multifilament
By optimizing the fineness and entanglement of multifilaments through a two-stage entangling process, the multifilament achieves a marshmallow powder touch, addressing the limitations of existing technologies in achieving a soft and chewy texture.
Patent Information
- Application Number
- PCT/JP2024/011485
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Existing multifilaments fail to achieve a marshmallow powder touch due to limitations in fineness and entanglement, resulting in a smooth but not chewy texture, as finer yarns become too soft and lose elasticity, and high entanglement leads to a paper-like texture.
A multifilament with a single filament fineness of 0.8 dtex or less and a controlled degree of entanglement, measured by specific CF values, achieved through a two-stage entangling process using different nozzles and pneumatic pressures to create a uniform, soft, and chewy texture.
The resulting multifilament achieves a marshmallow powder touch by optimizing fineness and entanglement, providing a soft, smooth, and chewy fabric texture that surpasses the peach skin feel.
Smart Images

Figure JP2024011485_03102024_PF_FP_ABST
Abstract
Description
Multifilament
[0001] The present invention relates to a multifilament having a small single yarn fineness.
[0002] A fabric called "peach touch" combines the softness of fine single yarns with a pleasant feel due to the fine surface irregularities, and development is underway in both the raw yarn and advanced processing. However, consumer needs for stockings, innerwear, and sportswear demand even greater comfort and ease of wear, and there is a desire to pursue a fabric with a marshmallow powder touch that goes beyond peach touch. To achieve this, design studies are underway on the multifilament that will form the basis of the fabric.
[0003] For example, Patent Document 1 discloses a technology for producing a single-yarn ultrafine fiber having a single-yarn fineness of 0.1 to 0.5 dtex and an average number of fluffs of 1.0 or less per 12,000 m in the longitudinal direction, and for providing a polyamide ultrafine multifilament that can impart excellent softness, smoothness, drapeability, high water absorbency, high density, and high quality after dyeing to woven and knitted fabrics.
[0004] Patent Document 2 discloses a technology for providing a multifilament that has a total fineness of 6 to 18 dtex, a single yarn fineness of 0.8 dtex or less, and a degree of entanglement of 25 or more, thereby enabling the production of a thin woven fabric that is excellent in the convergence of filaments during molding, is light, has a good wearing feel, fits well, and has reduced breathability.
[0005] Patent Document 3 discloses a technology for providing a nylon mixed-fiber entangled yarn that has a spun-like texture, is excellent in lightness, has sufficient firmness, and also has appropriate stretch performance and can be imparted with excellent water repellency, by mixed-fiber entanglement of a nylon yarn having a single filament fineness of 0.55 to 2.0 dtex and a nylon crimped yarn having a single filament fineness of 0.3 to 1.0 dtex.
[0006] Patent Document 4 discloses a technology in which, in a composite polyamide fiber made of two components with different viscosities, the CF value is 10 or less when the trip tension is total fineness dtex × 0.18 cN / dtex + total fineness dtex / number of filaments, and the CF value measured at 65% of the trip tension is 100 or more, thereby achieving a uniform crimp state and excellent woven quality.
[0007] International Publication No. 2012 / 073737 Japanese Patent Application Laid-Open No. 2009-13511 International Publication No. 2018 / 092737 Japanese Patent Application Laid-Open No. 2018-3190
[0008] However, the multifilaments with small single yarn fineness described in Patent Documents 1 to 3 have a soft and smooth texture like the surface of peach skin (peach skin), but have not been able to achieve a soft, smooth, and chewy texture like marshmallow (marshmallow powder touch).This is because, although softness increases as the single yarn fineness decreases, the texture becomes smooth and paper-like.
[0009] In particular, the polyamide multifilaments described in Patent Documents 1 and 2 did not deviate from the peach skin region and lacked a smooth and bouncy texture. Because the degree of entanglement was low at less than 50 and the number of filaments was also small, when the yarn side form was observed, the bulge of the spread portions and the entanglement length were in a random state.
[0010] The nylon mixed entangled yarn described in Patent Document 3 has a smooth texture. Observation of the yarn side shape revealed that the mixed entangled yarn was made by post-mixing two types of multifilaments, so there was no bulge in the spread parts, the number of entanglements was large, and the yarn was in a strong entangled state. In addition, since the total fineness was relatively large, even if the fineness was reduced to achieve a soft texture, the texture of the fabric was smooth and lacked a bouncy texture because one of the single yarn finenesses was large.
[0011] The side-by-side composite polyamide multifilament described in Patent Document 4 has a smooth texture due to coil crimping, but lacks softness due to the large single yarn fineness, and the texture is far from a marshmallow powder touch.
