Composition for forming resist underlayer film, method for producing semiconductor substrate, and polymer for forming resist underlayer film

The composition of a polymer with aromatic rings and halogen atoms in the resist underlayer film addresses the challenges of solvent resistance and pattern rectangularity, enhancing the manufacturing of semiconductor substrates by promoting crosslinking and improving solubility differences during EUV exposure.

WO2024203153A1PCT designated stage expired Publication Date: 2024-10-03JSR CORPORATION
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008969
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-08
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

In the manufacturing of semiconductor devices, existing resist underlayer films struggle to provide sufficient solvent resistance and pattern rectangularity, especially with the trend towards shorter exposure wavelengths, leading to issues with pattern trailing and rectangularity during the etching process.

Method used

A composition comprising a polymer with specific repeating units and a solvent is used to form a resist underlayer film, which includes aromatic rings, halogen atoms, and urethane or ether bonds, enhancing solvent resistance and pattern rectangularity by promoting crosslinking and improving solubility differences during extreme ultraviolet exposure.

Benefits of technology

The solution effectively forms a resist underlayer film with excellent solvent resistance and pattern rectangularity, enabling efficient manufacturing of semiconductor substrates with improved pattern quality and reduced trailing, suitable for use in high-integration semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008969_03102024_PF_FP_ABST
    Figure JP2024008969_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is: a composition for forming a resist underlayer film, the composition being capable of forming a resist underlayer film that is excellent in terms of solvent resistance and pattern rectangularity; a method for producing a semiconductor substrate; and a polymer for forming a resist underlayer film. This composition for forming a resist underlayer film contains: a polymer that has a repeating unit represented by formula (1) or a repeating unit represented by formula (2); and a solvent. (In formula (1), Ar1 represents a divalent group that has an aromatic ring having 6 to 20 ring members. RA represents a substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms. In formula (2), Ar1 represents a divalent group that has an aromatic ring having 6 to 20 ring members. R1 and R3 each independently represent a substituted or unsubstituted trivalent hydrocarbon group having 1 to 20 carbon atoms. R2 and R4 each independently represent a hydroxy group or a monovalent organic group. L1 and L2 each independently represent a single bond or a divalent linking group. RB represents a divalent organic group having 1 to 20 carbon atoms.)
Need to check novelty before this filing date? Find Prior Art

Description

Composition for forming resist underlayer film, method for manufacturing semiconductor substrate, and polymer for forming resist underlayer film

[0001] The present invention relates to a composition for forming a resist underlayer film, a method for producing a semiconductor substrate, and a polymer for forming a resist underlayer film.

[0002] In the manufacture of semiconductor devices, for example, a multilayer resist process is used in which a resist pattern is formed by exposing and developing a resist film laminated on a substrate via a resist underlayer film such as an organic underlayer film or a silicon-containing film. In this process, the resist underlayer film is etched using the resist pattern as a mask, and the substrate is further etched using the resulting resist underlayer film pattern as a mask, thereby forming a desired pattern on the semiconductor substrate.

[0003] In recent years, the integration of semiconductor devices has become increasingly advanced, and the wavelength of the exposure light used has tended to be shortened from KrF excimer lasers (248 nm) and ArF excimer lasers (193 nm) to extreme ultraviolet light (13.5 nm, hereinafter also referred to as "EUV"). Various studies have been conducted on compositions for forming resist underlayer films (see International Publication No. 2021 / 157551).

[0004] See International Publication No. WO 2021 / 157551

[0005] The resist underlayer film is required to have solvent resistance to the solvent in the resist composition, and pattern rectangularity that prevents pattern footing at the bottom of the resist film and ensures rectangularity of the resist pattern.

[0006] The present invention has been made in light of the above circumstances, and an object of the present invention is to provide a composition for forming a resist underlayer film, a method for producing a semiconductor substrate, and a polymer for forming a resist underlayer film, which are capable of forming a resist underlayer film that is excellent in solvent resistance and pattern rectangularity.

[0007] In one embodiment, the present invention relates to a composition for forming a resist underlayer film, comprising: a polymer (hereinafter also referred to as “polymer [A]”) having a repeating unit represented by the following formula (1) (hereinafter also referred to as “repeating unit (1)”) or a repeating unit represented by the following formula (2) (hereinafter also referred to as “repeating unit (2)”); and a solvent (hereinafter also referred to as “solvent [B]”). (In formula (1), Ar 1 is a divalent group having an aromatic ring with 6 to 20 ring members. A is a substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms. 1 is a divalent group having an aromatic ring with 6 to 20 ring members. 1 and R 3 are each independently a substituted or unsubstituted trivalent hydrocarbon group having 1 to 20 carbon atoms. 2 and R 4 are each independently a hydroxy group or a monovalent organic group. 1 and L 2 are each independently a single bond or a divalent linking group. B is a divalent organic group having 1 to 20 carbon atoms.

[0008] In another embodiment, the present invention provides a method for producing a semiconductor substrate, comprising: a step of applying a composition for forming a resist underlayer film directly or indirectly to a substrate; a step of applying a composition for forming a resist film to the resist underlayer film formed in the step of applying the composition for forming a resist film; a step of exposing the resist film formed in the step of applying the composition for forming a resist film to radiation; and a step of developing at least the exposed resist film, wherein the composition for forming a resist underlayer film comprises: a polymer having a repeating unit represented by the following formula (1) or a repeating unit represented by the following formula (2); and a solvent. (In formula (1), Ar 1 is a divalent group having an aromatic ring with 6 to 20 ring members. A is a divalent organic group. 1 is a divalent group having an aromatic ring with 6 to 20 ring members. 1 and R3 are each independently a substituted or unsubstituted trivalent hydrocarbon group having 1 to 20 carbon atoms. 2 and R 4 are each independently a hydroxy group or a monovalent organic group. 1 and L 2 are each independently a single bond or a divalent linking group. B is a divalent organic group.

[0009] In yet another embodiment, the present invention relates to a polymer for forming a resist underlayer film, obtained by reacting a compound represented by the following formula (α) with a compound represented by the following formula (β1) or a compound represented by the following formula (β2): (In formula (α), Ar 1 is a divalent group having an aromatic ring with 6 to 20 ring members. A is a substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms. 1a and R 3a R are each independently a monovalent group having an epoxy structure or an oxetane structure. B is a divalent organic group having 1 to 20 carbon atoms.

[0010] In this specification, the term "number of ring members" refers to the number of atoms constituting the ring. For example, a biphenyl ring has 12 ring members, a naphthalene ring has 10 ring members, and a fluorene ring has 13 ring members. Furthermore, the term "organic group" refers to a group having at least one carbon atom.

[0011] The composition for forming a resist underlayer film can form a film having excellent solvent resistance and pattern rectangularity. The method for producing a semiconductor substrate uses a composition for forming a resist underlayer film that can form a resist underlayer film having excellent solvent resistance and pattern rectangularity, allowing for efficient production of semiconductor substrates. The polymer for forming a resist underlayer film is suitable for use in a composition for forming a resist underlayer film. Therefore, these can be suitably used in the production of semiconductor devices, etc.

[0012] The composition for forming a resist underlayer film, the method for producing a semiconductor substrate, and the polymer for forming a resist underlayer film according to each embodiment of the present invention will be described in detail below. Combinations of preferred aspects in the embodiments are also preferred.

[0013] <<Composition for forming a resist underlayer film>> The composition for forming a resist underlayer film (hereinafter also referred to as the “composition”) contains a polymer (A) and a solvent (B). The composition may contain optional components as long as the effects of the present invention are not impaired.

