Method for producing joined member and joining device
The method of plasma treatment to create nanoscale unevenness on metal surfaces addresses the limitations of conventional joining techniques by enabling strong, low-temperature bonding of dissimilar materials, reducing environmental impact and costs, and improving processing efficiency for thin metal members.
Patent Information
- Application Number
- PCT/JP2024/011025
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional methods for joining dissimilar materials, such as metal and resin, face challenges including environmental impact, long processing times, and high costs, particularly when using chemical treatments, laser irradiation, and nanoparticle pastes, which are not suitable for thin metal members or semiconductor chip connections.
A method and device that impart nanoscale unevenness to metal surfaces through plasma treatment without a mask, using hydrogen or helium gases, allowing for low-temperature joining of metal and resin members by promoting atomic diffusion and anchor effects, thereby overcoming the limitations of existing techniques.
This approach enables strong mechanical bonding at low temperatures, reduces environmental impact, and is cost-effective, making it suitable for thin metal members and improving processing efficiency compared to conventional methods.
Smart Images

Figure JP2024011025_03102024_PF_FP_ABST
Abstract
Description
Method for manufacturing joined member and joining device
[0001] The present invention relates to a method for manufacturing a joint member and a joining device.
[0002] Various joining techniques for joining dissimilar materials (joining a metal member and a resin member, or joining metal members together) have been known. In particular, in joining dissimilar materials, it has been found that a strong mechanical joint between a metal member and another member can be obtained by welding or pressing another member onto the surface of a metal member that has been subjected to a surface treatment (e.g., formed with irregularities). Non-Patent Document 1 describes forming irregularities on the surface of a metal member by chemical treatment, and Non-Patent Document 2 describes forming irregularities on the surface of a metal member by laser irradiation.
[0003] Another known method is to join metal members by welding or pressing another metal member onto a metal member to which nanoparticles have been pasted.
[0004] Shin Horiuchi, "International Standard for Evaluation Test Methods of Metal-Dissimilar Material Composite Joint Characteristics," Instrumentation and Control, Vol. 54, No. 10, 2015, pp. 743-747 Masahiko Itakura, "Laser Surface Processing Technology for Metal / Dissimilar Material Joints," Surface Technology, Vol. 71, No. 11, 2020, pp. 667-671
[0005] The method described in Non-Patent Document 1 uses chemicals that have a large environmental impact. The method described in Non-Patent Document 2 requires a long time for surface treatment and generates relatively large irregularities due to laser irradiation, making it extremely difficult to apply to thin metal members (for example, metal members that connect semiconductor chips together).
[0006] Furthermore, in the method of bonding metal members together by pasting nanoparticles, a dispersant or stabilizer is required, and the nanoparticles are expensive.
[0007] One aspect of the present invention has been made in consideration of the above problems, and has an object to realize joining of dissimilar materials by a method different from conventional methods.
[0008] In order to solve the above problems, the manufacturing method of a joining member according to aspect 1 of the present invention includes a texture processing step of imparting a nanoscale texture to the surface of a first member, which is a metal, by plasma treatment without using a mask, and a joining step of joining a second member to the surface of the first member to which the texture has been imparted.
[0009] In order to solve the above problem, the bonding device according to aspect 5 of the present invention includes an unevenness processing unit that imparts a nanoscale uneven shape to the surface of a first member, which is metal, by plasma treatment without using a mask, and a bonding unit that joins a second member to the surface of the first member to which the uneven shape has been imparted.
[0010] According to one aspect of the present invention, it is possible to realize joining of dissimilar materials by a method different from the conventional method.
[0011] Fig. 1 is a schematic diagram showing the joining of metal members by a manufacturing method of a bonded member according to one embodiment; Fig. 2 is a schematic diagram showing the joining of a metal member and a resin member by the manufacturing method of the bonded member; Fig. 3 is a diagram showing a bonding apparatus for manufacturing the bonded member; Fig. 4 is a flowchart showing an example of a manufacturing method of the bonded member; Fig. 5 is a diagram showing an electron microscope image of the uneven processed surface of a metal member that has been surface-treated.
