Photocurable composition for pressure-sensitive adhesive sheet, pressure-sensitive adhesive sheet, optical laminate, and image display device

The photocurable composition with a specific ratio of photoinitiators addresses the issue of adhesive sheet peeling and foaming in high-temperature environments by enhancing the polymerization rate and molecular weight of the adhesive, improving the reliability and image quality of image display devices.

WO2024203367A1PCT designated stage expired Publication Date: 2024-10-03NITTO DENKO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009903
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-13
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Image display devices, particularly those with optical laminates, face issues with image quality due to adhesive sheet peeling and monomer foaming at high temperatures, which affects the reliability of the optical laminate in high-temperature environments.

Method used

A photocurable composition combining a monomer group, a first photoinitiator with a relatively small reaction rate, and a second photoinitiator with a larger reaction rate, where the ratio of the second reaction rate to the first is 1.1 or more, is used to form a pressure-sensitive adhesive sheet with improved polymerization rates and molecular weights, enhancing the adhesive's thermal stability and resistance to peeling.

Benefits of technology

The composition effectively suppresses peeling and foaming of the adhesive sheet at high temperatures, improving the reliability and image quality of image display devices by increasing the molecular weight and polymerization rate of the adhesive, thereby enhancing stress relaxation properties and maintaining adhesive integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009903_03102024_PF_FP_ABST
    Figure JP2024009903_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a photocurable composition comprising monomers and / or a product of partial polymerization of the monomers, a first photopolymerization initiator, and a second photopolymerization initiator. The first photopolymerization initiator and the second photopolymerization initiator respectively have a first reaction rate, which is relatively low, and a second reaction rate, which is relatively high. The ratio of the second reaction rate to the first reaction rate is 1.1 or greaterin in terms of the ratio between respective polymerization rates A evaluated by a determination method in which the photopolymerization initiators are each used alone. This photocurable composition is suitable for the formation of a pressure-sensitive adhesive sheet which has a reduced residual monomer content and is suitable for use in an image display device that can be exposed to high-temperature environments.
Need to check novelty before this filing date? Find Prior Art

Description

Photocurable composition for pressure-sensitive adhesive sheet, pressure-sensitive adhesive sheet, optical laminate, and image display device

[0001] The present invention relates to a photocurable composition for a pressure-sensitive adhesive sheet, a pressure-sensitive adhesive sheet, an optical laminate, and an image display device.

[0002] Various image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices, generally include an optical laminate including an optical film such as a polarizing film and an adhesive sheet. An adhesive sheet is typically used to bond the optical films included in the optical laminate or to bond the optical laminate to an image display panel. A typical adhesive sheet is a sheet obtained by curing a group of monomers, such as an acrylic monomer or a silicone monomer, through polymerization and crosslinking. Patent Document 1 discloses an adhesive sheet formed from a photocurable composition (hereinafter referred to as a photocurable adhesive sheet).

[0003] Japanese Patent Application Laid-Open No. 2019-70150

[0004] When a photocurable pressure-sensitive adhesive sheet is used in an optical laminate, problems tend to occur in the quality of images displayed in an image display device that may be exposed to a high-temperature environment.

[0005] An object of the present invention is to provide a pressure-sensitive adhesive sheet suitable for use in an image display device that may be exposed to a high-temperature environment, and a photocurable composition capable of forming the pressure-sensitive adhesive sheet.

[0006] The present inventors have focused on the photopolymerization initiator contained in the photocurable composition and found that the above-mentioned problems can be solved by combining photopolymerization initiators with different reaction rates.

[0007] That is, the present invention provides a photocurable composition for pressure-sensitive adhesive sheets, comprising a group of monomers and / or a partial polymer of the group of monomers, a first photopolymerization initiator, and a second photopolymerization initiator, wherein the first photopolymerization initiator and the second photopolymerization initiator have a relatively small first reaction rate and a relatively large second reaction rate, respectively, and the ratio of the second reaction rate to the first reaction rate is 1.1 or greater, expressed as the ratio of polymerization rates A evaluated by the following measurement method using only each of the photopolymerization initiators. [Measurement Method] A mixed solution containing 99 parts by weight of n-butyl acrylate and 1 part by weight of 4-hydroxybutyl acrylate as monomers, and 0.1 parts by weight of the photopolymerization initiator to be evaluated, is irradiated with ultraviolet light to prepare a monomer syrup in which the monomers are partially polymerized. The ultraviolet light irradiation is continued until the viscosity of the mixed solution at 30°C reaches 20 Pa·s. Next, a 20 μm thick coating layer made of the prepared monomer syrup is formed between a pair of polyethylene terephthalate (PET) sheets, each having a thickness of 75 μm. Next, the coating layer is irradiated with ultraviolet light from an LED light source having a peak wavelength of 340 nm±10 nm from one of the PET sheets. The illuminance and irradiation time of the irradiated ultraviolet light are 4 mW / cm. 2 and 1200 seconds. The polymerization rate A is determined by measuring the polymerization rate of the monomer in the coating layer photocured by the irradiation of ultraviolet light.

[0008] The present invention further provides a pressure-sensitive adhesive sheet formed from the above photocurable composition.

[0009] The present invention further provides an optical laminate comprising the above pressure-sensitive adhesive sheet and an optical film.

[0010] The present invention further provides an image display device comprising the above optical laminate.

[0011] According to the present invention, it is possible to provide a pressure-sensitive adhesive sheet suitable for use in an image display device that may be exposed to a high-temperature environment, and a photocurable composition capable of forming the pressure-sensitive adhesive sheet.

[0012] FIG. 1 is a cross-sectional view schematically showing an example of a pressure-sensitive adhesive sheet of the present invention. FIG. 2 is a schematic view for explaining an example of a method for forming the pressure-sensitive adhesive sheet of the present invention from the photocurable composition of the present invention. FIG. 3 is a cross-sectional view schematically showing an example of an optical laminate of the present invention. FIG. 4 is a cross-sectional view schematically showing an example of an optical laminate of the present invention. FIG. 5 is a cross-sectional view schematically showing an example of an optical laminate of the present invention. FIG. 6 is a cross-sectional view schematically showing an example of an image display device of the present invention.

[0013] A photocurable composition according to a first aspect of the present invention comprises a group of monomers and / or a partial polymer of the group of monomers, a first photopolymerization initiator, and a second photopolymerization initiator, wherein the first photopolymerization initiator and the second photopolymerization initiator have a relatively small first reaction rate and a relatively large second reaction rate, respectively, and the ratio of the second reaction rate to the first reaction rate is 1.1 or more, expressed as the ratio of polymerization rates A evaluated by the following measurement method using only each of the photopolymerization initiators. [Measurement Method] A mixed solution containing 99 parts by weight of n-butyl acrylate and 1 part by weight of 4-hydroxybutyl acrylate as monomers, and 0.1 parts by weight of the photopolymerization initiator to be evaluated, is irradiated with ultraviolet light to prepare a monomer syrup in which the monomers are partially polymerized. The ultraviolet light irradiation is continued until the viscosity of the mixed solution at 30°C reaches 20 Pa·s. Next, a 20 μm thick coating layer made of the prepared monomer syrup is formed between a pair of polyethylene terephthalate (PET) sheets, each having a thickness of 75 μm. Next, the coating layer is irradiated with ultraviolet light from an LED light source having a peak wavelength of 340 nm±10 nm from one of the PET sheets. The illuminance and irradiation time of the irradiated ultraviolet light are 4 mW / cm. 2 and 1200 seconds. The polymerization rate A is determined by measuring the polymerization rate of the monomer in the coating layer photocured by the irradiation of ultraviolet light.

[0014] In a second aspect of the present invention, for example, in the photocurable composition according to the first aspect, the polymerization rate A of the first photopolymerization initiator is 80% or less, and the polymerization rate A of the second photopolymerization initiator is 90% or more.

[0015] In a third aspect of the present invention, for example, in the photocurable composition according to the first or second aspect, the first photopolymerization initiator is an α-hydroxyacetophenone-based compound.

[0016] In a fourth aspect of the present invention, for example, in the photocurable composition according to any one of the first to third aspects, the number of α-hydroxyacetophenone structures contained in one molecule of the first photopolymerization initiator is 1.

[0017] In a fifth aspect of the present invention, for example, in the photocurable composition according to any one of the first to fourth aspects, the second photopolymerization initiator is an α-hydroxyacetophenone-based compound.

[0018] In a sixth aspect of the present invention, for example, in the photocurable composition according to any one of the first to fifth aspects, the first photopolymerization initiator is 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methylpropanone.

[0019] In a seventh aspect of the present invention, for example, in the photocurable composition according to any one of the first to sixth aspects, the group of monomers includes a (meth)acrylic monomer.

[0020] An adhesive sheet according to an eighth aspect of the present invention is an adhesive sheet formed from the photocurable composition according to any one of the first to seventh aspects.

