Method for manufacturing thermally conductive sheet
The method of blending thermally conductive fillers and unreacted silicone oil in a thermally conductive resin composition and forming it into a sheet addresses the heat dissipation and flexibility issues in electronic components, resulting in a sheet with enhanced thermal conductivity and flexibility.
Patent Information
- Application Number
- PCT/JP2024/010518
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-03
AI Technical Summary
Thermally conductive sheets used in heat-producing electronic components face challenges in efficiently dissipating heat and maintaining flexibility, especially when mounted on surfaces with steps, as existing materials lack sufficient thermal conductivity and flexibility.
A method involving the preparation of a thermally conductive resin composition by blending a thermally conductive filler, a radical-curable silicone resin, and unreacted silicone oil with a kinematic viscosity of 1×10^-2 m^2/s or more, which is then formed into a sheet and heated and pressurized to enhance thermal conductivity and flexibility.
The method produces a thermally conductive sheet with improved thermal conductivity and flexibility, effectively addressing the heat dissipation challenges in complex electronic components.
Smart Images

Figure JP2024010518_03102024_PF_FP_ABST
Abstract
Description
Manufacturing method of thermally conductive sheet
[0001] The present invention relates to a method for producing a thermally conductive sheet.
[0002] For heat-generating electronic components such as power devices, transistors, thyristors, and CPUs, efficient heat dissipation is an important issue. Conventional heat dissipation strategies include (1) increasing the thermal conductivity of the insulating layer of the printed wiring board on which the heat-generating electronic components are mounted, and (2) attaching the heat-generating electronic components or the printed wiring board on which the heat-generating electronic components are mounted to a heat sink via electrically insulating thermal interface materials. Silicone resin or epoxy resin filled with ceramic powder is commonly used as the insulating layer and thermal interface material for printed wiring boards.
[0003] As a ceramic powder, boron nitride powder has attracted attention due to its properties such as high thermal conductivity, high insulation, low dielectric constant, etc. For example, Patent Document 1 discloses a boron nitride powder formed by agglomeration of primary particles of boron nitride, which has, in its volumetric particle size distribution, Peak A existing in a region of 5 μm or more and less than 30 μm, and Peak B existing in a region of 50 μm or more and less than 100 μm.
[0004] Japanese Patent Application Laid-Open No. 2020-164365
[0005] The boron nitride powder described in Patent Document 1 can be used to obtain a thermally conductive sheet with excellent thermal conductivity and insulation. However, with the increasing complexity of electronic devices in recent years, heat-generating electronic components are sometimes mounted on mounting surfaces with uneven surfaces, and this has created a demand for thermally conductive sheets with excellent flexibility. Therefore, an object of the present invention is to provide a method for producing a thermally conductive sheet with excellent flexibility.
[0006] The present inventors have conducted extensive research to achieve the above object, and have found that the above object can be achieved by using unreacted silicone oil having a predetermined kinematic viscosity. The present invention is based on the above findings and is summarized as follows: [1] A method for producing a thermally conductive resin composition by blending a thermally conductive filler, a silicone resin, and unreacted silicone oil, a thermally conductive resin composition sheet by forming the thermally conductive resin composition into a sheet, and a thermally conductive resin composition sheet by heating and pressurizing the thermally conductive resin composition sheet, wherein the kinematic viscosity of the unreacted silicone oil is 1×10 -2 m 2 [2] The method for producing a thermally conductive sheet according to the above [1], wherein the silicone resin contains a radical-curable silicone resin. [3] The method for producing a thermally conductive sheet according to the above [1] or [2], wherein the amount of unreacted silicone oil is 2 to 20 parts by mass per 100 parts by mass of the total amount of the thermally conductive filler, the silicone resin, and the unreacted silicone oil.
[0007] According to the present invention, a method for producing a thermally conductive sheet having excellent flexibility can be provided.
[0008] FIG. 1 is a conceptual diagram of the particle size distribution of a thermally conductive filler.
[0009] [Method for manufacturing a thermally conductive sheet] The method for manufacturing a thermally conductive sheet of the present invention includes the steps of: (A) blending a thermally conductive filler, a silicone resin, and unreacted silicone oil to prepare a thermally conductive resin composition; (B) forming the thermally conductive resin composition into a sheet to prepare a thermally conductive resin composition sheet; and (C) heating and pressurizing the thermally conductive resin composition sheet. Each step will be described below.
[0010] (Step (A)) In step (A), a thermally conductive resin composition is prepared by blending a thermally conductive filler, a silicone resin, and unreacted silicone oil. By blending unreacted silicone oil in addition to the silicone resin, a thermally conductive sheet with excellent flexibility can be produced.
[0011] 1. Thermally Conductive Filler The thermally conductive filler used in step (A) is not particularly limited as long as it is a thermally conductive filler commonly used in thermally conductive sheets. Examples of thermally conductive fillers used in the thermally conductive sheet of the present invention include boron nitride particles, aluminum nitride particles, aluminum oxide particles, silicon carbide particles, aluminum nitride, and magnesium oxide. These thermally conductive fillers can be used alone or in combination of two or more. Among these thermally conductive fillers, boron nitride particles are preferred from the viewpoints of thermal conductivity and chemical stability. Furthermore, because of the small anisotropy of thermal conductivity, the thermally conductive filler is preferably agglomerated particles formed by agglomeration of primary particles. Furthermore, from the viewpoints of thermal conductivity and chemical stability, agglomerated boron nitride particles formed by agglomeration of primary particles are more preferred.
