Wind turbine blade
The wind turbine blade design addresses mechanical deficiencies by using composite spar caps with carbon and glass fibers to enhance rigidity and introduce a fail-safe area, preventing tower hits and ensuring safe operation by delaying rupture and managing loads effectively.
Patent Information
- Application Number
- PCT/JP2024/009303
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-11
- Publication Date
- 2024-10-03
AI Technical Summary
Long wind turbine blades face mechanical property deficiencies due to bending deformation, leading to potential tower hits and breakage, with existing materials like glass fiber-reinforced resin not providing sufficient rigidity, and lack of fail-safe design to prevent fragment scattering.
A wind turbine blade design incorporating a pressure-side and suction-side spar cap made of composite materials with carbon and glass fibers, arranged in specific ratios and distributions to enhance elastic modulus and bending/torsional rigidity, with a fail-safe area that delays complete rupture and prevents tower hits.
The design achieves high rigidity and strain suppression, preventing tower hits and ensuring safe operation by delaying complete blade rupture, even in large turbines, and effectively managing loads during gusts and rated wind conditions.
Smart Images

Figure JP2024009303_03102024_PF_FP_ABST
Abstract
Description
Wind turbine blades
[0001] The present invention relates to a wind turbine blade used in wind turbines for wind power generation and the like.
[0002] In recent years, wind turbine blades for wind power generation have become longer and larger in order to generate greater amounts of power. While increasing the length of wind turbine blades increases the area that receives wind, it is also necessary to ensure that the blades are rigid enough to withstand the centrifugal force and wind force that accompanies rotation. Until now, glass fiber reinforced resin, which is relatively inexpensive, has often been used as a material for wind turbine blades. As wind turbine blades have become longer, blades longer than 100 meters have experienced significant bending deformation, and glass fiber reinforced resin does not have sufficient mechanical properties. As a result, the occurrence of so-called tower hits, in which the wind turbine blade comes into contact with the tower that supports it and is damaged, has become more apparent.
[0003] To address this issue, Non-Patent Document 1 studies how to increase the rigidity of 117m wind turbine blades by using carbon fiber reinforced resin, which has better mechanical properties. Patent Document 1 also studies how to increase the rigidity of wind turbine blades while keeping costs down by combining glass fiber reinforced resin and carbon fiber reinforced resin.
[0004] Definition of the IEA Wind 15MW Offshore Reference Wind Turbine (2020)
[0005] U.S. Pat. No. 1,046,5653
[0006] In general, when designing wind turbine blades, it goes without saying that the tower hit described above should be avoided. In addition, in the unlikely event that a wind turbine blade is about to break, it is important to buy time before the worst-case scenario of the wind turbine blade completely breaking apart and fragments scattering around occurs. In other words, in preparation for the wind turbine blade breaking, it is necessary to incorporate a fail-safe design that allows for safe action before the wind turbine blade completely breaks apart and fragments scatter, so that the system always operates on the safe side. However, in the prior art, such a fail-safe perspective is not suggested at all, and no design concepts for such a fail-safe have been disclosed or considered.
[0007] To provide a wind turbine blade that satisfies the requirement for a fail-safe, which can avoid a tower hit even in a large wind turbine and can gain time from the start of damage until complete breakage.
[0008] The gist of the present invention for solving the above problems is as follows: [1] A wind turbine blade having a pressure-side spar cap arranged in contact with the interior surface of the pressure-side skin of the wind turbine blade, a contraction-side spar cap arranged in contact with the interior surface of the contraction-side skin, and a long, plate-shaped share web arranged so that both ends are in contact with the pressure-side spar cap and the contraction-side spar cap, wherein the pressure-side spar cap and the contraction-side spar cap are made of a composite in which composite plates containing reinforcing fibers aligned in one direction are arranged in the width direction of the wind turbine blade and stacked in the height direction and bonded to each other, and at least one of the pressure-side spar cap and the contraction-side spar cap has a fail-safe region that satisfies the following 1 to 3 in a region of at least a certain length in the longitudinal direction of the wind turbine blade: 1. 1. The spar cap is constructed by arranging and stacking a plurality of carbon composite plates containing carbon fibers with an elastic modulus of 250 GPa or more and glass composite plates containing glass fibers with an elastic modulus of 80 GPa or more in the width direction of the wind turbine blade. 2. In the spar cap, the ratio of the glass composite to the carbon composite in the stacking direction of the composite plates is within the range of 0.3 to 0.7. 3. When the cross section of the spar cap is divided equally into three regions in the width direction of the wind turbine blade, the ratio of the glass composite to the carbon composite in each of the three regions is within the range of -0.1 to +0.1 of the average ratio of the three regions.
