Method for manufacturing honeycomb structure

The method of kneading silicon carbide and metal silicon powders with an aqueous dopant solution in honeycomb structure manufacturing ensures uniform dopant distribution, addressing the challenge of inconsistent resistivity and improving the performance of electrically heated catalysts, especially at low voltages.

WO2024203088A1PCT designated stage expired Publication Date: 2024-10-03NGK INSULATORS LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008589
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-06
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional methods for manufacturing honeycomb structures used in electrically heated catalysts face challenges in achieving uniform dopant distribution, leading to inconsistent volume resistivity and increased costs due to high viscosity of molten silicon and potential impurity contamination.

Method used

A method involving kneading a molding raw material containing silicon carbide powder, metal silicon powder, and an aqueous solution of a dopant source to produce clay, which is then molded and fired, ensuring uniform dopant distribution and controlled volume resistivity, using dopants from Group 13 and 15 elements like phosphorus for effective heat management.

Benefits of technology

The method achieves high uniformity of dopant distribution, reducing excessive current generation across a wide range of voltages and enhancing the stability and performance of electrically heated carriers, particularly in low-voltage applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008589_03102024_PF_FP_ABST
    Figure JP2024008589_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a method for manufacturing a honeycomb structure having highly uniform dopant distribution. The method for manufacturing a honeycomb structure comprises: a step in which a molding raw material containing a silicon carbide powder, a metal silicon powder and a dopant-source aqueous solution is kneaded to produce a paste; a step in which the paste is molded to make a honeycomb molded body having external walls and partition walls formed inside the external walls, the partition walls establishing, as a result of partitioning, a plurality of cells that form a flow path from a first end surface to a second end surface; and a step in which the honeycomb molded body is fired to produce a honeycomb fired body. The dopant source contains one or more dopants selected from group 13 elements and group 15 elements in the periodic table. The number of atoms of at least one of the dopants in the aqueous solution of the dopant source, in terms of the number of atoms of the dopant with respect to the volume of the metal silicon, is 1 × 1016 to 5 × 1020 / cm3.
Need to check novelty before this filing date? Find Prior Art

Description

Manufacturing method of honeycomb structure

[0001] The present invention relates to a method for manufacturing a honeycomb structure, and more particularly to a method for manufacturing a honeycomb structure that can be suitably used as an electrically heated carrier.

[0002] Conventionally, catalysts supported on honeycomb structures made of cordierite or silicon carbide have been used to treat harmful substances in exhaust gases emitted from automobile engines. When treating exhaust gases using a catalyst supported on a honeycomb structure, the catalyst must be heated to a predetermined temperature. However, a problem has traditionally arisen in that the catalyst temperature is low at engine start-up, preventing sufficient purification of the exhaust gas. To address this problem, a system called an electrically heated catalyst (EHC) has been developed. This system involves arranging electrodes on a honeycomb structure made of conductive ceramics, and heating the honeycomb structure itself by passing electricity through it, thereby heating the catalyst supported on the honeycomb structure to its activation temperature before or during engine start-up.

[0003] An EHC generally includes an outer peripheral wall, a conductive honeycomb structure portion disposed inside the outer peripheral wall and having partition walls that define a plurality of cells that form flow paths from a first end face to a second end face, and a pair of electrode layers disposed on the outer peripheral wall of the honeycomb structure portion. When an EHC is mounted on, for example, an automobile, the EHC shares a common power source with the electrical system of the automobile. Therefore, excessive current flowing through the EHC may damage the power supply circuit. Because various voltages are used for the power source of the EHC, it is important to adjust the resistance of the honeycomb structure for the EHC for each voltage to prevent excessive current flow.

[0004] Patent Document 1 describes a honeycomb structure in which the partition walls and peripheral walls contain silicon carbide particles as aggregate and silicon as a binder that bonds the silicon carbide particles, and the honeycomb structure has a volume electrical resistance of 1 to 40 Ωcm at 400°C. Patent Document 1 also describes that by setting the average particle size of the silicon carbide particles to 3 to 40 μm, the volume electrical resistance of the honeycomb structure at 400°C can be set to 1 to 40 Ωcm. It also describes that because the honeycomb structure has a volume electrical resistance of 1 to 40 Ωcm at 400°C, even when a current is passed through it using a high-voltage power supply, excessive current does not flow, making it suitable for use as a heater.

[0005] However, a wide range of voltages is used for the power supply of an EHC, depending on, for example, the type of vehicle in which it is installed. In particular, when a low voltage of 60 V or less, for example 48 V, is used for the power supply of an EHC, the volume resistivity appropriate for suppressing the generation of excess current is around 0.1 Ω cm. As such, in recent EHCs that use a wide range of voltages, research and development of technology that effectively suppresses the generation of excess current even when used at low voltages is desired.

[0006] Therefore, Patent Documents 2 and 3 specify the range of the amount of dopant contained in the silicon constituting the EHC. In Patent Documents 2 and 3, the concentration of the dopant in the silicon in the ceramic constituting the partition walls and the outer wall of the honeycomb structure is set to 1×10 16 ~5 x 10 20 pieces / cm 3 It is stated that:

[0007] Patent Document 2 describes a method for manufacturing a honeycomb structure, which includes the steps of: preparing a molding raw material by adding a binder, a surfactant, a pore-forming material, water, etc. to silicon powder to which a dopant has been added, or a powder obtained by mixing the silicon powder to which the dopant has been added with other ceramic materials; kneading the obtained molding raw material to form a clay; extruding the clay to prepare an unfired columnar honeycomb structure; and firing the unfired columnar honeycomb structure.

[0008] Patent Document 3 describes a method for manufacturing a honeycomb structure, which includes the steps of: preparing a molding raw material by adding a binder, a surfactant, water, etc. to a ceramic powder containing silicon carbide powder; kneading the obtained molding raw material to form a clay; extruding the clay to prepare an unfired honeycomb molded body; drying and degreasing the obtained honeycomb molded body to prepare a honeycomb degreased body; and impregnating and firing the honeycomb degreased body with silicon (metallic silicon), wherein the impregnation and firing are performed together with silicon doped with a dopant or a dopant source in the honeycomb degreased body.

[0009] Japanese Patent No. 5735428 Japanese Patent Application Laid-Open No. 2020-204300 Japanese Patent Application Laid-Open No. 2022-142543

[0010] As proposed in Patent Documents 2 and 3, controlling the concentration of dopant in silicon in the ceramics that constitute the partition walls and outer wall of a honeycomb structure is useful for adjusting the volume resistivity of the honeycomb structure. However, conventional methods for manufacturing honeycomb structures leave room for improvement in terms of uniform distribution of dopant in the honeycomb structure. Uniform distribution of dopant in the honeycomb structure is desirable from the viewpoint of quality stability of the honeycomb structure.

[0011] Patent Documents 2 and 3 describe adding a dopant to silicon, but do not describe a specific method. Doping silicon with a dopant can be achieved by melting the silicon and then dissolving the dopant, but this method has the following problems. First, the viscosity of molten silicon is high, making it difficult to uniformly disperse the dopant in the silicon. Second, melting silicon requires heating to approximately 1400°C, which can introduce impurities from the melting furnace and reduce the purity. Furthermore, melting Si requires labor and costs.

[0012] In semiconductor manufacturing, doping is a method for controlling dopants in silicon, and known doping methods include doping partially molten silicon as a gas (FZ method) and ion implantation, but these methods are not suitable for uniformly doping a honeycomb structure.

[0013] The present invention has been made in view of the above circumstances, and an object of one embodiment is to provide a method for manufacturing a honeycomb structure having a highly uniform distribution of dopants.

