Reinforcing film, optical member, and electronic member

The reinforcing film with a specific adhesive layer composition addresses the challenge of initial low adhesive strength and flexibility in flexible electronic devices by providing easy releasability and high adhesive strength, ensuring effective adhesion and handling in flexible electronic devices and optical components.

WO2024203752A1PCT designated stage expired Publication Date: 2024-10-03NITTO DENKO CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011107
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional adhesive sheets used in flexible electronic devices exhibit low initial adhesive strength that increases significantly over time, posing challenges in handling and flexibility, particularly in repeated bending and bending applications.

Method used

A reinforcing film with an adhesive layer composed of a polymer (A) containing nitrogen-containing monomer units and a polymer (B) with a polyorganosiloxane skeleton, along with a zirconium-containing compound, which provides easy releasability initially and high adhesive strength after heating, ensuring flexibility and strong adhesion.

Benefits of technology

The solution enables a reinforcing film that maintains flexibility suitable for repeated bending while achieving high adhesive strength, suitable for flexible electronic devices and optical components, with improved ease of handling and reworkability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011107_03102024_PF_FP_ABST
    Figure JP2024011107_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a reinforcing film comprising an adhesive layer that includes a polymer (A) and a polymer (B). The polymer (B) contains a monomer unit that has a polyorganosiloxane skeleton and a (meth)acrylic monomer unit. The polymer (A) is an acrylic polymer containing a monomer unit derived from a nitrogen-containing monomer. The amount WN [parts by weight] of the monomer unit derived from the nitrogen-containing monomer contained in 100 parts by weight of the polymer (A) is 14 parts by weight or less. The adhesive layer further contains a zirconium-containing compound in an amount of WZr [parts by weight] with respect to 100 parts by weight of the polymer (A), and has a ratio (WN / WZr) of at least 4.
Need to check novelty before this filing date? Find Prior Art

Description

Reinforcing films, optical and electronic components

[0001] The present invention relates to a reinforcing film and an optical component and an electronic component to which the reinforcing film is attached. This application claims priority to Japanese Patent Application No. 2023-050192, filed on March 27, 2023, the entire contents of which are incorporated herein by reference.

[0002] Pressure-sensitive adhesives in the form of pressure-sensitive adhesive sheets are widely used in various applications, such as for bonding adherends to each other or for fixing articles to adherends, in portable electronic devices such as mobile phones, smartphones, and tablet PCs, as well as other electronic devices. For example, pressure-sensitive adhesive sheets are used as reinforcing materials (reinforcing films) that impart rigidity and impact resistance to optical components, electronic components, and the like that make up the above-mentioned devices. Patent Documents 1 and 2 disclose this type of prior art.

[0003] Furthermore, in recent years, portable electronic devices that can be bent or rolled have been attracting attention, and the development of adhesive sheets that can be used for fixing flexible devices (typically image display devices such as organic EL and liquid crystal display devices) built into such electronic devices has been progressing (Patent Documents 3 to 6).

[0004] Meanwhile, looking at the performance of adhesives, recently, a pressure-sensitive adhesive sheet has been proposed that exhibits low adhesive strength when initially attached to an adherend, but can subsequently increase significantly in adhesive strength (Patent Document 7). Pressure-sensitive adhesive sheets with such properties exhibit reworkability (reworkability), which is useful for preventing yield losses due to incorrect or failed application of the pressure-sensitive adhesive sheet, before the increase in adhesive strength, and can exhibit strong adhesive strength suitable for the intended use of the pressure-sensitive adhesive sheet after the increase in adhesive strength.

[0005] Japanese Patent No. 6366199 Japanese Patent No. 6366200 Japanese Patent No. 6376271 Japanese Patent Application Publication No. 2016-108555 Japanese Patent Application Publication No. 2017-095657 Japanese Patent Application Publication No. 2017-095659 Japanese Patent No. 6373458

[0006] The reinforcing film can also be used in the flexible device. For example, in the production of the flexible device, the components constituting the device are often thin, so it is desirable to reinforce the device by attaching a pressure-sensitive adhesive sheet as a reinforcing film to prevent defects caused by deformation and improve handleability. Flexible devices can be repeatedly folded or bent, so the pressure-sensitive adhesive constituting the reinforcing film used in flexible devices is required to have flexibility that allows it to conform well to the adherend even in such usage modes. Pressure-sensitive adhesives having such flexibility and reinforcing films comprising the pressure-sensitive adhesive can be used in various applications, including flexible devices, and are therefore useful with few limitations on the range of application.

[0007] For example, even for adhesives that exhibit low adhesive strength initially after application but subsequently increase significantly, as proposed in Patent Document 7, when used as a reinforcing film, it is desirable for the adhesive to have flexibility suitable for repeated folding and bending. One method for achieving this is to appropriately set the storage modulus of the adhesive at low temperatures. However, in adhesives designed to increase in adhesive strength as described above, changing the storage modulus at low temperatures affects both the initial low adhesive strength and the adhesive strength after increase. It would be practically useful to be able to improve the flexibility of adhesives that exhibit low adhesive strength initially after application but subsequently increase significantly in adhesive strength.

[0008] The present invention has been made in view of the above circumstances, and aims to provide a reinforcing film having an adhesive that exhibits easy peelability in the initial stage after being attached to an adherend, and that is capable of significantly increasing adhesive strength thereafter and exhibits good flexibility. Another aim of the present invention is to provide an optical element or an electronic element to which the reinforcing film is attached.

[0009] According to the present specification, there is provided a reinforcing film including a pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer includes a polymer (A) and a polymer (B). The polymer (B) includes a monomer unit having a polyorganosiloxane skeleton and a (meth)acrylic monomer unit. The polymer (A) is an acrylic polymer including a monomer unit derived from a nitrogen-containing monomer, and the amount W of the monomer unit derived from the nitrogen-containing monomer contained in 100 parts by weight of the polymer (A) is N The adhesive layer contains 100 parts by weight of the polymer (A) and 14 parts by weight of the polymer (B). Zr [parts by weight] of a zirconium-containing compound. Zr [Parts by weight] N [weight parts] ratio (W N / W Zr ) is 4 or more.

[0010] According to the reinforcing film of the above configuration, the pressure-sensitive adhesive layer contains the polymer (A) and the polymer (B) containing the monomer unit having a polyorganosiloxane skeleton, so that it exhibits easy peelability at the initial stage after being attached to the adherend, and thereafter, the adhesive strength can be significantly increased. In addition, the amount W of the monomer unit derived from the nitrogen-containing monomer contained per 100 parts by weight of the polymer (A) is N By limiting the [parts by weight] to 14 parts by weight or less, the pressure-sensitive adhesive layer exhibits flexibility suitable for repeated bending and flexing. Zr [Parts by weight] N [weight parts] ratio (W N / W Zr ) is 4 or more, so that W N By limiting the amount of the adhesive to 14 parts by weight or less, it is possible to achieve both easy initial releasability and high adhesive strength after the adhesive strength has increased.

[0011] In some embodiments of the technology disclosed herein (including reinforcing films, optical components, electronic components, pressure-sensitive adhesives used therein, and pressure-sensitive adhesive compositions for forming the pressure-sensitive adhesives; the same applies hereinafter), the pressure-sensitive adhesive layer contains a crosslinking agent. Use of a crosslinking agent allows the cohesive strength of the pressure-sensitive adhesive layer to be appropriately adjusted. Here, "containing a crosslinking agent" means containing the crosslinking agent in a form after a crosslinking reaction.

[0012] In some embodiments, the content of the polymer (B) in the pressure-sensitive adhesive layer is 0.1 to 10 parts by weight per 100 parts by weight of the polymer (A). By setting the amount of polymer (B) to 0.1 parts by weight or more per 100 parts by weight of polymer (A), easy peelability at the initial stage of application is likely to be achieved. By setting the amount of polymer (B) to 10 parts by weight or less, high adhesive strength after adhesive strength increase is likely to be achieved. Furthermore, by setting the amount of polymer (B) used within the above range, it is easy to achieve both low initial adhesive strength, high adhesive strength after adhesive strength increase, and good flexibility (e.g., low storage modulus at low temperatures).

[0013] In some embodiments, the polymer (A) contains a monomer unit derived from a monomer having a nitrogen atom-containing ring as the monomer unit derived from the nitrogen-containing monomer. The polymer (A) containing the monomer unit derived from the monomer having a nitrogen atom-containing ring is likely to provide a high post-rise adhesive strength.

[0014] In some preferred embodiments, the reinforcing film has an adhesive strength (initial adhesive strength) N1 of 200 gf / 25 mm or less after being attached to a polyimide film and 30 minutes have elapsed at 23° C. A reinforcing film having an initial adhesive strength N1 of 200 gf / 25 mm or less can exhibit good easy peelability suitable for rework, etc., in the early stages after being attached to an adherend.

[0015] In some preferred embodiments, the reinforcing film has an adhesive strength (post-heating adhesive strength) N2 of 1000 gf / 25 mm or more after being attached to a polyimide film and heated at 60° C. for 1 hour, and then left at 23° C. for 30 minutes. A reinforcing film having a post-heating adhesive strength N2 of 1000 gf / 25 mm or more can exhibit high adhesive strength after the adhesive strength has increased.

[0016] In some preferred embodiments, the reinforcing film has an adhesive strength N2 [gf / 25 mm] after being attached to a polyimide film and heated at 60° C. for 1 hour and then left at 23° C. for 30 minutes, which shows an increase rate [%] of 900% or more, relative to the adhesive strength N1 [gf / 25 mm] after being attached to a polyimide film and left at 23° C. for 30 minutes. A reinforcing film with an adhesive strength increase rate (N2 / N1) of 900% or more exhibits easy peelability suitable for rework, etc., at the initial stage of attachment, and can greatly increase its adhesive strength by subsequent heating, etc.

[0017] In some preferred embodiments, the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer has a storage modulus (G' -20 ) is 1000 kPa or less. A pressure-sensitive adhesive having such a low storage modulus at -20°C exhibits high flexibility suitable for repeated bending and flexing.

[0018] The reinforcing film disclosed herein is suitable as a reinforcing film that imparts rigidity and impact resistance to optical members such as polarizing plates, wavelength plates, etc. during processing or transport of the optical members. Therefore, this specification provides an optical member to which any of the reinforcing films disclosed herein is attached.

[0019] The reinforcing film disclosed herein is also suitable as a reinforcing film for electronic components of devices such as portable electronic devices, etc. Therefore, according to the present specification, there is provided an electronic component to which any of the reinforcing films disclosed herein is attached.

[0020] Appropriate combinations of the elements described in this specification may also be included within the scope of the invention for which patent protection is sought by this application.

[0021] Fig. 1 is a cross-sectional view schematically showing the configuration of a reinforcing film according to one embodiment; Fig. 2 is a cross-sectional view schematically showing the configuration of a reinforcing film according to another embodiment; Fig. 3 is a cross-sectional view schematically showing the configuration of a reinforcing film according to another embodiment.

[0022] Preferred embodiments of the present invention are described below. Matters necessary for carrying out the present invention other than those specifically mentioned in this specification can be understood by those skilled in the art based on the teachings for carrying out the invention described in this specification and the common general technical knowledge at the time of filing. The present invention can be carried out based on the contents disclosed in this specification and the common general technical knowledge in the relevant field. In the following drawings, components and parts that perform the same function may be denoted by the same reference numerals, and redundant explanations may be omitted or simplified. Furthermore, the embodiments shown in the drawings are schematic to clearly explain the present invention and do not necessarily accurately represent the size or scale of the actual product provided.

[0023] In this specification, the term "acrylic polymer" refers to a polymer containing monomer units derived from (meth)acrylic monomers in the polymer structure, typically a polymer containing more than 50% by weight of monomer units derived from (meth)acrylic monomers. The term "(meth)acrylic monomer" refers to a monomer having at least one (meth)acryloyl group per molecule. Here, the term "(meth)acryloyl group" refers to both acryloyl and methacryloyl groups. Therefore, the term "(meth)acrylic monomer" as used herein encompasses both monomers having an acryloyl group (acrylic monomers) and monomers having a methacryloyl group (methacrylic monomers). Similarly, in this specification, the term "(meth)acrylic acid" refers to both acrylic acid and methacrylic acid, and the term "(meth)acrylate" refers to both acrylate and methacrylate.

[0024] <Structural Example of Reinforcing Film> The reinforcing film disclosed herein has the form of a pressure-sensitive adhesive sheet having an adhesive surface formed by a pressure-sensitive adhesive. The pressure-sensitive adhesive sheet used as the reinforcing film is configured to include a pressure-sensitive adhesive layer. The reinforcing film disclosed herein may be in the form of a substrate-attached pressure-sensitive adhesive sheet in which the pressure-sensitive adhesive layer is laminated on one or both sides of a supporting substrate, or in the form of a substrate-less pressure-sensitive adhesive sheet without a supporting substrate. Hereinafter, the supporting substrate may be simply referred to as the "substrate." Note that in this specification, the term "reinforcing film" refers to a pressure-sensitive adhesive sheet (reinforcing pressure-sensitive adhesive film) used to reinforce an adherend, as described below. The reinforcing film can be in the form of a substrate-less pressure-sensitive adhesive sheet, for example, by attaching a support material or the like to one adhesive surface and then attaching the other adhesive surface to the adherend to be reinforced, and therefore is not limited to the form of a substrate-attached pressure-sensitive adhesive sheet. In this respect, it is understood as a broader concept than the "reinforcing film" described below, which has the form of a substrate-attached pressure-sensitive adhesive sheet.

[0025] The structure of a reinforcing film according to one embodiment is shown schematically in FIG. 1 . This reinforcing film 1 is configured as a substrate-attached single-sided pressure-sensitive adhesive sheet including a sheet-like support substrate 10 having a first surface 10A and a second surface 10B, and a pressure-sensitive adhesive layer 21 provided on the first surface 10A side. The pressure-sensitive adhesive layer 21 is fixed to the first surface 10A side of the support substrate 10. The reinforcing film 1 is used by attaching the pressure-sensitive adhesive layer 21 to an adherend. Before use (i.e., before being attached to an adherend), the reinforcing film 1 can be a component of a release-liner-attached reinforcing film 100 in which, as shown in FIG. 1 , the surface (adhesive surface) 21A of the pressure-sensitive adhesive layer 21 is in contact with a release liner 31, at least the side facing the pressure-sensitive adhesive layer 21 being a releasable surface (release surface). The release liner 31 can preferably be, for example, a sheet-like substrate (liner substrate) configured so that one side serves as a release surface by providing a release layer made of a release treatment agent on that surface. Alternatively, the release liner 31 may be omitted, and a supporting substrate 10 having a release surface at its second surface 10B may be used, with the reinforcing film 1 rolled up to bring the adhesive surface 21A into contact with the second surface 10B of the supporting substrate 10. When attaching the reinforcing film 1 to an adherend, the release liner 31 or the second surface 10B of the supporting substrate 10 is peeled off from the adhesive surface 21A, and the exposed adhesive surface 21A is pressed against the adherend.

[0026] The structure of a reinforcing film according to another embodiment is shown schematically in Figure 2. This reinforcing film 2 is configured as a substrate-attached double-sided pressure-sensitive adhesive sheet including a sheet-like support substrate 10 having a first surface 10A and a second surface 10B, a pressure-sensitive adhesive layer 21 provided on the first surface 10A side, and a pressure-sensitive adhesive layer 22 provided on the second surface 10B side. The pressure-sensitive adhesive layer (first pressure-sensitive adhesive layer) 21 is adhered to the first surface 10A of the support substrate 10, and the pressure-sensitive adhesive layer (second pressure-sensitive adhesive layer) 22 is adhered to the second surface 10B of the support substrate 10. The reinforcing film 2 is used by adhering the pressure-sensitive adhesive layers 21 and 22 to different locations on an adherend. The locations to which the pressure-sensitive adhesive layers 21 and 22 are adhered may be locations on different members, or may be different locations within a single member. As shown in Figure 2, the reinforcing film 2 before use can be a component of a release-liner-attached reinforcing film 200 in which the surface (first adhesive surface) 21A of the pressure-sensitive adhesive layer 21 and the surface (second adhesive surface) 22A of the pressure-sensitive adhesive layer 22 are in contact with release liners 31, 32, each of which has a release surface on at least the side facing the pressure-sensitive adhesive layers 21, 22. As the release liners 31, 32, for example, a sheet-like substrate (liner substrate) having a release layer made of a release treatment agent on one side thereof, so that the one side serves as the release surface, can be preferably used. Alternatively, the release liner 32 can be omitted, and a release liner 31 having release surfaces on both sides can be used. This can be superimposed on the reinforcing film 2 and wound spirally to form a release-liner-attached reinforcing film in a roll form in which the second adhesive surface 22A is in contact with the back surface of the release liner 31.

[0027] The structure of a reinforcing film according to yet another embodiment is shown schematically in Figure 3. This reinforcing film 3 is configured as a substrate-less double-sided pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer 21. The reinforcing film 3 is used by attaching a first adhesive surface 21A, which is configured as one surface (first surface) of the pressure-sensitive adhesive layer 21, and a second adhesive surface 21B, which is configured as the other surface (second surface) of the pressure-sensitive adhesive layer 21, to different locations on an adherend. Before use, the reinforcing film 3 can be a component of a release-liner-attached reinforcing film 300, as shown in Figure 3, in which the first adhesive surface 21A and the second adhesive surface 21B are in contact with release liners 31 and 32, each of which has a release surface at least on the side facing the pressure-sensitive adhesive layer 21. Alternatively, the release liner 32 may be omitted, and a release liner 31 having release surfaces on both sides may be used, which may be superimposed on the reinforcing film 3 and wound in a spiral shape to form a reinforcing film with a release liner in a form (roll form) in which the second adhesive surface 21B is in contact with the back surface of the release liner 31.

[0028] The reinforcing film may be in the form of a roll or a sheet, and may be cut, punched, or otherwise processed into an appropriate shape depending on the application or mode of use. The pressure-sensitive adhesive layer in the technology disclosed herein is typically formed continuously, but is not limited thereto, and may be formed in a regular or random pattern such as a dotted or striped pattern.

[0029] <Pressure-Sensitive Adhesive Layer> The reinforcing film disclosed herein includes a pressure-sensitive adhesive layer containing a polymer (A) and a polymer (B). Such a pressure-sensitive adhesive layer may be formed from a pressure-sensitive adhesive composition containing a polymer (A) that is a complete or partial polymer of a monomer raw material A, and a polymer (B). The form of the pressure-sensitive adhesive composition is not particularly limited, and may be in various forms, such as a solvent-based, water-dispersible, hot-melt, or active energy ray-curable (e.g., photocurable) form.

[0030] (Polymer (A)) An acrylic polymer can be preferably used as the polymer (A) in the pressure-sensitive adhesive layer. When an acrylic polymer is used as the polymer (A), good compatibility with the polymer (B) tends to be easily obtained. Good compatibility between the polymer (A) and the polymer (B) is preferable because it can contribute to reducing the initial adhesive strength and improving the adhesive strength after heating by improving the mobility of the polymer (B) within the pressure-sensitive adhesive layer. In addition, acrylic polymers, which have a high degree of freedom in molecular design, are suitable as pressure-sensitive adhesive materials that can improve adhesive properties and flexibility in a well-balanced manner. While limiting the amount of nitrogen-containing monomer to a predetermined value or less, N / W Zr The desired effect achieved by making the ratio (R) equal to or greater than a predetermined value is effectively achieved in a configuration in which an acrylic polymer is used as the polymer (A).

