Ethylene resin composition and molded body

The ethylene resin composition, combining ultra-high molecular weight and low to high molecular weight ethylene polymers with carbon fillers, addresses the challenges of processing and conductivity, achieving effective electrical conductivity and wear resistance for diverse applications.

WO2024203987A1PCT designated stage expired Publication Date: 2024-10-03MITSUI CHEMICALS INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011552
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Ultra-high molecular weight ethylene polymers exhibit excellent impact resistance, abrasion resistance, and chemical resistance but are difficult to process via melt molding due to their high molecular weight, and existing compositions that improve conductivity often compromise wear resistance.

Method used

A composition comprising 100 parts by mass of ethylene polymer and 1 to 30 parts by mass of carbon filler, specifically ultra-high molecular weight ethylene polymer and low to high molecular weight ethylene polymer, with a carbon filler such as carbon nanotubes, achieving both electrical conductivity and injection moldability while maintaining wear resistance.

Benefits of technology

The composition enables excellent electrical conductivity, injection moldability, and wear resistance, balancing mechanical properties and processability, making it suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

One embodiment of the present invention pertains to an ethylene resin composition or a molded body of said composition. The ethylene resin composition comprises 100 parts by mass of an ethylene polymer composition (A) and 1-30 parts by mass of a carbon-based filler (B), in which the ratio of the shear viscosity η1330 measured at a temperature of 250°C and a shear rate of 1330 s-1 to the shear viscosity η13.3 measured at a temperature of 250°C and a shear rate of 13.3 s-1 (η1330 / η13.3) is less than 0.027.
Need to check novelty before this filing date? Find Prior Art

Description

Ethylene-based resin composition and molded article

[0001] One embodiment of the present invention relates to an ethylene-based resin composition or a molded article using the composition.

[0002] Ethylene polymers having an extremely high molecular weight, so-called ultra-high molecular weight ethylene polymers, are superior to general-purpose ethylene polymers in impact resistance, abrasion resistance, chemical resistance, and strength, and have excellent characteristics as engineering plastics.

[0003] It is known that such ultra-high molecular weight ethylene polymers can be obtained using known catalysts such as so-called Ziegler catalysts comprising a halogen-containing transition metal compound and an organometallic compound, or magnesium compound-supported catalysts.

[0004] Due to their high molecular weights, ultra-high molecular weight ethylene polymers are difficult to process by melt molding, which is a common molding method for resins. Ram extrusion is already a commonly used method for producing molded bodies of ultra-high molecular weight ethylene polymers (Patent Document 1).

[0005] Furthermore, dispersing cellulose fibers in an ethylene polymer has been proposed as a method for improving the sliding properties and mechanical properties of an ethylene polymer (Patent Document 2). Meanwhile, depending on the application, an ultra-high molecular weight ethylene polymer composition with improved electrical conductivity may be required. As a composition containing an ultra-high molecular weight ethylene polymer and having improved electrical conductivity, a composition containing an ethylene polymer and a carbon-based filler and having a melt flow rate (MFR, measured at 230°C and under a 10 kg load) in the range of 0.1 to 20 g / 10 min has been proposed (Patent Document 3).

[0006] Japanese Patent Application Laid-Open No. 55-28896 Japanese Patent Application Laid-Open No. 2019-35005 International Publication No. 2022 / 038941

[0007] The composition of Patent Document 3 has excellent electrical conductivity and further has the excellent feature of being moldable by injection molding despite containing an ultra-high molecular weight ethylene polymer. However, depending on the application, there may be cases where improvement in abrasion resistance is required.

[0008] One embodiment of the present invention provides a composition that is excellent in both electrical conductivity and injection moldability, and also in abrasion resistance.

[0009] As a result of further research, the present inventors have found that the above-mentioned problems can be solved by the following configuration examples. Configuration examples of the present invention are as shown in [1] to [8] below. In this specification, "A to B" indicating a numerical range means A or more and B or less.