[0012] <Crushing Strength> The crushing strength of the agglomerated particles formed by agglomeration of primary particles used in step (A) is preferably 5 to 15 MPa. When the crushing strength of the agglomerated particles formed by agglomeration of primary particles is 5 MPa or more, the agglomerated particles can be prevented from collapsing during the production of the thermally conductive sheet, thereby suppressing a decrease in the thermal conductivity of the thermally conductive sheet. Furthermore, when the crushing strength of the agglomerated particles formed by agglomeration of primary particles is 15 MPa or less, the deformation of the agglomerated particles can reduce voids within the sheet, further improving the thermal conductivity of the thermally conductive sheet. From this perspective, the crushing strength of the agglomerated particles formed by agglomeration of primary particles is more preferably 6 to 13 MPa, and even more preferably 7 to 11 MPa. The crushing strength of the agglomerated particles formed by agglomeration of primary particles can be measured by the method described in the Examples below.
[0013] <Particle Size Distribution of Thermally Conductive Filler> The particle size distribution of the thermally conductive filler is not particularly limited. For example, the particle size distribution of the thermally conductive filler used in the thermally conductive sheet of the present invention may have only a first maximum point, or may have only a first maximum point and a second maximum point whose particle size is larger than that of the first maximum point. However, as shown in Figure 1, it is preferable that the particle size distribution of the thermally conductive filler used in step (A) has at least a first maximum point (MAX1), a second maximum point (MAX2) whose particle size is larger than that of the first maximum point (MAX1), and a third maximum point (MAX3) whose particle size is larger than that of the second maximum point (MAX2). It is preferable that the particle size at the first maximum point (MAX1) is 0.4 μm or more and less than 10 μm, the particle size at the second maximum point (MAX2) is 10 μm or more and less than 40 μm, and the particle size at the third maximum point (MAX3) is 40 μm or more and 110 μm or less. This can improve the filling efficiency of the thermally conductive filler in the thermally conductive sheet, thereby further improving the thermal conductivity of the thermally conductive sheet. The particle size distribution of the thermally conductive filler used in step (A) can be measured by the method described in the Examples below.
[0014] The particle size at the first maximum point (MAX1) is preferably 0.4 μm or more and less than 10 μm. When the particle size at the first maximum point (MAX1) is 0.4 μm or more and less than 10 μm, the filling efficiency of the thermally conductive filler in the thermally conductive sheet can be further increased, and the thermal conductivity of the thermally conductive sheet can be further improved. From this perspective, the particle size at the first maximum point (MAX1) is more preferably 1.0 to 9.0 μm, and even more preferably 2.0 to 8.0 μm.
[0015] The particle size at the second maximum point (MAX2) is preferably 10 μm or more and less than 40 μm. When the particle size at the second maximum point (MAX2) is 10 μm or more and less than 40 μm, the filling efficiency of the thermally conductive filler in the thermally conductive sheet can be further increased, and the thermal conductivity of the thermally conductive sheet can be further improved. From this perspective, the particle size at the second maximum point (MAX2) is more preferably 15 to 36 μm, and even more preferably 18 to 30 μm.
[0016] The particle size at the third maximum point (MAX3) is preferably 40 to 110 μm. When the particle size at the third maximum point (MAX3) is 40 to 110 μm, the filling efficiency of the thermally conductive filler in the thermally conductive sheet can be further increased, and the thermal conductivity of the thermally conductive sheet can be further improved. From this perspective, the particle size at the third maximum point (MAX3) is more preferably 50 to 100 μm, and even more preferably 65 to 90 μm.
[0017] The integrated value (V1) of the frequency between the peak start and peak end in a peak having a first maximum point (MAX1) is preferably 1 to 27% by volume. When the integrated value (V1) is 1 to 27% by volume, the packing density of the thermally conductive filler in the thermally conductive sheet can be further increased, and the thermal conductivity of the thermally conductive sheet can be further improved. From this perspective, the integrated value (V1) is more preferably 5 to 20% by volume. The peak start in a peak having a first maximum point (MAX1) is a minimum point on the smaller particle size side relative to the first maximum point (MAX1). If there is no minimum point on the smaller particle size side relative to the first maximum point (MAX1), the peak start is the end (DS) of the particle size distribution on the smaller particle size side. Furthermore, the peak end in a peak having a first maximum point (MAX1) is a minimum point (MIN1) on the larger particle size side relative to the first maximum point (MAX1). The integrated amount of frequency (V1) is a value obtained by subtracting the frequency of the particle size of the minimum point (MIN1) on the larger particle size side than the first maximum point (MAX1) from the integrated amount of frequency from the particle size of the minimum point on the smaller particle size side than the first maximum point (MAX1) or the particle size at the end (DS) of the particle size distribution on the smaller particle size side to the particle size of the minimum point (MIN1) on the larger particle size side than the first maximum point (MAX1). The reason for subtracting the frequency of the particle size of the minimum point (MIN1) on the larger particle size side than the first maximum point (MAX1) is to prevent the frequency of the particle size of the minimum point (MIN1) on the larger particle size side than the first maximum point (MAX1) from being added to both the integrated amount of frequency from the peak start to the peak end of the peak having the first maximum point (MAX1) and the integrated amount of frequency from the peak start to the peak end of the peak having the second maximum point (MAX2).
