Metal-resin composite and use for same

The metal-resin composite with controlled zeta potential and particle size addresses dispersibility and sensitivity issues in immunoassays, offering enhanced stability and detection capabilities without requiring specialized equipment.

WO2024203979A1PCT designated stage expired Publication Date: 2024-10-03NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011542
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing metal-resin composites for immunoassays face issues with dispersibility in water, leading to clogging and reduced detection sensitivity due to aggregation, and they often require specialized equipment or additional processing steps.

Method used

A metal-resin composite with gold or alloy particles immobilized on resin particles, where the resin particles have a specific zeta potential range and a low coefficient of variation in particle size, enhancing dispersibility and stability, and allowing for effective binding with various antigens and antibodies without the need for additional equipment or processes.

Benefits of technology

The composite exhibits improved handling properties, durability, and sensitivity in immunoassays, reducing aggregation and clogging, while maintaining stability and sensitivity across a wide pH range, making it suitable for various applications including immunochromatography.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011542_03102024_PF_FP_ABST
    Figure JP2024011542_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: a metal-resin composite comprising resin particles and a plurality of metal particles immobilized to the resin particles, wherein in the pH range of 3-6, the maximum value of zeta potential is not less than 5 mV, in the pH range of 8-10, the minimum value of the zeta potential is not more than -20 mV, and the zero charge point of the zeta potential exists in the pH range of 6.1-9.0; a labeling substance comprising the metal-resin composite; and an immunoassay method and an immunoassay reagent which use the labeling substance. The metal particles are particles of gold or an alloy thereof, and a CV value of the particle diameter of the metal particles is not more than 0.45.
Need to check novelty before this filing date? Find Prior Art

Description

Metal-resin composite and its use

[0001] The present invention relates to a metal-resin composite that can be preferably used for applications such as immunoassays, a labeled substance that utilizes the same, an immunoassay method, a reagent for immunoassays, a method for measuring an analyte, an analyte measurement kit, and a lateral flow chromatography test strip.

[0002] Immunoassays are methods for qualitatively and quantitatively analyzing trace components by utilizing specific reactions between antigens and antibodies. In immunoassays, detection sensitivity is increased by binding a labeling substance to an antibody, an antigen, or a complex of these. Therefore, the labeling ability of a labeling substance can be said to be an important factor that determines the detection ability in immunoassays. It has been proposed to use composite particles, which are composites of metal particles and resin particles, as labeling substances for immunoassays (Patent Documents 1 to 3).

[0003] Patent Document 1 discloses a colored latex consisting of gold nanoparticles bound to the surface of polymer-based latex particles. The colored latex in Patent Document 1 is obtained by irradiating a dispersion of styrene-acrylic acid copolymer latex and HAuCl, a gold nanoparticle precursor, with gamma rays, thereby binding gold nanoparticles to the surface of the latex. However, since the gold nanoparticles are bound only to the surface of the colored latex, there is a limit to the amount of gold nanoparticles that can be loaded to induce surface plasmon resonance, and the gold nanoparticles are prone to detachment. As a result, the visibility and sensitivity of the latex may be insufficient as a reagent for immunoassays. Furthermore, the latex may be damaged due to the irradiation of electromagnetic radiation such as gamma rays.

[0004] Patent Document 2 proposes a metal-resin composite in which a specific proportion of metal particles are present in the surface layer of resin particles, which has excellent durability and visibility and enables highly sensitive determination in immunoassays without requiring any additional special equipment or work processes.

[0005] Patent Document 3 proposes a metal-resin composite that has a maximum zeta potential of 5 mV or more and a minimum zeta potential of −5 mV or less in the pH range of 3 to 10, and therefore has excellent dispersibility and is less likely to aggregate when bound to many types of ligands such as antigens and antibodies or to blocking agents.

[0006] Non-Patent Document 1 discloses a microgel in which gold nanoparticles are supported on poly-2-vinylpyridine latex particles, and the pH response of the microgel particle size is confirmed by changes in the behavior of the localized surface plasmon resonance of the gold nanoparticles. However, in this microgel, the gold nanoparticles are supported in a single layer near the surface of the latex particles. Therefore, the amount of gold nanoparticles supported is low, and it is thought that a deep color tone effective for immunoassays cannot be obtained. Furthermore, no investigation has been conducted into the material, structure, composition, etc. of the microgel, and its effectiveness in specific applications such as immunoassay reagents is unknown.

[0007] JP 2009-168495 A International Publication WO2016 / 002742 International Publication WO2018 / 123952

[0008] K. Akamatsu, M. Shimada, T. Tsuruoka, H. Nawafune, S. Fujii and Y. Nakamura; Langmuir 2010,26,1254-1259.

[0009] In order to use a metal-resin complex as a labeling substance in immunoassays, it is necessary to stably bind it to a ligand such as an antigen or antibody, or to a blocking agent. However, when labeling a ligand with a metal-resin complex, even if a stable binding state can be formed, excellent detection sensitivity is not necessarily obtained. For example, fine metal-resin complexes are prone to aggregation. Aggregation not only significantly reduces handleability, but can also cause unevenness in the concentration of the metal-resin complex, which is the labeling substance, and significantly reduces detection sensitivity.

[0010] Furthermore, antigens, antibodies, and blocking agents used in immunoassays include various types, such as proteins, synthetic polymers, and low-molecular-weight compounds, some of which have strong anionic properties (e.g., casein) and others of strong cationic properties (e.g., whey). Therefore, a labeling substance that can be used with all of these antigens and antibodies would be highly desirable for reasons such as reducing material costs.

[0011] The metal-resin composite of Patent Document 3 exhibits improved dispersibility when bound to a variety of ligands and blocking agents due to its characteristic zeta potential behavior, making it highly useful. Among the metal-resin composites described in Patent Document 3, gold-resin composites having gold particles and a resin have been prepared by treating the resin particles with sodium hydroxide, a strong alkali (Example 4), or by treating the gold-resin composite with mercaptopropionic acid or polyglutamic acid after formation (Examples 5 and 7). These treatments result in gold-resin composites exhibiting the same characteristic zeta potential as platinum-resin composites having platinum particles and a resin. However, the gold-resin composites prepared in this manner have low dispersibility in water, and when used as labeled substances in immunochromatography, problems such as clogging and background color development have been observed, leaving room for improvement.

[0012] An object of the present invention is to provide a metal-resin composite which has improved dispersibility in water while utilizing the advantages of a metal-resin composite, and which can avoid problems such as clogging when used as a labeling substance in immunochromatography.

[0013] As a result of extensive research, the present inventors discovered that in a metal-resin composite in which multiple gold particles are immobilized on resin particles, the above-mentioned problems can be solved by selecting the type of resin used in the resin particles and controlling the particle size of the gold particles, and thus completed the present invention.

[0014] That is, the metal-resin composite of the present invention is a metal-resin composite having resin particles and a plurality of metal particles immobilized on the resin particles, characterized in that the maximum value of the zeta potential is 5 mV or more in the pH range of 3 to 6, the minimum value of the zeta potential is -20 mV or less in the pH range of 8 to 10, the zero charge point of the zeta potential is in the pH range of 6.1 to 9.0, and the metal particles are particles of gold or an alloy thereof, and the coefficient of variation (CV value) of the particle size is 0.45 or less.

[0015] In the metal-resin composite of the present invention, the resin particles may contain a first polymer and a second polymer of a different type from the first polymer, and one of the first polymer and the second polymer may be a polymer having a cationic functional group, and the other may be a polymer having an anionic functional group.

[0016] In the metal-resin composite of the present invention, the first polymer may be a polymer having a cationic functional group, and the second polymer may be a polymer having an anionic functional group. In this case, the molar ratio of the cationic functional group contained in the first polymer to the anionic functional group contained in the second polymer may be within a range of 99.5:0.5 to 80:20, in terms of the cationic functional group contained in the first polymer:the anionic functional group contained in the second polymer.

[0017] In the metal-resin composite of the present invention, the first polymer may be a polymer having in its structure a substituent capable of adsorbing metal ions.

[0018] In the metal-resin composite of the present invention, the metal particles may have an average particle size in the range of 1 nm to 100 nm.

[0019] In the metal-resin composite of the present invention, the metal particles may be formed by reducing metal ions adsorbed on resin particles with a reducing agent solution obtained by mixing a buffer solution adjusted to a pH of 3 to 8 with a reducing agent.

[0020] The metal-resin composite of the present invention may have an average particle size in the range of 30 nm to 1000 nm.

[0021] The labeling substance of the present invention comprises the above-mentioned metal-resin composite. In this case, the labeling substance may be used by adsorbing an antigen or an antibody onto the surface of the metal-resin composite.

[0022] The immunological assay of the present invention uses the above-mentioned labeling substance.

[0023] The immunoassay reagent of the present invention comprises the above-mentioned labeling substance.

[0024] The method for measuring an analyte of the present invention is a method for detecting or quantifying an analyte contained in a sample, and comprises the following steps (I) to (III) using a lateral flow chromatography test strip including a membrane and a determination zone in which a capture ligand that specifically binds to the analyte is immobilized on the membrane: step (I): contacting the analyte contained in the sample with a labeled antibody, which is an antibody that specifically binds to the analyte and is labeled with a metal-resin complex; step (II): contacting the complex containing the analyte and the labeled antibody formed in step (I) with the capture ligand in the determination zone; and step (III): measuring the color intensity resulting from light energy absorption due to localized surface plasmon resonance and / or electron transition of the metal-resin complex. The metal-resin composite comprises resin particles and a plurality of metal particles immobilized on the resin particles, and is characterized in that the maximum value of the zeta potential is 5 mV or more in the pH range of 3 to 6, the minimum value of the zeta potential is -20 mV or less in the pH range of 8 to 10, the zero charge point of the zeta potential is in the pH range of 6.1 to 9.0, the metal particles are particles of gold or an alloy thereof, and the CV value (Coefficient of Variation) of the particle diameter is 0.45 or less.

[0025] The analyte measurement kit of the present invention is an analyte measurement kit for detecting or quantifying an analyte contained in a sample, comprising a lateral flow chromatography test strip including a membrane and a determination zone in which a capture ligand that specifically binds to the analyte is immobilized on the membrane, and a detection reagent including a labeled antibody in which an antibody that specifically binds to the analyte is labeled with a metal-resin complex, wherein the metal-resin complex has a structure in which a plurality of metal particles are immobilized on resin particles, and has a maximum zeta potential of 5 mV or more in the pH range of 3 to 6, a minimum zeta potential of -20 mV or less in the pH range of 8 to 10, and a zero charge point of the zeta potential in the pH range of 6.1 to 9.0, and the metal particles are gold or its alloy particles, and the CV value (Coefficient of Variation) of the particle diameter is 0.45 or less.

[0026] The lateral flow chromatography test strip of the present invention is for detecting or quantifying an analyte contained in a sample. This lateral flow chromatography test strip includes a membrane, a determination zone in which a capture ligand that specifically binds to the analyte is immobilized on the membrane in the direction of sample development, and a reaction zone upstream of the determination zone containing a labeled antibody obtained by labeling an antibody that specifically binds to the analyte with a metal-resin complex, wherein the metal-resin complex has a structure in which a plurality of metal particles are immobilized on resin particles, and the maximum zeta potential is 5 mV or more in the pH range of 3 to 6, the minimum zeta potential is -20 mV or less in the pH range of 8 to 10, and the zero charge point of the zeta potential is in the pH range of 6.1 to 9.0, and the metal particles are gold or gold alloy particles, and the coefficient of variation (CV) of the particle diameter is 0.45 or less.

[0027] The metal-resin composite of the present invention exhibits characteristic zeta potential behavior by selecting the type of resin used for the resin particles and controlling the particle size of the gold particles. Therefore, while utilizing the advantages of conventional metal-resin composites, it has improved dispersibility in water and, when used as a labeling substance in immunochromatography, minimizes problems such as clogging and background color development. Here, "zeta potential" refers to the potential of the slip surface of the electric double layer formed around the metal-resin composite in an acidic or alkaline solution. It is measured, for example, by electrophoretic light scattering as the potential difference between the slip surface and an electrically neutral region sufficiently distant from the metal-resin composite. Furthermore, the metal-resin composite of the present invention can interact with various substances, regardless of whether they are anionic or cationic, due to its specific zeta potential. Therefore, it exhibits excellent dispersibility and reduced aggregation even when bound to many types of ligands, such as antigens and antibodies, or to blocking agents. Furthermore, the metal-resin composite of the present invention has a structure in which multiple metal particles are immobilized on resin particles, resulting in a high metal particle loading and reduced metal particle detachment from the resin particles. Furthermore, the metal particles exhibit light energy absorption due to electron transition in addition to localized surface plasmon resonance. Therefore, the metal-resin composite of the present invention is excellent in handleability, durability, visibility, visual determination, and detection sensitivity. Therefore, it can be preferably applied for purposes such as labeling substances in various immunoassays, immunoassay reagents, pharmaceuticals, solid catalysts, pigments, paints, conductive materials, electrodes, and sensor elements. In particular, when the metal-resin composite of the present invention is used in immunoassays, it is excellent in handleability, durability, and visibility, nonspecific reactions are suppressed, and highly sensitive determination of various antigens and antibodies is possible without the need for additional special equipment or work processes.