[0014] The present inventors have conducted extensive research to solve the above problems and have found that a process of preparing a clay by kneading a forming raw material containing silicon carbide powder, metallic silicon powder, and an aqueous solution of a dopant source adjusted to a predetermined concentration is advantageous in obtaining a honeycomb structure having a highly uniform distribution of dopant. The present invention was completed based on this finding and is exemplified below. [Aspect 1] The method includes the steps of: kneading forming raw materials including silicon carbide powder, metallic silicon powder, and an aqueous solution of a dopant source to prepare a puddle; molding the puddle to prepare a honeycomb formed body having an outer peripheral wall and partition walls disposed inside the outer peripheral wall to define a plurality of cells that form flow paths from a first end face to a second end face; and firing the honeycomb formed body to prepare a fired honeycomb body, wherein the dopant source contains one or more dopants selected from Group 13 elements and Group 15 elements of the periodic table, and the number of atoms of at least one of the dopants in the aqueous solution of the dopant source is 1×10, expressed in terms of the number of atoms of the dopant relative to the volume of the metallic silicon. 16 ~5 x 10 20 pieces / cm 3A method for manufacturing a honeycomb structure, wherein the dopant source comprises one or more compounds selected from an inorganic salt containing the dopant and an organic compound containing the dopant. [Aspect 2] The method for manufacturing a honeycomb structure according to Aspect 1, wherein the dopant source comprises one or more compounds selected from an inorganic salt containing the dopant and an organic compound containing the dopant. [Aspect 3] The method for manufacturing a honeycomb structure according to Aspect 1 or 2, wherein the dopant source comprises P. [Aspect 4] The method for manufacturing a honeycomb structure according to any one of Aspects 1 to 3, wherein the dopant source comprises one or more compounds selected from an inorganic salt containing P and an organic compound containing P. [Aspect 5] The method for manufacturing a honeycomb structure according to any one of Aspects 1 to 4, wherein the dopant source comprises an organic phosphate. [Aspect 6] The method for manufacturing a honeycomb structure according to any one of Aspects 1 to 5, wherein the dopant source comprises a compound containing the dopant, and the solubility of the compound in water at 20°C is 1 g / 100 g H2O or more. [Aspect 7] The method for manufacturing a honeycomb structure according to any one of Aspects 1 to 6, wherein the partition walls of the honeycomb structure have a metallic silicon content of 20 mass% or more. [Embodiment 8] The average concentration of at least one of the dopants in the metallic silicon in the partition walls of the honeycomb structure is 1×10 16 ~5 x 10 20 pieces / cm 3 Aspect 9 is a manufacturing method of a honeycomb structure according to any one of Aspects 1 to 8, further comprising, before firing the honeycomb formed body, applying a pair of electrode layer forming pastes to an outer surface of the outer peripheral wall so as to extend in a band-like shape in an extension direction of the cells with a central axis of the honeycomb formed body therebetween, thereby manufacturing a honeycomb formed body with electrode layer forming pastes.

[0015] According to one embodiment of the present invention, a method for manufacturing a honeycomb structure with a highly uniform dopant distribution can be provided. An electrically heated carrier can be manufactured by joining a metal terminal to the honeycomb structure. The electrically heated carrier can be suitably used, for example, as a catalyst carrier for an exhaust gas purification device.

[0016] 1 is a schematic view of an electrically heated carrier according to an embodiment of the present invention when viewed from a first end surface;

[0017] Next, embodiments of the present invention will be described in detail with reference to the drawings. It should be understood that the present invention is not limited to the following embodiments, and that appropriate design changes and improvements may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.

[0018] (1. Electrically Heated Carrier) Fig. 1 is a schematic diagram of an electrically heated carrier 100 according to one embodiment of the present invention when viewed from a first end surface 116. Fig. 2 is a schematic perspective view of the electrically heated carrier 100 according to one embodiment of the present invention.

[0019] The electrically heated carrier 100 includes a honeycomb structure 110 and a metal terminal 130. By supporting a catalyst on the electrically heated carrier 100, the electrically heated carrier 100 can be used as a catalyst body. Examples of the catalyst include precious metal catalysts and other catalysts. Precious metal catalysts include three-way catalysts and oxidation catalysts in which a precious metal such as platinum (Pt), palladium (Pd), or rhodium (Rh) is supported on the surface of alumina pores and a promoter such as ceria or zirconia is included, or alkaline earth metals and platinum are used to reduce nitrogen oxides (NO x ) as a storage component of NO x Examples of catalysts that do not use precious metals include NOx storage reduction catalysts (LNT catalysts) containing copper-substituted or iron-substituted zeolites. x Examples of the catalyst include a selective catalytic reduction catalyst (SCR catalyst). Two or more catalysts selected from these catalysts may be used. There are no particular limitations on the method for supporting the catalyst, and any known method for supporting a catalyst on a honeycomb structure may be used.

[0020] (1-1. Honeycomb structure) In one embodiment, the honeycomb structure 110 comprises: a honeycomb structure portion having an outer peripheral wall 114 and partition walls 113 disposed inside the outer peripheral wall 114 and defining a plurality of cells 115 that form flow paths from a first end face 116 to a second end face 118; a first electrode layer 112a disposed on the outer surface of the outer peripheral wall 114 and extending in a strip-like shape in the extension direction of the cells 115; and a second electrode layer 112b disposed on the outer surface of the outer peripheral wall 114 and extending in a strip-like shape in the extension direction of the cells 115, the second electrode layer 112b being disposed opposite to the first electrode layer 112a across the central axis O of the honeycomb structure portion. If unnecessary, the first electrode layer 112a and the second electrode layer 112b may be omitted.

[0021] The outer shape of the honeycomb structure 110 is not particularly limited, and may be, for example, a columnar body having a round end face such as a circular, oval, elliptical, racetrack, or oval shape, a columnar body having a polygonal end face such as a triangular or rectangular shape, or a columnar body having an end face with other irregular shapes. The illustrated honeycomb structure 110 has a circular end face shape and is cylindrical as a whole.

[0022] There is no particular limitation on the height of the honeycomb structure 110 (the length from one end face to the other end face), and it may be set appropriately depending on the application and required performance. There is also no particular limitation on the relationship between the height of the honeycomb structure 110 and the maximum diameter of each end face (the maximum length of the diameters passing through the center of gravity of each end face of the honeycomb structure). Therefore, the height of the honeycomb structure 110 may be longer than the maximum diameter of each end face, or the height of the honeycomb structure 110 may be shorter than the maximum diameter of each end face.

[0023] The size of the honeycomb structure 110 is set to 2000 to 20000 mm2 in order to improve heat resistance (to suppress cracks in the circumferential direction of the outer peripheral wall). 2 It is preferable that the thickness is 5000 to 15000 mm 2 It is more preferable that:

[0024] <Honeycomb Structure Portion> The outer peripheral wall 114 and partition walls 113 constituting the honeycomb structure portion have higher volume resistivity than the electrode layers 112a and 112b, but are conductive. The volume resistivity of the outer peripheral wall 114 and partition walls 113 is not particularly limited as long as they can generate heat by Joule heating when current is applied, and may be set appropriately depending on the applied voltage. For example, the volume resistivity may be 0.001 to 100 Ω·cm. For high voltages greater than 60 V, the volume resistivity may be 2 to 100 Ω·cm, typically 5 to 100 Ω·cm. For low voltages of 60 V or less, such as 48 V, the volume resistivity may be 0.001 to 2 Ω·cm, typically 0.001 to 1 Ω·cm, and more typically 0.01 to 1 Ω·cm. In this specification, the volume resistivities of the electrode layers, partition walls, and outer peripheral wall are values ​​measured at 25°C using a four-terminal method.

