Light-diffusing device, backlight device, and image display device

The light diffusion device addresses the issue of non-uniform in-plane luminance by incorporating a low refractive index layer between the light source and diffusion film, enhancing interfacial reflection and diffusing light for improved uniformity in image display devices.

WO2024203122A1PCT designated stage expired Publication Date: 2024-10-03NITTO DENKO CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008810
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-07
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing light diffusion devices, particularly those used in direct type backlight devices for image display, suffer from insufficient uniformity of in-plane luminance due to interfacial reflection issues between optical films.

Method used

A light diffusion device is designed with a light source layer, a sealing resin layer, and a low refractive index layer positioned between the light source layer and the diffusion film, which includes a polymer matrix and dispersed liquid crystal particles, to enhance in-plane brightness uniformity by increasing interfacial reflection and diffusing light effectively.

Benefits of technology

The solution achieves improved in-plane brightness uniformity by reducing directivity of light entering the diffusion film, resulting in a more uniform surface light emission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008810_03102024_PF_FP_ABST
    Figure JP2024008810_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a light-diffusing device having a diffusion film and capable of achieving more uniform surface light emission. This light-diffusing device includes, in the following order: a light-source layer that includes a light-source part and a sealing resin layer that seals the light-source part; a first low refractive index layer that has a lower refractive index than the sealing resin layer; and a first diffusion film that includes a diffusion layer. The diffusion layer includes: a polymer matrix; and dispersed particles that are dispersed in the polymer matrix and include at least one type selected from a liquid crystal compound and a liquid crystal polymer.
Need to check novelty before this filing date? Find Prior Art

Description

Light diffusion device, backlight device, and image display device

[0001] The present invention relates to a light diffusion device including a diffusion film, and a backlight device and an image display device using the light diffusion device.

[0002] A PDLC film having a polymer dispersed liquid crystal (hereinafter sometimes referred to as "PDLC") layer between a pair of transparent electrode layers is a type of light control film that can be switched between a light scattering state (scattering state) and a light transmitting state (non-scattering state or transparent state) by switching between a voltage applied state and a voltage not applied state. Specifically, the PDLC layer includes a polymer matrix and droplets of a liquid crystal compound (hereinafter sometimes referred to as "liquid crystal droplets") dispersed in the polymer matrix, and the liquid crystal droplets act as scattering particles, causing light scattering due to the difference in refractive index between the liquid crystal compound in the liquid crystal droplets and the polymer matrix, etc.

[0003] In recent years, display devices and lighting devices that use light-emitting diodes (hereinafter referred to as LEDs) as light sources have become widespread due to their low power consumption and the ability to be made smaller and thinner, and one or more diffusion films are placed over the light source in order to obtain uniform surface light emission.

[0004] The above-mentioned diffusion film includes a surface-type diffusion film in which a diffusion pattern is formed on the surface by textured processing, dot printing, etc. When a surface-type diffusion film is laminated to an adjacent member without an adhesive layer, scratches may be caused on the adjacent member due to rubbing, or the diffusion pattern may change over time, etc. Furthermore, when the surface-type diffusion film is laminated to an adjacent member via an adhesive layer, the diffusion pattern may change or disappear due to the adhesive, or air bubbles may be generated in the textured portions, etc.

[0005] Another type of diffusion film is an internal diffusion film that contains scattering particles inside. A PDLC film can be used as an internal diffusion film by utilizing the scattering effect of the liquid crystal droplets (for example, Patent Document 1).

[0006] Japanese Patent Application Laid-Open No. 2021-077534

[0007] A light diffusion device including a light source and a PDLC film as a diffusion film can be applied to a backlight device in an image display device, but when applied to a direct-type backlight device, the uniformity of the in-plane luminance may be insufficient. Therefore, a main object of the present invention is to provide a light diffusion device having a diffusion film that can realize more uniform surface light emission.

[0008] [1] A light diffusion device according to an embodiment of the present invention includes, in this order: a light source layer including a light source unit and an encapsulating resin layer encapsulating the light source unit; a first low-refractive index layer having a refractive index lower than that of the encapsulating resin layer; and a first diffusion film including a diffusion layer. The diffusion layer includes a polymer matrix and dispersed particles in the polymer matrix, the particles including at least one selected from a liquid crystal compound and a liquid crystal polymer. [2] In the above [1], the refractive index of the first low-refractive index layer may be lower than that of the first diffusion film. [3] In the above [1] or [2], the first low-refractive index layer may be a layer including voids or an air layer. [4] In any of the above [1] to [3], the encapsulating resin layer may include at least one selected from a silicone resin and an epoxy resin. [5] In any of the above [1] to [4], the first diffusion film may further include a transparent substrate disposed on at least one side of the diffusion layer. [6] In any of the above [1] to [5], the light source unit may include a plurality of point light sources. [7] In any one of [1] to [6] above, the dispersed particles may include at least the liquid crystal polymer. [8] In [7] above, the first diffusion film may have multiple regions with different hazes in a planar view. [9] In [8] above, the multiple regions may be arranged in a predetermined pattern.

[10] In any one of [1] to [9] above, a second low refractive index layer and a second diffusion film may be arranged in this order on the side of the first diffusion film opposite to the side on which the first low refractive index layer is arranged, and the second diffusion film may include a diffusion layer including a polymer matrix and dispersed particles containing at least one selected from a liquid crystal compound and a liquid crystal polymer, the second low refractive index layer having a lower refractive index than the first diffusion film and the second diffusion film.

[11] A backlight device according to an embodiment of the present invention includes the light diffusion device according to any one of [1] to

[10] above.

[12] An image display device according to an embodiment of the present invention includes the backlight device according to

[11] above and a display element.

[0009] In the manufacture of image display devices, in order to ensure good visibility, it is common to reduce interfacial reflection between adjacent optical films by using adhesive layers with a relatively high refractive index comparable to that of the optical films themselves. However, according to an embodiment of the present invention, a low-refractive index layer is disposed between the light source layer and the diffusion film, thereby obtaining a light diffusion device with improved in-plane luminance uniformity. The reason for this effect is presumed to be as follows, without limiting the present invention in any way. By disposing a low-refractive index layer between the light source layer and the diffusion film, interfacial reflection between the light source layer and the low-refractive index layer increases. As a result, light with reduced directivity enters the diffusion film compared to a configuration in which the light source layer and the diffusion film are directly laminated. It is presumed that the diffusion film further diffuses this reduced-directivity light, thereby improving in-plane luminance uniformity.

[0010] FIG. 1 is a schematic cross-sectional view showing the configuration of a light diffusion device according to one embodiment of the present invention. FIG. 2 is a schematic cross-sectional view showing the configuration of a light diffusion device according to one embodiment of the present invention. FIG. 3 is a schematic plan view of a diffusion film that can be used in the present invention, and FIG. 4 is a schematic cross-sectional view of the diffusion film shown in FIG. 4A is a schematic view illustrating step C of a method for manufacturing a diffusion film. FIG. 5 is a schematic cross-sectional view illustrating an electrode having convex portions. FIG. 6 is a schematic cross-sectional view of an example of a diffusion film that can be used in the present invention. FIG. 7 is a schematic cross-sectional view of an example of a diffusion film that can be used in the present invention. FIG. 8 is a schematic cross-sectional view of an example of a diffusion film that can be used in the present invention. FIG. 9 is a schematic cross-sectional view illustrating an example of a low refractive index layer that is an air layer. FIG. 10 is a schematic cross-sectional view of an image display device according to one embodiment of the present invention.

[0011] Preferred embodiments of the present invention will be described below, but the present invention is not limited to these embodiments. In this specification, the term "to" indicating a range of values ​​includes the upper and lower limits.

[0012] A. Light Diffusion Device A light diffusion device according to an embodiment of the present invention includes, in this order: a light source layer including a light source unit and a sealing resin layer that seals the light source unit; a first low refractive index layer that has a refractive index lower than that of the sealing resin layer; and a first diffusion film including a diffusion layer, wherein the diffusion layer includes a polymer matrix and dispersed particles that are dispersed in the polymer matrix and include at least one type selected from a liquid crystal compound and a liquid crystal polymer.

[0013] 1 is a schematic cross-sectional view showing the configuration of a light diffusion device according to one embodiment of the present invention. The light diffusion device 100A includes a light source layer 10 including a light source unit 12 and a sealing resin layer 14 sealing the light source unit 12, a first diffusion film 20, and a first low-refractive-index layer 30 disposed therebetween. The first low-refractive-index layer 30 has a refractive index lower than that of the sealing resin layer 14. Although not shown, the light diffusion device 100A may further include a reflective layer on the side of the light source layer 10 opposite the side on which the first low-refractive-index layer 30 is disposed.

[0014] FIG. 2 is a schematic cross-sectional view showing the configuration of a light diffusion device according to another embodiment of the present invention. The light diffusion device 100B includes a light source layer 10 including a light source unit 12 and a sealing resin layer 14 sealing the light source unit 12, a first low-refractive index layer 30 having a refractive index lower than that of the sealing resin layer 14, a first diffusion film 20, a second low-refractive index layer 40, and a second diffusion film 50, in this order. In other words, the light diffusion device 100B has a configuration in which the second low-refractive index layer 40 and the second diffusion film 50 are disposed in this order on the first diffusion film 20 of the light diffusion device 100A. The second low-refractive index layer 40 preferably has a refractive index lower than those of the first diffusion film 20 and the second diffusion film 50. By laminating the second low-refractive index layer 40 and the second diffusion film 50 on the first low-refractive index layer 30 and the first diffusion film 20, the effect of improving the in-plane luminance uniformity can be more effectively achieved. Although not shown, the light diffusing device 100B may further include a reflective layer on the side of the light source layer 10 opposite to the side on which the first low refractive index layer 30 is disposed.

[0015] A-1. Light Source Layer The light source layer 10 includes a light source section 12 and a sealing resin layer 14 that seals the light source section 12 .

