Transfer sheet, method for manufacturing article, and article equipped with release film
The transfer sheet with a release film and transfer layer, having specific stiffness and peel strength characteristics, addresses lifting and peeling issues during the transfer process, ensuring effective adhesion and easy removal, thus enhancing the transfer process and product quality.
Patent Information
- Application Number
- PCT/JP2024/011314
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
The existing transfer sheets face issues with lifting at corner portions and partial peeling of the release film due to springback when transferring a transfer layer onto adherends with multiple surfaces, leading to product defects and difficulties in peeling off the release film.
A transfer sheet with a release film and a transfer layer, where the loop stiffness of the release film is 0.18 N/15 mm or less and the peel strength is 0.7 N/25 mm or less, satisfying the relationship Y≧0.67X+0.17, allowing for effective suppression of lifting and peeling issues.
The solution prevents lifting at corner portions, suppresses partial peeling due to springback, and enables easy peeling of the release film from the transfer layer, ensuring a smooth transfer process and maintaining the integrity of the transfer sheet.
Smart Images

Figure JP2024011314_03102024_PF_FP_ABST
Abstract
Description
Transfer sheet, article manufacturing method, and article with release film
[0001] The present disclosure relates to a transfer sheet, a method for manufacturing an article, and an article with a release film.
[0002] It is known to decorate an adherend, such as a metal member or a resin member, by transferring a transfer layer (a layer transferred from the transfer sheet) of a transfer sheet to the adherend. For example, Patent Document 1 discloses a rain gutter having an oxide film layer disposed on the outer surface of an aluminum base material, a decorative layer disposed on the outer surface of the oxide film layer, and a pattern applied to the surface of the decorative layer. Specifically, Patent Document 1 discloses forming a decorative layer on the outer surface of an anodized aluminum base material by hydraulic transfer processing.
[0003] Japanese Patent Application Laid-Open No. 2020-12283
[0004] When transferring the transfer layer of the transfer sheet to an adherend having multiple surfaces, the stiffness of the release film of the transfer sheet may cause the transfer sheet to lift off the adherend at the corners of the adherend. Furthermore, after the transfer sheet is adhered to the adherend, the stiffness of the release film may cause the release film to partially peel off from the transfer layer (partial peeling of the release film due to springback). Furthermore, the transfer sheet is required to be able to easily peel the release film from the transfer layer after the transfer sheet is adhered to the adherend.
[0005] The present disclosure has been made in consideration of the above-mentioned situation, and its main purpose is to provide a transfer sheet that suppresses the lifting of the transfer sheet at the corners, suppresses partial peeling of the release film due to springback, and enables the release film to be easily peeled off from the transfer layer.
[0006] The present disclosure provides a transfer sheet having a release film and a transfer layer disposed on one side of the release film, wherein the loop stiffness of the release film is 0.18 N / 15 mm or less, the peel strength of the release film and the transfer layer is 0.7 N / 25 mm or less, and when the loop stiffness is X and the peel strength is Y, X and Y satisfy Y≧0.67X+0.17.
[0007] The present disclosure provides a method for manufacturing an article, comprising: a preparation step of preparing an adherend having multiple surfaces and the above-mentioned transfer sheet; and a wrapping step of sequentially bonding the transfer layer of the transfer sheet to the multiple surfaces of the adherend using a roller.
[0008] The present disclosure provides an article with a release film, comprising: an adherend having a plurality of surfaces; a transfer layer disposed so as to follow the plurality of surfaces; and a release film disposed so as to follow the transfer layer, wherein the loop stiffness of the release film is 0.18 N / 15 mm or less; the peel strength of the release film and the transfer layer is 0.7 N / 25 mm or less; and, when the loop stiffness is X and the peel strength is Y, X and Y satisfy Y≧0.67X+0.17.
[0009] The present disclosure has the effect of providing a transfer sheet that suppresses lifting of the transfer sheet at the corners, suppresses partial peeling of the release film due to springback, and enables the release film to be easily peeled off from the transfer layer.
[0010] 3 is a schematic cross-sectional view illustrating a transfer sheet according to the present disclosure. FIG. 4 is an explanatory diagram outlining a method for measuring loop stiffness according to the present disclosure. FIG. 5 is a schematic side view illustrating a lapping process according to the present disclosure. FIG. 6 is a cross-sectional view of the A-A cross-section, the B-B cross-section, the C-C cross-section, the D-D cross-section, and the E-E cross-section in FIG. 3. FIG. 7 is an explanatory diagram illustrating the axial direction of each roller. FIG. 8 is a schematic cross-sectional view illustrating a part of an article with a release film according to the present disclosure and a part of an article according to the present disclosure. FIG. 9 is a graph showing the relationship between loop stiffness and peel strength in Examples 1 to 5 and Comparative Examples 1 to 3.
[0011] Below, embodiments will be described with reference to the drawings etc. However, the present disclosure can be implemented in many different forms and should not be limited to the description of the embodiments exemplified below. Furthermore, to make the explanation clearer, the drawings may show the width, thickness, and shape of each part schematically compared to the actual form, but this is merely an example and should not be interpreted as limiting.
[0012] In this specification, when describing a mode in which another component is disposed on a certain component, the term "above" or "below" refers to both a case in which another component is disposed directly above or below the certain component so as to be in contact with the component, and a case in which another component is disposed above or below the certain component with another component interposed therebetween, unless otherwise specified. Also, in this specification, when describing a mode in which another component is disposed on the surface of a certain component, the term "on the surface" refers to both a case in which another component is disposed directly above or below the certain component so as to be in contact with the component, and a case in which another component is disposed above or below the certain component with another component interposed therebetween, unless otherwise specified.
[0013] The transfer sheet, the method for manufacturing an article, and the article with a release film according to the present disclosure will be described in detail below.
[0014] A. Transfer Sheet Fig. 1(a) is a schematic cross-sectional view illustrating a transfer sheet in the present disclosure. As shown in Fig. 1(a), a transfer sheet 10 has a release film 1 and a transfer layer X arranged on one side of the release film 1. The transfer layer X shown in Fig. 1(a) is formed by attaching a first protective layer 2 and a second protective layer 3 from the release film 1 side in the thickness direction D. T In this order, the second protective layer 3 and the transfer layer X are present. As shown in FIG. 1(b), the transfer sheet 10 may also have a design layer 4 on the surface of the second protective layer 3 opposite the first protective layer 2. In the present disclosure, the loop stiffness of the release film 1 is within a predetermined range. Furthermore, the peel strength of the release film 1 and the transfer layer X is within a predetermined range. Furthermore, the loop stiffness of the release film 1 and the peel strength of the release film 1 and the transfer layer X satisfy a predetermined relationship.
[0015] According to the present disclosure, the loop stiffness and the peel strength are each within a specific range, and further, the loop stiffness and the peel strength satisfy a specific relationship, resulting in a transfer sheet that simultaneously suppresses lifting of the transfer sheet at the corners, suppresses partial peeling of the release film due to springback, and enables the release film to be easily peeled from the transfer layer.
[0016] As described above, when transferring the transfer layer of the transfer sheet to an adherend having multiple surfaces, the stiffness of the release film of the transfer sheet may cause the transfer sheet to not adhere sufficiently to the adherend at the corners of the adherend, resulting in the transfer sheet floating away from the adherend. The corners of the adherend are the boundaries between adjacent surfaces. Lifting of the transfer sheet at the corners can lead to product defects, so it is preferable to prevent this. Furthermore, after the transfer sheet is adhered to the adherend, the stiffness of the release film may cause the release film to partially peel away from the transfer layer (partial peeling of the release film due to springback). After the transfer sheet is adhered to the adherend, the release film functions as a protective film that protects the adherend and the transfer layer from external impact. Therefore, it is preferable that partial peeling of the release film due to springback does not occur. Furthermore, the transfer sheet is required to be able to easily peel away from the transfer layer after the transfer sheet is adhered to the adherend.
[0017] In particular, immediately after the transfer sheet is adhered to the adherend, it is necessary to prevent the release film from partially peeling off from the transfer layer due to springback. On the other hand, it is ultimately necessary to ensure that the release film, which also functions as a protective film, can be smoothly peeled off from the transfer layer. The present inventors have conducted extensive research to address these conflicting objectives and have found that the above conflicting objectives can be resolved by ensuring that the peel strengths of the release film and transfer layer are within a specific range and that the peel strength and the loop stiffness of the release film satisfy a specific relationship. Furthermore, the present inventors have found that by ensuring that the loop stiffness of the release film is within a specific range, lifting of the transfer sheet at corners can be prevented, even when the transfer layer is attached to an adherend having multiple surfaces.
[0018] As described below, the transfer sheet of the present disclosure is preferably used in a wrapping process. The wrapping process involves sequentially laminating the transfer layer of the transfer sheet to multiple surfaces of an adherend using a roller. Because the peel strength of the release film and the transfer layer is lower than the peel strength of each layer constituting the transfer layer, for example, laminating the transfer sheet sequentially to multiple surfaces, as in a wrapping process, partial peeling of the release film due to the above-mentioned springback is likely to occur. In contrast, in the present disclosure, the peel strength of the release film and the transfer layer is within a specific range, and further, the above-mentioned peel strength and the loop stiffness of the release film satisfy a specific relationship, thereby suppressing partial peeling of the release film from the transfer layer due to springback, and ultimately enabling the release film, which also functions as a protective film, to be successfully peeled from the transfer layer.
