Diamond electrode

The diamond electrode with a niobium carbide and niobium oxide transition layer addresses the durability issues of diamond electrodes by improving adhesion and reducing peeling, ensuring effective ozone generation in acidic environments.

WO2024202936A1PCT designated stage expired Publication Date: 2024-10-03SUMITOMO CHEM CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/007809
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-01
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Diamond electrodes used for electrochemical reactions, such as ozone generation, face durability issues due to peeling of the conductive diamond film, particularly in strong acidic environments, where existing intermediate layers like carbides have poor corrosion resistance.

Method used

A diamond electrode with a transition layer composed of niobium carbide and niobium oxide microcrystals is formed between the substrate and the conductive diamond film, enhancing adhesion and reducing pinhole formation, thereby improving durability and preventing peeling.

Benefits of technology

The use of a transition layer with niobium carbide and niobium oxide microcrystals increases the nucleation density of diamond crystals, suppresses peeling, and enhances the durability of the diamond electrode, even in harsh acidic conditions, maintaining high ozone generation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024007809_03102024_PF_FP_ABST
    Figure JP2024007809_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This diamond electrode includes: a substrate formed of niobium metal; a conductive diamond film that is formed on at least one main surface of the substrate; and a transition layer that is formed between the substrate and the conductive diamond film. The transition layer is formed of an aggregate of microcrystals containing niobium and carbon as the main components and microcrystals containing niobium and oxygen as the main components.
Need to check novelty before this filing date? Find Prior Art

Description

Diamond electrodes

[0001] The present invention relates to a method for manufacturing a diamond electrode.

[0002] Conductive diamond has a wide potential window in both aqueous and non-aqueous systems and a small background current, making it known as an electrode material capable of stable electrochemical reactions over a wide potential range.

[0003] For example, Patent Document 1 discloses a method for producing a conductive diamond electrode, which comprises plastically processing at least the surface of an electrode substrate comprising a material selected from a valve metal selected from the group consisting of niobium, tantalum, titanium, and zirconium and a metal-based alloy thereof, and then heat-treating the electrode substrate in a vacuum or in an inert atmosphere to form a conductive diamond film on the heat-treated surface of the electrode substrate.

[0004] Patent No. 4456378

[0005] An object of the present invention is to provide a technique capable of suppressing peeling of a conductive diamond film and improving the durability of a diamond electrode.

[0006] According to one aspect of the present invention, there is provided a diamond electrode having: a substrate made of metal niobium; a conductive diamond film formed on at least one major surface of the substrate; and a transition layer formed between the substrate and the conductive diamond film, wherein the transition layer is composed of microcrystals mainly composed of niobium and carbon, and an aggregate of microcrystals mainly composed of niobium and oxygen.

[0007] According to the present invention, it is possible to provide a technique that can suppress peeling of the conductive diamond film and improve the durability of the diamond electrode.

[0008] Fig. 1 is a schematic diagram showing a cross section of a diamond electrode 10 according to an embodiment of the present invention. Fig. 2 is an enlarged schematic diagram of the vicinity of the boundary between the transition layer 30 and the conductive diamond film 40 of the diamond electrode 10 according to an embodiment of the present invention. Fig. 3 is a flowchart showing an example of a method for manufacturing the diamond electrode 10 according to an embodiment of the present invention. Fig. 4 is a schematic diagram illustrating the porous portion formation step S102 according to an embodiment of the present invention. Fig. 5 is a flowchart showing an example of a method for manufacturing the diamond electrode 10 according to another embodiment of the present invention. Fig. 6 is a cross-sectional photograph of sample 1 according to an example of the present invention. Fig. 7 is a diagram showing the results of composition analysis by TEM-EDX of sample 1 according to an example of the present invention.

[0009] <Insights Gained by the Inventors> First, insights gained by the inventors will be described.

[0010] Diamond electrodes that have been made conductive by incorporating boron or other elements can be used to generate oxidizing agents such as ozone. Durability is a major issue for such diamond electrodes. While the technology described in Patent Document 1 and elsewhere has improved the adhesion and peel strength between the substrate and the diamond film, it has proven difficult to achieve a practical level of durability.

[0011] For example, paragraph 0009 of Patent Document 1 states that "if the intermediate layer is made of carbide derived from the substrate, it is expected that the adhesion of the diamond film will be improved due to the relationship between the substrate, the carbide growing from the substrate, and the diamond that generates using the carbide as a nucleus. However, in reality, carbides are often inferior in corrosion resistance to oxides when a potential is applied as an anode in a strong acidic environment. Carbide is likely to be formed in a substrate that comes into contact with hydrocarbon radicals or diamond at high temperatures, so care must be taken when using it as an anode." From the perspective of improving durability, it has been thought that it is preferable to prevent carbide from being formed as much as possible in the intermediate layer between the substrate and the diamond film.

[0012] The inventors of the present invention have conducted extensive research into the above-mentioned problems. As a result, they have found that by forming an intermediate layer (transition layer) consisting of an aggregate of carbide microcrystals and oxide microcrystals, it is possible to suppress the occurrence of pinholes, and furthermore, the binder effect of the oxide microcrystals can suppress the peeling of the diamond film. This makes it possible to further improve the durability of diamond electrodes.

[0013] [Details of the embodiment of the present invention] Next, an embodiment of the present invention will be described below with reference to the drawings. Note that the present invention is not limited to these examples, but is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims.

[0014] <Embodiments of the present invention> (1) Configuration of diamond electrode 10 First, the configuration of the diamond electrode 10 of this embodiment will be described. The diamond electrode 10 of this embodiment can be used, for example, as a diamond electrode 10 for electrochemical reactions (for example, for ozone generation). In this case, it is possible to suppress deterioration of the diamond electrode 10 due to electrical conduction and improve durability. It is also possible to suppress peeling of the conductive diamond film 40 and improve durability of the diamond electrode 10.

[0015] 1 is a schematic diagram showing a cross section of a diamond electrode 10 of this embodiment. As shown in FIG. 1, the diamond electrode 10 has, for example, a substrate 20, a transition layer 30, and a conductive diamond film 40. The transition layer 30 also has a first transition layer 31 and a second transition layer 32.

[0016] The substrate 20 is, for example, a flat niobium metal plate material for depositing the conductive diamond film 40 and for supporting the conductive diamond film 40. The size and thickness of the main surface of the substrate 20 are not particularly limited, but for example, the main surface has a rectangular shape with one side measuring 20 mm or more and 500 mm or less, and the thickness is 0.5 mm or more and 5 mm or less.

[0017] The transition layer 30 is formed, for example, between the substrate 20 and the conductive diamond film 40, and functions as an intermediate layer for increasing the nucleation density of diamond crystals. The transition layer 30 is made up of an aggregate of microcrystals whose main components are niobium and carbon (niobium carbide microcrystals) and microcrystals whose main components are niobium and oxygen (niobium oxide microcrystals). The presence of the transition layer 30 makes it possible to efficiently increase the nucleation density of diamond crystals for forming the conductive diamond film 40. Furthermore, the microcrystals whose main components are niobium and oxygen exert a binder effect, which makes it possible to suppress peeling of the conductive diamond film 40.

[0018] The thickness of the transition layer 30 is preferably, for example, 0.5 μm or more and 10 μm or less (more preferably, 0.8 μm or more and 2.5 μm or less). In other words, it is preferable that the minimum thickness and the maximum thickness of the transition layer 30 are within the range of 0.5 μm or more and 10 μm or less (more preferably, 0.8 μm or more and 2.5 μm or less). If the thickness of the transition layer 30 is less than 0.5 μm, it may be difficult to form a continuous transition layer 30. In contrast, by setting the thickness of the transition layer 30 to 0.5 μm or more, it is easier to form a continuous transition layer 30. On the other hand, if the thickness of the transition layer 30 exceeds 10 μm, internal stress increases and the diamond electrode 10 may warp. In contrast, by setting the thickness of the transition layer 30 to 10 μm or less, it is possible to reduce the internal stress and reduce the warpage of the diamond electrode 10.