[0018] The integrated value (V2) of the frequency between the peak start and peak end in the peak having the second maximum point (MAX2) is preferably 5 to 40% by volume. When the integrated value (V2) is 5 to 40% by volume, the filling efficiency of the thermally conductive filler in the thermally conductive sheet can be further increased, and the thermal conductivity of the thermally conductive sheet can be further improved. From this perspective, the integrated value (V2) is more preferably 10 to 30% by volume. Note that the peak start in the peak having the second maximum point (MAX2) is the minimum point (MIN1) on the smaller particle size side relative to the second maximum point (MAX2). Furthermore, the peak end in the peak having the second maximum point (MAX2) is the minimum point (MIN2) on the larger particle size side relative to the second maximum point (MAX2). The integrated quantity of frequency (V2) is a value obtained by subtracting the frequency of the particle size at the minimum point (MIN2) on the larger particle size side of the second maximum point (MAX2) from the integrated quantity of frequency from the particle size at the minimum point (MIN1) on the smaller particle size side of the second maximum point (MAX2) to the particle size at the minimum point (MIN2) on the larger particle size side of the second maximum point (MAX2). The reason for subtracting the frequency of the particle size at the minimum point (MIN2) on the larger particle size side of the second maximum point (MAX2) is to prevent the frequency of the particle size at the minimum point (MIN2) on the larger particle size side of the second maximum point (MAX2) from being added to both the integrated quantity of frequency from the peak start to the peak end at the peak having the second maximum point (MAX2) and the integrated quantity of frequency from the peak start to the peak end at the peak having the third maximum point (MAX3).
[0019] The integrated value (V3) of the frequency between the peak start and peak end in a peak having a third maximum point (MAX3) is preferably 50 to 90% by volume. When the integrated value (V3) is 50 to 90% by volume, the filling of the thermally conductive filler in the thermally conductive sheet can be further increased, and the thermal conductivity of the thermally conductive sheet can be further improved. From this perspective, the integrated value (V3) is more preferably 60 to 80% by volume. The peak start in a peak having a third maximum point (MAX3) is the minimum point (MIN2) on the smaller particle size side relative to the third maximum point (MAX3). The peak end in a peak having a third maximum point (MAX3) is the minimum point on the larger particle size side relative to the third maximum point (MAX3). If there is no minimum point on the larger particle size side relative to the third maximum point (MAX3), the peak end is the end (DE) of the particle size distribution on the larger particle size side. The integrated amount of frequency (V3) is the value obtained by subtracting the frequency of the particle size of the minimum point (MIN2) on the larger particle size side than the third maximum point (MAX3) from the integrated amount of frequency from the particle size of the minimum point (MIN2) on the smaller particle size side than the third maximum point (MAX3) to the particle size of the minimum point on the larger particle size side than the third maximum point (MAX3), or is the integrated amount of frequency from the particle size of the minimum point (MIN2) on the smaller particle size side than the third maximum point (MAX3) to the particle size at the larger particle size end (DE) of the particle size distribution. The frequency of particle sizes at minimum points on the larger particle size side of the third maximum point (MAX3) is subtracted to prevent the frequency of particle sizes at minimum points on the larger particle size side of the third maximum point (MAX3) from being added to both the cumulative amount of frequency from the peak start to the peak end of a peak having the third maximum point (MAX3) and the cumulative amount of frequency from the peak start to the peak end of a peak having a maximum point adjacent to the third maximum point (MAX3) on the larger particle size side of the third maximum point.
[0020] As long as the packing property of the thermally conductive filler in the thermally conductive sheet can be improved, the particle size distribution of the thermally conductive filler used in step (A) may have other maximum points in addition to the first to third maximum points described above.
[0021] <Method for producing thermally conductive filler> An example of a method for producing the thermally conductive filler used in step (A) is described below. The thermally conductive filler used in step (A) can be produced, for example, by producing a first thermally conductive filler having a particle size distribution with the first maximum point, a second thermally conductive filler having a particle size distribution with the second maximum point, and a third thermally conductive filler having a particle size distribution with the third maximum point, and then mixing the produced first to third thermally conductive fillers.
[0022] Of the first to third thermally conductive fillers, the second and third thermally conductive fillers each preferably contain at least aggregate boron nitride particles. The first thermally conductive filler may be aggregate boron nitride particles, but is preferably hexagonal boron nitride primary particles. The maximum point of each of the first to third thermally conductive fillers refers to the apex of the peak in the particle size distribution of each of the first to third thermally conductive fillers. The particle size distributions of the first to third thermally conductive fillers are measured in the same manner as the particle size distribution of the thermally conductive fillers described above.
[0023] In the mixing step, the first to third thermally conductive fillers may be mixed so that the volume fraction of the third thermally conductive filler is greater than the volume fraction of the first thermally conductive filler and the volume fraction of the second thermally conductive filler. This can further enhance the packing properties of the thermally conductive fillers. From the viewpoint of improving the thermal conductivity of the thermally conductive sheet, the volume fraction of the third thermally conductive filler is preferably 50 to 90 parts by volume, more preferably 60 to 80 parts by volume, per 100 parts by volume of the first to third thermally conductive fillers combined. From the viewpoint of improving the thermal conductivity of the thermally conductive sheet, the volume fraction of the second thermally conductive filler is preferably 5 to 40 parts by volume, more preferably 10 to 30 parts by volume, per 100 parts by volume of the first to third thermally conductive fillers combined. From the viewpoint of improving the thermal conductivity of the thermal conductive sheet, the volume ratio of the first thermally conductive filler is preferably 1 to 27 parts by volume, and more preferably 5 to 20 parts by volume, relative to 100 parts by volume of the total of the first to third thermally conductive fillers.