[0009] [2] The wind turbine blade according to [1], wherein in the fail-safe region, the ratio of the glass composite to the carbon composite in the spar cap is in the range of 0.4 to 0.6. [3] The wind turbine blade according to [1] or [2], wherein in the fail-safe region, the glass composite plates in the spar cap are alternately arranged so as not to be adjacent in the height direction and width direction of the spar cap. [4] The wind turbine blade according to [1] or [2], wherein in the fail-safe region, the carbon composite plates in the spar cap are unevenly arranged in the stacking direction.
[0010] [5] The wind turbine blade according to any one of [1] to [4], wherein the fail-safe area is located at least closer to the root of the wind turbine blade (hub side) than the center of the wind turbine blade in the longitudinal direction. [6] The wind turbine blade according to any one of [1] to [5], wherein the fail-safe area is located in an area that accounts for 70% or more of the longitudinal length of the wind turbine blade, assuming that the length is 100%. [7] The wind turbine blade according to any one of [1] to [6], wherein the pressure side spar cap has the fail-safe area. [8] A wind turbine for wind power generation, comprising the wind turbine blade according to any one of [1] to [7].
[0011] In this specification, the length of a wind turbine blade is indicated by L in FIG. 2 . The longitudinal length L of a wind turbine blade refers to the length of a line connecting the center of gravity in a cross section near the part fixed to the hub to the part farthest from the part fixed to the hub (the tip of the wind turbine blade). The longitudinal direction of the wind turbine blade is indicated as the z-direction in each drawing. The width direction of the wind turbine blade refers to the direction connecting the leading edge and the trailing edge in a cross section perpendicular to the longitudinal direction of the wind turbine blade, and is indicated as the y-direction in each drawing. The height direction of the wind turbine blade refers to the direction perpendicular to the y-direction and z-directions, and is indicated as the x-direction in each drawing. The height direction of the wind turbine blade is also called the thickness direction. The height of the wind turbine blade refers to the maximum length in the x-direction, indicated by T in FIG. 2 . The longitudinal direction z', width direction y', and height direction x' of the spar cap are substantially the same as the longitudinal direction z, width direction y, and height direction x of the wind turbine blade, as shown in FIG. 2( b).
[0012] According to the present invention, a wind turbine blade can be obtained that can avoid tower hits even in large wind turbines and that satisfies fail-safe requirements. That is, the wind turbine blade of the present invention is made of a carbon composite and a glass composite, and therefore has a high elastic modulus, high bending rigidity and torsional rigidity, and in the event of fracture, the high elastic modulus of the glass composite allows for a large strain to be tolerated before complete fracture.
[0013] FIG. 1 is an overall view of a wind turbine for wind power generation. FIG. 2 is a perspective view including a cross section when cutting a wind turbine blade 1 in a plane perpendicular to the longitudinal direction of the wind turbine blade. FIG. 3 is a schematic view showing an overview of a spar cap on a wind turbine blade. FIG. 4 is a conceptual diagram explaining the fail-safe concept of the spar cap of the present invention. FIG. 5 is a schematic cross-sectional view of a spar cap according to an embodiment of the present invention. FIG. 6 is a schematic cross-sectional view of a spar cap according to an embodiment of the present invention. FIG. 7 is a schematic cross-sectional view of a spar cap according to an embodiment of the present invention. FIG. 8 is a schematic cross-sectional view of a spar cap according to an embodiment of the present invention. FIG. 9 is a schematic cross-sectional view of a spar cap according to an embodiment of the present invention. FIG. 10 is a schematic view for evaluating the amount of displacement when a pressure simulating wind is applied to a wind turbine blade. FIG. 11 is a schematic cross-sectional view of a spar cap according to comparative example 1.