[0014] The composition is suitable as a composition for forming an underlayer film of a resist film to be exposed to extreme ultraviolet rays. Examples of resist film-forming compositions include positive- or negative-type chemically amplified resist compositions containing a radiation-sensitive acid generator, positive-type resist compositions containing an alkali-soluble resin and a quinone diazide photosensitizer, negative-type resist compositions containing an alkali-soluble resin and a crosslinker, and metal-containing resist compositions containing metals such as tin, zirconium, and hafnium. The underlayer film formed using the composition contains a polymer [A] containing multiple aromatic rings in its main chain. Therefore, in the development step after exposure to extreme ultraviolet rays, the organic resist film or metal-containing resist film has sufficient developer solubility in the interface region on the underlayer film side, suppressing pattern tailing at the bottom of the resist film and ensuring rectangularity of the resist pattern. Furthermore, the underlayer film formed using the composition contains a polymer [A] also containing a urethane bond or an ether bond, ensuring solvent resistance to the solvent of the resist composition. The lower limit of the content of the metal or metal compound in the components other than the solvent in the metal-containing resist composition is preferably 50 mass %, more preferably 70 mass %, even more preferably 80 mass %, and particularly preferably 85 mass %. The upper limit of the content is, for example, 100 mass % or 95 mass %.

[0015] Each component contained in the composition will be described below.

[0016] <Polymer [A]> The polymer [A] has the repeating unit (1) or repeating unit (2). The polymer [A] can contain one or more types of repeating unit (1) or repeating unit (2). The composition may contain a combination of the polymer [A] having the repeating unit (1) and the polymer [A] having the repeating unit (2). The polymer [A] may have a repeating unit other than the repeating unit (1) and the repeating unit (2). The composition may contain one or more types of the polymer [A].

[0017] The polymer [A] preferably has at least one halogen atom per repeating unit, and more preferably has two, three, or four halogen atoms. Examples of halogen atoms include fluorine, chlorine, bromine, and iodine atoms. Among these, fluorine and iodine atoms are preferred, and iodine atoms are more preferred. This can increase the efficiency of secondary electron generation due to absorption of extreme ultraviolet rays, and can create a sufficient solubility difference in the interface region of the organic resist film on the underlayer film side during exposure to extreme ultraviolet rays, or can promote insolubilization of the metal-containing resist film. As a result, footing of the pattern at the bottom of the resist film can be suppressed, thereby ensuring the rectangularity of the resist pattern.

[0018] Hereinafter, the case where the polymer [A] has the repeating unit (1) will be described as a first embodiment, and the case where the polymer [A] has the repeating unit (2) will be described as a second embodiment.

[0019] [First embodiment] The polymer [A] has the repeating unit (1) described above.

[0020] (Repeating Unit (1)) The repeating unit (1) is represented by the following formula (1). (In formula (1), Ar 1 is a divalent group having an aromatic ring with 6 to 20 ring members. A is a substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms.

[0021] In the above formula (1), Ar 1Examples of the aromatic ring having 6 to 20 ring members in Ar include aromatic hydrocarbon rings such as a benzene ring, a naphthalene ring, an anthracene ring, an indene ring, a pyrene ring, and a fluorene ring, aromatic heterocyclic rings such as a pyridine ring, a pyrazine ring, a pyrimidine ring, a pyridazine ring, and a triazine ring, and combinations thereof. 1 The aromatic ring is preferably an aromatic hydrocarbon ring, more preferably a benzene ring, a fluorene ring or a combination thereof.

[0022] In the above formula (1), Ar 1 As the divalent group having an aromatic ring with 6 to 20 ring members represented by the formula 1 and a group (hereinafter also referred to as "group (iii)") formed by combining group (i) with a divalent linking group not containing an aromatic ring (hereinafter also referred to as "group (ii)").

[0023] Examples of the group (ii) include a divalent linear or branched chain hydrocarbon group having 1 to 20 carbon atoms; a divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms; a divalent heteroatom-containing linking group; a group having the divalent heteroatom-containing linking group between carbon atoms in a chain or alicyclic hydrocarbon group; or a group formed by combining two or more of these groups.

[0024] Examples of the divalent linear or branched hydrocarbon group having 1 to 20 carbon atoms include alkanediyl groups having 1 to 20 carbon atoms, such as methanediyl, ethanediyl, propanediyl, butanediyl, and hexanediyl groups; alkenediyl groups having 2 to 20 carbon atoms, such as ethenediyl and propenediyl groups; and alkynediyl groups having 2 to 20 carbon atoms, such as ethynediyl and propynediyl groups. Of these, alkanediyl groups having 1 to 5 carbon atoms are preferred.

[0025] Examples of the divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms include monocyclic cycloalkanediyl groups such as cyclopentanediyl and cyclohexanediyl groups, and polycyclic cycloalkanediyl groups such as norbornanediyl and adamantanediyl groups. Of these, cycloalkanediyl groups having 5 to 12 carbon atoms are preferred.

[0026] Examples of the divalent heteroatom-containing linking group include —CO—, —CS—, —NR′—, —O—, —S—, and —SO 2 - or a group combining these, etc. R' is a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms.

[0027] In the above formula (1), Ar 1 is preferably a divalent group having an aromatic ring having 6 to 20 ring members substituted with at least one halogen atom. 1 The number of halogen atoms in is preferably 2, 3, or 4. Examples of halogen atoms include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms. Among these, iodine atoms are preferred as halogen atoms. This can further increase the efficiency of secondary electron generation due to absorption of extreme ultraviolet rays, suppress pattern footing at the bottom of the resist film, and improve the rectangularity of the resist pattern. When multiple halogen atoms are present, the multiple halogen atoms may be present on the same aromatic ring or on different aromatic rings.

[0028] Ar 1 Examples of the substituent that the divalent group represented by the formula (I) may have include, in addition to the above-mentioned halogen atoms, monovalent chain hydrocarbon groups having 1 to 10 carbon atoms; alkoxy groups such as a methoxy group, an ethoxy group, and a propoxy group; alkoxycarbonyl groups such as a methoxycarbonyl group and an ethoxycarbonyl group; alkoxycarbonyloxy groups such as a methoxycarbonyloxy group and an ethoxycarbonyloxy group; acyl groups such as a formyl group, an acetyl group, a propionyl group, and a butyryl group; a hydroxy group, a cyano group, a nitro group, an amino group, a sulfanyl group, and a carboxy group.

[0029] In the above formula (1), R A Examples of the substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms represented by the formula (I) include a divalent linear or branched chain hydrocarbon group having 1 to 20 carbon atoms; a divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms; and a divalent aromatic hydrocarbon group having 6 to 20 carbon atoms, or a combination thereof.

[0030] R AAs the divalent linear or branched chain hydrocarbon group having 1 to 20 carbon atoms in the above group (ii), the above divalent linear or branched hydrocarbon group having 1 to 20 carbon atoms and the like can be suitably used.

[0031] R A As the divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms in the above group (ii), the above divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms can be suitably used.

[0032] R A As the divalent aromatic hydrocarbon group having 6 to 20 carbon atoms in the formula (1), a group corresponding to the aromatic hydrocarbon among the above groups (i) can be suitably used.

[0033] In formula (1), R A Preferably, R contains a substituted or unsubstituted divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms or a substituted or unsubstituted divalent aromatic hydrocarbon group having 6 to 20 carbon atoms. A As the divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms in R, a cycloalkanediyl group having 5 to 12 carbon atoms is preferred, and a cyclopentanediyl group or a cyclohexanediyl group is more preferred. A In the formula (I), the divalent aromatic hydrocarbon group having 6 to 20 carbon atoms is preferably a benzenediyl group.

[0034] R A When has a substituent, the substituent is Ar 1 The substituents that may be possessed by the group can be suitably employed.

[0035] Specific examples of the repeating unit (1) include repeating units represented by the following formulas (1-1) to (1-18).

