Steel material and method for producing steel material

The steel material achieves a balance between hardness and toughness through a specific composition and high-frequency induction heating process, forming band-like fine carbides, addressing the cost and performance limitations of existing high-strength steel production methods.

WO2024203886A1PCT designated stage expired Publication Date: 2024-10-03NHK SPRING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011369
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing steel materials face a challenge in achieving a balance between hardness and toughness, as increasing hardness to improve strength often compromises toughness and delayed fracture resistance, and current methods for producing high-strength steel with excellent hydrogen embrittlement resistance are costly.

Method used

A steel material composition with specific ranges of C, Si, Mn, Cr, P, S, Cu, Ni, Ti, and V, combined with a high-frequency induction heating process for quenching and tempering, forming row-like fine carbides that aggregate in a band shape across lath interfaces, enhancing both hardness and toughness.

Benefits of technology

The steel material achieves high hardness and toughness, with improved fatigue strength, delayed fracture resistance, and corrosion resistance, suitable for applications like automobile suspension springs and valve springs, while maintaining cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011369_03102024_PF_FP_ABST
    Figure JP2024011369_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a steel material that has a fine carbide band in which fine carbides are aggregated into a band shape, and has high hardness and toughness. A steel material according to the present invention contains 0.39% by mass to 0.64% by mass of C, 1.20% by mass to 2.50% by mass of Si and 0.10% by mass to 1.15% by mass of Mn, with the balance being made up of Fe and unavoidable impurities. This steel material is characterized by having a fine carbide band in which fine carbides are aggregated into a band shape.
Need to check novelty before this filing date? Find Prior Art

Description

Steel material and steel material manufacturing method

[0001] The present invention relates to a steel material and a method for manufacturing the steel material.

[0002] Steel materials used in automobiles and various industrial machinery parts are generally hardened by quenching. The hardness of steel materials, which are primarily martensitic due to quenching, is determined by the C content in the components, and the hardness of the steel material can be increased by increasing the C content. However, increasing the hardness of steel materials also reduces their toughness, significantly reducing their delayed fracture resistance and corrosion fatigue resistance, so steel materials must have a balance between hardness and toughness.

[0003] As a steel material having high strength and elongation, a technology has been proposed for obtaining a high-strength steel plate from a single-phase metal structure of tempered martensite, which contains C, Si, Mn, P, and S, and is quenched and tempered by high-frequency induction heating or resistance heating to have a tensile strength of 700 to 1,300 MPa and an elongation of 12% or more (see, for example, Patent Document 1).

[0004] Furthermore, as a high strength spring with excellent resistance to hydrogen embrittlement, the following components are used by mass: C: 0.40 to 0.50%, Si: 1.00 to 3.00%, Mn: 0.30 to 1.20%, Ni: 0.05 to 0.50%, Cr: 0.35 to 1.50%, Mo: 0.03 to 0.50%, Cu: 0.05 to 0.50%, Al: 0.005 to 0.100%, V: 0.05 to 0.50%, Nb: 0.005 to 0.150%, N: 0. It has been proposed to contain 0.0100 to 0.0200%, with P limited to 0.015% or less and S limited to 0.010% or less, with the balance being Fe and unavoidable impurities, and containing an Nb compound containing at least one of Nb carbide, Nb nitride, and Nb carbonitride, and a V compound containing at least one of V carbide and V carbonitride that precipitates around the Nb compound (see, for example, Patent Document 2).

[0005] JP 2018-524475 A JP 2018-154914 A

[0006] In the technology of Patent Document 1, by performing tempering at a high temperature of 500°C to the A1 transformation point, a steel material having excellent elongation can be obtained, but a steel material having high strength cannot be obtained.

[0007] Furthermore, in the technology of Patent Document 2, although a high strength spring can be obtained by using Nb and V compounds, there is a problem of cost because it is a special material.

