Kit for three-component coating composition, three-component coating composition, and in-mold coating method
The three-component coating composition kit addresses the challenges of VOC reduction and color consistency by optimizing the shear rates and viscosities of its components, resulting in improved adhesion and color uniformity and simplified cleaning processes.
Patent Information
- Application Number
- PCT/JP2024/010162
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional two-component coating compositions face challenges in reducing VOC content and efficiently changing colors, leading to increased cleaning efforts and potential color unevenness and decreased hardness and adhesion of the coating film.
A three-component coating composition kit comprising a base agent with an isocyanate-reactive group-containing compound, a curing agent with a polyisocyanate compound, and a pigment paste, where the shear rates and viscosities of the components are optimized to facilitate easy mixing and uniform curing, reducing VOC content and improving adhesion and color uniformity.
The three-component coating composition effectively reduces VOC content, simplifies the cleaning process when changing colors, and enhances the hardness and adhesion of the coating film while minimizing color unevenness.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Kit for three-component coating composition, three-component coating composition and method for coating inside a mold
[0001] The present invention relates to a kit for a three-component coating composition, a three-component coating composition, and an in-mold coating method using the kit or the three-component coating composition.
[0002] Conventionally, for the purpose of imparting excellent appearance, performance, etc. to a substrate surface, a coating film has been formed by applying a coating composition to the substrate surface and curing the formed wet coating film. In recent years, from the viewpoint of reducing the environmental load, there has been a demand for reducing volatile organic compounds (VOCs) in coating compositions and reducing the air conditioning energy required during painting.
[0003] Furthermore, in recent years, in various technical fields, there has been a demand for coating film performance such as high coating film hardness and high adhesion between the coating film and the substrate, as well as suppression of color unevenness.
[0004] Furthermore, when using a multicolored coating composition, there is a problem in that the time and effort required for cleaning the coating equipment is required when changing the coating color.
[0005] Patent Document 1 discloses a two-component coating material composition comprising a paint base component A and a curing component B, wherein the paint base component A comprises: i. one or more polyols A1 selected from the group of polyols containing ester groups, and having a hydroxyl value of 300 to 500 mg KOH / g and a hydroxyl group functionality of more than 2; ii. one or more polyols A1 selected from the group of polyols containing ester groups, and having a hydroxyl value of 300 to 500 mg KOH / g and a hydroxyl group functionality of more than 2; 1 -(OH) p (In the formula, R 1 is a p-valent branched, cyclic or straight-chain, saturated or unsaturated aliphatic hydrocarbon radical having 5 to 18 carbon atoms, and the radical R 1 optionally containing one or more tertiary amino groups, and p is 2 to 6), iii. one or more aliphatic polyols A2 of the general formula (II): R 2 -(C=O) r -O-(AO) s -R 3 (In the formula, R 2 is a saturated or unsaturated aliphatic hydrocarbon radical having 6 to 30 carbon atoms, R 3is H, radical PO(OH) 2 or a radical of an optionally partially phosphorylated mono- or disaccharide or a radical of an optionally partially phosphorylated alditol, where AO represents one or more alkylene oxide radicals selected from the group consisting of ethylene oxide, propylene oxide, and butylene oxide, r is 0 or 1, and s is 0 to 30), iv. one or more crosslinking catalysts A4 selected from the group of organotin compounds, v. one or more polyamines A5 having at least two secondary amino groups and an amine value of 120 to 280 mg KOH / g, and ix. one or more additives A9 selected from the group consisting of wetting agents and / or dispersants, rheological aids, and flow control agents, and wherein said curing component B comprises: i. The two-component coating material composition is described as comprising one or more polyisocyanates B1 having an average of 2.4 to 5 NCO groups, the two-component coating material composition having a solids content of at least 96% by weight according to ASTM D2369 (2015), based on the total weight of the two-component coating material composition, and characterized in that the molar ratio of NCO groups in the curing component B to the acidic hydrogen atoms of hydroxyl groups, primary amino groups and secondary amino groups in the paint base component A is from 1:1.15 to 1:0.95, allowing damage-free release from normally metal mold surfaces without the use of external mold release agents, while ensuring very good adhesion to the substrate and allowing recoating with further coating films, such as base coats and clear coats, to form surfaces of very good quality without costly and inconvenient cleaning and / or polishing steps.
[0006] Special Publication No. 2020-528103
[0007] Although the technology described in Patent Document 1 has a low VOC content in the resulting two-component coating composition, there is a problem in that when multiple colors are applied, the time and effort required for cleaning the coating equipment is required.
[0008] The present invention aims to provide a kit for a three-component paint composition that has a low VOC content, can shorten the process of cleaning the painting equipment when multiple colors are used, and can form a paint film that has excellent hardness and adhesion and suppresses color unevenness.
[0009] As a result of extensive research into achieving the above object, the present inventors have discovered a kit for a three-component coating composition, which kit comprises a base component (A) containing an isocyanate-reactive group-containing compound (a1), a curing agent (B) containing a polyisocyanate compound (b1), and a pigment paste (C) containing an isocyanate-reactive group-containing compound (c1) and a pigment (c2), wherein the base component (A) is heated at a shear rate of 100 sec -1 , viscosity at 65°C (V A ) is in the range of 20 to 1800 mPa s, and the shear rate of the curing agent (B) is 100 sec -1 , viscosity at 65°C (V B ) is in the range of 20 to 1800 mPa s, and the shear rate of the pigment paste (C) is 100 sec -1 , viscosity at 65°C (V C It has been found that the above object can be achieved by using a kit in which the viscosity is in the range of 20 to 1800 mPa·s.
[0010] That is, the present invention relates to the following items <1> to <7>.
[0011] <1> A kit for a three-component coating composition comprising (A) (a1) a base agent containing an isocyanate-reactive group-containing compound, (B) (b1) a curing agent containing a polyisocyanate compound, and (C) (c1) an isocyanate-reactive group-containing compound and (c2) a pigment paste, wherein the base agent (A) is cured at a shear rate of 100 sec -1 , viscosity at 65°C (V A ) is in the range of 20 to 1800 mPa s, and the shear rate of the curing agent (B) is 100 sec -1 , viscosity at 65°C (V B ) is in the range of 20 to 1800 mPa s, and the shear rate of the pigment paste (C) is 100 sec -1 , viscosity at 65°C (V C) is in the range of 20 to 1800 mPa·s. <2> The three-component coating composition according to <1>, wherein the solid content concentration is 95% by mass or more. <3> The kit according to <1> or <2>, wherein the solid content concentration of the pigment paste (C) is in the range of 85 to 98% by mass. <4> The kit according to any one of <1> to <3>, wherein the isocyanate-reactive group-containing compound (c1) includes an isocyanate-reactive group-containing compound having a number average molecular weight in the range of 250 to 2500. <5> The kit according to any one of <1> to <4>, wherein the content of the pigment (c2) is in the range of 1.0 to 65% by mass, based on the total amount of the pigment paste (C). <6> The three-component coating composition according to <1>, wherein the solid content concentration of the pigment paste (C) is 95% by mass or more. <7> The three-component coating composition according to <1>, wherein the solid content concentration of the pigment paste (C) is 95% by mass or more. <8> The three-component coating composition according to <1>, wherein the solid content concentration of the pigment paste (C) is 95% by mass or more. <9> The three-component coating composition according to <1>, wherein the solid content concentration of the pigment paste (C) is 95% by mass or more. <10> The three-component coating composition according to <1>, wherein the solid content concentration of the pigment paste (C) is 95% by mass or more. <11> The three-component coating composition according to <1>, wherein the solid content concentration of the pigment paste (C) is 95% by mass or more. <12> The three-component coating composition according to <1>, wherein the solid content concentration of the pigment paste (C) is 95% by mass or more. <13> The three-component coating composition according A ), the above (V B ) and (V C ) is satisfied by the following formula (1) and formula (2): 0.4≦(V B ) / (V A )≦2.5 Formula (1) 0.3≦(V C ) / (V A <7> A three-component coating composition comprising a base component (A) containing an isocyanate-reactive group-containing compound (a1), a curing agent (B) containing a polyisocyanate compound (b1), and a pigment paste (C) containing an isocyanate-reactive group-containing compound (c1) and a pigment (c2), wherein the base component (A) is cured at a shear rate of 100 sec -1 , viscosity at 65°C (V A ) is in the range of 20 to 1800 mPa s, and the shear rate of the curing agent (B) is 100 sec -1 , viscosity at 65°C (V B ) is in the range of 20 to 1800 mPa s, and the shear rate of the pigment paste (C) is 100 sec -1 , viscosity at 65°C (V C<8> An in-mold coating method comprising the steps of injecting an in-mold coating composition between a molded substrate and an inner wall of a mold, curing the in-mold coating composition, and then removing the coated molded article from the mold, wherein the in-mold coating composition is a three-component coating composition formed from the kit described in any one of <1> to <6>, or the three-component coating composition described in <7>.
[0012] According to the present invention, it is possible to provide a kit for a three-component paint composition which has a low VOC content, can shorten the process of cleaning the painting equipment when multiple colors are used, and can form a paint film which has excellent hardness and adhesion and suppresses color unevenness.
[0013] The present invention will be described in detail below, but these are examples of preferred embodiments, and the present invention is not limited to these details.
[0014] [Kit for three-component coating composition, and three-component coating composition] The kit for three-component coating composition according to the present invention (hereinafter, sometimes simply referred to as "kit") is a kit comprising a main component (A) containing an isocyanate-reactive group-containing compound (a1), a curing agent (B) containing a polyisocyanate compound (b1), and a pigment paste (C) containing an isocyanate-reactive group-containing compound (c1) and a pigment (c2), wherein the main component (A) is subjected to a shear rate of 100 sec -1 , viscosity at 65°C (V A ) is in the range of 20 to 1800 mPa s, and the shear rate of the curing agent (B) is 100 sec -1 , viscosity at 65°C (V B ) is in the range of 20 to 1800 mPa s, and the shear rate of the pigment paste (C) is 100 sec -1 , viscosity at 65°C (V C The three-component coating composition according to the present invention can be prepared by mixing a base component (A), a curing agent (B), and a pigment paste (C).
[0015] The viscosity (V A ), viscosity (VB ) and viscosity (V C The method for measuring the saturation temperature is described in the Examples.
[0016] The following is presumed to be the reason why the kit of the present invention can form a three-component paint composition that has a low VOC content, can shorten the process of cleaning the painting equipment when multiple colors are used, and can form a paint film that is excellent in hardness and adhesion and has reduced color unevenness.
[0017] When a two-component paint composition containing a pigment-containing base agent and a curing agent is made into multiple colors, either the base agent tank and piping must be cleaned when changing colors, or a base agent tank equal to the number of colors must be prepared and only the piping must be cleaned. Since tanks for base agents that are used in large quantities often have large capacities, cleaning the base agent tank and piping requires a lot of work, and when multiple base agent tanks are prepared, the size of the base agent tanks places a heavy burden on the painting site.
[0018] When a three-component paint composition containing a base agent (A), a curing agent (B), and a pigment paste (C) is used in multiple colors, the pigment paste (C) tank and piping must be cleaned when changing colors, or a pigment paste (C) tank equal in volume to the number of colors must be prepared and only the piping must be cleaned. Since tanks for pigment paste (C), which are used in small amounts, often have small volumes, cleaning the pigment paste (C) tank and piping reduces the effort required to clean the small-volume pigment paste (C) tank, and also, when multiple pigment paste (C) tanks are prepared, the pigment paste (C) tanks are small, so the burden on the painting site is small.
[0019] However, although a three-component paint composition can shorten the process of cleaning the painting equipment when changing colors when multiple colors are used, it has been found that when a paint composition with a low VOC content is used as a three-component paint composition, color unevenness is likely to occur and hardness and adhesion are likely to decrease.
[0020] When the above-mentioned coating composition having a low VOC content is used as a three-component coating composition, color unevenness is likely to occur and hardness and adhesion are likely to decrease. This is presumably because it is difficult to adjust the viscosity of the coating composition having a low VOC content using a solvent, making it difficult for the three components of the base resin (A), curing agent (B) and pigment paste (C) to mix.
[0021] Therefore, as a result of intensive research by the present inventors, it was found that the shear rate of the main component (A) was 100 sec -1 , viscosity at 65°C (V A ) is in the range of 20 to 1800 mPa s, and the shear rate of the curing agent (B) is 100 sec -1 , viscosity at 65°C (V B ) is in the range of 20 to 1800 mPa s, and the shear rate of the pigment paste (C) is 100 sec -1 , viscosity at 65°C (V C ) is in the range of 20 to 1800 mPa·s, it has been found that even with the above-mentioned three-component coating composition having a low VOC content, a coating film having excellent hardness and adhesion and suppressed color unevenness can be formed.
[0022] In the kit according to the present invention, even the three-component paint composition with a low VOC content suppresses color unevenness and exhibits excellent hardness and adhesion. This is presumably because the three components of the base resin (A), curing agent (B), and pigment paste (C) mix easily, allowing the entire paint film to cure uniformly.
[0023] The solids concentration of the three-component paint composition formed from the kit according to the present invention or the three-component paint composition according to the present disclosure is preferably 95% by mass or more, more preferably 96% by mass or more, and even more preferably 97% by mass or more, from the viewpoints of reducing the VOC content in the resulting paint composition and preventing hardness and color unevenness of the formed coating film, etc. The upper limit of the solids concentration is 100% by mass.
[0024] In this specification, the term "solid content" refers to non-volatile components such as resins, curing agents, and pigments that remain after drying for 30 minutes at 80° C. The solid content can be determined, for example, by weighing a sample into a heat-resistant container such as an aluminum foil cup, spreading the sample on the bottom of the container, drying it at 80° C. for 30 minutes, and weighing the mass of the components remaining after drying.
[0025] In this specification, the term "solid content concentration" refers to the mass ratio of the solid content in the composition. Therefore, the solid content concentration of the composition can be calculated by, for example, weighing 1.0 g of the composition into a heat-resistant container such as an aluminum foil cup, spreading the composition on the bottom of the container, drying at 80°C for 30 minutes, weighing the mass of the components remaining in the composition after drying, and determining the ratio of the mass of the components remaining after drying to the total mass of the composition before drying.
[0026] The shear rate of the main agent (A) is 100 sec -1 , viscosity at 65°C (V A ), the shear rate of the curing agent (B) is 100 sec -1 , viscosity at 65°C (V B ) and the pigment paste (C), a shear rate of 100 sec -1 , viscosity at 65°C (V C ) is determined based on the following formula (1) and formula (2): 0.1≦(V B ) / (V A )≦7.1 0.2≦(V C ) / (V A )≦5.6 is preferably satisfied.
[0027] The shear rate of the main agent (A) is 100 sec -1 , viscosity at 65°C (V A ), the shear rate of the curing agent (B) is 100 sec -1 , viscosity at 65°C (V B ) and the pigment paste (C), a shear rate of 100 sec -1 , viscosity at 65°C (V C ) is determined from the viewpoint of the hardness, adhesion, color unevenness, etc. of the coating film to be formed, by satisfying the following formula (1) and formula (2): 0.4≦(VB ) / (V A )≦2.5 Formula (1) 0.3≦(V C ) / (V A )≦3.0 It is more preferable that the following formula (2) is satisfied.
[0028] The shear rate of the main agent (A) is 100 sec -1 , viscosity at 65°C (V A ) and the curing agent (B), at a shear rate of 100 sec -1 , viscosity at 65°C (V B ) is set to 0.4≦(V B ) / (V A )≦2.0, and more preferably, 0.4≦(V B ) / (V A )≦1.5 is more preferable.
[0029] The shear rate of the main agent (A) is 100 sec -1 , viscosity at 65°C (V A ) and pigment paste (C), shear rate 100 sec -1 , viscosity at 65°C (V C ) is set to 0.3≦(V C ) / (V A )≦2.5, and more preferably 0.4≦(V C ) / (V A )≦2.0 is more preferable.
[0030] [Main ingredient (A)] The main ingredient (A) contains an isocyanate-reactive group-containing compound (a1). [Isocyanate-reactive group-containing compound (a1)] The isocyanate-reactive group-containing compound (a1) is a compound having at least one isocyanate-reactive group in one molecule.
[0031] The isocyanate-reactive group is not particularly limited as long as it is a group reactive with an isocyanate group. Examples of the isocyanate-reactive group include a hydroxyl group, an amino group, and a thiol group. From the viewpoints of the hardness, adhesion, and color unevenness of the coating film to be formed, it is preferable that the isocyanate-reactive group contains at least one selected from a hydroxyl group and an amino group, and more preferably contains a hydroxyl group.
