Electrolyte, electrode additive, electrode, and lithium ion secondary battery

By using lithium ion conductive materials and a mixed solvent with a low dielectric constant in lithium ion secondary batteries, the issues of resistance and performance degradation are addressed, enhancing the battery's input/output characteristics and retention rate.

WO2024203683A1PCT designated stage expired Publication Date: 2024-10-03OHARA INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010930
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium ion secondary batteries using glass-ceramic composite electrolytes and metal lithium ion secondary batteries with composite solid electrolytes face issues with input/output characteristics, increased resistance at the interface between the metal lithium negative electrode and the electrolyte after charge/discharge cycles, and deterioration of the metal lithium negative electrode.

Method used

Incorporating a specific lithium ion conductive material, such as glass ceramic, garnet-type oxide, or perovskite-type oxide powder, into the electrolyte or electrode, along with a mixed solvent with a dielectric constant of 50.0 or less, to enhance lithium ion conductivity and promote the insertion/desorption reaction, and using an ion-conductive polymer to improve the electrolyte's performance.

Benefits of technology

The solution improves the input/output characteristics, suppresses the increase in resistance at the interface between the metal lithium negative electrode and the electrolyte, and maintains the performance retention rate of the lithium ion secondary battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010930_03102024_PF_FP_ABST
    Figure JP2024010930_03102024_PF_FP_ABST
Patent Text Reader

Abstract

[Problem] To provide an electrolyte, an electrode additive, and an electrode that make it possible to manufacture a lithium ion secondary battery with which it is possible to improve output / input properties, to suppress an increase in resistance at an interface between a metal lithium negative electrode and an electrolyte after a charging / discharging cycle, and to suppress deterioration of the metal lithium negative electrode. [Solution] An electrolyte according to the present invention is characterized by comprising: a lithium ion-conductive material selected from a glass ceramic powder having a main crystal phase represented by formula (1) Li1+x+2y+zAxCayT2-(x+y)SizP3-zO12 (wherein A represents at least one component selected from the group consisting of Al, Ga and Y; T represents at least one component selected from the group consisting of Ti, Ge and Zr; and 0≤x≤1, 0≤y≤1, 0≤z≤1, 0≤x+y≤1 and 0≤x+2y+z≤2) and having an average particle diameter of 5 μm or less, a garnet-type oxide powder represented by formula (2) Li5+XLa3(ZrX,A2-X)O12 (wherein A represents at least one component selected from the group consisting of Sc, Ti, V, Y, Nb, Hf, Ta, Bi, Al, Si, Ga and Ge; and 1.4≤X<2), and a perovskite-type oxide powder represented by formula (3) LixLayTiO3 (wherein 0<x<2 and 0<y<3); and an electrolytic solution containing a mixed solvent having a dielectric constant of 50.0 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte, electrode additive, electrode, and lithium-ion secondary battery

[0001] The present invention relates to an electrolyte, an electrode additive, and an electrode. Furthermore, the present invention relates to a lithium ion secondary battery including the electrolyte, the electrode additive, or the electrode.

[0002] Conventionally, rechargeable lithium-ion secondary batteries with high energy density have been widely used for applications such as power sources for electric vehicles and mobile devices. Most of the lithium-ion secondary batteries currently available on the market generally use liquid electrolytes (electrolytic solutions) such as organic solvents due to their high energy density. These electrolytes are made by dissolving lithium salts in non-aqueous solvents such as carbonate esters and cyclic esters.

[0003] However, lithium-ion secondary batteries using such flammable organic electrolytes have problems such as leakage and fire due to heat generation, and various improvements have been attempted. One of these is lithium secondary batteries using polymer electrolytes. In lithium secondary batteries using polymer electrolytes, the liquid electrolyte is retained in the polymer electrolyte, making it possible to reduce the amount of electrolyte and reduce leakage.

[0004] Since such polymer electrolytes have low lithium ion conductivity, it has been proposed to further incorporate a lithium ion conductive inorganic compound into the polymer electrolyte in order to solve this problem. For example, Patent Document 1 proposes a glass ceramic composite electrolyte obtained by impregnating a non-aqueous electrolyte solution into a medium containing lithium ion conductive glass ceramic powder.

[0005] Furthermore, as another type of lithium ion secondary battery using a polymer electrolyte, for example, Patent Document 2 proposes a metal lithium ion secondary battery in which metallic lithium is disposed in the negative electrode in order to improve the energy density.

[0006] Furthermore, as a solution to the problem of heat generation and ignition in lithium ion secondary batteries due to a chemical reaction between an organic electrolyte solution and an electrode active material, Patent Document 3 proposes a technology in which an electrode contains a specific amount of a lithium ion conductive inorganic solid electrolyte, so that the electrode maintains a high capacity even when stored in a high-temperature environment or even when repeatedly charged and discharged.

[0007] JP 2001-15164 A JP 2017-191766 A JP 2008-117542 A

[0008] However, even the lithium-ion secondary battery using the glass-ceramic composite electrolyte described in Patent Document 1 had room for improvement in its input / output characteristics. Furthermore, even the metal lithium-ion secondary battery using the composite solid electrolyte described in Patent Document 2 had room for improvement in terms of the increase in resistance at the interface between the metal lithium negative electrode and the electrolyte and the deterioration of the metal lithium negative electrode after charge / discharge cycles. Furthermore, Patent Document 3 proposed a lithium-ion secondary battery with high reliability in high-temperature environments using an electrode containing a specific amount of glass ceramics, but there was room for further improvement in its input / output characteristics. In the present invention, the input / output characteristics refer to the capacity during high-current discharge relative to the capacity during low-current discharge when the discharge cutoff voltage is reached, or the capacity during high-current charge relative to the capacity during low-current charge when the charge cutoff voltage is reached, in a charge / discharge evaluation of a lithium-ion secondary battery.

[0009] As a result of intensive research into solving the above problems, the present inventors have surprisingly found that these problems can be solved by blending a specific lithium ion conductive material with an electrolyte solution containing a specific mixed solvent in an electrode or electrolyte, whereby the powder of the lithium ion conductive material is polarized in the electrolyte solution by an external electric field, thereby acting on the lithium salt and improving the degree of dissociation of the lithium salt, thereby increasing the number of lithium ions involved in the electrode reaction, thereby accelerating the insertion / desorption reaction of the electrode and the dissolution / precipitation reaction of lithium metal. Based on this finding, the present inventors have completed the present invention.

