Ultraviolet semiconductor light emitting element

The ultraviolet semiconductor light emitting device addresses the challenges of efficiency and reliability by utilizing a low dislocation density AlN substrate and a multi-quantum well structure with specific layer compositions and doping, achieving enhanced luminous efficiency and prolonged output maintenance.

WO2024203223A1PCT designated stage expired Publication Date: 2024-10-03STANLEY ELECTRIC CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009319
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-11
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional ultraviolet semiconductor light emitting devices face challenges in achieving high efficiency, high output characteristics, and high reliability, particularly when driven with large currents, leading to rapid deterioration and decreased optical output.

Method used

The device employs a substrate with a low dislocation density AlN substrate, a multi-quantum well structure with a main quantum well layer and sub-quantum well layers of the same crystal composition but varying thickness, and a p-type cladding layer with specific Al composition and doping, along with an electron blocking layer to enhance carrier injection and suppress overflow, fabricated using metal organic chemical vapor deposition (MOCVD).

Benefits of technology

This configuration results in improved luminous efficiency, increased optical output, and prolonged light output maintenance, effectively addressing the limitations of previous devices by enhancing carrier recombination and reducing nitrogen defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009319_03102024_PF_FP_ABST
    Figure JP2024009319_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides an ultraviolet semiconductor light emitting element which has high efficiency, high output characteristics and high reliability. This ultraviolet semiconductor light emitting element comprises: an n-type cladding layer which is an n-type AlXGa1-XN layer formed on a single crystal AlN substrate; a quantum well active layer which is formed on the n-type cladding layer and is composed of an AlGaN layer; an electron blocking layer which is an AlY1Ga1-Y1N layer formed on the quantum well active layer; and a p-type cladding layer which is a p-type AlY2GaN1-Y2 layer formed on the electron blocking layer. The quantum well active layer comprises: a barrier layer having the same crystal composition; and at least one sub quantum well layer and a main quantum well layer which is a quantum well layer closest to the electron blocking layer, the sub quantum well layer and the main quantum well layer being separated from each other by the barrier layer. The at least one sub quantum well layer has the same crystal composition and the same layer thickness, the sub quantum well layer and the main quantum well layer have the same crystal composition, and the main quantum well layer has a layer thickness that is not less than 1.2 times the layer thickness of the sub quantum well layer.
Need to check novelty before this filing date? Find Prior Art

Description

Ultraviolet semiconductor light emitting element

[0001] The present invention relates to an ultraviolet semiconductor light-emitting device, and more particularly to a nitride semiconductor light-emitting device that emits deep ultraviolet light.

[0002] In recent years, semiconductor light-emitting elements that emit light in the deep ultraviolet region have been attracting attention as light sources that have the effect of inactivating and sterilizing bacteria and viruses.

[0003] For example, Patent Document 1 discloses that by controlling the thickness of the quantum well layer of the active layer, the composition of the quantum well layer and the barrier layer, etc., a deep ultraviolet light-emitting device with high luminous efficiency and capable of stable operation even in a high injection current region is realized.

[0004] Furthermore, Patent Document 2 discloses a deep ultraviolet semiconductor light emitting device in which a p-type semiconductor layer is co-doped with Si.

[0005] Japanese Patent No. 6466653 Japanese Patent Application Laid-Open No. 2022-167231

[0006] In conventional ultraviolet semiconductor light-emitting devices, the stacking structure, composition, impurity concentration, layer thickness, and other aspects of each semiconductor layer have been studied, but it has been difficult to realize a device with sufficiently high efficiency and high output.

[0007] Furthermore, when driven with a large current to obtain a high optical output, the element deteriorates quickly, making it difficult to achieve both high output characteristics and high reliability (long life).

[0008] The present application has been made in view of the above problems, and has as its object to provide an ultraviolet semiconductor light-emitting element that has high efficiency, high output characteristics, and high reliability.

[0009] An ultraviolet semiconductor light emitting device according to one embodiment of the present invention comprises a substrate made of single crystal AlN; and an n-type AlN layer formed on the substrate. X Ga 1-X an n-type cladding layer which is an N layer; a quantum well active layer which is formed on the n-type cladding layer and is made of an AlGaN layer; and an AlGaN layer which is formed on the quantum well active layer. Y1 Ga 1-Y1 an electron blocking layer which is an N layer; and a p-type Al layer formed on the electron blocking layer.Y2 GaN layer 1-Y2 and a p-type cladding layer having a crystal composition of 1.2 or less, and the quantum well active layer has a barrier layer having the same crystal composition, and at least one sub-quantum well layer and a main quantum well layer which is the quantum well layer closest to the electron blocking layer and which are separated from each other by the barrier layer, the at least one sub-quantum well layer having the same crystal composition and thickness, the sub-quantum well layer and the main quantum well layer having the same crystal composition, and the main quantum well layer having a thickness which is 1.2 times or more that of the sub-quantum well layer.

[0010] 1 is a cross-sectional view schematically showing the structure of an ultraviolet semiconductor light-emitting device according to an embodiment of the present invention; 2 is a diagram schematically showing a band diagram of an ultraviolet LED; 3 is a table showing the configuration of each layer of the ultraviolet LED of the example (EMB); 4 is a table showing the layer thicknesses of the quantum well layer and barrier layer of the active layer in the ultraviolet LEDs of the example (EMB) and the comparative example (CMP); 5 is a cross-sectional STEM image of the semiconductor layers of the ultraviolet LEDs of the example and the comparative example; 6 is a diagram showing a histogram of the light output of samples of ultraviolet LEDs of the example and the comparative example; 7 is a diagram showing the forward voltage Vf and the emission wavelength λ of the ultraviolet LEDs of the example and the comparative example; 8 is a diagram showing the light output maintenance ratio relative to the initial light output of the ultraviolet LEDs of the example and the comparative example; 9 is a diagram showing the relationship between the quantum well layer thickness Lz and the ground levels of electrons and holes; 10 is a diagram schematically showing a band diagram of the active layer; 11 is a diagram showing the EL spectra of the ultraviolet LEDs of the example and the comparative example; 12 is a diagram showing the relationship between the quantum well layer thickness and the wave functions of electrons and holes; 13 is a diagram showing the relationship between the final barrier layer thickness and the initial light output; SIMS profile showing the Mg concentration in the depth direction from the p-type cladding layer to the main quantum well layer.

