Polybutylene terephthalate resin composition, method for producing same, and resin shaped article

The PBT resin composition with specific viscosity and terminal group ranges, along with epoxy-treated glass fibers, addresses hydrolysis and clogging issues, enhancing hydrolysis resistance and moldability by reducing undefibrated glass fibers, resulting in stronger and more reliable molded products.

WO2024203312A1PCT designated stage expired Publication Date: 2024-10-03POLYPLASTICS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009676
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-13
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Polybutylene terephthalate (PBT) resin compositions with glass fibers face challenges in hydrolysis resistance and clogging of injection molding machine nozzles due to undefibrated glass fiber bundles, leading to reduced strength and quality of molded products, especially in humid heat environments.

Method used

A PBT resin composition with an intrinsic viscosity of 0.70 dL/g to 1.10 dL/g and carboxylic acid terminal groups of 5 meq/kg to 18 meq/kg, combined with glass fibers surface-treated using a sizing agent containing a polymer derived from carboxylic acid and/or carboxylic acid anhydride and an epoxy resin, is used to enhance hydrolysis resistance and reduce undefibrated glass fiber bundles.

Benefits of technology

The solution significantly improves hydrolysis resistance and reduces the number of undefibrated glass fiber bundles, resulting in higher strength and improved moldability of the resin, while maintaining fluidity necessary for injection molding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

This polybutylene terephthalate resin composition comprises (A) a polybutylene terephthalate resin having an intrinsic viscosity of 0.70-1.10 dL / g, inclusive, and a carboxylic acid end group amount of 5-18 meq / kg, inclusive, and (B) glass fibers that have been surface-treated with a sizing agent containing an epoxy resin and a polymer comprising a constituent unit derived from a carboxylic acid and / or a carboxylic anhydride.
Need to check novelty before this filing date? Find Prior Art

Description

Polybutylene terephthalate resin composition, its production method, and resin molded article

[0001] The present invention relates to a polybutylene terephthalate resin composition, a method for producing the same, and a resin molded article.

[0002] Polybutylene terephthalate resin (hereinafter also referred to as "PBT resin") has excellent mechanical properties, electrical properties, heat resistance, and moldability. In particular, the addition of glass fibers improves mechanical properties and heat resistance, and therefore PBT resin is widely used in a variety of fields, including automotive parts, electrical and electronic equipment parts, and precision instrument parts. Such parts are often produced by injection molding, using a glass fiber-reinforced PBT resin composition prepared by kneading melted PBT resin, chopped-strand glass fibers, and various additives in an extruder and processing them into pellets.

[0003] On the other hand, because PBT resin contains ester groups in its molecules, it is prone to hydrolysis in high-temperature, high-humidity environments, and improved hydrolysis resistance is always desired for automotive parts, which are subject to large environmental changes. For example, PBT resin reinforced with glass fiber or the like is used in the housings of sensors and ECUs that control safety and automatic driving, and because it is combined with metal parts such as terminals and collars, it can crack due to heat shock. In particular, hydrolysis of PBT resin in a humid and hot environment accelerates cracking.

[0004] It is generally known that in order to improve the hydrolysis resistance of the PBT resin itself, an epoxy resin or a carbodiimide compound is added to reduce the amount of terminal carboxyl groups (see Patent Documents 1 and 2).

[0005] Patent Document 1 discloses a resin composition comprising a PBT resin having a terminal carboxyl group content of 30 meq / kg or less, a carbodiimide compound, a fibrous filler, and an elastomer. It also shows that, assuming the terminal carboxyl group content of the PBT resin is 1, compounding a carbodiimide functional group content of 0.3 to 1.5 equivalents improves heat shock resistance and hydrolysis resistance.

[0006] Patent Document 2 shows that hydrolysis resistance can be improved by blending an epoxy compound with a PBT resin having a terminal carboxyl group concentration of 0.1 μeq / g or more and less than 6 μeq / g and an intrinsic viscosity of 0.75 to 1 dL / g.

[0007] It is also known that the hydrolysis resistance of glass fibers themselves can be improved by using an epoxy resin as a sizing agent (see Patent Documents 3 and 4). Patent Document 3 discloses the use of glass fibers that have been surface-treated with a sizing agent containing, as essential components, an unsaturated carboxylic acid and / or a copolymer of an anhydride of an unsaturated carboxylic acid with an unsaturated monomer and an epoxy resin. Patent Document 4 discloses that surface-treated glass fibers containing a novolac-type epoxy resin have excellent long-term heat resistance.

[0008] On the other hand, for resin pellets used in injection molding, resin pellets containing glass fibers are generally prepared in the form of chopped strands, in which a plurality of glass fibers are bundled together and cut into pieces several millimeters long, for ease of feeding during extrusion. However, it is known that the glass fiber bundles are not defibrated during extrusion kneading (Patent Document 5). Patent Document 5 describes a method for preventing the glass fiber bundles from being defibrated during kneading, in which a screw and a die are inserted into the resin flow path of the extruder, each with an opening area of ​​38.47 mm. 2 It has been shown that by providing a plurality of flow paths that occupy less than 40% of the area of ​​the surface to which the openings of the plurality of flow paths belong, it is possible to prevent non-fibrillation.

[0009] International Publication No. 2009 / 150831 Japanese Patent Application Laid-Open No. 2004-277718 Japanese Patent Application Laid-Open No. 2003-201671 Japanese Patent Application Laid-Open No. 2015-129073 International Publication No. 2022 / 202096

[0010] As mentioned above, although proposals have been made to improve the hydrolysis resistance of PBT resin, the results are still insufficient and further improvement is desired. Another issue for glass fiber reinforced PBT resin is how to prevent nozzle clogging of injection molding machines and reduction in strength of molded products due to unopened glass fibers.

