Sealing material composition and sealing material

A silicone polymer-based sealing material composition with polysiloxane compounds and a vulcanizing agent addresses the limitations of existing materials by offering enhanced low-temperature and plasma resistance properties, suitable for semiconductor manufacturing, at a lower cost than perfluoroelastomers.

WO2024203645A1PCT designated stage expired Publication Date: 2024-10-03VALQUA LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010819
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current sealing materials, such as silicone rubber and fluorosilicone rubber, are limited in their low-temperature performance and plasma resistance, making them unsuitable for environments below -65°C, while perfluoroelastomers are expensive and inefficient at low temperatures, necessitating a more cost-effective solution with improved properties for semiconductor manufacturing equipment.

Method used

A sealing material composition incorporating a silicone polymer with a polysiloxane compound containing unsubstituted or substituted aromatic monovalent hydrocarbon groups, combined with a vulcanizing agent and optionally a perfluoropolyether compound, to achieve low glass transition temperatures and enhanced plasma resistance, suitable for use in semiconductor manufacturing equipment.

Benefits of technology

The proposed solution provides a sealing material with improved low-temperature characteristics and plasma resistance, comparable to or exceeding that of perfluoroelastomers, while being more cost-effective, suitable for environments as low as -70 to 150°C, and maintaining a weight loss rate of 1.0% or less in plasma resistance tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The present disclosure relates to: a sealing material composition which contains a silicone polymer and a vulcanizing agent, with the silicone polymer containing a polysiloxane-based compound having an unsubstituted or substituted monovalent aromatic hydrocarbon group in a side chain, and which exhibits plasma resistance in order to be used in a semiconductor production apparatus; a sealing material; a gate seal for a semiconductor production apparatus; and a semiconductor production apparatus. According to the present disclosure, provided is a sealing material composition which can be used in a low temperature environment, exhibits plasma resistance, and can produce a sealing material for a semiconductor production apparatus using relatively inexpensive materials.
Need to check novelty before this filing date? Find Prior Art

Description

Sealing material composition and sealing material

[0001] The present invention relates to a sealing material composition, and further relates to a sealing material, sealing materials in general including gate seals for semiconductor manufacturing equipment containing the same, and semiconductor manufacturing equipment.

[0002] Japanese Patent Laid-Open No. 2001-002923 (Patent Document 1) and Japanese Patent Laid-Open No. 2018-016795 (Patent Document 2) propose a fluorosilicone rubber composition and a perfluoroelastomer composition, respectively, for use in sealing materials.

[0003] JP 2001-002923 A JP 2018-016795 A

[0004] Low-temperature etching processes in low-temperature environments have been confirmed to be effective as one means for achieving circuit miniaturization and high integration in the semiconductor field. Generally, silicone rubber and fluorosilicone rubber are often used as sealing materials in low-temperature environments. However, silicone rubber, which is commonly used as a sealing material, can only be used at temperatures of approximately −45°C, and even fluorosilicone rubber, which has relatively good low-temperature properties, can only be used at temperatures up to −65°C, meaning that its low-temperature properties are insufficient. Therefore, there is a demand for sealing materials that can be used in environments with even lower temperatures (e.g., −70 to −100°C).

[0005] On the other hand, perfluoroelastomers, which have plasma resistance, are often used for sealing materials used in plasma-based environments. However, perfluoroelastomers are very expensive and have relatively poor low-temperature properties, making them difficult to use in low-temperature environments.

[0006] An object of the present invention is to provide a sealing material composition that can be used in low-temperature environments and has plasma resistance, and that can be used to produce a sealing material for semiconductor manufacturing equipment using relatively inexpensive materials. Another object of the present invention is to provide a sealing material composition containing a silicone polymer that has a relatively low glass transition temperature and that shows a suppressed decrease in weight loss rate in a plasma resistance test, and that can be used to produce a sealing material for semiconductor manufacturing equipment.