[0028] FIG. 1 is a schematic diagram showing the cross-sectional structure of a metal-resin composite according to one embodiment of the present invention. FIG. 2 is a schematic diagram showing the cross-sectional structure of one aspect of a metal-resin composite. FIG. 3 is a schematic diagram showing the cross-sectional structure of another aspect of a metal-resin composite. FIG. 4 is an explanatory diagram showing an outline of a method for measuring an analyte using a lateral flow chromatographic test strip according to one embodiment of the present invention. FIG. 5 is a cross-sectional view of an immunochromatographic strip prepared in an example.

[0029] Hereinafter, an embodiment of the present invention will be described in detail with reference to the accompanying drawings. The metal-resin composite of this embodiment is applied to a labeling substance for immunoassay (hereinafter simply referred to as a "labeling substance") or a reagent for immunoassay (hereinafter simply referred to as a "reagent").

[0030] [Metal-Resin Composite] The metal-resin composite of the present embodiment comprises resin particles and a plurality of metal particles immobilized on the resin particles, and has a maximum zeta potential of 5 mV or more in the pH range of 3 to 6, a minimum zeta potential of −20 mV or less in the pH range of 8 to 10, and a zero charge point of the zeta potential in the pH range of 6.1 to 9.0, the metal particles are gold or alloy particles, and the CV value (Coefficient of Variation) of the particle diameter is 0.45 or less.

[0031] FIG. 1 is a cross-sectional schematic diagram of a metal-resin composite according to one embodiment of the present invention. The metal-resin composite 100 includes resin particles 10 and metal particles 20. In the metal-resin composite 100, the metal particles 20 are fixed to the resin particles 10. The resin particles 10 are preferably relatively larger than the metal particles 20. In other words, in the metal-resin composite 100, a large number of relatively small metal particles 20 are fixed to the large resin particles 10. In this case, as shown in FIG. 1, the relationship between the particle diameter D1 of the entire metal-resin composite 100, the particle diameter D2 of the resin particles 10, and the particle diameter D3 of the metal particles 20 is D1>D2>D3.

[0032] The average particle diameter of the metal-resin composite 100 (i.e., the average of the particle diameters D1 in FIG. 1) is preferably, for example, 30 to 1000 nm. If the average particle diameter of the metal-resin composite 100 is less than 30 nm, for example, the amount of metal particles 20 supported tends to be smaller, resulting in a tendency for the metal particles 20 to be less colored than metal particles 20 of the same size. If the average particle diameter of the metal-resin composite 100 exceeds 1000 nm, when used as a labeled substance or reagent, the metal-resin composite 100 tends to clog the pores of a chromatographic medium such as a membrane filter, and the dispersibility tends to decrease. The average particle diameter of the metal-resin composite 100 is preferably 600 nm or more, more preferably 500 nm, from the viewpoints of improving the dispersibility when used as a labeled substance or reagent and obtaining high detection sensitivity when the metal-resin composite 100 is used in immunoassays. On the other hand, the preferred lower limit is 100 nm, more preferably 200 nm, and even more preferably 300 nm. In particular, when the average particle diameter of the metal-resin composite 100 is 300 nm or more, stable and excellent detection sensitivity can be obtained when the metal-resin composite 100 is used as a labeling substance for immunochromatography. Here, the particle diameter of the metal-resin composite 100 means the value obtained by adding the length of the protruding portion of the partially exposed particles 40 or the surface-adsorbed particles 50 described below to the particle diameter of the resin particles 10, and can be measured by laser diffraction / scattering, dynamic light scattering, or centrifugal sedimentation.

[0033] <Zeta Potential> The metal-resin composite 100 has a maximum zeta potential of 5 mV or more in the pH range of 3 to 6, and a minimum zeta potential of -20 mV or less in the pH range of 8 to 10 (first characteristic). When the zeta potential is in this range, in an acidic environment (for example, when dispersed in a dispersion medium with a pH of less than 7), the metal-resin composite 100 has cationic functional groups on the surface of the composite and is positively charged. On the other hand, in a basic environment (for example, when dispersed in a dispersion medium with a pH of more than 7), the metal-resin composite 100 has anionic functional groups on the surface of the composite and is negatively charged. In other words, when an antigen, antibody, or blocking agent is bound to the surface of the metal-resin composite 100, the surface charge state is suitable for binding of the antigen, antibody, or blocking agent depending on the pH of the dispersion medium (binding buffer). Specifically, in an acidic environment, it can bind to antigens or antibodies with strong anionic properties, and in a basic environment, it can bind to antigens or antibodies with strong cationic properties. In other words, the metal-resin composite 100 can stably bind to any antigen or antibody, regardless of whether it is anionic or cationic. Therefore, it has high durability, stability, and versatility as a labeling substance for immunoassays and a reagent for immunoassays.

[0034] On the other hand, if the maximum value of the zeta potential is less than 5 mV in the pH range of 3 to 6, or if the minimum value of the zeta potential exceeds -20 mV in the pH range of 8 to 10, the metal-resin composite 100 will have poor dispersibility due to electrostatic repulsion, and the metal-resin composite 100 itself will be prone to aggregation. This makes it difficult to handle as a labeling substance for immunoassays and as a reagent for immunoassays, which is disadvantageous. From this perspective, a larger maximum value of the zeta potential is preferable, and a smaller minimum value is preferable. In the pH range of 3 to 6, the maximum value of the zeta potential is preferably 10 mV or more, and more preferably 20 mV or more. Furthermore, in the pH range of 8 to 10, the minimum value of the zeta potential is preferably -25 mV or less, and more preferably -30 mV or less.

[0035] For the same reason, the metal-resin composite 100 preferably has a difference between the maximum and minimum values ​​of the zeta potential of 20 mV or more (second characteristic) in the range of pH 3 to pH 10. More preferably, it is 40 mV or more, and even more preferably, it is 60 mV or more.

[0036] It should be noted that with the alkali treatment of resin particles 10 disclosed in Patent Document 3, it was difficult to reduce the minimum zeta potential of the gold-resin composite to −20 mV or less in the pH range of 8 to 10. Furthermore, with the mercaptopropionic acid treatment and polyglutamic acid treatment disclosed in Patent Document 3, although it was possible to control the zeta potential of the gold-resin composite, there was a problem in that the gold-resin composite had low dispersibility in water and was prone to aggregation and precipitation. In the present embodiment, as described below, the above problems are solved by selecting the type of resin that constitutes resin particles 10.

[0037] Furthermore, the metal-resin composite 100 has a zero charge point of the zeta potential in the range of pH 6.1 to pH 9.0 (third characteristic). Here, the zero charge point is the point where the zeta potential is zero. If the zero charge point is within the above range, it is possible to make the surface charge of the metal-resin composite 100 have a wide range of charge states, both positive and negative, in weakly acidic to weakly basic environments where molecular biochemical reactions typically occur, which is preferable. In particular, if the third characteristic is also satisfied in addition to the first and second characteristics, this means that the zeta potential changes significantly from the positive side to the negative side or from the negative side to the positive side in the pH range of 6.1 to pH 9.0, thereby enabling excellent dispersibility to be exhibited in a wide pH range, both in acidic environments including weakly acidic and basic environments including weakly basic. A preferred lower limit is pH 6.2, more preferably pH 6.3. On the other hand, a preferred upper limit is pH 8.5, more preferably pH 8.0. An even more preferred upper limit is pH 7.8. On the other hand, if the point of zero charge is outside the above range, it tends to be impossible to achieve a bipolar charge state unless the environment is relatively strongly acidic or strongly basic.

[0038] The reason why the metal-resin composite 100 of the present embodiment exhibits characteristic zeta potential behavior is that the metal-resin composite particle 100 has both a "cationic functional group" and an "anionic functional group" on the surface thereof. This point will be described later.

[0039] <Resin Particles> The structure and composition of the resin particles 10 are not limited, but the resin particles 10 are preferably particles of a polymer having a substituent in its structure capable of adsorbing metal ions. Examples of polymers having a substituent in their structure capable of adsorbing metal ions include polymers capable of adsorbing anionic ions and polymers capable of adsorbing cationic ions.

[0040] As a polymer capable of adsorbing anionic ions, a nitrogen-containing polymer is particularly preferred. The nitrogen-containing polymer is a resin having nitrogen atoms in the main chain or side chain, such as polyamine, polyamide, polypeptide, polyurethane, polyurea, polyimide, polyimidazole, polyoxazole, polypyrrole, polyaniline, etc. Preferred are polyamines such as poly-2-vinylpyridine, poly-3-vinylpyridine, and poly-4-vinylpyridine. Furthermore, when a nitrogen atom is present in the side chain, a wide range of resins can be used, such as acrylic resins, phenolic resins, and epoxy resins. The nitrogen atoms in the nitrogen-containing polymer are useful for [AuCl] as a precursor of gold particles, which are metal particles 20 that have excellent visibility and are easy to immobilize antigens or antibodies on. 4 ] - In this embodiment, the metal ions adsorbed in the nitrogen-containing polymer are reduced to form metal particles 20, and some of the generated metal particles 20 become encapsulated particles 30 or partially exposed particles 40. Anionic ions of metal compounds such as platinum, palladium, silver, nickel, and copper can also be used in a similar manner.

[0041] The polymer capable of adsorbing cationic ions is a resin having a carboxylic acid group, a sulfonic acid group, or the like in the main chain or side chain. Specific examples of the polymer capable of adsorbing cationic ions include a carboxylic acid group-containing polymer such as an acrylic acid polymer and a sulfonic acid group-containing polymer such as polystyrene sulfonic acid, and more specifically, polyacrylic acid, vinyl carboxylate, polyvinyl acetate, polyvinyl sulfonic acid, polystyrene sulfonic acid, etc. The polymer capable of adsorbing cationic ions is capable of adsorbing Au due to the carboxylic acid group, sulfonic acid group, etc. contained therein. + For example, chemisorbed Au + to form metal particles 20 (gold particles in this case). Other cationic ions such as platinum, palladium, silver, nickel, and copper can also be used.

[0042] The polymer capable of adsorbing anionic ions is cationic, and therefore acts to shift the zeta potential of the metal-resin composite 100 to the positive side in an acidic environment. On the other hand, the polymer capable of adsorbing cationic ions is anionic, and therefore acts to shift the zeta potential of the metal-resin composite 100 to the negative side in a basic environment.

[0043] Note that examples of polymers other than those having a substituent capable of adsorbing metal ions in their structure include polystyrene, but in this case, it is difficult for metal ions to be adsorbed inside the resin particles 10. As a result, most of the generated metal particles 20 become surface-adsorbed particles 50. As will be described later, the surface-adsorbed particles 50 have a small contact area with the resin particles 10, and therefore the adhesive force between the resin particles 10 and the metal is small, and the metal particles 20 tend to detach from the resin particles 10 easily.

[0044] The polymer having a substituent capable of adsorbing metal ions in its structure may be a copolymer with a known polymerizable monomer. Examples of copolymers include random copolymers, block copolymers, alternating copolymers, and copolymers in which polymers are crosslinked. Furthermore, resin particles 10 may be formed by copolymerizing two or more types of monomers, or a monomer may be reacted with functional groups present on the surface of resin particles 10, and the resulting monomer may be used as an active terminal for polymerization and further polymerized. While the copolymerization composition is not limited, it is preferable that the monomer containing the substituent capable of adsorbing metal ions is 10 mol % or more. Polymerizable monomers can be selected without limitation depending on the application of the metal-resin composite 100. For example, polymerizable monomers with surfactant properties can be used to improve the shape and size uniformity and dispersion stability of resin particles 10. Examples of such polymerizable monomers include polyethylene glycol methyl ether methacrylate and polyethylene glycol dimethacrylate.

[0045] Furthermore, the resin particles 10 of this embodiment preferably contain two or more types of polymers. By having both "cationic functional groups" and "anionic functional groups" on the surface, the metal-resin composite 100 effectively exhibits the first to third characteristics, which are characteristic behaviors of the zeta potential. Therefore, when the resin particles 10 contain a first polymer and a second polymer of a different type from the first polymer, it is preferable that one of the first polymer and the second polymer is a "polymer having a cationic functional group" and the other is a "polymer having an anionic functional group." Here, examples of "cationic functional groups" include nitrogen-containing groups such as pyridinyl groups, amino groups, amide groups, imide groups, and imidazole groups. Examples of "anionic functional groups" include carboxyl groups, sulfonic acid groups, phosphonic acid groups, phosphate groups, and silanol groups. Furthermore, the resin particles 10 of this embodiment may be a copolymer having a polymer segment having the cationic functional group and a polymer segment having the anionic functional group. Here, preferred cationic functional groups and anionic functional groups are as described above. The copolymer may be a random copolymer, a block copolymer, an alternating copolymer, or the like.

