Touch sensor, touch panel, method for manufacturing touch sensor, and method for manufacturing touch panel
The touch sensor's adhesive layer with viscoelastic properties and uneven surface shape addresses air bubble issues, improving sensitivity and attachment reliability by effectively discharging air and reducing foreign matter adhesion.
Patent Information
- Application Number
- PCT/JP2024/011507
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Air bubbles often remain between the adherend and the touch sensor during attachment, affecting the sensitivity and reliability of touch panels.
A touch sensor with a base material and an adhesive layer, where the adhesive layer has a crosslinked cured product with viscoelastic properties and an uneven surface shape, allowing it to follow the sensor circuit and discharge air effectively, reducing adhesion to foreign matter and improving sensitivity.
The solution effectively suppresses air bubbles between the adherend and the touch sensor, enhancing sensitivity and reducing foreign matter adhesion, while allowing for easy attachment and improved manufacturing efficiency.
Smart Images

Figure JP2024011507_03102024_PF_FP_ABST
Abstract
Description
Touch sensor, touch panel, method of manufacturing touch sensor, and method of manufacturing touch panel
[0001] The disclosure of the present application relates to a touch sensor, a touch panel, a method for manufacturing a touch sensor, and a method for manufacturing a touch panel.
[0002] A touch panel is known as one of input devices for electronic devices (see, for example, Patent Document 1). A touch panel is an operation panel located on the outer surface of an electronic device, and an operator inputs by approaching or touching the operation panel. A touch sensor detects the operator's input to the operation panel.
[0003] JP 2016-081818 A, FIG. 1
[0004] A touch panel is created by attaching a touch sensor to a support member such as an operation panel. However, when attaching the touch sensor to the support member, air bubbles can get trapped between the support member and the touch sensor, which can be a problem.
[0005] An object of the present disclosure is to provide a technique that can suppress air remaining between an adherend and a touch sensor.
[0006] Some aspects disclosed in this application are configured to have the following characteristics.
[0007] That is, one aspect of the present disclosure is a touch sensor having a substrate and an adhesive layer, and attached to a support member. A sensor circuit is formed on the substrate. The adhesive layer has a first surface laminated to the substrate. Meanwhile, the adhesive layer has a transfer material on a second surface. The transfer material has convex portions protruding toward the adhesive layer on a surface that contacts the adhesive layer. The adhesive layer further has an uneven shape transferred to the surface that contacts the transfer material by contact with the convex portions. The adhesive layer is attached so that the surface having the uneven shape adheres to the support member when the transfer material is peeled off, and the uneven shape of the surface is maintained. This makes it possible to realize a touch sensor that reduces air remaining between the support member and the touch sensor.
[0008] In one aspect of the present disclosure, the adhesive layer is a crosslinked and cured product of an adhesive coating film. By configuring the adhesive layer laminated on the substrate as an adhesive coating film, it is possible to suppress air remaining between the substrate and the adhesive layer. Furthermore, by configuring the adhesive layer as a crosslinked and cured product of an adhesive coating film, it is possible to easily increase the elasticity of the adhesive layer simply by crosslinking and curing the adhesive coating film. This results in the adhesive layer having viscoelastic properties that combine viscosity and elasticity.
[0009] In one aspect of the present disclosure, the adhesive coating film is formed by covering the sensor circuit directly or via a resist layer. This adhesive coating film allows the adhesive layer to be applied directly or via a resist layer to the surface of a component having an uneven shape, such as a sensor circuit disposed on a substrate. This prevents air from being trapped between the sensor circuit and the adhesive layer. Therefore, this adhesive coating film can improve the sensitivity of the sensor.
[0010] In one aspect of the present disclosure, the adhesive coating film has a laminated surface that conforms to the shape of the sensor circuit directly or via a resist layer. This laminated surface indicates that adhesive layers are stacked to conform to the shape of the sensor circuit directly or via a resist layer. Therefore, when the adhesive coating film has a laminated surface that conforms to the shape of the sensor circuit, it is possible to prevent air from being trapped between the sensor circuit and the adhesive layer. Therefore, this laminated surface can improve the sensitivity of the sensor.
[0011] In one aspect of the present disclosure, the uneven shape is a parallel linear groove shape or an intersecting grid-like groove shape. By configuring the uneven shape of the surface of the adhesive layer to be a parallel linear groove shape or an intersecting grid-like groove shape, it is possible to ensure that the air discharge path from the area where the adhesive layer and the adherend are attached to the outside of the area is connected. Furthermore, by configuring the uneven shape of the surface of the adhesive layer to be a grid-like groove shape, it is possible to form multiple detours as air discharge paths in addition to the shortest route. Therefore, by configuring the surface of the adhesive layer to be a parallel linear groove shape or an intersecting grid-like uneven shape, it is possible to more effectively discharge air from between the adherend and the touch sensor.
[0012] In one aspect of the present disclosure, the crosslinked, cured product has viscoelasticity with a storage modulus E' of 0.1 MPa or more and 2 MPa or less. Here, the storage modulus E' is the component of energy generated by external force and strain on an object that is stored inside the object. This allows the uneven shape on the surface of the adhesive layer to be maintained over time. Therefore, this allows air to be more effectively discharged from between the adherend and the touch sensor.
[0013] In one aspect of the present disclosure, the crosslinked, cured product has a ball tackiness of No. 3 or more and No. 7 or less. This can reduce the stickiness (adhesive strength) of the adhesive layer exposed at the edge of the region where the adhesive layer adheres to the adherend, for example. Therefore, this can suppress the adhesion of foreign matter to the adhesive layer.
[0014] In one aspect of the present disclosure, the attachment member is any one of an operation panel (cover member), an equipment exterior plate (housing case), and an equipment internal plate. This allows the touch sensor to be attached and fixed to any one of the operation panel (cover member), equipment exterior plate (housing case), and equipment internal plate, which are surfaces that constitute the electronic device, and makes it possible to prevent air from remaining between the attachment member and the touch sensor.
[0015] One aspect of the present disclosure is a touch panel having any of the touch sensors attached to the attachment member, thereby realizing a touch panel that suppresses air remaining between the attachment member and the touch sensor.
[0016] One aspect of the present disclosure is a method for manufacturing a touch sensor to be attached to a substrate, the method comprising: applying a liquid adhesive to a substrate having a sensor circuit formed thereon to form an adhesive coating film; crosslinking and curing the adhesive coating film to form an adhesive layer made of a crosslinked and cured product; contacting a transfer material having convex portions protruding toward the adhesive layer with the surface of the adhesive layer to transfer a concave-convex shape to the surface; and, when the transfer material is peeled off and the surface having the concave-convex shape is attached to the substrate so that the concave-convex shape of the surface is maintained. This method makes it possible to realize a method for manufacturing a touch sensor to be attached to a touch panel that reduces air remaining between the substrate and the touch sensor.
[0017] According to one aspect of the present disclosure, there is provided a method for manufacturing a touch panel, which includes attaching any one of the touch sensors to the adherend, leaving the adherend with the touch sensor attached, and maintaining the uneven shape of the surface of the adhesive layer. This method makes it possible to realize a method for manufacturing a touch panel that suppresses air remaining between the adherend and the touch sensor.
[0018] 1 is a plan view of an automobile showing an application example of a touch sensor and a touch panel according to an embodiment; 2 is a plan view showing an appearance of a touch sensor according to an embodiment; 3 is a cross-sectional view of a touch sensor according to an embodiment; 4 is a cross-sectional view illustrating a method for manufacturing a touch sensor according to an embodiment; and 5 is a cross-sectional view illustrating a method for manufacturing a touch panel according to an embodiment.
[0019] A "touch sensor" and a "touch panel" according to one aspect of the present disclosure will be specifically described below. However, the following description is not intended to limit the scope of the present disclosure, but should be understood as a description explaining an exemplary embodiment. The following description does not unduly limit the scope of the claims, and not all of the configurations described in this embodiment are necessarily required as a solution.
[0020] In the following description, terms indicating directions such as "upper," "lower," "left," and "right" are used for convenience of explanation and do not indicate a method or mode of use unless the context clearly specifies that the direction is limited. Terms such as "first" and "nth" following "first" in this specification and claims are used as identifying terms to distinguish different elements and do not indicate a particular order, superiority, or inferiority.
[0021] The terms used in the following description are for the purpose of describing particular embodiments only and are not intended to limit the scope of the present disclosure. Elements according to an aspect described in the present specification and claims are intended to include the plural unless the context clearly dictates otherwise. The term "and / or" refers to and includes any and all possible combinations of one or more of the associated listed elements. The terms "includes," "including," "comprises," and / or "comprising" used in the present specification and claims specify the presence of features, operations, elements, or steps. However, these terms are not intended to exclude the presence or addition of one or more other features, operations, elements, steps, and / or groups thereof.
[0022] The "touch panel" disclosed in this application is an input device operated by an operator's finger or the like to activate a desired function, and is applicable to electronic devices in which the board, housing, container, etc. equipping the input unit are relatively large compared to the input unit. One example of a "touch panel" is an "in-vehicle interior panel," more specifically, an "in-vehicle interior panel containing a touch sensor." As shown in FIG. 1 , various large "in-vehicle interior panels" are installed around the driver's seat 2 and passenger seat 3 of an automobile 1. Examples of "in-vehicle interior panels" and "in-vehicle interior panels containing a touch sensor" include, for example, the center console armrest portion 4, the door armrest portion 5, and the instrument panel 6, as shown in FIG. 1 .