[0031] In the reinforcing film disclosed herein, the polymer (A) is typically the main component of the polymer components contained in the pressure-sensitive adhesive layer, i.e., a component that accounts for more than 50 wt%, and may be a component that accounts for, for example, 75 wt% or more, 85 wt% or more, 90 wt% or more, or 95 wt% or more (e.g., 97 wt% or more) of the above polymer components. In some embodiments, the polymer (A) may be a component that accounts for, for example, more than 50 wt% of the entire pressure-sensitive adhesive layer, a component that accounts for 70 wt% or more, a component that accounts for 80 wt% or more, a component that accounts for 90 wt% or more, or a component that accounts for 95 wt% or more (e.g., 97 wt% or more).

[0032] The polymer (A) contains at least a monomer unit derived from a nitrogen-containing monomer, and typically contains a monomer unit derived from a nitrogen-containing monomer and a monomer unit derived from an alkyl (meth)acrylate ester.

[0033] For example, the polymer (A) may be a polymer in which the amount of monomer units derived from (meth)acrylic acid alkyl ester contained in 100 parts by weight of the polymer (A) is 50 parts by weight or more, i.e., a polymer in which 50% by weight or more of the total amount of the monomer components (monomer raw material A) for preparing the polymer (A) is a (meth)acrylic acid alkyl ester. The (meth)acrylic acid alkyl ester may be a (meth)acrylic acid alkyl ester having 1 to 20 carbon atoms (i.e., C 1-20 Among the monomer raw materials A, (meth)acrylic acid C is preferably used because it is easy to balance the properties. 1-20 The proportion of alkyl ester may be, for example, 50% by weight or more, or 60% by weight or more. 1-20 The proportion of alkyl ester is 70% by weight or more, more preferably 80% by weight or more, and even more preferably 85% by weight or more. By using polymer (A) having such a monomer composition, it is easy to obtain a pressure-sensitive adhesive that achieves a good balance between increased adhesive strength and flexibility. In addition, from the viewpoint of easily obtaining the effect of using a nitrogen-containing monomer, (meth)acrylic acid C in the monomer raw material A is preferably used. 1-20 The proportion of alkyl ester is suitably 99.9% by weight or less or 99.8% by weight or less, and may be 99.5% by weight or less, or may be 99% by weight or less. 1-20 The proportion of alkyl ester may be, for example, 98% by weight or less, 95% by weight or less, or 92% by weight or less.

[0034] (Meth)acrylic acid C 1-20Non-limiting examples of alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and isopropyl (meth)acrylate. Examples of the acrylate include isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate.

[0035] Among these, at least (meth)acrylic acid C 1-18 It is preferable to use an alkyl ester, and at least (meth)acrylic acid C 1-14 It is more preferred to use alkyl esters. In some embodiments, the acrylic polymer is (meth)acrylic acid C 4-12 Alkyl ester (preferably acrylic acid C 4-10 Alkyl esters, such as acrylic acid C 6-10 For example, an acrylic polymer containing one or both of n-butyl acrylate (BA) and 2-ethylhexyl acrylate (2EHA) is preferred, and an acrylic polymer containing at least 2EHA is particularly preferred.

[0036] In some preferred embodiments, acrylic acid C is included in the monomer raw material A for preparing polymer (A). 6-10 Alkyl ester (preferably acrylic acid C 8-9The proportion of the acrylic acid C in the monomer raw material A is 70% by weight or more, more preferably 80% by weight or more, and even more preferably 85% by weight or more. An acrylic polymer having such a monomer composition is particularly suitable for achieving the effects of the technology disclosed herein. 6-10 Alkyl ester (preferably acrylic acid C 8-9 The proportion of the alkyl ester (typically 2EHA) may be, for example, 99.9% by weight or less, 99.5% by weight or less, or 99% by weight or less, and from the viewpoint of initial light release properties, etc., it may be 98% by weight or less, 95% by weight or less, or 92% by weight or less.

[0037] The monomer component (monomer raw material A) for preparing polymer (A) includes a nitrogen-containing monomer, i.e., a monomer containing a nitrogen atom. By appropriately using the nitrogen-containing monomer, the cohesive strength and polarity of the adhesive can be adjusted, and the adhesive strength after the adhesive strength increase (e.g., adhesive strength to a polyimide film) can be improved. The nitrogen-containing monomer can be used alone or in appropriate combination of two or more.

[0038] Non-limiting examples of nitrogen-containing monomers include: monomers having a nitrogen atom-containing ring: for example, N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-(meth)acryloyl-2-pyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-(meth)acryloylmorpholine, N-vinylmorpholine, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, N-vinylpyrazole, N-vinylisoxazole, N-vinylthiazole, N-vinylisothiazole, N-vinylpyridazine, etc.; For example, monomers having a succinimide skeleton, such as N-(meth)acryloyloxymethylene succinimide, N-(meth)acryloyl-6-oxyhexamethylene succinimide, and N-(meth)acryloyl-8-oxyhexamethylene succinimide; maleimides, such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, and N-phenylmaleimide; and itaconimides, such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide, and N-laurylitaconimide.Amide group-containing monomers: for example, (meth)acrylamide; N,N-dialkyl(meth)acrylamides such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, and N,N-di(t-butyl)(meth)acrylamide; N-alkyl(meth)acrylamides such as N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-butyl(meth)acrylamide, and N-n-butyl(meth)acrylamide; N-vinylcarboxylic acid amides such as N-vinylacetamide; monomers having a hydroxyl group and an amide group, for example, N-(2-hydroxyethyl)(meth)acrylamide; N-hydroxyalkyl(meth)acrylamides such as N-(meth)acrylamide, N-(2-hydroxypropyl)(meth)acrylamide, N-(1-hydroxypropyl)(meth)acrylamide, N-(3-hydroxypropyl)(meth)acrylamide, N-(2-hydroxybutyl)(meth)acrylamide, N-(3-hydroxybutyl)(meth)acrylamide, and N-(4-hydroxybutyl)(meth)acrylamide; monomers having an alkoxy group and an amide group, for example, N-alkoxyalkyl(meth)acrylamides such as N-methoxymethyl(meth)acrylamide, N-methoxyethyl(meth)acrylamide, and N-butoxymethyl(meth)acrylamide; and others, N,N-dimethylaminopropyl(meth)acrylamide, etc. Aminoalkyl(meth)acrylates such as aminoethyl(meth)acrylate, N,N-dimethylaminoethyl(meth)acrylate, N,N-diethylaminoethyl(meth)acrylate, and t-butylaminoethyl(meth)acrylate. Cyano group-containing monomers: for example, acrylonitrile, methacrylonitrile, etc. Isocyanate group-containing monomers: for example, 2-isocyanatoethyl (meth)acrylate, etc.

[0039] In some embodiments, from the viewpoint of ease of synthesis of the polymer (A) and copolymerizability with other monomer components (e.g., alkyl (meth)acrylate esters), a nitrogen-containing monomer having an N-vinyl group or an N-(meth)acryloyl group (e.g., one or more selected from the group consisting of a monomer having a nitrogen atom-containing ring, an amide group-containing monomer, and an aminoalkyl (meth)acrylate) can be preferably used as the nitrogen-containing monomer.

[0040] The amount of nitrogen-containing monomer used is the amount W of nitrogen-containing monomer contained in 100 parts by weight of polymer (A). N is 14 parts by weight or less, that is, the amount of the nitrogen-containing monomer is 14% by weight or less of the total amount of the monomer components (monomer raw material A) for preparing the polymer (A). N By limiting the amount of the nitrogen-containing monomer to 14 parts by weight or less, the flexibility of the PSA in the low temperature range can be improved (for example, the storage modulus at -20°C can be reduced), and flexibility suitable for repeated bending and flexing can be achieved. From the viewpoint of improving the flexibility, in some embodiments, the content of the nitrogen-containing monomer in the monomer raw material A is 12% by weight or less (i.e., W N The nitrogen-containing monomer content is suitably 12 parts by weight or less, advantageously 10% by weight or less, preferably 8.0% by weight or less, more preferably 5.0% by weight or less, and may be 4.0% by weight or less, 3.0% by weight or less, or 2.0% by weight or less. The amount of nitrogen-containing monomer used is usually suitably 0.01% by weight or more (preferably 0.1% by weight or more, e.g., 0.3% by weight or more) of the monomer raw material A. From the viewpoint of facilitating the attainment of a higher effect of use, in some embodiments, the amount of nitrogen-containing monomer used is 0.5% by weight or more of the monomer raw material A (i.e., W N The content may be 0.5 parts by weight or more), or may be 0.7% by weight or more, 1.0% by weight or more, 1.2% by weight or more, or 1.5% by weight or more.

[0041] In some embodiments, the monomer raw material A may contain a monomer having a nitrogen atom-containing ring as the nitrogen-containing monomer. By employing a monomer having a nitrogen atom-containing ring as at least a portion of the nitrogen-containing monomer, the compatibility between the polymer (A) formed from the monomer raw material A and the polymer (B) tends to be improved. This improves the increase in adhesive strength, making it easier to obtain a reinforcing film with high adhesive strength (e.g., adhesive strength to a polyimide film) after the increase.

[0042] The monomer having a nitrogen atom-containing ring can be appropriately selected from, for example, the above-mentioned examples and used alone or in combination of two or more. In some embodiments, the monomer raw material A preferably contains, as the monomer having a nitrogen atom-containing ring, at least one monomer selected from the group consisting of N-vinyl cyclic amides and cyclic amides having a (meth)acryloyl group.

[0043] Specific examples of N-vinyl cyclic amides include N-vinyl-2-pyrrolidone, N-vinyl-2-piperidone, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3-oxazin-2-one, and N-vinyl-3,5-morpholinedione. Preferred examples include N-vinyl-2-pyrrolidone (NVP) and N-vinyl-2-caprolactam. Specific examples of cyclic amides having a (meth)acryloyl group include N-(meth)acryloyl-2-pyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, and N-(meth)acryloylmorpholine. Preferred examples include N-acryloylmorpholine (ACMO).

[0044] The amount of the monomer having a nitrogen atom-containing ring used is not particularly limited, and the amount W of the monomer units derived from the monomer having a nitrogen atom-containing ring contained in 100 parts by weight of the polymer (A) RN [Parts by weight] is the amount W of the nitrogen-containing monomer described above. NIn other words, the amount [wt %] of the monomer having a nitrogen atom-containing ring in the total amount of the monomer raw material A can be appropriately set within a range that does not exceed the amount [wt %] of the nitrogen-containing monomer in the total amount of the monomer raw material A. Therefore, the amount W of the monomer having a nitrogen atom-containing ring contained in 100 parts by weight of polymer (A) is RN is 14 parts by weight or less, and the amount of the monomer having a nitrogen atom-containing ring of the total amount of monomer feed A is 14 weight % or less. In some embodiments, the amount of the monomer having a nitrogen atom-containing ring used is 12 weight % or less of the monomer feed A (i.e., W RN It is suitable that the amount of the monomer having a nitrogen atom-containing ring is 12 parts by weight or less, advantageously 10% by weight or less, preferably 8.0% by weight or less, more preferably 5.0% by weight or less, and may be 4.0% by weight or less, 3.0% by weight or less, or 2.0% by weight or less. The amount of the monomer having a nitrogen atom-containing ring used is usually 0.01% by weight or more (preferably 0.1% by weight or more, for example 0.3% by weight or more) of the monomer raw material A, and from the viewpoint of easily obtaining a higher effect of use, it is suitable that the amount of the monomer having a nitrogen atom-containing ring used is 0.5% by weight or more (i.e., W RN The content may be 0.5 parts by weight or more), or may be 0.7% by weight or more, 1.0% by weight or more, 1.2% by weight or more, or 1.5% by weight or more.

[0045] In embodiments using a monomer having a nitrogen atom-containing ring, the proportion of the nitrogen atom-containing ring among the nitrogen-containing monomers contained in monomer raw material A may be, for example, 30% by weight or more, preferably 50% by weight or more, more preferably 70% by weight or more, 85% by weight or more, 90% by weight or more, 95% by weight or more, or even 100% by weight. In some embodiments, the amount of nitrogen-containing monomers other than those containing a nitrogen atom-containing ring in the total amount of monomer raw material A is, for example, 5% by weight or less, preferably 3% by weight or less, more preferably 1% by weight or less, or may be 0.5% by weight or less, or may be 0.1% by weight or less. Nitrogen-containing monomers other than those containing a nitrogen atom-containing ring may not be used. In some embodiments, the monomer having a nitrogen atom-containing ring and other nitrogen-containing monomers may be used in appropriate combination. In such embodiments, the proportion of the nitrogen atom-containing ring among the nitrogen-containing monomers contained in monomer raw material A may be, for example, 98% by weight or less, 93% by weight or less, 80% by weight or less, 60% by weight or less, or 40% by weight or less.

[0046] The monomer raw material A may contain the nitrogen-containing monomer and typically further the (meth)acrylic acid alkyl ester, as well as, if necessary, another monomer (copolymerizable monomer) copolymerizable with the (meth)acrylic acid alkyl ester. As the copolymerizable monomer, a monomer having a polar group (e.g., a carboxy group, a hydroxyl group, etc.) can be suitably used. The monomer having a polar group can be useful for introducing crosslinking points into the polymer (A) or for increasing the cohesive strength of the polymer (A). The copolymerizable monomer can be used alone or in combination of two or more.

[0047] Non-limiting specific examples of copolymerizable monomers include the following: Hydroxyl group-containing monomers: for example, hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate; Carboxy group-containing monomers: for example, acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid; Acid anhydride group-containing monomers: for example, maleic anhydride and itaconic anhydride. Monomers containing a sulfonic acid group or a phosphoric acid group: for example, styrenesulfonic acid, allylsulfonic acid, sodium vinylsulfonate, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, (meth)acryloyloxynaphthalenesulfonic acid, 2-hydroxyethyl acryloyl phosphate, etc. Epoxy group-containing monomers: for example, epoxy group-containing acrylates such as glycidyl (meth)acrylate and 2-ethyl (meth)acrylate glycidyl ether, allyl glycidyl ether, (meth)acrylic acid glycidyl ether, etc. Alkoxy group-containing monomers: for example, alkoxyalkyl (meth)acrylates such as 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, propoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, and ethoxypropyl (meth)acrylate; and alkoxyalkylene (meth)acrylates such as methoxyethylene glycol (meth)acrylate and methoxypolypropylene glycol (meth)acrylate.(Meth)acrylic acid esters having an alicyclic hydrocarbon group: for example, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, etc. (Meth)acrylic acid esters having an aromatic hydrocarbon group: for example, phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, benzyl (meth)acrylate, etc. Vinyl ethers: for example, vinyl alkyl ethers such as methyl vinyl ether and ethyl vinyl ether. Vinyl esters: for example, vinyl acetate, vinyl propionate, etc. Aromatic vinyl compounds: for example, styrene, α-methylstyrene, vinyltoluene, etc. Olefins: for example, ethylene, butadiene, isoprene, isobutylene, etc. Other examples include heterocycle-containing (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate, halogen atom-containing (meth)acrylates such as vinyl chloride and fluorine atom-containing (meth)acrylates, silicon atom-containing (meth)acrylates such as silicone (meth)acrylate, and (meth)acrylic acid esters obtained from terpene compound derivative alcohols.

[0048] When such a copolymerizable monomer is used, its amount is not particularly limited, but is typically suitably 0.01 wt% or more of the monomer raw material A. From the viewpoint of better exerting the effects of the use of the copolymerizable monomer (e.g., the effect of improving cohesion), the amount of the copolymerizable monomer used may be 0.1 wt% or more, or even 0.5 wt% or more of the monomer raw material A. In some embodiments, the content of the copolymerizable monomer in the monomer raw material A is preferably 0.7 wt% or more, more preferably 1 wt% or more, or may be 3 wt% or more, 5 wt% or more, or 7 wt% or more (e.g., 8 wt% or more). Furthermore, the amount of the copolymerizable monomer used may be, for example, 50 wt% or less of the monomer raw material A, suitably 30 wt% or less, preferably 20 wt% or less, more preferably 15 wt% or less (e.g., 12 wt% or less), or may be 10 wt% or less, 8 wt% or less, 6 wt% or less, 4 wt% or less, or 2 wt% or less. Limiting the amount of copolymerizable monomer used can be advantageous from the viewpoint of improving the flexibility of the PSA (particularly flexibility in the low temperature range).

[0049] In some preferred embodiments, the monomer raw material A includes a hydroxyl group-containing monomer. The use of the hydroxyl group-containing monomer adjusts the cohesive strength and polarity of the PSA, thereby enabling the effects of the technology disclosed herein to be preferably realized. Furthermore, the hydroxyl group-containing monomer provides a reactive site with a crosslinking agent (e.g., an isocyanate-based crosslinking agent) described below, and can increase the cohesive strength of the PSA through a crosslinking reaction.

[0050] Suitable hydroxyl group-containing monomers include 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and N-(2-hydroxyethyl)(meth)acrylamide. Among these, preferred examples include 2-hydroxyethyl acrylate (HEA) and 4-hydroxybutyl acrylate (4HBA). 4HBA is particularly preferred from the viewpoint of improving cohesive strength while suppressing a decrease in flexibility of the PSA.

[0051] The amount of hydroxyl group-containing monomer used is not particularly limited, and is typically 40 wt% or less of the monomer raw material A, and may be 30 wt% or less, or 20 wt% or less. In some embodiments, from the viewpoint of the flexibility of the PSA (particularly flexibility at low temperatures), the content of the hydroxyl group-containing monomer in the monomer raw material A is preferably 15 wt% or less (e.g., less than 15 wt%), more preferably 12 wt% or less, and may be 10 wt% or less, 8 wt% or less, 6 wt% or less, 4 wt% or less, or 2 wt% or less. By limiting the amount of hydroxyl group-containing monomer used, the mobility of the polymer (B) within the PSA layer is improved, making it easier to achieve increased adhesive strength. Furthermore, the amount of hydroxyl group-containing monomer used is suitably 0.01 wt% or more of the monomer raw material A (preferably 0.1 wt% or more, for example 0.5 wt% or more). From the viewpoint of obtaining an appropriate cohesive strength, in some embodiments, the amount of the hydroxyl group-containing monomer used is preferably 0.7% by weight or more of the monomer raw material A, more preferably 1% by weight or more, and may be 3% by weight or more, 5% by weight or more, or 7% by weight or more (for example, 8% by weight or more).

[0052] In some embodiments, a nitrogen-containing monomer (e.g., a monomer having a nitrogen atom-containing ring) and a hydroxyl-containing monomer can be used in combination as the copolymerizable monomer. In this case, the total amount of the nitrogen-containing monomer and the hydroxyl-containing monomer can be, for example, 0.1% by weight or more of the monomer raw material A, preferably 1% by weight or more, more preferably 3% by weight or more, even more preferably 5% by weight or more, and particularly preferably 7% by weight or more (e.g., 9% by weight or more). It may also be 10% by weight or more, 15% by weight or more, 20% by weight or more, or 25% by weight or more. Furthermore, the total amount of the nitrogen-containing monomer and the hydroxyl-containing monomer can be, for example, 50% by weight or less of the monomer raw material A, preferably 30% by weight or less. In some preferred embodiments, the total amount of the nitrogen-containing monomer and the hydroxyl-containing monomer is 20% by weight or less of the monomer raw material A, more preferably 15% by weight or less (e.g., 12% by weight or less).

