Epoxy resin, curable resin composition, and cured product

The epoxy resin composition, with its optimized molecular structure and curing agent, addresses the low elastic modulus and high water absorption issues in CFRP materials, resulting in improved mechanical strength and stability.

WO2024203426A1PCT designated stage expired Publication Date: 2024-10-03NIPPON KAYAKU CO LTD

Patent Information

Application Number
PCT/JP2024/010157
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-15
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Thermosetting resins used in carbon fiber reinforced polymers (CFRP) materials lack high elastic modulus and exhibit high water absorption, leading to reduced mechanical strength and dimensional stability issues due to moisture absorption.

Method used

A specific epoxy resin composition is developed, represented by formula (1), which includes a phenol resin reacted with epihalohydrin, offering a high epoxy equivalent weight and optimized molecular weight distribution for improved mechanical properties and low water absorption, combined with a curing agent to form a curable resin composition suitable for CFRP.

Benefits of technology

The epoxy resin composition achieves a high flexural modulus and low water absorption, enhancing the mechanical strength and dimensional stability of CFRP materials, addressing the limitations of existing thermosetting resins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010157_03102024_PF_FP_ABST
    Figure JP2024010157_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides: an epoxy resin which has a high elastic modulus and excellent low water absorption; and a curable resin composition which contains the epoxy resin. The present invention specifically provides an epoxy resin represented by formula (1) (In formula (1), a plurality of R1 moieties each independently represent a hydrocarbon group having 1 to 10 carbon atoms. R2 moiety represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms. n is the average value of repetitions, and is a real number satisfying 1 < n < 15.)
Need to check novelty before this filing date? Find Prior Art

Description

Epoxy resin, curable resin composition, and cured product

[0001] The present invention relates to an epoxy resin, a curable resin composition, and a cured product.

[0002] Epoxy resins, when cured with various curing agents, become cured products with excellent mechanical properties, water resistance, chemical resistance, heat resistance, electrical properties, etc., and are used in a wide range of fields, such as adhesives, paints, laminates, molding materials, and casting materials. Carbon fiber reinforced composite materials (CFRP), which are made by impregnating and curing reinforcing fibers with epoxy resin and a curing agent as a matrix resin, can be imparted with properties such as light weight and high strength. In recent years, these materials have been widely used in aircraft structural components, wind turbine blades, automobile exterior panels, and computer applications such as IC trays and laptop computer housings, and demand for them is increasing. In particular, they are used as matrix resins for aircraft applications, taking advantage of the light weight and high strength properties of the molded products.

[0003] CFRP materials require high mechanical strength, but thermosetting resins such as epoxy resins used in the matrix resin of CFRP are generally brittle and have low bending strength, toughness, adhesiveness, etc. For this reason, a method of compensating for these properties by adding a highly tough thermoplastic resin to the thermosetting resin has been widely adopted (Patent Documents 1 to 3). Specifically, the bending strength and toughness of prepregs are improved by combining particles of thermoplastic resins such as polyethersulfone, polyetherimide, and polyamide with the thermosetting resin.

[0004] Japanese Patent Laid-Open No. 60-243113 Japanese Patent Laid-Open No. 09-100358 Japanese Patent Laid-Open No. 2013-155330 Japanese Patent Laid-Open No. 2007-211254

[0005] In recent years, there has been a strong demand for thermosetting resins with a higher modulus of elasticity to obtain even higher performance CFRP materials. This is because, when a high-modulus thermosetting resin fills and bonds the spaces between the carbon fibers, stress is transmitted to adjacent CF filaments through the thermosetting resin, allowing many CF filaments to contribute to the development of material strength, thereby achieving high strength as a composite material. Furthermore, there is a demand for thermosetting resins with even lower water absorption to prevent dimensional changes and a decrease in mechanical strength due to moisture absorption.

[0006] Patent Document 4 describes an epoxy resin with low water absorption. However, the epoxy resin described in Patent Document 4 does not have performance that satisfies the characteristics required in recent markets.

[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an epoxy resin having a high elastic modulus and excellent low water absorption, and a curable resin composition containing the epoxy resin.

[0008] That is, the present invention is as shown in the following [1] to [5]. In this application, "(Numerical value 1) to (Numerical value 2)" indicates that the upper and lower limits are included. [1] An epoxy resin represented by the following formula (1):

[0009]

[0010] (In formula (1), there are multiple R 1 R independently represents a hydrocarbon group having 1 to 10 carbon atoms. 2 represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms. n is the average number of repeating units, and is a real number in the range of 1<n<15.) [2] R in the formula (1) 1

[0013] The epoxy resin according to the preceding item [1], wherein R is a methyl group. [3] A curable resin composition comprising the epoxy resin according to the preceding item [1] or [2] and a curing agent. [4] The curable resin composition according to the preceding item [3], which is for use in carbon fiber reinforced plastics. [5] A cured product obtained by curing the curable resin composition according to the preceding item [3] or [4].