[0016] The light source 12 is typically composed of a plurality of point light sources 12a. The plurality of point light sources are, for example, arranged two-dimensionally in a predetermined pattern. As the point light source, a light source that emits light with high directionality is preferable, and for example, an LED element can be used.

[0017] Examples of resins that can form the encapsulating resin layer 14 include thermosetting resins such as silicone resin, epoxy resin, polyester resin, urethane resin, and ethylene vinyl acetate; ultraviolet-curable resins such as acrylic resin, urethane resin, vinyl ester resin, and alkyd resin; and thermoplastic resins such as polyolefin, polystyrene, polyisobutylene, and isobutylene-based elastomer. Among these, silicone resin and epoxy resin are preferred, and silicone resin is more preferred, because they have high adhesion to resin films in general and can favorably achieve the effects of the present invention. The encapsulating resin layer may be formed using a single resin or two or more resins in combination.

[0018] The Young's modulus of the encapsulating resin layer (at 23°C and 50% RH) may be, for example, 5 GPa or less, more specifically, 0.1 GPa to 4 GPa. An encapsulating resin layer having such a Young's modulus tends to have high adhesion to resin films in general, and therefore, when a PDLC layer or PDLC film is used as a diffusion film, the interfacial reflection is reduced, which may result in insufficient uniformity of in-plane luminance. In contrast, according to an embodiment of the present invention, the provision of a first low refractive index layer can favorably achieve uniformity of in-plane luminance. The Young's modulus can be measured, for example, in accordance with JIS K 7127.

[0019] A-2. First Diffusion Film The first diffusion film includes a diffusion layer and may further include a transparent substrate on one or both sides thereof. The diffusion layer includes a polymer matrix and dispersed particles, which are dispersed in the polymer matrix and include at least one selected from a liquid crystal compound and a liquid crystal polymer. In one embodiment (also referred to as "Embodiment I"), the diffusion layer has multiple regions with different hazes in a planar view. In a diffusion layer having multiple regions with different hazes, the dispersed particles typically include at least a liquid crystal polymer. The liquid crystal polymer may exist in a different orientation state depending on the haze in each region with a different haze. In another embodiment (also referred to as "Embodiment II"), the diffusion layer has a substantially uniform haze in a planar view.

[0020] A-2-1. Embodiment I Figure 3 illustrates an example of a diffusion film including a diffusion layer having multiple regions with different hazes in a plan view. Figure 3(a) is a schematic plan view of the diffusion film, and Figure 3(b) is a schematic cross-sectional view of the diffusion film shown in Figure 3(a). The diffusion film 20a includes a diffusion layer 22 including a polymer matrix 22a and dispersed particles 22b containing a liquid crystal compound 23a and a liquid crystal polymer 23b dispersed in the polymer matrix 22a; a first transparent substrate 24 disposed on one side of the diffusion layer 22; and a second transparent substrate 26 disposed on the other side. The diffusion layer 22 and the first transparent substrate 24 and / or the second transparent substrate 26 may be laminated via an adhesive layer or a pressure-sensitive adhesive layer, or may be laminated directly without an adhesive layer or pressure-sensitive adhesive layer. Depending on the purpose, one or both of the first transparent substrate 24 and the second transparent substrate 26 may be omitted.

[0021] The diffusion layer 22 has five regions (A1, A2, B1, B2, and C). Among these regions, the orientation states of the liquid crystal polymer 23b in the regions A1 and A2 are the same as each other, the orientation states of the liquid crystal polymer 23b in the regions B1 and B2 are the same as each other, and the orientation states of the liquid crystal polymer 23b in the regions A1 and A2, the regions B1 and B2, and the region C are different from each other (relationship of the orientation states of the liquid crystal polymer in each region: A1 = A2 ≠ B1 = B2 ≠ C, A1 ≠ C).

[0022] Specifically, the liquid crystal polymer 23b in the dispersed particles 22b is oriented substantially perpendicular to the main surface of the diffusion film 20a (diffusion layer 22) in regions A1 and A2, is non-oriented in region C, and is oriented in regions B1 and B2 in an intermediate state. Furthermore, the liquid crystal compound 23a in the dispersed particles 22b is oriented along the liquid crystal polymer 23b, in a state similar to the orientation state of the liquid crystal polymer 23b. Therefore, the dispersed particles in these multiple regions (A1, A2, B1, B2, and C) may exhibit different scattering properties due to differences in the orientation state of the liquid crystal polymer and / or liquid crystal compound. As a result, the diffusion film 20a, in a planar view, exhibits minimum haze (diffusion degree) in regions corresponding to regions A1 and A2, maximum haze in region C, and intermediate haze in regions B1 and B2.

[0023] In the diffusion film 20a, the dispersed particles 22b contain a liquid crystal compound 23a and a liquid crystal polymer 23b, but the dispersed particles 22b do not necessarily contain the liquid crystal compound 23a. Furthermore, in the diffusion film, the orientation of the liquid crystal compound in the dispersed particles can be controlled by the liquid crystal polymer, so there is no need to control the orientation of the liquid crystal compound by applying a voltage. Therefore, the diffusion film does not need to have an electrode layer, regardless of whether the dispersed particles contain a liquid crystal compound.

[0024] In the illustrated example, the diffusion layer has three orientation states of the liquid crystal polymer in the dispersed particles, but this is not limited to this embodiment. Specifically, the orientation state of the liquid crystal polymer is not particularly limited as long as it is two or more. Furthermore, the orientation state of the liquid crystal polymer in multiple regions with different orientation states of the liquid crystal polymer (in other words, the scattering properties of the dispersed particles in those regions or the haze of those regions) is not limited, and each region may have a desired orientation state independently. Furthermore, the arrangement pattern of these regions is not limited and can be freely designed as a predetermined pattern. Therefore, the diffusion film can exhibit a desired haze in a desired pattern. In one embodiment, the diffusion layer is configured to have a haze pattern corresponding to the arrangement pattern of the point light source. For example, the diffusion layer is configured so that the haze is high in regions close to the point light source and decreases as the distance from the point light source increases. This configuration can effectively achieve uniform in-plane brightness even for direct-type LED light sources.

[0025] In addition, in the illustrated diffusion layer, each of the multiple regions (A1, A2, B1, B2, C) in which the liquid crystal polymer in the dispersed particles has a different orientation state has a certain area, but the region does not need to have an area greater than a predetermined value. For example, in this specification, even if the orientation state of the liquid crystal polymer changes continuously in the in-plane direction and a region in a specific orientation state in a planar view cannot be identified as a region having a certain area, it is treated as "a diffusion layer having multiple regions in which the liquid crystal polymer has a different orientation state." In one embodiment, when the haze of the diffusion film (more specifically, the diffusion layer) changes continuously in the in-plane direction in a planar view, it is treated as "a diffusion layer having multiple regions with different hazes," and the orientation state of the liquid crystal polymer can be considered to change continuously in the in-plane direction.

[0026] <Diffusion Layer> The diffusion layer includes a polymer matrix and dispersed particles containing at least a liquid crystal polymer dispersed in the polymer matrix, and has multiple regions with different hazes in a planar view. The liquid crystal polymer may exist in different orientation states depending on the haze in each region with a different haze. As described above, the dispersed particles may further include a liquid crystal compound. In the diffusion film of embodiment I, a non-polymerizable liquid crystal compound is typically used as the liquid crystal compound that can be contained in the dispersed particles. A method for producing the multiple regions will be described later.

[0027] The haze in each of the multiple regions of the diffusion layer can be appropriately set depending on the purpose. The maximum and minimum haze values ​​and the difference therebetween in the multiple regions of the diffusion layer can be set so as to obtain the maximum and minimum haze values ​​and the difference therebetween desired for the diffusion film. The haze in the region with the highest haze of the diffusion film is, for example, 30% to 100%. The haze in the region with the lowest haze is, for example, 0% to 70%. The difference between the maximum and minimum haze values ​​in the diffusion film typically exceeds 0%, for example, 5% or more, preferably 10% or more, more preferably 20% to 100%, and even more preferably 30% to 100%. The total light transmittance of the region with the highest haze of the diffusion film is, for example, 10% to 70%, preferably 10% to 50%. The total light transmittance of the portion with the lowest haze is, for example, 60% to 100%, preferably 80% to 100%.

[0028] The polymer matrix may be composed of any appropriate resin. The resin for forming the polymer matrix may be appropriately selected depending on the light transmittance, the refractive index of the liquid crystal polymer or liquid crystal compound, the adhesion to the substrate, etc. For example, water-soluble or water-dispersible resins such as urethane-based resins, polyvinyl alcohol-based resins, polyethylene-based resins, polypropylene-based resins, and acrylic-based resins may be preferably used. The polymer matrix-forming resins may be used alone or in combination.

[0029] The content of the polymer matrix in the diffusion layer is, for example, 30 to 70% by weight, preferably 35 to 65% by weight, and more preferably 40 to 60% by weight. If the content of the polymer matrix is ​​within this range, good mechanical strength can be obtained, and effects such as prevention of liquid crystal leakage from the edges can be obtained.

[0030] Liquid crystal polymers are polymers of polymerizable liquid crystal compounds and are non-liquid crystals, i.e., they do not undergo the transition from liquid crystal phase to glass phase or crystalline phase due to temperature changes that are specific to liquid crystal compounds.

[0031] The polymerizable liquid crystal compound constituting the liquid crystal polymer can be appropriately selected depending on the light transmittance, compatibility with the non-polymerizable liquid crystal compound, etc. The polymerizable liquid crystal compound may be a crosslinked type having two or more functionalities. Examples of the polymerizable liquid crystal compound include polymerizable mesogen compounds described in, for example, JP-A-2002-533742 (WO 00 / 37585), EP 358208 (US 5,211,877), EP 66137 (US 4,388,453), WO 93 / 22397, EP 0,261,712, DE 19504224, DE 4,408,171, and GB 2,280,445. Nematic liquid crystal monomers are preferred as the polymerizable liquid crystal compound. The birefringence Δn (=ne−no; ne is the refractive index of the liquid crystal compound molecules in the major axis direction, and no is the refractive index of the liquid crystal compound molecules in the minor axis direction) of the polymerizable liquid crystal compound at a wavelength of 589 nm is preferably 0.05 to 0.50, more preferably 0.10 to 0.45.