[0046] For example, when the first polymer is a nitrogen-containing polymer, polyvinylpyridine, and the second polymer is polymethacrylic acid, the pyridine contained in the polyvinylpyridine is a "cationic functional group," and the carboxyl group contained in the polymethacrylic acid is an "anionic functional group." In an acidic environment, the nitrogen of the pyridine becomes NH + In a basic environment, the nitrogen of pyridine becomes uncharged in the N state and the carboxyl group becomes uncharged in the COO state, so that the metal-resin composite 100 has a positive surface charge as a whole. - Since the metal-resin composite 100 has a negative charge in this state, the surface charge of the metal-resin composite 100 is negative overall. As a result, it is believed that the zeta potential of the metal-resin composite 100 exhibits the first to third characteristics described above.

[0047] On the other hand, in Patent Document 3, for gold-resin composites, carboxyl groups, which are "anionic functional groups," are generated in the nitrogen-containing polymer polyvinylpyridine by hydrolysis of the surface of resin particles 10 through strong alkali treatment, or carboxyl groups are introduced into metal-resin composites 100 through mercaptopropionic acid treatment or polyglutamic acid treatment. However, hydrolysis of the surface of resin particles 10 damages the resin particles 10 themselves through strong alkali treatment, which may have resulted in large fluctuations in the particle size of the gold particles. Furthermore, with mercaptopropionic acid treatment or polyglutamic acid treatment, molecules containing carboxyl groups are merely adsorbed to the surface of the gold-resin composite, making them prone to detachment, which is thought to have led to reduced dispersibility in water. In contrast, in the present embodiment, resin particles 10 contain a second polymer polymerized on the surface or inside of the first polymer, preventing the "anionic functional groups" from detaching from resin particles 10 and effectively maintaining their function as "anionic functional groups." This is thought to be the reason why the first to third properties are fully exhibited, the dispersibility in water is improved, and a stable dispersed state can be maintained.

[0048] In general, polymers capable of adsorbing anionic ions often have a “cationic functional group,” and polymers capable of adsorbing cationic ions often have an “anionic functional group.” Therefore, in a combination of a first polymer and a second polymer, the first polymer may be selected from polymers capable of adsorbing anionic ions, and the second polymer may be selected from polymers capable of adsorbing cationic ions, or the first polymer may be selected from polymers capable of adsorbing cationic ions, and the second polymer may be selected from polymers capable of adsorbing anionic ions.

[0049] When the first polymer is the main polymer constituting the resin particle 10, it is presumed that the surface of the resin particle 10 preferably has a structure in which the second polymer is present on the surface or inside of the first polymer. Therefore, the molar ratio of the cationic functional groups contained in the first polymer to the anionic functional groups contained in the second polymer (cationic functional groups contained in the first polymer: anionic functional groups contained in the second polymer) is preferably within a range of, for example, 99.5:0.5 to 80:20. A more preferred upper limit for the molar ratio of the cationic functional groups contained in the first polymer is 99, and a more preferred lower limit is 90. By ensuring that the ratio of the cationic functional groups contained in the first polymer to the anionic functional groups contained in the second polymer falls within the above range, the amounts of the "cationic functional groups" and "anionic functional groups" become optimal, making it easier to control the zeta potential.

[0050] <Metal Particles> In the metal-resin composite 100, the metal particles 20 are gold or gold alloy particles. Compared to metal-resin composites containing particles of other metal species, gold-resin composites using gold particles as the metal particles 20 are less likely to aggregate when bound to a ligand such as an antibody, and are extremely dispersible. Furthermore, they have excellent visibility and facilitate the immobilization of antigens or antibodies. In particular, by controlling the particle diameter of the gold particles and the interparticle distance between the gold particles, various colors such as red, purple, and blue can be produced. Therefore, when using gold-resin composites as labeling substances for immunochromatography, labeling substances of various colors can be obtained. Furthermore, the effects of the present invention are more pronounced when the metal particles 20 are gold or gold alloy particles. Here, a gold alloy refers to an alloy composed of gold and a metal species other than gold, containing 1% by weight or more, preferably 10% by weight or more, more preferably 50% by weight or more, and even more preferably 60% by weight or more of gold. In this case, the other metal species that form an alloy with gold is not particularly limited, but for example, platinum, silver, nickel, copper, palladium, etc. are preferred.

[0051] Furthermore, the metal particles 20 may contain particles of other metals in addition to particles of gold or its alloy. Platinum, palladium, silver, nickel, and copper are preferred as such metals, from the viewpoint of ease of nano-composite formation of metal and resin. These metals can be used alone or as alloys. For example, a platinum alloy refers to an alloy consisting of platinum and a metal species other than platinum, containing 1 wt. % or more, preferably 10 wt. % or more, more preferably 50 wt. % or more, and even more preferably 60 wt. Even when the metal particles 20 are particles of a metal other than gold or its alloy, the zeta potential can be controlled in the same manner as in the present invention.

[0052] Furthermore, the average particle diameter of the gold particles as metal particles 20 measured by scanning electron microscope (SEM) observation (i.e., the average particle diameter D3 in FIG. 1 ) is preferably, for example, 1 to 100 nm. If the average particle diameter of the gold particles is less than 1 nm or more than 100 nm, localized surface plasmon resonance and light energy absorption by electronic transition are less likely to occur, and sensitivity tends to decrease. Furthermore, from the viewpoint of obtaining high detection sensitivity as a labeling substance for immunoassays and as a reagent for immunoassays, the average particle diameter of the gold particles preferably has an upper limit of 25 nm, more preferably 20 nm, and even more preferably 15 nm. Meanwhile, the preferred lower limit is 2 nm. In the metal-resin composite 100 of the present embodiment, the average particle diameter of the gold particles can be reduced to 20 nm or less by using a specific reducing agent solution described below in the process of reducing gold ions to gold particles.

[0053] Furthermore, the CV value (Coefficient of Variation) of the particle diameter of the gold particles serving as the metal particles 20 is 0.45 or less. If the CV value exceeds 0.45, the results tend to vary greatly when applied to immunochromatography, reducing the reliability of the immunological test. Therefore, the CV value is preferably 0.44 or less, and more preferably 0.43 or less. In the metal-resin composite 100 of this embodiment, the CV value of the particle diameter of the gold particles can be controlled to 0.45 or less by using a specific reducing agent solution in the process of reducing gold ions to gold particles.

[0054] <State of Presence of Metal Particles> The state of presence of the metal particles 20 in the metal-resin composite 100 is not limited. For example, the metal particles 20 may be two-dimensionally distributed on the surface of the resin particles 10, or the metal particles 20 may be encapsulated within the resin particles 10. Alternatively, a core-shell structure may be formed in which the resin particles 10 serve as the shell and the metal particles 20 serve as the core. Alternatively, some of the metal particles 20 may be three-dimensionally distributed in the surface layer 60 of the resin particles 10. In this case, some of the three-dimensionally distributed metal particles 20 may be partially exposed to the outside of the resin particles 10, or the remaining part may be encapsulated in the resin particles 10. Specifically, as shown in FIG. 1 , the metal particles 20 preferably include metal particles completely encapsulated in the resin particles 10 (also referred to as "encapsulated particles 30") and metal particles having a portion embedded in the resin particles 10 and a portion exposed to the outside of the resin particles 10 (also referred to as "partially exposed particles 40"). In addition, metal particles adsorbed on the surfaces of the resin particles 10 (also referred to as "surface-adsorbed particles 50") may also be present.

[0055] When the metal-resin composite 100 is used as a labeling substance for immunoassays or a reagent for immunoassays, an antigen, antibody, or blocking agent is immobilized on the surface of the resin particle 10 or on the surface of the partially exposed particle 40 or the surface-adsorbed particle 50. In this case, the antigen, antibody, or blocking agent is immobilized on the partially exposed particle 40 and the surface-adsorbed particle 50, while it is thought that the antigen, antibody, or blocking agent is not easily immobilized on the encapsulated particle 30. However, since the partially exposed particle 40, the surface-adsorbed particle 50, and the encapsulated particle 30 all exhibit localized surface plasmon resonance and light energy absorption due to electronic transition, not only the partially exposed particle 40 and the surface-adsorbed particle 50, but also the encapsulated particle 30 contributes to improving the visibility of the labeling substance for immunoassays and the reagent for immunoassays. Furthermore, the partially exposed particle 40 and the encapsulated particle 30 have a larger contact area with the resin particle 10 than the surface-adsorbed particle 50, and due to the anchoring effect and other effects of the embedded state, they have a stronger physical adsorption force and are less likely to detach from the resin particle 10. Furthermore, the antigen, antibody, or blocking agent adsorbed to the partially exposed particles 40 or the surface-adsorbed particles 50 is difficult to detach because it forms a coordinate bond with the metal, which makes it possible to improve the durability and stability of immunoassay labeling substances and immunoassay reagents that use the metal-resin composite 100.

[0056] In the metal-resin composite 100, the encapsulated particles 30 have their entire surfaces covered with the resin that constitutes the resin particles 10. The partially exposed particles 40 have 5% or more and less than 100% of their surface area covered with the resin that constitutes the resin particles 10, and from the viewpoint of the durability of the immunoassay labeling substance and the immunoassay reagent, the lower limit is preferably 20% or more, more preferably 30% or more of the surface area. The surface-adsorbed particles 50 preferably have more than 0% and less than 5% of their surface area covered with the resin that constitutes the resin particles 10.

[0057] Furthermore, the amount of metal particles 20 (the total of the encapsulated particles 30, the partially exposed particles 40, and the surface-adsorbed particles 50) supported on the metal-resin composite 100 is preferably 3 wt % to 80 wt % relative to the weight of the metal-resin composite 100. Within this range, the metal-resin composite 100 has excellent visibility, visual determination, and detection sensitivity as a labeled substance. If the amount of metal particles 20 supported is less than 3 wt %, the amount of immobilized antibody or antigen tends to decrease, and detection sensitivity tends to decrease. On the other hand, if the amount of metal particles 20 supported exceeds 80 wt %, the particle diameter of the metal particles 20 tends to increase significantly, and the light absorption characteristics of the metal particles 20 tend to decrease. The amount of metal particles 20 supported is more preferably 15 wt % to 70 wt %, and even more preferably 15 wt % to 60 wt %.

[0058] Furthermore, it is preferable that 10% by weight to 90% by weight of the metal particles 20 are partially exposed particles 40 and surface-adsorbed particles 50. Within this range, a sufficient amount of antibody or antigen can be immobilized on the metal particles 20, resulting in high sensitivity as a labeling substance. It is more preferable that 20% by weight to 80% by weight of the metal particles 20 are partially exposed particles 40 and surface-adsorbed particles 50, and from the viewpoint of the durability of the labeling substance for immunoassay and the immunoassay reagent, it is even more preferable that the surface-adsorbed particles 50 be 20% by weight or less.

[0059] Furthermore, when using the metal-resin composite 100 in immunoassays, in order to obtain excellent detection sensitivity, 60% to 100% by weight, preferably 75% to 100% by weight, more preferably 85% to 100% by weight of the metal particles 20 should be present in the surface layer 60, and even more preferably within 40% of the particle radius in the depth direction from the surface of the resin particle 10. Furthermore, it is preferable that 5% to 90% by weight of the metal particles 20 present in the surface layer 60 are partially exposed particles 40 or surface-adsorbed particles 50, since this ensures a sufficient amount of antibody or antigen immobilized on the metal particles 20, thereby increasing the sensitivity as a labeling substance. In other words, it is preferable that 10% to 95% by weight of the metal particles 20 present in the surface layer 60 are encapsulated particles 30.

[0060] Here, the "surface layer" refers to the range from the surface of the resin particle 10 to 50% of the particle radius in the depth direction, based on the outermost position of the metal-resin composite 100 (i.e., the protruding end of the partially exposed particle 40 or the surface-adsorbed particle 50). Furthermore, the "three-dimensionally distributed" refers to the metal particles 20 being dispersed not only in the plane direction of the resin particle 10 but also in the depth direction.

