Aqueous ink composition, ink set, and method for producing inkjet-printed matter
The water-based ink composition addresses nozzle clogging and quality issues in inkjet printing for corrugated boxes by incorporating specific solvents and humectants, ensuring effective printing on various substrates with reduced volatile organic solvents, thus enhancing printing stability and environmental sustainability.
Patent Information
- Application Number
- PCT/JP2024/010936
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-01-30
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
Current inkjet printing methods for corrugated boxes face issues with nozzle clogging due to low volatile organic solvent content, poor ink permeability, and quality deterioration when using water-based inks, especially on liner paper and surface-coated substrates, leading to environmental and health concerns from solvent volatility and increased costs from analog printing processes.
A water-based ink composition containing a non-white coloring material, a water-soluble organic solvent with specific ClogP values, a humectant like sugar alcohol, and a surfactant, which reduces the risk of nozzle clogging and improves ink permeability and drying properties, allowing for effective inkjet printing on various substrates without significant volatile organic solvent use.
The ink composition minimizes nozzle clogging, enhances ink permeability and drying properties, and maintains color development quality, even when applied on an ink layer, while reducing environmental impact and production costs.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Water-based ink composition, ink set, and method for producing inkjet printed matter
[0001] The present invention relates to a water-based ink composition, an ink set, and a method for producing an inkjet printed matter.
[0002] A known method for manufacturing cardboard boxes is the preprint method, which involves successively carrying out a printing process in which printing is performed on rolled liner paper or coated board, a laminating process in which the printed liner paper or coated board is bonded to a core to obtain a cardboard sheet, and a box-making process in which cutting is made into the obtained cardboard sheet to form a cardboard box.
[0003] The preprinting method mainly employs analog printing using solvent-based flexographic ink or solvent-based gravure ink. However, the inks used in analog printing contain large amounts of volatile organic solvents, which poses a significant burden on the environment and human health due to the volatilized organic solvents. Furthermore, analog printing requires plate-making, which increases costs and requires a long time before printing. Therefore, there is a demand for a preprinting method using inkjet printing that does not require plate-making and allows on-demand printing, and that uses water-based ink with as little volatile organic solvent as possible.
[0004] Generally, when inkjet printing is performed using ink with reduced volatile organic solvents, the ink dries inside the print head nozzles, which can cause nozzle blockage. In this regard, with the preprint method, which involves a continuous process from the printing process to the box-making process, if a printing problem occurs due to nozzle blockage or the like, it will affect each process after the printing process.
[0005] Furthermore, in the lamination process, i.e., the corrugator processing process, which is a unique manufacturing process for corrugated board, in which liner paper or coated board and a core are bonded together with an adhesive or the like, the ink-printed surface of the liner paper or coated board is exposed to harsh heat conditions in direct contact with a heating means (heating and pressurizing roll, hot platen, etc.), which can cause problems such as the ink layer fusing to the heating means, making it impossible to manufacture a corrugated board sheet, or the ink layer cracking due to this fusing, resulting in a decrease in quality. In particular, when printing on a surface-coated substrate such as coated board, serious problems can occur, such as the ink transferring to the heating means, due to insufficient ink penetration, insufficient fixation, poor drying, etc.
[0006] Furthermore, when inkjet printing is performed on liner paper, water-based white ink may be applied first, followed by water-based color inks to enhance aesthetic appeal. In this case, however, the water-based color inks may sink into the ink layer of the water-based white ink, resulting in problems such as a smaller dot diameter for the water-based color inks and reduced color development.
[0007] Under these circumstances, there is a strong demand in the market for a water-based ink for inkjet recording that uses a reduced amount of volatile organic solvents but is less likely to cause nozzle clogging, is less likely to cause transfer when printed on liner paper or a surface-coated substrate, and exhibits good color development even when applied on an ink layer of a water-based white ink.
[0008] Patent Document 1 discloses a liner paper in which an ink-receiving layer that is compatible with corrugator processing is provided on the surface of the liner base paper. However, the technology of Patent Document 1 requires the use of liner paper provided with an ink-receiving layer, which is more expensive than using regular liner paper. For this reason, it is desirable to improve the water-based ink itself so that regular liner paper can be used.
[0009] Patent Document 2 discloses a recording method using an inkjet head equipped with a circulation mechanism. Patent Document 3 discloses an aqueous ink containing a large amount of solvent and sorbitol. Patent Document 4 discloses an ink composition in which the total content of pigment, pigment dispersion resin, polymer particles, and water is 95.0 mass % or more based on the total composition.
[0010] Japanese Patent Application Laid-Open No. 2006-150694 Japanese Patent Application Laid-Open No. 2021-154610 Japanese Patent No. 6787264 Japanese Patent Application Laid-Open No. 2020-105481
[0011] An object of the present invention is to provide a water-based ink composition for inkjet recording that is less likely to cause nozzle clogging while reducing volatile organic solvents, is less likely to cause transfer when printed on liner paper or a surface-coated substrate, and exhibits good color development even when applied on an ink layer of a water-based white ink; an ink set comprising the water-based ink composition; and a method for producing an inkjet printed matter using the water-based ink composition.
[0012] Specific means for solving the above problems include the following embodiments. <1> A water-based ink composition comprising a non-white colorant, a water-soluble organic solvent, a humectant, a surfactant, and water, wherein the humectant comprises a sugar alcohol, the water-soluble organic solvent comprises one or more specific solvents having a ClogP value of 0.5 or more and 2.0 or less, the content of the water-soluble organic solvent is more than 0% by mass and 5% by mass or less, and the content of the water-soluble organic solvent having a boiling point of 250°C or less at 1 atmosphere is 3% by mass or less. <2> The water-based ink composition according to <1>, wherein the content of the sugar alcohol is 4% by mass or more and 10% by mass or less. <3> The water-based ink composition according to <1> or <2>, wherein the sugar alcohol comprises sorbitol. <4> An ink set comprising the water-based ink composition according to any one of <1> to <3>, and a water-based white ink composition containing a white colorant and water. <5> The ink set according to <4>, wherein the white colorant comprises titanium oxide. <6> A method for producing an inkjet printed product, comprising ejecting droplets of the aqueous ink composition according to any one of <1> to <3> from an inkjet head and depositing them on a printing medium to obtain a printed product. <7> A method for producing an inkjet printed product according to <6>, in which the printing medium is at least one selected from the group consisting of corrugated cardboard, liner paper, and coated board. <8> A method for producing an inkjet printed product according to <6>, in which the printing medium is coated paper. <9> A method for producing an inkjet printed product, comprising successively carrying out a printing step in which droplets of the aqueous ink composition according to any one of <1> to <3> are ejected from an inkjet head in a single pass and deposited on liner paper or coated board to obtain a printed product, and a laminating step in which the printed product and a medium are laminated to obtain a corrugated cardboard sheet. <10> A method for producing an inkjet printed product according to <9>, in which, in the printing step, droplets of an aqueous white ink composition containing a white colorant and water are deposited on the liner paper or coated board, and then droplets of the aqueous ink composition are deposited on the liner paper or coated board to obtain the printed product.
[0013] According to the present invention, it is possible to provide a water-based ink composition for inkjet recording that is less likely to cause nozzle clogging while reducing the amount of volatile organic solvent, is less likely to cause transfer when printed on liner paper or a surface-coated substrate, and exhibits good color development even when applied on an ink layer of a water-based white ink, an ink set including the water-based ink composition, and a method for producing an inkjet printed item using the water-based ink composition.
[0014] Specific embodiments to which the present invention is applied will be described in detail below. In this specification, "C.I." is an abbreviation for Color Index. In addition, in this specification, the term "(meth)acrylic acid" means both "acrylic acid" and "methacrylic acid." The same applies to terms such as "(meth)acrylate."
[0015] <Water-Based Ink Composition> The water-based ink composition according to this embodiment contains a non-white colorant, a water-soluble organic solvent, a humectant, a surfactant, and water, wherein the humectant contains a sugar alcohol, the water-soluble organic solvent contains a specific solvent having a ClogP value of 0.5 or more and 2.0 or less, the content of the water-soluble organic solvent is more than 0% by mass and 5% by mass or less, and the content of the water-soluble organic solvent having a boiling point of 250°C or less at 1 atmosphere is 3% by mass or less.
[0016] Each component contained in the water-based ink composition according to this embodiment will be described in detail below. Note that each of the following components may be used alone or in combination of two or more.
[0017] <Non-white coloring material> The water-based ink composition according to this embodiment contains a non-white coloring material. Examples of non-white coloring materials include pigments, disperse dyes, and solvent dyes. Among these, pigments are preferred from the viewpoint of image fastness, such as light fastness and water fastness, of the recorded image. Examples of pigments include inorganic pigments, organic pigments, and extender pigments.