[0012] The present invention aims to provide an ultrafine multifilament that can achieve a marshmallow powder touch different from conventional peach skin by reducing the single filament fineness and optimizing the entanglement state.
[0013] To achieve the above object, the present invention employs the following configurations: (1) A multifilament having a CF value of 100 to 300 measured by the method described in JIS L1013-2010 8.15 and a single yarn fineness of 0.8 dtex or less. (2) The multifilament described in (1) above, having a CF value of 50 or less measured at a trip tension five times the method described in JIS L1013-2010 8.15. (3) The multifilament described in (1) or (2) above, having a total fineness of 80 dtex or less.
[0014] According to the present invention, it is possible to provide an ultra-fine multifilament that can achieve a marshmallow powder touch in the fabric.
[0015] Fig. 1 is a schematic diagram of an entanglement nozzle of one embodiment for imparting entanglement. Fig. 2 is a schematic diagram of the entangled form of multifilaments obtained using only the entanglement nozzle of Fig. 1. Fig. 3 is a schematic diagram of an entanglement nozzle of one embodiment that can be used when producing the multifilament of the present invention. Fig. 4 is a schematic diagram of the entangled form of multifilaments obtained using the two entanglement nozzles of Fig. 1 and Fig. 3.
[0016] The multifilament of the present invention achieves a soft, smooth, and chewy texture (hereinafter referred to as marshmallow powder touch) by making the single yarn extremely thin, having a single yarn fineness of 0.8 dtex or less, and by making the spread portions have a uniform entangled state in which the entanglement spacing is uniform when the longitudinal shape is observed under no tension, as shown in FIG. 4 as an example.
[0017] The single yarn fineness of the single yarns constituting the multifilament of the present invention is 0.8 dtex or less. If the multifilament is assumed to be an elastic body, the soft bending moment is proportional to the fourth power of the single yarn diameter, and therefore a smaller single yarn fineness significantly affects softness. By setting the single yarn fineness to 0.8 dtex or less, a marshmallow powder touch can be obtained when the fabric is made. If the single yarn fineness exceeds 0.8 dtex, the bending rigidity of the multifilament increases, and the marshmallow powder touch cannot be obtained when the fabric is made. As the single yarn fineness decreases, the bending rigidity of the multifilament decreases, and the softness when the fabric is made is significantly exhibited. Therefore, the single yarn fineness is preferably 0.7 dtex or less, more preferably 0.5 dtex or less, and even more preferably 0.3 dtex or less. On the other hand, if the single yarn fineness is too small, spinning stability decreases, single yarn breakage easily occurs when the yarn passes through guides, and warping properties, weaving properties, and quality deteriorate. Therefore, the single yarn fineness is preferably 0.1 dtex or more.
[0018] The CF value in this specification refers to the degree of entanglement. The degree of entanglement is measured using the following entanglement tester with performance equivalent to that described in JIS L1013-2010 8.15. Apparatus: Entanglement Tester R2040 and Electronic Tension Meter R-1192, both manufactured by Zelvekar Overseas. Measurement conditions: Yarn running speed: 2.4 m / min, Reel speed: 17.6 m / min, Reel time: 3.4 seconds, Reel length: 99.7 cm, No. Show: 10 x 10 cm, Full scale: 25 g, Trip tension: Total fineness (tex) x 17.64 mN / tex + Total fineness (tex) x 88.2 mN / tex / Number of filaments, Test counter: 50. Using the measured average intertwined point length (mm), the CF value (degree of entanglement) is calculated as 1000 / average intertwined point length = 1000.
[0019] The multifilament of the present invention has a CF value (hereinafter referred to as CF value (R)) of 100 to 300 measured by the method described in JIS L1013-2010 8.15.
[0020] The CF value (R) is a value measured at the above trip tension and corresponds to the load described in JIS L1013-2010 8.15.
[0021] The entanglement occurs by causing entanglement between the single yarns constituting the multifilament, and the multifilament is composed of entangled portions and unentangled spread portions, as exemplified in Fig. 2 and Fig. 4. The multifilament of the present invention becomes finely entangled by setting the CF value (R) to 100 to 300, and realizes a marshmallow powder touch when made into a fabric. By setting the CF value (R) to 100 or more, the intervals between the entangled portions are short, as shown in Fig. 4, and the spread portions become an entangled form having fine bulges, and the appearance of the multifilament forms fine irregularities, resulting in a smooth powder touch. Furthermore, in combination with the reduction in the single yarn fineness, a marshmallow powder touch can be realized. When the CF value (R) is less than 100, as shown in Fig. 2 , the spacing between the entangled parts and the bulge of the spread parts become non-uniform, making it difficult to obtain a powdery feel, and the feeling does not deviate from the region of peach skin achieved by ultra-thinning the single yarn fineness, and the smooth and bouncy feel is lacking.