[0024] Each of the aggregate boron nitride particles used as the thermally conductive filler can be produced by a production method including, for example, a crushing step of crushing aggregate boron carbide, a nitriding step of nitriding the crushed boron carbide to obtain boron carbonitride, and a decarburizing step of decarburizing the boron carbonitride.
[0025] In the pulverization step, lumped boron carbide (boron carbide lumps) are pulverized using a general pulverizer or crusher. At this time, for example, by adjusting the pulverization time and the amount of boron carbide lumps charged, boron carbide powder having a desired maximum point can be obtained. The maximum point of the boron carbide powder can be measured in the same manner as the maximum point of the boron nitride particles described above. In this way, by adjusting the maximum point of the boron carbide powder to approach the maximum point of the desired boron nitride particles, the first to third boron nitride particles having the above-described maximum points can be obtained.
[0026] Subsequently, in the nitriding step, the boron carbide powder is fired under pressure in an atmosphere that promotes the nitriding reaction, thereby obtaining boron carbonitride.
[0027] The atmosphere in the nitriding step is an atmosphere that promotes the nitriding reaction, and may be, for example, nitrogen gas, ammonia gas, or the like, either alone or in combination. From the viewpoints of ease of nitriding and cost, the atmosphere is preferably nitrogen gas. The content of nitrogen gas in the atmosphere is preferably 95% by volume or more, more preferably 99.9% by volume or more.
[0028] The pressure in the nitriding step is preferably 0.6 MPa or more, more preferably 0.7 MPa or more, and preferably 1.0 MPa or less, more preferably 0.9 MPa or less. The pressure is further preferably 0.7 to 1.0 MPa. The firing temperature in the nitriding step is preferably 1800°C or more, more preferably 1900°C or more, and preferably 2400°C or less, more preferably 2200°C or less. The firing temperature is further preferably 1800 to 2200°C. The pressure conditions and firing temperature are preferably 1800°C or more and 0.7 to 1.0 MPa, as these conditions further favorably promote the nitriding of boron carbide and are industrially appropriate.
[0029] The firing time in the nitriding step is appropriately selected within a range in which nitriding proceeds sufficiently, and is preferably 6 hours or more, more preferably 8 hours or more, and is preferably 30 hours or less, more preferably 20 hours or less.
[0030] In the decarburization step, the boron carbonitride obtained in the nitriding step is subjected to a heat treatment in an atmosphere of atmospheric pressure or higher at a predetermined holding temperature for a certain period of time, thereby obtaining aggregated boron nitride particles formed by aggregation of decarburized and crystallized hexagonal boron nitride primary particles.
[0031] The atmosphere in the decarburization step may be an atmosphere of normal pressure (atmospheric pressure) or a pressurized atmosphere. In the case of a pressurized atmosphere, the pressure may be, for example, 0.5 MPa or less, preferably 0.3 MPa or less.
[0032] In the decarburization step, for example, the temperature is first raised to a predetermined temperature (the temperature at which decarburization can begin), and then further raised to a holding temperature at a predetermined heating rate. The predetermined temperature (the temperature at which decarburization can begin) can be set depending on the system, and may be, for example, 1000°C or higher, 1500°C or lower, and preferably 1200°C or lower. The rate at which the temperature is raised from the predetermined temperature (the temperature at which decarburization can begin) to the holding temperature may be, for example, 5°C / min or lower, and preferably 4°C / min or lower, 3°C / min or lower, or 2°C / min or lower.
[0033] The holding temperature is preferably 1800°C or higher, more preferably 2000°C or higher, from the viewpoint of favorable grain growth and further improving the thermal conductivity of the obtained boron nitride particles. The holding temperature may be preferably 2200°C or lower, more preferably 2100°C or lower.
[0034] The holding time at the holding temperature is appropriately selected within a range in which crystallization sufficiently progresses, and may be, for example, more than 0.5 hours, and from the viewpoint of favorable grain growth, is preferably 1 hour or more, more preferably 3 hours or more, even more preferably 5 hours or more, and particularly preferably 10 hours or more. The holding time at the holding temperature may be, for example, less than 40 hours, and from the viewpoint of preventing excessive grain growth and reducing particle strength, is preferably 30 hours or less, more preferably 20 hours or less.
[0035] In the decarburization step, a boron source may be mixed with the boron carbonitride obtained in the nitriding step as a raw material to carry out decarburization and crystallization. Examples of the boron source include boric acid, boron oxide, or a mixture thereof. In this case, other additives used in the art may be further used as necessary.
[0036] The mixing ratio of boron carbonitride and the boron source is appropriately selected. When boric acid or boron oxide is used as the boron source, the ratio of boric acid or boron oxide may be, for example, 100 parts by mass or more, preferably 150 parts by mass or more, and may be, for example, 300 parts by mass or less, preferably 250 parts by mass or less, relative to 100 parts by mass of boron carbonitride.
[0037] The boron nitride particles obtained as described above may be subjected to a step of classifying them using a sieve to obtain boron nitride particles having a desired particle size distribution (classification step), thereby obtaining the first to third aggregate boron nitride particles usable as the first to third thermally conductive fillers.
[0038] The resulting first to third aggregate boron nitride particles can be mixed to obtain a blend having the particle size distributions with the above-mentioned first to third maximum points. The mixing method is not particularly limited as long as it can uniformly mix the first to third aggregate boron nitride particles. For example, the first to third aggregate boron nitride particles may be mixed using a container rotation type mixer, a container fixed type mixer, or a fluid motion type mixer.
