Photochromic article, spectacles, and method for producing photochromic article

The use of a primer layer with a polymer containing hydroxyl and (meth)acryloyl groups and blocked isocyanate addresses the adhesion challenges in photochromic articles by suppressing viscosity increase and enhancing adhesion, resulting in a stable and effective photochromic solution.

WO2024203725A1PCT designated stage expired Publication Date: 2024-10-03HOYA LENS THAILAND LTD +2
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011028
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing photochromic articles face challenges in achieving excellent adhesion between the photochromic layer and the base material, particularly due to the viscosity increase of moisture-curable polyurethane resins during storage, which affects the coating properties.

Method used

A primer layer formed from a polymer composition containing a polymer with a hydroxyl group and a (meth)acryloyl group, along with blocked isocyanate, is used between the base material and the photochromic layer, which suppresses the reaction during storage and enhances adhesion by forming a cured layer through heat treatment.

Benefits of technology

This approach results in a photochromic article with improved adhesion between the photochromic layer and the base material, maintaining coating properties and preventing viscosity increase, thus providing a stable and effective photochromic solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

Provided is a photochromic article having a base material, a primer layer formed from a polymer composition for primer layer formation, and a photochromic layer including a photochromic compound, in the stated order. The polymer composition for primer layer formation includes a polymer having a hydroxy group and a (meth)acryloyl group, and a blocked isocyanate.
Need to check novelty before this filing date? Find Prior Art

Description

Photochromic article, eyeglasses, and method for manufacturing photochromic article

[0001] The present invention relates to photochromic articles, eyeglasses, and methods for making photochromic articles.

[0002] A photochromic compound is a compound that exhibits a color when irradiated with light in a photoresponsive wavelength range and fades in the absence of light (photochromic property). Hereinafter, an article containing a photochromic compound will be referred to as a photochromic article. For example, Patent Document 1 discloses an optical article having a layer containing a photochromic compound (photochromic layer) provided on a substrate.

[0003] Patent No. 4405833 specification

[0004] The present inventors have conducted extensive research to improve the adhesion between the photochromic layer and the substrate, with the aim of improving the performance of photochromic articles.

[0005] That is, an object of one aspect of the present invention is to provide a photochromic article having excellent adhesion between a photochromic layer and a substrate.

[0006] After extensive research, the inventors have discovered that a photochromic article with excellent adhesion between the photochromic layer and the substrate can be provided by providing a primer layer formed from a primer layer-forming polymer composition containing a polymer having a hydroxy group and a (meth)acryloyl group and a blocked isocyanate between the photochromic layer and the substrate. To improve adhesion between the photochromic layer and the substrate, Patent Document 1 (Japanese Patent No. 4405833) proposes providing a polyurethane resin layer formed from a moisture-curing polyurethane resin between the substrate and the photochromic layer. However, moisture-curing polyurethane resins cure by reacting with moisture in the air, and therefore tend to increase in liquid viscosity due to reaction with moisture in the air during storage. In contrast, it has been found that the primer layer-forming polymer composition can suppress viscosity increase during storage, thereby exhibiting excellent coatability after storage. This is presumably because the isocyanate contained in the polymer composition for forming a primer layer is a blocked isocyanate in which the isocyanate group is protected with a blocking agent, and therefore the reaction between the hydroxy group of the polymer and the isocyanate group during storage can be suppressed. However, the present invention is not limited to the presumption described in this specification.

[0007] One aspect of the present invention is as follows. [1] A photochromic article having, in this order: a substrate; a primer layer formed from a primer layer-forming polymer composition; and a photochromic layer containing a photochromic compound, wherein the primer layer-forming polymer composition contains a polymer having a hydroxy group and a (meth)acryloyl group, and a blocked isocyanate. [2] The photochromic article according to [1], wherein the polymer is a (meth)acrylic polymer. [3] The photochromic article according to [1], wherein the photochromic layer is a cured layer obtained by curing a (meth)acrylate-based polymerizable composition containing a photochromic compound. [4] The photochromic article according to [2], wherein the photochromic layer is a cured layer obtained by curing a (meth)acrylate-based polymerizable composition containing a photochromic compound. [5] The photochromic article according to any one of [1] to [4], which is a spectacle lens, a goggle lens, a visor portion of a sun visor, or a helmet shield member. [6] The photochromic article according to [5], wherein the photochromic article is a spectacle lens. [7] Eyeglasses equipped with the spectacle lens according to [6]. [8] A method for producing a photochromic article, comprising: applying a primer layer-forming polymer composition on a substrate to form a primer layer; and forming a photochromic layer containing a photochromic compound on the formed primer layer, wherein the primer layer-forming polymer composition contains a polymer having a hydroxy group and a (meth)acryloyl group, and a blocked isocyanate; and further comprising heat-treating a laminate obtained by forming the photochromic layer. [9] A method for producing a photochromic article according to [8], wherein the polymer is a (meth)acrylic polymer.

[10] A method for producing a photochromic article according to [8], comprising forming the photochromic layer by curing a (meth)acrylate-based polymerizable composition containing a photochromic compound.

[11] A method for producing a photochromic article according to [9], comprising forming the photochromic layer by curing a (meth)acrylate-based polymerizable composition containing a photochromic compound.

[12] The method for producing a photochromic article according to any one of [8] to

[11] , wherein the photochromic article is a spectacle lens, a goggle lens, a visor portion of a sun visor, or a shield member of a helmet.

[0008] According to one aspect of the present invention, a photochromic article having excellent adhesion between a photochromic layer and a substrate can be provided.

[0009] [Photochromic Article] The photochromic article according to one embodiment of the present invention will be described in further detail below.

[0010] The photochromic article has a substrate, a primer layer, and a photochromic layer in this order. In one embodiment, the primer layer can be a layer adjacent to the photochromic layer, and can be a layer adjacent to the substrate or a layer provided on the substrate. Here, "adjacent" means in direct contact without any other layer interposed therebetween.

