Electrode
The electrode with platinum-supported graphite and optimized paraffin content addresses metal elution and corrosion issues, enhancing the efficiency and stability of electrolytic manganese dioxide production by reducing moisture adhesion and electrolytic voltage.
Patent Information
- Application Number
- PCT/JP2024/008377
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-03
AI Technical Summary
Existing electrodes for producing electrolytic manganese dioxide face challenges such as metal elution and corrosion in high-temperature, sulfuric acid environments, leading to inefficiencies and increased costs, and the need to reduce moisture adherence during electrolysis.
An electrode structure is developed with platinum supported on graphite and containing paraffin, where the platinum loading is optimized between 3 μg/cm² and 500 μg/cm², and paraffin content is between 1 mg/g and 100 mg/g, with a melting point of 40°C to 80°C, to reduce moisture adhesion and electrolytic voltage.
This configuration effectively reduces metal elution, maintains electrode stability under high-temperature conditions, and decreases the electrolytic voltage, enabling efficient and stable production of electrolytic manganese dioxide.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
electrode
[0001] The present disclosure relates to an electrode, and more particularly to an electrode for producing electrolytic manganese dioxide, for example, an electrode used in producing electrolytic manganese dioxide used as a positive electrode active material in manganese dry batteries, particularly alkaline manganese dry batteries.
[0002] Electrolytic manganese dioxide is generally produced by electrolytic oxidation deposition on the anode by passing a current between the anode and cathode in a sulfuric acid-acidic manganese sulfate electrolyte at a temperature close to 100°C. While the anode is where the electrolytic manganese dioxide deposition reaction occurs, the cathode, where the hydrogen evolution reaction occurs, does not directly affect the quality of the electrolytic manganese dioxide. For this reason, the cathode has not received much attention, and there have been few previous studies on it.
[0003] Graphite is primarily used for the cathode, but copper and steel are also used (Patent Document 1). For example, Patent Document 2 studies a cathode in which graphite is coated with copper. However, when a copper-containing cathode is immersed in a high-temperature electrolyte containing sulfuric acid, copper dissolves into the electrolyte when no current is applied. Furthermore, in electrolysis at temperatures approaching 100°C in an acidic sulfuric acid environment, even corrosion-resistant metals such as titanium and stainless steel corrode when no current is applied. On the other hand, cathodes for salt electrolysis or water electrolysis (Patent Documents 3 and 4) are not designed for use in an acidic sulfuric acid environment at temperatures approaching 100°C. Therefore, these electrodes contain elements that may affect the quality of manganese dioxide, and are expensive to manufacture, making them difficult to use as cathodes for manganese dioxide electrolysis.
[0004] During the production of electrolytic manganese dioxide, the electrolyte is maintained at a high temperature of 93°C to 98°C. To prevent evaporation of the electrolyte, a layer of oil with a high boiling point, such as paraffin, is floated on top of the electrolyte. However, because paraffin affects the product quality of electrolytic manganese dioxide, methods for removing paraffin that has been incorporated into electrolytic manganese dioxide and electrolysis methods that do not incorporate paraffin have been investigated (Patent Document 2).
[0005] Furthermore, electrodes such as cathodes and anodes are inserted and removed from the top of an electrolytic cell or a cleaning cell during electrolysis or cleaning, and when they are pulled up, the electrolyte or cleaning solution adheres to them. Because the electrolyte or other liquid adhering to the electrodes is lost, there is a need to reduce the amount of water, such as the electrolyte, adhering to the electrodes.
[0006] International Publication No. 2000 / 037714 Japanese Patent Application Laid-Open No. 2022-7926 International Publication No. 2020 / 110527 Japanese Patent Application Laid-Open No. 6837342 Japanese Patent Application Laid-Open No. 2001-247987
[0007] The present disclosure provides an electrode for producing electrolytic manganese dioxide, which has been modified for the purpose of reducing the electrolysis voltage without causing metal detachment or elution even when immersed in a high-temperature, sulfuric acid-acidic electrolyte, and which has a small amount of water attached when pulled out from an aqueous solution.
[0008] In this disclosure, we have focused on the performance expression and metal elution of electrodes used in the production of electrolytic manganese dioxide, and have investigated electrode modification. As a result, we have found that the inclusion of paraffin reduces the amount of moisture attached when the electrode is pulled up, and that supporting platinum on graphite prevents an increase in bath voltage during electrolysis, even under high-temperature, highly concentrated sulfuric acid conditions.
[0009] That is, the present invention is as defined in the claims, and the gist of the present disclosure is as follows: [1] An electrode having a structure in which platinum is supported on graphite and containing paraffin. [2] The electrode according to [1] above, which is an electrode for producing electrolytic manganese dioxide. [3] The amount of platinum supported per unit area on the graphite is 3 μg / cm. 2 More than 500μg / cm 2[4] The electrode according to any one of [1] to [3] above, wherein the content of the paraffin is 1 mg / g or more and 100 mg / g or less, based on the weight of the portion of the electrode immersed in the electrolyte during electrolysis. [5] The electrode according to any one of [1] to [4] above, wherein the melting point of the paraffin is 40°C or more and 80°C or less. [6] The electrode according to any one of [1] to [5] above, wherein the contact angle of the electrode surface with pure water is more than 90° and less than 180°. [7] A method for producing electrolytic manganese dioxide, using the electrode according to any one of [1] to [6]. [8] A method for producing an electrode according to any one of [1] to [6] above, comprising a platinum supporting step of supporting platinum on graphite to obtain platinum-supported graphite, and a paraffin-containing step of contacting the platinum-supported graphite with paraffin to incorporate paraffin into the platinum-supported graphite. [9] A method for producing an electrode according to [8] above, wherein the method for supporting platinum on graphite in the platinum supporting step is a plating method.
[10] A method for producing an electrode according to [8] above, wherein the paraffin-containing step is a method in which paraffin is attached to the surface of the platinum-supported graphite and then penetrates into the platinum-supported graphite.
