Resin composition and molded article
The combination of propylene and polyhydroxyalkanoate polymers in a resin composition addresses the challenges of mold release and tensile strain in recycled material injection molding, enhancing the workability and performance of molded articles by using recycled automobile parts and inorganic fillers.
Patent Information
- Application Number
- PCT/JP2024/011353
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Injection molding of resin compositions containing recycled materials from end-of-life vehicles faces challenges such as difficulty in mold release and low tensile fracture strain due to high dimensional stability and impurities, leading to poor workability.
A resin composition combining a propylene polymer with a polyhydroxyalkanoate polymer, specifically containing 15-70% propylene polymer and 1-30% polyhydroxyalkanoate polymer, which facilitates easy mold extraction and achieves a sufficiently large tensile strain at break, utilizing recycled materials from automobile parts and incorporating fillers like inorganic fillers for improved properties.
The resin composition allows for easy extraction of molded products from the mold and enhances the tensile strain at break, improving the workability and performance of molded articles made from recycled materials.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Resin composition and molded article
[0001] The present invention relates to a resin composition and a molded article.
[0002] In order to reduce the burden on the environment, studies have been conducted on recovering and crushing resin parts such as bumpers from used automobiles and reusing them as synthetic resin materials. For example, Patent Document 1 discloses a resin composition for automobile interiors, which is obtained by mixing crushed car bumper material (A) containing 0.1 to 10% by weight of insoluble matter, crystalline polypropylene (B), elastomer (C), inorganic filler (D), and light-shielding pigment (E) in a specific ratio, and then heating and melting the mixture, and which is characterized in that the size of the insoluble matter mixed in the resin composition is such that it can pass through a 20-mesh screen.
[0003] Japanese Patent Application Laid-Open No. 2005-139421
[0004] When a resin composition containing recycled materials from end-of-life automobiles is injection molded, the molded product can be difficult to remove from the mold due to its high dimensional stability and resistance to molding shrinkage. Furthermore, even if a molded product obtained from a resin composition containing recycled materials is easy to remove from the mold, the molded product can have a small tensile breaking strain and poor processability due to the high content of foreign matter derived from the impurities contained in the recycled material.
[0005] Therefore, an object of the present invention is to provide a resin composition that, when injection-molded, can easily remove a molded article from a mold and can provide a molded article having a sufficiently large tensile breaking strain, and also to provide a molded article obtained from the resin composition.
[0006] The present invention includes, for example, the following [1] to
[26] . [1] A resin composition containing a recycled material (A) containing a propylene polymer and a polyhydroxyalkanoate polymer (B). [2] The resin composition according to [1], wherein the recycled material (A) is a recycled material derived from automobile parts. [3] The resin composition according to [1] or [2], wherein the recycled material (A) is a recycled material derived from automobile parts. [4] The resin composition according to any one of [1] to [3], wherein the recycled material (A) is a heterophasic propylene polymer material. [5] The resin composition according to [4], wherein the heterophasic propylene polymer material has an isotactic pentad fraction of 0.961 or more. [6] The resin composition according to any one of [1] to [5], wherein the recycled material (A) is an ethylene-α-olefin copolymer. [7] The resin composition according to any one of [1] to [6], wherein the recycled material (A) is an ethylene-α-olefin copolymer. [8] The resin composition according to any one of [1] to [7], wherein the recycled material (A) is an ethylene-α-olefin copolymer. [9] The resin composition according to [8], wherein the filler is an inorganic filler.
[10] The resin composition according to claim 1, wherein the recycled material (A) contains a filler.
[11] The resin composition according to any one of [1] to
[10] , further comprising a propylene polymer, wherein the content of the recycled material (A) is 15 to 70 mass% based on the total amount of the resin composition, the content of the polyhydroxyalkanoate polymer (B) is 1 to 30 mass% based on the total amount of the resin composition, and the content of the propylene polymer is 25 to 85 mass% based on the total amount of the resin composition.
[12] A molded article comprising the resin composition according to any one of [1] to
[11] .
[13] A resin composition comprising a recycled material (A) containing a propylene polymer and a polyhydroxyalkanoate polymer (B), wherein the content of xylene soluble components (CXS components) in the recycled material (A) is 1 mass% or more and 60 mass% or less.
[14] A resin composition comprising a recycled material (A) containing a propylene polymer and a polyhydroxyalkanoate polymer (B), wherein the recycled material (A) contains ash, and the ash content is 1 mass% or more and 50 mass% or less, relative to 100 mass% of the total mass of the recycled material (A).
[15] The resin composition according to
[13] or
[14] , which contains a heterophasic propylene polymer material.
[16] A resin composition comprising a recycled material (A) containing a propylene polymer, a polyhydroxyalkanoate polymer (B), and a virgin propylene polymer, wherein the virgin propylene polymer contains a heterophasic propylene polymer material.
[17] The resin composition according to
[15] or
[16] , wherein the heterophasic propylene polymer material has an isotactic pentad fraction of 0.961 or more.
[18] The resin composition according to any one of
[13] to
[17] , wherein the recycled material (A) is a recycled material derived from automobile parts.
[19] The resin composition according to any one of
[13] to
[18] , which contains a propylene homopolymer.
[20] The resin composition according to any one of
[13] to
[19] , which contains an ethylene-α-olefin copolymer.
[21] The resin composition according to any one of
[13] to
[20] , wherein the recycled material (A) comprises an ethylene-α-olefin copolymer.
[22] The resin composition according to any one of
[13] to
[21] , wherein the recycled material (A) comprises a filler.
[23] The resin composition according to
[22] , wherein the filler is an inorganic filler.
[24] The resin composition according to any one of
[13] to
[23] , wherein the recycled material (A) comprises a filler.
[25] The resin composition according to any one of
[13] to
[24] , further comprising a propylene polymer, wherein the content of the recycled material (A) is 15 to 70 mass% based on the total amount of the resin composition, the content of the polyhydroxyalkanoate polymer (B) is 1 to 30 mass% based on the total amount of the resin composition, and the content of the propylene polymer is 25 to 85 mass% based on the total amount of the resin composition.
[26] A molded article comprising the resin composition according to any one of
[13] to
[26] .
[0007] According to the present invention, it is possible to provide a resin composition that, when injection-molded, can easily remove a molded article from a mold and can obtain a molded article having a sufficiently large tensile breaking strain. Furthermore, according to the present invention, it is possible to provide a molded article obtained from the resin composition.
[0008] Hereinafter, several embodiments of the present invention will be described in detail, but the present invention is not limited to the following embodiments.
[0009] (Resin Composition) A resin composition according to one embodiment of the present invention contains a recycled material (A) containing a propylene polymer and a polyhydroxyalkanoate polymer (B).
[0010] The resin composition contains the polyhydroxyalkanoate polymer (B) together with the recycled material (A) containing a propylene polymer, and thus the molded article can be easily removed from the mold when the resin composition containing the recycled material is injection molded. Furthermore, the molded article has a superior tensile strain at break compared to a resin composition containing a virgin propylene polymer and a polyhydroxyalkanoate polymer.
[0011] <Recycled Material (A)> The resin composition contains a recycled material. The recycled material refers to a material that is recovered and reused after being processed, such as molded, or after being used for some final application. Examples of raw materials for the recycled material include automobile interior parts (instrument panels, door trims, etc.), automobile exterior parts (bumpers, etc.), other automobile parts (battery cases, etc.), packaging containers (retort pouches for food, refill pouches, detergent bottles, etc.), housings for household electrical appliances, office supplies (trays, etc.), and household commodities (contact lens cases, etc.). The recycled material may be a recycled material derived from automobile parts.
[0012] The recycled material may contain a propylene polymer (i.e., a recycled propylene polymer). The propylene polymer contained in the recycled material may be a propylene homopolymer or a heterophasic propylene polymer material. Propylene polymers, propylene homopolymers, and heterophasic propylene polymer materials will be described later.
[0013] The raw materials of the recycled material may contain components other than the propylene polymer. The recycled material may contain additives such as a resin component such as an ethylene-α-olefin copolymer, a filler such as an inorganic filler, a neutralizing agent, an antioxidant, an ultraviolet absorber, a nucleating agent, a lubricant, an antistatic agent, an antiblocking agent, a colorant (inorganic pigment, organic pigment, pigment dispersant, etc.), and a flame retardant.
[0014] The recycled material may be obtained by a method including, in addition to a recovery process for recovering raw materials, a crushing process, a refining process, a melting process, a kneading process with other substances, a molding process into pellets, etc. Examples of refining processes include washing with water, aqueous and / or oil-based chemicals, microbial treatment, magnetic separation, and gravity separation.
[0015] The melt mass flow rate (MFR) of the recycled material measured in accordance with JIS K7210-2014 under conditions of a temperature of 230°C and a load of 2.16 kgf is preferably 1 g / 10 min or more and 200 g / 10 min or less, from the viewpoint of making it easier to remove the molded article from the mold and making it easier to increase the tensile break strain of the resulting molded article. The MFR of the recycled material may be 180 g / 10 min or less, 160 g / 10 min or less, 140 g / 10 min or less, 120 g / 10 min or less, 100 g / 10 min or less, 80 g / 10 min or less, 60 g / 10 min or less, or 50 g / 10 min or less, from the viewpoint of making it easier to remove the molded article from the mold and making it easier to increase the tensile break strain of the resulting molded article. The MFR of the recycled material may be 5 g / 10 min or more, 10 g / 10 min or more, 20 g / 10 min or more, or 30 g / 10 min or more, and may be 40 g / 10 min or less, 30 g / 10 min or less, 20 g / 10 min or less, or 10 g / 10 min or less.
[0016] <Polyhydroxyalkanoate polymer (B)> The resin composition contains a polyhydroxyalkanoate polymer. The polyhydroxyalkanoate polymer is a polyester of a hydroxyalkanoic acid. Examples of the hydroxyalkanoic acid include 2-hydroxyalkanoic acid, 3-hydroxyalkanoic acid, and 4-hydroxyalkanoic acid.
