Laminated body, imprint mold, method for manufacturing imprint mold, method for manufacturing optical element, and method for manufacturing electronic component

The use of a laminate with specific materials and layers in the imprint mold manufacturing process addresses the challenges of precision and complexity in existing methods, resulting in high-precision imprint molds for producing accurate optical and electronic components.

WO2024203006A1PCT designated stage expired Publication Date: 2024-10-03HOYA CORPORATION

Patent Information

Application Number
PCT/JP2024/008180
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-05
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional methods for producing imprint molds face challenges in achieving high precision for fine pattern dimensions and desired uneven shapes, with complex design and manufacturing processes, and risk of substrate damage during etching.

Method used

A laminate comprising a substrate of CaO, La2O3, Nb2O5, and BaO with a functional layer and an etching mask layer, where the functional layer is made of silicon and nitrogen, and the etching mask layer contains chromium, tantalum, zirconium, hafnium, or tungsten, allowing for precise control of etching and reduced substrate damage.

Benefits of technology

Enables the formation of imprint molds with high precision and accuracy, simplifying the manufacturing process while minimizing substrate damage, and allows for the production of optical and electronic components with precise fine patterns.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008180_03102024_PF_FP_ABST
    Figure JP2024008180_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a laminated body that is suitably used as a blank for an imprint mold capable of obtaining a desired uneven shape with high accuracy without complicating a design process and a manufacturing process. The laminated body 10 comprises: a substrate 1 that contains at least one of CaO, La2O3, Nb2O5, and BaO; a functional layer 2 that is provided on the substrate 1; and an etching mask layer 3 that is provided on the functional layer 2.
Need to check novelty before this filing date? Find Prior Art

Description

Laminate, imprint mold, imprint mold manufacturing method, optical element manufacturing method, and electronic component manufacturing method

[0001] The present invention relates to an imprint mold that is applicable to the production of fine circuit patterns for electronic components such as semiconductor devices, and the production of optical elements that have optical functions added by fine patterns, and a method for producing the same, as well as a laminate that is suitably used as an imprint mold blank in the production of the imprint mold.

[0002] Imprinting methods for mass-transferring the same fine patterns have come to be used in the production of fine circuit patterns for electronic components such as semiconductor devices, and in the production of optical components (e.g., diffraction gratings) that have optical functions added by fine patterns.

[0003] The imprinting method uses an imprinting mold (stamper) on which a fine mold pattern is formed as an original, and transfers the mold pattern to the cured liquid resin by directly pressing the imprinting mold against a liquid resin, such as a photocurable resin, which is applied to a substrate and is then cured by ultraviolet light, etc. Therefore, the imprinting method makes it possible to transfer a large number of identical fine patterns.

[0004] As described above, since an imprint mold serves as a master for transferring a large number of identical fine patterns, the dimensional accuracy of the mold pattern formed on the mold directly affects the dimensional accuracy of the resulting fine pattern. Furthermore, since the imprint mold transfers the pattern by directly pressing it against a liquid resin applied to a substrate, the cross-sectional shape of the mold pattern also significantly affects the shape of the resulting fine pattern. As the integration density of semiconductor devices and the like increases, the required pattern dimensions become smaller, and since pattern transfer is now performed at full magnification, higher accuracy imprint molds are required.

[0005] Conventionally, in the fabrication of an imprint mold, a method has been known in which a thin film pattern provided on a substrate made of synthetic quartz or the like is used as a mask to etch the substrate (see, for example, Patent Document 1). In this way, a desired concave-convex shape can be formed on the substrate, thereby obtaining an imprint mold.

[0006] Furthermore, as an imprint substrate for producing an imprint mold, there is a structure in which a plurality of films (two-layer films) each consisting of two layers with etching selectivity relative to each other are stacked on a substrate made of synthetic quartz or the like (for example, Patent Document 2).

[0007] JP 2011-227950 A JP 6-258510 A

[0008] However, in the production of an imprint mold such as that disclosed in Patent Document 1, it is not easy to control the amount of digging into the substrate (digging depth) with high precision, and it is also not easy to form the recesses obtained by digging into the substrate into a desired shape with high precision or to make them uniform across the substrate surface.

[0009] On the other hand, with the imprint substrate for producing an imprint mold disclosed in Patent Document 2, precise control of the recess depth during etching is not required by adjusting the film thickness of the two-layer film. However, when producing such an imprint substrate, not only is it necessary to stack multiple two-layer films according to the number of recesses with different recess depths, but the film thickness of each layer must also be designed according to the desired recess depth and adjusted each time the film is formed. This makes the design and manufacturing processes for the imprint substrate extremely complicated. Furthermore, the upper layer of the two-layer film is made of a material with low etching selectivity to the substrate, such as SiO2. Therefore, when etching the upper layer of the two-layer film that contacts the substrate, the lower layer functions as an etching stopper film to protect the substrate. However, at the bottom of the recess with the deepest recess in the imprint mold, the lower layer is removed by etching, exposing the substrate. When etching this lower layer, damage to the substrate was unavoidable. This resulted in the inconvenience of not being able to accurately obtain the desired concave-convex shape.

[0010] Therefore, the present invention has been made in consideration of the above-mentioned conventional problems, and its objects are, first, to provide a laminate that is suitable for use as a blank for an imprint mold that allows a desired concave-convex shape to be obtained with high precision without complicating the design process or manufacturing process, second, to provide an imprint mold made using the above-mentioned laminate and a method for manufacturing the same, and third, to provide a method for manufacturing an optical element and a method for manufacturing an electronic component using the above-mentioned imprint mold.

[0011] As a result of extensive research by the present inventors, the present invention has the following configuration in order to solve the above problems.

[0012] (Configuration 1) CaO, La 2 O 3 , Nb 2 O 5and BaO; a functional layer provided on the substrate; and an etching mask layer provided on the functional layer.

[0013] (Configuration 2) The laminate according to configuration 1, wherein the functional layer is in contact with the substrate. (Configuration 3) The substrate contains CaO, La 2 O 3 , Nb 2 O 5 and BaO in a total content of 30 mass % or more.

[0014] (Configuration 4) The laminate according to Configuration 1, wherein the functional layer is made of a material containing silicon and at least one of oxygen and nitrogen. (Configuration 5) The laminate according to Configuration 1, wherein, in a state where the functional layer is laminated on the substrate, the transmittance of light having a wavelength of 365 nm transmitted through the substrate and the functional layer is 50% or more.

[0015] (Configuration 6) The laminate according to configuration 1, wherein the etching mask layer contains one or more selected from the group consisting of chromium, tantalum, zirconium, hafnium, and tungsten.