[0010] The present disclosure provides an electrode for producing electrolytic manganese dioxide, which has been modified for the purpose of reducing the electrolysis voltage without causing metal detachment or elution even when immersed in a high-temperature, sulfuric acid-acidic electrolyte, and which exhibits a small amount of adhering water when removed from an aqueous solution. Furthermore, the electrode of the present disclosure prevents metal elution from the electrode plate into the electrolyte even when no current is applied during electrolysis in the production of manganese dioxide, further reducing the electrolysis voltage. Furthermore, the amount of liquid adhering when the electrode is removed from an electrolytic bath or cleaning bath can be reduced, enabling efficient and stable production of electrolytic manganese dioxide.
[0011] An example of an embodiment of the present disclosure will be described in detail below. The present disclosure includes any combination of the configurations and parameters disclosed herein, and also any combination of the upper and lower limits of the numerical values disclosed herein. <Electrode> The electrode of this embodiment has a structure in which platinum is supported on graphite and contains paraffin, i.e., an electrode containing platinum-supported graphite and paraffin. Furthermore, the electrode of this embodiment can also be considered as an electrode having a graphite substrate on which platinum is supported and containing paraffin, or even as an electrode having a graphite substrate on which platinum is supported and containing paraffin.
[0012] Graphite is the electrode substrate of the electrode of this embodiment.
[0013] The type of graphite may be, for example, one or more selected from the group consisting of natural graphite, artificial graphite, carbon black, pyrolytic graphite, and carbon fiber, with artificial graphite being preferred from the viewpoint of ease of availability and processing.
[0014] The shape of the graphite may be any shape that can be used as an electrode for producing electrolytic manganese dioxide, and examples thereof include a plate shape or a rectangular parallelepiped shape that is also used in metal refining and plating, but the shape is not essentially limited to these. Preferred examples of the shape of graphite include a rectangular parallelepiped (columnar) and a plate shape.
[0015] Platinum is a catalyst for the electrolytic oxidation reaction in the production of electrolytic manganese dioxide. The platinum may be in a state that functions as a catalyst, and examples thereof include one or more selected from the group consisting of metallic platinum, platinum alloys, and platinum compounds. Metallic platinum is preferred as the platinum, as this allows for a further reduction in the bath voltage during the production of electrolytic manganese dioxide.
[0016] The platinum alloy is a metal containing platinum and a metal element other than platinum, and examples thereof include a metal containing platinum (Pt) and one or more elements selected from the group consisting of silver (Ag), gold (Au), cobalt (Co), copper (Cu), iron (Fe), iridium (Ir), manganese (Mn), nickel (Ni), palladium (Pd), ruthenium (Ru), titanium (Ti), and zirconium (Zr).
[0017] The platinum compound is a compound containing platinum and a non-metallic element, and examples thereof include compounds containing platinum (Pt) and one or more elements selected from the group consisting of carbon (C), chlorine (Cl), and oxygen (O).
[0018] The electrode of this embodiment has a structure in which platinum is supported on graphite, and in particular, a structure in which platinum is supported on the graphite surface. By supporting platinum on the graphite surface, that is, by supporting platinum on the graphite that is the electrode substrate, the bath voltage during the production of electrolytic manganese dioxide can be further reduced.
[0019] In the electrode of this embodiment, platinum may be supported on the portion of graphite where the electrolytic reaction of electrolytic manganese dioxide occurs, and platinum may be supported on part or all of the graphite surface. Because this allows for a reduction in the amount of platinum used, which is a precious metal, it is preferable that platinum be supported on part of the graphite surface. In other words, the graphite may have regions where platinum is supported and regions where platinum is not supported.
[0020] Platinum acts as an electrode catalyst by being present on graphite and maintaining electrical contact with it. It is known that platinum's hydrogen evolution electrode catalytic activity is superior to that of carbon, the source of graphite. For example, the minimum hydrogen evolution overvoltage under 2N sulfuric acid aqueous solution conditions is 335 mV for carbon, while that of platinum is 0.002 mV. Therefore, compared to graphite, platinum exhibits superior catalytic activity at a lower hydrogen evolution overvoltage.
[0021] The graphite in the electrode of this embodiment has a platinum carrying amount per unit area (hereinafter also simply referred to as "platinum carrying amount") of 3 μg / cm 2 More than 500μg / cm 2 It is preferable that the concentration is 10 μg / cm or less. 2 More than 400μg / cm 2 More preferably, 20 μg / cm 2 More than 200μg / cm 2 The following is even more preferable: When the amount of supported platinum is within the above range, the supported metal (i.e., platinum) does not fall off even under high-temperature and high-concentration sulfuric acid acid conditions, and the bath voltage during electrolysis in the production of electrolytic manganese dioxide can be reduced.
[0022] In this embodiment, the amount of supported platinum can be determined from the following formula using a composition obtained by composition analysis by inductively coupled plasma optical emission spectroscopy (ICP) of a solution obtained by pulverizing and dissolving the platinum-supported region of an electrode sample in acid.
[0023] G = M / A G is the amount of platinum supported (μg / cm 2 ), M is the amount of platinum (μg) determined from the platinum concentration of the solution obtained by ICP measurement, and A is the area (cm ) of the region where platinum is supported in the electrode sample. 2 )
[0024] The ICP method may be carried out using a general inductively coupled plasma emission spectrometer (for example, trade name: OPTIMA3000DV, manufactured by PERKIN ELMER).
[0025] The dissolution solution may be prepared by a known method capable of dissolving the electrode sample, such as a method in which the platinum-supported region of the electrode is crushed, the electrode sample is heated in an air atmosphere at 400°C to 700°C, a mixed solution of concentrated sulfuric acid and concentrated nitric acid is added to the crushed electrode sample, and the mixture is heated in an air atmosphere to evaporate and dry, and then the dried product is dissolved in aqua regia.