[0018] Examples of inorganic pigments include carbon black, metal oxides, metal hydroxides, metal sulfides, metal ferrocyanides, and metal chlorides.
[0019] When a black ink composition is prepared, the inorganic pigment is preferably carbon black such as furnace black, lamp black, acetylene black, or channel black. Commercially available carbon black products include, for example, Raven 760 ULTRA, Raven 780 ULTRA, Raven 790 ULTRA, Raven 1060 ULTRA, Raven 1080 ULTRA, Raven 1170, Raven 1190 ULTRA II, Raven 1200, Raven 1250, Raven 1255, Raven 1500, Raven 2000, Raven 2500U ULTRA, Raven 3500, Raven 5000 ULTRA II, Raven 5250, Raven 5750, Raven 7000 (all manufactured by Columbia Carbon); Monarch 700, Monarch 800, Monarch 880, Monarch 900, Monarch 1000, Monarch 1100, Monarch 1300, Monarch 1400, Regal 1330R, Regal 1400R, Regal 1660R, Mogul L (all manufactured by Cabot Corporation); Color Black FW1, Color Black FW2, Color Black FW2V, Color Black FW200, Color Black S150, Color Black S160, Color Black S170, Printex 35, Printex U, Printex V, Printex 140U, Printex 140V, Special Black 4, Special Black 4A, Special Black 5, Special Black 6, Nerox 305, Nerox 505, Nerox 510, Nerox 600, Nerox 605, NIPex 180IQ, NIPex 170IQ, NIPex 160IQ, NIPex 150IQ (all manufactured by Orion Engineered Carbons); MA7, MA8, MA100, MA600, MCF-88, No. 25, No. No. 33, No. 40, No. 47, No. 52, No. 900, No. 2300 (all manufactured by Mitsubishi Chemical Corporation);
[0020] Examples of organic pigments include various pigments such as azo, disazo, phthalocyanine, quinacridone, isoindolinone, dioxazine, perylene, perinone, thioindigo, anthraquinone, and quinophthalone. Specific examples of organic pigments include yellow pigments such as C.I. Pigment Yellow 1, 2, 3, 12, 13, 14, 16, 17, 24, 55, 73, 74, 75, 83, 93, 94, 95, 97, 98, 108, 114, 128, 129, 138, 139, 150, 151, 154, 155, 180, 185, 193, 199, 202, and 213; red pigments such as C.I. Pigment Red 5, 7, 12, 48, 48:1, 57, 88, 112, 122, 123, 146, 149, 150, 166, 168, 177, 178, 179, 184, 185, 202, 206, 207, 254, 255, 257, 260, 264, 272; blue pigments such as C.I. Pigment Blue 1, 2, 3, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 22, 25, 60, 66, 80; violet pigments such as C.I. Pigment Violet 19, 23, 29, 37, 38, 50; Examples of suitable pigments include orange pigments such as C.I. Pigment Orange 13, 16, 68, 69, 71, and 73; green pigments such as C.I. Pigment Green 7, 36, and 54; and black pigments such as C.I. Pigment Black 1.
[0021] Examples of extender pigments include silica, calcium carbonate, talc, clay, barium sulfate, and white carbon.
[0022] Among the above-mentioned pigments, the inorganic pigment is preferably carbon black.In addition, the organic pigment is preferably at least one selected from the group consisting of C.I. Pigment Blue 15:3, 15:4; C.I. Pigment Yellow 74, 155; C.I. Pigment Red 122, 150; and C.I. Pigment Violet 19;, and more preferably at least one selected from the group consisting of C.I. Pigment Blue 15:4; C.I. Pigment Yellow 155; C.I. Pigment Red 122, 150; and C.I. Pigment Violet 19. When a pigment is used as the non-white coloring material, two or more pigments having different hues can be used in combination for the purpose of adjusting the hue.
[0023] Specific examples of disperse dyes include C.I. Disperse Yellow 3, 4, 5, 7, 9, 13, 24, 30, 33, 34, 42, 44, 49, 50, 51, 54, 56, 58, 60, 63, 64, 66, 68, 71, 74, 76, 79, 82, 83, 85, 86, 88, 90, 91, 93, 98, 99, 100, 104, 114, 116, 118, 119, 122, 124, 1 Yellow dyes such as C.I. 26, 135, 140, 141, 149, 160, 162, 163, 164, 165, 179, 180, 184:1, 182, 183, 184, 186, 192, 198, 199, 201, 202, 204, 210, 211, 215, 216, 218, 224, 231, 232, 241; Orange dyes such as C.I. Disperse Orange 1, 3, 5, 7, 11, 13, 17, 20, 21, 25, 26, 29, 30, 31, 32, 33, 37, 38, 42, 43, 44, 45, 47, 48, 50, 53, 54, 55, 56, 57, 58, 59, 61, 66, 76, 78, 80, 89, 90, 91, 93, 96, 97, 119, 127, 130, 139, 142; 1, 4, 5, 7, 11, 12, 13, 15, 17, 27, 43, 44, 50, 52, 53, 54, 55, 56, 58, 59, 60, 65, 72, 73, 74, 75, 76, 78, 81, 82, 86, 88, 90, 91, 93, 96, 103, 105, 106, 107, 108, 110, 111, 113, 117, 118, 121, 122, 126, 127, 128, 131, 132, 134, 135, 137, 143, 145, 146, 151, 152, 153, 154 , 157, 159, 164, 167, 169, 177, 179, 181, 183, 184, 185, 188, 189, 190, 191, 192, 200, 201, 202, 203, 205, 206, 207, 210, 221, 224, 225, 227, 229, 239, 240, 257, 258, 277, 278, 279, 281, 288, 289, 298, 302, 303, 310, 311, 312, 320, 324, 328, 343, 362, 364, and the like red dyes;Violet dyes such as C.I. Disperse Violet 1, 4, 8, 17, 23, 26, 27, 28, 31, 33, 35, 36, 38, 40, 43, 46, 48, 50, 51, 52, 56, 57, 59, 61, 63, 69, and 77; green dyes such as C.I. Disperse Green 6:1 and 9; brown dyes such as C.I. Disperse Brown 1, 2, 4, 9, 13, 19, 26, and 27; and C.I. Disperse Blue. 3, 7, 9, 14, 16, 19, 20, 26, 27, 35, 43, 44, 54, 55, 56, 58, 60, 62, 64, 71, 72, 73, 75, 79, 81, 82, 83, 87, 91, 93, 94, 95, 96, 102, 106, 108, 112, 113, 115, 118, 120, 122, 125, 128, 130, 139, 141, 142, 143, 146, 148, 149, 153, 154, 158, Blue dyes such as C.I. Disperse Black 1, 3, 10, 24, and the like; and black dyes such as C.I. Disperse Black 1, 3, 10, and 24.
[0024] Specific examples of solvent dyes include yellow dyes such as C.I. Solvent Yellow 2, 6, 14, 16, 21, 25, 29, 30, 33, 51, 56, 77, 80, 82, 88, 89, 93, 116, 150, 160: 1, 163, 179; orange dyes such as C.I. Solvent Orange 1, 2, 14, 45, 60; red dyes such as C.I. Solvent Red 1, 3, 7, 8, 9, 18, 19, 23, 24, 25, 27, 49, 100, 109, 121, 122, 125, 127, 130, 132, 135, 218, 225, 230; Examples of suitable dyes include violet dyes such as C.I. Solvent Violet 13 and 31; green dyes such as C.I. Solvent Green 3; brown dyes such as C.I. Solvent Brown 3 and 5; blue dyes such as C.I. Solvent Blue 2, 11, 14, 24, 25, 35, 36, 38, 48, 55, 59, 63, 67, 68, 70, 73, 83, 105, 111, and 132; and black dyes such as C.I. Solvent Black 3, 5, 7, 23, 27, 28, 29, and 34.
[0025]
[0042] The content of the non-white colorant in the aqueous ink composition according to this embodiment is typically from 0.5% to 30% by mass, preferably from 1% to 10% by mass, more preferably from 2% to 7% by mass, even more preferably from 3% to 7% by mass, and particularly preferably from 3% to 6% by mass. By achieving such a content, the storage stability and printing stability of the aqueous ink composition and the scratch resistance of printed images tend to be improved, and even when applied onto an ink layer of an aqueous white ink composition, the dot diameter tends to be less likely to become small and good color development tends to be exhibited.
[0026] <Water-soluble organic solvent> The water-based ink composition according to this embodiment contains a water-soluble organic solvent. In this specification, the water-soluble organic solvent refers to an organic solvent whose solubility in 100 g of water at 25°C is 0.05 g or more.