[0011] In the following, preferred embodiments of the present invention will be described, but these may be modified and combined as appropriate. In the following description and accompanying drawings, substantially the same or equivalent parts are designated by the same reference numerals.

[0012] 1 is a cross-sectional view schematically illustrating the structure of an ultraviolet semiconductor light-emitting element 10 according to one embodiment of the present invention. The ultraviolet semiconductor light-emitting element 10 is an ultraviolet light-emitting diode (hereinafter also referred to as an ultraviolet LED 10), and can be manufactured by, for example, but not limited to, metal-organic chemical vapor deposition (MOCVD).

[0013] The ultraviolet LED 10 has an n-type cladding layer 12 (n-type AlGaN layer), an active layer 13, an electron blocking layer 14 (p-type AlGaN layer), a p-type cladding layer 15 (p-type AlGaN layer), and a p-type contact layer 16 (p-type GaN layer) stacked in this order on a substrate 11 by epitaxial growth.

[0014] 2 is a schematic diagram showing a band diagram of the ultraviolet LED 10. The ultraviolet LED 10 will be described in more detail below with reference to FIGS.

[0015] The substrate 11 has a dislocation density of 10 8 cm -2 The AlGaN-based semiconductor material constituting the ultraviolet light-emitting device of the present invention has a dislocation density of 10 or less, as described in, for example, OPTICS EXPRESS Vol. 25 No. 16 A639 (2017). 7 ~10 8 cm -2 It is known that the luminous efficiency drops sharply when the dislocation density exceeds 10. Therefore, the lower the dislocation density of the single crystal AlN substrate, the more preferable it is. 6 cm -2 More preferably, 10 4 cm -2 By using the AlN substrate 11 with such a low dislocation density, the dislocation density in the active layer 13 (described later) can be reduced to 10% or less without reducing the light emission efficiency. 7 cm -2 It can be the following:

[0016] The growth plane (surface) of the AlN substrate 11 of the present invention is not particularly limited and can be a C-plane, M-plane, or other growth plane, but is preferably the C-plane, which is commonly used as a growth plane for AlGaN-based materials. Furthermore, when the C-plane is used as the crystal growth plane, the AlN substrate 11 is preferably an OFF substrate that is slightly inclined from the C-plane, for purposes such as improving the smoothness of the AlGaN layer grown on the substrate. The inclination angle from the C-plane is not particularly limited and may be determined as appropriate so as to obtain a smooth AlGaN layer, but is typically selected in the range of 0.1 to 1.0°. The inclination direction from the C-plane is also not particularly limited and may be selected as appropriate, such as the A-axis direction or the M-axis direction, but it is preferable to select the M-axis direction, which increases the linearity of the step edges.

[0017] Furthermore, since a large surface roughness of the AlN substrate 11 can cause abnormal growth of the AlGaN layer grown on the substrate, the surface roughness (RSM) is preferably 1.0 nm or less, and more preferably 0.5 nm or less. In order to obtain such a smooth surface or to remove damaged layers formed on the substrate surface during the substrate manufacturing process, the substrate surface is preferably subjected to chemical mechanical polishing (CMP).

[0018] Furthermore, if the absorption coefficient of the substrate for the ultraviolet light emitted from the active layer is large, the total amount of ultraviolet light that can be extracted to the outside may decrease, which may lead to a decrease in light emission efficiency. Therefore, the absorption coefficient of the AlN substrate and the AlN layer of the AlN template is preferably 20 cm -1 It is preferably 10 cm or less. -1 Less than 10cm -1 By setting the thickness as below, even if the thickness of the AlN substrate 11 is 100 μm, for example, it is possible to ensure an in-line transmittance of 90% or more.

[0019] n-type cladding layer 12 (n-type Al X Ga 1-XThe n-type AlGaN layer 12 is an n-type conductive layer doped with silicon (Si). In an ultraviolet semiconductor light-emitting element, ultraviolet light emitted from the light-emitting layer is usually transmitted through the n-type AlGaN layer 12 and the substrate 11 before being emitted to the outside. As the Al composition of the n-type AlGaN layer increases, the band gap of the n-type AlGaN layer increases, and accordingly, ultraviolet light of a shorter wavelength can be transmitted. Therefore, the Al composition of the n-type AlGaN layer can be appropriately determined so as to obtain sufficient transmittance for the desired ultraviolet light emission wavelength.

[0020] The n-type cladding layer 12 may be formed of a plurality of layers with different Al compositions (X), and may be a compositionally graded layer in which the Al composition is graded in the stacking direction. For example, the first n-type cladding layer 12A (n-type Al X1 Ga 1-X1 N layer) and the second n-type cladding layer 12B (n-type Al X2 Ga 1-X2 N layers).

[0021] The first n-type cladding layer 12A is a compositionally graded layer in which the Al composition X1 decreases from 1.0 to 0.75 in the stacking direction (growth direction), and the second n-type cladding layer 12B is a compositionally graded layer in which the Al composition X2 decreases from 0.75 to 0.70. It is preferable that the Al compositions at the interfaces of the first n-type cladding layer 12A and the second n-type cladding layer 12B are equal.

[0022] Furthermore, the thickness of the n-type cladding layer 12 is not particularly limited and may be determined appropriately. However, if the thickness of the n-type cladding layer 12 is too large, lattice relaxation occurs between the AlN substrate 11 and the n-type cladding layer 12, making dislocations more likely to occur. Therefore, it is preferable to set the total thickness of the n-type cladding layer 12 in the range of 0.5 to 2.0 μm.