[0026] The electrode of this embodiment contains paraffin. By containing paraffin, the amount of liquid adhering to the electrode of this embodiment when it is removed from an electrolytic bath or a cleaning bath can be reduced. The paraffin is a hydrocarbon mixture primarily composed of linear hydrocarbons having 16 to 40 carbon atoms, and is preferably the same as that used to prevent evaporation of a manganese dioxide electrolytic bath (i.e., to prevent evaporation of the electrolyte used in the production of electrolytic manganese dioxide). To prevent evaporation, the paraffin preferably becomes liquid during electrolysis and solidifies at room temperature during recovery. Therefore, the melting point of the paraffin is preferably 40°C or higher and 80°C or lower, i.e., the paraffin has a melting point of 40°C or higher and 80°C or lower, and more preferably, a melting point of 50°C or higher and 65°C or lower. A specific example of paraffin is Paraffin Wax-125 (manufactured by Nippon Seiro Co., Ltd.; melting point: 53°C).
[0027] The content of paraffin is preferably 1 mg / g or more and 100 mg / g or less, more preferably 3 mg / g or more and 80 mg / g or less, and even more preferably 3 mg / g or more and 50 mg / g or less, relative to the mass (unit mass) of the portion immersed in the electrolyte (hereinafter also referred to as the "immersed portion") in the production of electrolytic manganese dioxide using the electrode of this embodiment. When the paraffin content is within the above range, the amount of moisture (amount of adhered liquid) is reduced. As long as it does not interfere with platinum support (i.e., within a range where platinum can be supported), paraffin may be contained in the graphite before platinum support, or may be impregnated into the electrode after platinum support.
[0028] The content of paraffin in this embodiment is the mass of paraffin relative to the weighed mass (g) of the electrode of this embodiment.
[0029] The unit moisture content of the electrode of this embodiment is 0 mg / cm 2 4.0mg / cm or more 2 Preferably, 0 mg / cm 2 3.0mg / cm or more 2 More preferably, 0 mg / cm 2 2.5mg / cm or more 2 The following is more preferable: When the unit moisture adhesion amount is within the above range, the amount of liquid adhering to the electrode of this embodiment when it is removed from the electrolytic bath or cleaning bath can be reduced, and loss of the electrolytic solution and cleaning solution can be reduced.
[0030] In this embodiment, the unit moisture content is calculated by dividing the mass difference between before and after immersion of the electrode in pure water by the surface area (cm 2 ) and the value (mg / cm 2 If the graphite has a region where platinum is not supported, the region may be masked and immersed in pure water.
[0031] The contact angle of the electrode of this embodiment is preferably greater than 90° and less than 180°, more preferably 95° or greater and less than 180°, and even more preferably 100° or greater and less than 180°. When the contact angle exceeds 90°, the amount of liquid adhering to the electrode of this embodiment when it is removed from the electrolytic bath or cleaning bath can be reduced, and loss of the electrolytic solution and cleaning solution can be further reduced.
[0032] The contact angle in this embodiment is a value determined by the following method.
[0033] That is, using a contact angle meter (for example, device name: DMo-501, manufactured by Kyowa Interface Science Co., Ltd.) and measurement and analysis software (for example, FAMAS1, manufactured by Kyowa Interface Science Co., Ltd.), 2.0±0.1 μL of pure water is dropped onto the platinum-supported area at room temperature (25°C±5°C). Assuming that the shape of the droplet 60 seconds after dropping is a part of a perfect circle, the contact angle (°) of the electrode with pure water is measured using the following θ / 2 method. The number of measurements is three, and the arithmetic average value can be used as the contact angle of the electrode of this embodiment.
[0034] Contact angle (°) = 2 × arctan (h / r), where h: distance (mm) from the electrode surface to the apex of the droplet, and r: radius (mm) of the contact surface between the electrode surface and the droplet. The electrode of this embodiment can be used as a cathode for producing electrolytic manganese dioxide. When a plate-shaped electrode of this embodiment having a height of 250 mm, a width of 200 mm, and a thickness of 10 mm is used as a cathode, the voltage in electrolysis under the following conditions (hereinafter also referred to as "bath voltage") is preferably 1.23 V or more and 2.00 V or less, more preferably 1.23 V or more and 1.80 V or less, and even more preferably 1.23 V or more and 1.70 V or less.
[0035] Anode: Titanium electrode (plate-shaped, 250 mm high, 200 mm wide, and 10 mm thick) Electrode spacing: 50 mm Electrolyte: 6 L of a mixed aqueous solution of 85.4 g / L manganese sulfate and 27.0 g / L sulfuric acid, and 50 g of paraffin Electrolyte replenisher: 118 g / L manganese sulfate aqueous solution Electrolysis temperature: 96°C Electrolysis current density: 0.65 A / dm 2 Prior to electrolysis, the cathode and anode are placed in this order, anode, cathode, and anode, with their main surfaces (height x width) facing each other, at an interval of 50 mm in an electrolytic cell filled with an electrolytic solution and paraffin and heated to 96° C. Thereafter, electrolysis is carried out for 24 hours.
[0036] During electrolysis, the concentration of manganese ions decreases due to the precipitation of electrolytic manganese dioxide as the electrolytic reaction progresses. To maintain a constant manganese ion concentration in the electrolyte, it is preferable to continuously supply an aqueous manganese sulfate solution (electrolyte replenisher) to the electrolytic cell during electrolysis. It is more preferable to supply the aqueous manganese sulfate solution while discharging the electrolyte in an amount equal to the amount of the aqueous manganese sulfate solution supplied. This allows the manganese ion concentration in the electrolyte to be maintained constant.
[0037] The electrode of this embodiment is resistant to platinum elution even when immersed in an electrolyte solution for producing electrolytic manganese dioxide. Therefore, the electrode of this embodiment has a platinum content in the sulfuric acid-manganese sulfate mixed aqueous solution (hereinafter also referred to as the "platinum elution amount") after immersion in the sulfuric acid-manganese sulfate mixed aqueous solution under the following immersion conditions, which may be 0 mg / L or more and 2 mg / L or less, 0 mg / L or more and 1 mg / L or less, 0 mg / L or more and 0.5 mg / L or less, or 0 mg / L or more and 0.1 mg / L or less.