[0011] <Substrate> The photochromic article can have a photochromic layer on a substrate selected depending on the type of article. As an example of the substrate, a spectacle lens substrate can be a plastic lens substrate or a glass lens substrate. The glass lens substrate can be, for example, a lens substrate made of inorganic glass. A plastic lens substrate is preferred as the lens substrate from the viewpoints of being lightweight, shatter-resistant, and easy to handle. Examples of plastic lens substrates include (meth)acrylic resins, styrene resins, polycarbonate resins, allyl resins, allyl carbonate resins such as diethylene glycol bisallyl carbonate resin (CR-39), vinyl resins, polyester resins, polyether resins, urethane resins obtained by reacting an isocyanate compound with a hydroxy compound such as diethylene glycol, thiourethane resins obtained by reacting an isocyanate compound with a polythiol compound, and cured products (commonly referred to as transparent resins) obtained by curing a curable composition containing a (thio)epoxy compound having one or more disulfide bonds in the molecule. The lens substrate may be undyed (colorless lenses) or dyed (dyed lenses). The refractive index of the lens substrate can be, for example, approximately 1.50 to 1.75. However, the refractive index of the lens substrate is not limited to the above range, and may be within the above range or may deviate above or below the above range. In this invention and this specification, the refractive index refers to the refractive index for light with a wavelength of 500 nm. Furthermore, the lens substrate may be a lens with refractive power (a so-called prescription lens) or a lens without refractive power (a so-called non-prescription lens).

[0012] The spectacle lens can be any of various lenses, such as a single-vision lens, a multifocal lens, or a progressive-power lens. The type of lens is determined by the surface shapes of both sides of the lens substrate. The surface of the lens substrate may be convex, concave, or flat. In typical lens substrates and spectacle lenses, the object-side surface is convex and the eyeball-side surface is concave. However, the present invention is not limited to this. The photochromic layer can usually be provided on the object-side surface of the lens substrate, but it may also be provided on the eyeball-side surface.

[0013] <Primer Layer> The primer layer is formed from a polymer composition for forming a primer layer, which contains a polymer having a hydroxy group and a (meth)acryloyl group, and a blocked isocyanate.

[0014] (Polymer) In the present invention and this specification, the term "(meth)acryloyl group" is used to encompass both acryloyl and methacryloyl groups, and the term "(meth)acryloyloxy group" is used to encompass both acryloyloxy and methacryloyloxy groups. In the polymer, the acryloyl group may be contained in the form of an acryloyloxy group, and the methacryloyl group may be contained in the form of a methacryloyloxy group. This also applies to (meth)acrylates, which will be described later.

[0015] The "polymer" of the present invention and the present specification may be a homopolymer or a copolymer.

[0016] The polymer may contain a hydroxy group and a (meth)acryloyl group in the side chain of the polymer. The inventors speculate that the hydroxy group contained in the polymer contributes to forming a bond between the substrate and the primer layer together with the isocyanate group regenerated by dissociating the blocking agent of the blocked isocyanate, and that the (meth)acryloyl group contained in the polymer contributes to forming a bond between the photochromic layer and the primer layer. It is believed that these bond formations can improve the adhesion between the photochromic layer and the substrate.

[0017] The main skeleton of the polymer is not particularly limited. In one embodiment, the polymer can be a (meth)acrylic polymer. In the present invention and this specification, the term "(meth)acrylic polymer" refers to a homopolymer or copolymer of (meth)acrylate. The term "(meth)acrylate" will be described in detail later.

[0018] The polymer having a hydroxy group and a (meth)acryloyl group may be a polymer synthesized by a known method, or may be a commercially available product, such as a reactive polymer (RP-274S) manufactured by KSM Co., Ltd.

[0019] (Blocked isocyanate) A blocked isocyanate is an isocyanate in which the isocyanate group is protected with a blocking agent. The blocking agent inhibits the reaction of the isocyanate group, and when the blocking agent is dissociated by heat treatment, the isocyanate group is regenerated, and the regenerated isocyanate group can undergo a crosslinking reaction with an active hydrogen-containing group (e.g., a hydroxy group).

[0020] Examples of blocked isocyanates include blocked isocyanates of polyisocyanates such as diisocyanates and triisocyanates. Examples of isocyanate types include adduct, biuret, and isocyanurate types, with biuret and isocyanurate types being preferred. Blocking agents that can dissociate at temperatures that are unlikely to cause deformation or deterioration of the substrate are preferred, and in this regard, preferred blocking agents include diethyl allomate (DEM) and dimethylpyrazole (DMP). Multiple isocyanate groups contained in the isocyanate may be protected by different blocking agents. For example, blocked isocyanates containing DEM and DMP as blocking agents can also be used.

[0021] (Preparation of Primer Layer-Forming Polymer Composition) In the primer layer-forming polymer composition, the content of the blocked isocyanate relative to 100% by mass of the total of the polymer and the blocked isocyanate can be, for example, 30.0% by mass or more and 60.0% by mass or less. The content of the polymer relative to 100% by mass of the total of the polymer and the blocked isocyanate can be, for example, 30.0% by mass or more, 40.0% by mass or more, or 50.0% by mass or more. The content of the polymer can be, for example, 90.0% by mass or less, 80.0% by mass or less, 70.0% by mass or less, or 60.0% by mass or less. The primer layer-forming polymer composition can contain one or more of the polymers and one or more of the blocked isocyanates. In the present invention and this specification, when two or more types of a certain component are contained, the content of that component refers to the total content of those two or more types.