[0010] That is, according to the present invention, the following inventions are provided: [1] Li1+x+2y+z A x Ca y T 2-(x+y) Si z P 3-z O 12 (1) A glass ceramic powder having a main crystalline phase represented by the formula (1), wherein A is at least one selected from the group consisting of Al, Ga, and Y; T is at least one selected from the group consisting of Ti, Ge, and Zr; and 0≦x≦1, 0≦y≦1, 0≦z≦1, 0≦x+y≦1, 0≦x+2y+z≦2, and having an average particle size of 5 μm or less. 5+X La 3 (Zr X , A 2-X ) O 12 (2) A garnet-type oxide powder represented by the formula (2), wherein A is at least one selected from the group consisting of Sc, Ti, V, Y, Nb, Hf, Ta, Bi, Al, Si, Ga, and Ge, and 1.4≦X<2; and Li x La y TiO 3(3) An electrolyte comprising: a lithium ion conductive material selected from perovskite-type oxide powders represented by the formula (3), where 0<x<2 and 0<y<3; and an electrolyte solution containing a mixed solvent having a relative dielectric constant of 50.0 or less. [2] The electrolyte according to [1], wherein the mixed solvent has a relative dielectric constant of 40.0 or less. [3] The electrolyte according to [1] or [2], wherein the mixed solvent contains a cyclic carbonate and a chain carbonate. [4] The electrolyte according to [3], wherein the cyclic carbonate is at least one selected from the group consisting of ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, and fluoroethylene carbonate. [5] The electrolyte according to [3] or [4], wherein the chain carbonate is at least one selected from the group consisting of diethyl carbonate, dimethyl carbonate, and ethyl methyl carbonate. [6] The electrolyte according to any one of [1] to [5], further comprising an ion-conducting polymer. [7] A lithium ion secondary battery comprising a positive electrode, a negative electrode, and the electrolyte according to any one of [1] to [6]. [8] An additive used in an electrode of a lithium ion secondary battery, comprising Li 1+x+2y+z A x Ca y T 2-(x+y) Si z P 3-z O 12 (1) A glass ceramic powder having a main crystalline phase represented by the formula (1), wherein A is at least one selected from the group consisting of Al, Ga, and Y; T is at least one selected from the group consisting of Ti, Ge, and Zr; and 0≦x≦1, 0≦y≦1, 0≦z≦1, 0≦x+y≦1, 0≦x+2y+z≦2, and having an average particle size of 5 μm or less. 5+X La 3 (Zr X , A 2-X ) O 12 (2) A garnet-type oxide represented by the formula (2), wherein A is at least one selected from the group consisting of Sc, Ti, V, Y, Nb, Hf, Ta, Bi, Al, Si, Ga, and Ge, and 1.4≦X<2; and Li x Lay TiO 3 (3) An electrode additive comprising: a lithium ion conductive material selected from perovskite oxides represented by the formula (3), where 0<x<2 and 0<y<3; and a mixed solvent having a relative dielectric constant of 50.0 or less. [9] The electrode additive according to [8], wherein the mixed solvent contains a cyclic carbonate and a chain carbonate.

[10] The electrode additive according to [9], wherein the cyclic carbonate is at least one selected from the group consisting of ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, and fluoroethylene carbonate.

[11] The electrode additive according to [9] or

[10] , wherein the chain carbonate is at least one selected from the group consisting of diethyl carbonate, dimethyl carbonate, and ethyl methyl carbonate.

[12] The electrode additive according to any of [8] to

[11] , further comprising an ion-conductive polymer.

[13] An electrode comprising an active material and the electrode additive according to any one of [8] to

[12] .

[14] A lithium ion secondary battery comprising an electrode comprising an active material and the electrode additive according to any one of [8] to

[12] .

[0011] According to the present invention, it is possible to provide an electrolyte, an electrode additive, and an electrode that can be used to manufacture a lithium ion secondary battery that has improved input / output characteristics, can suppress an increase in resistance at the interface between the metallic lithium negative electrode and the electrolyte after charge / discharge cycles, and can also suppress deterioration of the metallic lithium negative electrode.Furthermore, it is possible to provide a lithium ion secondary battery that has improved input / output characteristics, can suppress an increase in resistance at the interface between the metallic lithium negative electrode and the electrolyte after charge / discharge cycles, can also suppress deterioration of the metallic lithium negative electrode, and has excellent performance maintenance.

[0012] 1 is a diagram showing the measurement results of the resistance at the interface between the metallic lithium negative electrode and the electrolyte before and after charge-discharge cycles in Example 5, Comparative Example 7, and Comparative Example 8. 2 is a diagram showing the measurement results of the resistance at the interface between the metallic lithium negative electrode and the electrolyte before and after charge-discharge cycles in Example 6, Comparative Example 9, and Comparative Example 10. 3 is a diagram showing the measurement results of the resistance at the interface between the metallic lithium negative electrode and the electrolyte before and after charge-discharge cycles in Comparative Example 11, Comparative Example 12, and Comparative Example 13.

[0013] (Electrolyte) The electrolyte according to the present invention contains a lithium ion conductive material and an electrolytic solution, and may further contain an ion conductive polymer. Each component will be described in detail below.

[0014] (Lithium Ion Conductive Material) The lithium ion conductive material used in the present invention is at least one selected from glass ceramic powder, garnet-type oxide powder, and perovskite-type oxide powder, which will be described in detail below.

[0015] (Glass ceramic powder) Lithium ion conductive crystals that do not contain grain boundaries that inhibit ion conduction are advantageous in terms of ion conduction. In particular, glass ceramics have almost no voids or grain boundaries that inhibit ion conduction, so they have high ion conductivity and excellent chemical stability. Lithium ion conductive glass ceramic powders are also advantageous in terms of ease of production and cost.

[0016] Here, glass ceramics are materials obtained by heat-treating glass to precipitate a crystalline phase within a glass phase. They refer to materials composed of an amorphous solid and crystals, and further include materials in which the entire glass phase has undergone a phase transition to a crystalline phase, i.e., materials with a crystalline content (crystallinity) of 100% by mass. Even in 100% crystallized materials, glass ceramics have almost no voids between or within the crystal grains. In contrast, commonly referred to as ceramics and sintered bodies, the presence of voids and grain boundaries between or within the crystal grains is unavoidable due to the manufacturing process, and can be distinguished from the glass ceramics of the present invention. In particular, with regard to ionic conductivity, the presence of voids and grain boundaries in ceramics results in values ​​significantly lower than the conductivity of the crystal grains themselves. Controlling the crystallization process of glass ceramics can suppress the decrease in intercrystalline conductivity, making it easy to obtain conductivity comparable to the inherent conductivity of the crystal grains themselves.

[0017] The glass ceramic powder used in the present invention is a powder of the following formula (1): Li 1+x+2y+z A x Ca y T 2-(x+y) Si z P 3-z O 12 (1) (in formula (1), A is at least one selected from the group consisting of Al, Ga, and Y; T is at least one selected from the group consisting of Ti, Ge, and Zr; and 0≦x≦1, 0≦y≦1, 0≦z≦1, 0≦x+y≦1, 0≦x+2y+z≦2).