[0012] [Embodiment 1] (1. Features of one aspect of the present invention) Fig. 1 is a schematic diagram showing joining of metal members by a manufacturing method of a joining member 5 according to this embodiment. Fig. 2 is a schematic diagram showing joining of a metal member and a resin member by a manufacturing method of a joining member 5 according to this embodiment.
[0013] As shown in Figures 1 and 2, the first metal member 1 (first member) has a nanoscale uneven surface 4 (uneven shape) on its surface 1a. The uneven surface 4 has nanofuzz 41 (fibrous nanostructure), which are nanoscale protrusions, and / or nanoporous 42, which are nanoscale pores. The nanoscale protrusions are those with a diameter of less than 1 µm. The nanoscale pores are those with a diameter of less than 1 µm, including atomic vacancies.
[0014] The surface energy of the surface 1a on which such nanoscale irregularities 4 are formed is extremely high. Therefore, atomic migration is promoted at low temperatures on the surface 1a. In particular, atomic diffusion is promoted on the surface 1a where interstitial atoms and atomic vacancies exist at or above the thermal equilibrium concentration. Therefore, as shown in FIG. 1 , by pressing a second metal member 2 (second member) against a first metal member 1 having an irregularity 4, it is possible to bond the metal members together at low temperatures. As shown in FIG. 1 , the surface 2a of the second metal member 2 may be provided with an irregularity 4. This can further strengthen the bond between the metal members. Note that, in this specification, metal bonding at "low temperatures" refers to metal bonding at a temperature lower than the melting point of the first metal member 1 (and the second metal member 2).
[0015] Furthermore, as shown in Figure 2, by pressing or welding a resin member 3 (second member) to the surface 1a of the first metal member 1, the resin becomes entangled with the nanofuzz 41 and / or nanoporous 42, resulting in a strong mechanical bond due to the anchor effect.
[0016] The first metal member 1 is a substrate made of a metal material such as copper, silver, gold, iron, aluminum, magnesium, nickel, zinc, titanium, or stainless steel.
[0017] The uneven workpiece surface 4 is formed by plasma treatment (details of which will be described later). In this plasma treatment, hydrogen gas or helium gas is used as the treatment gas, and no chemicals that have a large environmental impact are used. In other words, the manufacturing method according to this embodiment is advantageous over conventional manufacturing methods that use chemical treatment in terms of environmental impact.
[0018] Furthermore, the plasma treatment allows for batch processing of the surface 1a. Furthermore, the height and / or depth of the region in which the nanofuzz 41 and / or nanoporous 42 are formed by the plasma treatment is approximately several tens of nanometers to several micrometers from the surface. Therefore, the first metal member 1 may be a thin metal member (thickness of 100 μm or less). In other words, the manufacturing method according to this embodiment is advantageous over conventional manufacturing methods using laser irradiation in terms of processing time and applicability.
[0019] Furthermore, low-temperature plasma processing using inexpensive hydrogen gas or helium gas as the processing gas enables joining of metal members at low temperatures. In other words, the manufacturing method according to this embodiment is advantageous over manufacturing methods using nanoparticle pastes from the viewpoint of cost.
[0020] As described above, the present inventors have discovered that by pressing the second metal member 2 or the resin member 3 against the surface 1 a of the first metal member 1 that has been given a nanoscale uneven shape by plasma treatment, the second metal member 2 or the resin member 3 can be firmly bonded to the first metal member 1. This manufacturing method has various advantages over manufacturing methods according to conventional technologies. This finding is highly unexpected and cannot be predicted from conventional common knowledge regarding the bonding of dissimilar materials.
[0021] (2. Manufacturing Apparatus) Figure 3 is a diagram showing a bonding apparatus 100 for manufacturing the bonded member 5. The bonding apparatus 100 includes a textured processing unit 10 and a bonding unit 20. The textured processing unit 10 imparts a nanoscale textured shape to the surface 1a of the first metal member 1 by plasma treatment. The bonding unit 20 bonds the second metal member 2 or the resin member 3 to the surface 1a of the first metal member 1 to which the textured shape has been imparted.