[0016] (Configuration 7) A method for manufacturing an imprint mold, comprising the steps of: preparing the laminate according to any one of Configurations 1 to 6; forming an etching mask pattern on the etching mask layer; etching the functional layer using the etching mask pattern as a mask; and removing the etching mask pattern.

[0017] (Configuration 8) An imprint mold comprising CaO, La 2 O 3 , Nb 2 O 5 and BaO; and a functional layer provided on the substrate, wherein the functional layer has a plurality of recesses that form a predetermined mold pattern.

[0018] (Configuration 9) The imprint mold according to configuration 8, wherein the functional layer is in contact with the substrate. (Configuration 10) The imprint mold according to configuration 8, wherein the functional layer is in contact with the substrate. 2 O 3 , Nb 2 O 5 and BaO in a total content of 30 mass % or more.

[0019] (Configuration 11) The imprint mold according to Configuration 8, wherein the functional layer is made of a material containing silicon and at least one of oxygen and nitrogen. (Configuration 12) The imprint mold according to Configuration 8, wherein when the functional layer is stacked on the substrate, the transmittance of light having a wavelength of 365 nm that passes through the substrate and the functional layer is 50% or more.

[0020] (Configuration 13) The imprint mold according to Configuration 8, wherein the substrate is exposed at the bottom of the recess.

[0021] (Structure 14) A method for manufacturing an optical element, comprising the steps of: preparing an imprint mold manufactured using the laminate described in any one of Structures 1 to 6, or the imprint mold described in any one of Structures 8 to 13; hardening a transfer target applied to a substrate for an optical element while pressing the imprint mold against the transfer target; and separating the imprint mold from the transfer target.

[0022] (Configuration 15) A method for manufacturing an electronic component, comprising the steps of: preparing an imprint mold manufactured using the laminate according to any one of Configurations 1 to 6, or the imprint mold according to any one of Configurations 8 to 13; curing a transfer target applied to an electronic component substrate while pressing the imprint mold against the transfer target; and separating the imprint mold from the transfer target.

[0023] According to the present invention, it is possible to provide a laminate that is suitably used as an imprint mold blank that allows for obtaining a desired concave-convex shape with high precision without complicating the design process or manufacturing process. Furthermore, according to the present invention, it is possible to provide an imprint mold having a high-precision mold pattern, which is produced using the above-mentioned laminate, and a method for manufacturing the same. Furthermore, according to the present invention, it is possible to provide a method for manufacturing an optical element and an electronic component on which a high-precision fine pattern is formed, using the above-mentioned imprint mold.

[0024] FIG. 1 is a cross-sectional view showing the layer structure of an embodiment of a laminate according to the present invention. FIG. 2 is a cross-sectional view showing an embodiment of an imprint mold according to the present invention. (a) to (i) are cross-sectional views illustrating a first embodiment of a manufacturing process for an imprint mold. (j) to (p) are cross-sectional views showing a continuation of the manufacturing process of FIG. 3. (a) to (i) are cross-sectional views illustrating a second embodiment of a manufacturing process for an imprint mold according to the present invention. (j) to (o) are cross-sectional views showing a continuation of the manufacturing process of FIG. 5. (a) to (i) are cross-sectional views illustrating a third embodiment of a manufacturing process for an imprint mold according to the present invention. (j) to (o) are cross-sectional views showing a continuation of the manufacturing process of FIG. 7. (a) to (c) are cross-sectional views illustrating pattern transfer to a transfer target by imprinting.

[0025] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings.

[0026] [Laminate] First, the laminate of the present invention will be described. The laminate of the present invention is suitably used as a blank for an imprint mold when producing an imprint mold.

[0027] 1 is a cross-sectional view showing the layer structure of one embodiment of a laminate according to the present invention. As shown in Fig. 1, a laminate 10 according to one embodiment of the present invention includes a substrate 1, a functional layer 2 provided on the substrate 1, and an etching mask layer 3 provided on the functional layer 2.

[0028] In the present invention, the substrate 1 has two main surfaces opposite to each other and four end faces. 2 O 3 , Nb 2 O 5 and BaO, and in particular, the substrate 1 contains CaO, La, 2 O 3 , Nb 2 O 5 and BaO in a total content of 30 mass % or more.

[0029] As will be described in detail later, when an imprint mold is manufactured using the laminate, in a step of etching the functional layer 2 with a fluorine-containing gas until the surface of the substrate 1 is exposed, to form a recess of a desired shape, the substrate 1 is made of, for example, SiO 2 Compared with a synthetic quartz substrate made of, for example, a silicon dioxide gas, the amount of processing damage caused by etching can be made negligible. Furthermore, since the substrate 1 has high resistance to chlorine-based gases, the amount of processing damage to the substrate 1 in the recess formation step using chlorine-based gases can also be made negligible. As a result, the recesses obtained by etching the functional layer 2 can be formed into the desired shape with high precision.

[0030] The refractive index n of the substrate 1 with respect to the d line (wavelength 587.56 nm) is d is preferably 1.5 or more, more preferably 1.7 or more. d is preferably 2.5 or less, more preferably 2.3 or less, and further preferably 2.2 or less. d is preferably 60 or less, more preferably 50 or less, and even more preferably 40 or less. d is preferably 10 or more, more preferably 15 or more. d is ν d = (n d −1) / (n F -n C ) where n Fis the refractive index of the substrate 1 with respect to the F line (wavelength 486.13 nm), n C means the refractive index of the substrate 1 with respect to the C-line (wavelength 656.27 nm).

[0031] Next, the functional layer 2 will be described. The functional layer 2 is preferably provided on one main surface of the substrate 1 in contact with the substrate 1. In other words, it is preferable that no other layer or film is interposed between the functional layer 2 and the substrate 1.

[0032] Furthermore, it is preferable that the functional layer 2 be a single layer. If the functional layer 2 is a single layer, the recess obtained by etching the functional layer 2 can be formed in a desired shape (cross-sectional shape) without any steps along the way.

[0033] Furthermore, the functional layer 2 preferably has a uniform composition in the film thickness direction, except for the interface with the substrate 1 (e.g., within a 5 nm thickness range from the substrate 1 side) and the interface with the etching mask layer 3 (e.g., within a 5 nm thickness range from the etching mask layer 3 side). If the functional layer 2 has a uniform composition in the film thickness direction, except for the interface with the substrate 1 and the interface with the etching mask layer 3, the recess obtained by etching the functional layer 2 can be formed into a desired cross-sectional shape without any steps, and the etching conditions for the functional layer 2 can be easily controlled. As long as the cross-sectional shape of the recess can be improved, the composition of the functional layer 2 may change continuously or stepwise in the film thickness direction.