[0018] In the above formula (1), X is preferably 0.05 or more, more preferably 0.1 or more, and even more preferably 0.2 or more. When X is equal to or greater than these values, the amount of lithium can be increased to increase the conductivity. Furthermore, X is preferably 0.8 or less, more preferably 0.7 or less, and even more preferably 0.6 or less. When X is equal to or less than these values, the stable crystal structure of the glass ceramic powder is maintained, the input / output characteristics are improved, the increase in resistance at the interface between the metal lithium negative electrode and the electrolyte after charge / discharge cycles can be suppressed, deterioration of the metal lithium negative electrode can be suppressed, and the performance retention rate can be improved. y is preferably 0.025 or more, more preferably 0.05 or more, and even more preferably 0.1 or more. When y is equal to or greater than these values, the amount of lithium can be increased to increase the conductivity. Furthermore, y is preferably 0.9 or less, more preferably 0.7 or less, and even more preferably 0.5 or less. When y is less than or equal to these values, the stable crystal structure of the glass ceramic powder is maintained, the input / output characteristics are improved, an increase in resistance at the interface between the metallic lithium anode and the electrolyte after charge / discharge cycles is suppressed, deterioration of the metallic lithium anode is suppressed, and the performance retention rate is improved. z is preferably 0.05 or more, more preferably 0.1 or more, and even more preferably 0.2 or more. When z is greater than or equal to these values, the amount of lithium can be increased to increase the conductivity. Furthermore, z is preferably 0.9 or less, more preferably 0.8 or less, and even more preferably 0.7 or less. When z is less than or equal to these values, the stable crystal structure of the glass ceramic powder is maintained, the input / output characteristics are improved, an increase in resistance at the interface between the metallic lithium anode and the electrolyte after charge / discharge cycles is suppressed, deterioration of the metallic lithium anode is suppressed, and the performance retention rate is improved.

[0019] In the above formula (1), in one preferred embodiment, A is Al and T is Ti. For example, Li 1+x+y Al x Ti 2-x Si y P 3-y O 12The glass ceramics in which the main crystalline phase is (0≦x≦0.4, 0<y≦0.6) contains, in mol % in terms of oxide, Li 2 O: 10-25%, Al 2 O 3 :0~15%, TiO 2 :25~50%, SiO 2 : 0 to 15%, P 2 O 5 : 26 to 40% of each component is melted and rapidly cooled to obtain glass, which is then heat-treated to precipitate crystals.

[0020] The average particle diameter of the glass ceramic powder (D 50 The upper limit of the average particle size (D ) is 5 μm or less, preferably 4 μm or less, and more preferably 3 μm or less. By setting the upper limit of the average particle size to these numerical values ​​or less, the specific surface area of ​​the glass ceramic powder increases, and the area in contact with the electrolyte increases, thereby improving the input / output characteristics, suppressing an increase in the resistance at the interface between the metallic lithium negative electrode and the electrolyte after charge / discharge cycles, suppressing deterioration of the metallic lithium negative electrode, and improving the performance retention rate. In addition, the average particle size (D 50 The lower limit of the average particle diameter is 0.01 μm or more, preferably 0.05 μm or more, and more preferably 0.1 μm or more. By setting the lower limit of the average particle diameter to these values ​​or more, it is possible to improve dispersibility within the electrode and adhesion between electrode materials. The average particle diameter in the present invention is the D50 (cumulative 50% diameter) value measured by laser diffraction after dispersing the glass ceramic powder in ethanol or NMP using an ultrasonic bath to a solids concentration of approximately 0.05 wt %. Specifically, the value measured using a particle size analyzer, Microtrac MT3300EXII, manufactured by Nikkiso Co., Ltd. can be used. The average particle diameter is a value expressed on a volume basis.

[0021] The ionic conductivity of the glass ceramic powder is preferably 1×10 -5 S / cm or more, more preferably 1×10 -4 S / cm or more, and more preferably 1×10 -3S / cm or more. By setting the lower limit of ionic conductivity to these values ​​or more, the powder of the lithium ion conductive material is polarized in the electrolyte by an external electric field, thereby acting on the lithium salt, improving the degree of dissociation of the lithium salt and increasing the number of lithium ions involved in the electrode reaction, thereby accelerating the insertion / desorption reaction of the electrode and accelerating the dissolution / precipitation reaction of lithium metal, thereby suppressing an increase in resistance at the interface between the metallic lithium negative electrode and the electrolyte after charge / discharge cycles, suppressing deterioration of the metallic lithium negative electrode, and improving the performance retention rate. The ionic conductivity in the present invention is determined by measuring impedance (1 MHz to 0.1 Hz, ±10 mV, 25°C) using a potentio / galvanostat (SP-300 manufactured by Bio-Logic Science Instruments), measuring the resistance R (Ω) of the sample from the impedance measurement results, and then calculating the resistance R (Ω) of the sample based on the thickness L (cm) of the sample and the electrode area S (cm 2 ) from the relationship between the ionic conductivity σ (S cm -1 ) is the calculated value.

[0022] The lower limit of the specific surface area of ​​the glass ceramic powder is preferably 1 m 2 / g or more, more preferably 3m 2 / g or more, and more preferably 5m 2 / g or more, and even more preferably 7m 2 / g or more, and most preferably 10m 2 / g or more. By setting the lower limit of the specific surface area to these values ​​or more, the area in contact with the electrolyte increases, the input / output characteristics are improved, the increase in resistance at the interface between the metallic lithium negative electrode and the electrolyte after charge / discharge cycles can be suppressed, deterioration of the metallic lithium negative electrode can be suppressed, and the performance retention rate can be improved. In addition, the upper limit of the specific surface area of ​​the glass ceramic powder is preferably 200 m 2 / g or less, more preferably 100m 2 / g or less, and more preferably 80m 2 / g or less. By setting the upper limit of the specific surface area to these numerical values ​​or less, it is possible to improve dispersibility within the electrode and improve the binding between electrode materials. The specific surface area in the present invention is a value that represents the average value of values ​​measured twice by the BET single-point method using a fully automatic specific surface area meter Macsorb HM-1201 manufactured by MOUNTECH.

[0023] (Garnet-type oxide powder) The garnet-type oxide powder used in the present invention is a garnet-type oxide powder represented by the following formula (2): Li 5+X La 3 (Zr X , A 2-X ) O 12 (2) (in formula (2), A is at least one selected from the group consisting of Sc, Ti, V, Y, Nb, Hf, Ta, Bi, Al, Si, Ga, and Ge, and 1.4≦X<2). The garnet-type oxide powder represented by the above formula (2) has high ionic conductivity, and therefore, like a glass ceramic powder, the powder of a lithium ion conductive material is polarized in the electrolyte by an external electric field, acting on the lithium salt to improve the degree of dissociation of the lithium salt and increase the number of lithium ions involved in the electrode reaction, thereby promoting the insertion / desorption reaction of the electrode and promoting the dissolution / precipitation reaction of lithium metal, and can suppress an increase in resistance at the interface between the metallic lithium negative electrode and the electrolyte after charge / discharge cycles, suppress deterioration of the metallic lithium negative electrode, and improve the performance retention rate.

