Composition for semiconductor device processing, method for producing modified substrate, and method for producing laminate
The use of a polymer-based composition with aromatic monomers and solvents in semiconductor processing addresses the accuracy challenges of top-down methods by forming films that inhibit ALD deposition, thereby improving the precision and performance of semiconductor devices.
Patent Information
- Application Number
- PCT/JP2024/010174
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional top-down photolithography methods for semiconductor device fabrication face challenges in achieving the required accuracy due to mechanical and optical limitations, necessitating a bottom-up approach for forming finer semiconductor elements.
A composition comprising a polymer with functional groups interacting with the substrate, derived from aromatic monomers, and a solvent is used to form a film that inhibits material deposition during atomic layer deposition (ALD), allowing for selective modification of the substrate and laminate manufacturing.
The composition achieves excellent ALD inhibition properties, enabling the formation of denser films that improve the accuracy and precision of semiconductor device fabrication, enhancing the performance of semiconductor devices.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Composition for treating semiconductor devices, method for producing modified substrate, method for producing laminate
[0001] The present invention relates to compositions for treating semiconductor devices, methods for producing modified substrates, and methods for producing laminates.
[0002] As semiconductor devices become more powerful, smaller and more precise semiconductor elements are required. Traditionally, top-down photolithography has been used to form semiconductor elements, but achieving the required precision is becoming increasingly difficult due to mechanical and optical factors, etc. Therefore, as a bottom-up method for forming semiconductor elements, a method for selectively modifying a substrate has been considered, in which a film of a compound is formed on a region of a substrate made of a specific material by selectively adsorbing the compound to the specific material, and the film is then used to modify regions of the substrate other than the region made of the specific material. Specifically, for example, a method has been devised in which a material that selectively adsorbs to a specific component is used to selectively form a coating that inhibits material deposition on a specific region of the substrate surface, followed by atomic layer deposition (ALD) processing to selectively deposit material in regions where the coating is not present, thereby modifying the substrate.
[0003] As a method for selectively modifying a substrate as described above, Patent Document 1 discloses a method for selectively modifying a substrate surface, the method comprising the steps of: preparing a substrate having a first region containing a metal atom on its surface; applying to the surface of the substrate a composition containing a first polymer having, at an end of its main chain or side chain, a group containing a first functional group that bonds to the metal, and a solvent; and heating the coating film formed by the application step.
[0004] International Publication No. 2018 / 043304
[0005] The coating used for selective modification of a substrate as described above is required to suppress the amount of material deposited on the coating when atomic layer deposition (ALD) processing is performed on the coating, i.e., to have excellent ALD inhibition properties.
[0006] The present inventors formed a coating using the composition disclosed in Patent Document 1 and subjected the coating to ALD treatment, and found that there was room for further improvement in ALD inhibition. Therefore, an object of the present invention is to provide a composition for semiconductor device processing that can form a coating with excellent ALD inhibition properties. Another object of the present invention is to provide a method for producing a modified substrate and a method for producing a laminate using the above composition.
[0007] As a result of extensive research into solving the above problems, the present inventors have found that the problems can be solved by the following configuration.
[0008] [1] A composition for treating a semiconductor device, comprising: a polymer having at least one functional group that interacts with a substrate at an end of the main chain or in a side chain, and having a repeating unit derived from an aromatic monomer; an aromatic monomer; and a solvent. [2] The composition for treating a semiconductor device according to [1], wherein the polymer is a polymer having a repeating unit derived from an aromatic vinyl monomer. [3] The composition for treating a semiconductor device according to [1] or [2], wherein the content of the aromatic monomer is 1 to 50,000 ppm by mass with respect to the content of the polymer. [4] The composition for treating a semiconductor device according to any one of [1] to [3], wherein the aromatic monomer comprises at least one selected from the group consisting of a compound represented by formula (1) described below and vinylpyridine. [5] The composition for treating a semiconductor device according to any one of [1] to [4], wherein the polydispersity of the polymer is 1.0 to 1.5. [6] R 1 [7] The composition for treating a semiconductor device according to [4] or [5], wherein R is a hydrogen atom. 2 ~R 6is a hydrogen atom or an alkyl group. [8] The composition for treating a semiconductor device according to any one of [1] to [7], wherein the solvent comprises at least one selected from the group consisting of propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, cyclohexanone, ethyl lactate, and methyl isobutyl carbinol. [9] The composition for treating a semiconductor device according to any one of [1] to [8], wherein the total content of the polymer and the aromatic monomer is 0.1 mass % or more and less than 10 mass % with respect to the total mass of the composition for treating a semiconductor device.
[10] A method for producing a modified substrate, comprising a step of contacting a substrate with the composition for treating a semiconductor device according to any one of [1] to [9].
[11] A method for producing a laminate, comprising: Step 1 of contacting a substrate having at least two surfaces, a first surface and a second surface, each of which is made of a different material, with the composition for treating a semiconductor device according to any one of [1] to [9] to form a first coating on the first surface; and Step 2 of subjecting the substrate obtained in Step 1 to atomic layer deposition to form a second coating on the second surface.
[0009] According to the present invention, there is provided a composition for semiconductor device treatment that can form a coating film with excellent ALD inhibitory properties. The present invention also provides a method for producing a modified substrate and a method for producing a laminate using the composition.
[0010] The present invention will be described in detail below. The following description of the components may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments.
[0011] In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. In this specification, "ppm" means "parts-per-million (10 -6 ) and "ppb" stands for "parts-per-billion (10 -9 ) and "ppt" stands for "parts-per-trillion (10-12 In this specification, when two or more types of a component are present, the "content" of the component means the total content of those two or more components.
[0012] In this specification, when there are a plurality of substituents, linking groups, etc. (hereinafter referred to as "substituents, etc.") represented by a specific symbol, or when a plurality of substituents, etc. are simultaneously specified, it means that the respective substituents, etc. may be the same or different from each other. This also applies to the specification of the number of substituents, etc.
[0013] In this specification, "(meth)acrylic" is a concept that includes either or both of acrylic and methacrylic, "(meth)acrylate" is a concept that includes either or both of acrylate and methacrylate, and "(meth)acryloyl" is a concept that includes either or both of acryloyl and methacryloyl.
[0014] In this specification, unless otherwise specified, the weight average molecular weight (Mw), number average molecular weight (Mn), and polydispersity index (PDI) (Mw / Mn) of a polymer are defined as polystyrene-equivalent values measured by gel permeation chromatography (GPC) using a GPC apparatus (HLC-8120GPC, manufactured by Tosoh Corporation) (solvent: tetrahydrofuran, flow rate (sample injection amount): 10 μL, column: TSK gel Multipore HXL-M (manufactured by Tosoh Corporation), column temperature: 40° C., flow rate: 1.0 mL / min, detector: differential refractive index detector).
[0015] [Composition for treating semiconductor devices] The composition for treating semiconductor devices of the present invention (hereinafter also referred to as "the composition") will be described in detail below. The composition contains a polymer having repeating units derived from an aromatic monomer and having at least one functional group that interacts with a substrate at the end of the main chain or on a side chain, an aromatic monomer, and a solvent.
[0016] While the reason why the composition having the above configuration can solve the problems of the present invention is not entirely clear, the inventors speculate as follows. The following speculation does not limit the mechanism by which the effect is obtained. In other words, even if the effect is obtained by a mechanism other than the one described below, it is still within the scope of the present invention. It is preferable that the coating that inhibits the deposition of materials during ALD processing is formed densely on the substrate without any voids. The polymer forms a coating by adsorbing to the substrate surface via functional groups at the end or side chain of its main chain that interact with the substrate. The polymer can form a dense coating due to the repeating unit structure derived from an aromatic monomer with high stacking properties. Furthermore, in this composition, the aromatic monomer that can interact with the polymer and the substrate forms a coating in the voids not covered by the polymer, thereby forming a denser film overall, which is thought to result in superior ALD inhibition properties. Hereinafter, the ability of this composition to form a coating with superior ALD inhibition properties is also referred to as "excellent effects of the present invention."