[0038] (Immersion conditions) Electrode shape: Plate-like, 250 mm high, 200 mm wide, and 10 mm thick Sulfuric acid-manganese sulfate mixed aqueous solution: 6 L (sulfuric acid concentration 27.0 g / L) (manganese sulfate concentration 85.4 g / L) Heat-up start temperature: 86°C Heat-up rate: 0.1°C / min Immersion temperature: 96°C Immersion time: 80 min Furthermore, the electrode of this embodiment is preferably resistant to platinum elution even when no current is applied after the electrolysis reaction. After electrolysis under the following electrolysis conditions, the electrode of this embodiment preferably has a platinum concentration in the electrolyte three hours after the electrolysis is stopped (hereinafter also referred to as "amount of elution without current application") of 0 mg / L or more and 2 mg / L or less, 0 mg / L or more and 1 mg / L or less, 0 mg / L or more and 0.5 mg / L or less, or 0 mg / L or more and 0.1 mg / L or less.
[0039] (Electrolysis conditions) Anode: Titanium electrode (plate-shaped, 250 mm high, 200 mm wide, and 10 mm thick) Electrode spacing: 50 mm Electrolyte: 6 L of a mixed aqueous solution of 85.4 g / L manganese sulfate and 27.0 g / L sulfuric acid, and 50 g of paraffin Electrolyte replenisher: 118 g / L manganese sulfate aqueous solution Electrolysis temperature: 96°C Electrolysis current density: 0.65 A / dm 2 Electrolysis period: 6 days. By keeping the amount of platinum eluted without current application within the above range, it is possible to suppress an increase in bath voltage during electrolysis in the production of electrolytic manganese dioxide. Furthermore, by keeping the amount of platinum eluted in the electrolyte at the end of the electrolysis within the above range, the life of the electrodes is extended, and electrolytic manganese dioxide can be repeatedly produced.
[0040] The electrode of this embodiment can reduce the electrolysis voltage in the electrolytic reaction using the electrode. Therefore, the electrode of this embodiment can be used as an electrode (cathode) for producing electrolytic manganese dioxide, thereby enabling efficient production of electrolytic manganese dioxide. <Electrode Manufacturing Method> The electrode of this embodiment can be manufactured, for example, by using platinum and supporting it by electroplating or electroless plating in an electrolyte containing precious metal ions using a graphite plate as the working electrode so that the above-mentioned loading amount is achieved. Alternatively, the electrode can be manufactured by an electrode manufacturing method including a paraffin-containing step of incorporating paraffin into platinum-supported graphite. A preferred method for manufacturing the electrode of this embodiment is an electrode manufacturing method including a platinum-supporting step of supporting platinum on graphite to obtain platinum-supported graphite, and a paraffin-containing step of contacting the platinum-supported graphite with paraffin to incorporate paraffin into the platinum-supported graphite.
[0041] The method for supporting platinum on graphite in the platinum supporting step may be any method that can support platinum on graphite, and is preferably a plating method, more preferably at least one of electroplating and electroless plating, and even more preferably electroplating.
[0042] A preferred electroplating method for supporting platinum on graphite is to use a titanium platinum electrode as the anode, graphite as the cathode, and a mixed solution of chloroplatinic acid (VI) and hydrochloric acid as the plating solution, at a temperature of 50°C to 100°C, and a current density of 0.3 A / dm 2 Above, 2.0A / dm 2 Electroplating can be performed at a temperature of 60°C to 90°C and a current density of 0.5 A / dm 2 Above, 1.5A / dm 2 It is preferable to electroplate with the following:
[0043] The longer the electroplating time, the greater the amount of platinum supported. The plating time may be any time depending on the desired amount of platinum supported and the size of the graphite (electrode substrate), and may be, for example, from 15 seconds to 2 minutes.
[0044] In order to prevent the platinum from falling off after plating, it is preferable to polish the graphite prior to supporting platinum.
[0045] After the platinum supporting step, a washing step of washing the platinum-supported graphite may be performed prior to the paraffin-containing step. The washing step can reduce impurities such as plating solution remaining on the surface. The washing method in the washing step may be any method capable of reducing impurities, and includes washing with pure water. A preferred washing method includes immersion in warm water at 30°C or higher and 100°C or lower for 10 minutes or longer and then washing with pure water.
[0046] The washed platinum-supported graphite is preferably dried by any method. The drying conditions are arbitrary, but examples include drying in the air at 30° C. or higher and 100° C. or lower for 1 hour or longer and 24 hours or shorter.
[0047] The paraffin-containing step is a step of contacting the platinum-supported graphite with paraffin to cause the platinum-supported graphite to contain paraffin.
[0048] The contact of the platinum-supported graphite with paraffin may be carried out by any method, as long as paraffin is attached to the surface of the platinum-supported graphite and then penetrated into the interior of the platinum-supported graphite. For example, a method may be used in which the platinum-supported graphite is immersed in pure water having a paraffin layer on the surface and a temperature of 60°C or higher but lower than 100°C, with pure water of 80°C or higher but lower than 100°C being preferred. The platinum-supported graphite passes through the paraffin layer, causing paraffin to adhere to the surface of the platinum-supported graphite. The platinum-supported graphite is then immersed in pure water at the above-mentioned temperature range, allowing the molten paraffin to penetrate the platinum-supported graphite. The thickness of the paraffin layer may be any thickness that allows the paraffin to adhere uniformly to the surface of the platinum-supported graphite, and may be, for example, 1 cm or higher but 2 cm or lower. The immersion time is optional, but may be 1 hour or higher but 24 hours or lower, and preferably 5 hours or higher but 24 hours or lower.
[0049] After the immersion, the platinum-supported graphite is preferably immersed in warm water containing no paraffin, washed with warm water, and dried, thereby removing the paraffin remaining on the outermost surface of the platinum-supported graphite.