[0014] Hereinafter, embodiments of the present invention will be described with reference to the drawings. Note that the description of the specific embodiments shown in the drawings can also be understood as a description of the present invention as a general concept.
[0015] 1(a) and (b) show elevation views of a wind turbine. A typical wind turbine for wind power generation consists of a wind turbine blade 1, a tower 2, a nacelle 3, and a hub 4. The wind turbine blade 1 is attached to the hub 4. The wind turbine blade 1 rotates due to wind force, and this rotation is transmitted to a power transmission shaft in the nacelle 3 via the hub 4, driving a generator in the nacelle 3. Note that hereinafter, the wind turbine blade may be simply referred to as the blade.
[0016] The wind turbine blade 1 may be configured so that the tip side is bent in advance (pre-bent) in a direction away from the tower 2 so as to be less likely to collide with the tower 2. In the case of a pre-bend, the longitudinal direction of the wind turbine blade refers to the direction connecting the center of gravity of the cross section of the blade base and the center of gravity of the cross section of the part farthest from the part fixed to the hub within the range up to the start position of the pre-bend.
[0017] FIG. 2 is a perspective view of a wind turbine blade 1 according to one embodiment of the present invention, including a cross section taken along a plane perpendicular to the longitudinal direction of the wind turbine blade. The wind turbine blade 1 of the present invention includes at least skins 13, which become the pressurized and contracted sides when the blade is exposed to wind, spar caps 12 disposed on portions of the pressurized and contracted side skin materials, and shear webs 11 connecting the spar caps to each other. The spar caps 12 are configured inside the skins 13, and in FIG. 2, are disposed on the upper and lower inner walls of the skin 13. The spar caps 12 are structured to bear bending and torsional loads on the wind turbine blade 1. The shear webs 11 are long, plate-like structures arranged so that both ends contact the pressurized and contracted side spar caps, and extend in the longitudinal direction of the wind turbine blade along the inner wall of the wind turbine blade 1. The pressurized side spar cap 12, on which a load is applied to the wind turbine blade, is referred to as the pressurized side spar cap. The method for manufacturing the wind turbine blade is not particularly limited, but one example is the resin infusion method, in which the skin 13 is placed on a mold that will become the outer shape of the wind turbine blade, the spar cap 12 is placed on top of that, and covered with a film that will become the upper mold, and while maintaining an airtight space with the lower mold, the skin is filled and impregnated with resin using vacuum pressure. Then, the separately molded share web 11 is assembled in a predetermined position and fixed using an adhesive or the like to manufacture the wind turbine blade.
[0018] A thickness of 50 mm or less for the shear web 11 is preferable because the bending rigidity is not too high and can be easily corrected when joining to the spar cap. On the other hand, a thickness of less than 20 mm may not provide the rigidity required for the shear web. Furthermore, a high modulus of elasticity in the ±45° direction from the blade longitudinal direction is preferable to suppress shear deformation. Therefore, a biaxial woven fabric is preferably used. A sandwich structure consisting of a core material and a skin material is also preferably used. The core material is made of wood such as balsa or a foamed resin material, and the skin material is made of the aforementioned biaxial woven fabric or the like.
[0019] The spar cap 12 is disposed in contact with the interior surface of the pressure-side skin and the interior surface of the suction-side skin of the blade. The spar cap 12 is constructed by arranging plate-shaped composites (fiber-reinforced composite materials) in the width direction of the wind turbine blade, stacking them in the height direction, and bonding them together. Such composites are generally long plate-shaped members, and are typically pultruded materials obtained by impregnating carbon fiber or glass fiber with resin and pultrusion molding them. The resin contained in the composite is not particularly limited, and examples include thermosetting resins such as epoxy resins, unsaturated polyester resins, and vinyl ester resins, as well as thermoplastic resins such as polyamide resins, polyolefin resins, polyester resins, polyphenylene sulfide resins, ABS resins, polycarbonate resins, polyacetal resins, and polybutylene terephthalate resins. Vinyl ester resins are particularly preferred because they have an excellent balance between moldability and mechanical properties, and epoxy resins are also preferred because they have excellent mechanical properties and adhesion to carbon fibers.