[0024] (Perovskite-type oxide powder) The perovskite-type oxide powder used in the present invention is a perovskite-type oxide powder represented by the following formula (3): Li x La y TiO 3(3) (in formula (3), 0<x<2, 0<y<3) The perovskite oxide powder represented by formula (3) has high ionic conductivity, and therefore, like glass ceramic powder, the powder of the lithium ion conductive material is polarized in the electrolyte by an external electric field, which acts on the lithium salt to improve the degree of dissociation of the lithium salt and increase the number of lithium ions involved in the electrode reaction, thereby accelerating the insertion / desorption reaction of the electrode and accelerating the dissolution / precipitation reaction of lithium metal, and thereby suppressing an increase in resistance at the interface between the metallic lithium negative electrode and the electrolyte after charge / discharge cycles, suppressing deterioration of the metallic lithium negative electrode, and improving the performance retention rate.

[0025] The amount of the lithium ion conductive material is preferably 5% by mass or more and 95% by mass or less, more preferably 10% by mass or more and 90% by mass or less, and even more preferably 15% by mass or more and 85% by mass or less, based on the total amount of the electrolyte. If the amount of the lithium ion conductive material is within the above range, the structure of the electrolyte can be maintained while improving the input / output characteristics, suppressing an increase in resistance at the interface between the metallic lithium negative electrode and the electrolyte after charge / discharge cycles, suppressing deterioration of the metallic lithium negative electrode, and improving the performance retention rate.

[0026] (Electrolyte) The electrolyte used in the present invention is a non-aqueous electrolyte that contains a specific mixed solvent and may further contain a lithium salt having a specific composition.

[0027] (Mixed Solvent) The mixed solvent used in the present invention can be a mixture of conventionally known organic solvents for electrolytes, as long as the mixed solvent has a dielectric constant of 50.0 or less. The dielectric constant of the mixed solvent is preferably 40.0 or less, preferably 30.0 or less, and may be 1.0 or more, 5.0 or more, or 10.0 or more. If the dielectric constant of the mixed solvent is within the above-mentioned range, it can improve input / output characteristics, suppress an increase in resistance at the interface between the metallic lithium negative electrode and the electrolyte after charge / discharge cycles, suppress deterioration of the metallic lithium negative electrode, and improve performance retention. The dielectric constant of the mixed solvent can be adjusted within a desired range by appropriately selecting the type of organic solvent used and its blending ratio. In the present invention, the dielectric constant and viscosity of the mixed solvent are values ​​calculated in accordance with the volumetric mixing rule from the dielectric constant and viscosity of a single solvent described in the literature (Battery Handbook, published February 10, 2010, edited by the Battery Technology Committee of the Electrochemical Society, published by Ohmsha Co., Ltd., p. 534).

[0028] The mixed solvent preferably contains a cyclic carbonate and a chain carbonate. Examples of the cyclic carbonate include ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, and fluoroethylene carbonate. These cyclic carbonates may be used alone or in combination of two or more. Examples of the chain carbonate include diethyl carbonate, dimethyl carbonate, and ethyl methyl carbonate. These chain carbonates may be used alone or in combination of two or more. For example, it is preferable to use a combination of at least one of ethylene carbonate and propylene carbonate as the cyclic carbonate and at least one of diethyl carbonate and ethyl methyl carbonate as the chain carbonate.

[0029] The blending amount of the mixed solvent is preferably 5% by mass or more and 50% by mass or less, more preferably 10% by mass or more and 40% by mass or less, and even more preferably 15% by mass or more and 30% by mass or less, based on the total amount of the electrolyte. When the blending amount of the mixed solvent is within the above numerical range, the shape of the electrolyte is maintained, the ionic conductivity of the electrolyte solution is increased, the input / output characteristics are improved, an increase in the resistance at the interface between the metallic lithium negative electrode and the electrolyte after charge / discharge cycles can be suppressed, deterioration of the metallic lithium negative electrode can be suppressed, and the performance retention rate can be improved.

[0030] (Lithium Salt) The lithium salt used in the present invention is represented by the following formula (4): LiMF m (C 2 F 5 ) n (4) (in formula (4), M is at least one selected from the group consisting of P, B, Sb, Ta, and Nb; when M is P, Sb, Ta, or Nb, m+n=6, 3≦m≦6, 0≦n≦3; when M is B, m+n=4, 2≦m≦4, 0≦n≦2).

[0031] In the above formula (4), when M is P, Sb, Ta, or Nb, m is preferably 3.5 or more, more preferably 4.0 or more, and even more preferably 5.0 or more. Furthermore, m is preferably 5.5 or less, more preferably 5.9 or less, and even more preferably 5.8 or less. When M is B, m is preferably 2.5 or more, more preferably 3.0 or more, and even more preferably 3.5 or more. Furthermore, m is preferably 3.95 or less, more preferably 3.9 or less, and even more preferably 3.8 or less. Lithium salts with m within these numerical ranges are lithium salts with a high degree of dissociation, and can be said to be salts that easily undergo hydrolysis and generate HF. When these salts are used in the present invention, it is possible to improve input / output characteristics, suppress an increase in resistance at the interface between the metallic lithium negative electrode and the electrolyte after charge / discharge cycles, suppress deterioration of the metallic lithium negative electrode, and improve the performance retention rate. When M is P, Sb, Ta, or Nb, n is preferably 0.05 or more, more preferably 0.1 or more, and even more preferably 0.2 or more. Furthermore, n is preferably 2.5 or less, more preferably 2.0 or less, and even more preferably 1.0 or less. When M is B, n is preferably 0.05 or more, more preferably 0.1 or more, and even more preferably 0.2 or more. Furthermore, n is preferably 1.5 or less, more preferably 1.0 or less, and even more preferably 0.5 or less. When n is within these numerical ranges, the salts have high stability against hydrolysis. Therefore, when these salts are used in the present invention, the input / output characteristics can be improved, an increase in the resistance at the interface between the metallic lithium negative electrode and the electrolyte after charge / discharge cycles can be suppressed, deterioration of the metallic lithium negative electrode can be suppressed, and the performance retention rate can be improved.

[0032] The lithium salt represented by the formula (4) is LiPF 6 , LiBF 4 , LiSbF 6 , LiTaF 6 , LiNbF 6 , LiBF 3 (C 2 F 5 ), and LiPF 3 (C 2F 5 ) 3 Among these lithium salts, LiPF is preferred in that it can improve the input / output characteristics, has high ionic conductivity of the electrolyte, can suppress the increase in resistance at the interface between the metallic lithium anode and the electrolyte after charge / discharge cycles, can suppress the deterioration of the metallic lithium anode, and can improve the performance retention rate. 6 , LiBF 4 , and LiSbF 6 These lithium salts may be used alone or in combination of two or more.

[0033] The blending amount of the lithium salt is preferably 2% by mass or more and 40% by mass or less, more preferably 3% by mass or more and 30% by mass or less, and even more preferably 4% by mass or more and 20% by mass or less, based on the total amount of the electrolyte. When the blending amount of the lithium salt is within the above numerical range, it is possible to maintain the shape of the electrolyte, improve the input / output characteristics, increase the ionic conductivity of the electrolyte, suppress an increase in the resistance at the interface between the metallic lithium negative electrode and the electrolyte after charge / discharge cycles, suppress deterioration of the metallic lithium negative electrode, and improve the performance retention rate.