[0023] For example, the n-type cladding layer 12 may be the first n-type cladding layer 12A (n-type Al X1 Ga 1-X1 N layer) and the second n-type cladding layer 12B (n-type Al X2 Ga 1-X2In the case of a laminated structure consisting of a first n-type cladding layer 12A and a second n-type cladding layer 12B, the first n-type cladding layer 12A may have a thickness of 200 nm and the second n-type cladding layer 12B may have a thickness of 1000 nm. Naturally, the thicknesses of the first and second n-type cladding layers 12A and 12B are not limited to the values ​​shown in the example, and may be appropriately determined so that the total thickness is 2.0 μm or less.

[0024] The Si concentration to be doped into the n-type cladding layer 12 may be determined appropriately so as to obtain a desired n-type conductivity. However, from the viewpoint of reducing the resistance value of the n-type cladding layer 12, it is preferable to set the Si concentration to 1×10 18 ~1 x 10 20 cm -3 It is preferable that the 18 ~5 x 10 19 cm -3 It is preferable that:

[0025] The Si doping concentration may be constant in the layer thickness direction in the n-type cladding layer 12, or may be modulation doping in which the Si concentration varies in the layer thickness direction. The Si concentration and the Mg concentration described later can be measured by known Secondary Ion Mass Spectrometry (SIMS) analysis. The Si concentration and Mg concentration in this application are measured using AlN, AlGaN, and GaN layers, respectively. 0.65 Ga 0.35 Quantitative values ​​using standard samples of N and GaN are used.

[0026] The active layer 13 (ACT) is made of Al A1 Ga 1-A1 A plurality of barrier layers 13B made of N layers and Al A2 Ga 1-A2 It has a multi-quantum well (MQW) structure consisting of three quantum well layers QS1, QS2, and QM, each of which is made up of N layers.

[0027] More specifically, the active layer 13 (ACT) has one main quantum well layer QM and two sub-quantum well layers QS1 and QS2, which are provided in this order from the substrate 11 side.

[0028] More specifically, the active layer 13 includes a first barrier layer 13B1 (thickness: TB1) provided on the n-type cladding layer 12, a second barrier layer 13B2 (thickness: TB2) provided between the first sub-quantum well layer QS1 and the second sub-quantum well layer QS2, a third barrier layer 13B3 (thickness: TB3) provided between the second sub-quantum well layer QS2 and the main quantum well layer QM, and an electron blocking layer 14 (p-type Al Y1 Ga 1-Y1 A final barrier layer 13L (layer thickness: TL) is provided between the first and second layers.

[0029] The first sub-quantum well layer QS1 and the second sub-quantum well layer QS2 have the same crystal composition and layer thickness TS. The first sub-quantum well layer QS1, the second sub-quantum well layer QS2, and the main quantum well layer QM also have the same crystal composition (A2).

[0030] In this specification, the term "same" in terms of crystal composition and layer thickness includes "substantially same" and refers to the degree of sameness obtained in the crystal growth of the semiconductor layer.

[0031] The barrier layers 13B, i.e., the first barrier layer 13B1, the second barrier layer 13B2, the third barrier layer 13B3, and the final barrier layer 13L, have the same crystal composition (A1). When there is no need to distinguish between the individual barrier layers, they will be collectively referred to as the barrier layer 13B.

[0032] It is preferable that the thickness of the barrier layer between each sub-quantum well layer (TB2 in the above case) is the same as the thickness of the barrier layer between the sub-quantum well layer closest to the main quantum well layer QM (TB3 in the above case).

[0033] The main quantum well layer QM is the quantum well layer closest to the electron blocking layer 14. The two sub-quantum well layers QS1 and QS2 have the same layer thickness TS, and the main quantum well layer QM has a layer thickness TM (TS<TM) greater than that of the sub-quantum well layers QS1 and QS2.

[0034] Although the example shows the case where two sub-quantum well layers are provided, it is sufficient to provide at least one sub-quantum well layer QS1, QS2, ..., QSn (n is an integer of 1 or more). When multiple sub-quantum well layers are provided, the multiple sub-quantum well layers have the same crystal composition and layer thickness. When multiple sub-quantum well layers are not particularly distinguished from one another, they will be collectively referred to as sub-quantum well layer QS.

[0035] The emission peak wavelength of the active layer 13 is in the range of 200 to 360 nm. The wavelength of light emitted from the active layer 13 is determined by the Al composition and layer thickness of the main quantum well layer QM, and therefore the Al composition and layer thickness can be appropriately determined so as to obtain a desired emission wavelength within the above wavelength range.

[0036] It is preferable that the emission peak wavelength of the active layer 13 is in the UVC region, which is a short wavelength region of deep ultraviolet, and particularly in the range of 200-280 nm, which has an excellent bactericidal effect.

[0037] The main quantum well layer QM, the sub-quantum well layers QS1 and QS2, and the barrier layer 13B may be n-type layers doped with Si. The main quantum well layer QM, the sub-quantum well layers QS1 and QS2, and the barrier layer 13B may be Si-doped layers, or either the main quantum well layer QM or the sub-quantum well layers QS1 and QS2 may be doped with Si, or only the barrier layer 13B may be doped with Si. The doping Si concentration is not particularly limited, but may be 1×10 17 ~5 x 10 18 cm -3 The range is preferred.

[0038] The final barrier layer 13L may contain a p-type dopant such as Mg. The Mg contained in the final barrier layer 13L is used in the electron blocking layer 14 (p-type Al Y1 Ga 1-Y1 The doping may be by diffusion from the N layer) or by intentional doping with Mg.

[0039] An electron blocking layer (EBL) 14 on the active layer 13 prevents electrons injected into the active layer 13 from being blocked by a p-type cladding layer 15 (p-type Al Y2 Ga 1-Y2 Therefore, the electron blocking layer 14 (AlN layer) has a function of suppressing overflow of the electrons. Y1 Ga 1-Y1 The electron blocking layer 14 preferably has a band gap larger than that of the active layer 13 and the p-type cladding layer 15, and the Al composition Y1 of the electron blocking layer 14 is determined in the range of 0.8<Y1≦1.0.