[0010] [1] A method for producing a cellulose ester copolymer comprising the steps of: (A) 100 parts by mass of an ethylene-based polymer composition; and (B) 1 to 30 parts by mass of a carbon-based filler; and (C) a method for producing a cellulose ester copolymer copolymer comprising the steps of: (A) 100 parts by mass of an ethylene-based polymer composition; (B) a carbon-based filler; and (C) a method for producing a cellulose ester copolymer ... -1 Shear viscosity η measured at 1330 and temperature 250°C, shear rate 13.3 s -1 Shear viscosity η measured at 13.3 The ratio of 1330 / η 13.3 ) is less than 0.027.

[0011] [2] The ethylene-based resin composition (X) according to [1], wherein the carbon-based filler (B) is a carbon nanotube.

[0012] [3] The ethylene-based resin composition (X) according to [1] or [2], wherein the ethylene-based polymer composition (A) comprises: 20 to 60 parts by mass of an ultra-high molecular weight ethylene polymer (a1) having an intrinsic viscosity [η] of 10 to 40 dl / g as measured in decalin at 135°C; and 40 to 80 parts by mass of a low- to high-molecular weight ethylene polymer (a2) having an intrinsic viscosity [η] of 0.1 to 9 dl / g as measured in decalin at 135°C (wherein the total amount of the ultra-high molecular weight ethylene polymer (a1) and the low- to high-molecular weight ethylene polymer (a2) is 100 parts by mass).

[0013] [4] The ethylene-based resin composition (X) according to any one of [1] to [3], which has a melt flow rate (MFR) of 0.1 g / 10 min or less at 190°C under a 10 kg load.

[0014] [5] The ethylene polymer composition (A) has an intrinsic viscosity [η] of 3.0 to 15 dl / g measured in decalin at 135°C and a density of 930 to 980 kg / m 3 The ethylene-based resin composition (X) according to any one of [1] to [4],

[0015] [6] A molded article comprising the ethylene-based resin composition (X) according to any one of [1] to [5].

[0016] [7] The molded article according to [6], which is an injection molded article.

[0017] [8] The molded article according to [6] or [7], which is a coating material or a sliding material.

[0018] According to one embodiment of the present invention, there is provided a composition that is excellent in both electrical conductivity and injection moldability, and further, also in abrasion resistance.

[0019] <<Ethylene-Based Resin Composition (X)>> The ethylene-based resin composition (X) (hereinafter also referred to as “resin composition (X)”) contains 100 parts by mass of an ethylene-based polymer composition (A) and 1 to 30 parts by mass of a carbon-based filler (B).

[0020] <Ethylene-Based Polymer Composition (A)> The ethylene-based polymer composition (A) preferably contains a specific ultra-high molecular weight ethylene polymer (a1) and a specific low- to high-molecular weight ethylene polymer (a2) (hereinafter also referred to as "ethylene polymer (a2)").

[0021] [Ultra-high molecular weight ethylene polymer (a1)] The ultra-high molecular weight ethylene polymer (a1) preferably satisfies the following requirement (a1-a).

[0022] [Requirement (a1-a)] The ultra-high molecular weight ethylene polymer (a1) preferably has an intrinsic viscosity [η] of 10 to 40 dl / g, more preferably 15 to 35 dl / g, and even more preferably 20 to 35 dl / g, measured in decalin solvent at 135° C. Details of the measurement conditions and the like are as described in the Examples section below.

[0023] When the intrinsic viscosity [η] of the ultra-high molecular weight ethylene polymer (a1) measured in decalin at 135°C is 10 dl / g or more, the abrasion resistance of the ethylene polymer composition (A) tends to be good. As a result, the abrasion resistance, self-lubrication, impact strength, and chemical resistance of the resin composition (X) containing the ethylene polymer composition (A) and the molded article obtained from the resin composition (X) tend to be good. Furthermore, when the intrinsic viscosity [η] of the ultra-high molecular weight ethylene polymer (a1) measured in decalin at 135°C is 40 dl / g or less, the melt fluidity of the ethylene polymer composition (A) and the resin composition (X) containing the ultra-high molecular weight ethylene polymer (a1) tends to be high. That is, when the intrinsic viscosity [η] of the ultra-high molecular weight ethylene polymer (a1) is within the above range, the ethylene polymer composition (A) and the resin composition (X) containing the ultra-high molecular weight ethylene polymer (a1) can achieve both abrasion resistance and moldability.