[0017] Examples of 2-hydroxyalkanoic acids include glycolic acid, lactic acid, and 2-hydroxybutyric acid. Examples of polyesters of 2-hydroxyalkanoic acids, that is, poly(2-hydroxyalkanoate) polymers, include polyglycolic acid and polylactic acid.
[0018] Examples of 3-hydroxyalkanoic acids are 3-hydroxybutyric acid, 3-hydroxypropionic acid, 3-hydroxypentanoic acid, and 3-hydroxyhexanoic acid. Polyesters of 3-hydroxyalkanoic acids, i.e., poly(3-hydroxyalkanoate) polymers, will be described later.
[0019] Examples of 4-hydroxyalkanoic acids are 4-hydroxybutyric acid, 4-hydroxypentanoic acid, and 4-hydroxyhexanoic acid.
[0020] The polyhydroxyalkanoate polymer may be a homopolymer of a hydroxyalkanoic acid, or a polymer of two or more kinds of hydroxyalkanoic acids.
[0021] The poly(3-hydroxyalkanoate) polymer is a polyhydroxyalkanoate (i.e., a polyester of hydroxyalkanoic acid) and contains a 3-hydroxyalkanoate repeating unit represented by the following formula (1): [—O—CHR—CH 2 -CO-]... (1)
[0022] In formula (1), R represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 15 carbon atoms, a cyano group, an amino group having 1 to 18 carbon atoms, an alkoxy group (alkyloxy group) having 1 to 11 carbon atoms, an amide group having 1 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, or a monovalent heterocyclic group having 1 to 9 carbon atoms. These groups may have a substituent. From the viewpoint of compatibility with components other than the polyhydroxyalkanoate polymer (B), R may be an alkyl group having 1 to 8 carbon atoms, an amide group having 1 to 20 carbon atoms, or an aryl group having 6 to 8 carbon atoms.
[0023] Examples of halogen atoms are F, Cl, Br, and I.
[0024] The alkyl group having 1 to 15 carbon atoms may be linear or branched. The number of carbon atoms in the alkyl group may be 1 to 8 or 1 to 4. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a 2-methylbutyl group, a 1-methylbutyl group, a hexyl group, an isohexyl group, a 3-methylpentyl group, a 2-methylpentyl group, a 1-methylpentyl group, a heptyl group, an octyl group, an isooctyl group, a 2-ethylhexyl group, a 3,7-dimethyloctyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tetradecyl group, and a pentadecyl group.
[0025] Examples of the amino group having 1 to 18 or 1 to 11 carbon atoms include an amino group, an alkylamino group, a dialkylamino group, an arylamino group, an alkylarylamino group, a benzylamino group, and a dibenzylamino group.
[0026] Examples of the alkylamino group include a methylamino group, an ethylamino group, a propylamino group, a butylamino group, a pentylamino group, a hexylamino group, a heptylamino group, an octylamino group, a nonylamino group, a decylamino group, a dodecylamino group, an isopropylamino group, an isopentylamino group, a sec-butylamino group, a tert-butylamino group, a sec-pentylamino group, a tert-pentylamino group, a tert-octylamino group, a neopentylamino group, a cyclopropylamino group, a cyclobutylamino group, a cyclopentylamino group, a cyclohexylamino group, a cycloheptylamino group, a cyclooctylamino group, a 1-adamantamino group, and a 2-adamantamino group.
[0027] Examples of the dialkylamino group include a dimethylamino group, a diethylamino group, a dipropylamino group, a dibutylamino group, a dipentylamino group, a diisopropylamino group, a diisobutylamino group, a diisopentylamino group, a methylethylamino group, a methylpropylamino group, a methylbutylamino group, a methylisobutylamino group, a dicyclopropylamino group, a pyrrolidino group, a piperidino group, and a piperazino group.
[0028] Examples of the arylamino group include an anilino group, a 1-naphthylamino group, a 2-naphthylamino group, an o-toluidino group, an m-toluidino group, a p-toluidino group, a 1-fluoreneamino group, a 2-fluoreneamino group, a 2-thiazoleamino group, and a p-terphenylamino group.
[0029] Examples of the alkylarylamino group include an N-methylanilino group, an N-ethylanilino group, an N-propylanilino group, an N-butylanilino group, an N-isopropylanilino group, and an N-pentylanilino group.
[0030] Examples of the alkoxy group having 1 to 11 carbon atoms include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, a cyclopropoxy group, a cyclobutoxy group, and a cyclopentoxy group.
[0031] The term "amide group" refers to a group in which one hydrogen atom bonded to a nitrogen atom has been removed from a carboxylic acid amide. Examples of the amide group having 1 to 20 carbon atoms include -NH-C(=O)-R groups such as formamide, acetamide, propionamide, butylamide, benzamide, trifluoroacetamide, and pentafluorobenzamide. A (wherein R A represents a hydrogen atom or a monovalent organic group); -N(-C(=O)-R such as a diformamide group, a diacetamide group, a dipropionamide group, a dibutyroamide group, a dibenzamide group, a ditrifluoroacetamide group, or a dipentafluorobenzamide group; A )(-C(=O)-R B ) (wherein R A 、 R B are each independently a hydrogen atom or a monovalent organic group. The organic group is an alkyl group, an alkoxy group, an aryl group, or the like, which may be substituted with a halogen atom. The amide group may be a formamide group, an acetamide group, a propionamide group, a butyromide group, or a benzamide group.
[0032] Examples of the aryl group having 6 to 12 carbon atoms are a phenyl group, a tolyl group, a xylyl group, a naphthyl group, and a biphenyl group. The aryl group having 6 to 12 carbon atoms may be a phenyl group, a tolyl group, or a xylyl group.
[0033] Examples of heteroatoms in monovalent heterocyclic groups having 1 to 9 carbon atoms include N, O, and S. They may be saturated or unsaturated and may contain a single heteroatom or multiple heteroatoms of different types. Examples of such heterocyclic groups include thienyl, pyrrolyl, furyl, pyridyl, piperidinyl, quinolinyl, isoquinolinyl, pyrimidinyl, triazinyl, and thiazolyl groups.
[0034] The repeating units of the polyhydroxyalkanoate polymer may consist solely of one or more types of 3-hydroxyalkanoates represented by formula (1), or may consist of one or more types of 3-hydroxyalkanoates represented by formula (1) and one or more types of other hydroxyalkanoates.
[0035] From the viewpoint of making it easier to remove a molded article from a mold and making it easier for the tensile breaking strain of the obtained molded article to become larger, the polyhydroxyalkanoate polymer preferably contains 50 mol % or more, and more preferably 70 mol % or more, of the 3-hydroxyalkanoate repeating units represented by formula (1) relative to the total repeating units of the hydroxyalkanoate (100 mol %).
[0036] Examples of 3-hydroxyalkanoates represented by formula (1) include those in which R is a hydrogen atom or C n H 2n+1 where n is an integer of 1 to 15, examples thereof include 3-hydroxybutyrate (hereinafter, sometimes referred to as 3HB) where n=1, 3-hydroxyvalerate (hereinafter, sometimes referred to as 3HV) where n=2, 3-hydroxyhexanoate (hereinafter, sometimes referred to as 3HH) where n=3, 3-hydroxyoctanate (hereinafter, sometimes referred to as 3HH) where n=5, 3-hydroxyoctadecanate (hereinafter, sometimes referred to as 15), and 3-hydroxypropionate where R is a hydrogen atom.
[0037] An example of a polyhydroxyalkanoate polymer having only one type of repeating unit represented by formula (1) is poly(3-hydroxybutyrate) (hereinafter, sometimes referred to as P3HB).
[0038] Examples of polyhydroxyalkanoate polymers containing only multiple types of repeating units represented by formula (1) include poly(3-hydroxybutyrate-co-3-hydroxyhexanoate; hereinafter, sometimes referred to as P3HB3HH), poly(3-hydroxybutyrate-co-3-hydroxyvalerate; hereinafter, sometimes referred to as P3HB3HV), and poly(3-hydroxybutyrate-co-3-hydroxypropionate; hereinafter, sometimes referred to as P3HB3HP).
[0039] An example of a hydroxyalkanoate other than the 3-hydroxyalkanoate represented by formula (1) is one containing a repeating unit represented by formula (2): [—O—CHR 1 -C m H 2m+1 -CO-]... (2)
[0040] In formula (2), R 1 is a hydrogen atom or C n H 2n+1 In the alkyl group represented by the formula: n is an integer of 1 or more and 15 or less, and m is an integer of 2 to 10.
[0041] An example of a polyhydroxyalkanoate polymer containing repeating units of formula (1) and formula (2) is poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (for example, the following formula (P3HB4HB)).
[0042] From the viewpoint of increasing the melting point, it is preferred that the repeating unit of the polyhydroxyalkanoate polymer contains at least 3-hydroxybutyrate among the 3-hydroxyalkanoates represented by formula (1).
[0043] From the viewpoint of making it easier to remove a molded article from a mold and making it easier for the tensile breaking strain of the obtained molded article to become larger, the polyhydroxyalkanoate polymer preferably contains 50 mol % or more, and more preferably 70 mol % or more, of 3-hydroxybutyrate repeating units relative to the total repeating units of hydroxyalkanoate (100 mol %).
[0044] The polyhydroxyalkanoate polymer may have two or more types of ester repeating units, and may be, for example, a di-copolymer having two types of repeating units, a tri-copolymer having three types of repeating units, or a tetra-copolymer having four types of repeating units, as described above.
[0045] For example, an example of a tri-copolymer is poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate) (hereinafter, sometimes referred to as (P3HB3HV3HH)).
