrodeless discharge lamps, and LEDs, all of which emit light in the wavelength range of 150 to 450 nm.
[0115] The amount of active energy ray irradiation (cumulative light amount) is 10 to 6000 mJ / cm from the viewpoint of curing. 2 is preferred, and 50 mJ / cm 2~5500mJ / cm 2 more preferably 100 mJ / cm 2 ~5000mJ / cm 2 is more preferably 200 mJ / cm 2 ~4000mJ / cm 2 is particularly preferred, and 300 mJ / cm 2 ~3000mJ / cm 2 is particularly preferred.
[0116] In another embodiment of the method for producing the present pressure-sensitive adhesive sheet, the pressure-sensitive adhesive composition can be dissolved in an appropriate solvent and various coating methods can be used. When the pressure-sensitive adhesive composition is in a syrup form, it is also possible to coat it without using a solvent. When using a coating method, the present pressure-sensitive adhesive sheet can also be obtained by curing it with heat, in addition to curing it by irradiation with active energy rays. When coating, the thickness of the present pressure-sensitive adhesive sheet can be adjusted by the coating thickness and the solids concentration of the coating liquid.
[0117] For example, the pressure-sensitive adhesive composition can be dissolved in a solvent, coated on a release film, dried, and cured by active energy ray irradiation to form the pressure-sensitive adhesive sheet. Furthermore, a release film may be laminated, if necessary. In this case, the pressure-sensitive adhesive composition may be coated on a release film, dried, cured by active energy ray irradiation, and a release film may be laminated thereon. Alternatively, the pressure-sensitive adhesive sheet may be formed by coating on a release film, drying, laminating a release film, and then curing by active energy ray irradiation.
[0118] The solvent is not particularly limited as long as it dissolves the pressure-sensitive adhesive composition, and examples thereof include ester solvents such as methyl acetate, ethyl acetate, butyl acetate, methyl acetoacetate, and ethyl acetoacetate; ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; aromatic solvents such as toluene and xylene; and alcohol solvents such as methanol, ethanol, and propyl alcohol. These can be used alone or in combination of two or more. Among them, ethyl acetate, acetone, methyl ethyl ketone, and toluene are preferred in terms of solubility, drying properties, cost, etc., and ethyl acetate is particularly preferred.
[0119] The amount of the solvent used is preferably 600 parts by mass or less, more preferably 500 parts by mass or less, even more preferably 400 parts by mass or less, and particularly preferably 300 parts by mass or less, per 100 parts by mass of the (meth)acrylic polymer (A) in terms of drying property. On the other hand, it is preferably 1 part by mass or more, more preferably 50 parts by mass or more, even more preferably 100 parts by mass or more, and particularly preferably 150 parts by mass or more. The coating method can be, for example, a conventional method such as roll coating, die coating, gravure coating, comma coating, screen printing, or bar coating.
[0120] The solvent content in the pressure-sensitive adhesive composition after drying is preferably 1% by mass or less, more preferably 0.5% by mass or less, particularly preferably 0.1% by mass or less, and most preferably 0% by mass.
[0121] The drying temperature is usually 40 to 150° C., more preferably 45 to 140° C., even more preferably 50 to 130° C., and particularly preferably 55 to 120° C. When the temperature is within this range, the solvent can be removed efficiently and relatively stably while suppressing thermal deformation of the release film.
[0122] The drying time is usually 1 to 30 minutes, more preferably 3 to 25 minutes, and even more preferably 5 to 20 minutes. When the drying time is within this range, the solvent can be removed efficiently and sufficiently.
[0123] Drying methods include, for example, drying with a dryer, drying with a heated roll, drying by blowing hot air onto the film, etc. Among these, using a dryer is preferred because it allows for uniform and easy drying. These methods can be used alone or in combination of two or more.
[0124] <<Adhesive Sheet with Release Film>> The present adhesive sheet can also be provided as an adhesive sheet with a release film (adhesive sheet laminate) by laminating a release film on one or both sides of an adhesive layer (the present adhesive sheet) made of the present adhesive composition. When release films are provided on both sides of the present adhesive sheet, a laminate configuration is preferably used in which a light-release film with a relatively low release strength and a heavy-release film with a relatively high release strength are laminated. When using an adhesive sheet with release films provided on both sides, first, one release film (light-release film) is peeled off to expose one side of the adhesive sheet, which is then bonded to a component of an image display device (referred to as a first component), and the other release film (heavy-release film) is peeled off to expose the other side of the adhesive sheet, to which another component of an image display device (referred to as a second component) is then bonded.