[0007] The present invention provides the following sealing material composition, sealing material, gate seal for semiconductor manufacturing equipment, and semiconductor manufacturing equipment. [1] A plasma-resistant sealing material composition for use in semiconductor manufacturing equipment, comprising a silicone polymer and a vulcanizing agent, wherein the silicone polymer comprises a polysiloxane-based compound having an unsubstituted or substituted aromatic monovalent hydrocarbon group in a side chain. [2] The polysiloxane-based compound is represented by the following formula (1): [In the formula, R 1 R independently represents an unsubstituted or substituted aromatic monovalent hydrocarbon group; 2 each independently represents an unsubstituted or substituted aromatic monovalent hydrocarbon group, an unsubstituted or substituted unsaturated or saturated hydrocarbon group not containing an aromatic hydrocarbon group, an alkoxy group, a hydroxy group, or a hydrogen atom, and n represents an integer of 1 to 7000. [3] The sealing material composition according to [2], wherein the proportion of the structural unit represented by formula (1) in the polysiloxane compound is 1 to 70 mol %. [4] The polysiloxane compound has a main chain terminal at which a structural unit represented by (R 3 ) 3 Si-R 4 - [wherein, R 3 each independently represents an unsubstituted or substituted aromatic monovalent hydrocarbon group, an unsubstituted or substituted unsaturated or saturated hydrocarbon group not containing an aromatic hydrocarbon group, an alkoxy group, or a hydroxy group; R 4 [5] The sealing material composition according to any one of [1] to [3], wherein the polysiloxane compound has a group represented by the following formula (2): [In the formula, R 5 and R 6

[0023] The sealant composition according to any one of [1] to [4], containing a structural unit represented by the formula:

[0024] where each independently represents an unsubstituted or substituted, unsaturated or saturated hydrocarbon group, an alkoxy group, or a hydroxy group that does not contain an aromatic hydrocarbon group, and o represents an integer of 100 to 10,000. [6] The sealant composition according to any one of [1] to [5], wherein the polysiloxane compound has a vinyl group in at least one of a side chain and an end of the main chain. [7] The sealant composition according to any one of [1] to [6], further containing at least one of 1 to 160 parts by mass of a filler and 0.05 to 3 parts by mass of a pigment per 100 parts by mass of the silicone polymer. [8] The sealant composition according to any one of [1] to [7], wherein the vulcanizing agent comprises a peroxide-based compound. [9] The sealant composition according to any one of [1] to [8], wherein the content of the vulcanizing agent is 0.2 to 8 parts by mass per 100 parts by mass of the silicone polymer.

[10] The sealing material composition according to any one of [1] to [9], further comprising a perfluoropolyether-based compound.

[11] The sealing material composition according to any one of [1] to

[10] , having a metal ion content of 1000 ppm or less.

[12] A sealing material comprising a crosslinked product of the sealing material composition according to any one of [1] to

[11] .

[13] A gate seal for semiconductor manufacturing equipment, comprising the sealing material according to

[12] .

[14] A semiconductor manufacturing equipment, comprising the sealing material according to

[12] .

[0008] According to the present invention, it is possible to provide a sealing material composition that can be used in low-temperature environments, has excellent plasma resistance, and can be used to produce a sealing material for semiconductor manufacturing equipment using relatively inexpensive materials.The present invention provides a sealing material composition that contains a silicone polymer and has a relatively low glass transition temperature and exhibits a suppressed decrease in weight loss rate in a plasma resistance test, and can be used to produce a sealing material for semiconductor manufacturing equipment.

[0009] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the following embodiments.

[0010] <Sealing Material Composition> A sealing material composition according to one embodiment of the present invention is a plasma-resistant sealing material composition for use in semiconductor manufacturing equipment. The sealing material composition includes a silicone polymer and a vulcanizing agent. The silicone polymer includes a polysiloxane-based compound (hereinafter also referred to as a first polysiloxane-based compound) having an unsubstituted or substituted aromatic monovalent hydrocarbon group in its side chain. The present inventors have discovered that a sealing material composition having low-temperature properties and plasma resistance can be obtained, even though the first polysiloxane-based compound is a relatively inexpensive material. In this specification, "having plasma resistance" means that the weight loss rate (%) in the plasma resistance test described below is 1.0% or less. The use of the sealing material composition of the present invention allows the preparation of a sealing material that exhibits plasma resistance comparable to or superior to that of a sealing material composition containing a perfluoroelastomer. Furthermore, the use of the sealing material composition of the present invention allows the preparation of a sealing material that exhibits a weight loss rate comparable to or smaller than that of a sealing material composition containing a perfluoroelastomer in the plasma resistance test described below.

[0011] The first polysiloxane compound may have one or more unsubstituted or substituted aromatic monovalent hydrocarbon groups on the Si atoms that make up the main chain. In this specification, the polysiloxane compound is a compound having a skeleton (main chain) formed by a plurality of siloxane bonds (—Si—O—Si—).

