Filler array film and method for manufacturing same, and connection structure and method for manufacturing same
The filler array film with a structured insulating resin layer and filler arrangement addresses the challenges of connecting μLEDs by eliminating the need for complex transfer molds and expensive laser techniques, ensuring reliable and efficient anisotropic conductive connections for μLED displays.
Patent Information
- Application Number
- PCT/JP2024/010941
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
Existing methods for connecting micro LEDs (μLEDs) to display wiring boards face challenges with fine pitch electrodes, requiring complex transfer molds and expensive laser lift-off techniques, which are time-consuming and prone to errors and edge distortion.
A filler array film with a filler-holding insulating resin layer featuring concave and convex portions allows for the arrangement of fillers only on convex portions, eliminating the need for laser lift-off and enabling simple transfer mold formation, facilitating anisotropic conductive connections without short circuits.
The filler array film provides reliable anisotropic conductive connections for μLEDs, reducing manufacturing complexity and costs, while maintaining high optical transparency and preventing short circuits, thus enabling efficient production of μLED displays.
Smart Images

Figure JP2024010941_03102024_PF_FP_ABST
Abstract
Description
Filler-arranged film and manufacturing method thereof, and connection structure and manufacturing method thereof
[0001] The present invention relates to a filler-arranged film and a method for producing the same, and a connection structure and a method for producing the same.
[0002] In recent years, displays in which self-luminous μLEDs (micro light emitting diodes) are mass-transferred onto display wiring substrates and arranged in a matrix have attracted attention as next-generation displays for relatively small smartphone displays, relatively large TV displays, and signage displays. μLEDs typically have a pair of electrodes arranged on one side, but they are microelectronic components with an extremely narrow fine-pitch spacing between the electrodes.
[0003] As methods for connecting such tiny μLEDs to a wiring board, methods such as reflow soldering and eutectic methods have difficulty handling the fine pitch at the electrode level of μLEDs, and it is also difficult to uniformly and reliably mass-transfer a huge number of μLEDs. Therefore, conductive connection methods using conductive films, which are a type of filler-arranged film that can handle both fine pitch and mass transfer, and anisotropic conductive connection methods using anisotropic conductive films are attracting considerable attention.
[0004] For example, as anisotropic conductive films applicable to μLEDs, there have been proposed a film in which a group of conductive particles consisting of a plurality of conductive particles is regularly arranged at a distance from each other over the entire surface of an insulating resin sheet (Patent Document 1), and a filler-arranged film that can function as an anisotropic conductive film that has been diced into microLED-sized pieces by a so-called laser lift-off method (Patent Document 2).
[0005] JP 2016-103476 A JP 2022-151822 A
[0006] In the case of the anisotropic conductive film of Patent Document 1, a transfer mold must be created in advance to transfer a conductive particle group consisting of multiple conductive particles to a wiring substrate corresponding to the μLED. However, if the regular array pattern of the μLEDs in the μLED display to which the anisotropic conductive film is applied changes, a new transfer mold must be created each time. Moreover, even in this case, there is a problem in that even if the regular array pattern of the multiple conductive particles in the conductive particle group does not change, it is still necessary to create the regular array pattern of the conductive particles that make up the conductive particle group in the transfer mold. Furthermore, in the case of the filler-arranged film that can function as the anisotropic conductive film of Patent Document 2, although a transfer mold is not required, an expensive laser lift-off device is required to perform the laser lift-off method. Furthermore, roll-to-roll processing is not possible, which may increase the cycle time. Furthermore, if the film is made of a curable resin, there are concerns about unintended hardening due to radiant heat from the laser, distortion of the edge shape of the individual pieces, or chipping of the edge of the individual pieces.
[0007] The present invention seeks to solve the problems of the prior art. It aims to provide a structure that can be formed using a simple transfer mold without the need for a singulation process, such as the laser lift-off method, when creating an image display device in which a large number of fine optical elements, such as a μLED display, are arranged on a display substrate using a filler array film that can function as an anisotropic conductive film. While the problems, configuration, and effects of the present invention will be described using μLEDs as an example, the present invention can also achieve similar effects even for optical elements that are considered to be larger than μLEDs (mini-LEDs). It can also be applied to microcomponents other than optical elements.
[0008] The inventors have discovered that the object of the present invention can be achieved by providing preferably a plurality of recesses and protrusions on one side of the insulating resin layer for retaining filler of a filler-arranged film having an insulating resin layer for retaining filler and a filler, and by arranging a filler group consisting of a plurality of fillers in the protrusions, and have thus completed the present invention.
[0009] That is, the present invention provides a filler array film having a filler-retaining insulating resin layer and a filler, wherein recesses and protrusions are formed on one side of the filler-retaining insulating resin layer, and at least one filler group consisting of a plurality of fillers is arranged in the protrusion. Each filler constituting the filler group is preferably arranged on the top surface of the protrusion or at least partially embedded in the filler-retaining insulating resin layer constituting the protrusion. In this filler array film, the protrusions are preferably regularly arranged, and it is preferable that multiple fillers are regularly arranged within each filler group. It is also preferable that no filler is arranged in the recesses. Such recesses may penetrate the filler-retaining insulating resin layer. Another insulating resin layer may be laminated on at least one side of the filler-retaining insulating resin layer, in which case the protrusions may be separated from each other by the penetrating recesses. Furthermore, another insulating resin layer may be laminated. A black matrix-forming insulating resin layer can be preferably used as the other insulating resin layer to be laminated in this manner.
[0010] The present invention also provides a method for producing the filler array film of the present invention described above, comprising the following steps A to C: (Step A) forming a filler-retaining insulating resin layer on a release film that has been subjected to a release treatment; (Step B) forming recesses and protrusions on one side of the filler-retaining insulating resin layer by bringing a stamping die having recesses corresponding to the protrusions of the filler array film into contact with the filler-retaining insulating resin layer and performing hot pressing; and (Step C) opposing the filler-arranged surface of a filler transfer sheet, having a plurality of fillers arranged on one side of a transfer substrate, to the top surfaces of the protrusions, and pressing from the transfer substrate side, thereby transferring the fillers to the top surfaces of the protrusions.
[0011] In the manufacturing method of this filler array film, it is preferable to further include the following step D following step C: (Step D) a step of embedding each filler transferred to the top surface of the convex portion into an insulating resin layer for retaining fillers so that at least a portion of the fillers are embedded.
[0012] Furthermore, the present invention provides a connection structure in which a second article is connected to a first article via the filler array film of the present invention. It is preferable that the second article and the convex portions of the filler array film correspond (preferably one-to-one). In this case, it is preferable that the first article is a transparent display substrate having a transparent electrode disposed on one side thereof, the second article is a μLED having an electrode formed on one side thereof, the filler disposed in the convex portions of the filler array film is conductive particles, and the filler array film itself functions as a conductive film or an anisotropic conductive film.