[0023] The operation surface 7 of the "vehicle interior panel" is configured with a cover member 8 serving as an "operation panel." The "touch sensor" disclosed in the present application is attached to, for example, the cover member 8 serving as the operation panel, an equipment exterior plate (housing case), or an equipment interior plate provided within the equipment as an "attachment member." Here, an example of an embodiment of a touch sensor 10 attached to the armrest portion 4 of the center console will be described with reference to the drawings. The touch sensor 10 uses a capacitive method (projected capacitive method) to detect touch operations. However, there is no limitation on the method used for the touch sensor 10, and a resistive film method, an ultrasonic method, or various other methods can be used.
[0024] For convenience, in this specification and claims, the left-right direction of the touch sensor 10 as one embodiment of the "touch sensor" is referred to as the X direction, the front-rear direction as the Y direction, and the height direction (up-down direction) as the Z direction, as shown in Figures 2 and 3, etc. Furthermore, in the armrest portion 4 shown in Figure 5, the side on which the cover member 8 is placed is referred to as the upper side (outside) in the Z direction, and the side on which the touch sensor 10 is arranged is referred to as the lower side (inside) in the Z direction. However, these do not limit the arrangement orientation of the touch sensor 10 and the armrest portion 4, the input operation direction of the touch sensor 10 and the armrest portion 4, etc.
[0025] Configuration of touch sensor 10 (FIGS. 1 to 3)
[0026] 2, 3, etc., the touch sensor 10 has a base film 20 as a "base material" and an adhesive layer 30. The base film 20 is equipped with a sensor element that converts an input operation by an operator into an electrical signal. The base film 20 is in the form of a thin film (film, sheet) that is extremely short (thin) in length (thickness) in the Z direction compared to the X direction and the Y direction.
[0027] The base film 20 has a base body portion 21 and a tail portion 22. The base body portion 21 has a base surface 23 that is aligned with the X direction and the Y direction. In this embodiment, the base surface 23 is one of the two surfaces of the base film 20 on which the adhesive layer 30 is provided. The base surface 23 is rectangular in plan view. The base surface 23 is not limited to a rectangular shape and can be changed to correspond to the shape of the operation surface 7 of the "touch panel" or the like. The tail portion 22 extends outward in a rectangular shape from a portion of the outer periphery of the base surface 23. The tail portion 22 is also not limited to a rectangular shape and can be changed to correspond to the shape of the base surface 23 or the like.
[0028] The base film 20 is made of an insulating material. The base film 20 can be a thin film, sheet, or the like made of resin, synthetic rubber, thermoplastic elastomer, or the like. Examples of resins include thermoplastic resins such as polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polycarbonate (PC), polyamide (PA), acrylic (AC), and polyvinyl chloride (PVC). Examples of synthetic rubbers include urethane rubber, silicone rubber, and fluororubber. Examples of thermoplastic elastomers include urethane-based, olefin-based, styrene-based, polyester-based, silicone-based, and fluorine-based elastomers.
[0029] A sensor circuit 24 is formed on the base film 20. The base film 20 on which the sensor circuit 24 is formed has a function of increasing capacitance when an operating object such as an operator's finger or a stylus pen approaches. The sensor circuit 24 is formed on the base surface 23. The sensor circuit 24 is not limited to being formed on the top surface of the base film 20, which is the base surface 23 in this embodiment, but may also be formed on the bottom surface of the base film 20, which is the surface opposite to the base surface 23.
[0030] The sensor circuit 24 includes electrodes and circuit wiring. The electrodes generate electrical signals in response to the approach of an operating object. The electrodes are arranged corresponding to operation positions on the "touch panel" where an operator performs input operations. The circuit wiring transmits the electrical signals generated by the electrodes to a touch sensor IC (Integrated Circuit). The circuit wiring extends from the electrodes. The circuit wiring is formed on the substrate main body portion 21 and the tail portion 22. The tail portion 22 has a connection portion at its tip that connects to a substrate on which the touch sensor IC is mounted.
[0031] The electrodes, circuit wiring, etc. are formed by printing a conductive material on the base film 20. Formation of the electrodes, circuit wiring, etc. is not limited to printing, and methods such as metal etching may also be used. Metal pastes such as silver or copper, carbon pastes, conductive coatings such as conductive polymers, conductive metal foils, metal meshes, etc. can be used for the electrodes, circuit wiring, etc. Furthermore, pastes containing conductive nanoparticles such as PEDOT / PSS (Poly(3,4-EthyleneDiOxyThiophene) / PolyStyrene Sulfonate (a dispersion of polyethylenedioxythiophene and polystyrene sulfonate)), ITO (Indium Tin Oxide), nanoscale fine conductive powders, and fine conductive fibers can be used for the electrodes, circuit wiring, etc. Thin films or pastes of PEDOT / PSS or ITO, or transparent conductive films using pastes containing conductive nanoparticles, are translucent and allow backlight illumination to pass through.
[0032] The conductive layer that constitutes the sensor circuit 24 can also be configured to be covered with an electrically insulating resist layer.
[0033] The adhesive layer 30 functions to prevent air from remaining between the cover member 8 and the touch sensor 10. The adhesive layer 30 is a thin film having an extremely short (thin) length (thickness) in the Z direction compared to the X and Y directions. The length of the adhesive layer 30 in the Z direction is, for example, 10 μm or more and 500 μm or less, preferably 20 μm or more and 50 μm or less. The adhesive layer 30 is rectangular in plan view. The adhesive layer 30 is not limited to a rectangular shape and can be modified depending on the shape of the "touch panel" and the base surface 23. The adhesive layer 30 has an inner surface 31 as a "first surface" and an outer surface 32 as a "second surface." The inner surface 31 is located on the lower side in the Z direction, while the outer surface 32 is located on the upper side in the Z direction. The inner surface 31 of the adhesive layer 30 is laminated on the base film 20. On the other hand, the adhesive layer 30 has a release sheet 33 (mold release sheet) on the outer surface 32 as a "transfer material."
[0034] The release sheet 33 functions to protect the adhesive layer 30. In addition, the release sheet 33 functions to form an uneven shape on the adhesive layer 30. The release sheet 33 is a thin film whose length (thickness) in the Z direction is extremely short (thin) compared to the X and Y directions. The release sheet 33 has protrusions 35 that protrude toward the adhesive layer 30 on the contact surface 34 with the adhesive layer 30. In other words, a release sheet 33 having protrusions 35 can also be referred to as an "embossed release sheet." It is preferable that a thin film of a release agent (mold release agent) be adhered to the surface of the contact surface 34 on which the protrusions 35 of the release sheet 33 are formed. This allows the release sheet 33 to be easily and cleanly peeled from the adhesive layer 30 in the touch sensor 10.
[0035] The release sheet 33 is formed by forming convex portions 35 on the contact surface 34 of the substrate, and then laminating a release agent on the contact surface 34 side including the convex portions 35. The substrate of the release sheet 33 can be a thin resin film or sheet. Examples of resins include thermoplastic resins such as polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polycarbonate (PC), polyamide (PA), acrylic (AC), and polyvinyl chloride (PVC). Paper can also be used as the substrate of the release sheet 33. Examples of paper include fine paper, kraft paper, and glassine paper. At least the contact surface 34 side of the substrate of the release sheet 33 is embossed. Embossing is a process of applying heat and pressure to a substrate to create a textured pattern.
[0036] The protrusions 35 may be formed by the embossing process described above, or may be formed by piling up linearly raised shapes. Resin or the like may be used for piling up the protrusions 35. The protrusions 35 are formed in a linear shape, such as a straight line, a curved line, or a grid pattern, on the surface of the base material.
[0037] As the release agent, a silicone resin, a fluororesin, or the like can be used. The thin film of the release agent can be formed by applying, for example, a silicone resin to the contact surface 34 side where the convex portions 35 are formed, and then curing it by heating, ultraviolet light, or the like. When the substrate is paper, particularly high-quality paper, kraft paper, or the like, a layer of polyethylene (PE), polyvinyl alcohol (PVA), clay, or the like may be provided as a barrier layer (sealing layer) to prevent the release agent from penetrating into the substrate.
[0038] 4, the adhesive layer 30 is a crosslinked and cured product 30b (crosslinked polymer) of an adhesive coating film 30a. The adhesive coating film 30a is a film in which a liquid adhesive is applied to the base surface 23 of the base film 20. By using an OCA (Optically Clear Adhesive) as the adhesive, the adhesive layer 30 can be made to have excellent transparency.
[0039] The adhesive can be applied by printing. This also applies when printing OCA as the adhesive. The adhesive should have a viscosity that allows printing. Furthermore, the adhesive should have a viscosity that prevents air from accumulating when the adhesive coating film 30a is formed on the substrate surface 23. For this reason, the adhesive can be configured to have a viscosity of 0.1 to 100.0 [Pa·s, 25°C].
[0040] By applying the adhesive by printing, it is possible to form an adhesive coating film 30a in which the adhesive is applied only to the desired (necessary) area of the base surface 23. This makes it possible to reduce the amount of adhesive used in the touch sensor 10. Therefore, with a configuration in which the adhesive coating film 30a is used in the adhesive layer 30, it is possible to reduce the amount of adhesive used, and therefore the cost can also be reduced.
[0041] An example of a printing method is screen printing using a metal plate such as a stainless steel mesh plate. However, other printing methods such as a roll coater, knife coater, bar coater, dispenser, inkjet printing, spray coating, and dipping coating may also be used to form the adhesive coating film 30a as long as the liquid adhesive can be applied to the substrate surface 23.