[0034] In the present invention, the functional layer 2 may be made of a material that can be etched with a fluorine-containing gas. As long as the material can be etched with such a fluorine-containing gas, the functional layer 2 can be used without any particular restrictions. As the fluorine-containing gas, F 2 Gas, CF 4 Perfluorocarbon gases such as CFH 3 Hydrofluorocarbon gases such as SF 6 Gas, NF 3 Gas, SiF 4Examples of suitable fluorine-containing gases include fluorine-containing gases such as fluorine-containing fluorine dioxide (HF) and fluorine-containing fluorine dioxide (HF). These fluorine-containing gases may further contain a noble gas and / or oxygen. The noble gas is not particularly limited, but argon (Ar) can be used, for example. Etching using a fluorine-containing gas is preferred because it has high anisotropy and can produce a good recess shape.

[0035] Examples of materials that can be etched with a fluorine-containing gas include materials containing silicon. Particularly preferred silicon-containing materials are materials containing silicon and at least one of oxygen and nitrogen. Specific examples of silicon-containing materials include SiO 2 , SiNx and Si 3 N 4 , SiON, etc. Also preferred are materials containing titanium. Specific examples of materials containing titanium include TiO 2 Other examples include Nb 2 O 5 Materials containing niobium (Nb), such as:

[0036] Furthermore, since the substrate 1 has high resistance to chlorine-containing gases, the functional layer 2 can be made of a material that can be etched with a chlorine-containing gas. The substrate 1 can be made of any material that can be etched with such a chlorine-containing gas without any particular restrictions. For example, a material containing aluminum or a material containing hafnium can be used for the substrate 1. Examples of aluminum-containing materials include Al 2 O 3 , aluminum silicate (Al x Si y Examples of materials containing hafnium include HfO, HfSiO, and HfAlO, and the composition ratio is adjusted appropriately.

[0037] When the functional layer 2 is etched with a fluorine-containing gas, the etching selectivity of the functional layer 2 to the substrate 1 is preferably 2.5 or more, more preferably 3.0 or more, and even more preferably 3.5 or more.

[0038] Furthermore, when the etching mask layer 3 provided on the functional layer 2 is patterned by etching, in order to prevent the underlying functional layer 2 from being damaged, it is preferable that the functional layer 2 has resistance to the etching conditions of the etching mask layer 3. As will be described later, a material containing chromium, for example, is preferably used for the etching mask layer 3. As an etching gas for patterning the etching mask layer 3 made of a material containing chromium, a chlorine-containing gas (for example, Cl 2 , SiCl 2 , CHCl 3 , C.H. 2 Cl 2 , CCl 4 , BCl 3 ) or a mixed gas of oxygen and at least one of the above chlorine-containing gases. Therefore, when the etching mask layer 3 is made of a material containing chromium, the functional layer 2 is formed by etching the above chlorine-containing gas (for example, Cl 2 , SiCl 2 , CHCl 3 , C.H. 2 Cl 2 , CCl 4 , BCl 3 ) or a mixed gas of oxygen and at least one of the above chlorine-containing gases.

[0039] The preferred materials for the functional layer 2, such as silicon-containing materials and titanium-containing materials, are materials that are resistant to the chlorine-containing gases and mixed gases of the chlorine-containing gases and oxygen.

[0040] There are no particular restrictions on the film thickness of the functional layer 2. In other words, when an imprint mold is manufactured using the laminate 10 of the present invention, the film thickness of the functional layer 2 can be designed and formed according to the depth of the recesses formed by etching the functional layer 2 and / or the height of the protrusions described below.

[0041] There are no particular limitations on the method for forming the functional layer 2 on the substrate 1, but sputtering deposition is preferred. The sputtering deposition is suitable because it allows the formation of a uniform film with a constant thickness.

[0042] Furthermore, when an imprint mold is used as a master to transfer a mold pattern to a transfer target (transfer recipient), the imprint mold is pressed against a resin (transfer target) applied to, for example, an optical element substrate, and the resin is cured by generally applying light or heat. In particular, when applying light from the imprint mold side, the imprint mold must be optically transparent. Therefore, when applying light from the imprint mold side, with the functional layer 2 stacked on the substrate 1, the transmittance of light with a wavelength of, for example, 365 nm that passes through the substrate 1 and the functional layer 2 is preferably 50% or more, more preferably 70% or more.

[0043] Next, the etching mask layer 3 will be described. The etching mask layer 3 is preferably provided on the functional layer 2 in contact with the functional layer 2. In other words, it is preferable that no other layer or film is interposed between the etching mask layer 3 and the functional layer 2.

[0044] The etching mask layer 3 functions as a hard mask film when etching (digging) the functional layer 2 to form a mold pattern in the functional layer 2. Therefore, a material is selected for the etching mask layer 3 that has etching selectivity with respect to the functional layer 2 under the etching conditions of the functional layer 2 for forming a mold pattern in a subsequent process. As described above, the functional layer 2 is etched with a fluorine-containing gas or a chlorine-containing gas, so it is preferable that the etching mask layer 3 be resistant to these etching conditions. In the present invention, the etching mask layer 3 is preferably formed of a material containing one or more selected from, for example, chromium, tantalum, zirconium, hafnium, and tungsten. When the functional layer 2 is etched with a chlorine-containing gas, the etching mask layer 3 is preferably formed of a material that can be etched with a fluorine-containing gas, such as SiO 2 , SiON, SiN x and Si 3 N 4 The insulating layer 10 can be formed of a silicon-containing material such as

[0045] The etching mask layer 3 is preferably formed of, for example, a material containing chromium. When a fluorine-containing gas is used for dry etching of the functional layer 2, the chromium-containing material has etching selectivity with respect to the fluorine-containing gas relative to the functional layer 2. In addition, a chromium-containing material is preferable because it can be easily etched with a chlorine-containing gas and has excellent processability.

[0046] Examples of the chromium (Cr)-containing material (chromium-based material) include chromium metal, chromium nitride, chromium carbide, chromium carbonitride, and chromium oxide carbonitride. In this case, the etching mask layer 3 can be etched with a chlorine-containing gas. The metal contained most abundantly in the chromium-based material is preferably chromium. The metal contained in the chromium-based material preferably contains 5 atomic % or less of metals other than chromium, and more preferably contains no metals other than chromium. Since the etching rate when etching a chromium-based material with a chlorine-containing gas is higher than the etching rate when etching a silicon-containing material with a fluorine-containing gas, productivity can be improved by using a chromium-based material as the etching mask layer 3.