[0013] The present invention also provides a method for manufacturing a connection structure, characterized by sandwiching the filler array film of the present invention between a first article and a second article, preferably so that the convex portions of the filler array film correspond (preferably one-to-one), and then compressing, for example, by thermocompression bonding. In this case, it is preferable that the first article is a transparent display substrate with a transparent electrode disposed on one side, the second article is a μLED with an electrode formed on one side, the filler disposed on the convex portions of the filler array film is conductive particles, and the filler array film itself functions as a conductive film or an anisotropic conductive film. While the filler array film may be described using an anisotropic conductive film as an example, the same description can also be applied to a conductive film as an example. Furthermore, the second article may be a mini-LED or other small light-emitting element or small component (electronic component) instead of a μLED. An example of the size of the second article is one with a maximum side length of 200 μm or less. It may also be 10 to 30 μm square, making manual processing extremely difficult.
[0014] The filler array film of the present invention comprises a filler-retaining insulating resin layer and a filler, and preferably has multiple recesses and protrusions on one side of the filler-retaining insulating resin layer. At least one filler group consisting of multiple fillers is arranged in each protrusion. These protrusions can be created to essentially correspond one-to-one with the microelectronic components, such as μLEDs, to be connected with the filler array film. Furthermore, filler can be transferred from a filler transfer sheet in which the fillers are regularly arranged only to the top surfaces of the protrusions, while no filler is placed on the bottoms of the recesses. Therefore, when anisotropically connecting microelectronic components, such as fine-pitch μLEDs, to a wiring board or the like, the protrusions of the filler array film can essentially function as individual pieces of filler array film, enabling anisotropic conductive connection without concern for short circuits. Furthermore, a thin insulating resin layer can be left in the recesses, which has the advantage of making the protrusions less likely to fall off the filler array film during handling.
[0015] In addition, in the method for producing a filler array film of the present invention, a press mold having recesses corresponding to the protrusions of the filler array film is brought into contact with the filler-retaining insulating resin layer and hot-pressed to form multiple recesses and protrusions on one side of the filler-retaining insulating resin layer. Therefore, the planar shape and surface area of the top surface of the protrusions of the filler array film, as well as the cross-sectional shape and height of the protrusions, can be relatively easily formed using the press mold. Moreover, since this press mold does not require the creation of minute holes for regularly arranging the minute fillers, it is possible to produce the press mold at low cost. Furthermore, in the method for producing a filler array film of the present invention, the filler can be transferred only to the protrusions formed by the press mold using a conventional filler transfer sheet in which the filler is distributed over the entire surface. In other words, even if the arrangement of the filler groups in the filler array film is changed, a new press mold can be produced relatively easily and at low cost.
[0016] FIG. 1A is a schematic cross-sectional view of a filler array film of the present invention. FIG. 1B is a schematic cross-sectional view of a filler array film of the present invention. FIG. 1C is a schematic cross-sectional view of a filler array film of the present invention. FIG. 1D is a schematic cross-sectional view of a filler array film of the present invention. FIG. 2 is a schematic cross-sectional view of a filler array film of the present invention. FIG. 3 is a schematic cross-sectional view of a filler array film of the present invention. FIG. 4 is a schematic cross-sectional view of a filler array film of the present invention. FIG. 5 is a schematic cross-sectional view of a filler array film of the present invention. FIG. 6 is an explanatory diagram of a filler group on the top surface of a convex portion of a filler array film of the present invention. FIG. 7 is an explanatory diagram of a filler group on the top surface of a convex portion of a filler array film of the present invention. FIG. 8 is a schematic cross-sectional view of another embodiment of a filler array film of the present invention. FIG. 9A is a schematic cross-sectional view of another embodiment of a filler array film of the present invention. FIG. 9B is a schematic cross-sectional view of another embodiment of a filler array film of the present invention. FIG. 9C is a schematic cross-sectional view of another embodiment of a filler array film of the present invention. FIG. 10 is a schematic cross-sectional view of another embodiment of a filler array film of the present invention. FIG. 11 is a process diagram illustrating the method for manufacturing a filler array film of the present invention. FIG. 12 is a process diagram illustrating the method for manufacturing a filler array film of the present invention. FIG. 13 is a process diagram illustrating the method for manufacturing a filler array film of the present invention. FIG. 14 is a process diagram illustrating the method for manufacturing a filler array film of the present invention. FIG. 15 is a process diagram illustrating the method for manufacturing a filler array film of the present invention. FIG. 16 is a process diagram illustrating the method for manufacturing a filler array film of the present invention. FIG. 17A is a schematic cross-sectional view of a filler array film obtained by steps A to C of the method for manufacturing a filler array film of the present invention. FIG. 17B is a schematic cross-sectional view of a filler array film obtained by steps A to D of the method for manufacturing a filler array film of the present invention. FIG. 18 is an optical microscope photograph of the convex side surface of a filler array film of the present invention. FIG. 19 is a partially enlarged photograph of an anisotropic conductive film produced using a stamping die. FIG. 20 is a partially enlarged photograph of an anisotropic conductive film produced using a stamping die. FIG. 21 is a wiring pattern diagram of a glass substrate of a connection structure for insulating evaluation.
[0017] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings.
[0018] <Filler Array Film> As shown in Figure 1A, the filler array film 10 of the present invention has a filler-retaining insulating resin layer 1 and a filler 2. One side of the filler-retaining insulating resin layer 1 has recesses 3 and protrusions 4, preferably a plurality of each. The protrusions 4 are portions that retain the fillers 2, and at least one filler group 20 consisting of a plurality of fillers 2 is arranged in the protrusions 4. In Figure 1A, the fillers 2 that make up the filler group 20 are arranged on the top surface of the protrusions 4, but as shown in Figures 1B to 1D, each filler 2 that makes up the filler group 20 may be arranged so that at least a portion is embedded in the filler-retaining insulating resin layer 1 that makes up the protrusions 4. For example, in Figure 1B, approximately half of the particle diameter of the filler 2 is embedded in the filler-retaining insulating resin layer 1; in Figure 1C, the ends of the filler 2 are embedded so as to be flush with the filler-retaining insulating resin layer 1; and in Figure 1D, the filler 2 is completely embedded without being exposed in the filler-retaining insulating resin layer 1. In such a filler array film 10 of the present invention, when filler is arranged in the convex portions 4, the filler is not transferred to the inner bottom surfaces of the concave portions 3 (non-convex portions). This is because the filler contained in the openings of the transfer mold (Japanese Patent No. 6187665) used to arrange the filler in the convex portions 4, or the filler arranged on the filler arrangement surface of the filler transfer sheet 41 shown in Figure 16 (described later), does not reach (or has difficulty reaching) the bottom of the concave portions of the filler array film during filler transfer. Another factor is that the resin thickness at the bottom of the recesses in the filler array film is much thinner than the resin thickness at the protrusions, significantly reducing the adhesive strength of the recesses and making it difficult for the filler to be transferred. Therefore, each protrusion essentially functions as a piece of filler array film. Therefore, when the filler is conductive particles, the filler array film can essentially function as a piece of conductive film or an anisotropic conductive film.
[0019] The term "arrangement" in the term "filler array film" has two meanings. One meaning is that, as shown in FIG. 1A , the protrusions 4 rising from the recesses 3 themselves are randomly or regularly arranged (for example, a square lattice array, a hexagonal lattice array, etc., but not limited to a lattice array). The other meaning is that the filler 2 in the filler group 20 arranged in the protrusions 4 themselves are randomly or regularly arranged (for example, a square lattice array, a hexagonal lattice array, etc.). From the viewpoints of filler capture ability and manufacturing costs, it is preferable that the arrangement of the protrusions 4 and the arrangement of the filler 2 are each regularly arranged (particularly a hexagonal lattice array).