[0022] The polymer composition for forming a primer layer may contain one or more known polymerization initiators capable of functioning as a polymerization initiator for the (meth)acryloyl group of the polymer. The polymer composition for forming a primer layer may contain the polymerization initiator in a content ranging from 0.01 to 3.0 mass%, for example, based on 100 mass% of the total solid content. In the present invention and this specification, the "total solid content" of a certain composition refers to the total amount of all components excluding the solvent.

[0023] The polymerization initiator is preferably a radical polymerization initiator. In addition, a photopolymerization initiator or a thermal polymerization initiator can be used as the polymerization initiator, and a photopolymerization initiator is preferred from the viewpoint of progressing the polymerization reaction in a short time. Examples of the photoradical polymerization initiator include benzoin ketals such as 2,2-dimethoxy-1,2-diphenylethan-1-one; α-hydroxyketones such as 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, and 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one; α-aminoketones such as 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one and 1,2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one; oxime esters such as 1-[(4-phenylthio)phenyl]-1,2-octadione-2-(benzoyl)oxime; bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,6-dimethoxy ...hydroxybenzoyl)phenylphosphine oxide, bis(2,6-dihydroxybenzoyl)phenylpho 2,4,5-triarylimidazole dimers such as 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-di(methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer, and 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer; benzophenone compounds such as benzophenone, N,N'-tetramethyl-4,4'-diaminobenzophenone, N,N'-tetraethyl-4,4'-diaminobenzophenone, and 4-methoxy-4'-dimethylaminobenzophenone;quinone compounds such as 2-ethylanthraquinone, phenanthrenequinone, 2-tert-butylanthraquinone, octamethylanthraquinone, 1,2-benzanthraquinone, 2,3-benzanthraquinone, 2-phenylanthraquinone, 2,3-diphenylanthraquinone, 1-chloroanthraquinone, 2-methylanthraquinone, 1,4-naphthoquinone, 9,10-phenanthraquinone, 2-methyl-1,4-naphthoquinone, and 2,3-dimethylanthraquinone; benzoin ethers such as benzoin methyl ether, benzoin ethyl ether, and benzoin phenyl ether; benzoin compounds such as benzoin, methylbenzoin, and ethylbenzoin; benzyl compounds such as benzyl dimethyl ketal; acridine compounds such as 9-phenylacridine and 1,7-bis(9,9'-acridinylheptane); N-phenylglycine, coumarin, and the like. In the 2,4,5-triarylimidazole dimer, the substituents on the aryl groups of the two triarylimidazole moieties may be the same to give a symmetrical compound, or may be different to give an asymmetrical compound. A thioxanthone compound may also be combined with a tertiary amine, such as the combination of diethylthioxanthone with dimethylaminobenzoic acid. Among these, α-hydroxyketones and phosphine oxides are preferred from the viewpoints of curability, transparency, and heat resistance.

[0024] The polymer composition for forming a primer layer may contain a catalyst that catalyzes the crosslinking reaction of isocyanate groups. The catalyst content may be, for example, in the range of 0.1 to 15.0% by mass, with the total solid content being 100% by mass. Examples of the catalyst include dibutyltin dilaurate, dibutylthione octate, dimethylcyclohexylamine, dimethylbenzylamine, trioctylamine, and bis((2-morpholinoethyl)ether).

[0025] The polymer composition for forming the primer layer can contain any solvent in any amount.

[0026] The polymer composition for forming a primer layer may further contain any amount of known additives that can be usually added to compositions for forming a primer layer. Known compounds can be used as the additives.

[0027] The polymer composition for forming a primer layer can be prepared by mixing the various components described above simultaneously or sequentially in any order.

[0028] A primer layer can be formed on a substrate by applying the primer layer-forming polymer composition to the substrate and then drying the applied composition to remove part or all of the solvent. The drying process may be carried out so as to remove part or all of the solvent. For example, the drying process can be carried out by air drying at room temperature. "Room temperature" as used herein refers to a temperature in the range of 20 to 25°C. Prior to application, the substrate surface may be optionally subjected to one or more known pretreatments, such as alkali treatment and UV ozone treatment, for cleaning the substrate surface. Furthermore, a layer other than a hard coat layer may be formed on the substrate surface to which the primer layer is applied. Known application methods, such as spin coating and dip coating, can be used as the application method, with spin coating being preferred from the viewpoint of uniformity of application.

[0029] The curing treatment for reacting the (meth)acryloyl group of the polymer contained in the primer layer and the heat treatment for dissociating the blocking agent of the blocked isocyanate will be described later.

[0030] The thickness of the primer layer may be, for example, 3 μm or more, and preferably 4 μm or more, and may be, for example, 15 μm or less, and preferably 10 μm or less.

[0031] <Photochromic Layer> <<Polymerizable Compound>> The photochromic article has a photochromic layer containing a photochromic compound on the primer layer. The photochromic layer can be a cured layer obtained by curing a photochromic layer-forming polymerizable composition. The photochromic layer-forming polymerizable composition can be, for example, a (meth)acrylate-based polymerizable composition. In the present invention and this specification, the term "(meth)acrylate-based polymerizable composition" refers to a polymerizable composition containing (meth)acrylate. The term "(meth)acrylate" encompasses acrylate and methacrylate. An "acrylate" is a compound having one or more acryloyl groups per molecule. A "methacrylate" is a compound having one or more methacryloyl groups per molecule. The functionality of a (meth)acrylate is the number of groups selected from the group consisting of acryloyl groups and methacryloyl groups per molecule. In the present invention and this specification, the term "methacrylate" refers to a group containing only methacryloyl groups as (meth)acryloyl groups, and a group containing both acryloyl and methacryloyl groups as (meth)acryloyl groups is referred to as an acrylate. Unless otherwise specified, the groups described may be substituted or unsubstituted. When a group has a substituent, examples of the substituent include an alkyl group (e.g., an alkyl group having 1 to 6 carbon atoms), a hydroxy group, an alkoxy group (e.g., an alkoxy group having 1 to 6 carbon atoms), a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom), a cyano group, an amino group, a nitro group, an acyl group, a carboxy group, an aryl group, and a polyether group. Furthermore, the "number of carbon atoms" of a substituted group refers to the number of carbon atoms in the portion excluding the substituent.