[0019] Furthermore, as described below, the transfer sheet of the present disclosure is useful as a transfer sheet used in the manufacture of exterior products (items for outdoor use). Exterior products are exposed to harsher environments than interior products (items for indoor use), and therefore require high weather resistance. For example, when manufacturing exterior products using a decorative sheet, a transparent resin layer may be provided on the decorative sheet to improve its strength. In this case, since the transparent resin layer is a relatively thick layer, high weather resistance can be imparted by, for example, adding a sufficient amount of weather resistance agent to the transparent resin layer. In contrast, imparting high weather resistance to a transfer sheet that does not have a layer corresponding to a transparent resin layer is technically difficult. In the present disclosure, as described below, it is preferable that the transfer layer has a first protective layer and a second protective layer, and that both the first protective layer and the second protective layer contain a weather resistance agent. This allows for high weather resistance to be imparted while maintaining the properties required of the first protective layer (e.g., surface properties such as scratch resistance) and the properties required of the second protective layer (e.g., adhesion).
[0020] Furthermore, in the case of a transfer sheet, the adhesion between the first protective layer and the second protective layer is likely to be insufficient. Here, in the case of a decorative sheet, a design layer is typically formed on a base layer, then a second protective layer is formed on the design layer, and then a first protective layer is formed on the second protective layer. The first protective layer is typically formed by curing a composition for forming the first protective layer formed on the second protective layer, resulting in good adhesion between the first protective layer and the second protective layer. In contrast, in the case of a transfer sheet, the first protective layer is typically formed on a release film, then a second protective layer is formed on the first protective layer, and then a design layer is formed on the second protective layer. The first protective layer is typically formed by curing a composition for forming the first protective layer on a release film. Since the second protective layer is formed on the cured first protective layer, the adhesion between the first protective layer and the second protective layer is likely to be insufficient. In the present disclosure, it is preferable that the second protective layer be a layer with higher flexibility than the first protective layer. This allows for increased adhesion between the first protective layer and the second protective layer.
[0021] 1. Loop Stiffness and Peel Strength In the present disclosure, the loop stiffness of the release film is within a specific range. Also, in the present disclosure, the peel strength of the release film and the transfer layer is within a specific range. Furthermore, in the present disclosure, the loop stiffness and the peel strength satisfy a specific relationship.
[0022] (1) Loop Stiffness In the present disclosure, the loop stiffness of the release film is within a specific range. The degree of stiffness of the release film is determined by the loop stiffness. FIG. 2 is an explanatory diagram outlining the method for measuring loop stiffness in the present disclosure. As shown in FIG. 2, the release film 1 peeled from the transfer sheet is cut to prepare a rectangular sample, and the ends of the release film 1 are overlapped to deform the release film 1 into a loop shape. The overlapped ends are then fixed with a fixing jig 41 of a loop stiffness tester. A pressure jig 42 of the loop stiffness tester is pressed vertically against the loop-shaped release film 1 fixed with the fixing jig 41, and the stress during compression is measured. In the present disclosure, the release film peeled from the transfer sheet is cut into a rectangular shape with a width of 15 mm and a length of 150 mm to prepare a sample. Furthermore, the sample is fixed to a loop stiffness tester so that the loop length is 60 mm, and a pressure jig is pressed against it from the vertical direction to measure the stress during compression, and the maximum value of the stress is determined as the loop stiffness.
[0023] The loop stiffness of the release film is usually 0.18 N / 15 mm or less, and may be 0.15 N / 15 mm or less. If the loop stiffness of the release film is too high, the transfer sheet is likely to lift at the corners. On the other hand, the loop stiffness of the release film is, for example, 0.005 N / 15 mm or more, may be 0.010 N / 15 mm or more, or may be 0.012 N / 15 mm or more. The loop stiffness of the release film can be adjusted, for example, by the thickness of the release film. The thicker the release film, the greater the loop stiffness usually is.
[0024] (2) Peel Strength In the present disclosure, the peel strength of the release film and transfer layer is within a specific range. The peel strength of the release film and transfer layer is measured by the following method. First, a transfer sheet is cut to a width of 25 mm, double-sided tape is attached to the entire surface of the release film opposite the transfer layer, and the release film is fixed to a 25 mm wide metal plate. Next, a 25 mm wide piece of Nichiban Cellotape (registered trademark) is attached to the entire surface of the transfer layer opposite the release film. Next, using a peel strength tester, the peel strength is measured under the conditions of a peel rate of 200 mm / min and a peel angle of 90°. After exceeding the upper yield point, the integrated average value of the peel strength from the point where the lower yield point load is reached to 20 mm is taken, and the peel strength (N / 25 mm) is calculated.
[0025] The peel strength of the release film and the transfer layer is usually 0.7 N / 25 mm or less, and may be 0.6 N / 25 mm or less. If the peel strength of the release film and the transfer layer is too high, it becomes difficult to peel the release film from the transfer layer. On the other hand, the peel strength of the release film and the transfer layer is, for example, 0.17 N / 25 mm or more, and may be 0.19 N / 25 mm or more. The peel strength of the release film and the transfer layer can be adjusted, for example, by the surface properties of the surface of the release film facing the transfer layer and the hardness of the transfer layer (e.g., protective layer). For example, the greater the surface roughness of the surface of the release film facing the transfer layer, the smaller the peel strength of the release film and the transfer layer. Furthermore, the softer the transfer layer (e.g., protective layer), the greater the peel strength of the release film and the transfer layer.
[0026] (3) Relationship between Loop Stiffness and Peel Strength In the present disclosure, when the loop stiffness is X and the peel strength is Y, X and Y usually satisfy Y≧0.67X+0.17. When X and Y satisfy Relational Formula 1, partial peeling of the release film due to springback can be suppressed. As described in the examples below, X and Y may satisfy Y≧0.67X+0.19. Furthermore, X and Y may satisfy Y≦2.99X+0.03.
[0027] 2. Transfer Layer The transfer layer in the present disclosure is a layer transferred from the transfer sheet. The transfer layer preferably has a protective layer that protects the surface of the adherend. The transfer layer also preferably has a design layer on the side of the protective layer opposite the release film.
[0028] (1) Protective Layer The transfer layer in the present disclosure preferably has a protective layer. The protective layer is not particularly limited. The transfer layer may have only one protective layer, or may have two or more protective layers. For example, the transfer layer may be a single layer of the first protective layer described below, or a single layer of the second protective layer described below. In particular, the transfer layer preferably has the first protective layer and the second protective layer described below in this order in the thickness direction from the release film side. This is because it is particularly useful as a transfer sheet used for exterior products (items for outdoor use).
[0029] (i) First Protective Layer The transfer layer in the present disclosure preferably has a first protective layer. The first protective layer contributes to improving the surface properties (e.g., scratch resistance) of the article. The first protective layer and the release film may be arranged so as to be in direct contact with each other, or may be arranged via another layer.
[0030] The first protective layer preferably contains a cured product (crosslinked structure) of a curable resin composition as a resin component, and the proportion of the cured product of the curable resin composition relative to the total resin components constituting the first protective layer is, for example, 70% by mass or more, or may be 90% by mass or more, or may be 95% by mass or more, or may be 100% by mass.
[0031] Examples of the curable resin composition used for the first protective layer include an ionizing radiation curable resin composition and a heat curable resin composition. Examples of the ionizing radiation curable resin composition include an electron beam curable resin composition and an ultraviolet ray curable resin composition. Among these, an electron beam curable resin composition is preferred because it does not require a polymerization initiator, has little odor, and is less likely to cause coloration.
[0032] The ionizing radiation-curable resin composition is a composition containing a compound having an ionizing radiation-curable functional group (hereinafter also referred to as "ionizing radiation-curable compound"). The ionizing radiation-curable functional group is a group that crosslinks and cures upon irradiation with ionizing radiation, and examples thereof include functional groups having an ethylenic double bond, such as a (meth)acryloyl group, a vinyl group, and an allyl group. In the present disclosure, the (meth)acryloyl group refers to an acryloyl group or a methcroyl group.
[0033] Ionizing radiation refers to electromagnetic waves or charged particle beams that have an energy quantum capable of polymerizing or crosslinking molecules. Examples of ionizing radiation include electron beams (EB) and ultraviolet (UV) rays. Other examples of ionizing radiation include electromagnetic waves such as X-rays and gamma rays, and charged particle beams such as alpha rays and ion beams.
[0034] The ionizing radiation-curable resin composition preferably contains, as the ionizing radiation-curable compound, one or more compounds selected from, for example, urethane (meth)acrylate, epoxy (meth)acrylate, polyester (meth)acrylate, polyether (meth)acrylate, polycarbonate (meth)acrylate, and acrylic (meth)acrylate. Among these, the ionizing radiation-curable resin composition preferably contains at least a urethane (meth)acrylate as the ionizing radiation-curable compound. In the present disclosure, urethane (meth)acrylate refers to urethane acrylate or urethane methacrylate. The urethane (meth)acrylate is preferably a caprolactone-based urethane (meth)acrylate.
[0035] When the ionizing radiation curable resin composition contains a caprolactone-based urethane (meth)acrylate, the caprolactone-based urethane (meth)acrylate preferably has 2 or more and 4 or less functional groups, more preferably 2 or more and 3 or less functional groups.
[0036] The ionizing radiation curable resin composition may contain a caprolactone-based urethane (meth)acrylate and a non-caprolactone-modified urethane (meth)acrylate. In this case, the content of the caprolactone-based urethane (meth)acrylate in the first protective layer is set to MCLUA The content of the urethane (meth)acrylate that is not modified with caprolactone is M UA Let's say. UA and M CLUA M for the sum of CLUA Mass ratio (M CLUA / (M UA +M CLUA )) is, for example, 40% by mass or more and 90% by mass or less, or may be 45% by mass or more and 80% by mass or less, or may be 50% by mass or more and 70% by mass or less.