[0011] The present invention has been made in consideration of the above-mentioned conventional problems, and an object of the present invention is to provide a polybutylene terephthalate resin composition containing glass fibers, which has excellent hydrolysis resistance and reduced undefibrated glass fiber bundles, a method for producing the same, and a resin molded article obtained by molding the resin composition.

[0012] As a result of intensive research to solve the above problems, the present inventors have found that by using a PBT resin composition containing a PBT resin having an intrinsic viscosity of 0.70 dL / g or more and 1.10 dL / g or less and a carboxylic acid terminal group amount of 5 meq / kg or more and 18 meq / kg or less, and glass fibers that have been surface-treated with a sizing agent containing a polymer including structural units derived from carboxylic acid or the like and an epoxy resin, hydrolysis resistance is greatly improved and, further, undefibrated glass fiber bundles are reduced compared to conventional methods, leading to the completion of the present invention.

[0013] One aspect of the present invention that solves the above-mentioned problems is as follows: (1) A polybutylene terephthalate resin composition comprising: (A) a polybutylene terephthalate resin having an intrinsic viscosity of 0.70 dL / g or more and 1.10 dL / g or less and a carboxylic acid terminal group amount of 5 meq / kg or more and 18 meq / kg or less; and (B) glass fibers that have been surface-treated with a sizing agent containing an epoxy resin and a polymer including structural units derived from a carboxylic acid and / or a carboxylic acid anhydride.

[0014] (2) The polybutylene terephthalate resin composition according to (1), wherein the glass fibers (B) have an average fiber diameter of 3 to 50 μm, and the content of the sizing agent is 0.1 to 3.0 parts by mass per 100 parts by mass of the glass fibers (B).

[0015] (3) The polybutylene terephthalate resin composition according to (1) or (2) above, further comprising an elastomer (C).

[0016] (4) A resin molded article made of the polybutylene terephthalate resin composition according to (1) or (2).

[0017] (5) A method for producing the polybutylene terephthalate resin composition according to (1) or (2), comprising: a step of obtaining a polybutylene terephthalate resin (A) having an intrinsic viscosity of 0.70 dL / g or more and 1.10 dL / g or less and a carboxylic acid terminal group amount of 5 meq / kg or more and 18 meq / kg or less, using 1,4-butanediol and / or terephthalic acid obtained by chemical recycling; and a step of mixing the polybutylene terephthalate resin (A) with glass fibers (B) that have been surface-treated with a sizing agent containing an epoxy resin and a polymer including structural units derived from a carboxylic acid and / or a carboxylic acid anhydride.

[0018] (6) A method for producing the polybutylene terephthalate resin composition according to (1) or (2), comprising: a step of obtaining a polybutylene terephthalate resin (A) obtained by material recycling, the polybutylene terephthalate resin (A) having an intrinsic viscosity of 0.70 dL / g or more and 1.10 dL / g or less and an amount of carboxylic acid terminal groups of 5 meq / kg or more and 18 meq / kg or less; and a step of mixing the polybutylene terephthalate resin (A) with glass fibers (B) that have been surface-treated with a sizing agent containing an epoxy resin and a polymer including structural units derived from a carboxylic acid and / or a carboxylic acid anhydride.

[0019] According to the present invention, it is possible to provide a polybutylene terephthalate resin composition containing glass fibers, which has excellent hydrolysis resistance and reduced undefibrated glass fiber bundles, a method for producing the same, and a resin molded article obtained by molding the resin composition.

[0020] <PBT Resin Composition> The PBT resin composition of the present embodiment contains PBT resin (A) having an intrinsic viscosity of 0.70 dL / g or more and 1.10 dL / g or less and a carboxylic acid terminal group amount of 5 meq / kg or more and 18 meq / kg or less, and glass fiber (B) surface-treated with a sizing agent containing an epoxy resin and a polymer including structural units derived from a carboxylic acid and / or a carboxylic acid anhydride.

[0021] In the PBT resin composition of this embodiment, by using a PBT resin (A) having a predetermined intrinsic viscosity and a predetermined amount of carboxylic acid terminal groups and glass fiber (B) surface-treated with a predetermined sizing agent, the PBT resin composition has excellent hydrolysis resistance and reduces undisintegrated glass fiber bundles. Each component of the PBT resin composition of this embodiment will be described below.

[0022] [Polybutylene Terephthalate Resin (A)] PBT resin (A) is a PBT-based resin obtained by polycondensation of a dicarboxylic acid component containing at least terephthalic acid or an ester-forming derivative thereof (such as a C1-6 alkyl ester or an acid halide), and a glycol component containing at least an alkylene glycol having 4 carbon atoms (1,4-butanediol) or an ester-forming derivative thereof (such as an acetylated product). PBT resin (A) is not limited to homopolybutylene terephthalate resin, but may also be a copolymer containing 60 mol% or more (particularly 75 mol% to 95 mol%) of butylene terephthalate units. In this embodiment, the raw materials for the PBT resin, 1,4-butanediol and terephthalic acid or terephthalic acid alkyl ester, may be derived from either fossil resources or biomass resources.

[0023] The amount of carboxylic acid end groups in the PBT resin (A) is 5 meq / kg or more and 18 meq / kg or less, preferably 5 meq / kg or more and 13 meq / kg or less. By using a PBT resin with a carboxylic acid end group amount within this range, the resulting PBT resin composition is less susceptible to strength reduction due to hydrolysis in a humid and hot environment. Furthermore, the amount of carboxylic acid end groups is set to 5 meq / kg or more in order to ensure the dispersibility of glass fibers surface-treated with a sizing agent and to prevent the inclusion of undispersed matter. If the amount of carboxylic acid end groups is less than 5 meq / kg, the reactivity between the glass fibers and the PBT resin during melt processing decreases, thereby reducing the dispersibility of the glass fibers and making the inclusion of undispersed matter more likely.