[0020] (Filler-Retaining Insulating Resin Layer 1) The filler-retaining insulating resin layer 1 constituting the filler-arranged film 10 of the present invention can have a configuration similar to that of the insulating resin layer that retains the filler in conventional anisotropic conductive films, conductive films, etc., and can be formed, for example, from a thermosetting resin composition. Such a thermosetting resin composition preferably contains a rubber component, a film-forming resin, a thermosetting resin, a thermosetting agent, and an inorganic filler. This inorganic filler is different from the filler disposed in the protrusions 4 and is uniformly dispersed in the filler-retaining insulating resin layer 1. If necessary, the filler-retaining insulating resin layer 1 can contain other known additives as long as they do not impair the effects of the invention. The thickness of the filler-retaining insulating resin layer 1 can be determined appropriately depending on the shape and surface area of the recesses 3 and protrusions 4, but is preferably at least equal to but not more than twice the average particle diameter of the filler 2. If the layer thickness is too thick, the bottom thickness of the recesses 3 will not be thin, and there is a concern that the filler may be arranged in the recesses 3 or that the light transmittance of the recesses 3 will be reduced. Furthermore, when connecting articles with the filler-arranged film, there is a concern that the separated protrusions 4 may come into contact with each other. Conversely, if the layer is too thin, there is a concern that the amount of resin in the protrusions 4 will be insufficient, making it impossible to form them into the intended shape. Note that an example of the filler-retaining insulating resin layer 1 can be one that functions as an adhesive film or connecting film with adhesive properties, such as a general anisotropic conductive film.
[0021] *Rubber component The rubber component contained in the thermosetting resin composition is a component for imparting cushioning properties (shock absorption) to the filler-retaining insulating resin layer. It is not particularly limited as long as it is an elastomer with good cushioning properties. Specific examples include acrylic rubber, silicone rubber, butadiene rubber, and polyurethane resin (polyurethane-based elastomer). Among these, one or more types selected from acrylic rubber and silicone rubber are preferred. The content of the rubber component is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and preferably 20 parts by mass or less, and more preferably 10 parts by mass or less, per 100 parts by mass of the total of the rubber component, film-forming resin, thermosetting resin, thermosetting agent, and inorganic filler.
[0022] *Film-forming resin: From the viewpoint of film-forming properties, examples of the film-forming resin include various resins such as phenoxy resin, polyester resin, polyurethane resin, polyester urethane resin, acrylic resin, polyimide resin, and butyral resin, each having a weight-average molecular weight of preferably about 10,000 to 80,000. These may be used alone or in combination of two or more. Among these, phenoxy resin is preferred from the viewpoint of film formation state, connection reliability, and the like. The content of the film-forming resin is preferably 20 parts by mass or more, more preferably 25 parts by mass or more, even more preferably 35 parts by mass or more, and preferably 50 parts by mass or less, more preferably 45 parts by mass or less, and even more preferably 40 parts by mass or less, per 100 parts by mass of the total of the rubber component, film-forming resin, thermosetting resin, thermosetting agent, and inorganic filler.
[0023] *Thermosetting resin Examples of thermosetting resins include epoxy compounds and (meth)acrylate compounds, with epoxy compounds being particularly preferred. These compounds may be monomers, oligomers, or polymers. The content of the thermosetting resin is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 35 parts by mass or less, per 100 parts by mass of the total of the rubber component, film-forming resin, thermosetting resin, thermosetting agent, and inorganic filler.
[0024] The epoxy compound that can be used as the thermosetting resin is not particularly limited as long as it is an epoxy compound having one or more epoxy groups in the molecule. For example, it may be a bisphenol A type epoxy resin, a bisphenol F type epoxy resin, or a urethane-modified epoxy resin. Among these, high-purity bisphenol A type epoxy resin is preferably used. A specific example of a high-purity bisphenol A type epoxy resin is the product name "YL980" manufactured by Mitsubishi Chemical Corporation. When an epoxy compound is used as the thermosetting resin, the content of the epoxy compound is preferably 30 parts by mass or more, more preferably 35 parts by mass or more, preferably 60 parts by mass or less, more preferably 55 parts by mass or less, and even more preferably 45 parts by mass or less, per 100 parts by mass of the total of the rubber component, film-forming resin, thermosetting resin, thermosetting agent, and inorganic filler.
[0025] *Thermosetting Agent The thermosetting agent is selected depending on the thermosetting resin. For example, when the thermosetting resin is an epoxy compound, a thermal anionic polymerization initiator or a thermal cationic polymerization initiator can be preferably selected, and a thermal cationic polymerization initiator that suppresses the curing reaction caused by laser light and enables rapid curing by heat can be more preferably selected. The content of the thermosetting agent can be determined depending on the type of thermosetting agent and the type of thermosetting resin. The content of the thermosetting agent is preferably 1 part by mass or more, more preferably 2 parts by mass or more, even more preferably 3 parts by mass or more, and preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 6 parts by mass or less, per 100 parts by mass of the total of the rubber component, film-forming resin, thermosetting resin, thermosetting agent, and inorganic filler.
[0026] Incidentally, thermal cationic polymerization initiators that are preferably applicable to epoxy compounds are those that generate an acid capable of cationic polymerization of a cationic polymerizable compound by heat, and known iodonium salts, sulfonium salts, phosphonium salts, ferrocenes, etc. can be used. Among these, aromatic sulfonium salts that exhibit good temperature latency can be preferably used. A specific example of an aromatic sulfonium salt-based polymerization initiator is "San-Aid SI-60L" manufactured by Sanshin Chemical Industry Co., Ltd. The content of such a thermal cationic polymerization initiator is preferably 1 part by mass or more, more preferably 2 parts by mass or more, even more preferably 3 parts by mass or more, and preferably 15 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 8 parts by mass or less, per 100 parts by mass of the total of the rubber component, film-forming resin, thermosetting resin, thermosetting agent, and inorganic filler.
[0027] *Inorganic Filler The inorganic filler in the thermosetting resin composition is used for the purpose of adjusting the durometer A hardness, storage modulus at a frequency of 200 Hz, and storage modulus after curing of the filler-retaining insulating resin layer 1, and can be silica filler, talc filler, titanium oxide filler, calcium carbonate filler, magnesium oxide filler, silane coupling agent filler, bulking agent filler, softener filler, colorant filler, flame retardant filler, thixotropic agent filler, etc. The inorganic filler may be used alone or in combination of two or more types.
[0028] The content of the inorganic filler is preferably 1 part by mass or more, more preferably 5 parts by mass or more, even more preferably 8 parts by mass or more, and preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 12 parts by mass or less, per 100 parts by mass of the total of the rubber component, film-forming resin, thermosetting resin, thermosetting agent, and inorganic filler. In particular, when the content of the rubber component is 2 parts by mass or more and 10 parts by mass or less, per 100 parts by mass of the total of the rubber component, film-forming resin, thermosetting resin, thermosetting agent, and inorganic filler, by setting the content of the inorganic filler to 8 parts by mass or more and 12 parts by mass or less, the desired durometer A hardness, storage modulus at a frequency of 200 Hz, and storage modulus after curing can be easily achieved.