[0022] The concave-convex processing unit 10 includes a housing 11 , a stage 12 , a temperature adjustment unit 13 , a processing gas supply unit 14 , and a high-frequency power supply 15 .
[0023] The housing 11 constitutes a processing chamber in which plasma processing is performed on the first metal member 1. The processing chamber is set to a predetermined pressure by a vacuum pump (not shown). A stage 12, a temperature adjustment unit 13, and a processing gas supply unit 14 are arranged in the processing chamber.
[0024] The stage 12 is a platform on which the first metal member 1 is placed. The temperature adjustment unit 13 is disposed on the bottom surface of the housing 11 and supports the stage 12. The temperature adjustment unit 13 includes, for example, piping (not shown) through which a circulating refrigerant for cooling the stage 12 passes and / or a heater (not shown) for heating the stage 12. With this configuration, the first metal member 1 can be cooled and / or heated via the stage 12.
[0025] The process gas supply unit 14 is disposed on the upper surface of the housing 11. The process gas supply unit 14 includes a base 141 and a generally cylindrical extension 142 extending downward from the base 141. The base 141 and the extension 142 are electrically conductive. The base 141 has a cavity 141a formed therein that receives a process gas from the outside, and the cavity is connected to an interior 142a of the extension 142. The tip of the extension 142 faces the first metal member 1 in the vicinity of the first metal member 1 placed on the stage 12. With this configuration, the process gas supply unit 14 supplies a process gas to the surface 1a of the first metal member 1 that is placed in a process chamber at a predetermined pressure.
[0026] One end of the high-frequency power supply 15 is electrically connected to the process gas supply unit 14. The other end of the high-frequency power supply 15 is electrically connected to ground. Because the base 141 and the extension 142 are conductive, the high-frequency power supply 15 applies an alternating voltage between the tip 142b of the extension 142 and the surface 1a of the first metal member 1. In other words, the extension 142 functions as a pipe-shaped needle electrode. With this configuration, the process gas supplied from the tip opening of the extension 142 is converted into a plasma state by the alternating voltage. In other words, a plasma generation region is formed between the tip of the extension 142 and the surface 1a of the first metal member 1. The surface 1a of the first metal member 1 is exposed to the process gas in a plasma state. This allows plasma processing to be performed on the surface 1a of the first metal member 1.
[0027] The joining unit 20 includes a housing 21 , a stage 22 , and a pressing unit 23 .
[0028] The housing 21 constitutes a processing chamber for joining the first metal member 1 and the second metal member 2 or the resin member 3. At least when joining the metal members, the processing chamber is set to a low-oxygen atmosphere or a predetermined atmosphere. The predetermined atmosphere is an atmosphere that can suppress the generation of an oxide film when joining the metal members, and may be, for example, room air.
[0029] The housing 21 may be shared with the housing 11, which is a processing chamber for performing plasma processing. In particular, when joining the first metal member 1 and the second metal member 2, the first metal member 1 and the second metal member 2 are quickly joined in the same processing chamber after the plasma processing in order to prevent the generation of an oxide film.
[0030] The stage 22 places the first metal member 1 that has been subjected to plasma treatment, and the second metal member 2 or resin member 3 on the first metal member 1. The pressing unit 23 presses the second metal member 2 or resin member 3 against the first metal member 1. This bonds the first metal member 1 and the second metal member 2 or resin member 3 together.
[0031] (3. Manufacturing Method of Bonded Member) Fig. 4 is a flowchart showing an example of a manufacturing method of the bonded member 5. The manufacturing method of the bonded member 5 will be described below with reference to Fig. 4 .