[0125] As such a release film, a known release film can be appropriately used. Examples of the material for the release film include films such as polyester films, polyolefin films, polycarbonate films, polystyrene films, acrylic films, triacetyl cellulose films, and fluororesin films that have been subjected to a release treatment by coating with a release agent such as silicone resin, and release paper, etc., and these can be appropriately selected and used. Among these, polyester films, and even more so polyethylene terephthalate (PET) films, particularly biaxially oriented PET films, are preferred because of their excellent transparency, mechanical strength, heat resistance, flexibility, etc. A release film can be used in which a release layer formed by curing a curable silicone-based release agent containing silicone resin as the main component on the above-mentioned substrate is provided.
[0126] The thickness of the release film is not particularly limited. In particular, from the viewpoint of processability and handling, the thickness is preferably 10 to 250 μm, more preferably 25 to 200 μm, and even more preferably 35 to 190 μm.
[0127] <Preferred use of the present pressure-sensitive adhesive sheet> The present pressure-sensitive adhesive sheet is suitably used for bonding optical components.Specifically, it is suitably used for bonding components constituting a display, particularly components used for manufacturing a display, and is used as a pressure-sensitive adhesive sheet for bonding image display panel and image display device components such as a protective panel or touch panel arranged on its front side (viewing side), or components constituting the image display device components.In addition, the same components as those described below can be used for the image display device components.
[0128] <<Laminate for Image Display Device>> A laminate for an image display device according to one example of the embodiment of the present invention (hereinafter, may be referred to as "the present laminate for an image display device") is a laminate for an image display device having a configuration in which two components of the image display device are laminated with the present pressure-sensitive adhesive sheet interposed therebetween. The present laminate for an image display device is preferably a laminate for an image display device having a configuration in which two components of the image display device are laminated with the present pressure-sensitive adhesive sheet interposed therebetween.
[0129] Of the components of the present laminate for an image display device, the present pressure-sensitive adhesive sheet has been described above, and the components other than the pressure-sensitive adhesive sheet will be described below.
[0130] <Image Display Device Components> Examples of image display device components constituting the present laminate for an image display device include flat panel image display device components and flexible image display device components. Examples of such image display device components include flexible displays such as liquid crystal displays and organic electroluminescence (EL) displays, cover lenses (cover films), polarizing plates, polarizers, retardation films, barrier films, viewing angle compensation films, brightness enhancement films, contrast enhancement films, diffusion films, semi-transmitting reflective films, electrode films, transparent conductive films, metal mesh films, and touch sensor films. Any one of these may be used alone or in combination. Examples include a combination of a flexible display with another image display device component, or a combination of a cover lens with another image display device component.
[0131] The term "flexible image display device component" refers to a bendable component, such as a component used in an image display device having a curved surface or a component that can be repeatedly bent. In particular, it is preferable that the component be a component that can be fixed to a curved shape with a curvature radius of 25 mm or more, and particularly a component that can withstand bending at a curvature radius of less than 25 mm, more preferably less than 3 mm.
[0132] In the above-described configuration, examples of components constituting the image display device components include resin sheets and glass. Examples of materials for such resin sheets include polyester resins, cycloolefin resins, triacetyl cellulose resins, polymethyl methacrylate resins, polyurethanes, epoxy resins, polyimide resins, and aramid resins. These may be one type of resin or two or more types of resins. Among these, a resin sheet containing at least one resin selected from the group consisting of polyester resins, cycloolefin resins, triacetyl cellulose resins, polymethyl methacrylate resins, epoxy resins, polyimide resins, aramid resins, and polyurethane resins as a primary component is preferred. Here, the term "primary component" refers to the component that accounts for the largest weight percentage among the components constituting the image display device components. Specifically, the resin sheet should account for 50% by weight or more of the resin composition (resin sheet) forming the image display device component, preferably 55% by weight or more, and particularly preferably 60% by weight or more.
[0133] <Method for manufacturing the present laminate for an image display device> The method for manufacturing the present laminate for an image display device is not particularly limited, and as described above, for example, the pressure-sensitive adhesive composition may be applied to a component of an image display device to form a pressure-sensitive adhesive sheet, or a pressure-sensitive adhesive sheet with a release film may be formed in advance and then laminated to a component of an image display device.