[0019] The conductive diamond film 40 is, for example, a polycrystalline film having conductivity, which is formed on at least one main surface of the substrate 20 via the transition layer 30. The conductive diamond film 40 may be either a polycrystalline diamond film or a diamond-like carbon (DLC) film. The conductive diamond film 40 may be, for example, a film containing 1×10 boron. 19 cm -3 1x10 or more 22 cm -3 It is preferable that the conductive diamond film 40 contains the following concentration: The thickness of the conductive diamond film 40 is, for example, 0.5 μm or more and 10 μm or less, and from the viewpoint of maintaining a balance between durability and cost, it is preferably 1 μm or more and 5 μm or less.

[0020] When the surface of the conductive diamond film 40 is observed using, for example, a scanning electron microscope (for example, 5000 times magnification), it is preferable that there are no pinholes within a 20 μm × 20 μm field of view that reach the substrate 20 or the transition layer 30. This reduces the risk that the strongly acidic liquid will come into contact with the substrate 20 or the transition layer 30, even if the diamond electrode 10 is used in a strongly acidic solution, and therefore makes it possible to improve the durability of the diamond electrode 10. From the viewpoint of further improving the durability of the diamond electrode 10, it is more preferable that there are no pinholes within a 1 mm × 1 mm field of view that reach the substrate 20 or the transition layer 30, and it is particularly preferable that there are no pinholes across the entire surface of the conductive diamond film 40.

[0021] Furthermore, even when the cross section (longitudinal or transverse section) of the conductive diamond film 40 is observed using, for example, a scanning electron microscope (for example, 5000 times magnification), it is preferable that there are no pinholes that reach the substrate 20 or the transition layer 30 within a field of view of 20 μm × 20 μm. In other words, the conductive diamond film 40 has reduced pinholes not only visible from the surface but also internal pinholes. This makes it possible to further improve the durability of the diamond electrode 10. It is more preferable that there are no pinholes that reach the substrate 20 or the transition layer 30 within a field of view of 1 mm × 1 mm in the cross section (longitudinal or transverse section) of the conductive diamond film 40, and it is particularly preferable that there are no pinholes across the entire cross section of the conductive diamond film 40.

[0022] When the cross section of the diamond electrode 10 is observed using, for example, a scanning electron microscope (for example, 5000 times magnification), it is preferable that a continuous transition layer 30 having a thickness of 0.5 μm or more is formed over a width of 20 μm or more (the length in the direction parallel to the main surface of the substrate 20). This sufficiently increases the nucleation density of diamond crystals for forming the conductive diamond film 40, and can suppress the occurrence of pinholes. Note that, from the viewpoint of further suppressing the occurrence of pinholes, it is more preferable that a continuous transition layer 30 having a thickness of 0.5 μm or more is formed over a width of 1 mm or more, and it is particularly preferable that a continuous transition layer 30 having a thickness of 0.5 μm or more is formed over the entire main surface of the substrate 20.

[0023] It is preferable that the average composition of niobium in the transition layer 30 continuously decreases from the substrate 20 side to the conductive diamond film 40 side, thereby making it possible to suppress peeling of the conductive diamond film 40.

[0024] The microcrystals mainly composed of niobium and carbon contained in the transition layer 30 are niobium carbide microcrystals of the chemical formula NbC (hereinafter also referred to as NbC microcrystals) or niobium carbide microcrystals of the chemical formula Nb 2 Niobium carbide microcrystals (hereinafter referred to as Nb 2 This makes it possible to efficiently increase the density of nuclei generated from diamond crystals for forming the conductive diamond film 40.

[0025] The first transition layer 31 has an NbC microcrystal content of Nb 2 The second transition layer 32 contains Nb 2 It is preferable that the abundance ratio of C microcrystals is higher than the abundance ratio of NbC microcrystals. Since the transition layer 30 is carbonized from the surface side, NbC with a high C component is likely to be formed in the first transition layer 31 where the carbon source 22 diffused from the surface side is large, and NbC with a high Nb component is likely to be formed in the second transition layer 32 where the carbon source 22 diffused from the surface side is small. 2C is easily formed. In this way, the first transition layer 31 of the transition layer 30 that is present on the conductive diamond film 40 side has a higher C component than the second transition layer 32 that is present on the substrate 20 side, and therefore the nucleation density of diamond crystals for forming the conductive diamond film 40 can be sufficiently increased and the occurrence of pinholes can be suppressed.

[0026] The crystallite diameter of the niobium carbide microcrystals contained in the first transition layer 31 is smaller than the crystallite diameter of the niobium carbide microcrystals contained in the second transition layer 32. Specifically, the crystallite diameter of the niobium carbide microcrystals contained in the first transition layer 31 is, for example, 5 nm or more and 100 nm or less, and the crystallite diameter of the niobium carbide microcrystals contained in the second transition layer 32 is, for example, 10 nm or more and 2000 nm or less. The crystallite diameter of each microcrystal can be measured, for example, by the Scherrer method of XRD. When the first transition layer 31 is measured by XRD, peaks such as NbC(111), NbC(200), NbC(222), and NbC(400) are observed, but the NbC(200) peak is the strongest. Therefore, in this specification, unless otherwise specified, the crystallite diameter of the niobium carbide microcrystals contained in the first transition layer 31 is calculated from the NbC(200) peak in the XRD. Similarly, the crystallite diameter of the niobium carbide microcrystals contained in the second transition layer 32 is calculated from the NbC(200) peak in the XRD. 2 Therefore, in this specification, the crystallite diameter of the niobium carbide microcrystals contained in the first transition layer 31 may be rephrased as the crystallite diameter of the NbC microcrystals, and the crystallite diameter of the niobium carbide microcrystals contained in the second transition layer 32 may be rephrased as the crystallite diameter of the NbC microcrystals. 2 It may also be rephrased as the crystallite size of the C crystallites.

[0027] The crystallite diameter of the NbC microcrystals contained in the first transition layer 31 is, for example, preferably 5 nm or more and 100 nm or less, and more preferably 5 nm or more and 60 nm or less. If the crystallite diameter of the NbC microcrystals is outside the above range, it may be difficult to form a continuous transition layer 30 having a thickness of 0.5 μm or more. In contrast, by setting the crystallite diameter of the NbC microcrystals within the above range, it becomes easier to form a continuous transition layer 30 having a thickness of 0.5 μm or more, and as a result, it becomes easier to suppress the occurrence of pinholes. In addition, the NbC microcrystals contained in the second transition layer 32 2The crystallite size of the C microcrystals is, for example, preferably 10 nm or more and 2000 nm or less, and more preferably 20 nm or more and 1000 nm or less.

[0028] The microcrystals contained in the transition layer 30 and containing niobium and oxygen as main components are niobium oxide microcrystals (hereinafter also referred to as NbO microcrystals) of the chemical formula NbO, and it is preferable that the NbO microcrystals are mixed in the first transition layer 31. This enhances the binder effect, and makes it possible to further suppress peeling of the conductive diamond film 40.

[0029] The crystallite diameter of the NbO microcrystals is preferably, for example, 5 nm or more and 100 nm or less, and more preferably 5 nm or more and 60 nm or less. By setting the crystallite diameter of the NbO microcrystals within the above range, the binder effect is more effectively exhibited, and peeling of the conductive diamond film 40 can be further suppressed. The crystallite diameter of the NbO microcrystals can also be measured by the Scherrer method of XRD. When measuring NbO microcrystals by XRD, peaks such as NbO (100), NbO (110), NbO (111), NbO (200), and NbO (220) are observed, but the peak of NbC (111) is the strongest. Therefore, in this specification, unless otherwise specified, the crystallite diameter of the niobium oxide microcrystals contained in the transition layer 30 is calculated from the peak of NbO (111) in XRD.