[0047] In addition to materials containing chromium, examples of materials that can be used include materials containing tantalum, zirconium, hafnium, tungsten, etc. (single metals, alloys, oxides, nitrides, carbides, oxynitrides, carbonitrides, or oxynitride carbides of single metals, and similarly, oxides, nitrides, carbides, oxynitrides, carbonitrides, or oxynitride carbides of alloys). Materials containing tantalum are preferred because they can be easily etched with a chlorine-containing gas and / or a fluorine-containing gas and have excellent processability.

[0048] The etching mask layer 3 may be a single layer or multiple layers. For example, the etching mask layer 3 may be a single layer film of the chromium-based material. Alternatively, the etching mask layer 3 may be a laminated film of at least an upper layer and a lower layer, with the upper layer being made of the chromium-based material and the lower layer being made of a material primarily containing tantalum (Ta). In this case, the tantalum-based material may be a Ta compound such as TaHf, TaZr, or TaHfZr, or a material based on these Ta compounds and containing additional materials such as B, Ge, Nb, Si, C, or N. Furthermore, a tantalum-based material is preferable because it can provide the necessary conductivity to prevent charge-up during electron beam writing when forming a resist pattern on the etching mask layer 3 and enable mold pattern inspection using a scanning electron microscope (SEM). The etching mask layer 3 may be a compositionally graded film whose composition changes continuously or stepwise in the film thickness direction. Of course, the above-described examples of the configuration and materials of the etching mask layer 3 are merely examples, and the present invention is not limited to these.

[0049] The thickness of the etching mask layer 3 is not particularly limited, but can be, for example, 2 nm to 80 nm, more preferably 70 nm or less, and even more preferably 60 nm or less. By making the thickness of the etching mask layer 3 2 nm or more, when etching the functional layer 2 using the pattern of the etching mask layer 3 as a mask during mold pattern production, the pattern of the etching mask layer 3 can be sufficiently retained until processing is completed. The thickness of the etching mask layer 3 is more preferably 5 nm or more, and even more preferably 10 nm or more. On the other hand, by making the thickness of the etching mask layer 3 80 nm or less, the shape of the fine pattern can be improved. Furthermore, the etching mask layer 3 can be finally removed without damaging the material of the functional layer 2.

[0050] Although there is no particular limitation on the method for forming the etching mask layer 3 on the functional layer 2, a sputtering film formation method is preferred among others. The sputtering film formation method is suitable because it can form a uniform film with a constant thickness.

[0051] Furthermore, the laminate 10 according to one embodiment of the present invention may have a resist film, which will be described later, formed on the etching mask layer 3 .

[0052] [Imprint mold] Next, the imprint mold of the present invention will be described. Fig. 2 is a cross-sectional view showing one embodiment of the imprint mold according to the present invention. The imprint mold 20 of one embodiment of the present invention shown in Fig. 2 is produced using the above-mentioned laminate 10 as an imprint mold blank.

[0053] That is, the imprint mold 20 includes a substrate 1 and functional layers 2a, 2b, and 2c having a plurality of recesses 5 that form a predetermined mold pattern formed on the substrate 1. The bottom surfaces of the plurality of recesses 5 all expose the main surface of the substrate 1. Furthermore, in the imprint mold 20 of this embodiment, as shown in the figure, the functional layers 2a, 2b, and 2c are each at different heights from the main surface of the substrate 1. In short, the imprint mold 20 of this embodiment includes a substrate 1 and functional layers 2a, 2b, and 2c having a concavo-convex structure of different heights that form a predetermined mold pattern formed on the substrate 1. The functional layers 2a, 2b, and 2c have shapes that protrude from the main surface of the substrate 1 and are sometimes collectively referred to as convex portions. The imprint mold 20 can have a plurality of convex portions with different heights. The top surfaces of the convex portions can all be parallel to the main surface of the substrate 1. The top surfaces of the convex portions refer to the surfaces of the functional layers 2a, 2b, and 2c opposite to the surfaces that contact the substrate 1. Furthermore, being parallel to the main surface of the substrate 1 means that a plane A determined by the least squares method with the top surface of the convex portion as a reference is parallel or approximately parallel to a plane B determined by the least squares method with the main surface of the substrate 1 as a reference. "Approximately parallel" means that the angle between plane A and plane B is 10 degrees or less.

[0054] The imprint mold 20 is produced using the laminate 10. Therefore, the substrate 1 in the imprint mold 20 is made of CaO, La, 2 O 3 , Nb 2 O 5 and BaO. The functional layers 2a, 2b, and 2c constituting the predetermined mold pattern are made of a material that can be etched with the fluorine-containing gas. The functional layers 2a, 2b, and 2c may also be made of a material that can be etched with a chlorine-containing gas.

[0055] In the imprint mold 20, the functional layers 2a, 2b, and 2c are in contact with the substrate 1. In the imprint mold 20, it is preferable that the transmittance of light with a wavelength of 365 nm in the laminated state of the substrate 1 and the functional layers 2a, 2b, and 2c is 50% or more.

[0056] In the imprint mold 20, the width of the recess 5 is preferably 10 μm or less, more preferably 1 μm or less, and even more preferably 0.8 μm. The width of the recess 5 can be, for example, 3 nm or more, but can also be 10 nm or more, or 100 nm or more.

[0057] Furthermore, in the imprint mold 20, a recess may be formed on the back surface side of the substrate 1. Here, the back surface refers to the main surface opposite to the main surface on which the functional layers 2 a, 2 b, and 2 c of the substrate 1 are formed. Forming a recess on the back surface side of the substrate 1 is preferable because it makes it easier to peel the imprint mold 20 from the transfer target after the mold pattern has been transferred to the transfer target by imprinting.

[0058] [Method for manufacturing imprint mold] Next, a method for manufacturing an imprint mold of the present invention will be described. The method for manufacturing an imprint mold of the present invention includes the steps of preparing the above-mentioned laminate 10, forming an etching mask pattern on the etching mask layer 3 of the laminate 10, etching the functional layer 2 of the laminate 10 using the etching mask pattern as a mask, and removing the etching mask pattern.

[0059] Specific embodiments of the method for manufacturing an imprint mold of the present invention will be described below with reference to the drawings. <First Embodiment> Figures 3(a) to 3(i) are cross-sectional views illustrating a first embodiment of the manufacturing process for an imprint mold, and Figures 4(j) to 4(p) are cross-sectional views showing a continuation of the manufacturing process shown in Figure 3.

[0060] A resist film 4 made of, for example, a liquid photocurable resin is applied to the upper surface of the laminate 10 according to one embodiment of the present invention (see FIG. 3( a)). In this case, the resist film 4 is preferably a negative resist, but a positive resist may also be used.