[0017] [Polymer] The composition contains a polymer, and the polymer has at least one functional group (hereinafter also referred to as "interactive group") that interacts with the substrate at the end of the main chain or in a side chain, and has a repeating unit derived from an aromatic monomer. In this specification, the term "main chain" refers to the longest atomic chain among the atomic chains that constitute the polymer, and the term "side chain" refers to an atomic chain other than the main chain among the atomic chains that constitute the polymer. In this specification, the term "end" refers to an atomic group connected to the end of the main chain or the side chain.
[0018] <Interactive Group> The polymer has at least one interactive group at an end of the main chain or at a side chain. In terms of being able to form a denser coating and achieving better effects of the present invention, it is preferable that the polymer has an interactive group at one end (one end) of the main chain or at a side chain. The number of interactive groups in the polymer is not particularly limited as long as it is 1 or more, but is preferably 1 to 100, more preferably 1 to 60, more preferably 1 or 2, and even more preferably 1.
[0019] The mode of interaction between the interactive group and the substrate is not particularly limited, and may be bonding to the substrate surface or adsorption to the substrate surface. Specific examples of the mode of interaction include covalent bonding, coordinate bonding, ionic bonding, hydrogen bonding, acid-base interaction, van der Waals bonding, and metallic bonding. When the composition is used to form a coating on a metal surface A of a substrate composed of a material containing metal atoms, the mode of the interaction is preferably coordinate bonding or ionic bonding, and more preferably coordinate bonding. When the composition is used to form a coating on a non-metal surface B of a substrate composed of a non-metal material, the mode of the interaction is preferably hydrogen bonding, acid-base interaction, or covalent bonding. Details of the substrate and the surface of the substrate will be described later.
[0020] The interactive group is preferably either a group that interacts with a metal surface A of the substrate (also referred to as "interactive group A") or a group that interacts with a non-metal surface B of the substrate (also referred to as "interactive group B"), and is more preferably interactive group A.
[0021] The interactive group A is preferably a functional group capable of forming a coordinate bond with a metal. The interactive group A can be appropriately selected depending on the type of metal to be interacted with, and examples thereof include a nitrogen-containing group, an acidic group, a hydroxy group (—OH), a thiol group (—SH), a cyano group (—CN), a phosphonate ester bond-containing group, a sulfonate ester bond-containing group, an ethylenically unsaturated group, a carbon-carbon triple bond, a boronic acid group (—BO 2 H 2 ), epoxy groups, and disulfide bond-containing groups, and acidic groups, nitrogen-containing groups, hydroxy groups, and cyano groups are preferred.
[0022] Examples of the nitrogen-containing group include an amino group (—NR N 2 ), quaternary ammonium group (-N + R N 3 ), a hydrazine group, a guanidine group, and a nitrogen-containing heterocyclic group, and a tertiary amino group or a nitrogen-containing heterocyclic group is preferred. Neach independently represents a hydrogen atom or an alkyl group (preferably having 1 to 5 carbon atoms, more preferably having 1 to 3 carbon atoms). Examples of the nitrogen-containing heterocyclic group include nitrogen-containing aromatic heterocyclic groups such as a pyridyl group, an oxazolyl group, a triazine group, a pyrrole group, a pyrazole group, an imidazole group, a pyrazole group, a triazole group, a benzimidazole group, and a benztriazole group, and nitrogen-containing aliphatic heterocyclic groups such as an imidazolidinyl group, a pyrrolidinyl group, a pyrazolidinyl group, a piperidinyl group, and a piperazinyl group, and a pyridyl group, an oxazolyl group, an imidazolidinyl group, or a pyrrolidinyl group is preferred.
[0023] The acidic group may be, for example, a phosphate group (—PO 4 H 2 ), a phosphonic acid group (—PO 3 H 2 ), a carboxylic acid group (—COOH), and a sulfo group (—SO 3 H), etc., with a phosphonic acid group or a carboxylic acid group being preferred. The acidic group may form a salt in the present composition. Examples of the salt of the acidic group include salts with inorganic metal ions such as alkali metal ions and alkaline earth metal ions.
[0024] The hydroxy group may be either an alcoholic hydroxy group (a hydroxy group bonded to an aliphatic group) or a phenolic hydroxy group (a hydroxy group bonded to an aromatic group), with a phenolic hydroxy group being preferred.
[0025] The interactive group B is preferably a group capable of forming a hydrogen bond, an acid-base interaction, or a covalent bond (e.g., an Si—O bond, an Si—C bond, etc.) with a nonmetal. Examples of the interactive group B include hydrolyzable silyl groups such as alkoxysilyl groups and chlorosilyl groups, siloxane bond-containing groups, silanol groups, ethylenic double bonds, cyano groups, and thiol groups.
[0026] <Repeating Units Derived from Aromatic Monomers> The polymer contains repeating units derived from aromatic monomers. The aromatic monomer is a monomer compound having an aromatic group and a polymerizable group. The polymerizable group is not particularly limited as long as it is a functional group having polymerizability, but is preferably a polymerizable group capable of radical polymerization or anion polymerization, and more preferably an ethylenically unsaturated group. Examples of the ethylenically unsaturated group include a vinyl group, an allyl group, a (meth)acryloyl group, and a (meth)acrylamide group, and the vinyl group is preferred.
[0027] The aromatic group may be either an aromatic hydrocarbon group or an aromatic heterocyclic group, with an aromatic hydrocarbon group being preferred. The aromatic group may be either monocyclic or polycyclic, with a monocyclic group being preferred. The aromatic group preferably has 5 to 15 ring atoms, more preferably 5 to 10, and even more preferably 5 to 6. Examples of the aromatic hydrocarbon group include a phenyl group, a naphthyl group, an anthryl group, and a fluorenyl group, with a phenyl group or a naphthyl group being preferred, and a phenyl group being more preferred. The aromatic heterocyclic group is preferably a nitrogen-containing aromatic heterocyclic group, with an oxazolyl group, a pyridyl group, a triazine group, a pyrrole group, a pyrazole group, an imidazole group, a pyrazole group, a triazole group, a benzimidazole group, or a benzotriazole group being more preferred, and a pyridyl group being even more preferred. The aromatic group and the polymerizable group in the aromatic monomer may be the interactive group described above. For example, the nitrogen-containing aromatic heterocyclic group constituting the aromatic monomer may function as the interactive group A present in the side chain in the polymer.
[0028] The aromatic group may have a substituent. Examples of the substituent include, but are not limited to, an alkyl group, an alkoxy group, an alkyloxycarbonyl group, a halogen atom, and the above-described interactive group. When the polymer has an interactive group at the end of the main chain, the substituent is preferably an alkyl group, an alkoxy group, an alkyloxycarbonyl group, or a halogen atom; more preferably an alkyl group, an alkoxy group, or an alkyloxycarbonyl group; and even more preferably an alkyl group. When the polymer does not have an interactive group at the end of the main chain, the substituent is preferably the above-described interactive group; preferably a carboxy group, a hydroxy group, a cyano group, or a thiol group; more preferably a carboxy group or a hydroxy group. The number of substituents that the aromatic group may have is not particularly limited, and is preferably 1 to 3, and more preferably 1.