[0025] In one embodiment, the outer peripheral wall 114 and the partition walls 113 contain a silicon carbide-silicon composite. From the viewpoint of achieving both heat resistance and electrical conductivity, the outer peripheral wall 114 and the partition walls 113 preferably contain a silicon carbide-silicon composite as a main component. When the material of the outer peripheral wall 114 and the partition walls 113 is said to contain a silicon carbide-silicon composite as a main component, it means that the outer peripheral wall 114 and the partition walls 113 each contain 80 mass% or more of the silicon carbide-silicon composite (total mass). Here, the silicon carbide-silicon composite contains silicon carbide particles as an aggregate and metallic silicon as a binder that bonds the silicon carbide particles. The outer peripheral wall 114 and the partition walls 113 may contain, as an aggregate, one or two types selected from silicon nitride particles and aluminum nitride particles in addition to silicon carbide particles. They may also contain one or more types of other aggregate. Other aggregates include, for example, oxide ceramics such as alumina, mullite, zirconia, and cordierite.

[0026] However, if the main component of the aggregate is silicon carbide, it is preferable because the thermal conductivity is higher and the difference in thermal expansion coefficient with silicon is smaller. When the main component of the aggregate is silicon carbide, it means that the aggregate contains silicon carbide (total mass) in an amount of 80 mass% or more, more preferably 90 mass% or more of the aggregate.

[0027] The metallic silicon contained in the outer wall 114 and the partition walls 113 of the honeycomb structure 110 is preferably present as a continuous layer. Such a configuration makes it easier to control the volume resistivity to a low level. Here, the metallic silicon being present as a continuous layer refers to a matrix-domain structure in which the silicon carbide or other particles form domains and silicon forms the matrix.

[0028] In order for the metallic silicon in the peripheral wall 114 and partition walls 113 of the honeycomb structure 110 to form a continuous layer, the metallic silicon content in the peripheral wall 114 and partition walls 113 is preferably 20% by mass or more. When the metallic silicon content in the peripheral wall 114 and partition walls 113 is 20% by mass or more, a structure in which the metallic silicon is microstructurally arranged in series is easily achieved. As a result, the volume resistivity of the honeycomb structure 110 can be effectively reduced, and the generation of excess current can be appropriately suppressed even when used at low voltages of 60 V or less, such as 48 V. Furthermore, when the metallic silicon content in the peripheral wall 114 and partition walls 113 is 80% by mass or less, the shape stability of the honeycomb structure 110 can be achieved. Therefore, the metallic silicon content in the peripheral wall 114 and partition walls 113 of the honeycomb structure 110 is preferably 20 to 80% by mass, more preferably 25 to 60% by mass, and even more preferably 25 to 45% by mass.

[0029] The metallic silicon content in the peripheral wall 114 and partition walls 113 of the honeycomb structure 110 can be measured by the following method. The following method describes a calculation method when metallic silicon and silicon carbide are used as ceramic raw materials. When metallic silicon and silicon carbide are used as ceramic raw materials, the peripheral wall 114 and partition walls 113 are composed of metallic silicon (Si), silicon carbide (SiC), and silicon dioxide (SiO). The contents of Si, SiC, and SiO in the peripheral wall 114 and partition walls 113 can be determined by measuring the amounts of silicon and oxygen using an X-ray fluorescence method and measuring the amount of carbon using a resistance heating infrared absorption method. Regarding the amount of SiC, all carbon is assumed to be SiC, and the amount of SiC in the peripheral wall 114 and partition walls 113 is calculated by molecular weight calculation. Regarding the amount of SiO, all oxygen is assumed to be SiO, and the amount of SiO in the peripheral wall 114 and partition walls 113 is calculated by molecular weight calculation. The amount of Si constituting metallic silicon can be calculated by subtracting the total amount of Si, which is the sum of the amount of Si in SiC and the amount of Si in SiO, from the amount of SiC and the amount of SiO calculated above. When a ceramic raw material other than silicon carbide is used, the composition of the honeycomb structure based on the ceramic raw material is confirmed, and then the amount of elements can be measured by a fluorescent X-ray method or a resistance heating infrared absorption method, and the amount of element can be calculated in the same way.

[0030] The metallic silicon in the outer wall 114 and the partition walls 113 of the honeycomb structure 110 can contain a dopant. The dopant in the metallic silicon is one or more kinds selected from Group 13 elements and Group 15 elements of the periodic table. The at least one dopant selected from Group 13 elements and Group 15 elements has a ratio of 1×10 to the volume of the metallic silicon, expressed in terms of the number of atoms of the dopant. 16 ~5 x 10 20 pieces / cm 3Preferably, the dopant is contained in the metallic silicon at an average concentration of 1×10. Here, the Group 13 elements refer to boron (B), aluminum (Al), gallium (Ga), indium (In), etc., and the Group 15 elements refer to nitrogen (N), phosphorus (P), arsenic (As), antimony (Sb), bismuth (Bi), etc. If the dopant in the metallic silicon contained in the honeycomb structure 110 is an element of the same group, it can exhibit conductivity without being affected by counter doping, so it may contain multiple types of elements. Furthermore, it is more preferable that the dopant is one or two types selected from B and Al. Furthermore, it is also preferable that the dopant is one or two types selected from N and P. Each of B, Al, N, and P has an average concentration of 1×10 16 ~5 x 10 20 pieces / cm 3 It is particularly preferable to include P as a dopant because P has an atomic radius close to that of silicon and is easy to handle in practice.

[0031] The average concentration of at least one dopant selected from Group 13 elements and Group 15 elements of the periodic table in the metallic silicon in the outer wall 114 and the partition walls 113 of the honeycomb structure 110 is 1×10 16 ~5 x 10 20 pieces / cm 3In this case, it is advantageous to reduce the volume resistivity of the honeycomb structure 110 so that excessive current does not occur even when used at a low voltage of 60 V or less, such as 48 V. The concentration of the dopant in the metallic silicon in the outer wall 114 and partition walls 113 of the honeycomb structure 110 can be appropriately adjusted depending on the desired volume resistivity of the honeycomb structure 110. Generally, as the concentration of the dopant in the metallic silicon increases, the volume resistivity of the honeycomb structure 110 decreases, and as the concentration of the dopant in the metallic silicon decreases, the volume resistivity of the honeycomb structure 110 increases. The volume resistivity of the honeycomb structure 110 can be effectively reduced by doping metallic silicon (elemental silicon) rather than compounds such as silicon carbide particles that function as aggregates. The average concentration of at least one dopant selected from Group 13 elements and Group 15 elements of the periodic table in the metallic silicon in the outer wall 114 and partition walls 113 of the honeycomb structure 110 is 5×10 17 ~5 x 10 20 pieces / cm 3 From the viewpoint of facilitating control of the volume resistivity, it is more preferable that the average concentration of one kind of dopant selected from Group 13 elements and Group 15 elements of the periodic table in the metallic silicon in the outer wall 114 and the partition walls 113 of the honeycomb structure 110 is 5×10 17 ~5 x 10 20 pieces / cm 3 and for each of the dopants belonging to Group 13 and Group 15 of the periodic table other than the one dopant, it is preferably 1×10 18 pieces / cm 3 It is preferable that:

[0032] The average concentration of each dopant in the metallic silicon in the peripheral wall 114 and partition walls 113 of the honeycomb structure 110 can be measured by the following method. For the peripheral wall, a total of five peripheral wall samples, each weighing 10 g, are taken from the peripheral wall of the honeycomb structure so as to ensure uniformity, and the concentration of the dopant in the metallic silicon for each is measured using the procedure below to obtain an average value. For the partition walls, a total of five partition wall samples, each weighing 10 g, are taken from near the center in the height direction and radial direction of the honeycomb structure, and the concentration of the dopant in the metallic silicon for each is measured using the procedure below to obtain an average value.