[0024] The intrinsic viscosity (IV) of the PBT resin (A) is 0.70 dL / g or more and 1.10 dL / g or less, preferably 0.80 dL / g or more and 1.00 dL / g or less, and more preferably 0.83 dL / g or more and 0.90 dL / g or less. When a PBT resin having an intrinsic viscosity within this range is used, the resulting PBT resin composition has excellent hydrolysis resistance and moldability. When a PBT resin having an intrinsic viscosity of less than 0.70 dL / g is used, the shear stress applied to the glass fibers surface-treated with a sizing agent during melt processing is reduced. This reduces the dispersibility of the glass fibers, making them more susceptible to inclusion of undispersed material. When a PBT resin having an intrinsic viscosity greater than 1.10 dL / g is used, the glass fibers break during melt processing, resulting in a decrease in strength, and the melt viscosity increases, resulting in poor moldability. The intrinsic viscosity (IV) of the PBT resin (A) can also be adjusted by blending PBT resins having different intrinsic viscosities. For example, a PBT resin having an intrinsic viscosity of 0.85 dL / g can be prepared by blending a PBT resin having an intrinsic viscosity of 1.0 dL / g with a PBT resin having an intrinsic viscosity of 0.8 dL / g. The intrinsic viscosity (IV) of the PBT resin (A) can be measured, for example, in o-chlorophenol at 35°C.

[0025] In the PBT resin (A), examples of dicarboxylic acid components (comonomer components) other than terephthalic acid and its ester-forming derivatives include C8-14 aromatic dicarboxylic acids such as isophthalic acid, phthalic acid, 2,6-naphthalenedicarboxylic acid, and 4,4'-dicarboxydiphenyl ether; C4-16 alkanedicarboxylic acids such as succinic acid, adipic acid, azelaic acid, and sebacic acid; C5-10 cycloalkanedicarboxylic acids such as cyclohexanedicarboxylic acid; and ester-forming derivatives of these dicarboxylic acid components (C1-6 alkyl ester derivatives, acid halides, etc.). These dicarboxylic acid components can be used alone or in combination of two or more.

[0026] Among these dicarboxylic acid components, C8-12 aromatic dicarboxylic acids such as isophthalic acid, and C6-12 alkanedicarboxylic acids such as adipic acid, azelaic acid, and sebacic acid are more preferred.

[0027] In the PBT resin (A), examples of glycol components (comonomer components) other than 1,4-butanediol include C2-10 alkylene glycols such as ethylene glycol, propylene glycol, trimethylene glycol, 1,3-butylene glycol, hexamethylene glycol, neopentyl glycol, and 1,3-octanediol; polyoxyalkylene glycols such as diethylene glycol, triethylene glycol, and dipropylene glycol; alicyclic diols such as cyclohexanedimethanol and hydrogenated bisphenol A; aromatic diols such as bisphenol A and 4,4'-dihydroxybiphenyl; C2-4 alkylene oxide adducts of bisphenol A, such as an ethylene oxide 2-mol adduct of bisphenol A and a propylene oxide 3-mol adduct of bisphenol A; and ester-forming derivatives of these glycols (acetylated products, etc.). These glycol components can be used alone or in combination of two or more.

[0028] Among these glycol components, C2-6 alkylene glycols such as ethylene glycol and trimethylene glycol, polyoxyalkylene glycols such as diethylene glycol, or alicyclic diols such as cyclohexanedimethanol are more preferred. Examples of comonomer components that can be used in addition to the dicarboxylic acid component and the glycol component include aromatic hydroxycarboxylic acids such as 4-hydroxybenzoic acid, 3-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, and 4-carboxy-4'-hydroxybiphenyl; aliphatic hydroxycarboxylic acids such as glycolic acid and hydroxycaproic acid; C3-12 lactones such as propiolactone, butyrolactone, valerolactone, and caprolactone (e.g., ε-caprolactone); and ester-forming derivatives of these comonomer components (e.g., C1-6 alkyl ester derivatives, acid halides, and acetylated products).

[0029] Any of the polybutylene terephthalate copolymers obtained by copolymerizing the comonomer components described above can be suitably used as the PBT resin (A). Also, a homopolybutylene terephthalate polymer and a polybutylene terephthalate copolymer may be used in combination as the PBT resin (A).

[0030] As long as the intrinsic viscosity and the amount of carboxylic acid end groups of the PBT resin (A) are within the above ranges, recycled PBT resins can be used (material recycling). Alternatively, PBT resins can be produced by decomposing 1,4-butanediol, terephthalic acid, etc. from PBT resin waste to the monomer level (chemical recycling) and polycondensing the resulting raw materials. The manufacturing method using such PBT resins will be described later.

[0031] [Glass Fiber (B)] In the PBT resin composition of this embodiment, the glass fiber (B) is surface-treated with a sizing agent containing a polymer containing structural units derived from carboxylic acid and / or carboxylic anhydride and an epoxy resin. The inclusion of the glass fiber (B) improves the mechanical strength of the molded article, and the surface treatment with the specified sizing agent provides excellent hydrolysis resistance. Furthermore, the amount of glass fiber that remains undisintegrated due to the sizing agent can be significantly reduced.

[0032] The type of glass used as the raw material for the glass fiber (B) is not particularly limited, but in terms of quality, E-glass or corrosion-resistant glass containing zirconium element in its composition is preferably used.