[0032] A (meth)acrylate-based polymerizable composition, which is one embodiment of the polymerizable composition for forming a photochromic layer, will be described below. However, the following embodiment is merely an example, and the present invention is not limited to this example.

[0033] In one embodiment, the polymerizable composition for forming a photochromic layer can be a (meth)acrylate-based polymerizable composition containing one or more polymerizable compounds selected from the group consisting of the following component A, the following component B, and the following component C:

[0034] (Component A) Component A is a polyfunctional (meth)acrylate containing a polyalkylene glycol moiety and having a molecular weight of 500 or more. In the present invention and this specification, the term "polyalkylene glycol moiety" refers to a polyfunctional (meth)acrylate represented by the following formula 2: In Formula 2, R represents an alkylene group, n represents the number of repeating alkoxy groups represented by RO and is 2 or more. * indicates the bonding position where the partial structure represented by Formula 2 is bonded to an adjacent atom. The number of carbon atoms in the alkylene group represented by R can be 1 or more or 2 or more, and can be, for example, 5 or less or 4 or less. Specific examples of the alkylene group represented by R include an ethylene group, a propylene group, and a tetramethylene group. n is 2 or more and can be, for example, 30 or less, 25 or less, or 20 or less. In one embodiment, Component A can have the above partial structure in which R represents an ethylene group, i.e., a polyethylene glycol moiety. In another embodiment, Component A can have the above partial structure in which R represents a propylene group, i.e., a polypropylene glycol moiety.

[0035] The molecular weight of component A is 500 or more. In the present invention and this specification, the molecular weight of the multimer is determined by the structural formula determined by structural analysis of the compound or the theoretical molecular weight calculated from the raw material charging ratio during production. The molecular weight of component A is 500 or more, preferably 510 or more, more preferably 520 or more, preferably 550 or more, more preferably 570 or more, even more preferably 600 or more, even more preferably 630 or more, and even more preferably 650 or more. From the viewpoint of increasing the hardness of the photochromic layer, the molecular weight of component A is preferably, for example, 2000 or less, 1500 or less, 1200 or less, 1000 or less, or 800 or less.

[0036] Component A is a polyfunctional (meth)acrylate, and may be, for example, a difunctional, trifunctional, tetrafunctional, or pentafunctional (meth)acrylate, and is preferably a difunctional or trifunctional (meth)acrylate. Component A may contain only acryloyl groups, only methacryloyl groups, or both acryloyl groups and methacryloyl groups as (meth)acryloyl groups. That is, Component A may be an acrylate or methacrylate.

[0037] In one embodiment, component A can be an acyclic polyfunctional (meth)acrylate. In the present invention and this specification, "acyclic" means not containing a cyclic structure. In contrast, "cyclic" means containing a cyclic structure. An acyclic polyfunctional (meth)acrylate refers to a bifunctional or higher functional (meth)acrylate that does not contain a cyclic structure. A specific example of such component A is a polyalkylene glycol di(meth)acrylate represented by the following formula 3.

[0038]

[0039] In formula 3, R 1 and R 2 each independently represents a hydrogen atom or a methyl group, R represents an alkylene group, and n represents the number of repetitions of the alkoxy group represented by RO, and is 2 or more. R and n are as described above for the partial structure represented by Formula 2. The polyalkylene glycol di(meth)acrylate represented by Formula 3 may contain only acryloyl groups, only methacryloyl groups, or both acryloyl groups and methacryloyl groups as the (meth)acryloyl group. Specific examples of the polyalkylene glycol di(meth)acrylate represented by Formula 3 include polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, and polytetramethylene glycol di(meth)acrylate.

[0040] Specific examples of component A include tri(meth)acrylates represented by the following formula 4. The tri(meth)acrylates represented by formula 4 may contain only acryloyl groups, only methacryloyl groups, or both acryloyl and methacryloyl groups as (meth)acryloyl groups.

[0041]

[0042] In formula 4, R 40 , R 41 , R 44 , R 45 , R 47 and R 48 each independently represents an alkylene group; R 43 represents an alkyl group, and R 42 , R 46 and R 49 each independently represents a hydrogen atom or a methyl group. 41 n2 represents the number of repeating alkoxy groups represented by the formula: 45 n3 represents the number of repeating alkoxy groups represented by the formula: 48 The number of repetitions of the alkoxy group represented by the formula (I) is 2 or more.

[0043] Equation 4 will be explained in more detail below.

[0044] R in Formula 4 41 , R 45 and R 48 In Formula 4, n1, n2, and n3 are as described above for n in Formula 2. In Formula 4, R 41 , R 45 and R 48 may be the same, or two or three may be different. This also applies to n1, n2, and n3.

[0045] R 42 , R 46 and R 49each independently represents a hydrogen atom or a methyl group. The tri(meth)acrylate represented by Formula 4 may contain only acryloyl groups, only methacryloyl groups, or both acryloyl groups and methacryloyl groups as (meth)acryloyl groups.

[0046] R 43 The number of carbon atoms in the alkyl group represented by R may be 1 or more, or 2 or more, and may be, for example, 5 or less, or 4 or less. 43 The alkyl group represented by R can be a linear alkyl group or a branched alkyl group. 43 Specific examples of the alkyl group represented by the formula include a methyl group and an ethyl group.

[0047] R 40 , R 44 and R 47 each independently represents an alkylene group. The number of carbon atoms in such an alkylene group may be 1 or more or 2 or more, and may be, for example, 5 or less or 4 or less. Specific examples thereof include an ethylene group, a propylene group, and a tetramethylene group.