[0042] Here, when attaching a conventional touch sensor to the back surface of a substrate, a transparent double-sided tape, particularly an OCA tape, is widely used for optical applications. However, OCA tape is expensive and suffers from a large amount of material loss (cutting and waste). Specifically, OCA tape is not manufactured to correspond to the shape of the touch sensor, and a space for peeling the backing is required between the adhesive and the backing for protecting the adhesive. As a result, the area of the adhesive, particularly the area of the adhesive, that is not used in the product is large, resulting in a large amount of waste.
[0043] In contrast, the adhesive layer 30 is configured such that the adhesive is applied directly to the base surface 23 of the base film 20. This allows the adhesive to be applied in a desired shape corresponding to the shape of the base film 20, etc. In other words, the adhesive layer 30 is obtained by obtaining an adhesive coating film 30a that matches the shape of the base film 20, rather than removing unnecessary portions that are outside the area of the shape of the base film 20 from a ready-made OCA tape, etc. Therefore, the adhesive coating film 30a can reduce waste. Furthermore, the adhesive coating film 30a reduces material loss, especially of the adhesive, and can also reduce cost, waste disposal costs, etc.
[0044] A liquid adhesive is used to form the adhesive coating film 30a. That is, the adhesive coating film 30a is applied in an uncrosslinked (non-crosslinked) state. By configuring the adhesive layer 30 laminated on the base film 20 to be an adhesive coating film 30a that is applied in an uncrosslinked (non-crosslinked) state, it is possible to suppress air remaining between the base film 20 and the adhesive layer 30.
[0045] When applying an adhesive such as transparent double-sided tape or OCA tape to a conventional touch sensor, the adhesive, which has a predetermined hardness rather than a liquid state, is forcibly pressed against a surface having an uneven shape due to the electrodes and circuit wiring of the sensor circuit. In other words, the ability of the adhesive to conform to the uneven shape of transparent double-sided tape, OCA tape, etc. depends on the hardness inherent to the adhesive, and does not match the ability of a liquid adhesive. Therefore, with transparent double-sided tape, OCA tape, etc., air is likely to remain in the side areas of the uneven shape of the circuit, etc. This air residue can adversely affect the sensitivity of the touch sensor.
[0046] In contrast, the adhesive coating film 30a is formed by coating the sensor circuit 24 with a liquid adhesive. Therefore, the adhesive coating film 30a allows the adhesive layer 30 to cover the surface of a component having an uneven shape, such as the sensor circuit 24, which is disposed on the base film 20. This makes it possible to prevent air from being trapped between the exposed surface of the sensor circuit 24 and the adhesive layer 30. Therefore, the adhesive coating film 30a can improve the sensitivity of the sensor. Even when the liquid adhesive is formed by coating the sensor circuit 24 with a resist layer interposed therebetween, the thin resist layer has an uneven shape due to the sensor circuit 24, and the adhesive coating film 30a can similarly prevent air from being trapped.
[0047] Furthermore, the adhesive coating film 30a covers both the circuit surface 25, which is a protruding portion on the substrate surface 23 where the sensor circuit 24 is formed, and the non-circuit surface, which is a non-protruding portion on the substrate surface 23 where the sensor circuit 24 is not formed, i.e., the substrate surface 23. Therefore, the adhesive coating film 30a can absorb steps such as the sensor circuit 24 that protrudes from the substrate surface 23 in the Z direction. In particular, when the adhesive coating film 30a is formed thicker than the height of the sensor circuit 24 in the Z direction, the top surface of the adhesive coating film 30a can be made flat. This makes it possible to prevent air from remaining on the outer surface 32, which serves as the "attachment surface," of the adhesive layer 30 attached to the cover member 8.
[0048] The adhesive forming the adhesive coating film 30a is a liquid material that can conform (flow and deform) to the shape of the sensor circuit 24. The adhesive coating film 30a has a lamination surface 36 that conforms to the shape of the sensor circuit 24. This lamination surface 36 indicates that the adhesive layer 30 is formed by stacking layers of adhesive to conform to the shape of the sensor circuit 24. Therefore, when the adhesive coating film 30a has a lamination surface 36 that conforms to the shape of the sensor circuit 24, it is possible to prevent air from being trapped between the sensor circuit 24 and the adhesive layer 30. This lamination surface 36 therefore improves the sensitivity of the sensor. Even when the adhesive coating film 30a has a lamination surface that conforms to the shape of the sensor circuit 24 via a resist layer, it is possible to similarly prevent air from being trapped and improve the sensitivity of the sensor.
[0049] The cross-linked and cured product 30b is obtained by cross-linking and curing the adhesive coating film 30a. The cross-linked and cured product 30b of the adhesive coating film 30a makes it possible to easily increase the elasticity (cross-linking elasticity) (elastic limit and elastic modulus) of the adhesive layer 30 simply by cross-linking and curing the adhesive coating film 30a. This gives the adhesive layer 30 a viscoelastic property that combines viscosity and elasticity.
[0050] Conventional transparent double-sided tapes and OCA tapes have adhesives with a certain level of tackiness. Therefore, there is a risk that foreign matter such as cutting scraps and hair will adhere to the cut surfaces where the adhesive is exposed. Furthermore, with conventional transparent double-sided tapes and OCA tapes, there is a risk that the exposed adhesive will come into contact with another touch sensor, resulting in adhesive stains that cause the touch sensors to stick to each other. To solve these problems, there is a method for reducing the exposure of the cut surfaces by adding a process for cutting the transparent double-sided tape or OCA tape into a shape that is shifted inward from the outer shape of the touch sensor, but this adds an extra manufacturing process.
[0051] In contrast, in the touch sensor 10, by cross-linking the adhesive coating film 30a, the tackiness of the adhesive layer 30 can be reduced, even though the adhesive layer 30 has viscoelastic properties. Therefore, in the touch sensor 10, the tackiness of the adhesive layer 30 is reduced, which can prevent foreign matter from adhering to the cut surface (edge adhesive surface) of the adhesive layer 30. Furthermore, because the tackiness of the adhesive layer 30 is reduced, even if the exposed adhesive layer 30 comes into contact with another touch sensor 10, the occurrence of adhesive stains is suppressed, and sticking of the touch sensors 10 to each other can be prevented. Therefore, the touch sensor 10 can be transported without hindrance, which can contribute to automation of the manufacturing and processing processes of the touch sensor 10.
[0052] Furthermore, in the touch sensor 10, the adhesive layer 30 has reduced tackiness, which can prevent the adhesive from adhering to the cutting blade that cuts the touch sensor 10. This can improve the work efficiency of the manufacturing and processing steps of the touch sensor 10. Furthermore, in the touch sensor 10, the adhesive layer 30 has reduced tackiness, which can reduce the amount of touch sensors 10 that cannot be used as products due to the adhesion of foreign matter, adhesive stains, etc. to the touch sensor 10 and are discarded.
[0053] The crosslinked, cured product 30b can be configured to have a ball tackiness of No. 3 or more and No. 7 or less. This can reduce the stickiness (adhesive strength) of the adhesive layer 30 exposed at the edge of the region where the adhesive layer 30 and the cover member 8 are attached. Therefore, this can suppress adhesion of foreign matter to the adhesive layer 30. When the ball tackiness is No. 3 or more, the tackiness is not too small, and the adhesive strength of the adhesive layer 30 is sufficient. When the ball tackiness is No. 7 or less, the tackiness is not too large, and adhesion of foreign matter to the adhesive layer 30 can be suppressed. Tackiness can be evaluated using an inclined ball tack test in accordance with JIS Z0237:2009 (inclination angle 30 degrees, temperature 23°C, humidity 50%).
[0054] The cross-linked, cured material 30b constituting the adhesive layer 30 is also laminated on at least a portion of the tail portion 22. The outer periphery of the substrate film 20 on which the cross-linked, cured material 30b is formed is cut off in areas other than the tail portion 22. In contrast, since the adhesive layer 30 is not provided in the tail portion 22, the outer edge of the adhesive layer 30 formed by printing remains uncut on the surface covering the base material main body 21 to the base of the tail portion 22. As shown in Figure 2, in the tail portion 22, the cross-linked, cured material 30b forms an obliquely shaped portion 37 that is inclined so that its length in the Z direction decreases outward.
[0055] Tail portion 22 is often bent into a curved shape approaching a 180-degree bend when connecting touch sensor 10 to a substrate on which a touch sensor IC is mounted. However, because adhesive layer 30 with enhanced elasticity is formed on the surface covering the base of tail portion 22, the occurrence of wiring cracks and the like can be suppressed even when tail portion 22 is bent. Furthermore, cross-linked, cured material 30b has a predetermined length in the Z direction, particularly as it approaches substrate body 21 from the base of tail portion 22, making it less likely to bend sharply, i.e., with a large curvature. Therefore, tail portion 22 formed with cross-linked, cured material 30b has a curved shape with a reduced curvature even when bent 180 degrees, thereby suppressing the occurrence of circuit wiring cracks and the like.
[0056] Furthermore, in tail portion 22, cross-linked, cured material 30b is configured as obliquely shaped portion 37, so that the tip side (outside) of tail portion 22 is more easily bent than the base of tail portion 22, which is the boundary between substrate body portion 21 and tail portion 22. Therefore, obliquely shaped portion 37 protects the base of tail portion 22 so that substrate film 20 does not bend sharply and stress is not concentrated, thereby suppressing the occurrence of wiring cracks and the like.