[0027] The water-soluble organic solvent contains one or more specific solvents, preferably two or more specific solvents, and more preferably three or more specific solvents, each having a ClogP value of 0.5 or more and 2.0 or less. When the water-soluble organic solvent contains a specific solvent, the water-based ink composition tends to have good redispersibility when dried, and nozzle clogging can be prevented.
[0028] Here, the ClogP value refers to a calculated logP value (1-octanol / water partition coefficient). The ClogP value can be calculated by the fragment method, the atomic approach method, or the like. More specifically, the ClogP value can be calculated using the fragment method described in the literature (C. Hansch and A. Leo, "Substitute Constants for Correlation Analysis in Chemistry and Biology" (John Wiley & Sons, New York, 1969)) or a commercially available software package. The ClogP values described herein were calculated using the commercially available software package ChemDraw Ultra (CambridgeSoft Corporation, USA). In this specification, the ClogP value may be written to one to three decimal places, and the lowest decimal place written is the number one decimal place below the lowest decimal place rounded up or down.
[0029] Examples of specific solvents include diethylene glycol diethyl ether (0.52), 1,2-hexanediol (0.53), diethylene glycol monoisobutyl ether (0.54), propylene glycol monopropyl ether (0.62), diethylene glycol monobutyl ether (0.67), dipropylene glycol monopropyl ether (0.75), 2,2-diethyl-1,3-propanediol (0.82), propylene glycol monobutyl ether (1.15), triethyl citrate (1.17), diethylene glycol monophenyl ether (1.25), 2-ethyl-1,3-hexanediol (1.26), 1,2-octanediol (1.59), diethylene glycol monohexyl ether (1.72), and ethylene glycol monohexyl ether (1.90). The numbers in parentheses indicate the ClogP values of each organic solvent. Among these, a specific solvent having a ClogP value of 0.52 or more and 1.9 or less is preferred, and a specific solvent having a ClogP value of 0.53 or more and 1.8 or less is more preferred.
[0030] The content of the specific solvent in the water-based ink composition according to this embodiment is more than 0% by mass and not more than 5% by mass, and may be 0.4% by mass to 5% by mass, 0.4% by mass to 3.5% by mass, 0.4% by mass to 3% by mass, 0.4% by mass to 2.5% by mass, 0.4% by mass to 2% by mass, or 0.4% by mass to 1.5% by mass.
[0031] The water-soluble organic solvent may further include a water-soluble organic solvent having a Clog P value of less than 0.5 or a water-soluble organic solvent having a Clog P value of greater than 2.0. Examples of water-soluble organic solvents having a Clog P value of less than 0.5 include ethyl lactate (0.33), 3-methoxy-1-butanol (0.02), propylene glycol (-1.06), 1,4-butanediol (-1.16), diethylene glycol (-1.30), ethylene glycol (-1.37), triethylene glycol (-1.48), glycerin (-1.54), and tetraethylene glycol (-1.66). Examples of water-soluble organic solvents having a Clog P value of greater than 2.0 include 1-heptanol (2.41), dibutyl carbitol (2.63), diethylene glycol mono-2-ethylhexyl ether (2.65), and Texanol (2.74). The values in parentheses indicate the ClogP values of each organic solvent.
[0032] The content of the water-soluble organic solvent including the specific solvent in the aqueous ink composition according to this embodiment is more than 0% by mass and not more than 5% by mass, and may be 0.4% by mass to 5% by mass, 0.4% by mass to 3.5% by mass, 0.4% by mass to 3% by mass, 0.4% by mass to 2.5% by mass, 0.4% by mass to 2% by mass, or 0.4% by mass to 1.5% by mass. By setting the content in this range, it tends to be possible to reduce the amount of organic solvent that volatilizes into the atmosphere during printing.
[0033] In the aqueous ink composition according to this embodiment, the content of the water-soluble organic solvent having a boiling point of 250° C. or less at 1 atmosphere is 3% by mass or less, preferably 2.5% by mass or less, and more preferably 2% by mass or less. By setting the content to such a level, the amount of organic solvent volatilized into the atmosphere during printing tends to be further reduced, and harmfulness to humans and the environment can be reduced.
[0034] <Humectant> The aqueous ink composition according to this embodiment contains a humectant. The humectant is preferably one that is miscible with water and has the effect of preventing clogging in the ejection nozzles of an inkjet head and resolubilizing the aqueous ink composition when it dries. A humectant that is solid at room temperature (25°C) can also be used as the humectant. Solid humectants can hold more water than liquid humectants, making them suitable for aqueous ink compositions for inkjet recording. Examples of solid humectants include ethylene carbonate, urea, ethylene urea, dimethylethylene urea, acetamide, and ε-caprolactam. Of these, a water-soluble solid humectant (hereinafter also referred to as a "water-soluble solid humectant") is preferred. The water-soluble solid humectant is added to prevent the aqueous ink composition from drying out in the ejection nozzles of an inkjet head.
[0035] The aqueous ink composition according to this embodiment contains a sugar alcohol as a water-soluble solid humectant. Sugar alcohols are compounds formed by reducing sugar compounds (e.g., aldoses and ketoses). Sugar alcohols have many hydroxyl groups and therefore have excellent solubility in water.
[0036] The melting point of sugar alcohols under 1 atmosphere is above 25°C. Therefore, sugar alcohols are solid at room temperature (25°C). The melting point of sugar alcohols is usually above 25°C and not more than 270°C, preferably from 50°C to 250°C, more preferably from 50°C to 200°C, even more preferably from 50°C to 170°C, and particularly preferably from 50°C to 150°C. By using sugar alcohols within such a melting point range, images with excellent fixability, drying properties, abrasion resistance, and transfer resistance tend to be obtained.
[0037] Examples of sugar alcohols include threitol (melting point: 88-90°C), erythritol (melting point: 121°C), arabitol (melting point: 103°C), ribitol (melting point: 102°C), xylitol (melting point: 92-96°C), sorbitol (glucitol) (melting point: 95°C), mannitol (melting point: 164-169°C), iditol (melting point: 75-79°C), galactitol (melting point: 186-191°C), allitol (melting point: 150-154°C), maltitol (melting point: 145°C), isomaltitol (melting point: 98-103°C), lactitol (melting point: 146°C), and pentaerythritol (melting point: 190-263°C). Among these, sorbitol (glucitol) is preferred. The sugar alcohol may contain unreduced sugar compounds (e.g., glucose) as impurities.
[0038] The sugar alcohol content in the aqueous ink composition according to this embodiment is typically 4% by mass to 10% by mass, preferably 4% by mass to 9% by mass, more preferably 4.5% by mass to 8% by mass, even more preferably 5% by mass to 8% by mass, and particularly preferably 6% by mass to 7.5% by mass. By setting the content in this range, it is possible to achieve a good balance between redispersibility, drying property, and transfer resistance.
[0039] The above-mentioned specific solvent and sugar alcohol can be used in any ratio. By changing the ratio of the specific solvent and sugar alcohol, it is possible to improve redispersibility, drying property, and transfer resistance, and further improve color development. When the content of the specific solvent in the aqueous ink composition according to this embodiment is A (parts by mass), the content of the sugar alcohol is B (parts by mass), and the ratio is expressed as the value calculated by "A / B," A / B is usually 0.01 or more and 1.25 or less, preferably 0.10 or more and 1.00 or less, more preferably 0.10 or more and 0.90 or less, even more preferably 0.10 or more and 0.80 or less, and particularly preferably 0.10 or more and 0.70 or less.
[0040] <Surfactant> The aqueous ink composition according to this embodiment contains a surfactant for the purpose of adjusting the surface tension, etc. Examples of surfactants include anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, silicone surfactants, and fluorine-based surfactants. Among these, anionic, nonionic, and silicone surfactants are preferred, and nonionic and silicone surfactants are more preferred.
[0041] Examples of anionic surfactants include alkyl sulfocarboxylates, α-olefin sulfonates, polyoxyethylene alkyl ether acetates, polyoxyethylene alkyl ether sulfates, N-acylamino acids or salts thereof, N-acylmethyltaurines, alkyl sulfates, polyoxyalkyl ether sulfates, alkyl sulfates, polyoxyethylene alkyl ether phosphates, rosin acid soaps, castor oil sulfates, lauryl alcohol sulfates, alkylphenol phosphates, alkyl phosphates, alkylaryl sulfonates, diethyl sulfosuccinates, diethylhexyl sulfosuccinates, dioctyl sulfosuccinates, etc. Examples of commercially available products include Hitenol LA-10, LA-12, LA-16, Neo Hitenol ECL-30S, and ECL-45 (all manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.).
[0042] Examples of cationic surfactants include 2-vinylpyridine derivatives and poly(4-vinylpyridine) derivatives.