[0048] Specific examples of the tri(meth)acrylate represented by formula 4 include trimethylolpropane polyoxyethylene ether tri(meth)acrylate.

[0049] Monofunctional (meth)acrylates From the viewpoint of increasing the (meth)acryloyl group content of a polymerizable composition containing a (meth)acrylate, (meth)acrylates having a high proportion of (meth)acryloyl groups in the molecule are preferred. From this viewpoint, low-molecular-weight monofunctional (meth)acrylates are preferred, and monofunctional (meth)acrylates having a molecular weight of 150 or less are more preferred. Monofunctional (meth)acrylates having a molecular weight of 150 or less may be cyclic monofunctional (meth)acrylates or acyclic monofunctional (meth)acrylates. Specific examples of cyclic monofunctional (meth)acrylates having a molecular weight of 150 or less include glycidyl (meth)acrylate. Specific examples of acyclic monofunctional (meth)acrylates having a molecular weight of 150 or less include n-butyl (meth)acrylate. The molecular weight of monofunctional (meth)acrylates having a molecular weight of 150 or less may be, for example, 100 or more, but is not limited thereto.

[0050] Polyfunctional (meth)acrylates As described above, from the viewpoint of increasing the (meth)acryloyl group content of a polymerizable composition containing a (meth)acrylate, (meth)acrylates having a high proportion of (meth)acryloyl groups in the molecule are preferred. From this viewpoint, polyfunctional (meth)acrylates having a lower molecular weight than Component A are also preferred. As such polyfunctional (meth)acrylates, polyfunctional (meth)acrylates having a higher functionality than the polyfunctional (meth)acrylate used as Component A are also preferred. The molecular weight of such polyfunctional (meth)acrylates is preferably less than 500, 400 or less, 300 or less, or 200 or less. The molecular weight can be, for example, 100 or more, but is not limited thereto. Furthermore, such polyfunctional (meth)acrylates can be, for example, polyfunctional (meth)acrylates having 10 or more functionalities (e.g., 10 or more and 15 or less). Specific examples include poly[(3-methacryloyloxypropyl)silsesquioxane] derivatives described in the Examples section below.

[0051] Examples of (meth)acrylates that can be contained in the (meth)acrylate-based polymerizable composition, which is the polymerizable composition for forming a photochromic layer, include a monofunctional (meth)acrylate represented by the following formula 1 (hereinafter also referred to as "component B") and a bifunctional (meth)acrylate represented by the following formula 5 (hereinafter also referred to as "component C"). In one embodiment, the (meth)acrylate-based polymerizable composition can be a polymerizable composition containing one or more (meth)acrylates selected from the group consisting of a monofunctional (meth)acrylate represented by the following formula 1 and a bifunctional (meth)acrylate represented by the following formula 5. In another embodiment, the (meth)acrylate-based polymerizable composition can be a polymerizable composition that does not contain one or more (meth)acrylates selected from the group consisting of a monofunctional (meth)acrylate represented by the following formula 1 and a bifunctional (meth)acrylate represented by the following formula 5. In one embodiment, the (meth)acrylate-based polymerizable composition can also contain component B as a monofunctional (meth)acrylate having a molecular weight of 150 or less.

[0052] (Component B) Component B is a monofunctional (meth)acrylate represented by the following formula 1.

[0053]

[0054] Formula 1 will be explained in more detail below.

[0055] In formula 1, R 10 represents a hydrogen atom or a methyl group. The monofunctional (meth)acrylate represented by Formula 1 may be an acrylate or a methacrylate.

[0056] R 11 R represents a linear alkyl group having 3 or more carbon atoms or a branched alkyl group having 3 or more carbon atoms. These alkyl groups may be unsubstituted or may have a substituent. The substituent is not particularly limited, and examples thereof include the various substituents described above. 11The number of carbon atoms in the linear or branched alkyl group represented by the formula (I) is 3 or more, preferably 4 or more, more preferably 5 or more, and further preferably 6 or more, 7 or more, 8 or more, 9 or more, 10 or more, and 11 or more in that order. On the other hand, from the viewpoint of the solubility of the photochromic compound in the composition, the number of carbon atoms is preferably 15 or less, more preferably 14 or less, and further preferably 13 or less, and 12 or less in that order.

[0057] The molecular weight of the monofunctional (meth)acrylate represented by Formula 1 can be, for example, 100 or more, and can be, for example, 300 or less. However, it is not limited to the above range. As described above, in one embodiment, the monofunctional (meth)acrylate represented by Formula 1 can be a monofunctional (meth)acrylate having a molecular weight of 150 or less. Specific examples of the monofunctional (meth)acrylate represented by Formula 1 include n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isodecyl (meth)acrylate, and n-lauryl (meth)acrylate.

[0058] (Component C) Component C is a compound represented by the following formula 5: It is a (meth)acrylate represented by the formula:

[0059] In formula 5, R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and m represents an integer of 1 or greater. m is 1 or greater and can be, for example, 10 or less, 9 or less, 8 or less, 7 or less, or 6 or less.

[0060] The molecular weight of component C can be, for example, 400 or less, and from the viewpoint of further increasing the color density of the photochromic layer, it is preferably 350 or less, more preferably 300 or less, and even more preferably 250 or less. The molecular weight of component C can be, for example, 100 or more, 150 or more, or 200 or more.

[0061] Component C may contain only acryloyl groups, only methacryloyl groups, or both acryloyl groups and methacryloyl groups as (meth)acryloyl groups. Specific examples of Component C include 1,9-nonanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and 1,10-decanediol di(meth)acrylate.