[0037] Caprolactone-based urethane (meth)acrylates can usually be obtained by reacting caprolactone-based polyols, organic isocyanates, and hydroxy (meth)acrylates. Examples of synthesis methods include reacting polycaprolactone-based polyols with organic polyisocyanates to produce polyurethane prepolymers containing -NCO groups (isocyanate groups) at both ends, followed by reaction with hydroxy (meth)acrylates.
[0038] Commercially available caprolactone polyols can be used, preferably those having two hydroxyl groups and a number-average molecular weight of 500 to 3,000, more preferably 750 to 2,000. Non-caprolactone polyols, such as ethylene glycol, diethylene glycol, 1,4-butanediol, and 1,6-hexanediol, can also be used singly or in combination in any ratio. Preferred organic polyisocyanates are diisocyanates having two isocyanate groups. From the viewpoint of suppressing yellowing, preferred examples include isophorone diisocyanate, hexamethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, and trimethylhexamethylene diisocyanate. Preferred hydroxy(meth)acrylates include 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, and caprolactone-modified 2-hydroxyethyl acrylate.
[0039] When the ionizing radiation-curable resin composition contains a caprolactone polyol, the caprolactone urethane (meth)acrylate is preferably a caprolactone diol urethane (meth)acrylate. The caprolactone diol urethane (meth)acrylate refers to a caprolactone urethane (meth)acrylate having a diethylene glycol terminal. The use of a caprolactone diol urethane (meth)acrylate can prevent cracking and whitening of the first protective layer.
[0040] The ionizing radiation-curable resin composition may contain a hydroxyl group-containing (meth)acrylate as the ionizing radiation-curable compound. Examples of the hydroxyl group-containing (meth)acrylate include hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, 1,4-cyclohexanedimethanol monoacrylate, polyethylene glycol monoacrylate, polyethylene glycol monomethacrylate, trimethylolpropane diacrylate, trimethylolpropane dimethacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, dipentaerythritol hexaacrylate, dipentaerythritol hexamethacrylate, glycidyl acrylate, glycidyl methacrylate, isocyanuric acid monoacrylate, isocyanuric acid monomethacrylate, isocyanuric acid diacrylate, isocyanuric acid dimethacrylate, glycerin diacrylate, and glycerin dimethacrylate. The hydroxyl group-containing (meth)acrylate may be a hydroxyl group-containing (meth)acrylate modified with ethylene oxide (EO), propylene oxide (PO), caprolactone, etc. The proportion of the hydroxyl group-containing (meth)acrylate in the ionizing radiation-curable resin composition is, for example, 10% by mass or more and 90% by mass or less.
[0041] The number average molecular weight of the ionizing radiation-curable compound is, for example, from 200 to 10,000, or from 1,000 to 10,000, or from 2,000 to 10,000. The number average molecular weight is an average molecular weight measured by GPC analysis and converted into standard polystyrene.
[0042] For example, when the ionizing radiation-curable compound is an ultraviolet-curable compound, the ionizing radiation-curable compound preferably contains at least one of a photopolymerization initiator and a photopolymerization accelerator. Examples of photopolymerization initiators include acetophenone, benzophenone, α-hydroxyalkylphenone, Michler's ketone, benzoin, benzyl dimethyl ketal, benzoyl benzoate, α-acyloxime ester, acylphosphine oxide, and thioxanthones. Examples of photopolymerization accelerators include p-dimethylaminobenzoic acid isoamyl ester and p-dimethylaminobenzoic acid ethyl ester.
[0043] The first protective layer preferably contains a weathering agent. Examples of weathering agents include an ultraviolet absorber and a light stabilizer. The first protective layer preferably contains at least one of an ultraviolet absorber and a light stabilizer. The first protective layer may contain one or more ultraviolet absorbers. Similarly, the first protective layer may contain one or more light stabilizers.
[0044] Examples of the ultraviolet absorber contained in the first protective layer include organic ultraviolet absorbers such as triazine-based ultraviolet absorbers, benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, oxybenzophenone-based ultraviolet absorbers, salicylic acid ester-based ultraviolet absorbers, and cyano(meth)acrylate-based ultraviolet absorbers, and inorganic ultraviolet absorbers such as titanium dioxide, cerium oxide, and zinc oxide. Among these, triazine-based ultraviolet absorbers are more preferred.
[0045] Examples of triazine-based ultraviolet absorbers include hydroxyphenyltriazine-based ultraviolet absorbers, such as 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, and 2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine. azine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5[2-(2-ethylhexanoyloxy)ethoxy]phenol.
[0046] The content of the ultraviolet absorber in the first protective layer is, for example, 0.5 parts by mass to 10 parts by mass, or alternatively, 0.8 parts by mass to 8 parts by mass, or alternatively, 1 part by mass to 5 parts by mass, relative to 100 parts by mass of the ionizing radiation-curable compound. If the content of the ultraviolet absorber is too high, bleeding out of the ultraviolet absorber may occur, whereas if the content of the ultraviolet absorber is too low, sufficient ultraviolet absorption performance may not be obtained.
[0047] Examples of the light stabilizer contained in the first protective layer include hindered amine light stabilizers, such as 1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate, methyl(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate, and 2,4-bis[N-butyl-N-(1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)amino]-6-(2-hydroxyethylamine)-1,3,5-triazine).
[0048] The content of the light stabilizer in the first protective layer is, for example, 1 part by mass to 10 parts by mass, or alternatively 1.5 parts by mass to 8 parts by mass, or alternatively 2 parts by mass to 5 parts by mass, relative to 100 parts by mass of the ionizing radiation-curable compound. If the content of the light stabilizer is too high, bleed-out of the light stabilizer may occur, whereas if the content of the light stabilizer is too low, sufficient light stability may not be obtained.
[0049] The first protective layer may contain additives such as a silicone compound, a polymerization inhibitor, a crosslinking agent, an antistatic agent, an adhesion improver, an antioxidant, a leveling agent, a thixotropy-imparting agent, a coupling agent, a plasticizer, an antifouling agent, an antifoaming agent, and a filler. The thickness of the first protective layer is, for example, 2 μm or more and 20 μm or less, or 3 μm or more and 15 μm or less, or 4 μm or more and 10 μm or less. If the first protective layer is too thin, sufficient weather resistance may not be obtained. If the first protective layer is too thick, cracks may easily occur in the first protective layer, and good adhesion may not be obtained.
[0050] (ii) Second Protective Layer The transfer layer in the present disclosure preferably has a second protective layer on the side of the first protective layer opposite the release film. The second protective layer is preferably a layer that is more flexible than the first protective layer. The second protective layer and the first protective layer may be disposed so as to be in direct contact with each other, or may be disposed via another layer.
[0051] The second protective layer preferably contains a cured product (crosslinked structure) of a curable resin composition as a resin component. The proportion of the cured product of the curable resin composition relative to the total resin components constituting the second protective layer is, for example, 70% by mass or more, or may be 90% by mass or more, or 95% by mass or more, or may be 100% by mass.
[0052] Examples of the curable resin composition used in the second protective layer include thermosetting resin compositions. The thermosetting resin composition is a composition containing at least a thermosetting resin and is a composition that cures when heated. Examples of the thermosetting resin include (meth)acrylic resins, phenolic resins, urea melamine resins, epoxy resins, unsaturated polyester resins, and silicone resins. The thermosetting resin composition preferably contains a urethane (meth)acrylic resin as the thermosetting resin. The thermosetting resin composition may further contain a curing agent such as an isocyanate curing agent or an epoxy curing agent.
[0053] Furthermore, when the curable resin composition contains a urethane(meth)acrylic resin, the urethane(meth)acrylic resin is preferably a urethane(meth)acrylic copolymer, more preferably a polycarbonate-based urethane(meth)acrylic copolymer. The polycarbonate-based urethane(meth)acrylic copolymer is a resin obtained by radical polymerization of a (meth)acrylic monomer with a polycarbonate-based polyurethane polymer obtained by reacting a polycarbonate diol with a (di)isocyanate.
[0054] Examples of the (di)isocyanate include aromatic isocyanates such as 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 1,5-naphthalene diisocyanate, n-isocyanate phenylsulfonyl isocyanate, o-isocyanate phenylsulfonyl isocyanate, and p-isocyanate phenylsulfonyl isocyanate; aliphatic isocyanates such as 1,6-hexamethylene diisocyanate; and alicyclic isocyanates such as isophorone diisocyanate, hydrogenated xylylene diisocyanate, and hydrogenated diphenylmethane diisocyanate.
[0055] Examples of the (meth)acrylic monomer include (meth)acrylic acid, alkyl (meth)acrylate esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, and isobutyl (meth)acrylate.
[0056] In the polycarbonate-based urethane (meth)acrylic copolymer, the mass ratio of the urethane component to the total of the (meth)acrylic component and the urethane component ([urethane component] / ([(meth)acrylic component]+[urethane component]) is, for example, 70% by mass or more and 95% by mass or less, alternatively 75% by mass or more and 95% by mass or less, or alternatively 80% by mass or more and 90% by mass or less.
[0057] The second protective layer preferably contains a weathering agent. Examples of weathering agents include an ultraviolet absorber and a light stabilizer. The second protective layer preferably contains at least one of an ultraviolet absorber and a light stabilizer. Preferred types and modes of weathering agents are the same as those described above in "(i) First Protective Layer," and therefore will not be described here. In particular, the second protective layer preferably contains a triazine-based ultraviolet absorber. Furthermore, the second protective layer preferably contains a hindered amine-based light stabilizer.
