Laminate including transparent electroconductive film and porous film, biochip including laminate, and method for manufacturing these

The laminate of a transparent conductive film and a porous film with specific properties addresses the challenges of miniaturization and sensitivity in electrochemiluminescence immunoassay devices, enabling efficient and sensitive detection of luminescence and facilitating the use of graphene electrodes for immunoassays in a cost-effective, disposable format.

WO2024203970A1PCT designated stage expired Publication Date: 2024-10-03WATANABE TAKESHI
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011524
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-23
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current electrochemiluminescence immunoassay devices face challenges in miniaturization and sensitivity due to the requirement of electrodes, with conventional transparent conductive films like ITO being unsuitable for disposable use and having issues with oxidation reactions, and existing methods struggle to combine immunochromatography with electrochemiluminescence effectively.

Method used

A laminate comprising a transparent conductive film and a porous film with electrolyte permeability, where the porous membrane has a specific pore structure and composition, is used as a biochip for electrochemiluminescence immunoassay, allowing for efficient detection of luminescence and antibody immobilization without rare elements, enabling the creation of a disposable, flexible, and sensitive testing device.

Benefits of technology

The laminate enables efficient detection of electrochemiluminescence without attenuation, supports high sensitivity, and facilitates the use of graphene electrodes for immunoassays, addressing the limitations of existing technologies by providing a cost-effective, disposable, and flexible testing solution compatible with point-of-care testing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011524_03102024_PF_FP_ABST
    Figure JP2024011524_03102024_PF_FP_ABST
Patent Text Reader

Abstract

[Problem] To provide a transparent electroconductive film that can be supplied for use in quick and simple inspection equipment, and a biochip in which the transparent electroconductive film is used. In particular, to provide a transparent electroconductive film that can be used for immunoassay utilizing electrochemical light emission, and a biochip in which the transparent electroconductive film is used. [Solution] The present invention provides a laminate comprising a transparent electroconductive film and a porous film that is laminated on the transparent electroconductive film, wherein the porous film is permeable with respect to an electrolyte solution.
Need to check novelty before this filing date? Find Prior Art

Description

Laminate including transparent conductive film and porous film, biochip including laminate, and methods for manufacturing the same

[0001] The present invention relates to a laminate including a transparent conductive film laminated with a porous film having micropores, a biochip including the laminate, and methods for producing them. The present invention also relates to an electrochemiluminescence immunoassay method using the laminate and the biochip.

[0002] In recent years, point-of-care testing (POCT), a rapid and simple test performed near the patient, has become increasingly important from the perspectives of disease prevention, health promotion, and infectious disease control. In particular, the spread of COVID-19 has led to an increased demand for the development of instruments that combine simple and highly sensitive measurement. Immunochromatography, a representative rapid and simple testing method, involves antigens in a sample forming immune complexes with gold colloid-labeled antibodies while migrating through a nitrocellulose membrane. This immune complex is then trapped by the capture antibody, producing a color that can be visually determined. While this method is simple and rapid, it is difficult to achieve high sensitivity due to the visual nature of the test, and its application is generally limited to qualitative testing.

[0003] Electrochemiluminescence immunoassay is known as a highly sensitive immunoassay. Electrochemiluminescence is a luminescence phenomenon that occurs through an electrode reaction. Unlike conventional immunoassays that use fluorescence or absorbance measurements, electrochemiluminescence does not require excitation light or incident light. This allows for safe, inexpensive, low-noise measurements and highly sensitive analysis. Generally, tris(2,2'-bipyridyl)ruthenium(II) is used as the electrochemiluminescence labeling reagent, with tripropylamine as the coreactant. Immunoassays using these reagents have also been reported (Patent Document 1). The method described in Patent Document 1 involves labeling an antibody that specifically binds to the target molecule with tris(2,2'-bipyridyl)ruthenium(II). An immune complex is formed by an antigen-antibody reaction. The tripropylamine or both tripropylamine and tris(2,2'-bipyridyl)ruthenium(II) are then oxidized in a tripropylamine solution to emit light, thereby determining the amount of antibody bound to the target substance or the amount of unbound antibody, thereby estimating the concentration of the target molecule.

[0004] Currently, electrochemiluminescence immunoassay is being adopted in Roche's automated analytical clinical testing equipment (Non-Patent Document 1). This automated analytical clinical testing equipment forms an immune complex labeled with tris(2,2'-bipyridyl)ruthenium(II) on magnetic beads, and then utilizes the properties of the magnetic beads to immobilize the complex on the surface of a platinum electrode. An electrolyte containing tripropylamine is used to generate electrochemiluminescence near the platinum electrode, and the luminescence intensity is measured. However, electrochemiluminescence immunoassay requires electrodes, and automated analytical clinical testing equipment that uses a single electrode to measure multiple analytes requires a cleaning process for the electrodes between measurements of different analytes. This makes it difficult to miniaturize the equipment and simplify the measurement process, posing a challenge to the development of a measuring device compatible with POCT.

[0005] With regard to immunoassay methods compatible with POCT, there have been many reports on measurement techniques that combine immunochromatography with fluorescence, chemiluminescence, or chemiluminescent enzyme methods, and devices and kits that use fluorescence chromatography as their measurement principle have been put into practical use, such as Arkray Inc.'s mobile immunofluorescence analyzer "SpotChem FLORA" and Eiken Chemical Co., Ltd.'s SARS coronavirus antigen kit "Exdia EK Test COVID-19 Ag."

[0006] On the other hand, there have been no reported examples of measurement methods combining electrochemiluminescence and immunochromatography. Electrochemiluminescence is a technique that requires electrodes, and combining it with immunochromatography measurement chips, which are generally disposable, necessitates the use of disposable electrodes. Furthermore, the thickness of membranes typically used in immunochromatography is approximately 100 μm, and the diameter of magnetic beads used in practical electrochemiluminescence immunoassay devices is approximately 3 μm. This 100 μm thickness increases the probability that active species generated by the electrode reaction will be deactivated before reaching the electrochemiluminescent labeling substance immobilized on the membrane, potentially significantly reducing luminescence efficiency. These factors are thought to be the causes of the difficulty in combining immunochromatography and electrochemiluminescence.

[0007] Regarding research on POCT devices using electrochemiluminescence immunoassay, many studies have been reported using low-cost electrodes such as paper-based electrodes and screen-printed electrodes, but these have not yet been put into practical use as clinical testing devices.

[0008] Developing an electrochemiluminescence immunoassay device compatible with POCT requires miniaturization of the device itself. Using transparent conductive films as electrodes allows for greater flexibility in device configuration, making miniaturization easier. However, indium tin oxide (ITO), a typical transparent conductive film, contains the rare element indium and is therefore unsuitable for use as a disposable electrode. Furthermore, oxide-based transparent conductive films, such as ITO, are less likely to undergo oxidation reactions with organic compounds such as tripropylamine, making it difficult to achieve high luminescence intensity in immunoassay measurement systems.

[0009] One study that applied transparent conductive films that do not contain rare elements to electrochemiluminescence was a report using a carbon-based transparent conductive film prepared by thermal decomposition of a photoresist (Non-Patent Document 2). However, achieving both high electrical conductivity and high optical transparency with such conductive polymers remains a challenge.

[0010] The present inventors have previously proposed that graphene, a transparent carbon material, can be used as a disposable electrode for electrochemiluminescence immunoassays to construct a system suitable for rapid and simple testing. The present inventors have successfully performed immunoassays of carcinoembryonic antigen (CEA), a cancer marker, using graphene electrodes fabricated by chemical vapor deposition (CVD), demonstrating and reporting that graphene transparent electrodes have excellent properties as electrodes for electrochemiluminescence immunoassays (Non-Patent Document 3). Research into the use of graphene electrodes for such electrochemiluminescence immunoassay applications has not been reported anywhere other than by the present inventors, and this is an original and unique technology.

[0011] Japanese Patent Application Publication No. 10-111293

[0012] S. Parveen, MS Aslam, L. Hu, and, G. (2012). https: / / doi.org / 10.1021 / la2042394.T. Watanabe et al., “Single-layer graphene as a transparent electrode for electrogenerated chemiluminescence biosensing”, Electrochemistry Communications, 138, 107290 (2022). https: / / doi.org / 10.1016 / j.elecom.2022.1

[0013] The present invention aims to provide a transparent conductive film that can be used in rapid and simple testing devices and a biochip using the same, particularly a transparent conductive carbon film that can be used in immunoassays that utilize electrochemiluminescence and a biochip using the same.

[0014] As described above, the inventors have demonstrated that CVD graphene electrodes possess properties suitable for electrochemiluminescence immunoassays, which are suitable for rapid and simple testing. However, the challenge of antibody modification to graphene electrodes needed to be overcome in order to utilize them in immunoassays. To address this challenge, the inventors have investigated various methods for binding graphene to antibody molecules, including a covalent bond via diazonium salt reduction and a bond utilizing the π-π interaction between pyrene groups and graphene. However, these methods have not been able to secure a sufficient amount of antibody modification due to the two-dimensional nature of graphene. Furthermore, modification methods utilizing covalent bonds have encountered problems such as the destruction of the π-conjugated system in graphene, resulting in increased sheet resistance. Consequently, it has been impossible to simultaneously immobilize antibodies to graphene electrodes and maintain their properties. Therefore, the inventors conceived a method for immobilizing proteins on a polymer film, which is used as a support material in the transfer process required for the fabrication of CVD graphene electrodes. Conventional graphene transfer methods use polymethyl methacrylate (PMMA) as a support material. A PMMA film is formed on a graphene film grown on a metal catalyst substrate, and the metal catalyst substrate is then etched to transfer the laminate consisting of the PMMA and graphene film to any substrate. A CVD graphene electrode is obtained by dissolving and removing the PMMA film after transfer or before use as an electrode. The inventors first considered using the PMMA film, which serves as the transfer support film, as a membrane for protein immobilization without removing it. However, graphene electrodes with the PMMA film still laminated on them were unable to perform electrochemical measurements because the electrolyte containing the electrochemiluminescent substance did not sufficiently permeate the PMMA film. After extensive research, the inventors came up with the idea of ​​using a porous membrane instead of the PMMA membrane, which can ensure sufficient transport of electrochemiluminescent reactants through the membrane. Using an electrode consisting of this porous membrane and a graphene membrane, they successfully performed electrochemiluminescence immunoassays. The present invention was completed based on the above findings and includes the following aspects:

[0015] One aspect of the present invention relates to: [1] a laminate comprising a transparent conductive film and a porous film laminated on the transparent conductive film, wherein the porous film is permeable to an electrolyte solution. Here, in one embodiment of the laminate of the present invention, [2] the laminate according to [1] above, wherein the porous film has pores with an average pore diameter of 20 nm or more. In another embodiment of the laminate of the present invention, [3] the laminate according to [1] or [2] above, wherein the pore area ratio to the film surface of the porous film is 20% or more. In another embodiment of the laminate of the present invention, [4] the laminate according to any of [1] to [3] above, wherein the porous film has a film thickness of 100 nm or more. In another embodiment of the laminate of the present invention, [5] the laminate according to any of [1] to [4] above, wherein the laminate further includes a transparent insulating substrate, wherein the porous film is laminated on a first surface of the transparent conductive film, and the transparent insulating substrate is laminated on a second surface of the transparent conductive film. In one embodiment of the laminate of the present invention, [6] the laminate according to [5] above, further comprising an electrical conductor, wherein the electrical conductor is laminated on the surface of the porous film, on the surface opposite to the surface on which the transparent conductive film is laminated, or on the surface of the transparent insulating substrate, on the same surface as the surface on which the transparent conductive film is laminated. In one embodiment of the laminate of the present invention, [7] the laminate according to any of [1] to [6] above, characterized in that at least a portion of the porous film has a compressed structure. In one embodiment of the laminate of the present invention, [8] the laminate according to any of [5] to [7] above, characterized in that the transparent insulating substrate is coated with a transparent conductive additive. In one embodiment of the laminate of the present invention, [9] the laminate according to any of [1] to [4] above, further comprising an electrical conductor, wherein the transparent conductive film is laminated on a first surface of the porous film, and the electrical conductor is laminated on a second surface of the porous film.In one embodiment, the laminate of the present invention is:

[10] the laminate according to any one of [1] to [9] above, wherein the porous film is a film made of a material selected from the group consisting of nitrocellulose, cellulose acetate, polyethersulfone, polytetrafluoroethylene, polyamide, polyvinylidene fluoride, regenerated cellulose, polycarbonate, polypropylene, polyvinylidene chloride, aluminum oxide, glass fiber, quartz fiber, polymethyl methacrylate, polystyrene, polyethylene, polyethylene terephthalate, and ceramic, or a mixed film made of two or more materials selected from the group. In one embodiment, the laminate of the present invention is:

[11] the laminate according to any one of [1] to

[10] above, wherein the transparent conductive film is a carbon conductive film. In one embodiment, the laminate of the present invention is:

[12] the laminate according to any one of [1] to

[11] above, wherein the transparent conductive film is a graphene film.

[0016] Another aspect of the present invention relates to:

[13] a biochip comprising the laminate described in any one of [5] to

[12] above. Another aspect of the present invention relates to:

[14] a kit comprising the biochip described in

[13] above and an electrochemiluminescent substance. Another aspect of the present invention relates to:

[15] the laminate described in [5] above, further comprising a transparent conductive film, a transparent insulating substrate, and an electrical conductor, wherein the laminate is stacked in the following order: transparent insulating substrate, transparent conductive film, porous film, transparent conductive film, transparent insulating substrate, and the electrical conductor is arranged so as to contact the transparent conductive film. Another aspect of the present invention relates to:

[16] a method of using the laminate described in [5] above as a transparent electrode, wherein a solvent having the same refractive index as that of the porous film is used. Another aspect of the present invention relates to

[17] a method for detecting a target compound by electrochemiluminescence immunoassay using the laminate according to any one of [5] to

[12] above or the biochip according to

[13] above, the method comprising: (a) a step of binding the target compound to an electrochemiluminescent substance; (b) a step of capturing the target compound in a porous membrane of the laminate, wherein the target compound is captured by a substance that specifically binds to the target compound and is immobilized in the porous membrane; and (c) a step of applying a potential to the laminate and measuring electrochemiluminescence after the steps (a) and (b). Another aspect of the present invention relates to

[18] a method for producing a laminate in which a transparent insulating substrate, a carbon conductive film, and a porous film are laminated in this order, the method further comprising: (a) a step of forming a carbon conductive film on a metal catalyst substrate by a CVD method; (b) a step of further forming a porous film on the carbon conductive film to produce a laminate; and (c) a step of removing the metal catalyst substrate by etching and transferring the laminate onto a transparent insulating substrate so that the carbon conductive film is in contact with the transparent insulating substrate. In one embodiment, the method for producing a laminate of the present invention is as follows:

[19] the method for producing a laminate according to the above

[18] , characterized in that in the step (b), the solvent for dissolving the polymer used to form the porous film is a mixed solvent containing a good solvent and a poor solvent for the polymer.

[0017] The laminate of the present invention, which is composed of a transparent conductive film, a porous film, and a transparent insulating substrate, allows proteins such as antibodies to be immobilized on the porous film, enabling electrochemiluminescence immunoassays using the laminate as an electrode. Because the laminate of the present invention, which is composed of a transparent conductive film, a porous film, and a transparent substrate, does not contain rare elements, it is inexpensive to manufacture and can be used as a disposable electrode, making it suitable for use in rapid and simple testing devices. Furthermore, when used in electrochemiluminescence immunoassays, the laminate of the present invention enables efficient detection of luminescence generated within the porous film without attenuation, thereby contributing to the high sensitivity of rapid and simple testing devices.