[0046] As described above, from the viewpoint of making it easier to remove a molded article from a mold and increasing the tensile breaking strain of the resulting molded article, the polyhydroxyalkanoate polymer preferably contains 3-hydroxybutyrate among the 3-hydroxyalkanoate repeating units represented by formula (1). The proportion XX of 3-hydroxybutyrate repeating units relative to 100 moles of all hydroxyalkanoate ester repeating units is preferably 90 mol% or more, more preferably 95 mol% or more, and even more preferably 98 mol% or more. The proportion XX is typically 100 mol% or less, and may be 99.9 mol% or less, or 99.8 mol% or less.
[0047] The arrangement of the copolymer may be any of a random copolymer, an alternating copolymer, a block copolymer, a graft copolymer, and the like.
[0048] The polyhydroxyalkanoate polymer may have ester repeating units other than those represented by formula (1) and formula (2), but the main chain of the other ester repeating units does not contain an aromatic hydrocarbon structure. That is, the polyhydroxyalkanoate polymer is an aliphatic polyester. However, a group having an aromatic hydrocarbon group may be bonded to a carbon atom in the main chain of the other ester repeating units.
[0049] The composition ratio of the repeating units in the polyhydroxyalkanoate polymer is, as described in L. Tripathi, M. C. Factories, 11, 44 (2012), 1 H-NMR and 13 It can be determined by calculation from the results of NMR measurements such as C-NMR.
[0050] The polyhydroxyalkanoate polymer may also be a blend of two or more types of polyhydroxyalkanoate polymers.
[0051] The weight-average molecular weight (Mw) of the polyhydroxyalkanoate polymer may be 10,000 to 1,000,000, preferably 20,000 to 800,000, and more preferably 30,000 to 600,000, from the viewpoint of making it easier to remove the molded article from the mold and increasing the tensile breaking strain of the resulting molded article. By setting the weight-average molecular weight to 10,000 or more, a molded article with excellent impact strength and tensile elongation can be obtained. By setting the weight-average molecular weight to 500,000 or less, the dispersibility of the polyhydroxyalkanoate polymer is excellent. The weight-average molecular weight may be 400,000 or less, 300,000 or less, 200,000 or less, or 100,000 or less. In this specification, the weight-average molecular weight (Mw) is measured by GPC using standard polystyrene as a molecular weight standard.
[0052] The polyhydroxyalkanoate polymer may be a thermoplastic resin, and is preferably crystalline.
[0053] The melt mass flow rate (MFR) of the polyhydroxyalkanoate polymer, measured in accordance with JIS K7210-2014 under conditions of a temperature of 190°C and a load of 2.16 kgf, is preferably 0.1 g / 10 min or more and 200 g / 10 min or less, from the viewpoint of making it easier to remove the molded article from the mold and making it easier to increase the tensile break strain of the resulting molded article. The MFR of the polyhydroxyalkanoate polymer may be 0.5 g / 10 min or more, 1 g / 10 min or more, 1.5 g / 10 min or more, or 2 g / 10 min or more. The MFR of the polyhydroxyalkanoate polymer may be 150 g / 10 min or less, 100 g / 10 min or less, 70 g / 10 min or less, 50 g / 10 min or less, 30 g / 10 min or less, or 20 g / 10 min or less.
[0054] The melting point (Tm) of the polyhydroxyalkanoate polymer may be 150° C. or higher, 155° C. or higher, 160° C. or higher, 165° C. or higher, 170° C. or higher, or 175° C. or higher. The melting point (Tm) of the polyhydroxyalkanoate polymer may be 220° C. or lower, 200° C. or lower, or 190° C. or lower.
[0055] The melting point (Tm) of the polyhydroxyalkanoate polymer is measured by differential scanning calorimetry (DSC) in accordance with JIS K7121, based on the position of the main peak due to the melting of crystals.
[0056] The polyhydroxyalkanoate polymer may be produced by a microorganism, or may be derived from a compound (such as a cyclic lactone) derived from petroleum or plant materials.
[0057] The polyhydroxyalkanoate polymer may be one in which each repeating unit of hydroxyalkanoate is composed only of the D-form (R-form), as in those produced from microorganisms, or one in which the repeating unit of hydroxyalkanoate contains both the D-form (R-form) and the L-form (S-form), as in those derived from a mixture of the D-form (R-form) and the L-form (S-form).
[0058] In the poly(3-hydroxyalkanoate) polymer produced from a microorganism, the repeating unit of formula (1) can be represented by the following formula: In formula (BI-1), n represents the degree of polymerization.
[0059]
[0060] Poly-(3-hydroxybutyrate) produced from a microorganism has, for example, the following structure: In formula (BI-2), n represents the degree of polymerization.
[0061]
[0062] Poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) produced from a microorganism has, for example, the following structure: In formula (BI-3), m and n represent the degree of polymerization.
[0063]
[0064] Poly-(3-hydroxybutyrate-co-4-hydroxybutyrate) produced from a microorganism has, for example, the following structure: In formula (BI-4), m and n represent the degree of polymerization.
[0065]
[0066] The polyhydroxyalkanoate polymer can be biodegradable.
[0067] Poly(3-hydroxyalkanoate) polymers can be produced by, for example, microorganisms such as Alcaligenes eutrophus AC32 strain (international deposit under the Budapest Treaty, international depositary authority: National Institute of Advanced Industrial Science and Technology International Patent Organism Depositary (6-1 Central, 1-1 Higashi, Tsukuba, Ibaraki Prefecture, Japan), original deposit date: August 12, 1996, transferred on August 7, 1997, accession number FERMBP-6038 (transferred from original deposit FERMP-15786)) (J. Bacteriol., 179, 4821 (1997)), which is obtained by introducing a PHA synthase gene derived from Aeromonas caviae into Alcaligenes eutrophus.
[0068] <Propylene Polymer> The resin composition may contain a propylene polymer. The propylene polymer contained in the resin composition may be a propylene polymer derived from a recycled material (contained in the recycled material), or may contain a propylene polymer not derived from a recycled material (i.e., a virgin propylene polymer). In this specification, the term "virgin propylene polymer" refers to a propylene polymer that, unlike a recycled material, has not been molded into a product such as an automobile or a part thereof after being produced by a process including a polymerization step, and has not been used for any end use.
[0069] A propylene-based polymer is a polymer containing more than 50% by mass of structural units derived from propylene, and examples thereof include a propylene homopolymer, a propylene-ethylene copolymer, a propylene-1-butene copolymer, a propylene-1-hexene copolymer, a propylene-1-octene copolymer, a propylene-ethylene-1-butene copolymer, a propylene-ethylene-1-hexene copolymer, and a propylene-ethylene-1-octene copolymer. The propylene-based polymer may be a combination of two or more propylene-based polymers.
[0070] As described above, the propylene polymer is a polymer containing more than 50% by mass of propylene units when the amount of all structural units contained in the propylene polymer is taken as 100% by mass. The amount of propylene units may be 60% by mass or more, or 70% by mass or more.
[0071] Examples of the propylene-based polymer include a propylene homopolymer and a copolymer of propylene and another monomer copolymerizable with propylene. Such a copolymer may be a random copolymer (hereinafter also referred to as a polypropylene-based random copolymer) or a block copolymer.
[0072] The propylene polymer may contain one kind of propylene polymer alone, or may contain two or more kinds of propylene polymers in any combination and in any ratio.
[0073] Examples of combinations of two or more propylene polymers include combinations of two or more propylene homopolymers having different weight average molecular weights, and combinations of the following polymers (I) and (II).
[0074] The propylene polymer may contain a heterophasic propylene polymer material. The heterophasic propylene polymer material refers to a propylene polymer (composition) containing the following polymer (I) and polymer (II), in which polymer (I) and polymer (II) are not miscible with each other and form different phases. The proportion of the heterophasic propylene polymer in the propylene polymer (A) may be 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass, or 90% by mass. When the resin composition contains recycled material (A) containing a propylene polymer, polyhydroxyalkanoate polymer (B), and virgin heterophasic propylene polymer material, the molded article is more easily removed from the mold and the tensile strain at break of the resulting molded article is more likely to be large.
[0075] The polymer (I) is a propylene-based polymer containing more than 80% by mass and 100% by mass or less of propylene units, where the amount of all structural units is taken as 100% by mass. The polymer (I) may be a propylene homopolymer or a copolymer of propylene and another monomer.
[0076] The polymer (II) is a propylene-based polymer which is a copolymer of a propylene unit and at least one monomer unit selected from the group consisting of an ethylene unit and an α-olefin unit having 4 or more carbon atoms.
[0077] The polymer (I) and the polymer (II) may each be a single polymer or a combination of two or more polymers.
[0078] From the viewpoint of improving the appearance, the resin composition preferably contains a heterophasic propylene polymer material.
[0079] The propylene-based polymer is used from the viewpoint of further improving the rigidity of the molded article of the resin composition. 13The isotactic pentad fraction (also referred to as the [mmmm] fraction) measured by C-NMR may be 0.961 or more, preferably 0.97 or more, and more preferably 0.98 or more.
[0080] The closer the isotactic pentad fraction of a propylene polymer is to 1, the higher the stereoregularity of the molecular structure of the propylene polymer, and the higher the crystallinity of the polypropylene polymer.
[0081] When the propylene polymer is a copolymer, the isotactic pentad fraction can be measured for the chain of propylene units in the copolymer.
[0082] From the viewpoint of improving the molding processability of the resin composition, the propylene-based polymer preferably has a melt flow rate (MFR) of 10 g / 10 min or more, more preferably 15 g / 10 min or more, as measured in accordance with JIS K7210 under conditions of 230°C and a load of 2.16 kgf. The melt flow rate of the polypropylene-based polymer is preferably 250 g / 10 min or less, more preferably 200 g / 10 min or less, from the viewpoint of making it easier to remove the molded article from the mold and of making the tensile break strain of the obtained molded article larger. The melt flow rate of the polypropylene-based polymer is preferably 10 to 200 g / 10 min.