[0011] According to the present invention, it is possible to provide an epoxy resin having a high elastic modulus and excellent low water absorption, and a curable resin composition containing the epoxy resin.

[0012] 1 is a high-performance liquid chromatograph chart of the epoxy resin of Synthesis Example 2. 2 is a GPC chart of the epoxy resin of Synthesis Example 2. 3 is a high-performance liquid chromatograph chart of the epoxy resin of Comparative Synthesis Example 2. 4 is a high-performance liquid chromatograph chart of the epoxy resin of Comparative Synthesis Example 4.

[0013] The epoxy resin of the present embodiment is represented by the following formula (1).

[0014]

[0015] In formula (1), there are multiple R 1 R independently represents a hydrocarbon group having 1 to 10 carbon atoms, preferably a hydrocarbon group having 1 to 3 carbon atoms, and more preferably a methyl group. 2 represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, preferably a hydrogen atom or a hydrocarbon group having 1 to 3 carbon atoms, and more preferably a hydrogen atom. n represents the average number of repeating units, and is preferably a real number satisfying 1<n<15, more preferably 1<n<10, and particularly preferably 1<n<5.

[0016] R in formula (1) 1 , R 2 Examples of the hydrocarbon group having 1 to 10 carbon atoms represented by include an alkyl group, an allyl group, a phenyl group, and an alkoxy group. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, and a decyl group. Examples of the alkoxy group include a methoxy group or an ethoxy group.

[0017] In the formula (1), the value of n can be calculated from the number average molecular weight determined by measurement of the epoxy resin by gel permeation chromatography (GPC, detector: RI) or from the area ratio of each separated peak.

[0018] In this embodiment, gel permeation chromatography analysis is performed under the following conditions: GPC (gel permeation chromatography) analysis Manufacturer: Waters Column: Guard column SHODEX GPC KF-601, KF-602 KF-602.5, KF-603 Flow rate: 0.5 ml / min Column temperature: 40°C Solvent used: THF (tetrahydrofuran) Detector: RI (differential refractive index detector)

[0019] The epoxy equivalent of the epoxy resin of this embodiment is preferably 240 g / eq. or more and 260 g / eq. or less, and more preferably 245 g / eq. or more and less than 255 g / eq. When the epoxy equivalent is 240 g / eq. or more, good heat resistance is achieved, and when it is 260 g / eq. or less, high strength is achieved.

[0020] The epoxy resin of this embodiment preferably has a resinous form with a softening point, and the softening point is preferably 40° C. or higher and 80° C. or lower, and more preferably 60° C. or higher and 70° C. or lower. A softening point of 40° C. or higher means that the resin has an appropriate molecular weight distribution or that no solvent or the like remains, and problems such as poor curing and voids during molding can be suppressed. Conversely, a softening point of 80° C. or lower allows for easy handling when kneading with other resins.

[0021] The ICI melt viscosity (150°C) is preferably 0.01 to 0.15 Pa s, and more preferably 0.01 to 0.10 Pa s. Viscosities higher than 0.15 Pa s are undesirable because they cause problems with fluidity, resulting in problems with flowability and embeddability during pressing.

[0022] The epoxy resin represented by the formula (1) can be obtained by reacting a phenolic resin represented by the following formula (2) with epihalohydrin.

[0023]

[0024] R in the formula (2) 1 , R 2 The value and preferred range of n are the same as those in formula (1).

[0025] The epihalohydrin is readily available on the market. The amount of epihalohydrin used is usually 2.0 to 10 mol, preferably 3.0 to 8.0 mol, more preferably 3.5 to 6.0 mol per mol of hydroxyl groups in the raw material phenol mixture.

[0026] In the above reaction, an alkali metal hydroxide can be used as a catalyst to promote the epoxidation step. Usable alkali metal hydroxides include sodium hydroxide, potassium hydroxide, etc. A solid or an aqueous solution thereof may be used, but in this embodiment, the use of a solid formed into flakes is particularly preferred from the standpoints of solubility and handling. The amount of alkali metal hydroxide used is typically 0.90 to 1.5 mol, preferably 0.95 to 1.25 mol, and more preferably 0.99 to 1.15 mol, per mol of hydroxyl groups in the raw material phenol mixture.

[0027] To promote the reaction, a quaternary ammonium salt such as tetramethylammonium chloride, tetramethylammonium bromide, or trimethylbenzylammonium chloride may be added as a catalyst. The amount of the quaternary ammonium salt used is usually 0.1 to 15 g, and preferably 0.2 to 10 g, per mole of hydroxyl groups in the starting phenol mixture.