[0043] Examples of nonionic surfactants include ether-based surfactants such as polyoxyethylene nonylphenyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene dodecylphenyl ether, polyoxyethylene oleyl ether, polyoxyethylene lauryl ether, and polyoxyethylene alkyl ether; ester-based surfactants such as polyoxyethylene oleate, polyoxyethylene distearate, sorbitan laurate, sorbitan monostearate, sorbitan monooleate, sorbitan sesquioleate, polyoxyethylene monooleate, and polyoxyethylene stearate; acetylene glycol (alcohol)-based surfactants such as 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 3,6-dimethyl-4-octyne-3,6-diol, and 3,5-dimethyl-1-hexyne-3-ol; Surfynol 104, 104PG50, 105PG50, 82, 420, 440, 465, 485, and Olfine. Examples of suitable surfactants include STG (both manufactured by Nissin Chemical Industry Co., Ltd.); polyglycol ether-based surfactants (for example, TergItol 15-S-7 manufactured by SIGMA-ALDRICH); and the like.
[0044] Examples of amphoteric surfactants include lauryl dimethylaminoacetic acid betaine, 2-alkyl-N-carboxymethyl-N-hydroxyethyl imidazolinium betaine, coconut oil fatty acid amidopropyl dimethylaminoacetic acid betaine, polyoctyl polyaminoethyl glycine, and imidazoline derivatives.
[0045] Examples of silicone surfactants include polyether-modified siloxanes and polyether-modified polydimethylsiloxanes. Commercially available products include BYK-306, BYK-307, BYK-333, BYK-341, BYK-345, BYK-346, BYK-347, BYK-348, BYK-349, BYK-3420, BYK-3450, BYK-3455, BYK-3565, and BYK-3760 (all manufactured by BYK-Chemie); and KF-3 51A, KF-352A, KF-353, KF-354L, KF-355A, KF-615A, KF-945, KF-640, KF-642, KF-643, KF-6020, X-22-4515, KF-6011, KF-6012, KF-6015, KF-6017 (all manufactured by Shin-Etsu Chemical Co., Ltd.); and the like.
[0046] Examples of fluorine-based surfactants include perfluoroalkyl sulfonic acid compounds, perfluoroalkyl carboxylic acid compounds, perfluoroalkyl phosphate ester compounds, perfluoroalkyl ethylene oxide compounds, polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups on the side chain, etc. Commercially available products include Zonyl TBS, FSP, FSA, FSN-100, FSN, FSO-100, FSO, and FS-300 (all manufactured by DuPont); Capstone FS-30, FS-31, and FS-3100 (all manufactured by Chemours); PF-151N and PF-154N (all manufactured by Omnova); F-114, F-410, F-444, EXP. TF-2066, EXP. TF-2148, and EXP. Examples of suitable acrylic resins include TF-2149, F-430, F-477, F-552, F-553, F-554, F-555, F-556, F-557, F-558, F-559, F-561, F-562, R-40, R-41, RS-72-K, RS-75, RS-76-E, RS-76-NS, RS-77, EXP. TF-1540, and EXP. TF-1760 (all manufactured by DIC Corporation); BYK-340, BYK-3440, and BYK-3441 (all manufactured by BYK-Chemie).
[0047] The surfactant content in the aqueous ink composition according to this embodiment is typically 0.1% by mass to 5% by mass, preferably 0.3% by mass to 4% by mass, and more preferably 0.5% by mass to 3% by mass. This content tends to improve the penetration into the substrate and the dispersion stability of non-white colorants in the aqueous ink composition.
[0048] <Water> The water-based ink composition according to this embodiment contains water. As the water, water with a low content of impurities such as metal ions, that is, ion-exchanged water, distilled water, or the like, is preferred.
[0049] The water content in the water-based ink composition according to this embodiment is typically 50% by mass or more and 90% by mass or less, preferably 60% by mass or more and 90% by mass or less, and more preferably 70% by mass or more and 90% by mass or less.
[0050] Ink Preparation Agents The aqueous ink composition according to this embodiment may further contain ink preparation agents in addition to the components described above. Examples of ink preparation agents include viscosity adjusters, antifoaming agents, antifungal agents, preservatives, pH adjusters, chelating agents, rust inhibitors, water-soluble UV absorbers, water-soluble polymer compounds, dispersants, resin emulsions, waxes, and antioxidants.
[0051] [Viscosity Adjuster] The viscosity range of ink that can be ejected from an industrial inkjet printer is usually determined based on the specifications of the printer head installed in the printer, and therefore it may be important to add a viscosity adjuster to the ink composition to adjust the viscosity within an appropriate range.
[0052] The viscosity adjuster is not particularly limited as long as it is a substance that can adjust the viscosity of the water-based ink composition, and known substances can be used. Specific examples include the water-soluble polymer compounds described below.
[0053] [Antifoaming Agent] Examples of antifoaming agents include silicone-based, silica mineral oil-based, olefin-based, acetylene-based compounds, etc. Commercially available products include Surfynol DF37, DF58, DF110D, DF220, MD-20, and Olfine SK-14 (all manufactured by Nissin Chemical Industry Co., Ltd.); BYK-1719, BYK-1724, and BYK-1770 (all manufactured by BYK-Chemie).
[0054] [Anti-fungal Agent] Examples of anti-fungal agents include sodium dehydroacetate, sodium benzoate, sodium pyridinethione-1-oxide, p-hydroxybenzoic acid ethyl ester, 1,2-benzisothiazolin-3-one and salts thereof.
[0055] [Preservatives] Examples of preservatives include organic sulfur compounds, organic nitrogen sulfur compounds, organic halogen compounds, haloarylsulfone compounds, iodopropargyl compounds, haloalkylthio compounds, nitrile compounds, pyridine compounds, 8-oxyquinolines, benzothiazole compounds, isothiazolinone compounds, dithiols, pyridine oxide compounds, nitropropane compounds, organic tin compounds, phenol compounds, quaternary ammonium salt compounds, triazine compounds, thiazine compounds, anilides, adamantane compounds, dithiocarbamates, brominated indanone compounds, benzyl bromoacetate compounds, and inorganic salt compounds. Specific examples of organic halogen compounds include sodium pentachlorophenol. Specific examples of pyridine oxide compounds include sodium 2-pyridinethiol-1-oxide. Specific examples of isothiazoline compounds include 1,2-benzisothiazolin-3-one, 2-n-octyl-4-isothiazolin-3-one, 5-chloro-2-methyl-4-isothiazolin-3-one, 5-chloro-2-methyl-4-isothiazolin-3-one magnesium chloride, 5-chloro-2-methyl-4-isothiazolin-3-one calcium chloride, 2-methyl-4-isothiazolin-3-one calcium chloride, etc. Specific examples of other antiseptics and antifungals include anhydrous sodium acetate, sodium sorbate, sodium benzoate; Proxel GXL(S), Proxel XL-2(S) (all manufactured by Arch Chemical Co., Ltd.); etc.
[0056] [pH Adjuster] Examples of pH adjusters include alkanolamines such as diethanolamine, triethanolamine, N-methyldiethanolamine, and 2-amino-2-methyl-1-propanol; alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, and potassium hydroxide; ammonium hydroxide (aqueous ammonia); alkali metal carbonates such as lithium carbonate, sodium carbonate, sodium bicarbonate, and potassium carbonate; alkali metal salts of organic acids such as sodium silicate and potassium acetate; and inorganic bases such as disodium phosphate. Note that pH adjusters are not considered to be the water-soluble organic solvents described above.
[0057] [Chelating Reagents] Examples of chelating agents include disodium ethylenediaminetetraacetate, sodium nitrilotriacetate, sodium hydroxyethylethylenediaminetriacetate, sodium diethylenetriaminepentaacetate, and sodium uracildiacetate.
[0058] [Rust Inhibitor] Examples of the rust inhibitor include acid sulfite, sodium thiosulfate, ammonium thioglycolate, diisopropylammonium nitrite, pentaerythritol tetranitrate, and dicyclohexylammonium nitrite.
[0059] [Water-Soluble UV Absorber] Examples of water-soluble UV absorbers include sulfonated benzophenone compounds, benzotriazole compounds, salicylic acid compounds, cinnamic acid compounds, and triazine compounds.
[0060] [Water-Soluble Polymer Compounds] Examples of water-soluble polymer compounds include polyethylene glycol, polyvinyl alcohol, cellulose derivatives, polysaccharides, polyamines, polyimines, and neutralized aqueous solutions of styrene-acrylic copolymers.
[0061] [Dispersant] Examples of dispersants include copolymers composed of at least two monomers (preferably at least one of which is a hydrophilic monomer) selected from the group consisting of styrene and its derivatives, vinylnaphthalene and its derivatives, aliphatic alcohol esters of α,β-ethylenically unsaturated carboxylic acids, (meth)acrylic acid and its derivatives, maleic acid and its derivatives, itaconic acid and its derivatives, fumaric acid and its derivatives, vinyl acetate, vinyl alcohol, vinylpyrrolidone, acrylamide, and their derivatives. Examples of hydrophilic monomers include monomers that leave a carboxy group after polymerization, such as (meth)acrylic acid.