[0083] The propylene polymer can be produced, for example, by a polymerization method using a polymerization catalyst.
[0084] Examples of the polymerization catalyst include Ziegler catalysts, Ziegler-Natta catalysts, catalysts containing an alkylaluminoxane and a compound containing a transition metal element of Group 4 of the periodic table and having a cyclopentadienyl ring, catalysts containing a compound containing a transition metal element of Group 4 of the periodic table and having a cyclopentadienyl ring, a compound that reacts with the compound to form an ionic complex, and an organoaluminum compound, and catalysts in which a catalyst component (e.g., a compound containing a transition metal element of Group 4 of the periodic table and having a cyclopentadienyl ring, a compound that forms an ionic complex, an organoaluminum compound, etc.) is supported on inorganic particles (e.g., silica, clay minerals, etc.) and modified.
[0085] As the polymerization catalyst, a prepolymerization catalyst prepared by prepolymerizing a monomer such as ethylene or an α-olefin in the presence of a catalyst may be used.
[0086] Examples of Ziegler-Natta type catalysts include catalysts that combine a titanium-containing solid transition metal component with an organometallic component.
[0087] Specific examples of the polymerization catalyst include the conventionally known catalysts described in JP-A Nos. 61-218606, 5-194685, 7-216017, 9-316147, 10-212319, and 2004-182981.
[0088] Examples of polymerization methods include bulk polymerization, solution polymerization, and gas-phase polymerization. Here, bulk polymerization refers to a method in which polymerization is carried out using an olefin that is liquid at the polymerization temperature as a medium. Solution polymerization refers to a method in which polymerization is carried out in an inert hydrocarbon solvent such as propane, butane, isobutane, pentane, hexane, heptane, or octane. Gas-phase polymerization refers to a method in which gaseous monomers are used as a medium and the gaseous monomers are polymerized in that medium.
[0089] Examples of the polymerization method (polymerization method) include a batch method, a continuous method, and a combination thereof. The polymerization method may be a multi-stage method in which a plurality of polymerization reactors connected in series are used.
[0090] Various conditions in the polymerization step according to the above polymerization method (polymerization temperature, polymerization pressure, monomer concentration, catalyst input amount, polymerization time, etc.) can be appropriately determined as appropriate depending on the desired propylene-based polymer.
[0091] In producing a propylene polymer, in order to remove impurities such as residual solvent contained in the propylene polymer polymerized by the above polymerization method and oligomers by-produced in the polymerization step, the propylene polymer polymerized by the above polymerization method may be maintained at a temperature at which impurities such as residual solvent and oligomers can volatilize but at which the propylene polymer cannot melt, denature, etc. Examples of such methods for removing impurities include any suitable conventionally known methods described in JP-A-55-75410, JP-A-2565753, etc.
[0092] (Propylene Homopolymer) From the viewpoint of improving the fluidity of the resin composition and the toughness of a molded article of the resin composition, the propylene homopolymer preferably has an intrinsic viscosity [η] of 0.1 to 4 dL / g, more preferably 0.5 to 3 dL / g, and even more preferably 0.7 to 2 dL / g.
[0093] From the viewpoint of improving the fluidity of the resin composition and the toughness of a molded article of the resin composition, the propylene homopolymer preferably has a molecular weight distribution Mw / Mn of 3 or more and less than 7, more preferably 3 to 5. Here, Mw represents the weight average molecular weight, and Mn represents the number average molecular weight. The molecular weight distribution is a value measured by gel permeation chromatography (GPC).
[0094] (Propylene-Based Random Copolymer) Examples of propylene-based random copolymers include a random copolymer containing propylene units and ethylene units (hereinafter referred to as random copolymer (1)), a random copolymer containing propylene units and α-olefin units having 4 or more carbon atoms (hereinafter referred to as random copolymer (2)), and a random copolymer containing propylene units, ethylene units, and α-olefin units having 4 or more carbon atoms (hereinafter referred to as random copolymer (3)).
[0095] The α-olefin having 4 or more carbon atoms that can constitute the propylene-based random copolymer is preferably an α-olefin having 4 to 10 carbon atoms, from the viewpoint of making it easier to remove the molded article from the mold and making it easier for the tensile breaking strain of the obtained molded article to become larger. Examples of α-olefins having 4 to 10 carbon atoms include 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene, and preferably 1-butene, 1-hexene, and 1-octene.
[0096] Examples of the random copolymer (2) include propylene-1-butene random copolymer, propylene-1-hexene random copolymer, propylene-1-octene random copolymer, and propylene-1-decene random copolymer.
[0097] Examples of the random copolymer (3) include propylene-ethylene-1-butene copolymer, propylene-ethylene-1-hexene copolymer, propylene-ethylene-1-octene copolymer, and propylene-ethylene-1-decene copolymer.
[0098] The content of ethylene units in the random copolymer (1) is preferably 0.1 to 40% by mass, more preferably 0.1 to 30% by mass, and even more preferably 2 to 15% by mass, from the viewpoint of making it easier to remove the molded article from the mold and making the tensile breaking strain of the obtained molded article larger.
[0099] The content of the α-olefin unit having 4 or more carbon atoms in the random copolymer (2) is preferably 0.1 to 40% by mass, more preferably 0.1 to 30% by mass, and even more preferably 2 to 15% by mass, from the viewpoint of making it easier to remove the molded article from the mold and making the tensile breaking strain of the obtained molded article larger.
[0100] The total content of ethylene units and α-olefin units having 4 or more carbon atoms in the random copolymer (3) is preferably 0.1 to 40% by mass, more preferably 0.1 to 30% by mass, and even more preferably 2 to 15% by mass, from the viewpoint of making it easier to remove the molded article from the mold and making the tensile breaking strain of the obtained molded article larger.
[0101] The content of propylene units in the random copolymers (1) to (3) is preferably 60 to 99.9% by mass, more preferably 70 to 99.9% by mass, and even more preferably 85 to 98% by mass, from the viewpoint of making it easier to remove the molded article from the mold and making it easier to increase the tensile breaking strain of the obtained molded article.
[0102] (Heterophagic Propylene Polymerization Material) As already explained, the polymer (I) that can be contained in the heterophasic propylene polymerization material is a polymer containing more than 80 mass% and 100 mass% or less of propylene units. The total content of monomer units other than propylene units in the polymer (I) is usually 0 mass% or more and less than 20 mass%, and may be 0 mass% or more.
[0103] Examples of monomers other than propylene that can constitute the polymer (I) include ethylene and α-olefins having 4 or more carbon atoms.
[0104] The α-olefin having 4 or more carbon atoms which can constitute polymer (I) is preferably an α-olefin having 4 to 10 carbon atoms, more preferably 1-butene, 1-hexene, and 1-octene, and even more preferably 1-butene, from the viewpoint of making it easier to remove a molded article from a mold and making it easier for the tensile breaking strain of the obtained molded article to become large.
[0105] Examples of the polymer (I) include propylene homopolymer, propylene-ethylene copolymer, propylene-1-butene copolymer, propylene-1-hexene copolymer, propylene-1-octene copolymer, propylene-ethylene-1-butene copolymer, propylene-ethylene-1-hexene copolymer, and propylene-ethylene-1-octene copolymer.
[0106] Among these, polymer (I) is preferably a propylene homopolymer, a propylene-ethylene copolymer, a propylene-1-butene copolymer, or a propylene-ethylene-1-butene copolymer, from the viewpoint of making it easier to remove the molded article from the mold and making it easier to obtain a molded article with a large tensile breaking strain, and is more preferably a propylene homopolymer from the viewpoint of the rigidity of a molded article containing the resin composition.
[0107] The molecular weight distribution (Mw / Mn) of the polymer (I) measured by GPC is preferably 3 or more and less than 7, more preferably 3 to 5, from the viewpoint that the molded article can be more easily removed from the mold and that the tensile break strain of the obtained molded article tends to be larger.
[0108] As already explained, the polymer (II) is a copolymer of a propylene unit and at least one monomer unit selected from the group consisting of an ethylene unit and an α-olefin unit having 4 or more carbon atoms.
[0109] The total content of ethylene units and α-olefin units having 4 or more carbon atoms in polymer (II) is preferably 20 to 80% by mass, more preferably 20 to 60% by mass, from the viewpoint of making it easier to remove the molded article from the mold and making the tensile breaking strain of the obtained molded article larger.
[0110] The α-olefin having 4 or more carbon atoms that can constitute polymer (II) is preferably an α-olefin having 4 to 10 carbon atoms, from the viewpoint of making it easier to remove the molded article from the mold and making it easier for the tensile breaking strain of the obtained molded article to become large. Examples of α-olefins that can constitute polymer (II) include the same examples as the examples of α-olefins that can constitute polymer (I) already described above.
[0111] Examples of the polymer (II) include a propylene-ethylene copolymer, a propylene-ethylene-1-butene copolymer, a propylene-ethylene-1-hexene copolymer, a propylene-ethylene-1-octene copolymer, a propylene-ethylene-1-decene copolymer, a propylene-1-butene copolymer, a propylene-1-hexene copolymer, a propylene-1-octene copolymer, and a propylene-1-decene copolymer. From the viewpoint of making it easier to remove the molded article from the mold and of making the tensile breaking strain of the obtained molded article larger, preferred are a propylene-ethylene copolymer, a propylene-1-butene copolymer, and a propylene-ethylene-1-butene copolymer, and more preferred is a propylene-ethylene copolymer.
[0112] The content of polymer (II) in the heterophasic propylene polymerization material is preferably 1 to 50% by mass, more preferably 1 to 40% by mass, even more preferably 5 to 30% by mass, and particularly preferably 8 to 15% by mass, when the total of polymer (I) and polymer (II) is taken as 100% by mass, from the viewpoint of making it easier to remove the molded article from the mold and making it easier for the tensile breaking strain of the obtained molded article to become larger.