[0021] In a ninth aspect of the present invention, for example, in the pressure-sensitive adhesive sheet according to the eighth aspect, the polymerization rate of the monomer group in the pressure-sensitive adhesive sheet is 97% or more, and the weight-average molecular weight of the polymer contained in the pressure-sensitive adhesive sheet is more than 700,000.

[0022] In a tenth aspect of the present invention, for example, in the pressure-sensitive adhesive sheet according to the eighth or ninth aspect, the thickness of the pressure-sensitive adhesive sheet is 300 μm or less.

[0023] An optical laminate according to an eleventh aspect of the present invention comprises the pressure-sensitive adhesive sheet according to any one of the eighth to tenth aspects and an optical film.

[0024] In a twelfth aspect of the present invention, for example, in the optical laminate according to the eleventh aspect, the optical film is a polarizing film, and the pressure-sensitive adhesive sheet is in contact with the polarizing film.

[0025] An image display device according to a thirteenth aspect of the present invention includes the optical laminate according to the eleventh or twelfth aspect.

[0026] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be implemented in any modified form without departing from the gist of the present invention.

[0027] [Photocurable composition] The photocurable composition of this embodiment contains a monomer group and / or a partial polymer of the monomer group, a first photopolymerization initiator, and a second photopolymerization initiator. The photocurable composition of this embodiment is for use in a pressure-sensitive adhesive sheet. A pressure-sensitive adhesive sheet can be formed from the photocurable composition of this embodiment.

[0028] (Photopolymerization Initiator) The first photopolymerization initiator and the second photopolymerization initiator each have a relatively small first reaction rate and a relatively large second reaction rate. The reaction rate of each photopolymerization initiator can be determined by the polymerization rate achieved when a monomer is polymerized using only that photopolymerization initiator. The ratio of the second reaction rate to the first reaction rate is 1.1 or more, expressed as the ratio of polymerization rates A evaluated by the following measurement method using only each photopolymerization initiator. The ratio of polymerization rates A may be 1.15 or more, 1.2 or more, 1.22 or more, 1.25 or more, or even 1.27 or more. The upper limit of the ratio is not particularly limited, but may be, for example, 3 or less. The ratio of polymerization rates A is determined by [polymerization rate A when only the second photopolymerization initiator is used] / [polymerization rate A when only the first photopolymerization initiator is used]. [Measurement Method] A mixed solution containing 99 parts by weight of n-butyl acrylate and 1 part by weight of 4-hydroxybutyl acrylate as monomers, and 0.1 parts by weight of the photopolymerization initiator to be evaluated, is irradiated with ultraviolet light to prepare a monomer syrup in which the monomers are partially polymerized. The ultraviolet light irradiation is continued until the viscosity of the mixed solution at 30°C reaches 20 Pa·s. Next, a 20 μm thick coating layer made of the prepared monomer syrup is formed between a pair of polyethylene terephthalate (PET) sheets, each having a thickness of 75 μm. Next, the coating layer is irradiated with ultraviolet light from an LED light source having a peak wavelength of 340 nm±10 nm from one of the PET sheets. The illuminance and irradiation time of the irradiated ultraviolet light are each 4 mW / cm. 2 and 1200 seconds. The polymerization rate A is determined by measuring the polymerization rate of the monomer in the coating layer photocured by irradiation with ultraviolet light.

[0029] According to the inventors' research, it has been found that one of the factors behind the deterioration of image quality due to exposure to high-temperature environments is the tendency for the adhesive sheet in the optical laminate and the adjacent optical film, typically a polarizing film, to peel off at high temperatures. Another factor may be the deterioration of visibility due to the foaming of monomers remaining in the adhesive sheet at high temperatures. The combination of the first and second photopolymerization initiators creates a polymerization state suitable for increasing both the molecular weight and polymerization rate of the polymer during the formation of the adhesive sheet. While the peeling is thought to be caused by the shrinkage of the optical film at high temperatures, a polymer with a high molecular weight can improve the stress relaxation properties of the adhesive sheet and resist peeling. The combination of the first and second photopolymerization initiators is believed to create a state suitable for the generation and movement of radicals in the polymerization system for the progression of the polymerization. The composition of the monomer syrup used to evaluate the polymerization rate A is known as a common composition for forming acrylic adhesive sheets. Furthermore, the ultraviolet irradiation conditions described above are suitable for evaluating the polymerization state.

[0030] The polymerization rate A of the first photopolymerization initiator may be 80% or less, 79% or less, or even 78% or less. The lower limit of the polymerization rate A is, for example, 65% or more, and may be 66% or more, 67% or more, 68% or more, 69% or more, or even 70% or more.

[0031] The polymerization rate A of the second photopolymerization initiator may be 90% or more, 91% or more, 92% or more, 93% or more, 94% or more, 95% or more, 96% or more, 97% or more, 98% or more, or even 99% or more. The upper limit of the polymerization rate A is, for example, 99.9% or less, or even 99.5% or less.

[0032] The polymerization rate A of the first photopolymerization initiator and the polymerization rate A of the second photopolymerization initiator may simultaneously satisfy the above-mentioned ranges. For example, the polymerization rate A of the first photopolymerization initiator may be 80% or less, and the polymerization rate A of the second photopolymerization initiator may be 90% or more.

[0033] Examples of the first and second photopolymerization initiators include benzoyl ethers, substituted benzoyl ether compounds, substituted acetophenone compounds, α-hydroxyacetophenone compounds, substituted alpha-ketol compounds, aromatic sulfonyl chloride compounds, photoactive oximes, benzophenone compounds, thioxanthone compounds, triazine compounds, oxime ester compounds, phosphine compounds, quinone compounds, borate compounds, carbazole compounds, imidazole compounds, and titanocene compounds.

[0034] The first photopolymerization initiator is preferably an α-hydroxyacetophenone-based compound. A first photopolymerization initiator that is an α-hydroxyacetophenone-based compound is particularly suitable for increasing the molecular weight of a polymer in combination with a second photopolymerization initiator. The number of α-hydroxyacetophenone structures contained in one molecule of the first photopolymerization initiator is, for example, 1 to 3, preferably 1 or 2, and more preferably 1.

[0035] A specific example of the first photoinitiator is 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methylpropanone, which is an α-hydroxyacetophenone-based compound and is commercially available as Omnirad 2959 (manufactured by IGM Resins).

[0036] The second photopolymerization initiator is not limited, but may be an α-hydroxyacetophenone-based compound. A second photopolymerization initiator that is an α-hydroxyacetophenone-based compound is particularly suitable for increasing the molecular weight of a polymer when combined with a first photopolymerization initiator, particularly a first photopolymerization initiator that is an α-hydroxyacetophenone-based compound. The number of α-hydroxyacetophenone structures contained in one molecule of the second photopolymerization initiator is, for example, 1 to 3, preferably 1 or 2, and more preferably 2.

[0037] The photocurable composition may include one or more first photoinitiators. The photocurable composition may include one or more second photoinitiators.

[0038] The amount of the photopolymerization initiator in the photocurable composition, in total, of all photopolymerization initiators including the first and second photopolymerization initiators, is 0.01 to 1 part by weight per 100 parts by weight of the total of the monomer group and the partially polymerized product. The upper limit of the amount may be 0.9 parts by weight or less, 0.8 parts by weight or less, 0.7 parts by weight or less, 0.6 parts by weight or less, 0.5 parts by weight or less, 0.4 parts by weight or less, 0.3 parts by weight or less, 0.25 parts by weight or less, or even 0.2 parts by weight or less. The lower limit of the amount may be 0.05 parts by weight or more, 0.08 parts by weight or more, 0.1 parts by weight or more, or even 0.15 parts by weight or more.

[0039] The ratio of the amount X1 of the first photopolymerization initiator to the amount X2 of the second photopolymerization initiator is, for example, 5:1 to 1:5, and may be 4:1 to 1:4, 3:1 to 1:3, 2:1 to 1:2, or even 1.5:1 to 1:1.5, in terms of weight ratio.

[0040] The ratio of the remaining amounts B of the first and second photopolymerization initiators evaluated by the following measurement method B is, for example, 0.6 or less, and may be 0.55 or less, or even 0.5 or less. The lower limit of the ratio may be, for example, 0.01 or more. The ratio of the remaining amounts B is determined by [remaining amount B when only the second photopolymerization initiator is used] / [remaining amount B when only the first photopolymerization initiator is used]. [Measurement Method B] A mixed solution containing 99 parts by weight of n-butyl acrylate and 1 part by weight of 4-hydroxybutyl acrylate as monomers, and 0.1 parts by weight of the photopolymerization initiator to be evaluated, is irradiated with ultraviolet light to prepare a monomer syrup in which the monomers are partially polymerized. The ultraviolet light irradiation is continued until the viscosity of the mixed solution at 30°C reaches 20 Pa·s. Next, a 20 μm-thick coating layer of the prepared monomer syrup is formed between a pair of polyethylene terephthalate (PET) sheets, each 75 μm thick. Next, the coating layer is irradiated with ultraviolet light from an LED light source having a peak wavelength of 340 nm±10 nm from one of the PET sheets. The illuminance and irradiation time of the irradiated ultraviolet light are 14 mW / cm. 2 and 100 seconds. The remaining amount B is determined as the remaining amount of the photopolymerization initiator measured in the coating layer photocured by the irradiation of ultraviolet rays.