[0022] For example, the multifilaments having a single yarn fineness of 0.8 dtex or less described in Patent Documents 1 and 2 are imparted with only a degree of entanglement that is sufficient to prevent deterioration of weaving properties, and are not finely entangled as defined in this specification.
[0023] In the 11 dtex 16 filament multifilament described in the examples of Patent Document 2, the CF value (R) was 34, and even in the 8 dtex 16 filament multifilament, the CF value (R) was a low degree of entanglement of about 41. With this, the number of convergence points was small, the swelling of the spread portions was nonuniform, the number of spread portions was also small, and although a soft hand could be obtained, a smooth powdery touch could not be obtained.
[0024] The larger the CF value (R), the better the feel of a fabric due to fine unevenness can be obtained, and therefore the CF value (R) is preferably 180 or more. If the CF value (R) exceeds 300, the spread parts appear to disappear and the bouncy feel is lost when the side form of the yarn is observed under no tension, although this is not shown in the figure. The CF value is preferably 250 or less.
[0025] The multifilament of the present invention preferably has a CF value (hereinafter referred to as CF value (S)) of 50 or less, measured at a trip tension five times that of the method described in JIS L1013-2010 8.15.
[0026] The CF value (S) referred to here is a value measured using an entanglement tester described in JIS L1013-2010 8.15 Degree of entanglement, with the trip tension set to five times the trip tension used in measuring the CF value (R), and since the measurement is performed at a higher load than the CF value (R), the CF value (S) measures the number of entanglements with a higher entanglement strength than the number of entanglements measured with the CF value (R). Therefore, it can be said that a multifilament with a small CF value (S) is a multifilament having entanglements with a low entanglement strength.
[0027] In multifilaments, increasing the CF value (R) increases the number of convergence points and creates many fine loops, making it possible to create a smooth, powdery texture due to the fine irregularities that result when the fabric is made. However, if the intertwining strength is excessively high, the filaments in the non-converging portions that create the loops will adhere to each other, preventing the formation of loops on the surface of the yarn, resulting in a slippery fabric. Therefore, in order to create fine loops, the preferred CF value (S) is 35 or less. The lower limit of the CF value (S) is not particularly limited, but is, for example, 3 or more.
[0028] A method of achieving the desired entangled state is to set the compressed air pressure during entanglement higher than normal.
[0029] However, since the single yarns constituting the multifilament of the present invention are ultrafine filaments with a single yarn fineness of 0.8 dtex or less, high compressed air pressure excessively damages the yarns, causing deterioration in quality and physical properties such as fuzz and reduction in strength and elongation. Furthermore, simply increasing the compressed air pressure during entanglement results in a strong entanglement state as illustrated in Fig. 2, the swelling of the spread portions is likely to be lost, and the CF value (S) increases.
[0030] Therefore, the inventors have earnestly studied various types of entangling nozzles and combinations thereof, compressed air pressure, entangled locations, and the like, in order to achieve an entangled state in which the swelling of the spread portions and the entanglement spacing are uniform, as illustrated in FIG. 4 , when the side surface form of the yarn is observed under no tension, without giving excessive damage to the yarn.
[0031] As a result, by combining different entanglement methods in two stages using compressed air pressure that does not cause excessive damage to the yarn, it was possible to obtain a high CF value (R) and a low CF value (S) by applying strong convergence and then unwinding the convergence.
[0032] In the first stage of entanglement, a high compressed air pressure of 0.15 MPa or more is applied to impart strong convergence. Preferably, compressed air is injected from two injection holes at a V-angle toward the yarn, as shown in Figure 1, to restrain the yarn and impart entanglement. The entanglement nozzle used here is a two-hole intersecting line parallel flow type (EDV nozzle).
[0033] The entanglement nozzle preferably has a jet hole diameter of 0.8 mm to 1 mm, a jet hole angle between two holes of 100° to 150°, and an inclined jet angle of 0 to 45° relative to the running yarn. The compressed air pressure is preferably 0.15 MPa to 0.35 MPa, and more preferably 0.20 MPa to 0.30 MPa. When controlling the degree of entanglement of filaments with a single yarn fineness of 0.8 dtex or less, the yarn tension during entanglement is preferably 0.04 cN / dtex to 0.30 cN / dtex, and more preferably 0.08 cN / dtex to 0.20 cN / dtex. This first-stage entanglement results in a yarn with a clearly defined convergence point and a non-convergence point, as in the conventional method, and with a CF value (R) and a CF value (S) of approximately 20 to 30, as shown in Figure 2.