[0053] In an embodiment in which the monomer raw material A contains a nitrogen-containing monomer (for example, a monomer having a nitrogen atom-containing ring) in combination with a hydroxyl group-containing monomer, the content of the nitrogen-containing monomer in the monomer raw material A (W N ) and the content of hydroxyl group-containing monomer (W OH The relationship (weight basis) between W and W is not particularly limited. N / W OH may be, for example, 0.01 or more, and usually 0.05 or more is appropriate, and may be 0.10 or more, or 0.12 or more. N / W OH may be, for example, 10 or less, and is usually suitably 1 or less, and is preferably 0.50 or less, or may be 0.30 or less, or may be 0.20 or less, or may be 0.15 or less.

[0054] In some embodiments, it is preferable that monomer raw material A does not contain a monomer having a polyorganosiloxane skeleton (monomer S1), which is preferably used as a constituent component of monomer raw material B described below, or that the content of this monomer is less than 10 wt% (more preferably less than 5 wt%, for example less than 2 wt%) of monomer raw material A. Monomer raw material A having such a composition can suitably realize a reinforcing film that favorably achieves both initial reworkability and strong adhesion after adhesive strength is increased. For the same reason, in other embodiments, it is preferable that monomer raw material A does not contain monomer S1, or if it contains monomer S1, its content (by weight) is lower than the content of monomer S1 in monomer raw material B.

[0055] Glass transition temperature T of polymer (A) A is not particularly limited and can be selected to obtain desirable properties in the reinforcing film disclosed herein. A A polymer (A) having a temperature of less than 0° C. can be preferably used. A pressure-sensitive adhesive containing such a polymer (A) exhibits appropriate fluidity (for example, mobility of the polymer chains contained in the pressure-sensitive adhesive), and is therefore suitable for realizing a reinforcing film whose adhesive strength increases to a predetermined value or more upon heating. The reinforcing film disclosed herein is Amay be preferably carried out using a polymer (A) where T is less than −10° C., less than −20° C., less than −30° C., or less than −35° C. A may be less than −40° C. or less than −45° C. In some embodiments, from the viewpoint of improving flexibility in a low temperature range, T A is preferably −50° C. or lower, more preferably −55° C. or lower, and even more preferably −58° C. or lower, and may be −60° C. or lower, −62° C. or lower, or −65° C. or lower. A There is no particular restriction on the lower limit of T. From the viewpoint of material availability and improving the cohesive strength of the adhesive layer, it is usually A Preferably, the polymer (A) has a T of −80° C. or higher, −75° C. or higher, or −70° C. or higher. A may be, for example, −65° C. or higher, or −63° C. or higher.

[0056] In this specification, the glass transition temperature (Tg) of a polymer refers to either a nominal value described in literature, catalogs, etc., or a Tg calculated by the Fox formula based on the composition of the raw monomer materials used to prepare the polymer. The Fox formula, as shown below, is a relationship between the Tg of a copolymer and the glass transition temperature Tgi of a homopolymer obtained by homopolymerizing each of the monomers constituting the copolymer: 1 / Tg = Σ(Wi / Tgi) In the Fox formula, Tg represents the glass transition temperature of the copolymer (unit: K), Wi represents the weight fraction of monomer i in the copolymer (copolymerization ratio on a weight basis), and Tgi represents the glass transition temperature of a homopolymer of monomer i (unit: K). When the target polymer for which Tg is specified is a homopolymer, the Tg of the homopolymer and the Tg of the target polymer will be the same.

[0057] The glass transition temperature of a homopolymer used to calculate Tg is a value listed in a publicly available document. Specifically, values ​​are listed in "Polymer Handbook" (3rd Edition, John Wiley & Sons, Inc., 1989). For monomers for which multiple values ​​are listed in the Polymer Handbook, the highest value is used.

[0058] The glass transition temperature of a homopolymer of a monomer not listed in the Polymer Handbook is determined by the value obtained by the following measurement method. Specifically, 100 parts by weight of the monomer, 0.2 parts by weight of 2,2'-azobisisobutyronitrile, and 200 parts by weight of ethyl acetate as a polymerization solvent are charged into a reactor equipped with a thermometer, a stirrer, a nitrogen inlet tube, and a reflux condenser, and the mixture is stirred for 1 hour while passing nitrogen gas through. After removing oxygen from the polymerization system in this manner, the temperature is raised to 63°C and the reaction is allowed to proceed for 10 hours. The mixture is then cooled to room temperature to obtain a homopolymer solution with a solids concentration of 33% by weight. This homopolymer solution is then cast onto a release liner and dried to prepare a test sample (sheet-like homopolymer) with a thickness of approximately 2 mm. This test sample was punched out into a disk shape with a diameter of 7.9 mm, sandwiched between parallel plates, and the viscoelasticity was measured in shear mode using a viscoelasticity tester (manufactured by TA Instruments Japan, model name "DHR-2") while applying a shear strain at a frequency of 1 Hz in a temperature range of -70°C to 150°C at a heating rate of 5°C / min, and the temperature corresponding to the peak top temperature of tan δ was taken as the Tg of the homopolymer.

[0059] Although not particularly limited, the weight average molecular weight (Mw) of the polymer (A) is usually about 20 × 10 4 It is suitable that the Mw of the polymer (A) is 30×10 or more. A PSA exhibiting good cohesive strength is easily obtained by using the polymer (A) having such an Mw. From the viewpoint of obtaining higher cohesive strength, in some preferred embodiments, the Mw of the polymer (A) is, for example, 30×10 4 or more, 40 × 10 4 More than 50 x 10 4 More than 60 x 10 4 Or more, 80 x 10 4 The Mw of the polymer (A) is usually about 500×10 4It is suitable that the Mw of the polymer (A) is not too high. The polymer (A) having such a Mw is likely to form an adhesive that exhibits moderate fluidity (mobility of the polymer chain), and is therefore suitable for realizing a reinforcing film that has low initial adhesive strength after application and a large increase in adhesive strength. It is also preferable from the viewpoint of improving compatibility with the polymer (B) that the Mw of the polymer (A) is not too high. In some preferred embodiments, the Mw of the polymer (A) is, for example, 250 × 10 4 may be less than or equal to 200×10 4 Less than 150 x 10 4 It can be less than 100 x 10 4 Less than 70 x 10 4 The following is also acceptable.

[0060] In this specification, the Mw of polymer (A) and polymer (B) described later can be determined in terms of polystyrene by gel permeation chromatography (GPC). More specifically, the Mw can be measured according to the method and conditions described in the examples described later.

[0061] The method for obtaining the polymer (A) is not particularly limited, and various polymerization methods such as solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization, and photopolymerization can be appropriately employed. In some embodiments, solution polymerization can be preferably employed. The polymerization temperature during solution polymerization can be appropriately selected depending on the types of monomers and solvents used, the type of polymerization initiator, and the like, and can be, for example, about 20°C to 170°C (typically about 40°C to 140°C).

[0062] The initiator used for polymerization can be appropriately selected from conventionally known thermal polymerization initiators, photopolymerization initiators, etc., depending on the polymerization method. The polymerization initiators can be used alone or in combination of two or more.

[0063] Examples of the thermal polymerization initiator include azo-based polymerization initiators (e.g., 2,2'-azobisisobutyronitrile, 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2-methylpropionic acid)dimethyl, 4,4'-azobis-4-cyanovaleric acid, azobisisovaleronitrile, 2,2'-azobis(2-amidinopropane)dihydrochloride, 2,2'-azobis[2-(5-methyl-2 Examples of suitable thermal polymerization initiators include 2,2'-azobis(N,N'-imidazolin-2-yl)propane dihydrochloride, 2,2'-azobis(2-methylpropionamidine) disulfate, 2,2'-azobis(N,N'-dimethyleneisobutylamidine) dihydrochloride, etc.; persulfates such as potassium persulfate; peroxide polymerization initiators (e.g., dibenzoyl peroxide, t-butyl permaleate, lauroyl peroxide, etc.); and redox polymerization initiators. The amount of the thermal polymerization initiator used is not particularly limited, but can be, for example, in the range of 0.01 to 5 parts by weight, preferably 0.05 to 3 parts by weight, per 100 parts by weight of the monomer component (monomer raw material A) used in preparing the acrylic polymer.

[0064] The photopolymerization initiator is not particularly limited, and examples thereof include benzoin ether-based photopolymerization initiators, acetophenone-based photopolymerization initiators, α-ketol-based photopolymerization initiators, aromatic sulfonyl chloride-based photopolymerization initiators, photoactive oxime-based photopolymerization initiators, benzoin-based photopolymerization initiators, benzyl-based photopolymerization initiators, benzophenone-based photopolymerization initiators, ketal-based photopolymerization initiators, thioxanthone-based photopolymerization initiators, and acylphosphine oxide-based photopolymerization initiators. The amount of the photopolymerization initiator used is not particularly limited, and can be, for example, in the range of 0.01 to 5 parts by weight, and preferably 0.05 to 3 parts by weight, per 100 parts by weight of the monomer raw material A.

[0065] In some embodiments, the polymer (A) may be included in the PSA composition for forming a PSA layer in the form of a partially polymerized product (polymer syrup) obtained by irradiating a mixture of the monomer raw material A and a polymerization initiator with ultraviolet (UV) light to polymerize a portion of the monomer component. The PSA composition containing such a polymer syrup can be applied to a predetermined substrate and then irradiated with ultraviolet light to complete the polymerization. In other words, the polymer syrup can be considered a precursor of the polymer (A). The PSA layer disclosed herein can be formed, for example, using a PSA composition containing the polymer syrup and polymer (B).

[0066] (Polymer (B)) The polymer (B) in the technology disclosed herein is a polymer of a monomer component (monomer raw material B) containing a monomer having a polyorganosiloxane skeleton (hereinafter also referred to as "monomer S1") and a (meth)acrylic monomer. The polymer (B) can be said to be a copolymer of the monomer S1 and the (meth)acrylic monomer. The polymer (B) can be used alone or in combination of two or more types. The polymer (B) suppresses the initial adhesive strength when attached to the adherend due to the low polarity and mobility of the polyorganosiloxane structure derived from the monomer S1, and can function as an adhesive strength increase retarder that increases the adhesive strength to the adherend by heating. The monomer S1 is not particularly limited, and any monomer containing a polyorganosiloxane skeleton can be used. Due to the low polarity inherent in its structure, monomer S1 promotes uneven distribution of polymer (B) on the surface of the adhesive layer of the reinforcing film before use (before application to the substrate), thereby achieving easy peelability (low adhesion) at the initial stage of application. Monomer S1 having a structure with a polymerizable reactive group at one end is preferably used. A configuration containing such monomer S1 units and (meth)acrylic monomer units results in the formation of polymer (B) having a polyorganosiloxane skeleton in the side chain. Polymer (B) with such a structure tends to have low initial adhesion and high adhesion after heating due to the mobility and ease of movement of the side chain. Furthermore, in some embodiments, monomer S1 having a polymerizable reactive group at one end and no functional group at the other end that undergoes a crosslinking reaction with polymer (A) can be preferably used. Polymer (B) copolymerized with monomer S1 of such a structure tends to have low initial adhesion and high adhesion after heating due to the mobility of the polyorganosiloxane structure derived from monomer S1.

[0067] As the monomer S1, for example, a compound represented by the following general formula (1) or (2) can be used. More specifically, examples of the single-end reactive silicone oils manufactured by Shin-Etsu Chemical Co., Ltd. include X-22-174ASX, X-22-2426, X-22-2475, and KF-2012. The monomer S1 can be used alone or in combination of two or more. Here, R in the above general formulas (1) and (2) 3 is hydrogen or methyl, and R 4 is a methyl group or a monovalent organic group, and m and n are integers of 0 or more.

[0068] The functional group equivalent of the monomer S1 can be any value within the range in which the desired effect is achieved using the monomer S1, and is not limited to a specific range. From the viewpoint of sufficiently suppressing the initial adhesive strength, the functional group equivalent is, for example, 100 g / mol or more, or 200 g / mol or more, and is suitably 300 g / mol or more (e.g., 500 g / mol or more), preferably 800 g / mol or more, and more preferably 1500 g / mol or more. In a particularly preferred embodiment, from the viewpoint of achieving both low adhesive strength at the initial stage of application and a high level of increase in adhesive strength after heating, the functional group equivalent is suitably 2000 g / mol or more, and may be, for example, 2500 g / mol or more, 3000 g / mol or more, 4000 g / mol or more, or 5000 g / mol or more. In some other embodiments, the functional group equivalent weight may be, for example, 9000 g / mol or more, 12000 g / mol or more, or 15000 g / mol or more.

[0069] From the viewpoint of sufficiently increasing the adhesive strength, the functional group equivalent weight is suitably, for example, 30,000 g / mol or less, and may be 20,000 g / mol or less, less than 15,000 g / mol, or less than 10,000 g / mol. In some preferred embodiments, the functional group equivalent weight of the monomer S1 is 7,000 g / mol or less, more preferably 5,500 g / mol or less, even more preferably 5,000 g / mol or less, and may be 4,500 g / mol or less, 4,200 g / mol or less, 4,000 g / mol or less, 3,500 g / mol or less, or 3,200 g / mol or less. When the functional group equivalent weight of monomer S1 is within the above range, compatibility within the adhesive layer (e.g., compatibility with polymer (A)) tends to be good, the mobility of the polyorganosiloxane skeleton (chain) of polymer (B) is good, and the mobility of polymer (B) can be easily adjusted within an appropriate range, making it easier to realize an adhesive layer that achieves both a high level of initial low adhesion and an increase in adhesive strength after heating.

[0070] Here, "functional group equivalent" means the weight of the main skeleton (e.g., polydimethylsiloxane) bonded to one functional group. The unit g / mol is calculated based on 1 mol of functional group. The functional group equivalent of the monomer S1 can be calculated, for example, by nuclear magnetic resonance (NMR) analysis. 1 It can be calculated from the spectral intensity of H-NMR (proton NMR). 1 The functional group equivalent weight (g / mol) of the monomer S1 was calculated based on the H-NMR spectrum intensity as follows: 1 This can be done based on a general structural analysis method involving H-NMR spectrum analysis, and if necessary, by referring to the description in Japanese Patent No. 5951153. In the functional group equivalent of the monomer S1, the functional group means a polymerizable functional group (for example, an ethylenically unsaturated group such as a (meth)acryloyl group, a vinyl group, or an allyl group).

[0071] When two or more types of monomers having different functional group equivalents are used as the monomer S1, the arithmetic mean value can be used as the functional group equivalent of the monomer S1. 1 , Monomer S12 ...Monomer S1 n The functional group equivalent of the monomer S1 consisting of (g / mol) can be calculated by the following formula: Functional group equivalent of the monomer S1 (g / mol) = (monomer S1 1 functional group equivalent × monomer S1 1 + Monomer S1 2 functional group equivalent × monomer S1 2 + ... + Monomer S1 n functional group equivalent × monomer S1 n (amount of monomer S1) / (amount of monomer S1) 1 + Monomer S1 2 + ... + Monomer S1 n (amount of blend)

[0072] The content of monomer S1 can be an appropriate value within the range in which the desired effect is achieved using the monomer S1, and is not limited to a specific range. From the viewpoint of sufficiently suppressing the initial adhesive strength, in some embodiments, the content of monomer S1 in the total amount of monomer components (monomer raw material B) used to prepare polymer (B) may be, for example, 5% by weight or more. From the viewpoint of better exerting the effect as an adhesive strength increase retarder, it is preferably 10% by weight or more, more preferably 12% by weight or more, even more preferably 15% by weight or more, particularly preferably 18% by weight or more, and may even be 20% by weight or more. Furthermore, from the viewpoint of polymerization reactivity and compatibility, the content of monomer S1 in monomer raw material B may be, for example, 80% by weight or less, and it is appropriate to set it to 60% by weight or less, preferably 50% by weight or less, more preferably 40% by weight or less, and even more preferably 30% by weight or less. By setting the polymerization ratio of monomer S1 within an appropriate range, an increase in adhesive strength can be suitably achieved.

[0073] In addition to the monomer S1, the monomer raw material B contains a (meth)acrylic monomer copolymerizable with the monomer S1. The use of one or more (meth)acrylic monomers can favorably adjust the mobility of the polymer (B) within the pressure-sensitive adhesive layer. This can also be useful for improving the compatibility between the polymer (B) and the polymer (A). The polymer (B) containing a (meth)acrylic monomer unit is highly compatible with the polymer (A) (acrylic polymer), and therefore, by improving the mobility of the polymer (B) within the pressure-sensitive adhesive layer, it is easy to reduce the initial adhesive strength and improve the adhesive strength after heating.

[0074] In the polymer (B) used in the technology disclosed herein, the composition of the (meth)acrylic monomer contained in the monomer raw material B is such that the glass transition temperature T B1 is the glass transition temperature T A It is preferable that the temperature is set to be higher than T B1 can be set to be higher than 0° C., for example. Here, the glass transition temperature T B1 means the Tg determined by the Fox formula based on the composition of only the (meth)acrylic monomer among the monomer components used in the preparation of the polymer (B). B1 The glass transition temperature T can be calculated from the glass transition temperature of a homopolymer of each (meth)acrylic monomer and the weight fraction of each (meth)acrylic monomer in the total amount of the (meth)acrylic monomers by applying the above-mentioned Fox equation to only the (meth)acrylic monomers among the monomer components used in preparing the polymer (B). B1 The polymer (B) having a relatively high glass transition temperature T B1 When the polymer (B) has a relatively high Tc (typically higher than 0°C), a reinforcing film having a large rate of increase in adhesive strength is likely to be obtained.

[0075] In some preferred embodiments, T B1is 10°C or higher, more preferably 30°C or higher, even more preferably 40°C or higher, and may be 45°C or higher. B1 When T is higher, the adhesive strength at the initial stage of application generally tends to be better suppressed. B1 It is believed that, with the polymer (B) having a temperature of at least a predetermined temperature, the improvement in the mobility and mobility of the polyorganosiloxane structural portion that accompanies a rise in temperature to room temperature or a region somewhat higher than room temperature is effectively suppressed by the monomer units derived from the (meth)acrylic monomer contained in the polymer (B), and the low adhesiveness resulting from the presence of the polyorganosiloxane structural portion can be better maintained. From the viewpoint of more stably maintaining the low adhesiveness at the initial stage of application, in some embodiments, T B1 may be, for example, 50°C or higher, 55°C or higher, or 60°C or higher. B1 may be, for example, 120°C or less, or 100°C or less. B1 When T is lower, the adhesive strength tends to increase more easily by heating. B1 is, for example, 90° C. or less, more preferably 70° C. or less, even more preferably 60° C. or less, and particularly preferably 55° C. or less (for example, 50° C. or less).

[0076] T B1 From the viewpoint of making it easier to exert the effect of appropriately setting the above, the total amount of the monomer S1 and the (meth)acrylic monomer in all the monomer components for preparing the polymer (B) may be, for example, 50% by weight or more, 70% by weight or more, 85% by weight or more, 90% by weight or more, 95% by weight or more, or even substantially 100% by weight.

[0077] Glass transition temperature T of polymer (B) B is not particularly limited and can be selected so as to obtain desirable properties in the reinforcing film disclosed herein. B The T of the polymer (B) may be, for example, less than 50°C, 30°C or less, 20°C or less, 15°C or less, or 10°C or less. BWhen the T of the polymer (B) is lowered, the mobility (typically temperature-sensitive mobility) of the polymer (B) is improved, and the adhesive strength can be significantly increased. B is 5° C. or less, and may be less than 0° C., may be −5° C. or less, or may be −10° C. or less. In some embodiments, the T B may be, for example, −40° C. or higher, or −30° C. or higher. B The higher the T of the polymer (B), the more the polymer (B) unevenly distributed on the surface side of the pressure-sensitive adhesive layer when attached to an adherend contributes to a decrease in the initial adhesive strength, and the easier peelability at the initial stage of attachment tends to be excellent. B is -20°C or higher, and may be -15°C or higher. B By setting this within an appropriate range, it is possible to control the easy peelability at the initial stage of application and the increase in adhesive strength after heating within a preferred range.