[0062] Examples of such copolymers include styrene-(meth)acrylic acid copolymers, styrene-(meth)acrylic acid-(meth)acrylic acid ester copolymers, (meth)acrylic acid ester-(meth)acrylic acid copolymers, polyethylene glycol (meth)acrylate-(meth)acrylic acid copolymers, and styrene-maleic acid copolymers. Among these, styrene-(meth)acrylic acid copolymers, styrene-(meth)acrylic acid-(meth)acrylic acid ester copolymers, (meth)acrylic acid ester-(meth)acrylic acid copolymers, and polyethylene glycol (meth)acrylate-(meth)acrylic acid copolymers are preferred, with styrene-(meth)acrylic acid copolymers, styrene-(meth)acrylic acid-(meth)acrylic acid ester copolymers, and (meth)acrylic acid ester-(meth)acrylic acid copolymers being more preferred, with (meth)acrylic acid ester-(meth)acrylic acid copolymers being even more preferred, and methacrylic acid ester-methacrylic acid copolymers being particularly preferred. Examples of copolymer types include block copolymers, random copolymers, and graft copolymers, with block copolymers being preferred. These copolymers may be in the form of a salt.
[0063] Dispersants can be synthesized or commercially available.
[0064] Examples of commercially available dispersants include JONCRYL 62, 67, 68, 678, and 687 (styrene-acrylic copolymers manufactured by BASF); MOVINYL S-100A (modified vinyl acetate copolymer manufactured by Japan Coating Resins Co., Ltd.); and JURYMER AT-210 (polyacrylic acid ester copolymer manufactured by Nippon Junyaku Co., Ltd.).
[0065] Examples of dispersants obtained by synthesis include the A-B block polymer disclosed in WO 2013 / 115071. The monomer constituting the A block of the A-B block polymer disclosed in WO 2013 / 115071 is at least one monomer selected from (meth)acrylic acid and linear or branched C4 alkyl (meth)acrylates, with at least one monomer selected from methacrylic acid and n-butyl methacrylate being preferred, and a combination of these two monomers is even more preferred. Furthermore, the monomer constituting the B block of the A-B block polymer disclosed in WO 2013 / 115071 is at least one monomer selected from benzyl methacrylate and benzyl acrylate, with benzyl methacrylate being preferred. Specific examples of A-B block polymers include the block copolymers disclosed in Synthesis Examples 3 to 8 of WO 2013 / 115071.
[0066] [Resin Emulsion] The resin emulsion is not particularly limited as long as it is different from the dispersant described above, and examples thereof include urethane-based resins, polyester resins, acrylic-based resins, vinyl acetate-based resins, vinyl chloride-based resins, acrylic styrene-based resins, and acrylic silicone-based resins. Commercially available products include, for example, Superflex 126, 150, 170, 210, 420, 470, 820, 830, 860, and 890 (urethane resin emulsions manufactured by Daiichi Kogyo Seiyaku Co., Ltd.); Hydran HW-350, HW-178, HW-163, HW-171, AP-20, AP-30, AP-40F, WLS-201, and WLS-210 (urethane resin emulsions manufactured by DIC Corporation); 0569, 0850Z, and 2108 (styrene-butadiene resin emulsions manufactured by JSR Corporation); AE980, AE981A, AE982, AE986B, and AE104 (acrylic resin emulsions manufactured by E-Tech Co., Ltd.); and Saivinol. SK-200 (acrylic resin emulsion manufactured by Saiden Chemical Co., Ltd.); Boncoat 4001, 5454 (acrylic resin emulsions manufactured by DIC Corporation); and the like.
[0067] When the aqueous ink composition according to this embodiment contains a resin emulsion, the solids content is typically from 0.1% by mass to 10% by mass, preferably from 0.3% by mass to 9% by mass, more preferably from 0.5% by mass to 8% by mass, even more preferably from 1% by mass to 8% by mass, and particularly preferably from 1.5% by mass to 8% by mass.
[0068] [Waxing Agent] The waxing agent is preferably a wax emulsion, and more preferably an aqueous wax emulsion. Natural waxes and synthetic waxes can be used as the waxing agent. Examples of natural waxes include petroleum-based waxes such as paraffin wax and microcrystalline wax; lignite-based waxes such as montan wax; plant-based waxes such as carnauba wax and candelilla wax; and animal and plant-based waxes such as beeswax and lanolin. Examples of synthetic waxes include polyalkylene waxes (preferably poly C2-C4 alkylene wax), oxidized polyalkylene waxes (preferably poly C2-C4 alkylene wax), and paraffin wax. Among these synthetic waxes, at least one wax selected from polyethylene wax, polypropylene wax, oxidized polyethylene wax, oxidized polypropylene wax, and paraffin wax is preferred, with oxidized polyethylene wax being more preferred. Furthermore, the average particle size of the wax is preferably 50 nm or more and 5 μm or less, and more preferably 100 nm or more and 1 μm or less, in order to prevent clogging of the inkjet head.
[0069] Examples of commercially available wax emulsions include AQUACER 515 (acid value: 5 mgKOH / g) manufactured by BYK Japan KK and HYTEC E-6500 (acid value: 10 to 20 mgKOH / g) manufactured by Toho Chemical Industry Co., Ltd.
[0070] When the aqueous ink composition according to this embodiment contains a wax agent, the solids content is typically from 0.1% by mass to 5% by mass, preferably from 0.2% by mass to 3% by mass, more preferably from 0.5% by mass to 3% by mass, even more preferably from 0.5% by mass to 2% by mass, and particularly preferably from 0.5% by mass to 1.5% by mass.
[0071] [Antioxidant] As the antioxidant, for example, various organic and metal complex anti-fading agents can be used. Examples of organic anti-fading agents include hydroquinones, alkoxyphenols, dialkoxyphenols, phenols, anilines, amines, indanes, chromans, alkoxyanilines, and heterocycles.
[0072] <Method for preparing aqueous ink composition> The method for preparing the aqueous ink composition according to this embodiment is not particularly limited, and any known preparation method can be used. Examples of the preparation method include a method in which an aqueous dispersion containing a non-white colorant and a dispersant is prepared, and water, a water-soluble organic solvent, a sugar alcohol, a surfactant, and, if necessary, an ink preparation agent are added to the aqueous dispersion and mixed.
[0073] When the water-based ink composition according to this embodiment is used in inkjet recording, it is preferable to filter the water-based ink composition to remove aggregates and the like. As a filtration method, any known method can be appropriately adopted. For example, suction filtration using filter paper such as glass filter paper GC-50 (retention particle diameter: 0.5 μm, manufactured by Advantec Co., Ltd.) or glass filter paper GA-100 (retention particle diameter: 1.0 μm, manufactured by Advantec Co., Ltd.) can be used.
[0074] The viscosity of the water-based ink composition according to this embodiment at 25°C is typically from 2.0 mPa·s to 10 mPa·s, preferably from 3.0 mPa·s to 8.0 mPa·s, more preferably from 3.5 mPa·s to 7.5 mPa·s, and even more preferably from 4.0 mPa·s to 7.5 mPa·s. The viscosity of the water-based ink composition can be measured using a commercially available E-type viscometer. Examples of commercially available E-type viscometers include a TR-100E viscometer, a TV-100E viscometer, a TP-200E viscometer, and a RE-215 viscometer (all manufactured by Toki Sangyo Co., Ltd.).
[0075] The aqueous ink composition according to this embodiment has excellent redispersibility and storage stability. Furthermore, images recorded with the aqueous ink composition according to this embodiment, whether or not the images are formed on an ink layer of an aqueous white ink composition, have excellent color development and saturation, and also have excellent fastness properties such as abrasion resistance, heat abrasion resistance, transfer resistance, water resistance, light resistance, heat resistance, and oxidizing gas resistance (for example, ozone gas resistance). Furthermore, the aqueous ink composition according to this embodiment has excellent drying properties during image formation, little coating unevenness and bleeding, and large dot diameters, resulting in excellent image formability.
[0076] Ink Set The ink set according to this embodiment includes the water-based ink composition according to this embodiment described above, and a water-based white ink composition containing a white colorant and water.
[0077] <Water-based white ink composition> The water-based white ink composition contains a white colorant and water. Each component contained in the water-based white ink composition will be described in detail below. Note that each of the following components may be used alone or in combination of two or more.