[0018] FIG. 1 is a schematic diagram showing one embodiment of a laminate according to the present invention. The laminate comprises a porous membrane and a transparent conductive film. FIG. 2 is a schematic diagram showing one embodiment of a laminate according to the present invention. The laminate comprises a porous membrane, a transparent conductive film, and a transparent insulating substrate. FIG. 3 is a schematic diagram showing one embodiment of a biochip according to the present invention. FIG. 4AB is a schematic diagram showing a modified embodiment of a biochip according to the present invention. FIG. 4CD is a schematic diagram showing a modified embodiment of a biochip according to the present invention. FIG. 4E is a schematic diagram showing a modified embodiment of a biochip according to the present invention. FIG. 4F is a schematic diagram showing a modified embodiment of a biochip according to the present invention. FIG. 4G is a schematic diagram showing a modified embodiment of a biochip according to the present invention. FIG. 4H is a schematic diagram showing a modified embodiment of a biochip according to the present invention. FIG. 5 shows a scheme for one embodiment of a method for producing a laminate according to the present invention. FIG. 6 shows a scheme for a conventional method for producing a CVD graphene electrode including a transfer step. FIG. 7 shows an SEM image of the porous membrane surface of a porous membrane / graphene laminate produced in Example 1 below. FIG. 8 shows a histogram of pore sizes present on the porous membrane surface of a porous membrane / graphene laminate prepared in Example 1 below. FIG. 9 shows a histogram of pore sizes present on the porous membrane surface of a porous membrane / graphene laminate prepared in Example 1 below. FIG. 10 shows a schematic diagram of the electrochemiluminescence measurement cell used in Example 4 below. FIG. 11 shows a photograph (FIG. 11A) of a porous membrane / graphene film / transparent insulating substrate laminate in the electrochemical measurement cell and a photograph (FIG. 11B) of electrochemiluminescence generation in Example 4 below. FIG. 12 is a graph showing the results of electrochemiluminescence measurement by cyclic voltammetry (CV) using a porous membrane / graphene film / transparent insulating substrate laminate as the working electrode in Example 4 below. FIG. 13 shows a schematic diagram of a three-electrode measurement chip used in electrochemiluminescence measurement in Example 5 below. FIG. 14 is a graph showing the results of electrochemiluminescence measurement using a laminate according to the present invention as a three-electrode measurement chip in Example 5 below. FIG. 15 is a graph showing the results of immunoassay based on electrochemiluminescence using the laminate according to the present invention in Example 6 below.Fig. 16 is a graph showing ECL intensities obtained by multiple ECL measurements using a cellulose membrane / graphene membrane laminate according to the present invention, as conducted in Example 7 below (left side of Fig. 16). For comparison, the results of ECL measurements using a graphene electrode are shown (right side of Fig. 16). Fig. 17 shows SEM images of the porous membrane surface of a porous membrane / graphene laminate prepared by a casting method in Example 8 below. Fig. 17(a) shows an image of a porous membrane formed using an acetone solvent, and Fig. 17(b) shows an image of a porous membrane formed using an acetone / formamide mixed solvent. Fig. 18 shows SEM images of the porous membrane surface of six types of porous membrane / graphene laminate prepared by a casting method in Example 8 below. The concentrations of the cellulose mixed ester solutions and the conditions for immersion in ultrapure water in Figures 18(a) to (f) are as follows: (a) 4% by mass, no immersion; (b) 4% by mass, with immersion; (c) 8% by mass, without immersion; (d) 8% by mass, with immersion; (e) 12% by mass, without immersion; and (f) 12% by mass, with immersion. Figure 19 shows a photograph of a porous cellulose mixed ester film / graphene film / quartz substrate laminate prepared in Example 8 below. Figure 20(a) shows a Raman spectrum of the porous cellulose mixed ester film / graphene film / quartz substrate laminate prepared in Example 8 below. Figure 20(b) shows a Raman spectrum of the graphene film on a quartz glass substrate from which the porous cellulose mixed ester film has been removed. Figure 21 is a graph showing the results of electrochemiluminescence measurement of the porous cellulose mixed ester film / graphene film / quartz substrate laminate prepared in Example 8 below. FIG. 21(a) shows a graph of the current-potential curve, and FIG. 21(b) shows a graph of the ECL intensity-potential curve. FIG. 22 is a schematic diagram showing the process for producing a porous cellulose film / graphene film laminate by the phase inversion method prepared in Example 9 below. FIG. 23 shows an SEM image of the cellulose film in a laminate consisting of a porous cellulose film / graphene film / copper foil prepared in Example 9 below. FIG. 23(a) shows an SEM image of the cellulose film in the laminate when the applicator gap height during production was 25 μm. Furthermore, FIGS. 23(b) to 23(d) show SEM images of the cellulose film in the laminate when the applicator gap height during production was 50 μm, 75 μm, and 100 μm, respectively.Figure 24 is a schematic diagram illustrating the protein adsorption measurement method used in Example 9 below. Figure 25 shows a calibration curve constructed based on the protein adsorption measurement results used in Example 9 below. Figure 26 shows the quantitative results of protein adsorption measured using four types of cellulose membranes and a commercially available nitrocellulose membrane in Example 9 below. Figure 27 shows a schematic diagram of the compression method for a porous structure using a hydraulic flask press used in Example 10 below. Figure 28 shows a photograph of a laminate consisting of a porous mixed cellulose ester membrane / graphene membrane on a quartz substrate with gold / chromium vapor-deposited on both ends, used in Example 10 below. Figure 29 shows photographs of the porous structure of a laminate consisting of a porous mixed cellulose ester membrane / graphene membrane on a quartz substrate before and after compression using an aluminum plate with 4 mm diameter holes, used in Example 10 below (the left side of Figure 29 shows the before-compression image, and the right side shows the after-compression image). Figure 30 shows an SEM image of the cellulose surface of a laminate having a compressed porous structure in part, prepared in Example 10 below. Figure 30(a) shows an SEM image of a compressed porous structure portion, and Figure 30(b) shows an SEM image of an uncompressed porous structure portion. Figure 31 is a graph (solid line) showing the results of electrochemiluminescence measurement of a porous cellulose mixed ester film / graphene film / quartz substrate laminate having a compressed porous structure in part, performed in Example 10 below. For comparison, the measurement results (dotted line) of a porous cellulose mixed ester film / graphene film / quartz substrate laminate without a compressed porous structure are shown. Figure 32 is a graph showing the current-potential curve of the ECL immunoanalysis of a porous cellulose mixed ester film / graphene film / quartz substrate laminate performed in Example 11 below. Figure 33 is a graph showing the ECL intensity-potential curve of a porous cellulose mixed ester film / graphene film / quartz substrate laminate performed in Example 11 below. Fig. 34 is a graph showing the transmittance measurement results (left) and Raman spectra (right) of a graphene / PEDOT:PSS electrode, a graphene electrode, and a PEDOT:PSS electrode, performed in Example 12 below. Fig. 35 is a graph showing the results of electrochemical measurements by CV using graphene, graphene / PEDOT:PSS, and glassy carbon electrodes, performed in Example 12 below.Figure 36(a) shows the results of ECL measurements of a graphene / PEDOT:PSS electrode, a graphene electrode, and a PEDOT:PSS electrode performed in Example 12 below, showing a graph of ECL intensity vs. potential curve. Figure 36(b) shows a graph showing the total luminescence intensity over 30 seconds from the start of potential application obtained by chronoamperometry. Figure 37 shows Ru(bpy) using graphene or graphene / PEDOT:PSS as an electrode, performed in Example 12 below. 3 Cl 2 37(a)) or tripropylamine (FIG. 37(b)). FIG. 38 is a graph showing the relationship between the refractive index and the glycerin ratio in a water / glycerin mixed solvent, as measured in Example 13 below. FIG. 39 is a graph showing the transmittance spectra of a porous PVDF film in glycerin / water mixed solutions with various ratios, as measured in Example 13 below. FIG. 40 is a graph showing the transmittance spectra of a PVDF / graphene / quartz substrate laminate in a water / glycerin solution, as measured in Example 13 below. FIG. 41 is a schematic diagram of a film-shaped electrochromic device prepared in Example 13 below. FIG. 42 is a graph showing the current-voltage curve of a film-shaped electrochromic device prepared in Example 13 below. FIG. 43 is a photograph showing the reversible color change between a colored state and a bleached state of a film-shaped electrochromic device prepared in Example 13 below.

[0019] One aspect of the present invention provides a laminate comprising a transparent conductive film and a porous film laminated on the transparent conductive film, wherein the porous film has permeability to an electrolyte solution. One embodiment of the laminate according to this aspect is shown in Figure 1. As shown in Figure 1, the laminate 1 comprises a transparent conductive film 2 and a porous film 3.

[0020] The transparent conductive film 2 is a film that combines high electrical conductivity and visible light transmittance. Examples of transparent conductive films 2 that can be used in the present invention include, but are not limited to, thin metal wires such as indium tin oxide, fluorine-doped tin oxide, zinc oxide, tin oxide, titanium oxide, and silver nanowires, conductive polymers such as polyethylenedioxythiophene (PEDOT), and carbon-based transparent conductive films such as carbon nanotubes and graphene. In a preferred embodiment, the transparent conductive film 2 can be used as an electrode in an electrochemiluminescence immunoassay. In this case, the transparent conductive film 2 may be used as either a working electrode or a counter electrode.

[0021] Because the transparent conductive film 2 is transparent to visible light, a photodetector can be placed on the transparent conductive film side of the laminate when used in electrochemiluminescence immunoassays. Furthermore, in embodiments where the laminate further includes a transparent insulating substrate, a photodetector can be placed on the transparent insulating substrate side of the laminate. This enables electrochemiluminescence detection near the light-emitting interface, increases the collection angle, and prevents reabsorption of the electrochemiluminescence signal by components in the solution, thereby enabling high sensitivity. Furthermore, when the laminate is used as a biochip for electrochemiluminescence immunoassays, high sensitivity is achieved because the luminescence from the electrochemiluminescent substance immobilized in the porous film can be efficiently collected. In the electrochemiluminescence process of a biochip including the laminate, luminescence occurs when the active species generated by the electrode reaction of the coreactant reach the electrochemiluminescent substance before being deactivated, so the luminescence from the electrochemiluminescent substance immobilized in the porous film near the transparent conductive film is the main source of luminescence. If a non-light-transparent conductive film were used, the photodetector would need to be placed on the surface of the porous film opposite the conductive film, and luminescence generated near the electrode would attenuate within the porous film before reaching the photodetector. On the other hand, when a laminate consisting of a transparent conductive film and a porous film is used, the distance from the light-emitting site to the photodetector is short, making it possible to detect electrochemiluminescence without significant attenuation.

[0022] In this specification, the term "transparent conductive film" refers to a conductive film having a light transmittance of at least 50% or more, preferably 75% or more, and more preferably 90% or more. The light transmittance can be measured using, for example, an ultraviolet-visible spectrophotometer.

[0023] The transparent conductive film 2 preferably has low electrical resistance, for example, a sheet resistance of 2000 Ω / sq or less. A sheet resistance exceeding 2000 Ω / sq is undesirable because a large voltage drop occurs within the transparent conductive film when a current flows through the film during electrochemical measurement, limiting the current and reducing the luminescence intensity. In a more preferred embodiment, the sheet resistance of the transparent conductive film 2 is 1000 Ω / sq or less, and even more preferably 500 Ω / sq or less. Sheet resistance is the actual electrical resistance of a conductive film, defined as the specific resistance / film thickness. By reducing the specific resistance of the transparent conductive film and increasing its film thickness, the sheet resistance can be adjusted to a desirable value. However, increasing the film thickness reduces light transmittance, which may result in a decrease in the intensity of the electrochemiluminescence signal obtained in electrochemiluminescence measurement. In a preferred embodiment, the transparent conductive film 2 is a transparent carbon conductive film, and in a more preferred embodiment, the transparent conductive film 2 is a graphene film.

[0024] The transparent carbon conductive film is a conductive film having optical transparency and made of a carbon material such as graphene, graphite, glassy carbon, carbon nanotubes, fullerene, etc. The transparent carbon conductive film also includes a transparent conductive film produced by thermal decomposition of a polymer material such as a photoresist, as disclosed in Non-Patent Document 2.

[0025] Methods for forming a transparent carbon conductive film are known to those skilled in the art. Any known method suitable for each carbon conductive film can be used. For example, the following can be used.

[0026] When a graphene film is used as a transparent carbon conductive film, the graphene film may be a single layer or may be formed of multiple layers. When the graphene film is formed of multiple layers, it is preferably formed of two to three layers from the viewpoint of light transmittance, but is not limited to this. The graphene film may be doped by substituting carbon atoms of graphene with nitrogen or boron, or by molecular adsorption. In a multilayer graphene film, metal chlorides or the like may be intercalated between layers. The graphene film is preferably a continuous film. A continuous film refers to a film in which the components constituting the film are continuously connected without holes or tears. A continuous graphene film is preferable because it has a uniform surface and can reduce sheet resistance. In this specification, the term "single-layer graphene film" includes a multilayer graphene film as a part of the term, but also includes a graphene film substantially formed of a single-layer graphene film. A graphene film substantially formed of a single-layer graphene film refers, for example, to a graphene film in which the area of ​​the multilayer graphene film on the graphene film is 15% or less, 10% or less, 5% or less, or 3% or less. When the area of ​​the multilayer graphene film is 3% or less, the coverage rate of the single layer graphene in the graphene film is 97% or more.

[0027] Methods for forming a graphene film are known to those skilled in the art (see, for example, Non-Patent Document 3), and it is preferable to form the graphene film by, for example, chemical vapor deposition (CVD). Note that graphene films formed by known methods such as mechanical peeling, chemical peeling, SiC pyrolysis, and graphene oxide reduction can also be used as long as the laminate 1 functions.

[0028] The porous film 3 is laminated on the first surface of the transparent conductive film 2. The porous film 3 may be laminated so as to cover the entire surface of the transparent conductive film 2, or may be laminated so as to cover only a portion of the surface. The porous film 3 may be permeable to an electrolyte. Permeability to an electrolyte means that the target compound for detection in electrochemiluminescence, the electrochemiluminescence labeling compound, the coreactant, cations such as sodium ions, anions such as chloride ions, and water molecules contained in the electrolyte immersed in the porous film 3 can pass through the porous film 3 and penetrate to or near the surface of the transparent conductive film 2. Being permeable to an electrolyte allows the electrochemiluminescent substance and the coreactant in the electrolyte to approach the surface of the transparent conductive film 2, enabling electron transfer between these substances and the transparent conductive film 2 when a potential is applied to the transparent conductive film 2. In other words, the porous film 3 has continuous pores from one surface to the other, allowing the electrochemiluminescent substance and the coreactant to pass through the film.

[0029] Examples of the porous membrane 3 that can be used in the present invention include, but are not limited to, membranes made of a material selected from the group consisting of nitrocellulose, cellulose acetate, polyethersulfone, polytetrafluoroethylene, polyamide, polyvinylidene fluoride, regenerated cellulose, polycarbonate, polypropylene, polyvinylidene chloride, aluminum oxide, glass fiber, quartz fiber, polymethyl methacrylate, polystyrene, polyethylene, polyethylene terephthalate, and ceramic, or mixed membranes made of two or more materials selected from the above group. Furthermore, the porous membrane 3 may be a laminate of two or more types of porous membranes.

[0030] The structure and pore size of the porous membrane 3 can be optimized as appropriate. For example, it is desirable to optimize the thickness taking into consideration the combination with other constituent materials in the biochip of the present invention. While not limited to the following, the thickness of the porous membrane 3 is preferably 10 nm to 100 μm. If the thickness is thinner than 10 nm, it will be smaller than the size of the antibody, and the benefit of increasing the amount of modification by using a porous membrane to make the modified site three-dimensional will not be obtained. If the thickness is thicker than 100 μm, the radical species generated by the electrode reaction of the coreactant in the electrochemiluminescence process will be deactivated faster than they react with the electrochemiluminescent labeling substance immobilized on the porous membrane, resulting in a decrease in luminescence intensity, which is undesirable. In preferred embodiments, the lower limit of the thickness of the porous membrane 3 is 100 nm or more, and in more preferred embodiments, it is 300 nm or more. In preferred embodiments, the upper limit of the thickness of the porous membrane 3 is 50 μm or less, and in more preferred embodiments, it is 10 μm or less.

[0031] In an embodiment in which a graphene film produced by CVD is used as the transparent conductive film 2, the porous film 3 is preferably capable of supporting the graphene film grown on a metal catalyst substrate after the metal catalyst substrate is removed by etching in order to transfer the graphene film to a desired substrate. For the porous film 3 to function as such a support film, the thickness of the porous film 3 is preferably 100 nm or more. If the thickness is less than 100 nm, the support force of the graphene film formed by CVD is insufficient, increasing the likelihood of tearing during transfer. Furthermore, when transferring a carbon conductive film such as a graphene film to a hydrophilic substrate such as a glass substrate, the thickness of the porous film 3 is preferably 200 μm or less. Since the internal stress of the porous film increases with increasing thickness, a thickness greater than 200 μm may cause the transferred film to peel off from the substrate.

[0032] Although not limited to the following, the average pore size of the porous membrane 3 is preferably 20 nm to 20 μm. If the average pore size is less than 20 nm, other components such as retained particles (e.g., antibodies) and blocking agents may clog the pores of the porous membrane, inhibiting the movement of components in the solution. If the average pore size exceeds 20 μm, the density of the porous membrane decreases, weakening the supporting force during graphene film transfer and increasing the likelihood of membrane tearing, which is undesirable. In a preferred embodiment, the average pore size of the porous membrane 3 is 200 nm to 10 μm. The average pore size of the porous membrane 3 refers to the average value of the pore sizes of the pores present on the surface of the porous membrane. The average pore size of the pores is determined by observing the surface of the porous membrane using a scanning electron microscope (SEM) or the like and measuring the area of ​​several hundred (e.g., 300) randomly selected pores. From the area of ​​each pore, the diameter of each pore, assuming that the pore is circular, is calculated as the pore size, and the average of these values ​​can be used as the surface average pore size.