[0036]

[0037]

[0038]

[0039] (Other Repeating Units) Examples of other repeating units include a repeating unit represented by the following formula (3) (hereinafter also referred to as "repeating unit (3)"). (In formula (3), R C is a divalent organic group having 1 to 20 carbon atoms and no aromatic ring.

[0040] R C As the divalent organic group having 1 to 20 carbon atoms and no aromatic ring, Ar in the above formula (1) 1 The group (ii) in the following formula can be preferably employed. C As the alkyl group, a divalent linear or branched chain hydrocarbon group having 1 to 20 carbon atoms or a combination thereof with a divalent heteroatom-containing linking group is preferred.

[0041] Specific examples of the repeating unit (3) include repeating units represented by the following formulas (3-1) to (3-6).

[0042]

[0043] (Method for Producing Polymer [A] Having Repeating Unit (1)) The method for producing the polymer [A] having the repeating unit (1) is not particularly limited. Typically, the polymer [A] having the repeating unit (1) can be obtained by reacting (polyaddition) a compound represented by the following formula (α) (hereinafter also referred to as "compound (α)") with a compound represented by the following formula (β1) (hereinafter also referred to as "compound (β1)"): (In formula (α) and formula (β1), Ar 1 and R A has the same meaning as the above formula (1).

[0044] The lower limit of the molar ratio ((α) / (β1)) of the number of moles of compound (α) to the number of moles of compound (β1) is preferably 0.1, more preferably 0.5. The upper limit of the molar ratio ((α) / (β1)) is preferably 0.9, more preferably 0.5.

[0045] Furthermore, when the polymer (A) has the repeating unit (3), the compound (α), the compound (β1), and a compound represented by the following formula (γ) (hereinafter also referred to as “compound (γ)”) may be subjected to a polyaddition reaction: (In formula (γ), RC is the same as the above formula (3).

[0046] When compound (γ) is used, the content of compound (γ) should be such that the ratio of the total number of moles of compound (α) and compound (γ) to the number of moles of compound (β1) ({(α)+(γ)} / (β1)) satisfies the above range of molar ratio ((α) / (β1)).

[0047] As the reaction solvent, the solvent [B] described below can be used. The lower limit of the reaction temperature is preferably 40°C, more preferably 60°C. The upper limit of the reaction temperature is preferably 140°C, more preferably 100°C. The lower limit of the reaction time is preferably 1 hour, more preferably 4 hours. The upper limit of the reaction time is preferably 24 hours, more preferably 12 hours. After the reaction, the polymer [A] can be obtained through separation, purification, drying, etc.

[0048] Specific examples of the compound (α) include compounds represented by the following formulae (α-1) to (α-11).

[0049]

[0050] Specific examples of the compound (β1) include compounds represented by the following formulae (β1-1) to (β1-9).

[0051]

[0052] Specific examples of the compound (γ) include compounds represented by the following formulas (γ-1) to (γ-6).

[0053]

[0054] [Second embodiment] The polymer (A) has the repeating unit (2) described above.

[0055] (Repeating Unit (2)) The repeating unit (2) is represented by the following formula (2). (In formula (2), Ar 1 is a divalent group having an aromatic ring with 6 to 20 ring members. 1 and R 3are each independently a substituted or unsubstituted trivalent hydrocarbon group having 1 to 20 carbon atoms. 2 and R 4 are each independently a hydroxy group or a monovalent organic group. 1 and L 2 are each independently a single bond or a divalent linking group. B is a divalent organic group having 1 to 20 carbon atoms.

[0056] In the above formula (2), Ar 1 As the Ar in the above formula (1), 1 can be suitably adopted.

[0057] R 1 and R 3 The trivalent hydrocarbon group having 1 to 20 carbon atoms represented by the formula (1) is A A group in which one hydrogen atom has been removed from a divalent hydrocarbon group having 1 to 20 carbon atoms, represented by the following formula: 1 and R 3 are each preferably independently a substituted or unsubstituted trivalent chain hydrocarbon group having 1 to 20 carbon atoms or a substituted or unsubstituted trivalent alicyclic hydrocarbon group having 3 to 20 carbon atoms. 1 and R 3 are each independently preferably an alkanetriyl group having 3 to 8 carbon atoms or a cycloalkanetriyl group having 5 to 10 carbon atoms, more preferably a propanetriyl group, a butanetriyl group or a cyclohexanetriyl group.

[0058] R 2 and R 4 Examples of the monovalent organic group represented by the formula (I) include a monovalent hydrocarbon group having 1 to 20 carbon atoms, a group having a divalent heteroatom-containing linking group between the carbon atoms of this hydrocarbon group, a group in which some or all of the hydrogen atoms of the hydrocarbon group have been substituted with substituents, or a combination thereof. The organic group is a group having at least one carbon atom.

[0059] R 2 and R 4In the formula (I), examples of the monovalent hydrocarbon group having 1 to 20 carbon atoms include a monovalent chain hydrocarbon group having 1 to 20 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms, and combinations thereof.

[0060] Examples of the monovalent chain hydrocarbon group having 1 to 20 carbon atoms include alkyl groups such as methyl, ethyl, n-propyl, i-propyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, and neopentyl; alkenyl groups such as ethenyl, propenyl, and butenyl; and alkynyl groups such as ethynyl, propynyl, and butynyl.

[0061] Examples of the monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms include cycloalkyl groups such as a cyclopentyl group and a cyclohexyl group; cycloalkenyl groups such as a cyclopropenyl group, a cyclopentenyl group and a cyclohexenyl group; bridged ring saturated hydrocarbon groups such as a norbornyl group, an adamantyl group and a tricyclodecyl group; and bridged ring unsaturated hydrocarbon groups such as a norbornenyl group and a tricyclodecenyl group.

[0062] Examples of the monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms include a phenyl group, a tolyl group, a naphthyl group, an anthracenyl group, and a pyrenyl group.

[0063] R 2 and R 4 As the divalent heteroatom-containing linking group in the formula (1), Ar 1 The divalent heteroatom-containing group shown as group (ii) in the above formula can be suitably employed.

[0064] R 2 and R 4 When has a substituent, the substituent is Ar 1 The substituents that may be possessed by the group can be suitably employed.

[0065] In the above formula (2), R 2 and R 4each independently has a group containing at least one group selected from the group consisting of a hydroxy group, a group represented by the following formula (2-1), and a group represented by the following formula (2-2): (In formulas (2-1) and (2-2), R 7 are each independently a divalent organic group having 1 to 20 carbon atoms or a single bond. * is R 2 and R 4 is the bond to the atoms that make up the atom.)

[0066] In the above formula (2-1) and formula (2-2), R 7 The divalent organic group having 1 to 20 carbon atoms represented by the formula (2) is R 2 and R 4 A group in which one hydrogen atom has been removed from a monovalent organic group represented by the following formula can be suitably used.

[0067] R 7 As the alkyl group, a divalent hydrocarbon group having 1 to 10 carbon atoms is preferred, and a methanediyl group, an ethanediyl group, a propanediyl group, a benzenediyl group, or a combination thereof is more preferred.

[0068] L 1 and L 2 The divalent linking group represented by the formula (1) is Ar 1 Among these, groups (i), (ii) and (iii) in the formula (1) can be preferably used. 1 and L 2 is preferably a single bond or —O—.

[0069] R B As the divalent organic group having 1 to 20 carbon atoms represented by the formula (1), Ar 1 Among these, groups (i), (ii) and (iii) in the formula (1) can be preferably used. BAs the alkyl group, a group in which two hydrogen atoms have been removed from an aromatic hydrocarbon ring having 6 to 20 carbon atoms, a divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, a divalent linear or branched chain hydrocarbon group having 1 to 20 carbon atoms, or a combination of any of these with a divalent heteroatom-containing linking group is preferred, and an arenediyl group having 6 to 12 carbon atoms, a cycloalkanediyl group having 5 to 12 carbon atoms, a linear or branched alkanediyl group having 1 to 10 carbon atoms, or a combination of any of these with a divalent heteroatom-containing linking group is more preferred.