[0062] In the (meth)acrylate polymerizable composition, the content of component A is preferably 50% by mass or more, more preferably 55% by mass or more, and even more preferably 60% by mass or more, based on 100% by mass of the total amount of polymerizable compounds contained in the composition. In one embodiment, component A may be the component that accounts for the largest proportion of the multiple polymerizable compounds contained in the composition. Furthermore, the content of component A may be 90% by mass or less, 85% by mass or less, or 80% by mass or less, based on 100% by mass of the total amount of polymerizable compounds contained in the composition. In one embodiment, the composition may contain only one type of component A, or in another embodiment, two or more types. When two or more types of component A are contained, the content of component A above is the total content of the two or more types. This also applies to the contents of other components in the present invention and this specification.

[0063] The (meth)acrylate polymerizable composition may contain the various (meth)acrylates in an amount such that the (meth)acryloyl group content of the composition is 3.50 mmol / g or more. For example, the (meth)acrylate polymerizable composition preferably contains 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more of a monofunctional (meth)acrylate having a molecular weight of 150 or less, based on 100% by mass of the total amount of polymerizable compounds contained in the composition. Furthermore, the content of the monofunctional (meth)acrylate having a molecular weight of 150 or less is preferably 30% by mass or less, more preferably 25% by mass or less, based on 100% by mass of the total amount of polymerizable compounds contained in the composition.

[0064] From the viewpoint of improving the weather resistance of the photolayer, the (meth)acryloyl group content of the (meth)acrylate polymerizable composition is preferably 3.50 mmol / g or more, more preferably 3.55 mmol / g or more, even more preferably 3.60 mmol / g or more, even more preferably 3.65 mmol / g or more, even more preferably 3.70 mmol / g or more, and even more preferably 3.75 mmol / g or more. The (meth)acryloyl group content of the (meth)acrylate polymerizable composition can be, for example, 5.00 mmol / g or less, 4.50 mmol / g or less, or 4.00 mmol / g or less, or may exceed the values ​​exemplified here.

[0065] The "(meth)acryloyl group content" of a polymerizable composition containing a (meth)acrylate is calculated as follows: The total amount of (meth)acrylates contained in the polymerizable composition is set to "1" by mass, and the content of each (meth)acrylate is calculated. For each (meth)acrylate, the "(meth)acryloyl group content x the above content" is calculated. The sum of the values ​​thus calculated for all (meth)acrylates contained in the polymerizable composition is the (meth)acryloyl group content of the polymerizable composition.

[0066] For example, the photochromic compound contained in the photochromic layer undergoes a structural change upon irradiation with light such as sunlight, passing through an excited state. The structure after structural change upon light irradiation can be called a "colored body." In contrast, the structure before light irradiation can be called a "colorless body." Note that "colorless" in the colorless body does not necessarily mean completely colorless, but also encompasses a case where the color is lighter than the colored body. After structural change to a colored body upon light irradiation, the faster the rate of structural change from the colored body to the colorless body, the faster the fading rate. In the photochromic layer, the easier the molecular movement of the photochromic compound in the matrix formed by the polymerization reaction of the polymerizable compound is thought to be the faster the rate of the structural change. From the perspective of accelerating this rate, a flexible matrix is ​​considered desirable. In relation to the above points, it is presumed that component A can contribute to making the matrix flexible. Specifically, the molecular weight of component A being 500 or more and the presence of a polyalkylene glycol moiety in component A are thought to be the reasons why a flexible matrix can be formed by component A. Furthermore, the (meth)acryloyl group content of 3.50 mmol / g or more in the (meth)acrylate polymerizable composition is thought to contribute to the formation of a rigid polymer network between molecules in a matrix formed from such a composition. In a matrix having a rigid polymer network, the diffusion of active species that can cause a decrease in weather resistance can be suppressed, which is presumably the reason why the (meth)acrylate polymerizable composition can form a photochromic layer with excellent weather resistance.

[0067] The content of the polymerizable compound in the (meth)acrylate polymerizable composition (when multiple polymerizable compounds are included, the total content of these compounds) can be, for example, 80% by mass or more, 85% by mass or more, or 90% by mass or more, based on 100% by mass of the total amount of the composition. Furthermore, the content of the polymerizable compound in the (meth)acrylate polymerizable composition can be, for example, 99% by mass or less, 95% by mass or less, 90% by mass or less, or 85% by mass or less, based on 100% by mass of the total amount of the composition. The (meth)acrylate polymerizable composition may or may not contain a solvent. When a solvent is included, any solvent can be used in any amount as long as it does not inhibit the polymerization reaction of the polymerizable composition.

[0068] <<Photochromic Compound>> The composition contains a photochromic compound in addition to the polymerizable compound. Known compounds exhibiting photochromic properties can be used as the photochromic compound contained in the composition. The photochromic compound can exhibit photochromic properties, for example, when exposed to ultraviolet light. Examples of photochromic compounds include compounds having known photochromic skeletons, such as azobenzenes, spiropyrans, spirooxazines, naphthopyrans, indenonaphthopyrans, phenanthropyrans, hexaarylbisimidazoles, donor-acceptor Stenhouse adducts (DASA), salicylideneanilines, dihydropyrenes, anthracene dimers, fulgides, diarylethenes, phenoxynaphthacenequinones, and stilbenes. Preferred photochromic compounds include fulgimide compounds, spirooxazine compounds, chromene compounds, and indeno-fused naphthopyran compounds. The photochromic compound may also be one or more compounds selected from the group consisting of photochromic compounds represented by general formula A, photochromic compounds represented by general formula B, and photochromic compounds represented by general formula C, as described in WO 2022 / 138966. The photochromic compounds may be used alone or in combination of two or more. The content of the photochromic compound in the composition may be, for example, about 0.1 to 15% by mass, with the total amount of the composition being 100% by mass, but is not limited to this range.

[0069] <<Other Components>> In addition to the polymerizable compound and the photochromic compound, the polymerizable composition for forming a photochromic layer may contain one or more of the various additives that may typically be contained in a polymerizable composition, at any content. Examples of additives that may be contained in the polymerizable composition for forming a photochromic layer include a polymerization initiator for promoting the polymerization reaction. The above description of the polymerization initiator can be referenced. The content of the polymerization initiator may be, for example, in the range of 0.1 to 5.0% by mass, with the total amount of the composition being 100% by mass.