[0034] (Ion-Conductive Polymer) The ion-conductive polymer used in the present invention is not particularly limited, and conventionally known polymers having lithium ion conductivity can be used, but polymers that swell in an electrolyte solution consisting of a lithium salt and an organic solvent and have high ion conductivity are preferred. Examples of ion-conductive polymers include polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyacrylonitrile, polyethylene oxide, polyacetylene, polydimethylsiloxane, and poly(vinylene carbonate-co-acrylonitrile). Among these ion-conductive polymers, polyvinylidene fluoride-hexafluoropropylene, polyacrylonitrile, and the like are preferred. These ion-conductive polymers may be used alone or in combination of two or more.

[0035] The amount of the ion-conductive polymer blended is preferably 5% by mass or more and 70% by mass or less, more preferably 7% by mass or more and 50% by mass or less, and even more preferably 10% by mass or more and 30% by mass or less, relative to the total amount of the electrolyte. When the amount of the ion-conductive polymer blended is within the above range, the electrolyte exhibits high ionic conductivity while maintaining its shape, improves input / output characteristics, suppresses an increase in resistance at the interface between the metallic lithium negative electrode and the electrolyte after charge / discharge cycles, suppresses deterioration of the metallic lithium negative electrode, and improves the performance retention rate.

[0036] The electrolyte can be obtained as a self-supporting membrane by forming a slurry containing a mixture of a lithium ion conductive material, an ion conductive polymer, and a solvent in which the ion conductive polymer dissolves into a sheet and drying the solvent. Alternatively, the slurry can be directly coated onto an electrode to form an electrolyte layer. The self-supporting membrane or the electrolyte layer coated on an electrode, which is made of a lithium ion conductive material and an ion conductive polymer, can be impregnated with an electrolyte solution containing a lithium salt and an organic solvent and swelled after the solvent has been thoroughly dried, thereby maintaining the shape of the electrolyte and exhibiting high ionic conductivity.

[0037] The thickness of the electrolyte layer coated on the self-supporting membrane or electrode is preferably 1 μm to 50 μm, more preferably 2 μm to 40 μm, and even more preferably 3 μm to 30 μm. When the thickness of the electrolyte is within the above range, the electrolyte has a strength sufficient to maintain its shape and exhibits high ionic conductivity.

[0038] (Lithium-ion secondary battery) The lithium-ion secondary battery of the present invention comprises a positive electrode, a negative electrode, and the above-described electrolyte. Each electrode contains an active material and may further contain an electrode additive. Each component will be described in detail below.

[0039] (Positive electrode) The positive electrode is not particularly limited, and a conventionally known positive electrode for a lithium ion secondary battery can be used. The positive electrode is not particularly limited as long as it has a positive electrode active material, but for example, it includes a positive electrode current collector and a positive electrode active material layer provided on the surface of the positive electrode current collector. The positive electrode is arranged to face the negative electrode.

[0040] The positive electrode current collector collects current from the positive electrode active material layer. The type of positive electrode current collector is not particularly limited, but examples include metal foils such as aluminum foil, perforated metal foils such as perforated aluminum foil, expanded metal, and foam metal plates. The material of the positive electrode current collector is not particularly limited, but examples include aluminum, stainless steel, and titanium. The shape and manufacturing method of the positive electrode current collector are not particularly limited, and any shape and manufacturing method may be used.

[0041] The positive electrode active material layer is not particularly limited as long as it contains a positive electrode active material, but may contain, for example, a positive electrode active material, a conductive agent, and a binder.

[0042] The positive electrode active material is a material into which lithium ions are desorbed during charging and into which lithium ions desorbed from the negative electrode active material in the negative electrode active material layer are inserted during discharging. The positive electrode active material is not particularly limited as long as it is a material capable of reversibly inserting and desorbing lithium ions. For example, a lithium-containing compound containing lithium ions as a reactive species is preferred. Examples of the lithium-containing compound include, but are not limited to, lithium cobalt oxide, manganese-substituted lithium cobalt oxide, lithium manganate, lithium nickel oxide, lithium iron phosphate, and lithium manganese phosphate.

[0043] The conductive agent improves the conductivity of the positive electrode active material layer. The conductive agent is not particularly limited, but examples thereof include ketjen black, acetylene black, and graphite.

[0044] The binder binds together the positive electrode active material, the conductive agent, etc. in the positive electrode active material layer. The binder is not particularly limited, but examples thereof include polyvinylidene fluoride, styrene-butadiene rubber, carboxymethyl cellulose, cellulose acetate, ethyl cellulose, fluororubber, ethylene-propylene rubber, polyacrylic acid, polyimide, and polyamide.

[0045] (Negative Electrode) The negative electrode has a negative electrode current collector and a negative electrode active material layer provided on the surface of the negative electrode current collector that faces the positive electrode.

[0046] The negative electrode current collector collects current from the negative electrode active material layer. The type of negative electrode current collector is not particularly limited, but examples include metal foils such as copper foil, perforated metal foils such as perforated copper foil, expanded metal, and foam metal plates. The material of the negative electrode current collector is not particularly limited, but examples include copper, stainless steel, and titanium, with copper being preferred. The shape and manufacturing method of the negative electrode current collector are not particularly limited, and any shape and manufacturing method may be used.

[0047] The negative electrode active material layer is not particularly limited as long as it contains a negative electrode active material, and may contain, for example, a negative electrode active material, a conductive agent, and a binder.

[0048] The negative electrode active material is a material into which lithium ions desorbed from the positive electrode active material in the positive electrode active material layer during charging are inserted and into which lithium ions are desorbed during discharging. The negative electrode active material is not particularly limited as long as it is a material capable of reversibly inserting and desorbing lithium ions. Examples of the negative electrode active material include natural graphite, composite carbonaceous materials formed by coating natural graphite with a dry CVD method or a wet spray method, artificial graphite prepared by firing resin materials such as epoxy and phenol, or pitch-based materials obtained from petroleum or coal, silicon (Si), graphite mixed with silicon, non-graphitizable carbon materials, lithium titanate, and titanium niobium oxide negative electrodes. Metallic lithium, which deposits lithium ions during charging and dissolves lithium ions during discharging, can also be used as the negative electrode.

[0049] The conductive agent and binder may be the same as those used in the positive electrode active material layer.

[0050] (Electrode Additive) The additive used in the electrode of a lithium ion secondary battery is added to the above-mentioned positive electrode or negative electrode. The electrode additive includes a lithium ion conductive material and a mixed solvent, and may further include a lithium salt and an ion conductive polymer. The lithium ion conductive material, mixed solvent, lithium salt, and ion conductive polymer used in the electrode additive can be the same as the lithium ion conductive material, mixed solvent, lithium salt, and ion conductive polymer used in the electrolyte. The use of such an electrode additive can improve input / output characteristics, suppress an increase in resistance at the interface between the metallic lithium negative electrode and the electrolyte after charge / discharge cycles, suppress deterioration of the metallic lithium negative electrode, and improve the performance retention rate of the battery.