[0012] Examples of unsubstituted aromatic monovalent hydrocarbon groups include aryl groups such as phenyl and tolyl; and aralkyl groups such as benzyl and phenylethyl. Substituted aromatic monovalent hydrocarbon groups may be aromatic monovalent hydrocarbon groups in which some or all of the hydrogen atoms of the groups exemplified as the unsubstituted aromatic monovalent hydrocarbon groups have been substituted with halogen atoms such as fluorine or chlorine, such as a chlorophenyl group. From the viewpoint of low-temperature properties and plasma resistance, a phenyl group is preferred. The first polysiloxane compound preferably has a diphenylsilyl group in which two phenyl groups are bonded to one Si atom constituting the main chain.

[0013] The first polysiloxane compound is represented by the following formula (1): [In the formula, R 1 R independently represents an unsubstituted or substituted aromatic monovalent hydrocarbon group; 2 independently represent an unsubstituted or substituted aromatic monovalent hydrocarbon group, an unsubstituted or substituted unsaturated or saturated hydrocarbon group that does not contain an aromatic hydrocarbon group, an alkoxy group, a hydroxy group, or a hydrogen atom, and n represents an integer of 1 to 7000.

[0014] R 1 and R 2 Examples of the unsubstituted or substituted aromatic monovalent hydrocarbon group in R are the same as those listed above. 2 Examples of the unsubstituted saturated hydrocarbon group not containing an aromatic hydrocarbon group in R include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, hexyl, cyclohexyl, octyl, decyl, and dodecyl. 2 Examples of the unsubstituted unsaturated hydrocarbon group not containing an aromatic hydrocarbon group in R include alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, butenyl, and isobutenyl. 1 From the viewpoint of low temperature characteristics and plasma resistance, R is preferably a phenyl group. 2 The substituted unsaturated or saturated hydrocarbon group not containing an aromatic hydrocarbon group in R may be a group in which some or all of the hydrogen atoms of the groups exemplified as the unsubstituted unsaturated or saturated hydrocarbon group not containing an aromatic hydrocarbon group are substituted with halogen atoms such as fluorine or chlorine, and examples thereof include a chloromethyl group and a 3,3,3-trifluoropropyl group. 2 Examples of the alkoxy group in R include a methoxy group, an ethoxy group, a propoxy group, and a butoxy group. 1 From the viewpoint of low temperature characteristics and plasma resistance, R is preferably a phenyl group. 2 In terms of low temperature characteristics and plasma resistance, a phenyl group is preferred.

[0015] The ratio of the first constitutional unit in the first polysiloxane compound may be, for example, 1 to 70 mol %, and from the viewpoint of low temperature characteristics and plasma resistance, is preferably 2 to 65 mol %, and more preferably 3 to 60 mol %.

[0016] The first polysiloxane compound has a main chain terminal having (R 3 ) 3 Si-R 4 - [wherein, R 3 each independently represents an unsubstituted or substituted aromatic monovalent hydrocarbon group, an unsubstituted or substituted unsaturated or saturated hydrocarbon group not containing an aromatic hydrocarbon group, an alkoxy group, or a hydroxy group; R 4 R independently represent an oxygen atom or an alkylene group having 1 to 5 carbon atoms (hereinafter also referred to as a terminal group). 3 The above-mentioned examples are applicable to the unsubstituted or substituted aromatic monovalent hydrocarbon group, the unsubstituted or substituted unsaturated or saturated hydrocarbon group not containing an aromatic hydrocarbon group, and the alkoxy group in R. 4 Examples of the alkylene group having 1 to 5 carbon atoms in R include a methylene group, an ethylene group, and a propylene group. 3 R is preferably a methyl group, a methoxy group, or a hydroxy group. 4 is preferably an oxygen atom or an ethylene group.

[0017] The first polysiloxane compound is represented by the following formula (2): [In the formula, R 5 and R 6 each independently represents an unsubstituted or substituted, unsaturated or saturated hydrocarbon group that does not contain an aromatic hydrocarbon group, an alkoxy group, or a hydroxy group, and o represents an integer of 100 to 10,000. The proportion of the second constitutional unit in the first polysiloxane compound may be, for example, 30 to 99 mol %.

[0018] R 5 and R 6The above-mentioned examples are applicable to examples of the unsubstituted or substituted unsaturated or saturated hydrocarbon group and alkoxy group not containing an aromatic hydrocarbon group in the second constitutional unit, R 5 and R 6 At least one of R is preferably an unsubstituted unsaturated hydrocarbon group that does not contain an aromatic hydrocarbon group, and more preferably a vinyl group. 5 and R 6 When either one of the above is an unsubstituted unsaturated hydrocarbon group containing no aromatic hydrocarbon group, the other is preferably an unsubstituted saturated hydrocarbon group containing no aromatic hydrocarbon group, and more preferably a methyl group.