[0041]

[0013] Note that, regardless of the ratio of polymerization rates A, a combination of a first photopolymerization initiator and a second photopolymerization initiator in which the ratio of the residual amount B is within the above range may enable the polymerization state during the formation of a pressure-sensitive adhesive sheet to be suitable for increasing the molecular weight of the polymer. In view of this aspect, the present invention provides a photocurable composition for a pressure-sensitive adhesive sheet, comprising: a monomer group and / or a partial polymer of the monomer group, a first photopolymerization initiator, and a second photopolymerization initiator, wherein the first photopolymerization initiator and the second photopolymerization initiator have a relatively small first reaction rate and a relatively large second reaction rate, respectively, and the ratio of the second reaction rate to the first reaction rate, expressed as the ratio of the residual amount B evaluated by the above measurement method B using only each of the photopolymerization initiators, is 0.6 or less.

[0042] (Monomer Group) The monomer group may contain a (meth)acrylic monomer. The content of the (meth)acrylic component, i.e., the (meth)acrylic monomer and its partial polymer, in the photocurable composition may be 50% by weight or more, 60% by weight or more, 70% by weight or more, or even 80% by weight or more. In this case, an acrylic pressure-sensitive adhesive sheet containing a (meth)acrylic polymer and its crosslinked product as the main components can be formed. However, the photocurable composition is not limited to the above examples. In this specification, (meth)acrylic means acrylic and methacrylic. (Meth)acrylate means acrylate and methacrylate.

[0043] An example of the (meth)acrylic monomer is a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 20 carbon atoms on the side chain. The number of carbon atoms in the alkyl group may be 7 or less, 6 or less, 5 or less, or even 4 or less. The alkyl group may be linear or branched. Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. acrylate, n-octyl(meth)acrylate, isooctyl(meth)acrylate, n-nonyl(meth)acrylate, isononyl(meth)acrylate, n-decyl(meth)acrylate, isodecyl(meth)acrylate, n-dodecyl(meth)acrylate (lauryl(meth)acrylate), n-tridecyl(meth)acrylate, n-tetradecyl(meth)acrylate, pentadecyl(meth)acrylate, hexadecyl(meth)acrylate, heptadecyl(meth)acrylate, and octadecyl(meth)acrylate. The (meth)acrylic acid alkyl ester may be n-butyl(meth)acrylate.

[0044] The content of the (meth)acrylic acid alkyl ester in the monomer group is, for example, 40% by weight or more, and may be 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, or even 95% by weight or more. In calculating the content, the weight of the partially polymerized product is converted into the weight of each monomer before polymerization.

[0045] The monomer group may contain a carboxyl group-containing monomer. The carboxyl group-containing monomer may be a (meth)acrylic monomer; in other words, the (meth)acrylic monomer may contain a carboxyl group-containing monomer. Examples of carboxyl group-containing monomers include (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. The content of the carboxyl group-containing monomer in the monomer group may be, for example, 10% by weight or less, 9% by weight or less, 8% by weight or less, 7% by weight or less, 6% by weight or less, 5.5% by weight or less, or even 5% by weight or less. The lower limit of the content may be, for example, 0.1% by weight or more, 0.5% by weight or more, or even 1% by weight or more. The monomer group may not contain a carboxyl group-containing monomer.

[0046] The monomer group may contain a hydroxy group-containing monomer. The hydroxy group-containing monomer may be a (meth)acrylic monomer, in other words, the (meth)acrylic monomer may contain a hydroxy group-containing monomer. The hydroxy group-containing monomer may contribute to improving the cohesive strength of the PSA sheet. Examples of hydroxy group-containing monomers are 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methyl acrylate. The hydroxy group-containing monomer is preferably 2-hydroxyethyl (meth)acrylate or 4-hydroxybutyl (meth)acrylate. The content of the hydroxy group-containing monomer in the monomer group is, for example, 10% by weight or less, and may be 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, 0.8% by weight or less, 0.5% by weight or less, 0.3% by weight or less, 0.2% by weight or less, or even 0.1% by weight or less. The lower limit of the content may be, for example, 0.01% by weight or more, 0.03% by weight or more, or even 0.05% by weight or more. The monomer group may not contain a hydroxy group-containing monomer.

[0047] The monomer group may include a nitrogen atom-containing monomer. The nitrogen atom-containing monomer means a monomer having at least one nitrogen atom in the molecule (per molecule).

[0048] As the nitrogen atom-containing monomer, from the viewpoint of improving foaming and peeling resistance, N-vinyl cyclic amide, (meth)acrylamide, etc. are preferred. The nitrogen atom-containing monomer may be used alone or in combination of two or more kinds.

[0049] The N-vinyl cyclic amide is preferably one represented by the following formula (1):

[0050] In formula (1), R 1 is a divalent organic group, preferably a divalent saturated or unsaturated hydrocarbon group, and more preferably a divalent saturated hydrocarbon group (e.g., an alkylene group having 3 to 5 carbon atoms). 1 are directly bonded via a single bond to form a ring structure.

[0051] As the N-vinyl cyclic amide represented by formula (1), from the viewpoint of improving foaming and peeling resistance, N-vinyl-2-pyrrolidone (NVP), N-vinyl-2-piperidone, N-vinyl-2-caprolactam, N-vinyl-3-morpholinone, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, etc. are preferred, more preferably N-vinyl-2-pyrrolidone and N-vinyl-2-caprolactam, and even more preferably N-vinyl-2-pyrrolidone.

[0052] Examples of (meth)acrylamides include (meth)acrylamide, N-alkyl(meth)acrylamide, N,N-dialkyl(meth)acrylamide, etc. Examples of N-alkyl(meth)acrylamides include N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-n-butyl(meth)acrylamide, N-octylacrylamide, etc. N-alkyl(meth)acrylamides also include (meth)acrylamides having an amino group, such as dimethylaminoethyl(meth)acrylamide, diethylaminoethyl(meth)acrylamide, and dimethylaminopropyl(meth)acrylamide.

[0053] Examples of N,N-dialkyl(meth)acrylamides include N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, and N,N-di(t-butyl)(meth)acrylamide.

[0054] (Meth)acrylamides also include, for example, various N-hydroxyalkyl(meth)acrylamides, such as N-methylol(meth)acrylamide, N-(2-hydroxyethyl)(meth)acrylamide, N-(2-hydroxypropyl)(meth)acrylamide, N-(1-hydroxypropyl)(meth)acrylamide, N-(3-hydroxypropyl)(meth)acrylamide, N-(2-hydroxybutyl)(meth)acrylamide, N-(3-hydroxybutyl)(meth)acrylamide, N-(4-hydroxybutyl)(meth)acrylamide, and N-methyl-N-2-hydroxyethyl(meth)acrylamide.

[0055] (Meth)acrylamides also include, for example, various N-alkoxyalkyl(meth)acrylamides, such as N-methoxymethyl(meth)acrylamide and N-butoxymethyl(meth)acrylamide.

[0056] Examples of nitrogen atom-containing monomers other than N-vinyl cyclic amides and (meth)acrylamides include amino group-containing monomers such as aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate; cyano group-containing monomers such as acrylonitrile and methacrylonitrile; (meth)acryloylmorpholine, N-vinylpiperazine, N-vinylpyrrole, N-vinylimidazole, N-vinylpyrazine, N-vinylmorpholine, N-vinylpyrazole, vinylpyridine, vinylpyrimidine, vinyloxazole, vinylisoxazole, vinylthiazole, vinylisothiazole, vinylpyridazine, (meth)acryloylpyrrolidone, (meth)acryloylpyrrolidine, (meth)acryloylpiperidine, N-methyl Examples of the monomer include heterocycle-containing monomers such as vinylpyrrolidone; maleimide-based monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, and N-phenylmaleimide; itaconimide-based monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-laurylitaconimide, and N-cyclohexylitaconimide; and imide group-containing monomers such as succinimide-based monomers such as N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, and N-(meth)acryloyl-8-oxyoctamethylenesuccinimide; and isocyanate group-containing monomers such as 2-(meth)acryloyloxyethylisocyanate.