[0033] Although not limited thereto, it is preferable that the area ratio of the pores to the membrane surface of the porous membrane 3 is 20% or more. If the area ratio of the pores to the membrane surface is less than 20%, the electrolyte permeability of the porous membrane 3 decreases, which is undesirable. The upper limit of the area ratio of the pores to the membrane surface is not limited as long as the porous membrane 3 functions as a transfer support membrane for the transparent conductive film 2, but can be, for example, 60% or less. In a preferred embodiment, the area ratio of the pores to the membrane surface is 25% or more, and in a more preferred embodiment, the area ratio of the pores to the membrane surface is 30% or more. The area ratio of the pores to the membrane surface of the porous membrane 3 refers to the ratio of the total area of ​​all pores present on one surface of the porous membrane to the geometric area of ​​that surface. The pore area is measured by observing the surface of the porous membrane using a SEM or the like.

[0034] In one embodiment, the porous film 3 is optically transparent at the emission wavelength of the electrochemiluminescent substance. In particular, it is preferable that the porous film 3 does not absorb the luminescence generated by electrochemiluminescence. When the porous film 3 is optically transparent, it means that it has a light transmittance of 50% or more. Preferably, it has a light transmittance of 75% or more, and more preferably, it has a light transmittance of 90% or more. The light transmittance can be measured using, for example, a UV-visible spectrophotometer.

[0035] In one embodiment, the porous membrane 3 has the ability to adsorb proteins. Protein adsorption ability means that proteins such as antibodies for electrochemiluminescence immunoassays can be immobilized on the porous membrane so as to be measurable. Protein adsorption ability can be evaluated by quantifying the amount of protein contained in a solution before and after adsorption onto the porous membrane 3 using a Bradford reagent or the like. The ability of the porous membrane 3 to adsorb proteins facilitates the immobilization of proteins required for electrochemiluminescence immunoassays. The term "protein" as used herein is not limited as long as it can be used in immunoassays. Examples include, but are not limited to, antibodies, or fragments or variants thereof, lectins, and protein portions (domains, polypeptides).

[0036] In one embodiment, the porous membrane 3 may contain an immobilized compound. In the present invention, the compound immobilized on the porous membrane 3 is a substance that specifically binds to the target compound. Such a specific binding substance is not limited to proteins, as long as it can be immobilized on the porous membrane 3 and can immobilize the target compound within the porous membrane 3 through specific interaction. Examples of such specific binding substances include proteins, peptides, amino acids, lipids, carbohydrates, DNA, RNA, receptors, haptens, etc., and are not particularly limited in terms of molecular weight or origin (natural or synthetic). Preferred examples include antibodies or antigens that can be used in immunoassays that utilize immune reactions. Other specific binding substances may include low-molecular-weight compounds, high-molecular-weight compounds, organic compounds, inorganic compounds, polysaccharides, polymers, lectins, and compounds composed of combinations thereof. The method for immobilizing these compounds on the porous membrane 3 is not limited as long as electrochemiluminescence immunoassays are possible; known methods for immobilizing compounds on porous membranes, such as physical adsorption or chemical bonding, can be used. Furthermore, the term "electrochemiluminescence immunoassay" as used herein is not limited to electrochemiluminescence assays that utilize antigen-antibody reactions, but may also refer to electrochemiluminescence assays that utilize the binding between compounds as described above.

[0037] In one embodiment, the laminate of the present invention further includes a transparent insulating substrate, with a porous film laminated on a first surface of the transparent conductive film and a transparent insulating substrate laminated on a second surface of the transparent conductive film. One embodiment of this laminate is shown in FIG. 2. As shown in FIG. 2, laminate 1' is composed of a transparent conductive film 2, a porous film 3, and a transparent insulating substrate 4. The transparent insulating substrate 4 is not limited to any substrate that can transmit the electrochemiluminescent light generated on the transparent conductive film 2, and any known transparent insulating substrate can be used. By using a transparent insulating substrate, the light generated by electrochemiluminescence can be captured by a photodetector installed on the transparent substrate 4 side of laminate 1. By installing the photodetector on the transparent substrate 4 side of laminate 1, the distance from the light-emitting site to the photodetector can be shortened, thereby improving the light capture efficiency. Transparent insulating substrates that can be used in the present invention include, but are not limited to, quartz, glass, other transparent glass materials, polyethylene terephthalate, polyester, acrylic resin, polyethylene, nylons, polyvinyl chloride, polyimide, etc.

[0038] In one embodiment, the transparent insulating substrate 4 may further include other components used in measuring electrochemiluminescence, such as a conductive electrode or a conductive additive. The conductive electrode may be in direct contact with the transparent conductive film and can pass current, and its shape and material are not limited. For example, a conductive electrode made of chromium or gold can be used. Known conductive additives can be used. An example of a transparent conductive additive is a composite (PEDOT:PSS) made of polyethylenedioxythiophene and polystyrene sulfonic acid. When the transparent insulating substrate 4 is coated with a conductive additive, a porous film / transparent conductive film laminate is laminated on the surface of the transparent insulating substrate 4 coated with the conductive additive.

[0039] In one embodiment, the laminate according to the present invention can be used as an electrode for electrochemical measurements. When used for electrochemical measurements, it can be used as the working electrode or counter electrode in a two-electrode system consisting of a working electrode and a counter electrode, a three-electrode system consisting of a working electrode, a counter electrode, and a reference electrode, or an electrode system of four or more electrodes. In a preferred embodiment, the laminate is used as the working electrode.

[0040] When the laminate according to the present invention is used as an electrode for electrochemical measurements, since a porous film is formed on the solution side, the laminate is less likely to peel off or break from the substrate and has excellent durability compared to graphene electrodes that do not have a typical porous film laminated thereon, etc. Although it depends on the measurement conditions, the laminate according to the present invention can be used multiple times (2, 3, 4, 5, 6, 7, 8, 9, 10 or more times) as an electrode for electrochemical measurements.

[0041] Another aspect of the present invention provides a biochip including a laminate in which a porous film, a transparent conductive film, and a transparent insulating substrate are laminated in this order. The biochip according to the present invention is preferably a biochip for electrochemical measurements. More preferably, it is a biochip for electrochemiluminescence immunoassays. A schematic diagram of one embodiment of the biochip according to the present invention is shown in FIG. 3. As shown in FIG. 3, the biochip 11 includes a laminate in which a transparent conductive film 2, a porous film 3, and a transparent insulating substrate 4 are laminated. A substance that specifically binds to a target compound is immobilized on the porous film 3. A conduction electrode 5 is laminated partially between the transparent conductive film 2 and the transparent insulating substrate 4. The biochip 11 further includes a membrane 6 on the surface of the porous film 3 of the laminate 1, and further includes an electrical conductor 7, a conjugate pad 8, and an absorbent pad 10 on the surface of the membrane 6. The conjugate pad 8 further includes a sample pad 9. The biochip 11 having such a configuration enables electrochemiluminescence immunoassays by placing the transparent substrate 4 side facing the photodetector 12. The schematic diagram shown in FIG. 3 shows only one example, and the biochip of the present invention is not limited to this configuration as long as it can be used for electrochemiluminescence immunoassay.

[0042] When a sample containing a premixed target compound and coreactant is supplied to the sample pad 9 of such a biochip, the target compound passes through the sample pad 9 and flows downstream to the conjugate pad 8. In the conjugate pad 8, the target compound and the electrochemiluminescent-labeled compound come into contact with each other to form a complex, which then passes through the pad. The complex and coreactant are then spread onto the membrane 6, which is placed in contact with the underside of the conjugate pad. The complex and coreactant spread onto the membrane 6 infiltrate the porous membrane 3 of the laminate 1. A specific binding substance that binds to the target compound is immobilized on a portion of the porous membrane 3, where the complex binds and is immobilized. Since the electrochemiluminescent-labeled compound is bound to the immobilized complex, applying a voltage between the transparent conductive film 2 and the electrical conductor 7 causes an electrode reaction of the coreactant, which then reacts with the electrochemiluminescent substance to produce electrochemiluminescence. The target compound is detected by measuring this luminescence with a photodetector 12.

[0043] In one embodiment, the biochip of the present invention includes a laminate formed by laminating a transparent conductive film, a porous film, and a transparent substrate, and a membrane. In another embodiment, the biochip of the present invention includes a laminate formed by laminating a transparent conductive film, a porous film, and a transparent insulating substrate, a membrane, and an electrical conductor. In another embodiment, the biochip of the present invention includes a laminate formed by laminating a transparent conductive film, a porous film, and a transparent insulating substrate, a membrane, an electrical conductor, and a conjugate pad. In another embodiment, the biochip of the present invention includes a laminate formed by laminating a transparent conductive film, a porous film, and a transparent insulating substrate, a membrane, an electrical conductor, a conjugate pad, and a sample pad. Additionally, the biochip may be configured for use in a lateral flow immunochromatographic detection method using a known test strip such as a nitrocellulose membrane. Such a configuration is disclosed, for example, in Japanese Patent Publication No. 6,464,308. Either the laminate or the additional electrical conductor included in the biochip may be used as the working electrode, as long as one is the working electrode and the other is the counter electrode.

[0044] 4A to 4F show exemplary embodiments of biochips. FIG. 4A shows a biochip having a conduction electrode 5 partially between a laminate 1 and a transparent insulating substrate 4. FIG. 4B shows a biochip in which a laminate 1 and an electrical conductor 7 are stacked in this order on a transparent insulating substrate 4, and the conduction electrode 5 partially between the laminate 1 and the transparent insulating substrate 4. FIG. 4C shows a biochip in which a laminate 1 and an electrical conductor 7 are stacked independently on the same surface of the transparent insulating substrate 4, and the conduction electrode 5 partially between the laminate 1 and the transparent insulating substrate 4. FIG. 4D shows a biochip in which two laminates 1 and electrical conductors 7 are stacked independently on the same surface of the transparent insulating substrate 4, and the conduction electrode 5 partially between the laminate 1 and the transparent insulating substrate 4. FIG. 4E shows a biochip having three transparent conductive films and one electrical conductor 7, each independent of the other, on the same surface of a transparent insulating substrate 4, with one conduction electrode 5 between the three laminates 1 and the transparent insulating substrate 4. FIG. 4F shows the biochip shown in FIG. 3, further comprising a reference electrode 13 on the transparent insulating substrate. FIGS. 4G and 4H show the biochip shown in FIG. 4F, but with multiple laminates 1. FIGS. 4G and 4H also show embodiments in which electrochemiluminescence is measured using an image sensor 14 instead of the photodetector 12. In the embodiments shown in FIGS. 4C to 4E, a membrane is placed in contact with the laminate 1 and the electrical conductor 7, and an electrolyte is infiltrated into the membrane, so that the transparent conductive film 2 and the electrical conductor 7 form a two-electrode system.

[0045] The membrane 6 can be made of any material that allows the analyte, electrochemiluminescent labeling reagent, and coreactant to permeate and develop. Examples include, but are not limited to, porous membranes made of polyethylene, polyethylene terephthalate, nylons, glass, polysaccharides such as cellulose and cellulose derivatives such as nitrocellulose, or ceramics. In a preferred embodiment, the membrane 6 does not absorb the emission wavelength of electrochemiluminescence. In a more preferred embodiment, the membrane 6 is transparent to light at the emission wavelength of electrochemiluminescence.

[0046] The electrical conductor 7 is used as a counter electrode or a working electrode in a two-electrode system, a three-electrode system, or an electrode system having four or more electrodes for electrochemical measurement. Known electrodes used in measuring electrochemiluminescence can be used as the electrical conductor 7. For example, platinum, gold, silver, copper, stainless steel, nickel, aluminum, and carbon electrodes can be used. The electrical conductor 7 can be fixed to the membrane 6 using an adhesive, a pressing member, or the like. In a preferred embodiment, the electrical conductor 7 functions as a reflective material. The electrical conductor 7 reflects photons emitted in the direction opposite the transparent insulating substrate from electrochemiluminescence generated near the surface of the transparent conductive film 2 of the biochip, thereby improving the light collection efficiency of the photodetector. Materials for the electrical conductor 7 include, but are not limited to, platinum, gold, silver, copper, stainless steel, nickel, aluminum, and graphene films formed on these metal substrates.

[0047] The conjugate pad 8 contains an electrochemiluminescent labeling reagent that specifically reacts with the target substance. The method for producing the conjugate pad containing the reagent is not limited, and it can be produced, for example, by impregnating the conjugate pad with the reagent and drying it. Suitable materials for the conjugate pad include, but are not limited to, paper, cellulose mixtures, nitrocellulose, polyester, acrylonitrile copolymers, glass fibers, and nonwoven fibers such as rayon.

[0048] The sample pad 9 is a portion that serves as a sample supply portion for receiving a sample, and includes any substance and form that can absorb a liquid sample when molded into a pad and allow the liquid and components of the substance to be detected to pass through. Materials for the sample pad 9 include, but are not limited to, glass fiber, acrylic fiber, hydrophilic polyethylene material, dry paper, paper pulp, woven fabric, etc. The sample pad 9 may also have the function of the conjugate pad 8. The sample pad 9 may additionally contain suitable reagents, such as a red blood cell agglutinating agent or a blocking reagent.

[0049] The configuration and form of the membrane 6, conjugate pad 8, sample pad 9, and absorbent pad 10, the materials of each component, and the method of stacking and holding each component together can be those used in known immunochromatography. In addition to the above configuration, the biochip of the present invention may also have a configuration such as an additional pad, a reference electrode, or a reflective material that is placed between the sample pad 9 or conjugate pad 8 and the porous membrane to remove components unnecessary for detecting the target substance.

[0050] In electrochemiluminescence immunoassays using the laminate or biochip of the present invention, the target compound can be any compound that can be captured in a porous membrane by a specific binding substance and detected by electrochemiluminescence immunoassay. Examples of such target compounds include low molecular weight compounds, high molecular weight compounds, organic compounds, inorganic compounds, polysaccharides, polymers, lipids, nucleic acids and their analogs, polypeptides, proteins, antibodies, lectins, and compounds formed by combinations thereof. In preferred embodiments, the target compound is a compound that is present or likely to be present in a biological sample. Suitable examples of such target compounds include microorganisms such as bacteria and viruses, and disease-related markers such as cancer markers. More specifically, examples of target compounds include proteins, polypeptides, amino acids, nucleic acids (DNA, RNA), and sugar chains contained in a biological sample.

[0051] As used herein, biological samples refer to, for example, tissues, cells, body fluids, or peritoneal lavage fluid. The term "body fluid" as used herein refers to a liquid biological sample collected from a living organism. Examples include blood (including serum, plasma, and interstitial fluid), cerebrospinal fluid (cerebrospinal fluid), urine, feces, saliva, lymph, digestive fluid, ascites, pleural effusion, periradicular fluid, and extracts of various tissues or cells. Blood is preferred. Depending on the compound derived from the biological sample, a sample that has been pretreated, such as purified or concentrated, may be used. For purification or concentration of the biological sample, appropriate known methods can be used depending on the target detection target.

[0052] Another aspect of the present invention provides an electrochemiluminescence immunoassay kit comprising the biochip described above. The kit comprises at least the biochip and may also comprise other reagents necessary for the assay (e.g., a reagent containing an electrochemiluminescent substance, a reagent containing a coreactant, and an electrolyte), a sample dilution solution, test tubes, devices for collecting, storing, or transporting biological samples, and an instruction manual.

[0053] Another aspect of the present invention provides a method for detecting a target compound by electrochemiluminescence immunoassay using the laminate or biochip according to the present invention described above. The detection method includes the following steps: (a) binding the target compound to an electrochemiluminescent substance; (b) capturing the target compound in the porous membrane of the laminate, where the target compound is captured by a substance that specifically binds to the target compound and is immobilized in the porous membrane; and (c) applying a potential to the laminate to measure electrochemiluminescence after steps (a) and (b). In the detection method according to the present invention, either the step (a) of binding the target compound to an electrochemiluminescent substance or the step (b) of capturing the target compound in the porous membrane of the laminate can be performed first. That is, the detection method according to the present invention may include step (a) followed by step (b), or step (a) followed by step (b), and both embodiments are included.

[0054] Electrochemiluminescence immunoassay is a method in which a target compound is captured on or near a working electrode using an antigen-antibody reaction or compound-compound binding, and then an electrochemiluminescent substance is further bound to the captured target compound, causing electrochemiluminescence on the working electrode and detecting the target compound. The laminate used in the detection method of the present invention is composed of a transparent conductive film, a porous film, and a transparent insulating substrate, and does not contain rare elements, making it inexpensive to manufacture and disposable. Therefore, it is suitable for use in rapid, simple tests and POCT devices.

