Modified polyolefin resin composition
The modified polyolefin resin composition, achieved by dispersing a high-temperature modified resin in a low-temperature polyolefin resin with α,β-unsaturated carboxylic acid derivatives, addresses the adhesion and stability challenges of polyolefin resins, providing excellent heat-resistant adhesion and solution stability for use in coatings and adhesives.
Patent Information
- Application Number
- PCT/JP2024/010595
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-03
AI Technical Summary
Polyolefin resins exhibit poor adhesion to hard-to-adhere substrates and have stability issues in solution form, limiting their application in coatings and adhesives due to their non-polar and crystalline nature.
A modified polyolefin resin composition is developed by modifying polyolefin resin (A) with a melting point of 100°C or less and polyolefin resin (B) with an extrapolated melting start temperature of 120°C or higher, using α,β-unsaturated carboxylic acids or their derivatives, with the modified resin (B) dispersed in resin (A), achieving a 50:50 to 95:5 mass ratio, and incorporating a hydrophobic solvent for improved adhesion and stability.
The modified resin composition demonstrates excellent heat-resistant adhesion to difficult-to-adhere substrates and enhanced solution stability, with a reduced water vapor permeation rate, making it suitable for use in primers, adhesives, and inks.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Modified polyolefin resin composition
[0001] The present invention relates to a resin composition containing a modified polyolefin obtained by modifying an α,β-unsaturated carboxylic acid and / or a derivative thereof.
[0002] Polyolefin resins have many excellent properties, such as excellent mechanical properties such as tensile strength, tear strength, and impact strength, as well as excellent water resistance and chemical resistance, and are therefore used in a variety of applications such as sheets, films, molded products, etc. However, unlike polar substrates such as polyurethane-based resins, polyamide-based resins, acrylic-based resins, and polyester-based resins, polyolefin resins are non-polar and crystalline, which can make coating and adhesion difficult.
[0003] In the automotive industry, modified polyolefin resins modified with highly adhesive α,β-unsaturated carboxylic acids or derivatives thereof are used as adhesion promoters for adhering poorly adhesive paints to polyolefin resins (in the automotive industry, paints that are applied directly to substrates and are composed mainly of adhesion promoters are particularly called primer paints) (Patent Document 1).
[0004] Japanese Patent Application Laid-Open No. 2001-279048
[0005] It has been known that modified polyolefin resins obtained by modifying polyolefin resins with relatively high melting points can achieve excellent heat-resistant adhesion to poorly adhesive substrates such as polyolefins. However, such resins have the problem of poor solution stability and poor handling.
[0006] An object of the present invention is to provide a resin composition that has excellent heat resistance to adhesion to poorly adhesive substrates and excellent solution stability.
[0007] The present invention provides the following: [1] A resin composition comprising: a modified product obtained by modifying polyolefin resin (A) having a melting point of 100°C or less, as measured in accordance with JIS K7121-1987 by a differential scanning calorimeter at a heating rate of 10°C / min, with one or more compounds selected from the group consisting of α,β-unsaturated carboxylic acids and their derivatives; and a modified product obtained by modifying polyolefin resin (B) having an extrapolated melting onset temperature (Tim) of 120°C or more, as measured in accordance with JIS K7121-1987 by a differential scanning calorimeter at a heating rate of 10°C / min, with one or more compounds selected from the group consisting of α,β-unsaturated carboxylic acids and their derivatives, wherein the modified product of resin (B) is dispersed in the modified product of resin (A), and the average particle size of the modified product of resin (B) is 0.1 to 100 μm. [2] The resin composition according to [1] above, wherein the one or more compounds selected from the group consisting of α,β-unsaturated carboxylic acids and derivatives thereof include maleic anhydride. [3] The resin composition according to [1] or [2] above, wherein the one or more compounds selected from the group consisting of α,β-unsaturated carboxylic acids and derivatives thereof include a (meth)acrylic acid ester. [4] The resin composition according to any one of [1] to [3] above, wherein the melting point of resin (B) is 140 to 200°C as measured at a heating rate of 10°C / min using a differential scanning calorimeter in accordance with JIS K7121-1987. [5] The resin composition according to any one of [1] to [4] above, wherein the mass ratio of the modified product of resin (A) to the modified product of resin (B) is 50:50 to 95:5 (modified product of resin (A) : modified product of resin (B)). [6] The resin composition according to any one of [1] to [5] above, wherein the difference (Tem - Tim) between the extrapolated melting end temperature (Tem) and the extrapolated melting onset temperature (Tim) of resin (B) measured at a heating rate of 10°C / min using a differential scanning calorimeter in accordance with JIS K7121-1987 is 5 to 20°C. [7] The resin composition according to any one of [1] to [6] above, further comprising a hydrophobic solvent. [8] A primer comprising the resin composition according to any one of [1] to [7] above. [9] An adhesive comprising the resin composition according to any one of [1] to [7] above.
[10] A paint containing the resin composition according to any one of [1] to [7] above.
[11] An ink containing the resin composition according to any one of [1] to [7] above.
[12] A method for producing the resin composition according to any one of [1] to [7] above, comprising: (1) a step of simultaneously modifying a mixture of resin (A) and resin (B) with one or more compounds selected from the group consisting of α,β-unsaturated carboxylic acids and derivatives thereof to obtain the resin composition, or (2) a step of modifying resin (A) with one or more compounds selected from the group consisting of α,β-unsaturated carboxylic acids and derivatives thereof to obtain a modified product of resin (A), a step of modifying resin (B) with one or more compounds selected from the group consisting of α,β-unsaturated carboxylic acids and derivatives thereof to obtain a modified product of resin (B), and a step of mixing the modified product of resin (A) and the modified product of resin (B) obtained to obtain the resin composition.
[0008] According to the present invention, it is possible to provide a resin composition that can exhibit excellent heat resistance to adhesion to poorly adhesive substrates and excellent solution stability.
[0009] In the following description, unless otherwise specified, the expression "AA to BB" means "greater than or equal to AA and less than or equal to BB." Here, "AA" and "BB" each represent a numerical value, with AA<BB. The unit of "AA" is the same as the unit attached to "BB" unless otherwise specified.