[0033] The method for measuring dopants in metallic silicon (Si) in the outer wall or partition wall is as follows. According to the silicon separation ICP atomic emission spectroscopy specified in JIS G 1322-3:2010 "Metallic Silicon Analysis Method," a sample of the outer wall or partition wall is decomposed with nitric acid and hydrofluoric acid, perchloric acid is added, and the mixture is heated to generate white fumes of perchloric acid. The silicon is volatilized and separated as silicon tetrafluoride, and the salts are then dissolved in water. The amount of each dopant contained in the solution is then measured by ICP atomic emission spectroscopy, and the concentration in Si is calculated.

[0034] The metallic silicon contained in the honeycomb structure 110 may contain impurities such as Al and Fe. In this case, it is preferable that the content of the impurities Al and Fe in the metallic silicon contained in the honeycomb structure 110 is 2 mass% or less, respectively, relative to the metallic silicon. When the content of the impurities Al and Fe in the metallic silicon contained in the honeycomb structure 110 is 2 mass% or less, respectively, relative to the metallic silicon, variation in the shape of the honeycomb structure 110 during manufacturing can be effectively suppressed. The content of the impurities Al and Fe in the metallic silicon contained in the honeycomb structure 110 is more preferably 1 mass% or less, and even more preferably 0.1 mass% or less.

[0035] In the embodiment of the present invention, when the metallic silicon contained in the honeycomb structure 110 contains impurities, the impurities are present in a form that adheres to the metallic silicon. In contrast, in the embodiment of the present invention, when the metallic silicon contained in the honeycomb structure 110 contains a dopant, the dopant is thought to be present dissolved in the metallic silicon particles, but the value measured by the dopant concentration measurement method in this specification does not take into account whether or not the dopant is dissolved.

[0036] Providing the honeycomb structure with the peripheral wall 114 is useful from the viewpoint of ensuring the structural strength of the honeycomb structure and suppressing leakage of the fluid flowing through the cells 115 from the peripheral wall 114. In this regard, the thickness of the peripheral wall 114 is preferably 0.1 mm or more, more preferably 0.15 mm or more, and even more preferably 0.2 mm or more. However, if the peripheral wall 114 is made too thick, the strength becomes too high, which disrupts the strength balance with the partition walls 113 and reduces thermal shock resistance. Therefore, the thickness of the peripheral wall 114 is preferably 1.0 mm or less, more preferably 0.7 mm or less, and even more preferably 0.5 mm or less. Here, the thickness of the peripheral wall 114 is defined as the thickness in the direction normal to the tangent to the outer surface of the peripheral wall 114 at the measurement point when the portion of the peripheral wall 114 whose thickness is to be measured is observed in a cross section perpendicular to the extension direction of the cells 115.

[0037] The thickness of the partition walls 113 that define the cells 115 is preferably 0.1 to 0.3 mm, and more preferably 0.1 to 0.2 mm. When the thickness of the partition walls 113 is 0.1 mm or more, it is possible to prevent a decrease in the strength of the honeycomb structure portion. When the thickness of the partition walls 113 is 0.3 mm or less, it is possible to prevent an increase in pressure loss when exhaust gas flows through the honeycomb structure portion when the honeycomb structure portion is used as a catalyst carrier and a catalyst is carried thereon. In the present invention, the thickness of the partition walls 113 is defined as the length of a portion of a line segment that connects the centers of gravity of adjacent cells 115 and that passes through the partition walls 113 in a cross section perpendicular to the extension direction of the cells 115.

[0038] The partition walls 113 may be dense, such as in the form of Si-impregnated SiC, but are preferably porous. The porosity of the partition walls 113 is preferably 35 to 60%, and more preferably 35 to 45%. A porosity of 35% or more can increase the heat generation rate of the EHC. A porosity of 60% or less ensures sufficient strength of the honeycomb structure. The porosity is a value measured using a mercury porosimeter. Note that dense refers to a porosity of 5% or less.

[0039] The honeycomb structure has a cell density of 40 to 150 cells / cm in a cross section perpendicular to the extension direction of the cells 115. 2 Preferably, the density is 70 to 100 cells / cm 2 By setting the cell density in this range, it is possible to increase the purification performance of the catalyst while reducing the pressure loss when exhaust gas flows through the honeycomb structure. 2 If the cell density is 150 cells / cm or more, a sufficient catalyst carrying area is ensured. 2 When the honeycomb structure 110 is used as a catalyst carrier and a catalyst is carried thereon, the pressure loss during the flow of exhaust gas is prevented from becoming too large if the honeycomb structure 110 is used as a catalyst carrier and the cell density is a value obtained by dividing the number of cells by the area of ​​one end face of the honeycomb structure part on the inner peripheral side of the outer peripheral wall 114.

[0040] Although there are no limitations on the shape of the cells in a cross section perpendicular to the extension direction of the cells 115, a square, a hexagon, an octagon, or a combination thereof is preferred. Among these, a square and a hexagon are preferred. By using such a cell shape, the pressure loss when exhaust gas flows through the honeycomb structure 110 is reduced, and the purification performance of the catalyst is improved. From the viewpoint of easily achieving both structural strength and heating uniformity, a hexagon is particularly preferred.

[0041] The cells 115 may penetrate from the first end face 116 to the second end face 118. In this case, the cells 115 may be open at both the first end face 116 and the second end face 118. Alternatively, first cells having plugged first end faces 116 and openings at the second end faces 118 and second cells having openings at the first end faces 116 and plugged second end faces 118 may be alternately arranged adjacent to each other with the partition wall 113 interposed therebetween.

[0042] <Electrode Layer> A first electrode layer 112a and a second electrode layer 112b facing the first electrode layer 112a across the central axis O of the honeycomb structure section can be provided on the outer surface of the outer peripheral wall 114. By providing the electrode layers 112a, 112b having a lower volume resistivity than the outer peripheral wall 114, current is more likely to spread in the circumferential direction of the honeycomb structure 110 and in the extension direction of the cells 115, thereby improving the uniform heat generation of the honeycomb structure 110. Referring to FIG. 1 , in a cross section perpendicular to the extension direction of the cells 115, the angle θ (0°≦θ≦180°) formed by two line segments extending from the circumferential centers of the pair of electrode layers 112a, 112b to the central axis O (center of gravity) of the honeycomb structure 110 is preferably 150°≦θ≦180°, more preferably 160°≦θ≦180°, even more preferably 170°≦θ≦180°, and most preferably 180°.