[0050] Hereinafter, the present disclosure will be described with reference to examples, but the present disclosure is not limited to the following examples.
[0051] <Measurement of Metal Support Amount> The metal support amount was measured by measuring the metal concentration in the measurement solution by inductively coupled plasma optical emission spectrometry (ICP method) using a general inductively coupled plasma optical emission spectrometer (trade name: OPTIMA3000DV, manufactured by PERKIN ELMER).
[0052] The measurement solution was prepared as follows. First, a stamp mill was used to pulverize the platinum-loaded region of the electrode sample until it could pass through a 0.5 mm mesh sieve. The electrode samples were cut out from the portion immersed in the plating bath described below. Specifically, samples were used: those cut out from the bottom of a graphite rod (described below) up to 5 cm (Examples 1 and 2, Comparative Examples 1 to 4); and those cut out from the largest surface (i.e., the height × width surface, hereinafter also referred to as the "main surface") of a graphite plate (described below) 4 cm from the bottom edge of the graphite plate, extending 2 cm to 6 cm to the right or left and 5 cm above the center in the width direction (the point that bisects a perpendicular line drawn parallel to the width direction from the left edge to the right edge of the graphite plate) (i.e., a 5 cm high, 4 cm wide range) (Examples 3 to 8, Comparative Examples 5 to 8).
[0053] The crushed electrode sample (pieces) was then placed in a porcelain crucible and heated at 600°C for 70 hours in an air atmosphere. 1 mL of concentrated sulfuric acid and 2 mL of concentrated nitric acid were added and heated to evaporate and dry, followed by dissolution with aqua regia to obtain a solution. Pure water was added to the solution until the volume reached 1 L, and the metal concentration of the resulting solution was measured.
[0054] The metal loading amount was calculated from the metal concentration of the measurement solution obtained by ICP measurement using the following formula.
[0055] G = C × W1 / W2 × V / A In the above formula, G is the metal loading amount (mg / cm 2 ), C is the metal concentration (mg / L) of the measurement solution obtained by ICP measurement, W1 is the mass (g) of the cut-out electrode sample, W2 is the mass (g) of the crushed electrode sample (pieces), V is the volume of the measurement solution (=1 (L) except for Example 7, which was 0.1 L), and A is the surface area (cm 2 )
[0056] <Paraffin Content> The paraffin content of the electrode sample was measured by gas chromatography using a gas chromatograph (Agilent 7890A GC, manufactured by Agilent Technologies, Inc.).
[0057] 1.0 g of electrode sample (fragments) pulverized in the same manner as in the measurement of metal loading and 5 mL of hexane were added to a screw-cap sample tube and shaken for 15 minutes. The mixture was then centrifuged at 3000 rpm for 15 minutes and filtered using a filter (product name: MyShoriDisc H-13-5, manufactured by Tosoh Corporation). The hexane layer recovered was used as the measurement sample. The measurement sample was subjected to gas chromatography, and the signal detected by the FID detector attached to the instrument was compared with the signal of a standard sample to determine the paraffin content.
[0058] As a standard sample, a hexane solution containing paraffin (trade name: Paraffin Wax-125, manufactured by Nippon Seiro Co., Ltd.) at a concentration of 10 mg / L was used.
[0059] <Measurement of Amount of Metal Dissolved into Electrolyte at Start> The amount of metal dissolved into the electrolyte at the start of the electrode sample was measured by ICP method using a general inductively coupled plasma emission spectrometer (product name: OPTIMA3000DV, manufactured by PERKIN ELMER).
[0060] The metal concentration in the diluted electrolyte solution obtained by diluting the initial electrolyte solution (described later) 10 times with pure water was measured by ICP. The metal concentration obtained by multiplying the measured value by 10 was defined as the metal concentration (mg / L) in the initial electrolyte solution.
[0061] <Measurement of Adhesion Amount of Water and Unit Adhesion Amount of Water> The amount of water in the electrodes of each Example or Comparative Example was measured by measuring the mass of the electrode before and after immersion in pure water. That is, a screw cap bottle filled with pure water was placed on an electronic balance. A rod-shaped electrode was immersed in the screw cap bottle so that the entire electrode surface was immersed in pure water. After immersion for 10 seconds, the rod-shaped electrode was removed from the screw cap bottle. The difference in the values on the electronic balance before and after immersion of the electrode (i.e., the difference between the mass of the rod electrode before immersion and the mass of the rod electrode after removal) was calculated and used as the adhesion amount of water (mg).
[0062] The measurement sample used was a rod-shaped electrode whose portion above 5 cm from the bottom was covered with PTFE tape.
[0063] The measurement was carried out three times, and the arithmetic mean value was taken as the amount of attached water (mg).
[0064] The resulting amount of water adhering (mg) was then calculated based on the surface area (cm 2 ) to obtain the unit moisture content (mg / cm 2 )
[0065] Electrode surface area (cm 2 ) is the surface area (cm) of the platinum-supported region 2 )
[0066] <Measurement of Contact Angle> The contact angle of the electrode was measured using a contact angle meter (device name: DMo-501, manufactured by Kyowa Interface Science Co., Ltd.) and the measurement and analysis software (FAMAS1, manufactured by Kyowa Interface Science Co., Ltd.) attached to the device. A 2.0±0.1 μL droplet of pure water was dropped onto the electrode surface in an environment at room temperature of 25° C., and the shape of the droplet 60 seconds after dropping was assumed to be a part of a perfect circle, and the contact angle (°) of the electrode with respect to pure water was measured using the following θ / 2 method.
[0067] Contact angle (°) = 2 × arctan (h / r), where h is the distance (mm) from the electrode surface to the apex of the droplet, and r is the radius (mm) of the contact surface between the electrode surface and the droplet. The measurement was performed three times, and the arithmetic mean value was taken as the contact angle (°).