[0113] Examples of heterophasic propylene polymeric materials include those in which polymer (I) is a propylene homopolymer, a combination of a propylene homopolymer and a (propylene-ethylene) copolymer, a combination of a propylene homopolymer and a (propylene-ethylene-1-butene) copolymer, a combination of a propylene homopolymer and a (propylene-ethylene-1-hexene) copolymer, a combination of a propylene homopolymer and a (propylene-ethylene-1-octene) copolymer, a combination of a propylene homopolymer and a (propylene-1-butene) copolymer, a combination of a propylene homopolymer and a (propylene-1-hexene) copolymer, a combination of a propylene homopolymer and a (propylene-1-octene) copolymer, and a combination of a propylene homopolymer and a (propylene-1-decene) copolymer.
[0114] Other examples of heterophasic propylene polymer materials include those in which polymer (I) is a polymer containing propylene units and monomer units other than propylene units, such as a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene-1-butene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene-1-hexene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene-1-octene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene-1-decene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-1-butene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-1-hexene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-1-octene) copolymer, and a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene) copolymer. a combination of a (propylene-1-butene) copolymer and a (propylene-ethylene) copolymer; a combination of a (propylene-1-butene) copolymer and a (propylene-ethylene-1-butene) copolymer; a combination of a (propylene-1-butene) copolymer and a (propylene-ethylene-1-butene) copolymer; a combination of a (propylene-1-butene) copolymer and a (propylene-ethylene-1-hexene) copolymer; a combination of a (propylene-1-butene) copolymer and a (propylene-ethylene-1-octene) copolymer; a combination of a (propylene-1-butene) copolymer and a (propylene-ethylene-1-decene) copolymer, a combination of a (propylene-1-butene) copolymer and a (propylene-1-butene) copolymer, a combination of a (propylene-1-butene) copolymer and a (propylene-1-hexene) copolymer, a combination of a (propylene-1-butene) copolymer and a (propylene-1-octene) copolymer, a combination of a (propylene-1-butene) copolymer and a (propylene-1-decene) copolymer;Examples of the combination include a combination of a (propylene-1-hexene) copolymer and a (propylene-1-hexene) copolymer, a combination of a (propylene-1-hexene) copolymer and a (propylene-1-octene) copolymer, a combination of a (propylene-1-hexene) copolymer and a (propylene-1-decene) copolymer, a combination of a (propylene-1-octene) copolymer and a (propylene-1-octene) copolymer, a combination of a (propylene-1-octene) copolymer and a (propylene-1-decene) copolymer, etc. In the examples of the above combinations, polymer (I) is described first, and polymer (II) is described later.
[0115] From the viewpoint of making it easier to remove the molded article from the mold and making it easier to obtain a larger tensile breaking strain of the resulting molded article, the heterophasic propylene polymer material that can be contained in the resin composition is preferably a combination of a propylene homopolymer and a (propylene-ethylene) copolymer, a combination of a propylene homopolymer and a (propylene-ethylene-1-butene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene-1-butene) copolymer, or a combination of a (propylene-1-butene) copolymer and a (propylene-1-butene) copolymer, and more preferably a combination of a propylene homopolymer and a (propylene-ethylene) copolymer.
[0116] The heterophasic propylene polymer material can be produced by a production method including a multi-stage polymerization process including a first polymerization process for producing polymer (I) and a second polymerization process for producing polymer (II) in the presence of polymer (I) produced in the first polymerization process. The polymerization of the heterophasic propylene polymer material can be carried out using a catalyst already described as an example of a catalyst that can be used in the production of polypropylene-based polymers.
[0117] The intrinsic viscosity of the polymer (I) (hereinafter referred to as [η] IFrom the viewpoint of making it easier to remove the molded article from the mold and making it easier for the tensile breaking strain of the obtained molded article to become large, the viscosity is preferably 0.1 to 4 dL / g, more preferably 0.5 to 3 dL / g, and even more preferably 0.7 to 2 dL / g.
[0118] The intrinsic viscosity of the polymer (II) (hereinafter referred to as [η] II From the viewpoint of making it easier to remove the molded article from the mold and making it easier for the tensile breaking strain of the obtained molded article to become large, the viscosity is preferably 1 to 10 dL / g, more preferably 2 to 10 dL / g, and even more preferably 5 to 8 dL / g.
[0119] [η] II [η] I Ratio to ([η] II / [η] I ) is preferably 1 to 20, more preferably 2 to 10, and even more preferably 2 to 9, from the viewpoint that the molded article can be more easily removed from the mold and that the tensile breaking strain of the obtained molded article tends to be larger.
[0120] In the case where the polypropylene-based polymer is a heterophasic propylene polymer material composed of polymer (I) and polymer (II) formed by the multi-stage polymerization steps as described above, a portion of the polymer (I) produced in the first polymerization step is extracted from the polymerization vessel in which the first polymerization step was carried out, and the intrinsic viscosity is measured. The intrinsic viscosity of the heterophasic propylene polymer material finally produced in the second polymerization step (hereinafter, referred to as ([η] Total The limiting viscosity of the polymer (II) produced in the second polymerization step is calculated using the limiting viscosity and the content of the polymer (II).
[0121] When a heterophasic propylene polymer material consisting of polymer (I) and polymer (II) is produced by a production method in which polymer (I) is obtained in a first polymerization step and polymer (II) is obtained in a second polymerization step, the content of each of polymer (I) and polymer (II), the intrinsic viscosity ([η] Total , [η] I , [η] IIThe procedure for measuring and calculating ) is as follows.
[0122] The intrinsic viscosity ([η]) of the polymer (I) obtained in the first polymerization step I ), the intrinsic viscosity ([η]) of the final polymer obtained in the second polymerization step (i.e., the heterophasic propylene polymer material consisting of the polymer (I) and the polymer (II)) measured by the method already described. Total ), the content of polymer (II) in the final polymer, the intrinsic viscosity number [η] of polymer (II) II is calculated using the following formula: Formula: [η] II = ([η] Total - [η] I ×X I ) / X II In the formula, [η] Total represents the intrinsic viscosity of the final polymer (unit: dL / g), and [η] I represents the intrinsic viscosity number (unit: dL / g) of the polymer (I), and X I represents the mass ratio of polymer (I) to the final polymer, and X II represents the mass ratio of polymer (II) to the final polymer. I and X II can be determined from the material balance in the polymerization process.
[0123] Here, the mass ratio X of the polymer (II) to the final polymer II may be calculated by the following formula using the heat of crystalline fusion of the polymer (I) and the final polymer: II = 1 - (ΔHf) T / (ΔHf) P In the formula, (ΔHf) T represents the heat of fusion (unit: cal / g) of the final polymer (polymer (I) and polymer (II)), and (ΔHf) P represents the heat of fusion (unit: cal / g) of polymer (I).
[0124] (Ethylene-α-olefin copolymer) The resin composition may contain an ethylene-α-olefin copolymer. The ethylene-α-olefin copolymer contained in the resin composition may be an ethylene-α-olefin copolymer derived from a recycled material (contained in a recycled material), or may contain an ethylene-α-olefin copolymer not derived from a recycled material (virgin ethylene-α-olefin copolymer).
[0125] The ethylene-α-olefin copolymer is a copolymer of ethylene and an α-olefin containing more than 50% by mass of structural units derived from ethylene. The content of structural units derived from ethylene in the ethylene-α-olefin copolymer may be 60% by mass or more, or 70% by mass or more.
[0126] The ethylene-α-olefin copolymer may be a copolymer having monomer units derived from an α-olefin having 3 to 20 carbon atoms and monomer units derived from ethylene. Examples of the α-olefin having 3 to 20 carbon atoms include propylene, 1-butene, isobutene, 1-pentene, 2-methyl-1-butene, 3-methyl-1-butene, 1-hexene, 2-methyl-1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-octene, 1-nonene, 1-decene, 1-undecene, and 1-dodecene. From the viewpoints of making it easier to remove the molded article from the mold and of making the tensile breaking strain of the obtained molded article larger, propylene, 1-butene, 1-hexene, or 1-octene is preferred.
[0127] Examples of the ethylene-α-olefin copolymer include an ethylene-propylene copolymer, an ethylene-1-butene copolymer, an ethylene-1-hexene copolymer, an ethylene-1-octene copolymer, and an ethylene-1-butene-1-hexene copolymer. The ethylene-α-olefin copolymer may be used alone or in combination of two or more. The ethylene-α-olefin copolymer is preferably an ethylene-1-butene copolymer or an ethylene-1-octene copolymer, from the viewpoints that the molded article can be more easily removed from the mold and that the tensile breaking strain of the resulting molded article is likely to be larger.
[0128] In one embodiment of the resin composition, the content of the ethylene-α-olefin copolymer may be 1% by mass or more, or 5% by mass or more, relative to 100% by mass of the total mass of the resin composition. The content of the ethylene-α-olefin copolymer may be 50% by mass or less, or 30% by mass or less, relative to 100% by mass of the total mass of the resin composition.
[0129] The recycled material (A) may contain an ethylene-α-olefin copolymer. The content of the ethylene-α-olefin copolymer may be 1% by mass or more, or 5% by mass or more, relative to 100% by mass of the total mass of the recycled material (A). Furthermore, the content of the ethylene-α-olefin copolymer may be 50% by mass or less, or 30% by mass or less, relative to 100% by mass of the total mass of the recycled material (A).
[0130] (Filler) The resin composition may contain a filler. Examples of the filler include glass powder such as glass beads, glass balloons, and glass flakes, silicate minerals, alumina, magnesium oxide, antimony oxide, barium ferrite, strontium ferrite, beryllium oxide, magnesium hydroxide, aluminum hydroxide, basic magnesium carbonate, magnesium carbonate, carbonate minerals, calcium sulfate, magnesium sulfate, basic magnesium sulfate, calcium sulfite, cadmium sulfide, asbestos, mica, calcium carbonate, talc, silica, calcium silicate, hydrotalcite, kaolin, diatomaceous earth, graphite, pumice, ebonized powder, cotton flock, cork powder, barium sulfate, fluororesin, cellulose powder, and at least one selected from the group consisting of wood flour.