[0028] The reaction temperature is typically 30 to 90°C, preferably 35 to 80°C. In particular, in this embodiment, a temperature of 50°C or higher is preferred, with 60°C or higher being particularly preferred, for higher purity epoxidation. The reaction time is typically 0.5 to 10 hours, preferably 1 to 8 hours, and particularly preferably 1 to 3 hours. A short reaction time is not preferred because the reaction does not proceed fully, while a long reaction time is undesirable because by-products are formed. The reaction product of these epoxidation reactions is washed with water, or heated under reduced pressure without washing, to remove epihalohydrin and solvent. Furthermore, to obtain an epoxy resin with a reduced hydrolyzable halogen content, the recovered epoxy resin can be dissolved in a ketone compound having 4 to 7 carbon atoms (e.g., methyl isobutyl ketone, methyl ethyl ketone, cyclopentanone, cyclohexanone, etc.) as a solvent, and an aqueous solution of an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide is added to the solution to carry out the reaction, ensuring ring closure. In this case, the amount of alkali metal hydroxide used is usually 0.01 to 0.3 mol, preferably 0.05 to 0.2 mol, per mol of hydroxyl groups in the starting phenol mixture used in the epoxidation. The reaction temperature is usually 50 to 120°C, and the reaction time is usually 0.5 to 2 hours.

[0029] After the reaction is complete, the salt formed is removed by filtration, washing with water, or the like, and the solvent is then distilled off under heating and reduced pressure to obtain the epoxy resin of the present embodiment.

[0030] The phenolic resin represented by the formula (2) can be obtained, for example, by a condensation reaction between furfural and a phenol. In this case, the phenol is preferably used in an amount of 1.5 to 20 moles, more preferably 3 to 10 moles, per mole of furfural.

[0031] Specific examples of usable phenols include cresol, xylenol, trimethylphenol, octylphenol, phenylphenol, diphenylphenol, guaiacol, hydroquinone, resorcinol, catechol, and allylphenol, and these may be used either alone or in combination.

[0032] Examples of the solvent include, but are not limited to, methanol, ethanol, propanol, isopropanol, toluene, xylene, etc., and these may be used alone or in combination of two or more. When a solvent is used, the amount used is usually in the range of 5 to 500 parts by weight, preferably 10 to 300 parts by weight, per 100 parts by weight of phenol.

[0033] In the condensation reaction, a basic catalyst is preferably used. Polycondensation is possible with an acidic catalyst, but reactions between furfurals occur, resulting in increased by-products. Alternatively, a method using an organometallic compound can be used, but this is cost-inefficient. Specific examples of basic catalysts include alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, and potassium hydroxide; alkaline earth metal hydroxides such as magnesium hydroxide and calcium hydroxide; alkali metal alkoxides such as sodium methoxide, sodium ethoxide, potassium methoxide, potassium ethoxide, and potassium tert-butoxide; and alkaline earth metal alkoxides such as magnesium methoxide and magnesium ethoxide. However, the basic catalyst is not limited to these, and may be used alone or in combination of two or more. The amount of catalyst used is typically 0.005 to 2.0 moles, preferably 0.01 to 1.1 moles, per mole of phenol.

[0034] The condensation reaction in the presence of these base catalysts is preferably carried out in the range of 40 to 180° C., particularly preferably in the range of 80 to 165° C., and the reaction time can usually be selected in the range of 0.5 to 10 hours. The reaction product thus obtained is neutralized to neutralize the system or repeatedly washed with water in the presence of a solvent, and then the water is separated and drained, and the solvent and unreacted materials are removed under heating and reduced pressure to obtain the phenolic resin represented by formula (2).

[0035] The phenolic resin represented by formula (2) can be combined with commonly available epoxy resins and curing accelerators to produce curable resin compositions. It can also be used as an olefin resin by reacting it with a cyanate resin raw material, a benzoxazine raw material, chloromethylstyrene, or the like, and then reacting it with vinylbenzyl ether, allyl halide, methallyl halide, or the like.

[0036] The epoxy resin of this embodiment can be mixed with a curing agent to form a curable resin composition. Examples of curing agents that can be used include amine-based curing agents, acid anhydride-based curing agents, amide-based curing agents, and phenol-based curing agents.

[0037] In the curable resin composition of the present embodiment, an amine curing agent is preferred, since it can achieve a good balance between the resin viscosity of the curable resin composition and the heat resistance of the cured resin. Examples of amine-based curing agents include 3,3'-diaminodiphenyl sulfone (3,3'-DDS), 4,4'-diaminodiphenyl sulfone (4,4'-DDS), diaminodiphenylmethane (DDM), 3,3'-diisopropyl-4,4'-diaminodiphenylmethane, 3,3'-di-t-butyl-4,4'-diaminodiphenylmethane, 3,3'-diethyl-5,5'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-diisopropyl-5,5'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-di-t-butyl-5,5'-dimethyl-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetraethyl-4,4'-diaminodiphenylmethane, 3,3'-diisopropyl-5,5'-diethyl-4,4' -diaminodiphenylmethane, 3,3'-di-t-butyl-5,5'-diethyl-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetraisopropyl-4,4'-diaminodiphenylmethane, 3,3'-di-t-butyl-5,5'-diisopropyl-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetra-t-butyl-4,4'-diaminodiphenylmethane, diaminodiphenyl ether (DADPE), bisaniline, benzyldimethylaniline, 2-(dimethylaminomethyl)phenol (DMP-10), 2,4,6-tris(dimethylaminomethyl)phenol (DMP-30), 2-ethylhexanoate ester of 2,4,6-tris(dimethylaminomethyl)phenol, and the like can be used. Other examples include aniline novolak, orthoethylaniline novolak, aniline resins obtained by reacting aniline with xylylene chloride, and aniline resins obtained by polycondensation of aniline with substituted biphenyls (4,4'-bis(chloromethyl)-1,1'-biphenyl, 4,4'-bis(methoxymethyl)-1,1'-biphenyl, etc.) or substituted phenyls (1,4-bis(chloromethyl)benzene, 1,4-bis(methoxymethyl)benzene, 1,4-bis(hydroxymethyl)benzene, etc.).