[0055] Known electrochemiluminescent substances can be used in electrochemiluminescent immunoassays using the laminate or biochip of the present invention. Examples of electrochemiluminescent substances or coreactants include those disclosed in S. Parveen, MS Aslam, L. Hu, and G. Xu, Electrogenerated Chemiluminescence. Protocols and Applications, Heidelberg, 2013, pp. 18-31 and 44-60, and Z. Liu et al., "Recent advances in electrochemiluminescence," Chemical Society Reviews, 44, pp. 3117-3142 (2015). https: / / doi.org / 10.1039 / C5CS00086F, and Japanese Patent No. 3574457. Examples include, but are not limited to, a combination of tris(2,2'-bipyridyl)ruthenium(II) and its co-reactant tripropylamine, a combination of tris(2,2'-bipyridyl)ruthenium(II) and its co-reactant 2-(di-n-butylamino)ethanol, and a combination of luminol and its co-reactant hydrogen peroxide.

[0056] The detection method of the present invention includes (a) a step of binding a target compound to an electrochemiluminescent substance. The electrochemiluminescent substance binds to the target compound via a structure that specifically binds to the target compound. Such a structure preferably includes, but is not limited to, an antibody. That is, the electrochemiluminescent substance includes an electrochemiluminescent-labeled compound. An example of an electrochemiluminescent-labeled compound is an antibody bound to a compound such as tris(2,2'-bipyridyl)ruthenium(II). To bind the target compound to the electrochemiluminescent substance, the two compounds can be mixed in a solution. The solution can be appropriately selected depending on the target compound and the electrochemiluminescent substance used. Commonly used buffers, such as, but not limited to, phosphate buffer, Tris buffer, and Good's buffer, can be used. The pH of the buffer is preferably in the range of 6.0 to 9.5 and can be appropriately set depending on the properties of the target compound and the electrochemiluminescent substance used. Mixing conditions can be, for example, gentle mixing using a shaker at 37°C for 30 minutes. When step (a) is carried out after step (b), a solution containing an electrochemiluminescent substance may be added to the porous membrane so that the target compound captured in the porous membrane binds to the electrochemiluminescent substance. If necessary, the electrochemiluminescent substance that has not bound to the target compound may be washed away with a buffer solution or the like.

[0057] The detection method of the present invention includes (b) a step of capturing a target compound in a porous membrane of a laminate, in which the target compound is captured by a substance that specifically binds to the target compound and is immobilized in the porous membrane. To capture the target compound in the porous membrane, a substance that specifically binds to the target compound is immobilized in the porous membrane. The method for immobilizing the specific binding substance to the porous membrane is not limited, and known methods for immobilizing compounds to porous membranes, such as physical adsorption or chemical bonding, can be used. For example, a solution containing a desired protein (e.g., an antibody against an antigen) can be adjusted to a predetermined concentration (e.g., 0.1 to 5 mg / mL) and a certain amount of this solution can be applied to the porous membrane. In this way, the protein can be immobilized to the porous membrane. The solution for applying the specific binding substance to the porous membrane is not limited to the following, but commonly used buffers such as phosphate buffer, Tris buffer, and Good's buffer can be suitably used. The pH of the buffer is preferably in the range of 6.0 to 9.5 and can be set appropriately depending on the properties of the specific binding substance. The buffer solution may further contain salts such as NaCl, stabilizers and preservatives such as sucrose, antiseptics such as Proclin, etc. Salts include those such as NaCl that are added to adjust the ionic strength, as well as those such as sodium hydroxide that are added in the process of adjusting the pH of the buffer solution. After the specific binding substance is immobilized on the porous membrane, a commonly used blocking agent can be further used in solution or vapor form to cover the specific binding substance immobilization site or other areas, thereby performing blocking.

[0058] A solution containing the target compound is infiltrated into the porous membrane on which the specific binding substance has been immobilized as described above. This allows the target compound to be captured within the porous membrane. In one embodiment, the method further includes a washing step of washing away excess target compound after the step of capturing the target compound within the porous membrane.

[0059] The solution for infiltrating the target compound into the porous membrane and the washing solution can be the same as the solution used to coat the porous membrane with a specific binding substance. Alternatively, an electrolyte solution used in electrochemiluminescence immunoassays can be used. Examples of electrolyte solutions suitable for electrochemiluminescence immunoassays using the laminate of the present invention as an electrode include, but are not limited to, commonly used buffer solutions such as phosphate buffer, Tris buffer, and Good's buffer. The electrolyte also contains a coreactant. The concentration of the coreactant is, but is not limited to, 0.01 to 0.3 mol / L, for example. The electrolyte may also contain other components such as a surfactant. Examples of surfactants include, but are not limited to, Tween 20, Tween 80, and Triton X-100. The concentration of the surfactant is, but is not limited to, 0.01 to 2% by mass, for example.

[0060] The detection method according to the present invention includes (c) a step of applying a potential to the laminate and measuring electrochemiluminescence after steps (a) and (b). Through steps (a) and (b), a target compound is captured in the porous membrane of the laminate, and an electrochemiluminescent substance is bound to the target compound. By immersing this laminate in an electrolyte solution containing a coreactant and applying a potential, the electrochemiluminescent substance in the porous membrane generates electrochemiluminescence. By measuring the generated electrochemiluminescence, the target compound can be detected qualitatively or quantitatively. An additional electrode is used in this case so that it is in contact with the electrolyte. The position of the additional electrode is not limited as long as a current flows between it and the transparent conductive film. Either the additional electrode or the transparent conductive film may be the working electrode.

[0061] A potential is applied to the working electrode using a voltage supply source such as a potentiostat, depending on the potential at which an electrode reaction of the coreactant contained in the electrolyte occurs. For example, when an electrolyte containing tripropylamine (TPrA) as a coreactant is used, the potential of the working electrode is swept from 0 V to 1.6 V relative to the silver / silver chloride reference electrode. At this time, TPrA is oxidized on the working electrode at a potential range of around 0.8 V and even higher to form tripropylamine radical cations (TPrAH +) is generated near the surface of the working electrode. + Some of the hydrogen ions (H + ), which is converted into a tripropylamine radical (TPrA·). TPrA· moves through the electrolyte and reacts with the target compound and a specific binding substance to tris(2,2'-bipyridyl)ruthenium(II) (Ru(bpy)), an electrochemiluminescent substance immobilized on the porous membrane. 3 2+ ), upon collision with or near Ru(bpy) 3 2+ is reduced by TPrA to Ru(bpy) 3 + Furthermore, H + TPrAH not released + Ru(bpy) 3 + When it collides with or reaches the vicinity of Ru(bpy), 3 + is oxidized to the excited state Ru(bpy) 3 2+* is generated, and the ground state Ru(bpy) 3 2+ When the light returns to the original state, it emits light. The luminescence intensity can be measured using commercially available photodiodes or photomultiplier tubes. Photomultiplier tubes can measure weaker light than photodiodes, allowing for more sensitive measurements. It is also possible to use an imaging device such as a CMOS image sensor. Using an imaging device makes it possible to obtain an image of the luminescence distribution on the working electrode. Therefore, by pre-coating different types of specific binding substances at different positions on the porous membrane, it can be used as a test line and a control line in immunochromatography, or for multi-item analysis.

[0062] Another aspect of the present invention provides a method for using the above-described laminate as a transparent electrode. This method for using the laminate as a transparent electrode is characterized by using a solvent with the same refractive index as the porous membrane. This method, for example, enables ECL immunoassays to be captured by a photodetector without scattering within the porous membrane. This allows for a clearer boundary between luminescent and non-luminescent regions. This method contributes to the integration of multiple test items when associating the luminescent position of an analytical device with multiple test items. Those skilled in the art can adjust the refractive index of the solvent used when using the laminate as an electrode to match the refractive index of the porous membrane. Examples of such solvents include a combination of solvents with different refractive indices, such as glycerin and water, and adjusting the composition ratio to match the refractive index of the porous membrane. There are no particular restrictions on the solvent that can be used, as long as it does not interfere with the use of the laminate as an electrode.

[0063] Another aspect of the present invention provides a laminate that can be used as an electrochromic device. The laminate comprises a transparent insulating substrate, a transparent conductive film, a porous film, a transparent conductive film, and a transparent insulating substrate, stacked in this order. By adding a solvent having the same refractive index as the porous film to the porous film, the laminate can function as an electrochromic device using two transparent conductive films as a working electrode and a counter electrode. Such a laminate may also include an electrical conductor in contact with the transparent conductive film. Furthermore, the graphene film in the laminate may be electrodeposited with Prussian blue or silver.

[0064] Another aspect of the present invention provides a method for producing a laminate in which a transparent insulating substrate, a carbon conductive film, and a porous film are laminated in this order. The method for producing the laminate includes the following steps: (a) forming a carbon conductive film on a metal catalyst substrate by a CVD method, (b) further forming a porous film on the carbon conductive film to form a laminate, and (c) removing the metal catalyst substrate by etching and transferring the laminate onto a transparent insulating substrate so that the carbon conductive film is in contact with the laminate. A scheme of the production method according to the present invention is shown in Figure 5.

[0065] Conventionally, when manufacturing an electrode having a graphene film as a carbon conductive film, a process has been included in which a PMMA film is formed as a transfer support film on a graphene film formed on a metal catalyst substrate, and then the metal catalyst substrate is etched and transferred to the desired substrate, followed by removal of the PMMA film. However, according to the manufacturing method of the present invention, which includes the above process, a porous film can be formed instead of the transfer support film and serve the role of the transfer support film. This eliminates the need for a transfer support film removal step, thereby reducing the labor, time, and cost required for manufacturing. Furthermore, in conventional graphene film transfer methods using PMMA as a transfer support film, PMMA residue remains on the graphene film surface after PMMA removal. Such residue adversely affects the properties of the graphene film. In contrast, the manufacturing method of the present invention does not include a transfer support film removal step, thereby avoiding the above problem. Figure 6 shows a manufacturing scheme for a graphene electrode using a conventional transfer support film.

[0066] The method for producing a laminate according to the present invention includes (A) a step of forming a graphene film on a metal catalyst substrate by a CVD method. Methods for forming a graphene film 2′ on a metal catalyst substrate 15 by a CVD method are known, and can be carried out by referring to, for example, Non-Patent Document 3. The metal catalyst substrate 15 that can be used in the present invention is not limited, and any known substrate used for forming a graphene film 2′ can be used. Preferred examples include copper substrates, nickel substrates, cobalt substrates, iridium substrates, platinum substrates, gold substrates, and alloy substrates thereof. Alternatively, a heat-resistant substrate on which these metals are vapor-deposited may be used.

[0067] After forming a graphene film on the metal catalyst substrate in step (A), step (B) is carried out to further form a porous film on the graphene film. The method for forming the porous film 3 on the graphene film is not limited, and known methods such as spin coating, spray coating, a coating method using an applicator or bar coater, and vapor deposition can be used. Hereinafter, a method for forming a porous film by spin coating will be described.

[0068] A polymer, which is the raw material for the porous film 3, is dissolved in a solvent to prepare a porous film-forming solution. An appropriate polymer can be selected depending on the porous film 3 to be formed. One or more types of polymers may be used to form the porous film 3. It is known that when forming the porous film 3 by spin coating, the thickness and average pore size of the porous film change depending on conditions such as the solvent selected, the concentration of the polymer in the solvent, the rotation speed of the spin coater, the viscosity of the solution, and the average molecular weight of the polymer (which affects the viscosity). Those skilled in the art can appropriately set the above conditions to form a porous film with the desired thickness and average pore size depending on the polymer and solvent used. The following are examples of conditions for forming the porous film 3 by spin coating, but are not limited to these.

[0069] The solvent is not limited as long as it can dissolve the polymer and form a porous film by spin coating. Examples of solvents that can be used include acetone, methanol, diethyl ether, and ethyl acetate. A low-boiling solvent is preferred. In a preferred embodiment, the solvent has a boiling point of 100°C or less, and in a more preferred embodiment, the solvent has a boiling point of 80°C or less. Low-boiling solvents generally have a fast evaporation rate, so using a low-boiling solvent increases the precipitation rate of the polymer in the solution, resulting in random precipitation of the polymer, which is preferable, and thus forms a porous structure. In one embodiment, the solvent is preferably a mixed solvent of a good solvent and a poor solvent for the polymer. In a mixed solvent of a good solvent and a poor solvent, as the solvent evaporates, the mixed solvent gradually changes to a bad solvent as the good solvent decreases, resulting in phase separation. This phase separation promotes the formation of porous polymers. Those skilled in the art can appropriately select the good solvent and poor solvent for the polymer. For example, when the polymer is cellulose acetate, an acetone / formamide mixed solvent can be used. Another example of a mixed solvent is acetone / dimethyl sulfoxide. However, the mixed solvent is not limited to these. The mixing ratio of the good solvent to the poor solvent is not limited as long as the formation of porosity is promoted. For example, the volume ratio of good solvent to poor solvent can be 99:1 to 1:1. The concentration of the polymer in the solvent is not limited to the following, but can be, for example, 0.5 to 20 mass%. A laminate of a metal catalyst substrate 15 and a graphene film 2' is fixed on the stage of a spin coater, and the prepared porous film forming solution is dripped onto the surface and near the center of the graphene film 2'. The amount of the dripped porous film forming solution is sufficient as long as it sufficiently covers the graphene film 2'. The rotation speed and rotation time of the spin coater are not limited as long as the desired porous film can be formed. For example, the rotation speed can be 200 to 5000 rpm, and the rotation time of the spin coater can be 10 to 120 seconds. After that, if any solvent remains, it is dried by heating.

[0070] In a preferred embodiment, the porous film 3 can be formed on the graphene film by a phase inversion method, such as casting using an applicator. Phase inversion is a method of making a material, such as a polymer, porous by converting it from a liquid phase to a solid phase under controlled conditions. Representative phase inversion methods include nonsolvent-induced phase separation and thermally induced phase separation. Nonsolvent-induced phase separation involves two distinct phenomena: the evaporation of a solvent in a polymer solution containing a nonsolvent or poor solvent, destabilizing the polymer solution and resulting in the precipitation of the polymer in the presence of the nonsolvent; and the nonsolvent contacting the polymer and simultaneously extracting the solvent into the nonsolvent, resulting in the infiltration of the nonsolvent into the polymer solution, destabilizing the polymer solution and resulting in the precipitation of the polymer. The former is called the dry phase inversion method, and the latter is called the wet phase inversion method. There is also a dry / wet phase inversion method, which combines the two. The method for forming a porous film by the phase inversion method is known, and reference can be made, for example, to Masahiro Tamura, Tadashi Uragami, Mizuho Sugihara, "Permeation Characteristics on Cellulose Nitrate-Cellulose Acetate Blend Polymer Membranes," Journal of the Japan Society of Color Material, Vol. 50 (6), 317-322 (1977). The solvent used in the phase inversion method can be the same as that used in the spin coating method. The concentration of the polymer in the solvent can be 0.5 to 20% by mass.

[0071] After forming a porous film on the graphene film in step (A), step (C) is performed to remove the metal catalyst substrate by etching. Known methods can be used to remove the metal catalyst substrate 15. For example, when copper foil is used as the metal catalyst substrate 15, etching with an iron (III) nitrate solution is possible. If graphene is also formed on the back side of the metal catalyst substrate 15, where the porous film 3 is not formed, the graphene film on the back side is removed using oxygen plasma treatment or the like before etching the metal catalyst substrate 15. The porous film 3 / graphene film 2′ / metal catalyst substrate 15 is floated in an etching solution so that the surface from which the graphene film has been removed comes into contact with the etching solution, and the metal catalyst substrate 15 is removed. After removing the metal catalyst substrate 15, the laminate consisting of the porous film 3 and the graphene film 2′ is washed by transferring it to the surface of a pure water pool. The washing process is preferably performed three or more times. The laminate 1 floating on the pure water is then scooped up using any transparent insulating substrate 4. After scooping up, the laminate 1 is dried, completing the graphene transfer process. Before this scooping, it is preferable to form a conduction electrode 5 for conducting graphene on the transparent insulating substrate 4 in advance. The graphene film 2' is scooped so that a part of the graphene film 2' is placed on the conduction electrode 5. In this way, a laminate 1' consisting of the graphene film 2', the porous film 3, and the transparent insulating substrate 4 can be produced.

[0072] The present invention will be specifically described below using examples, but the present invention is not limited to the following embodiments.