[0029] The aromatic monomer is preferably an aromatic vinyl monomer. That is, the polymer is preferably a polymer having a repeating unit derived from an aromatic vinyl monomer. The aromatic vinyl monomer is a monomer compound in which at least one hydrogen atom of an aromatic ring is substituted with a vinyl group. As the aromatic vinyl monomer, a compound represented by the following formula (1-1) is preferred.
[0030]
[0031] In formula (1-1), R A represents a hydrogen atom or an alkyl group. The alkyl group may be linear, branched, or cyclic, and is preferably linear. The alkyl group preferably has 1 to 5 carbon atoms, more preferably 1 to 3 carbon atoms, and even more preferably 1 carbon atom. R A is preferably a hydrogen atom in that the effects of the present invention are more excellent.
[0032] In formula (1-1), X 1 ~X 5 are each independently -CR Ar = or represents a nitrogen atom. ArR each independently represents a hydrogen atom or a substituent. Examples of the substituent include an alkyl group, an alkoxy group, an alkyloxycarbonyl group, a halogen atom, and the above-mentioned interactive group. Ar Among these, a hydrogen atom, an alkyl group, an alkoxy group, an alkyloxycarbonyl group, a carboxy group, or a hydroxy group is preferred, and a hydrogen atom or an alkyl group is more preferred. The alkyl group may be linear, branched, or cyclic, and linear or branched is preferred. The number of carbon atoms in the alkyl group is preferably 1 to 12, more preferably 1 to 8, and even more preferably 1 to 3. The alkyl group contained in the alkoxy group and alkyloxycarbonyl group may be linear, branched, or cyclic, and branched or cyclic is preferred. The number of carbon atoms in the alkyl group contained in the alkoxy group and alkyloxycarbonyl group is preferably 1 to 12, more preferably 3 to 10, and even more preferably 3 to 5. X 1 ~X 5 At least three of them are -CR Ar Preferably, at least three of them represent -CH= and the rest represent -CR Ar It is more preferred that the aryl group is a nitrogen atom.
[0033] As the aromatic vinyl monomer, a compound represented by the following formula (1) or vinylpyridine is more preferred.
[0034]
[0035] In formula (1), R 1 represents a hydrogen atom or a methyl group, and preferably a hydrogen atom. 2 ~R 6each independently represents a hydrogen atom, an alkyl group, an alkoxy group, an alkyloxycarbonyl group, a carboxy group, or a hydroxy group. The alkyl group may be linear, branched, or cyclic, and is preferably linear or branched. The alkyl group preferably has 1 to 12 carbon atoms, more preferably 1 to 8, and even more preferably 1 to 3. The alkyl group contained in the alkoxy group and alkyloxycarbonyl group may be linear, branched, or cyclic, and is preferably branched or cyclic. The alkyl group contained in the alkoxy group preferably has 1 to 12 carbon atoms, more preferably 3 to 10, and even more preferably 3 to 5. R 2 ~R 6 are each independently preferably a hydrogen atom or an alkyl group, more preferably a hydrogen atom. 2 ~R 6 It is preferable that four or more of R 2 ~R 6 is preferably a hydrogen atom.
[0036] Examples of the aromatic vinyl monomer represented by formula (1) include styrene, α-methylstyrene, p-octylstyrene, p-hexylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, p-t-butylstyrene, 2,4,6-trimethylstyrene, p-methoxystyrene, p-t-butoxystyrene, p-ethoxystyrene, o-hydroxystyrene, m-hydroxystyrene, p-hydroxystyrene, p-carboxystyrene (4-vinylbenzoic acid), p-(t-butoxycarbonyl)styrene (4-vinylbenzoate t-butyl), and p-methoxystyrene. Of these, styrene, p-hexylstyrene, p-t-butoxystyrene, p-hydroxystyrene, p-carboxystyrene, or p-(t-butoxycarbonyl)styrene is preferred, styrene or p-hexylstyrene is more preferred, and styrene is even more preferred.
[0037] Examples of aromatic vinyl monomers other than the compound represented by (1) above include styrene derivatives such as p-chlorostyrene, m-chlorostyrene, p-bromostyrene, p-iodostyrene, and p-cyanostyrene, 2-vinylnaphthalene, 1-vinylnaphthalene, β-methyl-1-vinylnaphthalene, 9-vinylanthracene, and vinylpyridine, with 2-vinylnaphthalene or vinylpyridine being preferred, and vinylpyridine being more preferred.
[0038] Other aromatic monomers include, for example, phenyl (meth)acrylate, naphthyl (meth)acrylate, and benzyl (meth)acrylate.
[0039] The polymer may have one type of repeating unit derived from an aromatic monomer alone, or may have two or more types in combination, but preferably has one type alone. The content of the repeating units derived from the aromatic monomer is preferably 25% by mass or more, more preferably 75% by mass or more, and even more preferably 90% by mass or more, based on the total repeating units of the polymer. The upper limit is not particularly limited and may be 100% by mass. The content of the repeating units derived from a monomer selected from the group consisting of an aromatic vinyl monomer represented by formula (1) and vinylpyridine is preferably 50% by mass or more, more preferably 75% by mass or more, and even more preferably 90% by mass or more, based on the total repeating units of the polymer. The upper limit is not particularly limited and may be 100% by mass. In particular, the content of the repeating units derived from styrene is preferably 50% by mass or more, more preferably 75% by mass or more, and even more preferably 90% by mass or more, based on the total repeating units of the polymer. The upper limit is not particularly limited and may be 100% by mass.
[0040] <Other Repeating Units> The polymer may have other repeating units besides the repeating units derived from aromatic monomers. Examples of other repeating units include repeating units derived from monomers that do not contain an aromatic group, and specific examples include repeating units derived from (meth)acrylic acid, repeating units derived from (meth)acrylamide, and repeating units derived from (meth)acrylic acid alkyl esters. The number of carbon atoms in the alkyl group of the (meth)acrylic acid alkyl ester is preferably 1 to 12, more preferably 1 to 8. The alkyl group may have a substituent. Examples of the substituent include the above-mentioned interactive group and a halogen atom. When the alkyl group has a halogen atom, the alkyl group may be, for example, a perfluoroalkyl group. Examples of (meth)acrylic acid alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-(perfluorohexyl)ethyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, 1-methylcyclopentyl (meth)acrylate, 2-ethyladamantyl (meth)acrylate, 2-(adamantan-1-yl)propyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 3-hydroxyadamantyl (meth)acrylate, and 3-glycidylpropyl (meth)acrylate.
[0041] Examples of monomers that provide repeating units other than those mentioned above include propene, butene, pentene, vinylcyclopentane, vinylcyclohexane, cyclopentene, cyclohexene, 4-hydroxy-1-butene, and vinyl glycidyl ether.
[0042] The other repeating units may be used alone or in combination of two or more. The content of the other repeating units is preferably 0.1 to 80 mass%, more preferably 1 to 50 mass%, and even more preferably 1 to 10 mass%, based on the total repeating units of the polymer.
[0043] The polymer can be synthesized according to a known method. Examples include radical polymerization and anionic polymerization, with anionic polymerization being preferred because it is easy to introduce an interactive group into the terminal of the polymer. A method for synthesizing a polymer having an interactive group at its terminal includes, for example, a method in which anionic polymerization is performed using a compound having an interactive group or a functional group convertible into an interactive group as a terminator, and then, if necessary, converting the functional group derived from the terminator. A method for synthesizing a polymer having an interactive group in its side chain includes, for example, a method in which a monomer having an interactive group or a functional group convertible into an interactive group is polymerized, and then, if necessary, converting the functional group.