[0051] The amount of the electrode additive is preferably 0.1% by mass or more and 20% by mass or less, more preferably 0.2% by mass or more and 15% by mass or less, and even more preferably 0.3% by mass or more and 10% by mass or less, based on the total amount of the electrode. When the amount of the electrode additive is within the above range, the input / output characteristics can be improved, an increase in the resistance at the interface between the metallic lithium negative electrode and the electrolyte after charge / discharge cycles can be suppressed, deterioration of the metallic lithium negative electrode can be suppressed, and the performance retention rate of the battery can be improved.

[0052] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention should not be construed as being limited to the contents of the following examples.

[0053] (Production Example 1 of Lithium Ion Conductive Glass-Ceramic Powder) 3 P.O. 4 , Al(PO 3 ) 3 , Li 2 CO 3 , SiO 2 , TiO 2 These were used and converted into oxide equivalent mol% P 2 O 5 35.0%, Al 2 O 3 7.5%, Li 2 15.0% O, TiO 2 38.0%, SiO 2The components were weighed to a composition of 4.5% and mixed uniformly. Subsequently, this mixture was placed in a platinum pot and heated in an electric furnace at 1500°C for 4 hours while stirring the molten glass. The molten glass was then dropped into running water to obtain glass flakes, which were then crystallized by heat treatment at 950°C for 12 hours to obtain the desired glass ceramics. The precipitated crystalline phase was identified by powder X-ray diffraction. 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0≦x≦0.4, 0<y≦0.6) was confirmed to be the main crystalline phase. The ionic conductivity of this glass-ceramic was 1.0×10 -3 The viscosity was about S / cm.

[0054] The obtained glass ceramic flakes were each pulverized by a laboratory-scale jet mill and classified by a rotating roller made of zirconia to measure the average particle diameter (D 50 The glass ceramics thus obtained were milled in a dry bead mill to obtain glass ceramics having an average particle diameter (D 50 Subsequently, the grinding time was extended under the same conditions to obtain an average particle diameter (D 50 ) The powder was pulverized to 0.4 μm and spray-dried to obtain glass ceramic powder 1.

[0055] (Production Example 1 of Nonaqueous Electrolyte) Lithium hexafluorophosphate (LiPF) was added to a solvent in which ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed in a mass ratio of 1:1. 6 ) was dissolved in a concentration of 1 mol / L to obtain non-aqueous electrolyte solution 1.

[0056] (Production Example 2 of Nonaqueous Electrolyte) Lithium hexafluorophosphate (LiPF) was added to a solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a mass ratio of 3:7. 6 ) was dissolved in a concentration of 1 mol / L to obtain non-aqueous electrolyte solution 2.

[0057] (Production Example 3 of Nonaqueous Electrolyte) Lithium hexafluorophosphate (LiPF) was added to a solvent in which ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed in a mass ratio of 3:7. 6 ) was dissolved in a concentration of 1 mol / L to obtain non-aqueous electrolyte solution 3.

[0058] (Production Example 4 of Nonaqueous Electrolyte) Lithium hexafluorophosphate (LiPF) was added to a solvent in which propylene carbonate (PC) and diethyl carbonate (DEC) were mixed in a mass ratio of 3:7. 6 ) was dissolved in a concentration of 1 mol / L to obtain non-aqueous electrolyte solution 4.

[0059] (Production Example 5 of Nonaqueous Electrolyte) Lithium hexafluorophosphate (LiPF) was added to a solvent prepared by mixing ethylene carbonate (EC), propylene carbonate (PC), and diethyl carbonate (DEC) in a mass ratio of 1:1:1. 6 ) was dissolved in a concentration of 1 mol / L to obtain non-aqueous electrolyte solution 5.

[0060] The dielectric constant and viscosity of the non-aqueous electrolyte solution prepared above were calculated from the values ​​of a single solvent using the volumetric mixing rule, and are shown in Table 1.

[0061] Test Example 1 (Positive Electrode Production Example 1-1) Using a mixer (manufactured by Thinky Corporation), Li(Ni 0.6 Co 0.2 Mn 0.2 ) O 2 (NCM622):AB:PVdF:glass ceramic powder 1 were mixed in a weight ratio of 96.5:1.5:1.5:0.5 using NMP as a solvent to obtain a positive electrode slurry 1-1.

[0062] The obtained positive electrode slurry 1-1 was applied to a 20 μm aluminum current collector foil using a blade coater, and then dried at 120° C. The electrode had a capacity of 3.5 mAh / cm 2 It was compressed with a roll press to have a particle size of 66 μm and a density of 3.5 g / cm 3 Subsequently, the mixture was cut into a size of 30 mm x 40 mm using a Thomson punching machine and vacuum dried at 160°C for 24 hours using a glass tube oven to prepare a positive electrode 1-1.

[0063] (Positive Electrode Production Example 1-2) Using a mixer (manufactured by Thinky Corporation), NCM622:AB:PVdF were mixed in a weight ratio of 97:1.5:1.5 using NMP as a solvent to obtain a positive electrode slurry 1-2.

[0064] The obtained positive electrode slurry 1-2 was applied to a 20 μm aluminum current collector foil using a blade coater, and then dried at 120° C. The electrode had a capacity of 3.5 mAh / cm 2 It was compressed with a roll press to have a particle size of 66 μm and a density of 3.5 g / cm 3 Subsequently, the mixture was cut into a size of 30 mm x 40 mm using a Thomson punching machine and vacuum dried at 160°C for 24 hours using a glass tube oven to prepare a positive electrode 1-2.

[0065] (Negative Electrode Production Example 1-1) A 15 μm thick metallic lithium foil cut to 32 mm×42 mm was attached to a 15 μm thick copper current collector foil to produce a negative electrode 1-1.

[0066] (Separator Production Example) A PP separator (P2010H, manufactured by CSTech) was cut into a size of 40 mm x 50 mm using a Thomson punching machine, and vacuum dried at 60°C for 24 hours using a glass tube oven.

[0067] (Examples of Manufacturing a Lithium-Ion Secondary Battery Cell) [Example 1] The electrode surfaces of the positive electrode 1-1 and negative electrode 1-1 manufactured above were placed face to face, a separator was sandwiched between them, and the resulting mixture was wrapped in an aluminum laminate. 0.3 ml of the nonaqueous electrolyte solution 1 obtained above was injected and vacuum impregnated for 30 seconds, and then the mixture was sealed to manufacture a lithium-ion secondary battery cell.

[0068] Comparative Example 1 A lithium ion secondary battery cell was produced in the same manner as in Example 1, except that the positive electrode 1-2 was used instead of the positive electrode 1-1.

[0069] Example 2 A lithium ion secondary battery cell was produced in the same manner as in Example 1, except that non-aqueous electrolyte solution 2 was used instead of non-aqueous electrolyte solution 1.

[0070] Comparative Example 2 A lithium ion secondary battery cell was produced in the same manner as in Example 2, except that the positive electrode 1-2 was used instead of the positive electrode 1-1.