[0032] Any appropriate non-polymerizable liquid crystal compound can be used as the liquid crystal compound. As described below, the diffusion layer can be formed by performing a polymerization reaction while controlling the orientation of a polymerizable liquid crystal compound. In this case, by using a non-polymerizable liquid crystal compound in combination with a polymerizable liquid crystal compound, the temperature range of the liquid crystal phase (e.g., nematic phase) can be broadened, and orientation control can be more suitably performed. As the liquid crystal compound, a non-polymerizable liquid crystal compound having a birefringence Δn (=ne-no; ne is the refractive index of the liquid crystal compound molecules in the long axis direction and no is the refractive index of the liquid crystal compound molecules in the short axis direction) of 0.05 to 0.50 at a wavelength of 589 nm, more preferably 0.10 to 0.45, is used.

[0033] The dielectric anisotropy of the non-polymerizable liquid crystal compound may be positive or negative. The non-polymerizable liquid crystal compound may be, for example, a nematic, smectic, or cholesteric liquid crystal compound. It is preferable to use a nematic liquid crystal compound because it can achieve excellent transparency in the transparent state.

[0034] Examples of nematic liquid crystal compounds include biphenyl-based compounds, phenylbenzoate-based compounds, cyclohexylbenzene-based compounds, azoxybenzene-based compounds, azobenzene-based compounds, azomethine-based compounds, terphenyl-based compounds, biphenylbenzoate-based compounds, cyclohexylbiphenyl-based compounds, phenylpyridine-based compounds, cyclohexylpyrimidine-based compounds, cholesterol-based compounds, fluorine-based compounds, etc. These low-molecular-weight liquid crystal compounds may be used alone or in combination.

[0035] The total content of the liquid crystal polymer and the liquid crystal compound, if present, in the diffusion layer (the content of the liquid crystal polymer when the liquid crystal compound is not present) is, for example, 30% to 70% by weight, preferably 35% to 65% by weight, and more preferably 40% to 60% by weight. The content of the liquid crystal polymer relative to the total content of the liquid crystal polymer and the liquid crystal compound in the diffusion layer (more specifically, the dispersed particles) is, for example, 5% by weight or more, preferably 7% by weight or more, more preferably 10% by weight or more, and may be, for example, 100% by weight or less, preferably 80% by weight or less, and more preferably 50% by weight or less. The total content of the polymer matrix, the liquid crystal polymer, and the liquid crystal compound, if present, in the diffusion layer may be, for example, 90% by weight to 99.9% by weight, and preferably 95% by weight to 99.9% by weight.

[0036] As described below, in the preparation of the diffusion film of embodiment I, the diffusion layer can be formed by preparing a PDLC layer containing liquid crystal droplets containing a polymerizable liquid crystal compound and, optionally, a non-polymerizable liquid crystal compound, and polymerizing the polymerizable liquid crystal compound while applying a voltage from the first principal surface side and the second principal surface side of the PDLC layer so as to generate regions of different electric field strength. Therefore, the diffusion layer (more specifically, the dispersed particles) can further contain a polymerization initiator. The type and content of the polymerization initiator will be described later. Furthermore, unreacted polymerizable liquid crystal compound may remain in the dispersed particles. The content of the unreacted polymerizable liquid crystal compound in the diffusion layer is, for example, 3 wt % or less, preferably 1 wt % or less.

[0037] The average particle diameter of the dispersed particles can be, for example, 0.2 μm to 9 μm, preferably 0.3 μm to 8 μm. If the average particle diameter of the dispersed particles is too small, the dispersed particle size is smaller than the wavelength of light, so light passes through the dispersed particles without being scattered, which can result in a problem of insufficient haze being obtained. If the average particle diameter is too large, the dispersed particle size is larger than the wavelength of light, so can a problem of insufficient haze being obtained. Note that the average particle diameter of the dispersed particles in the diffusion layer is the volume average particle diameter of the dispersed particles when viewed from a direction perpendicular to the main surface of the diffusion film.

[0038] The thickness of the diffusion layer is, for example, 20 μm to 150 μm, preferably 30 μm to 120 μm, and more preferably 40 μm to 100 μm.

[0039] <First Transparent Substrate> The first transparent substrate 24 includes a first transparent film. The first transparent substrate may have a hard coat (HC) layer on one or both sides of the first transparent film, as needed.

[0040] The haze of the first transparent substrate is preferably 20% or less, more preferably 10% or less, and even more preferably 0.1% to 10%.

[0041] The total light transmittance of the first transparent substrate is preferably 30% or more, more preferably 60% or more, and even more preferably 80% or more. The total light transmittance can be measured in accordance with JIS K 7361.

[0042] The first transparent film may be formed using any suitable material. Specific examples include glass films and polymer films. Polymer films are preferred because they have excellent smoothness and can be continuously produced using rolls, significantly improving productivity.

[0043] The polymer film is typically a polymer film primarily composed of a thermoplastic resin. Examples of thermoplastic resins include polyester resins; cycloolefin resins such as polynorbornene; acrylic resins; polycarbonate resins; and cellulose resins. Among these, polyester resins, cycloolefin resins, and acrylic resins are preferred. These resins are excellent in transparency, mechanical strength, thermal stability, moisture barrier properties, and the like. The thermoplastic resins may be used alone or in combination of two or more. Optical films used in polarizing plates, such as low-retardation substrates, high-retardation substrates, retardation plates, absorptive polarizing films, and polarized selective reflection films, can also be used as the first transparent film.

[0044] The total light transmittance of the first transparent film is preferably 30% or more, more preferably 60% or more, and even more preferably 80% or more.

[0045] The thickness of the first transparent substrate (thickness including the HC layer if it has one) is preferably 200 μm or less, more preferably 3 μm to 150 μm, and even more preferably 5 μm to 100 μm.

[0046] <Second Transparent Substrate> The second transparent substrate 26 includes a second transparent film. The second transparent substrate may have a hard coat layer on one or both sides of the second transparent film, as needed.

[0047] The haze of the second transparent substrate is preferably 20% or less, more preferably 10% or less, and even more preferably 0.1% to 10%.

[0048] The total light transmittance of the second transparent substrate is preferably 30% or more, more preferably 60% or more, and even more preferably 80% or more.

[0049] The thickness of the second transparent substrate (thickness including the HC layer if it has one) is preferably 200 μm or less, more preferably 3 μm to 150 μm, and even more preferably 5 μm to 100 μm.

[0050] The same explanation as for the first transparent film can be applied to the second transparent film. The second transparent substrate may have the same configuration as the first transparent substrate, or may have a different configuration.

[0051] <Production Method> The diffusion film can be produced by any appropriate production method. The production method for the diffusion film includes, for example, (Step A) applying a coating liquid containing a polymer matrix-forming resin, a polymerizable liquid crystal compound, and a solvent to a first substrate to obtain a coating layer; (Step B) drying the coating layer to obtain a PDLC layer containing a polymer matrix and droplets containing the polymerizable liquid crystal compound dispersed in the polymer matrix; and (Step C) polymerizing the polymerizable liquid crystal compound while applying voltages from the first and second main surfaces of the PDLC layer to generate regions of different electric field strengths, thereby obtaining a diffusion layer. The production method for the diffusion film may optionally further include (Step D) placing a second substrate on the side of the PDLC layer or the diffusion layer opposite the side where the first substrate is provided, before or after polymerizing the polymerizable liquid crystal compound. According to the production method for the diffusion film, the polymerizable liquid crystal compound is polymerized in each of the regions of different electric field strength in a different orientation state depending on the electric field strength. As a result, a diffusion layer having a plurality of regions in which the liquid crystal polymer in the dispersed particles has different orientation states (as a result, a diffusion layer having a plurality of regions with different hazes) can be formed.

[0052] (Step A) In step A, a coating liquid containing a polymer matrix-forming resin, a polymerizable liquid crystal compound, and a solvent is applied to a first substrate to obtain a coating layer. The coating liquid may further contain a non-polymerizable liquid crystal compound.

[0053] The coating liquid is preferably an emulsion containing liquid crystal particles as a dispersoid, the liquid crystal particles including a polymerizable liquid crystal compound and optionally a non-polymerizable liquid crystal compound (hereinafter, this may be referred to as an "emulsion coating liquid"). In one embodiment, the coating liquid is an emulsion coating liquid in which polymer matrix-forming resin particles and liquid crystal particles including a polymerizable liquid crystal compound and optionally a non-polymerizable liquid crystal compound are dispersed in a solvent. The emulsion coating liquid preferably further contains a polymerization initiator in the liquid crystal particles, and may further contain any appropriate additives depending on the purpose.

[0054] As the solvent, water or a mixed solvent of water and a water-miscible organic solvent can be preferably used. Examples of the water-miscible organic solvent include C1-3 alcohol, acetone, DMSO, etc. The polymerizable liquid crystal compound, non-polymerizable liquid crystal compound, and polymer matrix-forming resin are as described above. Optional additives include a dispersant, a leveling agent, a crosslinking agent, etc.

[0055] The content of the liquid crystal compound in the solid content of the coating liquid (the total content of the polymerizable liquid crystal compound and the non-polymerizable liquid crystal compound, if present) may be, for example, 30% by weight to 70% by weight, preferably 35% by weight to 65% by weight, and more preferably 40% by weight to 60% by weight.