[0040] As the emission wavelength becomes shorter, the Al composition of the AlGaN layer epitaxially grown on the substrate 11 becomes higher, and when the emission wavelength is shorter than 270 nm, the Al composition Y1 is preferably 0.9≦Y1≦1.0 in order to fully exhibit the function as an electron blocking layer. Y1 Ga 1-Y1 The N layer 14 is made of AlN (Y1=1).

[0041] Furthermore, the electron blocking layer 14 may be an undoped layer or may be doped with a p-type dopant, as long as it can function as an electron blocking layer.

[0042] Examples of p-type dopant materials that can be used in the electron blocking layer 14 include magnesium (Mg), zinc (Zn), beryllium (Be), and carbon (C). In particular, it is preferable to use Mg, which is commonly used as a p-type dopant material for AlGaN layers, and Mg is also used in the examples of the present invention described below.

[0043] The p-type dopant material may be doped uniformly in the stacking direction of the electron blocking layer 14, or the concentration of the dopant material may vary in the stacking direction. For example, a stacked structure may be formed from an undoped AlN layer 14A (Y1=1) and a Mg (magnesium)-doped p-type AlN layer 14B in contact with the active layer. The p-type dopant concentration in the electron blocking layer 14 is set to 1.0×10 from the viewpoint of obtaining the function of the electron blocking layer and increasing the efficiency of carrier injection into the light-emitting layer. 19 ~8.0 x 10 19 cm -3 is preferably 3.0 × 10 19 ~5.0×10 19 cm -3、 Particularly preferably, 3.0 × 10 19 ~4.0×10 19 cm -3 is.

[0044] The electron blocking layer 14 preferably has a thickness in the range of 4 to 10 nm. If the thickness is less than 4 nm, the effect as an electron blocking layer is reduced due to the tunneling effect, and if the thickness is 10 nm or more, the efficiency of hole injection decreases.

[0045] p-type cladding layer 15 (p-type Al Y2 Ga 1-Y2 N layer) is p-type Al Y1 Ga 1-Y1 The electron blocking layer 14 (p-type Al) is formed on the N layer 14 and functions as a cladding layer doped with Mg. The above-mentioned materials can be used without limitation as the p-type dopant material. Y1 Ga 1-Y1 As with the N layer, it is preferable to use Mg.

[0046] In the ultraviolet light emitting device of the present invention, the Mg concentration in the p-type cladding layer 15 is 2.0×10 19 ~1.0 x 10 20 cm -3 is preferably 2.0 × 10 19 ~5.0 x 10 19 cm -3By setting the Mg concentration in the p-type cladding layer 15 within the above range, high luminous efficiency can be obtained.

[0047] p-type cladding layer 15 (p-type Al Y2 Ga 1-Y2 In the case of a structure in which Y2 is a constant value in the stacking direction, the Al composition Y2 of the p-type cladding layer 15 preferably exceeds the Al composition of the barrier layer of the active layer and is equal to or less than the Al composition Y1 of the electron blocking layer 14. By setting the Al composition Y2 of the p-type cladding layer 15 within the above range, a high carrier overflow suppression effect can be obtained even when the injection current of the ultraviolet light-emitting device is large. To achieve a higher effect, the difference between the Al composition of the barrier layer of the active layer and the Al composition Y2 of the p-type cladding layer 15 is preferably 0.5 to 1.0.

[0048] Furthermore, it is preferable that the Al composition Y2 of the p-type cladding layer 15 is larger than the Al composition of the n-type cladding layer 12, which enhances the effect of suppressing carrier overflow to the p-type layer and increases the light-emitting efficiency of the ultraviolet light-emitting element.

[0049] The p-type cladding layer 15 may also be a compositionally graded layer in which the Al composition Y2 varies in the stacking direction. In particular, a structure in which the Al composition Y2 decreases in the stacking direction from the side in contact with the electron blocking layer 14 is preferred. This provides a polarization doping effect within the p-type cladding layer 15, making it easier to obtain a higher hole concentration and, as a result, increasing the efficiency of hole injection into the active layer. For example, when the emission wavelength is 270 nm or less, the Al composition on the side in contact with the electron blocking layer 14 is preferably 0.95 to 1.0, and the Al composition in the surface layer of the p-type cladding layer 15 on the opposite side is preferably 0.60 to 0.85. Adopting such a structure enhances the polarization doping effect described above while maintaining transparency at the emission wavelength, making it easier to obtain high luminous efficiency.

[0050] The thickness of the p-type cladding layer 15 is not particularly limited, but may be appropriately determined within the range of 10 to 150 nm. If the thickness of the p-type cladding layer 15 is less than 10 nm, the aforementioned carrier overflow suppression effect is difficult to achieve. On the other hand, if the thickness is greater than 150 nm, the resistance of the p-type cladding layer 15 increases, resulting in an increase in the operating voltage of the ultraviolet light-emitting device. From this perspective, the thickness of the p-type cladding layer 15 is preferably 40 to 120 nm, and more preferably 50 to 100 nm. In this embodiment of the present invention, a compositionally graded layer is employed in which the Al composition Y2 decreases in the growth direction from the Al composition of the electron blocking layer 14 (the Al composition Y2 decreases from 1.0 to 0.8). The thickness of the p-type cladding layer 15 is 60 nm.

[0051] The p-type cladding layer 15 (p-type Al Y2 Ga 1-Y2 The p-type cladding layer 15 is co-doped with p-type impurities that act as acceptors and n-type impurities that act as donors. It is preferable that the p-type cladding layer 15 is co-doped, but this is not a limitation. Co-doping will be described below.

[0052] Examples of p-type impurities that can be used to dope the p-type cladding layer 15 include magnesium (Mg), zinc (Zn), beryllium (Be), and carbon (C). Of these, it is preferable to use Mg, which is commonly used as a p-type dopant material for AlGaN semiconductors. Examples of n-type impurities that can be used include silicon (Si), germanium (Ge), selenium (Se), sulfur (S), and oxygen (O). Of these, it is preferable to use silicon (Si), which is commonly used as an n-type dopant material.