[0078] [White Colorant] The water-based white ink composition contains a white colorant. The white colorant is not particularly limited as long as it is visually recognizable as white by the human eye, and examples thereof include white inorganic pigments such as titanium oxide, zinc oxide, zinc sulfide, antimony oxide, and zirconium oxide; and white organic pigments such as white hollow resin particles and polymer particles. Specific examples include C.I. Pigment White 1 (basic lead carbonate), C.I. Pigment White 4 (zinc oxide), C.I. Pigment White 5 (mixture of zinc sulfide and barium sulfate), C.I. Pigment White 6 (titanium oxide), C.I. Pigment White 6:1 (titanium oxide containing other metal oxides), C.I. Pigment White 7 (zinc sulfide), C.I. C.I. Pigment White 18 (Calcium Carbonate), C.I. Pigment White 19 (Clay), C.I. Pigment White 20 (Titanium Mica), C.I. Pigment White 21 (Barium Sulfate), C.I. Pigment White 22 (Natural Barium Sulfate), C.I. Pigment White 23 (Gloss White), C.I. Pigment White 24 (Alumina White), C.I. Pigment White 25 (Gypsum), C.I. Pigment White 26 (Magnesium Oxide-Silicon Oxide), C.I. Pigment White 27 (Silica), C.I. Pigment White 28 (anhydrous calcium silicate), and the like.
[0079] Titanium oxide may be surface-treated with silica or alumina. Such surface-treated titanium oxide is preferred because it has excellent coloring and hiding properties. The rutile type is preferred as the crystalline form of titanium oxide.
[0080] Commercially available titanium oxide products include, for example, Tipaque R-580, R-670, R-780, R-850, R-855, and CR-60 (all manufactured by Ishihara Sangyo Kaisha, Ltd.); JR-301, JR-403, JR-405, JR-804, JR-806, JR-600A, and JR-800 (all manufactured by Teika Corporation); and the like.
[0081] The white colorant may also be preferably used in the form of a dispersion (slurry) in which the white colorant is dispersed. Commercially available dispersions (slurries) include, for example, TF-5760 WHITE (D2B) (titanium oxide slurry, titanium oxide solids concentration: 60%, average particle size: 300 nm, manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd.).
[0082] The white colorant in a solid state can also be dispersed using a dispersant to form a dispersion liquid.
[0083] As the white hollow resin particles, for example, known white hollow resin particles described in U.S. Pat. No. 4,880,465, Japanese Patent No. 3,562,754, Japanese Patent No. 6,026,234, Japanese Patent No. 5,459,460, JP-A-2003-268694, Japanese Patent No. 4,902,216, etc. can be used.
[0084] The water-based white ink composition may further contain other coloring materials for the purpose of adjusting whiteness and brightness, as long as the effects of the present invention are not impaired.
[0085] The content of the white colorant in the water-based white ink composition is typically 1% by mass or more and 30% by mass or less, preferably 1% by mass or more and 20% by mass or less, more preferably 2% by mass or more and 15% by mass or less, and particularly preferably 5% by mass or more and 15% by mass or less.
[0086] [Water] The water-based white ink composition contains water. As the water, water with a low content of impurities such as metal ions, that is, ion-exchanged water, distilled water, etc., is preferred.
[0087] The water content in the water-based white ink composition is typically 10% by mass or more and 90% by mass or less, preferably 20% by mass or more and 80% by mass or less, more preferably 30% by mass or more and 80% by mass or less, and particularly preferably 40% by mass or more and 80% by mass or less.
[0088] [Other Components] In addition to the components described above, the water-based white ink composition may further contain a water-soluble organic solvent, a surfactant, and an ink preparation agent. Examples of the water-soluble organic solvent, surfactant, and ink preparation agent include those exemplified in the water-based ink composition according to this embodiment.
[0089] [Method for preparing water-based white ink composition] The method for preparing the water-based white ink composition is not particularly limited, and any known preparation method can be used. Examples of the preparation method include a method in which an aqueous dispersion containing a white colorant is prepared, and water and, if necessary, an ink preparation agent are added to the aqueous dispersion and mixed.
[0090] The water-based white ink composition is preferably microfiltered using glass filter paper or the like, similar to the water-based ink composition according to this embodiment described above.
[0091] The viscosity of the water-based white ink composition at 25°C is typically 2.0 mPa·s or more and 10 mPa·s or less, preferably 3.0 mPa·s or more and 8.0 mPa·s or less, more preferably 3.5 mPa·s or more and 7.5 mPa·s or less, and even more preferably 4.0 mPa·s or more and 7.5 mPa·s or less.
[0092] <<Method for Producing Inkjet Printed Material>> The method for producing an inkjet printed material according to this embodiment includes ejecting droplets of the water-based ink composition according to this embodiment described above from an inkjet head and depositing them on a printing medium to obtain a printed material.
[0093] The print media refers to a medium to which the water-based ink composition according to this embodiment can be adhered, and can be broadly divided into ink-absorbent print media and ink-poorly absorbent print media.
[0094] Examples of ink-absorbent printing media include inkjet paper, inkjet film, glossy paper, corrugated cardboard, liner paper contained in corrugated cardboard, etc. Specific examples of liner paper include K liner, C liner, lightweight liner, etc., commercially available from Oji Materia Co., Ltd., Nippon Paper Industries Co., Ltd., Daio Paper Co., Ltd., etc.
[0095] Examples of printing media that are poorly ink absorbent include various types of paper such as coated paper, lightweight coated paper, lightly coated paper, coated board, and art paper used in applications such as gravure printing and offset printing; cast coated paper used for label printing; etc. These printing media are formed by applying a coating agent to untreated fine paper or the like to provide a coating layer to impart whiteness, etc. Specific examples include OK Top Coat+ and Mirror Coat Platinum (both manufactured by Oji Paper Co., Ltd.); Aurora Coat (manufactured by Nippon Paper Industries Co., Ltd.); Pearl Coat (manufactured by Mitsubishi Paper Mills, Ltd.); Mari Coat (manufactured by Hokuetsu Corporation); Raicho Coat (manufactured by Chuetsu Pulp Industries Co., Ltd.); etc.
[0096] The water-based ink composition according to this embodiment can be applied to any printing medium, but is particularly suitable for use on liner paper and printing media that are poorly ink-absorbent, and is particularly suitable for use on corrugated cardboard, liner paper, and coated board.
[0097] When using a printing medium that is poorly ink-absorbent, it is preferable to subject the printing medium to a surface modification treatment in order to improve the fixation of coloring materials.
[0098] The surface modification treatment is preferably at least one treatment selected from the group consisting of corona discharge treatment, plasma treatment, and flame treatment. The surface modification of the printing medium can be performed by appropriately adjusting the number of treatments, treatment time, applied voltage, etc., so as to obtain the desired effect. The state of the surface modification can be confirmed by measuring the contact angle using a known method. It is generally known that the effect of the surface modification treatment weakens over time. Therefore, after the surface modification treatment has been performed on the printing medium, it is preferable to perform inkjet recording promptly.
[0099] There are no particular limitations on the nozzles of the inkjet printer used in the method for producing an inkjet printed matter according to this embodiment, and they can be selected appropriately depending on the purpose.
[0100] Known printing methods can be used for inkjet printers. Examples include a charge control method that uses electrostatic attraction to eject ink; a drop-on-demand method (pressure pulse method) that uses the vibration pressure of a piezoelectric element; an acoustic inkjet method that converts an electric signal into an acoustic beam and irradiates the ink with the resulting radiation pressure to eject the ink; and a thermal inkjet method that heats the ink to form bubbles and uses the resulting pressure. The above printing methods also include a method that improves the fixation of colorants by using a colorless and transparent ink composition. For industrial inkjet printers, single-pass printing using a linehead inkjet printer is also preferred for the purpose of increasing printing speed. The aqueous ink composition according to this embodiment can produce good printed products even under such printing conditions.
[0101] The inkjet head may be either one having an ink circulation mechanism or one not having an ink circulation mechanism. From the viewpoint of preventing the ink composition from drying in the vicinity of the nozzles, it is preferable to use an inkjet head having an ink circulation mechanism.
[0102] [Manufacturing of Corrugated Board Sheets] The method for manufacturing inkjet printed matter according to this embodiment can be suitably employed when manufacturing corrugated board sheets by a preprinting method.
[0103] When producing a cardboard sheet, a printing step in which droplets of the water-based ink composition according to the present embodiment described above are ejected from an inkjet head in a single pass and adhered to liner paper or coated board to obtain a printed matter, and a lamination step in which the obtained printed matter is laminated to a core to obtain a cardboard sheet are carried out successively.
[0104] (Printing Process) In the printing process, droplets of the water-based ink composition according to this embodiment are ejected from an inkjet head in a single pass and deposited on liner paper or a coated board to obtain a printed matter.