[0070] Specific examples of the repeating unit (2) include repeating units represented by the following formulas (2-1) to (2-15).

[0071]

[0072]

[0073]

[0074] (Other Repeating Units) Examples of the other repeating units include the repeating unit (3) described above.

[0075] (Method for Producing Polymer [A] Having Repeating Unit (2)) The method for producing the polymer [A] having the repeating unit (2) is not particularly limited. Typically, the polymer [A] having the repeating unit (2) can be obtained by reacting (polyaddition) a compound represented by the following formula (α) (i.e., the above-mentioned compound (α)) with a compound represented by the following formula (β2) (hereinafter, also referred to as "compound (β2)"). (In formula (α) and formula (β2), Ar 1 and R B has the same meaning as in formula (2). 1a and R 3a are each independently a monovalent group having an epoxy structure or an oxetane structure.

[0076] In the above formula (β2), R 1a and R 3aThe monovalent group having an epoxy structure or an oxetane structure represented by the formula (2) is a monovalent group having an epoxy structure or an oxetane structure represented by the formula (2) when the epoxy structure or the oxetane structure is ring-opened by an addition reaction between the hydroxy group of the compound (α) and the epoxy structure or the oxetane structure of the compound (β2). 1 -L 1 -R 2 Part and R 3 -L 2 -R 4 There are no particular limitations as long as the structure of the R moiety can be obtained. 1a and R 3a As the substituent, a glycidyl group, a glycidylmethyl group, an oxetanylmethyl group, an oxetanylethyl group, a 3,4-epoxycyclohexylmethyl group, a 3,4-epoxycyclohexylethyl group, and groups obtained by substituting these groups with a substituent are preferred. 1 The substituents that may be possessed by the group can be suitably employed.

[0077] The lower limit of the molar ratio ((α) / (β2)) of the number of moles of compound (α) to the number of moles of compound (β2) is preferably 0.1, more preferably 0.5. The upper limit of the molar ratio ((α) / (β2)) is preferably 0.9, more preferably 0.5.

[0078] Furthermore, when the polymer [A] has the repeating unit (3), the compound (α), the compound (β2), and the compound (γ) may be subjected to a polyaddition reaction. The method for introducing a group containing at least one group selected from the group consisting of the group represented by the formula (2-1) and the group represented by the formula (2-2) is not particularly limited, and a method of reacting a hydroxy group generated upon ring-opening of the epoxy structure or oxetane structure with a halide containing at least one group selected from the group consisting of the group represented by the formula (2-1) and the group represented by the formula (2-2) can be suitably employed.

[0079] When compound (γ) is used, the content of compound (γ) should be such that the ratio of the total number of moles of compound (α) and compound (γ) to the number of moles of compound (β2) ({(α) + (γ)} / (β2)) satisfies the above range of molar ratio ((α) / (β2)).

[0080] The reaction solvent, reaction temperature, and reaction time may be suitably selected from the conditions for producing the polymer (A) of the first embodiment.

[0081] Specific examples of the compound (β2) include compounds represented by the following formulae (β2-1) to (β2-8).

[0082]

[0083] <Solvent (B)> The solvent (B) is not particularly limited as long as it can dissolve or disperse the polymer (A) and any optional components contained as needed.

[0084] Examples of the solvent (B) include hydrocarbon solvents, ester solvents, alcohol solvents, ketone solvents, ether solvents, nitrogen-containing solvents, etc. The solvent (B) can be used alone or in combination of two or more.

[0085] Examples of hydrocarbon solvents include aliphatic hydrocarbon solvents such as n-pentane, n-hexane, and cyclohexane, and aromatic hydrocarbon solvents such as benzene, toluene, and xylene.

[0086] Examples of ester-based solvents include carbonate-based solvents such as diethyl carbonate, acetate monoester-based solvents such as methyl acetate and ethyl acetate, lactone-based solvents such as γ-butyrolactone, polyhydric alcohol partial ether carboxylate-based solvents such as diethylene glycol monomethyl ether acetate and propylene glycol monomethyl ether acetate, and lactate-based solvents such as methyl lactate and ethyl lactate.

[0087] Examples of alcohol solvents include monoalcohol solvents such as methanol, ethanol, n-propanol, 4-methyl-2-pentanol, and 2,2-dimethyl-1-propanol, and polyalcohol solvents such as ethylene glycol and 1,2-propylene glycol.

[0088] Examples of the ketone solvent include chain ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, and 2-heptanone, and cyclic ketone solvents such as cyclohexanone.

[0089] Examples of the ether solvent include chain ether solvents such as n-butyl ether, polyhydric alcohol ether solvents such as cyclic ether solvents such as tetrahydrofuran, and polyhydric alcohol partial ether solvents such as diethylene glycol monomethyl ether and propylene glycol monomethyl ether.

[0090] Examples of nitrogen-containing solvents include chain nitrogen-containing solvents such as N,N-dimethylacetamide, and cyclic nitrogen-containing solvents such as N-methylpyrrolidone.

[0091] The solvent (B) is preferably a ketone solvent, an ether solvent, or an ester solvent, more preferably a cyclic ketone solvent, a polyhydric alcohol partial ether solvent, or a polyhydric alcohol partial ether carboxylate solvent, and still more preferably cyclohexanone, propylene glycol monomethyl ether, or propylene glycol monomethyl ether acetate.

[0092] [Optional Components] The composition for forming a resist underlayer film may contain optional components within a range that does not impair the effects of the present invention. Examples of optional components include a crosslinking agent, an acid generator, a dehydrating agent, an acid diffusion controller, a surfactant, etc. The optional components may be used alone or in combination of two or more. The content of the optional components relative to the total mass of the polymer [A] and the optional components is preferably 30 mass% or less, and more preferably 20 mass% or less.

[0093] [Method for preparing a composition for forming a resist underlayer film] The composition for forming a resist underlayer film can be prepared by mixing the polymer [A], the solvent [B], and, if necessary, any optional components in a predetermined ratio, and preferably filtering the resulting mixture through a membrane filter or the like having a pore size of 0.5 μm or less.

[0094] <<Method for Manufacturing Semiconductor Substrate>> The method for manufacturing a semiconductor substrate includes a step of applying a composition for forming a resist underlayer film directly or indirectly to a substrate (hereinafter also referred to as a “coating step (I)”), a step of applying a composition for forming a resist film to the resist underlayer film formed in the above-mentioned coating step of the composition for forming a resist film (hereinafter also referred to as a “coating step (II)”), a step of exposing the resist film formed in the above-mentioned coating step of the composition for forming a resist film to radiation (hereinafter also referred to as an “exposure step”), and a step of developing at least the exposed resist film (hereinafter also referred to as a “development step”).

[0095] According to the method for producing a semiconductor substrate, by using a predetermined composition for forming a resist underlayer film in the coating step (I), a resist underlayer film having excellent solvent resistance and pattern rectangularity can be formed, and therefore a semiconductor substrate having a good pattern shape can be produced.

[0096] It is preferable that the method for producing a semiconductor substrate further includes, before the coating step (II), a step of heating the resist underlayer film formed in the resist underlayer film-forming composition coating step at 200°C or higher (hereinafter also referred to as a "heating step").

[0097] The method for producing a semiconductor substrate may further include, as necessary, a step of forming a silicon-containing film directly or indirectly on the substrate (hereinafter also referred to as a "silicon-containing film-forming step") prior to the coating step (I).

[0098] Hereinafter, each step in the case where the heating step, which is a preferred step, and the silicon-containing film forming step, which is an optional step, are included will be described.