[0024] The ultra-high molecular weight ethylene polymer (a1) is a homopolymer of ethylene or a copolymer of ethylene and an α-olefin such as propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 4-methyl-1-pentene, or 3-methyl-1-pentene. The ultra-high molecular weight ethylene polymer (a1) is preferably a homopolymer of ethylene or a copolymer of ethylene and the above α-olefin, and is a copolymer composed of ethylene as the main component, and more preferably an ethylene homopolymer. Here, the term "main component" refers to the component having the highest content (mol %) of the structural units contained in the polymer.

[0025] [Low- to High-Molecular-Weight Ethylene Polymer (a2)] The ethylene polymer (a2) preferably satisfies one or more of the following requirements (a2-a) and (a2-b).

[0026] [Requirement (a2-a)] The ethylene polymer (a2) preferably has an intrinsic viscosity [η] of 0.1 to 9.0 dl / g, more preferably 0.1 to 5.0 dl / g, still more preferably 0.5 to 3.0 dl / g, and particularly preferably 1.0 to 2.5 dl / g, as measured in decalin at 135° C. Details of the measurement conditions and the like are as described in the Examples section below.

[0027] When the intrinsic viscosity [η] of the ethylene polymer (a2) measured in decalin at 135°C is 0.1 dl / g or more, the abrasion resistance of the ethylene polymer composition (A) is likely to be good. As a result, the abrasion resistance of the resin composition (X) containing the ethylene polymer composition (A) and the molded article obtained from the resin composition (X) is likely to be good. Furthermore, when the intrinsic viscosity [η] of the ethylene polymer (a2) measured in decalin at 135°C is 9.0 dl / g or less, the melt fluidity of the ethylene polymer composition (A) and the resin composition (X) containing the ethylene polymer composition (A) is likely to be high. That is, when the intrinsic viscosity [η] of the ethylene polymer (a2) measured in decalin at 135°C is 0.1 to 9.0 dl / g, it is easy to obtain an ethylene polymer composition (A) and a resin composition (X) that are excellent in both abrasion resistance and moldability. Furthermore, when the intrinsic viscosity [η] of the ethylene polymer (a2) measured in decalin solvent at 135°C is within the above range, the carbon-based filler (B) used for preparing the resin composition (X) can be easily dispersed, and the carbon-based filler (B) can be contained in an amount sufficient to impart the desired electrical conductivity to the resin composition (X).

[0028] [Requirement (a2-b)] The density of the ethylene polymer (a2) is preferably 920 to 985 kg / m 3 and more preferably 940 to 985 kg / m 3 and more preferably 950 to 980 kg / m 3 and more preferably 950 to 975 kg / m 3 and more preferably 960 to 975 kg / m 3The details of the measurement conditions and the like are as described in the Examples section below. 3 When the ethylene polymer (a2) has a crystallinity of 985 kg / m or more, the crystallinity of the ethylene polymer (a2) tends to be high enough to prevent the surface slippage of the ethylene polymer (a2) from being impaired. Therefore, the resulting ethylene polymer composition (A) and the resin composition (X) containing the ethylene polymer composition (A) tend to have excellent abrasion resistance. In addition, the density of polyethylene is usually 985 kg / m 3 Because the density is 985 kg / m or less 3 The following polyethylenes are used as the ethylene polymer (a2).

[0029] The ethylene polymer (a2) is an ethylene homopolymer or a copolymer of ethylene and an α-olefin. Preferably, the ethylene polymer (a2) is an ethylene homopolymer. Examples of the α-olefin constituting the copolymer include linear or branched α-olefins having 3 to 20 carbon atoms, such as propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 3,4-dimethyl-1-pentene, 4-methyl-1-hexene, 3-ethyl-1-pentene, 3-ethyl-4-methyl-1-pentene, 3,4-dimethyl-1-hexene, 4-methyl-1-heptene, 3,4-dimethyl-1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene. Among these, propylene and 1-butene are preferably used in view of the density range of the ethylene polymer (a2).