[0061] Next, a fine pattern (mold pattern) is drawn on the resist film 4 by laser, and after drawing, the resist film is developed to form a resist pattern 4a (see FIG. 3(b)).

[0062] Next, the laminate 10 on which the resist pattern 4a is formed is introduced into a dry etching device, and etching gas (for example, chlorine-based gas, Cl 2 The etching mask layer 3 is etched using the resist pattern 4a as a mask by dry etching using a resist such as a resist film, thereby forming an etching mask pattern 3a as shown in FIG. 3(c).

[0063] Here, the laminate with the etching mask pattern 3a formed thereon is temporarily removed from the dry etching apparatus, and the remaining resist pattern 4a is removed (see FIG. 3(d)). Here, the next step may be carried out without removing the remaining resist pattern 4a. For convenience of explanation, the laminate 10 with the etching mask pattern 3a and the like formed thereon will also be referred to as a "laminate" hereinafter.

[0064] Next, in the same dry etching apparatus, a fluorine-based gas (CHF 3 , CF4, etc.), the functional layer 2 is etched using the etching mask pattern 3a as a mask until the main surface of the substrate 1 is exposed, forming a recess, and a functional layer pattern 2a with a concave-convex structure is formed on the substrate 1, as shown in Figure 3(e). In the present invention, the amount of processing damage to the substrate 1 due to etching can be made negligible at the bottom of the recess where the main surface of the substrate 1 is exposed. As a result, the recess obtained by etching the functional layer 2 can be formed into the desired shape with high precision.

[0065] Here, if the remaining etching mask pattern 3a is peeled off, an imprint mold having a functional layer pattern 2a in which a plurality of convex portions have the same height is completed.

[0066] Next, a resist film 4 is again applied to the upper surface of the laminate on which the etching mask pattern 3a and the functional layer pattern 2a have been formed (see FIG. 3(f)). In this case, the resist film 4 is preferably a positive resist so that the subsequent drawing area can be made small, and the following description will be given of the case where a positive resist is used. Of course, a negative resist may also be used.

[0067] Next, a predetermined region (a region where a functional layer pattern 2c, described later in this first embodiment, will be formed) is laser-drawn on the resist film 4, and after the drawing, the resist film is developed to form a resist pattern 4b (see FIG. 3(g)). The substrate 1 has high resistance to fluorine-containing gases and chlorine-containing gases, and when etching the functional layer pattern 2a in the step of FIG. 3(i), damage to the substrate 1 is either negligible or not. Therefore, it is not necessary to draw the predetermined region so that it completely coincides with the first region where the functional layer pattern 2a to be etched in the step of FIG. 3(i) is located. Therefore, as long as the predetermined region includes this first region, the predetermined region can be drawn so that it is larger than the first region. That is, according to this first embodiment, there is no need to precisely control the alignment between the first drawing ( FIG. 3(b)) and the second drawing ( FIG. 3(g)).

[0068] Next, the laminate on which the resist pattern 4b is formed is introduced into a dry etching device, and etching gas (e.g., chlorine-based gas, Cl 2 The exposed etching mask pattern 3a is removed by dry etching using a mask such as a masking agent (see FIG. 3(h)).

[0069] Next, a fluorine-based gas (CHF 3 , CF4, etc.) to dig down the exposed functional layer pattern 2a to a predetermined height (depth), thereby forming a functional layer pattern 2c (see FIG. 3(i)).

[0070] Next, after peeling off the remaining resist pattern 4b (see FIG. 4(j)), a resist film 4 is again applied to the upper surface of the laminate (see FIG. 4(k)). In this case, a positive resist is also preferable for the resist film 4 so that the subsequent drawing area can be made small, and the following description will be given of the case where a positive resist is used. Of course, a negative resist may also be used.

[0071] Next, a predetermined region (in the first embodiment, a region where a functional layer pattern 2b (FIG. 4(n)) described later is to be formed) is laser-drawn on the resist film 4, and after the drawing, the resist film is developed to form a resist pattern 4c (see FIG. 4(l)). Here, as in the above, there is no need to precisely control alignment between the first and second drawing (FIGS. 3(b) and (g)) and the third drawing (FIG. 4(l)).

[0072] Next, the laminate on which the resist pattern 4c is formed is introduced into a dry etching device, and etching gas (e.g., chlorine-based gas, Cl 2 The exposed etching mask pattern 3a is removed by dry etching using a dry etching mask such as a fluorine-containing compound (eg, fluorine-containing compound) (see FIG. 4(m)).

[0073] Next, a fluorine-based gas (CHF 3 , CF4, etc.) to dig down the exposed functional layer pattern 2a to a predetermined height (depth), thereby forming the functional layer pattern 2b (see FIG. 4(n)).

[0074] Next, the remaining resist pattern 4c is peeled off (see Figure 4(o)), and then the etching mask pattern 3a remaining on the functional layer pattern 2a is removed, thereby completing an imprint mold 20 as shown in Figure 4(p), which includes a substrate 1 and functional layers 2a, 2b, and 2c with uneven structures of different heights that constitute a predetermined mold pattern formed on the substrate 1.

[0075] Second Embodiment (a) to (i) of FIG. 5 are cross-sectional views for explaining a second embodiment of the manufacturing process of an imprint mold, and (j) to (o) of FIG. 6 are cross-sectional views showing a continuation of the manufacturing process of FIG. 5.

[0076] A resist film 4 is applied to the upper surface of the laminate 10 according to one embodiment of the present invention (see FIG. 5(a)). In this case, the resist film 4 is preferably a negative resist, but a positive resist may also be used.

[0077] Next, a fine pattern (mold pattern) is drawn on the resist film 4 by laser, and after drawing, the resist film is developed to form a resist pattern 4a (see FIG. 5(b)).

[0078] Next, the laminate on which the resist pattern 4a is formed is introduced into a dry etching device, and etching gas (e.g., chlorine-based gas, Cl 2 The etching mask layer 3 is etched using the resist pattern 4a as a mask by dry etching using a resist such as a resist film, thereby forming an etching mask pattern 3a as shown in FIG. 5(c).

[0079] Here, the laminate having the etching mask pattern 3a formed thereon is temporarily removed from the dry etching apparatus, and the remaining resist pattern 4a is removed (see FIG. 5(d)). Here, the next step may be carried out without removing the remaining resist pattern 4a.

[0080] Next, in the same dry etching apparatus, a fluorine-based gas (CHF 3 , CF4, etc.), the functional layer 2 is etched using the etching mask pattern 3a as a mask until the main surface of the substrate 1 is exposed, forming a recess, and a functional layer pattern 2a with a concave-convex structure is formed on the substrate 1, as shown in Figure 5(e). As described above, in the present invention, the amount of processing damage to the substrate 1 due to etching can be made negligible at the bottom of the recess where the main surface of the substrate 1 is exposed. As a result, the recess obtained by etching the functional layer 2 can be formed into the desired shape with high precision.