[0099] [Silicon-containing film forming step] In this step, which is carried out before the coating step (I), a silicon-containing film is formed directly or indirectly on a substrate.

[0100] Examples of the substrate include metal or semimetal substrates such as silicon substrates, aluminum substrates, nickel substrates, chromium substrates, molybdenum substrates, tungsten substrates, copper substrates, tantalum substrates, and titanium substrates, among which silicon substrates are preferred.The substrate may also be a substrate on which a silicon nitride film, an alumina film, a silicon dioxide film, a tantalum nitride film, a titanium nitride film, or the like is formed.

[0101] The silicon-containing film can be formed by coating a silicon-containing film-forming composition, chemical vapor deposition (CVD), atomic layer deposition (ALD), or the like. Examples of methods for forming a silicon-containing film by coating a silicon-containing film-forming composition include a method in which the silicon-containing film-forming composition is directly or indirectly applied to a substrate, and the resulting coating film is then cured by exposure and / or heating. Examples of commercially available silicon-containing film-forming compositions include "NFC SOG01," "NFC SOG04," and "NFC SOG080" (all from JSR Corporation). Silicon oxide films, silicon nitride films, silicon oxynitride films, and amorphous silicon films can be formed by chemical vapor deposition (CVD) or atomic layer deposition (ALD).

[0102] Examples of radiation used for the exposure include electromagnetic waves such as visible light, ultraviolet light, far ultraviolet light, X-rays and gamma rays, and particle beams such as electron beams, molecular beams and ion beams.

[0103] The lower limit of the temperature when heating the coating film is preferably 90° C., more preferably 150° C., and still more preferably 200° C. The upper limit of the temperature is preferably 550° C., more preferably 450° C., and still more preferably 300° C.

[0104] The lower limit of the average thickness of the silicon-containing film is preferably 1 nm, more preferably 10 nm, and even more preferably 15 nm. The upper limit is preferably 20,000 nm, more preferably 1,000 nm, and even more preferably 100 nm. The average thickness of the silicon-containing film can be measured in the same manner as the average thickness of the resist underlayer film.

[0105] Examples of cases in which a silicon-containing film is formed indirectly on a substrate include cases in which a silicon-containing film is formed on a low dielectric insulating film or an organic underlayer film formed on a substrate.

[0106] [Coating step (I)] In this step, the resist underlayer film-forming composition is coated on the silicon-containing film formed on the substrate.The coating method of the resist underlayer film-forming composition is not particularly limited, and can be carried out by any suitable method such as spin coating, casting coating, roll coating, etc.This forms a coating film, and the resist underlayer film is formed by the evaporation of the solvent [B].

[0107] The lower limit of the average thickness of the resist underlayer film formed is preferably 0.5 nm, more preferably 1 nm, and even more preferably 2 nm. The upper limit of the average thickness is preferably 50 nm, more preferably 20 nm, even more preferably 10 nm, and particularly preferably 7 nm. The average thickness is measured according to the method described in the Examples.

[0108] When the composition for forming a resist underlayer film is applied directly to the substrate, the silicon-containing film forming step may be omitted.

[0109] [Heating Step] Next, the resist underlayer film formed in the coating step (I) is heated. Heating the resist underlayer film promotes the formation of a crosslinked structure in the polymer (A). This step is carried out before the coating step (II).

[0110] The coating film may be heated in an air atmosphere or a nitrogen atmosphere. The lower limit of the heating temperature is 180°C, but is preferably 200°C, more preferably 210°C, and even more preferably 220°C. The upper limit of the heating temperature is preferably 400°C, more preferably 350°C, and even more preferably 280°C. The lower limit of the heating time is preferably 15 seconds, more preferably 30 seconds. The upper limit of the time is preferably 800 seconds, more preferably 400 seconds, and even more preferably 200 seconds.

[0111] [Coating Step (II)] In this step, a resist film-forming composition is coated onto the resist underlayer film formed in the resist underlayer film-forming composition coating step. The method for coating the resist film-forming composition is not particularly limited, and examples thereof include a rotary coating method.

[0112] To explain this step in more detail, for example, a resist composition is applied so that the resist film to be formed has a predetermined thickness, and then the applied resist film is pre-baked (hereinafter also referred to as "PB") to volatilize the solvent in the applied film, thereby forming the resist film.

[0113] The PB temperature and PB time can be appropriately determined depending on the type of the resist film-forming composition used, etc. The lower limit of the PB temperature is preferably 30°C, more preferably 50°C. The upper limit of the PB temperature is preferably 200°C, more preferably 150°C. The lower limit of the PB time is preferably 10 seconds, more preferably 30 seconds. The upper limit of the PB time is preferably 600 seconds, more preferably 300 seconds.

[0114] The resist film-forming composition used in this step is preferably a composition that is subjected to exposure to extreme ultraviolet rays, and examples thereof include positive or negative chemically amplified resist compositions that contain a radiation-sensitive acid generator, and metal-containing resist compositions that contain a metal such as tin, zirconium, or hafnium.

[0115] [Exposure Step] In this step, the resist film formed in the resist film-forming composition application step is exposed to radiation, which causes a difference in solubility in a developer between the exposed and unexposed areas of the resist film.

[0116] The radiation used for exposure can be appropriately selected depending on the type of the resist film-forming composition used, etc. Examples include visible light, ultraviolet light, far ultraviolet light, electromagnetic waves such as X-rays and gamma rays, and particle beams such as electron beams, molecular beams, and ion beams. Among these, far ultraviolet light is preferred, and KrF excimer laser light (wavelength 248 nm), ArF excimer laser light (wavelength 193 nm), F 2 Excimer laser light (wavelength 157 nm), Kr 2Excimer laser light (wavelength 147 nm), ArKr excimer laser light (wavelength 134 nm), or extreme ultraviolet light (wavelength 13.5 nm, etc., also referred to as "EUV") is more preferred, and ArF excimer laser light or EUV is even more preferred. The exposure conditions can be appropriately determined depending on the type of resist film-forming composition used, etc.

[0117] Furthermore, in this process, after the exposure, post-exposure baking (hereinafter also referred to as "PEB") can be performed to improve the performance of the resist film, such as resolution, pattern profile, and developability. The PEB temperature and PEB time can be appropriately determined depending on the type of resist film-forming composition used, etc. The lower limit of the PEB temperature is preferably 50°C, more preferably 70°C. The upper limit of the PEB temperature is preferably 200°C, more preferably 150°C. The lower limit of the PEB time is preferably 10 seconds, more preferably 30 seconds. The upper limit of the PEB time is preferably 600 seconds, more preferably 300 seconds.

[0118] [Development Step] In this step, the exposed resist film is developed. At this time, a part of the resist underlayer film may also be developed. Examples of the developer used in this development include an alkaline aqueous solution (alkaline developer), a liquid containing an organic solvent (organic solvent developer), etc.

[0119] The basic liquid for alkaline development is not particularly limited, and known basic liquids can be used. Examples of basic liquids for alkaline development include aqueous alkaline solutions containing at least one alkaline compound dissolved therein, such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, aqueous ammonia, ethylamine, n-propylamine, diethylamine, di-n-propylamine, triethylamine, methyldiethylamine, ethyldimethylamine, triethanolamine, tetramethylammonium hydroxide (TMAH), pyrrole, piperidine, choline, 1,8-diazabicyclo-[5.4.0]-7-undecene, and 1,5-diazabicyclo-[4.3.0]-5-nonene. Among these, aqueous TMAH solutions are preferred, and 2.38% by mass aqueous TMAH solutions are more preferred.