[0030] The copolymer of ethylene and an α-olefin preferably contains 90 mol % or more of structural units derived from ethylene, and even more preferably 95 mol % or more of structural units derived from ethylene. The copolymer of ethylene and an α-olefin preferably contains 10 mol % or less of structural units derived from α-olefin, and even more preferably contains 5 mol % or less of structural units derived from α-olefin. When the ethylene polymer (a2) is a copolymer of ethylene and an α-olefin, the greater the amount of structural units derived from ethylene, the better. The ethylene polymer (a2) may also be a wax.

[0031] [Ethylene-based polymer composition (A)] The content of the ultra-high molecular weight ethylene polymer (a1) in the ethylene-based polymer composition (A) is preferably 20 to 60 parts by mass, more preferably 30 to 50 parts by mass (where the total amount of the ultra-high molecular weight ethylene polymer (a1) and the ethylene polymer (a2) is 100 parts by mass). The content of the ethylene polymer (a2) in the ethylene-based polymer composition (A) is preferably 40 to 80 parts by mass, more preferably 50 to 70 parts by mass (where the total amount of the ultra-high molecular weight ethylene polymer (a1) and the ethylene polymer (a2) is 100 parts by mass).

[0032] When the content of the ultra-high molecular weight ethylene polymer (a1) in the ethylene polymer composition (A) is 60 parts by mass or less and the content of the ethylene polymer (a2) is 40 parts by mass or more, the melt fluidity of the ethylene polymer composition (A) can be relatively high. Therefore, the moldability of the ethylene polymer composition (A) and the resin composition (X) containing the ethylene polymer composition (A) tends to be good. On the other hand, when the content of the ultra-high molecular weight ethylene polymer (a1) is 20 parts by mass or more and the content of the ethylene polymer (a2) is 80 parts by mass or less, the ethylene polymer composition (A) and the resin composition (X) containing the ethylene polymer composition (A) can sufficiently exhibit the wear resistance derived from the ultra-high molecular weight ethylene polymer (a1). As a result, the wear resistance of the ethylene polymer composition (A) and the resin composition (X) containing the ethylene polymer composition (A) tends to be good, and the wear resistance of the molded article obtained from the resin composition (X) tends to be excellent.

[0033] The ethylene polymer composition (A) preferably satisfies one or more of the requirements (Aa) and (Ab).

[0034] [Requirement (A-a)] The intrinsic viscosity [η] of the ethylene polymer composition (A) measured in decalin solvent at 135°C is preferably 3.0 to 15 dl / g, more preferably 3.0 to 10 dl / g, and even more preferably 5.0 to 10 dl / g. Details of the method for measuring the intrinsic viscosity [η] of the ethylene polymer composition (A) are as described in the Examples. When the intrinsic viscosity [η] in decalin solvent at 135°C is 3.0 dl / g or more, the abrasion resistance of the ethylene polymer composition (A) and the resin composition (X) containing the ethylene polymer composition (A) is improved. As a result, molded articles obtained from the resin composition (X) also tend to have excellent abrasion resistance. On the other hand, when the intrinsic viscosity [η] in decalin solvent at 135°C is 15 dl / g or less, the fluidity of the ethylene polymer composition (A) is not reduced, and therefore the moldability of the resin composition (X) containing the ethylene polymer composition (A) is likely to be improved. That is, when the intrinsic viscosity [η] of the ethylene polymer composition (A) in decalin solvent at 135°C satisfies the above range, the resin composition (X) has high melt fluidity that facilitates molding and processing, and also has good abrasion resistance.

[0035] [Requirement (A-b)] The density of the ethylene polymer composition (A) is preferably 930 to 980 kg / m 3 and more preferably 940 to 980 kg / m 3 The density of the ethylene polymer composition (A) is 930 kg / m 3 When the density of the ethylene polymer composition (A) is 980 kg / m or more, the crystallinity of the ethylene polymer (a2) tends to be high enough not to impair the surface slipperiness of the ethylene polymer (a2). Therefore, the resulting ethylene polymer composition (A) and the resin composition (X) containing the ethylene polymer composition (A) tend to be excellent in abrasion resistance. 3 When the density is less than or equal to 1000 kJ / g, the resulting ethylene polymer composition (A) is light in weight and has excellent processability. As a result, the resulting resin composition (X) also tends to be light in weight and has excellent processability. The density of the ethylene polymer composition (A) is measured by the method described in the Examples.