[0058] The content of the ultraviolet absorber in the second protective layer is, for example, 0.1 parts by mass or more and 50 parts by mass or less, or may be 3 parts by mass or more and 40 parts by mass or less, or may be 10 parts by mass or more and 35 parts by mass or less, relative to 100 parts by mass of the resin component. Furthermore, the content of the ultraviolet absorber in the second protective layer (content relative to 100 parts by mass of the resin component) may be greater than the content of the ultraviolet absorber in the first protective layer (content relative to 100 parts by mass of the resin component).
[0059] The content of the light stabilizer in the second protective layer is, for example, 0.1 to 15 parts by mass, or alternatively 1 to 15 parts by mass, or alternatively 3 to 10 parts by mass, relative to 100 parts by mass of the resin component. The content of the light stabilizer in the second protective layer (per 100 parts by mass of the resin component) may be greater than the content of the light stabilizer in the first protective layer (per 100 parts by mass of the resin component).
[0060] The second protective layer may contain additives such as silicone compounds, polymerization inhibitors, crosslinking agents, antistatic agents, adhesion improvers, antioxidants, leveling agents, thixotropy-imparting agents, coupling agents, plasticizers, antifouling agents, antifoaming agents, and fillers. The thickness of the second protective layer is, for example, 2 μm to 10 μm, or 3 μm to 8 μm, or 3 μm to 5 μm. If the second protective layer is thin, adhesion (particularly initial adhesion) with the relatively hard first protective layer may be reduced. On the other hand, if the second protective layer is thick, the second protective layer may move more due to heat, making the first protective layer more susceptible to cracking.
[0061] (2) Other Layers The transfer layer in the present disclosure may or may not have a design layer on the side of the protective layer opposite the release film. By providing a design layer, the design of the article is improved. The design layer and the protective layer may be arranged so as to be in direct contact with each other, or may be arranged via another layer.
[0062] Examples of the design layer include a solid layer (a layer coated with ink) and a picture layer (a layer printed with ink). The transfer sheet may have, as the design layer, a picture layer and a solid layer in this order from the release film side. Examples of the picture (pattern) in the picture layer include wood grain patterns, stone grain patterns, sand grain patterns, tile patterns, brickwork patterns, fabric patterns, leather-striped patterns, geometric shapes, letters, symbols, abstract patterns, and floral patterns.
[0063] The design layer usually contains a colorant and a binder resin. Examples of the colorant include inorganic pigments such as carbon black (ink), iron black, titanium white, antimony white, yellow lead, titanium yellow, red iron oxide, cadmium red, ultramarine blue, and cobalt blue; organic pigments (including dyes) such as quinacridone red, isoindolinone yellow, nickel azo complex, phthalocyanine blue, and azomethine azo black; metal pigments such as aluminum and brass; and pearl pigments such as titanium dioxide-coated mica and basic lead carbonate.
[0064] Examples of binder resins include urethane-based resins, acrylic polyol-based resins, (meth)acrylic resins, ester-based resins, amide-based resins, butyral-based resins, styrene-based resins, urethane-acrylic copolymers, vinyl chloride-vinyl acetate copolymers, vinyl chloride-vinyl acetate-acrylic copolymers, chlorinated propylene-based resins, nitrocellulose-based resins, and cellulose acetate-based resins.
[0065] The design layer may contain additives such as ultraviolet absorbers, light stabilizers, curing agents, plasticizers, catalysts, etc. The thickness of the design layer is, for example, 0.5 μm to 20 μm, or may be 1 μm to 10 μm, or may be 2 μm to 5 μm.
[0066] The transfer layer in the present disclosure may or may not have an adhesive layer on the surface of the protective layer opposite the release film. The adhesive layer and the protective layer may be arranged so as to be in direct contact with each other, or may be arranged via another layer (e.g., a design layer). The adhesive layer may contain a component having adhesive properties. Examples of the component having adhesive properties include (meth)acrylic resins, vinyl chloride-vinyl acetate copolymers, vinyl acetate resins, ester resins, epoxy resins, imide resins, and rubber resins.
[0067] The adhesive layer may be a so-called pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer has adhesiveness at room temperature. Examples of resins contained in the pressure-sensitive adhesive layer include (meth)acrylic resins, vinyl resins, ester resins, urethane resins, amide resins, epoxy resins, rubber resins, and ionomer resins. The adhesive layer may also be a so-called heat-seal layer. The heat-seal layer exhibits adhesiveness upon application of heat. Examples of resins contained in the heat-seal layer include (meth)acrylic resins, urethane resins, olefin resins, ester resins, epoxy resins, urea resins, melamine resins, phenolic resins, and vinyl resins. The thickness of the adhesive layer is, for example, 1 μm or more and 30 μm or less.
[0068] (3) Transfer Layer The thickness of the transfer layer is, for example, 8 μm or more, or may be 10 μm or more, 12 μm or more, or 14 μm or more, while the thickness of the transfer layer is, for example, 50 μm or less, or may be 40 μm or less, or may be 30 μm or less.
[0069] 3. Release Film The transfer sheet of the present disclosure has a release film facing the transfer layer.
[0070] The release film is preferably a resin film. Examples of the resin contained in the resin film include ester-based resins, olefin-based resins, styrene-based resins, vinyl-based resins, (meth)acrylic resins, amide-based resins, imide-based resins, and carbonate-based resins.
[0071] The release film preferably contains an ester resin or an olefin resin. Examples of ester resins include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), and polyethylene terephthalate-isophthalate copolymer. Among these, PET or PBT are preferred, with PET being more preferred, from the viewpoint of being less susceptible to thermal shrinkage during production of the transfer sheet and shrinkage due to irradiation with ionizing radiation.
[0072] Examples of olefin resins include polyethylene, polypropylene, polybutene, ethylene-propylene copolymer, and ethylene-propylene-butene copolymer. Among these, polypropylene is preferred from the viewpoint of being less susceptible to thermal shrinkage during the production of the transfer sheet and to shrinkage due to irradiation with ionizing radiation. The release film may also be, for example, polypropylene (PP)-processed paper.
[0073] The release film may be a stretched film or an unstretched film. The stretching ratio in the machine direction (MD) of the stretched film is, for example, 5 to 30 times. The stretching ratio in the width direction (TD) of the stretched film is, for example, 5 to 30 times. The thickness of the release film is, for example, 10 μm to 200 μm, or may be 15 μm to 150 μm, or may be 20 μm to 100 μm.
[0074] The release film may contain a matting agent kneaded therein. A portion of the kneaded matting agent is usually exposed from the release film. By adding a matting agent to the release film, the peel strength of the release film and the transfer layer can be adjusted. Examples of matting agents include inorganic particles and organic particles. Examples of inorganic particles include silica, alumina, calcium carbonate, magnesium carbonate, calcium sulfate, barium sulfate, and kaolin. Examples of organic particles include acrylic beads, urethane beads, nylon beads, silicone beads, silicone rubber beads, polycarbonate beads, and polyolefin wax (e.g., polypropylene wax, polyethylene wax). The average particle size of the matting agent is, for example, 1.0 μm or more and 10 μm or less, and may be 2.0 μm or more and 8.0 μm or less. The average particle size of the matting agent is determined by the D of particle size distribution measurement (volume basis) by laser light diffraction method. 50 This refers to...
[0075] The release film may have a matte layer containing a matting agent on the surface facing the transfer layer. The matte agent used in the matte layer is the same as described above. The matte layer may also contain a cured product (crosslinked structure) of a curable resin composition as a resin component. Examples of curable resin compositions used in the matte layer include ionizing radiation curable resin compositions and thermosetting resin compositions. Details of the ionizing radiation curable resin composition and the thermosetting resin composition are the same as described above. The matte layer may also contain a thermoplastic resin as a resin component. The matte layer may contain additives such as a release agent, an ultraviolet absorber, an infrared absorber, a light stabilizer, a polymerization inhibitor, a crosslinking agent, an antistatic agent, an antioxidant, a leveling agent, a coupling agent, a plasticizer, an antifoaming agent, a filler, a thermal radical generator, and an aluminum chelating agent, as necessary. The thickness of the matte layer is not particularly limited, but is, for example, 0.1 μm or more and 10 μm or less.
[0076] 4. Transfer Sheet The transfer sheet of the present disclosure has a release film (first release film) and a transfer layer. The transfer sheet may have a second release film on the side of the transfer layer opposite the release film. For example, when the transfer sheet is produced by winding it into a roll, the occurrence of blocking can be suppressed. Details of the second release film are the same as those described above for the first release film, so further description here is omitted. In addition, the transfer sheet of the present disclosure is preferably used for wrapping processing. Details of the wrapping processing will be described in "B. Method for producing an article" below.
[0077] 5. Method for Producing Transfer Sheet The method for producing the transfer sheet in the present disclosure is not particularly limited. For example, when producing the transfer sheet shown in FIG. 1( a), it is preferable to form a first protective layer 2 on one side of a release film 1, and then form a second protective layer 3 on the side of the first protective layer 2 opposite the release film 1. Furthermore, when producing the transfer sheet shown in FIG. 1( b), it is preferable to form a first protective layer 2 on one side of a release film 1, then form a second protective layer 3 on the side of the first protective layer 2 opposite the release film 1, and then form a design layer 4 on the side of the second protective layer 3 opposite the first protective layer 2.
[0078] The first protective layer can be formed, for example, by applying a composition for forming the first protective layer to the surface of a release film and then curing the composition. Examples of the composition application method include gravure printing, bar coating, roll coating, reverse roll coating, and comma coating. Examples of the curing method include irradiation with ionizing radiation such as electron beams and ultraviolet rays.