[0056] The weight ratio of the polymerizable liquid crystal compound to the non-polymerizable liquid crystal compound in the coating liquid (polymerizable liquid crystal compound:non-polymerizable liquid crystal compound) may be, for example, 5:95 to 100:0, preferably 7:93 to 80:20, and more preferably 10:90 to 50:50.

[0057] The content of the polymer matrix-forming resin in the solid content of the coating liquid may be, for example, 30 to 70% by weight, preferably 35 to 65% by weight, and more preferably 40 to 60% by weight.

[0058] The weight ratio of the content of the liquid crystal compound in the coating liquid (the total content of the polymerizable liquid crystal compound and, if present, the non-polymerizable liquid crystal compound) to the content of the polymer matrix-forming resin (liquid crystal compound:polymer matrix-forming resin) can be, for example, 30:70 to 70:30, preferably 35:65 to 65:35, and more preferably 40:60 to 60:40. Furthermore, the total content of the polymer matrix-forming resin and the polymerizable liquid crystal compound and, if present, the non-polymerizable liquid crystal compound in the solid content of the coating liquid can be, for example, 90% by weight to 99.9% by weight, preferably 95% by weight to 99.9% by weight.

[0059] The average particle size of the liquid crystal particles is preferably 0.2 μm or more, more preferably 0.3 μm or more. The average particle size of the liquid crystal particles is preferably 9 μm or less, more preferably 8 μm or less. If the average particle size of the liquid crystal particles is within this range, the average particle size of the dispersed particles in the diffusion layer can be set within a desired range. The average particle size of the liquid crystal particles is a volume-average particle size.

[0060] The particle size of the liquid crystal particles preferably has a relatively narrow particle size distribution. The coefficient of variation (CV value) of the particle size of the liquid crystal particles may be, for example, less than 0.40, preferably 0.35 or less, and more preferably 0.30 or less. In one embodiment, an emulsion coating liquid may be used that is substantially free of liquid crystal particles having a particle size of less than 0.2 μm or more than 9 μm (for example, an emulsion coating liquid in which the volume ratio of liquid crystal particles having a particle size of less than 0.2 μm or more than 9 μm to the total volume of liquid crystal particles is 10% or less).

[0061] The average particle size of the resin particles for forming a polymer matrix is ​​preferably 10 nm to 500 nm, more preferably 30 nm to 300 nm, and even more preferably 50 nm to 200 nm. Two or more types of resin particles differing in type and / or average particle size may be used. The average particle size of the resin particles for forming a polymer matrix means the volume average particle size, and can be measured using a dynamic light scattering particle size distribution analyzer.

[0062] As the polymerization initiator, any appropriate photopolymerization initiator or thermal polymerization initiator can be used depending on the purpose, desired properties, etc., and a photopolymerization initiator is preferably used. Specific examples of the photopolymerization initiator include 2,2-dimethoxy-2-phenylacetophenone, acetophenone, benzophenone, xanthone, 3-methylacetophenone, 4-chlorobenzophenone, 4,4'-dimethoxybenzophenone, benzoin propyl ether, benzil dimethyl ketal, N,N,N',N'-tetramethyl-4,4'-diaminobenzophenone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,4-dipentoxyphenylphosphine oxide, bis(2,6-dimethoxy-benzoyl)-(2,4,4-trimethyl-pentyl)-phosphine oxide, and thioxanthone compounds. The polymerization initiators may be used alone or in combination of two or more. The content of the polymerization initiator is preferably 0.1 to 10 parts by weight, more preferably 0.5 to 5 parts by weight, based on 100 parts by weight of the polymerizable liquid crystal compound.

[0063] Examples of dispersants include anionic surfactants, cationic surfactants, amphoteric surfactants, nonionic surfactants, etc. The content of the dispersant is preferably 0.05 to 10 parts by weight, more preferably 0.1 to 1 part by weight, relative to 100 parts by weight of the coating liquid.

[0064] Examples of the leveling agent include an acrylic leveling agent, a fluorine-based leveling agent, a silicone-based leveling agent, etc. The content of the leveling agent is preferably 0.05 to 10 parts by weight, more preferably 0.1 to 1 part by weight, relative to 100 parts by weight of the coating liquid.

[0065] Examples of the crosslinking agent include an aziridine-based crosslinking agent, an isocyanate-based crosslinking agent, etc. The content of the crosslinking agent is preferably 0.5 parts by weight to 10 parts by weight, more preferably 0.8 parts by weight to 5 parts by weight, relative to 100 parts by weight of the coating liquid.

[0066] The coating liquid, preferably an emulsion coating liquid, can be prepared by, for example, mixing a resin emulsion or resin particle dispersion containing polymer matrix-forming resin particles, a liquid crystal emulsion containing liquid crystal particles containing a polymerizable liquid crystal compound, a polymerization initiator, and optionally a non-polymerizable liquid crystal compound, and optional additives (e.g., dispersants, leveling agents, crosslinking agents). If necessary, a solvent may be added during mixing. Alternatively, the emulsion coating liquid can be prepared by adding a polymerizable liquid crystal compound, a polymer matrix-forming resin, a polymerization initiator, and optionally a non-polymerizable liquid crystal compound and additives to a solvent and mechanically dispersing the mixture.

[0067] The resin emulsion and liquid crystal emulsion can be prepared by, for example, a mechanical emulsification method, an ultrasonic emulsification method, a microchannel method, a membrane emulsification method, or the like.

[0068] The solid content of the coating liquid may be, for example, 20% to 60% by weight, and preferably 30% to 50% by weight.

[0069] The viscosity of the coating liquid can be appropriately adjusted to ensure successful application to the first substrate. The viscosity of the coating liquid during application is preferably 20 mPa·s to 400 mPa·s, more preferably 30 mPa·s to 300 mPa·s, and even more preferably 40 mPa·s to 200 mPa·s. If the viscosity is less than 20 mPa·s, solvent convection becomes significant when the solvent is dried, which may result in an unstable thickness of the PDLC layer (and consequently, the diffusion layer). Furthermore, if the viscosity exceeds 400 mPa·s, the coating liquid bead may become unstable. The viscosity of the coating liquid can be measured, for example, using an Anton Paar MCR302 rheometer. The viscosity used here is the shear viscosity value at 20°C and a shear rate of 1000 (1 / s).

[0070] Any appropriate substrate can be used as the first substrate. By using the first transparent substrate as the first substrate, a diffusion film having the first transparent substrate and a diffusion layer can be suitably obtained. Depending on the purpose, the first substrate may be peeled off and removed from the diffusion layer after completion of step C.

[0071] Any appropriate method can be used as the coating method, such as roll coating, spin coating, wire bar coating, dip coating, die coating, curtain coating, spray coating, and knife coating (such as comma coating).

[0072] The thickness of the coating layer is preferably 40 μm to 300 μm, more preferably 60 μm to 240 μm, and even more preferably 80 μm to 200 μm. Within such a range, a diffusion layer having excellent in-plane brightness improving effect and excellent thickness uniformity can be obtained.

[0073] (Step B) In step B, the coating layer is dried to obtain a PDLC layer containing a polymer matrix and droplets containing a polymerizable liquid crystal compound and, optionally, a non-polymerizable liquid crystal compound dispersed in the polymer matrix. The solvent is removed from the coating layer by drying, and the resin particles for forming the polymer matrix are fused to each other, forming a PDLC layer having a structure in which liquid crystal droplets are dispersed in a polymer matrix.

[0074] The coating layer can be dried by any appropriate method. Specific examples of the drying method include natural drying, heat drying, hot air drying, etc. When the coating liquid contains a crosslinking agent, a crosslinked structure of the polymer matrix can be formed during drying.

[0075] The drying temperature is preferably 20° C. to 150° C., more preferably 25° C. to 80° C. The drying time is preferably 1 minute to 100 minutes.

[0076] (Step C) In step C, the polymerizable liquid crystal compound is polymerized while applying a voltage from the first principal surface side and the second principal surface side of the PDLC layer so as to generate regions with different electric field strengths, thereby forming a diffusion layer containing a polymer matrix and dispersed particles that are dispersed in the polymer matrix and contain a liquid crystal polymer, which is a polymer of the polymerizable liquid crystal compound.

[0077] The polymerization of the polymerizable liquid crystal compound is carried out by irradiation with active energy rays, heating, or a combination thereof, and is preferably carried out by irradiation with active energy rays.

[0078] Examples of active energy rays that can be used include ultraviolet rays, infrared rays, X-rays, α rays, β rays, γ rays, and electron beams. Of these, ultraviolet rays are preferred. Furthermore, the active energy rays are preferably collimated rays that have a high degree of linearity from the irradiation source.

[0079] The ultraviolet irradiation conditions can be appropriately set depending on the type of polymerizable liquid crystal compound, the transmittance of the substrate, the absorption wavelength of the photopolymerization initiator, etc. The irradiation intensity is, for example, 0.1 mW / cm 2 ~1000mW / cm 2 , preferably 1 mW / cm 2 ~100mW / cm 2 The irradiation dose can be, for example, 10 mJ / cm 2 ~10000mJ / cm 2 , preferably 100 mJ / cm 2 ~5000mJ / cm 2 The irradiation temperature may be, for example, from -20°C to 80°C, preferably from -20°C to 60°C.

[0080] In one embodiment, voltage application is performed using a first electrode disposed on the first principal surface side of the PDLC layer and a second electrode disposed on the second principal surface side, and regions with different electric field strengths are formed by controlling the separation distance between the first and second electrodes. Step C will now be described with reference to FIG. 4 . In the embodiment shown in FIG. 4 , step D is performed before step C, and a first transparent substrate 24 as a first substrate is disposed on the first principal surface side of the PDLC layer 22′, and a second transparent substrate 26 as a second substrate is disposed on the second principal surface side. Unlike the illustrated example, the first principal surface and / or the second principal surface of the PDLC layer may be exposed.