[0010] In the following description, unless otherwise specified, the term "(meth)acrylic acid" includes "acrylic acid," "methacrylic acid," and combinations thereof, and the term "(meth)acrylate" includes "acrylate," "methacrylate," and combinations thereof.
[0011] The present invention provides a resin composition comprising a modified product of polyolefin resin (A) having a melting point of 100°C or less modified with an α,β-unsaturated carboxylic acid and / or a derivative thereof, and a modified product of polyolefin resin (B) having an extrapolated melting onset temperature (Tim) of 120°C or more modified with an α,β-unsaturated carboxylic acid and / or a derivative thereof, wherein the modified product of resin (B) is dispersed in the modified product of resin (A), and the modified product of resin (B) has an average particle size of 0.1 to 100 μm. Such a resin composition can exhibit excellent heat adhesion resistance and solution stability to poorly adhesive substrates. Hereinafter, resin (A) will be referred to simply as component (A), and resin (B) will be referred to simply as component (B).
[0012] (1. Polyolefin Resin) The resin composition of the present invention comprises a modified product obtained by modifying a polyolefin resin (A) having a melting point of 100°C or less with an α,β-unsaturated carboxylic acid and / or a derivative thereof, and a modified product obtained by modifying a polyolefin resin (B) having an extrapolated melting onset temperature (Tim) of 120°C or more with an α,β-unsaturated carboxylic acid and / or a derivative thereof.
[0013] The polyolefin resin is a polymer of an olefin (preferably an α-olefin), such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, or 1-octene.
[0014] The polyolefin resin may be a polymer of one kind of olefin (preferably α-olefin) or a copolymer of two or more kinds of olefins (preferably α-olefins). When the polyolefin resin is a copolymer, the polyolefin resin may be a random copolymer or a block copolymer.
[0015] The mass ratio of the modified product of component (A) to the modified product of component (B) (modified product of component (A):modified product of component (B)) is preferably 40:60 to 95:5, more preferably 50:50 to 95:5, even more preferably 60:40 to 95:5, still more preferably 70:30 to 95:5, and particularly preferably 75:25 to 95:5.
[0016] (1-1. Component (A): Polyolefin resin having a melting point of 100°C or less) From the viewpoint of exhibiting sufficient adhesiveness, the polyolefin resin of component (A) is preferably polypropylene (propylene homopolymer), ethylene-propylene copolymer, propylene-1-butene copolymer, ethylene-propylene-1-butene copolymer, or a mixture thereof.
[0017] Here, "polypropylene" refers to a polymer whose structural units are propylene-derived structural units. "Ethylene-propylene copolymer" refers to a copolymer containing ethylene-derived structural units and propylene-derived structural units as structural units. "Propylene-1-butene copolymer" refers to a copolymer containing propylene-derived structural units and 1-butene-derived structural units as structural units. "Ethylene-propylene-1-butene copolymer" refers to a copolymer containing ethylene-derived structural units, propylene-derived structural units, and 1-butene-derived structural units as structural units. These (co)polymers may contain small amounts of other olefin-derived structural units as structural units, as long as the amount does not significantly impair the inherent performance of the resin.
[0018] The polyolefin resin of component (A) preferably contains 15 mol % or more, and more preferably 50 mol % or more, of propylene-derived structural units relative to 100 mol % of all structural units. When the propylene-derived structural units are contained in the above range, good adhesion can be maintained.
[0019] When the polyolefin resin of component (A) is an ethylene-propylene copolymer or a propylene-1-butene copolymer, preferably, out of 100 mol% of all structural units, structural units derived from ethylene or structural units derived from 1-butene account for 3 to 85 mol% (more preferably 3 to 50 mol%), and structural units derived from propylene account for 15 to 97 mol% (more preferably 50 to 97 mol%).
[0020] The lower limit of the melting point (Tm) of the polyolefin resin of component (A) is preferably 60°C or higher, more preferably 80°C or higher, even more preferably 90°C or higher, and particularly preferably 95°C or higher. When the melting point of the polyolefin resin of component (A) is within the above range, sufficient coating strength can be achieved when the resin composition is used for applications such as inks and paints. Therefore, sufficient adhesion to substrates can be exhibited. Furthermore, when used as an ink, blocking during printing can be suppressed. The melting point (Tm) of the polyolefin resin of component (A) can be measured using a differential scanning calorimeter at a heating rate of 10°C / min in accordance with JIS K7121-1987.
[0021] The weight average molecular weight (Mw) of the polyolefin resin of component (A) is preferably 5,000 or more, more preferably 10,000 or more, even more preferably 30,000 or more, still more preferably 50,000 or more, and particularly preferably 100,000 or more, and the upper limit is preferably 200,000 or less, more preferably 180,000 or less, even more preferably 170,000 or less, still more preferably 160,000 or less, and particularly preferably 150,000 or less. The weight average molecular weight (Mw) can be measured by gel permeation chromatography (GPC) using polystyrene as a standard substance.
[0022] (1-2. Component (B): Polyolefin resin having an extrapolated melting onset temperature of 120°C or higher) The polyolefin resin of component (B) is preferably polypropylene (propylene homopolymer), ethylene-propylene copolymer, propylene-1-butene copolymer, ethylene-propylene-1-butene copolymer, or a mixture thereof.
[0023] The lower limit of the melting point (Tm) of the polyolefin resin of component (B) is preferably 140° C. or higher, more preferably 145° C. or higher, even more preferably 150° C. or higher, and particularly preferably 155° C. or higher, and the upper limit is preferably 200° C. or lower, more preferably 190° C. or lower, even more preferably 180° C. or lower, and particularly preferably 170° C. or lower. The melting point (Tm) of the polyolefin resin of component (B) can be measured by a differential scanning calorimeter at a heating rate of 10° C. / min in accordance with JIS K7121-1987.