[0020] FIG. 3( a ) is a side view of a wind turbine blade 1, and FIG. 3( b ) is a schematic cross-sectional view perpendicular to the blade's width direction (y direction), showing the longitudinal stacking of the spar cap 12 disposed in contact with the blade's internal skin 13. In the spar cap 12, composites 121 of different lengths (here, the carbon composite plate 1211 and the glass composite plate 1212 are depicted without distinction) are stacked in the height direction of the wind turbine blade, thereby varying the thickness of the spar cap along the longitudinal direction. As shown in FIG. 3( b ), the spar cap has a thicker stacking thickness Ta near the center of the blade and a thinner stacking thickness Tb at the tip of the blade. In other words, the composites are stacked to correspond to the spar cap thickness required for the design depending on the longitudinal position of the blade. If the stacking thickness of the spar cap 12 is too thick, the blade will become heavy.
[0021] The blade of the present invention uses a spar cap on at least one of the pressure-side and contraction-side spar caps, in which a fail-safe region exists in a certain region or more in the longitudinal direction, satisfying the following conditions 1 to 3: 1. The blade is constructed by arranging multiple carbon composite plates containing carbon fibers with an elastic modulus of 250 GPa or more and multiple glass composite plates containing glass fibers with an elastic modulus of 80 GPa or more in the width direction of the wind turbine blade and stacking them in the thickness direction. 2. The ratio of glass composite to carbon composite in the stacking direction of the composite is in the range of 0.3 to 0.7. When expressed in terms of cross-sectional area, the spar cap has a ratio of the total area of the glass composite plates to the total area of the carbon composite plates in the cross section in the stacking direction of the composite plates in the range of 0.3 to 0.7. Furthermore, the ratio of glass composite to carbon composite (hereinafter sometimes referred to as the G / C ratio) refers to the area ratio in a cross section perpendicular to the longitudinal direction of the wind turbine blade, and when the cross-sectional areas of the carbon composite and the glass composite are the same, this corresponds to the ratio of the number of layers of each. 3. When the cross section of the spar cap is equally divided into three regions in the width direction of the wind turbine blade, the ratio of glass composite to carbon composite in each of the three regions is within the range of -0.1 to +0.1 of the average ratio in the three regions. In other words, the ratio of glass composite to carbon composite in the three regions is within the range of plus or minus 0.1, and the three regions are substantially uniform.
[0022] In the present invention, the term "composite" refers to the entire fiber-reinforced resin molding, with those containing carbon fiber as the reinforcing fiber being called carbon composites and those containing glass fiber being called glass composites. Furthermore, a carbon composite is a fiber-reinforced resin molding formed by arranging and stacking long, strip-shaped carbon composite plates in one direction. In other words, a carbon and / or glass composite is formed by arranging and stacking multiple long carbon and / or glass composite plates in one direction to form the entire fiber-reinforced resin molding.
[0023] The volume content of the reinforcing fibers in the composite plate is not limited as long as the required elastic modulus and strength of the entire composite are obtained, but a volume content of the reinforcing fibers in the range of 45 to 75% when the entire composite plate is taken as 100% is preferable from the viewpoint of moldability and is preferably used. A more preferable volume content of the reinforcing fibers is in the range of 55 to 70%. The volume content of the reinforcing fibers in the composite (fiber-reinforced resin molding) can be calculated from the volume content of the reinforcing fibers in each of the above-mentioned composite plates and the proportion of each composite in the molding.
[0024] The elastic modulus of the reinforcing fibers in this specification is a value measured according to JIS K7161 (2014). The elastic modulus varies depending on the material of the reinforcing fibers, but is the proportional constant (stress / strain) between stress and strain in elastic deformation and is related to the strain caused by the load. Tensile strength is the maximum stress generated when a load is applied to a material until it breaks. Generally, for the same material, the higher the elastic modulus, the smaller the strain relative to stress, and therefore the higher the stress required to reach the breaking strain.
[0025] The spar cap of the present invention is preferably used as a pressure-side spar cap because it can effectively bear the tensile load that occurs in the spar cap when a wind load is applied to the wind turbine blade, but it is more preferable to use a similar spar cap as a contraction-side spar cap as well.
[0026] Next, the fail-safe concept of the spar cap used in the long wind turbine blade of the present invention will be explained. Figure 4 is a conceptual diagram showing the relationship between the tensile load acting on the spar cap on the vertical axis and the strain of the spar cap on the horizontal axis. The solid line shows the case of a conventional spar cap, and the dotted line shows the case of the spar cap of the present invention.