[0081] FIG. 4( a) is a schematic cross-sectional view showing the PDLC layer obtained in step B in a state where no voltage is applied. The PDLC layer 22′ includes a polymer matrix 22a and liquid crystal droplets 22b′ dispersed in the polymer matrix 22a. The liquid crystal droplets 22b′ include a non-polymerizable liquid crystal compound 23a and a polymerizable liquid crystal compound 23c. A first electrode 310 is disposed on the outer side of the first transparent substrate 24 (the side opposite the side where the PDLC layer is disposed), and a second electrode 320 is disposed on the outer side of the second transparent substrate 26 (the side opposite the side where the PDLC layer is disposed). Since no voltage is applied to the electrodes 310 and 320 from a power source 330 and no electric field is generated between them, the non-polymerizable liquid crystal compound 23a and the polymerizable liquid crystal compound 23c in the liquid crystal droplets 22b′ are in a non-oriented state. Furthermore, the first electrode 310 is formed so that the surface height on the PDLC layer 22′ side varies depending on the region, thereby forming regions with different inter-electrode distances.

[0082] The regions with different inter-electrode distances can be freely designed, for example, by changing the surface shape of the first electrode and / or second electrode on the PDLC layer side. Specifically, a desired inter-electrode distance can be achieved by providing any desired pattern of unevenness, steps, slopes, etc. on the surface of the first electrode and / or second electrode. For example, as shown in FIG. 5 , by providing tapered convex portions 312 on the surface of electrode 310a, the inter-electrode distance can be continuously changed, thereby continuously changing the in-plane orientation of the polymerizable liquid crystal compound and non-polymerizable liquid crystal compound in the liquid crystal droplets. In this case, by changing the height H and the tilt angle θ, the amount and rate of change in the inter-electrode distance can be controlled, resulting in a diffusion film with a haze gradient of any desired steepness or steepness. The height H and the tilt angle θ can each be set to any appropriate value depending on the haze pattern desired for the diffusion film.

[0083] FIG. 4B is a schematic diagram illustrating an embodiment in which the polymerizable liquid crystal compound 23c is polymerized by UV irradiation. UV irradiation is performed while a voltage is applied between the first electrode 310 and the second electrode 320 from a power source 330. The application of the voltage generates an electric field between the first electrode 310 and the second electrode 320, with the strength depending on the distance between them, resulting in the creation of multiple regions with different electric field strengths. In each of these multiple regions, the non-polymerizable liquid crystal compound 23a and the polymerizable liquid crystal compound 23c in the liquid crystal droplet 22b' are aligned according to the electric field strength. Specifically, in the region where the distance between the first electrode 310 and the second electrode 320 is smallest, the non-polymerizable liquid crystal compound 23a and the polymerizable liquid crystal compound 23c are aligned approximately perpendicular to the major surface of the PDLC layer 22'. As the distance between the first electrode 310 and the second electrode 320 increases, the degree of alignment weakens. By polymerizing the polymerizable liquid crystal compound 23c in this state, a diffusion layer 22 is formed having multiple regions with different orientation states of the liquid crystal polymer 23b in the dispersed particles 22b (as a result, multiple regions with different hazes), as shown in Figure 4(c).

[0084] The voltage applied during polymerization is not limited as long as the polymerizable liquid crystal compound exhibits the desired alignment, and can be appropriately set depending on the haze desired for the diffusion film, the distance between the electrodes, etc. The voltage can be, for example, 10 V to 100 kV, and preferably 100 V to 10 kV.

[0085] (Step D) In ​​step D, a second substrate is disposed on the side (second main surface side) of the PDLC layer or the diffusion layer opposite to the side (first main surface side) on which the first substrate is provided. Any appropriate substrate may be used as the second substrate, and the above-mentioned second transparent substrate may be preferably used. Step D may be performed before step C, i.e., before polymerizing the polymerizable liquid crystal compound, or after step C, i.e., after polymerizing the polymerizable liquid crystal compound.

[0086] According to the method for manufacturing a diffusion film including steps A to D, by using the first transparent substrate and the second transparent substrate as the first substrate and the second substrate, respectively, a diffusion film can be obtained that has the first transparent substrate and the second transparent substrate and a diffusion layer directly sandwiched therebetween.

[0087] From the viewpoint of obtaining sufficient adhesion, the second substrate is laminated on the second main surface side of the PDLC layer or the diffusion layer, preferably using a laminator, while applying a laminating pressure of 0.006 MPa / m to 7 MPa / m, more preferably 0.06 MPa / m to 0.7 MPa / m.

[0088] A-2-2. Embodiment II The diffusion film 20b shown in FIG. 6A includes a diffusion layer 22 including a polymer matrix 22a and dispersed particles 22b containing a liquid crystal compound 23a and a liquid crystal polymer 23b dispersed in the polymer matrix 22a, a first transparent substrate 24 disposed on one side of the diffusion layer 22, and a second transparent substrate 26 disposed on the other side. The diffusion layer 22 and the first transparent substrate 24 and / or the second transparent substrate 26 may be laminated via an adhesive layer or a pressure-sensitive adhesive layer, or may be laminated directly without an adhesive layer or a pressure-sensitive adhesive layer. Depending on the purpose, one or both of the first transparent substrate 24 and the second transparent substrate 26 may be omitted. In the diffusion film of Embodiment II, the diffusion layer may include dispersed particles containing a liquid crystal polymer but not a liquid crystal compound, or may include dispersed particles containing a liquid crystal compound but not a liquid crystal polymer. For example, a diffusion film 20c shown in Fig. 6B includes a diffusion layer 22 including a polymer matrix 22a and dispersed particles 22b containing a liquid crystal polymer 23b and not containing a liquid crystal compound, a first transparent substrate 24 disposed on one side of the diffusion layer 22, and a second transparent substrate 26 disposed on the other side. Also, for example, a diffusion film 20d shown in Fig. 6C includes a diffusion layer 22 including a polymer matrix 22a and dispersed particles 22b containing a liquid crystal compound 23a and not containing a liquid crystal polymer, a first transparent substrate 24 disposed on one side of the diffusion layer 22, and a second transparent substrate 26 disposed on the other side.

[0089] In the diffusion film of embodiment II, typically, the orientation state of the liquid crystal compound and / or liquid crystal polymer in the dispersed particles is substantially uniform throughout the entire diffusion layer, and as a result, the diffusion layer can have a substantially uniform haze when viewed in a plane.

[0090] Because the diffusion layer has a substantially uniform haze, the diffusion films of embodiment II (e.g., diffusion films 20b-20d) also have a substantially uniform haze. The difference between the maximum and minimum haze values ​​in the diffusion films of embodiment II is, for example, less than 10%, and preferably less than 5%. The haze of the diffusion films of embodiment II is, for example, 50% to 80%, or, for example, 70% to 100%.

[0091] The same explanation as for the diffusion film of embodiment I can be applied to the diffusion film of embodiment II, except that the orientation state of the liquid crystal compound and / or liquid crystal polymer in the dispersed particles is substantially uniform throughout the diffusion layer. For example, in diffusion films 20b and 20c, the liquid crystal compound 23a and / or the liquid crystal polymer 23b may be in a predetermined orientation state or in a non-oriented state. Also, for example, in diffusion film 20d, the liquid crystal compound 23a may be in a non-oriented state.

[0092] A diffusion film (e.g., diffusion film 20b or 20c) in which dispersed particles contain a liquid crystal polymer can be obtained by a method similar to that for the diffusion film of embodiment I, except that in step C above, the polymerizable liquid crystal compound is polymerized without applying a voltage to the PDLC layer or while applying a predetermined voltage so that the electric field strength between the electrodes is constant. For example, a diffusion film with high haze can be obtained by performing polymerization without applying a voltage. Furthermore, for example, the haze of the resulting diffusion film can be reduced by increasing the electric field strength between the electrodes during polymerization.

[0093] A diffusion film in which dispersed particles contain a liquid crystal compound but do not contain a liquid crystal polymer (e.g., diffusion film 20d) can be obtained by a method similar to that of the diffusion film of embodiment I, except that step C is not performed. In such a diffusion film, the liquid crystal compound may be a polymerizable liquid crystal compound, a non-polymerizable liquid crystal compound, or a combination of both. In one embodiment, a coating liquid may be used that contains a non-polymerizable liquid crystal compound but does not contain a polymerizable liquid crystal compound or a polymerization initiator.

[0094] A-3. First Low Refractive Index Layer The first low refractive index layer 30 has a refractive index lower than that of the encapsulating resin layer 14. The refractive index of the first low refractive index layer is, for example, 1.30 or less, preferably 1.20 or less, and more preferably 1.15 or less, and is even more preferably equivalent to the refractive index of air (1.00). The lower limit of the refractive index of the first low refractive index layer is, for example, the refractive index of air (1.00). If the refractive index of the first low refractive index layer is within this range, the interfacial reflection at the interface with the light source layer is increased, thereby realizing a light diffusion device with high in-plane luminance uniformity. The difference between the refractive index of the first low refractive index layer and the refractive index of the encapsulating resin layer is, for example, 0.1 or more and 0.4 or less, preferably 0.2 or more and 0.4 or less.

[0095] The first low-refractive index layer preferably has a refractive index lower than that of the first diffusion film. The difference between the refractive index of the first low-refractive index layer and that of the first diffusion film is, for example, 0.2 or more and 0.6 or less, preferably 0.3 or more and 0.6 or less. The phrase "the first low-refractive index layer has a refractive index lower than that of the first diffusion film" means that the refractive index of the first low-refractive index layer is lower than the refractive index of the surface of the first diffusion film facing the first low-refractive index layer. Therefore, when the first diffusion film has a transparent substrate on the light source layer side of the diffusion layer, the refractive index is lower than that of the transparent substrate. When the first diffusion film does not have a transparent substrate, the refractive index is lower than that of the polymer matrix. The refractive index of the polymer matrix is ​​typically 1.49 to 1.60, for example, 1.49 to 1.55. The refractive index of the transparent substrate is typically 1.49 to 1.65, for example, 1.49 to 1.58.