[0105] The nozzles of the inkjet printer are not particularly limited and can be selected appropriately depending on the purpose. In addition, any known printing method can be used for the inkjet printer.
[0106] To enhance the aesthetic appeal, in the printing process, droplets of a water-based white ink composition containing a white colorant and water may be deposited on liner paper or a coated board, and then droplets of the water-based ink composition according to this embodiment may be deposited on the liner paper or the coated board to obtain a printed product. The water-based ink composition according to this embodiment exhibits good color development properties even when deposited on the ink layer of the water-based white ink composition in this manner.
[0107] (Laminating Step) In the laminating step, the printed matter obtained in the printing step and a core are laminated together to obtain a cardboard sheet.
[0108] In the lamination process, a corrugator process can be used, in which an adhesive layer is formed on the surface of the core by applying an adhesive substance, and then the printed material and the core are overlapped and bonded by pressure and heat. The core can be any material commonly used in corrugated cardboard sheets, without any particular restrictions. Examples of adhesive substances include starch glue; synthetic resins such as polyethylene, polypropylene, polyamide, polyester, ethylene-unsaturated carboxylic acid copolymer, styrene-butadiene copolymer, butadiene-acrylonitrile copolymer, styrene-butadiene-acrylonitrile copolymer, polyvinyl acetate, ethylene-vinyl acetate copolymer, polyacrylic acid ester copolymer, and styrene-acrylic acid ester copolymer; and the like.
[0109] A single-faced corrugated fiberboard sheet can be produced by performing the corrugator process once, and multiple repetitions can produce double-faced or multi-column corrugated fiberboard sheets. Double-faced corrugated fiberboard sheets can be produced, for example, using a corrugator equipped with a single facer (SF), which laminates liner paper and a corrugating medium with a heating and pressurizing roll to form a single-faced corrugated fiberboard sheet, and a double facer (DF), which adds liner paper to the medium side of the single-faced corrugated fiberboard sheet obtained by the single facer and laminates it by running the sheet over a heated platen while applying pressure. The heating and pressurizing conditions are not particularly limited, but it is preferable that the single facer have a heating temperature of 150 to 200°C, a linear pressure of 20 to 40 kN / m, and a pressurizing time of 0.01 to 0.20 seconds, and that the double facer have a heating temperature of 150 to 200°C, a linear pressure of 0.1 to 1.0 kN / m, and a pressurizing time of 2 to 7 seconds.
[0110] By forming cuts into the cardboard sheet obtained as described above, a cardboard box can be obtained.
[0111] For all of the above items, combinations of preferred items are more preferred, and combinations of more preferred items are even more preferred. The same applies to combinations of preferred items and more preferred items, and combinations of more preferred items and even more preferred items.
[0112] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0113] In the examples, unless otherwise specified, "parts" means parts by mass and "%" means % by mass. When quantitative determination of the pigment solid content in the dispersion was required, it was calculated as a converted value of only the pigment solid content by a dry weight method using an MS-70 manufactured by A&D Co., Ltd.
[0114] Preparation Example 1: Preparation of Black Dispersion A block copolymer (dispersant) was obtained by reproducing Synthesis Example 3 of WO 2013 / 115071. The obtained block copolymer (6 parts) was dissolved in methyl ethyl ketone (20 parts) to obtain a uniform solution. To this solution, a mixed solution prepared by dissolving sodium hydroxide (0.45 parts) in water (53.55 parts) was added, followed by carbon black (Nerox 605, manufactured by Orion Engineered Carbons) (20 parts). The mixture was dispersed in a sand grinder at 1500 rpm for 15 hours to obtain a liquid. Water (100 parts) was added to the obtained liquid, and the mixture was filtered using glass filter paper GA-100 to remove aggregates and the like, thereby obtaining a filtrate. The methyl ethyl ketone and a portion of the water in the filtrate were distilled under reduced pressure using an evaporator to obtain a black dispersion (Kdp) with a pigment solids content of 12.0%.
[0115] Preparation Example 2 Preparation of Cyan Dispersion A cyan dispersion (Cdp) having a pigment solids content of 12.5% was obtained in the same manner as in Preparation Example 1, except that C.I. Pigment Blue 15:4 (manufactured by Dainichiseika Color & Chemicals Co., Ltd., Chromofine Blue 4851) was used instead of the carbon black used in Preparation Example 1.
[0116] Preparation Example 3 Preparation of Magenta Dispersion A magenta dispersion (Mdp) having a pigment solids content of 12.1% was obtained in the same manner as in Preparation Example 1, except that C.I. Pigment Red 122 (Clariant, Inkjet Magenta E02VP2621) was used instead of the carbon black used in Preparation Example 1.
[0117] Preparation Example 4 Preparation of Yellow Dispersion A yellow dispersion (Ydp) having a pigment solids content of 11.8% was obtained in the same manner as in Preparation Example 1, except that C.I. Pigment Yellow 155 (Clariant, Ink Jet Yellow 4G VP2532) was used instead of the carbon black used in Preparation Example 1.
[0118] <Preparation Example 5: Preparation of resin emulsion> A resin emulsion having an acid value of 6 mg KOH / g and a solids content of 25% was prepared by reproducing Preparation Example 4 of WO 2015 / 147192. This resin emulsion is designated "Resin 1".
[0119] Examples 1 to 25 and Comparative Examples 1 to 9: Preparation of Water-Based Ink Compositions The components shown in Tables 1 to 3 below were mixed together, and then filtered through a membrane filter with a pore size of 3 μm to obtain water-based ink compositions for evaluation tests.
[0120] Reference Example 1 Preparation of Water-Based White Ink Composition The components shown in Table 4 below were mixed and then filtered through a membrane filter with a pore size of 3 μm to obtain a water-based white ink composition for evaluation tests.
[0121] The numerical value in the column for each component in Tables 1 to 4 below indicates the amount (parts) of the component added, and a blank column means that the component was not used. The abbreviations in Tables 1 to 4 below have the following meanings. Kdp: Black dispersion obtained in Preparation Example 1 Cdp: Black dispersion obtained in Preparation Example 2 Mdp: Black dispersion obtained in Preparation Example 3 Ydp: Black dispersion obtained in Preparation Example 4 TF-5760 WHITE (D2B): White dispersion (manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd., solid content: 60%, titanium oxide dispersion) DEGHe: Diethylene glycol monohexyl ether (Clog P: 1.72, boiling point: 259.1°C) EGHe: Ethylene glycol monohexyl ether (Clog P: 1.90, boiling point: 208°C) DEGPh: Diethylene glycol monophenyl ether (Clog P: 1.25, boiling point: 283°C) PnB: Propylene glycol monobutyl ether (Clog P: 1.15, boiling point: 171°C) 1,2HD: 1,2-hexanediol (Clog P: 0.53, boiling point: 223°C) EHDG: diethylene glycol mono-2-ethylhexyl ether (Clog P: 2.65, boiling point: 272°C) PG: propylene glycol (Clog P: -1.06, boiling point: 188°C) TEG: triethylene glycol (Clog P: -1.48, boiling point: 276°C) GL: glycerin (Clog P: -1.54, boiling point: 290°C) Glyceryl-26: polyoxyethylene glycerin (average number of moles of ethylene oxide added: 26) AMP: 2-amino-2-methyl-1-propanol TEA: triethanolamine BYK-3420: BYK-3420 (manufactured by BYK-Chemie) SF440: Surfynol 440 (manufactured by Nissin Chemical Industry Co., Ltd.) SF465: Surfynol 465 (manufactured by Nissin Chemical Industry Co., Ltd.) Resin 1: Resin emulsion obtained in Preparation Example 5 Water: Ion-exchanged water
[0122]
[0123]
[0124]
[0125]
[0126] <Evaluation> [Dot diameter evaluation test] Gradation printing was performed in 1% increments using the aqueous ink compositions of each Example and Comparative Example to obtain printed images. Printing was performed using a printing tool equipped with a KJ4B inkjet head manufactured by Kyocera Corporation, under conditions of a frequency of 10 kHz, binary (medium droplets), and a print gap of 1 mm. The printing media used were "OK Topcoat+" manufactured by Oji Paper Co., Ltd. and "Maricoat F" manufactured by Hokuetsu Paper Mills Co., Ltd. The obtained printed image was dried for 3 seconds under an IR heater set at 100°C to obtain a test piece.