[0044] The degree of polymerization of the polymer is preferably 10 to 100, more preferably 20 to 80, and even more preferably 30 to 70. The number average molecular weight (Mn) of the polymer is preferably 500 to 50,000, more preferably 2,000 to 15,000, and even more preferably 3,000 to 10,000. The weight average molecular weight (Mw) of the polymer is preferably 1,000 to 70,000, more preferably 2,000 to 20,000, and even more preferably 3,000 to 10,000. The polydispersity index (Mw / Mn, PDI) of the polymer is preferably 5.0 or less, more preferably 2.0 or less, even more preferably 1.5 or less, and particularly preferably 1.3 or less. The lower limit is usually 1.0, and preferably 1.05 or more.
[0045] The polymer may be used alone or in combination of two or more. The content of the polymer is preferably 0.01 to 10% by mass, more preferably 0.1 to 5% by mass, and even more preferably 0.5 to 3.0% by mass, based on the total mass of the composition. The content of the polymer is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 93% by mass or more, based on the total mass of all components in the composition excluding the solvent. The upper limit is less than 100% by mass, and preferably 99.9999% by mass or less.
[0046] [Aromatic Monomer] The present composition contains an aromatic monomer. The definition and preferred embodiments of the aromatic monomer contained in the present composition are the same as those of the aromatic monomer constituting the repeating unit contained in the above-mentioned polymer. As the aromatic monomer, an aromatic vinyl monomer is preferred, the compound represented by the above-mentioned formula (1-1) is more preferred, the compound represented by the above-mentioned formula (1) or vinylpyridine is even more preferred, and styrene is particularly preferred. The aromatic monomer constituting the repeating unit contained in the above-mentioned polymer and the aromatic monomer contained in the present composition may be the same or different, but are preferably the same in terms of high affinity between the polymer and the monomer and easy formation of a denser film.
[0047] The aromatic monomer may be used alone or in combination of two or more. The aromatic monomer content is preferably 0.1 ppm by mass or more, more preferably 1 ppm by mass or more, and even more preferably 10 ppm by mass or more, relative to the polymer content, in order to achieve better effects of the present invention. The aromatic monomer content is preferably 100,000 ppm by mass or less, more preferably 50,000 ppm by mass or less, and even more preferably 10,000 ppm by mass or less, relative to the polymer content, in order to form a coating with better heat resistance. The heat resistance refers to the property of the coating formed using the composition, in which the components that form the coating are difficult to remove under high-temperature conditions (e.g., 200°C). Since the coating is exposed to high-temperature conditions during ALD processing, excellent heat resistance is preferable, in order to prevent contamination of the ALD processing equipment and to suppress deterioration of the coating, thereby ensuring stable ALD inhibition. When the aromatic monomer content in the present composition satisfies the above range, the amount of aromatic monomer removed during heat treatment is reduced, resulting in better heat resistance. The aromatic monomer content can be determined by known methods such as gas chromatography and liquid chromatography.
[0048] [Solvent] The present composition contains a solvent. Examples of the solvent include water and organic solvents, with organic solvents being preferred. Examples of the organic solvent include alcohol-based solvents, ether-based solvents, ester-based solvents, ketone-based solvents, amide-based solvents, sulfur-containing solvents, and hydrocarbon-based solvents.
[0049] Examples of alcohol-based solvents include monoalcohol-based solvents, polyol-based solvents, and glycol monoether-based solvents. Examples of monoalcohol-based solvents include aliphatic monoalcohol-based solvents having 1 to 18 carbon atoms, such as methanol, ethanol (EtOH), 1-propanol, 2-propanol, 2-butanol, isobutyl alcohol, tert-butyl alcohol, isopentyl alcohol, and 4-methyl-2-pentanol (methyl isobutyl carbinol); alicyclic monoalcohol-based solvents having 3 to 18 carbon atoms, such as cyclohexanol; aromatic monoalcohol-based solvents, such as benzyl alcohol; and ketone monoalcohol-based solvents, such as diacetone alcohol. Examples of polyol-based solvents include glycol-based solvents having 2 to 18 carbon atoms, such as ethylene glycol, propylene glycol (1,2-propanediol), 1,3-propanediol, diethylene glycol, and dipropylene glycol. Examples of glycol monoether solvents include glycol monoether solvents having 3 to 19 carbon atoms, such as propylene glycol monomethyl ether (PGME), ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol monoisopropyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol monobutyl ether, 1-methoxy-2-propanol, 2-methoxy-1-propanol, 1-ethoxy-2-propanol, 2-ethoxy-1-propanol, propylene glycol mono-n-propyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, tripropylene glycol monoethyl ether, tripropylene glycol monomethyl ether, ethylene glycol monobenzyl ether, and diethylene glycol monobenzyl ether.The alcohol solvent preferably has 1 to 19 carbon atoms, more preferably 2 to 12 carbon atoms, and even more preferably 3 to 8 carbon atoms.
[0050] Examples of ether solvents include dialkyl ether solvents such as diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, t-butyl methyl ether, dihexyl ether, and cyclohexyl methyl ether; cyclic ether solvents such as tetrahydrofuran and tetrahydropyran; anisole; and diphenyl ether.
[0051] Examples of ester solvents include glycol ester solvents, monocarboxylic acid ester solvents such as n-butyl acetate and ethyl lactate, lactone solvents such as γ-butyrolactone (GBL) and δ-valerolactone, and carbonate solvents such as dimethyl carbonate, diethyl carbonate, ethylene carbonate, and propylene carbonate. Examples of glycol ester solvents include glycol dicarboxylate solvents having 6 to 22 carbon atoms such as ethylene glycol diacetate, diethylene glycol diacetate, triethylene glycol diacetate, tetraethylene glycol diacetate, propylene glycol diacetate, dipropylene glycol diacetate, and methoxybutyl acetate, as well as propylene glycol monomethyl ether acetate (PGMEA), ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, and propylene glycol monomethyl ether acetate. Examples of the ester-based solvent include glycol monoether carboxylate solvents having 5 to 21 carbon atoms, such as ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, tetraethylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monobutyl ether acetate, dipropylene glycol monomethyl ether acetate, tripropylene glycol monomethyl ether acetate, tetrapropylene glycol monomethyl ether acetate, and butylene glycol monomethyl ether acetate. The number of carbon atoms in the ester-based solvent is preferably 3 to 22, and more preferably 4 to 12.
[0052] Examples of hydrocarbon solvents include aliphatic hydrocarbon solvents such as n-pentane and n-hexane, alicyclic hydrocarbon solvents such as cyclohexane and methylcyclohexane, and aromatic hydrocarbon solvents such as toluene and xylene.
[0053] Examples of ketone solvents include chain ketone solvents such as methyl isobutyl ketone, acetone, methyl ethyl ketone, diethyl ketone, methyl-n-butyl ketone, 2-heptanone, ethyl-n-butyl ketone, methyl-n-ketone, diisobutyl ketone, and trimethylnonane; cyclic ketone solvents such as cyclohexanone, cyclopentanone, cycloheptanone, and methylcyclohexanone; and acetophenone.
[0054] Examples of amide solvents include formamide, monomethylformamide, dimethylformamide, acetamide, monomethylacetamide, dimethylacetamide, monoethylacetamide, diethylacetamide, and N-methylpyrrolidone.
[0055] Examples of sulfur-containing solvents include dimethyl sulfone, dimethyl sulfoxide, and sulfolane.
[0056] The solvent is preferably an alcohol solvent, an ether solvent, an ester solvent, or a ketone solvent, more preferably an aliphatic monoalcohol solvent, a glycol monoether solvent, a glycol ester solvent, a monocarboxylic acid ester solvent, an ether solvent, or a lactone solvent, and even more preferably a glycol monoether solvent or a glycol ester solvent. Among these, the solvent preferably contains at least one selected from the group consisting of PGMEA, PGME, cyclohexanone, ethyl lactate, methyl isobutyl carbinol, EtOH, and γ-butyrolactone, and more preferably contains at least one selected from the group consisting of PGMEA, PGME, cyclohexanone, ethyl lactate, or methyl isobutyl carbinol. The solvent also preferably contains an ether solvent, more preferably diethyl ether or tetrahydrofuran.