[0038] Examples of the acid anhydride curing agent include phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, and methylhexahydrophthalic anhydride.

[0039] Examples of the amide-based curing agent include dicyandiamide, or a polyamide resin synthesized from a dimer of linolenic acid and ethylenediamine.

[0040] Examples of phenolic curing agents include polyhydric phenols (bisphenol A, bisphenol F, bisphenol S, fluorene bisphenol, terpene diphenol, 4,4'-dihydroxybiphenyl, 2,2'-dihydroxybiphenyl, 3,3',5,5'-tetramethyl-(1,1'-biphenyl)-4,4'-diol, hydroquinone, resorcinol, naphthalenediol, tris-(4-hydroxyphenyl)methane, and 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane, etc.); phenols (for example, phenol, alkyl-substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, and dihydroxynaphthalene, etc.); and aldehydes (formaldehyde, acetaldehyde, benzaldehyde, p-hydroxybenzaldehyde, o-hydroxybenzoates, benzophenone ... phenolic resins obtained by condensation of the phenols with 4,4'-bis(chloromethyl)-1,1'-biphenyl and 4,4'-bis(methoxymethyl)-1,1'-biphenyl, or substituted phenyls (1,4-bis(chloromethyl)benzene, 1,4-bis(methoxymethyl)benzene, 1,4-bis(hydroxymethyl)benzene, or the like); modified products of the phenols and / or the phenolic resins; and halogenated phenols such as tetrabromobisphenol A and brominated phenolic resins.

[0041] In the curable resin composition of this embodiment, it is preferable to use the phenolic resin represented by the formula (2) as the entire amount of the curing agent or as a part thereof.

[0042] In the curable resin composition of this embodiment, the amount of curing agent used is preferably 0.7 to 1.2 equivalents relative to 1 equivalent of the epoxy group of the epoxy resin. If the amount is less than 0.7 equivalents relative to 1 equivalent of the epoxy group or if it exceeds 1.2 equivalents, curing may be incomplete and good cured physical properties may not be obtained.

[0043] Furthermore, a curing accelerator may be blended into the curable resin composition of this embodiment as needed. The gelation time can also be adjusted by using a curing accelerator. Examples of usable curing accelerators include imidazoles such as 2-methylimidazole, 2-ethylimidazole, and 2-ethyl-4-methylimidazole; tertiary amines such as 2-(dimethylaminomethyl)phenol and 1,8-diaza-bicyclo[5.4.0]undecene-7; phosphines such as triphenylphosphine; and metal compounds such as tin octoate. The curing accelerator is used in an amount of 0.01 to 5.0 parts by weight per 100 parts by weight of the epoxy resin, as needed.

[0044] The curable resin composition of the present embodiment may contain other epoxy resins. Specific examples thereof include phenols (phenol, alkyl-substituted phenol, aromatic-substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.) and various aldehydes (formaldehyde, acetaldehyde, alkyl aldehyde, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, etc.). , glutaraldehyde, phthalaldehyde, crotonaldehyde, cinnamaldehyde, etc.), polymers of phenols and various diene compounds (dicyclopentadiene, terpenes, vinylcyclohexene, norbornadiene, vinylnorbornene, tetrahydroindene, divinylbenzene, divinylbiphenyl, diisopropenylbiphenyl, butadiene, isoprene, etc.), polymers of phenols and ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, benzo[a]thiazolinone, benzo[b ... phenolic resins obtained by polycondensation of phenols and substituted biphenyls (4,4'-bis(chloromethyl)-1,1'-biphenyl and 4,4'-bis(methoxymethyl)-1,1'-biphenyl, etc.) or substituted phenyls (1,4-bis(chloromethyl)benzene, 1,4-bis(methoxymethyl)benzene, 1,4-bis(hydroxymethyl)benzene, etc.); polycondensates of bisphenols and various aldehydes; glycidyl ether epoxy resins obtained by glycidylating alcohols, etc.; alicyclic epoxy resins typified by 4-vinyl-1-cyclohexene diepoxide and 3,4-epoxycyclohexylmethyl-3,4'-epoxycyclohexanecarboxylate, etc.; glycidylamine epoxy resins typified by tetraglycidyldiaminodiphenylmethane (TGDDM) and triglycidyl-p-aminophenol, etc.; glycidyl ester epoxy resins, etc., but are not limited to these, so long as they are commonly used epoxy resins.