[0068] <Measurement of Bath Voltage and Electrode Durability> The bath voltage and electrode durability of the electrodes of each Example or Comparative Example were confirmed by electrolytically synthesizing electrolytic manganese dioxide using an electrolytic cell equipped with a graphite plate of each Example or Comparative Example as the cathode, a titanium plate as the anode, and a manganese sulfate-sulfuric acid mixed aqueous solution as the electrolyte.
[0069] First, 6 L of the electrolyte and 50 g of paraffin for preventing evaporation of the electrolyte were added to an electrolytic cell, and then the temperature was raised to 86° C. A manganese sulfate-sulfuric acid mixed aqueous solution having a manganese sulfate concentration of 85.4 g / L and a sulfuric acid concentration of 27.0 g / L was used as the electrolyte.
[0070] Next, one plate electrode (cathode) of each Example or Comparative Example and two titanium plate anodes (height 250 mm, width 200 mm, thickness 5 mm) were immersed in the electrolyte to a depth of 160 mm so that they were perpendicular to the liquid surface of the electrolyte. The cathode and anode were then fixed at a 50 mm interval so that their main surfaces (height x width surfaces) faced each other (i.e., anode, cathode, anode in that order). The electrolyte was then heated to 96 ° C. over 3 hours. After completion of the temperature rise, 50 mL of electrolyte was collected (hereinafter, the electrolyte collected after completion of the temperature rise is also referred to as the "initial electrolyte").
[0071] Thereafter, a DC stabilized power supply (PAN-18-10A, manufactured by Kikusui Electronics Co., Ltd.) was connected, and a current of 4.48 A (i.e., 0.65 A / dm 2 Electrolytic synthesis of electrolytic manganese dioxide was carried out at a constant current of 1000 kJ / s. During electrolysis, an aqueous manganese sulfate solution (electrolyte replenisher) with a manganese sulfate concentration of 118 g / L was continuously supplied to the electrolytic cell so as to prevent the composition of the electrolytic solution from changing, and the electrolytic solution was continuously withdrawn from the electrolytic cell so that the amount of electrolytic solution in the electrolytic cell was kept constant at 6 L. 24 hours after the start of electrolysis, the voltage display of the DC stabilized power supply was read and used as the bath voltage.
[0072] Electrolysis was continued for another 6 days, and then stopped on the 7th day after the start of electrolysis. 3 hours after the electrolysis was stopped, 50 mL of electrolyte was collected (hereinafter, the electrolyte collected 3 hours after the electrolysis was stopped 7 days after the start of electrolysis is also referred to as the "finishing electrolyte"). Furthermore, the amount of metal eluted into the finishing electrolyte, i.e., the amount of metal eluted without current application (mg / L), was measured using the same method as in the above <Measurement of the amount of metal eluted into the starting electrolyte>.
[0073] Example 1: All six surfaces of a rectangular parallelepiped (columnar) graphite rod (PSG322, manufactured by SEC Carbon Co., Ltd.) measuring 100 mm in length (height), 10 mm in width, and 10 mm in thickness were polished with #400 grit sandpaper (hereinafter, the graphite rod described above that had been polished will also be referred to as a "graphite rod"). The bottom of the rod was covered with masking tape for plating (manufactured by 3M Co.) from 50 mm to 70 mm from the bottom (the portion covering the length was 50 to 70 mm from the bottom).
[0074] Thereafter, the graphite rod was immersed in an electrolyte solution of 10 g / L of chloroplatinic acid (VI) and 20 g / L of hydrochloric acid at 70°C, and the graphite rod was used as a plating bath with the titanium platinum electrode as the anode and the graphite rod as the cathode. This plating bath was used at a cathode current density of 1.0 A / dm 2 The graphite rod was electroplated at 100° C. for 2 minutes to support platinum on the graphite rod (i.e., the portion of the graphite rod extending from the bottom surface to 50 mm in the longitudinal direction).
[0075] After platinum loading, the masking tape was removed from the graphite rod, which was then immersed in 50°C hot water for 30 minutes, rinsed with running water, and then dried in an ambient atmosphere at 50°C for 12 hours. (Hereinafter, the process from masking tape coating to drying at 50°C will also be referred to as the "platinization process.") The electrode was then immersed overnight to a height of 6.5 cm from the bottom in a solution containing 1.5 cm of paraffin (product name: Paraffin Wax-125, manufactured by Nippon Seiro Co., Ltd., melting point 53°C) melted in 97°C hot water. After removing the electrode from the hot water containing the paraffin, it was transferred to a beaker filled with 75°C hot water before the paraffin solidified. An additional 10 minutes of 75°C hot water was poured over the electrode to remove the surface paraffin. The electrode was then air-dried at room temperature for one day, resulting in the electrode of Example 1. (Hereinafter, the process from immersion in warm water containing floating paraffin to air drying will also be referred to as the "paraffin-containing process.") The unit platinum loading was 140 μg / cm 2 , paraffin content was 2.9 mg / g, moisture content was 41 mg, and unit moisture content was 2.0 mg / cm 2 , and the contact angle was 124°.
[0076] Example 2 An electrode of Example 2 was obtained in the same manner as in Example 1, except that the electroplating time was set to 30 seconds.
[0077] The unit platinum loading is 31 μg / cm 2 , paraffin content 4.5 mg / g, moisture adhesion amount 48 mg, unit moisture adhesion amount 2.3 mg / cm 2 , and the contact angle was 123°.
[0078] Comparative Example 1 A graphite rod prepared in the same manner as in Example 1 was used as the electrode of Comparative Example 1 (i.e., the same operations as in Example 1 were performed except that the platinum plating step and the paraffin impregnation step were not performed).
[0079] The water adhesion amount of the electrode of this comparative example was 95 mg, and the unit water adhesion amount was 4.5 mg / cm 2 , and the contact angle was 84°.
[0080] Comparative Example 2 A black electrode for comparative example was prepared in the same manner as in Example 1, except that the platinum plating step was not carried out.
[0081] No platinum was detected from this electrode (unit platinum content: 0 mg / g), the paraffin content was 18 mg / g, the water adhesion amount was 44 mg, and the unit water adhesion amount was 2.1 mg / cm 2 , and the contact angle was 113°.