[0057] The adhesive layer 30 further has air grooves 38 with an "uneven shape" that are transferred (shaped) by contact with the protrusions 35 on the surface (outer surface 32) that comes into contact with the release sheet 33. The air grooves 38 are deformed from the flat outer surface 32 by the force from the protrusions 35. The air grooves 38 can maintain the deformed uneven shape as it is.
[0058] The uneven shape of the air grooves 38 can be maintained as is. This ability to maintain the uneven shape of the air grooves 38 can be achieved by the high viscosity and viscoelasticity of the adhesive layer 30. The uneven shape of the air grooves 38 of the adhesive layer 30 is maintained (protected) by the release sheet 33. The uneven shape can be maintained without being crushed even after the release sheet 33 is peeled off.
[0059] The crosslinked, cured product 30b can be configured to have a storage modulus E' of 0.1 MPa or more and 2 MPa or less as measured with a dynamic viscoelasticity measuring device. This allows the uneven shape of the air grooves 38 on the surface of the adhesive layer 30 to be maintained as is. The storage modulus E' can be measured using a dynamic viscoelasticity measuring device (trade name "DMS6100", manufactured by Seiko Instruments Inc.) at a frequency of 1 Hz, a temperature of 25°C, and in tension mode.
[0060] The release sheet 33 has both the function of forming the air grooves 38 on the outer surface 32 of the adhesive layer 30 and the function of protecting the uneven shape of the air grooves 38. However, the release sheet 33 may have only the function of protecting the uneven shape of the air grooves 38. In other words, the air grooves 38 can also be formed by a "transfer material" separate from the release sheet 33. In this case, the release sheet 33 can be attached to the air grooves 38 after the "transfer material" is removed.
[0061] As the "transfer material", a member having an uneven surface can be used. As the type of uneven surface, for example, a parallel line shape or a lattice shape where parallel lines intersect is preferable, and other shapes such as a mesh shape and a grained shape are also possible. The uneven shape may be a shape in which the unevenness is regularly arranged. Alternatively, the uneven shape may be a shape in which the unevenness is irregularly arranged. As the "transfer material", a metal plate, a metal mesh, a resin plate, a resin mesh, a resin sheet, a resin film, etc. can be used.
[0062] The touch sensor 10 having the above configuration is attached to a cover member 8 as an "attachment member" in the armrest portion 4 as a "touch panel" as shown in FIG. 5. An operation surface 7 is formed on the front side of the cover member 8. On the other hand, the cover member 8 has a back side 9 on the side opposite the operation surface 7. The cover member 8 may be made of a material such as synthetic rubber, synthetic leather, fabric, or glass in addition to hard resin. Furthermore, the cover member 8 may be in the form of a plate, sheet, or film.
[0063] The touch sensor 10 is attached to the back surface 9 of the cover member 8 in a position corresponding to the operating surface 7 of the cover member 8. At this time, the adhesive layer 30 is attached so that the surface having the uneven shape of the air grooves 38 adheres to the cover member 8 with the release sheet 33 peeled away. The touch sensor 10 is characterized by maintaining the uneven shape of the air grooves 38 on the surface of the adhesive layer 30 as described above. This makes it possible to realize the touch sensor 10 that suppresses air remaining between the cover member 8 and the touch sensor 10, and the armrest portion 4 as a "touch panel."
[0064] That is, by maintaining the air groove 38 deformed into a concave linear shape over time, residual air is discharged without accumulating between the rear surface 9 of the cover member 8 and the outer surface 32 of the touch sensor 10. As a result, no air remains between the cover member 8 and the touch sensor 10.
[0065] Here, if the uneven shape of the air groove 38 were to be flattened and smoothed, the adhesive layer 30 surrounding the air would adhere seamlessly to the cover member 8 in a circular fashion before the air could be discharged outside the area, leaving no way for the air to escape.
[0066] In contrast, in a configuration in which the uneven shape of the air grooves 38 is maintained as it is, an air exhaust path remains. Furthermore, when the cover member 8, which is the adherend member, is made of resin, even if outgassing occurs from the resin between the cover member 8 and the adhesive layer 30, it can be exhausted in the same way as residual air. Therefore, air grooves 38 that maintain their uneven shape over time can impart to the adhesive layer 30 the function of exhausting air from between the cover member 8 and the touch sensor 10.
[0067] In the touch sensor 10, air is discharged from between the cover member 8 and the touch sensor 10, making it possible to configure the touch sensor 10 so that it is difficult to peel off from the cover member 8. That is, after the air is discharged, the surface of the adhesive layer 30 is firmly fixed to the cover member 8. Furthermore, in the touch sensor 10, air is discharged from between the cover member 8 and the touch sensor 10, which can improve the appearance, particularly when the cover member 8 is transparent.
[0068] Here, when attaching a conventional touch sensor to a substrate, there is a problem of air getting mixed in at the bonding surface between the two. Therefore, when bonding these components, it is necessary to use a relatively large-scale device such as an autoclave that creates a pressurized or reduced-pressure environment to forcibly expel air from the bonding surface. Furthermore, even when pressurized and heated using an autoclave, the air may only be thinly dispersed and not be expelled. Furthermore, if the substrate is, for example, 1 m or larger, it becomes difficult to accommodate it in a pressure-resistant container. In this case, it may be impossible to apply pressure to the substrate, and it may even be impossible to expel the air.
[0069] In contrast, in the touch sensor 10, the amount of air trapped between the adhesive layer 30 and the exposed surface (circuit surface 25) of the protruding portion of the sensor circuit 24 or the like is suppressed, thereby reducing the amount of trapped air in the first place. Furthermore, the touch sensor 10 has a function of discharging air from between the cover member 8 and the touch sensor 10. Therefore, the touch sensor 10 can bond the cover member 8 and the touch sensor 10 under atmospheric pressure. Furthermore, the touch sensor 10 can discharge air from between the cover member 8 and the touch sensor 10 regardless of the dimensions of the cover member 8. In this case, the touch sensor 10 does not require additional external energy input as a driving force to push the air out of the region.
[0070] The uneven shape of the air grooves 38 may be a chaotic shape. However, the uneven shape of the air grooves 38 can be a linear groove (groove shape) such as parallel straight lines, curved lines, or wavy lines, or an intersecting lattice pattern. The intersecting angles of the lattice lines can be right angles of 90 degrees, acute angles such as 30 degrees or 60 degrees, or obtuse angles such as 120 degrees. The lattice pattern can be a square lattice, or other intersecting shapes such as a rhombic lattice, triangular lattice, hexagonal lattice (honeycomb lattice), or kagome lattice. For example, as shown in FIG. 2 , a lattice pattern (square lattice) intersecting at right angles in a plan view can be used. By configuring the uneven shape of the surface of the adhesive layer 30 in a lattice pattern, air exhaust paths from the area where the adhesive layer 30 and the cover member 8 are attached to each other to the outside of the area can be connected. Furthermore, by configuring the uneven shape of the surface of the adhesive layer 30 in a lattice pattern, multiple detours can be formed as air exhaust paths in addition to the shortest route. Therefore, when the surface of the adhesive layer 30 has a grid-like uneven shape, air can be more effectively discharged from between the cover member 8 and the touch sensor 10 .
[0071] If the air grooves 38 have a lattice-like uneven shape, the uneven shape can be easily transferred when being formed in the air grooves 38 .
[0072] The adhesive layer 30 is formed from a material that is liquid in an uncrosslinked state and hardens upon crosslinking. The material for the adhesive layer 30 can be formulated to address not only residual air but also outgassing from the resin cover member 8. The adhesive layer 30 uses an adhesive capable of strongly adhering to materials commonly used as the "adhered member" for the cover member 8, such as polycarbonate and polymethyl methacrylate (PMMA). The adhesive can be, for example, a mixture of an acrylic adhesive, an epoxy curing agent, and a printing diluent. Other adhesives that can be used include urethane adhesives and silicone adhesives. Other curing agents that can be used include isocyanate crosslinking agents, hydrosilyl group-containing crosslinking agents, and peroxide crosslinking agents. The material for the adhesive layer 30 can be formulated to have a viscosity suitable for printing, such as screen printing, and to exhibit appropriate hardness and adhesive strength upon crosslinking. Examples of commercially available acrylic adhesives that can be used include SK Dyne (registered trademark) 2147, SK Dyne 2094, SK Dyne 1811L, SK Dyne 1442, SK Dyne 1435, and SK Dyne 1415 (all manufactured by Soken Chemical & Engineering Co., Ltd.), and Olivine (registered trademark) BPS5896 (manufactured by Toyochem Co., Ltd.).
[0073] A tackifier (tackifying resin) can be added to the material of the adhesive layer 30 to adjust the tackiness of the cross-linked, cured product 30b. Furthermore, a UV curing agent can be added to the adhesive material to cross-link the material by UV irradiation. Furthermore, the adhesive layer 30 can be made of any material that is liquid in an uncross-linked state and hardens by cross-linking, and a photo-curable resin, particularly a UV-curable resin, can also be used.