[0039] <Amount of Thermally Conductive Filler> The amount of thermally conductive filler is preferably 20 to 90 parts by volume, and more preferably 25 to 85 parts by volume, relative to 100 parts by volume of the total amount of the thermally conductive filler, silicone resin, and unreacted silicone oil. When the amount of thermally conductive filler is 20 parts by volume or more, the thermal conductivity of the thermally conductive sheet tends to be further improved. Furthermore, when the amount of thermally conductive filler is 90 parts by volume or less, the dispersibility of the thermally conductive filler in the thermally conductive sheet is improved.
[0040] 2. Silicone Resin The silicone resin used in step (A) is not particularly limited as long as it is a silicone resin commonly used in thermally conductive sheets. Examples of silicone resins used in step (A) include radical-curable silicone resins cured with organic peroxides such as acyl-based organic peroxides and alkyl-based organic peroxides, and addition-reaction-curable silicone resins cured with platinum catalysts. Among these silicone resins, radical-curable silicone resins are preferred from the viewpoint of the flexibility of the thermally conductive sheet. Examples of radical-curable silicone resins include silicone polymers with a degree of polymerization of approximately 4,000 to 10,000. Examples of silicone polymers include methyl vinyl-based silicone polymers, methyl phenyl vinyl-based silicone polymers, and methyl fluoroalkyl-based silicone polymers. The silicone resin may contain additives such as silica fillers and dispersants. The content of the radical-curable silicone resin in the silicone resin is preferably 80 to 100% by volume, more preferably 90 to 100% by volume, and even more preferably 95 to 100% by volume.
[0041] <Weight Average Molecular Weight> The silicone resin used in step (A) is preferably a silicone resin. The weight average molecular weight of the silicone resin is preferably 30,000 to 1,000,000, more preferably 40,000 to 800,000, and even more preferably 50,000 to 600,000. The weight average molecular weight of the silicone resin can be measured using gel permeation chromatography.
[0042] 3. Unreacted silicone oil The unreacted silicone oil used in step (A) is a silicone oil that does not have an unsaturated group. Examples of silicone oil that does not have an unsaturated group include methyl silicone oil, in which all organic substituents are methyl groups, and methylphenyl silicone oil, in which all organic substituents are methyl groups and phenyl groups. From the viewpoint of the flexibility of the thermal conductive sheet, among these silicone oils, methyl silicone oil is preferred, and dimethyl silicone oil is more preferred.
[0043] <Kinematic viscosity> The kinematic viscosity of unreacted silicone oil is 1 x 10 -2 m 2 / s or more. The kinematic viscosity of the unreacted silicone oil is 1×10 -2 m 2 If the kinematic viscosity is less than 5 × 10 / s, the unreacted silicone oil may seep out of the thermally conductive sheet, which may result in an insufficient improvement in the flexibility of the thermally conductive sheet due to the incorporation of the unreacted silicone oil. -2 m 2 / s or more, and 6×10 -2 m 2 / s or more, and more preferably 7 × 10 -2 m 2 From the viewpoint of further improving the flexibility of the thermally conductive sheet, the kinematic viscosity of the unreacted silicone oil is preferably 5 m / s or more. 2 / s or less, and 2 / s or less is more preferable, and 0.5 m 2 The kinematic viscosity of the unreacted silicone oil can be measured by the method described in the Examples below.
[0044] <Mass Average Molecular Weight> From the viewpoint of improving the flexibility of the thermally conductive sheet, the mass average molecular weight of the unreacted silicone oil used in step (A) is preferably 50,000 to 1,500,000, more preferably 60,000 to 1,200,000, and even more preferably 70,000 to 1,000,000. The mass average molecular weight of the unreacted silicone oil can be measured using gel permeation chromatography.
[0045] <Amount of Unreacted Silicone Oil> The amount of unreacted silicone oil is preferably 2 to 30 parts by volume per 100 parts by volume of the combined total of the thermally conductive filler, silicone resin, and unreacted silicone oil. When the amount of unreacted silicone oil is 2 parts by volume or more, the flexibility of the thermally conductive sheet can be further improved. When the amount of unreacted silicone oil is 30 parts by volume or less, the exudation of unreacted silicone oil from the thermally conductive sheet can be suppressed. From this perspective, the amount of unreacted silicone oil is more preferably 3 to 25 parts by volume, and even more preferably 4 to 22.5 parts by volume, per 100 parts by volume of the combined total of the thermally conductive filler, silicone resin, and unreacted silicone oil.
[0046] <Proportion of Unreacted Silicone Oil to Silicone Resin and Unreacted Silicone Oil> The ratio of the amount of unreacted silicone oil (parts by volume) to the total amount (parts by volume) of the silicone resin (parts by volume) and the unreacted silicone oil (parts by volume) (unreacted silicone oil amount / (silicone resin amount + unreacted silicone oil amount)) is preferably 5 to 55%. When the proportion of unreacted silicone oil is 5% or more, the flexibility of the thermally conductive sheet can be further improved. When the proportion of unreacted silicone oil is 55% or less, insufficient curing of the thermally conductive sheet can be suppressed. From this perspective, the proportion of unreacted silicone oil is more preferably 7 to 40%, and even more preferably 10 to 30%.