[0061] As described above, the encapsulated particles 30 also exhibit light energy absorption due to electronic transition in addition to localized surface plasmon resonance. Therefore, not only the partially exposed particles 40 and the surface-adsorbed particles 50, but also the encapsulated particles 30 contribute to improving the visibility of the immunoassay labeling substance and the immunoassay reagent. From the perspective of such improved visibility, it is preferable that the encapsulated particles 30 in the metal-resin composite 100 are concentrated and distributed within a certain range from the surface of the resin particle 10 in the depth direction, as shown in FIG. 2A , for example, and that no encapsulated particles 30 are present near the center of the resin particle 10. More specifically, in order to effectively exhibit light energy absorption due to electronic transition in addition to localized surface plasmon resonance by the encapsulated particles 30, for example, when the particle diameter D2 of the resin particle 10 is 800 nm, 70% by weight or more, preferably 80% by weight or more, and more preferably 90 to 100% by weight of the encapsulated particles 30 are present within a range of, for example, 0 to 200 nm from the surface of the resin particle 10 in the depth direction. In particular, it is preferable that the region where all of the encapsulated particles 30 (100% by weight) are distributed (encapsulated particle distribution region) is within a range of, for example, 0 to 100 nm from the surface of the resin particle 10, because this maximizes the occurrence of light energy absorption due to electronic transition in addition to localized surface plasmon resonance due to the encapsulated particles 30.

[0062] Furthermore, the metal-resin composite 100 may not have encapsulated particles 30. For example, as shown in FIG. 2B , in the metal-resin composite 100, all of the metal particles 20 may be fixed to the surface of the resin particle 10 without overlapping with each other in the radial direction of the resin particle 10. In this case, the metal particles 20 are composed of partially exposed particles 40 and / or surface-adsorbed particles 50.

[0063] [Method for Manufacturing Metal-Resin Composite] The method for manufacturing the metal-resin composite 100 is not particularly limited, but an example is as follows: Here, an example is given in which the first polymer is a nitrogen-containing polymer, polyvinylpyridine, and the second polymer is polymethacrylic acid.

[0064] First, a dispersion of polyvinylpyridine particles is produced by emulsion polymerization. Next, an aqueous solution of methacrylic acid is added dropwise to the resulting dispersion to cause soap-free polymerization. This results in polymethacrylic acid being incorporated into the polyvinylpyridine particles, resulting in a dispersion of resin particles 10 having numerous carboxyl groups derived from methacrylic acid on their surfaces or interiors. At this time, it is estimated that the surface or interior of the resin particles 10 has a structure in which polymethacrylic acid, as a second polymer, is present within polyvinylpyridine, as a first polymer.

[0065] Next, a solution containing metal ions is added to the dispersion of the resin particles 10 to adsorb the metal ions to the resin particles 10 (hereinafter referred to as "metal ion-adsorbed resin particles"). For example, when gold particles are to be produced as the metal particles 20, a solution containing gold ions is added to the dispersion of the resin particles 10 (hereinafter referred to as "metal ion-adsorbed resin particles"). 4 In place of gold ions, a gold complex may be used.

[0066] Alternatively, instead of water, a solvent for the solution containing metal ions may be used, such as a hydrous alcohol or alcohol, such as methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, or t-butanol, or an acid, such as hydrochloric acid, sulfuric acid, or nitric acid. If necessary, additives may be added to the solution, such as water-soluble polymers, such as polyvinyl alcohol; surfactants; alcohols; ethers, such as tetrahydrofuran, diethyl ether, or diisopropyl ether; polyols, such as alkylene glycol, polyalkylene glycol, their monoalkyl ethers, or dialkyl ethers, or glycerin; or various water-miscible organic solvents, such as ketones, such as acetone or methyl ethyl ketone. Such additives are effective in accelerating the reduction reaction rate of the metal ions and controlling the size of the generated metal particles 20.

[0067] Next, the metal ion-adsorbing resin particles are added to a reducing agent solution to reduce the metal ions and generate metal particles 20, thereby obtaining a metal-resin composite 100. Known reducing agents can be used. Examples of reducing agents include sodium borohydride, dimethylamine borane, citric acid, sodium hypophosphite, hydrazine hydrate, hydrazine hydrochloride, hydrazine sulfate, formaldehyde, sucrose, glucose, ascorbic acid, erythorbic acid, sodium phosphinate, hydroquinone, and Rochelle salt. Of these, sodium borohydride, dimethylamine borane, and citric acid are preferred.

[0068] The reducing agent solution used in the reduction step is preferably a mixture of a buffer solution adjusted to a pH of 3 to 8, more preferably a pH of 4 to 7, and even more preferably a pH of 5 to 6.5, and a reducing agent. Using such a reducing agent solution makes it easier to control the average particle size of the gold particles serving as metal particles 20 to 20 nm or less, and the CV value of the particle size can be 0.45 or less. The reason why it was difficult to control the average particle size of the gold particles to 20 nm or less in the gold-resin composite of Patent Document 3 is thought to be that the pH of the reducing agent solution shifts toward the acidic side due to the influence of hydrogen ions and halogen ions generated from metal halides such as chloroauric acid during the reduction process, making it difficult for the hydrogen ions and halogen ions to desorb from the resin particles 10, slowing the reduction reaction, and causing the gold particles to enlarge. It is presumed that the reducing agent solution, which is a mixture of a pH-adjusted buffer solution and a reducing agent, promotes the detachment of halogen ions from the resin particles 10, thereby accelerating the reduction reaction and generating a large number of gold particle nuclei, making it easier to control the average particle diameter of the gold particles to 20 nm or less.

[0069] The compound used in the buffer solution is not particularly limited. However, in order to prevent metal ions from detaching from the resin particles 10 and to achieve uniform nucleation and growth of gold particles, it is preferable to use a primary buffer in combination with a basic compound that exhibits a basicity of pH 7 or higher when dissolved in water as an additive to the primary buffer. Examples of the primary buffer include Good's buffers with a pKa of 5.5 to 7.5 at 20°C. Examples of preferred Good's buffers include 2-morpholinoethanesulfonic acid (MES), bis(2-hydroxyethyl)iminotris(hydroxymethyl)methane (Bis-Tris), N-(2-acetamido)iminodiacetic acid (ADA), piperazine-1,4-bis(2-ethanesulfonic acid) (PIPES), and N-(2-acetamido)-2-aminoethanesulfonic acid (ACES). Examples of basic compounds used as additives include buffers, alkali metal compounds, and nitrogen-containing compounds having a pKa of 7.6 to 12 at 20°C. Nitrogen-containing compounds that exhibit a basicity of pH 7 or higher when dissolved in water are particularly preferred. Nitrogen-containing compounds preferably used in the reduction step include 2-amino-2-(hydroxymethyl)-1,3-propanediol, ammonia, methylamine, dimethylamine, trimethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine methyl, dimethylaminoethanol, isopropylaminoethanol, isobutylamine, and morpholine. When a primary buffer and a basic compound are used in combination, a molar ratio of 2:8 to 8:2 is preferred, and a molar ratio of 3:7 to 7:3 is more preferred. The pH of the buffer can be adjusted by adding an acid such as hydrochloric acid or sulfuric acid, or an alkali such as sodium hydroxide or potassium hydroxide, as needed. Furthermore, in the reduction step, a surfactant is preferably used in combination to form a stable metal-resin composite 100. Examples of surfactants include nonionic surfactants.Examples of nonionic surfactants preferably used in the reduction step include polyethylene glycol octylphenyl ether (Triton X-100), polyoxyethylene sorbitan monolaurate (Tween 20), glycerin laurate, glycerin monostearate, sorbitan fatty acid esters, polyoxyethylene alkyl ethers, pentaethylene glycol monododecyl ether, polyoxyethylene alkylphenyl ethers, octylphenol ethoxylate, nonylphenol ethoxylate, and polyoxyethylene polyoxypropylene glycol.

[0070] Furthermore, the particle size of the metal particles 20 to be produced can be controlled by adjusting the reduction rate of the metal ions through the temperature of the reducing agent solution.

[0071] When reducing the metal ions in the metal ion-adsorbing resin particles to generate metal particles 20, the metal ion-adsorbing resin particles may be added to a reducing agent solution, or the reducing agent may be added to the metal ion-adsorbing resin particles, but the former is preferred from the viewpoint of ease of generating the encapsulated particles 30 and the partially exposed particles 40.

[0072] Furthermore, in order to maintain the dispersibility of the metal-resin composite 100 in water, a dispersant such as citric acid, poly-L-lysine, polyvinylpyrrolidone, polyvinylpyridine, polyvinyl alcohol, DISPERBYK194, DISPERBYK180, or DISPERBYK184 (manufactured by BIGChemie Japan) may be added. Furthermore, the dispersibility can be maintained by adjusting the pH with a buffer such as boric acid or phosphoric acid, an acid such as hydrochloric acid or sulfuric acid, or an alkali such as sodium hydroxide or potassium hydroxide.

[0073] The metal-resin composite 100 having the above configuration can be preferably used as a labeling substance in various immunoassays, particularly by adsorbing an antigen or antibody onto the surface of the metal particles 20. Furthermore, the metal-resin composite 100 can be preferably used as a material for a labeling substance for immunoassays or a reagent for immunoassays, which has excellent visual recognition in the low concentration range (high sensitivity range). In this embodiment, as described above, the resin particles 10 contain a second polymer polymerized on the surface or inside of a first polymer, thereby obtaining resin particles 10 that are both anionic and cationic. As a result, the resin particles 10 exhibit the first to third properties related to the zeta potential, while also improving dispersibility in water and maintaining a stable dispersion state. Furthermore, the form of the labeling substance for immunoassays or the reagent for immunoassays is not particularly limited. For example, the metal-resin composite 100 can be used as a dispersion in water or a pH-adjusted buffer solution.

[0074] The method for adsorbing the antigen or antibody onto the surface of the metal particles 20 is not particularly limited, and known physical adsorption and chemical adsorption methods can be used. Chemical adsorption is preferred because it strengthens the bond between the metal particles 20 and the antigen or antibody. Physical adsorption and chemical adsorption may be used in combination.

[0075] Examples of physical adsorption include a method of immersing the metal-resin composite 100 in a buffer solution containing an antigen or antibody and incubating it, and a method of immersing the metal-resin composite 100 in a buffer solution and then adding an antigen or antibody.

[0076] Examples of chemical adsorption include a method of introducing an SH group into an antigen or antibody and reacting it with the metal-resin composite 100 to form a metal-SH bond, and a method of introducing a carboxyl group onto the surface of the metal-resin composite 100, followed by succinimidylation and reaction with the amino group of the antigen or antibody to form a chemical bond. Compounds suitable for introducing a carboxyl group onto the surface of the metal-resin composite 100 include compounds having both a carboxyl group and a functional group capable of coordinating with the metal, such as an amino group, an SH group, a carbonyl group, an amide group, or an imide group. Because of their strong coordinate bond with the metal, an SH group is preferred as the functional group. Examples of compounds having an SH group and a carboxyl group at both ends include mercaptopropionic acid, mercaptoundecanoic acid, and mercaptolauric acid. Furthermore, polymeric compounds having multiple carboxyl groups and functional groups capable of coordinating with the metal within a single molecule are more likely to form a stable bond with the metal-resin composite 100. For example, polyglutamic acid and polyaspartic acid, which are polypeptides of glutamic acid and aspartic acid, are more preferable as polymer compounds for introducing carboxyl groups onto the surface of the metal-resin composite 100 .

[0077] Next, a method for measuring an analyte using the metal-resin composite 100 as a labeling substance, a test strip for lateral flow chromatography, and an analyte detection and quantification kit will be described.

[0078] [Lateral flow chromatography test strip] First, a lateral flow chromatography test strip (hereinafter, sometimes simply referred to as a "test strip") according to one embodiment of the present invention will be described with reference to Figure 3. This test strip 200 is preferably usable in the analyte measurement method according to one embodiment of the present invention, as will be described later.

[0079] The test strip 200 includes a membrane 110. The membrane 110 is provided with a sample application section 120, a determination section 130, and a liquid absorption section 140, which are arranged in this order in the direction in which the sample develops.

[0080] <Membrane> The membrane 110 in the test strip 200 can be made of materials commonly used as membranes in general test strips. The membrane 110 is formed of an inert material (a material that does not react with the analyte 160, various ligands, etc.) that exhibits capillary action and is made of a microporous material that allows the sample to develop upon application. Specific examples of the membrane 110 include fibrous or nonwoven fibrous matrices made of polyurethane, polyester, polyethylene, polyvinyl chloride, polyvinylidene fluoride, nylon, cellulose derivatives, etc., membranes, filter paper, glass fiber filter paper, cloth, cotton, etc. Among these, membranes, filter paper, glass fiber filter paper, etc. made of cellulose derivatives or nylon are preferred, and nitrocellulose membranes, mixed nitrocellulose ester (a mixture of nitrocellulose and cellulose acetate) membranes, nylon membranes, and filter paper are more preferred.