[0078] In some embodiments, the composition of the monomer components for preparing polymer (B) is T B1 T B To be higher, i.e., T B1 -T B can be set so that T is greater than 0° C. With such a composition, the effect of adjusting the mobility of the polymer (B) is easily exhibited favorably depending on the composition of the (meth)acrylic monomer contained in the monomer component. B1 -T B may be, for example, about 40°C to 100°C, or about 50°C to 90°C. B1 -T B is 45° C. or higher, more preferably 50° C. or higher, and even more preferably 55° C. or higher (for example, 58° C. or higher). B1 -T B is preferably 80°C or less, more preferably 70°C or less, and even more preferably 65°C or less (for example, 62°C or less).

[0079] From the viewpoint of facilitating control of the mobility of the polymer (B) in the pressure-sensitive adhesive layer, in some embodiments, the composition of the monomer components for preparing the polymer (B) is such that the polymer (B) has a glass transition temperature T A In relation to T B T A 20°C higher than T B -T A In some preferred embodiments, T B -T A is, for example, 30° C. or higher, more preferably 40° C. or higher, and even more preferably 50° C. or higher, and may be 60° C. or higher, or may be 70° C. or higher. B -T A For example, the temperature may be 130°C or less, 120°C or less, preferably 100°C or less, more preferably 80°C or less, and even more preferably 65°C or less, and may be 55°C or less, or may be 45°C or less.

[0080] Examples of (meth)acrylic monomers that can be used for the monomer raw material B include (meth)acrylic acid alkyl esters. The term "alkyl" used here refers to a chain (including linear and branched) alkyl (group) and does not include the alicyclic hydrocarbon group described below. For example, one or more of the monomers exemplified above as (meth)acrylic acid alkyl esters that can be used for the polymer (A) can be used as constituents of the monomer raw material B. In some embodiments, the monomer raw material B is (meth)acrylic acid C 4-12 Alkyl ester (preferably (meth)acrylic acid C 4-10 Alkyl esters, such as (meth)acrylic acid C 6-10 In some other embodiments, the monomer feedstock B may contain at least one of methacrylic acid C 1-18 Alkyl ester (preferably methacrylic acid C 1-14 Alkyl esters, such as methacrylic acid C 1-10Monomer raw material B may contain, as a (meth)acrylic monomer, one or more selected from the group consisting of MMA, n-butyl methacrylate (BMA), and 2-ethylhexyl methacrylate (2EHMA).

[0081] Other examples of the (meth)acrylic monomer include (meth)acrylic acid esters having an alicyclic hydrocarbon group. For example, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, 1-adamantyl (meth)acrylate, etc. can be used. In some embodiments, monomer raw material B may contain at least one (meth)acrylic monomer selected from dicyclopentanyl methacrylate, isobornyl methacrylate, and cyclohexyl methacrylate.

[0082] The content of the (meth)acrylic acid alkyl ester and the (meth)acrylic acid ester having an alicyclic hydrocarbon group in the monomer raw material B may be, for example, 10% by weight or more and 95% by weight or less, 20% by weight or more and 95% by weight or less, 30% by weight or more and 90% by weight or less, 40% by weight or more and 90% by weight or less, or 50% by weight or more and 85% by weight or less. From the viewpoint of ease of increasing adhesive strength by heating, the use of a (meth)acrylic acid alkyl ester may be advantageous. In some embodiments, the content of the (meth)acrylic acid ester having an alicyclic hydrocarbon group may be less than 50% by weight, less than 30% by weight, less than 15% by weight, less than 10% by weight, or less than 5% by weight of the monomer raw material B. The (meth)acrylic acid ester having an alicyclic hydrocarbon group need not be used.

[0083] In some preferred embodiments, the (meth)acrylic monomer, which is a component of the monomer raw material B, may contain a monomer M2 having a homopolymer Tg of 50°C or higher. By copolymerizing the monomer S1 and the monomer M2 in the polymer (B), the mobility and movability of the polyorganosiloxane structural portion with increasing temperature are suitably controlled, making it easier to achieve both easy initial releasability (reworkability) and increased adhesive strength after heating. In some embodiments, the Tg of the homopolymer of the monomer M2 may be 60°C or higher, 70°C or higher, 80°C or higher, or 90°C or higher. The upper limit of the Tg of the homopolymer of the monomer M2 is not particularly limited, but from the viewpoint of ease of synthesis of the polymer (B), it is usually appropriate for it to be 200°C or lower. In some embodiments, the Tg of the homopolymer of the monomer M2 may be, for example, 180°C or lower, 150°C or lower, or 120°C or lower.

[0084] As the monomer M2, for example, from among the (meth)acrylic monomers exemplified above, those whose homopolymer Tg satisfies the conditions can be used. For example, one or more monomers selected from the group consisting of (meth)acrylic acid alkyl esters and (meth)acrylic acid esters having an alicyclic hydrocarbon group can be used. As the (meth)acrylic acid alkyl ester, a methacrylic acid alkyl ester having an alkyl group with 1 to 4 carbon atoms can be preferably used.

[0085] In embodiments in which the monomer starting material B contains the monomer M2, the content of the monomer M2 may be, for example, 5% by weight or more, 10% by weight or more, 15% by weight or more, 20% by weight or more, 25% by weight or more, or 30% by weight or more of the monomer starting material B. In some embodiments, the content of the monomer M2 may be 35% by weight or more, 40% by weight or more, 45% by weight or more, 50% by weight or more, or 55% by weight or more of the monomer starting material B. The content of the monomer M2 may be, for example, 90% by weight or less, typically 80% by weight or less, preferably 75% by weight or less, or may be 70% by weight or less, or may be 65% by weight or less. In some preferred embodiments, the content of the monomer M2 is 60% by weight or less (e.g., 50% by weight or less, typically 42% by weight or less). By limiting the copolymerization ratio of monomer M2 having a Tg of 50° C. or higher in polymer (B) to a predetermined value or less, it is possible to preferably achieve an increase in adhesive strength after heating based on the mobility of polymer (B) at around 50° C. From the same viewpoint, the content of monomer M2 in monomer raw material B may be 35% by weight or less, 25% by weight or less, or 15% by weight or less (e.g., 5% by weight or less).

[0086] The content of the monomer M2 can be preferably applied, for example, to an embodiment in which the monomer M2 is composed of one or more monomers selected from the group consisting of (meth)acrylic acid alkyl esters and the (meth)acrylic acid esters having an alicyclic hydrocarbon group, or an embodiment in which the monomer M2 is composed of one or more monomers selected from (meth)acrylic acid alkyl esters (e.g., methacrylic acid alkyl esters). One preferred example of such an embodiment is an embodiment in which the monomer M2 is composed of MMA.

[0087] In some embodiments, the (meth)acrylic monomer may contain a monomer M3 having a homopolymer Tg of less than 50°C (typically, -20°C or more and less than 50°C). Use of the monomer M3 makes it easier to obtain a reinforcing film that has a good balance between adhesive strength and cohesive strength after the adhesive strength is increased. From the viewpoint of easily achieving this effect, it is preferable to use the monomer M3 in combination with the monomer M2.

[0088] As the monomer M3, for example, one or more monomers selected from the group consisting of (meth)acrylic acid alkyl esters can be used, the Tg of which of the homopolymer satisfies the conditions, selected from the (meth)acrylic monomers exemplified above.

[0089] In an embodiment in which monomer starting material B contains monomer M3, the content of monomer M3 may be, for example, 5% by weight or more, 10% by weight or more, 15% by weight or more, 20% by weight or more, 25% by weight or more, 30% by weight or more, or 35% by weight or more of monomer starting material B. The content of monomer M3 is usually suitably 70% by weight or less, 60% by weight or less, or 50% by weight or less of monomer starting material B. The above content of monomer M3 is preferably applied, for example, to an embodiment in which monomer M3 consists of one or more monomers selected from (meth)acrylic acid alkyl esters (e.g., methacrylic acid alkyl esters).

[0090] In some embodiments of the reinforcing film disclosed herein, the monomer raw material B preferably contains 30% by weight or less of a monomer whose homopolymer Tg is higher than 170°C. Herein, unless otherwise specified, the term "a monomer content of X% by weight or less" refers to an embodiment in which the content of the monomer is 0% by weight, i.e., an embodiment in which the monomer is substantially not contained. Furthermore, "substantially not contained" means that the monomer is not used, at least intentionally. If the copolymerization ratio of a monomer whose homopolymer Tg is higher than 170°C is high, the mobility of polymer (B) tends to be insufficient, and it may be difficult to increase the adhesive strength by heating to a temperature range higher than 50°C.

[0091] In some embodiments, the monomer raw material B preferably contains at least MMA as a (meth)acrylic monomer. Polymer (B) copolymerized with MMA facilitates the production of a reinforcing film with high adhesive strength after heating. The proportion of MMA in the total amount of (meth)acrylic monomers contained in the monomer raw material B may be, for example, 5% by weight or more, 10% by weight or more, 20% by weight or more, 30% by weight or more, or 40% by weight or more. Furthermore, the proportion of MMA in the total amount of the monomer raw material B is typically 95% by weight or less. In some preferred embodiments, the proportion of MMA in the total amount of the monomer raw material B may be 75% by weight or less, 65% by weight or less, 60% by weight or less, or 55% by weight or less (e.g., 50% by weight or less) from the viewpoint of increasing adhesive strength after heating.

[0092] Other examples of monomers that can be contained together with monomer S1 as a monomer unit constituting polymer (B) include the carboxyl group-containing monomers, acid anhydride group-containing monomers, hydroxyl group-containing monomers, epoxy group-containing monomers, cyano group-containing monomers, isocyanate group-containing monomers, amide group-containing monomers, monomers having a nitrogen atom-containing ring (N-vinyl cyclic amides, cyclic amides having a (meth)acryloyl group, monomers having a succinimide skeleton, maleimides, itaconimides, etc.), aminoalkyl (meth)acrylates, vinyl esters, vinyl ethers, olefins, (meth)acrylic acid esters having an aromatic hydrocarbon group, heterocyclic ring-containing (meth)acrylates, halogen atom-containing (meth)acrylates, and (meth)acrylic acid esters obtained from terpene compound derivative alcohols, etc.

[0093] Further examples of monomers that can be contained together with the monomer S1 as a monomer unit constituting the polymer (B) include oxyalkylene di(meth)acrylates such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, and tripropylene glycol di(meth)acrylate; monomers having a polyoxyalkylene skeleton, for example, polymerizable polyoxyalkylene ethers having a polymerizable functional group such as a (meth)acryloyl group, a vinyl group, or an allyl group at one end of the polyoxyalkylene chain, such as polyethylene glycol or polypropylene glycol, and an ether structure (such as an alkyl ether, an aryl ether, or an aryl alkyl ether) at the other end; methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, and propoxyethyl (meth)acrylate. alkoxyalkyl (meth)acrylates such as butoxyethyl (meth)acrylate and ethoxypropyl (meth)acrylate; salts such as alkali metal (meth)acrylate salts; polyvalent (meth)acrylates such as trimethylolpropane tri(meth)acrylate; halogenated vinyl compounds such as vinylidene chloride and 2-chloroethyl (meth)acrylate; oxazoline group-containing monomers such as 2-vinyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, and 2-isopropenyl-2-oxazoline; aziridine group-containing monomers such as (meth)acryloylaziridine and 2-aziridinylethyl (meth)acrylate; hydroxyl group-containing vinyl monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and adducts of lactones and 2-hydroxyethyl (meth)acrylate; fluorine-containing vinyl monomers such as fluorine-substituted alkyl (meth)acrylates; reactive halogen-containing vinyl monomers such as 2-chloroethyl vinyl ether and monochlorovinyl acetate;Examples of suitable vinyl monomers include organosilicon-containing vinyl monomers such as vinyltrimethoxysilane, γ-(meth)acryloxypropyltrimethoxysilane, allyltrimethoxysilane, trimethoxysilylpropylallylamine, and 2-methoxyethoxytrimethoxysilane; and macromonomers having a radically polymerizable vinyl group at the end of a monomer obtained by polymerizing a vinyl group. These may be copolymerized with monomer S1 either alone or in combination of two or more.

[0094] In some embodiments, the polymer (B) preferably does not have a functional group that undergoes a crosslinking reaction with the polymer (A). In other words, the polymer (B) is preferably contained in the pressure-sensitive adhesive layer in a form that is not chemically bonded to the polymer (A). A pressure-sensitive adhesive layer containing the polymer (B) in such a form has good mobility of the polymer (B) when heated, and is suitable for improving the rate of increase in adhesive strength. The functional group that undergoes a crosslinking reaction with the polymer (A) may vary depending on the type of functional group possessed by the polymer (A), and may be, for example, an epoxy group, an isocyanate group, a carboxy group, an alkoxysilyl group, an amino group, etc.

[0095] The Mw of polymer (B) is not particularly limited. The Mw of polymer (B) may be, for example, 1,000 or more, or 5,000 or more. In some preferred embodiments, from the viewpoint of favorably exhibiting an increase in adhesive strength after heating, the Mw of polymer (B) is 10,000 or more, more preferably 12,000 or more, or 15,000 or more, or 20,000 or more, or 22,000 or more, or 25,000 or more. In other embodiments, the Mw of polymer (B) may be 30,000 or more, or 50,000 or more, or 70,000 or more. The upper limit of the Mw of polymer (B) is, for example, 500,000 or less, or 350,000 or less, or 200,000 or less, or 150,000 or less. From the viewpoint of adjusting the compatibility and mobility within the pressure-sensitive adhesive layer within an appropriate range and suitably exhibiting low adhesiveness in the initial stage of application, in some preferred embodiments, the Mw of the polymer (B) is 100,000 or less, more preferably 80,000 or less, even more preferably 60,000 or less, particularly preferably 40,000 or less (e.g., 30,000 or less), and may be 25,000 or less, or even 20,000 or less. By setting the Mw of the polymer (B) within an appropriate range, a pressure-sensitive adhesive that is excellent in both easy peelability and increased adhesive strength in the initial stage of application can be easily obtained.

[0096] In some preferred embodiments, the Mw of the polymer (B) is preferably lower than the Mw of the polymer (A). This makes it easier to realize a reinforcing film that has both good reworkability at the initial stage of application and increased adhesive strength after heating. In some embodiments, the Mw of the polymer (B) may be, for example, 0.8 times or less, 0.75 times or less, 0.5 times or less, or 0.3 times or less of the Mw of the polymer (A). In some preferred embodiments, the Mw of the polymer (A) may be, for example, 0.8 times or less, 0.75 times or less, 0.5 times or less, or 0.3 times or less. A Mw of polymer (B) B The ratio (Mw B / Mw A ) is 0.3 or less, more preferably 0.2 or less, even more preferably 0.1 or less, and particularly preferably 0.06 or less (for example, 0.05 or less). B / MwA ) is suitably, for example, 0.010 or more, preferably 0.020 or more, more preferably 0.03 or more, and even more preferably 0.04 or more. By setting the Mw of polymer (A) and the Mw of polymer (B) within appropriate ranges, the effects of the technology disclosed herein can be better realized. In some other embodiments, the Mw of polymer (B) may be 0.03 times or less (e.g., 0.02 times or less) the Mw of polymer (A).

[0097] The polymer (B) can be prepared, for example, by polymerizing the above-mentioned monomers by a known method such as solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization, or photopolymerization.

[0098] A chain transfer agent can be used as needed to adjust the molecular weight of the polymer (B). Examples of the chain transfer agent include compounds having a mercapto group, such as octyl mercaptan, lauryl mercaptan, t-nonyl mercaptan, t-dodecyl mercaptan, mercaptoethanol, and α-thioglycerol; thioglycolic acid esters, such as thioglycolic acid, methyl thioglycolate, ethyl thioglycolate, propyl thioglycolate, butyl thioglycolate, t-butyl thioglycolate, 2-ethylhexyl thioglycolate, octyl thioglycolate, isooctyl thioglycolate, decyl thioglycolate, dodecyl thioglycolate, thioglycolic acid ester of ethylene glycol, thioglycolic acid ester of neopentyl glycol, and thioglycolic acid ester of pentaerythritol; and α-methylstyrene dimer. The chain transfer agent can be used alone or in combination of two or more.

[0099] The amount of chain transfer agent used is not particularly limited, but is typically 0.05 to 20 parts by weight, preferably 0.1 to 15 parts by weight, and more preferably 0.2 to 10 parts by weight, per 100 parts by weight of monomer. By adjusting the amount of chain transfer agent added in this manner, a polymer (B) with a suitable molecular weight can be obtained. In some preferred embodiments, the amount of chain transfer agent used is 5 parts by weight or less, more preferably 3 parts by weight or less, and even more preferably 2 parts by weight or less, per 100 parts by weight of monomer, and may be 1.5 parts by weight or less, or even 1 part by weight or less.

[0100] As a means for adjusting the molecular weight of polymer (B), various conventionally known means, including the use of the chain transfer agent, can be used alone or in appropriate combination. The same applies to the molecular weight of polymer (A). Non-limiting examples of such means include selection of the polymerization method, selection of the type and amount of polymerization initiator used, selection of the polymerization temperature, selection of the type and amount of polymerization solvent used in solution polymerization, selection of light irradiation intensity in photopolymerization, etc. Those skilled in the art would understand how to obtain a polymer having a desired molecular weight based on the description of the present specification, including the specific examples described below, and the common general technical knowledge at the time of filing of this application.

[0101] In the reinforcing film disclosed herein, the amount of polymer (B) used per 100 parts by weight of polymer (A) can be, for example, 0.1 parts by weight or more, and from the viewpoint of obtaining a higher effect (preferably, easy peelability at the initial stage of application), it is preferably 0.2 parts by weight or more. In some embodiments, from the viewpoint of improving reworkability, the amount of polymer (B) used is suitably 0.3 parts by weight or more, more preferably 0.5 parts by weight or more, and may be 0.8 parts by weight or more, 1.0 parts by weight or more, 1.5 parts by weight or more, 2.0 parts by weight or more, 3.0 parts by weight or more, 4.0 parts by weight or more, or 5.0 parts by weight or more. Furthermore, the amount of polymer (B) used per 100 parts by weight of polymer (A) may be, for example, 75 parts by weight or less, 30 parts by weight or less, or 20 parts by weight or less, or 15 parts by weight or less, or 10 parts by weight or less. From the viewpoint of facilitating the increase in adhesive strength after the increase in adhesive strength, in some embodiments, the amount of polymer (B) used relative to 100 parts by weight of polymer (A) is preferably 8.0 parts by weight or less, more preferably 5.0 parts by weight or less, and even more preferably 4.5 parts by weight or less, and may be 3.5 parts by weight or less, 3.0 parts by weight or less, or 2.5 parts by weight or less (for example, 2.0 parts by weight or less). By setting the amount of polymer (B) used within the above range, it is possible to better achieve both easy peelability at the initial stage of application and increased adhesive strength, and it is also easy to increase flexibility (particularly flexibility at low temperatures).