[0033] The average fiber diameter of the glass fiber (B) is preferably 3 to 50 μm, more preferably 6 to 15 μm, from the viewpoints of mechanical properties and prevention of gate clogging during injection molding. The average fiber length of the glass fiber (B) is not particularly limited and can be, for example, 0.1 to 20 mm. The average fiber diameter and average fiber length of the glass fiber (B) are values ​​calculated by analyzing images of the glass fiber after blending into the resin composition taken with a CCD camera and calculating the weighted average. For example, they can be calculated using a dynamic image analysis / particle (state) analyzer PITA-3 manufactured by Seishin Enterprise Co., Ltd. The blended glass fiber (B) can be obtained, for example, by treating it in a constant temperature bath at 600°C for about 2 to 3 hours.

[0034] The glass fiber (B) can be either one having a circular cross section or one having a noncircular cross section. Examples of noncircular cross sections include oval, elliptical, and cocoon shapes. The irregularity ratio (major axis diameter:minor axis diameter) of the noncircular cross section is not particularly limited, but is preferably 1.5:1 to 6:1, more preferably 2:1 to 5:1, and even more preferably 2.5:1 to 4:1. When the irregularity ratio is in the range of 1.5:1 to 6:1, effects such as dimensional stability and reduced warpage due to the flattened cross section can be easily obtained, and a decrease in strength caused by excessive flattening and increased susceptibility to cracking can also be easily suppressed.

[0035] The glass fiber (B) may be used alone or in combination of two or more kinds.

[0036] Furthermore, glass fiber (B) and a non-fibrous inorganic filler may be used in combination. By using glass fiber (B) and a non-fibrous inorganic filler in combination, both low warpage and mechanical properties such as tensile strength can be achieved. The ratio of glass fiber (B) to non-fibrous inorganic filler is not particularly limited, but the glass fiber (B) / non-fibrous inorganic filler (mass ratio) is preferably 80 / 20 to 45 / 55, more preferably 75 / 25 to 55 / 45, and even more preferably 70 / 30 to 60 / 40. When the content of non-fibrous inorganic filler is 20% by mass or more of the glass fiber, better low warpage is likely to be obtained, and when it is 55% by mass or less, better tensile strength is likely to be obtained. The combination of glass fiber (B) and a non-fibrous inorganic filler is not particularly limited, but examples include combinations of glass fiber (B) and a non-fibrous inorganic filler such as glass flakes, mica, and talc.

[0037] Next, the polymer having a structural unit derived from a carboxylic acid and / or a carboxylic acid anhydride and the epoxy resin contained in the sizing agent used in the surface treatment of the glass fiber (B) will be described below.

[0038] (Polymer Having Structural Units Derived from Carboxylic Acid and / or Carboxylic Acid Anhydride) In the polymer having structural units derived from carboxylic acid and / or carboxylic acid anhydride (hereinafter also simply referred to as "polymer"), examples of the carboxylic acid include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, fumaric acid, maleic acid, succinic acid, cinnamic acid, itaconic acid, mesaconic acid, and citraconic acid. These may have a substituent. Among these, acrylic acid, methacrylic acid, and maleic acid are preferred. Examples of the carboxylic acid anhydride include anhydrides of unsaturated carboxylic acids such as maleic anhydride, itaconic anhydride, succinic anhydride, phthalic anhydride, glutaric anhydride, dodecenylsuccinic anhydride, and chlorendic anhydride. The above polymers may be homopolymers in which each carboxylic acid or carboxylic acid anhydride is polymerized alone, or may be copolymers in which two or more carboxylic acids or carboxylic acid anhydrides are copolymerized.

[0039] In this embodiment, the weight-average molecular weight of the polymer is not particularly limited, but is particularly preferably 10,000 to 1,000,000. When the weight-average molecular weight is within the range of 10,000 to 1,000,000, sufficient hydrolysis resistance is obtained and sufficient adhesion to the surface of the glass fiber is achieved.

[0040] (Epoxy Resin) Examples of epoxy resins include glycidyl ether type epoxy resins, glycidyl ester type epoxy resins (diglycidyl phthalate, diglycidyl tetrahydrophthalate, diglycidyl hexahydrophthalate, dimethylglycidyl phthalate, dimethylglycidyl hexahydrophthalate, dimer acid glycidyl ester, aromatic diglycidyl ester, cycloaliphatic diglycidyl ester, etc.), glycidyl amine type epoxy resins (tetraglycidyldiaminodiphenylmethane, triglycidyl-paraaminophenol, triglycidyl-methamine), and the like. phenol, diglycidyl toluidine, tetraglycidyl metaxylylenediamine, diglycidyl tribromoaniline, tetraglycidyl bisaminomethylcyclohexane, etc.), heterocyclic epoxy resins (triglycidyl isocyanurate (TGIC), hydantoin-type epoxy resins, etc.), cycloaliphatic epoxy resins (vinylcyclohexene dioxide, dicyclopentadiene oxide, alicyclic diepoxy acetal, alicyclic diepoxy adipate, alicyclic diepoxy carboxylate, etc.), epoxidized polybutadiene, etc.

[0041] Glycidyl ether type epoxy resins include glycidyl ethers of polyhydroxy compounds [glycidyl ethers of aromatic polyhydroxy compounds such as bisphenol type epoxy resins (e.g., bisphenol A type, bisphenol AD ​​type, or bisphenol F type epoxy resins), resorcinol type epoxy resins, etc.; aliphatic epoxy resins (glycidyl ethers of alkylene glycols, polyoxyalkylene glycols, etc.)], novolac type epoxy resins (phenol novolac type, cresol novolac type epoxy resins, etc.), and the like.

[0042] Among epoxy resins, aromatic epoxy resins (such as bisphenol-type epoxy resins, resorcinol-type epoxy resins, and phenol novolac-type epoxy resins) and cyclic aliphatic epoxy resins are preferred, and glycidyl ether-type aromatic epoxy resins, such as bisphenol-type epoxy resins and phenol novolac-type epoxy resins, are particularly preferred.