[0032] Therefore, examples of the isocyanate-reactive group-containing compound (a1) include a hydroxyl group-containing compound (a11), an amino group-containing compound (a12), and a thiol group-containing compound (a13). From the viewpoints of the hardness, adhesion, and color unevenness of the coating film to be formed, it is preferable for the compound to contain at least one compound selected from the hydroxyl group-containing compound (a11) and the amino group-containing compound (a12), and it is more preferable for the compound to contain the hydroxyl group-containing compound (a11).
[0033] From the viewpoints of reducing the VOC content in the resulting coating composition and improving the hardness, adhesion, and color unevenness of the coating film formed, the isocyanate-reactive group-containing compound (a1) preferably contains an isocyanate-reactive group-containing compound having a number average molecular weight in the range of 250 to 2500, more preferably in the range of 300 to 1800, and even more preferably in the range of 300 to 1500.
[0034] [Hydroxyl group-containing compound (a11)] The above-mentioned hydroxyl group-containing compound (a11) is a compound having at least one hydroxyl group in one molecule.As the hydroxyl group-containing compound (a11), as hydroxyl group-containing oligomer and hydroxyl group-containing polymer, for example, hydroxyl group-containing polyester resin, hydroxyl group-containing polycaprolactone resin, hydroxyl group-containing polyether resin, hydroxyl group-containing polycarbonate resin, hydroxyl group-containing acrylic resin, hydroxyl group-containing polyurethane resin, hydroxyl group-containing epoxy resin, hydroxyl group-containing alkyd resin etc. can be enumerated.Among them, from the viewpoint of reducing the VOC content in the obtained coating composition, and the hardness, adhesion and color unevenness of the coating film formed, it is preferable to comprise at least one resin selected from hydroxyl group-containing polyester resin, hydroxyl group-containing polycaprolactone resin and hydroxyl group-containing polyether resin, more preferably comprise at least one resin selected from hydroxyl group-containing polyester resin and hydroxyl group-containing polycaprolactone resin. These can be used alone or in combination of two or more.
[0035] The hydroxyl group-containing polyester resin can usually be produced by an esterification reaction or transesterification reaction between an acid component and an alcohol component.
[0036] The acid component may be a compound that is commonly used as a polycarboxylic acid in the production of the hydroxyl group-containing polyester resin, such as an aliphatic polybasic acid, an alicyclic polybasic acid, or an aromatic polybasic acid.
[0037] The aliphatic polybasic acid is generally an aliphatic compound having two or more carboxyl groups per molecule, an acid anhydride of the aliphatic compound, or an ester of the aliphatic compound. Examples of the aliphatic polybasic acid include aliphatic polycarboxylic acids such as succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, brassylic acid, octadecanedioic acid, citric acid, and butanetetracarboxylic acid; anhydrides of the aliphatic polybasic carboxylic acids; and lower alkyl esters of the aliphatic polybasic carboxylic acids having 1 to 6 carbon atoms, preferably 1 to 4 carbon atoms. The aliphatic polybasic acids can be used alone or in combination of two or more.
[0038] The alicyclic polybasic acids are generally compounds having one or more alicyclic structures and two or more carboxyl groups per molecule, acid anhydrides of such compounds, and esterified products of such compounds. The alicyclic structures can be primarily 4- to 6-membered ring structures. Examples of alicyclic polybasic acids include alicyclic polycarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 4-cyclohexene-1,2-dicarboxylic acid, 3-methyl-1,2-cyclohexanedicarboxylic acid, 4-methyl-1,2-cyclohexanedicarboxylic acid, 1,2,4-cyclohexanetricarboxylic acid, and 1,3,5-cyclohexanetricarboxylic acid; anhydrides of such alicyclic polycarboxylic acids; and lower alkyl esters of such alicyclic polycarboxylic acids having 1 to 6 carbon atoms, preferably 1 to 4 carbon atoms. The alicyclic polybasic acids can be used alone or in combination of two or more.
[0039] The aromatic polybasic acid is generally an aromatic compound having two or more carboxyl groups per molecule, an acid anhydride of the aromatic compound, or an ester of the aromatic compound. Examples of the aromatic polybasic acid include aromatic polycarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, trimellitic acid, and pyromellitic acid; anhydrides of the aromatic polycarboxylic acids; and lower alkyl esters of the aromatic polycarboxylic acids having 1 to 6 carbon atoms, preferably 1 to 4 carbon atoms. The aromatic polybasic acids can be used alone or in combination of two or more.
[0040] Acid components other than the above-mentioned aliphatic polybasic acids, alicyclic polybasic acids, and aromatic polybasic acids can also be used. Such acid components are not particularly limited, and examples include fatty acids such as coconut oil fatty acids, cottonseed oil fatty acids, hempseed oil fatty acids, rice bran oil fatty acids, fish oil fatty acids, tall oil fatty acids, soybean oil fatty acids, linseed oil fatty acids, tung oil fatty acids, rapeseed oil fatty acids, castor oil fatty acids, dehydrated castor oil fatty acids, and safflower oil fatty acids; monocarboxylic acids such as isononanoic acid, neodecanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, benzoic acid, p-tert-butylbenzoic acid, cyclohexanoic acid, and 10-phenyloctadecanoic acid; and hydroxycarboxylic acids such as lactic acid, 3-hydroxybutanoic acid, and 3-hydroxy-4-ethoxybenzoic acid. These acid components can be used alone or in combination of two or more.
[0041] As the alcohol component, a polyhydric alcohol having two or more hydroxyl groups in one molecule can be suitably used. Examples of the polyhydric alcohol include ethylene glycol, propylene glycol, diethylene glycol, trimethylene glycol, tetraethylene glycol, triethylene glycol, dipropylene glycol, 1,4-butanediol, 1,3-butanediol, 2,3-butanediol, 1,2-butanediol, 2-methyl-1,3-propanediol, 3-methyl-1,2-butanediol, 2-butyl-2-ethyl-1,3-propanediol, 1,2-pentanediol, 1 ,5-pentanediol, 1,4-pentanediol, 2,4-pentanediol, 2,3-dimethyltrimethylene glycol, tetramethylene glycol, 3-methyl-4,3-pentanediol, 3-methyl-1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 1,6-hexanediol, 1,5-hexanediol, 1,4-hexanediol, 2,5-hexanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, tricyclohexane dihydric alcohols such as candimethanol, hydroxypivalic acid neopentyl glycol ester, hydrogenated bisphenol A, hydrogenated bisphenol F, and dimethylolpropionic acid; polylactone diols obtained by adding a lactone compound such as ε-caprolactone to these dihydric alcohols; ester diol compounds such as bis(hydroxyethyl) terephthalate; polyether diol compounds such as alkylene oxide adducts of bisphenol A, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; trihydric or higher alcohols such as glycerin, trimethylolethane, trimethylolpropane, diglycerin, triglycerin, 1,2,6-hexanetriol, pentaerythritol, dipentaerythritol, tris(2-hydroxyethyl)isocyanuric acid, sorbitol, and mannite; polylactone polyol compounds obtained by adding a lactone compound such as ε-caprolactone to these trihydric or higher alcohols; and fatty acid esters of glycerin.
[0042] Alcohol components other than the above polyhydric alcohols can also be used. Examples of such alcohol components include, but are not limited to, monoalcohols such as methanol, ethanol, propyl alcohol, butyl alcohol, isobutyl alcohol, pentyl alcohol, 2-ethylhexyl alcohol, stearyl alcohol, benzyl alcohol, phenethyl alcohol, and 2-phenoxyethanol; and alcohol compounds obtained by reacting a monoepoxy compound such as propylene oxide, butylene oxide, or "Cardura E10P" (trade name, manufactured by Hexion, a glycidyl ester of synthetic highly branched saturated fatty acid) with an acid.
[0043] The method for producing the hydroxyl group-containing polyester resin is not particularly limited and can be carried out according to a conventional method. For example, the hydroxyl group-containing polyester polyol resin can be produced by a method in which the acid component and the alcohol component are heated in a nitrogen stream at about 150 to 250°C for about 5 to 10 hours to cause an esterification reaction or a transesterification reaction between the acid component and the alcohol component.
[0044] When the acid component and the alcohol component are subjected to an esterification reaction or transesterification reaction, these components may be added to a reaction vessel all at once, or one or both may be added in several portions. Alternatively, the hydroxyl-containing polyester resin may be first synthesized, and then the resulting hydroxyl-containing polyester resin may be reacted with an acid anhydride to half-esterify it into a carboxyl- and hydroxyl-containing polyester resin. Alternatively, the carboxyl-containing polyester resin may be first synthesized, and then the alcohol component may be added to produce the hydroxyl-containing polyester resin.
[0045] In the above-mentioned esterification or transesterification reaction, a catalyst known per se, such as dibutyltin oxide, antimony trioxide, zinc acetate, manganese acetate, cobalt acetate, calcium acetate, lead acetate, tetrabutyl titanate, or tetraisopropyl titanate, can be used as a catalyst for promoting the reaction.
[0046] The hydroxyl group-containing polyester resin can be modified during or after production with a fatty acid, a monoepoxy compound, a polyisocyanate compound, etc. Examples of the fatty acid include coconut oil fatty acid, cottonseed oil fatty acid, hempseed oil fatty acid, rice bran oil fatty acid, fish oil fatty acid, tall oil fatty acid, soybean oil fatty acid, linseed oil fatty acid, tung oil fatty acid, rapeseed oil fatty acid, castor oil fatty acid, dehydrated castor oil fatty acid, and safflower oil fatty acid. An example of the monoepoxy compound that can be suitably used is "Cardura E10P" (trade name, manufactured by Hexion, a glycidyl ester of a synthetic highly branched saturated fatty acid).
[0047] Examples of the polyisocyanate compound include aliphatic diisocyanate compounds such as lysine diisocyanate, hexamethylene diisocyanate, and trimethylhexane diisocyanate; alicyclic diisocyanate compounds such as hydrogenated xylylene diisocyanate, isophorone diisocyanate, methylcyclohexane-2,4-diisocyanate, methylcyclohexane-2,6-diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), 1,3-(isocyanatomethyl)cyclohexane, and 1,4-(isocyanatomethyl)cyclohexane; Examples of suitable organic polyisocyanates include aromatic diisocyanate compounds such as isocyanate, xylylene diisocyanate, tetramethylxylylene diisocyanate, and diphenylmethane diisocyanate; organic polyisocyanates themselves, such as trivalent or higher polyisocyanates, such as lysine triisocyanate and 4-(isocyanatomethyl)octamethylene diisocyanate; adducts of these organic polyisocyanates with polyhydric alcohols, low-molecular-weight polyester resins, water, etc.; and cyclized polymers of these organic polyisocyanates (for example, isocyanurates), biuret adducts, and allophanate adducts. These polyisocyanate compounds can be used alone or in combination of two or more.
[0048] From the viewpoint of the hardness and adhesion of the coating film to be formed, the hydroxyl value of the hydroxyl-containing polyester resin is preferably within a range of 50 to 800 mgKOH / g, more preferably within a range of 100 to 700 mgKOH / g, and even more preferably within a range of 300 to 600 mgKOH / g.
[0049] The number average molecular weight of the hydroxyl group-containing polyester resin is preferably in the range of 250 to 2500, more preferably in the range of 300 to 1800, and even more preferably in the range of 350 to 1500, from the viewpoints of reducing the VOC content in the resulting coating composition and improving the hardness, adhesion, and color unevenness of the coating film formed. The glass transition temperature (Tg) of the hydroxyl group-containing polyester resin is preferably in the range of -80 to 10°C, more preferably in the range of -70 to 5°C, and even more preferably in the range of -60 to 0°C, from the viewpoints of reducing the VOC content in the resulting coating composition and improving the hardness, adhesion, and color unevenness of the coating film formed. In this specification, the number average molecular weight and weight average molecular weight are values calculated by converting the retention time (retention volume) measured using gel permeation chromatography (GPC) to the molecular weight of polystyrene using the retention time (retention volume) of a standard polystyrene of known molecular weight measured under the same conditions. Specifically, the gel permeation chromatograph uses "HLC-8120GPC" (trade name, manufactured by Tosoh Corporation) as the apparatus, and uses a total of four columns, "TSKgel G4000HXL," "TSKgel G3000HXL," "TSKgel G2500HXL," and "TSKgel G2000HXL" (trade names, all manufactured by Tosoh Corporation), and a differential refractometer as the detector. Measurement can be performed under the following conditions: mobile phase: tetrahydrofuran, measurement temperature: 40°C, flow rate: 1 mL / min.
[0050] The glass transition temperature can be measured, for example, using a differential scanning calorimeter "DSC-50Q" (trade name, manufactured by Shimadzu Corporation), by placing a sample in a measuring cup, vacuum suctioning to completely remove the solvent, and then measuring the change in calorific value in the range of -100°C to 150°C at a temperature increase rate of 3°C / min, and defining the first change point in the baseline on the low temperature side as the static glass transition temperature.
[0051] When the hydroxyl group-containing compound (a11) contains a hydroxyl group-containing polyester resin, the content of the hydroxyl group-containing polyester resin is preferably in the range of 50 to 100 mass %, more preferably in the range of 60 to 95 mass %, and even more preferably in the range of 70 to 90 mass %, based on the total solid content of the hydroxyl group-containing compound (a11), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film to be formed.
[0052] The hydroxyl group-containing polycaprolactone resin can be obtained, for example, by ring-opening polymerization of ε-caprolactone using a dihydric to tetrahydric polyhydric alcohol as an initiator. Examples of the dihydric or higher polyhydric alcohol include polyhydric alcohol compounds obtained by reacting ethylene glycol, glycerin, trimethylolethane, trimethylolpropane, diglycerin, ditrimethylolpropane, 1,2,6-hexanetriol, pentaerythritol, tris(2-hydroxyethyl)isocyanuric acid, or dimethylolalkanoic acid with a monoepoxy compound (e.g., "Cardura E10P; glycidyl ester of synthetic highly branched saturated fatty acid" manufactured by HEXION Specialty Chemicals). These compounds can be used alone or in combination of two or more. Commercially available hydroxyl group-containing polycaprolactone resins can also be used.Commercially available products include, for example, "Placcel 205," "Placcel 205H," "Placcel L205AL," "Placcel 205U," "Placcel 208," "Placcel 210," "Placcel 210N," "Placcel 210CP," "Placcel 212," "Placcel L212AL," "Placcel 220," "Placcel 220N," "Placcel 220CPB," "Placcel 220CPT," and "Placcel 2 20UA," "Placcel 220NP1," "Placcel L220AL," "Placcel 220EB," "Placcel 230," "Placcel 230N," "Placcel 240," "Placcel 303," "Placcel 305," "Placcel 308," "Placcel 309," "Placcel 312," "Placcel 320," "Placcel L320AL," "Placcel 410" (all trade names, manufactured by Daicel Corporation), "TONE 0201'', ``TONE 0230'', ``TONE 0249'', ``TONE 0301'', ``TONE 0305'', ``TONE 0310'', ``TONE 1241'', ``TONE 1278'', ``TONE 2221'' (the above, product name, The Dow Chemical), "Capa 2043", "Capa 2101", "Capa 2201", "Capa 2205", "Capa 2209", "Capa 2201A", "Capa 2203A", "Capa 7201A", "Capa 7203'', ``Capa 3031'', ``Capa 3050J'', ``Capa 3091'', ``Capa 4101" (trade name, manufactured by Ingevity Inc.) and the like.
[0053] From the viewpoint of the hardness and adhesion of the coating film to be formed, the hydroxyl value of the hydroxyl group-containing polycaprolactone resin is preferably within a range of 50 to 900 mgKOH / g, more preferably within a range of 100 to 750 mgKOH / g, and even more preferably within a range of 130 to 600 mgKOH / g.
[0054] Furthermore, from the viewpoints of reducing the VOC content in the resulting coating composition and improving the hardness, adhesion, and color unevenness of the coating film formed, the number average molecular weight of the hydroxyl group-containing polycaprolactone resin is preferably within the range of 250 to 2500, more preferably within the range of 280 to 1500, and even more preferably within the range of 300 to 1000. When the hydroxyl group-containing compound (a11) contains the hydroxyl group-containing polycaprolactone resin, the content of the hydroxyl group-containing polycaprolactone resin is preferably within the range of 5 to 100 mass%, more preferably within the range of 10 to 75 mass%, and even more preferably within the range of 10 to 50 mass%, based on the total solids content of the hydroxyl group-containing compound (a11), from the viewpoints of reducing the VOC content in the resulting coating composition and improving the hardness, adhesion, and color unevenness of the coating film formed.