[0074] The properties of the adhesive layer 30 are exhibited by blending a curing agent for the adhesive, and can be adjusted by the blending amount of the curing agent. As the blending amount of the curing agent decreases, the adhesive layer 30 becomes softer and the adhesion to the cover member 8 becomes stronger, thereby suppressing peeling of the adhesive layer 30. Furthermore, as the blending amount of the curing agent decreases, the adhesive layer 30 can be made more shapable. As the blending amount of the curing agent increases, the adhesive layer 30 becomes harder and the blister resistance of the adhesive layer 30 improves, making it more difficult for outgassing to penetrate the adhesive layer 30 and suppressing the generation of residual air. This also suppresses peeling of the touch sensor 10 from the cover member 8 due to outgassing.
[0075] The adhesive layer 30 can be configured with multiple layers. By configuring the adhesive layer 30 with multiple layers, the thickness of the adhesive layer 30 can be increased. Furthermore, by having a large thickness, the adhesive layer 30 can be attached to an "attachment surface" of an "adherend" that has large irregularities.
[0076] The adhesive layer 30 can use different adhesives depending on the material of the cover member 8 as the "adhered member." For example, the adhesive layer 30 can use different adhesives suited to the metal portion and the resin portion.
[0077] In addition to the base film 20 and the adhesive layer 30, the touch sensor 10 may be provided with intermediate layers such as functional layers and decorative layers as needed.
[0078] The base film 20 as the "substrate" is not limited to a flat surface, but can be configured as a three-dimensional surface. In this case, the adhesive layer 30 can be formed on the "substrate" before three-dimensional molding, or the adhesive layer 30 can be formed on the three-dimensionally molded "substrate."
[0079] Manufacturing method of touch sensor 10 (FIG. 4)
[0080] Next, a method for manufacturing the touch sensor 10 will be described.
[0081] First, a material for the substrate film 20 is prepared. For example, a film-shaped polyethylene terephthalate can be used as the material for the substrate film 20. The substrate film 20 has dimensions larger than the desired shapes of the substrate body portion 21 and tail portion 22. Then, a sensor circuit 24 is formed on the substrate surface 23 of the substrate film 20 (step S101). For example, a liquid conductive polymer is used as the material for the sensor circuit 24. An example of the conductive polymer is PEDOT / PSS. PEDOT / PSS is transparent. The sensor circuit 24 can be formed by printing the liquid conductive polymer. For example, a printing method is screen printing. Furthermore, a resist layer is formed by screen printing so as to cover at least the sensor circuit 24.
[0082] Next, an adhesive coating film 30a is formed on the substrate surface 23 of the substrate film 20 using a liquid adhesive composition (step S102). The adhesive layer 30 is made of a liquid adhesive composition. Examples of the adhesive composition include a mixture of an acrylic adhesive, an epoxy curing agent, and a printing dilution solvent. The adhesive coating film 30a can be formed by printing the liquid adhesive composition. Examples of printing methods include screen printing. The adhesive coating film 30a is provided so as to cover the entire substrate body portion 21 and at least a portion (base portion) of the tail portion 22.
[0083] The use of a liquid adhesive composition as the material for the adhesive layer 30 can prevent air from remaining between the base film 20 and the adhesive layer 30. Furthermore, the use of a liquid adhesive composition can allow the adhesive layer 30 to cover the surface of a component having an uneven shape, such as the sensor circuit 24, which is disposed on the base film 20. This prevents air from being trapped between the sensor circuit 24 and the adhesive layer 30. Furthermore, the use of a liquid adhesive composition as the material for the adhesive layer 30 allows printing to be used to apply the adhesive. This allows the formation of an adhesive-coated film 30a in which the adhesive is applied only to the desired (required) area of the base surface 23.
[0084] Furthermore, the adhesive coating film 30a is crosslinked and cured to obtain a crosslinked and cured product 30b that constitutes the adhesive layer 30 (step S103). The adhesive coating film 30a can be crosslinked and cured, for example, by heating and drying the adhesive coating film 30a in an oven. By crosslinking and curing the adhesive coating film 30a, the elasticity of the adhesive layer 30 can be easily increased. Therefore, an adhesive layer 30 having viscoelastic properties that combine viscosity and elasticity can be formed.
[0085] Next, the contact surface 34 of the release sheet 33, which has protrusions 35 protruding toward the adhesive layer 30, is brought into contact with the outer surface 32 of the adhesive layer 30, thereby transferring the air grooves 38 to the outer surface 32 (step S104) (see also FIG. 3 ). The release sheet 33 has a thin film of silicone resin, which serves as a release agent, formed to cover the contact surface 34. Furthermore, the contact surface 34 of the release sheet 33 has protrusions 35 embossed in a grid pattern formed thereon. The release sheet 33 is then pressed against the adhesive layer 30, thereby forming air grooves 38 in which the shape of the grid-like protrusions 35 is transferred to the adhesive layer 30.
[0086] At this time, because the adhesive layer 30 has viscoelastic properties, the uneven shape of the air grooves 38 is maintained over time. Therefore, the air grooves 38 can be configured to have the function of discharging air from between the cover member 8 and the touch sensor 10.
[0087] Here, when forming a touch sensor 10 having a three-dimensional shape, the base film 20 may be three-dimensionally molded using a molding die.
[0088] Finally, the touch sensor 10 is obtained by cutting the base film 20 into a shape including the base body portion 21 and the tail portion 22. However, the base film 20 may be cut into a shape including the base body portion 21 and the tail portion 22 at any time, for example, before the sensor circuit 24 is formed, before the adhesive layer 30 is formed, or after the adhesive layer 30 is formed.
[0089] As described above, according to this embodiment, a manufacturing method for the touch sensor 10 that suppresses air remaining between the cover member 8 and the touch sensor 10 can be realized.
[0090] Manufacturing method of "touch panel" (armrest portion 4) [Figure 5]
[0091] Next, a method for manufacturing the armrest portion 4 will be described.
[0092] First, the cover member 8 of the armrest portion 4, which is the attachment member, is prepared. The cover member 8 can be made of, for example, polycarbonate, which is a plate-shaped hard resin. The cover member 8 is an exterior member that is larger than the touch sensor 10. The cover member 8 is molded to have the shape of the armrest portion 4.
[0093] Next, the touch sensor 10 is attached to the cover member 8 (step S201). At this time, the release sheet 33 is peeled off from the adhesive layer 30. The touch sensor 10 is aligned to correspond to the area of the operation surface 7 of the cover member 8. Then, the "attachment surface" of the adhesive layer 30 of the touch sensor 10 (the surface exposed on the outer surface 32 side) is pressed against the back surface 9 of the cover member 8. The "attachment surface" of the adhesive layer 30 has air grooves 38 formed thereon, with a grid-like pattern transferred to the adhesive layer 30.
[0094] The touch sensor 10 is then left attached to the cover member 8 in this manner (step S202). At this time, the air grooves 38 that have been pressed into the convex portions 35 and deformed into a concave shape maintain their concave and convex shapes, allowing any remaining air trapped in the area between the back surface 9 of the cover member 8 and the outer surface 32 of the adhesive layer 30 to be discharged to the outside. Therefore, according to this embodiment, a manufacturing method for a "touch panel" (armrest portion 4) that suppresses air from remaining between the cover member 8 and the touch sensor 10 can be realized.
[0095] The touch sensor 10 and the like of this embodiment will be described in more detail and specifically below with reference to examples. However, this embodiment is not limited to the following examples.
[0096] Example 1
[0097] (Creation of Adhesive Layer 30) In Example 1, a touch sensor 10 having the shape shown in FIG. 3 was fabricated. A 0.1 mm-thick polyethylene terephthalate film was used for the base film 20. The adhesive used was a mixture of 100 parts by mass of an acrylic adhesive (SK Dyne (registered trademark) 2094, manufactured by Soken Chemical & Engineering Co., Ltd.), 0 parts by mass of an epoxy resin curing agent (E-AX, manufactured by Soken Chemical & Engineering Co., Ltd.), and 20 parts by mass of a printing dilution solvent (T-980, manufactured by Seiko Advance Corporation). In other words, in Example 1, no epoxy resin curing agent was mixed. Table 1 shows the mass ratios of each mixture, including each example and comparative example described below. The mixture was laminated on the base surface 23 of the base film 20 by screen printing, forming an adhesive coating film 30a. The adhesive coating film 30a was heated and dried for 2 minutes in an oven set at 90°C, and then cured for 24 hours to evaporate the solvent and promote the crosslinking reaction, thereby obtaining an adhesive layer 30 made of a 50 μm thick crosslinked, cured material 30b.
[0098] (Physical Properties of Adhesive Layer 30) The adhesive layer 30 of Example 1 had the physical properties shown below (Table 1). That is, the adhesive layer 30 of Example 1 had a tackiness of ball number 7 in an inclined ball tack test at an inclination angle of 30° in accordance with JIS Z 0237:2009. Furthermore, the adhesive layer 30 of Example 1 had a peel adhesive strength of 17.0 N / 20 mm against a polycarbonate plate in a 180° peel test at a speed of 50 mm / min in accordance with JIS Z 0237:2009. The adhesive layer 30 of Example 1 also had a storage modulus E' of 0.3 MPa in a test measured at a frequency of 1 Hz, a temperature of 25°C, and a tension mode using a dynamic viscoelasticity measuring device (product name "DMS6100", manufactured by Seiko Instruments Inc.).
[0099]
[0100] (Transfer of concave-convex shape to adhesive layer 30) In Example 1, two different methods were used to transfer the concave-convex shape to the adhesive layer 30, and different types of "transfer material" were used for each method. That is, a convex-stripe plate was used as the "transfer material" in the first method, and a convex-stripe film was used as the "transfer material" in the second method. The convex-stripe here refers to linear protrusions.