[0081] Here, if the remaining etching mask pattern 3a is peeled off, an imprint mold having a functional layer pattern 2a in which a plurality of convex portions have the same height is completed.

[0082] Next, a resist film 4 is again applied to the upper surface of the laminate on which the etching mask pattern 3a and the functional layer pattern 2a are formed (see FIG. 5(f)). In this case, a positive resist is preferably used for the resist film 4 so that the subsequent drawing area can be made small, and the following description will be given of the case where a positive resist is used. Of course, a negative resist may also be used.

[0083] Next, predetermined regions (regions where functional layer patterns 2b and 2c will be formed in the second embodiment) are laser-drawn on the resist film 4, and after the drawing, the resist film is developed to form a resist pattern 4d (see FIG. 5(g)). Here, as in the above, there is no need to precisely control the alignment between the first drawing (FIG. 5(b)) and the second drawing (FIG. 5(g)).

[0084] Next, the laminate on which the resist pattern 4d is formed is introduced into a dry etching device, and etching gas (for example, chlorine-based gas, Cl 2 The exposed etching mask pattern 3a is removed by dry etching using a dry etching mask such as a dry etching mask (see FIG. 5(h)).

[0085] Next, a fluorine-based gas (CHF 3 , CF4, etc.) to dig down the exposed functional layer pattern 2a to a predetermined height (depth), thereby forming a functional layer pattern 2b (see FIG. 5(i)).

[0086] Next, after peeling off the remaining resist pattern 4d (see FIG. 6(j)), a resist film 4 is again applied to the upper surface of the laminate (see FIG. 6(k)). In this case, a positive resist is also preferable for the resist film 4 so that the subsequent drawing area can be made small, and the following description will be given of the case where a positive resist is used. Of course, a negative resist may also be used.

[0087] Next, a predetermined region (a region where a functional layer pattern 2c, which will be described later in this second embodiment, is formed) is laser-drawn on the resist film 4, and after the drawing, the resist film is developed to form a resist pattern 4e (see FIG. 6(l)). Here, as in the above, there is no need to precisely control alignment between the two drawing operations.

[0088] Next, the laminate on which the resist pattern 4e is formed is introduced into a dry etching device, and a fluorine-based gas (CHF 3 , CF4, etc.) to dig down the exposed functional layer pattern 2b to a predetermined height (depth), thereby forming a functional layer pattern 2c (see FIG. 6(m)).

[0089] Next, the remaining resist pattern 4e is peeled off (see Figure 6(n)), and then the etching mask pattern 3a remaining on the functional layer pattern 2a is removed, thereby completing an imprint mold 20 as shown in Figure 6(o), which includes a substrate 1 and functional layers 2a, 2b, and 2c with uneven structures of different heights that constitute a predetermined mold pattern formed on the substrate 1.

[0090] Third Embodiment (a) to (i) of FIG. 7 are cross-sectional views for explaining a third embodiment of the manufacturing process of an imprint mold, and (j) to (o) of FIG. 8 are cross-sectional views showing a continuation of the manufacturing process of FIG. 7.

[0091] A resist film 4 is applied to the upper surface of the laminate 10 according to one embodiment of the present invention (see FIG. 7(a)). In this case, the resist film 4 is preferably a negative resist, but a positive resist may also be used.

[0092] Next, a fine pattern (mold pattern) is drawn on the resist film 4 by laser, and after drawing, the resist film is developed to form a resist pattern 4a (see FIG. 7(b)).

[0093] Next, the laminate on which the resist pattern 4a is formed is introduced into a dry etching device, and etching gas (e.g., chlorine-based gas, Cl 2The etching mask layer 3 is etched using the resist pattern 4a as a mask by dry etching using a resist such as a fluorine-containing compound (e.g., fluorine-containing compound), thereby forming an etching mask pattern 3a as shown in FIG. 7(c).

[0094] Here, the laminate having the etching mask pattern 3a formed thereon is temporarily removed from the dry etching apparatus, and the remaining resist pattern 4a is removed (see FIG. 7(d)). Here, the next step may be carried out without removing the remaining resist pattern 4a.

[0095] Next, in the same dry etching apparatus, a fluorine-based gas (CHF 3 , CF4, etc.), the functional layer 2 is etched using the etching mask pattern 3a as a mask until the main surface of the substrate 1 is exposed, forming a recess, and a functional layer pattern 2a with a concave-convex structure is formed on the substrate 1, as shown in Figure 7(e). As described above, in the present invention, the amount of processing damage to the substrate 1 due to etching can be made negligible at the bottom of the recess where the main surface of the substrate 1 is exposed. As a result, the recess obtained by etching the functional layer 2 can be formed into the desired shape with high precision.

[0096] Here, if the remaining etching mask pattern 3a is peeled off, an imprint mold having a functional layer pattern 2a in which a plurality of convex portions have the same height is completed.

[0097] Next, a resist film 4 is again applied to the upper surface of the laminate on which the etching mask pattern 3a and the functional layer pattern 2a are formed (see FIG. 7(f)). In this case, the resist film 4 is preferably a positive resist so that the subsequent drawing area can be made small, and the following description will be given of the case where a positive resist is used. Of course, a negative resist may also be used.

[0098] Next, predetermined regions (regions including regions where functional layer patterns 2b and 2c, described later in the third embodiment, are formed) are laser-drawn on the resist film 4, and after the drawing, the resist film is developed to form a resist pattern 4f (see FIG. 7(g)). Here, as in the above, there is no need to precisely control alignment between the two drawing operations.

[0099] Next, the laminate on which the resist pattern 4f is formed is introduced into a dry etching device, and etching gas (e.g., chlorine-based gas, Cl 2 The exposed etching mask pattern 3a is removed by dry etching using a mask such as a masking agent (see FIG. 7(h)).

[0100] Next, a fluorine-based gas (CHF 3 , CF4, etc.) to dig down the exposed functional layer pattern 2a to a predetermined height (depth), thereby forming a functional layer pattern 2b (see FIG. 7(i)).

[0101] Next, after peeling off the remaining resist pattern 4f (see FIG. 8(j)), a resist film 4 is again applied to the upper surface of the laminate (see FIG. 8(k)). In this case, a positive resist is also preferable for the resist film 4 so that the subsequent drawing area can be made small, and the following description will be given of the case where a positive resist is used. Of course, a negative resist may also be used.