[0034] Next, in the second stage of entanglement, a weak compressed air pressure of 0.30 MPa or less is applied to unwind the strong entanglement imparted in the first entanglement and impart new entanglement with weaker convergence. Therefore, as shown in Figure 3, it is preferable to impart entanglement using an entanglement nozzle of a single-hole inclined flow type (PolyJet nozzle), which injects compressed air from a single injection hole and can generate turbulent flow without strongly constraining the yarn within the nozzle. More preferably, an entanglement nozzle with an injection hole diameter of 0.8 mm to 1.5 mm and an inclined injection angle of 0 to 45° is used. Furthermore, the compressed air pressure is preferably 0.10 MPa to 0.30 MPa, more preferably 0.10 MPa to 0.25 MPa, and particularly preferably 0.15 MPa to 0.20 MPa. When controlling the degree of entanglement of filaments having a single yarn fineness within the above range, the yarn tension during entanglement is preferably 0.04 cN / dtex to 0.30 cN / dtex, and particularly preferably 0.08 cN / dtex to 0.20 cN / dtex.
[0035] By combining different entanglement methods in two stages, an entanglement form having many fine loops and a CF value (R) of 100 or more and a CF value (S) of 50 or less can be obtained, as shown in Figure 4.
[0036] The total fineness of the multifilament of the present invention may be any fineness commonly used for clothing applications, and is preferably 80 dtex or less, since the thickness of the fabric made into a woven material is small and the fabric is soft. It is more preferably 33 dtex or less. The total fineness of the multifilament is not particularly limited, but is, for example, 6 dtex or more.
[0037] The strength and elongation of the multifilament of the present invention may be those normally used for clothing applications, and preferably the elongation is 30% to 60% and the strength is 2.5 cN / dtex to 7.0 cN / dtex.
[0038] The cross-sectional shape of the single yarns constituting the multifilament of the present invention can be any shape depending on the individual required properties for inner and outer applications, such as gloss, water absorbency, and low breathability, and may be irregular cross sections other than circular, such as trilobal, pentalobular, octalobular, flat, T-shaped, cross-shaped, X-shaped, Y-shaped, and star-shaped.
[0039] The polymer constituting the multifilament of the present invention is not particularly limited, but is preferably a thermoplastic polymer such as polyamide, polyester, polyolefin, etc. In particular, since the multifilament is required to have low bending rigidity, polyamide is more preferred.
[0040] The polyamide is a high molecular weight compound in which so-called hydrocarbon groups are linked to the main chain via amide bonds, and is preferably a polyamide such as polycaproamide or polyhexamethylene adipamide. The polymer may also be polyamide 510 or polyamide 610, which are produced by polymerizing non-petroleum raw materials such as sebacic acid or pentamethylenediamine. The degree of polymerization of the polyamide may be appropriately selected taking into consideration the required thread strength, initial tensile resistance, etc., but a relative viscosity in 98% sulfuric acid of 2.0 to 3.5 is preferred.
[0041] The polyester is preferably a polyester composed of 90 mol% or more of ethylene terephthalate repeating units, with terephthalic acid as the primary acid component and ethylene glycol as the primary glycol component. It may also contain less than 10 mol% of a copolymerizable component capable of forming other ester bonds. Examples of copolymerizable components include, but are not limited to, dicarboxylic acids such as isophthalic acid, cyclohexanedicarboxylic acid, adipic acid, and dimer acid as acid components, and glycol components such as ethylene glycol, diethylene glycol, butanediol, neopentyl glycol, cyclohexanedimethanol, polyethylene glycol, and polypropylene glycol. The degree of polymerization of the polyester may be selected appropriately taking into account the required thread strength, initial tensile resistance, etc., but the intrinsic viscosity is preferably in the range of 0.51 to 1.0.
[0042] Furthermore, with environmental issues receiving increasing attention, the use of plant-derived biopolymers and recycled polymers in the present invention is also preferable from the viewpoint of reducing the environmental load, and recycled polymers that have been recycled by any of chemical recycling, material recycling, and thermal recycling methods can be used as the above-mentioned polymers.
[0043] Furthermore, light stabilizers, heat stabilizers, antioxidants, antistatic agents, terminal group regulators, dyeability improvers, etc. may be added as needed. It is also possible to add inorganic particles or organic functional agents to impart UV absorption, a cool feel to the touch, antibacterial properties, etc. However, the addition of inorganic particles with a particle size exceeding 1 μm is not preferred because it reduces spinnability and durability. The amount of inorganic particles, including white pigments, added is not limited, but is preferably 2.0% by mass or less, and more preferably less than 1.0% by mass, of the multifilament.