[0079] The second protective layer can be formed, for example, by applying a composition for forming the second protective layer to the surface of the first protective layer opposite the release film, and then curing the composition as needed. Examples of methods for applying the composition include gravure printing, bar coating, roll coating, reverse roll coating, and comma coating. Examples of curing methods include heat. The design layer can be formed, for example, by applying an ink containing a colorant, a binder resin, and a solvent to the surface of the second protective layer opposite the first protective layer.
[0080] B. Article Manufacturing Method The article manufacturing method according to the present disclosure includes a preparation step of preparing an adherend having a plurality of surfaces and the transfer sheet described above, and a wrapping step of sequentially bonding the transfer layer of the transfer sheet to the plurality of surfaces of the adherend using a roller.
[0081] 3 is a schematic cross-sectional view illustrating a lapping process according to the present disclosure. In FIG. 3, the adherend 20 is oriented in the longitudinal direction D L While conveying the transfer sheet 10 along the axis, the transfer layer X of the transfer sheet 10 is sequentially bonded to multiple surfaces of the adherend 20 using multiple rollers 60 (60a to 60e).
[0082] According to the present disclosure, by using the above-mentioned transfer sheet, it is possible to simultaneously suppress the lifting of the transfer sheet at the corners, suppress partial peeling of the release film due to springback, and enable the release film to be easily peeled off from the transfer layer.
[0083] 1. Preparation Step The preparation step in the present disclosure is a step of preparing an adherend having multiple surfaces and the transfer sheet described above. The transfer sheet is the same as that described above in "A. Transfer Sheet," so a description thereof will be omitted here.
[0084] An example of an adherend in the present disclosure is a metal member. Because the metal member and the resin contained in the transfer layer are different materials, the adhesion between them tends to be low. In this case, the adhesion between the adherend and the transfer layer can be improved by adhering the adherend and the transfer layer, for example, via an adhesive layer described below. In particular, exterior products (items for outdoor use) are exposed to harsh environments, so high adhesion between the adherend and the transfer layer is desirable.
[0085] The metal member is a member containing a simple metal or a metal alloy. Examples of metals used for the metal member include aluminum, iron, steel, and copper. The metal member is preferably an aluminum member. This is because aluminum members are lightweight and have excellent corrosion resistance, making them useful as adherends for exterior parts (items for outdoor use). The aluminum member is a member containing aluminum or an aluminum alloy. The aluminum member preferably has an aluminum oxide coating on the surface. This is because the corrosion resistance of the aluminum member is improved. Examples of methods for forming the aluminum oxide coating include anodizing.
[0086] Another example of an adherend is a resin member. Examples of resins used in resin members include polycarbonate resins, vinyl chloride resins, acrylic resins, ester resins, styrene resins, olefin resins, acrylonitrile-butadiene-styrene copolymers (ABS resins), phenolic resins, cellulose resins, and rubber. Another example of an adherend is a wooden member. Examples of wooden members include wood veneers, wood plywood, particle boards, and wood fiberboards. Examples of wood used in wooden members include cedar, cypress, pine, and lauan. Another example of an adherend is a ceramic member. The material of the ceramic member may be glass, ceramics, or other ceramics; it may be a non-cement ceramic material such as gypsum; or a non-ceramic ceramic material such as ALC (lightweight aerated concrete).
[0087] The shape of the adherend is not particularly limited, but examples thereof include a plate, a sheet, and a three-dimensional shape. A three-dimensional shape refers to a three-dimensional shape expressed by coordinates of the X-axis, the Y-axis, and the Z-axis. The adherend has multiple surfaces. The surfaces may be flat or curved.
[0088] 2. Adhesive Layer Forming Step The adhesive layer forming step in the present disclosure is a step of forming an adhesive layer on the surface of the transfer layer opposite the release film or on the multiple surfaces of the adherend. The method for manufacturing an article in the present disclosure preferably includes an adhesive layer forming step after the preparation step and before the wrapping step described below.
[0089] The adhesive used in the adhesive layer is not particularly limited, and known adhesives can be used. Examples include heat-sensitive adhesives and pressure-sensitive adhesives. Examples of resins used in adhesives include acrylic resins, urethane resins, vinyl chloride resins, vinyl acetate resins, ester resins, amide resins, vinyl chloride-vinyl acetate copolymers, and styrene-acrylic copolymers. Two-component curing polyurethane adhesives using an isocyanate compound as a curing agent, and polyester adhesives may also be used. Preferably, the adhesive is a solvent-based adhesive or a polyurethane reactive (PUR) adhesive.
[0090] In the adhesive layer forming step, an adhesive layer coating liquid may be applied to the surface of the transfer sheet opposite the release film to form an adhesive layer. In this case, there is an advantage that the adhesive layer coating liquid can be uniformly applied to the transfer sheet. On the other hand, in the adhesive layer forming step, an adhesive layer coating liquid may be applied to multiple surfaces of the adherend to form an adhesive layer. In this case, there is an advantage that the influence of thermal shrinkage of the adhesive is less likely to occur. The thickness of the adhesive layer is not particularly limited, but may be, for example, 2 μm or more and 100 μm or less, 2 μm or more and 50 μm or less, or 2 μm or more and 35 μm or less. Note that, for example, when the transfer sheet has the above-mentioned adhesive layer, the adhesive layer forming step may not be performed.
[0091] 3. Lapping Process The lapping process in the present disclosure is a process of sequentially laminating the transfer layer of the transfer sheet to the multiple surfaces of the adherend using a roller. "Sequential lamination" refers to laminating a transfer sheet to one surface of the adherend, and then laminating a transfer sheet to the surface adjacent to the surface to which the transfer sheet was laminated. Typically, the operation of laminating a transfer sheet to the surface adjacent to the surface to which the transfer sheet was laminated is repeated. For example, a transfer sheet is laminated to a first surface of the adherend, then a transfer sheet is laminated to a second surface adjacent to the first surface, and then a transfer sheet is laminated to a third surface adjacent to the second surface.
[0092] Preferably, each of the multiple surfaces of the adherend extends in the longitudinal direction of the adherend. In the lapping process, a single roller may be used to sequentially bond the transfer sheet to the multiple surfaces of the adherend, or multiple rollers may be used to sequentially bond the transfer sheet to the multiple surfaces of the adherend. In addition, in the lapping process, it is preferable to fix the positions of the rollers and transport the adherend and the transfer sheet.
[0093] As shown in FIG. 3, in the lapping process, the adherend 20 is L It is preferable to use a plurality of rollers 60 (60a to 60e) to sequentially bond the transfer layer X of the transfer sheet 10 to a plurality of surfaces of the adherend 20 while conveying the adherend 20 along the lamination path. In the lapping process, the transfer layer X of the transfer sheet 10 is bonded to one surface of the adherend 20 using the rollers 60, and then the transfer layer X of the transfer sheet 10 is bonded to another surface of the adherend 20 using successive rollers 60.
[0094] As shown in FIG. 4( a ), the first surface S of the adherend 20 1 The first roller 60a is pressed against the first surface S of the adherend 20 via the transfer sheet 10. 1The transfer sheet 10 (transfer layer X) is attached to the adherend. Although not shown, it is preferable that the above-mentioned adhesive layer is formed between the adherend and the transfer sheet (transfer layer). In addition, in FIG. 4(a), the axial direction A of the first roller 60a is 1 is the horizontal direction.
[0095] Next, as shown in FIG. 4(b), the transfer sheet 10 is guided by the first guide rollers 60b, 60b' so as to be folded, and then, as shown in FIG. 4(c), the second surface S of the adherend 20 is 2 , S 2 The second rollers 60c and 60c' are pressed against the second surface S of the adherend 20 via the transfer sheet 10. 2 , S 2 In FIG. 4C, the transfer sheet 10 (transfer layer X) is attached to the second rollers 60c and 60c′ in the axial direction A 2 , A 2 ´ is the vertical direction.
[0096] Next, as shown in FIG. 4(d), the transfer sheet 10 is guided by the second guide roller 60d so as to be folded, and then, as shown in FIG. 4(e), the third surface S of the adherend 20 is 3 The third roller 60e is pressed against the third surface S of the adherend 20 via the transfer sheet 10. 3 In FIG. 4( e ), the transfer sheet 10 (transfer layer X) is attached to the third roller 60 e in the axial direction A 3 is the horizontal direction.
[0097] As shown in FIG. 5, the axial direction A of the first roller 1 to the axial direction A of the second roller 2 The angle to 12 and the axial direction A of the first roller 1 Axial direction A from the first guide roller M The angle to 1M The above angle (central angle) is an angle in the same circumferential direction. 12 and θ 1M is θ 12 >θ 1MIt is preferable that the following condition is satisfied. By gradually changing the axial direction of each roller along the longitudinal direction of the adherend 20, it is possible to further suppress the occurrence of cracks in the transfer layer when the transfer layer is transferred to the adherend.
[0098] As shown in FIG. 5, the axial direction A of the second roller 2 to the axial direction A of the third roller 3 The angle to 23 and the axial direction A of the second roller 2 Axial direction A from the second guide roller N The angle to 2N The above angle (central angle) is an angle in the same circumferential direction. 23 and θ 2N is θ 23 >θ 2N It is preferable that the following condition is satisfied. By gradually changing the axial direction of each roller along the longitudinal direction of the adherend 20, it is possible to further suppress the occurrence of cracks in the transfer layer when the transfer layer is transferred to the adherend.
[0099] In the lapping process, a heated roller may be used. The heating temperature of the roller is, for example, 200°C or lower, and may be 180°C or lower. If the heating temperature is high, the transfer sheet may be softened more than necessary. On the other hand, the heating temperature of the roller is, for example, 100°C or higher, and may be 110°C or higher, or 120°C or higher.