[0102] The pressure-sensitive adhesive layer may optionally contain a polymer (optional polymer) other than polymer (A) and polymer (B), provided that the performance of the reinforcing film disclosed herein is not significantly impaired. Non-limiting examples of such optional polymers include rubber-based polymers, polyester-based polymers, urethane-based polymers, polyether-based polymers, silicone-based polymers, polyamide-based polymers, fluorine-based polymers, and the like known in the field of pressure-sensitive adhesives, as well as acrylic polymers that do not fall under either polymer (A) or polymer (B). The amount of the optional polymer used is typically 20% by weight or less of the total polymer components contained in the pressure-sensitive adhesive layer, and may be 15% by weight or less, or 10% by weight or less. In some embodiments, the amount of the optional polymer used may be 5% by weight or less, 3% by weight or less, or 1% by weight or less of the total polymer components. The pressure-sensitive adhesive layer may essentially contain no polymers other than polymer (A) and polymer (B).

[0103] (Zirconium-Containing Compound) The pressure-sensitive adhesive layer disclosed herein further contains a zirconium (Zr)-containing compound in addition to the polymer (A) and polymer (B). Appropriate use of the Zr-containing compound makes it possible to achieve both good flexibility (particularly flexibility in the low temperature range), easy initial peelability, and high adhesive strength after adhesive strength increase. The Zr-containing compound can be used alone or in combination of two or more. The Zr-containing compound is preferably an organic zirconium-containing compound. For example, one or more selected from Zr-containing organometallic catalysts (typically organic compounds having Zr in the active center) can be used as the Zr-containing compound in the technology disclosed herein.

[0104] The Zr-containing compound (organic zirconium-containing compound) is not particularly limited, and examples thereof include zirconium tetraacetylacetonate, zirconium monoacetylacetonate, zirconium ethylacetoacetate, zirconium octylate compounds, etc. More specific examples include zirconium alkoxides such as tetraethoxyzirconium, tetra-n-propoxyzirconium, tetra-i-propoxyzirconium, tetra-n-butoxyzirconium (normal butyl zirconate), tetra-i-butoxyzirconium, tetra-sec-butoxyzirconium, and tetra-t-butoxyzirconium; triethoxy mono(acetylacetonate)zirconium, tri-n-propoxy mono(acetylacetonate)zirconium; Tri-i-propoxy mono(acetylacetonate)zirconium, tri-n-butoxy mono(acetylacetonate)zirconium, tri-sec-butoxy mono(acetylacetonate)zirconium, tri-t-butoxy mono(acetylacetonate)zirconium, diethoxy bis(acetylacetonate)zirconium, di-n-propoxy bis(acetylacetonate)zirconium, di-i-propoxy bis(acetylacetonate)zirconium, -n-butoxy bis(acetylacetonate)zirconium, di-sec-butoxy bis(acetylacetonate)zirconium, di-t-butoxy bis(acetylacetonate)zirconium, monoethoxy tris(acetylacetonate)zirconium, mono-n-propoxy tris(acetylacetonate)zirconium, mono-i-propoxy tris(acetylacetonate)zirconium, mono-n-butoxy tris(acetylacetonate)zirconium , mono-sec-butoxy tris(acetylacetonate)zirconium, mono-t-butoxy tris(acetylacetonate)zirconium, tetrakis(acetylacetonate)zirconium, triethoxy mono(ethylacetoacetate)zirconium, tri-n-propoxy mono(ethylacetoacetate)zirconium, tri-i-propoxy mono(ethylacetoacetate)zirconium, tri-n-butoxy mono(ethylacetoacetate)zirconium,Tri-sec-butoxy mono(ethylacetoacetate)zirconium, tri-t-butoxy mono(ethylacetoacetate)zirconium, diethoxy bis(ethylacetoacetate)zirconium, di-n-propoxy bis(ethylacetoacetate)zirconium, di-i-propoxy bis(ethylacetoacetate)zirconium, di-n-butoxy bis(ethylacetoacetate)zirconium, di-sec-butoxy bis(ethylacetoacetate)zirconium, di-t-butoxy bis(ethylacetoacetate)zirconium, monoethoxy tris(ethylacetoacetate)zirconium , zirconium chelates such as mono-n-propoxy tris(ethylacetoacetate)zirconium, mono-i-propoxy tris(ethylacetoacetate)zirconium, mono-n-butoxy tris(ethylacetoacetate)zirconium, mono-sec-butoxy tris(ethylacetoacetate)zirconium, mono-t-butoxy tris(ethylacetoacetate)zirconium, tetrakis(ethylacetoacetate)zirconium, mono(acetylacetonato)tris(ethylacetoacetate)zirconium, bis(acetylacetonato)bis(ethylacetoacetate)zirconium, and tris(acetylacetonato)mono(ethylacetoacetate)zirconium; and the like. The above organic zirconium-containing compounds can be used alone or in combination of two or more.

[0105] The preferred amount of the Zr-containing compound to be used is the ratio of the amount of the polymer (A) to the amount of the nitrogen-containing monomer-derived monomer units contained in the polymer (A), W N In some embodiments, the amount of the Zr-containing compound W relative to 100 parts by weight of the polymer (A) may be set based on the following: Zr [Parts by weight] is the amount W of monomer units derived from the nitrogen-containing monomer per 100 parts by weight of the polymer (A). N In relation to [parts by weight], the above W Zr [Parts by weight] N [weight parts] ratio (W N / W Zr) is an amount such that the value of the Zr-containing compound is 4 or more. Zr [Parts by weight] N [weight parts] ratio (W N / W Zr ) is 4 or more, so that W N By limiting the ratio (W) to 14 parts by weight or less, in a configuration suitable for improving flexibility (particularly flexibility in a low temperature range), it is possible to achieve both easy initial peelability and high adhesive strength after the adhesive strength has increased. Without wishing to be bound by theory, the reason for obtaining such an effect is that in a pressure-sensitive adhesive containing a combination of a polymer (A) containing a monomer unit derived from a nitrogen-containing monomer, a polymer (B), and a Zr-containing compound, the Zr-containing compound has the effect of making the polymer (A) more easily attracted to the surface of an adherend (for example, a polyimide film), and this effect becomes apparent with the passage of time and / or by heating after application to the adherend, and the ratio (W) N / W Zr ) in an appropriate range is thought to contribute to improving the adhesive strength after the adhesive strength has increased. However, the present invention is not limited to this reason alone.

[0106] In order to more effectively enhance the adhesive strength after the adhesive strength increase (for example, adhesive strength after heating N2), in some embodiments, the ratio (W N / W Zr ) is suitably 5 or more, advantageously 7 or more, and preferably 9 or more, and may be, for example, 10 or more, 12 or more, 14 or more, or 16 or more. N / W Zr The upper limit of the ratio (W) is not particularly limited and can be appropriately set within a range in which the desired effect is obtained. N / W Zr ) may be, for example, 2000 or less, 1400 or less, 1000 or less, 700 or less, 500 or less, 300 or less, 250 or less, or 200 or less.

[0107] In some embodiments in which the polymer (A) contains a monomer unit derived from a monomer having a nitrogen atom-containing ring, the amount W of the monomer unit derived from the monomer having a nitrogen atom-containing ring contained in 100 parts by weight of the polymer (A) is RN [Parts by weight] of the above W Zr The ratio to [parts by weight] (i.e., the ratio (W RN / W Zr The lower limit of the ratio (W N / W Zr ) can be used. RN / W Zr ) is the upper limit of the above ratio (W N / W Zr ) or the lower limit thereof may be adopted.

[0108] The amount of Zr-containing compound W relative to 100 parts by weight of polymer (A) Zr is not particularly limited, and can be, for example, in the range of about 0.0001 to 3 parts by weight. Zr In an embodiment in which the Zr-containing compound can also function as a crosslinking catalyst (for example, an embodiment in which the pressure-sensitive adhesive layer contains an isocyanate-based crosslinking agent), the amount W of the Zr-containing compound can be, for example, 0.001 parts by weight or more, 0.005 parts by weight or more, or 0.008 parts by weight or more. Zr In view of this, in some embodiments, the amount W of the Zr-containing compound is preferably 0.1 to 0.5. Zr The amount W of the Zr-containing compound relative to 100 parts by weight of the polymer (A) may be 0.01 parts by weight or more, 0.03 parts by weight or more, 0.05 parts by weight or more, or 0.1 parts by weight or more. Zr is preferably 2 parts by weight or less, more preferably 1.5 parts by weight or less (e.g., 1 part by weight or less, 0.7 parts by weight or less, or 0.5 parts by weight or less), and the ratio (W N / W Zr ) can be set to be 4 or more (for example, 5 or more, 7 or more, or 9 or more). ZrAppropriately limiting the adhesive strength can be advantageous in terms of adhesive strength and flexibility after the adhesive strength is increased.

[0109] The adhesive layer disclosed herein may contain one or more metal compounds (typically organometallic catalysts) other than the Zr-containing compound for the purpose of promoting crosslinking reactions, etc. Examples of such metal compounds include tin (Sn)-containing compounds (tin-based catalysts), titanium (Ti)-containing compounds (titanium-based catalysts), hafnium (Hf)-containing compounds (hafnium-based catalysts), iron (Fe)-containing compounds (iron-based catalysts), aluminum (Al)-containing compounds (aluminum-based catalysts), zinc (Zn)-containing compounds (zinc-based catalysts), and bismuth (Bi)-containing compounds (bismuth-based catalysts). In some embodiments, the amount of metal compounds other than the Zr-containing compound used is suitably less than the amount of the Zr-containing compound used (i.e., less than 1 times the amount of the Zr-containing compound used) by weight, preferably less than 0.5 times, more preferably less than 0.3 times or less than 0.1 times. Metal compounds other than the Zr-containing compound may not be used.

[0110] (Crosslinking Agent) A crosslinking agent may be used in the pressure-sensitive adhesive layer, if necessary, for purposes such as adjusting cohesive strength. Examples of crosslinking agents that can be used include crosslinking agents known in the field of pressure-sensitive adhesives, such as epoxy-based crosslinking agents, isocyanate-based crosslinking agents, silicone-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, silane-based crosslinking agents, and alkyl-etherified melamine-based crosslinking agents. Isocyanate-based crosslinking agents and epoxy-based crosslinking agents are preferably used. In some embodiments, isocyanate-based crosslinking agents can be preferably used as crosslinking agents suitable for achieving both increased adhesive strength and flexibility. The crosslinking agents can be used alone or in combination of two or more.

[0111] As the isocyanate-based crosslinking agent, a polyfunctional isocyanate (a compound having an average of two or more isocyanate groups per molecule, including those having an isocyanurate structure) can be preferably used. The isocyanate-based crosslinking agent can be used alone or in combination of two or more.

[0112] Examples of polyfunctional isocyanates include aliphatic polyisocyanates, alicyclic polyisocyanates, and aromatic polyisocyanates. Specific examples of aliphatic polyisocyanates include 1,2-ethylene diisocyanate; tetramethylene diisocyanates such as 1,2-tetramethylene diisocyanate, 1,3-tetramethylene diisocyanate, and 1,4-tetramethylene diisocyanate; hexamethylene diisocyanates such as 1,2-hexamethylene diisocyanate, 1,3-hexamethylene diisocyanate, 1,4-hexamethylene diisocyanate, 1,5-hexamethylene diisocyanate, 1,6-hexamethylene diisocyanate, and 2,5-hexamethylene diisocyanate; 2-methyl-1,5-pentane diisocyanate, 3-methyl-1,5-pentane diisocyanate, and lysine diisocyanate.

[0113] Specific examples of alicyclic polyisocyanates include isophorone diisocyanate; cyclohexyl diisocyanates such as 1,2-cyclohexyl diisocyanate, 1,3-cyclohexyl diisocyanate, and 1,4-cyclohexyl diisocyanate; cyclopentyl diisocyanates such as 1,2-cyclopentyl diisocyanate and 1,3-cyclopentyl diisocyanate; hydrogenated xylylene diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated tetramethylxylene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate.

[0114] Specific examples of aromatic polyisocyanates include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 4,4'-diphenylether diisocyanate, 2-nitrodiphenyl-4,4'-diisocyanate, 2,2'-diphenylpropane-4,4'-diisocyanate, Examples include 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, 4,4'-diphenylpropane diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, naphthylene-1,4-diisocyanate, naphthylene-1,5-diisocyanate, 3,3'-dimethoxydiphenyl-4,4'-diisocyanate, xylylene-1,4-diisocyanate, and xylylene-1,3-diisocyanate.

[0115] A preferred example of the polyfunctional isocyanate is a polyfunctional isocyanate having an average of three or more isocyanate groups per molecule. Such a tri- or higher functional isocyanate may be a multimer (e.g., a dimer or trimer) of a bifunctional or tri- or higher functional isocyanate, a derivative (e.g., an addition reaction product of a polyhydric alcohol with two or more molecules of a polyfunctional isocyanate), a polymer, or the like. Examples of the isocyanate include a dimer or trimer of diphenylmethane diisocyanate, an isocyanurate of hexamethylene diisocyanate (a trimer adduct of an isocyanurate structure), a reaction product of trimethylolpropane and tolylene diisocyanate, a reaction product of trimethylolpropane and hexamethylene diisocyanate, a trimethylolpropane adduct of xylylene diisocyanate, a trimethylolpropane adduct of isophorone diisocyanate, a trimethylolpropane adduct of hexamethylene diisocyanate, polymethylene polyphenyl isocyanate, polyether polyisocyanate, polyester polyisocyanate, and adducts of these with various polyols, and polyfunctional isocyanates such as polyisocyanates multifunctionalized with an isocyanurate bond, a biuret bond, an allophanate bond, or the like.

[0116] Commercially available products of the polyfunctional isocyanate include those manufactured by Asahi Kasei Chemicals Corporation under the trade name "Duranate TPA-100," those manufactured by Tosoh Corporation under the trade names "Coronate L," "Coronate HL," "Coronate HK," "Coronate HX," and "Coronate 2096," and those manufactured by Mitsui Chemicals, Inc. under the trade names "Takenate D110N," "Takenate D120N," "Takenate D140N," and "Takenate D160N."

[0117] Examples of epoxy crosslinking agents include bisphenol A, epichlorohydrin-type epoxy resins, ethylene glycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol glycidyl ether, trimethylolpropane triglycidyl ether, diglycidylaniline, diamine glycidylamine, N,N,N',N'-tetraglycidyl-m-xylylenediamine, and 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane. These may be used alone or in combination of two or more.

[0118] When a crosslinking agent is used, the amount used is not particularly limited and can be, for example, an amount greater than 0 parts by weight per 100 parts by weight of polymer (A). Furthermore, the amount of crosslinking agent used can be, for example, 0.01 parts by weight or more, preferably 0.05 parts by weight or more, per 100 parts by weight of polymer (A). Increasing the amount of crosslinking agent used tends to suppress the initial adhesive strength after application and improve reworkability. In some embodiments, the amount of crosslinking agent used per 100 parts by weight of polymer (A) may be 0.07 parts by weight or more, 0.1 parts by weight or more, or even 0.15 parts by weight or more. On the other hand, from the viewpoint of allowing a moderate amount of movement of polymer (B) and achieving increased adhesive strength after heating, the amount of crosslinking agent used per 100 parts by weight of polymer (A) is typically 15 parts by weight or less, and may be 10 parts by weight or less, or may be 5 parts by weight or less.

[0119] The technology disclosed herein can be preferably implemented in an embodiment using at least an isocyanate-based crosslinking agent as a crosslinking agent. From the viewpoint of achieving both good reworkability at the initial stage of application and increased adhesive strength after heating, in some embodiments, the amount of isocyanate-based crosslinking agent used per 100 parts by weight of polymer (A) can be, for example, 0.01 parts by weight or more, preferably 0.05 parts by weight or more, more preferably 0.07 parts by weight or more, and may be 0.10 parts by weight or more, or even 0.15 parts by weight or more (e.g., 0.20 parts by weight or more). By increasing the amount of isocyanate-based crosslinking agent used, moderate cohesive strength is obtained and initial easy peelability and processability also tend to be excellent. The amount of isocyanate crosslinking agent used per 100 parts by weight of polymer (A) can be, for example, 5 parts by weight or less, preferably less than 1.0 part by weight, more preferably less than 0.5 part by weight, and even more preferably less than 0.3 part by weight, and may be 0.2 parts by weight or less (e.g., less than 0.2 part by weight or less), or may be 0.15 parts by weight or less (e.g., less than 0.15 part by weight). Appropriately limiting the amount of isocyanate crosslinking agent used is advantageous from the viewpoint of improving the flexibility of the adhesive, and also makes it easier to obtain an increase in adhesive strength after heating.

[0120] (Tackifier Resin) The pressure-sensitive adhesive layer may contain a tackifier resin as needed. The tackifier resin is not particularly limited, but examples thereof include rosin-based tackifier resins, terpene-based tackifier resins, phenol-based tackifier resins, hydrocarbon-based tackifier resins, ketone-based tackifier resins, polyamide-based tackifier resins, epoxy-based tackifier resins, and elastomer-based tackifier resins. The tackifier resins may be used alone or in combination of two or more.

[0121] The content of the tackifier resin is not particularly limited and can be set so as to exhibit appropriate adhesive performance depending on the purpose and application. The content of the tackifier resin (when two or more types of tackifier resins are included, the total amount thereof) per 100 parts by weight of polymer (A) can be, for example, about 0.5 to 200 parts by weight, or may be about 0.5 to 100 parts by weight, or about 0.5 to 50 parts by weight. Furthermore, the technology disclosed herein can be preferably implemented in an embodiment in which the amount of tackifier resin used is limited. For example, the content of the tackifier resin per 100 parts by weight of polymer (A) can be less than 20 parts by weight, or may be less than 10 parts by weight, or may be less than 3 parts by weight, or may be less than 1 part by weight (0 parts by weight to less than 1 part by weight). In some embodiments, the PSA layer is substantially free of tackifier resin.

[0122] In addition, the pressure-sensitive adhesive layer in the technology disclosed herein may contain, as needed, known additives that can be used in pressure-sensitive adhesives, such as leveling agents, plasticizers, softeners, colorants (dyes, pigments, etc.), fillers, antistatic agents, antioxidants, UV absorbers, antioxidants, light stabilizers, and preservatives, as long as the effects of the present invention are not significantly impaired.

[0123] The pressure-sensitive adhesive layer constituting the reinforcing film disclosed herein may be a cured layer of a pressure-sensitive adhesive composition. That is, the pressure-sensitive adhesive layer can be formed by applying (e.g., coating) a water-dispersible, solvent-based, photocurable, hot-melt, or other pressure-sensitive adhesive composition to a suitable surface, followed by an appropriate curing treatment. When two or more curing treatments (drying, crosslinking, polymerization, cooling, etc.) are performed, these can be performed simultaneously or in multiple stages. For pressure-sensitive adhesive compositions using a partially polymerized product (polymer syrup) of a monomer raw material, the curing treatment typically involves a final copolymerization reaction. That is, the partially polymerized product is subjected to a further copolymerization reaction to form a fully polymerized product. For example, photocurable pressure-sensitive adhesive compositions are subjected to light irradiation. Curing treatments such as crosslinking and drying may be performed as needed. For example, if a photocurable pressure-sensitive adhesive composition requires drying, photocuring may be performed after drying. For pressure-sensitive adhesive compositions using a fully polymerized product, the curing treatment typically involves drying (heat drying), crosslinking, or other treatments as needed.

[0124] The pressure-sensitive adhesive composition can be applied using a conventional coater such as a gravure roll coater, reverse roll coater, kiss roll coater, dip roll coater, bar coater, knife coater or spray coater.