[0101] In the first method, a convex strip plate (TH-306, manufactured by Tanazawa Hakkosha) was used as a "transfer material" in place of the release sheet 33. On the contact surface 34 of the convex strip plate, convex portions 35 were formed, which were lines that intersected in a diamond-shaped lattice pattern in a plan view, extended along the tangential direction of the contact surface 34, and protruded along the normal direction of the contact surface 34. The convex portions 35 were formed with a line width of 0.5 mm, a pitch of 1.5 mm between adjacent convex portions 35, one of two pairs of interior angles of the diamond was 120° and the other was 60°, and the protruding height was 135 μm.
[0102] A convex strip plate was attached to the outer surface 32 of the adhesive layer 30 in place of the release sheet 33. The outer surface 32 did not have an uneven shape at this stage. The contact surface 34 of the convex strip plate was attached so that the convex portions 35 contacted the outer surface (exposed surface) of the adhesive layer 30. With the convex strip plate attached, the touch sensor 10 was pressed with a rubber roller from the side of the base film 20 and then left to stand at 25°C for 24 hours. The outer surface side of the release sheet 33 was then peeled off from the convex strip plate, yielding the touch sensor 10 of Example 1. The adhesive layer 30 of the obtained touch sensor 10 had air grooves 38 formed therein, in which the shape of the grid-like convex portions 35 of the convex strip plate was transferred to the adhesive layer 30. The touch sensor 10 produced by this first method was used only to determine whether the uneven shape could be transferred to the adhesive layer 30.
[0103] Next, as a second method for transferring the uneven shape to the adhesive layer 30, a 200 μm-thick release sheet (K11 White PL, manufactured by Lintec Corporation) was used as a "transfer material" instead of the release sheet 33. The contact surface 34 of the release sheet was formed with convex portions 35, each consisting of intersecting lines in a triangular lattice pattern, piled up with resin. The convex portions 35 had a line width of 0.5 mm, a pitch of 1.0 mm between adjacent convex portions 35, and a protrusion height of 50 μm. The release sheet was attached to the adhesive layer 30 with a hand roller so that the contact surface 34 of the release sheet was in contact with the adhesive layer 30, and the resulting material was left to stand at 25°C for 24 hours, thereby obtaining the touch sensor 10 of Example 1. The adhesive layer 30 of the resulting touch sensor 10 had air grooves 38 formed therein, in which the shape of the grid-like convex portions 35 of the release sheet was transferred to the adhesive layer 30.
[0104] Next, a 1.0 mm thick polycarbonate plate was prepared for the cover member 8. The ridge plate or ridge film serving as the "transfer material" was peeled off immediately before being attached to the cover member 8. The touch sensor 10 was attached to the cover member 8 such that the outer surface 32 serving as the "attachment surface" on which the air grooves 38 of the adhesive layer 30 of the touch sensor 10 were formed was pressed against the back surface 9 of the cover member 8. Then, the touch sensor 10 attached to the cover member 8 was left to stand for a predetermined period of time.
[0105] Example 2
[0106] (Creation of adhesive layer 30) In Example 2, the mixture used for the adhesive contained 0.1 parts by mass of an epoxy resin curing agent (E-AX, manufactured by Soken Chemical & Engineering Co., Ltd.). Other than that, the process was the same as in Example 1.
[0107] (Physical properties of adhesive layer 30) The adhesive layer 30 of Example 2 had the following physical properties in the same tests as Example 1. That is, the adhesive layer 30 of Example 2 had a tackiness of ball number 6. Furthermore, the adhesive layer 30 of Example 2 had a peel adhesive strength of 16.0 N / 20 mm against a polycarbonate plate. The adhesive layer 30 of Example 2 also had a storage modulus E' of 0.5 MPa.
[0108] Example 3
[0109] (Creation of adhesive layer 30) In Example 3, the mixture used for the adhesive contained 0.27 parts by mass of an epoxy resin curing agent (E-AX, manufactured by Soken Chemical & Engineering Co., Ltd.). Other than that, the process was the same as in Example 1.
[0110] (Physical properties of adhesive layer 30) The adhesive layer 30 of Example 3 had the following physical properties in the same tests as in Example 1. That is, the adhesive layer 30 of Example 3 had a tackiness of ball number 5. Furthermore, the adhesive layer 30 of Example 3 had a peel adhesive strength of 12.1 N / 20 mm against a polycarbonate plate. The adhesive layer 30 of Example 3 also had a storage modulus E' of 0.6 MPa.
[0111] Example 4
[0112] (Creation of adhesive layer 30) In Example 4, the mixture used for the adhesive contained 0.3 parts by mass of an epoxy resin curing agent (E-AX, manufactured by Soken Chemical & Engineering Co., Ltd.). Other than that, the process was the same as in Example 1.
[0113] (Physical properties of adhesive layer 30) The adhesive layer 30 of Example 4 had the following physical properties in the same tests as in Example 1. That is, the adhesive layer 30 of Example 4 had a tackiness of ball number 5. Furthermore, the adhesive layer 30 of Example 4 had a peel adhesive strength of 13.0 N / 20 mm against a polycarbonate plate. The adhesive layer 30 of Example 4 also had a storage modulus E' of 0.6 MPa.
[0114] Example 5
[0115] (Creation of adhesive layer 30) In Example 5, the mixture used for the adhesive contained 0.4 parts by mass of an epoxy resin curing agent (E-AX, manufactured by Soken Chemical & Engineering Co., Ltd.). Other than that, the process was the same as in Example 1.
[0116] (Physical properties of adhesive layer 30) The adhesive layer 30 of Example 5 had the following physical properties in the same tests as in Example 1. That is, the adhesive layer 30 of Example 5 had a tackiness of ball number 5. Furthermore, the adhesive layer 30 of Example 5 had a peel adhesive strength of 12.1 N / 20 mm against a polycarbonate plate. The adhesive layer 30 of Example 5 also had a storage modulus E' of 1.1 MPa.
[0117] Example 6
[0118] (Creation of adhesive layer 30) In Example 6, the epoxy resin curing agent (E-AX, manufactured by Soken Chemical & Engineering Co., Ltd.) constituting the mixture used for the adhesive was 0.6 parts by mass. Other than that, the process was the same as in Example 1.
[0119] (Physical properties of adhesive layer 30) The adhesive layer 30 of Example 6 had the following physical properties in the same tests as in Example 1. That is, the adhesive layer 30 of Example 6 had a tackiness of ball number 4. Furthermore, the adhesive layer 30 of Example 6 had a peel adhesive strength of 9.0 N / 20 mm against a polycarbonate plate. The adhesive layer 30 of Example 6 also had a storage modulus E' of 1.5 MPa.
[0120] Example 7
[0121] (Creation of adhesive layer 30) In Example 7, the epoxy resin curing agent (E-AX, manufactured by Soken Chemical & Engineering Co., Ltd.) constituting the mixture used for the adhesive was 0.8 parts by mass. Other than that, the process was the same as in Example 1.
[0122] (Physical properties of adhesive layer 30) The adhesive layer 30 of Example 7 had the following physical properties in the same tests as in Example 1. That is, the adhesive layer 30 of Example 7 had a tackiness of ball number 3. Furthermore, the adhesive layer 30 of Example 7 had a peel adhesive strength of 7.6 N / 20 mm against a polycarbonate plate. The adhesive layer 30 of Example 7 also had a storage modulus E' of 2.0 MPa.
[0123] Comparative Example 1
[0124] (Creation of adhesive layer 30) In Comparative Example 1, the epoxy resin curing agent (E-AX, manufactured by Soken Chemical & Engineering Co., Ltd.) constituting the mixture used for the adhesive was 1.0 part by mass. Other than that, the process was the same as in Example 1.
[0125] (Physical properties of adhesive layer 30) The adhesive layer 30 of Comparative Example 1 had the following physical properties in the same tests as in Example 1. That is, the adhesive layer 30 of Comparative Example 1 had a tackiness of ball number 2. Furthermore, the adhesive layer 30 of Comparative Example 1 had a peel adhesive strength of 4.1 N / 20 mm against a polycarbonate plate. The adhesive layer 30 of Comparative Example 1 also had a storage modulus E' of 2.5 MPa.
[0126] Comparative Example 2
[0127] (Creation of adhesive layer 30) In Comparative Example 2, the mixture used for the adhesive contained 1.5 parts by mass of an epoxy resin curing agent (E-AX, manufactured by Soken Chemical & Engineering Co., Ltd.). Other than that, the process was the same as in Example 1.
[0128] (Physical properties of adhesive layer 30) The adhesive layer 30 of Comparative Example 2 had the following physical properties in the same tests as in Example 1. That is, the adhesive layer 30 of Comparative Example 2 had a tackiness of ball number 2. Furthermore, the adhesive layer 30 of Comparative Example 2 had a peel adhesive strength of 2.0 N / 20 mm against a polycarbonate plate. The adhesive layer 30 of Comparative Example 2 also had a storage modulus E' of 1.9 MPa.
[0129] Comparative Example 3
[0130] (Creation of adhesive layer 30) In Comparative Example 3, the epoxy resin curing agent (E-AX, manufactured by Soken Chemical & Engineering Co., Ltd.) constituting the mixture used for the adhesive was 2.0 parts by mass. Other than that, the process was the same as in Example 1.