[0081] For easier handling, test strip 200 preferably includes a support for supporting membrane 110. The support may be made of, for example, plastic.

[0082] <Sample Addition Section> The test strip 200 may have a sample addition section 120 for adding a sample containing an analyte 160. The sample addition section 120 is a site for receiving the sample containing the analyte 160 in the test strip 200. The sample addition section 120 may be formed on the membrane 110 upstream of the determination section 130 in the direction in which the sample develops, or the sample addition section 120 may be formed by providing a sample addition pad made of a material such as cellulose filter paper, glass fiber, polyurethane, polyacetate, cellulose acetate, nylon, or cotton cloth on the membrane 110.

[0083] <Determination Unit> A capture ligand 131 that specifically binds to the analyte 160 is immobilized on the determination unit 130. Any capture ligand 131 can be used without particular limitation as long as it forms a specific bond with the analyte 160, and for example, an antibody against the analyte 160 can be preferably used. The capture ligand 131 is immobilized so that it does not move from the determination unit 130 even when a sample is provided to the test strip 200. The capture ligand 131 may be immobilized directly or indirectly to the membrane 110 by physical or chemical bonding, adsorption, or the like.

[0084] The determination unit 130 is not particularly limited as long as it has a configuration that allows the complex 170 containing the labeled antibody 150 and the analyte 160 to come into contact with the capture ligand 131 that specifically binds to the analyte 160. For example, the capture ligand 131 may be immobilized directly on the membrane 110, or the capture ligand 131 may be immobilized on a pad made of cellulose filter paper, glass fiber, nonwoven fabric, or the like that is immobilized on the membrane 110.

[0085] <Liquid-Absorbing Section> The liquid-absorbing section 140 is formed by a pad of a water-absorbent material such as cellulose filter paper, nonwoven fabric, cloth, or cellulose acetate. The speed at which the development front of the added sample moves after it reaches the liquid-absorbing section 140 varies depending on the material and size of the liquid-absorbing section 140. Therefore, by selecting the material, size, etc. of the liquid-absorbing section 140, it is possible to set an optimal speed for detecting and quantifying the analyte 160. The liquid-absorbing section 140 is an optional configuration and may be omitted.

[0086] Test strip 200 may further include any desired portions such as a reaction portion and a control portion, as needed.

[0087] <Reaction Unit> Although not shown, the test strip 200 may have a reaction unit containing a labeled antibody 150 formed on the membrane 110. The reaction unit may be located upstream of the determination unit 130 in the direction of sample flow. The sample addition unit 120 in FIG. 3 may also be used as the reaction unit. When the test strip 200 has a reaction unit, when a sample containing an analyte 160 is supplied to the reaction unit or sample addition unit 120, the analyte 160 contained in the sample can be brought into contact with the labeled antibody 150 in the reaction unit. In this case, simply supplying the sample to the reaction unit or sample addition unit 120 can form a complex 170 containing the analyte 160 and the labeled antibody 150, thereby enabling so-called one-step immunochromatography.

[0088] The reaction area is not particularly limited as long as it contains labeled antibody 150 that specifically binds to analyte 160, but may be formed by directly applying labeled antibody 150 to membrane 110. Alternatively, the reaction area may be formed by immobilizing a pad (conjugate pad) made of, for example, cellulose filter paper, glass fiber, nonwoven fabric, or the like, impregnated with labeled antibody 150, on membrane 110.

[0089] <Control Section> Although not shown, the test strip 200 may have a control section formed on the membrane 110 downstream of the determination section 130 in the direction of sample development, where a capture ligand that specifically binds to the labeled antibody 150 is immobilized. By measuring the color intensity in the control section as well as the determination section 130, it is possible to confirm that the sample provided to the test strip 200 developed and reached the reaction section and the determination section 130, and that the test was performed normally. The control section can be fabricated in the same manner as the above-described determination section 130 and can have the same configuration, except that the capture ligand 131 is replaced with a different type of capture ligand that specifically binds to the labeled antibody 150.

[0090] [Method for Measuring Analyte] Next, a method for measuring analyte 160 using test strip 200 according to one embodiment of the present invention will be described.

[0091] The method for measuring analyte 160 according to this embodiment is a method for detecting or quantifying analyte 160 contained in a sample. The method for measuring analyte 160 according to this embodiment uses a test strip 200 including a membrane 110 and a determination part 130 having a capture ligand 131 that specifically binds to analyte 160 immobilized on the membrane 110. The method for measuring analyte 160 in this embodiment can include the following steps (I) to (III): step (I): bringing analyte 160 contained in a sample into contact with labeled antibody 150, which is an antibody that specifically binds to analyte 160 and is labeled with metal-resin composite 100 having a structure in which a plurality of metal particles 20 are immobilized on resin particle 10; step (II): bringing complex 170 containing analyte 160 and labeled antibody 150, which was formed in step (I), into contact with capture ligand 131 in determination unit 130; and step (III): measuring the color intensity resulting from light energy absorption due to localized surface plasmon resonance and / or electron transition of metal-resin composite 100.

[0092] Step (I): Step (I) is a step of contacting the analyte 160 contained in the sample with the labeled antibody 150. The manner of contact is not particularly limited as long as a complex 170 containing the analyte 160 and the labeled antibody 150 is formed. For example, the sample may be provided to the sample application section 120 or a reaction section (not shown) of the test strip 200, and the analyte 160 may be contacted with the labeled antibody 150 in the sample application section 120 or the reaction section, or the analyte 160 in the sample may be contacted with the labeled antibody 150 before the sample is provided to the test strip 200.

[0093] The complex 170 formed in step (I) develops and moves on the test strip 200 and reaches the determination section 130 .

[0094] Step (II): In step (II), the complex 170 containing the analyte 160 and the labeled antibody 150 formed in step (I) is brought into contact with the capture ligand 131 in the determination zone 130 of the test strip 200. When the complex 170 is brought into contact with the capture ligand 131, the capture ligand 131 specifically binds to the analyte 160 of the complex 170. As a result, the complex 170 is captured in the determination zone 130.

[0095] Note that because the capture ligand 131 does not specifically bind to the labeled antibody 150, when the labeled antibody 150 that is unbound to the analyte 160 reaches the determination zone 130, the unbound labeled antibody 150 passes through the determination zone 130. If the test strip 200 has a control zone (not shown) to which another capture ligand that specifically binds to the labeled antibody 150 is immobilized, the labeled antibody 150 that has passed through the determination zone 130 continues to develop and binds to the other capture ligand in the control zone. As a result, the labeled antibody 150 that has not formed a complex 170 with the analyte 160 is captured in the control zone.

[0096] After step (II), and before step (III), if necessary, a washing step may be performed to wash the test strip 200 with a buffer solution commonly used in biochemical tests, such as water, physiological saline, or phosphate buffer solution. The washing step can remove labeled antibodies 150 that have not been captured in the determination zone 130 or in the determination zone 130 and control zone (labeled antibodies 150 that have not bound to the analyte 160 and have not formed complexes 170).

[0097] By carrying out the washing step, when measuring color development due to light energy absorption caused by localized surface plasmon resonance and / or electron transition of the metal-resin composite 100 in the determination section 130, or in the determination section 130 and the control section, in step (III), the background color development intensity can be reduced, the signal / background ratio can be increased, and detection sensitivity and quantitation can be further improved.

[0098] Step (III): Step (III) is a step of measuring the color intensity resulting from light energy absorption due to localized surface plasmon resonance and / or electron transition of the metal-resin composite 100. After performing the above step (II) or a washing step as needed, the color intensity resulting from light energy absorption due to localized surface plasmon resonance and / or electron transition of the metal-resin composite 100 is measured in the test strip 200.

[0099] If a control section is formed on the test strip 200, the labeled antibody 150 is captured by another capture ligand in the control section in step (II), forming a complex. Therefore, in step (III), color development due to light energy absorption by localized surface plasmon resonance and / or electron transition can be caused not only in the determination section 130 but also in the control section of the test strip 200. In this way, by measuring the color development intensity in both the determination section 130 and the control section, it is possible to confirm whether the sample provided to the test strip 200 has developed normally and reached the reaction section and the determination section 130.

[0100] <Sample and Analyte> The sample used in the analyte measurement method of this embodiment is not particularly limited as long as it contains a substance that can serve as an antigen, such as a protein, as the analyte 160. Examples include biological samples containing the target analyte 160 (i.e., whole blood, serum, plasma, urine, saliva, sputum, nasal or pharyngeal swabs, cerebrospinal fluid, amniotic fluid, nipple secretions, tears, sweat, skin exudates, tissue, cell, and fecal extracts, etc.), food extracts, etc. If necessary, the analyte 160 contained in the sample may be pretreated prior to step (I) to facilitate the specific binding reaction between the labeled antibody 150 and the capture ligand 131 and the analyte 160. Examples of pretreatment include chemical treatment using various chemicals such as acids, bases, and surfactants, and physical treatment using heating, stirring, ultrasound, etc. In particular, when the analyte 160 is a substance that is not normally exposed on the surface, such as influenza virus NP antigen, treatment with a surfactant or the like is preferable. As the surfactant used for this purpose, a non-ionic surfactant can be used in consideration of the binding reactivity between the capture ligand 131 and the analyte 160, such as a specific binding reaction, for example, an antigen-antibody reaction.

[0101] The sample may be diluted appropriately with a solvent (water, physiological saline, buffer solution, etc.) or a water-miscible organic solvent used in a typical immunological analysis method.

[0102] The analyte 160 is not particularly limited and may be any known analyte, including those with strong anionic properties, strong cationic properties, and other analytes. Examples of the analyte 160 include proteins (including polypeptides, oligopeptides, etc.) such as tumor markers, signal transduction substances, and hormones, nucleic acids (including single-stranded or double-stranded DNA, RNA, polynucleotides, oligonucleotides, PNA (peptide nucleic acids), etc.) or substances having nucleic acids, sugars (including oligosaccharides, polysaccharides, sugar chains, etc.) or substances having sugar chains, lipids, and other molecules, and is not particularly limited as long as it specifically binds to the labeled antibody 150 and the capture ligand 131. Examples of the analyte 160 include carcinoembryonic antigen (CEA), HER2 protein, prostate cancer, and the like. Examples of such an antigen include prostate-specific antigen (PSA), CA19-9, α-fetoprotein (AFP), immunosuppressive acidic protein (IAP), CA15-3, CA125, estrogen receptor, progesterone receptor, fecal occult blood, troponin I, troponin T, CK-MB, CRP, human chorionic gonadotropin (HCG), luteinizing hormone (LH), follicle-stimulating hormone (FSH), syphilis antibody, influenza virus human hemoglobin, chlamydia antigen, group A beta-hemolytic streptococcal antigen, HBs antibody, HBs antigen, rotavirus, adenovirus, albumin, and glycated albumin. Among these, antigens that can be solubilized by a nonionic surfactant are preferred, and antigens that form self-aggregates such as viral nucleoproteins are more preferred.

[0103] <Labeled Antibody> In step (I), the labeled antibody 150 is brought into contact with an analyte 160 contained in a sample to form a complex 170 containing the analyte 160 and the labeled antibody 150. The labeled antibody 150 is an antibody that specifically binds to the analyte 160, labeled with a metal-resin composite 100 having a structure in which a plurality of metal particles 20 are immobilized on a resin particle 10. Here, "labeling" means that the metal-resin composite 100 is immobilized to the antibody directly or indirectly by chemical or physical bonding, adsorption, or the like, to the extent that the metal-resin composite 100 does not detach from the labeled antibody 150 in steps (I) to (III). For example, the labeled antibody 150 may be one in which the metal-resin composite 100 is directly bound to the antibody, or one in which the antibody and the metal-resin composite 100 are bound via an arbitrary linker molecule, or one in which each is immobilized on an insoluble particle.

[0104] In the present embodiment, the "antibody" is not particularly limited and known antibodies can be used, including those with strong anionic properties, those with strong cationic properties, and other antibodies. For example, polyclonal antibodies, monoclonal antibodies, antibodies obtained by genetic recombination, and antibody fragments having the ability to bind to antigens [for example, H chains, L chains, Fab, F(ab')], etc. 2 etc.] can be used. Furthermore, the immunoglobulin may be any of IgG, IgM, IgA, IgE, and IgD. Antibody-producing animal species may include humans as well as non-human animals (e.g., mice, rats, rabbits, goats, horses, etc.). Specific examples of antibodies include anti-PSA antibodies, anti-AFP antibodies, anti-CEA antibodies, anti-adenovirus antibodies, anti-influenza virus antibodies, anti-HCV antibodies, anti-IgG antibodies, and anti-human IgE antibodies.