[0071] Example 3 A lithium ion secondary battery cell was produced in the same manner as in Example 1, except that non-aqueous electrolyte solution 3 was used instead of non-aqueous electrolyte solution 1.

[0072] Comparative Example 3 A lithium ion secondary battery cell was produced in the same manner as in Example 3, except that the positive electrode 1-2 was used instead of the positive electrode 1-1.

[0073] Example 4 A lithium ion secondary battery cell was produced in the same manner as in Example 1, except that non-aqueous electrolyte solution 4 was used instead of non-aqueous electrolyte solution 1.

[0074] Comparative Example 4 A lithium ion secondary battery cell was produced in the same manner as in Example 4, except that the positive electrode 1-2 was used instead of the positive electrode 1-1.

[0075] Comparative Example 5 A lithium ion secondary battery cell was produced in the same manner as in Example 1, except that non-aqueous electrolyte solution 5 was used instead of non-aqueous electrolyte solution 1.

[0076] Comparative Example 6 A lithium ion secondary battery cell was produced in the same manner as in Comparative Example 5, except that the positive electrode 1-2 was used instead of the positive electrode 1-1.

[0077] (Chemical conversion treatment / degassing) After one cycle of charge / discharge (4.2 V-2.5 V) at 0.05 C, the laminate was opened once, and after vacuum degassing for 30 seconds again, it was sealed.

[0078] (Evaluation Method 1) For the cells of Examples 1 to 4 and the cells of Comparative Examples 1 to 6, a charge / discharge tester manufactured by Asuka Electronics was used to carry out charge / discharge (25°C) in the following sequence: CC-CV charge (0.2C, 4.2V-0.05C cutoff) → rest (10 minutes) → CC discharge (0.2C or 3C, 2.5V cutoff) → rest (10 minutes), and the discharge capacities were compared. The evaluation results are shown in Tables 2 to 6.

[0079] (Evaluation Result 1) Comparing Examples 1 to 4, in which glass ceramic powder was added, with Comparative Examples 1 to 4, in which no glass ceramic powder was added, the addition of glass ceramic powder resulted in improved input / output characteristics. In particular, the use of a mixed solvent with a low dielectric constant resulted in improved input / output characteristics. On the other hand, comparing Comparative Example 5, in which glass ceramic powder was added, with Comparative Example 6, in which no glass ceramic powder was added, no improvement in input / output characteristics was observed when a mixed solvent with a high dielectric constant was used. This result indicates that mixed solvents with a high dielectric constant have a high degree of dissociation of the lithium salt, making it difficult to obtain the effect of improving the degree of dissociation due to polarization of the glass ceramic powder. Mixed solvents with a low dielectric constant have low viscosity and high ion mobility, but have the problem of low degree of dissociation. However, the use of glass ceramic powder can improve input / output characteristics by increasing ion mobility and dissociation.

[0080] [Test Example 2] [Example 5] Using a mixer (manufactured by Thinky Corporation), glass ceramic powder 1:polyvinylidene fluoride-hexafluoropropylene (PVdF-HFP) in a weight ratio of 1:1 was mixed with a mixed solvent of acetone and octane (mixing ratio 20:1) as a solvent to obtain a slurry 2-1.

[0081] The obtained slurry 2-1 was applied to a PET film using a blade coater and then dried at 80°C. The film thickness after drying was 20 μm. It was then punched out to a size of 30 mm x 30 mm using a Thomson punching machine and vacuum dried at 100°C using a glass tube oven. It was then immersed in nonaqueous electrolyte solution 2 (mixed solvent EC:EMC = 3:7, relative dielectric constant 28.7) for 5 hours, and 20 mm x 20 mm lithium foil with copper foil attached to serve as a current collecting lead was sandwiched between both sides of the electrolyte, followed by vacuum sealing using an aluminum laminate film to produce a lithium ion secondary battery cell.

[0082] Comparative Example 7 Using a mixer (manufactured by Thinky Corporation), polyvinylidene fluoride-hexafluoropropylene was mixed with a mixed solvent of acetone and octane (mixing ratio 20:1) as a solvent to obtain a slurry 2-2.

[0083] A lithium ion secondary battery cell was produced in the same manner as in Example 5, except that slurry 2-2 was used instead of slurry 2-1.

[0084] Comparative Example 8 A PP separator (P2010H, manufactured by CSTech) was punched out to a size of 30 mm × 30 mm using a Thomson punching machine and vacuum dried in a glass tube oven at 60° C. Subsequently, the separator was immersed in nonaqueous electrolyte solution 2 for 5 hours, and 20 mm × 20 mm lithium foils with copper foils attached thereto to serve as current collecting leads were sandwiched between both sides of the electrolyte, followed by vacuum sealing using an aluminum laminate film to produce a lithium ion secondary battery cell.

[0085] Example 6 A lithium ion secondary battery cell was produced in the same manner as in Example 5, except that non-aqueous electrolyte solution 1 (mixed solvent EC:DEC=1:1, relative dielectric constant 45.9) was used instead of non-aqueous electrolyte solution 2.

[0086] Comparative Example 9 A lithium ion secondary battery cell was produced in the same manner as in Comparative Example 7, except that non-aqueous electrolyte solution 1 was used instead of non-aqueous electrolyte solution 2.

[0087] Comparative Example 10 A lithium ion secondary battery cell was produced in the same manner as in Comparative Example 8, except that the non-aqueous electrolyte solution 1 was used instead of the non-aqueous electrolyte solution 2.

[0088] Comparative Example 11 A lithium ion secondary battery cell was produced in the same manner as in Example 5, except that nonaqueous electrolyte solution 5 (mixed solvent EC:PC:DEC=1:1:1, relative dielectric constant 51.7) was used instead of nonaqueous electrolyte solution 2.

[0089] Comparative Example 12 A lithium ion secondary battery cell was produced in the same manner as in Comparative Example 7, except that non-aqueous electrolyte solution 3 was used instead of non-aqueous electrolyte solution 2.

[0090] Comparative Example 13 A lithium ion secondary battery cell was produced in the same manner as in Comparative Example 8, except that the non-aqueous electrolyte solution 3 was used instead of the non-aqueous electrolyte solution 2.

[0091] (Evaluation Method 2) For the cells of the lithium ion secondary batteries of Examples 5 and 6 and Comparative Examples 7 to 13, impedance (1 MHz to 0.1 Hz, ±10 mV, 25°C) was measured using a potentio / galvanostat (SP-300 manufactured by Bio-Logic Science Instruments). Subsequently, for each cell, a charge-discharge cycle (current density 50 μA / cm) was performed using a charge-discharge tester manufactured by Asuka Electronics. 2 The battery was then charged for 15 minutes, discharged for 15 minutes, and cycled 200 times (total 100 hours) at 25°C. The impedance was then measured again using a potentio / galvanostat. A Cole-Cole plot was obtained from the impedance results, revealing two arcs. The low-frequency arc was attributed to the reaction resistance at the interface between the lithium metal and the electrolyte, and the two arcs were compared using Zview.