[0008] The present invention has been made in view of the above, and has an object to provide a steel material having high hardness and toughness, and a method for manufacturing the steel material.

[0009] In order to solve the above-mentioned problems and achieve the object, the steel material according to the present invention contains C in proportions of 0.39 mass% or more and 0.64 mass% or less, Si in proportions of 1.20 mass% or more and 2.50 mass% or less, Mn in proportions of 0.10 mass% or more and 1.15 mass% or less, with the balance being Fe and unavoidable impurities, and is characterized in that the steel material has row-shaped fine carbides in which fine carbides are aggregated in a band shape.

[0010] In addition, in the steel material according to the present invention, the fine carbides have a length of 1 nm or more and 100 nm or less, and the linear fine carbides have a length of 100 nm or more and 50 μm or less.

[0011] In the steel material according to the present invention, the linear fine carbides are formed so as to cross lath boundaries, which are the smallest units constituting prior austenite grain boundaries.

[0012] Further, the steel material according to the present invention has a Charpy impact value of 60 J / cm 2 That's all.

[0013] Furthermore, the steel material according to the present invention contains 0.10 mass % or more and 1.10 mass % or less of Cr, 0.025 mass % or less of P, and 0.025 mass % or less of S in the above invention.

[0014] Furthermore, in the steel material according to the present invention, Cu is contained in an amount of 0.15 mass % or more and 0.40 mass % or less, and Ni is contained in an amount of 0.15 mass % or more and 0.70 mass % or less.

[0015] Furthermore, in the steel material according to the present invention, Ti is contained in a proportion of 0.05 mass % or more and 0.11 mass % or less.

[0016] Furthermore, in the steel material according to the present invention, V is contained in a proportion of 0.10 mass % or more and 0.20 mass % or less.

[0017] Furthermore, in a method for producing a steel material according to the present invention, a steel material containing 0.39 mass% or more and 0.64 mass% or less of C, 1.20 mass% or more and 2.50 mass% or less of Si, 0.10 mass% or more and 1.15 mass% or less of Mn, with the balance being Fe and unavoidable impurities, is quenched and tempered, characterized in that the tempering step involves tempering the steel material at 460°C to 490°C for 5 seconds to 30 seconds using a high-frequency heating induction device, to form row-shaped fine carbides in which fine carbides are aggregated in a band shape.

[0018] The present invention has the effect of providing a steel material having high hardness and toughness.

[0019] Fig. 1 is a transmission electron microscope photograph of a steel material according to an embodiment of the present invention, and Fig. 2 is a diagram illustrating the mechanism of formation of linear fine carbides in the steel material according to an embodiment of the present invention.

[0020] Hereinafter, embodiments for carrying out the present invention (hereinafter referred to as "embodiments") will be described with reference to the accompanying drawings. Note that the drawings are schematic, and the relationship between the thickness and width of each part, the thickness ratio of each part, etc. may differ from the actual ones, and the drawings may also include parts with different dimensional relationships and ratios.

[0021] (Embodiment) A steel material according to the present invention contains C in an amount of 0.39 mass% or more and 0.64 mass% or less, Si in an amount of 1.20 mass% or more and 2.50 mass% or less, Mn in an amount of 0.10 mass% or more and 1.15 mass% or less, and the balance being Fe and unavoidable impurities, and is characterized in that the steel material has row-shaped fine carbides in which fine carbides are aggregated in a band shape.

[0022] <Material Composition> The steel material according to the present invention contains C in a proportion of 0.39% by mass or more and 0.64% by mass or less. C contributes to improving the strength of the steel material. If the C content is less than 0.39% by mass, the effect of improving strength is not sufficiently obtained, resulting in insufficient fatigue resistance and sag resistance. Furthermore, if the C content exceeds 0.64% by mass, toughness decreases and cracking becomes more likely to occur.