[0043] The epoxy equivalent of the epoxy resin may be, for example, about 100 to 1600 g / eq, preferably about 100 to 800 g / eq, and more preferably about 150 to 500 g / eq.

[0044] The number average molecular weight of the epoxy resin may be, for example, about 200 to 50,000, preferably about 300 to 10,000, and more preferably about 400 to 6,000.

[0045] In this embodiment, the mass ratio (X / Y) of the polymer (X) to the epoxy resin (Y) in the sizing agent is preferably 0.001 to 1.500 from the viewpoint of improving the mechanical strength of the molded product.

[0046] The sizing agent is preferably contained in an amount of 0.1 to 3.0 parts by mass, more preferably 0.3 to 2.5 parts by mass, per 100 parts by mass of the glass fibers (B). By containing the sizing agent in an amount of 0.1 to 3.0 parts by mass, hydrolysis resistance can be improved.

[0047] In addition to the above components, the sizing agent may contain other components such as urethane resin, silane coupling agent, lubricant, nonionic surfactant, antistatic agent, etc., and the blending ratio of each component may be determined as needed. The urethane resin contributes to the bundling and dispersibility of the glass fibers and is obtained from polyisocyanate and polyol, etc. As the silane coupling agent, aminosilane, epoxysilane, chlorosilane, mercaptosilane, vinylsilane, acrylicsilane, etc. can be used. As the lubricant, fatty acid amide, quaternary ammonium salt, etc. can be used. As the nonionic surfactant, synthetic alcohol, natural alcohol, fatty acid ester, etc. can be used.

[0048] In the PBT resin composition of the present embodiment, the glass fiber (B) is preferably contained in an amount of 10 to 100 parts by mass, and more preferably 20 to 80 parts by mass, per 100 parts by mass of the PBT resin (A).

[0049] [Elastomer (C)] The PBT resin composition of the present embodiment preferably further contains an elastomer (C). By containing the elastomer (C), it is possible to improve the heat shock resistance required when a molded article made of the PBT resin composition is used in an environment where heating and cooling are repeated.

[0050] The elastomer (C) imparts toughness to the PBT resin composition, thereby absorbing distortions that occur in the molded article. It is preferable to use a resin that not only has a small shrinkage rate and / or linear expansion coefficient during molding or heat treatment, but also has good compatibility with the PBT resin (A). Examples of such elastomers (C) include olefin-based elastomers, diene-based elastomers, core-shell elastomers, styrene-based elastomers, silicone-based elastomers, and combinations thereof. Among these, olefin-based elastomers and core-shell elastomers are preferred because they provide excellent heat shock resistance. In addition, known compatibilizers may be used in combination to improve the affinity between these elastomers (C) and the PBT resin (A).

[0051] Examples of olefin-based elastomers include ethylene-propylene copolymers (EP copolymers), ethylene-butene copolymers, ethylene-octene copolymers, ethylene-propylene-diene copolymers (EPD copolymers), ethylene-propylene-butene copolymers, ethylene-vinyl acetate copolymers, copolymers containing at least one unit selected from EP copolymers and EPD copolymers, and copolymers of olefins and (meth)acrylic monomers (ethylene-ethyl acrylate copolymers, ethylene-glycidyl methacrylate copolymers, etc.). Preferred olefin-based elastomers include EP copolymers, EPD copolymers, and copolymers of olefins and (meth)acrylic monomers, with ethylene-ethyl acrylate being particularly preferred. These olefin-based elastomers can be used alone or in combination.

[0052] A core-shell elastomer is a polymer in which the core layer is composed of a rubber component (soft component) and the shell layer is composed of a hard component, and the rubber component of the core layer is an acrylic rubber, etc. The rubber component used in the core layer preferably has a glass transition temperature (Tg) of less than 0°C (e.g., −10°C or less), more preferably −20°C or less (e.g., −180°C or more and −25°C or less), and particularly preferably −30°C or less (e.g., −150°C or more and −40°C or less).

[0053] When an acrylic rubber is used as the rubber component, a polymer obtained by polymerizing an acrylic monomer such as alkyl acrylate as the main component is preferred. The alkyl acrylate used as the monomer for the acrylic rubber is preferably a C1 to C12 alkyl ester of acrylic acid such as butyl acrylate, and more preferably a C2 to C6 alkyl ester of acrylic acid.

[0054] The acrylic rubber may be a homopolymer or copolymer of an acrylic monomer. When the acrylic rubber is a copolymer of an acrylic monomer, it may be a copolymer of acrylic monomers or a copolymer of an acrylic monomer and another unsaturated bond-containing monomer. When the acrylic rubber is a copolymer, it may be copolymerized with a crosslinkable monomer.

[0055] Vinyl polymers are preferably used for the shell layer. Vinyl polymers are obtained, for example, by polymerizing or copolymerizing at least one monomer selected from aromatic vinyl monomers, vinyl cyanide monomers, methacrylic acid ester monomers, and acrylic acid ester monomers. The core and shell layers of such core-shell elastomers may be bonded by graft copolymerization. This graft copolymerization can be achieved, if necessary, by adding a graft crossing agent that reacts with the shell layer during polymerization of the core layer, providing reactive groups to the core layer, and then forming the shell layer. When a silicone rubber is used as the graft crossing agent, an organosiloxane having a vinyl bond or an organosiloxane having a thiol group is used, preferably an acryloxysiloxane, a methacryloxysiloxane, or a vinylsiloxane.

[0056] [Epoxy Compound] In the PBT resin composition of this embodiment, an epoxy compound can be used as an additive to further improve hydrolysis resistance. Examples of the epoxy compound in this embodiment include aromatic epoxy compounds such as biphenyl-type epoxy compounds, bisphenol A-type epoxy compounds, phenol novolac-type epoxy compounds, and cresol novolac-type epoxy compounds. Two or more types of epoxy compounds may be used in any combination. The epoxy equivalent is preferably 200 to 1500 g / equivalent (g / eq).