[0100] Figure 6(a) is a schematic cross-sectional view illustrating a portion of an article with a release film in the present disclosure, and is a schematic cross-sectional view corresponding to region α in Figure 4(e). As shown in Figure 6(a), an article with a release film 50 having at least a transfer sheet 10 and an adherend 20 is obtained by the wrapping process. The article with a release film 50 shown in Figure 6(a) also has an adhesive layer 30 between the transfer sheet 10 and the adherend 20. The article with a release film 50 shown in Figure 6(a) also has a release film 1, a transfer layer X, an adhesive layer 30, and an adherend 20 arranged in a thickness direction D. T In this order,
[0101] The method for manufacturing an article according to the present disclosure may include a peeling step of peeling the release film from the transfer layer after the wrapping step. As shown in Fig. 6(b), the peeling step results in an article 100 having at least the transfer layer X and the adherend 20. The article 100 shown in Fig. 6(b) also has an adhesive layer 30 between the transfer layer X and the adherend 20. The article 100 shown in Fig. 6(b) also has the transfer layer X, the adhesive layer 30, and the adherend 20 arranged in the thickness direction D. T In this order,
[0102] 3. Articles The article of the present disclosure has an adherend having multiple surfaces and a transfer layer disposed in conformity with the multiple surfaces. An adhesive layer may be disposed between the adherend and the transfer layer. The article of the present disclosure is used, for example, as a building material. Building materials are used, for example, in buildings such as houses, offices, stores, hospitals, and clinics. The article may be an exterior product (an article for outdoor use) or an interior product (an article for indoor use). Specific examples of articles include exterior walls, roofs, soffits, louvers, door pockets, window frames, doors, door frames, handrails, fences, and drying racks.
[0103] C. Article with Release Film The article with a release film in the present disclosure comprises an adherend having a plurality of surfaces, a transfer layer disposed so as to follow the plurality of surfaces, and a release film disposed so as to follow the transfer layer, wherein the loop stiffness of the release film is 0.18 N / 15 mm or less, the peel strength of the release film and the transfer layer is 0.7 N / 25 mm or less, and when the loop stiffness is X and the peel strength is Y, X and Y satisfy Y≧0.67X+0.17.
[0104] According to the present disclosure, the loop stiffness and the peel strength are each within a specific range, and further, the loop stiffness and the peel strength satisfy a specific relationship, thereby providing an article with a release film that simultaneously suppresses lifting of the transfer sheet at the corners, suppresses partial peeling of the release film due to springback, and enables the release film to be satisfactorily peeled from the transfer layer. The article with a release film in the present disclosure is the same as that described above in "B. Method for manufacturing an article," and therefore will not be described here.
[0105] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included within the technical scope of the present disclosure.
[0106] [Example 1] A polyethylene terephthalate film (kneaded matte, thickness: 26 μm) that had not been subjected to an easy-adhesion treatment and had a matting agent kneaded into it was prepared as a release film. The composition for forming the first protective layer described below was applied to one side of the release film by gravure coating to form an uncured resin layer. The composition was then cured by irradiating with 50 kGy of electron beams at an acceleration voltage of 165 kV to form a first protective layer with a thickness of 5 μm. Then, corona irradiation was performed on the side of the first protective layer opposite the release film. <Composition for forming first protective layer (EB1)> Ionizing radiation curable resin composition: 100 parts by mass Caprolactone urethane acrylate: 30 parts by mass Pentaerythritol triacrylate (hydroxyl group-containing acrylate): 70 parts by mass Ultraviolet absorber: 2 parts by mass (product name: TINUVIN 479, BASF) Light stabilizer having a reactive functional group: 2 parts by mass (product name: SANOL LS-3410, Nippon Nyukazai Co., Ltd.)
[0107] Next, the following composition for forming a second protective layer was applied by gravure coating to the corona-irradiated surface of the first protective layer and dried to form a second protective layer with a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by mass Ultraviolet absorber: 17 parts by mass (product name: TINUVIN 400, BASF) Ultraviolet absorber: 13 parts by mass (product name: TINUVIN 479, BASF) Hindered amine-based light stabilizer: 8 parts by mass (product name: TINUVIN 123, BASF) Antiblocking agent: 9 parts by mass (silica particles, average particle size 3 μm) Curing agent: 25 parts by mass (hexamethylene diisocyanate)
[0108] Next, the following ink for forming the design layer was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in this order in the thickness direction. <Ink for forming the design layer> Resin composition: 100 parts by mass Acrylic resin: 80 parts by mass Vinyl chloride-vinyl acetate copolymer: 20 parts by mass Pigment
[0109] [Example 2] A mirror-finished polyethylene terephthalate film (thickness: 38 μm) that had not been subjected to an easy-adhesion treatment was prepared as a release film. The composition for forming the first protective layer described below was applied to one side of the release film by gravure coating to form an uncured resin layer. The composition was then cured by irradiating with 50 kGy of electron beams at an acceleration voltage of 165 kV to form a first protective layer with a thickness of 5 μm. The surface of the first protective layer opposite the release film was then subjected to corona irradiation. <Composition for forming first protective layer (EB2)> Ionizing radiation curable resin composition: 100 parts by mass Caprolactone urethane acrylate: 50 parts by mass Pentaerythritol triacrylate (hydroxyl group-containing acrylate): 50 parts by mass Ultraviolet absorber: 2 parts by mass (product name: TINUVIN 479, BASF) Light stabilizer having a reactive functional group: 2 parts by mass (product name: SANOL LS-3410, Nippon Nyukazai Co., Ltd.)
[0110] Next, the following composition for forming a second protective layer was applied by gravure coating to the corona-irradiated surface of the first protective layer and dried to form a second protective layer with a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by mass Ultraviolet absorber: 17 parts by mass (product name: TINUVIN 400, BASF) Ultraviolet absorber: 13 parts by mass (product name: TINUVIN 479, BASF) Hindered amine-based light stabilizer: 8 parts by mass (product name: TINUVIN 123, BASF) Antiblocking agent: 9 parts by mass (silica particles, average particle size 3 μm) Curing agent: 25 parts by mass (hexamethylene diisocyanate)
[0111] Next, the following ink for forming the design layer was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in this order in the thickness direction. <Ink for forming the design layer> Resin composition: 100 parts by mass Acrylic resin: 80 parts by mass Vinyl chloride-vinyl acetate copolymer: 20 parts by mass Pigment
[0112] [Example 3] A polyethylene terephthalate film (matte coat, thickness: 50 μm) having a matte layer containing a matting agent was prepared as a release film. The following composition for forming a first protective layer was applied to the matte layer side of the release film by gravure coating to form an uncured resin layer. The composition was then cured by irradiating with 50 kGy of electron beams at an acceleration voltage of 165 kV to form a first protective layer with a thickness of 5 μm. The surface of the first protective layer opposite the release film was then subjected to corona irradiation. <Composition for forming first protective layer (EB1)> Ionizing radiation curable resin composition: 100 parts by mass Caprolactone urethane acrylate: 30 parts by mass Pentaerythritol triacrylate (hydroxyl group-containing acrylate): 70 parts by mass Ultraviolet absorber: 2 parts by mass (product name: TINUVIN 479, BASF) Light stabilizer having a reactive functional group: 2 parts by mass (product name: SANOL LS-3410, Nippon Nyukazai Co., Ltd.)
[0113] Next, the following composition for forming a second protective layer was applied by gravure coating to the corona-irradiated surface of the first protective layer and dried to form a second protective layer with a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by mass Ultraviolet absorber: 17 parts by mass (product name: TINUVIN 400, BASF) Ultraviolet absorber: 13 parts by mass (product name: TINUVIN 479, BASF) Hindered amine-based light stabilizer: 8 parts by mass (product name: TINUVIN 123, BASF) Antiblocking agent: 9 parts by mass (silica particles, average particle size 3 μm) Curing agent: 25 parts by mass (hexamethylene diisocyanate)
[0114] Next, the following ink for forming the design layer was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in this order in the thickness direction. <Ink for forming the design layer> Resin composition: 100 parts by mass Acrylic resin: 80 parts by mass Vinyl chloride-vinyl acetate copolymer: 20 parts by mass Pigment
[0115] Example 4 A polyethylene terephthalate film (kneaded matte, thickness: 50 μm) that had not been subjected to an easy-adhesion treatment and had a matting agent kneaded into it was prepared as a release film. The following composition for forming a first protective layer was applied to one side of the release film by gravure coating to form an uncured resin layer. The composition was then cured by irradiating with 50 kGy of electron beams at an acceleration voltage of 165 kV to form a 5 μm-thick first protective layer. Corona irradiation was then performed on the side of the first protective layer opposite the release film. <Composition for Forming First Protective Layer (EB3)> Ionizing radiation curable resin composition (caprolactone-based urethane acrylate): 100 parts by mass Ultraviolet absorber: 2 parts by mass (product name: TINUVIN 479, BASF) Light stabilizer having a reactive functional group: 2 parts by mass (product name: Sanol LS-3410, Nippon Nyukazai Co., Ltd.)