[0030] The thickness of the first transition layer 31 is preferably, for example, 10 nm to 500 nm, and the thickness of the second transition layer 32 is preferably, for example, 1 μm to 10 μm. The thickness of the second transition layer 32 is preferably 1.5 to 10 times the thickness of the first transition layer 31. By setting the thicknesses of the first transition layer 31 and the second transition layer 32 within the above ranges, it becomes easier to form a continuous transition layer 30, and warping of the diamond electrode 10 can be reduced.

[0031] The volumetric abundance ratio of NbO microcrystals to NbC microcrystals in the first transition layer 31 is preferably, for example, 50% or more and 100% or less (i.e., the NbO microcrystals are present in an amount equal to or more than half the amount of the NbC microcrystals). If the volumetric abundance ratio of NbO microcrystals is less than 50%, the binder effect is insufficient and it may be difficult to suppress peeling of the conductive diamond film 40. On the other hand, by setting the volumetric abundance ratio of NbO microcrystals to 50% or more, the binder effect is fully exerted and peeling of the conductive diamond film 40 can be further suppressed. On the other hand, if the volumetric abundance ratio of NbO microcrystals exceeds 100%, the nucleation density of diamond crystals for forming the conductive diamond film 40 may decrease. On the other hand, by setting the volumetric abundance ratio of NbO microcrystals to 100% or less, the nucleation density of diamond crystals for forming the conductive diamond film 40 can be efficiently increased.

[0032] Figure 2 is an enlarged schematic view of the vicinity of the boundary between the transition layer 30 and the conductive diamond film 40. As shown in Figure 2, the transition layer 30 preferably has a porous portion 33 having a large number of voids. This reduces the difference in thermal expansion coefficient between niobium and the conductive diamond film 40, and prevents the conductive diamond film 40 from peeling off. In other words, it is possible to further improve the durability of the diamond electrode 10.

[0033] 2, the porous portion 33 is preferably present in the vicinity of the boundary between the conductive diamond film 40 inside the transition layer 30 (for example, the first transition layer 31). This can further enhance the effect of reducing the difference in thermal expansion coefficient between niobium and the conductive diamond film 40. In this specification, the vicinity of the boundary between the conductive diamond film 40 inside the transition layer 30 means, for example, a region from the boundary between the transition layer 30 and the conductive diamond film 40 toward the transition layer 30, up to a depth of 1 μm.

[0034] The porosity of the porous portion 33 is preferably, for example, 20% or more and 80% or less. If the porosity of the porous portion 33 is less than 20%, it may be difficult to obtain the effect of alleviating the difference in thermal expansion coefficients. In contrast, by setting the porosity of the porous portion 33 to 20% or more, the effect of alleviating the difference in thermal expansion coefficients can be sufficiently obtained. On the other hand, if the porosity of the porous portion 33 exceeds 80%, the strength of the diamond electrode 10 may be reduced. In contrast, by setting the porosity to 80% or less, the strength of the diamond electrode 10 can be maintained. When measuring the porosity of the porous portion 33, for example, the cross section of the porous portion 33 is observed using a scanning electron microscope, and the total area Sv of voids present within any observation field in the porous portion 33 is calculated by image analysis, and the ratio of the total area Sv of voids to the area S of the observation field is taken as the porosity of the porous portion 33.

[0035] (2) Manufacturing Method of Diamond Electrode 10 Next, a description will be given of a manufacturing method of the diamond electrode 10 of this embodiment. As described above, the diamond electrode 10 of this embodiment can be used as a diamond electrode 10 for electrochemical reactions (for example, for generating ozone).

[0036] Fig. 3 is a flow chart showing an example of the manufacturing method of the diamond electrode 10 of this embodiment. As shown in Fig. 3, the manufacturing method of the diamond electrode 10 of this embodiment has, for example, a porous portion forming step S102, a carbon source embedding step S103, a niobium carbide layer forming step S105, an oxidation step S106, and a diamond film depositing step S107. In this embodiment, the case where the diamond electrode 10 is manufactured from a substrate 20 made of metal niobium will be described.

[0037] (Porous portion forming step S102) Figure 4 is a schematic diagram illustrating the porous portion forming step S102. As shown in Figure 4, the porous portion forming step S102 is, for example, a step of forming a porous portion 33 having a large number of voids inside at least one main surface of the substrate 20. By forming the porous portion 33, the voids in the porous portion 33 relieve distortion caused by the difference in thermal expansion coefficient between niobium and the conductive diamond film 40, thereby suppressing peeling of the conductive diamond film 40.

[0038] In the porous portion forming step S102, for example, the main surface of the substrate 20 may be subjected to plastic deformation (e.g., rough-surface pressing) to a depth of 1 μm or more, followed by heat treatment of the substrate 20 in a hydrogen atmosphere to form the porous portion 33. The purpose of the plastic deformation is to increase the contact area between the niobium surface and hydrogen and to promote hydrogen diffusion by introducing processing strain into the niobium surface. Heat treatment of the substrate 20 in a hydrogen atmosphere embrittles the metallic niobium in the plastically deformed region. During subsequent cooling to room temperature, microcracks develop in the embrittled metallic niobium, which then propagate into voids. The number and size of the microcracks (or voids) that develop can be controlled by the heat treatment conditions (temperature, time, cooling rate, etc.). From the perspective of efficiently forming a large number of voids in the porous portion 33, the substrate 20 may be further subjected to mechanical processing such as pressing after heat treatment and cooling. The following are examples of heat treatment conditions in the porous portion forming step S102. Heat treatment temperature (substrate temperature): 600 to 800 degrees Heat treatment time: 30 to 90 minutes Cooling rate: 10 to 200 degrees / minute The hydrogen bonded to the metallic niobium by the above embrittlement treatment is removed in the niobium carbide layer formation step S105 described below, so that it does not ultimately remain in large amounts in the substrate 20 and does not adversely affect the strength of the diamond electrode 10, etc.

[0039] In the porous portion forming step S102, it is preferable to form the porous portion 33 so that the porosity of the porous portion 33 is, for example, 20% or more and 80% or less. If the porosity of the porous portion 33 is less than 20%, it may be difficult to obtain the effect of alleviating the difference in thermal expansion coefficients. In contrast, by setting the porosity of the porous portion 33 to 20% or more, it is possible to sufficiently obtain the effect of alleviating the difference in thermal expansion coefficients. On the other hand, if the porosity of the porous portion 33 exceeds 80%, the strength of the diamond electrode 10 may decrease. In contrast, by setting the porosity to 80% or less, the strength of the diamond electrode 10 can be maintained.

[0040] The porous portion forming step S102 may be omitted. In this case, the porous portion 33 is not formed, but the subsequent steps can form the transition layer 30 consisting of an aggregate of microcrystals mainly composed of niobium and carbon and microcrystals mainly composed of niobium and oxygen, thereby efficiently increasing the nucleation density of diamond crystals for forming the conductive diamond film 40. Furthermore, the microcrystals mainly composed of niobium and oxygen exert a binder effect, which can suppress peeling of the conductive diamond film 40.

[0041] (Carbon Source Embedding Step S103) The carbon source embedding step S103 is a step of embedding a carbon source 22 made of a solid carbon or carbon compound inside the main surface of the substrate 20. Specifically, for example, the carbon source 22 is sprinkled on the surface of the substrate 20 that has been subjected to plastic deformation processing to form a porous portion 33, and the surface is rubbed against a substrate 20 of the same size, etc., to embed the carbon source 22 into the surface of the substrate 20 while pulverizing the carbon source 22 until it reaches a size similar to the voids in the porous portion 33 (for example, an average particle size of 200 nm or less). Because the carbon source 22 is solid, it is possible to introduce carbon atoms into the main surface of the substrate 20 at a higher concentration than with a hydrocarbon gas, etc. This facilitates diffusion of carbon atoms into the metal niobium, making it easier to form a continuous transition layer 30.

[0042] As the carbon source 22, for example, graphite, boron carbide, diamond powder, etc. can be used. When diamond powder is used as the carbon source 22, at least the outer periphery of the carbon source 22 should be an amorphous layer (sp 2 It is preferable to use diamond powder covered with carbon (carbon). From the viewpoints of increasing reactivity with metallic niobium and reducing costs, it is preferable to use graphite as the carbon source 22.