[0057] The content of the nitrogen atom-containing monomer in the monomer group is, for example, 40% by weight or less, and may be 35% by weight or less, 30% by weight or less, 25% by weight or less, 20% by weight or less, 15% by weight or less, 13% by weight or less, 10% by weight or less, 8% by weight or less, 6% by weight or less, or even 5% by weight or less. The lower limit of the content is, for example, 0.5% by weight or more, and may be 1% by weight or more, 2% by weight or more, 3% by weight or more, 4% by weight or more, 5% by weight or more, 7% by weight or more, or even 10% by weight or more. The monomer group may not contain a nitrogen atom-containing monomer.

[0058] The monomer group may include monomers other than those mentioned above.

[0059] In the photocurable composition, each of the above-mentioned monomers may be contained as a partial polymer. The partial polymer may be either a homopolymer or a copolymer. The photocurable composition may not contain a partial polymer.

[0060] The photocurable composition may contain a crosslinking agent. An example of the crosslinking agent is a polyfunctional monomer having two or more polymerizable functional groups in one molecule. The polyfunctional monomer may be a (meth)acrylic monomer. Examples of the polyfunctional monomer are a monomer having two or more C=C bonds in one molecule, and a monomer having one or more C=C bonds and one or more polymerizable functional groups such as epoxy groups, aziridine groups, oxazoline groups, hydrazine groups, methylol groups, etc. in one molecule. The polyfunctional monomer is preferably a monomer having two or more C=C bonds in one molecule.

[0061] Examples of the polyfunctional monomer include (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,2-ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol diacrylate (N Polyfunctional acrylates (e.g., ester compounds of polyhydric alcohols and (meth)acrylic acid) such as 1,12-dodecanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and tetramethylolmethane tri(meth)acrylate; allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, urethane acrylate, butyl di(meth)acrylate, and hexyl di(meth)acrylate. The polyfunctional monomer is preferably a polyfunctional acrylate, and more preferably 1,9-nonanediol diacrylate, trimethylolpropane tri(meth)acrylate, hexanediol di(meth)acrylate, or dipentaerythritol hexa(meth)acrylate.

[0062] The amount of crosslinking agent to be added varies depending on the molecular weight, the number of functional groups, etc., but may be, for example, 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, 0.5 parts by weight or less, or even 0.3 parts by weight or less, relative to 100 parts by weight of the total of the monomer group and its partial polymer. The lower limit of the amount to be added may be, for example, 0.01 parts by weight or more, or even 0.05 parts by weight or more. The photocurable composition may not contain a crosslinking agent.

[0063] The photocurable composition may contain additives other than those described above. Examples of the additives include a chain transfer agent, a silane coupling agent, a viscosity modifier, a tackifier, a plasticizer, a softener, an antioxidant, a filler, a colorant, an antioxidant, a surfactant, an antistatic agent, and an ultraviolet absorber. The photocurable composition may not contain any additives.

[0064] The viscosity of the photocurable composition is preferably 5 to 100 poise. Photocurable compositions having a viscosity in the above range are particularly suitable for forming pressure-sensitive adhesive sheets.

[0065] The solvent content in the photocurable composition is, for example, 5 wt% or less, and may be 4 wt% or less, 3 wt% or less, 2 wt% or less, 1 wt% or less, or even 0.5 wt% or less. The photocurable composition may be substantially free of solvent. "Substantially free of solvent" means that solvents derived from additives and the like are allowed in a content of, for example, 0.1 wt% or less, preferably 0.05 wt% or less, and more preferably 0.01 wt% or less.

[0066] [Adhesive Sheet] An example of the adhesive sheet of this embodiment is shown in Fig. 1. The adhesive sheet 1 of Fig. 1 is a sheet formed from the photocurable composition of this embodiment.

[0067] The polymerization rate of the monomer group in the pressure-sensitive adhesive sheet 1 is, for example, 90% or more, and may be 91% or more, 92% or more, 93% or more, 94% or more, 95% or more, more than 95%, 96% or more, 97% or more, 98% or more, 99% or more, 99.2% or more, 99.3% or more, 99.4% or more, 99.5% or more, or even 99.6% or more. The upper limit of the polymerization rate is, for example, 99.99% or less. A high polymerization rate can contribute to suppressing odor in the pressure-sensitive adhesive sheet 1 and suppressing foaming in high-temperature environments.

[0068] The weight-average molecular weight (Mw) of the polymer contained in the pressure-sensitive adhesive sheet 1 is, for example, 600,000 or more, and may be 650,000 or more, 700,000 or more, more than 700,000, 750,000 or more, 800,000 or more, 850,000 or more, or even 900,000 or more. The upper limit of Mw is not particularly limited, and is, for example, 3,000,000 or less. Pressure-sensitive adhesive sheet 1 containing a polymer having an Mw within the above range is suitable for suppressing peeling of the pressure-sensitive adhesive sheet 1 from an adhesive object in high-temperature environments, etc. The adhesive object is, for example, an optical film. An example of an optical film is a polarizing film. The number-average molecular weight (Mn) of the polymer is, for example, 150,000 or more, and may be 170,000 or more, 180,000 or more, 190,000 or more, 200,000 or more, 210,000 or more, 220,000 or more, 230,000 or more, 240,000 or more, or even 250,000 or more. The upper limit of Mn is not particularly limited, and is, for example, 600,000 or less. Mw / Mn, which means the molecular weight distribution, is, for example, 1.8 to 10, and may be 1.8 to 7, or even 1.8 to 5. Mw and Mn are determined from values ​​measured by GPC (gel permeation chromatography) and calculated in terms of polystyrene.

[0069] The polymerization rate of the monomer group and the molecular weight of the polymer can both be increased in the pressure-sensitive adhesive sheet 1. The polymerization rate of the monomer group in the pressure-sensitive adhesive sheet 1 may be 97% or higher, and the weight-average molecular weight of the polymer contained in the pressure-sensitive adhesive sheet 1 may be greater than 700,000. The polymerization rate and weight-average molecular weight may each be within the above-mentioned numerical ranges.

[0070] The gel fraction of the pressure-sensitive adhesive sheet 1 is, for example, 50% or more, and may be 75% or more, 80% or more, or even 85% or more.

[0071] The thickness of the pressure-sensitive adhesive sheet 1 is, for example, 2 to 500 μm, and may be 2 to 300 μm, 2 to 200 μm, or even 2 to 150 μm. The upper limit of the thickness may be 100 μm or less, 70 μm or less, 60 μm or less, 50 μm or less, 40 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the thickness may be 5 μm or more, 10 μm or more, or even 15 μm or more.

[0072] The pressure-sensitive adhesive sheet 1 can be used in, for example, an optical laminate or an image display device, but the uses of the pressure-sensitive adhesive sheet 1 are not limited to the above examples.

[0073] (Method of manufacturing pressure-sensitive adhesive sheet) The pressure-sensitive adhesive sheet 1 can be formed, for example, by irradiating light 14 onto a first laminate 10 including, in this order, a base sheet 11, a coating layer 12 containing the photocurable composition of the present embodiment, and a release liner 13 (see FIG. 2 ). The coating layer 12 is irradiated with light 14 and cured to form the pressure-sensitive adhesive sheet 1. Irradiation with light 14 is typically carried out from the side of the base sheet 11. In this case, the light 14 passes through the base sheet 11 and reaches the coating layer 12, curing the coating layer 12. However, irradiation with light 14 may also be carried out from the side of the release liner 13, or from both the side of the release liner 13 and the side of the base sheet 11.

[0074] The formed pressure-sensitive adhesive sheet 1 is sandwiched between the base sheet 11 and the release liner 13 until the release liner 13 is peeled off, and constitutes part of the second laminate 17. By peeling the release liner 13 from the second laminate 17, a third laminate 15 including the base sheet 11 and the pressure-sensitive adhesive sheet 1 is obtained. In the third laminate 15, the surface of the pressure-sensitive adhesive sheet 1 is exposed to the outside. An optical film can be laminated onto the exposed surface of the pressure-sensitive adhesive sheet 1 directly or via another layer.

[0075] The light 14 is, for example, visible light or ultraviolet light having a wavelength shorter than 450 nm. The light may include light having a wavelength in the same range as the absorption wavelength of the photopolymerization initiator contained in the photocurable composition. Light having a wavelength of 300 nm or less and cut out using a filter or the like may be irradiated. Cutting out short-wavelength light is suitable for suppressing deterioration of the base sheet 11 and / or the release liner 13 due to the light 14. The light source 18 of the light 14 is, for example, a light irradiation device equipped with an ultraviolet irradiation lamp. Examples of ultraviolet irradiation lamps include ultraviolet LEDs, low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, xenon lamps, microwave-excited mercury lamps, black light lamps, chemical lamps, germicidal lamps, low-pressure discharge mercury lamps, and excimer lasers. Two or more ultraviolet irradiation lamps may be combined. Using ultraviolet LEDs allows the wavelength band of the irradiated ultraviolet light to be narrower than when using other light sources.