[0105] <Preferred Method for Producing Labeled Antibody> Next, a preferred method for producing labeled antibody 150 will be described. The production of labeled antibody 150 includes at least the following step A: step A) mixing metal-resin composite 100 with an antibody under a first pH condition to allow binding, thereby obtaining labeled antibody 150, and preferably further includes step B: step B) treating labeled antibody 150 under a second pH condition.

[0106] [Step A] In step A, the metal-resin composite 100 is mixed with an antibody under a first pH condition to obtain a labeled antibody 150. In step A, it is preferable to bring the solid metal-resin composite 100, dispersed in a liquid phase, into contact with the antibody.

[0107] The first pH condition is preferably a condition in the range of pH 2 to 10, more preferably, for example, a range of pH 5 to 9, from the viewpoint of uniformly contacting the metal-resin composite 100 with the antibody while maintaining dispersion of the metal-resin composite 100 and activity of the antibody. If the conditions for binding the metal-resin composite 100 with the antibody are less than pH 2, the antibody may be altered and inactivated due to strong acidity, and if the pH exceeds 10, the metal-resin composite 100 and the antibody will aggregate when mixed, making dispersion difficult. However, if the antibody is not inactivated by strong acidity, treatment is possible even at a pH of less than 2.

[0108] Step A is preferably carried out in a binding buffer adjusted to the first pH condition. For example, a predetermined amount of metal-resin composite 100 is mixed with the binding buffer adjusted to the above pH and thoroughly mixed. For example, a boric acid solution adjusted to a predetermined concentration can be used as the binding buffer. The pH of the binding buffer can be adjusted using, for example, hydrochloric acid, sodium hydroxide, or the like.

[0109] Next, a predetermined amount of antibody is added to the resulting mixture, and the mixture is thoroughly stirred and mixed to obtain a labeled antibody-containing solution. From the labeled antibody-containing solution thus obtained, only the labeled antibody 150 can be separated as a solid portion by solid-liquid separation means such as centrifugation.

[0110] [Step B] In step B, the labeled antibody 150 obtained in step A is treated under second pH conditions to perform blocking, which suppresses nonspecific adsorption to the labeled antibody 150. In this case, the labeled antibody 150, which has been separated by solid-liquid separation means, is dispersed in a liquid phase under the second pH conditions.

[0111] The second pH condition is preferably, for example, in the range of pH 2 to 10 from the viewpoint of maintaining antibody activity and suppressing aggregation of labeled antibody 150, and more preferably in the range of pH 5 to 9 from the viewpoint of suppressing nonspecific adsorption of labeled antibody 150. If the blocking condition is below pH 2, the antibody may be denatured and inactivated due to strong acidity, and if the pH exceeds 10, labeled antibody 150 will aggregate, making dispersion difficult.

[0112] Step B is preferably performed using a blocking buffer in which the blocking agent is adjusted to a second pH condition. For example, a blocking buffer adjusted to the above pH is added to a predetermined amount of labeled antibody 150, and the labeled antibody 150 is uniformly dispersed in the blocking buffer. For example, a solution of a protein that does not bind to the analyte is preferably used as the blocking buffer. There are no particular limitations on the blocking agent that can be used in the blocking buffer, and known blocking agents can be used, including those with strong anionic properties, strong cationic properties, and other agents. Examples of proteins include bovine serum albumin, ovalbumin, casein, gelatin, and whey. More specifically, a bovine serum albumin solution adjusted to a predetermined concentration is preferably used. The pH of the blocking buffer can be adjusted using, for example, hydrochloric acid, sodium hydroxide, or the like. Dispersion means such as ultrasonication are preferably used to disperse the labeled antibody 150. In this manner, a dispersion in which the labeled antibody 150 is uniformly dispersed is obtained.

[0113] In the above steps A and B, the metal-resin composite 100 is resistant to aggregation due to pH and can be treated over a wide range of pH, from acidic to alkaline. Therefore, the metal-resin composite 100 used in the present invention has the advantage of being less subject to restrictions on the conditions for producing the labeled antibody 150.

[0114] In this manner, a dispersion of the labeled antibody 150 is obtained. From this dispersion, the labeled antibody 150 alone can be separated as a solid portion by solid-liquid separation means such as centrifugation. Furthermore, if necessary, washing treatment, preservation treatment, etc. can be carried out. The washing treatment and preservation treatment will be described below.

[0115] (Washing Treatment) In the washing treatment, a washing buffer solution is added to the labeled antibody 150 separated by the solid-liquid separation means, and the labeled antibody 150 is uniformly dispersed in the washing buffer solution. For dispersion, it is preferable to use a dispersing means such as ultrasonic treatment. The washing buffer solution is not particularly limited, but for example, a Tris buffer solution, a glycinamide buffer solution, an arginine buffer solution, or the like, adjusted to a predetermined concentration within the pH range of 8 to 9, can be used. The pH of the washing buffer solution can be adjusted using, for example, hydrochloric acid, sodium hydroxide, or the like. The washing treatment of the labeled antibody 150 can be repeated multiple times as necessary.

[0116] (Preservation Treatment) In the preservation treatment, a preservation buffer solution is added to the labeled antibody 150 separated by solid-liquid separation means, and the labeled antibody 150 is uniformly dispersed in the preservation buffer solution. Dispersion is preferably performed using a dispersing method such as ultrasonication. The preservation buffer solution may be, for example, a solution prepared by adding a predetermined concentration of an anti-aggregating agent and / or stabilizer to a washing buffer solution. Anti-aggregating agents include, for example, sugars such as sucrose, maltose, lactose, and trehalose, and polyhydric alcohols such as glycerin and polyvinyl alcohol. Stabilizers include, but are not limited to, proteins such as bovine serum albumin, ovalbumin, casein, and gelatin. In this manner, the preservation treatment of the labeled antibody 150 can be performed.

[0117] In each of the above steps, a surfactant or a preservative such as sodium azide or parahydroxybenzoic acid ester may be further used as needed.

[0118] [Analyte Measurement Kit] An analyte measurement kit according to one embodiment of the present invention is a kit for detecting or quantifying an analyte 160 contained in a sample, for example, using a test strip 200, based on the analyte measurement method of this embodiment.

[0119] The analyte measurement kit of this embodiment includes: a membrane 110; a test strip 200 including a determination portion 130 formed by immobilizing a capture ligand 131 that specifically binds to the analyte 160 on the membrane 110; and a detection reagent including a labeled antibody 150 in which an antibody that specifically binds to the analyte 160 is labeled with a metal-resin composite 100 having a structure in which a plurality of metal particles 20 are immobilized on a resin particle 10. The analyte measurement kit of this embodiment may further include other components as necessary.

[0120] When using the analyte measurement kit according to this embodiment, step (I) may be performed by contacting analyte 160 in a sample with labeled antibody 150 in a detection reagent, and then steps (II) and (III) may be performed sequentially by providing the sample to the reaction zone or sample addition zone 120 of test strip 200. Alternatively, a detection reagent may be applied upstream of determination zone 130 of test strip 200 and dried appropriately to form a reaction zone, and then a sample may be added to the formed reaction zone or to a position upstream of the reaction zone (e.g., sample addition zone 120), and steps (I) to (III) may be performed sequentially.

[0121] In addition to being used as a labeling substance or a reagent for immunoassay, the metal-resin composite 100 can also be preferably used as a solid catalyst, a pigment, a paint, a conductive material, an electrode, or a sensor element.

[0122] Next, the present invention will be described in detail with reference to examples, but the present invention is not limited to these examples. In the following examples and comparative examples, various measurements and evaluations were carried out as follows, unless otherwise specified.

[0123] <Measurement of absorbance of metal-resin composite particles> A metal-resin composite particle dispersion (dispersion medium: water) adjusted to 0.01 wt % was placed in a quartz glass cell (optical path length: 10 mm), and the absorbance at 570 nm was measured using a spectrophotometer (Shimadzu Corporation, UV3600).

[0124] <Measurement of solid content concentration and measurement of metal loading amount> 1 g of the metal-resin composite particle dispersion before concentration adjustment was placed in a porcelain crucible and dried for 3 hours at 70° C. The weights before and after drying were measured, and the solid content concentration was calculated using the following formula.

[0125] Solid content concentration (wt%) = [weight after drying (g) / weight before drying (g)] × 100

[0126] The dried sample was further heat-treated at 500°C for 3 hours, and the weights before and after the heat treatment were measured to calculate the amount of supported metal by the following formula: Metal supported amount (wt%) = [Weight after heat treatment (g) / Weight before heat treatment (g)] x 100

[0127] <Measurement of average particle size and particle size distribution of resin particles and metal-resin composite particles> Measurement was performed using a centrifugal sedimentation particle size distribution analyzer (LUMiSizer 610, manufactured by LUM GmbH) with the particles dispersed in water or a solution.

[0128] <Measurement of the average particle size of metal particles and calculation of the coefficient of variation (CV value)> A substrate was prepared by dropping a metal-resin composite particle dispersion onto a metallic mesh with a carbon support film, and the area-average diameter of 100 random metal particles was measured from the image observed using a field emission scanning electron microscope (FE-SEM; Hitachi High-Technologies Corporation, SU-9000), and this was used as the average particle size. In addition, the standard deviation of the particle sizes of the metal particles was divided by the average particle size to calculate the coefficient of variation (CV value).

[0129] <Zeta Potential Measurement> The zeta potential was measured by electrophoretic light scattering using a Malvern Zetasizer Nano-ZS as the measuring device. The sample was diluted to 0.01 wt % with pure water and adjusted to various pH values ​​between pH 3 and 10 using hydrochloric acid or an aqueous NaOH solution to prepare the measurement sample. After measuring the pH using a pH meter (HORIBA LAQUA twin), the zeta potential was measured to determine the behavior of changes in the zeta potential at multiple pH points between pH 3 and 10. The range of change in the zeta potential was calculated from the maximum value of the zeta potential in the acidic range of pH 3 to 6 and the minimum value of the zeta potential in the alkaline range of pH 8 to 10. In addition, a linear function connecting an arbitrary zeta potential point close to 0 mV, an arbitrary zeta potential point greater than 0 mV, and an arbitrary zeta potential point less than 0 mV was determined, and the pH at which the zeta potential became 0 mV, i.e., the zero point of charge, was calculated.

[0130] <Evaluation of Dispersibility> 1 mL of a sample diluted to 0.01 wt % with pure water was placed in a 2 cc tube (a polypropylene Violamo microtube manufactured by AS ONE Co., Ltd.) and allowed to stand at room temperature for 3 days. The resulting precipitate was then mixed with a vortex mixer (LSE TM After stirring (10 seconds) at 200°C, the dispersion state was visually observed and evaluated. Evaluation (◯: all precipitate dispersed, △: precipitate dispersed but some remained as precipitate, ×: precipitate hardly dispersed and remained as precipitate)

[0131] [Preparation Example 1] <Synthesis of Resin Particles> An 80 wt % aqueous solution of trioctylmethylammonium chloride (1.33 g, 2.63 mmol) and a 50 wt % aqueous solution of polyethylene glycol methyl ether methacrylate (10.00 g, 2.40 mmol) were dissolved in 300 g of pure water, and then 2-vinylpyridine (48.00 g, 457 mmol) and divinylbenzene (2.00 g, 15.4 mmol) were added. The mixture was stirred under a nitrogen stream at 30° C. for 50 minutes and then at 60° C. for 30 minutes. After stirring, 2,2-azobis(2-methylpropionamidine) dihydrochloride (0.250 g, 0.922 mmol) dissolved in 18.00 g of pure water was added dropwise, and the mixture was stirred at 60° C. for 3.5 hours to obtain resin particles A-1 having an average particle size of 345 nm. The mixture was centrifuged (9000 rpm, 40 minutes) to precipitate the resin particles, and the supernatant was removed. The resulting mixture was then dispersed in pure water again, and then filtered to remove impurities. The concentration was then adjusted to obtain a 10 wt % resin particle dispersion B-1.

[0132] [Preparation Example 2] <Synthesis of Resin Particles> 93.87 g of pure water was added to B-1 (51.01 g) obtained in Preparation Example 1 to dilute, and the mixture was stirred at 28°C for 80 minutes while blowing in nitrogen. After stirring, methacrylic acid (0.086 g, 0.999 mmol) dissolved in 0.475 g of pure water was added dropwise, and the mixture was stirred at 40°C for 30 minutes. After stirring, the mixture was heated to 70°C, and 2,2-azobis(2-methylpropionamidine) dihydrochloride (0.011 g, 0.041 mmol) dissolved in 0.664 g of pure water was added dropwise, and the mixture was stirred at 70°C for 150 minutes to obtain resin particles A-2 having an average particle size of 346 nm. The resulting mixture was precipitated by centrifugation (8,460 rpm, 30 minutes), the supernatant was removed, and the mixture was re-dispersed in pure water. The concentration was then adjusted to obtain a 10 wt % resin particle dispersion B-2. Resin particles A-2 had a molar ratio of cationic functional groups (pyridinyl groups) contained in poly(2-vinylpyridine), a polymer having cationic functional groups, to anionic functional groups (carboxyl groups) contained in polymethacrylic acid, a polymer having anionic functional groups, of 97.7:2.3.