[0055] Examples of the hydroxyl group-containing polyether resin that can be used include alkylene oxide adducts of hydroxyl group-containing monomers, and ring-opening (co)polymers of alkylene oxides or cyclic ethers (tetrahydrofuran, etc.), which will be described later. Specific examples include polyethylene glycol, polypropylene glycol, polytetramethylene glycol, ethylene glycol-propylene glycol (block or random) copolymers, polyhexamethylene glycol, and polyoctamethylene glycol. The hydroxyl group-containing polyether resins can be used alone or in combination of two or more.
[0056] From the viewpoint of the hardness and adhesion of the coating film to be formed, the hydroxyl value of the hydroxyl-containing polyether resin is preferably within a range of 50 to 600 mgKOH / g, more preferably within a range of 70 to 500 mgKOH / g, and even more preferably within a range of 90 to 400 mgKOH / g.
[0057] The number average molecular weight of the hydroxyl group-containing polyether resin is preferably in the range of 250 to 2500, more preferably in the range of 300 to 1500, and even more preferably in the range of 350 to 1000, from the viewpoints of reducing the VOC content in the resulting coating composition and of improving the hardness, adhesion, and color unevenness of the coating film formed.
[0058] When the hydroxyl group-containing compound (a11) contains the above-mentioned hydroxyl group-containing polyether resin, the content of the hydroxyl group-containing polyether resin is preferably in the range of 20 to 100 mass %, more preferably in the range of 40 to 100 mass %, and even more preferably in the range of 50 to 100 mass %, based on the total solid content of the hydroxyl group-containing compound (a11), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film to be formed.
[0059] The hydroxyl group-containing polycarbonate resin is a compound obtained by a conventional polycondensation reaction of a known polyol component with a carbonylating agent. Examples of the polyol component include a diol component and a polyhydric alcohol component such as a trihydric or higher alcohol.
[0060] Examples of the diol component include linear diols such as 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol; 2-methyl-1,3-propanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, 2-ethyl-1,6-hexanediol, 2,2-diethyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-methyl-1,8-octanediol, 2,2, Examples of suitable diol components include branched diols such as 4-trimethyl-1,3-pentanediol and 2-ethyl-1,3-hexanediol; alicyclic diols such as 1,3-cyclohexanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol and 2,2,4,4-tetramethyl-1,3-cyclobutanediol; aromatic diols such as p-xylenediol and p-tetrachloroxylenediol; ether-based diols such as diethylene glycol and dipropylene glycol; and polylactone diols obtained by adding a lactone compound such as ε-caprolactone to any of these diol components. These diol components can be used alone or in combination of two or more.
[0061] Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, a dimer of trimethylolpropane, and pentaerythritol; polylactone polyols obtained by adding a lactone compound such as ε-caprolactone to any of these trihydric or higher alcohols; and these trihydric or higher alcohols can be used alone or in combination of two or more.
[0062] As the carbonylating agent, known agents can be used. Specific examples include alkylene carbonate, dialkyl carbonate, diallyl carbonate, phosgene, etc., and these can be used alone or in combination of two or more. Among these, preferred examples include ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, dibutyl carbonate, diphenyl carbonate, etc.
[0063] From the viewpoint of the hardness and adhesion of the coating film to be formed, the hydroxyl value of the hydroxyl group-containing polycarbonate resin is preferably within a range of 50 to 800 mgKOH / g, more preferably within a range of 70 to 700 mgKOH / g, and even more preferably within a range of 90 to 600 mgKOH / g.
[0064] The number average molecular weight of the hydroxyl group-containing polycarbonate resin is preferably within the range of 250 to 2500, more preferably within the range of 300 to 1800, and even more preferably within the range of 400 to 1500, from the viewpoints of reducing the VOC content in the resulting coating composition and of improving the hardness, adhesion, and color unevenness of the coating film formed.
[0065] When the hydroxyl group-containing compound (a11) contains the above-mentioned hydroxyl group-containing polycarbonate resin, the content of the hydroxyl group-containing polycarbonate resin is preferably in the range of 5 to 80 mass %, more preferably in the range of 10 to 50 mass %, and even more preferably in the range of 10 to 40 mass %, based on the total solid content of the hydroxyl group-containing compound (a11), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film to be formed.
[0066] The hydroxyl group-containing acrylic resin can be produced, for example, by copolymerizing a hydroxyl group-containing polymerizable unsaturated monomer and another polymerizable unsaturated monomer copolymerizable with the hydroxyl group-containing polymerizable unsaturated monomer by a method known per se, such as a solution polymerization method in an organic solvent or an emulsion polymerization method in water.
[0067] The hydroxyl group-containing polymerizable unsaturated monomer is a compound having one or more hydroxyl groups and one or more polymerizable unsaturated bonds per molecule. Examples of the hydroxyl group-containing polymerizable unsaturated monomer include monoesters of (meth)acrylic acid with dihydric alcohols having 2 to 8 carbon atoms, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; ε-caprolactone-modified monoesters of (meth)acrylic acid with dihydric alcohols having 2 to 8 carbon atoms; N-hydroxymethyl (meth)acrylamide; allyl alcohol; and (meth)acrylates having a polyoxyethylene chain with a hydroxyl group at the molecular terminal.
[0068] However, in the present invention, a monomer corresponding to the polymerizable unsaturated monomer having an ultraviolet-absorbing functional group (xvii) described later should be defined as another polymerizable unsaturated monomer copolymerizable with the hydroxyl group-containing polymerizable unsaturated monomer, and is excluded from the hydroxyl group-containing polymerizable unsaturated monomer. These can be used alone or in combination of two or more kinds.
[0069] As other polymerizable unsaturated monomers copolymerizable with the above-mentioned hydroxyl group-containing polymerizable unsaturated monomers, for example, the following monomers (i) to (xx) can be used. These polymerizable unsaturated monomers can be used alone or in combination of two or more.
[0070] (i) Alkyl or cycloalkyl (meth)acrylates: for example, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, tridecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, cyclododecyl (meth)acrylate, tricyclodecanyl (meth)acrylate, and the like. (ii) Polymerizable unsaturated monomers having an isobornyl group: isobornyl(meth)acrylate, etc. (iii) Polymerizable unsaturated monomers having an adamantyl group: adamantyl(meth)acrylate, etc. (iv) Polymerizable unsaturated monomers having a tricyclodecenyl group: tricyclodecenyl(meth)acrylate, etc. (v) Polymerizable unsaturated monomers containing an aromatic ring: benzyl(meth)acrylate, styrene, α-methylstyrene, vinyltoluene, etc.
[0071] (vi) Polymerizable unsaturated monomers having an alkoxysilyl group: vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(2-methoxyethoxy)silane, γ-(meth)acryloyloxypropyltrimethoxysilane, γ-(meth)acryloyloxypropyltriethoxysilane, etc. (vii) Polymerizable unsaturated monomers having a fluorinated alkyl group: perfluoroalkyl (meth)acrylates such as perfluorobutylethyl (meth)acrylate and perfluorooctylethyl (meth)acrylate; fluoroolefins, etc. (viii) Polymerizable unsaturated monomers having a photopolymerizable functional group such as a maleimide group. (ix) Vinyl compounds: N-vinylpyrrolidone, ethylene, butadiene, chloroprene, vinyl propionate, vinyl acetate, etc. (x) Carboxyl group-containing polymerizable unsaturated monomers: (meth)acrylic acid, maleic acid, crotonic acid, β-carboxyethyl (meth)acrylate, etc.
[0072] (xi) Nitrogen-containing polymerizable unsaturated monomers: (meth)acrylonitrile, (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylamide, methylene bis(meth)acrylamide, ethylene bis(meth)acrylamide, adducts of glycidyl (meth)acrylate and amine compounds, etc. (xii) Polymerizable unsaturated monomers having two or more polymerizable unsaturated groups in one molecule: allyl (meth)acrylate, ethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, etc. (xiii) Epoxy group-containing polymerizable unsaturated monomers: glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 3,4-epoxycyclohexylethyl (meth)acrylate, 3,4-epoxycyclohexylpropyl (meth)acrylate, allyl glycidyl ether, etc. (xiv) (meth)acrylates having a polyoxyethylene chain whose molecular terminal is an alkoxy group. (xv) Sulfonic acid group-containing polymerizable unsaturated monomers: 2-acrylamido-2-methylpropanesulfonic acid, 2-sulfoethyl (meth)acrylate, allylsulfonic acid, 4-styrenesulfonic acid, etc.; sodium salts and ammonium salts of these sulfonic acids, etc.
[0073] (xvi) Polymerizable unsaturated monomers having a phosphate group: acid phosphooxyethyl (meth)acrylate, acid phosphooxypropyl (meth)acrylate, acid phosphooxypoly(oxyethylene)glycol (meth)acrylate, acid phosphooxypoly(oxypropylene)glycol (meth)acrylate, etc. (xvii) Polymerizable unsaturated monomers having an ultraviolet absorbing functional group: 2-hydroxy-4(3-methacryloyloxy-2-hydroxypropoxy)benzophenone, 2-hydroxy-4-(3-acryloyloxy-2-hydroxypropoxy)benzophenone, 2,2'-dihydroxy-4-(3-methacryloyloxy-2-hydroxypropoxy)benzophenone, 2,2'-dihydroxy-4-(3-acryloyloxy-2-hydroxypropoxy)benzophenone, 2-(2'-hydroxy-5'-methacryloyloxyethylphenyl)-2H-benzotriazole, etc. (xviii) Light-stable polymerizable unsaturated monomers: 4-(meth)acryloyloxy-1,2,2,6,6-pentamethylpiperidine, 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-crotonoyloxy-2,2,6,6-tetramethylpiperidine, 4-crotonoylamino-2,2,6,6-tetramethylpiperidine, 1-crotonoyl-4-crotonoyloxy-2,2,6,6-tetramethylpiperidine, and the like. (xix) Polymerizable unsaturated monomers having a carbonyl group: acrolein, diacetone acrylamide, diacetone methacrylamide, acetoacetoxyethyl methacrylate, formyl styrene, vinyl alkyl ketones having 4 to 7 carbon atoms (e.g., vinyl methyl ketone, vinyl ethyl ketone, vinyl butyl ketone), etc. (xx) Polymerizable unsaturated monomers having an acid anhydride group: maleic anhydride, itaconic anhydride, citraconic anhydride, etc.
[0074] In this specification, the term "polymerizable unsaturated group" refers to an unsaturated group that can undergo radical polymerization, such as a vinyl group, a (meth)acryloyl group, a (meth)acrylamide group, a vinyl ether group, an allyl group, a propenyl group, an isopropenyl group, or a maleimide group.
[0075] In addition, in this specification, "(meth)acrylate" means acrylate and / or methacrylate. "(meth)acrylic acid" means acrylic acid and / or methacrylic acid. "(meth)acryloyl" means acryloyl and / or methacryloyl. "(meth)acrylamide" means acrylamide and / or methacrylamide.
[0076] From the viewpoint of the hardness and adhesion of the coating film to be formed, the hydroxyl value of the hydroxyl-containing acrylic resin is preferably within a range of 5 to 240 mgKOH / g, more preferably within a range of 20 to 220 mgKOH / g, and even more preferably within a range of 25 to 200 mgKOH / g.
[0077] The number average molecular weight of the hydroxyl group-containing acrylic resin is preferably in the range of 250 to 2500, more preferably in the range of 300 to 1800, and even more preferably in the range of 500 to 1500, from the viewpoints of reducing the VOC content in the resulting coating composition and of improving the hardness, adhesion, and color unevenness of the coating film formed.
[0078] The glass transition temperature (Tg) of the hydroxyl group-containing acrylic resin is preferably within the range of -60 to 80°C, more preferably within the range of -50 to 70°C, and even more preferably within the range of -40 to 60°C, from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film formed.
[0079] In this specification, the glass transition temperature (Tg) of the hydroxyl group-containing acrylic resin is a value calculated by the following formula: 1 / Tg(K)=W1 / T1+W2 / T2+...Wn / Tn Tg(°C)=Tg(K)-273 In the formula, W1, W2,...Wn are the mass fractions of each monomer, and T1, T2,...Tn are the glass transition temperatures Tg(K) of the homopolymers of each monomer.
[0080] The glass transition temperature of the homopolymer of each monomer is a value according to POLYMER HANDBOOK Fourth Edition, edited by J. Brandrup, E. h. Immergut, and E. A. Grulke (1999). The glass transition temperature of a monomer not described in the document is the static glass transition temperature when a homopolymer of the monomer is synthesized so as to have a weight-average molecular weight of about 50,000.
[0081] When the hydroxyl group-containing compound (a11) contains the above-mentioned hydroxyl group-containing acrylic resin, the content of the hydroxyl group-containing acrylic resin is preferably in the range of 5 to 100 mass %, more preferably in the range of 10 to 75 mass %, and even more preferably in the range of 15 to 50 mass %, based on the total solid content of the hydroxyl group-containing compound (a11), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film to be formed.
[0082] The hydroxyl group-containing compound (a11) may be, for example, ethylene glycol, propylene glycol, diethylene glycol, trimethylene glycol, tetraethylene glycol, triethylene glycol, dipropylene glycol, 1,4-butanediol, 1,3-butanediol, 2,3-butanediol, 1,2-butanediol, 2-methyl-1,3-propanediol, 3-methyl-1,2-butanediol, 2 -butyl-2-ethyl-1,3-propanediol, 1,2-pentanediol, 1,5-pentanediol, 1,4-pentanediol, 2,4-pentanediol, 2,3-dimethyltrimethylene glycol, tetramethylene glycol, 3-methyl-4,3-pentanediol, 3-methyl-1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 1,6-hexanediol, 1,5-hexanediol, 1,4-hexanediol ethanol, 2,5-hexanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, tricyclodecane dimethanol, hydroxypivalic acid neopentyl glycol ester, hydrogenated bisphenol A, hydrogenated bisphenol F, glycerin, trimethylolethane, trimethylolpropane, diglycerin, triglycerin, 1,2,6-hexanetriol, pentaerythritol, dipentaerythritol, tris(2-hydroxyethyl)isocyanuric acid, sorbitol, mannite, hydroxyacetone, 4-(2-hydroxyethyl)morpholine, benzyl alcohol, 2-phenylethanol, 2-phenoxyethanol, naphthalen-1-ol, (1,3-benzoxol-5-yl)methanol, nonylphenol, dinonylphenol, nonylphenol ethoxylate, monostyrenated phenol, distyrenated phenol, tristyrenated phenol, etc. These can be used alone or in combination of two or more.
[0083] When the hydroxyl group-containing compound (a11) contains the hydroxyl group-containing monomer, the content of the hydroxyl group-containing monomer is preferably in the range of 5 to 100 mass %, more preferably in the range of 5 to 50 mass %, and even more preferably in the range of 5 to 30 mass %, based on the total solid content of the hydroxyl group-containing compound (a11), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film to be formed.
[0084] When the hydroxyl group-containing compound (a11) is contained as the isocyanate-reactive group-containing compound (a1), the content of the hydroxyl group-containing compound (a11) is preferably in the range of 50 to 100 mass%, more preferably in the range of 60 to 100 mass%, and even more preferably in the range of 70 to 100 mass%, based on the total solid content of the isocyanate-reactive group-containing compound (a1), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film to be formed.
[0085] [Amino Group-Containing Compound (a12)] The amino group-containing compound (a12) is a compound having at least one primary amino group and / or secondary amino group in the molecule.