[0082] Comparative Example 3 An electrode of Comparative Example 3 was prepared in the same manner as in Example 1, except that the paraffin impregnation step was not carried out.
[0083] The unit platinum loading is 140 μg / cm 2 , paraffin was not detected (paraffin content was 0 mg / g), the moisture adhesion amount was 95 mg, and the unit moisture adhesion amount was 4.5 mg / cm 2 , and the contact angle was 81°.
[0084] Comparative Example 4 An electrode of Comparative Example 4 was prepared in the same manner as in Example 2, except that the paraffin impregnation step was not carried out.
[0085] The unit platinum loading is 32 μg / cm 2 , no paraffin was detected, the moisture content was 110 mg, and the unit moisture content was 5.2 mg / cm 2 , and the contact angle was 74°.
[0086] The results of these examples and comparative examples are shown in the table below.
[0087] From the table above, we can see that when paraffin is impregnated into graphite, the amount of moisture adhering to the electrode decreases. Furthermore, we can see that for electrodes containing paraffin, the contact angle of pure water increases, and the amount of moisture adhering decreases, regardless of whether or not there is metal plating and the amount of metal plating.
[0088] Example 3: A rectangular parallelepiped graphite plate (PSG322, manufactured by SEC Carbon Co., Ltd.; hereinafter also referred to as "graphite plate") measuring 250 mm in height, 200 mm in width, and 10 mm in thickness was used. The graphite plate was covered with plating masking tape (manufactured by 3M) from 160 mm to 185 mm from its bottom. The portion from the bottom to 160 mm (160 mm in height from the bottom) was then immersed in an electrolyte solution containing 10 g / L of chloroplatinic acid (VI) and 20 g / L of hydrochloric acid maintained at 70°C. The two largest surfaces (height × width surfaces; hereinafter also referred to as "main surfaces") of the graphite plate were set facing each other. A plating bath was constructed using two titanium-platinum electrodes as the anode and the graphite plate as the cathode. This plating bath was used at a cathode current density of 1.0 A / dm 2 Electroplating was performed at 40°C for 4 minutes, and platinum was supported on the electrode. Thereafter, the masking tape was removed, and the electrode was immersed in 50°C warm water for 30 minutes, further washed with running water, and then dried at 50°C for 12 hours. Subsequently, the electrode was immersed overnight to a height of 15 cm from the bottom in 97°C warm water with a 1.5 cm thickness of paraffin (product name: Paraffin Wax-125, manufactured by Nippon Seiro Co., Ltd., melting point 53°C). After being removed from the warm water with the floating paraffin, the electrode was immersed in a container filled with 75°C warm water before the paraffin solidified, and then further 75°C warm water was poured over it for 10 minutes to remove the paraffin on the surface. The electrode was then air-dried at room temperature for 1 day, and used as the electrode of Example 3.
[0089] The unit platinum loading is 400 μg / cm 2 The paraffin content was 44 mg / g, the contact angle was 133°, and the bath voltage was 1.52 V. No platinum was detected in the initial or final electrolyte, and therefore the amount of platinum eluted and the amount of platinum eluted without current application were both 0 mg / L.
[0090] Example 4 An electrode was prepared in the same manner as in Example 3 except that the electroplating time was set to 2 minutes, to prepare the electrode of this example.
[0091] The unit platinum loading is 130 μg / cm 2 The paraffin content was 19 mg / g, the contact angle was 114°, and the bath voltage was 1.50 V. No platinum was detected in the initial or final electrolyte, and therefore the amount of platinum eluted and the amount of platinum eluted without current application were both 0 mg / L.
[0092] Example 5 An electrode of Example 5 was prepared in the same manner as in Example 3, except that the electroplating time was set to 1 minute.
[0093] The unit platinum loading is 59 μg / cm 2 The paraffin content was 9.4 mg / g, the contact angle was 107°, and the bath voltage was 1.54 V. No platinum was detected in the initial or final electrolyte, and therefore the amount of platinum eluted and the amount of platinum eluted without current application were both 0 mg / L.
[0094] Example 6 An electrode of Example 6 was prepared in the same manner as in Example 3, except that the electroplating time was changed to 30 seconds.
[0095] The unit platinum loading is 21 μg / cm 2 The paraffin content was 21 mg / g, the contact angle was 112°, and the bath voltage was 1.62 V. No platinum was detected in the initial or final electrolyte, and therefore the amount of platinum eluted and the amount of platinum eluted without current application were both 0 mg / L.
[0096] Example 7 An electrode of Example 7 was prepared in the same manner as in Example 3, except that the electroplating time was changed to 15 seconds.
[0097] The unit platinum loading is 3.5 μg / cm 2 The paraffin content was 39 mg / g, the contact angle was 115°, and the bath voltage was 1.68 V. No platinum was detected in the initial or final electrolyte, and therefore the amount of platinum eluted and the amount of platinum eluted without current application were both 0 mg / L.
[0098] Comparative Example 5 A graphite plate was used as the electrode of this example (that is, the same procedure as in Example 3 was carried out except that the platinum plating step and the paraffin impregnation step were not carried out).
[0099] Platinum, copper, palladium, and paraffin were not detected from this electrode (unit platinum loading, unit copper loading, and unit palladium loading were 0 μg / cm 2 , and the paraffin content was 0 mg / g).
[0100] The bath voltage of the electrode of this comparative example was measured, except that paraffin was not added to the electrolytic bath and the electrolyte was not analyzed.
[0101] The contact angle was 84° and the bath voltage was 1.67V.
[0102] Comparative Example 6 The same procedure as in Example 3 was carried out except that the platinum plating step was not carried out, and a graphite plate was impregnated with paraffin to prepare an electrode for Comparative Example 6.
[0103] No platinum, copper, or palladium was detected from this electrode (unit platinum loading, unit copper loading, and unit palladium loading were 0 μg / cm 2 ), the paraffin content was 48 mg / g, the contact angle was 115°, and the bath voltage was 2.09 V.