[0019] The first polysiloxane compound preferably has a vinyl group on at least one of the side chain and the terminal of the main chain. When the first polysiloxane compound has a vinyl group on at least one of the side chain and the terminal of the main chain, the first polysiloxane compound can have one or more vinyl groups. When the first polysiloxane compound has a vinyl group on at least one of the side chain and the terminal of the main chain, the proportion of the structural unit having a vinyl group in the first polysiloxane compound may be, for example, 0.001 to 10 mol %, and the lower limit of the proportion of the structural unit may be, for example, 0.005 mol %, 0.01 mol %, 0.05 mol %, or 0.1 mol %, and the upper limit of the proportion of the structural unit may be, for example, 8 mol %, 6 mol %, or 4 mol %.

[0020] The first polysiloxane compound is preferably a compound represented by the following formula (3): In formula (3), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , o and n are as defined above.

[0021] The first polysiloxane compound is more preferably a compound represented by the following formula (4): In formula (4), R 3and n are as defined above. p and q independently represent an integer, and the sum of p and q can be 100 to 10,000. The sum of p and q may be, for example, 1,000 to 10,000, or 2,000 to 10,000, or 3,000 to 10,000, or 5,000 to 10,000. The sum of p, q, and n may be, for example, 1,000 to 10,000, or 2,000 to 10,000, or 3,000 to 10,000, or 5,000 to 10,000.

[0022] The first polysiloxane compound may be a copolymer containing the first structural unit. The first polysiloxane compound can be obtained by copolymerizing a copolymerizable component containing the first structural unit with another copolymerizable component (e.g., a copolymerizable component containing the second structural unit). The compound represented by formula (4) can be obtained, for example, by copolymerizing a dimethylsiloxane copolymerization component, a diphenylsiloxane copolymerization component, and a methylvinylsiloxane copolymerization component.

[0023] The first polysiloxane compound can be used in the form of a silicone rubber compound filled with silica, as described below. Examples of commercially available products include "KE-186-U," "KE-183-U," and "KE-136Y-U" manufactured by Shin-Etsu Chemical Co., Ltd., and "SE-955-U" manufactured by Dow-Toray Industries, Inc.

[0024] The silicone polymer can contain one or more first polysiloxane compounds. The silicone polymer can also contain a polysiloxane compound other than the first polysiloxane compound (hereinafter also referred to as a second polysiloxane compound). Examples of the second polysiloxane compound include dimethyl silicone, vinyl methyl silicone, and fluorovinyl methyl silicone. The silicone polymer preferably contains only the first polysiloxane compound. Furthermore, the silicone polymer can also be used as a blend rubber with other rubbers, as long as the objectives of the present invention are not impaired.

[0025] As the vulcanizing agent, for example, a peroxide compound can be used. The peroxide compound is not particularly limited as long as it can be used in silicone polymers, and examples thereof include benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, di-tert-butyl peroxide, tert-butylcumyl peroxide, dicumyl peroxide, 1,1-di(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, 1,3-di(tert-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, tert-butylperoxybenzoate, tert-butylperoxyisopropyl carbonate, and n-butyl-4,4-di(tert-butylperoxy)valerate. The vulcanizing agent may contain one or more peroxide compounds.

[0026] The content of the vulcanizing agent in the sealing material composition may be, for example, 0.2 to 8 parts by mass, and preferably 0.5 to 4 parts by mass, per 100 parts by mass of the silicone polymer.

[0027] The sealing material composition may further contain a perfluoropolyether-based compound. The perfluoropolyether-based compound may be a low-molecular-weight compound such as an oligomer, or a high-molecular-weight compound such as a polymer. Among these, a perfluoropolyether-based polymer is preferred in terms of low-temperature properties and plasma resistance. The perfluoropolyether-based polymer may have, for example, a group capable of crosslinking with a silicone polymer at the end of the main chain. Commercially available perfluoropolyether-based polymers can be used. Examples of commercially available perfluoropolyether-based polymers include Cyfel (registered trademark) (manufactured by Shin-Etsu Chemical Co., Ltd.). The content of the perfluoropolyether-based polymer in the sealing material composition may be, for example, 0.5 to 50 parts by mass, preferably 1 to 25 parts by mass, per 100 parts by mass of the silicone polymer.

[0028] The sealing material composition may contain additives other than the above components, such as pigments, fillers, antioxidants, antioxidants, vulcanization accelerators, processing aids (such as stearic acid), stabilizers, tackifiers, silane coupling agents, plasticizers, flame retardants, mold release agents, waxes, and lubricants. Another example of an additive is a tackiness reducer (preventer) such as fluorine-based oil (such as perfluoroether). Only one type of additive may be used, or two or more types may be used in combination.