[0086] Examples of the amino group-containing compound (a12) include aliphatic polyamines such as ethylenediamine, pentamethylenediamine, hexamethylenediamine, trimethylhexamethylenediamine, diethylenetriamine, dipropylenetriamine, triethylenetetramine, N,N'-bis-(3-aminopropyl)ethylenediamine, and tetraethylenepentamine; 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 4-methyl-1,3-cyclohexanediamine, 2-methyl- Alicyclic polyamines such as 1,3-cyclohexanediamine, isophoronediamine, 4,4'-methylenebis(cyclohexylamine), 3,3'-dimethyl-4,4'-methylenebis(cyclohexylamine), N,N'-(isophoronediamino)bispropionitrile, N,N'-di-sec-butyl-4,4'-methylenebis(cyclohexylamine), 1,2-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, and norbornanediamine; Heterocyclic polyamines such as piperazine and N-(2-aminoethyl)piperazine; 2,4-toluenediamine, 2,6-toluenediamine, 4,4'-diaminodiphenylmethane, diethyltoluenediamine, dimethylthiotoluenediamine, 4,4'-methylenebis[N-(1-methylpropyl)aniline], 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl ether, 1,3-bis(3-aminophenoxy)benzene, 4,4'-(1,3-phenylenediisopropyl ... aromatic polyamines such as 4,4'-(1,4-phenylenediisopropylidene)bisaniline, 4,4'-(1,4-phenylenediisopropylidene)bisaniline, aminobenzylamine, m-xylylenediamine, p-xylylenediamine, and N,N'-di-sec-butyl-p-phenylenediamine; polyether polyamine compounds such as polyoxypropylenediamine, polyoxyethylenediamine, poly(oxyethylene / oxypropylene)diamine, trimethylolpropanepoly(oxypropylene)triamine, and glycerylpoly(oxypropylene)triamine;Examples of suitable polyaspartic acid ester compounds include tetraethyl N,N'-(2-methylpentane-1,5-diyl)bisaspartate, tetraethyl N,N'-[methylenebis(cyclohexane-4,1-diyl)]bisaspartate, tetraethyl N,N'-[methylenebis(2-methylcyclohexane-4,1-diyl)]bisaspartate, and α-{2-[(1,4-diethoxy-1,4-dioxobutan-2-yl)amino]propyl}-ω-{2-[(1,4-diethoxy-1,4-dioxobutan-2-yl)amino]propoxy}poly[oxy(methylethylene)]; and aminosilane compounds such as N-β(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β(aminoethyl)-γ-aminopropylmethyldimethoxysilane, and γ-anilinopropyltrimethoxysilane. These compounds can be used alone or in combination of two or more.
[0087] As the amino group-containing compound (a12), commercially available products can be used. Examples of commercially available product names include "Baxodur EC110", "DETA", "N4 Amine", "Baxodur EC210", "Baxodur EC201", "Baxodur EC330", "Baxodur EC331", "Baxodur PC136", "Baxodur EC130", "Baxodur EC280", "Baxodur EC301", "Baxxodur EC302", "Baxxodur EC303", "Baxxodur EC310", and "Baxxodur EC311" (all of which are product names manufactured by BASF), "Clearlink 1000", "Unilink 4200", and "Unilink 4100'' (all product names, manufactured by DORF KETAL), ``JEFFAMINE M-600'', ``JEFFAMINE M-1000'', ``JEFFAMINE M-2005'', ``JEFFAMINE M-2070'', ``JEFFAMINE M-3085'', ``JEFFAMINE D-230'', ``JEFFAMINE D-400'', ``JEFFAMINE D-2000'', ``JEFFAMINE D-4000'', ``JEFFAMINE ED-600'', ``JEFFAMINE ED-900", "JEFFAMINE ED-2003", "JEFFAMINE EDR-148", "JEFFAMINE RT-1000, JEFFAMINE T-403, JEFFAMINE T-3000, JEFFAMINE T-5000 (all trade names, manufactured by HUNTSMAN Corporation), MXDA, 1,3-BAC (all trade names, manufactured by Mitsubishi Gas Chemical Company, Inc.), WANAMINE MDA-100H, Ethacure 100 Plus, Ethacure 300, Ethacure 420, Bisaniline-M, Bisaniline-P (all trade names, manufactured by Mitsui Fine Chemicals, Inc.), VESTAMIN IPD, VESTAMIN TMD, VESTAMIN PACM, ANCAMINE 2049, AMICURE IC-321, AMICURE IC-322 (all trade names, manufactured by EVONIK Industries), “D.E.H.20”, “D.E.H.24”,"D.E.H.26", "D.E.H.29", "D.E.H.39", "D.E.H.444", "D.E.H.445", "D.E.H.4042" , "D.E.H.4044", "D.E.H.487", "D.E.H.488", "D.E.H.530", "D.E.H." Dow Chemical Co., Ltd.), "Desmophen NH1220", "Desmophen NH1420", "Desmophen NH1422", "Desmophen NH1423", "Desmophen NH1520", "Desmophen NH1521", "Desmophen NH1523", "Desmophen NH1723LF", "Desmophen NH2885", "Desmophen NH2886" (all trade names, manufactured by Covestro), "FEISPARTIC F220", "FEISPARTIC F420", "FEISPARTIC F520", "FEISPARTIC F2850", "FEISPARTIC F2872", "FEISPARTIC F221", "FEISPARTIC F321", "FEISPARTIC F525", "FEISPARTIC F421", "FEISPARTIC F524", "FEISPARTIC F330", "FEISPARTIC D2925", "FEISPARTIC D2903" (all trade names, manufactured by Feiyang Protech Co., Ltd.), "TSE-EZASP 7980", "TSE-EZASP 7981", "TSE-EZASP 9033", "TSE-EZASP 8443" (all trade names, manufactured by TSE Examples of such products include Altor 200, Altor 201, Altor 202, and Altor 205LV (all trade names, manufactured by Cargill).
[0088] From the viewpoints of reducing the VOC content in the resulting coating composition and improving the hardness, adhesion, and color unevenness of the coating film to be formed, the amino group-containing compound (a12) preferably contains at least one compound selected from aliphatic polyamines, alicyclic polyamines, polyether polyamine compounds, and polyaspartic acid ester compounds, more preferably at least one compound selected from alicyclic polyamines and polyaspartic acid esters, and even more preferably contains a polyaspartic acid ester compound.
[0089] As the polyaspartic acid ester compound, commercially available products can be used. Examples of commercially available product names include Desmophen NH1220, Desmophen NH1420, Desmophen NH1422, Desmophen NH1423, Desmophen NH1520, Desmophen NH1521, Desmophen NH1523, Desmophen NH1723LF, Desmophen NH2885, and Desmophen NH2886 (all trade names, manufactured by Covestro), FEI SPARTIC F220, FEI SPARTIC F420, and FEI SPARTIC F520", "FEISPARTIC F2850", "FEISPARTIC F2872", "FEISPARTIC F221", "FEISPARTIC F321", "FEISPARTIC F525", "FEISPARTIC F421", "FEISPARTIC F524", "FEISPARTIC F330", "FEISPARTIC D2925", "FEISPARTIC D2903" (all product names, manufactured by Feiyang Protech), "TSE-EZASP 7980'', ``TSE-EZASP 7981'', ``TSE-EZASP 9033'', ``TSE-EZASP 8443'' (all product names, manufactured by TSE Industries), ``Altor 200," "Altor 201," "Altor 202," and "Altor 205LV" (all trade names, manufactured by Cargill).
[0090] When the isocyanate-reactive group-containing compound (a1) contains the amino group-containing compound (a12), the content of the amino group-containing compound (a12) is preferably in the range of 10 to 100 mass%, more preferably in the range of 40 to 95 mass%, and even more preferably in the range of 50 to 90 mass%, based on the total solid content of the isocyanate-reactive group-containing compound (a1), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film to be formed.
[0091] [Thiol Group-Containing Compound (a13)] The thiol group-containing compound (a13) is a compound having at least one thiol group in one molecule.
[0092] Examples of the thiol group-containing compound (a13) include pentaerythritol tetrakis(3-mercaptopropionate), trimethylolpropane tris(3-mercaptopropionate), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, tetraethylene glycol bis(3-mercaptopropionate), tetramethylene glycol bis(3-mercaptopropionate), dipentaerythritol hexakis(3-mercaptopropionate), trimethylolpropane dipropanethiol, pentaerythritol hexakis(3-mercaptopropionate), trimethylolpropane dipropanethiol, and pentaerythritol hexakis(3-mercaptopropionate). Examples include thritol tripropanethiol, pentaerythritol tetrapropanethiol, 1,4-bis(mercaptomethyl)benzene, pentaerythritol tetrakis(3-mercaptobutyrate), trimethylolpropane tris(3-mercaptobutyrate), tetramethylene glycol bis(3-mercaptobutyrate), tris-[(3-mercaptobutyroyloxy)-ethyl]-isocyanurate, trimethylolpropane tris(thioglycolate), pentaerythritol tetrakis(thioglycolate), etc. These can be used alone or in combination of two or more.
[0093] Commercially available products can be used as the thiol group-containing compound (a13). Examples of commercially available products with trade names include "TMMP-LV", "TEMPIC", "PEMP-LV", "DPMP", "EGMP-4", "BDMP", "Multiol Y-2", "Multiol Y-3", "Multiol Y-4", and "PXDT" (all trade names, manufactured by SC Organic Chemical Co., Ltd.), "BDTG", "HDTG", "TMTG", "PETG", "EGTP", "BDTP", "TMTP", and "PETP" (all trade names, manufactured by Yodo Chemical Co., Ltd.), "ADEKA Hardener EH-317" (all trade names, manufactured by ADEKA Corporation), "Karenz MT PEI", "Karenz MT BDI", "Karenz MT BD1", "Karenz MT TPMB", and "Karenz MT Examples of such curing agents include "NRI" (trade names, manufactured by Showa Denko KK), "jER Cure QX11" and "jER Cure QX40" (trade names, manufactured by Mitsubishi Chemical Corporation).
[0094] When the isocyanate-reactive group-containing compound (a1) contains the thiol group-containing compound (a13), the content of the thiol group-containing compound (a13) is preferably in the range of 10 to 100 mass%, more preferably in the range of 30 to 95 mass%, and even more preferably in the range of 50 to 90 mass%, based on the total solid content of the isocyanate-reactive group-containing compound (a1), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film to be formed.
[0095] The content of the isocyanate-reactive group-containing compound (a1) in the main component (A) is preferably within the range of 30 to 99.5 mass %, more preferably within the range of 50 to 99 mass %, and even more preferably within the range of 70 to 98 mass %, based on the total amount of the main component (A), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film to be formed.
[0096] [Other Components] The main component (A) may further contain an ultraviolet absorber and / or a light stabilizer, and may also contain, as necessary, other additives commonly used in the field of coatings, such as an internal mold release agent, a solvent (organic solvent, water), a pigment, a catalyst, a dehydrating agent, an antioxidant, a surface conditioner, an antifoaming agent, an emulsifier, a surfactant, an antifouling agent, a wetting agent, a thickener, a dye, a scratch resistance improver, and a gloss adjuster.
[0097] <Ultraviolet Absorber> As the ultraviolet absorber, conventionally known ones can be used, for example, benzotriazole-based absorbers, triazine-based absorbers, salicylic acid derivative-based absorbers, benzophenone-based absorbers, etc. Furthermore, the ultraviolet absorber may have a polymerizable unsaturated group.
[0098] Specific examples of the benzotriazole-based absorbents include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-5'-t-butylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-t-butylphenyl)benzotriazole, 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-t-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-t-amylphenyl)benzotriazole, 2-(2'-hydroxy-4'-octoxyphenyl)benzotriazole, 2-{2'-hydroxy-3'-(3'',4'',5'',6''-tetrahydrophthalimidomethyl)-5'-methylphenyl}benzotriazole, 2-[2-hydroxy-5-[2-(methacryloyloxy)ethyl]phenyl]-2H-benzotriazole, and the like.
[0099] Specific examples of the triazine-based absorbent include 2,4-bis(2,4-dimethylphenyl)-6-(2-hydroxy-4-isooctyloxyphenyl)-1,3,5-triazine, 2-[4((2-hydroxy-3-dodecyloxypropyl)-oxy)-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-((2-hydroxy-3-tridecyloxypropyl)-oxy)-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, and 2-(2,4-dihydroxyphenyl)-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine.
[0100] Specific examples of the salicylic acid derivative-based absorbents include phenyl salicylate, p-octylphenyl salicylate, and 4-tert-butylphenyl salicylate.
[0101] Specific examples of the benzophenone-based absorbents include 4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, 2-hydroxy-4-methoxy-5-sulfobenzophenone trihydrate, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, 2-hydroxy-4-octadecyloxybenzophenone, and naphthalene. Examples include thorium 2,2'-dihydroxy-4,4'-dimethoxy-5-sulfobenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 4-dodecyloxy-2-hydroxybenzophenone, 5-chloro-2-hydroxybenzophenone, resorcinol monobenzoate, 2,4-dibenzoylresorcinol, 4,6-dibenzoylresorcinol, hydroxydodecylbenzophenone, and 2,2'-dihydroxy-4(3-methacryloxy-2-hydroxypropoxy)benzophenone.
[0102] Commercially available examples of the ultraviolet absorber include "TINUVIN 1130," "TINUVIN 900," "TINUVIN 928," "TINUVIN 384-2," "TINUVIN 479," "TINUVIN 477," "TINUVIN 405," "TINUVIN 400" (trade names manufactured by BASF, TINUVIN is a registered trademark), and "RUVA 93" (trade name manufactured by Otsuka Chemical Co., Ltd.).
[0103] When the main component (A) contains the ultraviolet absorber, the content of the ultraviolet absorber is preferably in the range of 0.5 to 10 mass %, more preferably in the range of 0.8 to 5.0 mass %, and even more preferably in the range of 1.0 to 4.0 mass %, based on the total amount of the main component (A), from the viewpoints of the weather resistance and adhesion of the coating film to be formed.
[0104] <Light Stabilizer> The light stabilizer is used as a radical chain inhibitor that captures active radical species generated during the deterioration process of the coating film, and examples thereof include light stabilizers of hindered amine compounds.
[0105] Examples of the hindered amine compound include bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(2,2,6,6-tetramethyl-4-piperidinyl)sebacate, bis(N-methyl-2,2,6,6-tetramethyl-4-piperidinyl)sebacate, 4-benzoyloxy-2,2',6,6'-tetramethylpiperidine, bis(1,2,2,6,6-pentamethyl-4-piperidyl){[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl}butylmalonate, Examples of the light stabilizer include, but are not limited to, monomeric types such as methyl acrylate, methyl meth ...
[0106] Examples of commercially available products of the light stabilizer include "TINUVIN 123", "TINUVIN 152", "TINUVIN 249", and "TINUVIN 292" (trade names, manufactured by BASF, TINUVIN is a registered trademark), "HOSTAVIN 3058" (trade name, manufactured by Clariant, Hostavin is a registered trademark), and "ADK STAB LA-82" (trade name, manufactured by ADEKA Corporation, ADK STAB is a registered trademark).
[0107] When the main component (A) contains the above-mentioned light stabilizer, the content of the light stabilizer is preferably in the range of 0.5 to 10 mass %, more preferably in the range of 0.8 to 9.0 mass %, and even more preferably in the range of 1.0 to 8.0 mass %, based on the total amount of the main component (A), from the viewpoints of the weather resistance and adhesion of the coating film to be formed.
[0108] <Internal Mold Release Agent> When the coating composition of the present invention is used as an in-mold coating composition, it is preferable that the main component (A) contains an internal mold release agent from the viewpoint of the releasability between the formed coating film and the mold.
[0109] Examples of the internal mold release agent include saturated fatty acids such as stearic acid and palmitic acid; saturated fatty acid salts such as zinc stearate, aluminum stearate, magnesium stearate, calcium stearate, sodium stearate, potassium stearate, barium stearate, zinc palmitate, aluminum palmitate, magnesium palmitate, calcium palmitate, and sodium palmitate; saturated fatty acid amides such as lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, N,N-dimethyllauric acid amide, N,N-dimethylmyristic acid amide, N,N-dimethylpalmitic acid amide, N,N-dimethylstearic acid amide, N,N-diethyllauric acid amide, N,N-diethylmyristic acid amide, N,N-diethylpalmitic acid amide, and N,N-diethylstearic acid amide; unsaturated fatty acids such as palmitoleic acid and oleic acid; zinc palmitoleate, aluminum palmitoleate, palmitic acid amide, and the like. unsaturated fatty acid salts such as magnesium oleate, calcium palmitoleate, sodium palmitoleate, potassium palmitoleate, barium palmitoleate, zinc oleate, aluminum oleate, magnesium oleate, calcium oleate, sodium oleate, potassium oleate, and barium oleate; unsaturated fatty acid amides such as palmitoleic acid amide, oleic acid amide, erucic acid amide, behenic acid amide, N-oleyl palmitic acid amide, N-stearyl erucic acid amide, N,N-dimethyl oleic acid amide, and N,N-diethyl oleic acid amide; nonionic surfactants such as polyoxyethylene alkyl ethers and sorbitan alkyl esters; fluorine-based compounds such as polytetrafluoroethylene, fluoropolyethers, perfluoroalkyl esters, and perfluoroalkyl ester salts; phosphate ester compounds such as phosphate monoesters and / or phosphate diesters having alkyl chains or oxyethylene chains, etc.;Stearic acid monoglyceride, stearic acid diglyceride, stearic acid triglyceride, stearate monosorbitate, stearate stearyl, palmitic acid monoglyceride, palmitic acid diglyceride, palmitic acid triglyceride, behenic acid monoglyceride, behenic acid diglyceride, behenic acid triglyceride, behenyl behenate, pentaerythritol monostearate, pentaerythritol tetrastearate, pentaerythritol tetrapelargonate, propyl Examples of fatty acid esters include ethylene glycol monostearate, stearyl stearate, palmityl palmitate, methyl stearate, butyl stearate, methyl laurate, methyl palmitate, isopropyl palmitate, biphenyl biphenate, sorbitan monostearate, and 2-ethylhexyl stearate; soybean oil lecithin, silicone oil, and fatty acid alcohol dibasic acid esters, which can be used alone or in combination of two or more types;
[0110] When the main component (A) contains the internal release agent, the content of the internal release agent is preferably in the range of 0.4 to 5.0 mass%, more preferably in the range of 0.5 to 4.0 mass%, and even more preferably in the range of 0.5 to 3.0 mass%, based on the total amount of the main component (A), from the viewpoints of the adhesion of the coating film to be formed and the releasability between the coating film to be formed and the mold.