[0057] In this embodiment, the epoxy compound is preferably added in an amount of 0.5 to 5 parts by mass per 100 parts by mass of the PBT resin (A). A content of 0.5 parts by mass or more can improve hydrolysis resistance, while a content of 5 parts by mass or less can suppress the generation of char during molding and can prevent unfilled or discolored components due to increased viscosity.

[0058] [Other Components] The PBT resin composition of the present embodiment may contain other components as needed, including, but not limited to, inorganic fillers other than the glass fiber (B), antioxidants, weather stabilizers, molecular weight modifiers, ultraviolet absorbers, antistatic agents, dyes, pigments, lubricants, crystallization accelerators, crystal nucleating agents, near-infrared absorbers, flame retardants, flame retardant assistants, organic fillers, and colorants.

[0059] The PBT resin composition of the present embodiment described above has a reduced amount of unopened glass fiber bundles, and therefore the dispersibility of the glass fibers is improved. In addition, the fluidity of the PBT resin composition is determined in accordance with ISO 11443, under conditions of a furnace temperature of 260°C, a capillary diameter of 1 mm, a length of 20 mm, and a shear rate of 1000 sec. -1 The melt viscosity measured by is preferably 0.15 kPa·s or more and 0.30 kPa·s or less, more preferably 0.16 kPa·s or more and 0.25 kPa·s or less, and even more preferably 0.17 kPa·s or more and 0.23 kPa·s or less. By setting the melt viscosity to 0.30 kPa·s or less, the fluidity required for injection molding can be ensured, the dispersibility of glass fibers can be excellent, and breakage of glass fibers can be suppressed. Therefore, the PBT resin composition of this embodiment has high strength and excellent appearance. Furthermore, by setting the melt viscosity to 0.16 kPa·s or more, undispersed glass fibers can be reduced.

[0060] <Resin Molded Article> The resin molded article of this embodiment is obtained by molding the PBT resin composition of this embodiment described above. Therefore, similar to the PBT resin composition of this embodiment, the resin molded article has the effects of significantly improving hydrolysis resistance compared to conventional resins and containing no or few undefibrated glass fibers.

[0061] The method for producing a resin molded article using the PBT resin composition of the present embodiment is not particularly limited, and any known method can be used. For example, the PBT resin composition of the present embodiment can be fed into an extruder, melt-kneaded, and pelletized, and the pellets can be fed into an injection molding machine equipped with a predetermined mold and injection-molded to produce a resin molded article.

[0062] The resin molded article of this embodiment can be suitably used as a resin composition for molded articles exposed to high-temperature, high-humidity environments for long periods of time, such as in automobiles, trains, and the aviation industry. Molded articles made from this resin composition can prevent degradation due to hydrolysis even when used for long periods of time in sufficiently high-temperature, high-humidity environments, and because of its excellent fluidity, it can be used in narrow, thin-walled relays and connectors. In particular, the reduction in undispersed glass fibers reduces filling defects due to clogging in thin-walled sections and the protrusion of undispersed glass fiber bundles on the surface of the molded article. Furthermore, when an elastomer is incorporated, the improved heat shock resistance allows the resin composition to be used in electrical components such as ECUs, housings, and sensors installed around vehicle engines, motors, and batteries.

[0063] <Method for producing polybutylene terephthalate resin composition> There are two methods for producing the PBT resin composition of this embodiment, a first method and a second method, both of which are methods for producing the PBT resin composition of this embodiment. The first method includes a step of obtaining a PBT resin (A) having an intrinsic viscosity of 0.70 dL / g or more and 1.10 dL / g or less and a carboxylic acid terminal group amount of 5 meq / kg or more and 18 meq / kg or less, using 1,4-butanediol and / or terephthalic acid obtained by chemical recycling, and a step of mixing the PBT resin (A) with glass fiber (B).

[0064] In addition, the second embodiment includes a step of obtaining a PBT resin (A) obtained by material recycling, the PBT resin (A) having an intrinsic viscosity of 0.70 dL / g or more and 1.10 dL / g or less and an amount of carboxylic acid terminal groups of 5 meq / kg or more and 18 meq / kg or less, and a step of mixing the PBT resin (A) with glass fiber (B).

[0065] In the first and second embodiments described above, PBT resin (A) is obtained by chemical recycling and material recycling, respectively, but the production of the PBT resin composition of the present embodiment is not limited to the production methods according to the first and second embodiments. That is, there are no limitations on the method for obtaining PBT resin (A) as long as a PBT resin having an intrinsic viscosity of 0.70 dL / g or more and 1.10 dL / g or less and a carboxylic acid terminal group amount of 5 meq / kg or more and 18 meq / kg or less can be obtained.

[0066] The first and second embodiments differ in the process for obtaining the PBT resin (A). That is, in the first embodiment, the PBT resin (A) is obtained using 1,4-butanediol and / or terephthalic acid obtained by chemical recycling, whereas in the second embodiment, the PBT resin (A) is obtained by material recycling.

[0067] In both the first and second embodiments, PBT resin, which is waste plastic, can be reused, which contributes to saving natural resources and reducing the environmental burden.

[0068] In the first embodiment, PBT resin (A) is produced by decomposing 1,4-butanediol, terephthalic acid, etc. from PBT resin waste or the like down to the monomer level (chemical recycling), and then polycondensing the obtained raw materials. In chemical recycling, PBT resin and alcohols are filled into a reaction vessel and heated to depolymerize the alcohols under supercritical conditions, and 1,4-butanediol and terephthalic acid can be recovered.