[0029] Examples of pigments include at least one selected from the group consisting of inorganic pigments and organic pigments. Inorganic pigments include white pigments (e.g., silica, zinc oxide, white lead, lithopone, titanium dioxide, precipitated barium sulfate, and baryte powder), red pigments (e.g., red lead, iron oxide red), yellow pigments (e.g., yellow lead, zinc yellow), blue pigments (e.g., ultramarine blue, Prussian blue, YInMn blue), and black pigments (e.g., carbon black). Organic pigments include azo pigments (azo lake pigments, insoluble azo pigments, condensed azo pigments, etc.); anthraquinone pigments, thioindigo pigments, perinone pigments, perylene pigments, quinacridone pigments, isoindolinone pigments, isoindoline pigments, dioxazine pigments, quinophthalone pigments, and polycyclic pigments such as diketopyrrolopyrrole pigments; and phthalocyanine pigments. Organic pigments classified as pigments in the Color Index can be used. The pigment preferably used is an organic pigment that does not contain metal elements. Organic pigments that do not contain metal elements are unlikely to cause substances derived from metal elements to scatter even when the sealing material is used in a harsh plasma environment or ozone environment, such as in semiconductor applications, and the annular sealing material is etched. When the sealing material composition contains a pigment, the content of the pigment in the sealing material composition may be, for example, 0.05 to 3 parts by mass per 100 parts by mass of the silicone polymer.

[0030] Examples of fillers include silica, quartz powder, clay, talc, diatomaceous earth, barium sulfate, mica, graphite, aluminum hydroxide, aluminum silicate, calcium silicate, hydrotalcite, calcium oxide, titanium oxide, zinc oxide, iron oxide, alumina, magnesium carbonate, calcium carbonate, zinc carbonate, carbon black, granular or powdered resins (such as fluororesins), metal powders, glass powders, and ceramic powders. The inclusion of a filler in the sealing material composition is advantageous from the viewpoint of improving the mechanical strength of the sealing material. The filler is preferably at least one selected from the group consisting of silica, carbon black, and fluororesins.

[0031] Examples of silica include fumed silica, precipitated silica, and fused silica. When the sealing material composition contains silica, the content of silica in the sealing material composition may be, for example, 6 to 120 parts by mass per 100 parts by mass of silicone polymer. When the sealing material composition contains silica, a silicone rubber compound in which silica is blended with a silicone polymer can be used. As the silicone rubber compound, "KE-186-U" manufactured by Shin-Etsu Chemical Co., Ltd., "SE-955-U" manufactured by Dow-Toray, Inc., and the like can be used as is. Furthermore, the silicone rubber can also be blended with other rubbers within a range that does not impair the object of the present invention.

[0032] Examples of carbon black include MT carbon. The sealing material composition preferably does not contain a metal-based filler, in view of preventing filler scattering during use in semiconductor manufacturing equipment. When the sealing material composition contains carbon black, the content of carbon black in the sealing material composition may be, for example, 1 to 30 parts by mass per 100 parts by mass of the silicone polymer.

[0033] When the sealing material composition contains a fluororesin filler, it tends to be advantageous in improving plasma resistance. The fluororesin can be contained in the sealing material composition, for example, as fluororesin particles. When the sealing material composition contains a fluororesin filler, the content of the fluororesin filler in the sealing material composition may be, for example, 1 to 30 parts by mass, preferably 5 to 25 parts by mass, and more preferably 10 to 20 parts by mass, per 100 parts by mass of the silicone polymer.

[0034] The fluororesin used as a filler is a resin having fluorine atoms in the molecule, and can be, for example, polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-ethylene copolymer (ETFE), polychlorotrifluoroethylene (PCTFE), chlorotrifluoroethylene-ethylene copolymer (ECTFE), polyvinylidene fluoride (PVDF), polyvinyl fluoride (PVF), vinylidene fluoride-hexafluoropropylene copolymer (VDF-HFP copolymer), vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer (VDF-HFP-TFE copolymer), etc. One type of fluororesin may be used alone, or two or more types may be used in combination.

[0035] Among the above, it is preferable to use fluororesins with a relatively high melting point, such as PFA and PTFE, from the viewpoint of preventing the resin from melting in a high-temperature environment and impairing properties such as compression set.