[0133] [Preparation Example 3] <Synthesis of Resin Particles> B-1 (51.01 g) obtained in Preparation Example 1 was diluted with 98.54 g of pure water and then stirred at 28°C for 80 minutes while blowing in nitrogen. After stirring, methacrylic acid (0.257 g, 2.99 mmol) dissolved in 0.476 g of pure water was added dropwise, and the mixture was stirred at 40°C for 30 minutes. After stirring, the mixture was heated to 70°C, and 2,2-azobis(2-methylpropionamidine) dihydrochloride (0.011 g, 0.041 mmol) dissolved in 0.665 g of pure water was added dropwise, and the mixture was stirred at 70°C for 150 minutes to obtain resin particles A-3 having an average particle size of 347 nm. The mixture was precipitated by centrifugation (8,460 rpm, 30 minutes), the supernatant was removed, and the mixture was re-dispersed in pure water. The concentration was then adjusted to obtain a 10 wt% resin particle dispersion B-3. In resin particles A-3, the molar ratio of the cationic functional group (pyridinyl group) contained in poly(2-vinylpyridine), which is a polymer having a cationic functional group, to the anionic functional group (carboxyl group) contained in polymethacrylic acid, which is a polymer having an anionic functional group, was 93.4:6.6.

[0134] Preparation Example 4 Preparation of Buffer 15.14 g (125 mmol) of 2-amino-2-(hydroxymethyl)-1,3-propanediol was dissolved in 500 g of pure water, and then 26.66 g (125 mmol) of 2-morpholinoethanesulfonic acid monohydrate was added and dissolved with stirring. The mixture was then filtered to obtain Buffer 1.

[0135] Preparation Example 5 Synthesis of Resin Particles An 80 wt % aqueous solution of trioctylmethylammonium chloride (1.50 g, 2.96 mmol) and a 50 wt % aqueous solution of polyethylene glycol methyl ether methacrylate (10.00 g, 4.50 mmol) were dissolved in 300 g of pure water, and then 2-vinylpyridine (48.00 g, 457 mmol) and divinylbenzene (2.00 g, 15.4 mmol) were added. The mixture was stirred under a nitrogen stream at 30° C. for 50 minutes and then at 60° C. for 30 minutes. After stirring, 2,2-azobis(2-methylpropionamidine) dihydrochloride (0.250 g, 0.922 mmol) dissolved in 18.00 g of pure water was added dropwise, and the mixture was stirred at 60° C. for 3.5 hours. Then, 20 g (250 mmol) of a 50 wt % aqueous sodium hydroxide solution was added, and the mixture was stirred at 60°C for 2 hours to obtain resin particles A-4 with an average particle size of 312 nm. After precipitation by centrifugation (9000 rpm, 40 minutes) and removal of the supernatant, the particles were re-dispersed in pure water and then dialyzed to remove impurities. The concentration was then adjusted to obtain a 10 wt % resin particle dispersion B-4.

[0136] [Preparation Example 6] <Synthesis of Resin Particles> Resin particles A-5 having an average particle size of 439 nm and a 10 wt % resin particle dispersion B-5 were obtained in the same manner as in Preparation Example 1, except that 0.39 g (0.77 mmol) of an 80 wt % aqueous solution of trioctylmethylammonium chloride and 0.50 g (1.84 mmol) of 2,2-azobis(2-methylpropionamidine) dihydrochloride were used.

[0137] Example 1 Synthesis of Gold-Resin Composite Particles 75 g of pure water was added to B-2 (30.00 g) obtained in Preparation Example 2, followed by addition of a 7 wt % aqueous solution of chloroauric acid (42.91 g) and stirring at 30°C for 3 hours. This mixture was centrifuged (3000 rpm, 15 minutes) and the supernatant was removed to remove excess chloroauric acid. The concentration was then adjusted to obtain a 5 wt % dispersion of gold ion-adsorbing resin particles, C-1.

[0138] Next, 473.00 g of buffer 1 was added to 4257.48 g of pure water, and 1 M hydrochloric acid was added while stirring until the pH reached 6.0. Subsequently, 100.00 g of a 1 wt % Triton X-100 aqueous solution was added, and while stirring at 3 °C, a reducing agent solution was prepared by adding 528 mM dimethylamine borane aqueous solution (48 mL). Subsequently, a diluted dispersion of C-1 (65.00 g) and 65.00 g of pure water was added dropwise to this reducing agent solution over 13 minutes while stirring at 3 °C. After stirring for 80 minutes at 3 °C and then for 3 hours at room temperature, gold-resin composite particles D-1 with an average particle size of 348 nm were obtained. D-1 was concentrated by centrifugation, purified by dialysis, and the concentration was adjusted to obtain a 1 wt % gold-resin composite particle dispersion E-1. The absorbance of gold-resin composite particles F-1 in E-1 was 1.43. The gold particles in F-1 had an average particle size of 7.3 nm, a CV value of 0.36, and a gold loading of 49.4 wt%. The results of zeta potential measurement of F-1 are shown in Table 1. In these gold-resin composite particles F-1, the gold particles included at least encapsulated gold particles that were completely encapsulated in the resin particles, and partially exposed gold particles that had portions embedded in the resin particles and portions exposed outside the resin particles, and at least some of the gold particles were distributed three-dimensionally within the resin particles. Furthermore, 97% of the gold particles were present within a range of 40% of the particle radius in the depth direction from the surface of the resin particles.

[0139] Example 2 Synthesis of Gold-Resin Composite Particles 26 g of pure water was added to B-3 (30.00 g) obtained in Preparation Example 3, followed by addition of a 7 wt % aqueous solution of chloroauric acid (14.30 g) and stirring at 30°C for 3 hours. This mixture was centrifuged (3000 rpm, 15 minutes) and the supernatant was removed to remove excess chloroauric acid. The concentration was then adjusted to obtain a 5 wt % dispersion of gold ion-adsorbing resin particles, C-2.

[0140] Next, 4.73 g of buffer 1 was added to 42.57 g of pure water, and 1 M hydrochloric acid was added while stirring until the pH reached 6.0. Subsequently, 1.00 g of a 1 wt % Triton X-100 aqueous solution was added, and while stirring at 3 °C, a 528 mM dimethylamine borane aqueous solution (0.48 mL) was added to prepare a reducing agent solution. Subsequently, a diluted dispersion of C-2 (0.65 g) with 0.65 g of pure water was added dropwise to this reducing agent solution over 5 minutes while stirring at 3 °C, and then stirred for 60 minutes at 3 °C and 60 minutes at room temperature to obtain gold-resin composite particles D-2 with an average particle size of 348 nm. D-2 was concentrated by centrifugation, purified by dialysis, and the concentration was adjusted to obtain a 1 wt % gold-resin composite particle dispersion E-2. The absorbance of gold-resin composite particles F-2 in E-2 was 1.39. The gold particles in F-2 had an average particle size of 8.7 nm, a CV value of 0.41, and a gold loading of 54.4 wt%. The results of zeta potential measurement of F-2 are shown in Table 1. In these gold-resin composite particles F-2, the gold particles included at least encapsulated gold particles that were completely encapsulated in the resin particles, and partially exposed gold particles that had portions embedded in the resin particles and portions exposed outside the resin particles, and at least some of the gold particles were distributed three-dimensionally within the resin particles. Furthermore, 97% of the gold particles were present within a range of 40% of the particle radius in the depth direction from the surface of the resin particles.

[0141] Comparative Example 1 Synthesis of Gold-Resin Composite Particles 255 g of pure water was added to 91.5 g of B-4 obtained in Preparation Example 5, followed by 147 g of a 400 mM aqueous solution of chloroauric acid. The mixture was then centrifuged (3000 rpm, 30 minutes) and the supernatant was removed to remove excess chloroauric acid. The concentration was then adjusted to obtain a 2.5 wt % dispersion of gold ion-adsorbing resin particles, C-3.

[0142] Next, C-3 (43.3 g) was added to 1,580 g of pure water, and while stirring at 3°C, 528 mM dimethylamine borane aqueous solution (10.0 g) was added dropwise over 2 minutes. The mixture was then stirred at 3°C ​​for 1 hour and at room temperature for 3 hours, yielding gold-resin composite particles D-3 with an average particle size of 322 nm. D-3 was concentrated by centrifugation and then purified by dialysis, and the concentration was adjusted to obtain a 1 wt% gold-resin composite particle dispersion E-3. The absorbance of gold-resin composite particles F-3 in E-3 was 1.27. The average particle size of the gold particles in F-3 was 30 nm, the CV value was 0.49, and the gold loading was 53.8 wt%. The results of zeta potential measurement of F-3 are shown in Table 1. In this gold-resin composite particle F-3, the gold particles included at least encapsulated gold particles that were completely encapsulated in the resin particle and partially exposed gold particles that had a portion embedded in the resin particle and a portion exposed outside the resin particle, and at least some of the gold particles were distributed three-dimensionally in the surface layer of the resin particle. Furthermore, 97% of the gold particles were present within a range of 40% of the particle radius in the depth direction from the surface of the resin particle.

[0143] Comparative Example 2 Synthesis of Gold-Resin Composite Particles 255 g of pure water was added to 91.5 g of B-5 obtained in Preparation Example 6, followed by 147 g of a 400 mM aqueous solution of chloroauric acid. The mixture was then centrifuged (3000 rpm, 30 minutes) and the supernatant was removed to remove excess chloroauric acid. The concentration was then adjusted to obtain a 2.5 wt % dispersion of gold ion-adsorbing resin particles, C-4.

[0144] Next, C-4 (43.3 g) was added to 1,580 g of pure water, and while stirring at 3°C, 528 mM dimethylamine borane aqueous solution (10.0 g) was added dropwise over 2 minutes. The mixture was then stirred at 3°C ​​for 1 hour and at room temperature for 3 hours, yielding gold-resin composite particles D-4 with an average particle size of 322 nm. D-4 was concentrated by centrifugation and then purified by dialysis, and the concentration was adjusted to obtain a 1 wt% gold-resin composite particle dispersion E-4. The absorbance of gold-resin composite particles F-4 in E-4 was 1.27. Furthermore, the average particle size of the gold particles in F-4 was 30 nm, the CV value was 0.31, and the gold loading was 53.8 wt%. In this gold-resin composite particle F-4, the gold particles included at least encapsulated gold particles that were completely encapsulated in the resin particle and partially exposed gold particles that had a portion embedded in the resin particle and a portion exposed outside the resin particle, and at least some of the gold particles were distributed three-dimensionally in the surface layer of the resin particle. Furthermore, 97% of the gold particles were present within a range of 40% of the particle radius in the depth direction from the surface of the resin particle.

[0145] <Mercaptopropionic Acid Treatment> E-4 (0.1 g) and a 10 mM aqueous solution of mercaptopropionic acid (1.0 g) were mixed and stirred for 1 hour at 23° C. The mixture was precipitated by centrifugation (12,000 rpm, 5 minutes), the supernatant was removed, and then the mixture was redispersed in pure water (1.0 g) to remove excess mercaptopropionic acid, thereby producing mercaptopropionic acid-treated gold-resin composite particles F-4A.

[0146] The average particle size of F-4A was 455 nm, and the absorbance was 1.36. The average particle size of gold particles in F-4A was 20 nm, and the amount of gold supported was 48.3 wt %. The results of the zeta potential measurement of F-4A are shown in Table 1.

[0147] The mercaptopropionic acid-treated gold-resin composite particles F-4A were dispersed in pure water to prepare a mercaptopropionic acid-treated gold-resin composite particle dispersion E-4A.

[0148] Comparative Example 3 Polyglutamic Acid Treatment E-4 (0.1 g) obtained in Comparative Example 2 was mixed with a 0.5 wt % aqueous solution of polyglutamic acid (1.0 g) and stirred at 23°C for 1 hour. The mixture was precipitated by centrifugation (12,000 rpm, 5 minutes), the supernatant was removed, and then pure water (1.0 g) was added to remove excess polyglutamic acid, producing polyglutamic acid-treated gold-resin composite particles F-4B. ​​The zeta potential measurement results for F-4B are shown in Table 1.

[0149] The polyglutamic acid-treated gold-resin composite particles F-4B were dispersed in pure water to prepare a polyglutamic acid-treated gold-resin composite particle dispersion E-4B.