[0023] The steel material according to the present invention contains Si in a proportion of 1.20% by mass or more and 2.50% by mass or less. Si is effective in deoxidizing the steel material and contributes to improving strength and temper softening resistance. If the Si content is less than 1.20% by mass, the above effects are not sufficiently obtained, and carbides formed during tempering become coarse. If the Si content exceeds 2.50% by mass, toughness decreases, making the wire more susceptible to cracking, and decarburization is promoted, resulting in a decrease in wire surface strength.

[0024] The steel material according to the present invention contains Mn in a proportion of 0.10% by mass or more and 1.15% by mass or less. Mn contributes to improving hardenability. If the Mn content is less than 0.10% by mass, it becomes difficult to ensure sufficient hardenability, and the effect of fixing S (MnS formation), which is detrimental to ductility and toughness, becomes poor. Furthermore, if the Mn content exceeds 1.15% by mass, ductility decreases, and cracks and surface scratches are more likely to occur.

[0025] The steel material according to the present invention is required to contain C, Si, and Mn in the above-mentioned proportions, but may contain elements other than those mentioned above.The steel material according to the present invention may contain, in addition to C, Si, and Mn, Cr in the proportions of 0.10 mass% to 1.10 mass%, P in the proportion of 0.025 mass% or less, S in the proportion of 0.025 mass% or less, Cu in the proportion of 0.15 mass% to 0.40 mass%, Ni in the proportion of 0.15 mass% to 0.40 mass%, Ti in the proportion of 0.05 mass% to 0.11 mass%, and V in the proportion of 0.10 mass% to 0.20 mass%.

[0026] Cr is effective in preventing decarburization, and also contributes to improving strength and temper softening resistance, thereby improving fatigue resistance. It is also effective in improving warm setting resistance. If the Cr content is less than 0.10 mass%, the above effects cannot be fully achieved. If the Cr content exceeds 1.10 mass%, toughness decreases, and cracks and surface scratches are more likely to occur.

[0027] S forms MnS in the steel material and improves machinability. If the S content exceeds 0.025% by mass, MnS may segregate at grain boundaries, resulting in a decrease in grain boundary strength. Therefore, the S content is preferably 0.025% by mass or less.

[0028] If the P content is high, it segregates at the austenite grain boundaries, reducing the grain boundary strength. The P content is preferably 0.025 mass% or less.

[0029] Cu is effective in improving hardenability and can improve fatigue strength by dissolving in ferrite. If the Cu content is less than 0.15 mass%, the above effect cannot be sufficiently obtained. If the Cu content exceeds 0.40 mass%, cracks may occur during hot working. The steel material according to the present invention preferably contains Cu in a proportion of 0.15 mass% or more and 0.40 mass% or less.

[0030] Ni is effective in improving hardenability, suppressing the formation of carbides, and improving fatigue strength. If the Ni content is less than 0.15 mass%, the effect of improving hardenability is insufficient. If the Ni content exceeds 0.40 mass%, not only will cost be a problem, but the amount of retained austenite will increase, reducing fatigue life. The steel material according to the present invention preferably contains Ni in a proportion of 0.05 mass% or more and 0.40 mass% or less.

[0031] Ti combines with C and N to form carbides and nitrides, which act as hydrogen trapping sites, thereby suppressing hydrogen diffusion into the steel material, improving corrosion resistance and delayed fracture resistance, and improving strength and toughness through grain refinement and precipitation strengthening. If the Ti content is less than 0.05 mass%, the above effects cannot be fully achieved. Furthermore, if it exceeds 0.11 mass%, a large amount of TiN is formed, resulting in a decrease in fatigue strength. The steel material according to the present invention preferably contains Ti in a proportion of 0.05 mass% or more and 0.11 mass% or less.

[0032] V combines with C and N in the steel material to act as a precipitation strengthening element and also improves fatigue strength. If the V content is less than 0.10 mass%, the above effect cannot be sufficiently obtained. Furthermore, if the V content exceeds 0.20 mass%, the above effect saturates. The steel material according to the present invention preferably contains V in a proportion of 0.10 mass% or more and 0.20 mass% or less.