[0029] (Protrusions 4) The protrusions 4 hold the filler 2, preferably on their top surfaces or on the filler-holding insulating resin layer 1 that constitutes the protrusions 4. When connecting a second item such as a μLED to a first item such as a wiring board, the protrusions 4 are preferably formed at positions corresponding to the second item. In this case, the second item and the protrusions 4 preferably correspond to each other on a one-to-one basis, but one protrusion 4 may correspond to two or more second items.
[0030] The planar shape and size (area) of the protrusion 4 preferably approximately match those of the second item to be connected or its electrode. For example, if the second item is a μLED, the planar shape and size of the protrusion 4 preferably approximately match those of the μLED's outer shape or the outer shape of one of its electrodes. For example, if the second item is a μLED, the planar shape and size of the protrusion 4 may be approximately the same as those of the μLED's outer shape or the outer shape of one of its electrodes. For example, the protrusion 4 may have a side of 5 μm or more and 100 μm or less, and is preferably a rectangle with a side of 10 μm or more and 30 μm or less. In addition, while the side of the protrusion 4 rises vertically from the recess 3 in FIGS. 1A to 1D, it may also have a tapered shape as shown in FIG. 2 or a stepped shape as shown in FIG. 3. While the planar shape and size (area) of the protrusion 4 have been described using a μLED as an example of the second item to be connected, relatively large items such as mini-LEDs can also be connected. The size of the protrusion 4 can be adjusted to match the size of the item to be connected. Even a component with an outer shape of 100 μm or more on a side can be considered a connection item as long as it does not impair the effects of the invention.
[0031] Height t of protrusion 4 0(See FIG. 1A ) corresponds to the thickness of the filler-retaining insulating resin layer 1. Considering the difficulty of filler arrangement and the strength when connecting a second article, the thickness is typically preferably 1 μm or more, more preferably 2 μm or more, preferably 20 μm or less, and more preferably 10 μm or less, and is preferably 1 to 2 times the average particle diameter of the filler 2. By making the height of the convex portion 4 greater than the bump height of the component to be connected and smaller than the sum of the thickness of the component to be connected and the bump height, a fillet can be formed around the component to be connected without the component being completely buried in the filler-retaining insulating resin layer 1. It is preferable that the planar shape, size (area), height, and relationship between the top surface of the convex portion 4 and the bottom surface of the concave portion 3 are all uniform, but this is not limited to this.
[0032] Number density of the protrusions 4 [pieces / mm 2 The optimum number density can be selected depending on the purpose of use of the filler array film, the object to be connected, etc. Generally, it is 50 [pieces / mm 2 ] or more 10,000 [pcs / mm 2 ] or less, but when the filler array film is used as an anisotropic conductive film or a conductive film and applied to the implementation of μLEDs, it is preferably 100 [pieces / mm 2 ] or more, more preferably 300 [pieces / mm 2 ] or more, preferably 3000 [pieces / mm 2 ] or less, more preferably 1500 [pieces / mm 2 The minimum distance between the protrusions 4 is preferably 5 μm or more in order to avoid contact between the protrusions 4 that should be spaced apart during the filler transfer step and component mounting.
[0033] The number of fillers provided in one protrusion 4 is not particularly limited, but the lower limit is preferably 2 or more and the upper limit is preferably 1500 or less. Assuming that the fillers are captured by a maximum of two electrodes provided on a component with a very small outer shape, it is preferable to set the number in this range.
[0034] (Recess 3) The recess 3 is formed reflectively when the protrusion 4 is formed, and has the function of separating the protrusion 4 from the adjacent protrusion 4. The depth t of the recess 31 and width w 1 There are no particular limitations on the size of the protrusion 4, and it can be determined appropriately taking into consideration the shape and size of the second article to be connected with the filler-arranged film. In Figures 1A to 1D, the inner walls of the recess 3 are vertical and the bottom is flat, but this is not limited thereto. As shown in Figure 4, the protrusion 4 may have a tapered shape that widens upward, or as shown in Figure 5, it may have a stepped shape. In the cases of Figures 4 and 5, the side surface of the protrusion 4 may be as shown in Figure 2 or 3.
[0035] Furthermore, if the thickness of the bottom of the recess 3 is reduced, the light transmittance of that part is improved, making it easier to optically distinguish it from the protrusion 4, and making it easier to handle the protrusion 4 as essentially individual pieces of the filler array film 10. Note that at least a part of the bottom of the recess 3 may be perforated, as long as the protrusion 4 is not completely separated from the filler array film 10. This is because the protrusion 4 that has been completely perforated through the recess 3 and separated into individual pieces cannot be handled as part of the filler array film 10.
[0036] (Filler 2) The filler 2 disposed in the convex portions 4 can be selected from various fillers used in known filler-arranged films, depending on the intended use of the filler-arranged film (e.g., conductive film, anisotropic conductive film, adhesive film, optical film, ferromagnetic film, etc.). For example, known inorganic fillers (e.g., metal particles, metal oxide particles, metal nitride particles), organic fillers (e.g., resin particles, rubber particles), and fillers containing a mixture of organic and inorganic materials (e.g., particles having a resin core and a metal-plated surface (metal-coated resin particles), conductive particles with insulating fine particles attached to the surface, conductive particles with an insulating treatment applied to the surface, etc.) can be selected depending on the hardness, optical performance, and other properties required for the intended use. For example, in optical films and matte films, silica fillers, titanium oxide fillers, styrene fillers, acrylic fillers, melamine fillers, and various titanate fillers can be used. Capacitor films can use fillers such as titanium oxide, magnesium titanate, zinc titanate, bismuth titanate, lanthanum oxide, calcium titanate, strontium titanate, barium titanate, barium zirconate titanate, lead zirconate titanate, and mixtures thereof. Adhesive films can contain polymeric rubber particles, silicone rubber particles, and the like. Conductive films or anisotropic conductive films contain conductive particles. Examples of conductive particles include metal particles such as nickel, cobalt, silver, copper, gold, and palladium, alloy particles such as solder, metal-coated resin particles, and metal-coated resin particles with insulating fine particles attached to their surfaces. Two or more types can also be used in combination. Among these, metal-coated resin particles are preferred because they repel resin particles after connection, making it easier to maintain contact with the terminal and stabilizing electrical conductivity. Furthermore, the surfaces of the conductive particles may be subjected to an insulating treatment using known techniques that does not impair electrical conductivity. The fillers listed for each application are not limited to those applications, and may contain fillers for other applications as needed. In addition, in the filler-arranged film for each application, two or more fillers may be used in combination as needed.
[0037] The shape of the filler 2 is appropriately selected from spherical, elliptical, cylindrical, needle-like, a combination thereof, and the like, depending on the application of the filler-arranged film. A spherical shape is preferable because it makes it easier to check the filler arrangement and maintain a uniform state. In particular, in an anisotropic conductive film, it is preferable that the conductive particles are approximately spherical. By using approximately spherical conductive particles, when manufacturing an anisotropic conductive film in which conductive particles are arranged using a transfer mold, as described in JP 2014-60150 A, for example, the conductive particles roll smoothly on the transfer mold, allowing the conductive particles to be filled into the predetermined positions on the transfer mold with high precision. Therefore, the conductive particles can be accurately arranged.