[0096] The first low refractive index layer may have any configuration as long as it has the above-mentioned refractive index. In one embodiment, the first low refractive index layer is a low refractive index layer having an internal void. In another embodiment, the first low refractive index layer is an air layer.

[0097] A-3-1. Low refractive index layer having voids therein The porosity of the low refractive index layer having voids therein can be any appropriate value. The porosity is, for example, 5% to 99%, and preferably 25% to 95%. By having the porosity within the above range, the refractive index of the low refractive index layer can be sufficiently low and high mechanical strength can be obtained. Air typically exists in the voids.

[0098] The low refractive index layer may have a structure having at least one of the following shapes: particulate, fibrous, and flat. The particulate structures (structural units) may be solid or hollow particles, specifically silicone particles, silicone particles having micropores, hollow silica nanoparticles, and hollow silica nanoballoons. The fibrous structural units may be nanofibers with a nanometer diameter, specifically cellulose nanofibers and alumina nanofibers. The flat structural units may be nanoclays, specifically nanometer-sized bentonite (e.g., Kunipia F [trade name]). Furthermore, in the void structure of the low refractive index layer, the structural units that form the void structure may contain portions that are chemically bonded together, for example, directly or indirectly, via catalytic action. In the present invention, the term "indirectly bonded" between structural units refers to the structural units being bonded together via a small amount of binder component, the amount of which is equal to or less than the amount of the structural units. The phrase "structural units are directly bonded" means that the structural units are directly bonded to each other without the intervention of a binder component or the like.

[0099] Any appropriate material may be used as the material for the low refractive index layer. Examples of such materials include those described in International Publication No. 2004 / 113966, Japanese Patent Application Laid-Open No. 2013-254183, and Japanese Patent Application Laid-Open No. 2012-189802. Specific examples include silica-based compounds; hydrolyzable silanes and their partial hydrolysates and dehydration condensates; organic polymers; silicon compounds containing silanol groups; activated silica obtained by contacting silicate with acid or ion exchange resin; polymerizable monomers (e.g., (meth)acrylic monomers and styrene-based monomers); curable resins (e.g., (meth)acrylic resins, fluorine-containing resins, and urethane resins); and combinations thereof.

[0100] Examples of the organic polymer include polyolefins (e.g., polyethylene and polypropylene), polyurethanes, fluorine-containing polymers (e.g., fluorine-containing copolymers having, as constituent components, a fluorine-containing monomer unit and a constituent unit for imparting crosslinking reactivity), polyesters (e.g., poly(meth)acrylic acid derivatives (in this specification, (meth)acrylic acid means acrylic acid and methacrylic acid, and "(meth)" is used in this sense in all cases)), polyethers, polyamides, polyimides, polyureas, and polycarbonates.

[0101] The above-mentioned material preferably includes a silica-based compound; a hydrolyzable silane, and a partial hydrolyzate and dehydrated condensate thereof.

[0102] Examples of the silica-based compound include SiO 2 (silicic anhydride); SiO 2 And Na 2 Alumni 2 O 3 (borosilicate), Al 2 O 3 (Alumina), B 2 O 3 , TiO 2 , ZrO 2 , SnO 2 , Ce 2 O 3 , P 2O 5 , Sb 2 O 3 , MoO 3 , ZnO 2 , W.O. 3 , TiO 2 -Al 2 O 3 , TiO 2 -ZrO 2 , In 2 O 3 -SnO 2 , and Sb 2 O 3 -SnO 2 and a compound containing at least one compound selected from the group consisting of (the "-" above indicates a composite oxide).

[0103] Examples of the hydrolyzable silanes include those containing an alkyl group which may have a substituent (e.g., fluorine). The hydrolyzable silanes and their partial hydrolyzates and dehydration condensates are preferably alkoxysilanes and silsesquioxanes.

[0104] The alkoxysilane may be a monomer or an oligomer. The alkoxysilane monomer preferably has three or more alkoxyl groups. Examples of the alkoxysilane monomer include methyltrimethoxysilane, methyltriethoxysilane, phenyltriethoxysilane, tetramethoxysilane, tetraethoxysilane, tetrabutoxysilane, tetrapropoxysilane, diethoxydimethoxysilane, dimethyldimethoxysilane, and dimethyldiethoxysilane. The alkoxysilane oligomer is preferably a polycondensate obtained by hydrolysis and polycondensation of the above-mentioned monomer. By using an alkoxysilane as the material, a low refractive index layer with excellent uniformity can be obtained.

[0105] Silsesquioxanes have the general formula RSiO 1.5(where R represents an organic functional group). Examples of R include alkyl groups (which may be linear or branched and have 1 to 6 carbon atoms), phenyl groups, and alkoxy groups (e.g., methoxy and ethoxy groups). Examples of silsesquioxane structures include ladder and cage structures. By using silsesquioxane as the material, a low refractive index layer with excellent uniformity, weather resistance, transparency, and hardness can be obtained.

[0106] Any suitable particles can be used as the particles, and the particles are typically made of a silica-based compound.

[0107] The shape of the silica particles can be confirmed by observation with, for example, a transmission electron microscope. The average particle size of the particles is, for example, 5 nm to 200 nm, and preferably 10 nm to 200 nm. By having the above-mentioned structure, it is possible to obtain a low refractive index layer having a sufficiently low refractive index, and to maintain the transparency of the low refractive index layer. Here, the average particle size of the particles is the specific surface area (m ) measured by the nitrogen adsorption method (BET method). 2 / g), the average particle size is the value given by the formula: average particle size = (2720 / specific surface area) (see JP-A-1-317115).

[0108] The haze of the low refractive index layer is, for example, 0.1% to 30%, and preferably 0.2% to 10%.

[0109] The mechanical strength of the low refractive index layer is preferably such that the scratch resistance measured by Bemcot (registered trademark) is 60% to 100%.

[0110] The thickness of the low refractive index layer is preferably 0.1 μm to 100 μm, more preferably 0.2 μm to 30 μm, and even more preferably 1 μm to 20 μm. If the thickness is less than 0.1 μm, the effect of the low refractive index layer may not be sufficiently obtained. On the other hand, if the thickness is greater than 100 μm, the thickness of the light diffusing device becomes too large.

[0111] Examples of methods for obtaining the low refractive index layer include those described in JP 2010-189212 A, JP 2008-040171 A, JP 2006-011175 A, WO 2004 / 113966 pamphlet, and references thereto. Specific examples include a method of hydrolyzing and polycondensing at least one of silica-based compounds, hydrolyzable silanes, and their partial hydrolysates and dehydration condensates, a method using porous particles and / or hollow fine particles, a method of producing an aerogel layer by utilizing the springback phenomenon, and a method of using a pulverized gel obtained by pulverizing a gel obtained by sol-gel and chemically bonding the microporous particles in the pulverized liquid with a catalyst or the like.

[0112] The low refractive index layer may be formed on a substrate film and thereby supported by the substrate film. The same explanation as for the first transparent film in Section A-2 can be applied to the substrate film. The refractive index of the substrate film is not particularly limited as long as the effects of the present invention can be obtained.

[0113] A-3-2. Low-Refractive-Index Layer as Air Layer In one embodiment, the air layer serving as the low-refractive-index layer 30 can be formed spontaneously between the resin film 32 and the diffusion film 20 by placing the resin film 32 on the light source layer 10 and laminating the diffusion film 20 thereon without an adhesive layer, as shown in Fig. 7A. The thickness of the air layer formed in this embodiment is not particularly limited, but is, for example, 0.1 µm to 3 µm, and preferably 1 µm to 3 µm.

[0114] The resin film preferably has low adhesion to the diffusion film. The arithmetic mean roughness (Ra) of the resin film surface is, for example, 10 nm or more, preferably 50 nm or more. The upper limit of the Ra of the resin film is not particularly limited, but may be, for example, 100 nm or less. One or both sides of the resin film may be subjected to a surface roughening treatment. In this case, the Ra of the resin film may be 1 μm to 2 μm. Ra can be measured in accordance with JIS B 0601.

[0115] The resin forming the resin film is not limited as long as it can achieve the effects of the present invention, and examples thereof include polyester resins such as polyethylene terephthalate (PET); cycloolefin resins such as polynorbornene; acrylic resins; polycarbonate resins; and cellulose resins. These resins may be used alone or in combination of two or more. The thickness of the resin film is, for example, 10 μm to 100 μm.

[0116] In another embodiment, the air layer serving as the low refractive index layer 30 can be formed as a space having a height corresponding to the diameter of the spacer between the light source layer 10 and the diffusion film 20 by laminating the diffusion film 20 on the light source layer 10 via a spacer 34, as shown in Fig. 7B. The spacer 34 may be fixed to the light source layer 10 and / or the diffusion film 20 with an adhesive, or may be interposed between the light source layer 10 and the diffusion film 20 without being fixed with an adhesive. The thickness of the air layer formed in this embodiment is not particularly limited, but is, for example, 1 µm to 20 µm, preferably 5 µm to 20 µm, depending on the particle size of the spacer.

[0117] A-4. Second Diffusion Film The second diffusion film 50 includes, for example, a diffusion layer, a third transparent substrate disposed on one side of the diffusion layer, and a fourth transparent substrate disposed on the other side. As long as the effects of the present invention are obtained, one or both of the third transparent substrate and the fourth transparent substrate may be omitted.

[0118] The same explanation as for the first diffusion film 20 can be applied to the second diffusion film 50. The first diffusion film and the second diffusion film may have the same configuration or different configurations. For example, both the first diffusion film and the second diffusion film may have a substantially uniform haze in plan view, or both the first diffusion film and the second diffusion film may have a non-uniform haze in plan view (in other words, they may have multiple regions with different hazes). Also, for example, one of the first diffusion film and the second diffusion film may have a substantially uniform haze in plan view, and the other may have a non-uniform haze.