[0045] The curable resin composition of the present embodiment may contain known additives as needed. Specific examples of the additives that can be used include polybutadiene and its modified products, modified acrylonitrile copolymers, polyphenylene ether, polystyrene, polyethylene, polyimide, fluororesin, maleimide compounds, cyanate ester compounds, silicone gel, silicone oil, inorganic fillers such as silica, alumina, calcium carbonate, quartz powder, aluminum powder, graphite, talc, clay, iron oxide, titanium oxide, aluminum nitride, asbestos, mica, and glass powder, surface treatment agents for fillers such as silane coupling agents, release agents, and colorants such as carbon black, phthalocyanine blue, and phthalocyanine green.

[0046] The curable resin composition of this embodiment can contain a known maleimide compound as needed. Specific examples of usable maleimide compounds include 4,4'-diphenylmethane bismaleimide, polyphenylmethane maleimide, m-phenylene bismaleimide, 2,2'-bis[4-(4-maleimidophenoxy)phenyl]propane, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 4,4'-diphenylether bismaleimide, 4,4'-diphenylsulfone bismaleimide, 1,3-bis(3-maleimidophenoxy)benzene, 1,3-bis(4-maleimidophenoxy)benzene, and biphenylaralkyl maleimide, but are not limited to these. These compounds may be used alone or in combination of two or more. When a maleimide compound is blended, a curing accelerator is blended as necessary. The above-mentioned curing accelerators, as well as radical polymerization initiators such as organic peroxides and azo compounds can be used.

[0047] The curable resin composition of the present embodiment can be obtained by uniformly mixing the above-mentioned components. The method for producing the curable resin composition of the present embodiment is not particularly limited, but the composition can be obtained, for example, by thoroughly mixing an epoxy resin with a curing agent, a curing accelerator, an inorganic filler, a mold release agent, a silane coupling agent, additives, etc., using an extruder, kneader, rolls, planetary mixer, etc. until the mixture is uniform.

[0048] The obtained curable resin composition can be molded into various forms such as a resin sheet, a prepreg, etc. A prepreg form can be obtained, for example, by heating and melting the curable resin composition and / or a resin sheet of the present embodiment to reduce the viscosity and impregnating the composition into a fiber substrate.

[0049] The curable resin composition of this embodiment can also be dissolved in a solvent such as toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, dimethylformamide, dimethylacetamide, or N-methylpyrrolidone, as needed, to form a varnish-like composition (hereinafter simply referred to as a varnish), which can then be impregnated into a substrate such as glass fiber, carbon fiber, polyester fiber, polyamide fiber, alumina fiber, or paper, and dried by heating to produce a prepreg. In this case, the solvent is used in an amount that accounts for 10 to 70 wt %, preferably 15 to 70 wt %, of the mixture of the curable resin composition of this embodiment and the solvent.

[0050] The prepreg is cut into a desired shape, laminated, and then the epoxy resin composition is heat-cured while applying pressure to the laminate by press molding, autoclave molding, sheet winding molding, etc., to obtain a carbon fiber reinforced plastic (CFRP). Copper foil or an organic film can also be laminated during the lamination of the prepreg.

[0051] In addition to the above-mentioned methods, CFRP can also be obtained by molding using known methods, such as resin transfer molding (RTM), in which a carbon fiber substrate (usually a carbon fiber fabric) is cut, laminated, and shaped to produce a preform (a preform before being impregnated with resin), the preform is placed in a mold, the mold is closed, resin is injected to impregnate the preform, and the resin is cured, and the mold is then opened to remove the molded product. Also usable are types of RTM methods, such as the VaRTM method, the SCRIMP (Seeman's Composite Resin Infusion Molding Process), and the CAPRI (Controlled Atmospheric Pressure Resin Infusion) method, which is described in JP-A-2005-527410, in which a resin supply tank is evacuated to a pressure lower than atmospheric pressure, cyclic compression is used, and the net molding pressure is controlled to more appropriately control the resin injection process, particularly the VaRTM method. Furthermore, a film stacking method in which a fiber substrate is sandwiched between resin sheets (films), a method in which powdered resin is attached to a reinforcing fiber substrate to improve impregnation, a molding method in which a fluidized bed or fluid slurry method is used in the process of mixing resin into a fiber substrate (Powder Impregnated Yarn), and a method in which resin fibers are mixed into a fiber substrate can also be used.

[0052] Examples of carbon fibers include acrylic, pitch, and rayon carbon fibers, and among these, acrylic carbon fibers, which have high tensile strength, are preferably used. The carbon fiber may be in the form of twisted yarn, untwisted yarn, or non-twisted yarn, but untwisted yarn or non-twisted yarn is preferred because it provides a good balance between the formability and strength properties of the fiber-reinforced composite material.