[0070] The polymerizable composition for forming a photochromic layer may further contain any amount of known additives that are typically added to compositions containing a photochromic compound, such as surfactants, antioxidants, radical scavengers, light stabilizers, ultraviolet absorbers, color inhibitors, antistatic agents, fluorescent dyes, dyes, pigments, fragrances, plasticizers, and silane coupling agents. Known compounds may be used as these additives.

[0071] The polymerizable composition for forming a photochromic layer can be prepared by mixing the various components described above simultaneously or sequentially in any order.

[0072] The photochromic layer can be formed by applying a photochromic layer-forming polymerizable composition onto the primer layer and then curing the applied composition. The application method is described above. The curing treatment can be light irradiation and / or heat treatment, with light irradiation being preferred from the viewpoint of progressing the curing reaction in a short period of time. The curing treatment conditions can be determined based on the types of various components (such as the polymerizable compound and polymerization initiator described above) contained in the photochromic layer-forming polymerizable composition and the composition of the composition. The thickness of the photochromic layer thus formed is preferably in the range of, for example, 5 to 80 μm, and more preferably in the range of 20 to 60 μm. It is believed that the curing treatment here promotes the reaction of the (meth)acryloyl group of the polymer contained in the primer layer, thereby forming a bond between the photochromic layer and the primer layer.

[0073] The photochromic article having the above-mentioned photochromic layer may or may not further have one or more functional layers in addition to the various layers described above. Examples of functional layers include protective layers for improving durability, hard coat layers, anti-reflection layers, water-repellent or hydrophilic antifouling layers, anti-fogging layers, and other layers known as functional layers for optical articles. For example, for the protective layer, see paragraphs 0009 to 0021, 0026 of JP 2021-107909 A and the descriptions in the Examples of the same publication.

[0074] <Heat Treatment> A laminate having a primer layer and a photochromic layer formed on a substrate can be subjected to heat treatment before or after the formation of the functional layer. The heat treatment performed here dissociates the blocking agent of the blocked isocyanate, regenerating the isocyanate group. It is presumed that the regenerated isocyanate, together with the hydroxyl group of the polymer, can contribute to the formation of a bond between the substrate and the primer layer. The heat treatment may be performed at a temperature equal to or higher than the dissociation temperature of the blocking agent contained in the blocked isocyanate.

[0075] The photochromic article can be an optical article, and one example of the optical article is a spectacle lens. Other examples of the optical article include a goggle lens, a sun visor visor, and a helmet shield. A photochromic layer-forming polymerizable composition is applied to a substrate for such an optical article via a primer layer, and the applied composition is cured to form a photochromic layer, thereby obtaining an optical article with antiglare properties.

[0076] [Eyeglasses] One aspect of the present invention relates to eyeglasses equipped with eyeglass lenses, which are one form of the photochromic article. Details of the eyeglass lenses included in the eyeglasses are as described above. By including such eyeglass lenses, the eyeglasses can, for example, exhibit an anti-glare effect like sunglasses outdoors by coloring the photochromic compound included in the photochromic layer when exposed to sunlight, and regain their transparency when returning indoors by fading the photochromic compound. Known technologies can be applied to the construction of the frames and other components of the eyeglasses.

[0077] [Method for manufacturing a photochromic article] One aspect of the present invention relates to a method for manufacturing a photochromic article, comprising: applying a polymer composition for forming a primer layer onto a substrate to form a primer layer; forming a photochromic layer containing a photochromic compound on the formed primer layer, wherein the polymer composition for forming a primer layer contains a polymer having a hydroxy group and a (meth)acryloyl group, and a blocked isocyanate; and further comprising heat-treating the laminate obtained by forming the photochromic layer.

[0078] According to the above-mentioned manufacturing method, a photochromic article having excellent adhesion between the substrate and the photochromic layer can be manufactured. For details of the above-mentioned manufacturing method, please refer to the above description.

[0079] The present invention will be further described below with reference to examples, although the present invention is not limited to the embodiments shown in the examples.

[0080] <Substrate> The various substrates described below are plastic lens substrates as described below. In all substrates, the object-side surface is convex and the eyeball-side surface is concave. Substrate 4 (refractive index 1.59) is a substrate with hard coat layers on both sides, and the polymer composition for forming a primer layer described below was applied to the hard coat layer surface. Substrate 1: refractive index 1.50 (diethylene glycol bisallyl carbonate resin (CR-39)) Substrate 2: refractive index 1.53 (urea resin) Substrate 3: refractive index 1.55 (diallyl phthalate resin) Substrate 4: refractive index 1.59 (polycarbonate resin) Substrate 5: refractive index 1.60 (urethane resin) Substrate 6: refractive index 1.67 (thiourethane resin)