[0043] The average particle size of the carbon source 22 is preferably 200 nm or less. This makes it easier to embed the carbon source 22 inside the substrate 20. In addition, the surface area of ​​the carbon source 22 is increased, which can improve the reactivity with niobium metal. The lower limit of the average particle size of the carbon source 22 is not particularly limited, but is, for example, 5 nm or more.

[0044] In the carbon source embedding step S103, when graphite (average particle size 5 to 200 nm) is embedded inside the main surface of the substrate 20 as the carbon source 22, a niobium plate 1 cm 2 The amount of graphite (carbon source 22) used per cm is preferably, for example, 200 μg or more and 1000 μg or less. 2 If the amount of carbon source 22 is less than 200 μg / cm 3 , the carbonization of metal niobium may be insufficient, making it difficult to form a continuous transition layer 30. 2 If the amount of carbon source 22 used is less than 200 μg / cm, the hydrogen atoms bonded to the metal niobium cannot be completely released in the porous portion forming step S102, and embrittlement regions may remain, making the diamond film more susceptible to peeling. 2 By using the carbon source 22 in an amount of 1000 μg / cm or more, the niobium metal is sufficiently carbonized, making it easier to form a continuous transition layer 30, and also removing hydrogen atoms bonded to the niobium metal, thereby eliminating embrittlement regions of the niobium metal. 2 If the amount of carbon source 22 used exceeds 1000 μg / cm 3 , a large amount of carbon source 22 will remain after the formation of the transition layer 30, which may adversely affect the deposition of the conductive diamond film 40. 2 or less, it is possible to reduce the amount of residual carbon source 22. Furthermore, from the viewpoint of reducing the energy (cost) required for embedding the carbon source 22, it is preferable to embed the carbon source 22 to a depth of 1 μm or less. When checking the carbon source 22 inside the main surface of the substrate 20, for example, a cross-section of the substrate 20 (for example, at a depth of approximately 1 μm) may be observed using a transmission electron microscope.

[0045] (Niobium carbide layer forming step S105) The niobium carbide layer forming step S105 is a step in which the substrate 20 is heat-treated to react with metallic niobium and the carbon source 22, thereby forming a niobium carbide layer (which will become the transition layer 30 in a later step) that continuously covers the main surface of the substrate 20. This makes it possible to suppress the occurrence of pinholes on the surface of the conductive diamond film 40. Furthermore, because the niobium carbide layer (transition layer 30) has porous portions 33, peeling of the conductive diamond film 40 can be suppressed.

[0046] The niobium carbide layer forming step S105 also has the effect of removing hydrogen that has bonded to metallic niobium by the embrittlement treatment in the porous portion forming step S102 from the substrate 20. In addition, the voids formed in the porous portion forming step S102 can be transformed into a rounded shape by this heat treatment.

[0047] In the niobium carbide layer forming step S105, for example, a hot filament CVD apparatus described below can be used as a heating furnace for heat treatment to form the niobium carbide layer.

[0048] In the niobium carbide layer forming step S105, the heat treatment is preferably performed in an inert atmosphere (for example, a nitrogen atmosphere or a rare gas atmosphere). In an oxidizing atmosphere such as air, the niobium carbide layer may be reduced and converted into a pure niobium layer. In this case, it becomes difficult to form a uniform conductive diamond film 40. In contrast, by performing the heat treatment in an inert atmosphere, it becomes easier to form a niobium carbide layer, and the conductive diamond film 40 can be formed uniformly.

[0049] The conditions for the heat treatment in the niobium carbide layer forming step S105 are, for example, as follows: Heat treatment temperature (substrate temperature): 550 to 850 degrees; Pressure: 10 to 50 Torr; Heat treatment time: 30 to 120 minutes.

[0050] In the niobium carbide layer forming step S105, it is preferable to form the niobium carbide layer so that the crystallite diameter of the NbC microcrystals contained in the upper part of the niobium carbide layer (the part that will become the first transition layer 31) is, for example, 1 nm or more and 100 nm or less, more preferably 5 nm or more and 60 nm or less. This makes it easier to form a continuous niobium carbide layer, making it easier to suppress the occurrence of pinholes. Note that, in order to reduce the crystallite diameter of the NbC microcrystals contained in the upper part of the niobium carbide layer, it is effective to previously subject the metallic niobium in the region that will become the first transition layer 31 to plastic deformation processing in the porous portion forming step S102 to reduce the crystallite diameter of the metallic niobium.

[0051] (Oxidation step S106) The oxidation step S106 is a step of subjecting the substrate 20 to heat treatment in an atmosphere containing an oxidizing gas, and reacting the metallic niobium (or niobium carbide) of the niobium carbide layer with oxygen atoms to introduce niobium oxide microcrystals into a part of the niobium carbide layer, thereby forming the niobium carbide layer into the transition layer 30. Specifically, after the niobium carbide layer formation step S105 is performed in an inert atmosphere, oxygen gas or carbon dioxide gas is introduced into the heating furnace and heat treatment is performed. This allows the niobium oxide microcrystals to exert a binder effect, thereby suppressing peeling of the conductive diamond film 40. Note that using carbon dioxide does not rapidly oxidize the niobium surface, suppresses residual strain on the niobium surface, and allows for good subsequent deposition of the conductive diamond film 40, so it is preferable to use carbon dioxide gas in the oxidation step S106.

[0052] In the oxidation step S106, it is preferable to control the heat treatment conditions so that NbO microcrystals are introduced into the upper part of the niobium carbide layer (the part that will become the first transition layer 31). This enhances the binder effect, and makes it possible to further suppress peeling of the conductive diamond film 40.

[0053] In the oxidation step S106, it is preferable to control the heat treatment conditions so that the volumetric abundance ratio of NbO microcrystals to NbC microcrystals in the upper part of the niobium carbide layer (the part that will become the first transition layer 31) is 50% or more and 100% or less. This makes it possible to fully exert the binder effect and further suppress peeling of the conductive diamond film 40. In addition, the nucleation density of diamond crystals for forming the conductive diamond film 40 can be efficiently increased.

[0054] In the oxidation step S106, the transition layer 30 can be formed using, for example, a hot filament CVD apparatus (described later) as a heating furnace for heat treatment.

[0055] The conditions for the heat treatment in the oxidation step S106 are, for example, as follows: Heat treatment temperature (substrate temperature): 800 to 1000 degrees Pressure: 750 Torr (atmospheric pressure) Oxygen mole fraction (when oxygen gas is used): 0.4 (Note that when carbon dioxide gas is used, the amount of carbon dioxide gas may be adjusted to correspond to an oxygen mole fraction of 0.4, taking into account the reactivity of niobium with carbon dioxide gas.) Heat treatment time: 30 to 120 minutes

[0056] (Diamond Film Deposition Step S107) The diamond film deposition step S107 is, for example, a step of depositing a conductive diamond film 40 on the main surface of the substrate 20 via a transition layer 30. In this embodiment, a continuous transition layer 30 is formed in the above-mentioned niobium carbide layer formation step S105 and oxidation step S106, thereby suppressing the occurrence of pinholes on the surface of the conductive diamond film 40. In the diamond film deposition step S107, the conductive diamond film 40 can be deposited using, for example, a hot filament CVD apparatus. The hot filament CVD apparatus is configured to be able to supply various gases, such as hydrogen gas, carbon-containing gas, and boron-containing gas, to the growth chamber. Methane gas or ethane gas can be used as the carbon-containing gas. Trimethylboron (TMB) gas, trimethylborate gas, triethylborate gas, or diborane gas can be used as the boron-containing gas. Specifically, for example, after the inside of the hot filament CVD apparatus is evacuated, hydrogen gas, methane gas, and TMB gas are introduced to deposit the conductive diamond film 40. The hot filament CVD apparatus also has a temperature sensor, a tungsten filament, an electrode (e.g., a molybdenum electrode), etc., in an airtight container configured inside the growth chamber.