[0125] The thickness of the pressure-sensitive adhesive layer is not particularly limited and can be, for example, 6 μm or more. In some embodiments, the thickness of the pressure-sensitive adhesive layer may be 8 μm or more, 10 μm or more, 15 μm or more, or 20 μm or more or more than 20 μm. Increasing the thickness of the pressure-sensitive adhesive layer tends to increase the adhesive strength after heating. In addition, in some embodiments, the thickness of the pressure-sensitive adhesive layer may be, for example, 300 μm or less, 200 μm or less, 150 μm or less, 100 μm or less, 70 μm or less, 50 μm or less, or 40 μm or less. Not having an excessively thick pressure-sensitive adhesive layer can be advantageous from the perspective of reducing the thickness of the reinforcing film and preventing cohesive failure of the pressure-sensitive adhesive layer. A reinforcing film having a pressure-sensitive adhesive layer with a thickness within the above-mentioned range can have a good balance between adhesive properties such as adhesive strength and flexibility. In the case of a reinforcing film having a first pressure-sensitive adhesive layer and a second pressure-sensitive adhesive layer on the first and second surfaces of a substrate, the thickness of the pressure-sensitive adhesive layer described above can be applied to at least the thickness of the first pressure-sensitive adhesive layer. The thickness of the second pressure-sensitive adhesive layer can also be selected from a similar range. In the case of a reinforcing film without a substrate, the thickness of the reinforcing film is the same as the thickness of the pressure-sensitive adhesive layer.

[0126] (-20°C storage modulus (G' -20 In some embodiments of the technology disclosed herein, the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer has a storage modulus at −20° C. (hereinafter referred to as “storage modulus (G′ -20 The storage modulus (G') may be, for example, 10,000 kPa, suitably 5,000 kPa or less, advantageously 3,000 kPa or less, and preferably 1,000 kPa or less. -20By limiting the storage modulus (G') of the PSA to a predetermined value or less, the PSA exhibits good flexibility suitable for repeated bending and flexing. From the viewpoint of further enhancing flexibility, in some embodiments, the storage modulus (G') of the PSA is -20 The storage modulus (G') of the pressure-sensitive adhesive is preferably 700 kPa or less, more preferably 500 kPa or less, and even more preferably 300 kPa or less, and may be 200 kPa or less, 150 kPa or less, 140 kPa or less, 130 kPa or less, 120 kPa or less, or 110 kPa or less. -20 The lower limit of the storage modulus (G') of the PSA is not particularly limited, and may be, for example, 20 kPa or more or 30 kPa or more. In some embodiments, taking into consideration the ease of achieving compatibility with other properties (e.g., one or more properties of a low initial adhesive strength N1, a high adhesive strength after heating, and a high rate of increase N2 / N1), the storage modulus (G') of the PSA is -20 ) may be, for example, 50 kPa or more, 70 kPa or more, 80 kPa or more, 90 kPa or more, or 100 kPa or more.

[0127] (23°C storage modulus (G' 23 )) The storage modulus of the pressure-sensitive adhesive at 23°C (hereinafter referred to as "storage modulus (G' 23 The storage modulus (G') is not particularly limited. -20 In some embodiments, the storage modulus (G') of the PSA is preferably within a range in which the storage modulus (G') is equal to or less than any of the upper limits described above. 23 The storage modulus (G') is preferably 200 kPa or less. 23 Generally, adhesives having a storage modulus (G') of a predetermined value or less tend to have excellent strain relaxation properties at room temperature and are also likely to exhibit increased adhesive strength. 23 In some preferred embodiments, the bulk modulus G' is preferably 130 kPa or less, more preferably 80 kPa or less. 23 may be 50 kPa or less, or 40 kPa or less (for example, 35 kPa or less).

[0128] In some embodiments, the storage modulus (G' 23The storage modulus (G') is suitably 10 kPa or more. 23 By setting the storage modulus (G') to a predetermined value or more, the adhesive strength at the initial stage of application tends to fall within a suitable range in which the adhesive strength is excellent in easy peelability. 23 ) is preferably 15 kPa or more, more preferably 20 kPa or more, may be 25 kPa or more, or may be 30 kPa or more.

[0129] (80°C storage modulus (G' 80 )) The storage modulus of the pressure-sensitive adhesive at 80°C (hereinafter referred to as "storage modulus (G' 80 The storage modulus (G') is not particularly limited. -20 In some embodiments, the storage modulus (G') of the pressure-sensitive adhesive layer is preferably within a range in which the storage modulus (G') is equal to or less than any of the upper limits described above. 80 ) is suitably 100 kPa or less, preferably 70 kPa or less, more preferably 50 kPa or less, and may be 30 kPa or less, or may be 20 kPa or less.

[0130] In some embodiments, the storage modulus (G' 80 The storage modulus (G') is suitably 1 kPa or more, and preferably 2 kPa or more. 80 ) being a predetermined value or more can be advantageous in terms of heat resistance of the PSA (e.g., adhesive properties in a high temperature range). 80 ) may be, for example, 3 kPa or more, 5 kPa or more, 7 kPa or more, 9 kPa or more, or 10 kPa or more.

[0131] The storage modulus of the pressure-sensitive adhesive layer at each temperature can be adjusted by the type and characteristics (molecular weight, glass transition temperature, molecular structure, etc.) of the polymer (A), the type (chemical structure, etc.) and characteristics (molecular weight, glass transition temperature, etc.) of the polymer (B), the amount used, the type and amount used of the crosslinking agent, etc. The storage modulus (G') of the pressure-sensitive adhesive layer at -20°C -20 The storage modulus at other temperatures can also be measured in a similar manner.

[0132] <Supporting Substrate> The reinforcing film according to some embodiments may be in the form of a substrate-attached pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer on one or both sides of the supporting substrate. The material of the supporting substrate is not particularly limited and can be appropriately selected depending on the purpose and mode of use of the reinforcing film. Non-limiting examples of usable substrates include resin films such as plastic films; foam sheets made of foams such as polyurethane foam, polyethylene foam, and polychloroprene foam; woven and nonwoven fabrics made by single or mixed spinning of various fibrous materials (natural fibers such as hemp and cotton, synthetic fibers such as polyester and vinylon, semi-synthetic fibers such as acetate, etc.); papers such as Japanese paper, fine paper, kraft paper, and crepe paper; metal foils such as aluminum foil and copper foil; and the like. Substrates having a composite structure of these may also be used. Examples of such composite substrates include substrates having a structure in which metal foil and the above-mentioned plastic film are laminated, and plastic substrates reinforced with inorganic fibers such as glass cloth.

[0133] Various film substrates can be preferably used as the substrate of the reinforcing film disclosed herein. The film substrate may be a porous substrate such as a foam film or a nonwoven fabric sheet, a nonporous substrate, or a substrate having a structure in which a porous layer and a nonporous layer are laminated. In some embodiments, the film substrate preferably includes a base film that is capable of independently maintaining its shape (self-supporting or independent). Here, "resin film" refers to a resin film with a nonporous structure that is typically substantially bubble-free (void-free). Therefore, the resin film is a concept that is distinct from foam films and nonwoven fabrics. The resin film preferably has an independently shape-maintaining (self-supporting or independent) structure. The resin film may have a single-layer structure or a multilayer structure of two or more layers (e.g., a three-layer structure).

[0134] Examples of resin materials that can be used to form the resin film include polyester, polyolefin, polyamide (PA) such as nylon 6, nylon 66, and partially aromatic polyamide, polyimide (PI), polyamideimide (PAI), polyetheretherketone (PEEK), polyethersulfone (PES), polyphenylene sulfide (PPS), polycarbonate (PC), polyurethane (PU), ethylene-vinyl acetate copolymer (EVA), and fluororesins such as polytetrafluoroethylene (PTFE), acrylic resin, polyacrylate, polystyrene, polyvinyl chloride, and polyvinylidene chloride. The resin film may be formed using a resin material containing one of these resins alone, or may be formed using a resin material containing a blend of two or more of these resins. The resin film may be unstretched or stretched (e.g., uniaxially or biaxially stretched).

[0135] Suitable examples of resin materials constituting the resin film include polyimide-based resins, polyester-based resins, PPS resins, and polyolefin-based resins. Here, polyimide-based resins refer to resins containing more than 50% by weight of polyimide. Similarly, polyester-based resins refer to resins containing more than 50% by weight of polyester, PPS resins refer to resins containing more than 50% by weight of PPS, and polyolefin-based resins refer to resins containing more than 50% by weight of polyolefin.

[0136] Specific examples of polyester resins include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), and polybutylene naphthalate.

[0137] As the polyolefin resin, one type of polyolefin can be used alone, or two or more types of polyolefins can be used in combination. The polyolefin can be, for example, an α-olefin homopolymer, a copolymer of two or more types of α-olefins, or a copolymer of one or more types of α-olefins with other vinyl monomers. Specific examples include polyethylene (PE), polypropylene (PP), poly-1-butene, poly-4-methyl-1-pentene, ethylene-propylene copolymers such as ethylene propylene rubber (EPR), ethylene-propylene-butene copolymers, ethylene-butene copolymers, ethylene-vinyl alcohol copolymers, and ethylene-ethyl acrylate copolymers. Both low-density (LD) polyolefins and high-density (HD) polyolefins can be used. Examples of polyolefin resin films include unstretched polypropylene (CPP) films, biaxially oriented polypropylene (OPP) films, low-density polyethylene (LDPE) films, linear low-density polyethylene (LLDPE) films, medium-density polyethylene (MDPE) films, high-density polyethylene (HDPE) films, polyethylene (PE) films blended with two or more types of polyethylene (PE), and PP / PE blend films blended with polypropylene (PP) and polyethylene (PE).

[0138] Specific examples of resin films that can be preferably used as the base film of the reinforcing film disclosed herein include PI film, PET film, PEN film, PPS film, PEEK film, CPP film and OPP film.

[0139] The resin film may contain known additives such as light stabilizers, antioxidants, antistatic agents, colorants (dyes, pigments, etc.), fillers, slip agents, antiblocking agents, etc., as needed, provided that the effects of the present invention are not significantly impaired. The amount of additives added is not particularly limited and can be appropriately determined depending on the purpose, etc.

[0140] The method for producing the resin film is not particularly limited, and any conventionally known resin film forming method such as extrusion molding, inflation molding, T-die casting, or calendar roll molding can be appropriately employed.

[0141] The substrate may be substantially composed of such a base film. Alternatively, the substrate may include an auxiliary layer in addition to the base film. Examples of the auxiliary layer include an optical property adjusting layer (e.g., a coloring layer, an anti-reflection layer), a printing layer or a laminating layer for imparting a desired appearance to the substrate, an antistatic layer, an undercoat layer, a release layer, or other surface treatment layer.

[0142] The thickness of the substrate is not particularly limited and can be selected depending on the purpose and mode of use of the reinforcing film. The thickness of the substrate can be, for example, 1000 μm or less. In some embodiments, from the viewpoint of the handleability and processability of the reinforcing film, the thickness of the substrate can be, for example, 500 μm or less, 300 μm or less, 250 μm or less, or 200 μm or less. In some embodiments, from the viewpoint of miniaturization and weight reduction of the product to which the reinforcing film is applied, the thickness of the substrate can be, for example, 160 μm or less, 130 μm or less, 100 μm or less, 90 μm or less, 80 μm or less, 60 μm or less, 50 μm or less, 25 μm or less, 10 μm or less, or 5 μm or less. As the thickness of the substrate decreases, the flexibility of the reinforcing film and its ability to conform to the surface shape of the adherend tend to improve. Furthermore, from the viewpoint of handleability and processability, the thickness of the substrate may be, for example, 2 μm or more, 5 μm or more, 10 μm or more, 20 μm or more, 25 μm or more, or more than 25 μm. In some embodiments, the thickness of the substrate may be, for example, 30 μm or more, 35 μm or more, 55 μm or more, 70 μm or more, 75 μm or more, 90 μm or more, or 120 μm or more. From the viewpoint of reinforcement performance, in some embodiments, a substrate having a thickness of 30 μm or more (e.g., 45 μm or more, 55 μm or more, or 65 μm or more) may be preferably used.

[0143] The first surface of the substrate may be subjected to conventional surface treatments, such as corona discharge treatment, plasma treatment, ultraviolet irradiation treatment, acid treatment, alkali treatment, or the formation of an undercoat layer by applying a primer. Such surface treatments may be intended to improve the anchoring ability of the pressure-sensitive adhesive layer to the substrate. For example, a substrate that has been subjected to such an anchoring ability-improving treatment may be preferably used in a reinforcing film having a substrate containing a resin film as a base film. The above surface treatments may be applied alone or in combination. The composition of the primer used to form the undercoat layer is not particularly limited and may be appropriately selected from known primers. The thickness of the undercoat layer is not particularly limited, but is typically approximately 0.01 μm to 1 μm, and preferably approximately 0.1 μm to 1 μm. Other treatments that may be applied to the first surface of the substrate, if necessary, include antistatic layer formation, colored layer formation, printing, etc.

[0144] When the reinforcing film disclosed herein is in the form of a single-sided PSA sheet having a PSA layer only on the first surface of the substrate, the second surface of the substrate may be subjected to a conventional surface treatment, such as a release treatment or an antistatic treatment, as needed. For example, by surface treating the back surface of the substrate with a release agent (typically by providing a release layer made of a release agent), the unwinding force of the reinforcing film wound into a roll can be reduced. Examples of release agents that can be used include silicone-based release agents, long-chain alkyl-based release agents, olefin-based release agents, fluorine-based release agents, fatty acid amide-based release agents, molybdenum sulfide, and silica powder. Furthermore, for purposes such as improving printability, reducing light reflectivity, and improving overlapping properties, the second surface of the substrate may be subjected to a corona discharge treatment, plasma treatment, ultraviolet irradiation treatment, acid treatment, alkali treatment, or the like. Furthermore, in the case of a double-sided PSA sheet, the second surface of the substrate may be subjected to a surface treatment similar to the examples given above for the surface treatment that can be applied to the first surface of the substrate, as needed. The surface treatments applied to the first surface and the second surface of the substrate may be the same or different.

[0145] <Characteristics of the Reinforcing Film> The reinforcing film disclosed herein preferably has an initial adhesive strength N1 measured after laminating to a polyimide film and maintaining at 23°C for 30 minutes, which is limited to a predetermined value or less. In some embodiments, the adhesive strength N1 is suitably less than 500 gf / 25 mm, advantageously less than 300 gf / 25 mm, preferably 200 gf / 25 mm or less or 180 gf / 25 mm or less, more preferably 150 gf / 25 mm or less or 130 gf / 25 mm or less, and even more preferably 110 gf / 25 mm or less or 100 gf / 25 mm or less, and may be 90 gf / 25 mm or less, or even 80 gf / 25 mm or less. A low adhesive strength N1 is preferable from the viewpoint of reworkability. The lower limit of the adhesive strength N1 is not particularly limited, and may be, for example, 1 gf / 25 mm or more. From the viewpoints of ease of application to an adherend and prevention of misalignment before the adhesive strength increases, the adhesive strength N1 is usually suitably 10 gf / 25 mm or more. From the viewpoint of improving adhesive strength after heating, in some embodiments, the adhesive strength N1 may be, for example, 20 gf / 25 mm or more, 30 gf / 25 mm or more, 50 gf / 25 mm or more, 60 gf / 25 mm or more, or 70 gf / 25 mm or more.

[0146] The adhesive strength N1 [gf / 25 mm] is determined by pressing the film to a polyimide film as an adherend, leaving it in an environment of 23°C and 50% RH for 30 minutes, and then measuring the 180° peel adhesive strength in the same environment (i.e., at 23°C) under conditions of a peel angle of 180° and a tensile speed of 300 mm / min. From the viewpoint of measurement operability, the polyimide film as an adherend can be used in the form of a measurement polyimide plate (a plate-like adherend having a surface made of the polyimide film) formed by fixing the polyimide film to a support plate (glass plate, stainless steel plate, etc.). If necessary, the reinforcing film to be measured can be reinforced by attaching an appropriate backing material (e.g., a PET film with a thickness of approximately 25 μm). More specifically, the adhesive strength N1 can be measured according to the initial adhesive strength measurement method described in the Examples below.

[0147] The reinforcing film disclosed herein exhibits increased adhesive strength upon heating. For example, the adhesive strength N2 measured after being attached to a polyimide film as an adherend, heated at 60°C for 1 hour, and then held at 23°C for 30 minutes is suitably 800 gf / 25 mm or greater, advantageously 950 gf / 25 mm or greater, and preferably 1000 gf / 25 mm or greater. A reinforcing film satisfying these characteristics exhibits increased adhesive strength to a predetermined value or greater upon heating after being attached to an adherend. The technology disclosed herein makes it possible to achieve strong adhesive strength upon heating. In some embodiments, the adhesive strength N2 is more preferably 1100 gf / 25 mm or greater, even more preferably 1200 gf / 25 mm or greater, and may be 1300 gf / 25 mm or greater, or even 1400 gf / 25 mm or greater. There is no particular upper limit to the adhesive strength N2. From the viewpoint of easily achieving both flexibility of the pressure-sensitive adhesive layer (particularly flexibility in the low temperature range) and easy initial releasability, in some embodiments, the adhesive strength N2 may be, for example, 4000 gf / 25 mm or less, 3500 gf / 25 mm or less, 3000 gf / 25 mm or less, 2000 gf / 25 mm or less, 1800 gf / 25 mm or less, or 1600 gf / 25 mm or less.

[0148] The adhesive strength N2 [gf / 25 mm] is determined by pressing the adhesive to a polyimide film as an adherend, holding it in a 60°C environment for 60 minutes, then leaving it in a 23°C, 50% RH environment for 30 minutes, and then measuring the 180° peel adhesive strength in the same environment under conditions of a peel angle of 180° and a tensile speed of 300 mm / min. As with adhesive strength N1, a polyimide film (which may be in the form of a polyimide plate for measurement as described above) is used as the adherend. For measurement, if necessary, the reinforcing film to be measured can be reinforced by attaching an appropriate backing material (e.g., a PET film with a thickness of approximately 25 μm). More specifically, adhesive strength N2 can be measured according to the method for measuring adhesive strength after heating described in the Examples below.

[0149] The rate of increase in post-heat adhesive strength N2 [gf / 25 mm] relative to the initial adhesive strength N1 [gf / 25 mm], i.e., the adhesive strength increase rate N2 / N1 [%], is not particularly limited and may be, for example, 160% or more, 250% or more, 500% or more, or 750% or more. In some embodiments, N2 / N1 is suitably 850% or more, preferably 900% or more, more preferably 950% or more, and even more preferably 1000% or more. It may be 1200% or more, 1400% or more, 1500% or more, 1600% or more, 1700% or more, or 1800% or more. A reinforcing film with a high N2 / N1 exhibits good reworkability at the initial stage of application and can significantly increase adhesive strength upon subsequent heating, etc. The upper limit of N2 / N1 is not particularly limited and may be, for example, 10,000% or less, 7,000% or less, or 5,000% or less. In order to facilitate compatibility with the flexibility of the pressure-sensitive adhesive (particularly flexibility in the low temperature range), in some embodiments, N2 / N1 may be, for example, 4000% or less, 3000% or less, 2500% or less, or 2000% or less.