[0076] The light source 18 may be an LED. Compared to black light sources, LEDs not only allow for easier adjustment of illuminance, but also tend to have a longer light source life. Compared to black light sources that use mercury, LEDs are also superior in terms of reducing environmental impact. When using an ultraviolet LED as the light source, an LED with a peak wavelength of 325 to 350 nm may be selected. According to the inventors' studies, the use of an LED with a peak wavelength of 325 to 350 nm may contribute to improving the polymerization rate of the monomer group in the pressure-sensitive adhesive sheet 1 and / or reducing the amount of residual photopolymerization initiator compared to, for example, the use of a black light source. Furthermore, LEDs that emit light 14 with a peak wavelength of 325 to 350 nm tend to generate less heat and make it easier to control the temperature of the coating layer 12 compared to LEDs that emit light with a peak wavelength of approximately 365 nm. To the best of the inventors' knowledge, no examples have been reported of producing pressure-sensitive adhesive sheets using LEDs that emit light with a peak wavelength of 325 to 350 nm.

[0077] As the LED having a peak wavelength in the range of 325 to 350 nm, an LED having a peak wavelength of 340±10 nm (hereinafter referred to as LED 340) may be selected.

[0078] Focusing on the peak wavelength of the light 14, the peak wavelength of the light 14 irradiated onto the first laminate 10 (specifically, the coating layer 12) may be 325 nm to 350 nm. The peak wavelength of the light 14 is preferably 340±10 nm (330 nm to 350 nm), may be 340±5 nm (335 nm to 345 nm), may be 340±2 nm (338 nm to 342 nm), or may be 340 nm. The peak wavelength refers to the wavelength at which the intensity of the light 14 reaches a maximum value in a spectrum showing the relationship between the wavelength and intensity of the light 14. The light 14 may further have a peak wavelength in a wavelength range other than 325 nm to 350 nm, but preferably does not have such a peak wavelength.

[0079] The illuminance of the light 14 irradiated onto the first laminate 10 (specifically, the coating layer 12) is, for example, 2.0 to 30 mW / cm 2 The illuminance is 2.5 mW / cm 2 Above, 3.0mW / cm2 Above, 3.5mW / cm 2 Above, 4.0mW / cm 2 Above, 5.0mW / cm 2 Above, 6.0mW / cm 2 Above, 7.0mW / cm 2 Above, 8.0mW / cm 2 Above, 9.0mW / cm 2 or more, and even 10 mW / cm 2 The upper limit of the illuminance may be, for example, 25 mW / cm 2 less than 20 mW / cm 2 Below 15mW / cm 2 It may be the following:

[0080] The time for irradiating the first laminate 10 (specifically, the coating layer 12) with the light 14 is, for example, 10 to 1,000 seconds, and may be 60 seconds or more, 100 seconds or more, 150 seconds or more, 200 seconds or more, 250 seconds or more, or even 300 seconds or more. The upper limit of the time is, for example, 800 seconds or less, and may be 600 seconds or less, 500 seconds or less, 400 seconds or less, 350 seconds or less, 300 seconds or less, or even 250 seconds or less. The irradiation with the light 14 may be continuous or intermittent.

[0081] The integrated light amount of the light 14 on the first laminate 10 (specifically, the coating layer 12) is, for example, 25 mJ / cm 2 or more, and 100 mJ / cm 2 Above, 500mJ / cm 2 Above, 1000mJ / cm 2 Above, 2000mJ / cm 2 Above, 2500mJ / cm 2 or more, and even 2800 mJ / cm 2 The upper limit of the integrated light amount is not particularly limited, and may be, for example, 30,000 mJ / cm 2 or less, and 10,000 mJ / cm 2 Below, 5000mJ / cm 2 Below 4000 mJ / cm 2 It may be the following:

[0082] An example of the substrate of the release liner 13 (hereinafter referred to as "liner substrate") is a resin film. Examples of resins that can be contained in the liner substrate include polyesters such as polyethylene terephthalate and polyethylene naphthalate, acetate resins, polyethersulfone, polycarbonate, polyamide, polyimide, polyolefin, (meth)acrylic resins, polyvinyl chloride, polyvinylidene chloride, polystyrene, polyvinyl alcohol, polyarylate, and polyphenylene sulfide. The resin is preferably a polyester such as polyethylene terephthalate.

[0083] The release liner 13 may include a layer other than the liner substrate. The release liner 13 may include a release layer. The release liner 13 includes, for example, a liner substrate and a release layer formed on one surface of the liner substrate. This release liner 13 can be used so that the release layer faces the coating layer 12. The release layer is typically a cured layer of a release agent composition containing a release agent. Various release agents can be used as the release agent, such as silicone-based release agents, fluorine-based release agents, long-chain alkyl-based release agents, fatty acid amide-based release agents, and silica powder.

[0084] The release liner 13 may be in the form of a sheet or a continuous piece.

[0085] An example of the substrate sheet 11 is a resin film. Examples of the resin contained in the substrate sheet 11 are the same as the examples of the resin that can be contained in the liner substrate.

[0086] The thickness of the base sheet 11 is, for example, 10 to 200 μm, and may be 25 to 150 μm.

[0087] The base sheet 11 may have a release layer on the surface facing the coating layer 12. Examples of the release layer that may be provided on the base sheet 11 are the same as the examples of the release layer that may be provided on the release liner 13. Both the release liner 13 and the base sheet 11 may have a release layer.

[0088] For the base sheet 11 , a sheet having a greater peel strength from the pressure-sensitive adhesive sheet 1 than the release liner 13 can usually be selected.

[0089] The base sheet 11 may be in the form of a sheet or a continuous sheet.

[0090] The first laminate 10 can be formed, for example, by forming a coating layer 12 on a base sheet 11 (or a release liner 13) and then placing the release liner 13 (or base sheet 11) on the formed coating layer 12. Alternatively, the first laminate 10 may be formed by applying the photocurable composition in a poured manner into the space between the base sheet 11 and the release liner 13, which are held at a predetermined distance so that their main surfaces face each other.

[0091] The coating layer 12 can be formed by various coating methods such as roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating.

[0092] The thickness of the coating layer 12 can be adjusted depending on the desired thickness of the PSA sheet 1, and may be, for example, 2 to 500 μm, 2 to 300 μm, 2 to 200 μm, or even 2 to 150 μm. The upper limit of the thickness may be 100 μm or less, 70 μm or less, 60 μm or less, 50 μm or less, 40 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the thickness may be 5 μm or more, 10 μm or more, or even 15 μm or more.

[0093] The first laminate 10 may include a long base sheet 11, a long coating layer 12, and a long release liner 13, or in other words, may be long. The long first laminate 10 can be obtained, for example, by forming the coating layer 12 between the base sheet 11 and the release liner 13 while conveying them after they have been unwound from a roll.

[0094] As described above, the present invention further provides a method for producing a pressure-sensitive adhesive sheet, which comprises irradiating a coating layer of a photocurable composition containing a monomer group and / or a partial polymer of the monomer group, a first photopolymerization initiator, and a second photopolymerization initiator with light 14 to photocure the coating layer.

[0095] [Optical laminate] An example of the optical laminate of this embodiment is shown in Fig. 3. The optical laminate 20A in Fig. 3 includes a pressure-sensitive adhesive sheet 1 and an optical film 2. The pressure-sensitive adhesive sheet 1 and the optical film 2 are laminated to each other. The optical laminate 20A can be used as an optical film with a pressure-sensitive adhesive sheet.

[0096] Examples of the optical film 2 include a polarizing film, a retardation film, and a laminate film including a polarizing film and / or a retardation film. However, the optical film 2 is not limited to the above examples. The optical film 2 may also include a glass film.

[0097] The optical film 2 may be a polarizing film, and the pressure-sensitive adhesive sheet 1 may be in contact with the polarizing film. Among optical films, polarizing films tend to undergo large dimensional changes due to heat. Dimensional changes in the polarizing film can cause peeling from the pressure-sensitive adhesive film. For this reason, the present invention is particularly advantageous when the optical laminate further includes a polarizing film.

[0098] The polarizing film includes a polarizer. The polarizing film typically includes a polarizer and a protective film (transparent protective film). The protective film is disposed, for example, in contact with a main surface (the surface having the largest area) of the polarizer. The polarizer may be disposed between two protective films. The protective film may be disposed on at least one surface of the polarizer.

[0099] The polarizer is not particularly limited, and examples thereof include a hydrophilic polymer film such as a polyvinyl alcohol film, a partially formalized polyvinyl alcohol film, or an ethylene-vinyl acetate copolymer partially saponified film, which has been uniaxially stretched after adsorbing a dichroic substance such as iodine or a dichroic dye; a polyene-based oriented film such as a dehydrated polyvinyl alcohol or a dehydrochlorinated polyvinyl chloride; etc. A polarizer typically comprises a polyvinyl alcohol film (polyvinyl alcohol films include an ethylene-vinyl acetate copolymer partially saponified film) and a dichroic substance such as iodine.