[0053] In the p-type cladding layer 15 of this embodiment, the ratio (Nd / Na) of the n-type impurity concentration (Nd) to the p-type impurity concentration Na in the p-type cladding layer 15 satisfies the condition of formula (1).

[0054] 0.009≦(Nd / Na)<0.185 (1).

[0055] Furthermore, it is more preferable that the ratio Nd / Na satisfies either of the following formulas (2) and (3).

[0056] 0.009≦(Nd / Na)<0.135 (2).

[0057] 0.038≦(Nd / Na)<0.185 (3).

[0058] By co-doping the p-type cladding layer 15 so that the p-type impurity concentration ratio (Nd / Na) satisfies any one of the conditions of the above formulas (1) to (3), an ultraviolet LED having high luminous efficiency and good output maintenance rate (device life) is realized.

[0059] The amount of p-type impurities doped into the p-type cladding layer 15 is 1×10 17 ~1.2 × 10 20 cm -3 Furthermore, as theoretically shown in J. Applmaru Physmaru, Volmaru 95, No. 8, 15 April (2004), it is believed that the amount of nitrogen defects, which are considered to be a cause of degradation, increases with the amount of p-type impurities in the p-type cladding layer 15. Therefore, when the amount of p-type impurities is 1.2 × 10 20 cm -3 If the nitrogen vacancy amount exceeds 100%, the amount of nitrogen vacancies formed in the early stage becomes too large, making it difficult to obtain a high power retention rate.

[0060] Furthermore, when the p-type impurity concentration is low, particularly when the Al composition Y2 is constant, the hole concentration decreases and the minority carrier (electron) mobility increases, and when the Al composition Y2 is inclined, the minority carrier (electron) mobility increases, resulting in a decrease in output and making it difficult to obtain high luminous efficiency. Therefore, the p-type impurity concentration can be appropriately determined within the above range, taking such a trade-off into consideration. However, in order to obtain a higher output maintenance rate and high output, it is necessary to set the p-type impurity concentration within the above range. 19 ~5 x 10 19 cm -3 It is preferable that the concentration is 1×10 19 ~4 x 10 19 cm -3 is.

[0061] The amount of n-type impurities doped into the p-type cladding layer 15 is 1.1×10 18 Above 9.0 x 10 18 cm -3 It is preferably 1.8 × 10 or less, and more preferably 1.8 × 10 18 Above 8.0 x 10 18 cm -3 With these amounts of n-type impurities, a light emitting device 10 with high luminous efficiency can be obtained.

[0062] The concentrations of the p-type impurities and n-type impurities doped into the p-type cladding layer 15 may be constant within the layer, or may vary in concentration in the stacking direction. For example, the side in contact with the electron blocking layer 14 may be a co-doped layer, and the remaining p-type cladding layer 15 may be a layer that is not doped with n-type impurities.

[0063] A p-type contact layer 16 (p-type GaN layer) doped with a p-type dopant may be formed on the p-type cladding layer 15 in order to reduce the contact resistance with the electrode. The above-mentioned known p-type dopant materials can be used as the p-type dopant material, but for the same reason, it is preferable to use Mg. The Mg doping concentration in the p-type GaN layer 16 is not particularly limited, but in order to reduce the resistance value of the p-type GaN layer and the contact resistance, it is preferable to use a concentration of 1×10 18 ~2 x 10 20 cm -3 The thickness of the p-type GaN layer 16 is not particularly limited either, and may be appropriately determined within the range of 5 to 500 nm.

[0064] All of the AlGaN layers 12, 13, 14, and 15, except for the p-type GaN layer 16, are grown by crystal growth in a state of lattice matching with the AlN substrate 11, and therefore have a low dislocation density equivalent to that of the AlN substrate 11. 5 cm -2 The dislocation density is as follows:

[0065] Although the above description is given of the case where the ultraviolet semiconductor light emitting element of the present invention is an ultraviolet LED 10 (light emitting diode), it may also be configured as a semiconductor laser element (LD: Laser Diode).

[0066] Next, a method for manufacturing the ultraviolet LED 10 having the structure described above will be described. The ultraviolet LED 10 of the present invention can be manufactured by known crystal growth methods such as metalorganic chemical vapor deposition (MOCVD) and molecular beam epitaxy (MBE). Among these, MOCVD is preferred because it has high productivity and is widely used industrially. Known source gases can be used as the group III (Al, Ga) source gas and group V (N) source gas used in the present invention without any particular restrictions.

[0067] For example, the Group III source gas may be trimethylaluminum, triethylaluminum, trimethylgallium, triethylgallium, etc. The Group V source gas is usually ammonia.

[0068] Furthermore, known materials can be used without any restrictions as dopant source gases for Mg and Si, and examples that can be used include biscyclopentadienyl magnesium, monosilane, and tetraethylsilane.

[0069] The above-mentioned source gases are supplied onto the substrate 11 together with a carrier gas such as hydrogen and / or nitrogen to grow the element layers of the ultraviolet LED 10 .

[0070] The supply ratio of the Group III source gas to the Group V source gas (V / III ratio) may be determined appropriately so as to obtain desired characteristics, but is preferably set within the range of 500 to 10,000.

[0071] The growth temperature of the element layers constituting the UV-LED 10 is not particularly limited and may be determined appropriately so as to obtain the desired characteristics of each layer and the characteristics of the UV-LED 10. However, growth at a temperature of 1000 to 1200°C is preferred, and 1000 to 1150°C is more preferred.

[0072] In the following, the present invention will be specifically described using an example in which an ultraviolet LED 10 with an emission wavelength of 265 nm was fabricated, but the present invention is not limited to this example.

[0073] (a) Device Structure Figure 3 is a table showing the configuration of each layer of the fabricated ultraviolet LED 10 of Example (EMB). Figure 4 is a table showing the layer thicknesses of the quantum well layer and barrier layer of the active layer in the ultraviolet LED 10 of Example (EMB) and the ultraviolet LED of Comparative Example (CMP). The ultraviolet LED of Comparative Example (CMP) has the same structure as the ultraviolet LED 10 of Example (EMB), except for the layer thicknesses of the quantum well layer and barrier layer.