[0057] The diamond crystal growth conditions in the diamond film deposition step S107 are exemplified as follows: Heat treatment temperature (substrate temperature): 700 to 1000 degrees; Pressure: 5 to 50 Torr; Heat treatment time: 1 to 10 hours.

[0058] The above steps can be used to manufacture the diamond electrode 10. Furthermore, a plurality of diamond electrodes 10 may be combined to manufacture a diamond electrode 10 unit.

[0059] (3) Effects of the Present Embodiment The present embodiment provides one or more of the following effects.

[0060] (a) The diamond electrode 10 of this embodiment has a transition layer 30 consisting of microcrystals mainly composed of niobium and carbon, and an aggregate of microcrystals mainly composed of niobium and oxygen. This makes it possible to efficiently increase the nucleation density of diamond crystals for forming the conductive diamond film 40. In addition, the microcrystals mainly composed of niobium and oxygen exert a binder effect, making it possible to suppress peeling of the conductive diamond film 40.

[0061] (b) In the diamond electrode 10 of this embodiment, it is preferable that the average composition of niobium in the transition layer 30 continuously decreases from the substrate 20 side to the conductive diamond film 40 side. This makes it possible to suppress peeling of the conductive diamond film 40.

[0062] (c) In the diamond electrode 10 of this embodiment, the microcrystals mainly composed of niobium and carbon contained in the transition layer 30 are NbC microcrystals or Nb 2 C microcrystals are preferred, as this makes it possible to efficiently increase the density of nuclei generated from diamond crystals for forming the conductive diamond film 40.

[0063] (d) In the diamond electrode 10 of this embodiment, the transition layer 30 has an abundance ratio of NbC microcrystals of Nb 2 a first transition layer 31 having a higher content of C crystallites than that of Nb 2 and a second transition layer 32 in which the abundance ratio of C microcrystals is higher than the abundance ratio of NbC microcrystals, and it is preferred that the first transition layer 31 is present on the conductive diamond film 40 side and the second transition layer 32 is present on the substrate 20 side. The first transition layer 31 present on the conductive diamond film 40 side has a higher C component than the second transition layer 32 present on the substrate 20 side, so that the nucleation density of diamond crystals for forming the conductive diamond film 40 can be sufficiently increased and the occurrence of pinholes can be suppressed.

[0064] (e) In the diamond electrode 10 of this embodiment, the microcrystals mainly composed of niobium and oxygen contained in the transition layer 30 are NbO microcrystals, and it is preferable that the NbO microcrystals are mixed in the first transition layer 31. This enhances the binder effect, and makes it possible to further suppress peeling of the conductive diamond film 40.

[0065] (f) In the diamond electrode 10 of this embodiment, the crystallite diameter of the NbC microcrystals contained in the first transition layer 31 is, for example, preferably 5 nm or more and 100 nm or less, and more preferably 5 nm or more and 60 nm or less. If the crystallite diameter of the NbC microcrystals is outside the above range, it may be difficult to form a continuous transition layer 30 with a thickness of 0.5 μm or more. On the other hand, by setting the crystallite diameter of the NbC microcrystals within the above range, it becomes easier to form a continuous transition layer 30 with a thickness of 0.5 μm or more, and as a result, it becomes easier to suppress the occurrence of pinholes.

[0066] (g) In the diamond electrode 10 of this embodiment, the crystallite diameter of the NbO microcrystals is, for example, preferably 5 nm or more and 100 nm or less, and more preferably 5 nm or more and 60 nm or less. By setting the crystallite diameter of the NbO microcrystals within the above range, the binder effect is more effectively exerted, and peeling of the conductive diamond film 40 can be further suppressed.

[0067] (h) In the diamond electrode 10 of this embodiment, the thickness of the first transition layer 31 is, for example, 10 nm or more and 500 nm or less, and the thickness of the second transition layer 32 is, for example, 1 μm or more and 10 μm or less. Also, the thickness of the second transition layer 32 is preferably 1.5 times or more and 10 times or less the thickness of the first transition layer 31. By setting the thicknesses of the first transition layer 31 and the second transition layer 32 within the above ranges, it becomes easier to form a continuous transition layer 30 and warping of the diamond electrode 10 can be reduced.

[0068] (i) In the diamond electrode 10 of this embodiment, the volume abundance ratio of NbO microcrystals to NbC microcrystals in the first transition layer 31 is preferably, for example, 50% or more and 100% or less. If the volume abundance ratio of NbO microcrystals is less than 50%, the binder effect is insufficient and it may be difficult to suppress peeling of the conductive diamond film 40. In contrast, by setting the volume abundance ratio of NbO microcrystals to 50% or more, the binder effect is fully exerted and peeling of the conductive diamond film 40 can be further suppressed. On the other hand, if the volume abundance ratio of NbO microcrystals exceeds 100%, the nucleation density of diamond crystals for forming the conductive diamond film 40 may decrease. In contrast, by setting the volume abundance ratio of NbO microcrystals to 100% or less, the nucleation density of diamond crystals for forming the conductive diamond film 40 can be efficiently increased.

[0069] (j) In the diamond electrode 10 of this embodiment, it is preferable to provide a porous portion 33 having a large number of voids near the boundary with the conductive diamond film 40 inside the transition layer 30. This reduces the difference in thermal expansion coefficient between niobium and the conductive diamond film 40, and suppresses peeling of the conductive diamond film 40. In other words, it is possible to further improve the durability of the diamond electrode 10.

[0070] (k) In the diamond electrode 10 of this embodiment, when the surface of the conductive diamond film 40 is observed using, for example, a scanning electron microscope, it is preferable that there are no pinholes reaching the substrate 20 or the transition layer 30 within a 20 μm × 20 μm field of view. This reduces the risk of the strongly acidic liquid coming into contact with the substrate 20 or the transition layer 30, even when the diamond electrode 10 is used in a strongly acidic solution, thereby improving the durability of the diamond electrode 10. From the viewpoint of further improving the durability of the diamond electrode 10, it is more preferable that there are no pinholes reaching the substrate 20 or the transition layer 30 within a 1 mm × 1 mm field of view, and it is particularly preferable that there are no pinholes across the entire surface of the conductive diamond film 40. Specifically, for example, when the diamond electrode 10 of this embodiment is used as a diamond electrode 10 for generating ozone water, it is possible to suppress the deterioration of the diamond electrode 10 during electrical conduction and prevent the conductive diamond film 40 from peeling off. In other words, it is possible to improve the durability of the diamond electrode 10.

[0071] <Other embodiments of the present invention> Although the embodiments of the present invention have been specifically described above, the present invention is not limited to the above-described embodiments and can be modified in various ways without departing from the spirit of the present invention.

[0072] Fig. 5 is a flowchart showing an example of a method for manufacturing a diamond electrode 10 according to another embodiment of the present invention. In the above-described embodiment, each step of the method for manufacturing the diamond electrode 10 has been described, but for example, as shown in the flowchart of Fig. 5, the unevenness forming step S101 may be performed before the porous portion forming step S102, and the seeding step S104 may be performed before the niobium carbide layer forming step S105. In this case, as in the above-described embodiment, a continuous transition layer 30 may be formed, and pinholes in the conductive diamond film 40 may be suppressed. Furthermore, peeling of the conductive diamond film 40 may be suppressed. Below, the unevenness forming step S101 and the seeding step S104 will be described.

[0073] (Unevenness forming step S101) The unevenness forming step S101 is, for example, a step of processing at least one of the main surfaces of the substrate 20 to form uneven undulations. This makes it possible to suppress peeling caused by the difference in thermal expansion coefficient between the substrate 20 and the conductive diamond film 40. In other words, it is possible to further improve the peel strength of the diamond electrode 10. In the unevenness forming step S101, it is preferable to form unevenness so that the arithmetic mean roughness Ra (see JIS B0601-2001) of the main surface is 0.5 μm or more and 10 μm or less. Note that known methods such as grinding, blasting, wet etching, dry etching, etc. can be used as the processing for forming unevenness.