[0100] The thickness of the polarizer is not particularly limited and may be, for example, 80 μm or less, 50 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the polarizer thickness is not particularly limited and may be, for example, 1 μm or more, 5 μm or more, 10 μm or more, or even 15 μm or more. A thin polarizer (for example, a thickness of 20 μm or less) is suppressed in dimensional change and can contribute to improving the durability of the optical laminate, particularly durability at high temperatures.

[0101] The material for the protective film may be, for example, a thermoplastic resin having excellent transparency, mechanical strength, thermal stability, moisture-blocking properties, isotropy, etc. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene-based resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The material for the protective film may be a thermosetting resin or an ultraviolet-curable resin such as a (meth)acrylic, urethane, acrylic urethane, epoxy, or silicone-based resin. When the polarizing film has two protective films, the materials of the two protective films may be the same or different. For example, a protective film made of a thermoplastic resin may be bonded to one main surface of the polarizer via an adhesive, and a protective film made of a thermosetting resin or an ultraviolet-curable resin may be bonded to the other main surface of the polarizer. The protective film may contain one or more optional additives, such as ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, color inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants.

[0102] The thickness of the protective film can be determined as appropriate, but is generally about 5 to 200 μm in view of strength, workability such as handling, thinness, and the like.

[0103] The polarizer and the protective film are usually adhered to each other via an aqueous adhesive or the like. Examples of aqueous adhesives include isocyanate-based adhesives, polyvinyl alcohol-based adhesives, gelatin-based adhesives, vinyl latex, aqueous polyurethane, and aqueous polyester. Examples of adhesives other than the above-mentioned adhesives include ultraviolet-curable adhesives and electron beam-curable adhesives. Electron beam-curable polarizing film adhesives exhibit suitable adhesiveness to various protective films. The adhesive may contain a metal compound filler.

[0104] In the polarizing film, a retardation film or the like can be formed on the polarizer instead of the protective film. Another protective film or a retardation film or the like can be further provided on the protective film.

[0105] The protective film may have a hard coat layer on the surface opposite to the surface bonded to the polarizer, and may also be subjected to treatments for purposes such as anti-reflection, anti-sticking, diffusion, and anti-glare.

[0106] The polarizing film may be a circular polarizing film.

[0107] The thickness of the polarizing film is, for example, 500 μm or less, and may be 300 μm or less, 200 μm or less, 100 μm or less, or even 60 μm or less. The lower limit of the thickness may be, for example, 10 μm or more, 25 μm or more, or even 40 μm or more.

[0108] The retardation film is a film having birefringence in the in-plane direction and / or the thickness direction, and is, for example, a stretched resin film or a film in which a liquid crystal material is oriented and fixed.

[0109] The retardation film may be a λ / 4 plate, a λ / 2 plate, an anti-reflection retardation film (see, for example, paragraphs 0221, 0222, and 0228 of JP 2012-133303 A), a viewing angle compensation retardation film (see, for example, paragraphs 0225 and 0226 of JP 2012-133303 A), or an inclined orientation retardation film for viewing angle compensation (see, for example, paragraph 0227 of JP 2012-133303 A). The retardation film is not limited to the above examples as long as it has birefringence in the in-plane direction and / or the thickness direction. There are also no limitations on the retardation value, arrangement angle, three-dimensional birefringence, whether the retardation film is single-layer or multi-layer, etc. of the retardation film. Known films can be used as the retardation film.

[0110] The thickness of the optical film 2 is, for example, 1 to 200 μm.

[0111] The optical film 2 may be a single layer or a laminated film composed of two or more layers. When the optical film 2 is a laminated film, the pressure-sensitive adhesive sheet 1 may be used to bond the layers together.

[0112] Another example of the optical laminate of the present embodiment is shown in Fig. 4. The optical laminate 20B in Fig. 4 has a layered structure in which a release liner 3, a pressure-sensitive adhesive sheet 1, and an optical film 2 are layered in this order. By peeling off the release liner 3, the optical laminate 20B can be used as an optical film with a pressure-sensitive adhesive sheet.

[0113] The release liner 3 is typically a resin film. Examples of resins that make up the release liner 3 include polyesters such as polyethylene terephthalate (PET), polyolefins such as polyethylene and polypropylene, polycarbonate, acrylic, polystyrene, polyamide, and polyimide. The surface of the release liner 3 that comes into contact with the pressure-sensitive adhesive sheet 1 may be subjected to a release treatment. The release treatment is, for example, a treatment with a silicone compound. However, the release liner 3 is not limited to the above examples. The release liner 3 is peeled off when the optical laminate 20B is used, for example, when it is attached to the image forming layer.

[0114] Another example of the optical laminate of the present embodiment is shown in Fig. 5. The optical laminate 20C in Fig. 5 has a layered structure in which a release liner 3, a pressure-sensitive adhesive sheet 4, a retardation film 2B, a pressure-sensitive adhesive sheet 1, and a polarizing film 2A are layered in this order. After the release liner 3 is peeled off, the optical laminate 20C can be used by being attached to, for example, an image-forming layer.

[0115] A known adhesive sheet can be used as the adhesive sheet 4. The adhesive sheet 1 may also be used as the adhesive sheet 4.

[0116] Another example of the optical laminate of this embodiment is shown in Fig. 6. Optical laminate 20D in Fig. 6 has a layered structure in which a release liner 3, a pressure-sensitive adhesive sheet 4, a retardation film 2B, a pressure-sensitive adhesive sheet 1, a polarizing film 2A, and a protective film 5 are layered in this order. After peeling off the release liner 3, optical laminate 20D can be used by being attached to, for example, an image-forming layer.

[0117] The protective film 5 has the function of protecting the optical film 2 (polarizing film 2A), which is the outermost layer, during distribution and storage of the optical laminate 20D and when the optical laminate 20D is incorporated into an image display device. The protective film 5 may also function as a window to the external space when incorporated into an image display device. The protective film 5 is typically a resin film. Examples of resins constituting the protective film 5 include polyesters such as PET, polyolefins such as polyethylene and polypropylene, acrylics, cycloolefins, polyimides, and polyamides, with polyesters being preferred. However, the protective film 5 is not limited to the above examples. The protective film 5 may be a glass film or a laminate film including a glass film. The protective film 5 may be subjected to surface treatments such as anti-glare, anti-reflection, and anti-static.

[0118] The protective film 5 may be bonded to the optical film 2 by any adhesive. Bonding by an adhesive sheet 1 is also possible.

[0119] The optical laminate may have any configuration as long as it includes the pressure-sensitive adhesive sheet 1 and the optical film 2 .

[0120] The optical laminate of this embodiment can be distributed and stored, for example, as a rolled body obtained by rolling up a strip-shaped optical laminate, or as a sheet-shaped optical laminate.

[0121] The optical laminate of this embodiment is typically used in an image display device, such as a liquid crystal display, an organic EL display, or an inorganic EL display.

[0122] [Image Display Device] An example of an image display device according to this embodiment is shown in Figure 7. The image display device 21 in Figure 7 has a layered structure in which a substrate 7, an image forming layer (e.g., an organic EL layer or a liquid crystal layer) 6, a pressure-sensitive adhesive sheet 4, a retardation film 2B, a pressure-sensitive adhesive sheet 1, a polarizing film 2A, and a protective film 5 are layered in this order. The image display device 21 has the optical laminates 20A, 20B, 20C, and 20D shown in Figures 3 to 6 (excluding the release liner 3). The substrate 7 and the image forming layer 6 may have the same configurations as the substrate and the image forming layer, respectively, of known image display devices.

[0123] The image display device 21 in Fig. 7 may be an organic EL display or a liquid crystal display. However, the image display device 21 is not limited to this example. The image display device 21 may be an electroluminescence (EL) display, a plasma display (PD), a field emission display (FED), or the like. The image display device 21 may be used for home appliances, in-vehicle applications, public information displays (PID), and the like.

[0124] The image display device 21 may have any configuration as long as it includes the pressure-sensitive adhesive sheet 1 and / or the optical laminate 20 .

[0125] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the examples shown below.

[0126] [Evaluation of Photopolymerization Initiators] The polymerization rate A and residual amount of the photopolymerization initiators used in this example were measured as follows. (Monomer Syrup X1) 99 parts by weight of n-butyl acrylate (BA), 1 part by weight of 4-hydroxybutyl acrylate (HBA), and 0.1 parts by weight of 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methylpropanone (Omnirad 2959, manufactured by IGM Resin) as a photopolymerization initiator were placed in a four-neck flask. Next, the liquid in the flask was irradiated with ultraviolet light under a nitrogen atmosphere to obtain Monomer Syrup X1, in which the monomers were partially photopolymerized. UV irradiation was continued until the viscosity of the liquid in the flask (measurement conditions: BH viscometer No. 5 rotor, 10 rpm, measurement temperature 30°C) reached approximately 20 Pa s.