[0033] Examples of steel materials according to the present invention include, but are not limited to, SAE9254 and SUP7.

[0034] <Linear Fine Carbides> The steel material according to the present invention has linear fine carbides in which fine carbides are aggregated in a band shape. Fig. 1 is a transmission electron micrograph of a steel material according to an embodiment of the present invention. The left end of Fig. 1 is an enlarged photograph at 10,000x, the middle at 50,000x, and the right end at 200,000x. As shown in Fig. 1, the steel material according to the present invention has linear fine carbides with a length of 100 nm to 50 µm in which fine carbides with long ends of 1 nm to 100 nm are aggregated in a band shape. The fine carbides are ε-Fe 2-3 C, and a plurality of linear fine carbides are formed in approximately parallel rows. Furthermore, it is preferable that the linear fine carbides are formed so as to cross lath boundaries, which are the smallest units constituting prior austenite grain boundaries. This can further improve the toughness of the steel material.

[0035] FIG. 2 is a diagram illustrating the mechanism of formation of linear fine carbides in a steel material according to an embodiment of the present invention. Before quenching and tempering, the raw material has a lamellar pearlite structure composed of a ferrite layer with a high Si concentration and a cementite layer with a high Mn concentration. When heated for quenching, solute elements are typically dissolved into the austenitized steel material, resulting in homogenization. However, rapid heat treatment using a high-frequency induction heating device or the like results in the Si and Mn content not being homogenized and a concentration distribution remaining. Subsequent rapid tempering using a high-frequency induction heating device or the like does not resolve the Si and Mn concentration distribution, resulting in carbide precipitation in regions with low Si content. It is presumed that the carbides precipitate in an aggregated state without coarsening along the original pearlite structure, resulting in the formation of martensite with band-like aggregated linear fine carbides. The present inventors have discovered that linear fine carbides are formed by rapid tempering a steel material having a predetermined composition using a high-frequency heating device or the like. They also found that steel materials in which fine linear carbides are formed have high Charpy impact values ​​and excellent toughness.

[0036] <Physical Properties> The steel material according to the present invention has a hardness of 550 HV or more and 630 HV or less, and a Charpy impact value of 60 J / cm 2 It is preferable that the hardness and Charpy impact value satisfy the above ranges, resulting in a steel material with high hardness and high toughness. It is more preferable that the hardness of the steel material is 560 Hv or more and 620 Hv or less. In addition, the Charpy impact value of the steel material is 70 J / cm 2 The hardness of the steel material is measured in accordance with the Vickers hardness test method specified in JIS Z 2244, and the Charpy impact value is measured in accordance with the Charpy impact test method for metallic materials specified in JIS Z 2241.

[0037] Furthermore, the steel material according to the present invention preferably has a tensile strength of 1400 MPa or more. A tensile strength of 1400 MPa or more makes it suitable for use in applications requiring strength, such as suspension springs. The tensile strength is measured in accordance with the method specified in JIS Z 2241.

[0038] <Manufacturing Method> A manufacturing method of a steel material according to the present invention comprises quenching and tempering a steel material containing 0.39% by mass or more and 0.64% by mass or less of C, 1.20% by mass or more and 2.50% by mass or less of Si, 0.10% by mass or more and 1.15% by mass or less of Mn, with the balance being Fe and unavoidable impurities, characterized in that the tempering step comprises tempering the steel material at 460°C to 490°C for 5 to 30 seconds using a high-frequency induction heating device, to form row-shaped fine carbides in which fine carbides are aggregated in a band shape.

[0039] In the quenching process, the material is heated to the austenite region above the Ac3 point. Once heated to the austenite region, it is held for a time sufficient for the structure to transform into austenite. The quenching process is preferably carried out by heating to a temperature of 850°C to 950°C using a high-frequency induction heating device or the like for 5 to 30 seconds. The material is then rapidly cooled from the austenite region to produce martensite.