[0074] As shown in FIG. 4, in the ultraviolet LED 10 of the example and the ultraviolet LED of the comparative example, each quantum well layer and the final barrier layer 13L are undoped layers, and the first to third barrier layers 13B1 to 13B3 are doped with 1.0×10 18 cm -3 The final barrier layer 13L may be a doped layer. The first to third barrier layers 13B1 to 13B3 or the final barrier layer 13L are doped with Si at a concentration of 1.0×10 17 cm -3 ~5.0 x 10 18 cm -3 It is preferable that the first to third barrier layers 13B1 to 13B3 are undoped layers.

[0075] FIG. 5 shows cross-sectional scanning transmission electron microscope (STEM) images of the semiconductor layers of the example and comparative example, observed using a STEM.

[0076] As shown in Figure 5, the quantum well layers and barrier layers of the example and comparative example were evaluated using cross-sectional STEM images to confirm the layer thickness (Figure 4). The left side of the figure shows the STEM image of the comparative example (CMP), while the right side shows the STEM image of the example (EMB).

[0077] It can be seen that the thicknesses of the main quantum well layer QM and the final barrier layer 13L in the ultraviolet LED 10 of the example are each about twice as thick as those in the ultraviolet LED of the comparative example (see FIG. 4). Note that the thicknesses of the sub-quantum well layers QS1 and QS2 in the ultraviolet LED 10 of the example are approximately the same as the thicknesses of the first to third quantum well layers in the ultraviolet LED of the comparative example (FIG. 4).

[0078] (b) Device characteristics and considerations

[0079] (b-1) Light Output Characteristics FIG. 6 shows a histogram of the light output (mW) of the ultraviolet LED 10 of the example (EMB) and the ultraviolet LED sample of the comparative example (CMP), and FIG. 7 shows the forward voltage Vf and the emission wavelength λ of the ultraviolet LED 10 of the example and the ultraviolet LED sample of the comparative example.

[0080] 6, the UV LED 10 of the example had an average light output of 75 mW, which was a significant improvement over the average light output of the UV LED of the comparative example, which was 50 mW. In addition, the UV LED 10 of the example had an average external differential efficiency (EQE) of 3.1%, which was an improvement over the average external differential efficiency of 2.1% of the UV LED of the comparative example.

[0081] As shown in FIG. 7, the average value Vf (avg.) of the forward voltage Vf was 6.9 V for the ultraviolet LED 10 of the example, which was not significantly different from 7.1 V for the ultraviolet LED of the comparative example.

[0082] The average emission wavelength λ (avg.) of the ultraviolet LED 10 of the example was 265.0 nm, which was 4 nm longer than the 261.0 nm of the ultraviolet LED of the comparative example. The emission wavelength of the ultraviolet LED 10 of the example coincided with the emission wavelength due to recombination of energy between quantum levels in the main quantum well layer QM, which has a thickness twice that of the quantum well layer of the ultraviolet LED of the comparative example (i.e., the sub-quantum well layer thickness of the ultraviolet LED 10 of the example). In other words, it was found that the emission of the ultraviolet LED 10 of the example was dominated by the emission from the main quantum well layer QM.

[0083] (b-2) Reliability (Device Life) Figure 8 shows the light output maintenance rate (%), which indicates the rate of change in light output relative to the initial light output (arbitrary unit) of the ultraviolet LED 10 of the example (EMB) and the ultraviolet LED of the comparative example (CMP). More specifically, at room temperature (RT), the drive current of the device was kept constant, and the initial light output (arbitrary unit) was used as a reference, and the rate of change in light output 100 hours after the start of power application was taken as the light output maintenance rate (%). Samples with different light outputs were selected from the samples shown in Figure 6 to measure the light output maintenance rate. In addition, the p-type cladding layer 15 (p-type Al Y2 Ga 1-Y2 A comparative example (CMP0) in which the N layer is not co-doped is also plotted (shown in a dashed circle).

[0084] The light output maintenance rate of the ultraviolet LED 10 of the example is improved at all initial light outputs. In addition, the light output maintenance rate is less dependent on the initial light output, and therefore is significantly improved especially at high initial light outputs.

[0085] (c) Consideration of device structure

[0086] (c-1) Improvement of External Differential Efficiency (EQE) and Light Output First, in ultraviolet semiconductor light-emitting devices, the hole concentration in the p-type semiconductor layer is generally low, and the mobility of holes is lower than that of electrons, resulting in low external quantum efficiency and light output.

[0087] The reason for the increased light output in the ultraviolet LED 10 of this example is believed to be that the efficiency of hole injection from the p-type cladding layer 15 and the electron blocking layer 14 into the active layer 13 is increased.

[0088] That is, it is considered that by increasing the thickness of the main quantum well layer QM closest to the electron blocking layer 14, the efficiency of capturing hole carriers from the electron blocking layer 14 by the main quantum well layer QM increases, and the amount of carriers contributing to light emission increases, which in turn increases the recombination probability and the external differential efficiency (EQE) and light output.

[0089] Furthermore, as shown schematically in FIG. 9, it is believed that increasing the quantum well layer thickness Lz brings the ground levels of electrons and holes (quantum levels En1, Eh1) closer to the band edges of the quantum well, i.e., the conduction band Ec and the valence band Ev, making radiative recombination easier and increasing the light output.

[0090] (c-2) Light emission from the main quantum well layer QM is dominant. Figure 10 shows a band diagram of the active layer 13. Figure 11 shows the EL (electroluminescence) spectra of the ultraviolet LED 10 of the example (EMB) and the ultraviolet LED of the comparative example (CMP). Note that these are EL spectra when 450 mA is injected. The fact that light emission from the main quantum well layer QM is dominant in the ultraviolet LED 10 of the example will be explained below.

[0091] (i) First, as shown schematically in FIG. 10, the hole concentration in the p-type semiconductor layer is low and the mobility of holes is lower than that of electrons. Therefore, it is considered that the quantum well layer QM closest to the p-type semiconductor layer (electron blocking layer 14 in the embodiment) captures and confines most of the holes.