[0057] The solvent may be used alone or in combination of two or more. The content of the solvent is preferably 90.00% by mass or more, more preferably 95.00% by mass or more, and even more preferably 97.00% by mass or more, based on the total mass of the composition. The upper limit is less than 100% by mass, preferably 99.999% by mass or less, more preferably 99.9% by mass or less, and even more preferably 99.0% by mass or less. The content of one solvent in the composition is preferably 90% by mass or more, more preferably 99% by mass or more, and even more preferably 99.9% by mass or more, based on the total mass of all solvents. The upper limit is not particularly limited and may be 100% by mass.
[0058] When the composition contains two or more solvents, it is preferable that at least one of them is an ether-based solvent, and more preferably that at least one of them is tetrahydrofuran or diethyl ether. Furthermore, when the composition contains two or more solvents, it is also preferable that the composition contains at least one ether-based solvent and further contains at least one solvent selected from the group consisting of alcohol-based solvents, ester-based solvents, and ketone-based solvents. The content of the ether-based solvent is preferably 0.01 to 100,000 ppm by mass, more preferably 0.1 to 10,000 ppm by mass, and even more preferably 1.0 to 1,000 ppm by mass, relative to the total mass of all solvents.
[0059] [Other Components] The present composition may contain other components in addition to the polymer, aromatic monomer, and solvent. Examples of such other components include an acid generator, a polymerization inhibitor, and a surfactant. The acid generator is not particularly limited as long as it is a compound that generates an acid upon exposure to light or heating, and examples thereof include onium salt compounds, N-sulfonyloxyimide compounds, halogen-containing compounds, diazomethane compounds, sulfone compounds, sulfonate ester compounds, carboxylate ester compounds, phosphate ester compounds, and sulfonebenzotriazole compounds. Examples of polymerization inhibitors include phenolic compounds, quinone compounds, free radical compounds, amine compounds, and phosphine compounds. Examples of surfactants include cationic surfactants, anionic surfactants, and nonionic surfactants. As the surfactant, the compounds described in paragraphs
[0092] to
[0096] of JP-A-2015-158662, paragraphs
[0045] to
[0046] of JP-A-2012-151273, and paragraphs
[0014] to
[0020] of JP-A-2009-147389 can also be used, the contents of which are incorporated herein by reference.
[0060] The total content of the polymer and aromatic monomer is preferably 0.005% by mass or more, more preferably 0.01% by mass or more, and even more preferably 0.1% by mass or more, based on the total mass of the composition. The upper limit is often less than 15.0% by mass, preferably less than 10.0% by mass, and more preferably less than 5.0% by mass. The total content of the polymer and aromatic monomer is preferably 95.0% by mass or more, more preferably 99.0% by mass or more, and even more preferably 99.9% by mass or more, based on the total mass of all components in the composition excluding the solvent. The upper limit is not particularly limited, and is 100% by mass.
[0061] [Method for producing the present composition] The method for producing the present composition is not particularly limited, and the composition can be produced, for example, by mixing the above-mentioned components. The order or timing of mixing the components is not particularly limited, and the composition can be produced, for example, by adding the polymer and aromatic monomer to a stirrer such as a mixer containing a purified solvent, and then thoroughly stirring. In order to achieve better effects of the present invention, it is preferable that the raw materials for the present composition (e.g., the solvent, the polymer, and the aromatic monomer) have been subjected to a purification treatment.
[0062] The production process of the present composition may include a step selected from the group consisting of a distillation step of distilling raw materials, a dehydration step of dehydrating the present composition, a metal removal step of removing metal components from the present composition, a filtration step of filtering the present composition, and a destaticization step of destaticizing the present composition.
[0063] This composition can be filled into a known container for storage, transportation, and use. As a container, a container with a high degree of cleanliness within the container for semiconductor applications and which suppresses the elution of impurities from the inner wall of the container's storage section into each liquid is preferred. Examples of such containers include various containers commercially available as containers for semiconductor processing liquids, such as the "Clean Bottle" series manufactured by Aicello Chemical Co., Ltd. and the "Pure Bottle" manufactured by Kodama Resin Industry Co., Ltd., but are not limited to these. Furthermore, the containers exemplified in paragraphs
[0121] to
[0124] of WO 2022 / 004217 can also be used as containers, and the contents of these containers are incorporated herein.
[0064] [Uses of the composition] The composition is a composition for semiconductor device treatment and is preferably used for modifying a substrate in the manufacturing process of a semiconductor device. The above treatment results in a modified substrate having a coating formed on the substrate surface. The composition is also preferably used for manufacturing a laminate in which a material is deposited in the region where no coating is formed by the above treatment, by subjecting the modified substrate to an ALD treatment. Methods for manufacturing a modified substrate and a laminate will be described in detail below.
[0065] <Substrate> The substrate is not particularly limited, but preferably has at least one of a metal surface A made of a material containing metal atoms and a non-metal surface B made of a non-metal material, and more preferably has a metal surface A.
[0066] The metal atoms contained in the metal surface A are not particularly limited, but are preferably tungsten atoms, copper atoms, ruthenium atoms, cobalt atoms, titanium atoms, tantalum atoms, molybdenum atoms, germanium atoms, zirconium atoms, aluminum atoms, tin atoms, nickel atoms, palladium atoms, indium atoms, zinc atoms, gold atoms, silver atoms, or platinum atoms, more preferably tungsten atoms, ruthenium atoms, tantalum atoms, copper atoms, or cobalt atoms, and even more preferably tungsten atoms or copper atoms. The form of the metal atoms in the metal surface A is not particularly limited, but includes elemental metals, alloys, nitrides, oxides, and silicides, with elemental metals or alloys being preferred. Examples of alloys include alloys containing two or more of the metal atoms contained in the metal surface A described above. The method for forming the metal surface A is not particularly limited, and known methods can be used. For example, CVD, plating, and physical vapor deposition methods can be used.
[0067] Examples of non-metallic materials constituting the non-metallic surface B include insulators, such as non-metallic elements such as silicon and carbon, non-metallic oxides such as silicon oxide, non-metallic nitrides such as silicon nitride, non-metallic oxynitrides such as silicon oxynitride, and organic materials. The material constituting the non-metallic surface B is preferably a non-metallic material containing silicon atoms, more preferably silicon oxide. Specific examples of silicon oxide include SiO y (wherein y is preferably 0.5 to 2.0, more preferably 1.0 to 2.0), and SiO z C w (wherein z is preferably 0.5 to 2.0, more preferably 1.0 to 2.0, and w is preferably 0.5 to 2.0, more preferably 1.0 to 2.0). y and SiO z C wThe material represented by the composition may further contain hydrogen. z C w Examples of the material represented by the composition include Si(OC 2 H 5 ) 4 (tetraethyl orthosilicate, TEOS). Silicon oxides include SiO 2 A material represented by the formula (silicon dioxide) or TEOS is preferred.
[0068] The method for forming the non-metallic surface B is not particularly limited, and examples thereof include CVD, physical vapor deposition, plasma irradiation, and application of a precursor compound. It is also preferable that the non-metallic surface B is a surface treatment performed on a region made of silicon oxide. Examples of the treatment include contact with a treatment liquid such as an aqueous solution containing an acidic compound (preferably hydrogen fluoride water), plasma treatment, corona treatment, and ozone treatment.