[0047] 4. Solvent A solvent may be further blended to adjust the viscosity of the thermally conductive resin composition. The solvent is not particularly limited as long as it can dissolve the silicone resin and can be easily removed from the thermally conductive resin composition after application. When the resin is a silicone resin, examples of the solvent include toluene, xylene, and chlorinated hydrocarbons. Of these solvents, toluene is preferred from the viewpoint of ease of removal. The content of the solvent can be appropriately selected depending on the target viscosity of the thermally conductive resin composition. The blending amount of the solvent is, for example, 40 to 200 parts by mass per 100 parts by mass of the components of the thermally conductive resin composition other than the solvent.
[0048] (Step (B)) In step (B), the thermally conductive resin composition is formed into a sheet to produce a thermally conductive resin composition sheet. For example, the thermally conductive resin composition can be formed into a sheet by a doctor blade method or calendar processing. However, if the thermally conductive filler is in the form of agglomerated particles, the agglomerated particles in the thermally conductive resin composition may break down when the thermally conductive resin composition passes through a calendar roll. Therefore, it is preferable to form the thermally conductive resin composition into a sheet by a doctor blade method.
[0049] (Step (C)) In step (C), the thermally conductive resin composition sheet is heated and pressurized. This can further increase the filling of the thermally conductive filler in the thermally conductive sheet, thereby further improving the thermal conductivity of the thermally conductive sheet. From the viewpoint of improving the filling of the thermally conductive filler, the heating temperature of the thermally conductive resin composition sheet is preferably 120 to 200°C, more preferably 130 to 180°C. Furthermore, the pressure applied when pressing the thermally conductive resin composition sheet is preferably 1 to 25 MPa, more preferably 5 to 20 MPa.
[0050] In step (C), a laminate of the thermally conductive resin composition sheet and the glass cloth may be prepared, and the laminate may be heated and pressurized under vacuum to prepare a thermally conductive sheet including the glass cloth.
[0051] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0052] In the thermally conductive sheets of the Examples and Comparative Examples, boron nitride particles were used as the thermally conductive filler. Three types of raw boron nitride particles, each with a specific particle size maximum point, were mixed to produce boron nitride particles with three maximum points. The raw boron nitride particles used as the raw material for the boron nitride particles used in the thermally conductive sheets of the Examples and Comparative Examples were evaluated as follows. (Average Particle Size) The average particle size of the raw boron nitride particles was measured using a Beckman Coulter laser diffraction scattering particle size distribution analyzer (LS-13 320). The obtained average particle size was measured on the raw boron nitride particles without using a homogenizer before the measurement process. The obtained average particle size was the average particle size measured by volume statistics.
[0053] The following evaluations were carried out on boron nitride particles produced by mixing three types of raw material boron nitride particles. (Crushing Strength) The crushing strength of the boron nitride particles was measured in accordance with JIS R1639-5:2007. Specifically, the boron nitride particles were scattered on the sample stage of a microcompression tester ("MCT-211", manufactured by Shimadzu Corporation), and then 20 agglomerated boron nitride particles were selected from the boron nitride particles and subjected to a compression test one by one. The crushing strength (σ: MPa) was calculated using the dimensionless number (α = 2.48) that changes depending on the position within the particle, the crushing test force (P: N), and the particle size (d: μm), as follows: σ = α × P / (π × d 2 The crushing strength of 20 inorganic filler components was plotted in accordance with JIS R1625:2010, and the crushing strength at which the cumulative failure rate was 63.2% was determined as the crushing strength of the boron nitride particles.
[0054] (Particle size distribution) The particle size distribution of the boron nitride particles was measured using a laser diffraction scattering particle size distribution analyzer (LS-13 320) manufactured by Beckman Coulter Co., Ltd. Note that prior to measuring the particle size distribution, the boron nitride particles were not dispersed using a homogenizer or the like.
[0055] The unreacted silicone oil used in the thermally conductive sheets of the Examples and Comparative Examples was evaluated as follows: (Kinematic Viscosity) The kinematic viscosity of the unreacted silicone oil at 25°C was measured in accordance with the method described in JIS Z 8803:2011.
[0056] The thermally conductive sheets of the examples and comparative examples were evaluated as follows. (Breakdown voltage) The breakdown voltage of the thermally conductive sheet was calculated based on the value measured in a short-time breakdown test (room temperature 23°C) in accordance with JIS C 2110. The evaluation criteria for insulation are as follows: ◎: Breakdown voltage is 20 kV / mm or more ○: Breakdown voltage is 10 kV / mm or more but less than 20 kV / mm ×: Breakdown voltage is less than 10 kV / mm
[0057] (Thermal resistance) A thermally conductive sheet was placed between the TO-3 model heater and the copper plate. The thermally conductive sheet was then fastened using screws with a nominal diameter of M3 mm and a tightening torque of 0.5 N m. The contact area between one TO-3 model heater and the heat dissipation sheet was approximately 6 cm. 2 Thereafter, a power supply device (manufactured by Kikusui Electronics Co., Ltd., model number: PMC35-3) was used to apply 15 W of power to the TO-3 model heater. Then, 10 minutes after the application of 15 W of power, the temperature (T1) of the TO-3 model heater and the temperature (T2) of the copper plate were measured, and the thermal resistance was calculated using the following formula: Thermal resistance (°C / W) = (T1 - T2) / 15
[0058] (Thermal Conductivity) The thermal conductivity of the thermally conductive sheet was measured according to the method described in ASTM D5470:2017. The evaluation criteria for thermal conductivity are as follows: ◎: Thermal conductivity is 5 W / (m·K) or more ○: Thermal conductivity is 3 W / (m·K) or more but less than 5 W / (m·K) ×: Thermal conductivity is less than 3 W / (m·K)
[0059] (Flexibility) A sheet cut into 20 mm x 20 mm was subjected to a compression test using a universal material testing machine (Model 5967, manufactured by Instron) at a compression speed of 1 mm / min and a pressure of 0.5 MPa, and flexibility was evaluated from the compression rate. The evaluation criteria for flexibility are as follows: ○ Compression rate of 3% or more × Compression rate of less than 3%
[0060] The following materials were prepared as raw materials for the thermally conductive sheet. (1) Silicone resin - Silicone resin containing vinyl groups at both ends: manufactured by Dow-Toray Industries, Inc., trade name "CF-3110" (2) Unreacted silicone oil - Unreacted silicone oil 1: Dimethyl silicone oil, manufactured by Wacker Asahi Kasei Co., Ltd., trade name "SILICONE FLUID AK1000000", kinematic viscosity 1 m 2 / s (1 million cSt) Unreacted silicone oil 2: dimethyl silicone oil, manufactured by Wacker Asahi Kasei Co., Ltd., trade name "SILICONE FLUID AK100000", kinematic viscosity 0.1 m 2 / s (100,000 cSt) Unreacted silicone oil 3: dimethyl silicone oil, manufactured by Wacker Asahi Kasei Corporation, trade name "SILICONE FLUID AK1000", kinematic viscosity 0.001 m 2 / s (1000cSt)
[0061] Boron nitride particles A to E each having one maximum point, which serve as raw materials for boron nitride particles having three maximum points, were prepared as follows.