[0040] In the quenching process, any cooling method can be used as long as it can transform austenite into martensite. For example, the steel material heated to the austenite region can be immersed in oil or water, or can be rapidly cooled by spraying water mist onto the steel material.

[0041] The tempering process involves heating to 460°C to 490°C for 5 to 30 seconds using a high-frequency induction heating device, followed by rapid cooling. By rapidly heating to 460°C to 490°C for 5 to 30 seconds using a high-frequency induction heating device, followed by subsequent rapid cooling, band-like linear fine carbides are formed in which fine carbides aggregate, improving the toughness of the steel material. The tempering process preferably involves rapid heating to 460°C to 490°C at a rate of 50°C / second to 100°C / second. Rapid cooling can also be achieved by, for example, immersing the steel material in oil or water, or by spraying water mist onto the steel material.

[0042] As described above, the steel material according to the present invention has high hardness and high toughness, and therefore has excellent fatigue strength and delayed fracture resistance in the atmosphere and in corrosive environments. The steel material according to the present invention can be suitably used for spring applications, such as automotive suspension springs, valve springs, clutch damper springs, disc springs, stabilizer springs, and torsion bars.

[0043] Example 1 A steel material (SUP7) containing 0.56% by mass or more and 0.64% by mass or less of C, 1.80% by mass or more and 2.20% by mass or less of Si, and 0.70% by mass or more and 1.00% by mass or less of Mn was used, and the steel material was heated to a quenching temperature of 1000°C for 1.5 seconds using a high-frequency heating device, and then placed in a water tank and cooled. Thereafter, the steel material was rapidly heated to a temperature of 460°C to 490°C at a rate of 51°C / second using the high-frequency heating device, and tempered by heating at a temperature of 460°C to 490°C for 10 seconds, and then placed in a water tank and rapidly cooled to produce a steel material.

[0044] Example 2 The same steel material (SUP7) as in Example 1 was used, and was heated to a quenching temperature of 840°C for 8 seconds using a high-frequency heating device, then placed in a water tank and cooled. Thereafter, the steel material was rapidly heated to a temperature of 470°C at a rate of 51°C / second using a high-frequency heating device, and tempered by heating at a temperature of 470°C for 8 seconds, and then placed in a water tank and rapidly cooled to produce a steel material.

[0045] Example 3 A steel material (SAE9254) containing 0.51% by mass or more and 0.59% by mass or less of C, 1.20% by mass or more and 1.60% by mass or less of Si, 0.60% by mass or more and 0.90% by mass or less of Mn, and 0.60% by mass or more and 0.90% by mass or less of Cr was used, and the steel material was heated to a quenching temperature of 1000°C for 1.5 seconds using a high-frequency heating device, and then placed in a water bath for cooling. Thereafter, the steel material was rapidly heated to a temperature of 460°C to 490°C at a rate of 51°C / second using a high-frequency heating device, and tempered by heating at a temperature of 460°C to 490°C for 10 seconds, and then placed in a water bath for quenching, thereby producing a steel material.

[0046] Comparative Example 1 The same steel material (SUP7) as in Example 1 was used, and was heated at a quenching temperature of 950°C for 1 minute using a high-frequency heating device, then placed in a water tank for cooling. Thereafter, the steel material was heated to a temperature of 400°C at a rate of 0.2°C / second in a furnace, heated at a temperature of 400°C for 1800 seconds, and then placed in a water tank for quenching, thereby producing a steel material.

[0047] Comparative Example 2 The same steel material (SAE9254) as in Example 3 was used, and was heated to a quenching temperature of 840°C for 8 seconds using a high-frequency heating device, then placed in a water tank for cooling. Thereafter, the steel material was rapidly heated to a temperature of 420°C at a rate of 51°C / second using the high-frequency heating device, heated at a temperature of 420°C for 7 seconds, and then placed in a water tank for rapid cooling, thereby producing a steel material.