[0043] Although there are no particular restrictions on the formation regions of the pair of electrode layers 112a, 112b, from the viewpoint of improving the uniform heat generation of the honeycomb structure 110, it is preferable that the pair of electrode layers 112a, 112b are each provided in a band-like shape extending on the outer surface of the outer peripheral wall 114 in the circumferential direction of the honeycomb structure 110 and in the extension direction of the cells 115. Specifically, in a cross section perpendicular to the extension direction of the cells 115, the central angle α formed by two line segments connecting both circumferential ends of each electrode layer 112a, 112b to the central axis O (center of gravity) is preferably 30° or more, more preferably 40° or more, and even more preferably 60° or more, from the viewpoint of spreading the current in the circumferential direction and improving the uniform heat generation (see FIG. 1 ). However, if the central angle α is too large, less current passes through the interior of the honeycomb structure 110, and more current passes near the outer peripheral wall 114. Therefore, from the viewpoint of uniform heat generation of the honeycomb structure 110, the central angle α is preferably 140° or less, more preferably 130° or less, and even more preferably 120° or less. Furthermore, it is desirable that each of the electrode layers 112a, 112b extends over 80% or more of the length between both end faces of the honeycomb structure 110, preferably over 90% or more, and more preferably over the entire length. The electrode layers 112a, 112b may be composed of a single layer, or may have a laminated structure in which multiple layers are stacked.

[0044] The thickness of the electrode layers 112a, 112b is preferably 0.01 to 5 mm, and more preferably 0.01 to 3 mm. Setting the thickness within this range can improve uniform heat generation. When the thickness of the electrode layers 112a, 112b is 0.01 mm or more, the electrical resistance is appropriately controlled, allowing for more uniform heat generation. When the thickness of the electrode layers 112a, 112b is 5 mm or less, the risk of breakage during canning is reduced. The thickness of the electrode layers 112a, 112b is defined as the thickness in the direction normal to the tangent to the outer surface of the electrode layers 112a, 112b at the measurement location when the location of the electrode layers 112a, 112b where the thickness is to be measured is observed in a cross section perpendicular to the extension direction of the cell 115.

[0045] By making the volume resistivity of the electrode layers 112a, 112b lower than the volume resistivity of the partition walls 113 and the outer peripheral wall 114, electricity flows preferentially through the electrode layers 112a, 112b, and when energized, electricity spreads more easily in the circumferential direction of the honeycomb structure 110 and in the extension direction of the cells 115. The volume resistivity of the electrode layers 112a, 112b is preferably 1 / 10 or less of the volume resistivity of the partition walls 113 and the outer peripheral wall 114, more preferably 1 / 20 or less, and even more preferably 1 / 30 or less. However, if the difference in volume resistivity between the two becomes too large, current will concentrate between the ends of the opposing electrode layers 112 a, 112 b, causing uneven heat generation in the honeycomb structure 110, and therefore the volume resistivity of the electrode layers 112 a, 112 b is preferably 1 / 200 or more, more preferably 1 / 150 or more, and even more preferably 1 / 100 or more of the volume resistivity of the partition walls 113 and the outer peripheral wall 114. As described above, in this specification, the volume resistivities of the electrode layers, partition walls, and outer peripheral wall are values ​​measured at 25° C. by the four-terminal method.

[0046] The material of the electrode layers 112a and 112b is not limited to, but may be a composite (cermet) of metal and ceramic (especially conductive ceramic). Examples of metals include, for example, Cr, Fe, Co, Ni, Si, or Ti, or alloys containing at least one metal selected from these metals. Examples of ceramics include, but are not limited to, silicon carbide (SiC), as well as metal compounds such as metal silicides, such as tantalum silicide (TaSi) and chromium silicide (CrSi). Specific examples of composites (cermets) of metal and ceramic include composites of silicon carbide and metal silicon, composites of metal silicides, such as tantalum silicide or chromium silicide, and composites of silicon carbide and metal silicides, as well as composites in which one or more of the above metals are added with one or more insulating ceramics, such as alumina, mullite, zirconia, cordierite, silicon nitride, and aluminum nitride, in order to reduce thermal expansion. As the material for the electrode layers 112a, 112b, among the various metals and ceramics described above, a composite material of a metal silicide such as tantalum silicide or chromium silicide, metal silicon, and silicon carbide is preferred because it can be fired simultaneously with the partition wall and the outer peripheral wall, thereby contributing to simplification of the manufacturing process.

[0047] (1-2. Metal Terminal) The metal terminal 130 can be directly or indirectly bonded to the outer surfaces of each of the pair of electrode layers 112a, 112b. When a voltage is applied to the honeycomb structure 110 via the metal terminal 130, electricity flows and the honeycomb structure 110 can generate heat by Joule heat. Therefore, the honeycomb structure 110 can also be suitably used as a heater. This makes it possible to improve the uniform heat generation of the honeycomb structure 110. The applied voltage is preferably 12 to 900 V, more preferably 48 to 600 V, but the applied voltage can be changed as appropriate.

[0048] The metal terminal 130 and the electrode layers 112a, 112b may be directly bonded to each other, or may be bonded to each other via one or more base layers 120 in order to reduce the difference in thermal expansion between the electrode layers 112a, 112b and the metal terminal 130 and thereby improve the bonding reliability of the metal terminal 130. Therefore, in a preferred embodiment, the honeycomb structure 110 has a first electrode layer 112a and a second electrode layer 112b disposed on the outer peripheral wall 114 so as to face each other across the central axis O (center of gravity) of the honeycomb structure 110, and one or more metal terminals 130 are bonded to each of the electrode layers 112a, 112b via the base layer 120.

[0049] From the viewpoint of improving bonding reliability, it is preferable that the thermal expansion coefficient gradually decreases in the order of the metal terminal 130 → (underlying layer 120) → electrode layers 112a and 112b → outer peripheral wall 114. Note that the "thermal expansion coefficient" here refers to the linear expansion coefficient measured in accordance with JIS R1618:2002 when the temperature is changed from 25°C to 800°C.

[0050] The material of the metal terminal 130 is not particularly limited as long as it is a metal, and simple metals and alloys can be used, but from the viewpoints of corrosion resistance, volume resistivity, and linear expansion coefficient, an alloy containing at least one selected from the group consisting of Cr, Fe, Co, Ni, and Ti is preferable, and stainless steel and an Fe-Ni alloy are more preferable. The number, shape, and size of the metal terminals 130 are not particularly limited, and can be designed appropriately depending on the size, electrical conductivity, etc. of the honeycomb structure 110.

[0051] The material of the base layer 120 is not limited, but may be a composite material (cermet) of metal and ceramic (particularly conductive ceramic). The thermal expansion coefficient of the base layer 120 can be controlled by adjusting the compounding ratio of the metal and ceramic, for example.

[0052] The underlayer 120 preferably contains, but is not limited to, one or more metals selected from Ni-based alloys, Fe-based alloys, Ti-based alloys, Co-based alloys, metallic silicon, and Cr.

[0053] The underlayer 120 preferably contains one or more ceramics selected from, but not limited to, oxide ceramics such as alumina, mullite, zirconia, glass, and cordierite, and non-oxide ceramics such as silicon carbide, silicon nitride, and aluminum nitride.

[0054] The thickness of the base layer 120 is not particularly limited, but is preferably 0.1 to 1.5 mm, and more preferably 0.3 to 0.5 mm, from the viewpoint of crack suppression. The thickness of the base layer 120 is defined as the thickness in the direction normal to the tangent to the outer surface of the base layer 120 at the measurement point when the base layer 120 whose thickness is to be measured is observed in a cross section perpendicular to the extension direction of the cells.

[0055] The method for joining the metal terminal 130 to the electrode layers 112a, 112b or the base layer 120 is not particularly limited, but examples thereof include thermal spraying, welding, and brazing.