[0062] (Boron nitride particles A) Boron nitride particles A were produced by the following boron carbide synthesis, pressure nitriding step, and decarburization crystallization step.
[0063] (Boron carbide synthesis step) 100 parts by mass of orthoboric acid (hereinafter referred to as boric acid) manufactured by Nippon Denko Corporation and 35 parts by mass of acetylene black (HS100) manufactured by Denka Co., Ltd. were mixed using a Henschel mixer, and then the mixture was filled into a graphite crucible and heated in an arc furnace in an argon atmosphere at 2200°C for 5 hours to produce boron carbide (B 4 The synthesized boron carbide block was pulverized in a ball mill for 3 hours, sieved using a sieve to have a particle size of 75 μm or less, washed with an aqueous nitric acid solution to remove impurities such as iron, and then filtered and dried to produce boron carbide powder with an average particle size of 55 μm.
[0064] (Pressure nitriding step) The synthesized boron carbide was filled into a boron nitride crucible, and then heated in a resistance heating furnace under conditions of 2000°C and 9 atmospheres (0.8 MPa) for 10 hours in a nitrogen gas atmosphere to produce boron carbonitride (B 4CN 4 ) was obtained.
[0065] (Decarburization crystallization process) 100 parts by mass of the synthesized boron carbonitride and 90 parts by mass of boric acid were mixed using a Henschel mixer, then filled into a boron nitride crucible, and heated in a resistance heating furnace under a pressure of 0.2 MPa in a nitrogen gas atmosphere at a temperature increase rate of 10 ° C. / min from room temperature to 1000 ° C., and then at a temperature increase rate of 2 ° C. / min from 1000 ° C., and a holding time of 10 hours at a firing temperature of 2020 ° C. to synthesize aggregated boron nitride particles in which primary particles aggregated into clumps. The synthesized aggregated boron nitride particles were decomposed and crushed using a Henschel mixer, and then classified using a nylon sieve with 150 μm mesh size. Boron nitride particles A were obtained by crushing and classifying the fired product.
[0066] The average particle diameter (D50) of the obtained boron nitride particles A measured by a laser scattering method was 70 μm. SEM observation revealed that the obtained boron nitride particles A were aggregated boron nitride particles formed by aggregation of primary particles. The obtained boron nitride particles A had a crushing strength of 9 MPa.
[0067] (Boron nitride particles B) Boric acid, melamine, and calcium carbonate (all special reagent grade) were mixed in a mass ratio of 70:50:5, and the mixture was heated from room temperature to 1400°C over 1 hour in a nitrogen gas atmosphere, held at 1400°C for 3 hours, then heated to 1900°C over 4 hours, held at 1900°C for 2 hours, and then cooled to room temperature to produce hexagonal boron nitride. The mixture was then crushed, pulverized, and sieved to prepare boron nitride particles B. The average particle diameter (D50) of boron nitride particles B measured by a laser scattering method was 70 μm. SEM observation revealed that boron nitride particles B were aggregated boron nitride particles formed by aggregation of primary particles. The crushing strength of boron nitride particles B was 2 MPa.
[0068] (Boron nitride particles C) Boron nitride particles C were produced in the same manner as boron nitride particles A, except that boron carbide powder having an average particle size of 10 μm was used. The average particle size (D50) of the obtained boron nitride particles C measured by a laser scattering method was 20 μm. SEM observation revealed that the obtained boron nitride particles C were agglomerated boron nitride particles formed by agglomeration of primary particles. The crushing strength of the obtained boron nitride particles C was 8 MPa.
[0069] (Boron nitride particles D) Boric acid, melamine, and calcium carbonate (all special reagent grade) were mixed in a mass ratio of 70:50:5, and in a nitrogen gas atmosphere, the mixture was heated from room temperature to 1400°C over 1 hour, held at 1400°C for 3 hours, then heated to 1900°C over 4 hours, held at 1900°C for 2 hours, and then cooled to room temperature to produce hexagonal boron nitride. The mixture was then crushed, pulverized, and sieved to prepare boron nitride particles D. The average particle diameter (D50) of boron nitride particles D measured by a laser scattering method was 20 μm. SEM observation revealed that boron nitride particles D were aggregated boron nitride particles formed by aggregation of primary particles. The crushing strength of boron nitride particles D was 1.5 MPa.