[0092] (Evaluation Results 2) The measurement results are shown in Figures 1 to 3. When the resistances before charge-discharge cycles are compared in Figure 1 (Example 5, Comparative Examples 7 and 8), Figure 2 (Example 6, Comparative Examples 9 and 10), and Figure 3 (Comparative Examples 11, 12, and 13) for electrolytes containing a glass ceramic powder and an electrolyte solution containing a mixed solvent, the resistance reduction rate of Example 5 relative to Comparative Examples 7 and 8 and the resistance reduction rate of Example 6 relative to Comparative Examples 9 and 10 are higher than the resistance reduction rate of Comparative Example 11 relative to Comparative Examples 12 and 13. Furthermore, when attention is paid to the increase in resistance before and after charge-discharge cycles in Figures 1, 2, and 3, it is found that the electrolyte containing a glass ceramic powder and an electrolyte solution containing a mixed solvent exhibits an effect of suppressing the increase in resistance before and after charge-discharge cycles, regardless of which electrolyte solution was used. On the other hand, as seen in Figure 1 (Comparative Examples 7 and 8) and Figure 2 (Comparative Examples 9 and 10), the lower the dielectric constant of the mixed solvent, the more likely the resistance increases after charge-discharge cycling. Therefore, it can be said that using a glass ceramic powder in a mixed solvent with a low dielectric constant particularly suppresses the increase in resistance before and after charge-discharge cycling. In contrast, as seen in Figure 3 (Comparative Examples 12 and 13), when the mixed solvent has a high dielectric constant, the resistance is less likely to increase after charge-discharge cycling, but even if a glass ceramic powder is used, it is difficult to achieve the effect of suppressing the increase in resistance before and after charge-discharge cycling. Furthermore, when the mixed solvent has a high dielectric constant, the viscosity of the mixed solvent is high, which causes the problem of low lithium ion mobility. This is because mixed solvents with low dielectric constants tend to have low viscosity, resulting in high lithium ion mobility (especially at low temperatures). However, the low dielectric constant of the mixed solvent results in low dissociation of lithium ions, which prevents rapid deposition (charging) / elution (discharging) on ​​the lithium metal surface, resulting in the surrounding electrolyte being reduced and decomposed by the lithium metal. Furthermore, repeated charging and discharging causes a film to build up on the surface of the lithium metal, degrading its reactivity. However, by using glass ceramic powder, it is possible to increase the degree of dissociation of lithium ions and suppress the degradation of the lithium metal, even in solvents with low viscosity, which is expected to have the effect of adding variety to the design of the electrolyte.Generally, there is a trade-off between the degree of dissociation of lithium ions, which is determined by the dielectric constant of the mixed solvent, and the mobility of lithium ions, which is determined by the viscosity of the mixed solvent. While the electrolyte design is a constraint on battery performance, the use of glass-ceramic powder can eliminate this constraint.

Claims

1. Li 1+x+2y+z A x Ca y T 2-(x+y) S z P 3-z O 12 (1) A glass ceramic powder having a main crystal phase represented by the formula (1), in which A is at least one selected from the group consisting of Al, Ga, and Y, T is at least one selected from the group consisting of Ti, Ge, and Zr, and 0≦x≦1, 0≦y≦1, 0≦z≦1, 0≦x+y≦1, 0≦x+2y+z≦2, and having an average particle size of 5 μm or less; Li 5+X La 3 (Zr X , A 2-X ) O 12 (2) A garnet-type oxide powder represented by the formula (2), in which A is at least one selected from the group consisting of Sc, Ti, V, Y, Nb, Hf, Ta, Bi, Al, Si, Ga, and Ge, and 1.4≦X<2; and Li x La y TiO 3 (3) An electrolyte comprising: a lithium ion conductive material selected from perovskite oxide powders represented by the formula (3), where 0<x<2 and 0<y<3; and an electrolyte solution containing a mixed solvent having a relative dielectric constant of 50.0 or less.

2. The electrolyte according to claim 1, wherein the mixed solvent has a relative dielectric constant of 40.0 or less.

3. The electrolyte according to claim 1, wherein the mixed solvent contains a cyclic carbonate and a chain carbonate.

4. The electrolyte according to claim 3, wherein the cyclic carbonate is at least one selected from the group consisting of ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, and fluoroethylene carbonate.

5. The electrolyte according to claim 3, wherein the chain carbonate is at least one selected from the group consisting of diethyl carbonate, dimethyl carbonate, and ethyl methyl carbonate.

6. The electrolyte of claim 1 further comprising an ion-conducting polymer.

7. A lithium ion secondary battery comprising a positive electrode, a negative electrode, and the electrolyte according to any one of claims 1 to 6.

8. An additive for use in an electrode of a lithium ion secondary battery, comprising Li 1+x+2y+z A x Ca y T 2-(x+y) S z P 3-z O 12 (1) A glass ceramic powder having a main crystal phase represented by the formula (1), in which A is at least one selected from the group consisting of Al, Ga, and Y, T is at least one selected from the group consisting of Ti, Ge, and Zr, and 0≦x≦1, 0≦y≦1, 0≦z≦1, 0≦x+y≦1, 0≦x+2y+z≦2, and having an average particle size of 5 μm or less; Li 5+X La 3 (Zr X , A 2-X ) O 12 (2) A garnet-type oxide represented by the formula (2), in which A is at least one selected from the group consisting of Sc, Ti, V, Y, Nb, Hf, Ta, Bi, Al, Si, Ga, and Ge, and 1.4≦X<2, and Li x La y TiO 3 (3) An electrode additive comprising: a lithium ion conductive material selected from perovskite oxides represented by the formula (3): (wherein 0<x<2 and 0<y<3); and a mixed solvent having a relative dielectric constant of 50.0 or less.

9. The electrode additive according to claim 8, wherein the mixed solvent contains a cyclic carbonate and a chain carbonate.

10. The electrode additive according to claim 9, wherein the cyclic carbonate is at least one selected from the group consisting of ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, and fluoroethylene carbonate.

11. The electrode additive according to claim 9, wherein the chain carbonate is at least one selected from the group consisting of diethyl carbonate, dimethyl carbonate, and ethyl methyl carbonate.

12. The electrode additive of claim 8, further comprising an ion-conducting polymer.

13. An electrode comprising an active material and the electrode additive according to any one of claims 8 to 12.

14. A lithium ion secondary battery comprising an active material and an electrode containing the electrode additive according to any one of claims 8 to 12.

Citation Information

Patent Citations

  • Preparation method of lithium-supplementing functional electrolyte membrane for solid-state lithium battery

    CN113782823A

  • All-solid lithium ion secondary battery and method for manufacturing the same

    JP2019040709A

  • Active material and battery

    JP2020017513A

  • Positive electrode for lithium secondary battery, method for producing same, and lithium secondary battery including same

    JP2022532884A

  • Byproduct free methods for solid hybrid electrolyte

    WO2021203060A1