[0102] Next, a predetermined region (including a region where a functional layer pattern 2c, which will be described later in this third embodiment, is formed) is laser-drawn on the resist film 4, and after the drawing, the resist film is developed to form a resist pattern 4g (see FIG. 8(l)). Here, as in the above, there is no need to precisely control alignment between the two drawing operations.

[0103] Next, the laminate on which the resist pattern 4g is formed is introduced into a dry etching device, and a fluorine-based gas (CHF 3 , CF4, etc.) to dig down the exposed functional layer pattern 2b to a predetermined height (depth), thereby forming a functional layer pattern 2c (see FIG. 8(m)).

[0104] Next, the remaining resist pattern 4g is peeled off (see Figure 8(n)), and then the etching mask pattern 3a remaining on the functional layer pattern 2a is removed, thereby completing an imprint mold 20 as shown in Figure 8(o), which includes a substrate 1 and functional layers 2a, 2b, and 2c with a concave-convex structure of multiple different heights that constitute a predetermined mold pattern formed on the substrate 1.

[0105] [Method for manufacturing optical elements, method for manufacturing electronic components] The present invention also provides a method for manufacturing an optical element and a method for manufacturing an electronic component. That is, the method for manufacturing an optical element according to the present invention includes the steps of: preparing an imprint mold manufactured using the laminate of the present invention described above, or the imprint mold of the present invention described above; curing the resin while pressing the imprint mold against a resin (transfer target) applied to a substrate for an optical element; and separating the imprint mold from the resin.

[0106] Furthermore, a method for manufacturing an electronic component according to the present invention includes the steps of: preparing an imprint mold manufactured using the laminate of the present invention described above; or preparing the imprint mold of the present invention described above; curing the resin while pressing the imprint mold against a resin (subject to be transferred) applied to a substrate for electronic components; and separating the imprint mold from the resin.

[0107] 9 is a cross-sectional view illustrating pattern transfer to a transfer target by imprinting. The above-described imprint mold (master mold) 20 obtained by the present invention is pressed directly against a resin (e.g., a photocurable resin or a thermosetting resin) 40 of the transfer target (transfer target), and the resin 40 is cured while the imprint mold 20 is pressed against the resin 40 (see FIGS. 9( a) and 9(b)). When a photocurable resin is used, light irradiation may be from either the imprint mold side or the resin side.

[0108] This resin 40 may be applied onto another substrate, for example, a layer constituting a transfer recipient (a substrate for an optical element or a substrate for an electronic component (e.g., a silicon wafer)). Alternatively, the resin 40 may be applied onto the imprint mold 20. Next, by separating (releasing) the imprint mold 20 from the resin 40, a transfer body 30 onto which the mold pattern of the imprint mold 20 has been transferred is obtained, as shown in FIG. 9( c). Note that by transferring the mold pattern of the imprint mold 20 to the resin 40, a replica mold can also be produced from the master mold.

[0109] By using the imprint mold 20 obtained by the present invention, a highly accurate mold pattern can be transferred to an object with high precision, making it possible to manufacture optical elements and electronic components on which highly accurate fine patterns are formed.

[0110] As described above, the present invention can provide a laminate that is suitable for use as an imprint mold blank, allowing for obtaining a desired concave-convex shape with high precision without complicating the design process or manufacturing process. The present invention can also provide an imprint mold having a high-precision mold pattern, which is produced using the above laminate, and a manufacturing method thereof. Furthermore, the present invention can provide a manufacturing method for an optical element and a manufacturing method for an electronic component, each having a high-precision fine pattern formed thereon, using the above imprint mold.

[0111] Hereinafter, the embodiments of the present invention will be described in more detail with reference to examples. (Example 1) [Preparation of Laminate] A substrate made of glass having a main surface dimension of approximately 152 mm x approximately 152 mm and a thickness of approximately 6.25 mm was prepared. The substrate used in this Example 1 was a glass substrate containing CaO, La, 2 O 3 , Nb 2 O 5 and BaO, and the details of the composition are shown in Table 1 below.

[0112] First, a functional layer made of silicon and oxygen (SiO 2The layer (Si:O=34 atomic %:66 atomic %) was formed to a thickness of 100 nm. This functional layer was formed by placing the substrate in a single-wafer RF sputtering apparatus and sputtering SiO 2 Using a target and argon (Ar) gas as the sputtering gas, the film was formed by reactive sputtering (RF sputtering) using an RF power source.

[0113] Next, an etching mask layer made of chromium and nitrogen (CrN layer, Cr:N=75 atomic %:25 atomic %) was formed on the functional layer to a thickness of 50 nm. This etching mask layer was formed by placing the substrate on which the functional layer was formed in a single-wafer DC sputtering apparatus, and sputtering the substrate with a chromium (Cr) target using argon (Ar), helium (He), and nitrogen (N 2 ) was used as a sputtering gas, and reactive sputtering (DC sputtering) was performed using a DC power source. In this manner, a laminate of Example 1 was produced in which the functional layer and the etching mask layer were formed on the substrate.

[0114] [Fabrication of Imprint Mold] A negative resist film made of a liquid photocurable resin was applied to the upper surface of the laminate of Example 1. Next, a predetermined fine pattern (mold pattern) was laser-drawn on this resist film, and after drawing, the resist film was developed to form a resist pattern.

[0115] Next, the laminate on which the resist pattern is formed is introduced into a dry etching apparatus, and a chlorine-based gas (chlorine gas (Cl 2 ) and oxygen gas (O 2 ) was used as a mask to etch the etching mask layer, thereby forming an etching mask pattern.

[0116] Here, the laminate on which the etching mask pattern was formed was temporarily removed from the dry etching device, and the remaining resist pattern was removed.

[0117] Next, in the same dry etching apparatus, 3 and C.F. 4 Mixed gas containing CHF3 :CF 4 Dry etching was performed using a SiO 2 (SiO 3 ) / SiO 2 (SiO 2 ) ratio (1:2.5). The functional layer was etched using the etching mask pattern as a mask until the main surface of the substrate was exposed, forming recesses. As shown in FIG. 3( e ), a functional layer pattern with a concave-convex structure was formed on the substrate. Here, an ICP (Inductively Coupled Plasma) etching method was used. The etching conditions were an ICP power of 425 W as plasma excitation power, an RF power (bias power) of 125 W, and a pressure of 5 mTorr. The remaining etching mask pattern was then peeled off, and an imprint mold was produced on the substrate, having a functional layer pattern with multiple convex portions of the same height.