[0032] First, a nanoscale texture is imparted to the surface 1a of the first metal member 1 by plasma treatment (texture processing step S1). Specifically, the first metal member 1 is placed on the stage 12 inside the housing 11, and the processing chamber is depressurized to a predetermined pressure. Then, a plasma generation region is formed between the extension 142 and the surface 1a of the first metal member 1 by the high-frequency power supply 15, and processing gas is supplied to the plasma generation region from the tip opening of the extension 142. In this way, the surface 1a of the first metal member 1 is subjected to plasma treatment. Note that the surface 2a of the second metal member 2 may also be subjected to plasma treatment.
[0033] Next, the second metal member 2 or the resin member 3 is bonded to the surface 1a of the first metal member 1 to which the concave-convex shape has been imparted (bonding step S2). Specifically, the first metal member 1 to which the concave-convex shape has been imparted is moved to a stage 22 inside a housing 21. Then, the second metal member 2 or the resin member 3 is brought into contact with the surface 1a of the first metal member 1, and the pressing portion 23 presses the second metal member 2 or the resin member 3 against the first metal member 1. This makes it possible to bond a metal member to a resin member or to bond metal members together. Note that bonding of metal members together is performed in a low-oxygen atmosphere or a specified atmosphere to prevent the formation of an oxide film.
[0034] Here, in the asperity processing step S1, the processing gas may contain helium. By exposing the surface 1 a of the first metal member 1 to helium gas in a plasma state, nanofuzz 41 is formed on the surface 1 a of the first metal member 1.
[0035] Furthermore, the processing gas may contain, in addition to helium, diatomic or polyatomic molecules such as hydrogen molecules, nitrogen molecules, ammonia molecules, and / or water molecules. If the processing gas is only helium, the plasma power consumed by the helium is relatively small, and the plasma generation region expands within the processing chamber. This results in a decrease in plasma density. On the other hand, by including the above-mentioned molecules in the processing gas, the expansion of the plasma generation region can be suppressed. Therefore, the decrease in plasma density can be suppressed. Note that it is preferable to select the above-mentioned molecules that have little etching effect on the first metal member 1.
[0036] The processing gas may also contain hydrogen molecules. By exposing the surface 1 a of the first metal member 1 to hydrogen gas in a plasma state, nanoporous regions 42 are formed on the surface 1 a of the first metal member 1. Specifically, a large amount of hydrogen dissolves in the first metal member 1 exposed to hydrogen gas in a plasma state. This dissolved hydrogen generates interstitial atoms and vacancies in the first metal member 1. The vacancies then aggregate to form nanoporous regions 42. The excessive generation of interstitial atoms and vacancies promotes the diffusion of metal atoms at low temperatures. Therefore, by pressing the second metal member 2 against the first metal member 1, diffusion bonding between the first metal member 1 and the second metal member 2 is achieved at low temperatures. As described above, when bonding the first metal member 1 and the second metal member 2, it is preferable that the processing gas contain hydrogen molecules.
[0037] For example, the processing gas may be a mixed gas of hydrogen gas and helium gas (hereinafter referred to as a hydrogen-helium mixed gas). The proportion of helium gas (by volume under standard conditions) in the hydrogen-helium mixed gas is preferably 50 to 90%. This allows nanofuzz 41 to be formed on the surface 1a of the first metal member 1. Furthermore, compared to when the processing gas is helium gas alone, a decrease in plasma density can be suppressed.
[0038] For example, the processing gas may be hydrogen gas alone, which allows the nanoporous regions 42 to be formed on the surface 1 a of the first metal member 1 .
[0039] The processing gas may also contain oxygen molecules, water molecules, nitrogen molecules, or the like. By performing plasma processing in an atmosphere containing oxygen molecules, water molecules, or nitrogen molecules, the textured portion 10 can be oxidized, hydroxylated, or nitrided, respectively. Oxidizing, hydroxylating, or nitriding the textured portion 10 can promote bonding between the first metal member 1 and the resin member 3 due to the influence of surface functional groups.