[0131] When the resin composition contains a filler, the filler may be a filler derived from a recycled material (contained in a recycled material), or may be a filler not derived from a recycled material (i.e., a virgin filler).
[0132] When the filler is in the form of particles, the shape thereof is not particularly limited, and may be plate-like, needle-like, or fibrous.
[0133] From the viewpoints of the rigidity, impact resistance, and dimensional stability of the resin composition and the molded article, the filler is preferably an inorganic filler, more preferably talc, which is a plate-like silicate mineral, from the viewpoints that the molded article can be more easily removed from the mold and that the tensile breaking strain of the resulting molded article is likely to be larger.
[0134] In one embodiment of the resin composition, the content of the filler is preferably 1% by mass or more, and may be 5% by mass or more, relative to the total mass (100% by mass) of the resin composition, from the viewpoint of making it easier to remove the molded article from the mold and making it easier for the tensile breaking strain of the obtained molded article to become larger. The content of the filler may be 50% by mass or less, or 30% by mass or less, relative to the total mass (100% by mass) of the resin composition.
[0135] The recycled material (A) may contain a filler. The content of the filler may be 1% by mass or more, or 5% by mass or more, based on 100% by mass of the total mass of the recycled material (A). The content of the filler may be 50% by mass or less, or 30% by mass or less, based on 100% by mass of the total mass of the recycled material (A).
[0136] In one embodiment, the recycled material (A) may contain ash. The ash content refers to components remaining as ash after heating the recycled material (A) at 600° C. for 60 minutes. The ash content can be determined by the following method.
[0137] (Method for measuring ash content) The crucible is heated at 600°C for 60 minutes using an electric furnace, removed and cooled in a desiccator for 1 hour, and then weighed on a precision balance. 10 g of recycled material (A) is weighed into the crucible and heated at 600°C for 60 minutes using an electric furnace to completely incinerate it. Next, the crucible is cooled in a desiccator for 1 hour, and the mass of the ash is measured to the nearest 0.1 mg using a precision balance, and the ash content (mass%) relative to the recycled material (A) is calculated.
[0138] In the recycled material (A), the ash content is preferably 1% by mass or more, more preferably 5% by mass or more, relative to the total mass (100% by mass) of the recycled material (A), from the viewpoint that the tensile breaking strain of the resulting molded body is likely to be larger. In one embodiment, the ash content of the recycled material (A), relative to the total mass (100% by mass) of the recycled material (A), may be 1% by mass or more and 20% by mass or less, 1% by mass or more and 15% by mass or less, 1% by mass or more and 10% by mass or less, 2% by mass or more and 20% by mass or less, 2% by mass or more and 15% by mass or less, or 2% by mass or more and 10% by mass or less, relative to the total mass (100% by mass) of the recycled material (A).
[0139] When the recycled material (A) contains a filler, the majority of the filler is contained in the ash content of the recycled material (A). When the recycled material (A) contains a filler, the content of the filler roughly corresponds to the ash content of the recycled material (A).
[0140] The content of xylene-insoluble components (CXIS components) in the recycled material (A) is preferably 40% by mass or more and 99% by mass or less, more preferably 50% by mass or more and 95% by mass or less, relative to the total mass (100% by mass) of the recycled material (A), from the viewpoint of making it easier to remove the molded article from the mold and making it easier to obtain a molded article with a large tensile breaking strain. The content of xylene-soluble components (CXS components) in the recycled material (A) is preferably 1% by mass or more and 60% by mass or less, more preferably 5% by mass or more and 50% by mass or less, relative to the total mass (100% by mass) of the recycled material (A), from the viewpoint of making it easier to remove the molded article from the mold and making it easier to obtain a molded article with a large tensile breaking strain. In one embodiment, the content of xylene soluble components (CXS components) in the recycled material (A) may be 1% by mass or more and 40% by mass or less, 5% by mass or more and 40% by mass or less, 9% by mass or more and 40% by mass or less, 1% by mass or more and 30% by mass or less, 5% by mass or more and 30% by mass or less, or 9% by mass or more and 30% by mass or less, relative to the total mass of the recycled material (A) (100% by mass).
[0141] The content of xylene-soluble components (CXS components) in the recycled material (A) can be measured by the following method. That is, 4 g of the recycled material (A) is weighed out and refluxed in boiling xylene for 5 hours using a cylindrical filter paper and a Soxhlet extraction tube. Next, the extract is concentrated under reduced pressure using a rotary evaporator to obtain a polymer component. The obtained polymer component is weighed (the "mass of polymer component" is referred to as "a"). 2 g of the polymer component is weighed out and dissolved by heating in boiling xylene for 2 hours. Next, after cooling to 20°C, the solution is filtered using filter paper. The separated filtrate is concentrated under reduced pressure using a rotary evaporator to obtain the CXS component. The obtained CXS component is weighed (the "mass of CXS component" is referred to as "b"). The content of the CXS component in the recycled material (A) is calculated using the values a and b according to the following formula: CXS component amount (mass%) = (b / a) × 100
[0142] The CXIS component in the recycled material (A) is considered to be mainly composed of polymer (I) of the heterophasic propylene polymerization material contained in the recycled material (A) and / or a propylene homopolymer. The CXS component in the recycled material (A) is considered to be mainly composed of polymer (II) of the heterophasic propylene polymerization material contained in the recycled material (A) and / or an ethylene-α-olefin copolymer.
[0143] The resin composition according to one embodiment contains a recycled polypropylene polymer (recycled material (A)) having a xylene-insoluble component (CXIS component) content (or a xylene-soluble component (CXS component) content) within the above range, and a polyhydroxyalkanoate polymer (B). When a molded article is produced using the resin composition, the molded article can be easily removed from the mold and a molded article having a sufficiently large tensile break strain can be obtained. Even when the resin composition contains a virgin propylene polymer having a xylene-insoluble component (CXIS component) content (or a xylene-soluble component (CXS component) content) within the above range and a polyhydroxyalkanoate polymer (B), the molded article can be easily removed from the mold and a molded article having a sufficiently large tensile break strain can be obtained. However, compared to when the resin composition contains a recycled propylene polymer having a xylene-insoluble component (CXIS component) content (or a xylene-soluble component (CXS component) content) within the above range, the tensile break strain of the resulting molded article tends to be slightly inferior. In other words, when the content of xylene-insoluble components (CXIS components) (or the content of xylene-soluble components (CXS components)) of both the recycled propylene polymer and the virgin propylene polymer is within the above range, a resin composition containing a recycled propylene polymer whose content of xylene-insoluble components (CXIS components) (or the content of xylene-soluble components (CXS components)) is within the above range is more likely to improve the tensile breaking strain of the resulting molded product.
[0144] (Additives) The resin composition may contain components other than those described above (hereinafter also referred to as "other components") as necessary. Examples of other components include thermoplastic resins (polystyrenes (e.g., polystyrene, poly(p-methylstyrene), poly(α-methylstyrene), AS (acrylonitrile / styrene copolymer) resin), ABS (acrylonitrile / butadiene / styrene copolymer) resin, AAS (special acrylic rubber / acrylonitrile / styrene copolymer) resin, ACS (acrylonitrile / chlorinated polyethylene / styrene copolymer) resin, polychloroprene, chlorinated rubber, polyvinyl chloride, polyvinylidene chloride, acrylic resin, ethylene / vinyl alcohol copolymer resin, fluororesin, polyacetal, grafted polyphenylene ether resin and polyphenylene sulfide resin, polyurethane, polyamide, polyester resin (e.g., polyethylene terephthalate, polybutylene terephthalate), Examples of suitable additives include polylactic acid (PLA) resins (polylactic acid resins) produced by polymerizing plant-derived monomers extracted from biomaterials, such as styrene, polycarbonate, polysulfone, polyether ether ketone, polyether sulfone, aromatic polyester resins, polybutadiene, 1,2-polybutadiene, polyisoprene, styrene / butadiene copolymers, butadiene / acrylonitrile copolymers, and natural rubber), epoxy resins, diallyl phthalate prepolymers, silicone resins, silicone rubber, epichlorohydrin rubber, acrylic rubber, and PLA resins (polylactic acid) produced by polymerizing plant-derived monomers extracted from biomaterials, neutralizing agents, antioxidants, UV absorbers, nucleating agents, lubricants, antistatic agents, antiblocking agents, processing aids, organic peroxides, colorants (inorganic pigments, organic pigments, pigment dispersants, and the like), foaming agents, foam nucleating agents, plasticizers, flame retardants, crosslinking agents, crosslinking aids, brightness enhancers, antibacterial agents, and light diffusing agents. The resin composition may contain only one of the above components, or a combination of two or more of them.
[0145] Other components that may be contained in the resin composition may be virgin materials not derived from recycled materials, may be derived from recycled materials, may be included in the raw materials used during recycling, or may be included in the raw materials used to produce the resin composition together with the recycled propylene polymer.
[0146] <Resin Composition> The melt mass flow rate (MFR) of the resin composition, measured in accordance with JIS K7210-2014 at a temperature of 230°C and a load of 2.16 kgf, may be 1 g / 10 min or more, 10 g / 10 min or more, 30 g / 10 min or more, 50 g / 10 min or more, 70 g / 10 min or more, 100 g / 10 min or more, 120 g / 10 min or more, 140 g / 10 min or more, or 160 g / 10 min or more. The MFR of the resin composition may be 500 g / 10 min or less, 450 g / 10 min or less, 400 g / 10 min or less, 350 g / 10 min or less, 300 g / 10 min or less, or 250 g / 10 min or less.