[0038] Here, "substantially spherical" means that the sphericity calculated by the following formula is 70 to 100.
[0039] Sphericity = {1-(S 0 -Si) / S 0} x 100
[0040] In the above formula, So is the area of the circumscribing circle of the filler in the planar image of the filler, and Si is the area of the inscribing circle of the filler in the planar image of the filler.
[0041] In this calculation method, planar images of the filler are taken in the surface view and cross section of the filler array film, and the areas of the circumscribed circles and the inscribed circles of any 100 or more fillers (preferably 200 or more) are measured in each planar image. The average values of the circumscribed circle areas and the average values of the inscribed circle areas are calculated and used as the above-mentioned So and Si. Furthermore, it is preferable that the sphericity is within the above range in both the surface view and the cross section. The difference in sphericity between the surface view and the cross section is preferably within 20, more preferably within 10. Since inspection during the production of filler array films is primarily performed in the surface view, and detailed pass / fail judgment after thermocompression bonding to an article is performed in both the surface view and the cross section, a small difference in sphericity is preferable. Note that this sphericity can also be determined for the filler alone using a wet flow particle size and shape analyzer FPIA-3000 (manufactured by Malvern Panalytical).
[0042] The average particle size of the filler is determined appropriately depending on the application of the filler-arranged film. For example, in an anisotropic conductive film, the average particle size is preferably 1 μm or more, more preferably 2.5 μm or more, and preferably 30 μm or less, more preferably 9 μm or less, to accommodate variations in wiring height, suppress increases in conduction resistance, and prevent short circuits. Depending on the object to be connected, a particle size larger than 9 μm may be suitable.
[0043] The average particle diameter of the filler before being placed on the convex portions 4 of the filler array film 10 can be measured using a general particle size distribution measuring device, and the average particle diameter can also be determined using a particle size distribution measuring device. An example of a particle size distribution measuring device is the FPIA-3000 (manufactured by Malvern Panalytical). Meanwhile, the average particle diameter of the filler in the filler array film can be determined by observation using an electron microscope such as an SEM. In this case, it is desirable to measure the average particle diameter of the filler by 200 or more samples. Furthermore, if the shape of the filler is not spherical, the maximum length or the diameter of a shape simulating a sphere can be used as the average particle diameter of the filler.
[0044] In the present invention, the variation in the average particle size of the filler in the filler-arranged film is set to a CV value (standard deviation / average) of 20% or less. By setting the CV value to 20% or less, the filler-arranged film is more likely to be pressed evenly when being pressed onto an article. This prevents localized concentration of pressure, particularly when the filler is arranged, contributing to connection stability. Furthermore, accurate evaluation of the connection status by indentation after connection can be performed. Specifically, when the filler-arranged film is configured as an anisotropic conductive film, accurate confirmation of the connection status by indentation can be performed after anisotropic conductive connection between the anisotropic conductive film and an electronic component, regardless of whether the terminal size is large (e.g., FOG) or small (e.g., COG). This facilitates inspection after anisotropic conductive connection, which is expected to improve productivity in the connection process.
[0045] Here, the variation in average particle size can be calculated using an image particle size analyzer or the like. The average particle size of fillers not contained in the filler array film as raw material particles of the filler array film can also be determined using the above-mentioned wet flow particle size and shape analyzer FPIA-3000 (manufactured by Malvern Panalytical). In this case, measuring 1,000 or more fillers, preferably 3,000 or more, and more preferably 5,000 or more fillers, allows for accurate understanding of the variation in particle size of the filler alone. When fillers are arranged in the filler array film, the sphericity can be determined from planar or cross-sectional images, as with the above-mentioned sphericity.
[0046] (Filler Groups 20) The filler groups 20 are composed of a plurality of fillers arranged in the protruding portions 4 to enhance filler capture when connecting a first article to a second article via the filler array film 10. In the present invention, as described above, at least one filler group 20 consisting of a plurality of fillers 2 is arranged in the protruding portion 4. Therefore, a plurality of filler groups 20 may be arranged in a single protruding portion 4. In this case, as shown in FIG. 6 (a plan view of a single protruding portion), adjacent filler groups (20a and 20b) in a single protruding portion 4 are preferably completely separated from each other. However, as shown in FIG. 7, some fillers 2a may be common to both filler groups. In particular, when the filler groups are completely separated as shown in FIG. 6, for example, when connecting a μLED with the filler array film, the separated filler groups 20a and 20b can be associated with the anode and cathode electrodes of the μLED to prevent short circuits from occurring between them. As already mentioned, the fillers 2 in the filler group 20 may be arranged randomly, but a regular arrangement (for example, a square lattice arrangement, a hexagonal lattice arrangement, etc., but not limited to a lattice arrangement) is preferable from the viewpoint of filler capture and manufacturing costs. The filler group provided on one protrusion 4 also includes an embodiment in which multiple filler groups are present at a distance from each other. This is because, when the filler group 20 is arranged on the protrusion 4, it may be designed in advance to form multiple filler groups in accordance with the object to be connected (for example, arranged only on the electrode). In the present invention, it is preferable that the outer periphery or outer edge of the filler group and at least the outer shape of the top surface of the protrusion 4 are the same.
[0047] In the present invention, the convex portions are spaced apart from one another, and multiple fillers are disposed on each convex portion. While disposing one filler on each convex portion is effective for fixing each filler individually, from a practical standpoint, multiple such convex portions must be densely packed, necessitating increased thrust to press the filler into the resin. This tendency is exacerbated when the resin holding the filler has a high viscosity. Therefore, a low-viscosity resin design is required, but low viscosity makes it difficult to release the filler from the transfer mold in a balanced manner, making resin design difficult. On the other hand, in the present invention, in which multiple fillers are disposed on one convex portion, the amount of resin relative to the amount of filler is relatively small compared to when a single filler is disposed on one convex portion, so excessive thrust is not particularly required during pressing. In other words, there is the advantage that conditions such as resin flow and resin filling can be adjusted depending on the design conditions of the convex portions, and the increased flexibility in resin design can be said to be a major feature of the present invention. For example, by designing one or two protrusions to span two electrodes, the size of the protrusions and the area of the filler provided in the protrusions can be adjusted to suit design conditions such as the area of the electrodes and the distance between the electrodes, stabilizing the connection conditions and significantly contributing to productivity. For example, when the overall dimensions of the μLED element are 30 × 60 μm and the dimensions of one electrode are 20 × 20 μm (area: 400 μm), 2 ) When two electrodes are connected using two protrusions, the specifications of the protrusions are not particularly limited as long as the filler is captured by the electrodes, but the dimensions of the protrusions are preferably 20 x 20 μm or more, and it is preferable that there are three or more fillers on one protrusion. When two electrodes are connected using one protrusion, it is preferable that the dimensions of the protrusions are 30 x 60 μm or more, and it is preferable that there are ten or more fillers. When connecting tiny components, this reduces constraints on the pressing device, such as thrust force, and can be said to be a significant effect of the present invention.