[0048] (Evaluation Method) - Linear Fine Carbides - The structures of the steel materials of Examples 1 to 3 and Comparative Examples 1 and 2 were observed at 50,000 to 200,000 magnifications using a transmission electron microscope (field emission transmission microscope, TALOS F200X, manufactured by Japan FI Co., Ltd.) to observe whether or not they contained linear fine carbides in which fine carbides aggregated in a band shape. - Charpy Impact Strength - The Charpy impact value was measured using a 10 x 5 x 55 mm, U-notch (2 mm deep) test piece in accordance with the Charpy impact test method for metallic materials specified in JIS Z 2241. - Vickers Hardness - The Vickers hardness was measured in accordance with the Vickers hardness test method specified in JIS Z 2244. - Tensile Strength - The tensile strength was measured in accordance with the method specified in JIS Z 2241. Note that for some test specimens (marked with an asterisk in the table), the values ​​are estimated by converting the actual measured values ​​using the following regression formula: Tensile strength (MPa) = 4.3378 x (Vickers hardness (HV) - 560.06)

[0049]

[0050] As shown in Table 1, in Examples 1 to 3, which were rapidly heated to 460°C to 490°C using a high-frequency heating device and then tempered, linear fine carbides, in which fine carbides aggregated in bands, were observed, and the Charpy impact value was also high, i.e., it was confirmed that the steel had high toughness. On the other hand, in Comparative Example 1, which was tempered in a furnace, and Comparative Example 2, which was rapidly heated to 420°C using a high-frequency heating device and then tempered, no linear fine carbides were observed, and it was confirmed that the Charpy impact value was low.

Claims

1. A steel material containing 0.39% by mass or more and 0.64% by mass or less of C, 1.20% by mass or more and 2.50% by mass or less of Si, 0.10% by mass or more and 1.15% by mass or less of Mn, with the remainder being Fe and unavoidable impurities, characterized in that the steel material has row-shaped fine carbides in which fine carbides are aggregated in band shapes.

2. The steel material according to claim 1, wherein the fine carbides have a length of 1 nm or more and 100 nm or less, and the row-shaped fine carbides have a length of 100 nm or more and 50 μm or less.

3. The steel material according to claim 1, wherein the linear fine carbides are formed so as to cross a lath interface, which is the smallest unit constituting a prior austenite grain boundary.

4. Charpy impact value is 60 J / cm 2 The steel material according to claim 1 .

5. The steel material according to claim 1, containing Cr in the range of 0.10 mass% to 1.10 mass%, P in the range of 0.025 mass% or less, and S in the range of 0.025 mass% or less.

6. The steel material according to claim 1, containing Cu in an amount of 0.15 mass% or more and 0.40 mass% or less, and Ni in an amount of 0.15 mass% or more and 0.70 mass% or less.

7. The steel material according to claim 1, containing Ti in an amount of 0.05 mass% or more and 0.11 mass% or less.

8. The steel material according to claim 1, containing V in an amount of 0.10 mass% or more and 0.20 mass% or less.

9. A method for manufacturing a steel material, comprising quenching and tempering a steel material containing 0.39% by mass or more and 0.64% by mass or less of C, 1.20% by mass or more and 2.50% by mass or less of Si, 0.10% by mass or more and 1.15% by mass or less of Mn, with the balance being Fe and unavoidable impurities, characterized in that the tempering process involves tempering the steel material at 460°C to 490°C for 5 to 30 seconds using a high-frequency heating induction device, to form fine carbides in the form of bands.

Citation Information

Patent Citations

  • High strength cold formed spring steel wire and its production method

    JP2004143482A

  • High strength spring steel wire with excellent coiling property and hydrogen embrittlement resistance and manufacturing method thereof

    JP2014005532A