[0111] <Solvent> Examples of the solvent that can be used include organic solvents, water, etc. Examples of the organic solvent include ketone-based solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; ester-based solvents such as ethyl acetate, butyl acetate, methyl benzoate, ethyl ethoxypropionate, ethyl propionate, and methyl propionate; ether-based solvents such as tetrahydrofuran, dioxane, and dimethoxyethane; glycol ether-based solvents such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, and 3-methoxybutyl acetate; aromatic solvents such as toluene, xylene, and "Swasol 1000" (trade name, high-boiling point petroleum solvent, manufactured by Cosmo Oil Co., Ltd.); and aliphatic hydrocarbon-based solvents such as hexane and heptane.
[0112] When the main component (A) contains the above-mentioned solvent, from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, color unevenness, etc. of the coating film to be formed, the content of the solvent is preferably in the range of 0.1 to 5 mass %, more preferably in the range of 0.3 to 4 mass %, and even more preferably in the range of 0.5 to 3 mass %, based on the total amount of the main component (A).
[0113] <Catalyst> Conventionally known catalysts can be used as the catalyst. Examples of the catalyst include tin octoate, dibutyltin diacetate, dibutyltin di(2-ethylhexanoate), dibutyltin dilaurate, dioctyltin diacetate, dioctyltin di(2-ethylhexanoate), dioctyltin dineodecanoate, dioctyltin diversatate, dibutyltin oxide, dibutyltin sulfide, dioctyltin oxide, dibutyltin fatty acid salts, lead 2-ethylhexanoate, zinc octoate, zinc naphthenate, zinc fatty acids, bismuth octanoate, bismuth 2-ethylhexanoate, bismuth oleate, bismuth neodecanoate, and versatane. organometallic compounds such as bismuth titanate, bismuth naphthenate, cobalt naphthenate, calcium octylate, copper naphthenate, tetra(2-ethylhexyl)titanate, tetra(n-butyl)titanate, titanium diisopropoxybis(acetylacetonate), titanium tetraacetylacetonate, titanium diisopropoxybis(ethylacetoacetate), titanium butoxide dimer, zirconium tetra-n-propoxide, zirconium tetra-n-butoxide, zirconium tetraacetylacetonate, and zirconium tributoxymonoacetylacetonate;Triethylamine, N,N'-dimethylcyclohexylamine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethylhexamethylenediamine, N,N,N',N'',N'',N''-pentamethyldiethylenetriamine, N,N,N',N'',N'',N''-pentamethyldipropylenetriamine, 1,4-diazabicyclo[2.2.2]octane (DABCO), 1,8-diazabicyclo[5.4.0]-7-undecene (DBU), 1,5-diazabicyclo[4.3.0]-2-methylpropanediol (DABCO), 1,8-diazabicyclo[5.4.0]-2-methylpropanediol ... tertiary amine compounds such as 1-(2-dimethylaminoethyl)-5-nonene (DBN), N-methyl-N'-(2-dimethylaminoethyl)piperazine, N-ethylmorpholine, 1,2-dimethylimidazole, dimethylethanolamine, dimethylaminoethoxyethanol, N-methyl-N'-(2-hydroxyethyl)piperazine, 2-hydroxyethyl-1,4-diazabicyclo[2.2.2]octane, 1,1'-{[3-(dimethylamino)propyl]imino}bis(2-propanol), bis(2-dimethylaminoethyl)ether, and bis(2-morpholinoethyl)ether, as well as neutralized salts of the tertiary amine compounds; and quaternary ammonium salts such as carboxylates of tetraalkylammonium, tetraarylammonium, and alkylarylammonium, and halides of tetraalkylammonium, tetraarylammonium, and alkylarylammonium, which can be used alone or in combination of two or more kinds.
[0114] When the main component (A) contains the above-mentioned catalyst, the amount of the catalyst blended is preferably in the range of 0.005 to 5.0 mass %, and more preferably in the range of 0.01 to 3.0 mass %, based on the total amount of the main component (A), from the viewpoints of the hardness and adhesion of the coating film to be formed.
[0115] Furthermore, when the coating composition of the present invention contains the above-mentioned catalyst, it may also contain organic acids such as acetic acid, propionic acid, butyric acid, isopentanoic acid, hexanoic acid, 2-ethylbutyric acid, naphthenic acid, octylic acid, nonanoic acid, decanoic acid, 2-ethylhexanoic acid, isooctanoic acid, isononanoic acid, lauric acid, palmitic acid, stearic acid, oleic acid, linoleic acid, neodecanoic acid, versatic acid, isobutyric anhydride, itaconic anhydride, acetic anhydride, citraconic anhydride, propionic anhydride, maleic anhydride, butyric anhydride, citric anhydride, trimellitic anhydride, pyromellitic anhydride, and phthalic anhydride; inorganic acids such as hydrochloric acid and phosphoric acid; and metal coordination compounds such as acetylacetone and imidazole compounds.
[0116] <Dehydrating Agent> As the dehydrating agent, conventionally known inorganic and organic dehydrating agents can be used. Examples of the inorganic dehydrating agent include calcium compounds such as calcium hydride, calcium oxide (quicklime), calcium chloride, and calcium sulfate (gypsum); barium compounds such as barium oxide; magnesium compounds such as magnesium sulfate; sodium compounds such as sodium sulfate and sodium carbonate; copper compounds such as copper sulfate; inorganic silicon compounds such as silica gel; and aluminum compounds such as aluminum oxide (hydraulic alumina, lithium aluminum hydride, amorphous silica alumina, and crystalline aluminosilicates (molecular sieves). These can be used alone or in combination of two or more.
[0117] Examples of the organic dehydrating agent include alkyl orthoformate, alkyl orthoacetate, alkyl orthoborate, vinylsilane, alkoxysilane compounds, monoisocyanate compounds, aliphatic acid anhydrides such as acetic anhydride, and aromatic acid anhydrides such as benzoic anhydride, and these can be used alone or in combination of two or more. When the main component (A) contains the dehydrating agent, from the viewpoints of reducing the VOC content in the resulting coating composition and improving the adhesion of the coating film formed, the amount of the dehydrating agent is preferably within the range of 0.1 to 5.0 mass%, and more preferably within the range of 0.3 to 3.0 mass%, based on the total amount of the main component (A).
[0118] The shear rate of the main agent (A) is 100 sec. -1 , viscosity at 65°C (V A ) is in the range of 20 to 1800 mPa·s.
[0119] The shear rate of the main agent (A) is 100 sec. -1 , viscosity at 65°C (V A ) is preferably in the range of 50 to 1500 mPa·s, more preferably in the range of 100 to 1000 mPa·s, and even more preferably in the range of 150 to 800 mPa·s, from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film formed.
[0120] The solids concentration of the main component (A) is preferably in the range of 95 to 100% by mass, more preferably in the range of 96 to 99.5% by mass, and even more preferably in the range of 97 to 99% by mass, from the viewpoints of reducing the VOC content in the resulting paint composition and of improving the hardness, adhesion, and color unevenness of the paint film formed. In the kit according to the present invention and the three-component paint composition according to the present disclosure, the content of the main component (A) is preferably in the range of 10 to 70% by mass, more preferably in the range of 15 to 60% by mass, and even more preferably in the range of 25 to 50% by mass, based on the total amount of the three-component paint composition, from the viewpoints of reducing the VOC content in the resulting paint composition and of improving the hardness, adhesion, and color unevenness of the paint film formed.
[0121] [Curing Agent (B)] The curing agent (B) contains a polyisocyanate compound (b1).
[0122] [Polyisocyanate Compound (b1)] The polyisocyanate compound (b1) is a compound having at least two isocyanate groups in one molecule, and includes, for example, aliphatic polyisocyanates, alicyclic polyisocyanates, araliphatic polyisocyanates, aromatic polyisocyanates, and derivatives of the polyisocyanates.
[0123] The polyisocyanate compound (b1) preferably contains the aliphatic polyisocyanate from the viewpoints of reducing the VOC content in the resulting coating composition and improving the hardness, adhesion, and color unevenness of the coating film to be formed.
[0124] Examples of the aliphatic polyisocyanate include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, dimer acid diisocyanate, methyl 2,6-diisocyanatohexanoate (common name: lysine diisocyanate), aliphatic diisocyanates such as 2-isocyanatoethyl 2,6-diisocyanatohexanoate, 1,6-diisocyanato-3-isocyanatomethylhexane, 1,4,8-triisocyanatooctane, 1,6,11-triisocyanatoundecane, 1,8-diisocyanato-4-isocyanatomethyloctane, 1,3,6-triisocyanatohexane, and 2,5,7-trimethyl-1,8-diisocyanato-5-isocyanatomethyloctane.
[0125] Examples of the alicyclic polyisocyanate include alicyclic diisocyanates such as 1,3-cyclopentene diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (common name: isophorone diisocyanate), methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 1,3- or 1,4-bis(isocyanatomethyl)cyclohexane (common name: hydrogenated xylylene diisocyanate) or a mixture thereof, and norbornane diisocyanate; 1,3,5-triisocyanatocyclohexane, 1,3,5-trimethylisocyanatocyclohexane, 2-(3-isocyanatopropyl)-2,5-di(isocyanatomethyl)-bicyclo(2.2.1)hepta 2-(3-isocyanatopropyl)-2,6-di(isocyanatomethyl)-bicyclo(2.2.1)heptane, 3-(3-isocyanatopropyl)-2,5-di(isocyanatomethyl)-bicyclo(2.2.1)heptane, 5-(2-isocyanatoethyl)-2-isocyanatomethyl-3-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, 6-(2-isocyanatoethyl)-2-isocyanato alicyclic triisocyanates such as 2-isocyanatoethyl-3-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, 5-(2-isocyanatoethyl)-2-isocyanatomethyl-2-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, and 6-(2-isocyanatoethyl)-2-isocyanatomethyl-2-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane.
[0126] Examples of the araliphatic polyisocyanate include araliphatic diisocyanates such as 1,3- or 1,4-xylylene diisocyanate or a mixture thereof, ω,ω'-diisocyanato-1,4-diethylbenzene, 1,3- or 1,4-bis(1-isocyanato-1-methylethyl)benzene (common name: tetramethylxylylene diisocyanate) or a mixture thereof; and araliphatic triisocyanates such as 1,3,5-triisocyanatomethylbenzene.
[0127] Examples of the aromatic polyisocyanate include aromatic diisocyanates such as m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 2,4'- or 4,4'-diphenylmethane diisocyanate or mixtures thereof, 2,4- or 2,6-tolylene diisocyanate or mixtures thereof, 4,4'-toluidine diisocyanate, and 4,4'-diphenyl ether diisocyanate; aromatic triisocyanates such as triphenylmethane-4,4',4''-triisocyanate, 1,3,5-triisocyanatobenzene, and 2,4,6-triisocyanatotoluene; and aromatic tetraisocyanates such as 4,4'-diphenylmethane-2,2',5,5'-tetraisocyanate.
[0128] Examples of the polyisocyanate derivatives include dimers, trimers, biurets, allophanates, uretdione, uretonimine, isocyanurates, iminooxadiazinedione, polymethylene polyphenyl polyisocyanates (crude MDI, polymeric MDI), crude TDI, and the like of the polyisocyanate compounds described above. Among these, from the viewpoint of the hardness and adhesion of the coating film to be formed, it is preferable to contain at least one selected from allophanates, uretdione, and isocyanurates, it is more preferable to contain at least one selected from uretdione and isocyanurates, and it is even more preferable to contain isocyanurates.
[0129] The polyisocyanates and derivatives thereof may be used alone or in combination of two or more thereof. Among these polyisocyanates, it is preferable to use aliphatic diisocyanates, aliphatic triisocyanates, alicyclic diisocyanates, araliphatic diisocyanates, and derivatives thereof alone or in combination of two or more thereof.
[0130] The polyisocyanate compound (b1) may be a prepolymer obtained by reacting the polyisocyanate or a derivative thereof with a compound reactive with the polyisocyanate under conditions of excess isocyanate groups. Examples of the compound reactive with the polyisocyanate include compounds having an active hydrogen group such as a hydroxyl group or an amino group. Specific examples of the compound that can be used include polyhydric alcohols, low-molecular-weight polyester resins, amines, and water.
[0131] As the polyhydric alcohol, the polyhydric alcohols exemplified for the hydroxyl group-containing polyester resin can be used.
[0132] From the viewpoint of the hardness and adhesion of the coating film to be formed, the polyisocyanate compound (b1) is preferably used in such a proportion that the ratio of isocyanate groups in the polyisocyanate compound (b1) to isocyanate reactive groups in the isocyanate-reactive group-containing compound (a1) and the isocyanate-reactive group-containing compound (c1) described below falls within a range of 0.7 to 2.0, more preferably a range of 0.9 to 1.5.
[0133] Furthermore, from the viewpoints of reducing the VOC content in the resulting coating composition and preventing hardness, adhesion, and color unevenness of the coating film to be formed, the content of the polyisocyanate compound (b1) in the curing agent (B) is preferably within the range of 30 to 100 mass %, more preferably within the range of 40 to 99.5 mass %, and even more preferably within the range of 50 to 99 mass %, based on the total amount of the curing agent (B).
[0134] [Other Components] In addition to the above, the curing agent (B) can further contain a curing agent other than the polyisocyanate compound (b1). Furthermore, the curing agent (B) can appropriately contain other additive components commonly used in the field of coatings, such as ultraviolet absorbers, light stabilizers, internal mold release agents, solvents (organic solvents, water), pigments, catalysts, dehydrating agents, antioxidants, surface conditioners, antifoaming agents, emulsifiers, surfactants, antifouling agents, wetting agents, thickeners, dyes, scratch resistance improvers, gloss adjusters, etc., as needed.
[0135] <Curing Agents Other Than Polyisocyanate Compound (b1)> Examples of the curing agent other than the polyisocyanate compound (b1) include carbodiimide group-containing compounds.
[0136] <Carbodiimide Group-Containing Compound> The carbodiimide group-containing compound is a compound having at least one carbodiimide group in one molecule, and can be, for example, a compound obtained by subjecting isocyanate groups of an isocyanate group-containing compound to a carbon dioxide removal reaction. However, in the present invention, compounds having a carbodiimide group and two or more isocyanate groups are not included in the carbodiimide group-containing compound, but are included in the polyisocyanate compound (b1).
[0137] Commercially available products can be used as the carbodiimide group-containing compound. Examples of commercially available products with trade names include "Carbodilite V-02B," "Elastostab H01," "Carbodilite V-03," "Carbodilite V-09," "Carbodilite V-09GB," "Carbodilite V-09M," and "Carbodilite V-04PF" (all trade names, manufactured by Nisshinbo Chemical Inc.), "Stabaxol I," "Stabaxol I LF," "Stabaxol P," "Stabaxol P100," and "Stabaxol P200" (all trade names, manufactured by LANXESS).
[0138] The carbodiimide group-containing compound preferably comprises a solventless carbodiimide group-containing compound from the viewpoints of reducing the VOC content in the resulting coating composition and preventing adhesion and color unevenness of the coating film formed.
[0139] The solvent-free carbodiimide group-containing compound may be commercially available, such as "Carbodilite V-02B," "Elastostab H01," and "Carbodilite V-04PF" (all manufactured by Nisshinbo Chemical Inc.).