[0036] The fluororesin used as the filler may contain a functional group. The functional group can be introduced, for example, by copolymerizing a monomer having the functional group. When the above-mentioned crosslinking site monomer is copolymerized as the functional group-containing monomer, crosslinking between the fluororesin and the perfluoroelastomer also proceeds with the crosslinking agent, thereby further increasing the mechanical strength of the crosslinked product of the sealing material composition. An example of a fluororesin containing a functional group is the nitrile group-containing polytetrafluoroethylene described in JP 2013-177631 A. The fluororesin can also be a modified fluororesin, such as "TFM-modified PTFE" (manufactured by Dyneon).

[0037] When the sealing material composition contains a silicone polymer and a fluororesin filler, the silicone polymer and the fluororesin can be kneaded together by, for example, 1) kneading the silicone polymer and the fluororesin using a mixing roll, or 2) kneading the silicone polymer and the fluororesin using an apparatus such as a mixer or a twin-screw extruder.

[0038] When the sealing material composition contains a filler, the content of the filler in the sealing material composition (the total content when two or more types of filler are contained) may be, for example, 1 to 160 parts by mass, preferably 1 to 100 parts by mass, and more preferably 1 to 80 parts by mass, per 100 parts by mass of the silicone polymer.

[0039] The sealing material composition may have a metal ion content of, for example, 1000 ppm or less, 300 ppm or less, 100 ppm or less, or 50 ppm or less. When the metal ion content of the sealing material composition is within the above range, the sealing material composition is suitable as a sealing material used in semiconductor manufacturing equipment that performs plasma treatment.

[0040] The sealing material composition can be prepared by uniformly kneading a silicone polymer, a vulcanizing agent, and optionally added pigments, silica, etc. Conventional kneaders such as a mixing roll, a pressure kneader, and an internal mixer (Banbury mixer) can be used. The components may be mixed and kneaded at once, or they may be kneaded in multiple stages, such as first uniformly kneading the components excluding those that contribute to the crosslinking reaction (e.g., crosslinking accelerator, crosslinking retarder, crosslinking agent), and then kneading the components that contribute to the crosslinking reaction.

[0041] The seal of the present invention includes a crosslinked product of the above-mentioned seal composition. The seal can be produced by crosslinking (vulcanizing) and molding the rubber composition for the seal. The crosslinking and molding methods can be conventionally known methods such as injection molding, compression molding, and transfer molding.

[0042] The heating temperature (primary crosslinking temperature) during molding may be, for example, 100°C or higher and 220°C or lower, and the heating time (primary crosslinking time) may be, for example, 0.5 minutes or higher and 120 minutes or lower. After vulcanization molding, secondary crosslinking may be performed. The secondary crosslinking temperature may be, for example, 120°C or higher and 280°C or lower, and the secondary crosslinking time may be, for example, 0.5 hours or higher and 24 hours or lower.

[0043] The usable temperature range of the sealing material may be, for example, −70 to 150° C., preferably −100 to 200° C., and more preferably −130 to 230° C. In this specification, the usable temperature of the sealing material can be evaluated by measuring the glass transition temperature, which will be explained in the Examples section below.

[0044] The hardness (type A durometer hardness) of the sealing material may be, for example, about 25 to 90. Having the hardness of the sealing material in the above range is preferable in terms of ease of installation in semiconductor manufacturing equipment and airtightness.

[0045] The sealing material may have a weight loss rate (%) of, for example, 1.0% or less in a plasma resistance test. The plasma resistance test may be performed according to the method described in the Examples section below. The sealing material preferably has a weight loss rate (%) of 0.8% or less, more preferably 0.6% or less in a plasma resistance test. The weight loss rate of the sealing material of the present invention may be comparable to or smaller than that of a sealing material containing a perfluoroelastomer in a plasma resistance test.

[0046] Another aspect of the present invention is a sealant containing a crosslinked product of the above-mentioned sealant composition. The sealant of the present invention may be a sealant for semiconductor manufacturing equipment, and in particular, because it has plasma resistance, it is suitable as a sealant for fixed parts or moving parts of a vacuum chamber in semiconductor manufacturing equipment where plasma processing is performed. Furthermore, the sealant of the present invention can exhibit plasma resistance comparable to or superior to that of sealants containing perfluoroelastomers, and is therefore suitable for semiconductor manufacturing equipment in which sealants containing perfluoroelastomers are used. Examples of the use form of the sealant include various sealants such as rings, packings, and gaskets.

[0047] Another aspect of the present invention is a semiconductor manufacturing apparatus including the above-described sealant. The semiconductor manufacturing apparatus of the present invention includes, in addition to semiconductor manufacturing apparatus, for example, liquid crystal panel manufacturing apparatus, plasma panel manufacturing apparatus, plasma display panel manufacturing apparatus, plasma addressed liquid crystal panel manufacturing apparatus, organic EL panel manufacturing apparatus, field emission display panel manufacturing apparatus, solar cell substrate manufacturing apparatus, semiconductor conveying apparatus, etc.