[0120] Examples of organic solvent developers for use in organic solvent development include those exemplified above as the solvent [B]. As the organic solvent developer, an ester solvent, an ether solvent, an alcohol solvent, a ketone solvent, and / or a hydrocarbon solvent is preferred, a ketone solvent is more preferred, and 2-heptanone is particularly preferred.

[0121] In this step, washing and / or drying may be carried out after the development.

[0122] [Etching Step] In this step, etching is performed using the resist pattern (and resist underlayer film pattern) as a mask. The etching may be performed once or multiple times, i.e., etching may be performed sequentially using the pattern obtained by etching as a mask. From the viewpoint of obtaining a pattern with a better shape, multiple times is preferred. When etching is performed multiple times, for example, etching is performed sequentially in the order of the silicon-containing film and the substrate. Examples of etching methods include dry etching and wet etching. From the viewpoint of obtaining a better pattern shape on the substrate, dry etching is preferred. For this dry etching, for example, a gas plasma such as oxygen plasma is used. By the above etching, a semiconductor substrate having a predetermined pattern is obtained.

[0123] Dry etching can be performed using, for example, a known dry etching apparatus. The etching gas used for dry etching can be appropriately selected depending on the mask pattern, the elemental composition of the film to be etched, etc., and can be, for example, CHF 3 , C.F. 4 , C 2 F 6 , C 3 F 8 , S.F. 6 Fluorine-based gases such as Cl 2 , BCl 3 Chlorine gases such as O 2 , O 3 , H 2 Oxygen-based gases such as O, H 2 , N.H. 3 , CO, CO 2 , C.H.4 , C 2 H 2 , C 2 H 4 , C 2 H 6 , C 3 H 4 , C 3 H 6 , C 3 H 8 , HF, HI, HBr, HCl, NO, BCl 3 reducing gases such as He, N 2 and inert gases such as Ar. These gases may be used in combination. When etching a substrate using the pattern of the resist underlayer film as a mask, a fluorine-based gas is usually used.

[0124] After the substrate pattern is formed, if the silicon-containing film remains on the substrate, the silicon-containing film can be removed by carrying out a removal step.

[0125] <<Polymer for forming resist underlayer film>> The polymer for forming resist underlayer film is obtained by reacting a compound represented by the following formula (α) with a compound represented by the following formula (β1) or a compound represented by the following formula (β2): (In formula (α), Ar 1 is a divalent group having an aromatic ring with 6 to 20 ring members. A is a substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms. 1a and R 3a R are each independently a monovalent group having an epoxy structure or an oxetane structure. B is a divalent organic group having 1 to 20 carbon atoms.

[0126] As such a polymer for forming a resist underlayer film and a method for producing the same, the polymer (A) in the composition for forming a resist underlayer film and a method for producing the same can be suitably used.

[0127] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples.

[0128] [Weight-average molecular weight (Mw)] The Mw of the polymer was measured by gel permeation chromatography (detector: differential refractometer) using GPC columns (two "G2000HXL" and one "G3000HXL" columns) manufactured by Tosoh Corporation under the following analytical conditions: flow rate: 1.0 mL / min, elution solvent: tetrahydrofuran, column temperature: 40°C, with monodisperse polystyrene as the standard.

[0129] [Average Film Thickness] The average film thickness was determined by measuring the film thickness at 9 arbitrary positions at 5 cm intervals, including the center of the resist underlayer film formed on the silicon wafer, using a spectroscopic ellipsometer (J.A. WOOLLAM's "M2000D"), and calculating the average of these film thicknesses.

[0130] <Synthesis of Polymer [A]> Each polymer [A] was synthesized according to the procedure shown below. In the formulas shown in the synthesis examples below, the number attached to each repeating unit indicates the content (mol %) of that repeating unit. When no number is attached to a repeating unit, the content of that repeating unit is 100 mol %. The composition ratio is 13 This was confirmed by C-NMR.

[0131] <Synthesis of Monomers> The following compounds (a-1) to (a-6), compounds (b-1) to (b-4), compounds (c-1) to (c-4), and compound (d-1) were used in the synthesis of polymer [A].

[0132]

[0133]

[0134]

[0135]

[0136] Synthesis Example 1-1 Synthesis of Compound (a-1) 300 mL of methanol, 10 g of bisphenol A, and 12.29 g of potassium hydroxide were added to a reaction vessel and stirred at room temperature for 20 minutes. 55.6 g of iodine was added and stirred at room temperature for 2 hours. 300 mL of methyl isobutyl ketone and 100 mL of saturated aqueous ammonium chloride solution were added, and the organic layer was recovered. After separation with 100 mL of saturated sodium thiosulfate, the organic layer was washed with 100 mL of ultrapure water. The organic layer was concentrated to obtain 16.7 g of compound (a-1) represented by the above formula (a-1) as a white solid (yield: 52.3%).

[0137] Synthesis Example 1-2 Synthesis of Compound (a-2) By carrying out a reaction under the same conditions as in Synthesis Example 1-1, except that 15.3 g of the compound bisphenol fluorene was used instead of the compound bisphenol A, 19.5 g of the compound (a-2) represented by the above formula (a-2) was obtained as a white solid (yield: 52.3%).

[0138] Synthesis Example 1-3 Synthesis of Compound (a-3) By carrying out a reaction under the same conditions as in Synthesis Example 1-1, except that 8.2 g of the compound dihydroxybiphenyl was used instead of the compound bisphenol A, 15.7 g of the compound (a-3) represented by the above formula (a-3) was obtained as a white solid (yield: 52.3%).

[0139] Synthesis Example 1-4 Synthesis of Compound (a-4) By carrying out a reaction under the same conditions as in Synthesis Example 1-1, except that 15.2 g of the compound 1,4-bis[2-(4-hydroxyphenyl)-2-propyl]benzene was used instead of the compound bisphenol A, 19.4 g of compound (a-4) represented by the above formula (a-4) was obtained as a white solid (yield: 52.3%).

[0140] Synthesis Example 1-5 Synthesis of Compound (c-2) 10 g of compound (a-1), 37.9 g of epichlorohydrin, 7.7 g of potassium hydroxide, and 4.5 g of potassium iodide were added to a reaction vessel and stirred at room temperature for 6 hours. 200 mL of ethyl acetate was added and the mixture was washed with water. The organic layer was concentrated to obtain 8.9 g of compound (c-2) represented by the above formula (c-2) as a white solid (yield: 77%).

[0141] Synthesis Example A-1 (Synthesis of Polymer (A-1)) A reaction vessel was charged with 5.00 g of compound (a-1) and 5 g of dimethylacetamide and kept at 80°C, and a mixed solution of 1.14 g of compound (b-1) and 10 g of dimethylacetamide was added dropwise over 3 hours. After completion of the dropwise addition, the mixture was stirred at 80°C for 3 hours. The resulting polymerization solution was purified by precipitation with a 5-fold amount of methanol to obtain Polymer (A-1) represented by the following formula as a white solid. The resulting Polymer (A-1) had an Mw of 2800 and a PDI of 1.6.

[0142]

[0143] [Synthesis Examples A-2 to 12, 14 to 19] (Synthesis of Polymers (A-2) to (A-12), (A-14) to (A-19)) Polymers (A-2) to (A-12), (A-14) to (A-19) as shown in the following formulas (A-2) to (A-12), (A-14) to (A-19) were obtained as products under the same reaction conditions as in Synthesis Example A-1, except that compound (a) and compound (b) or compound (c) shown in Table 1 were used. The Mw and PDI of these polymers were determined and are listed in Table 1. In Table 1, "-" indicates that the corresponding component was not used. The same applies to the other tables.