[0044] The multifilament of the present invention can be obtained by melt spinning a single component. Alternatively, a composite cross-section filament having a hardly soluble polymer as a core or island component and an easily soluble polymer as a sheath or sea component can be knitted or woven using a composite spinning machine, and then the core or island component can be eluted with a chemical to obtain an ultrafine multifilament fabric. However, the elution process of the easily soluble polymer tends to result in a low-density fabric, making it difficult to achieve a bouncy texture. Furthermore, since it is difficult to achieve the desired entanglement pattern (intertwining is difficult) at the composite cross-section filament stage, it is difficult to achieve a marshmallow powder texture.
[0045] It is also possible to make a fabric using ultrafine multifilaments having a single yarn fineness of 0.8 dtex or less, for example, a blend of two types of ultrafine multifilaments. However, blended ultrafine multifilaments of two types tend to fall apart, making it difficult to achieve the desired entanglement pattern, and therefore making it difficult to achieve a marshmallow powder touch.
[0046] Furthermore, in the two-step method in which spinning and drawing are carried out in separate steps, the filaments in the non-converging portions that generate loops become closely attached to each other due to the introduction of actual twist into the multifilament yarn, and therefore, loops are not formed on the surface of the yarn, resulting in a smooth fabric when made into a fabric. Therefore, it is preferable to manufacture the fabric by direct spinning, in which the process from spinning to winding is carried out in one step.
[0047] A more preferred high-speed direct spinning and drawing method for obtaining the multifilament of the present invention in a single step is exemplified below. A thermoplastic polymer is melted, metered and transported by a gear pump, and discharged from a spinneret. The thread is cooled to room temperature by blowing cooling air onto it using a thread cooling device such as a chimney, oiled and concentrated using an oiling device, imparted with a first-stage entanglement, passed through a take-up roller and a drawing roller, and drawn according to the ratio of the peripheral speeds of the take-up roller and the drawing roller. After drawing, the thread is imparted with a second stage of entanglement, and then wound on a winder (winding device), thereby producing a multifilament.
[0048] In order to obtain the multifilament of the present invention with uniform strength and elongation, it is preferable to use a so-called annular cooling device in which a molten polymer is discharged from a spinneret having annularly arranged discharge holes, and cooling air is blown in radial directions from the center of the spinneret or from the circumferential direction toward the spinneret center so as to surround the spinneret discharge holes. The cooling start distance is preferably a relatively short distance of 10 mm to 100 mm from the spinneret surface. The cooling length is preferably 100 mm to 1000 mm.
[0049] Oiling is carried out after cooling. Spinning oil is applied to the multifilament by guide oiling or the like, and the amount of active ingredient attached at the time of winding is preferably 0.4% by weight to 1.0% by weight per weight of the multifilament. The application of oil may be carried out once or multiple times during the spinning process. When applied multiple times, it is preferable to apply an oil with a low amount of active ingredient first, and then apply an oil with a high amount of active ingredient. As the oil, a lubricant, an antistatic agent, an emulsifier, an additive, etc. are mixed and dispersed and used.
[0050] After oiling, a first stage of entanglement is imparted before drawing. In order to prevent the single yarns from separating during drawing and causing variations in elongation, the first stage of entanglement is preferably carried out before drawing. A preferred method for imparting the first stage of entanglement is as described above. Furthermore, the second stage of entanglement may be carried out immediately after the first stage of entanglement, but is preferably carried out after drawing. A preferred method for imparting the second stage of entanglement is as described above.
[0051] After the first stage of entanglement, the filament is then taken up by a take-up roller at a speed of 1500 m / min to 4500 m / min. The temperature of the take-up roller is preferably a temperature equal to or higher than the glass transition point specific to the thermoplastic polymer. For polyamides, the temperature is room temperature, approximately 20°C to 30°C, depending on the environmental conditions, and for polyesters, the temperature is approximately 80°C to 100°C. Next, the filament is stretched by approximately 1.0 to 2.5 times depending on the ratio of the peripheral speeds of the take-up roller and the stretching roller. The number of stretching roller stages is not important. Heat treatment is preferably performed by using a heated roller at 130 to 200°C as the final stretching roller. The take-up and stretching rollers may be Nelson rollers, drive rollers with a driven separate roller, or single-sided rollers. The roller surface may be smooth to prevent slippage between the roller and the filament, or may be grooved or matte to improve yarn separation. The filament is then wound up by a take-up roller at a speed of 3000 m / min or higher.
[0052] The present invention will be described in more detail below with reference to examples. Measurement values were obtained by the following methods.
[0053] A. Total fineness, single yarn fineness A yarn sample was wound 400 times on a measuring machine with a frame circumference of 1.125 m to prepare a skein, and after drying in a hot air dryer (105±2°C x 60 minutes), the skein was weighed on a balance and multiplied by the official moisture regain to calculate the fineness. The official moisture regain was set to 4.5% for polyamide and 0% for polyester. The single yarn fineness was calculated by dividing the obtained fineness by the number of filaments.