[0134] <<Image Display Device>> An image display device according to an example embodiment of the present invention (hereinafter may be referred to as "the image display device") is an image display device incorporating a laminate for an image display device having a configuration in which two image display device components are bonded together via the present pressure-sensitive adhesive sheet. For example, the image display device including the laminate can be formed by laminating the laminate for an image display device having a configuration in which two image display device components are bonded together via the present pressure-sensitive adhesive sheet onto another image display device component.
[0135] An example of an embodiment of the present invention will be described in detail below, but the present invention is not limited to the embodiment described below.
[0136] First, the raw materials of the pressure-sensitive adhesive compositions prepared in the examples will be described in detail.
[0137] <(Meth)acrylic polymer (A)> (Meth)acrylic polymer (A-1): An acrylic copolymer (weight average molecular weight: approximately 700,000) obtained by random copolymerization of 67 parts by mass of 2-ethylhexyl acrylate, 5 parts by mass of methyl acrylate, 10 parts by mass of ethyl acrylate, 4 parts by mass of 4-hydroxybutyl acrylate, and 14 parts by mass of hydroxyethyl acrylate.
[0138] <Photoinitiator (B)> Photoinitiator (b1-1): a photoinitiator having a radically polymerizable functional group having a carbon-carbon double bond represented by the following formula 2-1 and a thioxanthone structure as a radical generating group in the molecule (molar absorption coefficient at a wavelength of 405 nm: 1.7 × 10 3 L / mol cm)
[0139]
[0140] Photoinitiator (b1-2): A photoinitiator having a radical polymerizable functional group having a carbon-carbon double bond represented by the following formula 2-2 and a thioxanthone structure as a radical generating group in the molecule (molar absorption coefficient at a wavelength of 405 nm: 5.9 × 10 3 L / mol cm)
[0141]
[0142] Photoinitiator (b2-1): 2,4-diethylthioxanthone ("Omnirad DETX" manufactured by IGM, molar absorption coefficient at a wavelength of 405 nm: 3.3 × 10 3 L / mol cm)
[0143] Photoinitiator (b2-2): 4-methacryloyloxybenzophenone (manufactured by MCC Unitec Co., Ltd., molar absorption coefficient at a wavelength of 405 nm: 0 L / mol cm)
[0144] [Example 1] A pressure-sensitive adhesive composition was prepared by uniformly mixing 100 parts by mass of a (meth)acrylic polymer (A-1) and 0.3 parts by mass of a photoinitiator (b1-1). The pressure-sensitive adhesive composition was spread into a sheet having a thickness of 50 μm on a silicone release-treated release film (a PET film manufactured by Mitsubishi Chemical Corporation) having a thickness of 100 μm.
[0145] Next, a silicone release-treated 75 μm-thick release film (a PET film manufactured by Mitsubishi Chemical Corporation) was laminated on the sheet-like pressure-sensitive adhesive composition to form a laminate, and a pressure-sensitive adhesive sheet with a release film consisting of a release film / pressure-sensitive adhesive sheet / release film was obtained. Next, using a high-pressure mercury lamp, the integrated light amount at a wavelength of about 405 nm was measured using an ultraviolet integrating actinometer "UIT-250" (manufactured by Ushio Inc.) and a photodetector "UVD-C405" (manufactured by Ushio Inc.) through a UV-cut polyethylene terephthalate film ("O700E100" manufactured by Mitsubishi Chemical Corporation) (light transmittance at a wavelength of 380 nm of 0.7% and light transmittance at a wavelength of 405 nm of 87%), and the integrated light amount was measured at a wavelength of about 1000 mJ / cm on both surfaces of the pressure-sensitive adhesive sheet with a release film. 2 The adhesive sheet was semi-cured by irradiating it with light so that the adhesive sheet became curable with active energy rays.
[0146] Examples 2 and 3, Comparative Examples 1 and 2 Except for changing the adhesive composition to the formulation shown in Table 1, adhesive sheets with release films were prepared in the same manner as in Example 1.
[0147] [Measurement and Evaluation of Physical Properties] The pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples were subjected to the following various measurements and evaluations. The evaluation results are summarized in Table 1.