[0024] The lower limit of the extrapolated melting onset temperature (Tim) of the polyolefin resin of component (B) is 120° C. or higher, preferably 125° C. or higher, more preferably 130° C. or higher, even more preferably 135° C. or higher, and particularly preferably 140° C. or higher, and the upper limit is preferably 200° C. or lower, more preferably 190° C. or lower, even more preferably 180° C. or lower, and particularly preferably 170° C. or lower. The extrapolated melting onset temperature (Tim) of the polyolefin resin of component (B) can be measured using a differential scanning calorimeter at a heating rate of 10° C. / min in accordance with JIS K7121-1987.
[0025] The lower limit of the extrapolated melting end temperature (Tem) of the polyolefin resin of component (B) is preferably 135° C. or higher, more preferably 140° C. or higher, even more preferably 145° C. or higher, and particularly preferably 150° C. or higher, and the upper limit is preferably 210° C. or lower, more preferably 200° C. or lower, even more preferably 190° C. or lower, and particularly preferably 180° C. or lower. The extrapolated melting end temperature (Tem) of the polyolefin resin of component (B) can be measured using a differential scanning calorimeter at a heating rate of 10° C. / min in accordance with JIS K7121-1987.
[0026] The difference (Tem-Tim) between the extrapolated melting end temperature (Tem) and the extrapolated melting onset temperature (Tim) of the polyolefin resin of component (B) is preferably 5 to 20°C, more preferably 10 to 20°C, even more preferably 10 to 19°C, and particularly preferably 12 to 18°C.
[0027] The weight average molecular weight (Mw) of the polyolefin resin of component (B) is preferably 5,000 or more, more preferably 10,000 or more, even more preferably 30,000 or more, still more preferably 40,000 or more, and particularly preferably 50,000 or more, and the upper limit is preferably 500,000 or less, more preferably 400,000 or less, even more preferably 300,000 or less, still more preferably 200,000 or less, and particularly preferably 180,000 or less.
[0028] (2. Modification with α,β-unsaturated carboxylic acid and / or derivative thereof) The resin composition of the present invention can be produced by, for example, (1) a method comprising the step of simultaneously modifying a mixture of component (A) and component (B) with an α,β-unsaturated carboxylic acid and / or a derivative thereof to obtain the resin composition of the present invention (hereinafter may be referred to as "simultaneous modification"); or (2) a method comprising the steps of modifying component (A) with an α,β-unsaturated carboxylic acid and / or a derivative thereof to obtain a modified product of component (A), modifying component (B) with an α,β-unsaturated carboxylic acid and / or a derivative thereof to obtain a modified product of component (B), and mixing the obtained modified product of component (A) with the obtained modified product of component (B) to obtain the resin composition of the present invention (hereinafter may be referred to as "individual modification").
[0029] The modification with an α,β-unsaturated carboxylic acid and / or a derivative thereof can be carried out, for example, by graft copolymerizing the α,β-unsaturated carboxylic acid or a derivative thereof onto the polyolefin chain of the raw material polyolefin resin. The modification with an α,β-unsaturated carboxylic acid and / or a derivative thereof can be carried out using a melting method.
[0030] The modification with an α,β-unsaturated carboxylic acid and / or a derivative thereof is preferably carried out, for example, by heating and melting the polyolefin resin to react with the α,β-unsaturated carboxylic acid and / or a derivative thereof. The heating and melting temperature may be equal to or higher than the melting point of the raw polyolefin resin (component (B) in the case of simultaneous modification), preferably equal to or higher than the melting point of the raw polyolefin resin (component (B) in the case of simultaneous modification) and equal to or lower than 300°C, more preferably equal to or higher than the melting point of the raw polyolefin resin (component (B) in the case of simultaneous modification) and equal to or lower than 250°C, and particularly preferably equal to or higher than the melting point of the raw polyolefin resin (component (B) in the case of simultaneous modification) and equal to or lower than 200°C.
[0031] The modification with an α,β-unsaturated carboxylic acid and / or a derivative thereof can be carried out using equipment such as a Banbury mixer, a kneader, or an extruder, and is preferably carried out using an extruder (extrusion modification).
[0032] In the case of simultaneous modification, the extrusion modification method may, for example, be a method comprising feeding a mixture of components (A) and (B) as raw materials to the feed section of an extruder (e.g., a co-rotating multi-screw extruder, a twin-screw extruder), mixing the raw materials, melt-kneading, reacting, and devolatilizing the α,β-unsaturated carboxylic acid and / or its derivative in the extruder, for example, at the above-mentioned heating and melting temperature, and cooling the resin emerging from the tip die of the extruder (e.g., immersing in a water tank), to obtain the resin composition of the present invention. The progress of the modification reaction and kneading can be adjusted by adjusting the temperature of each part of the barrel of the extruder and the screw rotation speed.
[0033] In the case of individual modification, the extrusion modification method, for example, component (A) as a raw material is supplied to the supply section of an extruder, and in the extruder, together with an α,β-unsaturated carboxylic acid and / or a derivative thereof, for example, at the above-mentioned heat-melting temperature, raw material mixing, melt-kneading, reaction, and devolatilization, cooling, and further cooling the resin coming out of the tip die of the extruder, to obtain a modified product of component (A), component (B) as a raw material is supplied to the supply section of an extruder, and in the extruder, together with an α,β-unsaturated carboxylic acid and / or a derivative thereof, for example, at the above-mentioned heat-melting temperature, raw material mixing, melt-kneading, reaction, and devolatilization, cooling, and further cooling the resin coming out of the tip die of the extruder, to obtain a modified product of component (B), the obtained modified product of component (A) and the obtained modified product of component (B) are supplied to the supply section of an extruder, and in the extruder, for example, at a temperature similar to the above-mentioned heat-melting temperature, melt-kneaded, cooled, and further cooling the resin coming out of the tip die of the extruder, to obtain a resin composition of the present invention. The progress of the modification reaction and kneading can be adjusted by adjusting the temperature at each part of the barrel of the extruder and the screw rotation speed, as in the case of simultaneous modification.
[0034] Examples of derivatives of α,β-unsaturated carboxylic acids include α,β-unsaturated carboxylic anhydrides, α,β-unsaturated carboxylic esters, α,β-unsaturated carboxylic amides, α,β-unsaturated carboxylic imides, etc. In the case of individual modification, the α,β-unsaturated carboxylic acid and derivatives thereof used to modify component (A) and the α,β-unsaturated carboxylic acid and derivatives thereof used to modify component (B) may be the same or different.