[0056] (2. Manufacturing Method) Next, a method for manufacturing a honeycomb structure according to one embodiment of the present invention will be described. The honeycomb structure can be manufactured by a manufacturing method including step 1 of preparing a clay, step 2 of molding the clay to obtain a honeycomb molded body, step 3 of applying a pair of electrode layer forming pastes to the outer surface of the peripheral wall so that the pastes extend in strips in the cell extension direction across the central axis of the honeycomb molded body, thereby manufacturing a honeycomb molded body with the electrode layer forming pastes, and step 4 of firing the honeycomb molded body to manufacture a honeycomb fired body. If an electrode layer is not required, step 3 may be omitted.

[0057] (Step 1) In step 1, a forming raw material containing silicon carbide powder, metal silicon powder, and an aqueous solution of a dopant source is kneaded to prepare a clay. The dopant source may be any substance containing an element that serves as a dopant, and may include simple substances and compounds. However, simple substances have low solubility in water, so it is preferable to provide it as a compound. Suitable types of dopants are as described above. By providing the dopant source in the form of an aqueous solution, when the dopant source is kneaded with the silicon carbide powder and metal silicon powder, the dopant source is dispersed with high uniformity in the silicon carbide powder and metal silicon powder. The dopant in the dopant source mainly dissolves in the metal silicon, but some of the dopant may also dissolve in the silicon carbide.

[0058] In step 1, the forming raw materials are kneaded to prepare a clay. Any appropriate device or mechanism can be used as the kneading means. Specific examples include a kneader and a vacuum clay kneader.

[0059] By adjusting the number of dopant atoms in the aqueous solution, the concentration of the dopant in the metallic silicon in the peripheral wall and partition walls of the honeycomb structure can be controlled. From the viewpoint of widening the range of adjustment of the number of dopant atoms, the dopant source is preferably provided as a water-soluble compound containing a dopant. In this case, the solubility of the water-soluble compound containing a dopant in water at 20°C is preferably 1 g / 100 g HO or more, more preferably 5 g / 100 g HO or more, and even more preferably 10 g / 100 g HO or more. While no upper limit is specifically set for this solubility, from the viewpoint of ease of availability, it is generally 50 g / 100 g HO or less, typically 30 g / 100 g HO or less. Therefore, the solubility of the water-soluble compound containing a dopant in water at 20°C is preferably, for example, 1 to 50 g / 100 g HO, and more preferably 5 to 30 g / 100 g HO. In this specification, the solubility of a water-soluble compound containing a dopant in water at 20°C is measured by repeatedly adding various concentrations of the water-soluble compound to 100 mL of water (20°C) stored in a measuring flask, stirring (at 500 rpm for 20 minutes), and checking for the presence or absence of undissolved solids, thereby determining and measuring the concentration of the water-soluble compound in a saturated solution.

[0060] The amount of the aqueous solution of the dopant source may be appropriately set depending on the dopant concentration in the target forming raw material or honeycomb structure. For example, the number of atoms of at least one dopant in the aqueous solution of the dopant source may be 1×10, expressed as the number of atoms of the dopant relative to the volume of metallic silicon. 16 ~5 x 10 20 pieces / cm 3 It is preferable to set it so that 17 ~5 x 10 20 pieces / cm 3 The volume of the metallic silicon is determined by calculating the density of the metallic silicon (2.3290 g / cm 3 ) from the mass of the metallic silicon powder. 3 For example, when P is the dopant, if the dopant concentration in the forming raw material or the honeycomb structure is 1×10, expressed as the number of dopant atoms relative to the volume of metallic silicon, 16 pieces / cm 3 When the target is 1×10, the number of dopant atoms in the aqueous solution of the dopant source can be set according to the following calculation formula. Note that it is possible to incorporate substantially all of the dopant in the aqueous solution into metallic silicon. (a) Calculation of the number of dopants (number of P atoms) to be added: 1×10 16 pieces / cm 3 × volume of metallic silicon V (cm 3 ) = V × 10 16 (pieces) (b) Calculate the mass of the dopant to be added (P mass) V x 10 16 pieces ÷ 6.02×10 23 / mol (Avogadro's constant) × 30.97 g / mol (P atomic weight) = 5.14 × 10 -7 ×V (g)

[0061] As the water-soluble compound containing a dopant, one or more selected from inorganic salts and organic compounds can be suitably used. When the dopant is P, examples of the water-soluble inorganic salt containing P include tetraphosphorus decaoxide, phosphoric acid, and ammonium phosphate. Examples of the water-soluble organic compound containing P include phosphine oxide, phosphine alkene, phosphine alkyne, phosphonic acid ester, and phosphate ester, as well as organic phosphates such as phosphonic acid ester salts and phosphate ester salts. When the dopant is N, examples of the water-soluble inorganic salt containing N include dinitrogen pentoxide, aqueous ammonia, and nitric acid. When the dopant is B, examples of the water-soluble inorganic salt containing B include boric acid. Examples of the water-soluble organic compound containing B include methylboronic acid and boronic acid ester. When the dopant is Al, examples of the water-soluble inorganic salt containing Al include aluminum chloride, aluminum sulfate, and aluminum nitrate.

[0062] The mass of the metal silicon powder in the forming raw material is preferably 20 to 80 parts by mass, more preferably 25 to 60 parts by mass, and even more preferably 25 to 45 parts by mass, when the total mass of the silicon carbide powder and metal silicon powder is 100 parts by mass. The average particle size of the silicon carbide particles in the silicon carbide powder is preferably 3 to 50 μm, more preferably 3 to 40 μm. The average particle size of the metal silicon particles in the metal silicon powder is preferably 2 to 35 μm, more preferably 2 to 25 μm. The average particle sizes of the silicon carbide particles and metal silicon particles refer to the arithmetic mean diameter on a volume basis when the particle size frequency distribution is measured by laser diffraction. The silicon carbide particles are fine particles of silicon carbide that constitute the silicon carbide powder, and the metal silicon particles are fine particles of metal silicon that constitute the metal silicon powder.

[0063] The forming raw material may contain water from sources other than the dopant source aqueous solution, but the total water content in the forming raw material (including the water in the dopant source aqueous solution and other water, if present) is preferably 20 parts by mass or more, more preferably 25 parts by mass or more, when the total mass of the silicon carbide powder and the metal silicon powder is 100 parts by mass, in order to uniformly disperse the dopant source. Furthermore, the total water content in the forming raw material (including the water in the dopant source aqueous solution and other water, if present) is preferably 60 parts by mass or less, more preferably 50 parts by mass or less, when the total mass of the silicon carbide powder and the metal silicon powder is 100 parts by mass, in order to maintain the shape of the honeycomb structure. Therefore, the total water content in the forming raw material (including the water in the dopant source aqueous solution and other water, if present) is preferably 20 to 60 parts by mass, more preferably 25 to 50 parts by mass, when the total mass of the silicon carbide powder and the metal silicon powder is 100 parts by mass.

[0064] The forming raw material may contain a binder, a surfactant, and a pore former in addition to the silicon carbide powder, the metallic silicon powder, and the aqueous solution of the dopant source.

[0065] Examples of binders include methyl cellulose, hydroxypropyl methyl cellulose, hydroxypropoxyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, and polyvinyl alcohol. Among these, it is preferable to use methyl cellulose and hydroxypropoxyl cellulose in combination. The content of the binder is preferably 2.0 to 10.0 parts by mass when the total mass of the silicon carbide powder and the metallic silicon powder is 100 parts by mass.

[0066] Examples of surfactants that can be used include ethylene glycol, dextrin, fatty acid soap, and polyalcohol. These may be used alone or in combination of two or more. The content of the surfactant is preferably 0.1 to 2.0 parts by mass when the total mass of the silicon carbide powder and the metallic silicon powder is 100 parts by mass.