[0040] The processing gas pressure needs to be at least 1 Torr. The processing gas pressure may be 50 Torr or more. This is an extremely high pressure compared to surface processing techniques using etching processes using chlorine, fluorine, etc. By setting the processing gas pressure to 50 Torr or more, the plasma generation region can be intentionally localized (i.e., the plasma density can be improved), making maskless processing possible. Therefore, the processing time required for plasma processing can be shortened. In addition, the exhaust device can be realized at low cost. The processing gas pressure is preferably 100 Torr or more.
[0041] (4. Effects) According to the above configuration, a nanoscale texture is imparted to the surface 1a without using a mask, using a plasma-state processing gas containing hydrogen molecules or helium, which is inexpensive and harmless. In other words, it is possible to impart a texture in a dry environment without using chemical products that have a high environmental impact. Therefore, compared to conventional techniques that impart texture using chemical treatment, costs can be reduced and the environmental impact can be reduced. Furthermore, compared to conventional surface processing techniques using etching treatment, no mask treatment or mask material corresponding to the nanoscale texture is required.
[0042] Furthermore, by exposing the surface 1 a of the first metal member 1 to a plasma-state processing gas, the surface 1 a can be processed all at once, which reduces the processing time compared to the conventional technique of forming a textured surface by laser irradiation.
[0043] Furthermore, the depth of the region where the nanofuzz 41 and / or nanoporous 42 are formed by the plasma treatment is approximately several tens of nanometers to several micrometers, so the above-described plasma treatment can also be applied to thin metal members.
[0044] Furthermore, since the processing gas contains hydrogen molecules, the surface 1a of the first metal member 1 is always kept clean during the plasma processing, thereby improving the activity of the surface 1a on which the uneven processing surface 4 is formed.
[0045] (5. Example) <Plasma Treatment> Figure 5 is a diagram showing an electron microscope image of the uneven processed surface 4 of the first metal member 1 that has been surface treated using the above-mentioned bonding device 100. Reference numeral 5A in Figure 5 indicates nanoporous 42. Reference numeral 5B in Figure 5 indicates nanofuzz 41. The manufacturing conditions for forming the uneven processed surface 4 shown in Figure 5 will be described below.
[0046] A silver plate with a purity of 99.98% and a thickness of 200 μm was used as the first metal member 1. The extension 142 (pipe-shaped needle electrode) had a diameter of approximately 1 mm. The gap between the tip 142b of the extension 142 and the surface 1a of the first metal member 1 was approximately 0.7 mm. High-frequency power of 150 MHz was applied to the extension 142 to generate plasma in the gap.
[0047] Hydrogen gas or hydrogen-helium mixed gas (helium concentration: 90%) was used as the processing gas. The flow rate of the processing gas was 10 slm. When hydrogen gas was used as the processing gas, nanoporous 42 shown by reference numeral 5A in FIG. 5 was obtained. When hydrogen-helium mixed gas was used as the processing gas, nanofuzz 41 shown by reference numeral 5B in FIG. 5 was obtained.
[0048] Here, the high-frequency power input to the extension portion 142 was 30 W to 150 W. When the power was 30 W, the average pore diameter of the nanoporous portions 42 was approximately 30 nm. When the power was 50 W, the average pore diameter of the nanoporous portions 42 was approximately 50 nm. In other words, increasing the power increased the average pore diameter of the nanoporous portions 42. On the other hand, increasing the power decreased the number density of the nanoporous portions 42.
[0049] The exposure time for the plasma treatment using hydrogen gas was 5, 10, 20, and 30 minutes. When the exposure time was 5 minutes, numerous cavities were formed within a depth of 80 nm from the surface 1a. When the exposure time was 20 minutes, cavities were also formed within a depth of 80 nm from the surface 1a at the same number density as when the exposure time was 5 minutes. This indicates that the generation and disappearance of nanoporous structures 42 was repeated while the surface 1a was exposed to hydrogen gas in a plasma state.
[0050] The exposure time for the plasma treatment using the hydrogen-helium mixed gas was 1, 20, and 60 minutes. When the exposure time was 1 minute, the formation of nanofuzz 41 was confirmed, but it did not reach the point of being formed over the entire surface 1a. When the exposure time was 60 minutes, the formation of nanofuzz 41 over the entire surface was confirmed. This indicates that nanofuzz 41 gradually covers the surface 1a over time.