[0054] B. Strength, elongation, and strength-strain product Measurements were made in accordance with JIS L 1013-2010 8.5 Tensile strength and elongation percentage. Test conditions included a constant-speed tension type testing machine, a grip distance of 50 cm, and a pulling speed of 50 cm / min. If the strength at break was lower than the maximum strength, the maximum strength and the elongation percentage at that time were measured. Strength, strength-strain product, and elongation were calculated using the following formulas: Elongation (%) = elongation percentage at break Strength (cN / dtex) = strength at break (cN) / fineness (dtex) Strength-strain product = strength x (1 + elongation / 100)
[0055] C. CF Value (Degree of Entanglement) Measurement was carried out in accordance with JIS L 1013-2010 8.15 Degree of Entanglement. (a) Equipment: Entanglement Tester R2040 and Electronic Tension Meter R-1192, both manufactured by Zelvekar Overseas. (b) Measurement conditions: Yarn running speed 2.4 m / min, reel speed 17.6 m / min, reel time 3.4 seconds, reel length 99.7 cm, No. Show 10 x 10 cm, full scale 25 g. (c) When measuring CF(R), the trip tension was (total fineness tex x 17.64 mN / tex + total fineness tex x 88.2 mN / tex / number of filaments), and when measuring CF(S), the trip tension was 5 times that of CF(R). (d) When the average length of each intertwined point is taken as the average intertwined point length A (mm), the degree of intertwining = 1000 / A. (e) A weight is suspended and the fiber is run, and the tension indicator is adjusted so that it indicates the initial load. The test counter is set to N = 50, and the average value of the measurement results is taken as the degree of intertwining.
[0056] D. Amount of oil attached (a) 10 g of yarn sample weight (S) is immersed in 70 ml of n-hexane and stirred (20°C, 5 minutes) to extract the oil. (b) The same sample is again immersed in 70 ml of n-hexane and stirred (20°C, 5 minutes) to extract the oil. (c) The n-hexane extracted in (a) and (b) above is transferred to a flask whose weight (W0) has been measured after drying, and the n-hexane is evaporated at 100°C. (d) The sample is further dried in a vacuum dryer (40°C, 10 torr or less, 1 hour). (e) After allowing to cool in a desiccator containing a desiccant, the weight (W1) of the flask is measured. (f) The amount of oil attached is calculated using the following formula: Amount of oil attached (%) = (W1 - W0) / S x 100
[0057] E. Fabric Evaluation The evaluation targets were plain woven fabrics using 100% multifilament warp and weft, and were discussed by four technicians with extensive experience in texture evaluation, and were relatively rated according to the following criteria: (1) Powder Touch ×: Poor (smooth fabric) △: Slightly poor (smooth fabric with some unevenness) 〇: Good (smooth and soft fabric with excellent texture) ◎: Very good (smooth and soft fabric with excellent texture) (2) Softness ×: Poor (fabric with poor softness) △: Slightly poor (fabric with a soft level among woven fabrics) 〇: Good (fabric with excellent softness) ◎: Very good (fabric with excellent softness) (3) Marshmallow Powder Touch Fabrics that were rated ◎ or ○ in (1) above and ◎ or ○ in (2) above were deemed to have a marshmallow powder touch.
[0058] F. Evaluation of Knit Fabrics The evaluation targets were circular knit fabrics using 100% multifilament, which were discussed by four technicians with extensive experience in texture evaluation and relatively rated according to the following criteria: (1) Powder Touch ×: Poor (smooth fabric) △: Slightly poor (smooth fabric with some unevenness) 〇: Good (smooth and soft fabric with excellent texture) ◎: Very good (smooth and soft fabric with excellent texture) (2) Softness ×: Poor (fabric with poor softness) △: Slightly poor (fabric with a soft level among woven fabrics) 〇: Good (fabric with excellent softness) ◎: Very good (fabric with excellent softness) (3) Marshmallow Powder Touch Fabrics that were rated ◎ or ○ in (1) above and ◎ or ○ in (2) above were deemed to have a marshmallow powder touch.