[0144]

[0145]

[0146]

[0147]

[0148] Synthesis Example A-13 (Synthesis of Polymer (A-13)) A reaction vessel was charged with 5.00 g of compound (a-1), 0.59 g of compound (d-1), and 5 g of dimethylacetamide, and the mixture was maintained at 80°C. A mixed solution of 4.65 g of compound (c-1) and 10 g of dimethylacetamide was added dropwise over 3 hours. After completion of the dropwise addition, the mixture was stirred at 80°C for 3 hours. The resulting polymerization solution was purified by precipitation with a five-fold amount of methanol, to obtain a polymer (A-13) represented by the following formula (A-13) as a white solid. The resulting polymer (A-13) had an Mw of 3800 and a PDI of 1.6. The molar ratio of the respective repeating units was n:m:l=30:50:20.

[0149]

[0150] Comparative Example X-1 (Synthesis of Polymer (X-1)) A reaction vessel was charged with 10.0 g of glycidyl methacrylate, 17.4 g of 4-iodobenzoic acid, and 20 g of dimethylacetamide, and 0.75 g of triphenylantimony (III) was added. After heating and stirring at 100°C for 2 hours, 3.70 g of triphenylphosphine was added, and the mixture was stirred for 6 hours. 200 mL of water and 200 mL of ethyl acetate were added, and the mixture was separated. The mixture was then washed with water twice, and the organic layer was recovered. The organic layer was concentrated, yielding 24.7 g of 2-hydroxy-3-(methacryloxy)propyl-4-iodobenzoate.

[0151] 5 g of dimethylacetamide was placed in a reaction vessel and maintained at 80°C, and a mixed solution of 5.00 g of 2-hydroxy-3-(methacryloxy)propyl-4-iodobenzoate, 0.59 g of dimethyl-2,2-azobisisobutyrate, and 10 g of dimethylacetamide was added dropwise over 3 hours. After completion of the dropwise addition, the mixture was stirred at 80°C for 3 hours. The resulting polymerization solution was purified by precipitation with a five-fold amount of methanol to obtain a white solid of polymer (X-1) represented by the following formula (X-1). The resulting polymer (X-1) had an Mw of 4500 and a PDI of 1.62.

[0152]

[0153]

[0154] <Preparation of Composition> The polymer (A), comparative polymer (B), solvent (C), acid generator (C), and crosslinking agent (D) used in the preparation of the composition are shown below.

[0155] [[A] Polymer] Example: Polymers (A-1) to (A-19) synthesized above

[0156] [Comparative Polymer] Comparative Example: Polymer (X-1) synthesized above

[0157] [B] Solvent: B-1: Propylene glycol monomethyl ether acetate B-2: Cyclohexanone

[0158] [[C] Acid Generator] C-1: Compound represented by the following formula (C-1):

[0159]

[0160] [[D] Crosslinking Agent] D-1: Compound represented by the following formula (D-1) D-2: Compound represented by the following formula (D-2)

[0161] [Example 1-1] 25 parts by mass of (A-1) as the polymer [A] was dissolved in 7,900 parts by mass of (B-1) and 2,000 parts by mass of (B-2) as the solvent [B]. The resulting solution was filtered through a polytetrafluoroethylene (PTFE) membrane filter with a pore size of 0.45 μm to prepare composition (J-1).

[0162] [Examples 1-2 to 1-22 and Comparative Example 1-1] Compositions (J-2) to (J-22) and (CJ-1) were prepared in the same manner as in Example 1, except that the types and amounts of each component shown in Table 2 below were used.

[0163]

[0164] <Evaluation> Using the compositions prepared above, the solvent resistance and the rectangularity of the resist pattern formed by EUV exposure were evaluated by the following methods. The evaluation results are shown in Table 3 below.

[0165] [Solvent Resistance] The composition prepared above was applied to a 12-inch silicon wafer by spin coating using a spin coater (Tokyo Electron Limited's "CLEAN TRACK ACT12"). The wafer was then heated at 250°C for 60 seconds in an air atmosphere and then cooled at 23°C for 60 seconds to form a resist underlayer film with an average thickness of 5 nm, yielding a substrate with a resist underlayer film formed on the substrate. The resist underlayer film-attached substrate obtained above was immersed in cyclohexanone (23°C) for 1 minute. The average film thicknesses before and after immersion were measured. The absolute value of the value obtained by {(X-X0) / X0} x 100, where X0 is the average thickness of the resist underlayer film before immersion and X is the average thickness of the resist underlayer film after immersion, was calculated and used as the film thickness change rate (%). For solvent resistance, a film thickness change rate of less than 10% was rated "A" (good), and a film thickness change rate of 10% or greater was rated "B" (poor).

[0166] <Preparation of Resist Composition> Resist composition (R-1) was obtained by mixing 100 parts by mass of a polymer having a structural unit (1) derived from 4-hydroxystyrene, a structural unit (2) derived from styrene, and a structural unit (3) derived from 4-t-butoxystyrene (the proportions of the structural units were (1) / (2) / (3)=65 / 5 / 30 (mol %)), 1.0 part by mass of triphenylsulfonium trifluoromethanesulfonate as a radiation-sensitive acid generator, and 4,400 parts by mass of ethyl lactate and 1,900 parts by mass of propylene glycol monomethyl ether acetate as solvents, and filtering the resulting solution through a filter with a pore size of 0.2 μm.

[0167] [Pattern Rectangularity (EUV Exposure)] An organic underlayer film forming material (JSR Corporation's "HM8006") was applied to a 12-inch silicon wafer by a spin coating method using a spin coater (Tokyo Electron Limited's "CLEAN TRACK ACT12"), and then heated at 250°C for 60 seconds to form an organic underlayer film with an average thickness of 100 nm. A silicon-containing film-forming composition (JSR Corporation's "NFC SOG080") was applied to this organic underlayer film, heated at 220°C for 60 seconds, and then cooled at 23°C for 30 seconds to form a silicon-containing film with an average thickness of 20 nm. The composition prepared above was applied to the silicon-containing film formed above to form a resist underlayer film. The resist underlayer film formed above was heated at 250°C for 90 seconds, and then cooled at 23°C for 30 seconds to obtain a resist underlayer film with an average thickness of 5 nm. Resist composition (R-1) was applied onto the resist underlayer film formed above, heated at 130° C. for 60 seconds, and then cooled at 23° C. for 30 seconds to form a resist film with an average thickness of 50 nm. Next, the resist film was irradiated with extreme ultraviolet rays using an EUV scanner (ASML's "TWINSCAN NXE:3300B" (NA 0.3, sigma 0.9, quadrupole illumination, 1:1 line and space mask with on-wafer line width of 16 nm). After irradiation with extreme ultraviolet rays, the substrate was heated at 110°C for 60 seconds and then cooled at 23°C for 60 seconds. Thereafter, the substrate was developed by the puddle method using a 2.38 mass% aqueous solution of tetramethylammonium hydroxide (20°C to 25°C), followed by washing with water and drying, thereby obtaining an evaluation substrate on which a 1:1 line and space resist pattern with a line width of 16 nm was formed. A scanning electron microscope (Hitachi High-Technologies Corporation's "SU8220") was used to measure and observe the resist pattern of the evaluation substrate. The pattern rectangularity was evaluated as "A" (good) when the cross-sectional shape of the pattern was rectangular, and as "B" (poor) when there was a footing on the cross section of the pattern.

[0168]

[0169] <Evaluation> Using the compositions prepared above, the rectangularity of resist patterns obtained by EUV exposure was evaluated by the following method. The evaluation results are shown in Table 4 below.

[0170] <Preparation of EUV Exposure Resist Composition (R-2)> Compound (S-1) used in preparing EUV exposure resist composition (R-2) was synthesized according to the procedure shown below. In a reaction vessel, 6.5 parts by mass of isopropyltin trichloride was added to 150 mL of 0.5 N aqueous sodium hydroxide solution while stirring, and the reaction was carried out for 2 hours. The precipitate that formed was collected by filtration, washed twice with 50 parts by mass of water, and then dried to obtain compound (S-1). Compound (S-1) was a hydroxide oxide product (i-PrSnO) of the hydrolysis product of isopropyltin trichloride. (3/2-x/2) (OH) x (where 0<x<3 is the structural unit).