[0092] (ii) As mentioned above, in the ultraviolet LED 10 of the example, the thickness TM of the main quantum well layer QM was set to 7.9 nm, which is approximately twice the thickness TS (=3.9 nm) of the sub-quantum well layers QS1 and QS2. The ultraviolet LED 10 of the example emitted light with a wavelength 4 nm longer than that of the ultraviolet LED of the comparative example, and this wavelength shift coincided with the wavelength shift length in the simulation results for an increase in the quantum well layer thickness (4 nm).

[0093] (iii) As shown in FIG. 11, the full width at half maximum (FWHM) of the EL spectrum of the ultraviolet LED 10 of the example is 8.5 nm, which is not as broad as the full width at half maximum (FWHM) of the ultraviolet LED of the comparative example, which is 9.4 nm.

[0094] In other words, if the sub-quantum well layers QS1 and QS2 contribute to light emission to a certain extent, an emission peak due to emission at 261.0 nm from the sub-quantum well layers QS1 and QS2 and emission at 265.0 nm from the main quantum well layer QM should be observed, or an increase in the half-width of the EL spectrum should be observed.

[0095] However, the full width at half maximum FWHM does not increase but rather decreases in the EL spectrum of the ultraviolet LED 10 of the example, and it is therefore presumed that the light emission from the sub-quantum well layers QS1 and QS2 is very small.

[0096] The half-width (8.5 nm) of the EL spectrum of the ultraviolet LED 10 of the example was smaller than that of the ultraviolet LED of the comparative example (CMP) (9.4 nm). This is thought to be because the rate of change of the ground state relative to fluctuations in the layer thickness was lowered due to the thicker layer thickness TM of the main quantum well layer QM.

[0097] (c-3) Function of the Sub-Quantum Well Layer The following describes the function of the sub-quantum well layer QS provided in the active layer 13. Referring again to Figure 10, when the thickness TB3 of the third barrier layer 13B3 between the main quantum well layer QM and the sub-quantum well layer QS2 adjacent to the main quantum well layer QM is small (for example, several nm), electrons confined in the sub-quantum well layer QS2 tunnel due to the tunnel effect and are injected into the main quantum well layer QM, which has a low ground level.

[0098] It is believed that electron tunneling has the effect of confining and injecting carriers into the main quantum well layer QM, which has a thick well layer, and that electron tunneling can reduce electron overflow, thereby further increasing the probability of radiative recombination and increasing output power.

[0099] On the other hand, in the valence band, the hole concentration is low and the hole mobility is small, so most of the holes are captured in the third quantum well layer. Therefore, the sub-quantum well layer QS has the function of enhancing the carrier confinement in the main quantum well layer QM.

[0100] The thickness TB3 of the third barrier layer 13B3 is preferably 10 nm or less, more preferably 7 nm or less, and even more preferably 6 nm or less, from the viewpoint of electron tunneling.

[0101] (c-4) Thickness of the Main Quantum Well Layer FIG. 12 is a diagram showing the wave functions of electrons and holes when the quantum well layer thickness Lz is small (left side of the diagram) and large (right side of the diagram).

[0102] The difference in crystal composition between the quantum well layer and the barrier layer causes lattice distortion between the quantum well layer and the barrier layer, resulting in a piezoelectric field. As a result, the wave functions of electrons and holes in the quantum well layer are misaligned, reducing their overlap, which in turn reduces the probability of radiative transition and the luminous efficiency. Increasing the thickness Lz of the quantum well layer reduces the overlap of the wave functions, resulting in a decrease in the luminous efficiency.

[0103] Furthermore, when an AlGaN layer is stacked on an AlN substrate, the difference in lattice constant causes tension and compressive strain in the underlying layer. As the AlGaN layer is made thicker, lattice relaxation occurs when it reaches a critical thickness, causing threading dislocations in the AlGaN layer, reducing the internal quantum efficiency and light-emitting efficiency.

[0104] In the above embodiment, the thickness TM of the main quantum well layer QM is twice the thickness TS of the sub-quantum well layers QS1 and QS2, but the present invention is not limited to this.

[0105] Using band gap modeling software for semiconductor devices ("SiLENSe"), simulations were performed by varying the layer thicknesses of the sub-quantum well layers QS1, QS2 and the main quantum well layer QM based on the composition and layer thickness of the AlGaN stack.

[0106] According to this simulation, it was found that the internal quantum efficiency increases with increasing quantum well layer thickness, and that a thickness of 1.2 times or more the thickness of the sub-quantum well layer QS2 is effective. Furthermore, in order to fully and effectively exert the above-mentioned electron tunneling effect from the sub-quantum well layer QS2 to the main quantum well layer QM and the electron confinement effect, it is even more preferable that the thickness TM of the main quantum well layer QM be 1.5 times or more the thickness TS of the sub-quantum well layer QS (sub-quantum well layer QS2) adjacent to the main quantum well layer QM.

[0107] On the other hand, the thickness TM of the main quantum well layer QM is preferably 16 nm or less, which is the critical thickness when an AlGaN layer is stacked on an AlN substrate, and more preferably 10 nm or less, which is the range in which the overlap integral of electrons and holes takes a significant value, based on a simulation of the overlap integral of electrons and holes.

[0108] (c-5) Thickness of Final Barrier Layer Figure 13A shows the relationship between the thickness TL of the final barrier layer 13L and the initial light output. Increasing the thickness TL of the final barrier layer 13L increases the light output. This is because the hole injection efficiency decreases as the thickness of the final barrier layer 13L increases.

[0109] Therefore, the layer thickness TL of the final barrier layer 13L is preferably 30 nm or less, more preferably 27 nm or less, and even more preferably 21 nm or less.

[0110] FIG. 13B is a SIMS profile showing the concentration of Mg (p-type dopant) in the depth direction from the p-type cladding layer 15 to the main quantum well layer QM.