[0116] Next, the following composition for forming a second protective layer was applied by gravure coating to the corona-irradiated surface of the first protective layer and dried to form a second protective layer with a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by mass Ultraviolet absorber: 17 parts by mass (product name: TINUVIN 400, BASF) Ultraviolet absorber: 13 parts by mass (product name: TINUVIN 479, BASF) Hindered amine-based light stabilizer: 8 parts by mass (product name: TINUVIN 123, BASF) Antiblocking agent: 9 parts by mass (silica particles, average particle size 3 μm) Curing agent: 25 parts by mass (hexamethylene diisocyanate)
[0117] Next, the following ink for forming the design layer was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in this order in the thickness direction. <Ink for forming the design layer> Resin composition: 100 parts by mass Acrylic resin: 80 parts by mass Vinyl chloride-vinyl acetate copolymer: 20 parts by mass Pigment
[0118] Example 5 Transfer paper (matte PP, thickness: 75 μm) having a matte polypropylene (PP) layer was prepared as a release film. The following composition for forming a first protective layer was applied by gravure coating to the PP layer side of the release film to form an uncured resin layer. The composition was then cured by irradiating with 50 kGy of electron beams at an acceleration voltage of 165 kV to form a 5 μm-thick first protective layer. Corona irradiation was then performed on the side of the first protective layer opposite the release film. <Composition for Forming First Protective Layer (EB3)> Ionizing radiation curable resin composition (caprolactone-based urethane acrylate): 100 parts by mass Ultraviolet absorber: 2 parts by mass (product name: TINUVIN 479, BASF) Light stabilizer having a reactive functional group: 2 parts by mass (product name: Sanol LS-3410, Nippon Nyukazai Co., Ltd.)
[0119] Next, the following composition for forming a second protective layer was applied by gravure coating to the corona-irradiated surface of the first protective layer and dried to form a second protective layer with a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by mass Ultraviolet absorber: 17 parts by mass (product name: TINUVIN 400, BASF) Ultraviolet absorber: 13 parts by mass (product name: TINUVIN 479, BASF) Hindered amine-based light stabilizer: 8 parts by mass (product name: TINUVIN 123, BASF) Antiblocking agent: 9 parts by mass (silica particles, average particle size 3 μm) Curing agent: 25 parts by mass (hexamethylene diisocyanate)
[0120] Next, the following ink for forming the design layer was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in this order in the thickness direction. <Ink for forming the design layer> Resin composition: 100 parts by mass Acrylic resin: 80 parts by mass Vinyl chloride-vinyl acetate copolymer: 20 parts by mass Pigment
[0121] [Comparative Example 1] A polyethylene terephthalate film (kneaded matte, thickness: 50 μm) that had not been subjected to an easy-adhesion treatment and had a matting agent kneaded into it was prepared as a release film. The composition for forming the first protective layer described below was applied to one side of the release film by gravure coating to form an uncured resin layer. The composition was then cured by irradiating with 50 kGy of electron beams at an acceleration voltage of 165 kV to form a first protective layer with a thickness of 5 μm. Then, corona irradiation was performed on the side of the first protective layer opposite the release film. <Composition for forming first protective layer (EB1)> Ionizing radiation curable resin composition: 100 parts by mass Caprolactone urethane acrylate: 30 parts by mass Pentaerythritol triacrylate (hydroxyl group-containing acrylate): 70 parts by mass Ultraviolet absorber: 2 parts by mass (product name: TINUVIN 479, BASF) Light stabilizer having a reactive functional group: 2 parts by mass (product name: SANOL LS-3410, Nippon Nyukazai Co., Ltd.)
[0122] Next, the following composition for forming a second protective layer was applied by gravure coating to the corona-irradiated surface of the first protective layer and dried to form a second protective layer with a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by mass Ultraviolet absorber: 17 parts by mass (product name: TINUVIN 400, BASF) Ultraviolet absorber: 13 parts by mass (product name: TINUVIN 479, BASF) Hindered amine-based light stabilizer: 8 parts by mass (product name: TINUVIN 123, BASF) Antiblocking agent: 9 parts by mass (silica particles, average particle size 3 μm) Curing agent: 25 parts by mass (hexamethylene diisocyanate)
[0123] Next, the following ink for forming the design layer was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in this order in the thickness direction. <Ink for forming the design layer> Resin composition: 100 parts by mass Acrylic resin: 80 parts by mass Vinyl chloride-vinyl acetate copolymer: 20 parts by mass Pigment
[0124] Comparative Example 2: A mirror-finished polyethylene terephthalate film (thickness: 50 μm) that had not been subjected to an easy-adhesion treatment was prepared as a release film. The composition for forming the first protective layer described below was applied to one side of the release film by gravure coating to form an uncured resin layer. The composition was then cured by irradiating with 50 kGy of electron beams at an acceleration voltage of 165 kV to form a first protective layer with a thickness of 5 μm. The surface of the first protective layer opposite the release film was then subjected to corona irradiation. <Composition for forming first protective layer (EB1)> Ionizing radiation curable resin composition: 100 parts by mass Caprolactone urethane acrylate: 30 parts by mass Pentaerythritol triacrylate (hydroxyl group-containing acrylate): 70 parts by mass Ultraviolet absorber: 2 parts by mass (product name: TINUVIN 479, BASF) Light stabilizer having a reactive functional group: 2 parts by mass (product name: SANOL LS-3410, Nippon Nyukazai Co., Ltd.)
[0125] Next, the following composition for forming a second protective layer was applied by gravure coating to the corona-irradiated surface of the first protective layer and dried to form a second protective layer with a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by mass Ultraviolet absorber: 17 parts by mass (product name: TINUVIN 400, BASF) Ultraviolet absorber: 13 parts by mass (product name: TINUVIN 479, BASF) Hindered amine-based light stabilizer: 8 parts by mass (product name: TINUVIN 123, BASF) Antiblocking agent: 9 parts by mass (silica particles, average particle size 3 μm) Curing agent: 25 parts by mass (hexamethylene diisocyanate)
[0126] Next, the following ink for forming the design layer was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in this order in the thickness direction. <Ink for forming the design layer> Resin composition: 100 parts by mass Acrylic resin: 80 parts by mass Vinyl chloride-vinyl acetate copolymer: 20 parts by mass Pigment
[0127] Comparative Example 3 A mirror-finished polyethylene terephthalate film (thickness: 75 μm) that had not been subjected to an easy-adhesion treatment was prepared as a release film. The following composition for forming a first protective layer was applied to one side of the release film by gravure coating to form an uncured resin layer. The composition was then cured by irradiating with 50 kGy of electron beams at an acceleration voltage of 165 kV to form a 5 μm-thick first protective layer. Corona irradiation was then performed on the side of the first protective layer opposite the release film. <Composition for Forming First Protective Layer (EB3)> Ionizing radiation-curable resin composition (caprolactone-based urethane acrylate): 100 parts by mass Ultraviolet absorber: 2 parts by mass (product name: TINUVIN 479, BASF) Light stabilizer having a reactive functional group: 2 parts by mass (product name: Sanol LS-3410, Nippon Nyukazai Co., Ltd.)
[0128] Next, the following composition for forming a second protective layer was applied by gravure coating to the corona-irradiated surface of the first protective layer and dried to form a second protective layer with a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by mass Ultraviolet absorber: 17 parts by mass (product name: TINUVIN 400, BASF) Ultraviolet absorber: 13 parts by mass (product name: TINUVIN 479, BASF) Hindered amine-based light stabilizer: 8 parts by mass (product name: TINUVIN 123, BASF) Antiblocking agent: 9 parts by mass (silica particles, average particle size 3 μm) Curing agent: 25 parts by mass (hexamethylene diisocyanate)
[0129] Next, the following ink for forming the design layer was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in this order in the thickness direction. <Ink for forming the design layer> Resin composition: 100 parts by mass Acrylic resin: 80 parts by mass Vinyl chloride-vinyl acetate copolymer: 20 parts by mass Pigment
[0130] [Comparative Example 4] A polyethylene terephthalate film (matte coat, thickness: 38 μm) having a matte layer containing a matting agent was prepared as a release film. The following composition for forming a first protective layer was applied to one side of the release film by gravure coating to form an uncured resin layer. The composition was then cured by irradiating with 50 kGy of electron beams at an acceleration voltage of 165 kV to form a first protective layer with a thickness of 5 μm. The surface of the first protective layer opposite the release film was then subjected to corona irradiation. <Composition for forming first protective layer (EB1)> Ionizing radiation curable resin composition: 100 parts by mass Caprolactone urethane acrylate: 30 parts by mass Pentaerythritol triacrylate (hydroxyl group-containing acrylate): 70 parts by mass Ultraviolet absorber: 2 parts by mass (product name: TINUVIN 479, BASF) Light stabilizer having a reactive functional group: 2 parts by mass (product name: SANOL LS-3410, Nippon Nyukazai Co., Ltd.)
[0131] Next, the following composition for forming a second protective layer was applied by gravure coating to the corona-irradiated surface of the first protective layer and dried to form a second protective layer with a thickness of 3.5 μm. <Composition for forming second protective layer> Polycarbonate-based urethane acrylic copolymer: 100 parts by mass Ultraviolet absorber: 17 parts by mass (product name: TINUVIN 400, BASF) Ultraviolet absorber: 13 parts by mass (product name: TINUVIN 479, BASF) Hindered amine-based light stabilizer: 8 parts by mass (product name: TINUVIN 123, BASF) Antiblocking agent: 9 parts by mass (silica particles, average particle size 3 μm) Curing agent: 25 parts by mass (hexamethylene diisocyanate)
[0132] Next, the following ink for forming the design layer was applied to the surface of the obtained second protective layer by gravure coating and dried to form the design layer. This resulted in a transfer sheet having a release film, a first protective layer, a second protective layer, and a design layer in this order in the thickness direction. <Ink for forming the design layer> Resin composition: 100 parts by mass Acrylic resin: 80 parts by mass Vinyl chloride-vinyl acetate copolymer: 20 parts by mass Pigment
[0133] [Evaluation] (Measurement of Loop Stiffness) The loop stiffness of the release film in the transfer sheet obtained in each Example and Comparative Example was measured. First, the transfer layer was peeled off from the transfer sheet, leaving only the release film. Next, the release film was cut into a strip shape with a width of 15 mm and a length of 150 mm to prepare a sample. Next, the sample was fixed to a "Loop Stiffness Tester (Model: DR)" manufactured by Toyo Seiki so that the loop length was 60 mm, and a pressure jig was pressed against it from the vertical direction to measure the stress during compression, and the maximum value of the stress was determined as the loop stiffness (RS).