[0027] Generally, when a blade is subjected to a wind load, the strain and load of the composite that makes up the spar cap increase. The higher the elastic modulus of the blade, the steeper the slope of the strain-load relationship in Figure 4, indicating that the blade can withstand a higher load. Carbon fiber is stronger than glass fiber, but its fracture strain is low. Therefore, as the load increases, the carbon fiber in the spar cap first reaches point 41, where it breaks. The glass fiber, which has not yet reached its fracture strain, then bears the load and withstands it. However, at point 42, where the load reaches its fracture strain, the glass fiber also breaks. In an actual blade, when point 42, where the glass fiber breaks, is reached, the blade breaks and fragments fly.
[0028] On the other hand, the spar cap used in the blade of the present invention is constructed by laminating multiple carbon composite plates containing carbon fibers with an elastic modulus of 250 GPa or more and multiple glass composite plates containing glass fibers with an elastic modulus of 80 GPa or more, as described in Section 1 above. The spar cap of the present invention has the fail-safe region shown in Figure 4. When high-elasticity glass fibers are used, the carbon fibers will first reach point 41 where they break. However, when the high-elasticity glass fibers bear the load alone thereafter, their high breaking strength increases, resulting in a large strain until the load at which final break occurs: the final break point 43 of the high-elasticity glass fibers. The difference in load between point 42 where the glass fibers break and point 43 of the high-elasticity glass fibers represents the fail-safe design. In other words, it is possible to design the maximum load at point 41 where the carbon fibers break to be equal to or greater than the load 44 that the blade will experience when subjected to the maximum gust of wind, and the maximum load at point 42 where the glass fibers reach their breaking strain to be equal to or greater than the load 45 that the blade will experience at rated wind force. In other words, even in the case of large wind turbines, it is possible to avoid hitting the tower, and in case the wind turbine blades are damaged, it is always possible to operate on the safe side, and it is possible to safely respond before the blades are completely separated and fragments scatter.
[0029] Furthermore, as described in Section 2 above, the spar cap used in the blade of the present invention has a G / C ratio, i.e., a ratio of glass composite to carbon composite in the composite stacking direction (i.e., the height direction of the spar cap, i.e., the x-direction in Figure 3, etc.), in the fail-safe region, in the range of 0.3 to 0.7. If the carbon composite is more than this ratio, the load resistance at point 43 where final glass fiber breakage occurs is insufficient, and a complete fail-safe design cannot be achieved. On the other hand, if the ratio is less than this ratio, it becomes difficult to obtain the strength and rigidity required for the spar cap. The G / C ratio is most preferably in the range of 0.4 to 0.6.
[0030] Furthermore, as described in Section 3 above, in the fail-safe region of the spar cap, when the cross section of the spar cap is divided equally into three regions in the width direction, the G / C ratio in the three regions is within a range of plus or minus 0.1. In other words, in the fail-safe region, the ratio of carbon composite to glass composite is substantially uniform in the width direction. For example, if there is a region in the width direction where the G / C ratio is less than -0.1, the load capacity at point 43 where final breakage of the glass fiber occurs will be insufficient, and breakage will begin partially, resulting in an incomplete fail-safe design as a whole.
[0031] Specific embodiments of a spar cap having such a fail-safe region are described below with reference to the drawings. In the embodiment shown in Fig. 5, the carbon composite plates and the glass composite plates are arranged and stacked so that they are not adjacent to each other in the height and width directions of the spar cap. This configuration is a particularly preferred embodiment of the present invention, because it provides a fail-safe region in which the ratio of carbon composite to glass composite is constant in the height direction and in the width direction at the thickest part (AA cross section) from the root to the center of the blade shown in Fig. 5(a) and at the tip (BB cross section) shown in Fig. 5(b).
[0032] 5 to 8 and 10 are drawn assuming that the height of the thickest part (AA cross section) of the spar cap 12 is 90 mm, the thickness of the carbon composite plate 1211 or the glass composite plate 1212 is 5 mm each, the total width of the spar cap 12 is 900 mm, and the widths of the carbon composite plate 1211 and the glass composite plate 1212 aligned in one direction are 100 mm each, but these sizes can be designed as appropriate.