[0069] In the second embodiment, PBT resin (A) is obtained by material recycling. That is, recycled products can be used as long as the intrinsic viscosity and the amount of carboxylic acid end groups are within the specified ranges. Recycled products can be crushed using a crusher such as a single-screw crusher, twin-screw crusher, triple-screw crusher, or cutter mill. The crushed product can also be melt-kneaded using a single-screw or twin-screw extruder, granulated, and used as pellets. Furthermore, a stainless steel filter can be installed on the breaker plate during melt-kneading to remove foreign matter. Because foreign matter can be the starting point for fracture, removing the foreign matter can maintain the mechanical properties and improve the appearance of molded articles made from the PBT resin composition.

[0070] In any embodiment, there are no particular limitations on the production method as long as the step of obtaining PBT resin (A) can provide a PBT resin having an intrinsic viscosity of 0.70 dL / g or more and 1.10 dL / g or less and a carboxylic acid terminal group amount of 5 meq / kg or more and 18 meq / kg or less.

[0071] In the step of mixing components (A) and (B), the method for mixing the components is not particularly limited, and any known method can be used, such as a method in which the components are fed into an extruder, melt-kneaded, and pelletized.

[0072] The present embodiment will be described in more detail below with reference to examples, but the present embodiment is not limited to the following examples.

[0073] [Examples 1-8, Comparative Examples 1-6] In each Example and Comparative Example, components (A) to (C) were melt-kneaded and extruded in the ratios (parts by mass) shown in Tables 2-3 using a 30 mm diameter twin-screw extruder (TEX30C, manufactured by The Japan Steel Works, Ltd.) at a cylinder temperature of 260°C at the raw material supply section and die tip, and 220-260°C between them, at a discharge rate of 15 kg / h and a screw rotation speed of 130 rpm to obtain pellets of a PBT resin composition. For the evaluation of undispersed materials described below, the components were melt-kneaded and extruded at a screw rotation speed of 70 rpm to obtain pellets of a PBT resin composition. Details of each component shown in Tables 2-3 are provided below.

[0074] (1) PBT Resin: (A-1): PBT resin manufactured by Polyplastics Co., Ltd. Intrinsic viscosity: 0.86 dL / g Amount of carboxylic acid terminal groups: 12 meq / kg (A-2): PBT resin manufactured by Polyplastics Co., Ltd., obtained by drying DURANEX 500FP at 140°C for 3 hours and then preparing a 1A type ISO test piece (width 10 mm, thickness 4 mm) in accordance with ISO 3167 using an injection molding machine "ROBOSHOT S-2000i 100B" manufactured by FANUC Corporation at a cylinder temperature of 260°C and a mold temperature of 80°C, and pulverizing the obtained ISO test piece in a small pulverizer. Intrinsic viscosity: 0.89 dL / g, amount of carboxylic acid end groups: 14 meq / kg (A-3): PBT resin manufactured by Polyplastics Co., Ltd., intrinsic viscosity: 0.91 dL / g, amount of carboxylic acid end groups: 7 meq / kg (A-4): PBT resin manufactured by Polyplastics Co., Ltd., intrinsic viscosity: 0.86 dL / g, amount of carboxylic acid end groups: 3 meq / kg (A-5): PBT resin manufactured by Polyplastics Co., Ltd., intrinsic viscosity: 0.86 dL / g, amount of carboxylic acid end groups: 20 meq / kg (A-6): PBT resin manufactured by Polyplastics Co., Ltd., intrinsic viscosity: 0.66 dL / g, amount of carboxylic acid end groups: 13 meq / kg

[0075] (4) Glass Fiber (B) (B-1) Glass fiber: E-glass glass fiber, average fiber diameter 13 μm (sizing agent: phenol novolac resin 0.5% by mass, copolymer of maleic anhydride, methyl methacrylate and methyl acrylate (0.2% by mass)) (B-2) Glass fiber: E-glass glass fiber, average fiber diameter 13 μm (sizing agent: phenol novolac resin 0.5% by mass) (B-3) Glass fiber: E-glass glass fiber, average fiber diameter 13 μm (sizing agent: copolymer of maleic anhydride, methyl methacrylate and methyl acrylate (0.2% by mass))

[0076] Meanwhile, the components of the sizing agent used in the surface treatment of glass fibers (B-1) to (B-3) are shown in Table 1. The values ​​in Table 1 indicate the content (mass%) of each component relative to the total weight of the glass fiber. The content of the sizing agent relative to 100 parts by weight of the glass fiber is 0.7 parts by weight for glass fiber (B-1), 0.5 parts by weight for glass fiber (B-2), and 0.2 parts by weight for glass fiber (B-3).

[0077]

[0078] (5) Elastomer (C) (C-1) Elastomer: Ethylene ethyl acrylate copolymer NUC-6570 manufactured by ENEOS NUC Corporation (C-2) Elastomer: Core-shell elastomer Paraloid EXL-2311 manufactured by Dow Chemical Co., Ltd. (6) Epoxy compound: Epicoat 1004 manufactured by Mitsubishi Chemical Corporation

[0079] [Evaluation] The pellets obtained in each of the Examples and Comparative Examples were subjected to the following evaluation tests.