[0150]

[0151] As shown in Table 1, Examples 1 and 2 and Comparative Examples 2 and 3 had larger absolute values ​​of the maximum and minimum zeta potentials and larger variations in the range of change compared to Comparative Example 1, which was treated with alkali. Furthermore, while Examples 1 and 2 exhibited good dispersibility in pure water, Comparative Examples 2 and 3, which were treated with mercaptopropionic acid and polyglutamic acid, exhibited poor dispersibility due to precipitation. The reason for this is believed to be that with mercaptopropionic acid and polyglutamic acid treatments, molecules containing carboxyl groups were merely adsorbed onto the surface of the gold-resin composite, making them prone to detachment, thereby reducing dispersibility in pure water. In contrast, in Examples 1 and 2, the resin particles contained polymethacrylic acid polymerized on the surface or inside of poly(2-vinylpyridine), a polymer with cationic functional groups, making it difficult for the carboxyl groups, which are anionic functional groups, to detach from the resin particles. This not only improved dispersibility in pure water, but also contributed to suppressing clogging in immunochromatography, as shown in the test results below.

[0152] Preparation Example 6 Preparation of Binding Buffer A 0.1 mol / L free acid solution of 2-[4-(2-hydroxyethyl)-1-piperazinyl]ethanesulfonic acid (HEPES) was prepared, and purified water and a 0.1 mol / L sodium hydroxide solution were mixed to adjust the buffer concentration and pH to 7.0, thereby preparing a HEPES buffer solution.

[0153] Example 3 (Binding Step) 25 μg of anti-CRP antibody was mixed with 0.45 mL of 20 mM HEPES buffer (pH 7), and then 0.05 mL of 1 wt % gold-resin composite particle dispersion E-1 prepared in Example 1 was added. The mixture was stirred by end-over-end at room temperature for 2 hours to obtain labeled antibody dispersion G-1 containing anti-CRP antibody labeled with gold-resin composite particles F-1.

[0154] (Blocking step) Next, the labeled antibody dispersion G-1 was centrifuged at 3000 rpm for 5 minutes, and the supernatant was removed. 0.5 mL of a 5 mM Tris aqueous solution (pH 5) containing 1 wt % BSA was added to the sediment, followed by ultrasonic dispersion and further end-over-end stirring at room temperature for 2 hours to obtain a labeled antibody dispersion H-1.

[0155] (Washing Treatment) Next, the labeled antibody dispersion H-1 was centrifuged at 3000 rpm for 5 minutes, the supernatant was removed, and 0.5 mL of a 5 mM Tris aqueous solution (pH 8.5) containing less than 0.1 wt % of a surfactant was added to the sediment, followed by ultrasonic dispersion. This procedure was repeated three times as a washing treatment.

[0156] (Preservation Treatment) Next, after cooling on ice, the mixture was centrifuged at 3000 rpm for 5 minutes, and the supernatant was removed. 0.5 mL of a 5 mM Tris aqueous solution (pH 8.5) containing less than 0.1 wt % of a surfactant and 10 wt % of sucrose was added to the sediment, followed by ultrasonic dispersion to obtain labeled antibody dispersion I-1.

[0157] (Preparation of Conjugate Pad) 0.12 ml of labeled antibody dispersion I-1 was centrifuged at 3,000 rpm for 5 minutes, and the supernatant was removed. 0.333 ml of an aqueous solution (pH 8.0) containing 5 wt % sucrose and 2.5 wt % BSA was added to the sediment, followed by ultrasonic dispersion to obtain labeled antibody dispersion J-1. A glass fiber nonwoven fabric was uniformly impregnated with labeled antibody dispersion J-1 and then dried at 50°C for 1 hour to prepare conjugate pad K-1. The volume of labeled antibody dispersion J-1 was adjusted so that the content of gold-resin composite particles F-1 in conjugate pad K-1 was 3 μg per test evaluated by the immunochromatography method described below.

[0158] (Preparation of Immunochromatographic Strip) An immunochromatographic strip having the structure shown in Figure 4 was prepared. First, an anti-CRP antibody was applied to a 25 mm wide nitrocellulose membrane 4 to draw a test line 5. Furthermore, an anti-mouse IgG antibody was applied downstream of the test line 5 to draw a control line 6. After drying this nitrocellulose membrane 4 at 50°C for 1 hour, a backing sheet 1, a conjugate pad K-1 as a conjugate pad 3, a sample pad 2 (glass fiber nonwoven fabric), and an absorbent pad 7 (cotton nonwoven fabric) were laminated on top of each other as shown in the cross-sectional view of the immunochromatographic strip in Figure 4. Finally, the membrane was cut to a width of 3.5 mm to prepare an immunochromatographic strip L-1.

[0159] (Preparation of Developing Solution) An aqueous solution (pH 7.1) containing 50 mM Tris, 150 mM NaCl, 1.0 wt % BSA, and 1.0 wt % PEG cetyl ether was prepared and designated as developing solution M-1.

[0160] (Evaluation by immunochromatography) Positive control (antigen concentrations 312 ng / ml, 3.12 ng / ml) and negative control (antigen-free) sample solutions were prepared by diluting the CRP antigen with developing solution M-1. 50 μl of the sample solution was dropped onto sample pad 2 of Immunochromato Strip L-1. The color intensity of test line 5 after 30 minutes was then measured using an Immunochromato Reader (Hamamatsu Photonics C10066-10). Furthermore, the presence of clogging with gold-resin composite particles F-1 (or labeled antibody) at the interface between conjugate pad 3 and nitrocellulose membrane 4 and downstream thereof was visually determined. The results of the immunochromatographic evaluation are shown in Table 2.

[0161] (Calculation of the amount of bound antibody) The amount of antibody bound to gold-resin composite particles F-1 was calculated using the supernatant removed by centrifugation in the blocking step. The amount of bound antibody was calculated by measuring the supernatant using a spectrophotometer, determining the amount of antibody contained in the supernatant from the absorbance at a wavelength of 280 nm, and subtracting the amount of antibody in the supernatant from the amount of antibody used in the binding step (25 μg). The calculated amount of bound antibody and the antibody binding yield are shown in Table 2. The binding yield refers to the weight ratio (%) of the attached antibody to the total amount of antibody used.

[0162] [Example 4, Comparative Examples 4 to 6] The binding step, blocking step, washing treatment, preservation treatment, conjugate pad preparation, immunochromatographic strip preparation, immunochromatographic evaluation, and calculation of the amount of bound antibody and antibody binding yield were carried out in the same manner as in Example 3, except for using the gold-resin composite particle dispersion and binding buffer shown in Table 2. Table 2 shows the calculation results of the amount of bound antibody and antibody binding yield, as well as the immunochromatographic evaluation results.

[0163] From Table 2, it can be seen from the test results of Examples 3 and 4 and Comparative Examples 4 to 6 that the gold-resin composite particles of the present invention suppress clogging in the immunochromatographic evaluation results, provide good immunochromatographic results without any problems, and also increase the color intensity of the test line, improving the sensitivity of immunochromatography.

[0164]

[0165] Although the embodiments of the present invention have been described in detail above for the purpose of illustration, the present invention is not limited to the above-described embodiments.

[0166] This application claims priority based on Japanese Patent Application No. 2023-051708, filed on March 28, 2023, the entire contents of which are incorporated herein by reference.

[0167] 1...backing sheet, 2...sample pad, 3...conjugate pad, 4...nitrocellulose membrane, 5...test line, 6...control line, 7...absorbent pad, 10...resin particle, 20...metal particle, 30...encapsulated particle, 40...partially exposed particle, 50...surface-adsorbed particle, 60...surface layer, 100...metal-resin composite, 110...membrane, 120...sample addition section, 130...determination section, 131...capture ligand, 140...liquid absorption section, 150...labeled antibody, 160...analyte, 170...complex, 200...test strip

Claims

1. A metal-resin composite having resin particles and a plurality of metal particles fixed to the resin particles, characterized in that the maximum value of the zeta potential is 5 mV or more in the pH range of 3 to 6, the minimum value of the zeta potential is -20 mV or less in the pH range of 8 to 10, the zero charge point of the zeta potential is in the pH range of 6.1 to 9.0, the metal particles are particles of gold or an alloy thereof, and the CV value (Coefficient of Variation) of the particle diameter is 0.45 or less.

2. The metal-resin composite according to claim 1, wherein the resin particles contain a first polymer and a second polymer of a different type from the first polymer, and one of the first polymer and the second polymer is a polymer having a cationic functional group, and the other is a polymer having an anionic functional group.

3. The metal-resin composite according to claim 2, wherein the first polymer is a polymer having a cationic functional group, the second polymer is a polymer having an anionic functional group, and the molar ratio of the cationic functional group contained in the first polymer to the anionic functional group contained in the second polymer, expressed as the cationic functional group contained in the first polymer:the anionic functional group contained in the second polymer, is within the range of 99.5:0.5 to 80:

20.

4. The metal-resin composite according to claim 3, wherein the first polymer is a polymer having in its structure a substituent capable of adsorbing metal ions.

5. The metal-resin composite according to claim 1, wherein the average particle size of the metal particles is within the range of 1 nm to 100 nm.

6. The metal-resin composite according to claim 1, wherein the metal particles are formed by reducing metal ions adsorbed on the resin particles with a reducing agent solution prepared by mixing a reducing agent and a buffer solution adjusted to a pH of 3 to 8.

7. The metal-resin composite according to claim 1, wherein the average particle size of said metal-resin composite is within the range of 30 nm to 1000 nm.

8. An indicator substance comprising the metal-resin complex according to claim 1.

9. The labeling substance according to claim 8, which is used by adsorbing an antigen or an antibody onto the surface of the metal-resin complex.

10. An immunological assay method using the labeling substance according to claim 8.

11. A reagent for immunoassay comprising the labeling substance according to claim 8.

12. A method for measuring an analyte contained in a sample, which detects or quantifies the analyte, using a lateral flow type chromatography test strip including a membrane and a determination section in which a capture ligand that specifically binds to the analyte is immobilized on the membrane, comprising the following steps (I) to (III); step (I): contacting the analyte contained in the sample with a labeled antibody obtained by labeling an antibody that specifically binds to the analyte with a metal-resin complex; step (II): contacting the complex containing the analyte and the labeled antibody formed in step (I) with the capture ligand in the determination section; and step (III): measuring the color intensity resulting from light energy absorption due to localized surface plasmon resonance and / or electron transition of the metal-resin complex, The metal-resin composite has resin particles and a plurality of metal particles immobilized on the resin particles, and has a maximum zeta potential of 5 mV or more in the pH range of 3 to 6, a minimum zeta potential of -20 mV or less in the pH range of 8 to 10, and a zero charge point of the zeta potential in the pH range of 6.1 to 9.0, the metal particles are particles of gold or an alloy thereof, and the CV value (Coefficient of Variation) of the particle diameter is 0.45 or less.

13. An analyte measurement kit for detecting or quantifying an analyte contained in a sample, comprising: a lateral flow chromatography test strip including a membrane and a determination portion having a capture ligand that specifically binds to the analyte immobilized on the membrane; and a detection reagent including a labeled antibody obtained by labeling an antibody that specifically binds to the analyte with a metal-resin complex, wherein the metal-resin complex has a structure in which a plurality of metal particles are immobilized to a resin particle, and has a maximum zeta potential of 5 mV or more in the range of pH 3 to pH 6, a minimum zeta potential of -20 mV or less in the range of pH 8 to pH 10, and a zero charge point of the zeta potential in the range of pH 6.1 to pH 9.0, and the metal particles are particles of gold or an alloy thereof, and the coefficient of variation (CV) of the particle size is 0.45 or less.

14. A lateral flow chromatography test strip for detecting or quantifying an analyte contained in a sample, comprising: a membrane; a determination section in which a capture ligand that specifically binds to the analyte is immobilized on the membrane in the direction in which the sample develops; and a reaction section upstream of the determination section, containing a labeled antibody obtained by labeling an antibody that specifically binds to the analyte with a metal-resin complex; wherein the metal-resin complex has a structure in which a plurality of metal particles are immobilized to resin particles, and has a maximum zeta potential of 5 mV or more in the pH range of 3 to 6 and a minimum zeta potential of -20 mV or less in the pH range of 8 to 10, and a zero charge point of the zeta potential in the pH range of 6.1 to 9.0; and the metal particles are particles of gold or an alloy thereof, and the CV value (Coefficient of Variation) of the particle size is 0.45 or less.

Citation Information

Patent Citations

  • Method for recovering lithium from waste lithium-ion batteries

    JP2023051708A

  • Colored latex

    JP2009168495A

  • Immunoassay of high sensitivity

    JP2009192270A

  • Magnetic marker particles and method for manufacturing the same

    JP2012013687A

  • Composite body of metallic nanoparticles for immunological measurement and cellulose, labeled substance, method for immunological measurement, reagent for immunological measurement, method for measuring analyte, kit for measuring analyte, and lateral-flow type test strip for chromatograph

    JP2019120497A