[0053] The cured product of the curable resin composition of the present embodiment can be used for various applications other than the above-mentioned applications such as CFRP, and examples thereof include adhesives, paints, coating agents, molding materials (including sheets, films, CFRP, etc.), encapsulants for semiconductor elements, encapsulants for liquid crystal display elements, encapsulants for organic EL elements, electric and electronic parts such as printed wiring boards (BGA substrates, build-up substrates, etc.), 3D printing, and additives for other resins, etc.

[0054] Examples of the adhesive include adhesives for civil engineering, construction, automobiles, general office use, and medical use, as well as adhesives for electronic materials. Among these, adhesives for electronic materials include interlayer adhesives for multilayer substrates such as build-up substrates, die bonding agents, semiconductor adhesives such as underfills, underfills for reinforcing BGAs, and mounting adhesives such as anisotropic conductive films (ACFs) and anisotropic conductive pastes (ACPs), and are applicable to a variety of uses.

[0055] The cured product of the curable resin composition of this embodiment preferably has a flexural modulus of 2.5 GPa to 5.0 GPa, and more preferably 3.0 GPa to 4.0 GPa. A flexural modulus of less than 2.5 GPa is not preferred because the resulting carbon fiber reinforced composite material will have insufficient rigidity, resulting in reduced reliability. A flexural modulus of more than 5.0 GPa is also not preferred because the resulting material will be brittle.

[0056] When the curable resin composition of this embodiment is applied to an encapsulant for semiconductor elements, a lead frame equipped with a semiconductor element or a semiconductor package substrate is placed in a mold, and the curable resin composition of this embodiment is molded by a melt casting method, transfer molding method, injection molding method, compression molding method, or the like, and further heated for 2 to 10 hours at 80 to 200° C. to obtain a cured product. Examples of semiconductor devices manufactured using this encapsulant include potting, dipping, and transfer mold encapsulation for capacitors, transistors, diodes, light-emitting diodes, ICs, and LSIs, potting encapsulation for COB, COF, TAB, and the like for ICs and LSIs, underfill for flip chips, and encapsulation (including reinforcing underfill) when mounting IC packages such as QFP, BGA, and CSP.

[0057] When the curable resin composition of this embodiment is applied to printed wiring boards, it can be heated and melted to reduce viscosity, and then impregnated into reinforcing fibers such as glass fibers and polyamide fibers to obtain a prepreg. Specific examples include, but are not limited to, glass fibers such as E-glass cloth, D-glass cloth, S-glass cloth, Q-glass cloth, spherical glass cloth, NE-glass cloth, and T-glass cloth, and / or organic fibers. The shape of the substrate is not particularly limited, but examples include woven fabric, nonwoven fabric, roving, chopped strand mat, and the like. Known weaving methods for woven fabrics include plain weave, sieve weave, and twill weave, and these known methods can be appropriately selected depending on the intended application and performance. Furthermore, woven fabrics that have been opened or surface-treated with a silane coupling agent or the like are preferably used. The thickness of the substrate is not particularly limited, but is preferably approximately 0.01 to 0.4 mm. Furthermore, a prepreg can be obtained by impregnating reinforcing fibers with the varnish and drying them under heat, and a copper clad laminate (CCL) can be produced from this. A laminate can also be produced using the curable resin composition of this embodiment by hot-press molding the obtained prepreg and CCL. The laminate is not particularly limited as long as it comprises one or more prepregs, and may also have any other layer. Furthermore, a sheet-like adhesive can be obtained by applying the varnish to a release film, removing the solvent under heat, and B-staging the adhesive. This sheet-like adhesive can be used as an interlayer insulating layer in a multilayer substrate or as an adhesive sheet for mounting semiconductors. The curable resin composition of this embodiment can also be suitably used for special substrate materials such as package substrates and HDIs (high density interconnects).

[0058] The water absorption is preferably 2.0% or less, more preferably 1.5% or less, and particularly preferably 1.2% or less. If the water absorption exceeds 2.0%, the cured product will absorb moisture, causing the material to significantly soften and reduce its mechanical strength, which is undesirable.

[0059] The present invention will be explained in more detail below with reference to synthesis examples and examples. The materials, processing details, processing procedures, etc. shown below can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below. Various analytical methods used in the examples will be described below.

[0060] Various analytical methods were carried out under the following conditions. Epoxy equivalent: Measured according to the method described in JIS K-7236, and expressed in g / eq. Softening point: Measured according to the method conforming to JIS K-7234, and expressed in °C. Melt viscosity: Measured by the ICI melt viscosity (150°C) cone-plate method, and expressed in Pa s.