[0069] It is also preferable that the substrate has at least two types of surfaces, a first surface and a second surface, which are made of different materials. The first surface is a surface that interacts with the interactive group of the polymer. The second surface may be made of a material different from the first surface, but is preferably a surface on which no coating is formed when it comes into contact with the composition. In particular, it is preferable that at least one of the first surface and the second surface is a metal surface A or a non-metal surface B, and it is more preferable that at least one of the first surface and the second surface is a metal surface A.
[0070] A preferred embodiment of the substrate is embodiment 1, in which the first surface is a metal surface A. In embodiment 1, the interactive group possessed by the polymer is the interactive group A described above. In embodiment 1, the metal atoms contained in the metal surface A, which is the first surface, are preferably contained in the form of a metal element, an alloy, a conductive metal nitride, or a metal silicide, and more preferably a metal element or an alloy. Examples of the metal element and alloy include the metal elements and alloys thereof exemplified as the metals contained in the metal surface A. Examples of the conductive metal nitride include tantalum nitride, titanium nitride, iron nitride, and aluminum nitride. Examples of the metal silicide include iron silicide, molybdenum silicide, and tungsten silicide.
[0071] In Aspect 1, the second surface is preferably a metal surface A or a non-metal surface B different from the first surface, more preferably a non-metal surface B. In Aspect 1, the metal atoms contained in the metal surface A constituting the second surface are preferably in the form of a metal oxide, a metal nitride, or a metal oxynitride, more preferably a metal oxide. Examples of metal oxides include aluminum oxide, tantalum oxide, iron oxide, and copper oxide.
[0072] A preferred embodiment of the substrate also includes embodiment 2, in which the first surface is a non-metallic surface B. In embodiment 2, the interactive group possessed by the polymer is the above-described interactive group B. In embodiment 2, the second surface is preferably a metallic surface A. In embodiment 2, the metal atoms contained in the metallic surface A, which is the second surface, are preferably contained in the form of an elemental metal, an alloy, a conductive metal nitride, or a metal silicide, and more preferably in the form of an elemental metal or an alloy.
[0073] The shape of the first surface and the second surface is not particularly limited, and examples thereof include a planar shape, a dotted shape, and a striped shape.
[0074] The shape of the substrate is not particularly limited, and any shape of substrate generally used as a semiconductor substrate can be used. The substrate may be a substrate having the above-described surface, and may be a single-layer or multi-layer structure.
[0075] <Coating> The coating formed on a substrate using the present composition is a coating containing components other than the solvent contained in the composition (e.g., a polymer and an aromatic monomer). The coating preferably functions as a mask when depositing a material in an ALD process. That is, when an ALD process is performed on a modified substrate having a coating formed using the present composition on a specific region, the material preferably does not deposit in the region where the coating is formed, but deposits in the region where the coating is not formed, forming a film (hereinafter also referred to as an "ALD film"). This results in a laminate in which an ALD film is selectively formed in regions other than the region where the coating is formed.
[0076] The coating also preferably functions as a mask when forming a metal-containing film by chemical vapor deposition (CVD) other than ALD. That is, in a CVD process, deposition of a film by CVD (hereinafter also referred to as a "CVD film") can be suppressed in the region where the coating is formed, and a CVD film can be deposited in the region where the coating is not formed. This results in a laminate in which a CVD film is selectively formed in the region other than the region where the coating is formed. Examples of CVD other than ALD that can be preferably applied to the modified substrate include known methods such as thermal CVD and plasma CVD. As raw materials for the CVD film used in the CVD process, raw materials for the ALD film described below can be used.
[0077] The thickness of the coating is preferably 0.1 to 100.0 nm, more preferably 0.5 to 50.0 nm, and even more preferably 3.0 to 30.0 nm.
[0078] In order to obtain superior effects of the present invention, the water contact angle of the coating is preferably 60° or more, more preferably 80° or more, and even more preferably 90° or more. There is no particular upper limit, and it is often 120° or less. The water contact angle is the average value of three measurements of the contact angle 500 milliseconds after a water droplet contacts the surface of the measurement object using a contact angle meter (DMs-501, manufactured by Kyowa Interface Science Co., Ltd.).
[0079] [Method for producing a modified substrate] The method for producing a modified substrate of the present invention includes a step of contacting a substrate with the present composition to form a coating on the substrate. This results in a modified substrate having a coating formed on the substrate. The method for contacting the substrate with the present composition is not particularly limited, and known methods can be used. Examples include a method of applying (e.g., spin coating) or spraying the present composition onto the substrate, and a method of immersing the substrate in the present composition. When immersing the substrate in the present composition, the present composition may be subjected to convection. The temperature of the present composition when contacting the substrate with the present composition is not particularly limited, but is preferably 0 to 50°C, more preferably 10 to 30°C.
[0080] It is also preferable to heat-treat the coating film after contacting the substrate with the composition. Heat treatment promotes interaction (e.g., bond formation) between the substrate surface and the interactive groups of the polymer. The heating method is not particularly limited, and known methods can be used, such as an oven or a hot plate. The heating temperature is preferably 50 to 400°C, more preferably 100 to 350°C, even more preferably 130 to 300°C, and particularly preferably 150 to 250°C. The heating time is preferably 10 seconds to 60 minutes, more preferably 1 minute to 30 minutes, and even more preferably 3 minutes to 10 minutes.
[0081] It is also preferable to perform a rinsing treatment after contacting the substrate with the present composition. The rinsing treatment can remove the present composition and / or impurities adhering to regions on the substrate other than the desired region (e.g., the region that interacts with the interactive group contained in the polymer) from the substrate. The rinsing method is not particularly limited, and examples include a method of contacting the substrate with a rinsing liquid. As the contacting method, the same method as the method of contacting the present composition with the substrate can be used. The temperature of the rinsing liquid during contact is not particularly limited, but is preferably 0 to 50°C, more preferably 10 to 30°C. As the rinsing liquid, a known organic solvent can be used, such as the alcohol-based solvents, ether-based solvents, and ester-based solvents described above. It is also preferable to use the solvent contained in the present composition as the rinsing liquid.
[0082] [Method for Producing Laminate] The method for producing a laminate of the present invention includes step 1 of contacting a substrate having at least two surfaces, a first surface and a second surface, each made of a different material (hereinafter also referred to as a "specific substrate") with the present composition to form a first coating on the first surface, and step 2 of subjecting the substrate obtained in step 1 to an ALD treatment to form a second coating on the second surface. This results in a laminate having a second coating (ALD film) on the second surface.
[0083] [Step 1: Method for producing modified substrate] Step 1 is a step of bringing a specific substrate into contact with the present composition to form a first coating on the first surface. Step 1 results in a modified substrate 1 having a first coating formed on the first surface of the specific substrate. The first coating is a coating containing a polymer contained in the present composition and an aromatic monomer. The method for bringing the specific substrate into contact with the present composition is not particularly limited, and the method of bringing the present composition into contact with a substrate in the above-mentioned method for producing a modified substrate can be used.
[0084] It is also preferable to heat-treat the coating film after contacting the specific substrate with the composition. Heat treatment promotes interaction (e.g., bond formation) between the first surface and the interactive group of the polymer. The heating method is not particularly limited, and the heating method described in the above-mentioned method for producing a modified substrate can be used.
[0085] It is also preferable to perform a rinse treatment on the modified substrate 1 having the first coating formed on the first surface. The rinse treatment can remove the composition and / or impurities adhering to regions other than the first surface (e.g., the second surface) of the specific substrate from the specific substrate. The rinse method can be the same as the rinse method in the method for producing a modified substrate described above.