[0074] The unevenness forming step S101 is preferably performed, for example, before the porous portion forming step S102. If unevenness is formed on the surface on which the porous portion 33 has been formed, there is a possibility that the porous portion 33 will be removed. In contrast, by performing the unevenness forming step S101 before the porous portion forming step S102, the subsequent steps can be performed with the porous portion 33 remaining.

[0075] As in the above-described embodiment, the unevenness forming step S101 may be omitted. Even when the unevenness forming step S101 is omitted, the transition layer 30 can be formed by performing the niobium carbide layer forming step S105 and the oxidation step S106, and peeling of the conductive diamond film 40 can be suppressed.

[0076] (Seeding step S104) The seeding step S104 is, for example, a step of seeding diamond particles on the main surface of the substrate 20 (for example, the main surface on which the porous portion 33 is formed). In a typical seeding step S104, immediately before the diamond film deposition step S107, diamond particles are attached (seeded) to the surface of the substrate 20 on which the transition layer 30 is formed by a method such as rubbing, immersion, or blasting. By thus interposing diamond particles at the interface between the transition layer 30 and the conductive diamond film 40, the energy barrier required for initial nucleation to form the conductive diamond film 40 can be lowered.

[0077] The seeding step S104 can be performed, for example, before the formation of the transition layer 30 (i.e., before the niobium carbide layer forming step S105). That is, the seeding step S104 and the above-mentioned carbon source embedding step S103 can be performed simultaneously. This is possible by using the same diamond particles as the carbon source 22 used in the carbon source embedding step S103 and the diamond particles used in the seeding step S104. As described above, the carbon source 22 can be sp 2 It is preferable that the diamond structure (sp 3 The core of the structure is surrounded by an amorphous layer (sp 2 The diamond particles (e.g., nanodiamond particles obtained by detonation) covered with sp 2 Carbon is consumed and sp 3 The core of the structure can be left as seeded diamond particles. In this way, the niobium carbide layer forming step S105, the oxidation step S106, and the diamond film depositing step S107 can be performed consecutively in the same apparatus.

[0078] As in the above embodiment, the seeding step S104 may be omitted. Even when the seeding step S104 is omitted, by performing the above carbon source embedding step S103, the main surface of the substrate 20 is continuously covered with the transition layer 30 in the niobium carbide layer forming step S105 and the oxidation step S106, which promotes nucleation when depositing the diamond film, thereby suppressing the occurrence of pinholes in the conductive diamond film 40.

[0079] Furthermore, in the above-described embodiment, the carbon source 22 is embedded within the main surface of the substrate 20 in the carbon source embedding step S103. However, the carbon source 22 does not necessarily have to be embedded within the main surface of the substrate 20. For example, by making the crystallite diameter of the niobium metal within the main surface of the substrate 20 sufficiently small (e.g., 20 nm or less), a large number of grain boundaries where crystal defects are densely gathered and arranged can be formed. This ensures sufficient diffusion paths for the carbon source 22 and a sufficiently large surface area of ​​the niobium metal that contributes to the carbonization reaction. Therefore, even if the carbon source 22 is not embedded within the main surface of the substrate 20 but is introduced so as to be in contact with the surface of the substrate 20, it is possible to form the transition layer 30. Even if the carbon source 22 is not embedded within the main surface of the substrate 20, it can diffuse from the grain boundaries of the niobium metal into the interior, and therefore it is possible to obtain a transition layer 30 with a thickness corresponding to the diffusion length. However, from the viewpoint of facilitating the formation of a continuous transition layer 30 with a sufficient thickness (e.g., 0.5 μm or more), it is preferable to embed the carbon source 22 inside the main surface of the substrate 20, as in the above-described embodiment.

[0080] Furthermore, in the above-described embodiment, the case where the conductive diamond film 40 has a single layer structure has been described, but the conductive diamond film 40 may have a layered structure in which a plurality of conductive diamond layers are stacked. However, according to the present invention, even when the conductive diamond film 40 has a single layer structure as in the above-described embodiment, it is possible to suppress the occurrence of pinholes and to suppress peeling of the conductive diamond film 40.

[0081] Next, examples of the present invention will be described. These examples are merely examples of the present invention, and the present invention is not limited to these examples.

[0082] (1) Manufacturing of Diamond Electrode 10 (Sample 1) First, the diamond electrode 10 of Sample 1 was manufactured by the following procedure.

[0083] A substrate 20 made of metal niobium, measuring 50 mm x 50 mm and 1 mm thick, was prepared, and plastic deformation processing was performed on the main surface by pressing. Specifically, a cemented carbide mold with a rough surface (Ra of approximately 1 μm) was used, and the surface of the substrate 20 was pressed at a pressure of 60 t to perform plastic deformation processing.

[0084] After the plastic deformation process, the substrate 20 was subjected to a heat treatment in a hydrogen atmosphere at 600°C for 60 minutes, and then cooled to room temperature to form the porous portion 33. When the porous portion 33 was observed with a scanning electron microscope, the porosity of the porous portion 33 was found to be 70%.

[0085] Graphite (particle size 1 to 2 μm) as the carbon source 22 was applied at a rate of approximately 1 mg / cm on the main surface of the substrate 20 on which the porous portion 33 was formed. 2 The amount of graphite embedded in the main surface of the substrate 20 was calculated from the amount of carbon source 22 recovered after the rubbing operation, and the inside of the main surface of the substrate 20 was found to be about 300 μg / cm 2 It was confirmed that graphite (particle size: 5 to 70 nm) was embedded in the nanoparticles.

[0086] The crystallite diameters in this example were calculated from the results of wide-angle X-ray diffraction measurements using an X-ray diffractometer (RINT2500HLB) manufactured by Rigaku Corporation. The measurement conditions were as follows: Measurement wavelength: CuKα (0.15418 nm) X-ray output: 50 kV-250 mA Optical system: Parallel beam with monochromator Divergence slit (DS): 0.5° + 10 mmH Scattering slit (SS): 0.5° Receiving slit (RS): 0.15 mm Scan axis: 2θ / θ Scanning method: Continuous scanning Scan range: 5°≦2θ≦100° Scanning speed: 0.5° / min Sampling: 0.01°

[0087] The graphite-embedded substrate 20 was loaded into a hot filament CVD apparatus, where the formation of the transition layer 30 (niobium carbide layer formation step S105 and oxidation step S106) and the deposition of the conductive diamond film 40 (diamond film deposition step S107) were performed consecutively. Specifically, nitrogen gas was introduced, the pressure was set to 20-50 Torr, and the substrate temperature was maintained at 600-700°C for 60 minutes to form the niobium carbide layer. Next, carbon dioxide gas was introduced, and the substrate temperature was maintained at 800°C for 60 minutes at atmospheric pressure (equivalent to an oxygen molar partial pressure of 0.4). The apparatus was then evacuated to remove the oxidizing gas, after which methane gas was introduced and a voltage (120-150 V) was applied to the 40 cm filament until the filament carbonized and its resistance became constant. Thereafter, hydrogen gas, methane gas, and TMB gas were introduced, the pressure was set to 20 to 50 Torr, the filament voltage was increased to 175 V, and the filament temperature was kept at 2200 to 2400°C and the substrate temperature was kept at 700 to 800°C for 180 minutes, thereby depositing a conductive diamond film 40.

[0088] The diamond electrode 10 was removed from the hot filament CVD apparatus, and it was confirmed that a conductive diamond film 40 with a thickness of 3.21 μm had been deposited. Furthermore, when the diamond electrode 10 was measured by XRD from the conductive diamond film 40 side, the crystallite diameter of niobium carbide (NbC) was 30.8 nm, and the crystallite diameter of niobium oxide (NbO) was 43.4 nm.

[0089] (Sample 2) Furthermore, the diamond electrode 10 of Sample 2 was manufactured by the following procedure.

[0090] A substrate 20 made of metal niobium was prepared, and the main surface was subjected to plastic deformation processing by pressing in the same manner as in Sample 1.