[0048] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and mass parts unless otherwise specified.

[0049] Examples 1 to 10 and Comparative Examples 1 to 5 Sealing material compositions were prepared according to the following procedure, and then sealing materials were produced. First, predetermined amounts of each compounding ingredient were kneaded using an open roll according to the formulation shown in Table 1 (the units of blending amounts in Table 1 are parts by mass). Next, the resulting sealing material compositions were press-molded at 120°C for 20 minutes, and then subjected to secondary thermal crosslinking at 200°C for 4 hours to obtain sealing materials.

[0050]

[0051] The details of the ingredients in Table 1 are as follows: PVMQ1: Phenyl vinyl methyl silicone, "KE-186-U", Shin-Etsu Chemical Co., Ltd. PVMQ2: Phenyl vinyl methyl silicone, "KE-183-U", Shin-Etsu Chemical Co., Ltd. PVMQ3: Phenyl vinyl methyl silicone, "KE-136Y-U", Shin-Etsu Chemical Co., Ltd. PVMQ4: Phenyl vinyl methyl silicone, "SE-955-U", Dow-Toray Co., Ltd. Crosslinker 1: Paramethylbenzoyl peroxide, "C-23N", Shin-Etsu Chemical Co., Ltd. Crosslinker 2: Bis(4-methylbenzoyl) peroxide, "RC14", Dow-Toray Co., Ltd. Crosslinker 3: 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, "C-8A", Shin-Etsu Chemical Co., Ltd. Filler 1: PTFE, "Lubron L5", Daikin Industries, Ltd. Additive 1: Perfluoropolyether compound, "Cyfel 8070A", Shin-Etsu Chemical Co., Ltd. Additive 2: Perfluoropolyether compound, "Cypher 8070B", Shin-Etsu Chemical Co., Ltd. Pigment 1: "Violet #V4879", Resino Color Kogyo Co., Ltd.

[0052]

[0053] The details of the ingredients in Table 2 are as follows: FVMQ: Fluorosilicone compound, "FE-271-U", Shin-Etsu Chemical Co., Ltd. VMQ1: Silicone rubber compound, "KE-971-U", Shin-Etsu Chemical Co., Ltd. VMQ2: Silicone rubber compound, "KE-951-U", Shin-Etsu Chemical Co., Ltd. FFKM: Perfluoroelastomer, "PFE191T", 3M FKM: Fluoro rubber, "Dai-el G783", Daikin Industries, Ltd. Crosslinker 4: 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, "C-8A", Shin-Etsu Chemical Co., Ltd. Crosslinker 5: Benzoyl peroxide, "C1A", Shin-Etsu Chemical Co., Ltd. Crosslinker 6: 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, Tokyo Chemical Industry Co., Ltd. Acid acceptor 1: Magnesium oxide, "Kyowamag MA150", Kyowa Chemical Industry Co., Ltd. Acid acceptor 2: calcium hydroxide, "CALDIC #2000", Omi Chemical Industry Co., Ltd. Filler 2: MT carbon, "Thermax N990", Cancarb Pigment 2: "Ferrow Blue V-3285", Fellow Japan Pigment 3: "KE-COLOR-BR", Shin-Etsu Chemical Co., Ltd.

[0054] (Evaluation of sealing material) The obtained crosslinked molded articles (sealing materials) were evaluated as follows. The results are shown in Table 1.

[0055] [1] Measurement of Glass Transition Temperature The obtained molded body was measured in an air environment using a DVA-225 (manufactured by IT Measurement & Control Co., Ltd.) at a measurement temperature of -150 to 150°C, a temperature increase rate of 2°C / min, a frequency of 1 Hz, and a measurement mode of tension. The glass transition temperature was taken as the peak value of tan δ. The glass transition temperature is a temperature that serves as an indicator of the low-temperature use range of a sealing material. The lower the glass transition temperature, the more advantageous it is for use in a low-temperature environment.