[0048] There is no particular limitation on the number density of the fillers in the filler group 20, and it is determined appropriately depending on the purpose of use of the filler array film, the external size of the connection target, the electrode layout, and the degree of fine pitch. 2
[0046] (which may be considered as the area obtained by connecting only the convex portions), the lower limit is preferably 100 or more, more preferably 1,000 or more, and even more preferably 10,000 or more, and the upper limit is preferably 300,000 or less, more preferably 200,000 or less, and even more preferably 100,000 or less.
[0049] <Modifications of Filler Array Film> The filler array film of the present invention can have another insulating resin layer laminated on at least one side of the filler-retaining insulating resin layer. For example, as shown in FIG. 8, another insulating resin layer 5 may be provided on the convex portion 4 side of the filler-retaining insulating resin layer 1, or as shown in FIG. 9A, another insulating resin layer 6 may be provided on the opposite side of the convex portion 4. In this case, as shown in FIG. 9B, the concave portion 3 may penetrate all the way through the insulating resin layer 6, or as shown in FIG. 9C, the penetrating concave portion 3 may separate and separate the convex portion 4 from the other convex portions. Note that in the case of FIG. 9B, even if the insulating resin layer 6 is not provided, there are still non-penetrating concave portions 3, so the penetrating concave portions 3 can remain open. Alternatively, as shown in FIG. 10, insulating resin layers 5 and 6 may be provided on both sides. The configuration of the other insulating resin layers 5 and 6 can be considered to be substantially the same as that described for the filler-retaining insulating resin layer 1.
[0050] Such another insulating resin layer 5 and insulating resin layer 6 can be formed from the same composition as the filler-holding insulating resin layer 1. The composition may be changed or adjusted depending on the purpose. The total resin layer thickness of the filler-arranged film including these layers is preferably 1 μm or more, more preferably 2 μm or more, even more preferably 3 μm or more, and preferably 30 μm or less, more preferably 15 μm or less, even more preferably 8 μm or less.
[0051] 11 , when the filler array film 10 shown in FIG. 8 is sandwiched between the wiring board 100 (first article) and the μLED 200 (second article) and thermocompression-bonded using a heat tool H, as shown in FIG. 12 , a fillet F is formed on the side surface of the μLED 200 from the insulating resin layer 5 (black matrix-forming insulating resin layer), and this fillet F can function as a black matrix.
[0052] Known black pigments such as carbon black and titanium black can be used as the black pigment. Titanium black, which has an extremely low content of impurity ions and is itself insulating, is particularly preferred. When titanium black is used as the black pigment, the titanium black content in the black resin composition for black matrices is preferably 5% by mass or more, more preferably 10% by mass or more, and preferably 40% by mass or less, and more preferably 30% by mass or less. The average particle size of these black pigments is 10 to 100 nm. It is desirable that the average particle size of this black pigment be smaller than the average particle size of the filler.
[0053] <Method for Producing Filler Arranged Film> The filler arranged film of the present invention can be produced by a production method including the following steps A to C. This production method preferably includes step D following step C.
[0054] (Step A) Step A is a step of forming a filler-retaining insulating resin layer 1 on a release film (PET film) 30 that has been subjected to a release treatment, as shown in Fig. 13. The filler-retaining insulating resin layer can be formed by a conventional method, for example, by applying a filler-retaining insulating resin composition to a release film to form a film.
[0055] (Step B) In step B, as shown in FIG. 14, a press die 8 having recesses 7 corresponding to the protrusions of the filler-arranged film is brought into contact with the filler-retaining insulating resin layer 1 obtained in step A and heat-pressed to form recesses 3 and protrusions 4 on one side of the filler-retaining insulating resin layer 1 (see FIG. 15). A release film may be interposed during the contact. The press die 8 is preferably a single metal or resin plate having recesses 7, but a roll having recesses 7 may also be used. A film having recesses 7 may also be used. Typical heat tools, vacuum laminators, etc. may be used for the heat press. The shape, depth, pitch, etc. of the recesses 7 may be determined appropriately depending on the shape, height, and pitch of the protrusions of the filler-arranged film (in other words, the shape, thickness, pitch, surface area, etc. of the second article to be connected). For example, when a μLED is selected as the second article, if the depth of the recess 7 is too shallow, it becomes difficult to arrange the filler only on the top surface of the protrusion 4 of the filler-holding insulating resin layer 1, and if it is too deep, there is a concern that the μLED will be buried in the resin, so the depth is preferably 1 μm or more, more preferably 2 μm or more, and preferably 20 μm or less, more preferably 10 μm or less.
[0056] (Step C) In step C, as shown in FIG. 16, the filler-arranged surface of a filler transfer sheet 41, on one side of which a plurality of fillers 2 are arranged, is placed against the top surfaces of the convex portions 4 of the insulating resin layer 1 for filler retention, and pressure is applied from the transfer substrate 40 side, thereby transferring the plurality of fillers 2 to the top surfaces of the convex portions 4. After transfer, the filler transfer sheet 41 is peeled off and removed, yielding a filler array film 10 laminated to a release film 30, as shown in FIG. 17A. FIG. 18 shows an example of an optical microscope photograph of the filler array film 10 taken from the convex portion side. It can be seen that the filler 2 is arranged in a hexagonal lattice pattern on the surface of the convex portions 4, and that no filler is present in the concave portions 3. Note that in FIG. 16, the filler 2 is held on the surface of the adhesive transfer substrate 40 of the filler transfer sheet 41; however, a transfer mold having a concave portion for accommodating the filler may also be used as the transfer substrate 40.
[0057] (Step D) In the manufacturing method of the filler array film of the present invention, following step C, it is preferable to embed the filler 2 transferred to the top surface of the convex portion 4 in the filler-retaining insulating resin layer 1 by a known hot pressing method such as heat pressing via another release film (PET film). This results in a filler array film 10 as shown in Figure 17B. A detailed description of the lamination of another insulating resin layer will be omitted, but a laminated layer may be prepared in advance, or may be laminated after step D.
[0058] As described above, one feature of the filler array film manufacturing method is the use of a stamping die in step B. By using such a stamping die, a filler array film can be obtained in which fillers are arranged only in the convex portions formed at the intended positions of the filler array film, thereby functioning essentially as individual pieces. Furthermore, at least one filler group can be arranged in the convex portions of the filler array film, and the convex portions and concave portions can be arranged in the intended positions relative to the entire film. Furthermore, the concave portions have a thinner film thickness, resulting in excellent translucency and visibility. Furthermore, the presence of concave portions where no filler is present significantly reduces the risk of short circuits when the filler array film is used as an anisotropic conductive film. Furthermore, the filler array film can be constructed from a single resin film, and additional resin layers can be laminated thereon, thereby increasing design flexibility.
[0059] The filler transfer sheet 41 has filler 2 arranged on one side of the transfer substrate 40, but since the filler is not transferred to the recesses 3 of the filler-retaining insulating resin layer 1, the filler can be arranged randomly or regularly, preferably in a hexagonal lattice pattern, all over the surface of the filler transfer sheet 41, making it easy to produce the filler transfer sheet 41. The number density of the fillers in the filler transfer sheet 41 is the same as the number density of the fillers in the filler group of the filler array film.