[0051] In addition to silver plates, the above-described plasma treatment was also performed on substrates made of copper or gold as the first metal member 1. A hydrogen-helium mixed gas (helium concentration: 90%) was used as the treatment gas. The formation of nanofuzz 41 was confirmed in gold. Meanwhile, the formation of nanoporous regions 42 was confirmed in copper, but the formation of nanofuzz 41 was not. This is because copper is a material that is significantly etched by hydrogen. By replacing the hydrogen in the treatment gas with a gas that does not etch copper, such as nitrogen, nanofuzz 41 can also be formed in copper.
[0052] <Bonding> An experiment was also conducted to join plasma-treated metal members. The metal members were made of Ag or Cu. A 5 mm diameter metal rod (hereinafter simply referred to as the "sample") was used as the metal member. The metal rod was set on a high-frequency electrode and a ground electrode, respectively. Power was applied to hydrogen at a pressure of 200 Torr to generate hydrogen plasma. The metal rod was exposed to the hydrogen plasma for approximately 20 minutes to perform pretreatment (uneven processing step S1) on the joining surfaces of the metal rods. Here, the input power was 100 W, the discharge gap was 0.7 mm, and the gas flow rate was 0 slm.
[0053] Thereafter, the bonding process (bonding step S2) was performed using two methods. In the first method (hereinafter referred to as Example A1), after a predetermined time had elapsed since the plasma treatment, the bonding surfaces of the samples were brought into contact with each other while the plasma was still being generated, and a bonding pressure of 20 MPa was applied to the bonding surfaces, resulting in pressure bonding for 5 minutes. In this method, the plasma was extinguished when the samples came into contact with each other. It was confirmed that the temperature of the samples immediately before bonding was approximately 250°C due to plasma heating, and that the temperature of the samples was rapidly cooled to approximately 50°C 10 seconds after the light was turned off. Therefore, the bonding method in Example A1 will be referred to as "hydrogen plasma-treated sample / low-temperature pressure bonding in hydrogen."
[0054] In the second method (hereinafter referred to as Example A2), after plasma treatment, the hydrogen plasma was extinguished, the samples were then pressure-welded together in the plasma treatment chamber, and then the chamber was opened to the atmosphere while the bonding pressure was still applied, and the bonded portion of the samples was then heated to approximately 350° C. This bonding method in Example A2 will be referred to as "hydrogen plasma-treated sample / high-temperature pressure welding in air."
[0055] Table 1 below shows the experimental results of Examples A1 and A2 when the material of the metal member was Ag or Cu. Table 1 also shows the results of Comparative Example R1, in which the sample was not subjected to plasma treatment and was directly heated and pressure-welded in the atmosphere (i.e., high-temperature pressure welding in air). The joining method in Comparative Example R1 is referred to as "untreated sample / high-temperature pressure welding in air." In Table 1, "Good" indicates that bonding between the metals was confirmed, and "Poor" indicates that bonding between the metals was not confirmed.
[0056] As shown in Comparative Example R1 in Table 1, in the samples that had not been subjected to plasma treatment, no bonding was formed between the samples even when the samples were subjected to thermal pressure welding at 350° C. and 20 MPa.
[0057] On the other hand, as shown in Example A1 in Table 1, low-temperature solid-state bonding was possible in both the Ag and Cu samples that had been subjected to hydrogen plasma treatment.
[0058] Here, bonding between metals was confirmed not only during plasma treatment (low-temperature pressure welding in hydrogen), but also during heated pressure welding after the plasma was removed (high-temperature pressure welding in air). Therefore, it can be said that hydrogen plasma treatment contributes to the bonding of metal components, rather than welding caused by abnormal discharge that occurs the moment the samples come into contact.
[0059] Furthermore, it was found that even with copper, which is significantly affected by surface oxidation during bonding, bonding in the atmosphere is possible by carrying out the surface treatment according to this embodiment.