[0036] <Method for producing ethylene polymer composition (A)> The method for producing the ethylene polymer composition (A) is not particularly limited as long as it is a method that can contain the ultra-high molecular weight ethylene polymer (a1) and the ethylene polymer (a2) in a predetermined ratio. Preferred methods include the following methods (M-1) to (M-5).

[0037] Method (M-1): A method for producing an ultra-high molecular weight ethylene polymer (a1) and an ethylene polymer (a2) in advance in the presence of an olefin polymerization catalyst, and then blending these ultra-high molecular weight ethylene polymer (a1) and ethylene polymer (a2). Method (M-2): A method for producing an ultra-high molecular weight ethylene polymer (a1) in the presence of an olefin polymerization catalyst by a multistage polymerization method including at least two steps: a first step of producing an ultra-high molecular weight ethylene polymer (a1) and a second step of producing an ethylene polymer (a2). The second step is carried out in the presence of the ultra-high molecular weight ethylene polymer (a1) produced in the first step. Method (M-3): A method for producing an ultra-high molecular weight ethylene polymer (a1) in the presence of an olefin polymerization catalyst by a multistage polymerization method including at least two steps: a first step of producing an ethylene polymer (a2) and a second step of producing an ultra-high molecular weight ethylene polymer (a1). The second step is carried out in the presence of the ethylene polymer (a2) produced in the first step. Method (M-4): A plurality of ethylene polymer compositions (A) obtained by Method (M-2) or Method (M-3) are blended. Method (M-5): One or more selected from ultra-high molecular weight ethylene polymers (a1) and ethylene polymers (a2) are blended with the ethylene polymer compositions (A) obtained by Methods (M-2), (M-3), or (M-4). The ultra-high molecular weight ethylene polymers (a1) and (a2) can be produced by polymerizing a monomer containing ethylene in the presence of a known olefin polymerization catalyst, for example, as described in WO2008 / 013144 and WO2010 / 074073, under polymerization conditions such that the ethylene polymer composition (A) has desired physical properties.

[0038] Among the methods (M-1) to (M-3), the methods (M-2) and (M-3) using a multistage polymerization method are more preferred, and the method (M-2) in which an ultra-high molecular weight ethylene polymer (a1) is produced in the first step is even more preferred. The multistage polymerization method is preferred because the ultra-high molecular weight ethylene polymer (a1) and the ethylene polymer (a2) contained in the ethylene polymer composition (A) are compatible with each other and dispersibility is improved, making it easier to achieve both abrasion resistance and moldability. Furthermore, the multistage polymerization method improves the compatibility between the ultra-high molecular weight ethylene polymer (a1) and the ethylene polymer (a2), so the methods (M-4) and (M-5) are more preferred than the method (M-1). Furthermore, when the method (M-2) is compared with the method (M-3), when the ethylene polymer composition (A) is produced using the method (M-2), the addition of a chain transfer agent that induces a chain transfer reaction, the increase in polymerization temperature, and the like are carried out in the second step. This makes it easier to adjust the molecular weight of the polymer obtained in the second step (ethylene polymer (a2)) to be lower than the molecular weight of the polymer obtained in the first step (ultra-high molecular weight ethylene polymer (a1)), which is preferable in terms of excellent production efficiency.

[0039] In this case, the olefin such as ethylene used in the polymerization may be any of the various olefins described in the section on the ultra-high molecular weight ethylene polymer (a1) and the ethylene polymer (a2) without any restrictions.