[0140] The number average molecular weight of the carbodiimide group-containing compound is preferably within the range of 500 to 5,000, more preferably within the range of 600 to 3,000, and even more preferably within the range of 700 to 1,500, from the viewpoints of reducing the VOC content in the resulting coating composition and of improving the hardness, adhesion, and color unevenness of the coating film to be formed.
[0141] Furthermore, when the curing agent (B) contains the above-mentioned carbodiimide group-containing compound, the content of the carbodiimide group-containing compound is preferably in the range of 0.5 to 5.0 mass %, more preferably in the range of 0.8 to 4.0 mass %, and even more preferably in the range of 1.0 to 3.0 mass %, based on the total amount of the curing agent (B), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, color unevenness, etc. of the coating film to be formed.
[0142] <Solvent> As the solvent, for example, the solvents exemplified for the main component (A) can be used.
[0143] When the curing agent (B) contains the above-mentioned solvent, from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, color unevenness, etc. of the coating film to be formed, the content of the solvent is preferably in the range of 0.1 to 5 mass %, more preferably in the range of 0.2 to 4 mass %, and even more preferably in the range of 0.3 to 3 mass %, based on the total amount of the curing agent (B).
[0144] <Dehydrating Agent> As the dehydrating agent, for example, the dehydrating agents exemplified in the main component (A) can be used.
[0145] When the curing agent (B) contains the dehydrating agent, the amount of the dehydrating agent added is preferably in the range of 0.1 to 5 mass %, and more preferably in the range of 0.3 to 3 mass %, based on the total amount of the curing agent (B), from the viewpoints of the hardness and adhesion of the coating film to be formed.
[0146] The shear rate of the curing agent (B) is 100 sec. -1 , viscosity at 65°C (V B ) is in the range of 20 to 1800 mPa·s.
[0147] The shear rate of the curing agent (B) is 100 sec. -1 , viscosity at 65°C (V B ) is preferably in the range of 50 to 1500 mPa·s, more preferably in the range of 100 to 1000 mPa·s, and even more preferably in the range of 150 to 600 mPa·s, from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film formed.
[0148] The solids concentration of the curing agent (B) is preferably in the range of 95 to 100 mass %, more preferably in the range of 96 to 100 mass %, and even more preferably in the range of 97 to 100 mass %, from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film to be formed.
[0149] The content of the curing agent (B) in the kit according to the present invention and in the three-component paint composition according to the present disclosure is preferably in the range of 20 to 80 mass %, more preferably in the range of 30 to 75 mass %, and even more preferably in the range of 40 to 70 mass %, based on the total amount of the three-component paint composition, from the viewpoints of reducing the VOC content in the resulting paint composition and of the hardness, adhesion, color unevenness, etc. of the paint film to be formed.
[0150] [Pigment Paste (C)] The pigment paste (C) contains an isocyanate-reactive group-containing compound (c1) and a pigment (C2).
[0151] [Isocyanate-reactive group-containing compound (c1)] The isocyanate-reactive group-containing compound (c1) is a compound having at least one isocyanate-reactive group in one molecule.
[0152] From the viewpoints of reducing the VOC content in the resulting coating composition and improving the hardness, adhesion, and color unevenness of the coating film formed, the isocyanate-reactive group-containing compound (c1) preferably contains an isocyanate-reactive group-containing compound having a number average molecular weight in the range of 250 to 2500, more preferably in the range of 300 to 1800, and even more preferably in the range of 300 to 1500.
[0153] The isocyanate-reactive group is not particularly limited as long as it is a group reactive with an isocyanate group. Examples of the isocyanate-reactive group include a hydroxyl group, an amino group, and a thiol group. From the viewpoints of the hardness, adhesion, and color unevenness of the coating film to be formed, it is preferable that the isocyanate-reactive group contains at least one selected from a hydroxyl group and an amino group, and more preferably contains a hydroxyl group.
[0154] Therefore, examples of the isocyanate-reactive group-containing compound (c1) include a hydroxyl group-containing compound (c11), an amino group-containing compound (c12), a thiol group-containing compound (c13), etc., and from the viewpoints of the hardness, adhesion, color unevenness, etc. of the coating film to be formed, it is preferable to contain at least one compound selected from the hydroxyl group-containing compound (c11) and the amino group-containing compound (c12), and it is more preferable to contain the hydroxyl group-containing compound (c11).
[0155] [Hydroxyl group-containing compound (c11)] The above-mentioned hydroxyl group-containing compound (c11) is a compound having at least one hydroxyl group in one molecule.As the hydroxyl group-containing compound (c11), as hydroxyl group-containing oligomer and hydroxyl group-containing polymer, for example, hydroxyl group-containing polyester resin, hydroxyl group-containing polycaprolactone resin, hydroxyl group-containing polyether resin, hydroxyl group-containing polycarbonate resin, hydroxyl group-containing acrylic resin, hydroxyl group-containing polyurethane resin, hydroxyl group-containing epoxy resin, hydroxyl group-containing alkyd resin etc. can be enumerated.Among them, from the viewpoint of reducing the VOC content in the obtained coating composition, and the hardness, adhesion and color unevenness of the coating film formed, it is preferable to comprise at least one resin selected from hydroxyl group-containing polyester resin, hydroxyl group-containing polycaprolactone resin and hydroxyl group-containing polyether resin, more preferably comprise at least one resin selected from hydroxyl group-containing polyester resin and hydroxyl group-containing polycaprolactone resin. These can be used alone or in combination of two or more.
[0156] As the hydroxyl group-containing polyester resin, for example, the hydroxyl group-containing polyester resins exemplified above for the main component (A) can be used.
[0157] From the viewpoint of the hardness and adhesion of the coating film to be formed, the hydroxyl value of the hydroxyl-containing polyester resin is preferably within the range of 50 to 800 mgKOH / g, more preferably within the range of 100 to 700 mgKOH / g, and even more preferably within the range of 300 to 600 mgKOH / g.
[0158] The number average molecular weight of the hydroxyl group-containing polyester resin is preferably in the range of 250 to 2500, more preferably in the range of 300 to 1800, and even more preferably in the range of 350 to 1500, from the viewpoints of reducing the VOC content in the resulting coating composition and of improving the hardness, adhesion, and color unevenness of the coating film formed.
[0159] The glass transition temperature (Tg) of the hydroxyl group-containing polyester resin is preferably within the range of -80 to 10°C, more preferably within the range of -70 to 5°C, and even more preferably within the range of -60 to 0°C, from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film formed.
[0160] When the hydroxyl group-containing compound (c11) contains the above-mentioned hydroxyl group-containing polyester resin, the content of the hydroxyl group-containing polyester resin is preferably in the range of 50 to 100 mass%, more preferably in the range of 60 to 95 mass%, and even more preferably in the range of 75 to 90 mass%, based on the total solid content of the hydroxyl group-containing compound (c11), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film to be formed.
[0161] The hydroxyl group-containing polycaprolactone resin may be, for example, any of the hydroxyl group-containing polycaprolactone resins exemplified above for the main component (A). From the viewpoints of the hardness and adhesion of the coating film to be formed, the hydroxyl group value of the hydroxyl group-containing polycaprolactone resin is preferably within a range from 50 to 900 mgKOH / g, more preferably within a range from 100 to 750 mgKOH / g, and even more preferably within a range from 130 to 600 mgKOH / g.
[0162] The number average molecular weight of the hydroxyl group-containing polycaprolactone resin is preferably in the range of 250 to 2500, more preferably in the range of 280 to 1500, and even more preferably in the range of 300 to 1000, from the viewpoints of reducing the VOC content in the resulting coating composition and of improving the hardness, adhesion, and color unevenness of the coating film to be formed.
[0163] When the hydroxyl group-containing compound (c11) contains the above-mentioned hydroxyl group-containing polycaprolactone resin, the content of the hydroxyl group-containing polycaprolactone resin is preferably in the range of 5 to 100 mass%, more preferably in the range of 10 to 75 mass%, and even more preferably in the range of 10 to 50 mass%, based on the total solid content of the hydroxyl group-containing compound (c11), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, color unevenness, etc. of the coating film to be formed.
[0164] As the hydroxyl group-containing polyether resin, for example, the polyether resins exemplified in the main component (A) can be used.
[0165] From the viewpoint of the hardness and adhesion of the coating film to be formed, the hydroxyl value of the hydroxyl-containing polyether resin is preferably within a range of 50 to 600 mgKOH / g, more preferably within a range of 70 to 500 mgKOH / g, and even more preferably within a range of 90 to 400 mgKOH / g.
[0166] The number average molecular weight of the hydroxyl group-containing polyether resin is preferably in the range of 250 to 2500, more preferably in the range of 300 to 1500, and even more preferably in the range of 350 to 1000, from the viewpoints of reducing the VOC content in the resulting coating composition and of improving the hardness, adhesion, and color unevenness of the coating film formed.
[0167] When the hydroxyl group-containing compound (c11) contains the above-mentioned hydroxyl group-containing polyether resin, the content of the hydroxyl group-containing polyether resin is preferably in the range of 20 to 100 mass%, more preferably in the range of 40 to 100 mass%, and even more preferably in the range of 50 to 100 mass%, based on the total solid content of the hydroxyl group-containing compound (c11), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film to be formed.
[0168] The hydroxyl group-containing polycarbonate resin may be, for example, the polycarbonate resin exemplified in the main component (A). From the viewpoint of the hardness and adhesion of the coating film to be formed, the hydroxyl group value of the hydroxyl group-containing polycarbonate resin is preferably within a range of 50 to 800 mgKOH / g, more preferably within a range of 70 to 700 mgKOH / g, and even more preferably within a range of 90 to 600 mgKOH / g.
[0169] The number average molecular weight of the hydroxyl group-containing polycarbonate resin is preferably within the range of 250 to 2500, more preferably within the range of 300 to 1800, and even more preferably within the range of 400 to 1500, from the viewpoints of reducing the VOC content in the resulting coating composition and preventing adhesion and color unevenness of the coating film formed.
[0170] When the hydroxyl group-containing compound (c11) contains the above-mentioned hydroxyl group-containing polycarbonate resin, the content of the hydroxyl group-containing polycarbonate resin is preferably in the range of 5 to 80 mass %, more preferably in the range of 10 to 50 mass %, and even more preferably in the range of 10 to 40 mass %, based on the total solid content of the hydroxyl group-containing compound (c11), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film to be formed.
[0171] As the hydroxyl group-containing acrylic resin, for example, the acrylic resins exemplified in the main component (A) can be used.
[0172] From the viewpoint of the hardness and adhesion of the coating film to be formed, the hydroxyl value of the hydroxyl-containing acrylic resin is preferably within the range of 5 to 240 mgKOH / g, more preferably within the range of 20 to 220 mgKOH / g, and even more preferably within the range of 25 to 200 mgKOH / g.
[0173] The number average molecular weight of the hydroxyl group-containing acrylic resin is preferably in the range of 250 to 2500, more preferably in the range of 300 to 1800, and even more preferably in the range of 500 to 1500, from the viewpoints of reducing the VOC content in the resulting coating composition and of improving the hardness, adhesion, and color unevenness of the coating film formed.
[0174] The glass transition temperature (Tg) of the hydroxyl group-containing acrylic resin is preferably within the range of -60 to 80°C, more preferably within the range of -50 to 70°C, and even more preferably within the range of -40 to 60°C, from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film formed.
[0175] When the hydroxyl group-containing compound (c11) contains the above-mentioned hydroxyl group-containing acrylic resin, the content of the hydroxyl group-containing acrylic resin is preferably in the range of 5 to 100 mass%, more preferably in the range of 10 to 75 mass%, and even more preferably in the range of 15 to 50 mass%, based on the total solid content of the hydroxyl group-containing compound (c11), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film to be formed.
[0176] Furthermore, as the hydroxyl group-containing compound (c11), for example, the hydroxyl group-containing monomers exemplified in the main component (A) can be used. When the hydroxyl group-containing compound (c11) contains the hydroxyl group-containing monomer, the content of the hydroxyl group-containing monomer is preferably within the range of 5 to 100 mass%, more preferably within the range of 5 to 50 mass%, and even more preferably within the range of 5 to 30 mass%, based on the total solid content of the hydroxyl group-containing compound (c11), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film formed.
[0177] When the hydroxyl group-containing compound (c11) is contained as the isocyanate-reactive group-containing compound (c1), the content of the hydroxyl group-containing compound (c11) is preferably in the range of 50 to 100 mass%, more preferably in the range of 60 to 100 mass%, and even more preferably in the range of 70 to 100 mass%, based on the total solid content of the isocyanate-reactive group-containing compound (c1), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film to be formed.
[0178] [Amino group-containing compound (c12)] As the amino group-containing compound (c12), for example, the amino group-containing compound (c12) exemplified in the main component (A) can be used. When the isocyanate-reactive group-containing compound (c12) is contained as the isocyanate-reactive group-containing compound (c1), the content of the amino group-containing compound (c12) is preferably within the range of 10 to 100 mass%, more preferably within the range of 40 to 95 mass%, and even more preferably within the range of 50 to 90 mass%, based on the total solid content of the isocyanate-reactive group-containing compound (c1), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film formed.
[0179] [Thiol Group-Containing Compound (c13)] As the thiol group-containing compound (c13), for example, the thiol group-containing compound (c13) exemplified in the main component (A) can be used. When the thiol group-containing compound (c13) is contained as the isocyanate-reactive group-containing compound (c1), the content of the thiol group-containing compound (c13) is preferably within the range of 10 to 100 mass%, more preferably within the range of 30 to 95 mass%, and even more preferably within the range of 50 to 90 mass%, based on the total solid content of the isocyanate-reactive group-containing compound (c1), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film formed.
[0180] The content of the isocyanate-reactive group-containing compound (c1) in the pigment paste (C) is preferably within the range of 10 to 99 mass %, more preferably within the range of 15 to 90 mass %, and even more preferably within the range of 20 to 80 mass %, based on the total amount of the pigment paste (C), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film to be formed.
[0181] [Pigment (c2)] Examples of the pigment (c2) include luster pigments, color pigments, and extender pigments. These pigments can be used alone or in combination of two or more. Examples of the luster pigment include aluminum (including vapor-deposited aluminum), copper, zinc, brass, nickel, glass flakes, aluminum oxide, mica, aluminum oxide coated with titanium oxide and / or iron oxide, and mica coated with titanium oxide and / or iron oxide.
[0182] Examples of the color pigments include titanium oxide, zinc oxide, carbon black, molybdenum red, Prussian blue, cobalt blue, azo pigments, phthalocyanine pigments, quinacridone pigments, isoindoline pigments, threne pigments, perylene pigments, dioxazine pigments, diketopyrrolopyrrole pigments, heat-shielding pigments, etc. Examples of the extender pigments include clay, kaolin, barium sulfate, barium carbonate, calcium carbonate, talc, silica, alumina white, etc.
[0183] The content of the pigment (c2) in the pigment paste (C) is preferably in the range of 1.0 to 70 mass %, more preferably in the range of 1.0 to 65 mass %, even more preferably in the range of 2.0 to 64 mass %, and even more preferably in the range of 3.0 to 62 mass %, based on the total amount of the pigment paste (C), from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness and color unevenness of the coating film to be formed.
[0184] [Other Components] In addition to the above, the pigment paste (C) may further contain an ultraviolet absorber and / or a light stabilizer. Furthermore, if necessary, it may appropriately contain other additives commonly used in the field of coatings, such as an internal mold release agent, a solvent (organic solvent, water), a pigment, a catalyst, a dehydrating agent, an antioxidant, a surface conditioner, an antifoaming agent, an emulsifier, a surfactant, an antifouling agent, a wetting agent, a thickener, a dye, an abrasion resistance improver, and a gloss adjuster.
[0185] <Ultraviolet Absorber> As the ultraviolet absorber, for example, the ultraviolet absorbers exemplified in the main component (A) can be used. When the pigment paste (C) contains the ultraviolet absorber, the content of the ultraviolet absorber is preferably within a range of 0.5 to 10 mass %, more preferably within a range of 0.8 to 5.0 mass %, and even more preferably within a range of 1.0 to 4.0 mass %, based on the total amount of the pigment paste (C) coating composition, from the viewpoints of the weather resistance and adhesion of the coating film to be formed.
[0186] <Light Stabilizer> As the light stabilizer, for example, the light stabilizers exemplified in the main component (A) can be used. When the pigment paste (C) contains the light stabilizer, the content of the light stabilizer is preferably within a range of 0.5 to 10 mass %, more preferably within a range of 0.8 to 9.0 mass %, and even more preferably within a range of 1.0 to 8.0 mass %, based on the total amount of the pigment paste (C), from the viewpoints of the weather resistance and adhesion of the coating film to be formed.