[0086] [Step 2: ALD Treatment] Step 2 is a step of subjecting the modified substrate 1 obtained in step 1 to ALD treatment to form a second coating on the second surface. Step 2 results in a laminate 1 having a first coating formed on the first surface and a second coating formed on the second surface. The second coating is a film formed by ALD treatment (ALD film). Note that the modified substrate 1 may be any substrate having a first coating formed on the first surface of the specific substrate in step 1, and may be subjected to the above-mentioned heating treatment, rinsing treatment, etc. after step 1.
[0087] The ALD treatment method is not particularly limited, and known methods can be used. For example, a method can be used in which a precursor gas serving as a raw material for the ALD film is supplied to the surface of the modified substrate 1, and then the raw material is decomposed and / or chemically reacted with an oxidizing agent or the like to deposit the material, thereby forming an ALD film. The precursor is not particularly limited, and known precursors can be used depending on the type of ALD film to be formed, such as organometallic compounds. Examples of precursors that can be used include compounds described in paragraphs
[0021] to
[0025] of JP 2022-080800 A. The oxidizing agent is not particularly limited, and known oxidizing agents used in ALD treatments can be used, such as water, oxygen, and ozone.
[0088] The materials constituting the ALD film can be controlled by the type of precursor supplied, the supply atmosphere, the oxidizing agent, etc. The materials of the formed ALD film are not particularly limited, and include metals, metal oxides, and metal nitrides. Examples of metals include aluminum, titanium, chromium, iron, cobalt, nickel, copper, zinc, yttrium, zirconium, niobium, molybdenum, ruthenium, palladium, lanthanum, cerium, hafnium, tantalum, tungsten, platinum, and bismuth. Examples of metal oxides include aluminum oxide, titanium oxide, zinc oxide, zirconium oxide, hafnium oxide, and tantalum oxide. Examples of metal nitrides include titanium nitride and tantalum nitride. In the ALD process, a treatment for modifying the surface of the region where the first coating is not formed may be performed.
[0089] After the ALD process, the thickness of the material deposited on the first coating is preferably as thin as possible, and is preferably 4.0 nm or less, more preferably 2.0 nm or less, and even more preferably 1.0 nm or less. The lower limit is 0 nm, and may be 0 nm. The ratio of the thickness of the material deposited on the region where the first coating is formed to the thickness of the second coating is preferably 0.75 or less, more preferably 0.5 or less, and even more preferably 0.25 or less. The lower limit of the ratio is 0 or more, and may be 0.
[0090] [Step 3: Removal of Coating] The method for producing a laminate of the present invention may include, after step 2, step 3 of removing the first coating formed on the first surface in step 1. Step 3 results in a laminate 2 that has no coating on the first surface and has the second coating on the second surface.
[0091] The method for removing the first coating is not particularly limited, and examples thereof include dry etching, wet etching, and a combination thereof. Known methods can be used for dry etching, such as chemical dry etching, which supplies reactive ions or reactive radicals to the surface of the laminate 1, and physical dry etching, such as sputter etching and ion beam etching. Wet etching can be performed by supplying an etching solution to the laminate 1. Examples of the etching solution include etching solutions containing oxidizing agents such as ozone and hydrofluoric acid, and etching solutions containing an organic solvent. Examples of the organic solvent include the organic solvents contained in the above-mentioned chemical solutions, and alcohol-based solvents, ester-based solvents, ketone-based solvents, or hydrocarbon-based solvents are preferred. Among these, chemical dry etching or wet etching is preferred.
[0092] The present invention will be described in more detail below based on examples. The materials, amounts used, ratios, treatment details, and treatment procedures shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the examples shown below. The preparation, filling, storage, etc. of the composition were all carried out in a clean room meeting ISO Class 2 or lower. Furthermore, the containers used for the preparation, filling, storage, etc. of the composition were washed with the solvent used in the preparation or the prepared composition before use.
[0093] [Preparation of the Composition] [Polymer] Polymer P-1 was synthesized as follows. After drying the flask reaction vessel under reduced pressure, 240 g of tetrahydrofuran (THF) that had been subjected to distillation and dehydration treatment was poured into the flask under a nitrogen atmosphere and cooled to -78°C. Subsequently, 4.60 mL of a 1 N cyclohexane solution of sec-butyllithium (sec-BuLi) was poured into the THF. Subsequently, 26.6 mL of styrene that had been subjected to adsorption filtration with silica gel and distillation and dehydration treatment to remove the polymerization inhibitor was poured dropwise over 60 minutes, taking care not to raise the internal temperature of the reaction solution above -60°C, and the mixture was then stirred for 90 minutes. Next, 0.64 mL of chloro-N,N-diethylaminopropane was poured into the reaction vessel to carry out a termination reaction of the polymerization terminals. The reaction solution was then warmed to room temperature, concentrated, and substituted with methyl isobutyl ketone (MIBK). Subsequently, 400 g of ultrapure water was poured into the reaction vessel and stirred, and the lower aqueous layer was removed. This operation was repeated six times to remove the lithium salt, and then the solution was concentrated and added dropwise to 400 g of methanol to precipitate a polymer, and the solid was recovered using a Buchner funnel. The resulting solid was made into a 50 wt % solution of MIBK, and the solution was added dropwise to 400 g of methanol to precipitate a polymer, and the solid was recovered using a Buchner funnel. This polymer was dried under reduced pressure at 60°C to obtain 19.6 g of white polymer P-1.
[0094] Polymers other than polymer P-1 were synthesized according to the synthesis method of polymer P-1, while adjusting the types and amounts of monomers and end-terminators, and reaction conditions, so as to obtain the polymers shown below.
[0095] The structure and polydispersity of each polymer used in the compositions of the Examples and Comparative Examples are shown below. The numerical value attached to the bottom right of each repeating unit represents the degree of polymerization of that repeating unit. The polydispersity and degree of polymerization of each polymer were obtained by GPC measurement under the conditions described above. In polymer P-5, the content of repeating units derived from 4-t-butoxystyrene relative to all repeating units was 30 mol %, and the content of repeating units derived from styrene was 70 mol %. In polymer P-11, the content of repeating units derived from t-butyl 4-vinylbenzoate relative to all repeating units was 50 mol %, and the content of repeating units derived from 4-vinylbenzoic acid was 50 mol %. In polymer P-13, the content of repeating units derived from 4-t-butoxystyrene was 60 mol % and the content of repeating units derived from styrene was 40 mol % relative to all repeating units.In polymer P-16, the content of repeating units derived from 4-t-butoxystyrene was 60 mol % and the content of repeating units derived from 2-(perfluorohexyl)ethyl acrylate was 40 mol % relative to all repeating units.Polymer P-5, polymer P-11, polymer P-13, and polymer P-16 were all random copolymers.
[0096]
[0097]
[0098]
[0099] [Aromatic Monomer]
[0100]
[0101] [Solvent] PGMEA: Propylene glycol monomethyl ether acetate PGME: Propylene glycol monomethyl ether GBL: γ-butyrolactone EtOH: Ethanol
[0102] [Liquid Preparation] The polymer synthesized by the method described above, an aromatic monomer, and a solvent were mixed to obtain the composition shown in Table 1, thereby preparing the compositions of each of the Examples and Comparative Examples.
[0103] [Preparation of Modified Substrates] A W-layer wafer was prepared by forming a tungsten layer on one surface of a commercially available silicon wafer (12 inches in diameter) by CVD, and a Cu-layer wafer was prepared by forming a Cu layer on one surface by sputtering. The film formation conditions were adjusted so that the thickness of the W layer and Cu layer was 20 nm, respectively. The silicon wafer, W-layer wafer, and Cu-layer wafer were cut into 2 cm squares and cleaned by immersion in isopropyl alcohol (IPA). Cleaning was performed while stirring the IPA at a stirring speed of 250 rpm, at an IPA temperature of 25°C, and for 30 seconds. After cleaning, the wafers were dried by spraying with nitrogen gas. The W-layer wafer was a substrate having a metal surface A with tungsten atoms as the metal atoms, the Cu-layer wafer was a substrate having a metal surface A with copper atoms as the metal atoms, and the silicon wafer (Si substrate) was a substrate having a non-metal surface B with silicon oxide.