[0067] The pore-forming material is not particularly limited as long as it forms pores after firing, and examples thereof include graphite, starch, foamed resin, water-absorbent resin, silica gel, etc. The content of the pore-forming material is preferably 0.5 to 10.0 parts by mass when the total mass of the silicon carbide powder and metallic silicon powder is 100 parts by mass. The average particle diameter of the pore-forming material is preferably 10 to 30 μm. The average particle diameter of the pore-forming material refers to the arithmetic mean diameter on a volume basis when the frequency distribution of particle size is measured by laser diffraction. When the pore-forming material is a water-absorbent resin, the average particle diameter of the pore-forming material refers to the average particle diameter after water absorption.

[0068] (Step 2) In step 2, the clay produced in step 1 is molded to obtain a honeycomb molded body. Specifically, the clay is extrusion molded to produce a columnar honeycomb molded body having an outer peripheral wall and partition walls. A die having the desired overall shape, cell shape, partition wall thickness, cell density, etc. can be used during extrusion molding. Next, it is preferable to dry the obtained honeycomb molded body. If the length of the honeycomb molded body in the central axis direction is not the desired length, both ends of the honeycomb molded body can be cut to obtain the desired length. The honeycomb molded body after drying is called a dried honeycomb body.

[0069] The honeycomb formed body may be fired once as a modification of step 1. That is, in this modification, the honeycomb formed body is fired to prepare a honeycomb fired body, and step 3 is then carried out on the honeycomb fired body.

[0070] (Step 3) Step 3 is a step of applying a pair of electrode layer forming pastes to the outer surface of the peripheral wall of the honeycomb formed body so that the pastes extend in bands in the cell extension direction across the central axis of the honeycomb formed body, thereby producing a honeycomb formed body with electrode layer forming pastes. The electrode layer forming paste can be formed by appropriately adding various additives to raw material powders (metal powders, ceramic powders, etc.) blended according to the required characteristics of the electrode layer, and kneading the mixture. The average particle diameter of the raw material powders is not limited, but is preferably, for example, 5 to 50 μm, and more preferably 10 to 30 μm. The average particle diameter of the raw material powder refers to the arithmetic mean diameter on a volume basis when the particle size frequency distribution is measured by laser diffraction.

[0071] Next, the obtained electrode layer forming paste is applied to required locations on the outer surface of the peripheral wall of a honeycomb formed body (typically a dried honeycomb body) to obtain a honeycomb formed body with the electrode layer forming paste. The method of preparing the electrode layer forming paste and the method of applying the electrode layer forming paste to the honeycomb formed body can be performed in accordance with known methods for manufacturing honeycomb structures. However, in order to give the electrode layer a lower volume resistivity than the peripheral wall and partition walls, the metal content can be made higher than that of the peripheral wall and partition walls, or the particle size of the metal particles in the raw material powder can be made smaller. After application, it is preferable to dry the electrode layer forming paste.

[0072] (Step 4) Step 4 is a step in which the honeycomb formed body with the electrode layers is fired to obtain a fired honeycomb body, i.e., the desired honeycomb structure. Before firing, degreasing may be performed to remove binders and the like. The degreasing and firing methods are not particularly limited, and firing can be performed using an electric furnace, a gas furnace, or the like. Firing conditions vary depending on the material of the honeycomb structure, but preferably involve heating at 1400 to 1500°C for 1 to 20 hours in an inert atmosphere such as nitrogen or argon.

[0073] An electrically heated carrier can be manufactured by joining a metal terminal to the electrode layer of the honeycomb structure obtained in this manner. The joining method is not particularly limited, but examples thereof include thermal spraying, welding, and brazing. In order to improve the bonding between the electrode layer and the metal terminal, a base layer may be formed by a method such as thermal spraying.

[0074] An appropriate catalyst may be supported on the electrically heated carrier depending on the application. As a method for supporting a catalyst on a honeycomb structure, for example, a catalyst slurry is introduced into cells by a conventionally known suction method or the like, and is allowed to adhere to the surfaces and pores of the partition walls, and then high-temperature treatment is performed to bake the catalyst contained in the catalyst slurry onto the partition walls and support the catalyst.

[0075] The following examples are provided to provide a better understanding of the present invention and its advantages, but the present invention is not limited to these examples.

[0076] <Test No. 1> (1. Preparation of Cylindrical Puddles) 30 g of phosphate ester salt was added to 30 kg of pure water and stirred for 20 minutes to obtain an aqueous solution of the dopant source. The solubility of the phosphate ester salt in water at 20°C was measured using the method described above and found to be 8.4 g / 100 g HO. A ceramic raw material was also prepared by mixing silicon carbide (SiC) powder and metallic silicon (Si) powder in a mass ratio of 75:25. Hydroxypropyl methylcellulose as a binder, a water-absorbent resin as a pore-forming material, and the aqueous solution of the dopant source were added to this ceramic raw material to prepare a molding raw material. The molding raw material was then kneaded using a vacuum kneader to prepare a cylindrical moldable clay.

[0077] In the forming raw material, the content of the binder was 8 parts by mass when the total of the silicon carbide (SiC) powder and the metal silicon (Si) powder was 100 parts by mass. The content of the pore former was 3 parts by mass when the total of the silicon carbide (SiC) powder and the metal silicon (Si) powder was 100 parts by mass. The content of the aqueous solution of the dopant source was 30 parts by mass when the total of the silicon carbide (SiC) powder and the metal silicon (Si) powder was 100 parts by mass. As a result, the atomic concentration of P, which is the dopant, in the forming raw material was 100 parts by mass of the metal silicon (1 cm 3 ) for 2.9 × 10 18 pieces / cm 3 The average particle size of the silicon carbide powder was 20 μm, and the average particle size of the metallic silicon powder was 6 μm. The average particle size of the pore-forming material was 20 μm. The average particle sizes of the silicon carbide powder, metallic silicon powder, and pore-forming material refer to arithmetic mean diameters on a volume basis when the particle size frequency distribution is measured by laser diffraction.

[0078] (2. Production of dried honeycomb body) The obtained cylindrical clay was molded using an extrusion molding machine with a predetermined die structure to obtain a cylindrical honeycomb molded body in which each cell shape in a cross section perpendicular to the cell extension direction is hexagonal. This honeycomb molded body was dried by high-frequency dielectric heating, and then dried in an air atmosphere at 120°C for 2 hours using a hot air dryer, and both end faces were cut by a predetermined amount to produce a dried honeycomb body.

[0079] (3. Firing) The obtained dried honeycomb body was degreased in an air atmosphere at 550°C for 3 hours. Next, the degreased dried honeycomb body was fired in an Ar atmosphere at 1450°C for 0.5 hours. Finally, the honeycomb structure was heat-treated in a water vapor atmosphere at 950°C for 50 hours to obtain a cylindrical honeycomb structure. The number of honeycomb structures required for the following tests was manufactured.

[0080] (4. Specifications of Honeycomb Structure) The honeycomb structure obtained above had a circular end face with a diameter of 80 mm, a height (length in the cell extension direction) of 80 mm, a partition wall thickness of 0.125 mm, a peripheral wall thickness of 0.5 mm, and a cell density of 90 cells / cm 2 The porosity of the partition walls was 38%.

[0081] (5. Metallic Silicon Content) When the metallic silicon contents in the partition walls and the outer peripheral wall of the honeycomb structure obtained above were measured according to the method described above, they were both 30% by weight.