[0035] Examples of α,β-unsaturated carboxylic acids and derivatives thereof include maleic acid, maleic anhydride (maleic anhydride), fumaric acid, citraconic acid, citraconic anhydride, mesaconic acid, itaconic acid, itaconic anhydride, aconitic acid, aconitic anhydride, himic anhydride, (meth)acrylic acid, (meth)acrylic acid esters, etc. The α,β-unsaturated carboxylic acids and derivatives thereof preferably include at least one selected from maleic anhydride and (meth)acrylic acid esters.
[0036] In one embodiment, the α,β-unsaturated carboxylic acid and / or derivative thereof more preferably includes a (meth)acrylic acid ester. The (meth)acrylic acid ester is preferably an alkyl (meth)acrylate such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, 2,4,6-trimethylheptyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, or stearyl (meth)acrylate. In one embodiment, the number of carbon atoms in the alkyl group of the alkyl(meth)acrylate is preferably 1 to 30, more preferably 4 to 20, still more preferably 8 to 16, and particularly preferably 10 to 14. In one embodiment, the alkyl(meth)acrylate is most preferably lauryl(meth)acrylate.
[0037] In one embodiment, the α,β-unsaturated carboxylic acid and / or derivative thereof more preferably contains maleic anhydride. When the α,β-unsaturated carboxylic acid and / or derivative thereof contains maleic anhydride, the cyclic structure derived from maleic anhydride contained in the modified polyolefin resin may be partially hydrolyzed to open the ring.
[0038] The content of maleic anhydride in the α,β-unsaturated carboxylic acid and / or derivative thereof is preferably 10% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and particularly preferably 50% by mass or more, when the total amount of the α,β-unsaturated carboxylic acid and / or derivative thereof is taken as 100% by mass.
[0039] The amount of the α,β-unsaturated carboxylic acid and / or derivative thereof used for modification with the α,β-unsaturated carboxylic acid and / or derivative thereof is preferably 50% by weight or less, more preferably 30% by weight or less, even more preferably 20% by weight or less, and particularly preferably 10% by weight or less, relative to 100% by weight of the raw material polyolefin resin. The lower limit is not particularly limited, but is preferably 0.01% by weight or more, more preferably 0.1% by weight or more, even more preferably 1% by weight or more, and particularly preferably 3% by weight or more.
[0040] The modification with an α,β-unsaturated carboxylic acid and / or a derivative thereof is preferably carried out in the presence of a radical reaction initiator. Examples of the radical reaction initiator include a thermal polymerization initiator that generates free radicals when heated, such as organic peroxides and azonitriles. Examples of organic peroxides include di-tert-butyl peroxide, dicumyl peroxide, tert-butylcumyl peroxide, dibenzoyl peroxide, benzoyl m-tolyl peroxide, di(m-tolyl)benzoyl, dilauryl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, cumene hydroperoxide, tert-butyl hydroperoxide, 1,1-bis(tert-butylperoxy)- Examples of the azonitriles include 3,5,5-trimethylcyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, cyclohexanone peroxide, tert-butylperoxybenzoate, tert-butylperoxyisobutyrate, tert-butylperoxy-3,5,5-trimethylhexanoate, tert-butylperoxy-2-ethylhexanoate, tert-butylperoxyisopropyl carbonate, and cumyl peroxyoctoate. Examples of the azonitriles include 2,2-azobis(2-methylbutyronitrile), 2,2-azobisisobutyronitrile, 2,2-azobis(2,4-dimethylvaleronitrile), and 2,2-azobis(4-methoxy-2,4-dimethylvaleronitrile).
[0041] The amount of the radical reaction initiator used for the modification with an α,β-unsaturated carboxylic acid and / or a derivative thereof is preferably 0.01% by weight to 3% by weight, more preferably 0.1% by weight to 2% by weight, based on 100% by weight of the raw material polyolefin resin.
[0042] The mass ratio (component (A): component (B)) of the amount of raw material component (A) to the amount of raw material component (B) required to obtain the resin composition of the present invention is preferably 40:60 to 95:5, more preferably 50:50 to 95:5, even more preferably 60:40 to 95:5, even more preferably 70:30 to 95:5, and particularly preferably 75:25 to 95:5. In the case of simultaneous modification, a mixture of components (A) and (B) blended at the above mass ratio is used as a raw material to carry out modification and obtain a resin composition. In the case of individual modification, the above mass ratio is used as the mass ratio of the raw materials used, and modification of component (A) and modification of component (B) are carried out separately, and the resulting modified products are mixed to obtain a resin composition.
[0043] The total graft weight (degree of modification) of the α,β-unsaturated carboxylic acid and / or derivative thereof in the resin composition of the present invention is preferably 50% by weight or less, more preferably 30% by weight or less, even more preferably 20% by weight or less, and particularly preferably 10% by weight or less, when the total amount of the modified product of component (A) and the modified product of component (B) is taken as 100% by weight. The lower limit is not particularly limited, but is preferably 0.01% by weight or more, more preferably 0.1% by weight or more, and even more preferably 1% by weight or more. The graft weight (% by weight) can be measured, for example, by alkali titration, Fourier transform infrared spectroscopy, or 1 It can be determined by H-NMR or the like.
[0044] (3. Resin Composition) The resin composition of the present invention is in a form in which the modified product of component (B) is dispersed in the modified product of component (A). The modified product of component (B) may be in the form of particles in which the unmodified polyolefin resin of component (B) and the modified polyolefin resin of component (B) are heterogeneously mixed.
[0045] The resin composition of the present invention may contain a hydrophobic solvent. The resin composition of the present invention includes a solid form in which a solid particulate modified product of component (B) is dispersed in a solid modified product of component (A), and a liquid form in which a solid particulate modified product of component (B) is dispersed in a solution in which the modified product of component (A) is dissolved.
[0046] When the resin composition of the present invention is obtained using the extrusion modification method, the resin composition obtained by cooling the resin emerging from the tip die of the extruder can be in a solid form in which the solid particulate modified product of component (B) is dispersed in the solid modified product of component (A). The solid resin composition thus obtained can be mixed with a hydrophobic solvent to form a liquid form in which the solid particulate modified product of component (B) is dispersed in a solution in which the modified product of component (A) is dissolved.