[0148] <Gel Fraction> For the pressure-sensitive adhesive sheets with release films prepared in the Examples and Comparative Examples, approximately 0.1 g of pressure-sensitive adhesive sheet pieces were collected from the pressure-sensitive adhesive sheets after peeling off the release films. The collected pressure-sensitive adhesive sheet pieces were wrapped in a pre-formed bag of SUS mesh (#150) with a mass X (g), and the bag was closed to prepare a sample, and the mass Y (g) of the sample was measured. The sample was immersed in ethyl acetate and stored in a dark place at 23°C for 24 hours, then removed and heated at 70°C for 4.5 hours to evaporate the ethyl acetate, and the mass Z (g) of the dried sample was measured. The gel fraction (X0) after primary curing was calculated from each measured mass using the following formula: Gel fraction (%) = [(Z-X) / (Y-X)] x 100
[0149] Furthermore, the pressure-sensitive adhesive sheets with release film produced in the examples and comparative examples were exposed to a high-pressure mercury lamp through a UV-blocking polyethylene terephthalate film ("O700E100" manufactured by Mitsubishi Chemical Corporation) (light transmittance at a wavelength of 380 nm is 0.7%, and light transmittance at a wavelength of 405 nm is 87%). The integrated light intensity at a wavelength of around 405 nm was measured using an ultraviolet integrating actinometer "UIT-250" (manufactured by Ushio Inc.) and a photodetector "UVD-C405" (manufactured by Ushio Inc.). The integrated light intensity was 3000 mJ / cm 2 The pressure-sensitive adhesive sheet was cured by irradiating it with light so that the gel fraction (X1) after secondary curing was calculated using the cured pressure-sensitive adhesive sheet in the same manner as for the gel fraction (X0).
[0150] <Chromaticity> The release films were peeled off from the pressure-sensitive adhesive sheets with release films produced in the Examples and Comparative Examples, and the exposed adhesive surfaces were sandwiched between two sheets of soda-lime glass (thickness 0.55 mm) to prepare bonded samples. The chromaticity (b*) of the bonded samples was measured using a spectrophotometer (Suga Test Instruments Co., Ltd.) "SC-T" under a D65 light source and a 10° field of view according to a method based on JIS K7103.
[0151] <Adhesive Strength> One release film was peeled off from the pressure-sensitive adhesive sheets with release films produced in the Examples and Comparative Examples, and a 100 μm thick polyethylene terephthalate film (Cosmoshine A4300 manufactured by Toyobo Co., Ltd.) was attached as a backing film to prepare a laminate. After cutting the laminate to a length of 150 mm and a width of 10 mm, the remaining release film was peeled off, and the exposed adhesive surface was brought into contact with soda-lime glass and a roll was moved back and forth once to roll-press the pressure-sensitive adhesive sheet. The resulting bonded product was aged at 60°C for 30 minutes and then finish-pasted. After that, the integrated light amount at a wavelength of about 405 nm was measured using a high-pressure mercury lamp through a UV-blocking polyethylene terephthalate film (Mitsubishi Chemical Corporation's "O700E100") (light transmittance at a wavelength of 380 nm is 0.7%, and light transmittance at a wavelength of 405 nm is 87%) using an ultraviolet integrating actinometer "UIT-250" (Ushio Inc.) and a photodetector "UVD-C405" (Ushio Inc.). The integrated light amount was 3000 mJ / cm at a wavelength of about 405 nm. 2 The adhesive sheet was cured by irradiating light so that the adhesive strength was such ...
[0152]
[0153] As shown in Table 1, the pressure-sensitive adhesive sheets of Examples 1 to 3, which used photoinitiators having a radical polymerizable functional group with a carbon-carbon double bond and a radical generating group in the molecule and a molar absorption coefficient at 405 nm of 30 (L / mol cm) or more, had sufficient curability with light at a wavelength of 405 nm and low chromaticity (b*) values, resulting in favorable results. On the other hand, the pressure-sensitive adhesive sheet of Comparative Example 1 used a photoinitiator that did not have a radical polymerizable functional group with a carbon-carbon double bond, and despite having a sufficiently large molar absorption coefficient at a wavelength of 405 nm, it exhibited poor curability with light at a wavelength of 405 nm. Furthermore, the pressure-sensitive adhesive sheet of Comparative Example 2 used a photoinitiator that had a radical polymerizable functional group with a carbon-carbon double bond and a radical generating group in the molecule but had a molar absorption coefficient at 405 nm of 30 (L / mol cm) or less, and exhibited a small molar absorption coefficient at a wavelength of 405 nm and poor curability with light at a wavelength of 405 nm.
[0154] The pressure-sensitive adhesive composition of the present invention can be cured with energy rays on the relatively long wavelength side (for example, energy rays with a wavelength longer than 380 nm, particularly active energy rays with a wavelength of 405 nm), and produces few photodecomposition products, making it suitable for use as a pressure-sensitive adhesive sheet used for bonding optical members, particularly a pressure-sensitive adhesive sheet for an organic EL display device.