[0073] Example 1: Production of a Laminate Composed of Graphene Film and Porous Film In this example, a laminate composed of a single-layer graphene film and a cellulose film (porous film) (hereinafter also referred to as a "porous film / graphene laminate") was produced as follows. Copper foil (35 μm) was prepared as a metal catalyst substrate for graphene chemical vapor deposition (CVD) growth. Prior to graphene film formation by CVD, the copper foil was immersed in pure water, ethanol, and acetone, successively, and subjected to ultrasonic treatment to clean the copper foil surface. Thereafter, the copper foil was transferred to a thermal CVD furnace, and hydrogen was introduced, and hydrogen annealing of the copper substrate was performed for 30 minutes under conditions of a hydrogen atmosphere total pressure of 700 Pa and 1000°C. Thereafter, methane was introduced, and graphene was grown by CVD for 10 minutes at a total pressure of 750 Pa, with a flow rate of 2 sccm of methane and 20 sccm of hydrogen.

[0074] A porous film was fabricated on a graphene film formed on copper foil using spin coating. The support layer for graphene transfer was made of nitrocellulose (CN), cellulose acetate (CA), or a mixed film of nitrocellulose and cellulose acetate (cellulose mixed ester film (MCE)). Nitrocellulose (Nacalai Tesque, product number 24728-34), cellulose acetate (Sigma-Aldrich, product number 419028), and acetone as a solvent were prepared as raw materials for the porous film formation solution. The solution for porous film formation was prepared by mixing cellulose acetate or nitrocellulose with acetone so that the cellulose acetate or nitrocellulose content was 2% by mass. Three types of cellulose mixed ester solutions with different compositions were also prepared by mixing nitrocellulose, cellulose acetate, and acetone so that the total content of both nitrocellulose and cellulose acetate was 2% by mass and the mass ratios of nitrocellulose to cellulose acetate were 3:1, 1:1, and 1:3. For comparison, a PMMA solution, which has traditionally been used as a support film for graphene transfer, was prepared. A PMMA solution (Sigma-Aldrich, product number 182265) was prepared by dissolving it in ethyl lactate as a solvent to a content of 4% by mass. Next, the porous film-forming solution was dropped onto a graphene film formed on a copper foil, and spin coating was performed at 2000 rpm to form a nitrocellulose film, a cellulose acetate film, or a mixed cellulose ester film. Under similar conditions, a PMMA film serving as a transfer support film was formed on the graphene film formed on the copper foil. After forming the porous film or transfer support film, the unnecessary graphene film formed on the backside of the copper foil was removed by oxygen plasma treatment. This resulted in a laminate consisting of a porous film / graphene film / copper foil. A comparative example was also obtained, consisting of a PMMA film (transfer support film) / graphene film / copper foil laminate.

[0075] An etching tank was prepared, and a copper etching solution of an aqueous iron (III) nitrate solution (0.5 mol / L) was stored in the tank at 25°C. The size of the porous film / graphene film / copper foil laminate to be subjected to copper etching was 15 mm x 10 mm. The laminate was floated in the copper etching solution so that the copper foil was in contact with the solution, and the copper foil of the laminate was removed by etching for 5 hours. This resulted in a porous film / graphene film laminate comprising a porous film and a graphene film. A PMMA film (transfer support film) / graphene film laminate was also obtained as a comparative example.

[0076] The porous membrane surface of the prepared porous membrane / graphene membrane laminate was observed using a SEM (FE-SEM, manufactured by ZEISS), and the pore size and the percentage of the surface occupied by the pores were measured from the captured SEM images. The sample used for SEM observation was a porous membrane / graphene membrane laminate formed on a copper foil after spin coating, with a 3 nm coating of platinum. Similarly, the surface of a PMMA membrane was also observed as a comparative example. Figure 7 shows an SEM image. The PMMA membrane had a smooth surface and formed a dense membrane structure without any pores. The CN membrane and CA membrane contained pores, but these were composed of small pores, with no pores larger than 100 nm. The CA membrane also had a surface with a low pore density. All prepared cellulose mixed ester membranes had a porous structure, and a tendency for the pore diameter to increase with increasing nitrocellulose mass ratio was observed. The diameters of all pores visible in the SEM images were estimated using the scale bar as a reference. The pore diameter data was used to calculate the pore surface occupancy, which is the area ratio of the pores to the membrane surface of the porous membrane in the CN membrane. For the cellulose mixed ester membrane, the SEM image was converted to a black-and-white image, and the proportion of black areas was calculated as the pore surface occupancy. Figures 8 and 9 show the pore size distribution (histograms) for each sample. The histograms were created from the diameter values ​​of all pores visible in the SEM image in Figure 7. Therefore, histograms are shown for the PMMA membrane, in which no pores were observed, and the CA membrane, which had a low pore density. The CN membrane had only pores with diameters of 40 nm or less, with an average pore diameter of 17 nm. The pore surface occupancy for the CN membrane was 2.1%. The cellulose mixed ester membrane with a CN:CA = 1:3 ratio had only pores with diameters of 150 nm or less, with an average pore diameter of 49 nm. The CN:CA=1:1 and CN:CA=3:1 cellulose mixed ester membranes had pores of 150 nm or larger, with average pore diameters of 140 nm and 880 nm, respectively. The CN:CA=3:1 membrane had many large pores with diameters of approximately 550 nm, and also had a pore distribution with even larger pore sizes of 1.5 μm or larger. Furthermore, the surface occupancies of the pores in the CN:CA=1:3, CN:CA=1:1, and CN:CA=3:1 cellulose mixed ester membranes were 38%, 40%, and 32%, respectively.

[0077] Example 2: Production of a Laminate Comprising a Porous Film, a Graphene Film, and a Transparent Insulating Substrate In this example, the porous film / graphene film laminate produced in Example 1 was transferred onto a transparent insulating substrate to produce a laminate comprising a porous film, a graphene film, and a transparent insulating substrate. A quartz substrate (1 mm thick, 20 mm × 20 mm) was prepared as the transparent insulating substrate. Chromium was deposited to a thickness of 10 nm on a portion of this quartz substrate using a vacuum deposition apparatus, and gold was further deposited to a thickness of 50 nm on the chromium. This metal-deposited film functions as a conductive electrode when the porous film / graphene film laminate is laminated on the quartz substrate. A water tank filled with ultrapure water was prepared, and the porous film / graphene film laminate, which had been copper-etched and was floating in the etching solution, was transferred to the water surface of the prepared water tank and washed with water. The laminate was then repeatedly washed by transferring it to another water tank. This water-washing process was performed three times. The porous film / graphene film laminate floating in a pool of ultrapure water was scooped up using a quartz substrate on which chromium and gold had been vapor-deposited as a conductive electrode. The porous film / graphene film laminate was stacked so that a portion of the conductive electrode overlapped the porous film / graphene film laminate. In this way, a laminate consisting of a quartz substrate (transparent insulating substrate), a porous film, and a graphene film was produced.

[0078] The thickness of the porous film on the laminate was measured using a stylus step gauge (manufactured by BRUKER). The thickness of the laminate on the quartz substrate manufactured using a 2% by weight cellulose acetate and nitrocellulose mixed solution (CN:CA = 3:1) was approximately 400 nm. On the other hand, the thickness of the laminate manufactured using an ethyl lactate solution containing 4% by weight PMMA was approximately 150 nm.

[0079] Example 3: Verification of Transfer Support Ability of Porous Film In this example, the transfer support ability of a porous film in the etching process of a metal catalyst substrate or the subsequent transfer process to a transparent insulating substrate was verified. A porous film was formed on a graphene film under the same conditions as in Example 1, except that an acetone solution with a 1% by mass concentration of nitrocellulose was used. The thickness of the porous film formed on the graphene film was less than 100 nm. When copper foil was etched after the porous film formation, the film broke due to insufficient support strength. Furthermore, a porous film was formed on a graphene film under the same conditions as in Example 1, except that an acetone solution with a 6% by mass concentration of nitrocellulose or a 4% by mass concentration of cellulose acetate was used. The thickness of the porous film formed on the graphene film was 1 μm or more. The graphene film was able to be supported in the copper foil etching process after porous film formation, but some peeling from the quartz glass substrate was observed after transfer to the quartz glass substrate. This means that the internal stress of the support film increased with increasing film thickness, and the stress exceeded the adhesive force between the graphene and the quartz substrate. Furthermore, it is believed that under these support film formation conditions, a porous structure sufficient to relieve stress was not formed. On the other hand, when a PET substrate was used instead of a quartz substrate, no peeling occurred even when the porous film was 1 μm or thicker. When a support film with a thickness of about 1 μm was used, the film's high flexibility is thought to result in stronger adhesion to the PET substrate than to a quartz substrate with a smooth surface.

[0080] Example 4: Evaluation of a Laminate Composed of a Graphene Film and a Porous Film, and Electrochemiluminescence Measurement The applicability of the porous film / graphene film laminate transferred onto a quartz glass substrate produced in Example 2 to electrochemiluminescence measurement was examined. Electrochemiluminescence measurement was performed using the quartz substrate with the deposited film and the laminate composed of a porous film and a graphene film finally obtained in Example 2. The measurement cell shown in FIG. 10 was used for the electrochemiluminescence measurement. The porous film / single-layer graphene film laminate deposited on the quartz substrate produced in Example 2 was used as the working electrode, and a gold / chromium deposited film was used as the conductive electrode. A silver / silver chloride electrode manufactured by BAS was used as the reference electrode, and a platinum wire (Φ0.5 mm) manufactured by Nilaco was used as the counter electrode. In this example, an electrochemiluminescence system was employed that used tris(2,2'-bipyridyl)ruthenium(II) as the luminescent material and tripropylamine as the coreactant. The electrolyte used was a 0.15 mol / L phosphate buffer solution (pH 7.4) containing 10 mmol / L tripropylamine and 1 mmol / L tris(2,2'-bipyridyl)ruthenium(II). A measurement cell was constructed by placing a 4 mm diameter O-ring on top of the porous membrane / graphene film laminate and sandwiching it between PTFE resin blocks. A photomultiplier tube (H12690-300, manufactured by Hamamatsu Photonics) was placed on the quartz substrate side of the laminate as a photodetector to measure the electrochemiluminescence intensity.

[0081] Using cyclic voltammetry (CV), the potential of the working electrode, a porous film / graphene film / transparent insulating substrate laminate, was swept from 0 V to 1.4 V relative to a reference electrode, while measuring the current flowing between the working electrode and the counter electrode and the amount of electrochemiluminescence generated at the working electrode surface. Figure 11 shows a photograph of the electrode surface when a porous film / graphene film laminate consisting of a cellulose mixed ester film with a CN:CA ratio of 3:1 was used as the working electrode, demonstrating that luminescence was observed from the entire area in contact with the electrolyte. These results indicate that the electrolyte permeated the entire porous film surrounded by the O-ring, causing tripropylamine and tris(2,2'-bipyridyl)ruthenium(II) to react on the graphene film, resulting in electrochemiluminescence. Figure 12 shows the results of electrochemiluminescence measurements using a nitrocellulose film / graphene film laminate or a cellulose mixed ester porous film / graphene film laminate as the working electrode. An increase in current due to the oxidation reaction of tripropylamine was observed from 0.8 V. Additionally, an increase in current due to the oxidation reaction of tris(2,2'-bipyridyl)ruthenium(II) was observed around 1.0 V. At the same time, electrochemiluminescence was confirmed to occur around 1.0 V. In the CA / graphene film laminate, almost no current flowed, and electrochemiluminescence could not be observed. In the CN / graphene film laminate, both the current and electrochemiluminescence intensity were lower than in the cellulose mixed ester film. The current increasing from 1.2 V in the current-potential curve (CV curve) of the CN / graphene film laminate is likely due to the electrolysis of the solvent, water. Based on the SEM images, the pore size on the surface of the CN film was small and the surface occupancy of the pores was low. This suggests that the low luminescence intensity was due to the low amount of luminescent material and co-reactants that penetrated the CN film and reached the graphene film. When comparing the three types of mixed cellulose ester porous membrane / graphene membrane laminates, the sample with a CN:CA mass ratio of 1:3 used as the working electrode showed lower current and electrochemiluminescence intensity than the other two samples. From the SEM images, this is thought to be due to the smaller pore size of the CN:CA = 1:3 sample compared to the other two types of mixed cellulose ester membranes.The sample with a CN:CA ratio of 1:3 had an average pore size of approximately 50 nm, and all of the pores were 150 nm or smaller, whereas the other two types of cellulose mixed ester membranes had many pores 150 nm or larger. These results suggest that a relatively large pore size is desirable for increasing electrochemiluminescence intensity.

[0082] Example 5: Fabrication of a three-electrode measurement chip and electrochemiluminescence measurement A three-electrode measurement chip was fabricated by laminating a nitrocellulose membrane on a porous film / graphene film laminate laminated on a transparent insulating substrate, and then laminating a platinum counter electrode on the membrane, and its applicability for electrochemiluminescence measurement was verified. A schematic diagram of the fabricated three-electrode chip for electrochemiluminescence measurement is shown in Figure 13. A silver / gold / chromium vapor-deposited film (silver electrode) is formed on a transparent insulating substrate 4, in addition to the porous film / graphene film laminate 1 and the gold / chromium vapor-deposited film of its conduction electrode 5. The fabricated electrochemiluminescence measurement chip has a three-electrode system consisting of the porous film / graphene film laminate 1 as the working electrode, a silver electrode as the reference electrode 13, and a platinum counter electrode (electrical conductor 7) used as the counter electrode.

[0083] A porous film / graphene film laminate was prepared as in Example 1, and then transferred onto a quartz substrate on which chromium and gold had been vapor-deposited as in Example 2. The porous film was formed on the graphene film by spin coating using an acetone solution containing a total of 2% by weight of nitrocellulose and cellulose acetate (CN:CA = 3:1). In this example, a silver / gold / chromium vapor-deposited film was formed on the quartz substrate in addition to a gold / chromium vapor-deposited film. When transferring the porous film / graphene film laminate to the quartz substrate, the porous film / graphene film laminate was lifted up with the quartz substrate so as to overlap the gold / chromium vapor-deposited film but not the silver / gold / chromium vapor-deposited film. Subsequently, a nitrocellulose membrane (Cytiva, AE98, no backing sheet, thickness: 105-140 μm) was laminated on the quartz substrate on which the porous film / graphene film laminate had been transferred, overlapping both the porous film / graphene film laminate and the silver / gold / chromium vapor-deposited film. Furthermore, a platinum counter electrode was laminated on the nitrocellulose membrane as a counter electrode to prepare a three-electrode measurement chip. A silver / gold / chromium vapor-deposited film vapor-deposited on a quartz substrate was used as a reference electrode for electrochemiluminescence measurement. The nitrocellulose membrane was impregnated with a phosphate buffer solution (pH 7.4) containing a concentration of 10 mmol / L tripropylamine and a concentration of 1 mmol / L tris(2,2'-bipyridyl)ruthenium(II), and CV measurement was performed. The conditions other than the cell structure used for the measurement were the same as in Example 4. The area of ​​the working electrode was 1 cm. 2As a comparison, a three-electrode measurement chip was also fabricated in the same manner, using a PMMA film / graphene film laminate, which was previously used as a transfer support film, as the working electrode, and electrochemiluminescence measurements were performed. Figure 14 shows the results of the electrochemiluminescence measurements. In the measurement chip using the cellulose mixed ester porous film / graphene film laminate as the working electrode, a current derived from the oxidation reaction of tripropylamine was observed starting at 0.6 V, and an increase in current derived from the oxidation reaction of tris(2,2'-bipyridyl)ruthenium(II) was confirmed starting at 0.8 V. Accordingly, an increase in luminescence intensity was confirmed starting at 0.8 V. On the other hand, when using a measurement chip using the PMMA / graphene film laminate as the working electrode, neither current nor electrochemiluminescence was observed. This is because, as shown in the SEM image in Figure 7, the fabricated PMMA film had a dense membrane structure, preventing the electrolyte from penetrating the PMMA film and resulting in no electrode reaction. Thus, it was confirmed that a three-electrode measurement chip using a porous film / graphene film laminate as the working electrode can be used for electrochemiluminescence measurements.

[0084] Example 6: Electrochemiluminescence Immunoassay Using Porous Membrane / Graphene Film Laminate In this example, to verify whether the porous membrane / graphene film laminate according to the present invention can be used as an electrode for electrochemiluminescence immunoassay, detection of carcinoembryonic antigen (CEA) was attempted by electrochemiluminescence immunoassay using a porous membrane / graphene film laminate. Specifically, an anti-CEA antibody was immobilized on the porous membrane of the porous membrane / graphene film laminate, and a solution containing CEA as an antigen and an anti-CEA antibody bound to tris(2,2'-bipyridyl)ruthenium(II) as a labeling substance was dropped onto the porous membrane, forming a sandwich-type immune complex on the porous membrane of the porous membrane / graphene film laminate through an antigen-antibody reaction. A 0.15 mol / L phosphate buffer solution containing 10 mmol / L tripropylamine, a co-reactant of tris(2,2'-bipyridyl)ruthenium(II), was used as the electrolyte. Tripropylamine was oxidized on the electrode and reacted with tris(2,2'-bipyridyl)ruthenium(II) that was bound to the immune complex as a label, and the resulting electrochemiluminescence was observed to confirm whether immunoassay was possible.