[0080] (1) Hydrolysis Resistance PBT resin composition pellets of each Example and Comparative Example obtained with the compositions shown in Tables 2 and 3 were dried at 140°C for 3 hours and then injection molded at a cylinder temperature of 260°C and a mold temperature of 80°C to prepare 1A-type tensile test specimens in accordance with ISO 3167. The resulting test specimens were subjected to tensile strength measurements in accordance with ISO 527-1 and 2. The measurement results are shown in Tables 2 and 3. Next, using a PCT processing device (highly accelerated life test device), the test specimens were exposed to 121°C and 100% RH, and the tensile strength was measured after a moist heat test (50 hours, 100 hours, and 150 hours), and the strength retention before and after the moist heat test was calculated. The calculation results are shown in Tables 2 and 3. (2) Number of Undefibrated Pellets 1 kg of PBT resin composition pellets of each Example and Comparative Example obtained with the compositions shown in Tables 2 and 3 was spread in a single layer and visually observed, and the number of pellets in which glass fiber clumps were observed on the pellet surface or cross section was counted. The measurement results for each composition are shown in Tables 2 and 3. (3) Melt Viscosity The PBT resin composition pellets of each Example and Comparative Example obtained with the composition in Tables 2 and 3 were dried at 140°C for 3 hours, and then measured in accordance with ISO 11443 using a Capillograph 1B (manufactured by Toyo Seiki Seisakusho, Ltd.) at a furnace temperature of 260°C, a capillary diameter of 1 mm x 20 mmL, and a shear rate of 1000 sec. -1The melt viscosity was measured at 140°C. A melt viscosity of 0.30 kPa·s or less can be said to indicate low melt viscosity and good fluidity. (4) Heat Shock Resistance The PBT resin composition pellets of each Example and Comparative Example obtained with the compositions in Tables 2 and 3 were dried at 140°C for 3 hours, and then insert injection molded into a test piece molding mold (a mold in which an iron core measuring 18 mm in length, 18 mm in width, and 30 mm in height is inserted into a square pillar measuring 22 mm in length, 22 mm in width, and 51 mm in height) at a resin temperature of 260°C, a mold temperature of 65°C, an injection time of 25 seconds, and a cooling time of 10 seconds, so that the minimum thickness of the resin portion of the molded product was 1 mm, to produce an insert molded product. The obtained insert molded product was subjected to a heat shock resistance test using a thermal shock tester, in which one cycle consisted of heating at 140°C for 1 hour and 30 minutes, cooling to -40°C and cooling for 1 hour and 30 minutes, and then heating again to 140°C. The number of cycles until cracks appeared in the insert molded product was measured, and the heat shock resistance was evaluated.

[0081]

[0082]

[0083] Tables 2 and 3 show that Examples 1 to 8 obtained favorable evaluation results for hydrolysis resistance and glass fiber bundle defibration. On the other hand, Comparative Example 1, which differs from Example 1 only in that it used glass fiber (B-2) surface-treated with a phenol novolac resin sizing agent, and Comparative Example 2, which differs from Example 1 only in that it used glass fiber (B-3) surface-treated with a sizing agent containing only a copolymer of maleic anhydride, methyl methacrylate, and methyl acrylate, were inferior in hydrolysis resistance. Comparative Example 4, which used PBT resin (A-5) with a high amount of carboxylic acid end groups, and Comparative Example 6, which used PBT resin (A-4) with a low amount of carboxylic acid end groups, were inferior in hydrolysis resistance. Furthermore, Comparative Example 3, which used PBT resin (A-4) with a low amount of carboxylic acid end groups, and Comparative Example 5, which used PBT resin (A-6) with a low intrinsic viscosity, were inferior in glass fiber bundle defibration. In addition, Examples 5 to 8, in which the elastomer (C) was added, were excellent in heat shock resistance as well as hydrolysis resistance and defibration property of glass fiber bundles.

Claims

1. A polybutylene terephthalate resin composition comprising: (A) a polybutylene terephthalate resin having an intrinsic viscosity of 0.70 dL / g or more and 1.10 dL / g or less and a carboxylic acid end group amount of 5 meq / kg or more and 18 meq / kg or less; and (B) glass fibers that have been surface-treated with a sizing agent containing a polymer including structural units derived from a carboxylic acid and / or a carboxylic acid anhydride and an epoxy resin.

2. The polybutylene terephthalate resin composition according to claim 1, wherein the glass fibers (B) have an average fiber diameter of 3 to 50 μm, and the content of the sizing agent per 100 parts by mass of the glass fibers (B) is 0.1 to 3.0 parts by mass.

3. The polybutylene terephthalate resin composition according to claim 1 or 2, further comprising an elastomer (C).

4. A resin molded product made of the polybutylene terephthalate resin composition according to claim 1 or 2.

5. A method for producing the polybutylene terephthalate resin composition according to claim 1 or 2, comprising the steps of: obtaining polybutylene terephthalate resin (A) having an intrinsic viscosity of 0.70 dL / g or more and 1.10 dL / g or less and a carboxylic acid terminal group amount of 5 meq / kg or more and 18 meq / kg or less, from 1,4-butanediol and / or terephthalic acid obtained by chemical recycling; and mixing the polybutylene terephthalate resin (A) with glass fiber (B) that has been surface-treated with a sizing agent containing a polymer including structural units derived from a carboxylic acid and / or a carboxylic acid anhydride and an epoxy resin.

6. A method for producing the polybutylene terephthalate resin composition according to claim 1 or 2, comprising the steps of: obtaining polybutylene terephthalate resin (A) obtained by material recycling and having an intrinsic viscosity of 0.70 dL / g or more and 1.10 dL / g or less and a carboxylic acid terminal group amount of 5 meq / kg or more and 18 meq / kg or less; and mixing the polybutylene terephthalate resin (A) with glass fiber (B) that has been surface-treated with a sizing agent containing a polymer containing a structural unit derived from a carboxylic acid and / or a carboxylic acid anhydride and an epoxy resin.

Citation Information

Patent Citations

  • Fiber reinforced resin composition having smooth surface

    JP1994049344A

  • Chopped glass strand and glass fiber-reinforced thermoplastic resin produced by using the strand as reinforcing material

    JP2003201671A

  • Polybutylene terephthalate resin composition

    JP2022066646A

  • Molding material, molded body of same, and method for producing molded body

    WO2013183636A1

  • Polyalkylene terephthalate resin composition and resin molded article

    WO2023248879A1