[0059] Example 1: Titanium oxide-free polycaproamide chips (N6) with a relative viscosity of 2.8 in 98% sulfuric acid were melted at 285°C and extruded through circular nozzles arranged in a circular pattern in a spinneret. After extrusion, the yarn was cooled using an inward-blowing circular cooling device (cooling start distance from the nozzle face: 31 mm, cooling length: 300 mm) that blows cooling air inward from a cylindrical filter. Then, 0.32 ml / min of oil was extruded from an oiling guide to oil the multifilament. After oiling, a first stage of entanglement was carried out. Using a two-hole, cross-line parallel flow type entanglement nozzle (injection hole diameter: 0.9 mm, injection hole angle between the two holes: 120°, inclined injection angle: 0°) as illustrated in Figure 1, entanglement was imparted at a compressed air pressure of 0.25 MPa. After the first stage of entanglement, the fiber was taken up by passing it over the first godet roller. It was then stretched between the first godet roller and the second godet roller to an elongation of 45%, and then heat-treated by passing it over the second godet roller heated to 155°C. After the stretching and heat treatment, the second stage of entanglement was carried out. Using a single-hole inclined flow entanglement nozzle (injection hole diameter 1.2 mm, inclined injection angle 0°) as shown in Figure 3, the first stage of entanglement was unwound and new entanglement was imparted at a compressed air pressure of 0.17 MPa. After the second stage of entanglement, the fiber was wound up at 4500 m / min to obtain a polyamide multifilament of 22 dtex and 108 filaments (strength 5.8 cN / dtex, CF value (R) 182). The evaluation results of the obtained polyamide multifilament are shown in Table 1.
[0060] When the yarn side morphology was observed under no tension, the bulge of the spread portions and the entanglement spacing were uniform, as shown in Figure 4. The texture of the obtained woven and knitted fabrics was soft, smooth, and bouncy, with a marshmallow powder touch that was even better than a peach touch.
[0061] [Example 2] Polyethylene terephthalate with an intrinsic viscosity of 0.64 and containing 0.3% by mass of titanium oxide was melted at 300°C, discharged from a circular discharge hole arranged in a spinneret, and cooled using an inward-blowing annular cooling device that blows cooling air inward from a cylindrical filter. The multifilament was then oiled by discharging an oil solution at 0.32 ml / min from an oil supply guide. Subsequently, a first stage of entanglement was imparted using compressed air pressure of 0.25 MPa, followed by take-up. Subsequently, the multifilament was stretched to an elongation of 45%, heat-treated at 110°C, and then imparted with a second stage of entanglement using compressed air pressure of 0.17 MPa. The multifilament was then wound up at 4,500 m / min to obtain a polyester multifilament. The evaluation results of the resulting polyester multifilament are shown in Table 1.
[0062] [Example 3] A polyamide multifilament having 22 dtex and 108 filaments was obtained by increasing the compressed air pressure in the first stage to 0.40 MPa based on the spinning method in Example 1. The evaluation results of the obtained polyamide multifilament are shown in Table 1.
[0063] [Example 4] A polyamide multifilament having 22 dtex and 108 filaments was obtained by reducing the compressed air pressure in the first stage to 0.15 MPa based on the spinning method in Example 1. The evaluation results of the obtained polyamide multifilament are shown in Table 1.
[0064] [Example 5] A polyamide multifilament having 22 dtex and 108 filaments was obtained by increasing the compressed air pressure in the second stage to 0.30 MPa based on the spinning method in Example 1. The evaluation results of the obtained polyamide multifilament are shown in Table 1.
[0065] [Example 6] A polyamide multifilament of 44 dtex and 200 filaments was obtained by increasing the total fineness to 44 dtex and the filament count to 200 based on the spinning method in Example 1. The evaluation results of the obtained polyamide multifilament are shown in Table 1.
[0066] [Example 7] A polyamide multifilament of 100 dtex and 500 filaments was obtained by increasing the total fineness to 100 dtex and the filament count to 500 based on the spinning method of Example 1. The evaluation results of the obtained polyamide multifilament are shown in Table 1.
[0067] [Example 8] A polyamide multifilament of 22 dtex x 55 filaments was obtained by increasing the single yarn fineness to 0.4 dtex and decreasing the filament count to 55 based on the spinning method of Example 1. The evaluation results of the obtained polyamide multifilament are shown in Table 1.
[0068] [Example 9] A polyamide multifilament of 22 dtex x 28 filaments was obtained by increasing the single yarn fineness to 0.8 dtex and decreasing the filament count to 28 based on the spinning method of Example 1. The evaluation results of the obtained polyamide multifilament are shown in Table 1.
[0069] [Example 10] A polyamide multifilament of 22 dtex x 31 filaments was obtained by increasing the single yarn fineness to 0.7 dtex and decreasing the filament count to 31 based on the spinning method in Example 1. The evaluation results of the obtained polyamide multifilament are shown in Table 1.
[0070] [Example 11] A chemically recycled polyamide multifilament having 22 dtex and 108 filaments was obtained by spinning in the same manner as in Example 1, except that chemically recycled polycaproamide chips (N6) containing no titanium oxide and having a relative viscosity of 2.8 in 98% sulfuric acid were used. The evaluation results of the obtained chemically recycled polyamide multifilament are shown in Table 1.