[0085] 6-1. Reagents ・Eclusis Reagent CEA II (containing biotinylated anti-CEA antibody and tris(2,2'-bipyridyl)ruthenium(II)-labeled anti-CEA antibody) (Roche Diagnostics, product number 570444-016) ・CEA Calibrator (containing CEA) (Roche Diagnostics, product number 316457) ・Blocking Reagent N101 (NOF Corporation)

[0086] 6-2. Preparation of Laminate Nitrocellulose (CN) and cellulose acetate (CA) were dissolved in acetone at a mass ratio of CN:CA = 3:1 and a solute concentration of 2 mass % to prepare a solution for forming a porous membrane.

[0087] Using the prepared porous film-forming solution, a laminate consisting of a graphene film and a porous film was produced under the same conditions as in Example 1, and transferred to a quartz glass substrate (20 mm × 20 mm × 1 mm). Prior to transfer, the quartz glass substrate was cleaned using the same procedure as for cleaning the copper foil used for CVD formation. The quartz glass substrate had a vapor-deposited electrode made of chromium and gold pre-installed as a conductive electrode. In the following electrochemiluminescence immunoassay, the laminate transferred to the quartz glass substrate was used as the working electrode.

[0088] 6-3. Electrochemiluminescence Immunoassay 20 μL of a solution containing 3 mg / L of biotinylated anti-CEA antibody (hereinafter also referred to as "capture antibody") was dropped onto the porous membrane of a porous membrane / graphene film laminate (hereinafter also referred to as "electrode") on a quartz substrate, and the solution was placed in a sealed container to prevent drying and allowed to stand at 37°C for 60 minutes. After standing for 60 minutes, the solution containing the capture antibody on the porous membrane was absorbed with a nonwoven fabric, and the electrode was immersed in a blocking solution and allowed to stand at 37°C for 30 minutes. The blocking solution used was a solution prepared by diluting blocking reagent N101 five-fold with pure water. The electrode was removed from the blocking solution and immersed in pure water for 60 seconds twice to wash off the blocking solution adhering to the electrode. After air-drying the electrode, 3 μL of a solution sample containing 40 ng / L CEA and 15 μL of a solution containing 4 mg / L tris(2,2'-bipyridyl)ruthenium(II)-labeled anti-CEA antibody (hereinafter also referred to as "labeled antibody") were dropped onto the porous membrane of the electrode. The electrode was then placed in a sealed container and left at 37°C for 90 minutes to form a sandwich-type immune complex on the porous membrane via an antigen-antibody reaction. As a negative control, an electrode was prepared by similarly immobilizing the capture antibody and blocking the electrode, but without adding CEA, but only adding the labeled antibody. After removing these electrodes from the sealed container, they were immersed in pure water for 60 seconds twice to remove unreacted labeled antibody and CEA. Using the same apparatus as in Example 2, electrochemiluminescence measurements were performed by sweeping the electrode potential from 0 V to 1.6 V using cyclic voltammetry. The electrolyte used was a 0.15 mol / L phosphate buffer solution (pH 7.4) containing 10 mmol / L tripropylamine.

[0089] 6-4. Results The results of the immunoassay using electrochemiluminescence are shown in Figure 15. As shown in Figure 15, by sweeping the potential toward a higher potential, an increase in current resulting from the oxidation reaction of tripropylamine was confirmed. Furthermore, in the sample to which the CEA sample was added, an increase in luminescence intensity was confirmed as the amount of current increased.

[0090] 6-5. Comparative Test and Results To confirm that the above immunoassay results were not due to luminescence from a labeled antibody not bound to CEA, but rather from an immune complex of the capture antibody-CEA-labeled antibody immobilized on the porous membrane, electrochemiluminescence measurements were performed under the same conditions as above using an electrode prepared by dropping only the labeled antibody onto a porous membrane on which the capture antibody had been immobilized. The results are shown by the dashed line in Figure 15. As shown in Figure 15, no luminescence was observed on the electrode on which the complex had not been immobilized. Therefore, it was confirmed that the luminescence was derived from the labeled antibody bound to the capture antibody on the porous membrane together with CEA, and not from an unbound labeled antibody. In this way, the laminate according to the present invention can be used in electrochemiluminescence immunoassays.

[0091] Example 7: Evaluation of Durability of Porous Film / Graphene Film Laminate When using a single-layer graphene as an electrode for electrochemical analysis, a substrate supporting graphene with a thickness of one atomic layer is required. The adhesion between the substrate and graphene is achieved solely by van der Waals forces acting between the substrate and graphene. Therefore, when the fluid flow in contact with the graphene is strong or when a solution with a different composition is substituted, the solution may penetrate between the substrate and graphene, causing partial breakage of the graphene. Breaks in the single-layer graphene reduce electrical conductivity, leading to a decrease in current value. Since the porous film of the porous film / graphene film laminate according to the present invention is formed on the solution side, it is believed to be less susceptible to peeling or breakage from the substrate than a typical graphene electrode without a porous film. Therefore, in this example, repeated electrochemiluminescence measurements were conducted to evaluate the durability of the porous film / graphene film laminate. For comparison, a similar test was also conducted on a graphene electrode without a porous film.

[0092] 7-1. Fabrication of Laminates and ECL Measurements For the porous membrane / graphene film laminate, graphene electrodes were used, transferred onto a cellulose mixed ester film (CN:CA = 3:1) prepared by spin coating. The fabrication method was the same as in Example 2. The graphene electrodes were fabricated using the PMMA support transfer method, as in Example 2. Using these electrodes, ECL measurements were performed by cyclic voltammetry (CV) using a 0.15 mol / L phosphate buffer solution (pH 7.4) containing 10 mmol / L tripropylamine and 0.1 mmol / L tris(2,2'-bipyridyl)ruthenium(II) as the electrolyte. Measurements were repeated 10 times for both electrodes, with the electrodes washed with PBS for solution exchange after each measurement. Furthermore, the sum of the solution resistance and graphene resistance (Rs) was measured by electrochemical impedance spectroscopy (EIS) before, after the fifth, and after the tenth measurement.

[0093] 7-2. Results Figure 16 shows the ECL intensity at 1.2 V for each electrode when ECL measurements were performed 10 times. The ECL intensity increased by the fifth measurement, which is thought to be due to the gradual oxidation of the graphene surface and changes in the surface state. The sudden decrease in the ECL intensity of the graphene electrode after the sixth measurement is thought to be due to partial tearing of the graphene electrode. On the other hand, the electrode fabricated using a cellulose / graphene film laminate (cellulose / graphene electrode) temporarily decreased in ECL intensity after the sixth measurement, but maintained a high ECL intensity from the seventh measurement onwards. Table 1 shows the Rs measurement results using EIS. Repeated ECL measurements increased Rs, which is due to an increase in the resistance of the graphene film. This is thought to be due to partial oxidation of the graphene film caused by the side reaction of water oxidation and mechanical damage to the graphene during solution exchange. The smaller increase in Rs for the cellulose / graphene electrode also suggests that the cellulose / graphene electrode was not mechanically damaged by tearing. From the above results, it is considered that the cellulose mixed ester porous film protects the graphene and improves its durability.

[0094]

[0095] Example 8: Preparation of porous membrane / graphene laminate by casting method When using a porous membrane / transparent conductive film laminate electrode in ECL immunoassay, it is preferable to have a large amount of antibody supported in the porous membrane. In this example, a cellulose mixed ester membrane was produced by a casting method using an applicator in order to increase the amount of antibody supported in the porous membrane, and a method for making the cellulose mixed ester membrane porous was investigated.

[0096] 8-1. Solvent Consideration The cellulose mixed ester membrane used in this example was fabricated with a mass ratio of CA:CN = 1:2. First, the solvent was considered. A porous membrane-forming solution was prepared by dissolving 4% by mass of cellulose mixed ester in two solvents: acetone and a mixed solvent of acetone and formamide (mass ratio 1:1). The solution was manually cast onto a copper substrate using an applicator with a gap height of 75 μm. Figure 17 shows an SEM image of the surface of the cellulose mixed ester membrane that had been cast and dried (platinum coating was used to suppress charge buildup). When acetone solvent was used, no pore structure was observed (Figure 17(a)), whereas when an acetone / formamide mixed solvent was used, a pore structure was observed (Figure 17(b)). Acetone is a good solvent for CA and CN, whereas formamide is a good solvent only for CN and a poor solvent for CA. In the acetone / formamide mixed solvent, as the solvent evaporates, the casting liquid gradually becomes a poor solvent and undergoes phase separation as the good solvent acetone evaporates. It is believed that this phase separation caused the support membrane to become porous in the acetone / formamide mixed solvent.

[0097] 8-2. Investigation of Phase Inversion Method and SEM Observation Next, we investigated a method of immersing the cellulose mixed ester in ultrapure water after casting to induce porosity through phase inversion. At the same time, we also evaluated the effect of the concentration of the cellulose mixed ester solution on the porous structure. CN and CA were dissolved in an acetone / formamide mixed solvent (1:1 mass ratio) to prepare a porous film-forming solution with cellulose mixed ester concentrations of 4, 8, and 12 mass%. The solution was manually cast onto a copper substrate using an applicator with a gap height of 75 μm. Two types of samples were prepared for each solute concentration: one that was dried after casting, and the other that was immersed in ultrapure water for 24 hours immediately after casting and then dried. The surfaces of the prepared cellulose mixed esters were coated with platinum, and their surface structures were observed by SEM. Figure 18 shows SEM images of the surfaces of six types of cellulose mixed ester membranes prepared ((a) without 4% immersion, (b) with 4% immersion, (c) without 8% immersion, (d) with 8% immersion, (e) without 12% immersion, and (f) with 12% immersion). At all solute concentrations, immersion in water after casting tended to increase the pore diameter. This is because the immersion in water caused the casting solution to gel, exchanging the dissolved solvent in the casting solution for water, resulting in phase inversion.

[0098] 8-3. Film Thickness Measurement The film thickness of the porous film measured by DekTak is shown in Table 2.

[0099]

[0100] The film thickness measurements showed a tendency for film thickness to increase with increasing solute concentration and immersion in water. The significant increase in porous film thickness upon immersion in water indicates that the water-immersed sample contains a large amount of voids. The film thickness increased because the amount of solute contained in the casting solution increased with increasing solute concentration. The significant increase in film thickness for the sample immersed in 12% by weight water is thought to be related to the viscosity of the porous film-forming solution. The increased viscosity likely reduced the fluidity of the solute, suppressing aggregation of solutes and thereby reducing the shrinkage of the porous film relative to the applicator gap. Table 3 shows the viscosity of the porous film-forming solution measured using a viscometer (Anton Paar, Model: Visco QC100, Spindle: SC4-21).

[0101]

[0102] 8-4. Transfer to Substrate Next, we investigated whether graphene grown on copper foil using these cellulose mixed esters could be transferred to a quartz substrate. Using a cellulose mixed ester film prepared using an acetone solvent solution, as in the sample described in 8-1 above, as a support material, we attempted to transfer graphene to a quartz substrate using the same procedure as in Example 2. As a result, we found that these laminates peeled off from the quartz substrate during the drying process after transfer, making them untransferable. On the other hand, all samples prepared using a porous-forming solution prepared with a formamide / acetone mixed solvent were successfully transferred. It is believed that the increased thickness of the samples prepared using an applicator compared to spin coating also increases the tensile stress. While the cellulose mixed ester film prepared from an acetone solvent solution did not form a porous structure, the acetone / formamide mixed solvent formed a porous structure, which likely alleviated the tensile stress and prevented peeling. Figure 19 shows a photograph of a porous cellulose mixed ester film / graphene film / quartz substrate laminate transferred to a quartz substrate using a support film with a solute concentration of 12% by mass immersed in water. It was found that by making the support film porous in this way, it became possible to transfer the porous film / graphene film laminate to a substrate without causing peeling, even if the thickness was 10 μm or more.

[0103] 8-4. Raman Spectrum Measurement The Raman spectrum of the sample shown in Figure 19 is shown in Figure 20(a). -1 and 2950 cm -1 Cellulose CH appears nearby 3 Peaks derived from the C-H and C-H bonds were observed, but the 2D peak and G peak derived from graphene were not observed. This is thought to be because the support film was porous and thick, causing the laser light to be scattered by the support film and preventing the laser light from reaching the graphene. Therefore, the cellulose mixed ester / graphene film / quartz substrate laminate was immersed in hot acetone for 20 minutes to remove the cellulose mixed ester film, which was the support film, before performing Raman spectroscopy analysis. Figure 20(b) shows the Raman spectrum of graphene after the support film was removed. The 2D peak and G peak derived from graphene were observed, and the peak at 1350 cm -1 Since almost no D peak, which indicates defects, was observed near 2950 cm, it can be said that high-quality graphene was produced even when a cellulose mixed ester film prepared by the casting method was used as a support material. -1 The peak due to the C--H of cellulose, which appears around this point, was not observed, which indicates that the cellulose mixed ester was successfully removed by immersion in hot acetone at 50°C.

[0104] 8-5. Electrical Resistance Measurement The sheet resistance of the porous cellulose mixed ester / graphene film / quartz substrate laminate transferred in the same manner as the sample shown in Table 4 in FIG. 19 was measured by the van der Pauw method, and the sheet resistance was 560 Ω / sq.

[0105] For comparison, graphene prepared by transfer using the conventional PMMA-supported transfer method had a sheet resistance of approximately 550 Ω / sq after the PMMA film was removed. This indicates that the graphene transferred using the cellulose mixed esters formed by the casting method is of high quality, similar to that prepared by the PMMA-supported transfer method.

[0106] 8-6. Electrochemiluminescence Measurements Figure 21 shows the results of electrochemiluminescence measurements performed on a cellulose mixed ester / graphene film / quartz substrate laminate prepared using the same procedure as the sample shown in Figure 19 , using it as an electrode. The measurement solution was 0.15 M phosphate buffer (pH 7.4) containing 10 mmol / L tripropylamine and 0.1 mmol / L ruthenium bipyridyl complex. In the current-potential curve shown in Figure 21(a), current associated with the oxidation reaction of tripropylamine begins to flow around 0.8 V, and in the ECL curve shown in Figure 21(b), an increase in ECL is observed around 1.0 V. This indicates that the pore structure of the cellulose mixed ester extends to the graphene, allowing reactants in the electrolyte to sufficiently reach the graphene and cause an electrochemical reaction. SEM observations, Raman spectroscopy, electrical resistance measurements, and ECL measurements indicated that the cellulose mixed ester membranes prepared using the casting method had a continuous porous structure from the surface to the interior and graphene membrane, even when the membrane was 10 μm thick or thicker.

[0107] Example 9: Protein Adsorption Amount of Porous Membrane Formed by Casting Method In this example, we investigated whether increasing the thickness of the cellulose mixed ester membrane could increase the antibody loading capacity of the porous cellulose mixed ester / graphene laminate membrane in order to improve the luminescence intensity in ECL immunoassays. In this example, the thickness of the porous membrane was increased by using an applicator. Furthermore, because cellulose membranes are less likely to become porous when a thick cellulose solution is applied, we adopted a wet phase inversion process in which the membrane is immersed in water after application of the cellulose solution to replace the solvent with water. Figure 22 shows the process for fabricating a porous cellulose membrane / graphene membrane using the phase inversion method. The cellulose solution used to fabricate the porous cellulose membrane was a 1:1 mixture of acetone and formamide, mixed with cellulose acetate and nitrocellulose in a 1:2 mass ratio to prepare a 12% solution by weight. (609 mPa·s). Four types of porous cellulose mixed ester membranes with different thicknesses were fabricated by varying the applicator gap height: 25 μm, 50 μm, 75 μm, and 100 μm. The gap width of the applicator was 60 mm. For applying the solution with the applicator, a fully automatic linear motion coater ALC-mini2 manufactured by Cortec Co., Ltd., which can control the running speed during film formation, was used.

[0108] 9-1. Fabrication of Laminate Specifically, a laminate was fabricated as follows. Graphene was grown on copper foil in the same manner as in Example 8. In this example, the running speed of the applicator during film formation was set to 2 mm / s, and the four types of porous cellulose mixed ester films with different thicknesses were formed on graphene. After the porous film-forming solution was applied to the graphene film, the resulting laminate was transferred to a pool of pure water and immersed for 1 hour. The laminate was then removed from the pure water and allowed to dry naturally, yielding a laminate consisting of a porous cellulose film / graphene film / copper foil.