[0033] Alternatively, as in the embodiment shown in Figure 6, the composites may be arranged and stacked so that the carbon composite plate 1211 is unevenly distributed in the upper part of the spar cap in the height direction, i.e., on the inner side of the blade. With this arrangement, the thickest part (AA cross section) shown in Figure 6(a) is in the fail-safe region, but the tip part (BB cross section) shown in Figure 6(b) is composed only of glass composite and does not fall into the fail-safe region. However, even with this configuration, reinforcement can be applied to partially impart the necessary rigidity strength to the tip part, so this configuration is practical in that it simplifies the arrangement and stacking of each composite.
[0034] As another alternative, the composites may be arranged and stacked so that the carbon composite plate 1211 is located at the lower level in the height direction of the spar cap, i.e., on the outer side of the blade, as shown in Figure 7. With this arrangement, the thickest portion (AA cross section) shown in Figure 7(a) is in the fail-safe region, but the tip portion (BB cross section) shown in Figure 7(b) is composed only of carbon composite and does not fall within the fail-safe region. However, because a large load is generally not applied to the blade tip and the risk of fracture is low, it is possible to obtain a blade with sufficient fail-safe functionality for practical use, and this configuration is practically beneficial in that it simplifies the arrangement and stacking of each composite.
[0035] As another alternative, the composites may be arranged and stacked so that the carbon composite plate 1211 is unevenly positioned at the center of the spar cap height, i.e., the middle of the blade, as shown in Figure 8. With this arrangement, the thickest portion (AA cross section) shown in Figure 8(a) falls within the fail-safe region, but the tip portion (BB cross section) shown in Figure 8(b) does not fall within the fail-safe region because the glass composite ratio falls outside the above range. However, the presence of a certain amount of glass composite still provides a certain degree of fail-safe function. Furthermore, since large loads are generally not applied to the blade tip, and the risk of breakage is low, this configuration simplifies the arrangement and stacking of each composite while still providing sufficient fail-safe function.
[0036] It is preferable that the fail-safe area satisfying the above 1 to 3 is designed over the entire length of the spar cap, since this provides a fail-safe effect over the entire length of the blade. However, if such a fail-safe area is designed to cover the root portion of the blade, which is subject to particularly high loads, or the thickest part of the spar cap, the blade design will have sufficient fail-safe functionality for practical use. Specifically, it is preferable that the fail-safe area be located closer to the root than the center in the longitudinal direction of the blade. Furthermore, it is preferable that the fail-safe area be located in an area that is 70% or more of the longitudinal length of the wind turbine blade, assuming that the length is 100%, from the perspective of stably maintaining strength at fracture.
[0037] Although the blade of the present invention is not particularly limited, the above-mentioned effects are most pronounced when the blade is 80 m or longer in length. Furthermore, the blade of the present invention is effective not only against bending deformation but also against torsional deformation.
[0038] As an example, an example in which the effects of the present invention were verified by computer simulation is shown below. (Evaluation Method) The amount of displacement of the shear web was evaluated as shown in Figure 9. Figure 9(a) is a schematic diagram showing a distributed load of 5778 Pa, simulating wind (indicated by the arrow in the figure), being applied to the surface of the wind turbine blade, and the amount of displacement in the x direction of the tip 92 of the wind turbine blade is evaluated when the root end 91 of the wind turbine blade is completely constrained all around. Here, the surface refers to the surface that is expected to receive the wind load when the wind turbine is viewed in the xy plane as shown in Figure 9(b), and refers to the surface projected onto the yz plane as shown in Figure 9(c).
[0039] The simulation was performed using the structural analysis software "NX Nastran" manufactured by SIEMENS. The wind turbine model was based on the wind turbine model "Definition of the IEA Wind 15MW Offshore Reference Wind Turbine" published by the National Renewable Energy Laboratory (NREL).