[0061] GPC (gel permeation chromatography) analysis Manufacturer: Waters Column: Guard column SHODEX GPC KF-601, KF-602 KF-602.5, KF-603 Flow rate: 0.5 ml / min. Column temperature: 40°C Solvent used: THF (tetrahydrofuran) Detector: RI (differential refractive index detector)

[0062] High-performance liquid chromatography (HPLC) measurement: Liquid delivery unit LC-20AD, manufactured by Shimadzu Corporation; Photodiode array detector SPD-M20A, manufactured by Shimadzu Corporation; Column oven CTO-20A, manufactured by Shimadzu Corporation; Column: Inertsil ODS-2, 5 μm, 4.6 × 250 mm, 40°C; MobilePhase A: acetonitrile (AN); MobilePhase B: water (W); Time Program: (Synthesis Example 2): 0-10 min. AN / W = 60% / 40% → 100% / 0%; 10-20 min. AN / W = 100% / 0%; (Comparative Synthesis Examples 2 and 4): 0-28 min. AN / W=50% / 50% → 100% / 0% 28-40min. AN / W=100% / 0% FlowRate: 1.0mL / min. Detection: UV 274nm, PDA

[0063] Synthesis Example 1: 500 parts by weight of para-cresol, 87.5 parts by weight of water, and 37.5 parts by weight of sodium hydroxide were charged into a flask equipped with a stirrer, a reflux condenser, and a stirring device. After stirring and dissolving, the mixture was heated to 110°C, and 100 parts by weight of furfural was added dropwise over 1 hour. The mixture was then allowed to react at 110°C for 3 hours, and then heated to 145°C. During the temperature increase, the distilled water was removed from the system. After reaching 145°C, the mixture was cooled to 80°C, and 100 parts by weight of water was charged. 4 parts by weight of phosphoric acid and 79 parts by weight of 35% hydrochloric acid were added for neutralization. After repeated water washing, unreacted phenol was distilled off under reduced pressure with heating to obtain 219 parts by weight of a phenolic resin represented by the following formula (3A):

[0064]

[0065] Synthesis Example 2: 77 parts by weight of the phenolic resin obtained in Synthesis Example 1 were charged into a reaction vessel with 229 parts by weight of epichlorohydrin (ECH), 40 parts by weight of dimethyl sulfoxide (DMSO), and 13 parts by weight of water. After heating, stirring, and dissolution, 23 parts by weight of flaky sodium hydroxide was added in portions over 1.5 hours while maintaining the temperature at 55°C. The reaction was then continued for 1.5 hours at 55°C and 30 minutes at 70°C. After repeated water washing to remove DMSO and by-product salts, excess epichlorohydrin was distilled off from the oil layer under heating and reduced pressure, and 217 parts by weight of methyl isobutyl ketone was added to the residue and dissolved. This methyl isobutyl ketone solution was heated to 70°C, and 22 parts by weight of methanol, 22 parts by weight of water, and 5 parts by weight of a 30% aqueous sodium hydroxide solution were added. The reaction mixture was then allowed to react for 1 hour, after which the reaction solution was repeatedly washed with water until the wash solution became neutral. Methyl isobutyl ketone was then distilled off from the oil layer under heating and reduced pressure to obtain 68 parts by weight of an epoxy resin represented by the following formula (3B). The epoxy equivalent of the obtained epoxy resin was 251 g / eq, the softening point was 63.9°C, the ICI melt viscosity (150°C) was 0.06 Pa s, and n in the following formula (3B) was 1.9. The HPLC results are shown in Figure 1, and the GPC results are shown in Figure 2.

[0066]

[0067] Comparative Synthesis Example 1: 254 parts by weight of phenol, 63 parts by weight of water, and 27 parts by weight of sodium hydroxide were charged into a flask equipped with a stirrer, a reflux condenser, and a stirring device. After stirring and dissolving, the mixture was heated to 110°C, and 44 parts by weight of furfural was added dropwise over 2 hours. The mixture was then reacted at 110°C for 3 hours, and then heated to 145°C. During the temperature increase, the distilled water was removed from the system. After reaching 145°C, the mixture was cooled to 80°C, and 63 parts by weight of water was charged. 4 parts by weight of phosphoric acid and 63 parts by weight of 35% hydrochloric acid were added for neutralization. After repeated water washing, unreacted phenol was distilled off under reduced pressure with heating to obtain 107 parts by weight of a phenolic resin represented by the following formula (4A):

[0068]

[0069] Comparative Synthesis Example 2: 78 parts by weight of the phenolic resin obtained in Comparative Synthesis Example 1 were charged into a reaction vessel with 254 parts by weight of epichlorohydrin (ECH), 64 parts by weight of dimethyl sulfoxide (DMSO), and 13 parts by weight of water. After heating, stirring, and dissolution, 23 parts by weight of flaky sodium hydroxide were added in portions over 2 hours while maintaining the temperature at 45°C. The reaction was then continued for 2 hours at 45°C and 60 minutes at 70°C. After repeated water washing to remove by-product salts and dimethyl sulfoxide, excess epichlorohydrin was distilled off from the oil layer under heating and reduced pressure. 218 parts by weight of methyl isobutyl ketone was added to the residue and dissolved. This methyl isobutyl ketone solution was heated to 70°C, and 7 parts by weight of a 30% aqueous sodium hydroxide solution was added. The reaction mixture was then allowed to react for 1 hour. The reaction solution was then repeatedly washed with water until the washings became neutral. Methyl isobutyl ketone was then distilled off from the oil layer under heating and reduced pressure to obtain 97 parts by weight of an epoxy resin represented by formula (4). The epoxy equivalent of the obtained epoxy resin was 211 g / eq, the softening point was 44°C, the ICI melt viscosity (150°C) was 0.06 Pa s, and n in the following formula (4B) was 2.1. The HPLC results are shown in Figure 3.