[0150] The adhesive strength after heating of the reinforcing film disclosed herein represents one characteristic of the reinforcing film and does not limit the use of the reinforcing film. In other words, the use of the reinforcing film disclosed herein is not limited to heating at 60°C for 60 minutes. For example, the reinforcing film can also be used in a manner that does not specifically involve heating above room temperature (usually 20°C to 30°C, typically 23°C to 25°C). Even in such a use mode, the adhesive strength increases over the long term, achieving a strong bond. Furthermore, the reinforcing film disclosed herein can be heat-treated at a temperature above 30°C (e.g., approximately 50 to 70°C) or above 60°C at any time after application to promote an increase in adhesive strength. The heating temperature in such heat treatment is not particularly limited and can be set taking into consideration workability, economy, the heat resistance of the reinforcing film substrate and the adherend, and the like. The heating temperature may be, for example, less than 150°C, 120°C or less, 100°C or less, 80°C or less, or 70°C or less. The heating temperature can be, for example, 40°C or higher, 45°C or higher, 50°C or higher, 55°C or higher, 60°C or higher, or 70°C or higher, and may be 80°C or higher, or 100°C or higher. The heating time is not particularly limited and may be, for example, 3 hours or less, 1 hour or less, 30 minutes or less, or 10 minutes or less. The heating time may be, for example, 1 minute or more, 15 minutes or more, 30 minutes or more, or 1 hour or more. Alternatively, the heat treatment may be performed for a longer period of time as long as significant thermal degradation does not occur in the reinforcing film or the adherend. The heat treatment may be performed all at once or in multiple steps.

[0151] <Reinforcing Film with Substrate> When the reinforcing film disclosed herein is in the form of a pressure-sensitive adhesive sheet with a substrate, the thickness of the reinforcing film may be, for example, 1000 μm or less, 600 μm or less, 350 μm or less, or 250 μm or less. From the viewpoint of miniaturization, weight reduction, thinning, etc. of products to which the reinforcing film is applied, in some embodiments, the thickness of the reinforcing film may be, for example, 200 μm or less, 175 μm or less, 160 μm or less, 140 μm or less, or 120 μm or less. The reinforcing film disclosed herein can also be implemented in an embodiment having a thickness of 115 μm or less, 105 μm or less, 95 μm or less, or 85 μm or less. Furthermore, from the viewpoint of handleability, etc., the thickness of the reinforcing film may be, for example, 5 μm or more, 10 μm or more, 15 μm or more, 20 μm or more, 25 μm or more, or 30 μm or more. In some embodiments, the thickness of the reinforcing film may be, for example, 50 μm or more, 60 μm or more, 75 μm or more, 85 μm or more, 90 μm or more, 100 μm or more, or 120 μm or more. The upper limit of the thickness of the reinforcing film is not particularly limited. The thickness of the reinforcing film refers to the thickness of the portion that is attached to the adherend. For example, in the reinforcing film 1 configured as shown in FIG. 1 , the thickness refers to the thickness from the adhesive surface 21A of the reinforcing film 1 to the second surface 10B of the substrate 10, and does not include the thickness of the release liner 31.

[0152] The reinforcing film disclosed herein can be suitably implemented, for example, in an embodiment in which the thickness Ts of the support substrate is greater than the thickness Ta of the pressure-sensitive adhesive layer, i.e., in an embodiment in which Ts / Ta is greater than 1. Although not particularly limited, Ts / Ta may be, for example, 1.1 or more, 1.2 or more, 1.5 or more, or 1.7 or more. For example, an increase in Ts / Ta tends to make it easier to achieve good effects even when the reinforcing film is made thinner. In some embodiments, Ts / Ta may be 2 or more (e.g., greater than 2), 2.5 or more, or 2.8 or more. Furthermore, Ts / Ta may be, for example, 50 or less, or 20 or less. From the viewpoint of making it easier for the reinforcing film to exhibit high post-heat adhesive strength even when made thinner, Ts / Ta may be, for example, 10 or less, 8 or less, or 5 or less.

[0153] The pressure-sensitive adhesive layer is preferably adhered to the supporting substrate. Here, "adhesion" refers to a state in which, in a reinforcing film whose adhesive strength has increased after application to an adherend, the adhesive layer exhibits sufficient anchoring properties to the supporting substrate to such an extent that peeling does not occur at the interface between the adhesive layer and the supporting substrate when the reinforcing film is peeled from the adherend. A substrate-attached reinforcing film in which the adhesive layer is adhered to the supporting substrate can firmly integrate the adherend and the supporting substrate. A preferred example of a reinforcing film in which the adhesive layer is adhered to the substrate is a reinforcing film in which peeling (anchor failure) does not occur between the adhesive layer and the supporting substrate when measuring the adhesive strength after heating as described above. A reinforcing film in which anchor failure does not occur when measuring the adhesive strength after heating is a preferred example of a reinforcing film in which the adhesive layer is adhered to the substrate.

[0154] The reinforcing film disclosed herein can be preferably produced, for example, by a method comprising, in this order, contacting a liquid pressure-sensitive adhesive composition with a first surface of a substrate and curing the pressure-sensitive adhesive composition on the first surface to form a pressure-sensitive adhesive layer. Curing the pressure-sensitive adhesive composition may involve one or more of the following processes: drying, crosslinking, polymerization, and cooling of the pressure-sensitive adhesive composition. This method of curing a liquid pressure-sensitive adhesive composition on the first surface of a substrate to form a pressure-sensitive adhesive layer can enhance the anchoring ability of the pressure-sensitive adhesive layer to the substrate compared to a method in which the cured pressure-sensitive adhesive layer is attached to the first surface of the substrate, thereby disposing the pressure-sensitive adhesive layer on the first surface. Taking advantage of this, a reinforcing film in which a pressure-sensitive adhesive layer is fixed to a substrate can be preferably produced.

[0155] In some embodiments, the method for contacting the liquid PSA composition with the first surface of the substrate can be a method of directly applying the PSA composition to the first surface of the substrate. By contacting the first surface (adhesive surface) of the PSA layer cured on the first surface of the substrate with a release surface, a reinforcing film can be obtained in which the second surface of the PSA layer is fixed to the first surface of the substrate and the first surface of the PSA layer is in contact with the release surface. The release surface can be the surface of a release liner, the back surface of a release-treated substrate, or the like.

[0156] Furthermore, for example, in the case of a photocurable pressure-sensitive adhesive composition using a partial polymer (polymer syrup) of a monomer raw material, the pressure-sensitive adhesive composition may be applied to a release surface, and then the first surface of a substrate may be placed over the applied pressure-sensitive adhesive composition to bring the uncured pressure-sensitive adhesive composition into contact with the first surface of the substrate, and in this state, the pressure-sensitive adhesive composition sandwiched between the first surface of the substrate and the release surface may be irradiated with light to cure it, thereby forming a pressure-sensitive adhesive layer.

[0157] The methods exemplified above do not limit the manufacturing method of the reinforcing film disclosed herein. In manufacturing the reinforcing film disclosed herein, any suitable method capable of adhering a pressure-sensitive adhesive layer to the first surface of a substrate can be used, either alone or in combination. Examples of such methods include the method of forming a pressure-sensitive adhesive layer by curing a liquid pressure-sensitive adhesive composition on the first surface of a substrate, as described above, or a method of applying a surface treatment to the first surface of a substrate to enhance the anchoring ability of the pressure-sensitive adhesive layer. For example, if the anchoring ability of the pressure-sensitive adhesive layer to the substrate can be sufficiently improved by providing an undercoat layer on the first surface of the substrate, the reinforcing film may be manufactured by laminating the cured pressure-sensitive adhesive layer to the first surface of the substrate. The anchoring ability of the pressure-sensitive adhesive layer to the substrate can also be improved by selecting the material of the substrate and the composition of the pressure-sensitive adhesive. Furthermore, applying a temperature higher than room temperature to a reinforcing film having a pressure-sensitive adhesive layer on the first surface of the substrate can enhance the anchoring ability of the pressure-sensitive adhesive layer to the substrate. The temperature applied to enhance the anchoring property may be, for example, about 35°C to 80°C, about 40°C to 70°C, or about 45°C to 60°C.

[0158] When the reinforcing film disclosed herein is in the form of a pressure-sensitive adhesive sheet having a first pressure-sensitive adhesive layer provided on a first surface of a substrate and a second pressure-sensitive adhesive layer provided on a second surface of the substrate (i.e., a double-sided substrate-attached pressure-sensitive adhesive sheet), the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer may have the same or different configurations. When the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer have different configurations, the difference may be, for example, a difference in composition or structure (thickness, surface roughness, formation area, formation pattern, etc.). For example, the second pressure-sensitive adhesive layer may be a pressure-sensitive adhesive layer that does not contain polymer (B). The surface (adhesive surface) of the second pressure-sensitive adhesive layer may have an initial adhesive strength to the above-mentioned polyimide film of 200 gf / 25 mm or less, or may be greater than 200 gf / 25 mm, for example, 500 gf / 25 mm or more, 800 gf / 25 mm or more, or 1000 gf / 25 mm or more.

[0159] <Reinforcing film with release liner> The reinforcing film disclosed herein can be in the form of a pressure-sensitive adhesive product in which the surface (adhesive surface) of the pressure-sensitive adhesive layer is in contact with the release surface of a release liner. Thus, this specification can provide a reinforcing film with a release liner, comprising any of the reinforcing films disclosed herein and a release liner having a release surface in contact with the adhesive surface of the reinforcing film. In this specification, the term "release liner" is also referred to as "release liner," and is a concept that can encompass what are commonly referred to as release films and release sheets.

[0160] The thickness of the release liner is not particularly limited, but a thickness of approximately 5 μm to 200 μm is usually appropriate. A release liner having a thickness within the above range is preferred because it provides excellent workability in laminating to the pressure-sensitive adhesive layer and in peeling from the pressure-sensitive adhesive layer. In some embodiments, the thickness of the release liner may be, for example, 10 μm or more, 20 μm or more, 30 μm or more, or 40 μm or more. Furthermore, from the viewpoint of facilitating peeling from the pressure-sensitive adhesive layer, the thickness of the release liner may be, for example, 100 μm or less, 80 μm or less, 60 μm or less, 50 μm or less, or 40 μm or less. If necessary, the release liner may be subjected to a known antistatic treatment, such as a coating type, kneading type, or vapor deposition type.

[0161] The release liner is not particularly limited, and examples thereof include release liners having a release layer on the surface of a liner substrate such as a resin film or paper (which may be paper laminated with a resin such as polyethylene), and release liners made of a resin film formed from a low-adhesion material such as a fluorine-based polymer (e.g., polytetrafluoroethylene) or a polyolefin resin (e.g., polyethylene, polypropylene). Because of their excellent surface smoothness, release liners having a release layer on the surface of a resin film used as a liner substrate and release liners made of a resin film formed from a low-adhesion material are preferably used. The resin film is not particularly limited as long as it is a film capable of protecting the pressure-sensitive adhesive layer, and examples thereof include polyethylene film, polypropylene film, polybutene film, polybutadiene film, polymethylpentene film, polyvinyl chloride film, vinyl chloride copolymer film, polyester film (e.g., PET film, PBT film), polyurethane film, and ethylene-vinyl acetate copolymer film. The release layer can be formed using known release treatment agents, such as silicone-based release treatment agents, long-chain alkyl-based release treatment agents, olefin-based release treatment agents, fluorine-based release treatment agents, fatty acid amide-based release treatment agents, molybdenum sulfide, silica powder, etc. Silicone-based release treatment agents are particularly preferred.

[0162] The thickness of the release layer is not particularly limited, but is usually about 0.01 μm to 1 μm, and preferably about 0.1 μm to 1 μm. The method for forming the release layer is not particularly limited, and any known method can be appropriately adopted depending on the type of release treatment agent used, etc.

[0163] <Applications> The reinforcing film provided by this specification can exhibit good reworkability, for example, initially after being attached to an adherend, thereby contributing to suppressing yield declines and improving the quality of products containing the reinforcing film. Furthermore, after being attached to an adherend, the adhesive strength of the reinforcing film can be significantly increased by aging or heating. For example, by heating at an appropriate time after attachment to the adherend, the reinforcing film can be firmly adhered to the adherend. Taking advantage of these characteristics, the reinforcing film disclosed herein can be preferably used in various fields to reinforce components included in various products.

[0164] The reinforcing film disclosed herein can be preferably used as a reinforcing film attached to an adherend to reinforce the adherend, for example, in the form of a substrate-attached pressure-sensitive adhesive sheet having a film substrate having a first surface and a second surface and a pressure-sensitive adhesive layer provided on at least the first surface of the film substrate. In such a reinforcing film, a film substrate containing a resin film as a base film can be preferably used. Furthermore, from the viewpoint of enhancing reinforcing performance, it is preferable that the pressure-sensitive adhesive layer be adhered to the first surface of the film substrate. For example, optical components used in optical products and electronic components used in electronic products are becoming highly integrated, smaller, lighter, and thinner, and multiple thin optical / electronic components with different linear expansion coefficients and thicknesses may be laminated. By attaching such a reinforcing film to such components, appropriate rigidity can be imparted to the optical / electronic components. This can suppress curling and curvature caused by stress that may occur between multiple components with different linear expansion coefficients and thicknesses during the manufacturing process and / or in the manufactured product. Furthermore, in the manufacturing process of optical / electronic products, when thin optical / electronic components are subjected to shaping processes such as cutting, attaching a reinforcing film to the component can alleviate local stress concentrations on the optical / electronic component during processing, thereby reducing the risk of cracks, breakage, and peeling of laminated components. Attaching the reinforcing film to an optical / electronic component as a reinforcing member and handling it can also help alleviate local stress concentrations during transport, stacking, rotation, etc. of the component, and prevent the component from bending or bending due to its own weight. Furthermore, when devices such as optical and electronic products containing the reinforcing film are used by consumers in the market, the presence of the reinforcing film in the device can alleviate stress on the device even when the device is subjected to unintentional stress, such as when the device is dropped, placed under a heavy object, or hit by a flying object. Therefore, the presence of the reinforcing film in the device can improve the durability of the device.

[0165] The reinforcing film disclosed herein can be preferably used, for example, in a manner in which it is attached to components constituting various portable devices (portable devices). Here, "portable" does not simply mean being portable, but rather means having a level of portability that allows an individual (average adult) to carry it relatively easily. Examples of portable devices include mobile phones, smartphones, tablet computers, laptop computers, various wearable devices, digital cameras, digital video cameras, audio equipment (portable music players, IC recorders, etc.), calculators (calculators, etc.), portable game consoles, electronic dictionaries, electronic organizers, e-books, in-car information devices, portable radios, portable televisions, portable printers, portable scanners, and portable modems, as well as mechanical wristwatches, pocket watches, flashlights, and hand mirrors. Examples of components constituting the portable electronic devices include optical films and display panels used in image display devices such as thin-film displays (e.g., liquid crystal displays) and film-type displays. The reinforcing film disclosed herein can also be preferably used in a manner in which it is attached to various components in automobiles, home appliances, and the like.

[0166] Furthermore, the reinforcing film disclosed herein has a pressure-sensitive adhesive layer that exhibits good flexibility even at low temperatures, and thus can be preferably used by taking advantage of this feature in an embodiment in which it is attached to a component constituting a device having a bendable element (e.g., a flexible device such as a flexible display, which may also be referred to as a rollable device or a foldable device). Examples of such devices include the various mobile devices (portable devices) described above, and preferred examples include the various mobile electronic devices described above. Examples of components constituting the above-mentioned mobile electronic devices include optical films and display panels used in image display devices such as liquid crystal displays and organic EL (electroluminescence) displays. The reinforcing film disclosed herein can be preferably used in such mobile electronic devices to reinforce components constituting the device (typically, image display devices referred to as flexible devices, foldable devices, rollable devices, etc.).

[0167] The reinforcing film disclosed herein is suitable for applications such as reinforcing optical members during production, transportation, use, etc. of optical members used as components of liquid crystal display panels, plasma display panels (PDPs), organic EL displays, etc. The reinforcing film disclosed herein is useful as a reinforcing film applied to optical members such as polarizing plates (polarizing films), wave plates, retardation plates, optical compensation films, brightness enhancement films, light diffusion sheets, and reflective sheets for liquid crystal display panels.

[0168] The use of the reinforcing film disclosed herein is not particularly limited, and it can be used for various applications for the purpose of imparting rigidity, impact resistance, etc. The reinforcing film disclosed herein can be used not only preferably for flexible device applications as described above, but also for other applications not involving flexible devices. The fact that the reinforcing film has an adhesive with good flexibility (for example, flexibility in a low temperature range) means that there are fewer restrictions on the range of application of the reinforcing film, which has a great practical advantage.

[0169] The matters disclosed in this specification include the following: [1] A reinforcing film having a pressure-sensitive adhesive layer, wherein the pressure-sensitive adhesive layer comprises a polymer (A) and a polymer (B), the polymer (B) comprises a monomer unit having a polyorganosiloxane skeleton and a (meth)acrylic monomer unit, the polymer (A) is an acrylic polymer containing a monomer unit derived from a nitrogen-containing monomer, and the amount W of the monomer unit derived from the nitrogen-containing monomer contained in 100 parts by weight of the polymer (A) is N [Parts by weight] is 14 parts by weight or less, and the pressure-sensitive adhesive layer contains W Zr [parts by weight] of a zirconium-containing compound, Zr [Parts by weight] N [weight parts] ratio (W N / W Zr) is 4 or more. [2] The reinforcing film according to the above [1], wherein the pressure-sensitive adhesive layer contains a crosslinking agent. [3] The reinforcing film according to the above [1] or [2], wherein the content of the polymer (B) in the pressure-sensitive adhesive layer is 0.1 to 10 parts by weight per 100 parts by weight of the polymer (A). [4] The reinforcing film according to any of the above [1] to [3], wherein the polymer (A) contains a monomer unit derived from a monomer having a nitrogen-atom-containing ring as the monomer unit derived from the nitrogen-containing monomer. [5] The reinforcing film according to any of the above [1] to [4], wherein the adhesive strength N1 after being attached to a polyimide film and heated at 23°C for 30 minutes is 200 gf / 25 mm or less. [6] The reinforcing film according to any of the above [1] to [5], wherein the adhesive strength N2 after being attached to a polyimide film and heated at 60°C for 1 hour and then heated at 23°C for 30 minutes is 1000 gf / 25 mm or more. [7] The reinforcing film according to any one of [1] to [6] above, wherein the adhesive strength N2 [gf / 25 mm] after being attached to a polyimide film and heated at 60°C for 1 hour and then left at 23°C for 30 minutes has an increase rate [%] of 900% or more relative to the adhesive strength N1 [gf / 25 mm] after being attached to a polyimide film and left at 23°C for 30 minutes. [8] The reinforcing film according to any one of [1] to [7] above, wherein the adhesive constituting the adhesive layer has a storage modulus at -20°C of 1000 kPa or less. [9] An optical member to which the reinforcing film according to any one of [1] to [8] above is attached.

[10] An electronic member to which the reinforcing film according to any one of [1] to [8] above is attached.

[11] A polymer (A) and a polymer (B), wherein the polymer (B) contains a monomer unit having a polyorganosiloxane skeleton and a (meth)acrylic monomer unit, the polymer (A) is an acrylic polymer containing a monomer unit derived from a nitrogen-containing monomer, and the amount W of the monomer unit derived from the nitrogen-containing monomer contained in 100 parts by weight of the polymer (A) is N [Parts by weight] is 14 parts by weight or less, and W is 100 parts by weight of the polymer (A). Zr [parts by weight] of a zirconium-containing compound,Zr [Parts by weight] N [weight parts] ratio (W N / W Zr

[12] A pressure-sensitive adhesive composition comprising a polymer (A) and a polymer (B), wherein the polymer (B) comprises a monomer unit having a polyorganosiloxane skeleton and a (meth)acrylic monomer unit, the polymer (A) is an acrylic polymer containing a monomer unit derived from a nitrogen-containing monomer, and the amount W of the monomer unit derived from the nitrogen-containing monomer contained in 100 parts by weight of the polymer (A) is 4 or more. N [Parts by weight] is 14 parts by weight or less, and W is 100 parts by weight of the polymer (A). Zr [parts by weight] of a zirconium-containing compound, Zr [Parts by weight] N [weight parts] ratio (W N / W Zr ) is 4 or more.