[0127] (Monomer Syrups X2 to X6) Monomer syrups X2 to X6 were prepared in the same manner as for monomer syrup X1, except that the monomers and photopolymerization initiators were changed as shown in Table 1.

[0128]

[0129] The abbreviations in Table 1 are as follows. Note that Omnirad 2959 and Omnirad 127 are α-hydroxyacetophenone compounds. BA: n-butyl acrylate HBA: 4-hydroxybutyl acrylate Omnirad 2959: 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methylpropanone (Omnirad 2959, manufactured by IGM Resins) Omnirad 184: 1-hydroxycyclohexyl-phenyl ketone (Omnirad 184, manufactured by IGM Resins) Omnirad 651: 2,2-dimethoxy-1,2-diphenylethan-1-one (Omnirad 651, manufactured by IGM Resins) Omnirad 127: 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)2-methylpropan-1-one (Omnirad 127, manufactured by IGM Resins) Omnirad 819: bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad 819, manufactured by IGM Resins) Omnirad 1173: 2-hydroxy-2-methyl-1-phenylpropanone (Omnirad 1173, manufactured by IGM Resins)

[0130] (Preparation of Release Liner) 30 parts by weight of an addition reaction curable silicone (LTC761 containing a hexenyl group-containing polyorganosiloxane, a 30 wt% toluene solution, manufactured by Dow Corning Toray), 0.9 parts by weight of a release control agent (BY24-850 containing an unreactive silicone resin, manufactured by Dow Corning Toray), and 2 parts by weight of a curing catalyst (SRX212 containing a platinum catalyst, manufactured by Dow Corning Toray), and a toluene / hexane mixed solvent (volume ratio 1:1) as a dilution solvent were mixed to obtain a silicone-based release agent composition. The concentration of silicone solids in the release agent composition was 1.0 wt%. Next, the release agent composition was applied with a wire bar to one side of a liner substrate (Lumirror XD500P, a polyester film, 75 μm thick), and heated at 130° C. for 1 minute to prepare a release liner having a release layer (thickness 60 nm) on one side.

[0131] (Preparation of Pressure-Sensitive Adhesive Sheet) Monomer syrup X1 was applied to one side of a substrate sheet (Lumirror XD500P, a polyester film without a release layer, with a thickness of 75 μm) using an applicator to form a coating layer (thickness of 20 μm). Next, a release liner was placed on the formed coating layer to obtain a first laminate. The release liner was placed so that the release layer was in contact with the coating layer. Next, an illuminance of 4 mW / cm was applied from the substrate sheet side of the first laminate. 2 , irradiation time 1200 seconds (when evaluating polymerization rate A), or illuminance 14 mW / cm 2 The coating layer was irradiated with light from an LED under the condition of 100 seconds irradiation time (when evaluating the remaining amount of photopolymerization initiator). The peak wavelength of this light was 340 nm. As a result, the coating layer was photocured, and a pressure-sensitive adhesive sheet (20 μm thick) for evaluating the polymerization rate A or remaining amount sandwiched between the base sheet and the release liner was obtained. The illuminance of the light was measured using an illuminance meter (UD-T3040T2, manufactured by Topcon Technohouse Co., Ltd.) at a position near the ultraviolet light incident surface on the base sheet. Similarly, a pressure-sensitive adhesive sheet (20 μm thick) for evaluating the polymerization rate A or remaining amount was obtained for each of the monomer syrups X2 to X6.

[0132] (Polymerization Rate A) The polymerization rate A of each produced PSA sheet was calculated from the change in weight of the PSA sheet before and after 2 hours of heat drying at 130° C. Specifically, the weight of the PSA sheet immediately after peeling off the base sheet and release liner was defined as W0 (weight before drying), and the weight of the PSA sheet after cooling at room temperature (23° C.) for about 20 minutes after the heating was defined as W1 (weight after drying), and the polymerization rate A was calculated using the formula: polymerization rate (%) = W1 / W0 × 100.

[0133] [Remaining amount of photopolymerization initiator] The composition of each pressure-sensitive adhesive sheet was analyzed, and the remaining amount (content) of the photopolymerization initiator was calculated based on the results obtained. The composition analysis was performed using liquid chromatography (LC) under the following conditions. Instrument used: 1290 Infinity II (Agilent Technologies) Column: Acquity UPLC BEH C18 (Waters, 2.1 mmφ×100 mm, 1.7 μm) Eluent composition: ultrapure water / acetonitrile gradient conditions Column temperature: 40°C Column flow rate: 0.2 mL / min Injection volume: 2 μL Detector: photodiode array detector (PDA) Measurement wavelength: 190 to 400 nm Extraction wavelength: Omnirad 2959 = 278 nm, Omnirad 184 = 246 nm, Omnirad 651 = 253 nm, Omnirad 127 = 262 nm, Omnirad 819 = 296 nm, Omnirad 1173 = 246 nm Sample preparation method: Approximately 0.5 g of sample (adhesive sheet) was weighed, 2 mL of chloroform was added, and the mixture was shaken overnight. 8 mL of methanol was added to the resulting solution, and the supernatant was filtered through a 0.45 μm membrane filter. The resulting filtrate was injected into an LC and analyzed.

[0134] The evaluation results are shown in Table 2 below.

[0135]

[0136] [Examples 1 to 5, Comparative Examples 1 to 6] (Monomer Syrup A1) 95.2 parts by weight of BA, 4.75 parts by weight of acrylic acid (AA), and 0.05 parts by weight of HBA were added to a four-neck flask, along with 0.1 parts by weight of Omnirad 2959 (manufactured by IGM Resins) and 0.1 parts by weight of Omnirad 127 (manufactured by IGM Resins) as photopolymerization initiators. Next, the liquid in the flask was irradiated with ultraviolet light under a nitrogen atmosphere to obtain Monomer Syrup A1, in which the monomers were partially photopolymerized. UV irradiation was continued until the viscosity of the liquid in the flask (measurement conditions: BH viscometer No. 5 rotor, 10 rpm, measurement temperature 30°C) reached 20 Pa s.

[0137] (Monomer Syrups A2 to A11) Monomer syrups A2 to A11 were prepared in the same manner as for Monomer Syrup A1, except that the monomers and photopolymerization initiators were changed as shown in Table 3. Note that "AA" stands for acrylic acid.

[0138]

[0139] (Photocurable Compositions C1 to C11) Next, photocurable compositions C1 to C11 were obtained by mixing the monomer syrup and the crosslinking agent so as to obtain the compositions shown in Table 4 below. Note that "NVP" stands for N-vinyl-2-pyrrolidone, and "NDDA" stands for 1,9-nonanediol diacrylate.

[0140]

[0141] The final composition of the monomers contained in the photocurable composition C11 is shown in Table 5 below.

[0142]

[0143] (Preparation of Pressure-Sensitive Adhesive Sheet) Example 1 Photocurable composition C1 was applied to one side of a substrate sheet (Lumirror XD500P, a polyester film without a release layer, with a thickness of 75 μm) using an applicator to form a coating layer (thickness of 20 μm). Next, the release liner used for evaluating the photopolymerization initiator was placed on top of the formed coating layer to obtain a first laminate. The release liner was placed so that the release layer was in contact with the coating layer. Next, a light source with an illuminance of 9 mW / cm was applied from the substrate sheet side of the first laminate. 2 The coating layer was then photocured with light from an LED under the conditions of 1000 kJ / min, 1000 kJ / min, and 320 seconds of irradiation time. The peak wavelength of this light was 340 nm. This resulted in a PSA sheet of Example 1 (thickness: 20 μm) sandwiched between the base sheet and the release liner. The illuminance of the light was measured using an illuminance meter (UD-T3040T2, manufactured by Topcon Technohouse Co., Ltd.) at a position near the ultraviolet light incident surface of the base sheet.

[0144] <Examples 2 to 5, Comparative Examples 1 to 6> Pressure-sensitive adhesive sheets of Examples 2 to 5 and Comparative Examples 1 to 6 were obtained by the same method as in Example 1, except that the photocurable compositions used were changed as shown in Tables 6A and 6B.

[0145] (Polymerization Rate of Monomer Group) The polymerization rate of each of the pressure-sensitive adhesive sheets of the Examples and Comparative Examples was evaluated in the same manner as for polymerization rate A.