[0091] After the plastic deformation process, the main surface of the substrate 20 was subjected to a heat treatment in a hydrogen atmosphere at 600°C for 60 minutes, and then cooled to room temperature to form the porous portion 33. When the porous portion 33 was observed with a scanning electron microscope, the porosity of the porous portion 33 was found to be 68%.

[0092] In Sample 2, the carbon source 22 was not embedded, and the surface of the substrate 20 having the porous portion 33 formed thereon was seeded by applying a suspension containing fine diamond powder, and then the substrate 20 was thoroughly dried. Thereafter, the substrate 20 was placed in a hot filament CVD apparatus and heat-treated under the same conditions as Sample 1, thereby depositing a conductive diamond film 40.

[0093] The diamond electrode 10 was taken out of the hot filament CVD apparatus, and it was confirmed that a conductive diamond film 40 with a thickness of 2.72 μm had been deposited thereon.

[0094] (Sample 3) Furthermore, the diamond electrode 10 of Sample 3 was manufactured by the following procedure.

[0095] A substrate 20 made of metal niobium was prepared, and the main surface was subjected to plastic deformation processing by pressing in the same manner as in Sample 1.

[0096] In sample 3, the porous portion 33 was not formed, and graphite (particle size 1 to 2 μm) as the carbon source 22 was applied at 1 mg / cm to the main surface of the substrate 20 that had been subjected to plastic deformation processing. 2 The amount of embedded graphite was measured before and after embedding, and the inside of the main surface of the substrate 20 contained 50 μg / cm 2 It was confirmed that graphite (particle size: 5 to 70 nm) was embedded in the nanoparticles.

[0097] After the rubbing, the substrate 20 was placed in a hot filament CVD apparatus, and under the same conditions as those for sample 1, the formation of the transition layer 30 and the deposition of the conductive diamond film 40 were carried out successively.

[0098] The diamond electrode 10 was removed from the hot filament CVD apparatus, and it was confirmed that a conductive diamond film 40 with a thickness of 2.94 μm had been deposited. Furthermore, when the diamond electrode 10 was measured by XRD from the conductive diamond film 40 side, the crystallite diameter of the niobium carbide was 49.0 nm, and the crystallite diameter of the niobium oxide was 38.7 nm.

[0099] (Sample 4) Furthermore, the diamond electrode 10 of Sample 4 was manufactured by the following procedure.

[0100] The porous portion 33 was formed and the carbon source 22 was embedded under the same conditions as in Sample 1. Thereafter, the substrate 20 was placed in a hot filament CVD apparatus, and the formation of a niobium carbide layer and the deposition of a conductive diamond film 40 were carried out successively. That is, in Sample 4, the oxidation step S106 was not carried out, and NbO microcrystals were not introduced into a part of the niobium carbide layer. The formation of the niobium carbide layer and the deposition of the conductive diamond film 40 were carried out under the same conditions as in Sample 1.

[0101] (2) Evaluation of the diamond electrode 10 The cross sections of Samples 1 to 4 were observed using a scanning electron microscope (SEM). In Sample 2, in which the carbon source 22 was not embedded, island-shaped niobium carbide was observed at the interface between the substrate 20 and the conductive diamond film 40, and no continuous transition layer 30 was formed. In contrast, in Samples 1 and 3, in which the carbon source 22 was embedded inside the main surface of the substrate 20, it was confirmed that a continuous transition layer 30 was formed at the interface between the substrate 20 and the conductive diamond film 40. In Sample 4, it was confirmed that a continuous niobium carbide layer was formed at the interface between the substrate 20 and the conductive diamond film 40. It was also confirmed that the transition layer 30 of Sample 1 and the niobium carbide layer of Sample 4 had porous portions 33 near the boundary with the conductive diamond film 40. Figure 6 shows a cross-sectional photograph of Sample 1.

[0102] Furthermore, the surface of the conductive diamond film 40 was observed using an SEM for Samples 1 to 4. In Sample 2, in which the carbon source 22 was not embedded, pinholes were observed on the surface of the conductive diamond film 40. In contrast, in Samples 1, 3, and 4, in which the carbon source 22 was embedded inside the main surface of the substrate 20, no pinholes were observed on the surface of the conductive diamond film 40.

[0103] From the above, it was confirmed that a continuous transition layer 30 (or niobium carbide layer) can be formed by embedding carbon source 22 inside the main surface of substrate 20. It was also confirmed that the formation of a continuous transition layer 30 (or niobium carbide layer) can suppress the occurrence of pinholes on the surface of conductive diamond film 40.

[0104] Furthermore, composition analysis was performed on a cross section around the transition layer 30 of Sample 1 using TEM-EELS and TEM-EDX. TEM-EELS confirmed that oxygen was continuously distributed in the transition layer 30 (first transition layer 31) of Sample 1. Figure 7 shows the results of the composition analysis of Sample 1 using TEM-EDX. As shown in Figure 7, it was confirmed that the first transition layer 31 of Sample 1 contains oxygen. In other words, it was confirmed that NbO microcrystals are mixed in the first transition layer 31. It was also confirmed that the average composition of niobium in the transition layer 30 continuously decreases from the substrate 20 side to the conductive diamond film 40 side.

[0105] In this example, cross-sectional SEM observation and TEM-EELS and TEM-EDX compositional analysis were performed using the following procedures. (a) A sample containing the target observation area was cut to an appropriate size using a low-speed rotating diamond cutter. (b) The sample (a) was embedded in epoxy resin. The resin was cured at 120°C for 1 hour in an atmospheric furnace. (c) The cross section of the sample (b) near the target observation area was roughened using a rotary polisher and then buffed using polishing diamond paste (particle size 0.3 μm). (d) The cross section near the target observation area was finished using an ArBlade 5000 ion milling device manufactured by Hitachi High-Tech Corporation. This flattened the observation surface, facilitating observation of the microstructure. (e) The sample (d) was subjected to a conductive treatment using a platinum sputter coating device manufactured by JEOL Ltd. (f) SEM observation was performed on the sample (e). The accelerating voltage during observation was 5 kV. The SEM used was a Hitachi High-Tech S-4800. Thin film specimens for TEM observation were prepared from the samples observed with the SEM in (g) and (f) at the target observation locations. The thin film specimens were processed using the focused ion beam (FIB) method. The equipment used was a Hitachi High-Tech NB5000. The processing conditions were an acceleration voltage of 40 kV. (h) The thin film specimens in (g) were subjected to TEM observation and elemental analysis using TEM-EELS and TEM-EDX. The TEM equipment used was a Hitachi High-Tech HD-2700, with an acceleration voltage of 200 kV. For TEM-EELS, an EELS equipment (GATAN Enfinium) manufactured by Ametec was used. For TEM-EDX, an EDX equipment (EDAX Octane T Ultra W) manufactured by Ametec was used.

[0106] (3) Durability test of diamond electrode 10 The diamond electrodes 10 of samples 1 to 4 were used as the anode and cathode, respectively, to conduct a durability test for generating ozone water. The durability test was performed by using tap water (flow rate 200 mL / min) as the raw water, and driving the anode and cathode, which were fixed with a polymer electrolyte membrane sandwiched between them, at a voltage of 12 V for 1 minute and then resting for 4 minutes, repeating this cycle 10,000 times. The polymer electrolyte membrane used was Nafion 324 (manufactured by Du Pont). The current values ​​and the concentration of ozone water generated before and after the 10,000 cycles, as well as the area ratio of peeled conductive diamond film 40 after 10,000 cycles, were confirmed and the results are shown in Table 1.