[0081] Examples 1 to 6 Preparation of Spectacle Lenses (Photochromic Articles) A ​​plastic lens substrate was immersed in a 10% by weight aqueous solution of sodium hydroxide (liquid temperature: 60°C) for 5 minutes, then washed with pure water and dried. A primer layer was then formed on the convex surface (object-side surface) of the plastic lens substrate. Specifically, the components shown in Table 1 were mixed together, and the resulting mixture was thoroughly stirred and degassed using a rotation-revolution type stirring and degassing device. The resulting primer layer-forming polymer composition was stored at room temperature for one week, then applied by spin coating to the convex surface of a plastic lens substrate shown in Table 3 at a temperature of 25°C and a relative humidity of 50%, followed by air drying for five minutes in the same environment to form a primer layer. The formed primer layer had a thickness of 4 μm. The viscosity of the primer layer-forming polymer composition after one week of storage was the same as that before storage. A photochromic layer-forming polymerizable composition ((meth)acryloyl group content: 3.61 mmol / g) prepared as follows was applied by spin coating to the primer layer. Spin coating was performed using the method described in JP 2005-218994 A. The photochromic layer-forming polymerizable composition coated on the primer layer was then irradiated with ultraviolet light (wavelength 405 nm) in a nitrogen atmosphere (oxygen concentration 500 ppm or less), curing the composition to form a photochromic layer. The thickness of the formed photochromic layer was 40 μm. A protective layer was formed on the thus-formed photochromic layer using the method described in Example 1 of JP 2021-107909 A. The thickness of the formed protective layer was 15 μm. The laminate in which the primer layer, photochromic layer, and protective layer were formed in this order on the substrate was then heat-treated for 2 hours in a heating furnace at an atmospheric temperature of 90°C. In this way, a spectacle lens having the substrate, primer layer, photochromic layer, and protective layer in this order was produced.

[0082]

[0083] (Preparation of Polymerizable Composition for Forming Photochromic Layer) The components shown in Table 2 were mixed in the amounts shown in Table 2 in a plastic container. The resulting mixture of polymerizable compounds was mixed with the following photochromic compound (an indeno-fused naphthopyran compound represented by the structural formula described in U.S. Pat. No. 6,296,785), a photoradical polymerization initiator (bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad 819, manufactured by IGM Resin B.V.)), an antioxidant (bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionic acid][ethylenebis(oxyethylene)]), and a light stabilizer (bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate) and thoroughly stirred. The mixture was then degassed using a rotation-revolution type stirring and degassing apparatus. A polymerizable composition for forming a photochromic layer was thus prepared. The contents of the above components, relative to the total amount of the composition taken as 100% by mass, are 94.9% by mass for the mixture of polymerizable compounds, 3% by mass for the photochromic compound, 0.3% by mass for the photoradical polymerization initiator, 0.9% by mass for the antioxidant, and 0.9% by mass for the light stabilizer.

[0084]

[0085]

[0086] Comparative Example 1 A polymer composition for forming a primer layer was prepared by the method described in Example 1, except that biuret-type triisocyanate in which the isocyanate groups were not protected with a blocking agent was used instead of the blocked isocyanate. When the prepared polymer composition for forming a primer layer was stored in a room temperature environment for one week, the viscosity significantly increased compared to before storage, and the composition could not be used for application by spin coating.

[0087] [Adhesion Evaluation] Three eyeglass lenses were produced for each of Examples 1 to 6. Adhesion of each produced eyeglass lens was evaluated by the cross-cut method in accordance with JIS K5600-5-6:1999. The number of remaining squares per 100 total squares is shown in Table 3. If the number of remaining squares is 99 or more, it can be said that the adhesion is excellent. The results shown in Table 3 confirm that each of the eyeglass lenses of Examples 1 to 6 has excellent adhesion between the substrate and the photochromic layer.

[0088]

[0089] Two or more of the various aspects and configurations described herein may be combined in any combination.

[0090] The embodiments disclosed herein should be considered to be illustrative in all respects and not restrictive. The scope of the present invention is defined by the claims, not by the above description, and is intended to include all modifications within the meaning and scope of the claims.

[0091] The present invention is useful in the technical fields of eyeglasses, goggles, sun visors, helmets, etc.

Claims

1. A photochromic article comprising, in this order, a substrate, a primer layer formed from a polymer composition for forming a primer layer, and a photochromic layer containing a photochromic compound, wherein the polymer composition for forming a primer layer contains a polymer having a hydroxy group and a (meth)acryloyl group, and a blocked isocyanate.

2. The photochromic article of claim 1, wherein said polymer is a (meth)acrylic polymer.

3. The photochromic article according to claim 1, wherein the photochromic layer is a cured layer obtained by curing a (meth)acrylate-based polymerizable composition containing a photochromic compound.

4. The photochromic article according to claim 2, wherein the photochromic layer is a cured layer obtained by curing a (meth)acrylate-based polymerizable composition containing a photochromic compound.

5. The photochromic article according to any one of claims 1 to 4, which is a lens for glasses, a lens for goggles, a visor portion of a sun visor, or a shield member for a helmet.

6. The photochromic article of claim 5 which is a spectacle lens.

7. Eyeglasses comprising the eyeglass lens according to claim 6.

8. A method for producing a photochromic article, comprising: applying a polymer composition for forming a primer layer onto a substrate to form a primer layer; and forming a photochromic layer containing a photochromic compound on the formed primer layer, wherein the polymer composition for forming a primer layer comprises: a polymer having a hydroxy group and a (meth)acryloyl group; and a blocked isocyanate; and further comprising: heat-treating a laminate obtained by forming the photochromic layer.

9. The method of making a photochromic article according to claim 8, wherein the polymer is a (meth)acrylic polymer.

10. A method for producing a photochromic article according to claim 8, comprising forming the photochromic layer by curing a (meth)acrylate-based polymerizable composition containing a photochromic compound.

11. A method for producing the photochromic article of claim 9, comprising forming the photochromic layer by curing a (meth)acrylate-based polymerizable composition containing a photochromic compound.

12. The method for producing a photochromic article according to any one of claims 8 to 11, wherein the photochromic article is a spectacle lens, a goggle lens, a visor portion of a sun visor, or a shield member of a helmet.

Citation Information

Patent Citations

  • Coating method and method for manufacturing glasses-lens

    JP2005218994A

  • Polymerizable composition for forming protective layer of photochromic article, photochromic article and spectacles

    JP2021107909A

  • Laminates, optical components, methods for manufacturing them, and coating liquids

    JP4405833B2

  • Indeno-fused photochromic naphthopyrans

    US6296785B1

  • Photochromic composition, photochromic article, and spectacles

    WO2022138966A1