[0109] 9-2. Surface Structure Analysis of Laminates To analyze the surface structure of the porous cellulose film / graphene film laminate formed on copper foil, the film surface was observed using a scanning electron microscope as in Example 1, and the average pore size and pore surface occupancy were calculated from the captured images. To investigate how the actual film thickness changes when the applicator gap height is changed, film thickness measurements were performed using a laser microscope. Figure 23 shows SEM images of cellulose films prepared by varying the film thickness under the condition of CA:CN = 1:2 (Figure 23(a) 25 μm, (b) 50 μm, (c) 75 μm, (d) 100 μm). Four types of samples were prepared by setting the applicator gap height to 25 μm, 50 μm, 75 μm, and 100 μm. Comparing the individual samples, it was observed that the cellulose fiber structure became thicker with increasing film thickness. Table 4 shows the film thickness, the average pore size and pore surface occupancy on the film surface.

[0110]

[0111] Comparing the four samples, we observed that the film thickness increased with the applicator gap height. Furthermore, the average pore size and pore surface area decreased with increasing film thickness. This is thought to be because thick films are less likely to undergo solvent replacement when the cellulose solution is applied with the applicator and then immersed in water, making it difficult for voids to form when dried.

[0112] 9-3. Protein Adsorption Measurement To evaluate the antibody loading capacity of the porous cellulose membrane in the fabricated laminate, the protein adsorption capacity of the porous cellulose membrane was quantified. Protein adsorption was measured using Bradford reagent (APRO Science, product number: KY-1020), which changes absorbance at 595 nm in proportion to the protein concentration when dropped into a protein-containing solution. First, bovine serum albumin (BSA, Fujifilm Wako Pure Chemical Industries, product number: 017-15146) was dissolved in 5 mmol / L PBS to prepare five BSA solutions with known concentrations: 1000 μg / mL, 500 μg / mL, 250 μg / mL, 125 μg / mL, and 100 μg / mL. The Bradford reagent was then dropped into the solutions, and the absorbance at 595 nm corresponding to each concentration was measured to create a calibration curve. The cellulose membrane was then immersed in a 1000 μg / mL BSA solution, and the concentration of the BSA solution before and after immersion was calculated using a calibration curve from the absorbance obtained by absorbance measurement, thereby quantifying the amount of protein adsorbed per projected area of ​​the cellulose membrane. To compare the amount of protein adsorption, a similar experiment was also performed using a commercially available nitrocellulose membrane for immunochromatography (Cytiva, AE98, no backing sheet, thickness: 105-140 μm).

[0113] Bradford reagent was added dropwise to BSA solutions of known concentrations, and the absorbance at a wavelength of 595 nm corresponding to each concentration was measured. A calibration curve was created based on the results, as shown in Figure 25. As shown in Figure 25, when the absorbance at each concentration was plotted on a graph, a highly linear calibration curve was obtained. Using the equation for this approximate line, absorbance was measured after adding Bradford reagent, and the concentration of a BSA solution of unknown concentration was determined.

[0114] Figure 26 shows the quantitative results of protein adsorption measured using four types of cellulose membranes prepared with varying applicator gap heights and a commercially available nitrocellulose membrane. Comparing membranes with applicator gap heights of 25 μm, 50 μm, and 75 μm, the amount of BSA adsorption increased with increasing membrane thickness. On the other hand, the amount of BSA adsorption decreased for membranes with an applicator gap height of 100 μm. This is likely due to the fact that, as shown in Table 4, the cellulose fiber structure thickens with increasing membrane thickness, reducing the internal void space, thereby reducing the internal surface area for BSA adsorption. Based on these findings, we concluded that membranes prepared with applicator gap heights ranging from 25 μm to 75 μm are suitable cellulose membranes for ECL immunoassays. Furthermore, comparing these membranes with commercially available nitrocellulose membranes, we confirmed that the protein adsorption capacity was doubled despite being less than one-tenth the thickness of the membrane.

[0115] Example 10: Fabrication of a porous membrane / graphene membrane laminate having a compressed porous structure portion. To use a laminate electrode consisting of a porous membrane / transparent conductive membrane as an analytical electrode for biochips and the like, it is desirable to specify the area of ​​the graphene in contact with the solution. Because the sheet resistance of single-layer graphene is on the order of several hundred Ω / sq, when a high current flows, ohmic loss occurs within the graphene electrode, and the electrode reaction is limited by the electrical resistance of the graphene. Therefore, the electrode area should be appropriate so that this ohmic loss does not become large. Furthermore, to use a graphene electrode as an electrode, the end of the graphene sheet must be laminated with a conductive electrode. Since it is necessary to prevent the electrolyte from contacting this conductive electrode, one possible method for specifying the electrode area is to laminate an insulator on a portion of the graphene electrode surface to keep the area in contact with the electrolyte constant. However, if the thickness of the porous membrane in a laminate electrode consisting of a porous membrane / transparent conductive membrane increases, the electrolyte will penetrate into the porous membrane even if an insulator is placed on the porous membrane, making it difficult to specify the area of ​​the graphene electrode in contact with the solution. Therefore, in this example, we investigated whether applying pressure perpendicular to the surface of the laminate electrode would compress the porous membrane except for the portion that contacts the solution, thereby crushing the porous structure, thereby preventing horizontal movement of the electrolyte and using the compressed porous membrane as an insulator for defining the electrode area. To avoid damaging the graphene when compressing the porous membrane / graphene membrane laminate electrode, we determined an appropriate pressure for compressing the porous structure using the electrical resistance of the laminate electrode as an indicator. The surfaces of the porous membrane at the compressed and uncompressed portions were observed using a SEM.

[0116] 10-1. Fabrication of a Porous Film / Graphene Film Laminate with a Compressed Porous Structure Portion Using the same procedure as in Example 9, a porous cellulose mixed ester film was formed on graphene grown on copper at a gap height of 75 μm. Similarly, a laminate consisting of a porous cellulose mixed ester film / graphene film was transferred to a quartz substrate in the same manner as in Example 2. A portion of the porous structure of these two types of laminates on copper foil or quartz substrate was compressed using a hydraulic flask press (Morita Tokyo Manufacturing Co., Ltd., FP7) and aluminum as shown in Figure 27 . The surface of the aluminum in contact with the sample measured 20 mm x 20 mm. When an uncompressed portion was to be left, a 20 mm x 20 mm aluminum plate with a 4 mm or 8 mm diameter (Φ) hole was used on the porous film side.

[0117] 10-2. Loading Pressure on the Entire Stack First, as shown in Figure 28, a stack (15 mm x 10 mm, quartz substrate 20 mm x 20 mm, channel portion 10 mm x 10 mm) consisting of a porous mixed cellulose ester film / graphene film on a quartz substrate with gold / chromium vapor-deposited on both ends was subjected to pressure using a 20 mm x 20 mm aluminum plate (without holes), and the change in electrical resistance between the gold / chromium electrodes on both ends (corresponding to the change in resistance of the graphene film) was measured. Force was applied to the stack a total of eight times. The applied force was changed for each measurement. Table 5 shows the relationship between the force applied to the porous film / graphene stack and its electrical resistance.

[0118]

[0119] The "applied force [N]" in Table 5 is the force applied to the porous membrane / graphene electrode using a hydraulic flask press. The resistance of the laminate electrode before application of force was 400 Ω. A force of 5 kN was applied the first time, but the resistance value did not change. Furthermore, when the electrode was crushed with a force of 10 kN (approximately 1 ton) the fourth time, the resistance value increased to 420 Ω, confirming a slight increase in resistance, but not enough to degrade the electrode's performance. This suggests that the porous membrane / graphene laminate electrode is highly durable against pressure applied from above and below. It was found that application of a force of 1 ton (250 MPa) did not impair the electrode's performance. The porous membrane was then repeatedly compressed until it no longer functioned as an electrode. The resistance value further increased when the electrode was crushed with a force of 1 ton the sixth time, and when a force of 1.5 ton was applied the eighth time, the resistance value reached 2200 Ω, significantly deteriorating the electrode's performance. Since cracks occurred in the quartz glass substrate during this process, it is believed that the cracks in the quartz substrate were the cause of the significant increase in resistance.

[0120] 10-3. Loading of partial pressure on the laminate Next, as shown in Figure 29, a force of 1 ton was applied to the laminate electrode on the quartz substrate for 30 seconds using an aluminum plate with a 4 mm diameter hole. In the photograph before the force was applied (left side of Figure 29), the light appears white due to scattering by the porous structure of the cellulose mixed ester film, whereas in the photograph after the force was applied (right side of Figure 29), the part in contact with the aluminum plate has become transparent. This is thought to be because the porous structure has been compressed and light is no longer scattered.

[0121] 10-4. SEM Observation To examine whether the porous structure of the cellulose membrane was crushed after applying force, a 1.25 ton force was applied to a laminate formed on copper foil using an aluminum plate with 8 mm diameter holes, and the surface was observed using an SEM. A 10 nm thick platinum coating was applied during SEM observation to prevent charge-up. Figure 30 shows an SEM image. Figure 30(a) shows the area where force was applied, and Figure 30(b) shows the area where no force was applied (corresponding to the area of ​​the holes in the aluminum plate). Both images were observed at a magnification of 10,000x and an accelerating voltage of 3 kV. These results demonstrate that the porous structure of the cellulose mixed ester membrane was crushed using a hydraulic flask press and aluminum plate. Furthermore, the porous membrane area corresponding to the holes in the aluminum plate remained uncrushed, confirming the porous structure.

[0122] 10-5. Transfer of compressed porous film / graphene film Next, to examine whether the cellulose mixed ester film with a compressed porous structure functions as a transfer support material, a laminate on copper foil after a portion of the porous structure was crushed by applying force was transferred onto a quartz substrate in the same manner as in Example 2. As a result, it was confirmed that the film could be transferred without any problems, and that it functioned as a transfer support film even after the porous portion was crushed.

[0123] 10-6. Electrochemical Measurements Using a Compressed Porous Film / Graphene Film Laminate Electrode A porous cellulose mixed ester membrane was prepared using the same procedure as in 10-1 and transferred to a quartz substrate with chromium (10 nm) and silver (50 nm) vapor-deposited on the edges in the same manner as in Example 2. Two such laminates were prepared, and a force of 1 ton was applied to one of them for 30 seconds using an aluminum block with a 4 mm diameter (Φ) hole, as in the procedure shown in 10-3. Using this laminate electrode with a compressed porous structure and an uncompressed laminate electrode, cyclic voltammetry was performed in a pH 7.4 0.15 mol / L phosphate buffer solution in the range of 0 to 1.4 V vs. Ag / AgCl using the measurement cell shown in Figure 10. The scan rate was 0.1 V / s. The same reference electrode and counter electrode as in Example 4 were used. The measurement results are shown in Figure 31. An oxidation peak was observed at 0.15 V vs. Ag / AgCl for the laminate electrode with an uncompressed porous structure. This is an oxidation peak resulting from the oxidation reaction of silver in the conductive electrode. Therefore, it was found that in laminate electrodes where the porous structure is not compressed, the phosphate buffer electrolyte permeates horizontally into the conductive electrode area, affecting the measurement results. In the laminate electrode where the porous structure is compressed, a voltammogram was obtained that did not contain the oxidation peak of silver in the conductive electrode, which means that it was possible to compress the porous structure outside the measurement area without damaging the graphene, and it can be said that horizontal permeation of the electrolyte was successfully prevented.

[0124] In this way, we found that compressing the porous structure can define the electrode area while preventing contact of the solution with the conducting electrode. Furthermore, because there is almost no damage to the graphene underneath the compressed area, this method is advantageous from the perspective of charge transport to the active electrode area that comes into contact with the electrolyte in the non-compressed area. By designing the compressed and non-compressed areas, it is thought that an array of active electrode areas can be created using a simple process. Therefore, this method is also considered advantageous from the perspective of fabricating biochips for multi-item testing.

[0125] (Example 11. Immunoassay using a laminate electrode composed of a porous membrane / graphene membrane prepared by a casting method) 11-1. Preparation of a laminate electrode and ECL immunoassay Using the same procedure as in Example 9, a porous cellulose mixed ester membrane was formed on graphene grown on copper at a gap height of 50 μm. A force of 1 ton was applied to this laminate electrode composed of a porous cellulose mixed ester / graphene membrane for 30 seconds using an aluminum block with a hole having a diameter (Φ) of 4 mm, as in the procedure shown in Example 10. This laminate electrode was transferred to a quartz substrate on which gold / chromium had been vapor-deposited, as in Example 2. Using this laminate electrode, an ECL immunoassay for CEA was performed using the same procedure as in Example 6.

[0126] 11-2. Results The measurement results are shown in Figure 32 (current-potential curve) and Figure 33 (ECL intensity-potential curve). The current increased when the graphene electrode potential was around 0.8 V, confirming that this increase in current was due to the oxidation of tripropylamine at the electrode. In addition, an increase in ECL intensity was confirmed from around 1 V. This demonstrates that a laminate electrode consisting of a cellulose mixed ester porous film / graphene film prepared by the casting method can be used as an electrode for ECL immunoassay.

[0127] (Example 12. Graphene transparent electrode using PEDOT:PSS as a conductive additive) Because graphene is a material with a single atomic layer, it has a higher resistance than electrodes such as platinum, which are conventionally used as electrodes in ECL measurements, and resistance values ​​for each sample tend to vary. This electrode resistance value may affect the luminescence intensity of ECL measurements. Therefore, in order to use graphene transparent electrodes as electrodes with lower resistance, attention was focused on PEDOT:PSS, which is a transparent electrode material like graphene. In this example, with an eye toward applying CVD graphene as an electrode for electrochemiluminescence immunoassay, a ruthenium bipyridyl complex / tripropylamine (Ru(bpy)) used in bioanalysis was used. 3 Cl 2 To suppress the variation in ECL emission intensity in the ECL measurement system for PEDOT:PSS / TPrA, graphene and PEDOT:PSS were laminated and their electrochemical properties were evaluated.

[0128] 12-1. Fabrication of Graphene / PEDOT:PSS Electrode The graphene / PEDOT:PSS electrode was fabricated as follows. A 20 mm x 20 mm quartz substrate was cleaned in the same manner as the copper substrate used for graphene deposition. Then, 5 nm of Cr and 50 nm of Au were evaporated onto the edge of the quartz substrate. PEDOT:PSS (Sigma-Aldrich, product number 739316-25G) was dropped onto this substrate and spin-coated. The spin-coating was performed by increasing the rotation speed to 2500 rpm over 30 seconds, maintaining it for 60 seconds, and then stopping over 30 seconds. The resulting film was then baked at 140°C for 1 hour to form a PEDOT:PSS electrode. Single-layer graphene was transferred onto the surface of this PEDOT:PSS electrode using a PMMA-supported transfer method. The PMMA / graphene laminated film was transferred onto the PEDOT:PSS electrode, and then thoroughly dried and immersed in acetone to remove the PMMA, thereby producing a graphene / PEDOT:PSS electrode.

[0129] 12-2. Transmittance and Raman Spectroscopy Measurements The left graph in Figure 34 shows the transmittance measurement results for each electrode fabricated. While the graphene electrode exhibits a stable, high transmittance of approximately 90%, the graphene / PEDOT:PSS electrode exhibits a decrease in transmittance toward longer wavelengths, resulting in a blue appearance. Furthermore, focusing on the transmittance at the emission wavelength of 620 nm of the Ru bipyridyl complex used in this example, the graphene electrode exhibits a transmittance of approximately 90.6%, the PEDOT:PSS electrode exhibits a transmittance of approximately 89.7%, and the graphene / PEDOT:PSS electrode exhibits a transmittance of approximately 87.1%. Comparing the PEDOT:PSS electrode and the graphene / PEDOT:PSS electrode, the transmittance decreased by approximately 2.6%. Given that the absorbance per graphene layer is 2.3%, this decrease in transmittance is considered appropriate. Furthermore, although the use of PEDOT:PSS resulted in a transmittance decrease of approximately 3.5% compared to the graphene electrode, high transmittance was maintained. Therefore, it is believed that it can be used as a transparent electrode in ECL measurements.

[0130] The right figure in Figure 34 shows the Raman spectra of graphene, PEDOT:PSS, and graphene / PEDOT:PSS. -1The graphene-specific 2D peak at 1590 cm -1 The G peak was observed at 2000 s. The full width at half maximum of the 2D peak was 37 cm. -1 The intensity ratio I(2D) / I(G) was 1.2. In addition, since the 2D peak could be fitted with a single Lorentzian function, it was determined that the graphene obtained by CVD growth was a single layer. -1 No D peak due to graphene defects was observed near the 1598 cm region. This indicates that high-quality single-layer graphene was successfully grown and transferred. -1 , 2D peak at 2690 cm -1 It was also confirmed that the height was 1590 cm. -1 It can be confirmed that the Raman spectrum of the graphene / PEDOT:PSS electrode matches that of the PEDOT:PSS alone on the shorter wavelength side. This confirms that the PEDOT:PSS and graphene form a layered structure. Therefore, together with the transmittance measurement results, it can be said that the graphene / PEDOT:PSS electrode is a high-light transmittance electrode made by layering high-quality graphene and PEDOT:PSS.