[0187] <Internal Release Agent> When the coating composition of the present invention is used as an in-mold coating coating composition, the pigment paste (C) may contain an internal release agent from the viewpoint of the releasability between the formed coating film and the mold. Examples of the internal release agent that can be used include the internal release agents exemplified for the main component (A). When the pigment paste (C) contains the internal release agent, the content of the internal release agent is preferably within a range of 0.4 to 8.0 mass%, more preferably within a range of 0.5 to 7.0 mass%, and even more preferably within a range of 0.5 to 6.0 mass%, based on the total amount of the pigment paste (C), from the viewpoints of the adhesion of the formed coating film and the releasability between the formed coating film and the mold.
[0188] <Solvent> As the solvent, for example, the solvents exemplified for the main component (A) can be used. When the pigment paste (C) contains the solvent, from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, color unevenness, etc. of the coating film to be formed, the content of the solvent is preferably within the range of 2 to 15 mass%, more preferably within the range of 2 to 13 mass%, and even more preferably within the range of 2 to 10 mass%, based on the total amount of the pigment paste (C).
[0189] <Catalyst> As the catalyst, for example, the catalysts exemplified in the main component (A) can be used. When the pigment paste (C) contains the catalyst, from the viewpoints of the hardness and adhesion of the coating film to be formed, the blending amount of the catalyst is preferably in the range of 0.01 to 5.0 mass %, and more preferably in the range of 0.1 to 3.0 mass %, based on the total amount of the pigment paste (C).
[0190] <Dehydrating Agent> As the dehydrating agent, for example, the dehydrating agents exemplified in the main component (A) can be used. When the pigment paste (C) contains the dehydrating agent, from the viewpoints of the hardness and adhesion of the coating film to be formed, the blending amount of the dehydrating agent is preferably in the range of 0.1 to 5.0 mass %, and more preferably in the range of 0.3 to 3.0 mass %, based on the total amount of the pigment paste (C).
[0191] The shear rate of the pigment paste (C) is 100 sec. -1 , viscosity at 65°C (V C ) is in the range of 20 to 1800 mPa·s.
[0192] The shear rate of the pigment paste (C) is 100 sec. -1 , viscosity at 65°C (V C ) is preferably in the range of 50 to 1500 mPa·s, more preferably in the range of 100 to 1000 mPa·s, and even more preferably in the range of 150 to 800 mPa·s, from the viewpoints of reducing the VOC content in the resulting coating composition and of the hardness, adhesion, and color unevenness of the coating film formed.
[0193] The solids concentration of the pigment paste (C) is preferably within the range of 84 to 99 mass %, more preferably within the range of 85 to 98 mass %, even more preferably within the range of 87 to 98 mass %, and even more preferably within the range of 90 to 98 mass %, from the viewpoints of reducing the VOC content in the resulting coating composition and preventing adhesion and color unevenness of the coating film to be formed.
[0194] The content of the pigment paste (C) in the kit according to the present invention and the three-component paint composition according to the present disclosure is preferably in the range of 3 to 50 mass %, more preferably in the range of 4 to 40 mass %, and even more preferably in the range of 5 to 30 mass %, based on the total amount of the three-component paint composition, from the viewpoints of reducing the VOC content in the resulting paint composition and of the hardness, adhesion, color unevenness, etc. of the paint film to be formed.
[0195] <Method for forming a coating film using a kit and a three-component coating composition> The kit according to the present invention and the three-component coating composition according to the present disclosure are applied to a substrate to form a wet coating film (uncured coating film), and then the wet coating film is cured to form the desired coating film.
[0196] The substrate is preferably a resin material from the viewpoint of adhesion of the coating film to be formed, etc. Examples of the resin material include acrylic resins such as polymethyl methacrylate, polyester resins such as polyethylene terephthalate, polyethylene naphthalate, poly-1,4-cyclohexanedimethylene terephthalate, polyethylene-1,2-diphenoxyethane-4,4'-dicarboxylate, and polybutylene terephthalate, epoxy resins represented by commercially available products such as Epicoat (trade name: manufactured by Yuka Shell Epoxy Co., Ltd.), polycarbonate resins, polyimide resins, novolac resins, phenolic resins, acrylonitrile-butadiene-styrene (ABS) resins, acrylonitrile-ethylene-styrene (AES) resins, and acrylic resins. Examples of suitable resins include lylonitrile-styrene-acrylate (ASA) resins, vinyl chloride resins, vinylidene chloride resins, polyurethane resins, cellulose ester resins (e.g., triacetyl cellulose, diacetyl cellulose, propionyl cellulose, butyryl cellulose, acetylpropionyl cellulose, nitrocellulose), polyamide resins, polystyrene resins (e.g., syndiotactic polystyrene), polyolefin resins (e.g., polypropylene, polyethylene, polymethylpentene), polysulfone resins, polyethersulfone resins, polyarylate resins, polyetherimide resins, polyether ketone resins, various fiber reinforced plastic materials (Fiber Reinforced Plastics: hereinafter sometimes abbreviated as FRP materials or simply FRP), and polymer alloys thereof.
[0197] The substrate may also be one in which, for example, a primer coating, an intermediate coating, a top coating, or the like is applied onto the resin material, thereby forming a primer layer, an intermediate coating layer, a top coating layer, or the like in advance.
[0198] The substrate may be subjected to at least one physical treatment (physical treatment) selected from plasma treatment, corona discharge treatment, active energy ray treatment, flame treatment, blast treatment, polishing treatment, and the like.
[0199] The three-component coating composition formed from the kit of the present invention and the three-component coating composition of the present disclosure are preferably applied directly to a substrate. Furthermore, the applications of the substrates to which the three-component coating composition formed from the kit of the present invention and the three-component coating composition of the present disclosure are applied are not particularly limited, and examples thereof include the outer panels of automobile bodies such as passenger cars, trucks, motorcycles, and buses; automotive interior and exterior parts such as bumpers, center pillars, mirrors, door handles, instrument panels, door trims, and center consoles; furniture and building materials such as chairs, vanity mirrors, window frames, and gates; and the outer panels of household electrical appliances such as mobile phones and audio equipment. The method for applying the three-component coating composition formed from the kit of the present invention and the three-component coating composition of the present disclosure to a substrate is not particularly limited. For example, application can be performed using an air spray, airless spray, rotary atomizer, dip coating, applicator, brush, roller, in-mold coating, or the like. Electrostatic application may be performed during application.
[0200] The coating thickness, in terms of cured film thickness, is preferably within the range of 5 to 2000 μm, more preferably within the range of 10 to 1500 μm, and even more preferably within the range of 15 to 1000 μm.
[0201] The three-component coating composition formed from the kit according to the present invention and the three-component coating composition according to the present disclosure can be cured by heating the three-component coating composition.
[0202] <Heating> Heating can be performed by any method known in this field. Specifically, for example, hot air, hot gas, an infrared heater, an IR radiator, an oven, a heated roller, a hot press, a microwave, etc. In the present invention, from the viewpoint of ease of operation, etc., it is preferable to perform heating by hot air, an infrared heater, a hot press, etc.
[0203] From the viewpoints of productivity, workability, thermal stability of the substrate, etc., the heating temperature is preferably within a range of 30 to 200°C, more preferably within a range of 50 to 180°C, and even more preferably within a range of 70 to 160°C.
[0204] The heating time is preferably within a range of 20 seconds to 60 minutes, and more preferably within a range of 40 seconds to 10 minutes.
[0205] The three-component coating composition of the present invention can also be suitably used in in-mold coating, which has the advantage of being able to use coating compositions with low VOC content and reducing the air conditioning energy required during coating, thereby reducing the environmental impact.
[0206] <In-mold coating method> The in-mold coating method according to the present invention comprises the steps of injecting the coating composition of the present invention (hereinafter, when the coating composition of the present invention is used in the in-mold coating method, it will be referred to as the in-mold coating coating composition) between a molded substrate and the inner wall of a mold, curing the in-mold coating coating composition, and then removing the coated molded article from the mold.
[0207] The in-mold coating method can be any conventional method of molding and coating in a mold without any particular limitations, such as the methods described in JP-A-2000-141407 and JP-A-2008-525212.
[0208] It should be noted that the resin molding mold used when molding the resin material and the in-mold coating mold used when in-mold coating with the in-mold coating composition may be the same or different.When the resin molding mold and the in-mold coating mold are the same, for example, a heated and molten resin material is injected in an injection cylinder between the resin molding molds having the shape of the desired molded product, and then cooled and pressurized in the resin molding mold to form the resin material into a molded product, and then the resin molding mold is separated from the surface of the molded product made of the resin material.Next, the main component (A), the curing agent (B) and the pigment paste (C) are mixed to prepare an in-mold coating composition, and a gap sufficient to inject the in-mold coating composition is provided between the surface of the molded product made of the resin material and the in-mold coating mold, and the in-mold coating composition is injected between the surface of the molded product made of the resin material and the inner wall of the in-mold coating mold, and the in-mold coating mold is closed to form an uncured in-mold coating film on the molded product made of the resin material. Next, the uncured in-mold coating film formed on the molded product made of the resin material is heated and molded into a desired shape, thereby obtaining an in-mold coated molded product in which a cured in-mold coating film is formed on the molded product made of the resin material.
[0209] When the resin molding mold and the in-mold coating mold are different, for example, a resin material heated and melted in an injection cylinder is injected between the resin molding molds having the shape of the desired molded product, cooled and pressurized in the resin molding mold to form a molded product from the resin material, and then the resin molding mold is separated and removed from the surface of the molded product made of the resin material. Next, the main component (A), the curing agent (B), and the pigment paste (C) are mixed to prepare an in-mold coating paint composition, the in-mold coating mold is brought close to the surface of the resin molding, a gap sufficient to inject the in-mold coating paint composition is provided between the surface of the molded product made of the resin material and the in-mold coating mold, the in-mold coating paint composition is injected between the surface of the molded product made of the resin material and the inner wall of the in-mold coating mold, the in-mold coating mold is closed, and an uncured in-mold coating film is formed on the molded product made of the resin material. Next, the uncured in-mold coating film formed on the molded product made of the resin material is heated and molded into the desired shape, thereby obtaining an in-mold coated molded product in which a cured in-mold coating film is formed on the molded product made of the resin material. Furthermore, from the viewpoint of releasability between the in-mold coated molded product and the in-mold coated mold, an external mold release agent may be applied to the mold. Examples of the external mold release agent that can be used include fluorine-based, silicone-based, surfactant-based, and wax-based external mold release agents.
[0210] The heating temperature when melting the resin in the injection cylinder is determined arbitrarily depending on the type of resin material, etc., but is preferably 80 to 300° C. The temperature of the mold when injecting the resin material is determined arbitrarily depending on the molding time, type of resin material, etc., but is preferably 30 to 120° C.
[0211] When preparing the in-mold coating paint composition by mixing the main component (A), the curing agent (B), and the pigment paste (C), it is preferable to heat the main component (A), the curing agent (B), and the pigment paste (C) separately before mixing them, from the viewpoints of the hardness, adhesion, color unevenness, etc. of the coating film to be formed.
[0212] When the main agent (A), the curing agent (B), and the pigment paste (C) are each heated and then mixed, the temperature is preferably within a range of 30 to 100°C, more preferably within a range of 40 to 90°C, and even more preferably within a range of 50 to 80°C, from the viewpoints of the hardness, adhesion, color unevenness, etc. of the coating film to be formed.
[0213] Furthermore, since the main agent (A), the curing agent (B), and the pigment paste (C) may be heated when mixed, the flash point of the main agent (A) is preferably 70° C. or higher, and more preferably 100° C. or higher, the flash point of the curing agent (B) is preferably 70° C. or higher, and more preferably 100° C. or higher, and the flash point of the pigment paste (C) is preferably 70° C. or higher, and more preferably 100° C. or higher. The molding time for the resin material may be until the resin material is completely solidified, but it is sufficient if the resin material is solidified to a strength that does not impair the molded shape when the in-mold coating paint composition is injected, and is usually preferably about 20 seconds to 60 minutes.
[0214] The amount of the in-mold coating composition injected is an amount sufficient to obtain a desired film thickness, and is preferably an amount sufficient to obtain a cured film thickness of 15 to 2000 μm. The heating temperature when the uncured in-mold coating film is heated is preferably within a range of 20 to 160°C, more preferably within a range of 40 to 150°C, and even more preferably within a range of 60 to 140°C.
[0215] Furthermore, the heating time for heating the uncured in-mold coating film is preferably within a range of 20 seconds to 10 minutes, more preferably within a range of 30 seconds to 5 minutes, and even more preferably within a range of 40 seconds to 4 minutes.
[0216] When the uncured in-mold coating film is heated and cured, it is preferable to apply pressure. When applying pressure, the pressure is preferably within a range of 2 to 14 MPa from the viewpoints of the hardness and adhesion of the coating film to be formed.
[0217] The present invention will be explained in more detail below with reference to Production Examples, Examples, and Comparative Examples. Note that these Production Examples, Examples, and Comparative Examples are merely illustrative and are not intended to limit the scope of the present invention. In the Production Examples, Examples, and Comparative Examples, "parts" and "%" are based on mass unless otherwise specified. Furthermore, the film thickness of the coating film is based on the cured coating film.
[0218] The components used in the following examples are as follows:
[0219] <Preparation of Main Component (A)> Production Example 1 Into a container equipped with a stirrer, 80.0 parts of "Desmophen XP2488" (trade name, manufactured by Covestro, hydroxyl-containing polyester resin containing 26% of hydroxyl-containing monomer, number average molecular weight 500, solid content concentration 100%), 20.0 parts of "Placcel 303" (trade name, manufactured by Daicel Corporation, hydroxyl-containing polycaprolactone resin, number average molecular weight 310, solid content concentration 100%), 1.7 parts of "Moldwiz INT-120IMC" (trade name, manufactured by Axel Plastics, fatty acid tertiary dimethylamide-containing mixture, solid content concentration 100%), 0.2 parts of "BYK-333" (trade name, manufactured by BYK-Chemie, surface conditioner (polyether-modified polydimethylsiloxane), solid content concentration 100%), and 2.9 parts of "TINUVIN 400" (trade name, manufactured by BASF Corporation, triazine-based ultraviolet absorber, solids concentration 85%), 5.7 parts of "TINUVIN 292" (trade name, manufactured by BASF Corporation, hindered amine compound light stabilizer, solids concentration 100%), and 1.7 parts of "NEOSTAN U-830" (trade name, manufactured by Nitto Kasei Co., Ltd., dioctyltin diversatate, solids concentration 100%) were blended and mixed uniformly to obtain a main component (A-1) with a solids concentration of 98.5%.
[0220] Production Examples 2 to 11 Main components (A-1) to (A-11) were obtained in the same manner as in Production Example 1, except that the blending compositions in Production Example 1 were as shown in Table 1 below. -1 , viscosity at 65°C (V A Measurement of the shear rate of 100 sec for the main components (A-1) to (A-11) obtained in Production Examples 1 to 11. -1 , viscosity at 65°C (V A) was measured according to the following method. The results are also shown in Table 1.
[0221] Shearing rate 100sec -1 The temperature was increased from 20°C to 80°C at a rate of 5°C / min, and the shear rate was 100 sec. -1 , viscosity at 65°C (V A ) was measured using a cone and plate viscometer "MCR-302e" (trade name, manufactured by Anton Paar, 25 mm diameter, 2° inclined cone and plate).
[0222] The components listed in the table are as follows:
[0223] (Note 1) "Desmophen VPLS 2249 / 1": Trade name, manufactured by Covestro, hydroxyl-containing polyester resin containing 44% hydroxyl-containing monomer, number average molecular weight 1008, solid content 100%, (Note 2) "ETERNACOL PH-300": Manufactured by UBE, hydroxyl-containing polycarbonate resin, number average molecular weight 3000, solid content 100%, (Note 3) "Desmophen NH1220": Trade name, manufactured by Covestro, N,N'-(2-methylpentane-1,5-diyl)bisaspartate tetraethyl, number average molecular weight 461, solid content 100%, (Note 4) "Desmophen "NH1423": Trade name, manufactured by Covestro, N,N'-[methylenebis(cyclohexane-4,1-diyl)]bisaspartate tetraethyl, number average molecular weight 551, solids concentration 100%, (Note 5) "TMMP-LV": Trade name, manufactured by SC Organic Chemical Industry Co., Ltd., trimethylolpropane tris(3-mercaptopropionate), number average molecular weight 399, solids concentration 100%, (Note 6) "TEMPIC": Trade name, manufactured by SC Organic Chemical Industry Co., Ltd., tris-[(3-mercaptopropionyloxy)-ethyl]isocyanurate, number average molecular weight 526, solids concentration 100%, (Note 7) "PEMP-LV": Trade name, manufactured by SC Organic Chemical Industry Co., Ltd., pentaerythritol tetrakis(3-mercaptopropionate), number average molecular weight 489, solids concentration 100%.