Claims
1. A pressure-sensitive adhesive composition used for bonding optical components, comprising a (meth)acrylic polymer (A) and a photoinitiator (B), wherein the photoinitiator (B) is a compound having a radically polymerizable functional group having a carbon-carbon double bond and a radical generating group in its molecule, and the photoinitiator (b1) has a molar absorption coefficient at 405 nm of 30 (L / mol cm) or more.
2. The pressure-sensitive adhesive composition according to claim 1, wherein the photoinitiator (b1) comprises at least one selected from the group consisting of hydrogen abstraction photoinitiators having a structure in which the radical generating group is excited by irradiation with active energy rays and causes a hydrogen abstraction reaction to generate radicals, and intramolecular cleavage photoinitiators in which the radical generating group is excited by irradiation with active energy rays and cleaves intramolecularly to generate radicals.
3. The pressure-sensitive adhesive composition according to claim 1, wherein the photoinitiator (b1) is a hydrogen abstraction photoinitiator having a structure in which the radical polymerizable functional group thereof is a (meth)acryloyl group, and the radical generating group is excited by irradiation with active energy rays to cause a hydrogen abstraction reaction, thereby generating radicals.
4. The pressure-sensitive adhesive composition according to claim 1, wherein the radical generating group in the photoinitiator (b1) includes at least one structure selected from the group consisting of a benzoin structure, a benzil ketal structure, an acylphosphine oxide structure, an α-aminoacetophenone structure, an α-hydroxyacetophenone structure, a benzophenone structure, a thioxanthone structure, an anthraquinone structure, a phenylglyoxylate structure, and an oxime ester structure.
5. The pressure-sensitive adhesive composition according to claim 1, wherein the radical generating group in the photoinitiator (b1) has a thioxanthone structure.
6. The pressure-sensitive adhesive composition according to claim 1, wherein the content of the photoinitiator (B) is 0.01 parts by mass or more per 100 parts by mass of the (meth)acrylic polymer (A).
7. The pressure-sensitive adhesive composition according to claim 1, wherein the content of the photoinitiator (b1) in the photoinitiator (B) is 30 mass% or more based on the total mass of the photoinitiator (B).
8. The pressure-sensitive adhesive composition according to claim 1, wherein the (meth)acrylic polymer (A) comprises a structural unit derived from an alkyl (meth)acrylate (m1) having a linear or branched alkyl group having 3 to 30 carbon atoms in the alkyl group, and at least one structural unit selected from a structural unit derived from a hydroxyl group-containing monomer (a2) and a structural unit derived from a nitrogen-containing monomer (a3).
9. A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition according to any one of claims 1 to 8.
10. The pressure-sensitive adhesive sheet according to claim 9, having a gel fraction (X0) of 20% or more.
11. The pressure-sensitive adhesive sheet has active energy ray curing properties, and the pressure-sensitive adhesive sheet is irradiated with active energy rays having a wavelength of 405 nm at an integrated light amount of 2000 to 4000 mJ / cm 2 The pressure-sensitive adhesive sheet according to claim 10, wherein the gel fraction (X1) when irradiated at any irradiation amount within the range of 100 to 300 nm is 30% or more.
12. The pressure-sensitive adhesive sheet according to claim 11, wherein the difference (X1-X0) between the gel fraction (X1) and the gel fraction (X0) is 10% or more.
13. The pressure-sensitive adhesive sheet according to claim 9, which is used for bonding optical members.
14. An adhesive sheet with a release film, comprising the adhesive sheet according to claim 9 and a release film laminated together.
15. A laminate for an image display device, comprising two optical members laminated together via the pressure-sensitive adhesive sheet according to claim 9.
16. An image display device comprising the laminate for an image display device according to claim 15.
17. An adhesive sheet for an organic EL display device, comprising the adhesive sheet according to claim 9.
Citation Information
Patent Citations
Novel thioxanthone visible light initiator as well as preparation method and application thereof
CN113698382A
Non-yellowing polymerizable composition and method for producing polymerized material
JP2009203299A
Photocurable pressure-sensitive adhesive sheet, photocurable pressure-sensitive adhesive sheet laminate, production method for photocurable pressure-sensitive adhesive sheet laminate, and production method for image display panel laminate
WO2019031426A1