[0147] The tensile break strain of the resin composition may be 10% or more, 15% or more, 20% or more, or 25% or more. The tensile break strain of the resin composition may be 55% or less, 50% or less, 45% or less, or 40% or less. The tensile break strain of the resin composition can be measured by the method described in the examples below.
[0148] The content of the recycled material may be 15% by mass or more, 20% by mass or more, 25% by mass or more, or 30% by mass or more based on the total amount of the resin composition, and 90% by mass or less, 80% by mass or less, 70% by mass or less, 60% by mass or less, 50% by mass or less, or 40% by mass or less based on the total amount of the resin composition.
[0149] The content of the polyhydroxyalkanoate polymer may be 1% by mass or more, 5% by mass or more, 7% by mass or more, or 10% by mass or more based on the total amount of the resin composition, and 30% by mass or less, 27% by mass or less, 25% by mass or less, 22% by mass or less, or 20% by mass or less based on the total amount of the resin composition.
[0150] The ratio of the polyhydroxyalkanoate polymer content to the recycled material content (polyhydroxyalkanoate polymer content / recycled material content) may be 0.01 or more, 0.1 or more, 0.2 or more, or 0.3 or more, or may be 2 or less, 1.5 or less, 1 or less, or 0.8 or less.
[0151] The content of the propylene polymer may be 25% by mass or more, 35% by mass or more, 40% by mass or more, 45% by mass or more, or 50% by mass or more based on the total amount of the resin composition, and 85% by mass or less, 75% by mass or less, 70% by mass or less, 65% by mass or less, or 60% by mass or less based on the total amount of the resin composition.
[0152] The ratio of the propylene polymer content to the recycled material content (propylene polymer content / recycled material content) may be 0.1 or more, 0.5 or more, 1 or more, or 1.5 or more, and may be 6 or less, 5 or less, 4 or less, 3 or less, or 2.5 or less.
[0153] When the resin composition further contains a propylene polymer not derived from a recycled material (for example, a virgin propylene polymer), the recycled material content, the polyhydroxyalkanoate polymer content, and the propylene polymer content may be as follows, based on the total amount of the resin composition: The recycled material content may be 15 to 70 mass%, 20 to 60 mass%, or 25 to 50 mass%, the polyhydroxyalkanoate polymer content may be 1 to 30 mass%, 5 to 27 mass%, or 7 to 25 mass%, and the propylene polymer content may be 25 to 85 mass%, 35 to 75 mass%, or 40 to 70 mass%.
[0154] <Method of Manufacturing Resin Composition> A method of manufacturing the resin composition according to this embodiment will be described.
[0155] The method for producing a resin composition according to this embodiment includes at least the steps of obtaining a recycled material containing a propylene polymer from a part and mixing the recycled material with a polyhydroxyalkanoate polymer. Specifically, the resin composition can be obtained by melt-kneading the raw material components described above. The temperature during melt-kneading may be 180°C or higher, 180 to 300°C, or 180 to 250°C.
[0156] For melt kneading, a Banbury mixer, a single-screw extruder, a twin-screw co-rotating extruder, or the like can be used.
[0157] The order in which the raw material components are kneaded is not particularly limited. For example, the raw material components may be kneaded all at once, or some of the raw material components may be kneaded and then the resulting kneaded mixture may be kneaded with the other components.
[0158] The shape of the propylene resin composition is not particularly limited, and the propylene resin composition may be in the form of, for example, a strand, a sheet, a plate, or a pellet. The pellet-shaped resin composition can be produced, for example, by forming a strand-shaped resin composition and then cutting it to an appropriate length.
[0159] From the viewpoint of the moldability of the resin composition and the production stability when producing a molded article, the shape of the resin composition before being molded into a molded article is preferably in the form of pellets having a length of about 1 to 50 mm.
[0160] <Uses of Molded Article> Examples of uses of the molded article according to the present invention include automotive materials, home appliance materials, office automation equipment materials, building materials, drainage facilities, toiletry materials, various tanks, containers, sheets, and the like.
[0161] Examples of automotive materials include interior parts such as door trims, pillars, instrument panels, consoles, rocker panels, armrests, door inner panels, and spare tire covers; exterior parts such as bumpers, spoilers, fenders, side steps, and door outer panels; and other parts such as air intake ducts, coolant reserve tanks, radiator reserve tanks, window washer tanks, fender liners, and fans; and integrally molded parts such as front end panels.
[0162] Examples of home appliance materials include materials for washing machines (outer tubs, inner tubs, lids, pulsators, balancers, wash tubs, etc.), materials for dryers (exteriors, inner boxes, lids, etc.), materials for vacuum cleaners, materials for rice cookers, materials for pots, materials for warmers, materials for dishwashers, and materials for air purifiers.
[0163] Examples of materials related to office automation equipment and media include cases for magnetic recording media and optical recording media, parts for personal computers, and parts for printers.
[0164] Examples of building materials include frames for solidifying concrete and wall components. Examples of drainage equipment include pipes and pump parts. Examples of container materials include food containers, transport containers, clothing containers, and shipping pallets.
[0165] The present invention will be specifically described below with reference to examples, although the present invention is not limited to the examples shown below.
[0166] [Components used in Examples, Comparative Examples, and Reference Examples] The following raw materials were used in the Examples, Comparative Examples, and Reference Examples.
[0167] Component A: Recycled Material Containing Propylene Polymer The following recycled polypropylene composition was prepared as a recycled material containing a propylene polymer.
[0168] (A-1) Recycled polypropylene composition derived from automobile bumpers collected from the market Melt flow rate (MFR) (230°C, 2.16 kg load): 42.0 g / 10 min Ash content: 18.1 mass% CXIS content (xylene insoluble components): 70.0 mass% CXS content (xylene soluble components): 30.0 mass%
[0169] (A-2) Recycled polypropylene composition derived from automobile bumpers collected from the market CXIS content (xylene insoluble component): 99.7% by mass CXS content (xylene soluble component): 0.3% by mass
[0170] (A-3) Recycled polypropylene composition derived from automobile washer tanks collected from the market Melt flow rate (MFR) (230°C, 2.16 kg load): 5.3 g / 10 min Ash content: 2.3 mass% CXIS content (xylene insoluble components): 90.9 mass% CXS content (xylene soluble components): 9.1 mass%
[0171] <Method for measuring ash content> The crucible was heated at 800°C for 60 minutes using an electric furnace, removed and cooled in a desiccator for 1 hour, and then weighed on a precision balance. 10 g of the recycled polypropylene composition was weighed into the crucible and heated at 800°C for 60 minutes using an electric furnace to completely incinerate it. The crucible was then cooled in a desiccator for 1 hour, and the weight of the ash was measured to the nearest 0.1 mg using a precision balance, and the ash content (% by mass) relative to the recycled polypropylene composition was calculated.
[0172] <Method for measuring the contents of CXIS and CXS components> 4 g of the recycled polypropylene composition, A-2 or C-6, was weighed and refluxed in boiling xylene for 5 hours using a cylindrical filter paper and a Soxhlet extraction tube. Next, the extract was concentrated under reduced pressure using a rotary evaporator to obtain a polymer component. The obtained polymer component was weighed (hereinafter, the "mass of the polymer component" will be referred to as "a"). 2 g of the polymer component was weighed and dissolved by heating in boiling xylene for 2 hours. Next, after cooling to 20°C, the solution was filtered using filter paper. The separated filtrate was concentrated under reduced pressure using a rotary evaporator to obtain a CXS component. The obtained CXS component was weighed (hereinafter, the "mass of the CXS component" will be referred to as "b"). The contents of the CXIS and CXS components in the recycled polypropylene composition, A-2 or C-6, were calculated using the following formula using the values a and b. The CXIS component was obtained by vacuum drying the solid remaining on the filter paper. The obtained CXIS component was used to evaluate the molecular weight distribution. Amount of CXS component (mass%) = (b / a) × 100 Amount of CXIS component (mass%) = 100 - Amount of CXS component (mass%)
[0173] Component B: Polyhydroxyalkanoate Polymer The following poly(3-hydroxybutyrate) was prepared as a polyhydroxyalkanoate polymer.
[0174] Component B-1: Poly(3-hydroxybutyrate) manufactured by Newlight Technologies, Inc. Melt flow rate (MFR) (190°C, 2.16 kg load): 2.4 g / 10 min Melting point: 170.9°C
[0175] Component C: Propylene Polymer The following components C-1, C-2, C-3, C-4, C-5, and C-6 were prepared as propylene polymers.
[0176] (C-1) Virgin propylene homopolymer Virgin propylene homopolymer (C-1) was produced by liquid-gas phase polymerization using the polymerization catalyst obtained by the method described in Example 1 of JP-A No. 2004-182981. The physical properties were as follows: Melt flow rate (MFR) (230°C, 2.16 kg load): 118 g / 10 min
[0177] (C-2) Virgin propylene homopolymer Virgin propylene homopolymer (C-2) was produced by liquid phase-gas phase polymerization using the polymerization catalyst obtained by the method described in Example 1 of JP-A 2004-182981. The physical properties were as follows: Melt flow rate (MFR) (230°C, 2.16 kg load): 298 g / 10 min
[0178] (C-3) Virgin propylene homopolymer Virgin propylene homopolymer (C-3) was produced by liquid phase-gas phase polymerization using the polymerization catalyst obtained by the method described in Example 1 of JP-A No. 2004-182981. The physical properties were as follows: Melt flow rate (MFR) (230°C, 2.16 kg load): 700 g / 10 min
[0179] (C-4) Virgin propylene homopolymer MF650Y manufactured by LyondellBasell was used as the virgin propylene homopolymer (C-4). Melt flow rate (MFR) (230°C, 2.16 kg load): 1800 g / 10 min
[0180] (C-5) Virgin heterophasic propylene polymer material A heterophasic propylene polymer material was produced by gas phase polymerization in the presence of a polymerization catalyst obtained by the method described in Example 1 of JP-A-2004-182981. The physical properties of the obtained component C-5 are as follows: Melt flow rate (MFR) (230°C, 2.16 kg load): 32.4 g / 10 min (a) Propylene homopolymer (polymer (I)) Intrinsic viscosity: 1.00 dL / g (b) Ethylene-propylene random copolymer (polymer (II)) Intrinsic viscosity: 5.0 dL / g Content of ethylene-propylene random copolymer (polymer (II)): 16 mass% Content of structural units derived from ethylene in polymer (II): 43.0 mass% In component C-5, the "content of structural units derived from ethylene" in the "propylene-ethylene random copolymer" indicates the ethylene content in polymer (II) (the content of structural units derived from ethylene based on the total mass of polymer (II)).