[0134] (Peel Strength Measurement) The peel strength of the transfer sheet obtained in each Example and Comparative Example was measured. First, the transfer sheet was cut to a width of 25 mm, and double-sided tape was attached to the entire surface of the release film opposite the transfer layer, and the release film was fixed to a 25 mm wide metal plate. Next, a 25 mm wide piece of Nichiban Cellotape (registered trademark) was attached to the entire surface of the transfer layer opposite the release film. Next, using a Tensilon RTG1250 manufactured by A&D Co., Ltd., the peel strength was measured under the conditions of a peel rate of 200 mm / min and a peel angle of 90°. After exceeding the upper yield point, the integrated average value of the peel strength from the point where the lower yield point load was reached to 20 mm was taken, and the peel strength (N / 25 mm) was calculated. The results are shown in Table 1.
[0135] (Corner Lifting, Springback, and Release Film Peelability) The transfer sheets obtained in each Example and Comparative Example were evaluated for corner lifting (lifting of the transfer sheet at the corners), springback (partial peeling of the release film due to springback), and release film peelability (peelability of the release film after the transfer sheet is attached to the adherend). First, an aluminum substrate (adherend) having a cross section of 40 mm x 40 mm and a length of 2 m was prepared. Next, an adhesive (YR117-1 manufactured by Showa Denko Material, thickness 50 μm) was applied to the transfer layer of the transfer sheet, and the transfer sheet was attached to the aluminum substrate using a wrapping machine. Next, corner lifting, springback, and release film peelability were evaluated according to the following criteria. <Corner Lifting> A: The transfer sheet completely adhered to the corners. B: The transfer sheet slightly lifted from the corners, but this was at a level that did not cause any problems in use. C: The transfer sheet significantly lifted from the corners. <Springback> A: The release film did not lift from the transfer layer and adhered to it. B: The release film was slightly lifted from the edge of the transfer sheet, but this was at a level that did not cause any problems in use. C: The release film peeled off significantly from the edge of the transfer sheet. <Release film releasability> A: The release film was easily peeled off. B: Some force was required during peeling, but the release film was peeled off without remaining on the transfer layer. C: The release film could not be peeled off from the transfer layer, and the release film was damaged.
[0136]
[0137]
[0138] As shown in Tables 1 and 2, in Examples 1 to 5, corner lift, spring back, and release film releasability were all good. In contrast, in Comparative Examples 1 to 4, any of corner lift, spring back, and release film releasability was insufficient. The relationship between loop stiffness and peel strength in Examples 1 to 5 and Comparative Examples 1 to 3 is shown in Figure 7. Note that the peel strength of Comparative Example 4 is too high, so it is not shown in Figure 7.
[0139] As shown in FIG. 7 , it was confirmed that springback can be effectively suppressed when Y≧0.67X+0.17 is satisfied, where X is loop stiffness and Y is peel strength. Comparative Example 3 successfully suppressed springback, and the line connecting Comparative Example 3 and Example 1 was Y=0.67X+0.19 (line 1). Meanwhile, the line with a slope of 0.67 and passing through Comparative Example 1 was Y=0.67X+0.14 (line 2). It is estimated that springback can be effectively suppressed within the range of Y≧0.67X+0.17, with Y=0.67X+0.17, located midway between lines 1 and 2, as the boundary. Furthermore, the line connecting Example 1 and Example 5 was Y=2.25X+0.12. Furthermore, the line connecting Example 1 and Example 4 was Y=2.99X+0.03. Furthermore, as shown in FIG. 7, it was suggested that when the loop stiffness X exceeds 0.18 N / 15 mm, corner lifting is likely to occur, and when the peel strength Y exceeds 0.7 N / 25 mm, the releasability decreases.
[0140] Thus, the present disclosure provides, for example, the following inventions.
[0141] [1] A transfer sheet, comprising a release film and a transfer layer disposed on one side of the release film, wherein the loop stiffness of the release film is 0.18 N / 15 mm or less, and the peel strength of the release film and the transfer layer is 0.7 N / 25 mm or less, and where the loop stiffness is X and the peel strength is Y, X and Y satisfy Y≧0.67X+0.17.
[0142] [2] The transfer sheet according to [1], which is used for wrapping processing.
[0143] [3] The transfer sheet according to [1] or [2], wherein the transfer layer has a first protective layer and a second protective layer in this order in the thickness direction from the release film side.
[0144] [4] The transfer sheet according to [3], wherein the first protective layer contains a cured product of an ionizing radiation curable resin composition.
[0145] [5] The transfer sheet according to [3] or [4], wherein the second protective layer contains a cured product of a thermosetting resin composition.
[0146] [6] The transfer sheet according to any one of [3] to [5], wherein the first protective layer contains at least one of an ultraviolet absorber and a light stabilizer.
[0147] [7] The transfer sheet according to any one of [3] to [6], wherein the second protective layer contains at least one of an ultraviolet absorber and a light stabilizer.
[0148] [8] The transfer sheet according to any one of [3] to [7], wherein the transfer layer has a design layer on the surface of the second protective layer opposite to the first protective layer.
[0149] [9] The transfer sheet according to any one of [1] to [8], which is used in the manufacture of exterior products.
[0150]
[10] A method for manufacturing an article, comprising: a preparation step of preparing an adherend having a plurality of surfaces and a transfer sheet according to any one of [1] to [9]; and a wrapping step of sequentially laminating the transfer layer of the transfer sheet to the plurality of surfaces of the adherend using a roller.
[0151]
[11] The method for manufacturing an article according to
[10] , further comprising, after the preparation step and before the wrapping step, an adhesive layer forming step of forming an adhesive layer on the surface of the transfer layer opposite to the release film, or on the plurality of surfaces of the adherend.
[0152]
[12] An article with a release film, comprising: an adherend having a plurality of surfaces; a transfer layer disposed so as to follow the plurality of surfaces; and a release film disposed so as to follow the transfer layer, wherein the loop stiffness of the release film is 0.18 N / 15 mm or less; the peel strength of the release film and the transfer layer is 0.7 N / 25 mm or less; and, when the loop stiffness is X and the peel strength is Y, X and Y satisfy Y≧0.67X+0.17.
[0153]
[13] The article with a release film according to
[12] , wherein the article with a release film has an adhesive layer between the transfer layer and the adherend.
[0154] REFERENCE SIGNS LIST 1 release film 2 first protective layer 3 second protective layer 4 design layer 10 transfer sheet 20 adherend 50 article with release film 100 article
Claims
1. A transfer sheet comprising a release film and a transfer layer disposed on one side of the release film, wherein the loop stiffness of the release film is 0.18 N / 15 mm or less, and the peel strength of the release film and the transfer layer is 0.7 N / 25 mm or less, and wherein, when the loop stiffness is X and the peel strength is Y, the relationship Y≧0.67X+0.17 is satisfied.
2. The transfer sheet according to claim 1, which is used in wrapping processing.
3. The transfer sheet according to claim 1, wherein the transfer layer has a first protective layer and a second protective layer in this order in the thickness direction from the release film side.
4. The transfer sheet according to claim 3, wherein the first protective layer comprises a cured product of an ionizing radiation curable resin composition.
5. The transfer sheet according to claim 3, wherein the second protective layer comprises a cured product of a thermosetting resin composition.
6. The transfer sheet according to claim 3, wherein the first protective layer contains at least one of an ultraviolet absorbing agent and a light stabilizer.
7. The transfer sheet according to claim 3, wherein the second protective layer contains at least one of an ultraviolet absorbing agent and a light stabilizer.
8. The transfer sheet according to claim 3, wherein the transfer layer has a design layer on the side of the second protective layer opposite the first protective layer.
9. The transfer sheet of claim 1, wherein the transfer sheet is used in the manufacture of exterior products.
10. A method for manufacturing an article, comprising: a preparation step of preparing an adherend having multiple surfaces and a transfer sheet described in any one of claims 1 to 9; and a wrapping step of sequentially bonding the transfer layer of the transfer sheet to the multiple surfaces of the adherend using a roller.
11. The method for manufacturing an article described in claim 10, further comprising, after the preparation step and before the wrapping step, an adhesive layer formation step of forming an adhesive layer on the side of the transfer layer opposite the release film, or on the multiple sides of the adherend.
12. An article with a release film, comprising: an adherend having a plurality of surfaces; a transfer layer disposed so as to follow said plurality of surfaces; and a release film disposed so as to follow said transfer layer, wherein the loop stiffness of said release film is 0.18 N / 15 mm or less; the peel strength of said release film and said transfer layer is 0.7 N / 25 mm or less; and, when said loop stiffness is X and said peel strength is Y, said X and said Y satisfy Y≧0.67X+0.
17.
13. The article with a release film according to claim 12, wherein the article with a release film has an adhesive layer between the transfer layer and the adherend.
Citation Information
Patent Citations
Decorative sheet
JP2012040815A
Three-dimensional molding film and resin molding
JP2019064027A
Transfer sheet
JP2019081335A
Laminate and resin film
JP2019181949A
Transfer sheet, decorative molding and method for manufacturing decorative molding
JP2022155130A