[0082] (6. Concentration of dopant in metallic silicon) A total of five partition wall samples, each weighing 10 g, were taken from near the center in the height direction and the radial direction of the honeycomb structure obtained above. The concentration of dopant (P) in the metallic silicon for each was measured according to the method described above, and the average value was calculated. In addition, a total of five peripheral wall samples, each weighing 10 g, were taken from the peripheral wall of the honeycomb structure obtained above without bias. The concentration of dopant (P) in the metallic silicon for each was measured according to the method described above, and the average value was calculated. The ICP (inductively coupled plasma) analyzer used was a model PS3510DD manufactured by Hitachi High-Technologies Corporation. As a result, both were 2.8 x 10 18 pieces / cm 3 It was.

[0083] (7. Measurement of Concentration Distribution of Dopant in Metallic Silicon) The standard deviation was calculated based on the concentration of dopant (P) in metallic silicon of five partition wall samples whose average concentration of dopant (P) was calculated. The standard deviation was 7.0 × 10 16 pieces / cm 3 (σ=2.5% of the average value).

[0084] (8. Volume Resistivity Measurement) A total of five partition wall samples, each measuring 5 mm × 5 mm × 50 mm (the length in the cell extension direction), were collected from the honeycomb structure obtained above, and the volume resistivity of each was measured at 25°C by the four-terminal method. The partition wall samples were collected from near the center of the honeycomb structure. As a result, the average value was 61 Ω cm, and the standard deviation was 1.9 Ω cm (σ=3.1% of the average value).

[0085] <Test No. 2 (Comparative Example)> (1. Preparation of Cylindrical Particles) A ​​ceramic raw material was prepared by mixing silicon carbide (SiC) powder and P-doped metallic silicon (Si) powder in a mass ratio of 65:35. The P-doped metallic silicon (Si) powder was prepared by melting Si in a melting furnace, and then adding phosphate rock (3Ca3(PO4)2.CaF2) to the melting furnace to dope with P. By this method, the concentration of P as a dopant was adjusted to 1 / 3 of the concentration of the metallic silicon (1 cm 3 ) to 3.0 × 10 18 pieces / cm 3 Hydroxypropyl methylcellulose as a binder, a water-absorbent resin as a pore former, and pure water were added to this ceramic raw material to prepare a molding raw material. The molding raw material was then kneaded in a vacuum kneader to produce cylindrical clay.

[0086] In the molding raw material, the content of the binder was 7 parts by mass when the total of the silicon carbide (SiC) powder and the metallic silicon (Si) powder was 100 parts by mass. The content of the pore-forming material was 3 parts by mass when the total of the silicon carbide (SiC) powder and the metallic silicon (Si) powder was 100 parts by mass. The content of pure water was 30 parts by mass when the total of the silicon carbide (SiC) powder and the metallic silicon (Si) powder was 100 parts by mass. The average particle diameter of the silicon carbide powder was 20 μm, and the average particle diameter of the metallic silicon powder was 6 μm. The average particle diameter of the pore-forming material was 20 μm. The average particle diameters of the silicon carbide powder, the metallic silicon powder, and the pore-forming material refer to the arithmetic mean diameter on a volume basis when the particle size frequency distribution is measured by a laser diffraction method.

[0087] (2. Preparation of Honeycomb Structure) Using the obtained cylindrical clay, honeycomb structures in the number required for the following test were obtained in the same manner as in Test No. 1.

[0088] (3. Specifications of honeycomb structure) The honeycomb structure obtained above had a circular end face with a diameter of 80 mm, a height (length in the cell extension direction) of 80 mm, a partition wall thickness of 125 mm, a peripheral wall thickness of 0.5 mm, and a cell density of 90 cells / cm 2 The porosity of the partition walls was 38%.

[0089] (4. Metallic Silicon Content) When the metallic silicon contents in the partition walls and the outer peripheral wall of the honeycomb structure obtained above were measured according to the method described above, they were both 30% by weight.

[0090] (5. Concentration of Dopant in Metallic Silicon) With respect to the honeycomb structure obtained above, the average concentration of dopant (P) in the metallic silicon in the partition walls and the outer peripheral wall was measured according to the method described above. 18 pieces / cm 3 It was.

[0091] (6. Measurement of Concentration Distribution of Dopant in Metallic Silicon) As in Test No. 1, the standard deviation was calculated based on the concentration of dopant (P) in metallic silicon of five partition wall samples whose average concentration of dopant (P) was calculated. The standard deviation was 3.5×10 17 pieces / cm 3 (σ=14% of the average value).

[0092] (7. Volume Resistivity Measurement) As in Test No. 1, a total of five partition wall samples were collected from near the center of the honeycomb structure, and the volume resistivity was measured at 25° C. by the four-terminal method. As a result, the average value was 74 Ω cm, and the standard deviation was 11 Ω cm (σ=15% of the average value).

[0093] 100: Electrically heated carrier 110: Honeycomb structure 112a: First electrode layer 112b: Second electrode layer 113: Partition wall 114: Peripheral wall 115: Cell 116: First end face 118: Second end face 120: Base layer 130: Metal terminal

Claims

1. A method for manufacturing a honeycomb fired body comprising the steps of: kneading forming raw materials including silicon carbide powder, metal silicon powder, and an aqueous solution of a dopant source to prepare a puddle; molding the puddle to prepare a honeycomb formed body having an outer peripheral wall and partition walls disposed inside the outer peripheral wall to define a plurality of cells that form flow paths from a first end face to a second end face; and firing the honeycomb formed body to prepare a honeycomb fired body, wherein the dopant source contains one or more dopants selected from Group 13 elements and Group 15 elements of the periodic table, and the number of atoms of at least one of the dopants in the aqueous solution of the dopant source is 1×10, expressed in terms of the number of atoms of the dopant relative to the volume of the metal silicon. 16 ~5×10 20 pieces / cm 3 The method for manufacturing a honeycomb structure is as follows.

2. The method according to claim 1, wherein the dopant source contains one or more selected from an inorganic salt containing the dopant and an organic compound containing the dopant.

3. The method for manufacturing a honeycomb structure according to claim 1 or 2, wherein the dopant source contains P.

4. The method according to claim 1 or 2, wherein the dopant source comprises one or more selected from the group consisting of inorganic salts containing P and organic compounds containing P.

5. The method of claim 1 or 2, wherein the dopant source comprises an organic phosphate.

6. The method according to claim 1 or 2, wherein the dopant source comprises a compound containing the dopant, and the solubility of the compound in water at 20° C. is 1 g / 100 g H2O or more.

7. The manufacturing method according to claim 1 or 2, wherein the content of metallic silicon in the partition walls of the honeycomb structure is 20 mass % or more.

8. The average concentration of at least one of the dopants in the metallic silicon in the partition walls of the honeycomb structure is 1×10 16 ~5×10 20 pieces / cm 3 The method according to claim 1 or 2, wherein 9. A method for manufacturing a honeycomb structure as described in claim 1 or 2, further comprising a step of applying a pair of electrode layer forming pastes to the outer surface of the outer wall so as to extend in a band-like manner in the extension direction of the cells, sandwiching the central axis of the honeycomb formed body, before firing the honeycomb formed body, thereby producing a honeycomb formed body with electrode layer forming paste.

Citation Information

Patent Citations

  • Method for producing conductive ceramic sintered compact

    JP2012214306A

  • Honeycomb structure, electric heating-type honeycomb structure, electric heating-type carrier and exhaust emission control device

    JP2020204300A

  • Honey-comb structure and electric heating carrier

    JP2022142543A

  • Honeycomb structure, and electric heating support and exhaust gas treatment device each using the honeycomb structure

    JP2022148668A

  • Honeycomb structure

    WO2011037247A1