[0131] (Physical properties of adhesive layer 30) The adhesive layer 30 of Comparative Example 3 had the following physical properties in the same tests as in Example 1. That is, the adhesive layer 30 of Comparative Example 3 had a tackiness of ball number 2. Furthermore, the adhesive layer 30 of Comparative Example 3 had a peel adhesive strength of 1.5 N / 20 mm against a polycarbonate plate. The adhesive layer 30 of Comparative Example 3 also had a storage modulus E' of 1.6 MPa.
[0132] Comparative Example 4
[0133] (Creation of adhesive layer 30) In Comparative Example 4, the mixture used for the adhesive contained 3.0 parts by mass of an epoxy resin curing agent (E-AX, manufactured by Soken Chemical & Engineering Co., Ltd.). Other than that, the process was the same as in Example 1.
[0134] (Physical properties of adhesive layer 30) The adhesive layer 30 of Comparative Example 4 had the following physical properties in the same tests as in Example 1. That is, the adhesive layer 30 of Comparative Example 4 had a tackiness of ball number 1. Furthermore, the adhesive layer 30 of Comparative Example 4 had a peel adhesive strength of 1.0 N / 20 mm against a polycarbonate plate. The adhesive layer 30 of Comparative Example 4 also had a storage modulus E' of 0.1 MPa.
[0135] The storage modulus E' tended to increase as the mass ratio of the curing agent increased from Example 1 to Example 7. This means that as the mass ratio of the curing agent increases and the adhesive layer 30 becomes harder, an increased amount of the energy generated by the adhesive layer 30 being subjected to an external force is stored within the adhesive layer 30. From another perspective, this means that the adhesive layer 30 approaches the properties of a solid from that of a liquid. On the other hand, the storage modulus E' tended to decrease as the mass ratio of the curing agent increased from Comparative Example 1 to Comparative Example 4. This is presumed to be because the adhesive layer 30 approaches the properties of a liquid from that of a solid due to an increase in the amount of excess curing agent that does not contribute to the curing reaction within the adhesive layer 30.
[0136] Comparative Example 5
[0137] (Creation of Adhesive Layer 30) In Comparative Example 5, an acrylic adhesive transfer tape (467MC, manufactured by 3M) was used for the adhesive layer 30. The adhesive layer 30 in Comparative Example 3 was composed of a 50 μm thick adhesive and a paper liner laminated with polyethylene. A convex grid pattern (convex stripes) was formed on the paper liner, and grid-like grooves were transferred onto the adhesive material. Other than that, the process was the same as in Example 1.
[0138] (Physical properties of adhesive layer 30) The adhesive layer 30 of Comparative Example 5 had the following physical properties in the same tests as in Example 1. That is, the adhesive layer 30 of Comparative Example 5 had a tackiness of ball number 2. Furthermore, the adhesive layer 30 of Comparative Example 5 had a peel adhesive strength of 11.6 N / 20 mm against a polycarbonate plate. Furthermore, the storage modulus E' of the adhesive layer 30 of Comparative Example 5 was not measured.
[0139] Comparative Example 6
[0140] (Creation of adhesive layer 30) In Comparative Example 6, an acrylic OCA adhesive tape (8172CL, manufactured by 3M) was used for the adhesive layer 30. The adhesive layer 30 in Comparative Example 4 was composed of a 50 μm thick adhesive and a PET liner laminated with transparent polyester. The PET liner had no protrusions, and the adhesive material also had no uneven shape. Other than that, the adhesive layer was the same as in Example 1.
[0141] (Physical properties of adhesive layer 30) The adhesive layer 30 of Comparative Example 6 had the following physical properties in the same tests as in Example 1. That is, the adhesive layer 30 of Comparative Example 6 had a tackiness of ball number 2. Furthermore, the adhesive layer 30 of Comparative Example 6 had a peel adhesive strength of 10.4 N / 20 mm against a polycarbonate plate. The adhesive layer 30 of Comparative Example 6 also had a storage modulus E' of 1.7 MPa.
[0142] Comparative Example 7
[0143] (Creation of Adhesive Layer 30) In Comparative Example 7, a sample corresponding to the touch sensor 10 shown in Fig. 3 was also produced, as in Example 6. However, in Comparative Example 7, the lattice-shaped convex portions 35 were not transferred to the adhesive layer 30 using a release sheet, and the air grooves 38 were not formed. Other than that, the sample was the same as in Example 6, including the physical properties.
[0144] Evaluation items
[0145] <Transferability (Concave Shape Formability)> The transferability of the adhesive layer 30 of each of Examples 1-7 and Comparative Examples 1-6 was evaluated. In each case, the transferability was evaluated using both the convex stripe plate (transfer shape 1) and the convex stripe film (transfer shape 2). In this disclosure, as described above, the formation of the air grooves 38, which are concave grooves, is attempted by pressure-transferring the convex stripe shape of the "transfer material" to the adhesive layer 30. The transferability here was evaluated based on the presence or absence of concave grooves and their depth immediately after peeling the "transfer material" from the adhesive layer 30. The depth of the concave grooves was measured using a laser microscope ("VK-X150" manufactured by Keyence Corporation). The evaluation criteria were "A" for a concave groove depth of 30 μm or more, "B" for a concave groove depth of 10 μm or more but less than 30 μm, and "C" for no concave groove shape.
[0146] <Groove Maintenance Time> The time during which the grooves in the adhesive layer 30 of each of Examples 1-7 and Comparative Examples 1-4 were maintained was evaluated. For the following evaluation items, the adhesive layer 30 transferred using a ridge film was evaluated. As described above, the time during which the grooves were maintained without pressure was measured from the time when the outer surface 32 serving as the "attachment surface" of the touch sensor 10 was attached to the back surface 9 of the cover member 8. Whether the grooves were maintained on the "attachment surface" of the adhesive layer 30 of the touch sensor 10 was determined by visual inspection from the front surface (operation surface 7) of the cover member 8. The adhesive layer 30 was visually inspected continuously for two hours after the back surface 9 of the cover member 8 and the outer surface 32 of the touch sensor 10 were attached, then every three hours until 24 hours later, and every 24 hours thereafter.
[0147] <Blister resistance (non-retention of resin outgassing)> The blister resistance of the adhesive layer 30 of each of Examples 1-7 and Comparative Examples 1-7 was evaluated. The blister resistance of each adhesive layer 30 was evaluated under two test conditions, which differed in the ambient temperature and the time that each adhesive layer 30 was left at that ambient temperature. That is, under the first test condition, the adhesive layer 30 was left standing at an ambient temperature of 70°C for 30 minutes, and under the second test condition, the adhesive layer 30 was left standing at an ambient temperature of 80°C for 12 hours. Then, the adhesive layer 30 was removed from the atmosphere under each test condition and left standing for 30 minutes, and the appearance was observed.
[0148] Whether or not the appearance of the adhesive layer 30 had changed was judged visually from the surface (operation surface 7) side of the cover member 8. If there was a change in the appearance of the adhesive layer 30, the diameter of the blister caused by resin outgassing was measured using a digital microscope ("VHX-900" manufactured by Keyence Corporation). The judgment was made as "A" if there was no change in the appearance of the adhesive layer 30 (no blister caused by resin outgassing). Furthermore, if there was only a slight change in the appearance of the adhesive layer 30 (the diameter of the blister caused by resin outgassing was less than 1 mm), it was judged as "B," and if there was significant blistering of the adhesive layer 30 (the diameter of the blister caused by resin outgassing was 1 mm or more), it was judged as "C."
[0149] <Remaining Air> The transfer shape (transfer marks) and the presence or absence of remaining air on the "attachment surface" of the adhesive layer 30 of the touch sensor 10 were visually determined from the surface (operation surface 7) side of the cover member 8. The determination was performed immediately after attaching the adhesive layer 30 to the cover member 8, and 12 hours and 24 hours after attachment.
[0150] Results and Discussion
[0151] <Transferability (concave shape formability)> Within the scope of the examples and comparative examples of the present disclosure, no difference was observed in the transferability between the different types of "transfer materials" of the convex streak plate (transfer shape 1) and the convex streak film (transfer shape 2). In Examples 1-7, the depth of the formed concave grooves was 30 μm or more, which was a sufficient rating of A. On the other hand, in Comparative Examples 2 and 3, the depth of the formed concave grooves was 10 μm or more, which was a rating of B. Furthermore, in Comparative Example 4, which contained a high proportion of curing agent, the concave groove shape was not formed, which was a rating of C.
[0152] Here, the mass ratio of the curing agent in Example 3 of the present disclosure is the amount recommended by the curing agent manufacturer, and it is generally recommended to adhere to this amount. Therefore, applying the range of Examples 4-7 as the mass ratio of the curing agent is not normally considered due to issues such as the physical properties of the material and cost. However, in this example, it was found that an adhesive layer 30 with excellent transferability could be formed even if the mass ratio of the curing agent was deliberately in excess of the recommended amount. It was also found that grooves could be formed on the surface of the adhesive layer 30 in all examples of the present disclosure, allowing air to escape from the grooves to the outside, thereby preventing air bubbles from being trapped during lamination.
[0153] It is unclear what relationship exists between ball tack and peel adhesion and transferability. However, adhesive layers 30 with high ball tack tend to have excellent transferability. Similarly, adhesive layers 30 with high peel adhesion tend to have excellent transferability.