[0119] A-5. Second Low Refractive Index Layer The second low refractive index layer 40 typically has a refractive index lower than those of the first diffusion film 20 and the second diffusion film 50. The refractive index of the second low refractive index layer 40 is, for example, 1.30 or less, preferably 1.20 or less, and more preferably 1.15 or less, and is even more preferably equivalent to the refractive index of air (1.00). The lower limit of the refractive index of the second low refractive index layer is, for example, the refractive index of air (1.00). If the refractive index of the second low refractive index layer is within this range, interfacial reflection at the interface with the first diffusion film is increased, thereby achieving a light diffusion device with higher in-plane luminance uniformity. Note that "the second low refractive index layer has a refractive index lower than that of the first diffusion film" means that the refractive index of the second low refractive index layer is lower than the refractive index of the surface of the first diffusion film facing the second low refractive index layer. Therefore, if the first diffusion film has a transparent substrate on the second low refractive index layer side of the diffusion layer, it means that the refractive index is lower than the refractive index of the transparent substrate. If no transparent substrate is present, it means that the refractive index is lower than the refractive index of the polymer matrix. The same applies to "the second low refractive index layer has a refractive index lower than that of the second diffusion film."

[0120] The difference between the refractive index of the second low refractive index layer and the refractive index of the first diffusion film 20 is, for example, 0.2 or more and 0.6 or less, preferably 0.3 or more and 0.6 or less. The difference between the refractive index of the second low refractive index layer and the refractive index of the second diffusion film 50 is, for example, 0.2 or more and 0.6 or less, preferably 0.3 or more and 0.6 or less. The refractive index of the polymer matrix is ​​usually 1.49 to 1.60, for example, 1.49 to 1.55. The refractive index of the transparent substrate is usually 1.49 to 1.65, for example, 1.49 to 1.58.

[0121] The same description as for the first low refractive index layer 30 can be applied to the second low refractive index layer 40. The first low refractive index layer and the second low refractive index layer may have the same configuration or different configurations.

[0122] A-6. Reflective Layer Any appropriate configuration may be adopted as the reflective layer. For example, the reflective layer may be a specular reflective layer or a diffuse reflective layer. Specific examples of the reflective layer include a highly reflective resin sheet (e.g., an acrylic plate) mixed with a white pigment, a thin metal plate or metal foil such as aluminum or stainless steel, a vapor-deposited sheet in which aluminum, silver, or the like is vapor-deposited on a substrate such as a resin film such as polyester, a laminate of a substrate such as a resin film such as polyester and a metal foil such as aluminum, and a resin film in which voids are formed inside.

[0123] A-7. Method for Producing a Light Diffusing Device A light diffusing device can be obtained by laminating the above-mentioned components. A light diffusing device using an air layer as the low refractive index layer can be obtained, for example, by laminating a resin film on a light source layer with or without an adhesive layer; and laminating a diffusion film on the resin film without an adhesive layer. Alternatively, a light diffusing device using an air layer as the low refractive index layer can be obtained, for example, by interspersing spacers on the light source layer; and laminating a diffusion film on the spacers. An adhesive may or may not be present between the spacers and the light source layer and / or the diffusion film. A light diffusing device using a low refractive index layer other than an air layer can be obtained, for example, by laminating a low refractive index layer on a light source layer with or without an adhesive layer; and laminating a diffusion film on the low refractive index layer with or without an adhesive layer. As the adhesive layer, a pressure-sensitive adhesive layer, an adhesive layer, etc. can be used, and among these, an acrylic pressure-sensitive adhesive layer is preferably used. By fixing each component with an adhesive layer, problems such as deterioration due to friction between components, undulation of components, and the occurrence of water marks can be prevented.

[0124] B. Backlight Device The light diffusion device described in Section A can be used in a backlight device in an image display device. Therefore, a backlight device according to an embodiment of the present invention includes the light diffusion device described in Section A.

[0125] C. Image Display Device An image display device according to an embodiment of the present invention includes the backlight device described in Section B and a display element. In other words, an image display device according to an embodiment of the present invention includes the light diffusion device described in Section A and a display element. The display element is preferably a liquid crystal panel. In one embodiment, the image display device is a liquid crystal display device 200, as shown in FIG. 8, which includes the light diffusion device 100 described in Section A and a liquid crystal panel 110 arranged on the viewing side thereof.

[0126] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring each property are as follows. Unless otherwise specified, "parts" and "%" in the examples and comparative examples are by weight.

[0127] (1) Thickness: Measured using a digital micrometer (manufactured by Anritsu Corporation, product name "KC-351C"). (2) Volume average particle diameter of liquid crystal particles in liquid crystal emulsion: The volume average particle diameter was calculated using a particle size distribution measuring device (manufactured by Microtrac, product name "MT3300EXII"). (3) Average particle diameter of resin particles: A measurement sample was prepared by adding a few drops of resin dispersion to 100 mL of water. Using a dynamic light scattering particle size distribution measuring device (manufactured by Microtrac, product name "Nanotrac150"), the measurement sample was set in the measurement holder of the device, and after confirming on the monitor of the device that the concentration was measurable, measurement was performed. (4) Haze: Measured using a product name "NDH4000" manufactured by Nippon Denshoku Co., Ltd., based on JIS K 7136. (5) Refractive index of low refractive index layer After forming a low refractive index layer on the acrylic film, it was cut to a size of 50 mm x 50 mm and attached to the surface of a glass plate (thickness: 3 mm) via an adhesive layer. The center of the back surface of the glass plate (approximately 20 mm in diameter) was filled in with black marker to create a sample that was not reflective on the back surface of the glass plate. The sample was placed in an ellipsometer (VASE, manufactured by J.A. Woollam Japan) and the refractive index was measured at a wavelength of 500 nm and an incident angle of 50 to 80 degrees. (6) Refractive Index of Other Components The refractive index of components other than the low refractive index layer was measured using a Metricon Prism Coupler "Model 2010 / M."

[0128] [Production Example 1: Diffusion Film A] (Preparation of emulsion coating liquid) 34.1 parts of a non-polymerizable liquid crystal compound (manufactured by JNC Corporation, product name "JC-5240XX", birefringence Δn=0.252 (ne=1.766, no=1.514), viscosity=75 mPa s), 3.8 parts of a polymerizable liquid crystal compound (manufactured by BASF Corporation, product name "PALIOCOLOR LC-242"), 0.1 parts of a photopolymerization initiator (manufactured by IGM, product name "OMNIRAD651"), 60.0 parts of pure water, and 2.0 parts of a dispersant (manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., "Noigen ET159") were mixed and homogenized using an ultrasonic homogenizer (Hielscher The mixture was irradiated with ultrasonic waves at a frequency of 24 kHz for 1 minute using an ultrasonic wave emitting device (UP-200S, manufactured by Ultrasonics Corporation) to prepare a liquid crystal emulsion. The average particle size of the liquid crystal particles in the obtained liquid crystal emulsion was 0.8 μm. An emulsion coating liquid was obtained by mixing 19.03 parts of the liquid crystal emulsion, 9.16 parts of a polyether-based polyurethane resin aqueous dispersion (manufactured by DSM, trade name "NeoRez R967", polymer average particle size: 80 nm, solid content: 40 wt%), 8.12 parts of a polyester-based polyurethane resin aqueous dispersion (manufactured by Sanyo Chemical Industries, Ltd., trade name "Eucoat C-102", polymer average particle size: 168 nm, solid content: 45 wt%), 0.38 parts of a leveling agent (manufactured by DIC Corporation, product name "F-444"), 1.23 parts of a crosslinking agent (tris[3-(2-methylaziridin-1-yl)propionic acid]=propylidinetrimethyl), and 62.0 parts of pure water.

[0129] (Application and Drying of Emulsion Coating Liquid) The emulsion coating liquid was applied to one side of a PET film (thickness: 25 μm, refractive index: 1.49) as a first transparent substrate to form a coating layer with a thickness of 150 μm using a wire bar. The coating layer was then dried at 25° C. for 90 minutes to form a PDLC layer with a thickness of 46 μm.

[0130] (Lamination of second transparent substrate) A PET film (thickness 25 μm, refractive index 1.49) was laminated on the PDLC layer as a second transparent substrate using a laminator while applying a lamination pressure of 0.4 MPa / m. This resulted in a laminate having a configuration of [first transparent substrate / PDLC layer / second transparent substrate]. The resulting laminate exhibited a uniform haze (haze: 99%) across the entire main surface.

[0131] (UV irradiation) A flat metal electrode having a recess of 2 mm depth on its upper surface was used as the first electrode. The recesses were arranged to correspond to the point light sources in the light source unit described below. The laminate was placed so that the first transparent substrate was in contact with the upper surface of the first electrode, and an ITO-coated glass substrate was placed thereon as the second electrode so that the ITO surface was in contact with the second transparent substrate. Next, a high-voltage power supply was used to apply a voltage of 1.3 kV to these electrodes, while irradiating the electrodes with 20 mW / cm under a UV-LED lamp (manufactured by Hamamatsu Photonics, product name "C11924-101", peak wavelength 365 nm). 2 The film was then exposed to light at 25°C for 3 minutes. This polymerized the polymerizable liquid crystal compound, resulting in a diffusion film A having a structure of [first transparent substrate / diffusion layer / second transparent substrate]. The refractive index of the polymer matrix of the diffusion layer was 1.49 to 1.58.

[0132] The haze of the resulting diffusion film A was measured, and the haze was 99% in the region (region I) corresponding to the recesses of the first electrode, and 37% in the region (region II) corresponding to the areas other than the recesses of the first electrode. This indicates that the orientation state of the liquid crystal polymer and liquid crystal compound in the dispersed particles in region I of the diffusion layer is different from the orientation state of the liquid crystal polymer and liquid crystal compound in the dispersed particles in region II, and more specifically, the degree of orientation of the liquid crystal polymer and liquid crystal compound in the dispersed particles in region I is lower than the degree of orientation of these in region II.