[0127] Dot diameter was measured for a 2% density portion of the obtained test piece using a print image evaluation device PIAS-II manufactured by QEA, and the obtained value was rounded off to the nearest whole number and evaluated according to the following four-level evaluation criteria A to D. The evaluation results are shown in Tables 5 to 7 below. (Evaluation criteria: OK top coat +) (Black) A: 67.5 μm or more B: 65.5 μm or more and less than 67.5 μm C: 63.5 μm or more and less than 65.5 μm D: less than 63.5 μm (Cyan) A: 75.0 μm or more B: 73.0 μm or more and less than 75.0 μm C: 71.0 μm or more and less than 73.0 μm D: less than 71.0 μm (Magenta) A: 70.0 μm or more B: 68.0 μm or more and less than 70.0 μm C: 66.0 μm or more and less than 68.0 μm D: less than 66.0 μm (Yellow) A: 67.5 μm or more B: 65.5 μm or more and less than 67.5 μm C: 63.5 μm or more and less than 65.5 μm D: Less than 63.5 μm (Evaluation criteria: Maricoat F) (Black) A: 70.0 μm or more B: 68.0 μm or more and less than 70.0 μm C: 66.0 μm or more and less than 68.0 μm D: Less than 66.0 μm (Cyan) A: 77.0 μm or more B: 75.0 μm or more and less than 77.0 μm C: 73.0 μm or more and less than 75.0 μm D: Less than 73.0 μm (Magenta) A: 70.0 μm or more B: 68.0 μm or more and less than 70.0 μm C: 66.0 μm or more and less than 68.0 μm D: Less than 66.0 μm (Yellow) A: 70.0 μm or more B: 68.0 μm or more and less than 70.0 μm C: 66.0 μm or more and less than 68.0 μm D: Less than 66.0 μm
[0128] [Color development evaluation test] Gradation printing was performed in 1% increments using the aqueous ink compositions of each Example and Comparative Example, to obtain printed images. Printing was performed using a printing tool equipped with a KJ4B inkjet head manufactured by Kyocera Corporation, under conditions of a frequency of 10 kHz, 12 Pl, and a print gap of 1 mm. The printing media used were "OK Topcoat+" manufactured by Oji Paper Co., Ltd., "Maricoat F" manufactured by Hokuetsu Paper Mills Co., Ltd., and liner paper (K Liner, basis weight: 170 g / m 2 , brown liner), and "white ink-coated liner paper" prepared by coating the above liner paper with the water-based white ink composition of Reference Example 1 was used. The "white ink-coated liner paper" was prepared by printing 100% solid images twice on the liner paper at 12 PI using a printing tool equipped with a KJ4B inkjet head manufactured by Kyocera Corporation, followed by drying. The resulting printed image was dried for 3 seconds under an IR heater set at 100°C to obtain a test piece.
[0129] The color development (print density) of the 100% density portion of the obtained test piece was measured using a colorimeter (SpectroEye, manufactured by X-Rite), and the obtained values were evaluated according to the following four-level evaluation criteria, A to D. The evaluation results are shown in Tables 5 to 7 below. (Evaluation criteria: OK Top Coat+) (Black) A: 2.10 or more B: 2.00 or more and less than 2.10 C: 1.90 or more and less than 2.00 D: less than 1.90 (Cyan) A: 2.00 or more B: 1.90 or more and less than 2.00 C: 1.80 or more and less than 1.90 D: less than 1.80 (Magenta) A: 1.70 or more B: 1.60 or more and less than 1.70 C: 1.50 or more and less than 1.60 D: less than 1.50 (Yellow) A: 1.00 or more B: 0.90 or more and less than 1.00 C: 0.80 or more and less than 0.90 D: less than 0.80 (Evaluation criteria: Maricoat F) (Black) A: 2.00 or more B: 1.90 or more and less than 2.00 C: 1.80 or more and less than 1.90 D: less than 1.80 (Cyan) A: 1.90 or more B: 1.80 or more and less than 1.90 C: 1.70 or more and less than 1.80 D: less than 1.70 (Magenta) A: 1.60 or more B: 1.50 or more and less than 1.60 C: 1.40 or more and less than 1.50 D: less than 1.40 (Yellow) A: 1.05 or more B: 0.95 or more and less than 1.05 C: 0.85 or more and less than 0.95 D: less than 0.85 (Evaluation criteria: liner paper and white ink coated liner paper) (Black) A: 1.08 or more B: 1.07 or more and less than 1.08 C: 1.06 or more and less than 1.07 D: Less than 1.06 (Cyan) A: 1.00 or more B: 0.99 or more and less than 1.00 C: 0.98 or more and less than 0.99 D: Less than 0.98 (Magenta) A: 1.00 or more B: 0.99 or more and less than 1.00 C: 0.98 or more and less than 0.99 D: Less than 0.98 (Yellow) A: 0.85 or more B: 0.75 or more and less than 0.85 C: 0.65 or more and less than 0.75 D: Less than 0.65
[0130] [Transfer Resistance Test] The aqueous ink composition of each Example and Comparative Example was coated onto "OK Top Coat+" manufactured by Oji Paper Co., Ltd., and left at room temperature for 20 seconds to dry the ink. For coating, an automatic coater (PI-1210 manufactured by Tester Sangyo Co., Ltd.) and a bar coater No. 8 were used. Immediately after the ink dried, a blank OK Top Coat+ was placed on top of it, a 1 kg disk weight was placed on top of it, and left for 3 seconds, after which the overlaid OK Top Coat+ was peeled off. The coated product after peeling was scanned with a scanner (imageRUNNER ADVANCE C5535F manufactured by Canon Inc.) and analyzed using image analysis software ImageJ. The intermediate gray value was calculated and evaluated based on the following evaluation criteria. A better evaluation indicated better drying and fixation properties, and indicated that the ink was suitable for lamination processes and high-speed printing. A or B was evaluated as good transfer resistance, and C or D was evaluated as poor transfer resistance. The evaluation results are shown in Tables 5 to 7 below. (Evaluation Criteria) (Black) A: Less than 70 B: 70 or more and less than 80 C: 80 or more and less than 90 D: 90 or more (Cyan) A: Less than 95 B: 95 or more and less than 105 C: 105 or more and less than 115 D: 115 or more (Yellow) A: Less than 180 B: 180 or more and less than 190 C: 190 or more and less than 200 D: 200 or more (Magenta) A: Less than 120 B: 120 or more and less than 130 C: 130 or more and less than 140 D: 140 or more
[0131]
[0132]
[0133]
[0134] As shown in Tables 5 to 7, the water-based ink compositions of Examples 1 to 25 produced large dot diameters when inkjet printed and exhibited good color development. In particular, the water-based ink compositions of Examples 1 to 25 also exhibited good color development when inkjet printed on an ink layer of a water-based white ink composition. Furthermore, the water-based ink compositions of Examples 1 to 25 were less likely to transfer when printed on a surface-coated substrate.
Claims
1. A water-based ink composition comprising a non-white colorant, a water-soluble organic solvent, a humectant, a surfactant, and water, wherein the humectant comprises a sugar alcohol, the water-soluble organic solvent comprises one or more specific solvents having a ClogP value of 0.5 or more and 2.0 or less, the content of the water-soluble organic solvent is more than 0% by mass and 5% by mass or less, and the content of the water-soluble organic solvent having a boiling point of 250°C or less at 1 atmosphere is 3% by mass or less.
2. The water-based ink composition according to claim 1, wherein the sugar alcohol content is from 4% by mass to 10% by mass.
3. The water-based ink composition of claim 1, wherein the sugar alcohol comprises sorbitol.
4. An ink set comprising the water-based ink composition according to any one of claims 1 to 3 and a water-based white ink composition containing a white colorant and water.
5. The ink set according to claim 4, wherein the white colorant comprises titanium oxide.
6. A method for producing an inkjet print, comprising ejecting droplets of the water-based ink composition according to any one of claims 1 to 3 from an inkjet head and depositing the droplets on a printing medium to obtain a print.
7. The method for producing an inkjet printed matter according to claim 6, wherein the printing medium is at least one selected from the group consisting of corrugated cardboard, liner paper, and coated board.
8. The method for producing an inkjet printed matter according to claim 6, wherein the print medium is coated paper.
9. A method for producing an inkjet print, comprising the steps of: a printing step in which droplets of the water-based ink composition according to any one of claims 1 to 3 are ejected from an inkjet head in a single pass and deposited on liner paper or coated board to obtain a print; and a lamination step in which the printed matter is laminated to a core to obtain a cardboard sheet.
10. A method for producing an inkjet printed matter as described in claim 9, wherein in the printing step, droplets of a water-based white ink composition containing a white colorant and water are deposited on the liner paper or the coated ball, and then droplets of a water-based ink composition are deposited on the liner paper or the coated ball to obtain the printed matter.
Citation Information
Patent Citations
Coated paper for printing
JP2003268694A
Liner board of corrugated fiberboard for inkjet printing and corrugated fiberboard using the same
JP2006150694A
Ink jet ink composition, ink jet recording method, and ink jet recording apparatus
JP2020105481A
Recording method
JP2021154610A
White ink composition for inkjet printing
JP3562754B2