[0071]
[0072] [Comparative Example 1] A polyester multifilament of 22 dtex and 108 filaments was obtained by entangling only in the second stage without entangling in the first stage based on the spinning method in Example 2. The evaluation results of the obtained polyester multifilament are shown in Table 2.
[0073] Because a general entanglement treatment was performed, when the yarn side surface morphology was observed under no tension, the spacing between entangled parts and the bulge of the spread parts were non-uniform, as shown in Figure 2 , and the texture of the obtained woven and knitted fabrics was soft but smooth and paper-like.
[0074] [Comparative Example 2] A polyamide multifilament of 22 dtex and 108 filaments was obtained by entangling only in the first stage without performing the second stage entanglement, based on the spinning method of Example 1. The evaluation results of the obtained polyamide multifilament are shown in Table 2.
[0075] Because a general entanglement treatment was performed, when the yarn side surface morphology was observed under no tension, the entanglement morphology was such that the spacing between entangled parts and the bulge of the spread parts were non-uniform, as shown in Figure 2 , and the texture of the obtained woven and knitted fabrics was smooth and paper-like, although it had the softness characteristic of polyamide.
[0076] Comparative Example 3 A polyamide multifilament having 22 dtex and 108 filaments was obtained by changing the second-stage entanglement nozzle to the same entanglement nozzle as the first-stage entanglement nozzle based on the spinning method in Example 1. The evaluation results of the obtained polyamide multifilament are shown in Table 2.
[0077] Because the same type of entangling nozzle was used in both the first and second stages of entangling, when the yarn side surface morphology was observed under no tension, the entangled morphology was uneven in the spacing between entangled parts and the bulge of the spread parts, as shown in Figure 2, and the texture of the obtained woven and knitted fabrics was smooth and paper-like, although it had the softness characteristic of polyamide.
[0078] Comparative Example 4 A polyamide multifilament having 22 dtex and 108 filaments was obtained by reducing the compressed air pressure in the second stage to 0.08 MPa based on the spinning method in Example 1. The evaluation results of the obtained polyamide multifilament are shown in Table 2.
[0079] When the yarn side surface morphology was observed under no tension, the spacing between the entangled parts and the swelling of the spread parts were non-uniform, as shown in Figure 2. This was because the air pressure in the second stage was low, and the strong convergence imparted in the first stage of entanglement could not be unraveled. As a result, the hand of the obtained woven and knitted fabrics was soft but smooth and paper-like.
[0080] Comparative Example 5 A polyamide multifilament of 22 dtex x 22 filaments was obtained by increasing the single yarn fineness to 1.0 dtex and decreasing the filament count to 22 based on the spinning method of Example 1. The evaluation results of the obtained polyamide multifilament are shown in Table 2.
[0081] When the yarn side morphology was observed under no tension, the bulge of the spread portion and the entanglement spacing were uniform, as shown in Figure 4. However, although this was in the single yarn fineness range that is generally considered to be soft, the bending rigidity increased slightly, so no synergistic effect was produced, and the marshmallow powder touch was not achieved.
[0082] Comparative Example 6 A polyamide multifilament having 22 dtex and 108 filaments was obtained by increasing the compressed air pressure in the first stage to 0.40 MPa and the compressed air pressure in the second stage to 0.30 MPa based on the spinning method in Example 1. The evaluation results of the obtained polyamide multifilament are shown in Table 2.
[0083] When the yarn side morphology was observed under no tension, the bulge in the spread portions apparently disappeared and the yarn was in an entangled state. This was because the balance between the compressed air pressure in the first stage and the compressed air pressure in the second stage was poor, and the very strong convergence imparted in the first stage entanglement could not be completely unraveled. As a result, the texture of the obtained woven and knitted fabrics was smooth and paper-like.
[0084]
[0085] Although the present invention has been described in detail with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2023-54724) filed on March 30, 2023, the entirety of which is incorporated by reference.
Claims
1. A multifilament having a CF value of 100 to 300 measured by the method described in JIS L1013-2010 8.15 and a single yarn fineness of 0.8 dtex or less.
2. The multifilament according to claim 1, which has a CF value of 50 or less measured at a trip tension 5 times that of the method described in JIS L1013-2010 8.
15.
3. A multifilament according to claim 1 or 2, having a total fineness of 80 dtex or less.
Citation Information
Patent Citations
JP1981173672U
Method for manufacture yarn at high speed
JP1986028010A
Polyester false-twist textured yarn and woven knitted fabric made of the yarn
JP2002020935A
Polyamide fiber and fabric made thereof
JP2017155348A
Polyester false twist yarn
JP2019094595A