[0133] [Production Example 2: Low Refractive Index Layer A] A low refractive index layer was formed on the surface of an acrylic film (manufactured by Toyo Kohan Co., Ltd., product name "RX-30NC", thickness: 30 μm) as follows. 0.5 g of a 0.01 mol / L aqueous oxalic acid solution was added to a mixed solution prepared by dissolving 0.95 g of methyltrimethoxysilane (MTMS), a precursor of a silicon compound, in 2.2 g of dimethyl sulfoxide (DMSO), and the mixture was stirred at room temperature for 30 minutes to hydrolyze MTMS and produce tris(hydroxy)methylsilane. Subsequently, 0.38 g of 28% aqueous ammonia and 0.2 g of pure water were added to 5.5 g of DMSO, and the hydrolyzed mixed solution was further added and stirred at room temperature for 15 minutes to gel the tris(hydroxy)methylsilane and obtain a gel-like silicon compound. The mixed solution subjected to the gelation treatment was then incubated at 40°C for 20 hours to undergo an aging treatment. Next, the aged gel-like silicon compound was crushed into granules of several mm to several cm in size using a spatula. 40 g of isopropyl alcohol (IPA) was added thereto, and after light stirring, the mixture was left to stand at room temperature for 6 hours, and the solvent and catalyst in the gel were decanted. The same decantation process was repeated three times to complete the solvent substitution. Then, the gel-like silicon compound in the mixed solution was crushed. The crushing process was carried out using a homogenizer (trade name "UH-50", manufactured by SMT Co., Ltd.) with a 5 cm 31.18 g of gel and 1.14 g of IPA were weighed into a screw bottle and then milled for 2 minutes at 50 W and 20 kHz. The milling process pulverized the gel-like silicon compound in the mixed solution, resulting in the mixed solution becoming a sol solution of the pulverized material. The volume average particle diameter, which indicates the particle size variation of the pulverized material contained in the mixed solution, was confirmed to be 0.5 μm to 0.7 μm. Furthermore, a 0.3 wt % KOH aqueous solution was prepared, and 0.02 g of KOH was added to 0.5 g of the sol solution to prepare a coating solution. A 40 nm thick film of a silane coupling agent (manufactured by Shin-Etsu Silicones Co., Ltd., product name "KBM-403") was formed on the acrylic film surface, and the coating solution was further spray-coated onto the acrylic film and dried at 80°C for 1 minute, yielding a laminate A consisting of an acrylic film and a low refractive index layer A. The film thickness and refractive index of the low refractive index layer A were evaluated, revealing a film thickness of 1000 nm and a refractive index of 1.20.

[0134] Example 1 A light source layer including a light source unit and a silicone resin layer sealing the light source unit was removed from a liquid crystal display device (Apple iPad Pro (registered trademark) 12.9-inch (5th generation)) and used as light source layer A. The light source unit was composed of mini-LEDs arranged two-dimensionally in 119 rows and 88 columns. The refractive index of the silicone resin layer was 1.43. A PET film (manufactured by Toray Industries, Inc., product name "Lumirror S10", thickness 25 μm) was laminated on light source layer A without an adhesive layer, and a diffusion film A was further laminated on top of that without an adhesive layer to form an air layer between the PET film and the diffusion film A. This resulted in a light diffusion device having a configuration of [light source layer A / PET film / air layer / diffusion film A]. In the obtained light diffusion device, region I of the diffusion film corresponded to the arrangement positions of each LED in a planar view.

[0135] Example 2 A diffusion film A was laminated on the low refractive index layer A side of the laminate A obtained in Production Example 2 via an acrylic adhesive (thickness 10 μm), to obtain a laminate B having a configuration of [acrylic film / low refractive index layer A / adhesive layer / diffusion film A]. The laminate B was laminated on the same light source layer A as in Example 1 without an adhesive layer, so that the acrylic film was on the light source layer A side. This resulted in a light diffusion device having a configuration of [light source layer A / acrylic film / low refractive index layer A / adhesive layer / diffusion film A]. In the obtained light diffusion device, region I of the diffusion film corresponded to the arrangement positions of each LED in a planar view.

[0136] Example 3 Resin particles with a uniform particle size (product name "Micropearl SP-220" manufactured by Sekisui Chemical Co., Ltd., particle size 20 μm) were placed on the light source layer A without using an adhesive, and a diffusion film A was further laminated on top of them without an adhesive layer. This formed a low refractive index layer (air layer) between the light source layer A and the diffusion film A. One layer of resin particles was randomly laminated on the light source layer A, and the area occupied by the resin particles on the light source layer A when observed from the direction perpendicular to the surface was 20%. This resulted in a light diffusion device having a configuration of [light source layer A / resin particles+air layer / diffusion film A]. In the obtained light diffusion device, region I of the diffusion film corresponded to the arrangement positions of each LED in a planar view.

[0137] Comparative Example 1 The same light source layer A as in Example 1 was used as a light diffusing device.

[0138] [Comparative Example 2] A diffusion film A was laminated on the same light source layer A as in Example 1 without an adhesive layer. This resulted in a light diffusion device having a configuration of [light source layer A / diffusion film A]. The diffusion film A was in close contact with the light source layer A, and no air layer was formed at the interface between them. In the obtained light diffusion device, region I of the diffusion film corresponded to the arrangement positions of each LED in a planar view.

[0139] Reference Example 1 A diffusion film B (a surface-type diffusion film having prisms on its surface, thickness 132 μm) was laminated on the same light source layer A as in Example 1 without an adhesive layer, with the prism-shaped surface facing the light source layer A. This resulted in a light diffusion device having a configuration of [light source layer A / diffusion film B].

[0140] Reference Example 2 A PET film (manufactured by Toray Industries, Inc., product name "Lumirror S10", thickness 25 μm) was laminated on the same light source layer A as in Example 1 without an adhesive layer. Next, a diffusion film B was laminated on the PET film without an adhesive layer so that the surface having the prism shape faced the light source layer A. This resulted in a light diffusion device having a configuration of [light source layer A / PET film / diffusion film B].

[0141] The light diffusers obtained in the above Examples, Comparative Examples, and Reference Examples were turned on, and the in-plane luminance uniformity was evaluated as follows. The results are shown in Table 1. <In-plane luminance uniformity> The luminance of the diffusion film side surface of the light diffuser was measured with a 2D spectroradiometer (SR-5000HS, manufactured by Topcon Technohouse) at a resolution of 0.2 mm x 0.2 mm, and the in-plane luminance uniformity was calculated by substituting the maximum luminance (Lmax) and minimum luminance (Lmin) into the following formula: In-plane luminance uniformity (%) = [1 - (Lmax - Lmin) / (Lmax + Lmin)] x 100

[0142] A comparison between the Examples and Comparative Examples reveals that the uniformity of in-plane luminance is significantly improved by placing a low-refractive index layer with a lower refractive index than the light source layer between the light source layer and the diffusion film. On the other hand, this effect is not achieved in the Reference Example. This is thought to be because, in the surface-type diffusion film, the adhesion between the diffusion film and the light source layer is low, and sufficient interfacial reflection occurs even in the absence of a low-refractive index layer.

[0143] The light diffusing device of the present invention is suitably used in display devices such as liquid crystal display devices.

[0144] REFERENCE SIGNS LIST 10 light source layer 12 light source section 14 sealing resin layer 20 first diffusion film 22 diffusion layer 22a polymer matrix 22b dispersed particles 30 first low refractive index layer 40 second low refractive index layer 50 second diffusion film 100 light diffusion device 200 liquid crystal display device

Claims

1. A light diffusion device comprising, in this order, a light source layer including a light source unit and a sealing resin layer that seals the light source unit, a first low refractive index layer having a refractive index lower than that of the sealing resin layer, and a first diffusion film including a diffusion layer, wherein the diffusion layer comprises a polymer matrix and dispersed particles dispersed in the polymer matrix, the dispersed particles including at least one type selected from a liquid crystal compound and a liquid crystal polymer.

2. The light diffusing device of claim 1, wherein the refractive index of said first low refractive index layer is lower than the refractive index of said first diffusion film.

3. The light diffusing device according to claim 1, wherein the first low refractive index layer is a layer including voids or an air layer.

4. The light diffusing device according to claim 1, wherein the sealing resin layer contains at least one resin selected from the group consisting of a silicone resin and an epoxy resin.

5. The light diffusing device of claim 1, wherein said first diffusing film further comprises a transparent substrate disposed on at least one side of said diffusing layer.

6. The light diffusing device according to claim 1, wherein the light source section includes a plurality of point light sources.

7. The light diffusing device of claim 1, wherein said dispersed particles include at least said liquid crystal polymer.

8. The light diffusing device according to claim 7, wherein the first diffusion film has a plurality of regions having different hazes when viewed in a plan view.

9. The light diffusing device of claim 8, wherein the plurality of regions are arranged in a predetermined pattern.

10. A light diffusing device as described in claim 1, wherein a second low refractive index layer and a second diffusion film are arranged in this order on the side of the first diffusion film opposite to the side on which the first low refractive index layer is arranged, the second diffusion film includes a diffusion layer including a polymer matrix and dispersed particles dispersed in the polymer matrix and including at least one type selected from a liquid crystal compound and a liquid crystal polymer, and the refractive index of the second low refractive index layer is lower than those of the first diffusion film and the second diffusion film.

11. A backlight device comprising a light diffusing device according to any one of claims 1 to 10.

12. An image display device comprising the backlight device according to claim 11 and a display element.

Citation Information

Patent Citations

  • Transparent panel having light emitting function

    JP2018197830A

  • Backlight unit with quantum dots

    JP2022530624A

  • Polymer dispersion type liquid crystal film and method for manufacturing polymer dispersion type liquid crystal film

    JP2023035529A