[0060] As described above, it was confirmed that the plasma treatment has the effect of contributing to low-temperature bonding of metal members.
[0061] We also conducted an experiment to bond a plasma-treated metal component to a resin component. Specifically, a hydrogen-helium mixed gas was used as the treatment gas for 20 minutes, and a silver sample with nanofuzz 41 formed, as shown by reference numeral 5B in Figure 5, was bonded to polypropylene, a resin with poor adhesion. As a comparative example, untreated silver and polypropylene were bonded.
[0062] In the bonding process in this experiment, the bonding pressure was 0 MPa or 3 MPa, the bonding temperature was 170° C., and the bonding time was 20 minutes. This bonding process was also carried out in the atmosphere.
[0063] The shear strength of the bonded samples obtained by this bonding process was evaluated by a tensile test. When the bonding pressure was 0 MPa, the bonded sample of treated silver and polypropylene showed 34 times the bond strength of the bonded sample of untreated silver and polypropylene.
[0064] On the other hand, the bonded sample of silver and polypropylene treated with a bonding pressure of 3 MPa showed a bond strength approximately 12 times higher than that of the same bonded sample at 0 MPa. At this time, the shear strength reached 79 MPa. This value exceeds the tensile strength of polypropylene, and it was confirmed that the bonded sample broke due to the destruction of the polypropylene base material.
[0065] (Summary) The manufacturing method of a joining member according to aspect 1 of the present invention includes a texture processing step of imparting a nanoscale texture to the surface of a first member, which is a metal, by plasma treatment without using a mask, and a joining step of joining a second member to the surface of the first member to which the texture has been imparted.
[0066] In the method for manufacturing a bonded member according to Aspect 2 of the present invention, in the above-described Aspect 1, a processing gas used in the plasma processing may contain helium.
[0067] In the method for manufacturing a bonded member according to Aspect 3 of the present invention, in the above-described Aspect 1, a processing gas for the plasma processing may contain hydrogen molecules, and the second member may be a metal.
[0068] In the method for manufacturing a bonded member according to Aspect 4 of the present invention, in any of Aspects 1 to 3, the pressure of the processing gas in the plasma processing may be 50 Torr or more.
[0069] A bonding apparatus according to aspect 5 of the present invention includes an unevenness processing unit that imparts a nanoscale uneven shape to the surface of a first member, which is a metal, by plasma treatment without using a mask, and a bonding unit that joins a second member to the surface of the first member to which the uneven shape has been imparted.
[0070] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.
[0071] REFERENCE SIGNS LIST 1 First metal member (first member) 2 Second metal member (second member) 3 Resin member (second member) 4 Textured processed surface 41 Nanofuzz 42 Nanoporous 5 Joining member 10 Textured processed portion 20 Joining portion 100 Joining device
Claims
1. A method for manufacturing a bonded member, comprising: a step of processing the surface of a first metal member to form a nanoscale uneven shape by plasma treatment without using a mask; and a step of bonding a second member to the surface of the first member to which the uneven shape has been formed.
2. The method for manufacturing a joint member according to claim 1, wherein the processing gas used in the plasma processing contains helium.
3. The method for manufacturing a joint member according to claim 1, wherein a processing gas in the plasma processing contains hydrogen molecules, and the second member is a metal.
4. The method for manufacturing a joint member according to claim 1, wherein the pressure of the processing gas in the plasma processing is 50 Torr or more.
5. A bonding device comprising: an unevenness processing unit that applies a nanoscale uneven shape to the surface of a first metal member by plasma treatment without using a mask; and a bonding unit that bonds a second member to the surface of the first member to which the uneven shape has been applied.
Citation Information
Patent Citations
Semiconductor device, electronic device, and semiconductor device manufacturing method
JP2012204501A
Simplified copper-to-copper bonding method
JP2012531312A
Method of manufacturing multilayer substrate, and multilayer substrate
JP2013021126A
Joining method and device therefor
WO2005097396A1