[0060] <Connection Structure and Manufacturing Method> The filler array film of the present invention is preferably used as a filler array film in a connection structure in which a relatively large first article, such as a wiring board, is connected to multiple second articles via the filler array film. It is also preferably used as a filler array film in a manufacturing method for a connection structure, characterized in that the filler array film is sandwiched between the first and second articles, preferably so that the convex portions of the filler array film correspond to the convex portions of the second article, and then pressure-bonded (e.g., thermocompression bonding). In these cases, the convex portions of the filler array film may correspond to the convex portions of the second article in a multiple-to-one or one-to-multiple relationship, but a one-to-one relationship is preferred from the standpoints of ease of design, positional accuracy, etc. Furthermore, it is preferable that the first and second articles have electrodes that allow electrical conduction when facing each other. The filler array film can also be sandwiched between the first and second articles that have opposing electrodes, for use in conductive or anisotropic conductive connections. In particular, the connection structure of the present invention is preferably applicable to the manufacture of a connection structure in which the first article is a transparent display substrate with a transparent electrode disposed on one side, the second article is a μLED with an electrode formed on one side, the filler disposed in the convex portions of the filler array film is conductive particles, and the filler array film itself functions as a conductive film or an anisotropic conductive film. Therefore, not only such a connection structure itself but also its manufacturing method itself constitutes another modified embodiment of the present invention. Note that an anisotropic conductive film may also be used instead of the conductive film.
[0061] (μLED Display as Connection Structure) When manufacturing a μLED display using the filler array film of the present invention, in other words, when connecting the electrodes of μLEDs to the electrodes of a substrate in a state where multiple μLEDs are regularly arranged on a wafer, the filler array film is first aligned and attached to the electrodes of the substrate, and the filler array film is aligned and attached to the μLEDs arranged on the wafer, and then heated and pressurized to connect the electrodes of the μLEDs to the electrodes of the substrate. In this case, connection may be made by heating and pressurizing in a two-stage manner (see JP 2019-216097 A). Furthermore, when the conductive particles are solder particles or the like, connection may be made by reflow. While the connection structure has been described using a μLED display as an example, the connection structure of the present invention can also be applied to displays using larger light-emitting elements.
[0062] Although the filler array film of the present invention is substantially in the form of individual pieces, it can also be used as a filler array film in which the convex portions are completely separated from the entire film. In this case, the temporary attachment of the individualized filler array film can be performed using known methods such as a method using a stamp material or a laser (laser lift-off method) or a method based on such a method (for example, methods described in JP-A-9-124020, JP-A-2011-76808, JP-A-6636017, JP-A-6187665, etc.), and is not particularly limited as long as the method can exhibit the effects of the invention. Similarly, when creating a filler transfer sheet or mounting a μLED on a substrate, known methods such as a method using a stamp material or a laser (laser lift-off method) or a method based on such a method can be used.
[0063] The present invention will be described in more detail below with reference to examples and comparative examples, in which an anisotropic conductive film, which is a specific embodiment of a filler-arranged film, was prepared.
[0064] Reference Example 1 <Formation of an insulating resin layer for retaining conductive particles in an anisotropic conductive film> The compositions (unit: parts by mass) with the formulation shown in Table 1 were uniformly mixed, and the resulting mixture was applied to a 50 μm thick polyethylene terephthalate film that had been subjected to a release treatment to achieve the layer thickness shown in Table 1, and dried under conditions of 60°C and 3 minutes to obtain an adhesive film as an insulating resin layer for retaining conductive particles.
[0065]
[0066] Reference Example 2 <Molds used in Examples and Comparative Examples> When assuming that μLEDs would be mounted on a substrate using an anisotropic conductive film, the following stainless steel molds 1 and 2 were prepared as molds for forming convex portions in the insulating resin layer for retaining conductive particles of the anisotropic conductive film. Mold 1 is used when one concave portion corresponds to one μLED, and mold 2 is used when two concave portions correspond to one μLED.
[0067] *Mold 1: Recess size: 40 μm length x 60 μm width x 4 μm depth, recess pitch: 30 μm length and width. Figure 19 shows a partially enlarged photograph of an anisotropic conductive film created using mold 1. This photograph shows that conductive particles 2 are arranged only on the top surfaces of the protrusions 4. The dotted lines represent the outer shape of the μLEDs to be mounted, and indicate a one-to-one correspondence between the protrusions 4 and the μLEDs.
[0068] *Mold 2: Recess size: 40 μm length x 20 μm width x 4 μm depth, space between paired recesses: 20 μm, recess pitch: 30 μm length and width. Figure 20 shows a partially enlarged photograph of an anisotropic conductive film created using mold 2. This photograph shows that conductive particles 2 are arranged only on the top surfaces of the protrusions 4. The dotted lines represent the outer shape of the μLEDs to be mounted, indicating a two-to-one correspondence between the protrusions 4 and the μLEDs.
[0069] Reference Example 3 <Preparation of conductive particle transfer sheet> Conductive particles (Micropearl AU series, Sekisui Chemical Co., Ltd.) having the average particle diameter shown in Table 2 were arranged over the entire surface of a film to achieve the number density shown in Table 2, and a conductive particle transfer sheet was prepared in accordance with the conductive particle regular array process described in paragraphs 0111-0112 and FIG. 1A of Japanese Patent No. 6187665.
[0070] Examples 1-7, Comparative Examples 1-4 <Formation of Anisotropic Conductive Films> The anisotropic conductive films used in the examples and comparative examples were prepared according to Table 2. That is, in the examples, stamping die 1 or stamping die 2 was placed on the insulating resin layer for retaining conductive particles prepared in Reference Example 1, and stamping was performed using a vacuum laminator, thereby forming convex portions and concave portions in the insulating resin layer for retaining conductive particles corresponding to the concave portions and non-convex portions of the stamping die. Next, the conductive particle-arranged surface of the conductive particle transfer sheet of Reference Example 3 was superimposed on the convex portion-forming surface of the insulating resin layer for retaining conductive particles, and heating and pressing were performed with a heat tool to transfer the conductive particles only to the convex portions, thereby obtaining an anisotropic conductive film.
[0071] The conductive particle surface density in Example 1-7 is the surface density on the convex portions of the film, and the conductive particle surface density in Comparative Example 1-4 is the surface density over the entire surface of the film.
[0072] <Preparation of connection structure for evaluating conduction resistance and insulation properties> The Cr / Au layer of the glass substrate was patterned to match the convex pattern of the anisotropic conductive film of the example, as shown in Fig. 21. The anisotropic conductive films of the example and comparative example were aligned and attached to the obtained Cr / Au pattern of the glass substrate, and a 1.5 cm square IC chip simulating a μLED was placed on top and thermocompression bonded under conditions of 150°C, 10 Pa, and 30 seconds, thereby obtaining a connection structure for evaluating conduction resistance and insulation properties.