[0224] <Preparation of Curing Agent (B)> Production Example 12 Into a container equipped with a stirrer were added 40.0 parts of "Desmodur N3900" (trade name, manufactured by Sumika Covestro Urethane Co., Ltd., iminooxadiazinedione of hexamethylene diisocyanate, solids concentration 100%), 20.0 parts of "Desmodur N3400" (trade name, manufactured by Sumika Covestro Urethane Co., Ltd., a mixture of uretdione of hexamethylene diisocyanate and isocyanurate, solids concentration 100%), 40.0 parts of "Desmodur NZ200" (trade name, manufactured by Sumika Covestro Urethane Co., Ltd., a mixture of isocyanurate of hexamethylene diisocyanate and isocyanurate of isophorone diisocyanate, solids concentration 100%), and "Carbodilite V-05" (trade name, manufactured by Nisshinbo Chemical Inc., a carbodiimide group-containing compound having an aromatic ring structure and two isocyanate groups, a carbodiimide equivalent per solid content of 262, a number average molecular weight of 800, and a solid content of 100%) was blended and mixed uniformly to obtain a curing agent (B-1) with a solid content of 100.0%.
[0225] Production Examples 13 to 19 Curing agents (B-2) to (B-8) were obtained in the same manner as in Production Example 12, except that the blending compositions in Production Example 12 were as shown in Table 2 below.
[0226] <Shear rate of curing agent (B) 100 sec -1 , viscosity at 65°C (V B Measurement of shear rate of 100 sec for the curing agents (B-1) to (B-8) obtained in Production Examples 12 to 19. -1 , viscosity at 65°C (V B The results are also shown in Table 2. -1 The temperature was increased from 20°C to 80°C at a rate of 5°C / min, and the shear rate was 100 sec. -1 , viscosity at 65°C (V B ) was measured using a cone and plate viscometer "MCR-302e" (trade name, manufactured by Anton Paar, 25 mm diameter, 2° inclined cone and plate).
[0227] The components listed in the table are as follows:
[0228] (Note 8) "Desmodur N3600": Trade name, manufactured by Sumika Covestro Urethane Co., Ltd., isocyanurate of hexamethylene diisocyanate, solids concentration 100%, (Note 9) "Desmodur N3500": Trade name, manufactured by Sumika Covestro Urethane Co., Ltd., allophanate of hexamethylene diisocyanate, solids concentration 100%.
[0229] <Preparation of Pigment Paste (C)> Production Example 20
[0123] Into a vessel equipped with a stirrer were added 80.0 parts of "Desmophen XP2488" (trade name, manufactured by Covestro, hydroxyl-containing polyester resin containing 26% of hydroxyl-containing monomer, number average molecular weight 500, solid content concentration 100%), 20.0 parts of "Placcel 303" (trade name, manufactured by Daicel Corporation, hydroxyl-containing polycaprolactone resin, number average molecular weight 310, solid content concentration 100%), 4.8 parts of "Raven 5000 ULTRA III POWDER" (trade name, manufactured by BIRLA CARBON, carbon black pigment, solid content concentration 100%), and 10.0 parts of "SOLSPERSE 5000S (trade name, manufactured by LUBRISOL, phthalocyanine pigment derivative, solid content 100%) 0.5 parts, "DISPERBYK-2013" (trade name, manufactured by BYK, dispersant, solid content 100%) 2.4 parts, "Moldwiz INT-120IMC" (trade name, manufactured by AXEL PLASTICS, fatty acid tertiary dimethylamide-containing mixture, solid content 100%) 1.7 parts, "BYK-333" (trade name, manufactured by BYK, surface conditioner (polyether-modified polydimethylsiloxane), solid content 100%) 0.2 parts, "TINUVIN 400" (trade name, manufactured by BASF, triazine-based ultraviolet absorber, solid content 85%) 2.9 parts, "TINUVIN 292" (trade name, manufactured by BASF, hindered amine compound light stabilizer, solid content 100%) 5.7 parts, "Neostan 1.7 parts of "U-830" (trade name, manufactured by Nitto Kasei Co., Ltd., dioctyltin diversatate, solids concentration 100%) and 8.7 parts of butyl acetate were added and mixed uniformly. The resulting mixed solution was then placed in a wide-mouthed glass bottle, glass beads with a diameter of approximately 1.3 mm were added as a dispersing medium, the bottle was sealed, and the mixture was dispersed for 3 hours using a paint shaker to obtain a pigment paste (C-1) with a solids concentration of 92.0%.
[0230] Production Examples 21 to 81 Pigment pastes (C-2) to (C-62) were obtained in the same manner as in Production Example 20, except that the blending compositions in Production Example 20 were as shown in Table 3 below.
[0231] <Pigment paste (C) shear rate 100 sec -1 , viscosity at 65°C (V C Measurement of the shear rate of 100 sec for the pigment pastes (C-1) to (C-62) obtained in Production Examples 20 to 81. -1 , viscosity at 65°C (V C The results are also shown in Table 3. -1 The temperature was increased from 20°C to 80°C at a rate of 5°C / min, and the shear rate was 100 sec. -1 , viscosity at 65°C (V B ) was measured using a cone and plate viscometer "MCR-302e" (trade name, manufactured by Anton Paar, 25 mm diameter, 2° inclined cone and plate).
[0232]
[0233]
[0234]
[0235]
[0236]
[0237] The components listed in the table are as follows:
[0238] (Note 10) "PTMG-2000": Trade name, manufactured by Mitsubishi Chemical Corporation, polytetramethylene glycol, number average molecular weight 2000, solid content 100%, (Note 11) "PTMG-3000": Trade name, manufactured by Mitsubishi Chemical Corporation, polytetramethylene glycol, number average molecular weight 3000, solid content 100%, (Note 12) "Tipake CR-95": Trade name, manufactured by Ishihara Sangyo Kaisha, Ltd., titanium oxide, solid content 100%, (Note 13) "Chlorinated Cyanine Blue G-314": Trade name, manufactured by Sanyo Dye Co., Ltd., phthalocyanine blue pigment, solid content 100%, (Note 14) "YELLOW 2GLMA": Trade name, manufactured by Dominion Colour Corporation, bismuth vanadate yellow pigment, solid content 100%, (Note 15) "Irgazin Rubine L4025": Trade name, manufactured by BASF, diketopyrrolopyrrole red pigment, solid content 100%, (Note 16) "LG neo BLUE #325": Trade name, manufactured by Oike Metallic Design Co., Ltd., vapor deposition colored aluminum pigment, solid content 100%, (Note 17) "LG neo RED #325": Trade name, manufactured by Oike Metallic Design Co., Ltd., vapor deposition colored aluminum pigment, solid content 100%, (Note 18) "Xirallic T60-23 WNT Galaxy Blue": Trade name, manufactured by Merck, titanium oxide-coated alumina oxide flake pigment, solid content 100%, (Note 19) "Xirallic F60-51 SW RADIENT "RED": Trade name, manufactured by Merck, iron oxide coated alumina flake pigment, solids concentration 100%, (Note 20) "DISPERBYK-111": Trade name, manufactured by BYK-Chemie, dispersant, solids concentration 100%, (Note 21) "Borchi Gen 1757": Trade name, manufactured by Borchers Americas, dispersant, solids concentration 100%.
[0239] <Preparation of In-Mold Coated Molded Article> Example 1 (Preparation of In-Mold Coated Molded Article (M1)) First, "DIALAC TW20" (trade name, manufactured by Techno UMG, acrylonitrile-styrene-acrylate resin (ASA resin)) was filled into an injection molding cylinder and heated to melt at 230°C. Thereafter, it was injected between a resin molding die at 60°C, and the pressure was maintained for 30 seconds while cooling, thereby obtaining a 100 mm x 100 mm x 2 mm flat "DIALAC TW20" molded article. Next, a kit consisting of the base resin (A-1) obtained in Production Example 1, the curing agent (B-1) obtained in Production Example 12, and the pigment paste (C-1) obtained in Production Example 20 was prepared, and each of the kits was heated to 65°C. Next, the base agent (A-1), the curing agent (B-1), and the pigment paste (C-1) were blended in a container equipped with a stirrer so that the mass ratio of (A-1) / (B-1) / (C-1) was 30.3 / 62.1 / 7.6, and mixed uniformly to obtain an in-mold coating paint composition No. 1 with a solids concentration of 98.9%. Next, the resin molding mold was opened, and the in-mold coating paint composition No. 1 was injected between the obtained flat "DIALAC TW20" molded product and the coating film-coated mold, and the inside of the coating film-coated mold was heated to 80 ° C. and maintained at that temperature, and a molding pressure of 5 MPa was applied and maintained for 1 minute, after which the pressure was reduced and the coating film-coated mold was opened to produce an in-mold coated molded product (M1-1) in which a coating film with a cured film thickness of 200 μm was coated on the flat "DIALAC TW20" molded product.
[0240] (Preparation of In-Mold Coated Molded Product (M2)) First, "Makroblend UT235M" (trade name, manufactured by Covestro, a polymer alloy of polyethylene terephthalate resin and polycarbonate resin) was filled into an injection molding cylinder and heated to melt at 270°C. It was then injected into a resin molding die at 70°C, and the pressure was maintained for 30 seconds while cooling to obtain a 100 mm x 100 mm x 2 mm flat "Makroblend UT235M" molded product. Next, the base resin (A-1) obtained in Production Example 1, the curing agent (B-1) obtained in Production Example 12, and the pigment paste (C-1) obtained in Production Example 20 were each heated to 65°C. Next, the main component (A-1), the curing agent (B-1), and the pigment paste (C-1) were blended in a container equipped with a stirrer so that the mass ratio of (A-1) / (B-1) / (C-1) was 30.3 / 62.1 / 7.6, and mixed uniformly to obtain in-mold coating paint composition No. 1 with a solids concentration of 98.9%.
[0241] Next, the resin molding mold was opened, and the in-mold coating composition No. 1 was injected between the obtained flat-plate "Makroblend UT235M" molded product and the coating film-coated mold. The inside of the coating film-coated mold was heated to 80°C, and while maintaining this temperature, a molding pressure of 5 MPa was applied and maintained for 1 minute. Thereafter, the pressure was reduced and the coating film-coated mold was opened, thereby producing an in-mold coated molded product (M2-1) in which the flat-plate "Makroblend UT235M" molded product was coated with a coating film with a cured film thickness of 200 μm.
[0242] Examples 2 to 59, Comparative Examples 1 to 26 In-mold coated moldings (M1-2) to (M1-85) and (M2-2) to (M2-85) were produced in the same manner as in Example 1, except that the blending compositions in Example 1 were as shown in Table 4 below.
[0243] <Evaluation of in-mold coated moldings> The cured coating film of each in-mold coated molding was evaluated for color unevenness, hardness, and adhesion. The evaluation results are shown in Table 4.
[0244] (Color Unevenness) The surface of each of the in-mold coated moldings obtained in Examples 1 to 59 and Comparative Examples 1 to 26 was observed with the naked eye, and the degree of color unevenness was evaluated according to the following criteria. ◎ and ○ are acceptable. ◎: Almost no color unevenness is observed, ○: Slight color unevenness is observed, △: Color unevenness is observed, ×: Significant color unevenness is observed.
[0245] (Hardness) The Martens hardness (N / mm) of the cured coating film of each of the in-mold coated moldings obtained in Examples 1 to 59 and Comparative Examples 1 to 26 was 2 ) was measured using a "Fisherscope (registered trademark) HM2000S" (product name, manufactured by Fischer Instruments Inc.) and evaluated based on the following criteria. The measurement conditions were: indenter: square pyramidal Vickers indenter (material: diamond, facing angle: 136°), maximum test load: 20 mN, indentation speed: 20 mN / 25 seconds, temperature: 21±2°C, humidity: 50±5% relative humidity. ◎ and ◯ are acceptable. ◎: Martens hardness is 110 N / mm 2 ○: Martens hardness is 100 N / mm or more 2 Above, 110N / mm 2 △: Martens hardness is less than 75 N / mm 2 or more, 100N / mm 2 x: Martens hardness is less than 75 N / mm 2 is less than.
[0246] (Adhesion) The coating film of each of the in-mold coated moldings obtained in Examples 1 to 59 and Comparative Examples 1 to 26 was cut into a grid pattern with a cutter so as to reach the substrate, creating 100 2 mm x 2 mm squares. Next, adhesive cellophane tape was applied to the surface of each in-mold coated molding, and the adhesive cellophane tape was rapidly peeled off at a temperature of 23±2°C and a humidity of 50±5% relative humidity. The state of the cross-hatched coating film remaining after peeling was examined, and adhesion was evaluated based on the following criteria: ◎ and ○ indicate pass. ◎: 100 cross-hatched coating film remains, and there are no small chips or lifts in the coating film at the edges of the cutter cuts; ○: 100 cross-hatched coating film remains, and there are small chips or lifts in the coating film at the edges of the cutter cuts; △: 90 to 99 cross-hatched coating film remains; ×: 89 or fewer cross-hatched coating film remains.
[0247]
[0248]
[0249]
[0250]
[0251]
[0252]
[0253]
[0254]
Claims
1. A three-liquid coating composition kit comprising: a base agent (A) containing an isocyanate-reactive group-containing compound (a1); a curing agent (B) containing a polyisocyanate compound (b1); and a pigment paste (C) containing an isocyanate-reactive group-containing compound (c1) and a pigment (c2), -1 , viscosity at 65°C (V A ) is in the range of 20 to 1800 mPa s, and the shear rate of the curing agent (B) is 100 sec -1 , viscosity at 65°C (V B ) is in the range of 20 to 1800 mPa s, and the shear rate of the pigment paste (C) is 100 sec -1 , viscosity at 65°C (V C ) is in the range of 20 to 1800 mPa·s.
2. The kit according to claim 1, wherein the solids concentration of the three-component paint composition formed from the kit is 95 mass % or more.
3. The kit according to claim 1 or 2, wherein the solid content concentration of the pigment paste (C) is within the range of 85 to 98 mass %.
4. The kit according to any one of claims 1 to 3, wherein the isocyanate-reactive group-containing compound (c1) comprises an isocyanate-reactive group-containing compound having a number average molecular weight in the range of 250 to 2,500.
5. A kit according to any one of claims 1 to 4, wherein the content of the pigment (c2) is within the range of 1.0 to 65 mass% based on the total amount of the pigment paste (C).
6. The above (V A ), the above (V B ) and the above (V C ) is expressed by the following formula (1) and formula (2): 0.4≦(V B ) / (V A )≦2.5 Formula (1) 0.3≦(V C ) / (V A 6. The kit according to claim 1 , wherein the formula (2) is satisfied:
7. A three-liquid coating composition comprising: a base agent (A) containing an isocyanate-reactive group-containing compound (a1); a curing agent (B) containing a polyisocyanate compound (b1); and a pigment paste (C) containing an isocyanate-reactive group-containing compound (c1) and a pigment (c2), -1 , viscosity at 65°C (V A ) is in the range of 20 to 1800 mPa s, and the shear rate of the curing agent (B) is 100 sec -1 , viscosity at 65°C (V B ) is in the range of 20 to 1800 mPa s, and the shear rate of the pigment paste (C) is 100 sec -1 , viscosity at 65°C (V C ) is in the range of 20 to 1800 mPa·s.
8. An in-mold coating method comprising the steps of injecting an in-mold coating paint composition between a molded substrate and an inner wall of a mold, curing the in-mold coating paint composition, and then removing the coated molded article from the mold, wherein the in-mold coating paint composition is a three-component paint composition formed from the kit according to any one of claims 1 to 6, or the three-component paint composition according to claim 7.
Citation Information
Patent Citations
Mold-coating for polyurethane molded article
JP1989240577A
Coating composition
JP1990014273A
Curing composition, thermopotential acid catalyst, method of coating finish and coated product, and molding method and molded product
JP1996041208A
Method for in-mold coating using mold with multiple mold cavities, and substrate coated thereby
JP2017534477A
Two-part coating composition
JP2020183455A