[0111] According to this Mg concentration profile, the Mg concentration is 1×10 within a range of 9 nm from the electron blocking layer 14 (EBL). 18 cm -3 or more. Mg is 1×10 18 cm -3 If the concentration of nitrogen vacancies is greater than or equal to 9 nm in the main quantum well layer QM, that is, if a large number of nitrogen vacancies are introduced into the main quantum well layer QM, the device life will be degraded. Therefore, it is preferable that the thickness TL of the final barrier layer 13L is 9 nm or more.

[0112] (c-6) Co-doping of p-type cladding layer The p-type cladding layer 15 (p-type Al Y2 Ga 1-Y2 The N layer is co-doped with p-type impurities that act as acceptors and n-type impurities that act as donors.

[0113] Referring again to FIG. 8 , it can be seen that the ultraviolet LED of the comparative example (CMP0, shown surrounded by a dashed line in the figure) in which the p-type cladding layer is not co-doped has a higher light output than the ultraviolet LED of the comparative example (CMP) in which the p-type cladding layer is co-doped, but the light output maintenance rate (%) is lower and reliability (device life) is worsened.

[0114] In this embodiment, Si co-doping and a thick final barrier layer 13L are used. Co-doping the p-type cladding layer 15 with Si can reduce the amount of nitrogen defects that occur in the p-type cladding layer 15. In addition, the use of a thick final barrier layer 13L has a synergistic effect of suppressing the diffusion of nitrogen defects due to heat during current application, thereby improving the optical output and reliability (device life).

[0115] Although the case where the p-type cladding layer 15 is co-doped (FIG. 4) has been described, the electron blocking layer 14 may also be co-doped.

[0116] (c-7) Emission wavelength and composition of AlGaN layer The AlGaN layer formed on the AlN substrate, i.e., the n-type cladding layer 12 (n-type Al X Ga 1-X N layer), active layer 13, electron blocking layer 14 (Al Y1 Ga 1-Y1 N layer) and p-type cladding layer 15 (p-type Al Y1 Ga 1-Y1 It is preferable that the N layer is made of AlGaN with an Al composition (X, Y1, Y2, etc.), which is the ratio of Al to the group III elements, of 100% to 50%, and the ultraviolet LED 10 is a light-emitting element that emits light in the UVC region with a wavelength of 200 to 280 nm.

[0117] The Al composition is set to 50% or more to take into account the occurrence of dislocations due to increased lattice strain in the AlN substrate. According to theoretical calculations using the energy balance model (People and Bean's equation), when the Al composition is 40% or less, the critical film thickness is 45 nm. However, since this is close to the total thickness of the active layer 13 of this embodiment (44.3 nm in the above example), it is preferable that the Al composition be 50% or more to prevent lattice relaxation from occurring within the active layer 13 and resulting in a decrease in optical output. In addition, the absorption loss when extracting deep ultraviolet light (e.g., wavelength 265 nm), which has the highest sterilization effect, from the AlN substrate side is taken into account.

[0118] As explained above in detail, according to the present invention, it is possible to provide an ultraviolet semiconductor light-emitting element that has high efficiency, high output characteristics, and high reliability.

[0119] 10: Ultraviolet semiconductor light emitting element 11: Substrate 12: n-type cladding layer (n-type AlGaN layer) 12A: First n-type cladding layer (n-type Al X1 Ga 1-X1 N layer) 12B: Second n-type clad layer (Al X2 Ga 1-X2 N layer) 13: Quantum well active layer 13B1-13B3: Barrier layers 13L: Final barrier layer 14: Electron blocking layer (p-type Al Y1 Ga 1-Y1 N layer) 15: p-type cladding layer (p-type Al Y2 Ga 1-Y2 N layer) 16: p-type contact layer (p-type GaN layer) QM: Main quantum well layer QS1, QS2: Sub-quantum well layers

Claims

1. A substrate made of single crystal AlN; and an n-type AlN layer formed on the substrate. X G 1-X an n-type cladding layer, which is an N layer; a quantum well active layer, which is an AlGaN layer, formed on the n-type cladding layer; and an AlGaN layer formed on the quantum well active layer. Y1 G 1-Y1 an electron blocking layer which is an N layer; and a p-type Al layer formed on the electron blocking layer. Y2 GaN layer 1-Y2 and a p-type cladding layer having a structure in which the quantum well active layer is a p-type cladding layer having a structure in which the quantum well active layer is a p-type cladding layer having a structure in which the quantum well active layer is a p-type cladding layer having a structure in which the quantum well active layer is a p-type cladding layer having a structure in which the quantum well active layer is a p-type cladding layer having a structure in which the quantum well active layer is a p-type cladding layer having a structure in which the quantum well active layer is a p-type cladding layer having a structure in which the quantum well active layer is a p-type cladding layer having a structure in which the quantum well active layer is a 2. The ultraviolet semiconductor light-emitting element according to claim 1, wherein the thickness of the main quantum well layer is 16 nm or less.

3. An ultraviolet semiconductor light-emitting device according to claim 1 or 2, wherein the barrier layer between the main quantum well layer and the sub-quantum well layer adjacent to the main quantum well layer has a thickness of 7 nm or less.

4. An ultraviolet semiconductor light-emitting device according to claim 1 or 2, wherein the final barrier layer between the main quantum well layer and the electron blocking layer has a thickness within the range of 9 to 27 nm.

5. An ultraviolet semiconductor light-emitting element according to claim 1 or 2, wherein the p-type cladding layer is co-doped with p-type impurities that act as acceptors and n-type impurities that act as donors.

6. An ultraviolet semiconductor light-emitting device according to claim 5, wherein the electron blocking layer is co-doped with a p-type impurity that serves as an acceptor and an n-type impurity that serves as a donor.

7. An ultraviolet semiconductor light-emitting device according to claim 1, wherein the emission wavelength of said quantum well active layer is within the range of 200 to 280 nm.

Citation Information

Patent Citations

  • Nitride-based semiconductor light emitting element

    JP2011187621A

  • Light-emitting device

    JP2013026616A

  • Light emitting device

    JP2014165498A

  • Ultraviolet semiconductor light-emitting element

    JP2022167231A

  • Light-emitting device and lighting device including the same

    US20180351039A1