[0131] 12-3. Sheet Resistance The sheet resistance of the graphene, PEDOT:PSS, and graphene / PEDOT:PSS electrodes was measured. This measurement was performed using a 20 mm x 20 mm quartz substrate with a 20 mm x 20 mm graphene layer transferred onto it, with indium particles in contact with the four corners. Table 6 shows the sheet resistance of each sample measured using the four-terminal method. As shown in Table 6, graphene and PEDOT:PSS each showed high sheet resistance when used alone, but the sheet resistance was significantly reduced by stacking them. This is thought to be because the thickness of the electrode increased when graphene and PEDOT:PSS were stacked, and also because small tears that had occurred in the graphene during processes such as transfer were ameliorated by PEDOT:PSS.

[0132] 12-4. CV Measurement 1 Figure 35 shows the results of CV measurements performed using graphene, graphene / PEDOT:PSS, and glassy carbon electrodes in a 0.1 mol / L KCl aqueous solution containing 5 mmol / L hexaammineruthenium. The scan rate was 0.1 V / s. The peak-to-peak potential difference ΔEp, which is the difference in potential between the oxidation peak and the reduction peak, is shown in Table 7.

[0133] In the case of a reversible system where the electrode reaction is sufficiently fast, ΔEp is 59 mV for a single-electron transfer reaction. However, if the solution resistance or the internal resistance of the electrode is not negligible, ohmic loss, the product of current and resistance, occurs, resulting in a larger ΔEp. Because the internal resistance of the glassy carbon electrode is negligibly small compared to the solution resistance, the difference in ΔEp between the glassy carbon electrode and the other two electrodes is likely due to the electrode's internal resistance. In measurements where a relatively large current flows, such as those under these measurement conditions, the graphene electrode alone exhibits high internal resistance and large ohmic loss. The graphene / PEDOT:PSS electrode exhibits reduced sheet resistance (Table 7), which suggests that ohmic loss is reduced and ΔEp is closer to that of glassy carbon. Because luminescence intensity in electrochemiluminescence measurements is strongly correlated with current, high electrode internal resistance may make it difficult to achieve high luminescence intensity.

[0134] 12-5. ECL Measurement Figure 36(a) shows the results of ECL measurement by the CV method. Figure 36(b) shows the total luminescence amount for 30 seconds from the start of potential application obtained by the chronoamperometry method. The solution contained 10 mmol / L tripropylamine and 0.1 mmol / L Ru(bpy). 3 Cl 20.15 mol / L PBS containing PEDOT:PSS was used. When PEDOT:PSS was used alone as the working electrode for comparison, no luminescence was observed. This is thought to be because PEDOT:PSS has the property of dispersing in water, so PEDOT:PSS redispersed in the measurement solution and no longer functioned as an electrode. On the other hand, luminescence was confirmed in the graphene / PEDOT:PSS electrode in which graphene was laminated on PEDOT:PSS. Therefore, it can be said that by laminating PEDOT:PSS with graphene, which was not able to perform electrochemical measurements alone, the graphene prevented PEDOT:PSS from redispersing in the measurement solution, making it possible to use it for electrochemical measurements.

[0135] Furthermore, the ECL measurement results for the graphene / PEDOT:PSS electrode showed that luminescence was observed at a lower potential than for the graphene electrode. This indicates that lamination facilitates electrode reactions. The results in Figure 36(b) also show that the PEDOT:PSS / graphene electrode emitted more light than the graphene electrode, indicating that the presence of PEDOT:PSS contributes to improving ECL intensity.

[0136] 12-6. CV measurement 2 Figure 37(a) shows Ru(bpy) 3 Cl 2 Figure 37(b) shows the results of CV measurement of tripropylamine. It can be seen that for both reactants, the graphene electrode with PEDOT:PSS layered starts to flow current at a lower potential. In particular, Ru(bpy) 3 Cl 2 Regarding the reactivity of PEDOT:PSS, a significant improvement in reactivity was observed. Therefore, the increase in ECL intensity of the graphene electrode due to the PEDOT:PSS layering is attributed to the decrease in the internal resistance of the electrode as well as the improvement in the reactivity of the ECL reactant.

[0137] The average luminescence intensity and its standard error when five samples of each electrode were measured by the CV method are shown in Table 8. Table 8 also shows the coefficient of variation of the total luminescence intensity at 1.3 V, based on the ECL measurement results in Figure 37(b).

[0138] The average luminescence intensity measured by the CV method was approximately 1.3 times higher for the graphene / PEDOT:PSS electrode. Furthermore, the variability of approximately 8.8% for the graphene electrode was confirmed to be reduced to approximately 3.8% for the graphene / PEDOT:PSS electrode. Five samples were also measured by the CA method, and the coefficient of variation calculated from the luminescence intensity at an applied voltage of 1.3 V was also smaller for the graphene / PEDOT:PSS electrode. This indicates that stacking graphene and PEDOT:PSS not only increases the luminescence intensity of ECL, but also enables more stable measurements with less error. This is because stacking the PEDOT:PSS electrode reduces the variability in sheet resistance (internal resistance), leading to reduced variability in the electrochemical measurement results.

[0139] Example 13: Making a Laminate Comprising a Porous Film and a Transparent Conductive Film Transparent laminates can also be used as transparent conductive films with a separator. The separator is placed between two electrodes, an anode and a cathode, and serves to allow ions to pass through and prevent the two electrodes from contacting each other. Separators are generally made of porous resin materials or nonwoven fabrics. The porous film / graphene film laminate of this example can be used as a transparent electrode with a separator. By laminating another graphene film on the surface of the porous film of the porous film / graphene film laminate, an extremely thin and transparent thin-layer electrochemical cell can be fabricated. For example, to fabricate a thin electrochromic device, two electrodes, an anode and a cathode, must be arranged facing each other. However, by placing a separator between the electrodes, internal short circuits can be prevented, making it possible to fabricate the required laminate structure. However, to reversibly control the transparent state (bleached state) and the colored state, the separator itself must be transparent. Generally, porous materials scatter light even when the light has a wavelength that does not cause light absorption, and therefore appear white.

[0140] Therefore, in this example, we attempted to achieve device transparency by matching the refractive index of the separator placed between the graphene electrodes with that of the electrolyte impregnated into the separator. Specifically, to match the refractive index of the electrolyte and the separator, polyvinylidene fluoride (PVDF) was used for the separator, and a mixed solvent of water and glycerin was used for the electrolyte. The refractive index of water is 1.33, and the refractive index of glycerin, a miscible solvent, is 1.47. PVDF was selected for the separator because its refractive index, 1.41, is between the refractive indices of these two solvents. First, to determine the optimal mixture ratio of water and glycerin in the electrolyte impregnated into PVDF, we investigated the dependence of the refractive index of the water / glycerin mixed solvent on the glycerin ratio. A digital refractometer (Hanna Instruments, model number: HI96800) was used to measure the refractive index. Figure 38 shows the dependence of the refractive index of the mixed solvent on the glycerin ratio. As the ratio of glycerin increased, the refractive index of the mixed solvent increased, and when the ratio of glycerin to water was 6:4, the refractive index was close to 1.42, which is the refractive index of PVDF.

[0141] Next, a commercially available porous PVDF membrane (GVS, model number: 1213992) was immersed in methanol for 30 seconds to perform a hydrophilic treatment, and then impregnated with various ratios of glycerin / water mixed solutions containing 0.1 M potassium chloride. The membrane was sandwiched between two glass slides (Matsunami Glass Co., Ltd., model number: S1111) and subjected to transmittance measurements. Figure 39 shows the transmittance spectrum. The PVDF membrane impregnated with a 0.1 mol / L potassium chloride solution in a 6:4 glycerin / water ratio exhibited the highest transmittance. Since this value was equivalent to the transmittance of the glass slide alone, the difference from 100% was due to reflection at the air-glass interface. Since there was almost no scattering in the solution-impregnated PVDF layer, the transmittance of this layer is considered to be nearly 100%.

[0142] Next, a PVDF / graphene laminate electrode was fabricated by a casting method using an applicator with a gap height of 100 μm, following the same procedure as in Example 9. The PVDF porous membrane-forming solution was prepared by dissolving PVDF (Sigma-Aldrich, product number: 347078) at 12% by mass in a 1:1 acetone / dimethylformamide (DMF) mixed solvent. The fabricated PVDF / graphene / quartz substrate laminate was immersed in methanol for hydrophilization, then impregnated with water or a water / glycerin solution and placed on a cover glass for transmittance measurement. Transmittance spectra are shown in Figure 40. The transmittance at 550 nm of the PVDF membrane impregnated with water was 39%, while the transmittance of the laminate impregnated with a water / glycerin solution with a mass ratio of water:glycerin = 4:6 was 89%, demonstrating the success of rendering the PVDF porous membrane / graphene laminate transparent.

[0143] Next, a film-like electrochromic device was fabricated using two graphene electrodes with a PVDF separator and a water:glycerin mixture solution (4:6 by mass) as the electrolyte. Prussian blue (PB) was used as the electrochromic material. Specifically, the electrochromic device was fabricated as follows. First, CVD graphene was transferred to a PET substrate by thermocompression bonding using PMMA as an adhesive, producing a graphene electrode consisting of a graphene film / PMMA / PET substrate. Using two of the fabricated graphene electrodes, a PB-electrodeposited graphene electrode and a silver-electrodeposited graphene electrode were fabricated as follows. Using a solution containing 5 mmol / L iron(III) chloride, 5 mmol / L potassium ferricyanide, 0.1 mol / L hydrochloric acid, and 0.1 mol / L potassium chloride, the graphene electrode was used as the working electrode, and a current of −20 μA / cm was applied. 2 PB was electrodeposited on the graphene electrode by passing a current density of -100 μA / cm for 5 minutes. Since it was necessary to cause an equal amount of a reaction with the opposite sign to the oxidation-reduction of Prussian blue on the other graphene electrode, silver was electrodeposited to utilize the oxidation-reduction of silver and silver chloride. To electrodeposit silver on the graphene electrode, a solution containing 0.1 mol / L sodium nitrate and 1 mmol / L silver nitrate was used to apply a current density of -100 μA / cm to the graphene electrode. 2A current density of 0.01 was applied for 4 minutes. A porous PVDF membrane was sandwiched between the thus-prepared PB-electrodeposited graphene electrode (oxidized and colored) and the silver-electrodeposited graphene electrode (reduced, Ag) as a separator. A 4:6 water / glycerin solution containing 0.1 mol / L potassium chloride was impregnated into the PVDF. The voltage between the two electrodes (based on the silver-electrodeposited electrode) was varied from 0 V to -1.0 V to 1.2 V, and the current and color change of the device were observed. Figure 41 shows a schematic diagram of the fabricated electrochromic device. Figure 42 shows the current-voltage curves. It was confirmed that the color changed from blue (the left graph in Figure 43 shows the colored state) to transparent (the right graph in Figure 43 shows the bleached state) upon reduction of PB (concurrent oxidation of silver to silver chloride), and from transparent to blue upon oxidation of PB (concurrent reduction of silver chloride) (Figure 43).

[0144] In applications using ECL, such as ECL immunoassays, it is believed that matching the refractive index of the electrolyte and the porous membrane is effective. For example, if the refractive index of the electrolyte in an ECL immunoassay can be adjusted to match the refractive index of the mixed cellulose ester membrane, it would be possible to capture ECL with a photodetector without scattering it within the porous membrane. This would result in a clear, unblurred boundary between the luminescent and non-luminescent regions. Therefore, when considering associating multiple test items with the light-emitting position of an analytical device, this method can contribute to the integration of test items.

[0145] REFERENCE SIGNS LIST 1 Laminate (porous film / transparent conductive film) 1' Laminate (porous film / transparent conductive film / transparent insulating substrate) 2 Transparent conductive film 2' Graphene film 3 Porous film 4 Transparent insulating substrate 5 Conductive electrode 6 Membrane 7 Electrical conductor 8 Conjugate pad 9 Sample pad 10 Absorption pad 11 Biochip 12 Photodetector 13 Reference electrode 14 Image sensor 15 Metal catalyst substrate 16 Electrolyte 17 PET substrate 18 Au 19 PVDF film 20 PB 21 PMMA

Claims

1. A laminate comprising a transparent conductive film and a porous film laminated on the transparent conductive film, wherein the porous film is permeable to an electrolyte.

2. The laminate according to claim 1, wherein the porous film has pores with an average pore diameter of 20 nm or more.

3. The laminate according to claim 1, wherein the area ratio of the pores to the membrane surface of the porous membrane is 20% or more.

4. The laminate according to claim 1, wherein the porous film has a thickness of 100 nm or more.

5. A laminate according to claim 1, further comprising a transparent insulating substrate, the porous film being laminated on a first surface of the transparent conductive film, and the transparent insulating substrate being laminated on a second surface of the transparent conductive film.

6. A laminate according to claim 5, further comprising an electrical conductor, the electrical conductor being laminated on the surface of the porous film and on the surface opposite to the surface on which the transparent conductive film is laminated, or on the surface of the transparent insulating substrate and on the same surface as the surface on which the transparent conductive film is laminated.

7. A laminate according to claim 5, wherein said porous membrane has at least a part of a compressed structure.

8. The laminate according to claim 5, wherein the transparent insulating substrate is coated with a transparent conductive assistant.

9. A laminate according to claim 1, further comprising an electrical conductor, the transparent conductive film being laminated on a first surface of the porous film, and the electrical conductor being laminated on a second surface of the porous film.

10. A laminate according to claim 1, wherein the porous membrane is a membrane made of a material selected from the group consisting of nitrocellulose, cellulose acetate, polyethersulfone, polytetrafluoroethylene, polyamide, polyvinylidene fluoride, regenerated cellulose, polycarbonate, polypropylene, polyvinylidene chloride, aluminum oxide, glass fiber, quartz fiber, polymethyl methacrylate, polystyrene, polyethylene, polyethylene terephthalate, and ceramic, or a mixed membrane made of two or more materials selected from the group.

11. A laminate according to any one of claims 1 to 10, wherein the transparent conductive film is a transparent carbon conductive film.

12. The laminate according to any one of claims 1 to 10, wherein the transparent conductive film is a graphene film.

13. A biochip comprising a laminate according to any one of claims 5 to 9.

14. A kit comprising the biochip of claim 11 and an electrochemiluminescent substance.

15. A laminate according to claim 5, further comprising a transparent conductive film, a transparent insulating substrate, and an electrical conductor, the laminate being layered in the following order: transparent insulating substrate, transparent conductive film, porous film, transparent conductive film, transparent insulating substrate, and the electrical conductor being arranged so as to be in contact with the transparent conductive film.

16. A method for using the laminate according to claim 5 as a transparent electrode, comprising using a solvent having the same refractive index as that of the porous film.

17. A method for detecting a target compound by electrochemiluminescence immunoassay using the laminate according to any one of claims 5 to 9 or a biochip comprising the laminate according to any one of claims 5 to 7, comprising: (a) a step of binding the target compound to an electrochemiluminescent substance; (b) a step of capturing the target compound in a porous membrane of the laminate, the step capturing the target compound by a substance that specifically binds to the target compound and is fixed in the porous membrane; and (c) a step of applying a potential to the laminate and measuring electrochemiluminescence after steps (a) and (b).

18. A method for producing a laminate in which a transparent insulating substrate, a carbon conductive film, and a porous film are laminated in this order, the method further comprising: (a) a step of forming a carbon conductive film on a metal catalyst substrate by a CVD method; (b) a step of further forming a porous film on the carbon conductive film to produce a laminate; and (c) a step of removing the metal catalyst substrate by etching, and transferring the laminate onto a transparent insulating substrate so that the carbon conductive film is in contact with the laminate.

19. The method according to claim 18, wherein in step (i), the solvent for dissolving the polymer used to form the porous membrane is a mixed solvent containing a good solvent and a poor solvent for the polymer.

Citation Information

Patent Citations

  • Immunoassay apparatus

    JP1998111293A

  • Electrochemiluminescence detection method and apparatus

    JP3574457B2

  • Immunochromatographic test strips

    JP6464308B1

  • Transparent conductive film and method of preparing it

    JP2001126539A

  • Titanium oxide-containing porous film laminate, and production method thereof

    JP2013136216A