[0047] Examples of hydrophobic solvents include aromatic hydrocarbon solvents such as toluene and xylene; ester solvents such as methyl acetate, ethyl acetate, n-propyl acetate, isopropyl acetate, and butyl acetate; ketone solvents such as acetone, methyl ethyl ketone, and methyl butyl ketone; alicyclic hydrocarbon solvents such as cyclohexane, methylcyclohexane, and ethylcyclohexane; and aliphatic hydrocarbon solvents such as hexane, nonane, and decane.
[0048] The average particle size of the modified product of component (B) is 0.1 to 500 μm, and is not particularly limited, but is preferably 0.1 to 200 μm, more preferably 0.1 to 100 μm, even more preferably 0.3 to 50 μm, even more preferably 0.4 to 20 μm, and particularly preferably 0.5 to 10 μm. The average particle size of the modified product of component (B) may be the volume-based median diameter Dv50 (the maximum particle size below which 50% of the sample volume falls). The average particle size of the modified product of component (B) can be measured and calculated, for example, as in Test Example 1 below.
[0049] The resin composition of the present invention has a low water vapor permeability when molded into a film. The resin composition of the present invention has a water vapor permeability of preferably 15 g / (m) when molded into a film having a thickness of 30 μm. 2 24h) or less, more preferably 12g / (m 2 ・24h) or less, and is usually 0 g / (m 2 ・24h) or greater than 0.5g / (m 2 The water vapor transmission rate can be measured by the method described in the Examples section based on JIS K 7129-1 (humidity sensor method).
[0050] The resin composition of the present invention can be used for primers, adhesives, paints, or inks. The primers, adhesives, paints, or inks may contain, in addition to the resin composition of the present invention, additives such as a hydrophobic solvent, a hydrophilic solvent, a curing agent, an adhesive component, a basic substance, an emulsifier, a crosslinking agent, a diluent, a light stabilizer, an ultraviolet absorber, a pigment, a dye, or an inorganic filler.
[0051] Examples of hydrophilic solvents include water, glycol solvents such as ethylene glycol, alcohol solvents such as methanol, ethanol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, sec-butyl alcohol, tert-butyl alcohol, and 2-ethylhexanol, and glycol monoether solvents such as ethyl cellosolve, butyl cellosolve, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monoisopropyl ether, and propylene glycol monobutyl ether. The solvents may be used alone or in combination of two or more.
[0052] Examples of curing agents include polyisocyanate compounds, epoxy compounds, polyamine compounds, polyol compounds, crosslinking agents in which the functional groups thereof are blocked with protecting groups, and combinations of two or more of these. The content of the curing agent may be appropriately selected depending on the content of the modified polyolefin resin. When using a curing agent, a catalyst such as an organotin compound or a tertiary amine compound may be used in combination depending on the purpose. The curing agent may be used alone or in combination of two or more.
[0053] Examples of adhesive components include known adhesive components such as polyester adhesives, polyurethane adhesives, acrylic adhesives, etc. The adhesive components may be used alone or in combination of two or more.
[0054] When using, for example, water, an alcohol-based solvent, a glycol-based solvent, a ketone-based solvent, or an ester-based solvent as the solvent, the resin composition preferably contains a basic substance. This allows the pH to be appropriately adjusted, further improving the dispersibility and storage stability of the resin in the solvent. Examples of basic substances include sodium hydroxide, potassium hydroxide, ammonia, methylamine, propylamine, hexylamine, octylamine, ethanolamine, propanolamine, diethanolamine, N-methyldiethanolamine, dimethylamine, diethylamine, triethylamine, N,N-dimethylethanolamine, 2-dimethylamino-2-methyl-1-propanol, 2-amino-2-methyl-1-propanol, morpholine, dimethylethanolamine, and 2-amino-2-ethyl-1,3-propanediol. Preferred examples include ammonia, triethylamine, 2-amino-2-methyl-1-propanol, morpholine, dimethylethanolamine, and 2-amino-2-ethyl-1,3-propanediol. The basic substance may be used alone or in combination of two or more kinds.
[0055] When a hydrophobic solvent is used as the solvent, the resin composition preferably contains a diluent. This can improve storage stability. Examples of the diluent include alcohol and propylene-based glycol ether. Examples of the alcohol include methanol, ethanol, propanol, isopropanol, and butanol. Examples of the propylene-based glycol ether include propylene glycol methyl ether, propylene glycol ethyl ether, and propylene glycol tert-butyl ether. The diluent may be used alone or in combination of two or more.
[0056] When a hydrophobic solvent is used as the solvent, the resin composition preferably contains a crosslinking agent. The crosslinking agent may be a compound that can react with groups present in the resin composition, such as hydroxyl groups, carboxyl groups, and amino groups, to form a crosslinked structure, and may be, for example, either a water-soluble crosslinking agent or an aqueous dispersion of a crosslinking agent (a crosslinking agent dispersed in water by some method). Examples of crosslinking agents include blocked isocyanate compounds, aliphatic or aromatic epoxy compounds, amine compounds, and amino resins. The crosslinking agents may be used alone or in combination of two or more.
[0057] When a hydrophilic solvent is used as the solvent, the resin composition preferably contains an emulsifier. Examples of the emulsifier include surfactants such as nonionic surfactants and anionic surfactants, and nonionic surfactants are preferred.
[0058] Examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyethylene polyoxypropylene alkyl ethers, polyoxyethylene derivatives, polyoxyethylene fatty acid esters, polyoxyethylene polyhydric alcohol fatty acid esters, polyoxyethylene polyoxypropylene polyols, sorbitan fatty acid esters, polyoxyethylene hydrogenated castor oil, polyoxyalkylene polycyclic phenyl ethers, polyoxyethylene alkylamines, alkylalkanolamides, polyalkylene glycol (meth)acrylates, etc. Preferred are polyoxyethylene alkyl ethers, polyoxyethylene fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and polyoxyethylene alkylamines.