[0171] 2 parts by mass of the compound (S-1) synthesized above and 98 parts by mass of propylene glycol monoethyl ether were mixed, and the resulting mixture was passed through an activated 4 Å molecular sieve to remove residual water, followed by filtration through a filter with a pore size of 0.2 μm to prepare a resist composition for EUV exposure (R-2).

[0172] [Pattern Rectangularity (EUV Exposure)] An organic underlayer film-forming material ("HM8006" manufactured by JSR Corporation) was applied onto a 12-inch silicon wafer by spin coating using a spin coater ("CLEAN TRACK ACT12" manufactured by Tokyo Electron Limited), and then heated at 250°C for 60 seconds to form an organic underlayer film with an average thickness of 100 nm. The resist underlayer film-forming composition prepared above was applied onto this organic underlayer film, and then heated at 220°C for 60 seconds, and then cooled at 23°C for 30 seconds to form a resist underlayer film with an average thickness of 5 nm. Resist composition (R-2) for EUV exposure was applied onto this resist underlayer film by spin coating using the spin coater, and after a predetermined time had elapsed, the resist film was heated at 90°C for 60 seconds, and then cooled at 23°C for 30 seconds to form a resist film with an average thickness of 35 nm. The resist film was exposed to light using an EUV scanner (ASML's "TWINSCAN NXE:3300B" (NA 0.3, sigma 0.9, quadrupole illumination, 1:1 line and space mask with on-wafer line width of 16 nm). After exposure, the substrate was heated at 110°C for 60 seconds and then cooled at 23°C for 60 seconds. Thereafter, the substrate was developed by a puddle method using 2-heptanone (20-25°C) and then dried to obtain an evaluation substrate on which a 1:1 line and space resist pattern with a line width of 16 nm was formed. A scanning electron microscope (Hitachi High-Technologies Corporation's "CG-6300") was used to measure and observe the resist pattern of the evaluation substrate. The pattern rectangularity was evaluated as "A" (good) when the cross-sectional shape of the pattern was rectangular, and as "B" (poor) when there was a footing on the cross section of the pattern.

[0173]

[0174] As can be seen from the results in Tables 3 and 4, the resist underlayer films formed from the compositions of the Examples were superior in solvent resistance and pattern rectangularity compared to the resist underlayer films formed from the compositions of the Comparative Examples.

[0175] The composition for forming a resist underlayer film of the present invention can form a film having excellent solvent resistance and pattern rectangularity. The method for producing a semiconductor substrate of the present invention uses a composition for forming a resist underlayer film that can form a resist underlayer film having excellent solvent resistance and pattern rectangularity, allowing for efficient production of semiconductor substrates. The polymer for forming a resist underlayer film of the present invention is suitable for use in a composition for forming a resist underlayer film. Therefore, these can be suitably used in the production of semiconductor devices, etc.

Claims

1. A composition for forming a resist underlayer film, comprising: a polymer having a repeating unit represented by the following formula (1) or a repeating unit represented by the following formula (2); and a solvent. (In formula (1), Ar 1 R is a divalent group having an aromatic ring having 6 to 20 ring members. A In formula (2), Ar is a substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms. 1 R is a divalent group having an aromatic ring having 6 to 20 ring members. 1 and R 3 R is each independently a substituted or unsubstituted trivalent hydrocarbon group having 1 to 20 carbon atoms. 2 and R 4 Each of L is independently a hydroxy group or a monovalent organic group. 1 and L 2 R is each independently a single bond or a divalent linking group. B is a divalent organic group having 1 to 20 carbon atoms.

2. The composition for forming a resist underlayer film according to claim 1, wherein the polymer has at least one halogen atom per repeating unit.

3. In formula (1) and formula (2), Ar 1 The composition for forming a resist underlayer film according to claim 1, wherein is a divalent group having an aromatic ring having 6 to 20 ring members and substituted with at least one halogen atom.

4. In formula (1) and formula (2), Ar 1 The composition for forming a resist underlayer film according to claim 1, wherein is a divalent group having an aromatic ring having 6 to 20 ring members and substituted with at least one iodine atom.

5. In formula (1) and formula (2), R A and R B each independently comprises a substituted or unsubstituted divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, or a substituted or unsubstituted divalent aromatic hydrocarbon group having 6 to 20 carbon atoms.

6. In formula (2), R 2 and R 4 each independently has a group containing at least one group selected from the group consisting of a hydroxy group, a group represented by the following formula (2-1), and a group represented by the following formula (2-2): (In the formulas (2-1) and (2-2), R 7 are each independently a divalent organic group having 1 to 20 carbon atoms or a single bond. 2 and R 4 is a bond to the atoms that make up the molecule.) 7. In formula (2), R 1 and R 3 are each independently a substituted or unsubstituted trivalent chain hydrocarbon group having 1 to 20 carbon atoms, or a substituted or unsubstituted trivalent alicyclic hydrocarbon group having 3 to 20 carbon atoms.

8. The composition for forming a resist underlayer film according to any one of claims 1 to 8, which is a composition for forming an underlayer film of a resist film to be exposed to extreme ultraviolet rays.

9. A method for producing a semiconductor substrate, comprising: a step of applying a composition for forming a resist underlayer film directly or indirectly to a substrate; a step of applying a composition for forming a resist film to the resist underlayer film formed by the step of applying the composition for forming a resist film; a step of exposing the resist film formed by the step of applying the composition for forming a resist film to radiation; and a step of developing at least the exposed resist film, wherein the composition for forming a resist underlayer film comprises: a polymer having a repeating unit represented by the following formula (1) or a repeating unit represented by the following formula (2); and a solvent. (In formula (1), Ar 1 R is a divalent group having an aromatic ring having 6 to 20 ring members. A In formula (2), Ar is a divalent organic group. 1 R is a divalent group having an aromatic ring having 6 to 20 ring members. 1 and R 3 R is each independently a substituted or unsubstituted trivalent hydrocarbon group having 1 to 20 carbon atoms. 2 and R 4 Each of L is independently a hydroxy group or a monovalent organic group. 1 and L 2 R is each independently a single bond or a divalent linking group. B is a divalent organic group.

10. The method for manufacturing a semiconductor substrate according to claim 9, wherein said radiation is extreme ultraviolet radiation.

11. A polymer for forming a resist underlayer film, obtained by reacting a compound represented by the following formula (α) with a compound represented by the following formula (β1) or a compound represented by the following formula (β2): (In formula (α), Ar 1 is a divalent group having an aromatic ring having 6 to 20 ring members. A is a substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms. 1a and R 3a R is each independently a monovalent group having an epoxy structure or an oxetane structure. B is a divalent organic group having 1 to 20 carbon atoms.

12. In formula (α), Ar 1 The polymer for forming a resist underlayer film according to claim 11, wherein is a divalent group having an aromatic ring having 6 to 20 ring members substituted with at least one halogen atom.

13. In formula (α), Ar 1 The polymer for forming a resist underlayer film according to claim 11, wherein is a divalent group having an aromatic ring having 6 to 20 ring members substituted with at least one iodine atom.

Citation Information

Patent Citations

  • Polyurethane polymer having bisphenol group and photographic imaging composition containing the same

    JP2007308686A

  • Composition for forming resist underlay film and method for forming resist pattern using the composition

    JP2015145944A

  • Compound, binder resin, negative photosensitive resin composition, and display device including black bank formed using the same - Patents.com

    JP2022550733A

  • Composition for forming resist underlayer film and method for forming resist pattern using same

    WO2017154600A1