[0104] Next, each of the cleaned wafers was immersed in each of the compositions to perform a modification treatment. The immersion was performed while stirring the composition at a stirring speed of 250 rpm, with the composition temperature at 25°C and the immersion time at 10 minutes. After the immersion, each wafer was immersed in IPA to perform a rinse treatment. The rinsing treatment was performed while stirring the IPA at a stirring speed of 250 rpm, with the IPA temperature at 25°C and the rinsing time at 30 seconds. After the rinsing, the wafer was dried by spraying nitrogen gas onto it. A modified substrate was obtained by the above procedure.
[0105] [Evaluation] [Evaluation of ALD Inhibition] Each modified substrate obtained in [Preparation of Modified Substrate] and a substrate (unmodified substrate) before being immersed in each composition were subjected to ALD using an atomic layer deposition apparatus (AD-230LP, manufactured by Samco). 2 O 3) layer (ALD film). Trimethylaluminum was used as the organometallic source and water as the oxidizing agent, and the ALD treatment temperature was 200°C. Other conditions were adjusted so that the ALD film formed on the unmodified substrate would have a thickness of 5 nm. The thickness of the ALD film for each sample after the ALD treatment was measured using an X-ray fluorescence (XRF) analyzer (AZX400, manufactured by Rigaku Corporation). Measurements were performed at five points on the substrate, and the average value was taken as the film thickness. The ALD inhibitory properties were evaluated from the obtained film thickness according to the following evaluation criteria. The smaller the film thickness, the less likely a film formed by the ALD treatment will deposit on the coating formed by the composition, i.e., the better the ALD inhibitory properties. ALD inhibitory properties of C or higher are preferred.
[0106] S: The thickness of the ALD film is less than 1.0 nm. A: The thickness of the ALD film is 1.0 nm or more and less than 1.5 nm. B: The thickness of the ALD film is 1.5 nm or more and less than 2.0 nm. C: The thickness of the ALD film is 2.0 nm or more and less than 2.5 nm. D: The thickness of the ALD film is 2.5 nm or more.
[0107] [Evaluation of Heat Resistance] Each modified substrate was heated at 200°C for 15 minutes under vacuum conditions, and the weight was measured before and after heating. From the weight loss before and after heating, the weight loss rate (%) relative to the weight of the coating before heating was calculated (weight loss rate (%) = weight loss before and after heating / weight of coating before heating × 100). The above measurement was performed three times, and the arithmetic average of these was taken as the weight loss rate (%), and the heat resistance was evaluated according to the following evaluation criteria. Heat resistance of C or higher is preferred.
[0108] (Evaluation Criteria) S: The weight loss rate is less than 1.0%. A: The weight loss rate is 1.0% or more and less than 3.0%. B: The weight loss rate is 3.0% or more and less than 5.0%. C: The weight loss rate is 5.0% or more and less than 8.0%. D: The weight loss rate is 8.0% or more. [Results]
[0109] Tables 1 to 3 show the composition and evaluation results of each composition. In the tables, the "content (mass%)" of the polymer represents the content (unit: mass%) relative to the total mass of the composition. In the tables, the "content (ppm by mass)" of the aromatic monomer represents the content (unit: mass ppm) relative to the polymer content. In the tables, the content of the solvent is the remainder after subtracting the contents of the polymer and aromatic monomer from the total mass of the composition.
[0110]
[0111]
[0112]
[0113] The results in Tables 1 to 3 confirm that the composition of the present invention can form a coating film that has excellent ALD inhibitory properties.
[0114] A comparison of Examples A1 to A3 confirmed that the ALD inhibitory properties and heat resistance were superior when the content of the aromatic monomer in the composition was 1 to 50,000 ppm by mass relative to the content of the polymer. A comparison of Example A4 with Examples A1, A12, and A13 confirmed that the ALD inhibitory properties and heat resistance were superior when the aromatic monomer was at least one selected from the group consisting of a compound represented by Formula (1) and vinylpyridine. A comparison of Example A5 with Example A1 confirmed that the effects of the present invention were superior when the polydispersity of the polymer was 1.0 to 1.5. A comparison of Example A6 with Example A1, and a comparison of Examples A10 to A11 with Example A4 confirmed that the heat resistance was superior when the solvent included at least one selected from the group consisting of propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, cyclohexanone, ethyl lactate, and methyl isobutyl carbinol. Comparison of Example A7 with Example A1 confirmed that when the total content of the polymer and aromatic monomer is 0.1 mass% or more, the ALD inhibitory property and heat resistance are more excellent. Comparison of Example A8 with Example A1 confirmed that when the aromatic monomer is R 1It was confirmed that when the aromatic monomer is a compound represented by formula (1) in which R is a hydrogen atom, the heat resistance is more excellent. 2 ~R 6 is a hydrogen atom or an alkyl group, the ALD inhibitory property and heat resistance are more excellent.
Claims
1. A composition for semiconductor device processing, comprising: a polymer having at least one functional group at the end or side chain of the main chain that interacts with a substrate, and having repeating units derived from an aromatic monomer; an aromatic monomer; and a solvent.
2. The composition for treating a semiconductor device according to claim 1, wherein the polymer is a polymer having repeating units derived from an aromatic vinyl monomer.
3. The composition for treating semiconductor devices according to claim 1 or 2, wherein the content of the aromatic monomer is 1 to 50,000 ppm by mass relative to the content of the polymer.
4. The composition for treating semiconductor devices according to claim 1 or 2, wherein the aromatic monomer comprises at least one selected from the group consisting of a compound represented by formula (1) and vinylpyridine. In formula (1), R 1 represents a hydrogen atom or a methyl group. 2 ~R 6 each independently represents a hydrogen atom, an alkyl group, an alkoxy group, an alkyloxycarbonyl group, a carboxy group, or a hydroxy group.
5. The composition for semiconductor device processing according to claim 1 or 2, wherein the polydispersity of the polymer is from 1.0 to 1.
5.
6. R 1 The composition for treating a semiconductor device of claim 4 , wherein is a hydrogen atom.
7. R 2 ~R 6 The composition for treating a semiconductor device of claim 4 , wherein is a hydrogen atom or an alkyl group.
8. The composition for treating a semiconductor device according to claim 1 or 2, wherein the solvent comprises at least one selected from the group consisting of propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, cyclohexanone, ethyl lactate, and methyl isobutyl carbinol.
9. A composition for treating semiconductor devices as described in claim 1 or 2, wherein the total content of the polymer and the aromatic monomer is 0.1 mass % or more and less than 10 mass % based on the total mass of the composition for treating semiconductor devices.
10. A method for producing a modified substrate comprising the step of contacting a substrate with a composition for treating a semiconductor device according to claim 1 or 2.
11. A method for producing a laminate, comprising: step 1 of contacting a substrate having at least two surfaces, a first surface and a second surface, each of which is made of a different material, with a composition for treating a semiconductor device according to claim 1 or 2 to form a first coating on the first surface; and step 2 of subjecting the substrate obtained in step 1 to an atomic layer deposition process to form a second coating on the second surface.
Citation Information
Patent Citations
Inactivation of reaction sites for vapor deposition
JP2013520028A
Selective deposition process using polymer structure deactivation process
JP2020524402A
Method for forming cover film
WO2018235877A1
Resist composition and resist film
WO2019150966A1
Substrate with film formed thereon
WO2023033146A1