[0059] Examples of anionic surfactants include alkyl sulfates, polyoxyethylene alkyl ether sulfates, alkylbenzene sulfonates, α-olefin sulfonates, methyl taurates, sulfosuccinates, ether sulfonates, ether carboxylates, fatty acid salts, naphthalenesulfonic acid-formalin condensates, alkylamine salts, quaternary ammonium salts, alkyl betaines, and alkylamine oxides. Polyoxyethylene alkyl ether sulfates and sulfosuccinates are preferred. The emulsifiers may be used singly or in combination of two or more.
[0060] The present invention will be specifically described below using examples, but the present invention is not limited to these examples. The unit "parts" used below means "parts by weight." Unless otherwise specified, "%" means % by weight. In the following description, unless otherwise specified, the temperature conditions are normal temperature (25°C), and the pressure conditions are normal pressure (760 mmHg).
[0061] Example 1: 90 parts of propylene-butene copolymer (Tm = 97°C) as component (A), 10 parts of polyolefin-based thermoplastic elastomer (Tm = 166°C, Tim = 152°C, Temp = 169°C) as component (B), 4 parts of maleic anhydride, 4 parts of lauryl methacrylate, and 1.5 parts of di-tert-butyl peroxide were kneaded and reacted in a twin-screw extruder set at a reaction temperature of 170°C. Volatilization was carried out under reduced pressure in the extruder to remove any remaining unreacted material. After the reaction, the mixture was cooled to room temperature to obtain a modified polyolefin resin composition. The total graft weight of maleic anhydride in the modified polyolefin resin composition was 3.0% by weight, based on the total amount of modified polyolefin resin as 100% by weight. The total graft weight of maleic anhydride was measured by alkali titration. The same applies hereinafter.
[0062] The melting point (Tm) of component (A), and the melting point (Tm), extrapolated melting onset temperature (Tim), and extrapolated melting end temperature (Tem) of component (B) were measured using a differential scanning calorimeter at a heating rate of 10°C / min in accordance with JIS K7121-1987.
[0063] Example 2 A modified polyolefin resin composition was obtained in the same manner as in Example 1, except that the amount of propylene-butene copolymer (Tm = 97°C) used was changed from 90 parts to 80 parts, and the amount of polyolefin thermoplastic elastomer (Tm = 166°C, Tim = 152°C, Temp = 169°C) used was changed from 10 parts to 20 parts. The total graft weight of maleic anhydride in the modified polyolefin resin composition was 2.9% by weight, with the total amount of the modified polyolefin resin being 100% by weight.
[0064] Example 3 A modified polyolefin resin composition was obtained in the same manner as in Example 1, except that 10 parts of a polyolefin thermoplastic elastomer (Tm = 164°C, Tim = 153°C, Temp = 170°C) was used instead of 10 parts of a polyolefin thermoplastic elastomer (Tm = 166°C, Tim = 152°C, Temp = 169°C). The total graft weight of maleic anhydride in the modified polyolefin resin composition was 3.4% by weight, with the total amount of the modified polyolefin resin being 100% by weight.
[0065] Example 4 A modified polyolefin resin composition was obtained in the same manner as in Example 1, except that 10 parts of a propylene homopolymer (Tm = 156°C, Tim = 152°C, Temp = 165°C) was used instead of 10 parts of a polyolefin thermoplastic elastomer (Tm = 166°C, Tim = 152°C, Temp = 169°C). The total graft weight of maleic anhydride in the modified polyolefin resin composition was 3.1% by weight, with the total amount of the modified polyolefin resin being 100% by weight.
[0066] Example 5 A modified polyolefin resin composition (1) was obtained in the same manner as in Example 1, except that the amount of propylene-butene copolymer (Tm = 97°C) used was changed from 90 parts to 100 parts, and no polyolefin-based thermoplastic elastomer (Tm = 166°C, Tim = 152°C, Temp = 169°C) was used. A modified polyolefin resin composition (2) was obtained in the same manner as in Example 1, except that 100 parts of a propylene-ethylene copolymer (Tm = 142°C, Tim = 140°C, Temp = 155°C) was used instead of 90 parts of the propylene-butene copolymer (Tm = 97°C), and no polyolefin-based elastomer (Tm = 166°C, Tim = 152°C, Temp = 169°C) was used. 90 parts of the resin composition (1) as a modified product of component (A) and 10 parts of the resin composition (2) as a modified product of component (B) were kneaded in a twin-screw extruder set at a reaction temperature of 170°C. After kneading, the mixture was cooled to room temperature to obtain a modified polyolefin resin composition. The total graft weight of maleic anhydride in the modified polyolefin resin composition was 3.0% by weight, with the total amount of the modified polyolefin resin being 100% by weight.
[0067] Example 6 Except for not using lauryl methacrylate, a modified polyolefin resin composition was obtained in the same manner as in Example 1. The total graft weight of maleic anhydride in the modified polyolefin resin composition was 2.9% by weight, with the total amount of the modified polyolefin resin being 100% by weight.
[0068] Comparative Example 1 A modified polyolefin resin composition was obtained in the same manner as in Example 1, except that the amount of propylene-butene copolymer (Tm = 97°C) used was changed from 90 parts to 100 parts, and no polyolefin thermoplastic elastomer (Tm = 166°C, Tim = 152°C, Temp = 169°C) was used. The total graft weight of maleic anhydride in the modified polyolefin resin composition was 3.1% by weight, with the total amount of the modified polyolefin resin being 100% by weight.
[0069] Comparative Example 2 A modified polyolefin resin composition was obtained in the same manner as in Example 1, except that 100 parts of a propylene-ethylene copolymer (Tm = 105°C) was used instead of 90 parts of a propylene-butene copolymer (Tm = 97°C) and no polyolefin-based thermoplastic elastomer (Tm = 166°C, Tim = 152°C, Temp = 169°C) was used. The total graft weight of maleic anhydride in the modified polyolefin resin composition was 3.0% by weight, with the total amount of the modified polyolefin resin being 100% by weight.