[0104] Comparative Example 7 Using the same graphite plate as in Example 3, the area from 160 mm to 180 mm from the bottom of the graphite plate was covered with masking tape for plating (manufactured by 3M), and then the area from the bottom to 160 mm was coated with copper (Cu) 2+ The plate was immersed in an electrolyte containing 20 g / L of ions and 40 g / L of sulfuric acid, and a current density of 1.0 A / dm was applied to the two copper plate electrodes set facing the two largest surfaces of the graphite plate as the anode and the graphite plate as the cathode. 2 After that, the electrode was immersed in warm water at 50°C for 30 minutes, washed with running water, and dried at 50°C for 12 hours. After that, the same paraffin impregnation step as in Example 3 was carried out to obtain an electrode of Comparative Example 7.
[0105] The amount of copper supported per unit area on graphite is 1900 μg / cm 2The paraffin content was 36 mg / g, the contact angle was 112°, and the bath voltage was 1.74 V. 22 mg / L and 27 mg / L of copper were detected in the initial and final electrolytes, respectively, so the copper elution amount was 22 mg / L and the non-current elution amount was 27 mg / L.
[0106] Comparative Example 8 Using the same graphite plate as in Example 3, the area from 160 mm to 180 mm from the bottom of the graphite plate was covered with masking tape for plating (manufactured by 3M Company), and then the area from the bottom to 160 mm was immersed in a palladium plating solution (Palabrite SST-L, Japan High Purity Co., Ltd.) maintained at 50°C. Two titanium platinum electrodes set to face the two largest surfaces of the graphite plate were used as anodes, and the graphite plate was used as the cathode, at a current density of 1.0 A / dm 2 The electrode was then subjected to electroplating at 50°C for 15 seconds to deposit palladium on both sides. After the masking tape was removed, the electrode was immersed in hot water at 50°C for 30 minutes, then in a 5% aqueous hydrochloric acid solution at 50°C for 5 minutes, and then again in hot water at 50°C for 30 minutes. After that, the electrode was washed with running water and dried at 50°C for 12 hours. After that, the same paraffin impregnation step as in Example 3 was carried out to obtain an electrode of Comparative Example 8.
[0107] The amount of palladium supported per unit area on graphite is 47 μg / cm 2 The paraffin content was 30 mg / g, the contact angle was 126°, and the bath voltage was 1.62 V. No palladium was detected in the starting electrolyte, and 2.8 mg / L of palladium was detected in the ending electrolyte. Therefore, the amount of palladium eluted was 0 mg / L, and the amount of eluted without current application was 2.8 mg / L.
[0108] The performance of graphite electrodes that do not carry metal deteriorates when they contain paraffin. The results of the above examples and comparative examples are shown in the table below.
[0109] From Comparative Examples 5 and 6 in Table 2, it can be seen that the graphite electrodes containing paraffin and not plated with a metal (platinum, copper or palladium) increase the bath voltage and reduce the performance of the electrode.
[0110] However, the bath voltage was reduced by including paraffin and plating a metal (platinum, copper, or palladium). Furthermore, Examples 3 to 7 showed that using platinum as the plating metal could suppress metal elution.
[0111] As described above, the electrode of this example contains paraffin, thereby reducing adhesion of moisture to the electrode, and by supporting platinum, there is no metal elution into the electrolyte even when no current is applied, even under conditions of high temperature and containing sulfuric acid, and has the effect of reducing the voltage during electrolysis.
[0112] Patent Document 3 shows that paraffin penetrates graphite and that removing the paraffin improves the performance of the graphite electrode. However, it has now been discovered that the inclusion of paraffin in the graphite of the present invention has the effect of reducing the amount of liquid that adheres to the electrode when it is pulled out of the liquid.
[0113] Although the present disclosure has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present disclosure.
[0114] The entire contents of the specification, claims, drawings and abstract of Japanese Patent Application No. 2023-055509, filed on March 30, 2023, are hereby incorporated by reference as the disclosure of the specification of the present disclosure.
Claims
1. An electrode that consists of platinum supported on graphite and contains paraffin.
2. The electrode according to claim 1, wherein the electrode is an electrode for producing electrolytic manganese dioxide.
3. The amount of platinum supported per unit area of the graphite is 3 μg / cm 2 More than 500μg / cm 2 3. The electrode according to claim 1 or 2, wherein:
4. The electrode according to any one of claims 1 to 3, wherein the paraffin content is 1 mg / g or more and 100 mg / g or less based on the weight of the portion of the electrode immersed in the electrolyte during electrolysis.
5. The electrode according to any one of claims 1 to 4, wherein the melting point of the paraffin is 40°C or higher and 80°C or lower.
6. The electrode according to any one of claims 1 to 5, wherein the contact angle of the electrode surface with pure water is greater than 90° and less than 180°.
7. A method for producing electrolytic manganese dioxide, which uses the electrode according to any one of claims 1 to 6.
8. A method for producing an electrode according to any one of claims 1 to 6, comprising: a platinum supporting step of supporting platinum on graphite to obtain platinum-supported graphite; and a paraffin-containing step of contacting the platinum-supported graphite with paraffin to cause the platinum-supported graphite to contain paraffin.
9. The method for producing an electrode according to claim 8, wherein in the platinum supporting step, platinum is supported on graphite by a plating method.
10. The method for producing an electrode according to claim 8, wherein the paraffin-containing step comprises attaching paraffin to the surface of the platinum-supported graphite and then allowing paraffin to penetrate into the platinum-supported graphite.
Citation Information
Patent Citations
Method for manufacturing electrolytic manganese dioxide
JP2001247987A
Laminated film, structure, and preparation method of structure
JP2023055509A
Electrode for hydrogen generation and method of manufacturing the same
JP6837342B2
High discharge capacity electrolytic manganese dioxide and methods of producing the same
WO2000037714A1
Hydrogen generation electrode, method of producing same, and hydrogen production method
WO2020110527A1