[0170] Several examples of the present invention will be described below, but it is not intended that the present invention be limited to these specific examples. In the following description, "parts" and "%" are by weight unless otherwise specified.

[0171] <Polymer Synthesis> (Synthesis Example A1) A four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser was charged with 89.3 parts of 2-ethylhexyl acrylate (2EHA), 8.9 parts of 4-hydroxybutyl acrylate (4HBA), 1.8 parts of N-vinylpyrrolidone (NVP), 0.2 parts of 2,2'-azobisisobutyronitrile (AIBN) as a polymerization initiator, and ethyl acetate as a polymerization solvent. Nitrogen gas was introduced while gently stirring, and the liquid temperature in the flask was maintained at around 65°C, allowing the polymerization reaction to proceed for 6 hours to prepare a polymer A1 solution with a polymer concentration of 35%. The weight average molecular weight (Mw) of polymer A1 was 540,000.

[0172] Synthesis Example A2 A solution of Polymer A2 was obtained by solution polymerization in the same manner as in Synthesis Example A1, except that the monomer composition was changed to 2EHA / butyl acrylate (BA) / lauryl acrylate (LA) / 4HBA / NVP=70 parts / 20 parts / 8 parts / 1 part / 0.6 parts.

[0173] Synthesis Example A3 A solution of Polymer A3 was obtained by solution polymerization in the same manner as in Synthesis Example A1, except that the monomer composition was changed to 2EHA / methyl methacrylate (MMA) / 2-hydroxyethyl acrylate (HEA) / NVP=63 parts / 9 parts / 13 parts / 15 parts.

[0174] Synthesis Example A4 Solution polymerization was carried out in the same manner as in Synthesis Example A1, except that the monomer composition was changed to 2EHA / 4HBA=91 parts / 9 parts, to obtain a solution of polymer A4.

[0175] (Synthesis Example B1) 101.15 parts of ethyl acetate, 40 parts of MMA, 20 parts of n-butyl methacrylate (BMA), 20 parts of 2-ethylhexyl methacrylate (2EHMA), 8.7 parts of a polyorganosiloxane skeleton-containing methacrylate monomer having a functional group equivalent of 900 g / mol (trade name: X-22-174ASX, manufactured by Shin-Etsu Chemical Co., Ltd.), 11.3 parts of a polyorganosiloxane skeleton-containing methacrylate monomer having a functional group equivalent of 4600 g / mol (trade name: KF-2012, manufactured by Shin-Etsu Chemical Co., Ltd.), and 0.8 parts of thioglycerol as a chain transfer agent were charged into a four-necked flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, a condenser, and a dropping funnel. Then, after stirring for 30 minutes under a nitrogen atmosphere at 70 ° C., 0.2 parts of AIBN was added as a thermal polymerization initiator, and the mixture was allowed to react at 70 ° C. for 3 hours. Subsequently, the mixture was stirred at 80° C. for 30 minutes, and then 0.1 part of AIBN was further added, and the mixture was reacted at 80° C. for 2 hours. Thereafter, 0.05 part of AIBN was further added, and the mixture was reacted at 80° C. for 2 hours to obtain Polymer B1. The Mw of Polymer B1 was 20,000.

[0176] Polymers B2 and B3 were prepared in the same manner as in Synthesis Example B1, except that the amount of chain transfer agent (thioglycerol) used was changed to 0.6 parts (Synthesis Example B2) or 1.5 parts (Synthesis Example B3) per 100 parts of the starting monomer material. The Mw of Polymer B2 was 27,600, and the Mw of Polymer B3 was 12,600.

[0177] Polymer B4 was prepared in the same manner as in Synthesis Example B1, except that the monomer composition was changed to MMA / BMA / 2EHMA / X-22-174ASX / KF-2012=40 / 20 / 20 / 3.2 / 16.8. The Mw of Polymer B4 was 20,000.

[0178] The Mw of each of the above-mentioned polymers was measured using a GPC device (HLC-8220GPC, manufactured by Tosoh Corporation) under the following conditions and calculated in terms of polystyrene. [GPC conditions] Sample concentration: 0.2 wt% (tetrahydrofuran (THF) solution) Sample injection amount: 10 μL Eluent: THF Flow rate: 0.6 mL / min Measurement temperature: 40°C Columns: Sample column: TSKguardcolumn SuperHZ-H (1 column) + TSKgel SuperHZM-H (2 columns) Reference column: TSKgel SuperH-RC (1 column) Detector: differential refractometer (RI)

[0179] <Preparation of Reinforcing Film> (Example 1) To a polymer A1 solution, 2.0 parts of polymer B1, 0.1 part (solids equivalent) of an isocyanate compound C1 (an isocyanurate of hexamethylene diisocyanate, trade name "Coronate HX", manufactured by Tosoh Corporation) as a crosslinking agent, and 0.1 part of zirconium tetraacetylacetonate (trade name "ZC150", manufactured by Matsumoto Fine Chemical Co., Ltd.) as a Zr-containing compound were added per 100 parts of polymer A1 contained in the solution, and the mixture was diluted with ethyl acetate to a total solids content of 30% to obtain an acrylic pressure-sensitive adhesive solution according to this example. The pressure-sensitive adhesive solution obtained above was applied to a 75 μm-thick polyethylene terephthalate (PET) film (support substrate) having an untreated first side, and the solution was dried at 130° C. for 1 minute to remove the solvent, thereby forming a 25 μm-thick pressure-sensitive adhesive layer. The silicone-treated surface of a 25 μm-thick PET film (release liner) that had been silicone-treated on one side was bonded to the adhesive surface of this adhesive layer, and aging treatment was carried out for 4 days at 25° C. In this way, a reinforcing film (reinforcing film) consisting of the supporting substrate and the adhesive layer laminated and fixed onto the supporting substrate was obtained in the form of a reinforcing film with a release liner, in which the release liner was temporarily attached to the adhesive surface of the adhesive layer.

[0180] (Examples 2 to 7) An acrylic pressure-sensitive adhesive solution according to each example was obtained in the same manner as in Example 1, except that the amounts of polymer B1, isocyanate compound C1, and Zr-containing compound used per 100 parts of polymer A1 were as shown in Table 1. A reinforcing film according to each example was produced in the same manner as in the production of the reinforcing film according to Example 1, except that each of these acrylic pressure-sensitive adhesive solutions was used.

[0181] (Example 8) An acrylic pressure-sensitive adhesive solution according to each example was obtained in the same manner as in Example 1, except that an isocyanate compound C2 (a trimethylolpropane adduct of m-xylylene diisocyanate, product name "Takenate D110N", manufactured by Mitsui Chemicals, Inc.) was used instead of the isocyanate compound C1. A reinforcing film according to each example was produced in the same manner as in the production of the reinforcing film according to Example 1, except that each of these acrylic pressure-sensitive adhesive solutions was used.

[0182] (Examples 9 to 11) Except for using polymers B2 to B4 instead of polymer B1, acrylic pressure-sensitive adhesive solutions according to each example were obtained in the same manner as in Example 1. Except for using these acrylic pressure-sensitive adhesive solutions, reinforcing films according to each example were produced in the same manner as in the production of the reinforcing film according to Example 1.

[0183] (Example 12) Except for using polymer A2 instead of polymer A1, an acrylic pressure-sensitive adhesive solution according to this example was obtained in the same manner as in Example 1. Except for using this acrylic pressure-sensitive adhesive solution, a reinforcing film according to this example was produced in the same manner as in the production of the reinforcing film according to Example 1.

[0184] (Example 13) An acrylic pressure-sensitive adhesive solution according to this example was obtained in the same manner as in Example 12, except that the amount of Zr-containing compound used was as shown in Table 1. A reinforcing film according to this example was produced in the same manner as in the production of the reinforcing film according to Example 1, except that this acrylic pressure-sensitive adhesive solution was used.

[0185] (Examples 14 to 17) Instead of the Zr-containing compound used in Example 1, iron(III) acetylacetonate (trade name "Nacem Ferric", manufactured by Nippon Chemical Industry Co., Ltd.) was used in Example 14, aluminum trisacetylacetonate (trade name "AL3100", manufactured by Matsumoto Fine Chemical Co., Ltd.) in Example 15, titanium tetraacetylacetonate (trade name "TC401", manufactured by Matsumoto Fine Chemical Co., Ltd.) in Example 16, and dibutyltin(IV) dilaurate (trade name "OL-1", manufactured by Tokyo Fine Chemical Co., Ltd.) in Example 17. An acrylic pressure-sensitive adhesive solution according to each Example was obtained in the same manner as in Example 1, except that these acrylic pressure-sensitive adhesive solutions were used. Reinforcing films according to each Example were produced in the same manner as in the production of the reinforcing film according to Example 1.

[0186] (Example 18) An acrylic pressure-sensitive adhesive solution according to this example was obtained in the same manner as in Example 1, except that the amount of Zr-containing compound used was as shown in Table 1. A reinforcing film according to this example was produced in the same manner as in the production of the reinforcing film according to Example 1, except that this acrylic pressure-sensitive adhesive solution was used.

[0187] (Example 19) Except for not using polymer B1, an acrylic pressure-sensitive adhesive solution according to this example was obtained in the same manner as in Example 1. Except for using this acrylic pressure-sensitive adhesive solution, a reinforcing film according to this example was produced in the same manner as in the production of the reinforcing film according to Example 1.

[0188] (Example 20) An acrylic pressure-sensitive adhesive solution of this example was obtained in the same manner as in Example 8, except that polymer A3 was used instead of polymer A1 and the amount of isocyanate compound C2 used was as shown in Table 1. A reinforcing film of this example was produced in the same manner as in the production of the reinforcing film of Example 1, except that this acrylic pressure-sensitive adhesive solution was used.

[0189] (Example 21) Except for using polymer A4 instead of polymer A1, an acrylic pressure-sensitive adhesive solution according to this example was obtained in the same manner as in Example 1. Except for using this acrylic pressure-sensitive adhesive solution, a reinforcing film according to this example was produced in the same manner as in the production of the reinforcing film according to Example 1.

[0190] <Evaluation> [-20°C storage modulus (G' -20 ) A release liner R1 (trade name "Diafoil MRF75", manufactured by Mitsubishi Chemical Corporation) made of a 75 μm thick polyester resin with one side silicone-treated was prepared, and the acrylic adhesive solution according to each example was applied to the silicone-treated surface and dried at 130 ° C for 1 minute to form a 25 μm thick adhesive layer. Next, the surface of the obtained adhesive layer was covered with a release liner R2 (trade name "Diafoil MRE75", manufactured by Mitsubishi Chemical Corporation) made of a 75 μm thick polyester resin with one side silicone-treated, with the silicone-treated surface facing the adhesive layer, and aged at 50 ° C for 1 day. Only the obtained adhesive layer was removed and laminated to a thickness of approximately 1 mm, which was then punched out to a diameter of 8 mm to prepare a cylindrical pellet, which was used as a measurement sample. The measurement sample was fixed to a φ8 mm parallel plate jig, and the −20° C. storage modulus (G′ -20) [kPa] was measured. Measurement mode: Shear mode Temperature range: -30°C to 100°C Heating rate: 5°C / min Frequency: 1 Hz The storage modulus corresponds to the portion stored as elastic energy when a material is deformed, and is an index that indicates the degree of hardness.

[0191] [Initial Adhesion] The reinforcing film according to each example, together with the release liner, was cut into a measurement sample of 25 mm wide x 140 mm long. A polyimide plate for measurement was prepared by fixing a 25 μm thick polyimide film (manufactured by Ube Industries, Ltd., product name "Upilex 25S") to a glass plate using double-sided adhesive tape (manufactured by Nitto Denko, product name "No. 531"). The release liner was peeled off from the measurement sample to expose the adhesive surface, which was then pressed against the polyimide plate (adherend) using a 2 kg hand roller, moving back and forth once. The measurement sample thus adhered to the adherend was left at an ambient temperature of 23 ° C. for 30 minutes, and then a tensile tester (Shimadzu Corporation, product name "Autograph AG-Xplus HS 6000 mm / min high-speed model (AG-50NX plus)") was used to measure the load when peeling the reinforcing film from the adherend under conditions of a peel angle of 180 degrees and a peel speed (tensile speed) of 300 mm / min, and the average load during measurement was recorded as the initial adhesive strength [gf / 25 mm]. Note that the reinforcing film of Example 19 had a high initial adhesive strength of 1000 gf / 25 mm or more, so measurement of the adhesive strength after heating and calculation of the increase rate were not performed.

[0192] [Adhesive strength after heating] For each reinforcing film according to each example, a measurement sample was prepared in the same manner as in the initial adhesive strength measurement and pressure-bonded to the polyimide substrate (adherend). The measurement sample pressure-bonded to the adherend was then heated at an ambient temperature of 60 ° C for 60 minutes. After that, the sample was left at an ambient temperature of 23 ° C for 30 minutes, and the load when the reinforcing film was peeled from the adherend was measured using a tensile tester (Shimadzu Corporation, product name "Autograph AG-Xplus HS 6000 mm / min high-speed model (AG-50NX plus)") at a peel angle of 180 degrees and a peel rate (tensile speed) of 300 mm / min. The average load during the measurement was recorded as the adhesive strength after heating [gf / 25 mm].

[0193] [Increase Rate] Based on the initial adhesive strength [gf / 25 mm] and the adhesive strength after heating [gf / 25 mm] of the reinforcing film according to each example, the increase rate of adhesive strength was calculated using the following formula: Increase rate [%] = (adhesive strength after heating [gf / 25 mm] / initial adhesive strength [gf / 25 mm]) × 100

[0194] The evaluation results for the reinforcing film of each example are shown in Table 1. Table 1 also shows an outline of the composition of the pressure-sensitive adhesive layer of each example. N "[parts]" indicates the amount W of monomer units derived from nitrogen-containing monomers contained in 100 parts of polymer (A) used in each example. N The metal compound amount W in Table 1 is [parts]. Zr The "parts" indicates the amount of metal compound used relative to 100 parts of polymer (A) used in each example. For convenience, even in examples where the metal species of the metal compound is not Zr, "W" is used. Zr " is used. N / W Zr " is the amount of metal compound W used in each example Zr The amount of N monomer contained in polymer (A) relative to [parts] W N Similarly, in Table 1, the amount of monomer units derived from nitrogen-containing monomers, W N For convenience, polymer A3 containing more than 14 parts of a monomer unit derived from a nitrogen-containing monomer and polymer A4 containing no monomer unit derived from a nitrogen-containing monomer are also shown in the "Polymer (A)" column.

[0195]

[0196] As shown in Table 1, the PSA compositions according to Examples 1 to 13 contain a polymer (A), a polymer (B) and a Zr-containing compound. N is 14 parts or less, and the ratio (W N / W Zr) was 4 or more. The reinforcing films according to these examples better achieved a low initial adhesive strength and an increase in adhesive strength after heating than the reinforcing films according to Examples 14 to 19 and 21. Furthermore, the pressure-sensitive adhesives according to Examples 1 to 13 had a significantly lower -20°C storage modulus than the pressure-sensitive adhesive according to Example 20, and in addition to achieving a low initial adhesive strength and an increase in adhesive strength after heating, they also exhibited good flexibility.

[0197] More specifically, a comparison of Example 1, in which a Zr-containing compound was used as the metal compound, with Examples 14 to 16, in which a Zr-free metal compound was used instead of the Zr-containing compound, shows that the use of a Zr-containing compound tends to improve the adhesive strength to polyimide after heating. Example 17, in which a tin compound was used instead of the Zr-containing compound, showed higher adhesive strength after heating than Examples 14 to 16, but also showed higher initial adhesive strength than Examples 14 to 16, resulting in a lower rate of increase in adhesive strength. Furthermore, as can be seen from a comparison of Examples 1 to 3 and Example 18, in which a Zr-containing compound was used, the ratio (W N / W Zr When the W value was below 4, the adhesive strength after heating was rapidly reduced. The reinforcing film of Example 19, which used an adhesive containing no polymer (B), had a high initial adhesive strength, N The PSA of Example 20, which used polymer A3 with a molecular weight of more than 14 parts, had a high storage modulus at −20° C., while the PSA of Example 21, which used polymer A4 containing no monomer units derived from a nitrogen-containing monomer, had a low adhesive strength after heating.

[0198] Although specific examples of the present invention have been described above in detail, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations of the specific examples exemplified above.

[0199] REFERENCE SIGNS LIST 1, 2, 3 Reinforcing film 10 Supporting substrate 10A First surface 10B Second surface 21 Pressure-sensitive adhesive layer (first pressure-sensitive adhesive layer) 21A Pressure-sensitive adhesive surface (first pressure-sensitive adhesive surface) 21B Pressure-sensitive adhesive surface (second pressure-sensitive adhesive surface) 22 Pressure-sensitive adhesive layer (second pressure-sensitive adhesive layer) 22A Pressure-sensitive adhesive surface (second pressure-sensitive adhesive surface) 31, 32 Release liner 100, 200, 300 Reinforcing film with release liner

Claims

1. A reinforcing film having a pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer comprising a polymer (A) and a polymer (B), the polymer (B) comprising a monomer unit having a polyorganosiloxane skeleton and a (meth)acrylic monomer unit, the polymer (A) being an acrylic polymer comprising a monomer unit derived from a nitrogen-containing monomer, the amount W of the monomer unit derived from the nitrogen-containing monomer contained in 100 parts by weight of the polymer (A) being N [Parts by weight] is 14 parts by weight or less, and the pressure-sensitive adhesive layer is W Zr [parts by weight] of a zirconium-containing compound, Zr [Parts by weight] N [weight parts] ratio (W N / W Zr ) is 4 or more.

2. The reinforcing film according to claim 1, wherein the pressure-sensitive adhesive layer contains a crosslinking agent.

3. The reinforcing film according to claim 1 or 2, wherein the content of the polymer (B) in the pressure-sensitive adhesive layer is 0.1 to 10 parts by weight per 100 parts by weight of the polymer (A).

4. The reinforcing film according to claim 1 or 2, wherein the polymer (A) contains, as the monomer unit derived from the nitrogen-containing monomer, a monomer unit derived from a monomer having a nitrogen atom-containing ring.

5. The reinforcing film according to claim 1 or 2, which has an adhesive strength N1 of 200 gf / 25 mm or less after being attached to a polyimide film at 23° C. for 30 minutes.

6. The reinforcing film according to claim 5, which has an adhesive strength N2 of 1000 gf / 25 mm or more after being attached to a polyimide film and heated at 60° C. for 1 hour and then at 23° C. for 30 minutes.

7. A reinforcing film as described in claim 6, wherein the increase rate [%] of the adhesive strength N2 [gf / 25 mm] relative to the adhesive strength N1 [gf / 25 mm] is 900% or more.

8. The reinforcing film according to claim 1 or 2, wherein the adhesive constituting the adhesive layer has a storage modulus of elasticity at -20°C of 1000 kPa or less.

9. An optical member having the reinforcing film according to claim 1 or 2 attached thereto.

10. An electronic component to which the reinforcing film according to claim 1 or 2 is attached.

Citation Information

Patent Citations

  • Adhesive sheet with release sheet

    JP2024078310A

  • Adhesive composition, adhesive layer, and adhesive sheet

    JP6373458B2

  • Adhesive agent composition, adhesive agent, and surface protection film

    WO2022255210A1