[0070] Comparative Example 3 A modified polyolefin resin composition was obtained in the same manner as in Example 1, except that 10 parts of a polyolefin thermoplastic elastomer (Tm = 143°C, Tim = 120°C, Temp = 154°C) was used instead of 10 parts of a polyolefin thermoplastic elastomer (Tm = 166°C, Tim = 152°C, Temp = 169°C). The total graft weight of maleic anhydride in the modified polyolefin resin composition was 3.0% by weight, with the total amount of the modified polyolefin resin being 100% by weight.
[0071] Comparative Example 4 A modified polyolefin resin composition was obtained in the same manner as in Example 1, except that 10 parts of a polyolefin thermoplastic elastomer (Tm = 135°C, Tim = 112°C, Temp = 153°C) was used instead of 10 parts of a polyolefin thermoplastic elastomer (Tm = 166°C, Tim = 152°C, Temp = 169°C). The total graft weight of maleic anhydride in the modified polyolefin resin composition was 2.9% by weight, with the total amount of the modified polyolefin resin being 100% by weight.
[0072] Comparative Example 5 A modified polyolefin resin composition was obtained in the same manner as in Example 1, except that 10 parts of a polyolefin thermoplastic elastomer (Tm = 132°C, Tim = 118°C, Temp = 139°C) was used instead of 10 parts of a polyolefin thermoplastic elastomer (Tm = 166°C, Tim = 152°C, Temp = 169°C). The total graft weight of maleic anhydride in the modified polyolefin resin composition was 3.2% by weight, with the total amount of the modified polyolefin resin being 100% by weight.
[0073] Test Example 1: Measurement and Calculation of Average Particle Size of Modified Product of Component (B) The volumetric particle size distribution was measured using a Malvern Mastersizer 3000, and the average particle size was calculated as the volumetric median diameter Dv50 (the maximum particle size below which 50% of the sample volume falls). The measurement sample was prepared by adding a solution sample of the modified polyolefin resin composition obtained in the Examples and Comparative Examples (solid content: 15 wt %, solvent composition: methylcyclohexane / MEK=80 / 20 (w / w)) to a dispersion solvent (solvent composition: methylcyclohexane / MEK=80 / 20 (w / w)) so that the laser scattering intensity was approximately 12%.
[0074] In the measurement sample for measuring particle size distribution, it was confirmed by the following procedure that the modified resin (A) was completely dissolved, while the modified resin (B) was present as particles without dissolving. A 50 g aliquot of a solution sample of the modified polyolefin resin composition obtained in the example (solid content: 15 wt %, solvent composition: methylcyclohexane / MEK = 80 / 20 (w / w)) was placed in a centrifuge tube (250 cc) and centrifuged at 10,000 rpm (centrifugal force 15,600 × g) and 15°C for 3 hours. The resulting supernatant and precipitate were each dried, and then differential scanning calorimetry (DSC) was performed. The melting point peak of resin (A) was observed in the solid obtained from the supernatant, and the melting point peak of resin (B) was observed in the solid obtained from the precipitate (i.e., the solid obtained without dissolving and present as particles). Similarly, Fourier transform infrared spectroscopy (FT-IR) spectra (ATR method) were measured for each of the supernatant and precipitate obtained. Peaks derived from the carbonyl groups of the α,β-unsaturated carboxylic acid anhydride were observed in both the solid obtained from the supernatant and the solid obtained from the precipitate, confirming that the dissolved resin was a modified product of resin (A), and the undissolved resin present as particles was a modified product of resin (B). Details of the melting point measurement by DSC are as follows: According to JIS K7121 (1987), a DSC measurement device (e.g., "DISCOVERY DSC2500," manufactured by TA Instruments Japan) was used to heat approximately 5 mg of a sample to 150°C for 10 minutes, maintaining the sample in a molten state. The sample was then cooled at a rate of 10°C / min and held at a stable temperature of -50°C for 5 minutes. The sample was then heated to 150°C at 10°C / min, and the peak melting temperature was measured upon melting, and this temperature was designated the melting point. The details of the FT-IR (ATR) measurement are as follows: 400 to 4000 cm -1 The infrared absorption spectrum was observed. Analysis was performed using the attached software ("Spectro Manager", JASCO Corporation). Wavenumber: 1700 to 1750 cm -1 The peak appearing at a wave number of 1750 to 1820 cm is attributed to the peak derived from the carbonyl group of the ring-opened α,β-unsaturated carboxylic acid anhydride. -1The peak appearing at 1000 kJ / min was assigned to the peak derived from the carbonyl group of the unopened α,β-unsaturated carboxylic acid anhydride.
[0075] Test Example 2: Measurement of adhesive strength (heat-resistant adhesion) by Tensilon peel test. 0.52 g of HDI isocyanurate (solids 100%, NCO content 20%) as a curing agent was added to and mixed with a solution sample of the modified polyolefin resin composition obtained in the Examples and Comparative Examples (solids: 15%, solvent composition: methylcyclohexane / MEK = 80 / 20 (w / w)), and the resulting adhesive was applied to aluminum foil using a #16 Meyer bar so that the dry resin film thickness was 3 μm. The coating was then dried in a thermostatic oven adjusted to 100°C, and the coated aluminum foil was laminated with a non-oriented polypropylene (CPP) sheet. Thermocompression bonding was performed under conditions of 200°C, 0.1 MPa, and 1 second, followed by aging for 3 days in a thermostatic oven adjusted to 60°C. A test piece was prepared by cutting into a width of 15 mm, and the laminate adhesive strength was measured under the conditions of a peel angle of 180°, a peel rate of 100 mm / min, and an atmosphere of 120°C.
[0076] Test Example 3: Evaluation of solution stability 10 g of a solution sample of the modified polyolefin resin composition obtained in the Examples and Comparative Examples (solid content: 15%, solvent composition: methylcyclohexane / MEK=80 / 20 (w / w)) was placed in a screw tube and allowed to stand at 23° C., and the change in the state of the solution was observed. The evaluation criteria were as follows: a sample that maintained fluidity after standing for one day was rated "G", and a sample that had lost fluidity and was in a gel state or solidified was rated "NG".