[0181] <Method for measuring ethylene content in polymer (II)> The ethylene content in polymer (II) was measured under the following conditions. 13 It was determined from the C-NMR spectrum based on the report by Kakugo et al. (Macromolecules, 15, 1150-1152 (1982)). 13 The C-NMR spectrum was measured using a sample prepared by uniformly dissolving approximately 200 mg of heterophasic propylene polymer material in 3 mL of orthodichlorobenzene in a test tube with a diameter of 10 mm under the following conditions: Measurement temperature: 135°C, Pulse repetition time: 10 seconds, Pulse width: 45°, Number of accumulations: 2500.
[0182] (C-6) Virgin heterophasic propylene polymer material CXIS content (xylene insoluble component): 69.5 mass% CXS content (xylene soluble component): 30.5 mass%
[0183] <Method for Measuring Intrinsic Viscosity> The intrinsic viscosity (unit: dL / g) was measured at a temperature of 135°C using tetralin as a solvent by the following method.
[0184] Using an Ubbelohde viscometer, the reduced viscosity was measured at three concentrations: 0.1 g / dL, 0.2 g / dL, and 0.5 g / dL. The reduced viscosity was plotted against the concentration, and the intrinsic viscosity was calculated by extrapolation, in which the concentration was extrapolated to zero. The method for calculating the intrinsic viscosity by extrapolation is described, for example, on page 491 of "Polymer Solutions, Polymer Experiments 11" (published by Kyoritsu Shuppan Co., Ltd. in 1982).
[0185] Component D: Other Components The following components were used as other components: Hydrotalcite "DHT-4C" manufactured by Kyowa Chemical Industry Co., Ltd. "Sumilizer GA80" (antioxidant) manufactured by Sumitomo Chemical Co., Ltd. "Irgafos 168" (antioxidant) manufactured by BASF Co., Ltd. "Sumilizer TPM" (antioxidant) manufactured by Sumitomo Chemical Co., Ltd. "Sumisorb 400" (ultraviolet absorber) manufactured by Sumika Chemtex Co., Ltd. "Uvinul 5050H" (light stabilizer) manufactured by BASF Co., Ltd. "Alflo H-50P" (lubricant) manufactured by NOF Corporation
[0186] Examples 1 to 4 Propylene-based resin compositions were produced by the following method. 10 parts by mass of virgin propylene homopolymer (C-1), 90 parts by mass of poly(3-hydroxybutyrate) (B-1), and 0.1 parts by weight of "Sumilizer TPM" and 0.1 parts by weight of "Sumisorb 400" as additives were weighed out, and all components were mixed and kneaded using a single-screw kneader manufactured by Tanabe Plastic Machinery Co., Ltd. with a screw diameter of 40 mm at a barrel temperature of 175°C and a screw rotation speed of 45 rpm. The kneaded product was then extruded through a die hole, and the molten strand was immersed in a cooling water bath to cool and solidify, followed by palladium sintering. The raw materials having the composition shown in Table 1 and additives such as 0.03 parts by weight of "DHT-4C," 0.1 parts by weight of "Sumilizer GA80," 0.05 parts by weight of "Irgafos 168," 0.02 parts by weight of "Sumilizer TPM," 0.15 parts by weight of "Uvinul 5050H," 0.2 parts by weight of "Sumisorb 400," and 0.05 parts by weight of "Alflo H-50P" were weighed out, and all components were mixed and cut into pellets using a PET bottle manufactured by Technovel Co., Ltd. A propylene-based resin composition in pellet form was obtained by melt-kneading using a twin-screw kneader KZW-15 / 45MG (cylinder inner diameter 15.5 mm, screw outer diameter 15.0 mm, L / D = 45). The melt-kneading conditions were: cylinder temperature 200°C; screw rotation speed 500 rpm; two screens, one 100 mesh and one 50 mesh, stacked; and extrusion rate 6 kg / hr.
[0187] Comparative Examples 1 to 4 According to the formulations in Table 1, pellet-shaped propylene-based resin compositions were obtained in the same manner as in Examples 1 to 4.
[0188] Example 5, Comparative Example 5, Reference Example 1 Propylene-based resin compositions were produced by the following method. 10 parts by mass of virgin propylene homopolymer (C-1), 90 parts by mass of poly(3-hydroxybutyrate) (B-1), and 0.1 parts by weight of "Sumilizer TPM" and 0.1 parts by weight of "Sumisorb 400" as additives were weighed out, and all components were mixed and kneaded using a single-screw kneader manufactured by Tanabe Plastic Machinery Co., Ltd. with a screw diameter of 40 mm at a barrel temperature of 175°C and a screw rotation speed of 45 rpm. The kneaded product was then extruded through a die hole, and the molten strand was immersed in a cooling water bath to cool and solidify, followed by pelletization. The raw materials having the composition shown in Table 2 and additives such as 0.03 parts by weight of "DHT-4C," 0.1 parts by weight of "Sumilizer GA80," 0.05 parts by weight of "Irgafos 168," 0.02 parts by weight of "Sumilizer TPM," 0.15 parts by weight of "Uvinul 5050H," 0.2 parts by weight of "Sumisorb 400," and 0.05 parts by weight of "Alflo H-50P" were weighed out, and all components were mixed and cut into pellets using a PET bottle manufactured by Technovel Co., Ltd. A propylene-based resin composition in pellet form was obtained by melt-kneading using a twin-screw kneader KZW-15 / 45MG (cylinder inner diameter 15.5 mm, screw outer diameter 15.0 mm, L / D = 45). The melt-kneading conditions were: cylinder temperature 200°C; screw rotation speed 500 rpm; two screens, one 100 mesh and one 50 mesh, stacked; and extrusion rate 6 kg / hr.
[0189] <Measurement of Melt Flow Rate (MFR)> According to the method specified in JIS K7210, the MFR of the resulting propylene-based resin composition was measured under conditions of a temperature of 230°C and a load of 2.16 kg.
[0190] <Production of injection-molded articles for evaluating tensile strain at break> A pellet-shaped propylene-based resin composition was injection-molded under the following conditions within the range specified in JIS K7152 to produce an injection-molded article for evaluating tensile strain at break. The propylene-based resin composition melted in the injection molding machine was supplied from the gate into the mold cavity by the injection molding machine. The measurement results are shown in Tables 1 and 2. Injection molding machine: Toyo Machinery & Metal Si30III (clamping force 30 tons, cylinder diameter 18 mm) Cylinder temperature: 180°C Mold temperature: 50°C Injection speed: 20 mm / sec Cooling time: 30 sec
[0191] <Evaluation of sprue releasability> Pelletized propylene-based resin compositions were dried at 100°C for 1 hour and then injection molded under the following conditions. If the sprue runner remained on the fixed side of the mold when the mold was opened and closed, the mold releasability was judged to be poor. If the sprue runner did not remain on the fixed side of the mold when the mold was opened and closed, the mold releasability was judged to be good. Of 10 molding shots, the number of times when the mold releasability was judged to be good was evaluated. The evaluation results are shown in Tables 1 and 2. In the tables, "-" means that the value was not measured. Injection molding machine: Toyo Machinery & Metal Si30III (clamping force 30 tons, cylinder diameter 18 mm) Cylinder temperature: 180°C Mold temperature: 50°C Injection speed: 20 mm / sec Cooling time: 30 sec
[0192]
[0193]
Claims
1. A resin composition comprising a recycled material (A) containing a propylene polymer and a polyhydroxyalkanoate polymer (B), wherein the content of xylene soluble components (CXS components) in the recycled material (A) is 1% by mass or more and 60% by mass or less.
2. The resin composition according to claim 1, wherein the recycled material (A) is a recycled material derived from an automobile part.
3. The resin composition according to claim 1, which comprises a propylene homopolymer.
4. The resin composition of claim 1, comprising a heterophasic propylene polymeric material.
5. The resin composition according to claim 4, wherein the heterophasic propylene polymer material has an isotactic pentad fraction of 0.961 or more.
6. The resin composition according to claim 1, which comprises an ethylene-α-olefin copolymer.
7. The resin composition according to claim 1, wherein the recycled material (A) comprises an ethylene-α-olefin copolymer.
8. The resin composition according to claim 1, further comprising a filler.
9. The resin composition according to claim 8, wherein the filler is an inorganic filler.
10. The resin composition according to claim 1, wherein the recycled material (A) comprises a filler.
11. The resin composition according to claim 1, further comprising a propylene polymer, wherein the content of the recycled material (A) is 15 to 70 mass% based on the total amount of the resin composition, the content of the polyhydroxyalkanoate polymer (B) is 1 to 30 mass% based on the total amount of the resin composition, and the content of the propylene polymer is 25 to 85 mass% based on the total amount of the resin composition.
12. A molded article comprising the resin composition according to any one of claims 1 to 11.
Citation Information
Patent Citations
Drying method and apparatus for polyolefin
JP1980075410A
Production of alpha-olefin polymer
JP1986218606A
Ethylene-propylene block copolymer
JP1993194685A
Catalyst for polymerizing alpha-olefin and production of alpha-olefin polymer
JP1995216017A
Propylene / ethylene-alpha-olefin block copolymer and its production
JP1997316147A