[0070] (Boron nitride particles E) Commercially available boron nitride particles (trade name "HGP", manufactured by Denka Co., Ltd.) were used as the boron nitride particles E. The average particle diameter (D50) of the boron nitride particles E measured by a laser scattering method was 3.0 μm. As a result of SEM observation, the boron nitride particles E were found to be scaly primary particles.
[0071] Boron nitride particles 1 and 2 were prepared as follows: [Boron nitride particles 1] Boron nitride particles A, C, and E were mixed together so that the volume ratio of boron nitride particles A, C, and E was 70:15:15, thereby preparing boron nitride particles 1.
[0072] [Boron nitride particles 2] Boron nitride particles B, D, and E were mixed so that the volume ratio of boron nitride particles B, D, and E was 70:15:15, thereby producing boron nitride particles 2.
[0073] A thermally conductive sheet was prepared as follows. [Preparation of Thermally Conductive Sheet 1] Boron nitride particles 1, silicone resin, and unreacted silicone oil were weighed out so that the ratio of boron nitride particles 1 was 55 parts by volume, the ratio of silicone resin was 40.5 parts by volume, and the ratio of unreacted silicone oil 1 was 4.5 parts by volume, and then placed in a mixer (product name: Three-One Motor, manufactured by HEIDON). Furthermore, 1 part by mass of curing agent (2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, manufactured by Kayaku Nouryon Co., Ltd., product name "Trigonox 101") per 100 parts by mass of silicone resin, 0.5% by mass of silane coupling agent (dimethyldimethoxysilane, manufactured by Dow-Toray Co., Ltd., product name "DOWSIL Z-6329 Silane", viscosity at 25 ° C: 1 cp) per 100 parts by mass of boron nitride powder, and 15 parts by mass of water per 100 parts by mass of silane coupling agent were added. In addition, 100 parts by mass of toluene was further added to the mixer relative to a total of 100 parts by mass of the above-mentioned raw materials, and then the mixture was mixed for 15 hours using a turbine-type mixing blade to produce a thermally conductive resin composition slurry. The slurry was then coated to a thickness of 0.2 mm on a 0.05 mm thick PET film (carrier film) using the doctor blade method and dried at 75 ° C for 5 minutes to produce a sheet-like molded product with a PET film. Two PET film-attached sheet-like molded products were stacked to produce a laminate. The layer structure of this laminate was PET film / thermally conductive resin composition / thermally conductive resin composition / PET film. The resulting laminate was then subjected to a heat press under vacuum (pressure 3.5 kPa), at a temperature of 150 ° C, and a pressure of 15 MPa for 30 minutes, and the PET films on both sides were peeled off to produce a 0.2 mm thick sheet. This was then subjected to secondary heating at normal pressure and 150 ° C for 4 hours to produce a thermally conductive sheet.
[0074] [Preparation of Thermally Conductive Sheets 2 to 24] Thermally conductive sheets 2 to 24 were prepared in the same manner as thermally conductive sheet 1, except that the type and amount of boron nitride particles, the amount of silicone resin, and the type and amount of unreacted silicone oil were changed as shown in Table 1. The coating thickness of samples with different thicknesses was 0.3 mm.
[0075] The evaluation results of the boron nitride particles, unreacted silicone oil, and thermally conductive sheet are shown in Tables 1 to 4.
[0076]
[0077]
[0078]
[0079]
[0080] From the above evaluation results, it was found that the thermally conductive filler and silicone resin had a kinematic viscosity of 1×10 -2 m 2 It has been found that a thermally conductive sheet with excellent flexibility can be obtained by blending a thermally conductive resin composition with an unreacted silicone oil having a viscosity of 1 / s or more to prepare a thermally conductive resin composition, molding the thermally conductive resin composition into a sheet to prepare a thermally conductive resin composition sheet, and then heating and pressurizing the thermally conductive resin composition sheet to produce a thermally conductive sheet.
Claims
1. A method for producing a thermally conductive resin composition by blending a thermally conductive filler, a silicone resin, and an unreacted silicone oil, a step of forming the thermally conductive resin composition into a sheet shape to produce a thermally conductive resin composition sheet, and a step of heating and pressurizing the thermally conductive resin composition sheet, wherein the kinetic viscosity of the unreacted silicone oil is 1×10 -2 m 2 A method for producing a thermally conductive sheet, wherein the thermal conductivity is 1 / s or more.
2. The method for producing a thermally conductive sheet according to claim 1, wherein the silicone resin comprises a radical curing type silicone resin.
3. A method for producing a thermally conductive sheet as described in claim 1 or 2, wherein the amount of unreacted silicone oil is 2 to 20 parts by mass per 100 parts by mass of the total of the amount of the thermally conductive filler, the amount of the silicone resin, and the amount of the unreacted silicone oil.
Citation Information
Patent Citations
Resin composition, method for producing the same, and highly thermoconductive resin molded body
JP2015013949A
Insulating heat dissipation sheet
WO2019164002A1
Thermally conductive sheet, method for manufacturing thermally conductive sheet, and method for using thermally conductive sheet
WO2019189626A1
Cited By
Method for manufacturing thermally conductive sheet
JPWO2024203519A1