[0146] (Number-average molecular weight (Mn) and weight-average molecular weight (Mw) of polymer) Samples were prepared having the same composition as the photocurable compositions used in Examples 1 to 5 and Comparative Examples 1 to 6, except that they did not contain a crosslinking agent. The samples were irradiated with light under the conditions of the corresponding Examples and Comparative Examples. As a result, the monomer groups contained in the samples were polymerized to form polymers. The number-average molecular weight (Mn) and weight-average molecular weight (Mw) of these polymers were measured.

[0147] The Mn and Mw were measured by gel permeation chromatography (GPC) using the following measuring equipment and conditions. The measuring equipment and conditions were different for the NVP-containing composition and the NVP-free composition.

[0148] (NVP-free composition) Analytical equipment: HLC-8120GPC manufactured by Tosoh Corporation Column: G7000H manufactured by Tosoh Corporation XL +GMH XL +GMH XL Column size: 7.8 mm diameter x 30 cm, total 90 cm Column temperature: 40°C Flow rate: 0.8 mL / min Injection volume: 100 μL Eluent: tetrahydrofuran Detector: differential refractometer (RI) Standard sample: polystyrene

[0149] (NVP-containing composition) Analytical equipment: Agilent 1200, manufactured by Agilent Technologies Column: TSKgel SuperAWM-H + superAW4000 + superAW2500, manufactured by Tosoh Corporation Column size: 6.0 mmφ x 15 cm each, total 45 cm Column temperature: 40°C Flow rate: 0.4 mL / min Injection volume: 40 μL Eluent: N,N-dimethylformamide (DMF) Detector: differential refractometer (RI) Standard sample: polystyrene

[0150] (Reliability Test) <Preparation of Polarizing Film> An 80 μm thick polyvinyl alcohol film was stretched 3 times between rolls with different speed ratios while dyeing for 1 minute in a 0.3% iodine solution at 30°C. Next, the film was stretched to a total stretch ratio of 6 times while immersing for 0.5 minutes in an aqueous solution containing 4% boric acid and 10% potassium iodide at 60°C. The film was then immersed for 10 seconds in an aqueous solution containing 1.5% potassium iodide at 30°C for cleaning, followed by drying at 50°C for 4 minutes to obtain a 28 μm thick polarizer. A 30 μm thick transparent protective film made of a modified acrylic polymer having a lactone ring structure was attached to one side of the polarizer using a polyvinyl alcohol adhesive. Furthermore, a 47 μm-thick transparent protective film, which was a triacetyl cellulose film (manufactured by Konica Minolta, product name "KC4UY") with a hard coat layer (HC), was attached to the other surface of the polarizer using a polyvinyl alcohol adhesive. The polarizing film was prepared by heating and drying for 5 minutes in an oven set at 70°C. Furthermore, a discharge amount of 63 W / m was applied to the surface of the polarizing film on the transparent protective film side made of a modified acrylic polymer. 2 The corona treatment was carried out for 1 min.

[0151] <Preparation of Optical Laminate> Optical laminates were prepared by placing the above-described polarizing film on the exposed surface of the pressure-sensitive adhesive sheet prepared in Examples 1 to 5 and Comparative Examples 1 to 6. The polarizing film was placed so that the surface on the transparent protective film side made of a modified acrylic polymer was in contact with the pressure-sensitive adhesive sheet.

[0152] <Reliability Test (95°C)> The reliability (95°C reliability) of the prepared optical laminate was evaluated by the following method. First, the optical laminate was cut into a strip measuring 228 mm long x 128 mm wide to prepare a test specimen. Next, the test specimen was attached to the surface of 0.7 mm thick alkali-free glass (manufactured by Corning Incorporated, product name "EG-XG") using an adhesive sheet. The test specimen was attached to the alkali-free glass using a laminator. After attaching the test specimen, the specimen was placed in an autoclave at 50°C and 0.5 MPa for 15 minutes to homogenize the bond between the alkali-free glass and the adhesive sheet, and the adhesive sheet was adhered to the alkali-free glass. Next, the test specimen was heat-treated at 95°C for 500 hours under atmospheric pressure. The vicinity of the edge of the test specimen was observed with an optical microscope to evaluate peeling from the edge of the test specimen and to determine the presence or absence of bubbling near the edge. The evaluation criteria for edge peeling and bubbling are shown below. (Evaluation of peeling) A: There is slight peeling at the edge, but it is not at a level that affects the image display. B: There is peeling at the edge, but the effect on the image display is slight. C: There is significant peeling at the edge that affects the image display. (Foaming) A: No foaming C: Foaming

[0153] Based on the evaluation results of edge peeling and foaming, a comprehensive evaluation was made for the reliability test (95°C) according to the following criteria: (Comprehensive evaluation) A: Edge peeling is A and foaming is A B: Edge peeling is B and foaming is A C: Edge peeling is C and foaming is A D: Regardless of the evaluation result of edge peeling, foaming is C (foaming present)

[0154] <Reliability Test (105° C.)> The 105° C. reliability was evaluated in the same manner as for the 95° C. reliability, except that the heat treatment temperature was changed from 95° C. to 105° C. The evaluation criteria for peeling, bubbling, and overall evaluation were the same as for the 95° C.

[0155] The compositions and evaluation results of each photocurable composition are shown in Tables 6A and 6B below. In Table 6B, "-" indicates that no measurement was performed.

[0156]

[0157]

[0158] As shown in Table 6B, the pressure-sensitive adhesive sheets of the examples were able to suppress foaming and peeling of the polarizing film in a high-temperature environment, and were able to improve reliability when used in image display devices.

[0159] The curable composition of the present invention can be used to form a pressure-sensitive adhesive sheet.

Claims

1. A photocurable composition for adhesive sheets, comprising a monomer group and / or a partial polymer of the monomer group, a first photopolymerization initiator, and a second photopolymerization initiator, wherein the first photopolymerization initiator and the second photopolymerization initiator have a relatively small first reaction rate and a relatively large second reaction rate, respectively, and the ratio of the second reaction rate to the first reaction rate is 1.1 or more, expressed as a ratio of polymerization rates A evaluated by the following measurement method using only each of the photopolymerization initiators. [Measurement method] A mixed solution of 99 parts by weight of n-butyl acrylate and 1 part by weight of 4-hydroxybutyl acrylate as monomers, and 0.1 parts by weight of the photopolymerization initiator to be evaluated, is irradiated with ultraviolet light to prepare a monomer syrup in which the monomers are partially polymerized. The irradiation with ultraviolet light is continued until the viscosity of the mixed solution at 30°C becomes 20 Pa·s. Next, a 20 μm thick coating layer made of the monomer syrup is formed between a pair of polyethylene terephthalate (PET) sheets each having a thickness of 75 μm. Next, the coating layer is irradiated with ultraviolet light from an LED having a peak wavelength of 340 nm±10 nm as a light source from the side of one of the PET sheets. The illuminance and irradiation time of the irradiated ultraviolet light are, respectively, 4 mW / cm. 2 and 1200 seconds. As the polymerization rate A, the polymerization rate of the monomer measured for the coating layer photocured by irradiation with ultraviolet light is specified.

2. The photocurable composition according to claim 1, wherein the polymerization rate A of the first photopolymerization initiator is 80% or less, and the polymerization rate A of the second photopolymerization initiator is 90% or more.

3. The photocurable composition according to claim 1, wherein the first photopolymerization initiator is an α-hydroxyacetophenone compound.

4. The photocurable composition according to claim 3, wherein the number of α-hydroxyacetophenone structures contained in one molecule of the first photopolymerization initiator is one.

5. The photocurable composition according to claim 1, wherein the second photopolymerization initiator is an α-hydroxyacetophenone compound.

6. The photocurable composition of claim 1, wherein the first photoinitiator is 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methylpropanone.

7. The photocurable composition according to claim 1, wherein the monomer group includes a (meth)acrylic monomer.

8. An adhesive sheet formed from the photocurable composition according to claim 1.

9. The pressure-sensitive adhesive sheet according to claim 8, wherein the polymerization rate of the monomer group in the pressure-sensitive adhesive sheet is 97% or more, and the weight-average molecular weight of the polymer contained in the pressure-sensitive adhesive sheet is more than 700,000.

10. The adhesive sheet according to claim 8, wherein the thickness of the adhesive sheet is 300 μm or less.

11. An optical laminate comprising the pressure-sensitive adhesive sheet according to any one of claims 8 to 10 and an optical film.

12. The optical laminate according to claim 11, wherein the optical film is a polarizing film, and the pressure-sensitive adhesive sheet is in contact with the polarizing film.

13. An image display device comprising the optical laminate according to claim 11.

Citation Information

Patent Citations

  • Photopolymerizable composition and production of viscoelastic product

    JP1995033832A

  • Electroconductive adhesive and bioelectric pole

    JP2001181597A

  • Ultraviolet-curable adhesive, cured product, and adhesive sheet

    JP2018100403A

  • Photocurable adhesive resin composition

    JP2020045416A

  • Dicing tape with adhesive film

    JP2020149985A