[0107]

[0108] As shown in Table 1, in Sample 2, which did not contain the carbon source 22, the ozone water concentration at 10,000 cycles was significantly lower than that at the first cycle, confirming degradation due to electrical conduction and extensive peeling of the conductive diamond film 40. In Sample 3, which did not contain the porous portion 33, the ozone water concentration at 10,000 cycles was lower, confirming partial peeling of the conductive diamond film 40. In Sample 4, which did not contain the NbO microcrystals, the ozone water concentration at 10,000 cycles was lower, confirming partial peeling of the conductive diamond film 40. In contrast, in Sample 1, which contained the porous portion 33, the carbon source 22 embedded in the main surface of the substrate 20, and the NbO microcrystals, the ozone water concentration at the first cycle was higher than that of Samples 2 to 4, and even at 10,000 cycles, the ozone water concentration was comparable to that at the first cycle (more than 90% of that at the first cycle). Furthermore, almost no peeling of the conductive diamond film 40 was observed.

[0109] From the above, it was confirmed that by forming the transition layer 30 consisting of microcrystals mainly composed of niobium and carbon, and an aggregate of microcrystals mainly composed of niobium and oxygen, it is possible to suppress electrical degradation and prevent peeling of the conductive diamond film 40. In other words, it was confirmed that it is possible to improve the durability of the diamond electrode 10. It was also confirmed that by forming a porous portion 33 in the transition layer 30, it is possible to further improve the durability of the diamond electrode 10.

[0110] <Preferred Embodiments of the Present Invention> Preferred embodiments of the present invention will be additionally described below.

[0111] (Appendix 1) According to one aspect of the present invention, there is provided a diamond electrode having a conductive diamond film formed on at least one main surface of the substrate, and a transition layer formed between the substrate and the conductive diamond film, wherein the transition layer is composed of microcrystals mainly composed of niobium and carbon, and an aggregate of microcrystals mainly composed of niobium and oxygen.

[0112] (Supplementary Note 2) The diamond electrode according to Supplementary Note 1, wherein the average composition of niobium in the transition layer decreases continuously from the substrate side to the conductive diamond film side.

[0113] (Supplementary Note 3) The diamond electrode according to Supplementary Note 1, wherein the microcrystals mainly composed of niobium and carbon are represented by the chemical formula NbC or Nb 2 C is niobium carbide microcrystals.

[0114] (Supplementary Note 4) The diamond electrode according to Supplementary Note 3, wherein the transition layer has an abundance ratio of niobium carbide microcrystals of the chemical formula NbC. 2 A first transition layer having a higher content than the content of niobium carbide microcrystals of C, and a first transition layer having a chemical formula of Nb 2 and a second transition layer in which the proportion of niobium carbide microcrystals of the chemical formula NbC is greater than the proportion of niobium carbide microcrystals of the chemical formula NbC, wherein the first transition layer is present on the conductive diamond film side and the second transition layer is present on the substrate side.

[0115] (Appendix 5) The diamond electrode according to Appendix 4, wherein the microcrystals mainly composed of niobium and oxygen are niobium oxide microcrystals of the chemical formula NbO, and the niobium oxide microcrystals are mixed in the first transition layer.

[0116] (Appendix 6) The diamond electrode according to appendix 4, wherein the crystallite diameter of the niobium carbide microcrystals of the chemical formula NbC contained in the first transition layer is 5 nm or more and 100 nm or less, and the crystallite diameter of the niobium carbide microcrystals of the chemical formula NbC contained in the second transition layer is 5 nm or more and 100 nm or less. 2 The crystallite diameter of the niobium carbide microcrystals of C is 10 nm or more and 2000 nm or less.

[0117] (Supplementary Note 7) The diamond electrode according to Supplementary Note 5, wherein the niobium oxide microcrystals of the chemical formula NbO have a crystallite diameter of 5 nm or more and 100 nm or less.

[0118] (Supplementary Note 8) The diamond electrode according to Supplementary Note 4, wherein the thickness of the first transition layer is 10 nm or more and 500 nm or less, and the thickness of the second transition layer is 1 μm or more and 10 μm or less.

[0119] (Appendix 9) The diamond electrode according to appendix 5, wherein the volume abundance ratio of the niobium oxide microcrystals of the chemical formula NbO to the niobium carbide microcrystals of the chemical formula NbC in the first transition layer is 50% or more and 100% or less.

[0120] (Supplementary Note 10) The diamond electrode according to Supplementary Note 1, wherein a porous portion having voids is present in the transition layer near the boundary with the conductive diamond film.

[0121] (Appendix 11) A diamond electrode according to any one of appendices 1 to 10, wherein when the surface of the conductive diamond film is observed using a scanning electron microscope, there are no pinholes reaching the substrate or the transition layer within a 20 μm×20 μm field of view. Preferably, there are no pinholes reaching the substrate or the transition layer within a 1 mm×1 mm field of view. Particularly preferably, there are no pinholes reaching the substrate or the transition layer across the entire surface of the conductive diamond film.

[0122] REFERENCE SIGNS LIST 10 Diamond electrode 20 Substrate 22 Carbon source 30 Transition layer 31 First transition layer 32 Second transition layer 33 Porous portion 40 Conductive diamond film S101 Roughness formation step S102 Porous portion formation step S103 Carbon source embedding step S104 Seeding step S105 Niobium carbide layer formation step S106 Oxidation step S107 Diamond film deposition step

Claims

1. A diamond electrode comprising: a substrate made of metallic niobium; a conductive diamond film formed on at least one main surface of the substrate; and a transition layer formed between the substrate and the conductive diamond film, the transition layer being composed of microcrystals primarily composed of niobium and carbon, and an aggregate of microcrystals primarily composed of niobium and oxygen.

2. A diamond electrode as described in claim 1, wherein the average composition of niobium in the transition layer decreases continuously from the substrate side to the conductive diamond film side.

3. The niobium and carbon-based microcrystals have the formula NbC or Nb 2 The diamond electrode according to claim 1, which is a niobium carbide microcrystal of C.

4. The transition layer has a proportion of niobium carbide microcrystals of the formula NbC. 2 A first transition layer having a higher content of niobium carbide microcrystals than that of C, and a chemical formula of Nb 2 4. The diamond electrode of claim 3, further comprising a second transition layer in which the proportion of niobium carbide microcrystals of the formula NbC is greater than the proportion of niobium carbide microcrystals of the chemical formula NbC, the first transition layer existing on the conductive diamond film side, and the second transition layer existing on the substrate side.

5. A diamond electrode as described in claim 4, wherein the microcrystals mainly composed of niobium and oxygen are niobium oxide microcrystals of the chemical formula NbO, and the niobium oxide microcrystals are mixed in the first transition layer.

6. The crystallite diameter of the niobium carbide microcrystals of the chemical formula NbC contained in the first transition layer is 5 nm or more and 100 nm or less, and the crystallite diameter of the niobium carbide microcrystals of the chemical formula NbC contained in the second transition layer is 5 nm or more and 100 nm or less. 2 The diamond electrode according to claim 4, wherein the crystallite size of the niobium carbide microcrystals of C is 10 nm or more and 2000 nm or less.

7. A diamond electrode as described in claim 5, wherein the crystallite size of the niobium oxide microcrystals of the chemical formula NbO is 5 nm or more and 100 nm or less.

8. A diamond electrode as described in claim 4, wherein the thickness of the first transition layer is 10 nm or more and 500 nm or less, and the thickness of the second transition layer is 1 μm or more and 10 μm or less.

9. A diamond electrode as described in claim 5, wherein the volumetric abundance ratio of the niobium oxide microcrystals having the chemical formula NbO to the niobium carbide microcrystals having the chemical formula NbC in the first transition layer is 50% or more and 100% or less.

10. A diamond electrode as described in claim 1, wherein a porous portion having voids is present inside the transition layer near the boundary with the conductive diamond film.

11. A diamond electrode described in any one of claims 1 to 10, wherein when the surface of the conductive diamond film is observed using a scanning electron microscope, there are no pinholes reaching the substrate or the transition layer within a field of view of 20 μm x 20 μm.

Citation Information

Patent Citations

  • BDD membrane electrode material and preparation method thereof

    CN108486546A

  • Boron doped diamond electrode and preparation method thereof

    CN109750291A

  • JP1973099080A

  • Electrode for electrolysis and electrolytic cell using this electrode

    JP1997268395A

  • Electrically conductive diamond electrode and its production method

    JP2005240074A