[0070]

[0071] Comparative Synthesis Example 3 According to Example 7 of JP 2001-64339 A, 432 parts by weight of orthocresol, 93 parts by weight of water, and 40 parts by weight of sodium hydroxide were charged into a flask equipped with a stirrer, a reflux condenser, and a stirring device, and after stirring and dissolving, the mixture was heated to 110°C, to which 78 parts by weight of furfural was added dropwise over 2 hours. The mixture was then reacted at 110°C for 3 hours, and then heated to 145°C. During the temperature increase, the distilled water was removed from the system. After reaching 145°C, the mixture was cooled to 80°C, and 92 parts by weight of water was charged. 6 parts by weight of phosphoric acid and 92 parts by weight of 35% hydrochloric acid were added for neutralization. After repeated water washing, unreacted phenol was distilled off under reduced pressure with heating to obtain 210 parts by weight of a phenolic resin represented by the following formula (5A):

[0072]

[0073] Comparative Synthesis Example 4: 94 parts by weight of the phenolic resin obtained in Comparative Synthesis Example 3 were charged into a reaction vessel with 248 parts by weight of epichlorohydrin (ECH), 44 parts by weight of dimethyl sulfoxide (DMSO), and 13 parts by weight of water. After heating, stirring, and dissolution, 25 parts by weight of flaky sodium hydroxide were added in portions over 2 hours while maintaining the temperature at 45°C. The reaction was then continued for 2 hours at 45°C and 60 minutes at 70°C. After repeated water washing to remove by-product salts and dimethyl sulfoxide, excess epichlorohydrin was distilled off from the oil layer under heating and reduced pressure. 256 parts by weight of methyl isobutyl ketone was added to the residue and dissolved. This methyl isobutyl ketone solution was heated to 70°C, and 5 parts by weight of a 30% aqueous sodium hydroxide solution was added. The reaction mixture was then allowed to react for 1 hour. The reaction solution was then repeatedly washed with water until the washings became neutral. Methyl isobutyl ketone was then distilled off from the oil layer under heating and reduced pressure to obtain 116 parts by weight of an epoxy resin represented by the following formula (5B). The epoxy equivalent of the obtained epoxy resin was 231 g / eq, the softening point was 50.1°C, the ICI melt viscosity (150°C) was 0.06 Pa s, and n in the following formula (5B) was 1.6. The HPLC results are shown in Figure 4.

[0074]

[0075] The epoxy resins obtained in Synthesis Example 2 and Comparative Synthesis Examples 2 and 4 were used as the base resin, and 4,4'-methylenebis(2,6-diethylaniline) (abbreviation: M-DEA, manufactured by Tokyo Chemical Industry Co., Ltd., active hydrogen equivalent: 78 g / eq.) was used as the curing agent. These were mixed in the weight ratios shown in Table 1, and cured at 160°C for 6 hours to produce cured products.

[0076] The physical properties were measured under the following conditions. <Measurement conditions for flexural modulus> Measured according to JIS K-7074. <Water absorption> Water absorption: Weight increase (%) after boiling a disk-shaped test piece with a diameter of 5 cm and a thickness of 4 mm in water at 100°C for 24 hours.

[0077]

[0078] From the results in Table 1, it was confirmed that Example 1 had a high flexural modulus and excellent low water absorbency.

Claims

1. An epoxy resin represented by the following formula (1): (In formula (1), there are multiple R 1 R independently represents a hydrocarbon group having 1 to 10 carbon atoms. 2 represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms. n is the average number of repetitions and is a real number in the range of 1<n<15.) 2. R in the above formula (1) 1 2. The epoxy resin according to claim 1, wherein is a methyl group.

3. A curable resin composition comprising the epoxy resin according to claim 1 and a curing agent.

4. The curable resin composition according to claim 3, which is for use in carbon fiber reinforced plastics.

5. A cured product obtained by curing the curable resin composition according to claim 3 or 4.

Citation Information

Patent Citations

  • Epoxy resin composition having improved toughness

    JP1985243113A

  • Epoxy resin composition for carbon-fiber reinforced composite material

    JP1997100358A

  • Controlled atmospheric pressure resin infusion process

    JP2005527410A

  • Epoxy resin composition and method for producing epoxy resin

    JP2007211254A

  • Prepreg and carbon fiber-reinforced composite material

    JP2013155330A

Cited By

  • Epoxy resin mixture, curable resin composition, and cured object therefrom

    WO2026160390A1