[0154] <Groove Maintenance Time> In Example 1, the groove maintenance time of the adhesive layer 30 was 120 hours. On the other hand, in Example 7, the groove maintenance time of the adhesive layer 30 was 12 hours. In all Examples, the groove maintenance time of the adhesive layer 30 was in the range of 12 hours or more and 120 hours or less. Therefore, it was found that the concave and convex shapes of the grooves, i.e., the air grooves 38, in the adhesive layer 30 of all Examples were maintained for, for example, hours to days. Therefore, it was found that in all Examples, air grooves 38 that were maintained over time were formed, and the adhesive layer 30 was able to be endowed with the function of discharging air from between the cover member 8 and the touch sensor 10.
[0155] Furthermore, in Examples 4-7 in which the mass ratio of the curing agent was intentionally set to an amount greater than the recommended amount as described above, the groove retention time of the adhesive layer 30 was within the preferred range of 12 hours or more and 24 hours or less.
[0156] On the other hand, in Comparative Examples 1-3, the groove maintenance time of the adhesive layer 30 was in the range of 2-9 hours. However, this does not deny that Comparative Examples 1-3 have the function of maintaining the grooves of the adhesive layer 30 for at least 2 hours and discharging air from between the cover member 8 and the touch sensor 10. For this reason, the adhesive layer 30 formed of the cross-linked cured product 30b may have viscoelasticity with a storage modulus E' of 0.3 MPa or more and 2.5 MPa or less. However, from the viewpoint of more reliably discharging resin outgassing that occurs between the adherend and the touch sensor 10 when actually manufacturing a "touch panel" by attaching the touch sensor 10 to an adherend, a slightly longer groove maintenance time is preferable.
[0157] <Blister resistance (non-retention of resin outgassing)> In Example 2-7, even when the test conditions were changed from leaving the adhesive layer 30 for 30 minutes at an ambient temperature of 70°C to leaving the adhesive layer 30 for 12 hours at an ambient temperature of 80°C, there was no change in the evaluation in any of the examples. In Example 2-7, the adhesive layer 30 showed no change in appearance, resulting in an evaluation of A. In Example 1, the adhesive layer 30 showed only a slight change in appearance under the test conditions of leaving the adhesive layer 30 for 30 minutes at an ambient temperature of 70°C, resulting in an evaluation of B.
[0158] Furthermore, as described above, in Examples 4-7 in which the mass ratio of the curing agent was deliberately set to a value greater than the recommended amount, the adhesive layer 30 was rated A with no change in appearance, and it was found to have excellent blister resistance.
[0159] On the other hand, when the conditions were made stricter as described above, Comparative Example 5 received a rating of A, indicating no change in the appearance of the adhesive layer 30, but was changed to a rating of B, indicating minimal change in appearance. Comparative Example 4, which contained a high proportion of curing agent, and Comparative Examples 6-7, which did not have an uneven adhesive, received a rating of C, indicating significant swelling, even under test conditions of 30 minutes at an ambient temperature of 70°C. In other words, comparing Example 6 and Comparative Example 7, the presence or absence of an uneven surface resulted in differences in blister resistance. In Comparative Examples 3-7, under test conditions of 12 hours at an ambient temperature of 80°C, all of them, including Comparative Example 3, which received a rating of B, experienced swelling due to resin outgassing.
[0160] As described above, the air grooves 38 are maintained on the surface of the adhesive layer 30 of the example for a predetermined period of time. Therefore, outgassing generated from the cover member 8 serving as a resin "housing panel" is easily discharged to the outside through the air grooves 38. Therefore, the adhesive layer 30 of the example has excellent blister resistance.
[0161] The results of the above Examples and Comparative Examples show that the configurations of the Examples make it possible to form an adhesive layer 30 that does not retain resin outgassing, i.e., has excellent blister resistance.
[0162]
[0163] <Remaining Air> 1 Example 6 (1) Immediately after Adhesion of Adhesive Layer 30 to Cover Member 8 In Example 6, it was possible to visually confirm the transfer shape (transfer marks) on the attachment surface of the adhesive layer 30. Furthermore, in Example 6, it was possible to visually confirm the remaining air that had been enclosed when the adhesive layer 30 was attached to the cover member 8 on the attachment surface of the adhesive layer 30.
[0164] (2) 12 hours after the adhesive layer 30 was attached to the cover member 8 In Example 6, 12 hours after the adhesive layer 30 was attached to the cover member 8, the transferred shape of the attachment surface of the adhesive layer 30 was less noticeable than immediately after attachment. Furthermore, the area of the remaining air on the attachment surface of the adhesive layer 30 was reduced by half in plan view compared to immediately after attachment.
[0165] (3) 24 hours after the adhesive layer 30 was attached to the cover member 8 In Example 6, 24 hours after the adhesive layer 30 was attached to the cover member 8, the transferred shape of the attachment surface of the adhesive layer 30 was less noticeable than that 12 hours after attachment. Furthermore, the remaining air on the attachment surface of the adhesive layer 30 had disappeared and was not visible.
[0166] 2 Comparative Example 7 (1) Immediately after the adhesive layer 30 was attached to the cover member 8 In Comparative Example 7, there was no transfer shape (transfer mark) on the attachment surface of the adhesive layer 30. Furthermore, in Comparative Example 7, residual air that had been trapped when the adhesive layer 30 was attached to the cover member 8 was visible on the attachment surface of the adhesive layer 30. The residual air in Comparative Example 7 had a larger area in a plan view than in Example 6. This is presumed to be because the attachment surface of the adhesive layer 30 in Example 6 has lattice-shaped air grooves 38, and the uneven shape of these grooves separates the air.
[0167] (2) 24 hours after the adhesive layer 30 was attached to the cover member 8 In Comparative Example 7, 24 hours after the adhesive layer 30 was attached to the cover member 8, the area of the air remaining on the attachment surface of the adhesive layer 30 in a plan view was halved compared to immediately after attachment, but it had not disappeared.
[0168] The results of Example 6 and Comparative Example 7 above show that the configuration of Example 6 makes it possible to suppress air remaining between the cover member 8 and the touch sensor 10 .
[0169] In the "touch sensor" of the present disclosure, the configurations shown in the embodiments and modifications can be freely combined within a range that does not cause contradictions.
[0170] In this disclosure, a "touch sensor" that comes into contact with the operation area has been described. However, the "touch sensor" of this disclosure can also be applied to a "proximity sensor" that does not come into contact with the operation area.
[0171] Although the embodiments and examples of the present invention have been described in detail above, it will be readily apparent to those skilled in the art that many modifications are possible without substantially departing from the novel features and effects of the present invention. Therefore, all such modifications are intended to be included within the scope of the present invention.
[0172] 8 Cover member (adhered member) 10 Touch sensor 20 Base film 24 Sensor circuit 30 Adhesive layer 31 Inner surface 32 Outer surface (attached surface) 33 Release sheet 35 Convex portion 38 Air groove
Claims
1. A touch sensor to be attached to a member to be adhered, the touch sensor having a base material and an adhesive layer, a sensor circuit formed on the base material, the adhesive layer having a first surface laminated to the base material and a transfer material on a second surface, the transfer material having convex portions protruding toward the adhesive layer on a surface in contact with the adhesive layer, the adhesive layer further having an uneven shape transferred to the surface in contact with the transfer material by contact with the convex portions, the adhesive layer being affixed such that when the transfer material is peeled off, the surface having the uneven shape adheres to the member to be adhered, and the uneven shape of the surface is maintained.
2. The touch sensor according to claim 1, wherein the adhesive layer is a cross-linked and cured adhesive coating film.
3. The touch sensor according to claim 2, wherein the adhesive coating film is formed by covering the sensor circuit directly or via a resist layer.
4. The touch sensor according to claim 2 or 3, wherein the adhesive coating film has a laminated surface that conforms to the shape of the sensor circuit directly or via a resist layer.
5. The touch sensor according to any one of claims 1 to 4, wherein the uneven shape is a parallel linear groove shape or an intersecting lattice-like groove shape.
6. The touch sensor according to any one of claims 2 to 4, wherein the cross-linked, cured product has viscoelasticity with a storage modulus E' of 0.1 MPa or more and 2 MPa or less.
7. The touch sensor according to any one of claims 2 to 4, wherein the crosslinked and cured product has a ball tackiness of No. 3 or more and No. 7 or less.
8. The touch sensor according to any one of claims 1 to 7, wherein the attachment member is any one of an operation panel (cover member), an exterior panel of a device (housing case), and an internal panel of a device.
9. A touch panel comprising the touch sensor according to any one of claims 1 to 8 attached to the attachment member.
10. A method for manufacturing a touch sensor to be attached to a substrate, comprising the steps of: applying a liquid adhesive to a substrate on which a sensor circuit is formed to form an adhesive coating film; cross-linking and curing the adhesive coating film to form an adhesive layer of a cross-linked and cured product; contacting a transfer material having convex portions protruding toward the adhesive layer to a surface of the adhesive layer to transfer a concave-convex shape to the surface; and when the transfer material is peeled off and the surface having the concave-convex shape is attached to the substrate so as to adhere thereto, the adhesive layer maintains the concave-convex shape of the surface.
11. A method for manufacturing a touch panel, comprising: attaching a touch sensor according to any one of claims 1 to 8 to the adherend; leaving the touch sensor attached to the adherend; and maintaining the uneven shape of the surface of the adhesive layer.
Citation Information
Patent Citations
Pressure-sensitive adhesive sheet with release liner
JP2008222757A
Transparent adhesive sheet and image display device
WO2010044229A1
Sensor device, input device, and electronic device
WO2014147943A1