[0040] The stress in the fiber direction generated in the spar cap was read from the calculation results and compared with the maximum load required during a gust and the fail-safe load required at rated wind force. The maximum load was calculated by multiplying the tensile strength of the carbon fiber by the volume content and the carbon composite ratio, and the fail-safe load was calculated by multiplying the volume content and the glass composite ratio. The following values were used for the carbon fiber and glass fiber tensile strengths for each modulus of elasticity: Carbon fiber (modulus of elasticity: 264 GPa) Tensile strength: 4500 MPa Carbon fiber (modulus of elasticity: 240 GPa) Tensile strength: 4140 MPa Glass fiber (modulus of elasticity: 90 GPa) Tensile strength: 3300 MPa Glass fiber (modulus of elasticity: 70 GPa) Tensile strength: 1950 MPa. The maximum load required during a gust was 1600 MPa, and the rated load required at rated wind force equivalent to fail-safe was 400 MPa. Values above these values were considered good.
[0041] Example 1: A spar cap was constructed using a unidirectional composite consisting of a carbon composite and a high-modulus carbon fiber (264 GPa) at a volume content of 60%. A unidirectional composite consisting of a glass composite and a high-modulus glass fiber (90 GPa) at a volume content of 60% was also constructed. The composites were laminated so that the G / C ratio at the thickest point was 0.33. As shown in Figure 5, the carbon composite plate and the glass composite plate were assumed to be 100 mm wide and 5 mm thick. The physical properties of the spar cap were input, and the glass composite plates were arranged so that they were not adjacent in the height direction and width direction. A simulation was performed using the published wind turbine model. The analysis results showed a maximum load of 2025 MPa, exceeding the maximum load during a gust, and 495 MPa, exceeding the maximum load during a rated wind force, which were satisfactory values for withstanding the required load.
[0042] 10(a) and (b), a wind turbine model similar to that of Example 1 was created and a simulation was performed, except that the arrangement of the glass composite was unevenly distributed in the width direction of the spar cap, but was unevenly distributed in the center. As a result of the analysis, the strength of the portion where the glass composite was unevenly distributed was insufficient, and the strength was not strong enough to withstand the load assumed to be necessary in the event of a gust of wind, and sufficient strength for a wind turbine blade was not obtained.
[0043] (Comparative Example 2) A wind turbine model identical to that of Example 1 was created and a simulation was performed, except that the G / C ratio of the thickest part was changed to 0.2. As a result of the analysis, the value was not sufficient to withstand the load assumed to be necessary at rated wind force, and a fail-safe design could not be obtained.
[0044] (Comparative Example 3) A wind turbine model identical to that of Example 1 was created and a simulation was performed, except that the G / C ratio of the thickest part was changed to 1.0. As a result of the analysis, the value was not sufficient to withstand the load assumed to be necessary in the event of a gust of wind, and the strength required for a wind turbine blade was not obtained.
[0045] Comparative Example 4 A wind turbine model identical to that of Example 1 was created and a simulation was performed, except that glass fiber with a standard elastic modulus (70 GPa) was used in the glass composite. As a result of the analysis, the value was not sufficient to withstand the load assumed to be necessary at rated wind force, and a fail-safe design could not be obtained.
[0046] Comparative Example 5 A wind turbine model identical to that of Example 1 was created and simulated, except that carbon fiber (240 GPa) with a standard elastic modulus was used for the carbon composite and glass fiber (70 GPa) with a standard elastic modulus was used for the glass composite. As a result of the analysis, the values were not sufficient to withstand the load assumed to be necessary at rated wind force, and a fail-safe design could not be obtained.
[0047] (Example 2) A wind turbine model similar to that of Example 1 was created and a simulation was performed, except that the G / C ratio of the thickest part was set to 0.67. As a result of the analysis, it was found that the value was capable of withstanding the load assumed to be necessary during gusts and at rated wind force.
[0048] (Example 3) A wind turbine model similar to that of Example 1 was created and a simulation was performed, except that the G / C ratio of the thickest part was set to 0.5. As a result of the analysis, it was found that the value was capable of withstanding the load assumed to be necessary during gusts and at rated wind force.
[0049] Example 4 A wind turbine model similar to that of Example 1 was created and a simulation was performed, except that the arrangement of the carbon composite and glass composite in Example 1 was assumed to be such that the carbon composite was unevenly distributed on the inside of the blade, as shown in Figure 6. As a result of the analysis, it was found that the value was capable of withstanding the load assumed to be necessary during gusts and at rated wind force.