[0056] [2] Plasma Resistance Test The plasma resistance (weight loss rate) of the obtained molded body was measured. Specifically, it was measured as follows. Using a flat-plate plasma treatment device with an electrode diameter of φ240 mm, RF: 250 W, O 2 Gas and CF 4 Gas flow rate ratio (O 2 :CF4 The obtained molded body was irradiated with plasma for 1 hour under the conditions of: 180:20, gas flow rate: 200 sccm, and vacuum level: 133 Pa. Next, the weight of the molded body was measured before and after the test, and the weight loss rate (%) was calculated using the following formula to evaluate plasma resistance. The smaller the weight loss rate, the better the plasma resistance. Weight loss rate (%) = [(weight of molded body before test - weight of molded body after test) / weight of molded body before test] x 100

[0057] [3] Measurement of Metal Ion Content The obtained molded body was washed with dilute acid and then incinerated with nitric acid. After adding concentrated acid and concentrating by heating, dilute acid (recovered liquid) was added and subjected to a heat recovery operation. The liquid was transferred to a fluororesin container and subjected to qualitative analysis by ICP mass spectrometry. An internal standard element had been added to the recovered liquid in advance. Measurements were performed using an ICP-MS Agilent 750OCS (manufactured by Agilent Technologies).

[0058] [4] Measurement of physical properties in normal state Hardness (Type A durometer hardness) was measured using a Type A durometer hardness tester in accordance with JIS K6253: 2012. Tensile tests were performed in accordance with JIS K 6251 using a Schopper-type tensile tester with a No. 3 dumbbell specimen to measure tensile strength (MPa), elongation (%), and 100% modulus (MPa).

[0059] As shown in Table 1, in Examples 1 to 10, the glass transition temperatures were much lower than in Comparative Example 1, which used FFKM, and in the evaluation of plasma resistance, the weight loss rates were lower than in Comparative Examples 2 to 5, which used silicone polymers without phenyl groups. From this, it can be seen that according to the present invention, a sealing material composition that can be used in low-temperature environments and has plasma resistance can be provided at low cost.

Claims

1. A plasma-resistant sealing material composition for use in semiconductor manufacturing equipment, comprising a silicone polymer and a vulcanizing agent, wherein the silicone polymer comprises a polysiloxane compound having an unsubstituted or substituted aromatic monovalent hydrocarbon group in a side chain.

2. The polysiloxane compound is represented by the following formula (1): [In the formula, R 1 R independently represents an unsubstituted or substituted aromatic monovalent hydrocarbon group; 2 each independently represents an unsubstituted or substituted aromatic monovalent hydrocarbon group, an unsubstituted or substituted unsaturated or saturated hydrocarbon group not containing an aromatic hydrocarbon group, an alkoxy group, a hydroxyl group, or a hydrogen atom, and n represents an integer of 1 to 7,000.

3. The sealing material composition according to claim 2, wherein the ratio of the structural unit represented by formula (1) in the polysiloxane compound is 1 to 70 mol %.

4. The polysiloxane compound has a main chain end having (R 3 ) 3 Si-R 4 - [wherein, R 3 each independently represents an unsubstituted or substituted aromatic monovalent hydrocarbon group, an unsubstituted or substituted unsaturated or saturated hydrocarbon group not containing an aromatic hydrocarbon group, an alkoxy group, or a hydroxy group; R 4 each independently represents an oxygen atom or an alkylene group having 1 to 5 carbon atoms.

5. The polysiloxane compound is represented by the following formula (2): [In the formula, R 5 and R 6 each independently represents an unsubstituted or substituted unsaturated or saturated hydrocarbon group not containing an aromatic hydrocarbon group, an alkoxy group, or a hydroxy group, and o represents an integer of 100 to 10,000.

6. The sealing material composition according to claim 5, wherein the polysiloxane compound has a vinyl group on at least one of a side chain and an end of the main chain.

7. The sealant composition according to claim 1, further comprising at least one of 1 to 160 parts by mass of a filler and 0.05 to 3 parts by mass of a pigment, relative to 100 parts by mass of the silicone polymer.

8. The sealant composition according to claim 1, wherein the vulcanizing agent comprises a peroxide compound.

9. The sealing material composition according to claim 1, wherein the content of the vulcanizing agent is 0.2 to 8 parts by mass based on 100 parts by mass of the silicone polymer.

10. The sealant composition according to claim 1, further comprising a perfluoropolyether compound.

11. The sealing material composition according to claim 1, having a metal ion content of 1000 ppm or less.

12. A sealant comprising a crosslinked product of the sealant composition according to claim 1.

13. A gate seal for semiconductor manufacturing equipment, comprising the sealing material according to claim 12.

14. A semiconductor manufacturing device comprising the sealing material according to claim 12.

Citation Information

Patent Citations

  • Fluorosilicone rubber composition

    JP2001002923A

  • High purity perfluoroelastomer composite and production method therefor

    JP2013177631A

  • Perfluoro elastomer composition and sealant

    JP2018016795A

  • Additives for silicone encapsulants

    JP2016531988A