[0118] Examples 2 to 9 Laminates of Examples 2 to 9 were prepared by depositing the functional layer and the etching mask layer on a substrate in the same manner as in Example 1, except that substrates having the glass compositions of Examples 2 to 9 shown in Table 1 below were used. Next, using each of these laminates of Examples 2 to 9, the functional layer was etched in the same manner and under the same etching conditions as in Example 1 until the main surface of the substrate was exposed, forming recesses, and imprint molds of Examples 2 to 9 were prepared, each having a functional layer pattern on the substrate in which a plurality of protrusions had the same height.

[0119] (Comparative Example) The synthetic quartz substrate (SiO 2 A comparative laminate was produced by depositing the functional layer and the etching mask layer on a substrate in the same manner as in Example 1, except that a mask layer was used. Next, using this comparative laminate, the functional layer was etched in the same manner and under the same etching conditions as in Example 1 until the main surface of the substrate was exposed, forming recesses, thereby producing a comparative imprint mold having a functional layer pattern on the substrate in which a plurality of protrusions had the same height.

[0120]

[0121] <Evaluation> The amount of processing damage to the substrate was measured in the recesses of the obtained imprint molds of Examples 1 to 9 and the Comparative Example. The results are as follows: Example 1: 69.7 nm, Example 2: 90 nm, Example 3: 97 nm, Example 4: 145 nm, Example 5: 202 nm, Example 6: 269 nm, Example 7: 662 nm, Example 8: 663.1 nm, Example 9: 674 nm, Comparative Example: 2452 nm

[0122] As is clear from the above results, in each example, the amount of processing damage to the substrate was compared with the synthetic quartz substrate (SiO 2 ) was significantly reduced to less than 30% of the amount of processing damage. In the examples of the present invention, the amount of processing damage to the substrate due to etching of the functional layer at the bottom of the recess where the main surface of the substrate was exposed was reduced to a negligible level. As a result, the recess obtained by etching the functional layer was accurately formed into the desired shape. Note that the etching selectivity of the functional layer to the substrate in all examples was 2.5 or higher. In contrast, in the comparative examples, the amount of processing damage to the substrate was large, and the recess could not be formed into the desired shape. Furthermore, in the comparative examples, the bottom of the recess was roughened, and the transmittance of light with a wavelength of 365 nm was also significantly reduced.

[0123] In another embodiment, the functional layer may be made of SiON, Si 3 N 4 , TiO 2 The functional layer was etched in the same manner as above to produce an imprint mold. 2 Similarly to the case where the substrate of the other example was used, the damage to the substrate of the comparative example was negligibly small, while the damage to the substrate of the other example was large. Furthermore, the etching selectivity of each functional layer to the substrate of the other example was 2.5 or more.

[0124] Furthermore, when optical imprint lithography was performed using the imprint molds obtained in Examples 1 to 9 as master molds to produce replica molds (see FIG. 9 above), replica molds having the desired shape with high precision were obtained. On the other hand, when the imprint molds of the comparative examples were used, replica molds having the desired shape could not be obtained.

[0125] As described above, according to the embodiments of the present invention, an imprint mold having a mold pattern of a desired shape with high precision can be obtained without complicating the design process or manufacturing process. Furthermore, this imprint mold can be used to obtain a replica mold having a desired shape with high precision, and optical elements, electronic components, etc., on which high-precision fine patterns are formed can be manufactured.

[0126] REFERENCE SIGNS LIST 1 substrate 2 functional layer 2a, 2b, 2c functional layer (protruding portion) 3 etching mask layer 4 resist film 5 recessed portion 10 laminated body 20 imprint mold (master mold) 30 transfer body 40 resin (transfer target)

Claims

1. CaO, La 2 O 3 , Nb 2 O 5 and BaO; a functional layer provided on the substrate; and an etching mask layer provided on the functional layer.

2. The laminate according to claim 1, wherein the functional layer is in contact with the substrate.

3. CaO, La contained in the substrate 2 O 3 , Nb 2 O 5 2. The laminate according to claim 1, wherein the total content of BaO is 30 mass % or more.

4. The laminate according to claim 1, characterized in that the functional layer is made of a material containing silicon and at least one of oxygen and nitrogen.

5. The laminate according to claim 1, characterized in that when the functional layer is laminated on the substrate, the transmittance of light having a wavelength of 365 nm passing through the substrate and the functional layer is 50% or more.

6. The stack of claim 1, wherein the etching mask layer contains one or more selected from the group consisting of chromium, tantalum, zirconium, hafnium and tungsten.

7. A method for manufacturing an imprint mold, comprising the steps of: preparing a laminate according to any one of claims 1 to 6; forming an etching mask pattern on the etching mask layer; etching the functional layer using the etching mask pattern as a mask; and removing the etching mask pattern.

8. An imprint mold comprising CaO, La 2 O 3 , Nb 2 O 5 and BaO; and a functional layer provided on the substrate, the functional layer having a plurality of recesses that form a predetermined mold pattern.

9. The imprint mold according to claim 8, wherein the functional layer is in contact with the substrate.

10. CaO, La contained in the substrate 2 O 3 , Nb 2 O 5 and BaO in a total content of 30 mass % or more.

11. The imprint mold according to claim 8, wherein the functional layer is made of a material containing silicon and at least one of oxygen and nitrogen.

12. The imprint mold according to claim 8, characterized in that when the functional layer is laminated on the substrate, the transmittance of light having a wavelength of 365 nm passing through the substrate and the functional layer is 50% or more.

13. The imprint mold according to claim 8, wherein the bottom surface of the recess is such that the substrate is exposed.

14. A method for manufacturing an optical element, comprising the steps of: preparing an imprint mold manufactured using a laminate described in any one of claims 1 to 6, or an imprint mold described in any one of claims 8 to 13; hardening the transfer target while pressing the imprint mold against a transfer target applied to a substrate for optical elements; and separating the imprint mold from the transfer target.

15. A method for manufacturing an electronic component, comprising the steps of: preparing an imprint mold manufactured using a laminate described in any one of claims 1 to 6, or an imprint mold described in any one of claims 8 to 13; hardening the transfer target while pressing the imprint mold against a transfer target applied to a substrate for electronic components; and separating the imprint mold from the transfer target.

Citation Information

Patent Citations

  • Mold for producing diffraction grating and its production

    JP1994258510A

  • Mask blank and manufacturing method of imprint mold

    JP2011227950A

  • Photosensitive resin laminate

    JP2012104697A

  • Mold for imprinting, substrate for making patterned medium and patterned medium, and method for manufacturing the same

    JP2014241321A

  • Substrate for patterned media production, patterned media, and production method of them

    JP2017177821A

Cited By

  • Laminate, imprint mold, optical element, and electronic device

    WO2026100331A1