[0050] (Example 5) A wind turbine model similar to that of Example 1 was created and a simulation was performed, except that the arrangement of the carbon composite and glass composite in Example 1 was assumed to be such that the carbon composite was unevenly distributed on the outer side of the blade, as shown in Figure 7. As a result of the analysis, it was found that the model could withstand the load assumed to be necessary during gusts and at rated wind force.
[0051] (Example 6) A wind turbine model similar to that of Example 1 was created and a simulation was performed, except that a spar cap was assumed in which the carbon composite and glass composite were arranged so that they were unevenly distributed in the center of the spar cap height direction, as shown in Figure 8. As a result of the analysis, it was found that the value was capable of withstanding the load assumed to be necessary during gusts and at rated wind force.
[0052] Table 1 shows the composition and ratio of the composites that make up the spar cap used in the analysis, as well as the maximum load (at gusts) and fail-safe load (at rated wind force).
[0053]
[0054] 1 Wind turbine blade 11 Share web 12 Spar cap 13 Skin 2 Tower 3 Nacelle 4 Hub 121 Composite 1211 Carbon composite plate 1212 Glass composite plate 4 Hub 41 Point at which carbon fiber breakage occurs 42 Point at which glass fiber breakage occurs 43 Point at which final breakage of high-elasticity glass fiber occurs 44 Load received by blade when subjected to maximum gust of wind 45 Load received by blade at rated wind force L Wind turbine blade longitudinal length T Wind turbine blade height (thickness) 91 Wind turbine blade root 92 Wind turbine blade tip
Claims
1. A wind turbine blade having a pressure-side spar cap arranged in contact with the interior-surface of a pressure-side skin of a wind turbine blade, a contraction-side spar cap arranged in contact with the interior-surface of a contraction-side skin, and a long, plate-shaped share web arranged so that both ends are in contact with the pressure-side spar cap and the contraction-side spar cap, wherein: the pressure-side spar cap and the contraction-side spar cap are made of a composite in which composite plates containing reinforcing fibers arranged in one direction are arranged in the width direction of the wind turbine blade and stacked in the height direction and joined to each other, and at least one of the pressure-side spar cap and the contraction-side spar cap has a fail-safe area that satisfies the following 1 to 3 in a certain or larger area in the longitudinal direction of the wind turbine blade.
1. The spar cap is made by arranging and stacking multiple carbon composite plates containing carbon fibers with an elastic modulus of 250 GPa or more and multiple glass composite plates containing glass fibers with an elastic modulus of 80 GPa or more in the width direction of the wind turbine blade.
2. The spar cap has a ratio of the glass composite to the carbon composite in the lamination direction of the composite plate in the range of 0.3 to 0.
7.
3. When the cross section of the spar cap is equally divided into three regions in the width direction of the wind turbine blade, the ratio of glass composite to carbon composite in each of the three regions is within a range of −0.1 or more and +0.1 or less with respect to the average ratio of the three regions.
2. The wind turbine blade according to claim 1, wherein in the fail-safe region, the spar cap has a ratio of the glass composite to the carbon composite in the range of 0.4 to 0.
6.
3. The wind turbine blade according to claim 1 or 2, wherein in the fail-safe region, the spar caps are arranged alternately such that the glass composite plates are not adjacent to each other in the height direction and width direction of the spar cap.
4. The wind turbine blade according to claim 1 or 2, wherein in the fail-safe region, the spar cap is arranged such that the carbon composite plate is unevenly distributed in the lamination direction.
5. The wind turbine blade according to any one of claims 1 to 4, wherein the fail-safe area is present at least on the wind turbine blade root side (hub side) from the longitudinal center of the wind turbine blade.
6. A wind turbine blade according to any one of claims 1 to 5, wherein the fail-safe area exists in an area of 70% or more when the longitudinal length of the wind turbine blade is taken as 100%.
7. The wind turbine blade according to any one of claims 1 to 6, wherein the pressure side spar cap has the fail-safe area.
8. A wind turbine for wind power generation, comprising a wind turbine blade according to any one of claims 1 to 7.
Citation Information
Patent Citations
Blade for wind power generation and wind power generation device
JP2012112264A
Wind turbine rotor or wind power generator
JP2016031043A
Equipotential bonding of wind turbine rotor blade
US20220003215A1