[0077] Table 1 below summarizes the melting points, extrapolated melting start temperatures, and extrapolated melting end temperatures of the raw materials used in Examples 1 to 6 and Comparative Examples 1 to 5, as well as the evaluation and measurement results of Test Examples 1 to 3.
[0078] <Test Example 4: Evaluation of water vapor permeability> <Method of preparing evaluation sample> A solution sample of the prepared resin composition (solid content: 15 wt %, solvent composition: methylcyclohexane / MEK=80 / 20 (w / w)) was applied to a polyethylene terephthalate (PET) film with a thickness of 12 μm using a Mayer bar, and then dried at room temperature to prepare an evaluation sample.
[0079] <Evaluation Method> <Calculation Method of Numerical Values> The water vapor transmission rate was measured using an L80-5000 model manufactured by Lyssy. Measurement conditions were 40°C and 90% RH, with the sample set so that the coated surface faced the detector (low humidity side). Measurements were performed in accordance with JIS K 7129-1 (humidity sensor method), and water vapor transmission rate measurements were obtained. Based on the results of a 12 μm-thick PET film single layer and each evaluation sample, the water vapor transmission rate of each evaluation sample (a sample having a layer structure of 12 μm-thick PET film / coating film) was calculated to determine the thickness of the PET film in μm. The difference between the calculated value and the 12 μm thickness of the coated PET film was then taken to calculate the water vapor transmission rate of the coating film itself. The thickness of the coating film at the locations of the evaluation sample actually used for measurement was measured at three points using a JIS paper thickness measuring instrument MEI-10 manufactured by CITIZEN Watch Co., Ltd., and the average value was taken to calculate the average film thickness of the measured locations. From the calculated permeation amount of the coating film itself and the average film thickness of the measured locations, the water vapor permeation amount (g / (m)) when the resin composition is assumed to be a 30 μm film was calculated. 2 The results of Test Example 4 are summarized in Table 2 below.
[0080] The abbreviations in Table 1 have the following meanings: Tim: extrapolated melting start temperature Tem: extrapolated melting end temperature Adhesion strength: Tensilon peel test adhesion strength
[0081]
[0082]
[0083] From the above results, it can be seen that the resin composition of the present invention, which contains a modified product obtained by modifying a polyolefin resin (A) having a melting point of 100°C or less with an α,β-unsaturated carboxylic acid and / or a derivative thereof, and a modified product obtained by modifying a polyolefin resin (B) having an extrapolated melting onset temperature (Tim) of 120°C or more with an α,β-unsaturated carboxylic acid and / or a derivative thereof, wherein the modified product of component (B) is dispersed in the modified product of component (A), and the average particle size of the modified product of component (B) is 0.1 to 100 μm, can exhibit excellent heat resistance and excellent solution stability to poorly adhesive substrates such as polypropylene sheets and metal materials. It can also be seen that the resin compositions of the examples have significantly lower water vapor permeation rates than the resin composition of Comparative Example 1.
Claims
1. A resin composition comprising: a modified product obtained by modifying polyolefin resin (A) having a melting point of 100°C or less, as measured in accordance with JIS K7121-1987 at a heating rate of 10°C / min using a differential scanning calorimeter, with one or more compounds selected from the group consisting of α,β-unsaturated carboxylic acids and their derivatives; and a modified product obtained by modifying polyolefin resin (B) having an extrapolated melting onset temperature (Tim) of 120°C or more, as measured in accordance with JIS K7121-1987 at a heating rate of 10°C / min using a differential scanning calorimeter, with one or more compounds selected from the group consisting of α,β-unsaturated carboxylic acids and their derivatives, wherein the modified product of resin (B) is dispersed in the modified product of resin (A), and the average particle size of the modified product of resin (B) is 0.1 to 100 μm.
2. The resin composition according to claim 1, wherein the one or more compounds selected from the group consisting of α,β-unsaturated carboxylic acids and derivatives thereof include maleic anhydride.
3. The resin composition according to claim 1, wherein the one or more compounds selected from the group consisting of α,β-unsaturated carboxylic acids and derivatives thereof include a (meth)acrylic acid ester.
4. The resin composition according to claim 1, wherein the melting point of resin (B) is 140 to 200°C, as measured at a heating rate of 10°C / min using a differential scanning calorimeter in accordance with JIS K7121-1987.
5. The resin composition according to claim 1, wherein the mass ratio of the modified resin (A) to the modified resin (B) is (modified resin (A) : (modified resin (B)))=50:50 to 95:
5.
6. The resin composition according to claim 1, wherein the difference (Tem-Tim) between the extrapolated melting end temperature (Tem) and the extrapolated melting onset temperature (Tim) of resin (B) measured at a heating rate of 10°C / min using a differential scanning calorimeter in accordance with JIS K7121-1987 is 5 to 20°C.
7. The resin composition according to claim 1, further comprising a hydrophobic solvent.
8. A primer comprising the resin composition according to any one of claims 1 to 7.
9. An adhesive comprising the resin composition according to any one of claims 1 to 7.
10. A paint comprising the resin composition according to any one of claims 1 to 7.
11. An ink comprising the resin composition according to any one of claims 1 to 7.
12. A method for producing a resin composition according to any one of claims 1 to 7, comprising: (1) a step of simultaneously modifying a mixture of resin (A) and resin (B) with one or more compounds selected from the group consisting of α,β-unsaturated carboxylic acids and derivatives thereof to obtain the resin composition; or (2) a step of modifying resin (A) with one or more compounds selected from the group consisting of α,β-unsaturated carboxylic acids and derivatives thereof to obtain a modified product of resin (A), a step of modifying resin (B) with one or more compounds selected from the group consisting of α,β-unsaturated carboxylic acids and derivatives thereof to obtain a modified product of resin (B), and a step of mixing the modified product of resin (A) and the modified product of resin (B) obtained to obtain the resin composition.
Citation Information
Patent Citations
Modified polyolefin resin composition and its use
JP2001279048A
Modified polyolefin resin and uses thereof
WO2008013085A1
Adhesive composition and thermally adhesive member using same
WO2012090646A1
Olefin resin, method for producing same, composition, molded product and laminate
WO2017057724A1
Modified polyolefin resin and use of same
WO2022024476A1