[0073] <Preparation of connection structure for visible light transmittance evaluation> 30 μm × 50 μm IC chips were prepared as μLEDs for visible light transmittance evaluation. These IC chips were arranged in a 1.5 cm square area and similarly thermocompression bonded to obtain a connection structure for visible light transmittance evaluation.
[0074] <Evaluation of Conduction Resistance> The conduction resistance of the connection structure for evaluating conduction resistance and insulation was measured by a conventional method and evaluated according to the following criteria. The evaluation results are shown in Table 2. In practice, a rating of A or B is desirable.
[0075] (Conductivity resistance evaluation criteria) Rank: Criteria A: 30Ω or less B: Over 30Ω and up to 100Ω C: Over 100Ω and up to 300Ω D: Over 300Ω
[0076] <Insulation evaluation> Regarding the insulation of the connection structure for conducting resistance and insulation evaluation, 100 points between electrodes spaced 5 μm apart were selected, and the resistance value at each point was measured by a conventional method. The number of points where short circuits occurred was counted and evaluated according to the following criteria. The evaluation results are shown in Table 2. In practice, it is desirable to give a rating of A, B, or C. In addition, if the resistance is 10 7 A value of Ω or less was judged as a short circuit.
[0077] (Insulation evaluation criteria) Rank: Criteria A: 0 short circuits (no short circuits) B: 1 short circuit C: 2 short circuits D: 3 or more short circuits
[0078] <Light Transmittance Evaluation> The average light transmittance of the connection structure for light transmittance evaluation for visible light of 400 to 700 nm was measured using a commercially available light transmittance measuring device and evaluated according to the following criteria. The evaluation results are shown in Table 2. In practice, a rating of A, B, or C is desired.
[0079] (Light transmittance evaluation criteria) Rank: Criteria A: Visible light transmittance is 50% or more B: Visible light transmittance is 35% or more and less than 50% C: Visible light transmittance is 20% or more and less than 35% D: Visible light transmittance is less than 20%
[0080]
[0081] From the results in Table 2, the anisotropic conductive films of Examples 1-7, in which conductive particles were arranged only on the convex portions created by a stamping mold in the insulating resin layer for retaining conductive particles of the anisotropic conductive film, were able to make the convex portions essentially function as individual pieces of anisotropic conductive film, and showed results that were practically acceptable in terms of conduction resistance, insulation, and visible light transmittance.
[0082] In the case of the anisotropic conductive films of Comparative Examples 1 to 4, conductive particles were disposed over the entire surface of the film, which caused problems with visible light transmittance.
[0083] The filler array film of the present invention allows for anisotropic conductive connection of fine-pitch μLEDs and other microelectronic components to a wiring board or the like, without the risk of short circuits. The convex portions of the filler array film essentially function as individual pieces of the filler array film, enabling anisotropic conductive connection. Furthermore, the filler array film of the present invention has a structure that can be formed using a simple transfer mold. Therefore, the filler array film of the present invention incorporates a structure comparable to that obtained by laser lift-off, making it useful for the manufacture of μLED displays.
[0084] Although the filler array film of the present invention has been described using an anisotropic conductive film and an anisotropic conductive connection method using the same as an example, the contents of the description can also be applied to a case where a conductive film and a conductive connection method using the same are used as examples, as long as the effects of the present invention are not impaired.
[0085] REFERENCE SIGNS LIST 1 Filler-holding insulating resin layer 2, 2a Filler, conductive particles 3 Concave portion 4 Convex portion 5, 6 Another insulating resin layer 7 Concave portion of stamping die 8 Stamping die 10 Filler-arranged film 20, 20a, 20b Filler group 30 Release film 40 Transfer substrate 41 Filler transfer sheet 100 Wiring board 200 μLED F Fillet H Heat tool t 0 Height of the convex part t 1 Depth of recess w 1 Recess width
Claims
1. A filler-arranged film having an insulating resin layer for retaining a filler and a filler, wherein a concave portion and a convex portion are formed on one side of the insulating resin layer for retaining a filler, and at least one filler group consisting of a plurality of fillers is arranged in the convex portion.
2. A filler arrangement film as described in claim 1, wherein each filler constituting the filler group is arranged on the top surface of the convex portion or at least partially embedded in the insulating resin layer for retaining the filler constituting the convex portion.
3. A filler arranged film according to claim 1 or 2, wherein the protrusions are regularly arranged.
4. A filler arranged film according to claim 1 or 2, wherein a plurality of fillers are regularly arranged within the filler group.
5. The filler arranged film according to claim 1 or 2, wherein no filler is arranged in the recesses.
6. The filler arrangement film according to claim 1 or 2, wherein the recesses penetrate the insulating resin layer for holding the fillers.
7. The filler arrangement film according to claim 1 or 2, wherein another insulating resin layer is laminated on at least one side of the insulating resin layer for holding the fillers.
8. The filler arranged film according to claim 7, wherein the recesses penetrate the filler holding insulating resin layer, and the protrusions are separated from each other by the penetrating recesses.
9. The filler arrangement film according to claim 7, wherein the other insulating resin layer is an insulating resin layer for forming a black matrix.
10. A method for producing a filler array film as claimed in claim 1, comprising the following steps A to C: (Step A) forming an insulating resin layer for retaining filler on a release film that has been subjected to a release treatment; (Step B) forming concave and convex portions on one side of the insulating resin layer for retaining filler by contacting a pressing die having concave portions corresponding to the convex portions of the filler array film with the insulating resin layer for retaining filler and performing hot pressing; and (Step C) opposing the top surfaces of the convex portions to the filler arrangement surface of a filler transfer sheet, having a plurality of fillers arranged on one side of a transfer substrate, and transferring the filler to the top surfaces of the convex portions by pressing from the transfer substrate side.
11. A method for producing a filler array film as described in claim 10, further comprising the following step D following step C: (step D) a step of embedding each filler transferred to the top surface of the convex portion in an insulating resin layer for holding the fillers so that at least a portion of the fillers is embedded.
12. The method according to claim 10 or 11, wherein the mold is a concave veneer.
13. A connection structure in which a first article is connected to a second article via the filler-arranged film according to claim 1.
14. A connection structure according to claim 13, wherein the first article is a transparent display substrate having a transparent electrode disposed on one side thereof, the second article is a μLED having an electrode formed on one side thereof, the filler disposed in the convex portions of the filler array film is conductive particles, and the filler array film itself functions as a conductive film or an anisotropic conductive film.
15. A method for producing a connection structure, comprising: sandwiching the filler-arranged film according to claim 1 between a first article and a second article, and pressing the articles together.
16. A method for manufacturing a connection structure according to claim 15, wherein the first article is a transparent display substrate having a transparent electrode arranged on one side, the second article is a μLED having an electrode formed on one side, the filler arranged in the convex portions of the filler array film is conductive particles, and the filler array film itself functions as a conductive film or an anisotropic conductive film.
Citation Information
Patent Citations
Connection member
JP2003217354A
Connection structure and anisotropic conductive adhesive
JP2015056285A
Anisotropic conductive film and manufacturing method thereof
JP2020024932A
Anisotropic conductive film and connecting structure
JP2020177916A
Method for manufacturing display device
JP2022151818A
Cited By
Filler-containing film and method for manufacturing same, and connection structure and method for manufacturing same
WO2026074952A1