[0040] The resin composition (X), the ethylene polymer composition (A), the ultra-high molecular weight ethylene polymer (a1), and the ethylene polymer (a2) (referred to as the resin composition and polymer according to one embodiment of the present invention, etc.) may use, as their raw materials (e.g., monomers such as ethylene and α-olefin), only raw materials derived from biomass, only raw materials derived from fossil fuels, or both raw materials derived from biomass and fossil fuels. The biomass-derived raw materials are raw materials made from any (renewable) natural raw materials and their residues, such as those derived from plants or animals, including fungi, yeast, algae, and bacteria. For example, 14 C isotope 1×10 -12Examples of such raw materials include raw materials containing biomass-derived raw materials in a proportion of about 100 pMC, and having a biomass carbon concentration (unit: pMC) measured in accordance with ASTM D6866. Biomass-derived raw materials (e.g., monomers such as ethylene and α-olefins) can be obtained, for example, by conventionally known methods. It is preferable from the viewpoint of reducing the environmental load (mainly greenhouse gas reduction) that the resin composition and polymer, etc. according to one embodiment of the present invention contain structural units derived from biomass-derived raw materials. As long as the production conditions, such as the polymerization catalyst, polymerization process, polymerization temperature, and kneading method, are equivalent, the resin composition and polymer, etc. according to one embodiment of the present invention can be used in the same manner as the resin composition and polymer, etc., even if they contain biomass-derived raw materials. 14 C isotope 1×10 -12 ~1 x 10 -14 The molecular structure and physical properties, etc., other than the proportion of biomass-derived raw materials, are equivalent to those of resin compositions and polymers, etc. made from fossil fuel-derived raw materials. Therefore, it is believed that there is no difference in performance between resin compositions and polymers, etc. made from fossil fuel-derived raw materials and resin compositions and polymers, etc. made from fossil fuel-derived raw materials.

[0041] <Carbon-based filler (B)> Examples of the carbon-based filler (B), which is one of the components constituting the resin composition (X), include carbon nanotubes (CNT), conductive carbon black (CB), and carbon fibers. The carbon-based filler (B) is not particularly limited as long as it is a material having conductivity, but among these, carbon nanotubes are preferred because they have an excellent effect of reducing the surface electrical resistivity of the molded body.

[0042] Carbon nanotubes are cylindrical hollow fibrous substances made of carbon, and may be either multi-walled carbon nanotubes or single-walled carbon nanotubes. The average diameter of the carbon nanotubes is preferably 1 nm or more, more preferably 5 nm or more, even more preferably 7 nm or more, and preferably 20 nm or less. The average length of the carbon nanotubes is preferably 0.5 μm or more, more preferably 0.6 μm, and preferably 50 μm or less, more preferably 30 μm or less, and even more preferably 15 μm or less. An average diameter of 1 nm or more tends to make the carbon nanotubes less likely to break during kneading, while an average length of 20 nm or less tends to increase electrical conductivity. An average length of 0.5 μm or more tends to increase electrical conductivity, while an average length of 50 μm or less tends to suppress an increase in viscosity during kneading, making kneading and molding easier.

[0043] The average diameter and length of carbon nanotubes can be determined by observing the carbon nanotubes with an electron microscope (SEM, TEM) and calculating the arithmetic mean. Carbon nanotubes can be produced by, for example, arc discharge, chemical vapor deposition (CVD), or laser ablation. Commercially available carbon nanotubes may also be used.

[0044] Carbon nanotubes tend to exhibit high conductivity in relatively small amounts compared to, for example, carbon black, but are expensive, so it is advantageous from a cost perspective if they can be used in smaller amounts. In this embodiment, excellent conductivity can be obtained by using a resin composition (X) containing a carbon-based filler (B) and an ethylene-based polymer composition (A). That is, the resin composition (X) tends to exhibit high conductivity even with a small amount of carbon nanotubes.

[0045] Examples of conductive carbon black include furnace black, ketjen black, channel black, lamp black, thermal black, and acetylene black. Specific examples include HAF-LS, HAF, HAF-HS, FEF, GPF, APF, SRF-LM, SRF-HM, and MT.

[0046] The primary particle diameter of the conductive carbon black is preferably 0.005 μm or more, more preferably 0.01 μm or more, and preferably 1 μm or less, more preferably 0.2 μm or less. The primary particle diameter is the number-average particle diameter (Heywood diameter: the diameter of a circle having the same area as the projected area of ​​a primary particle) measured using an electron microscope or the like.

[0047] As the carbon fiber, various known carbon fibers can be used, for example, polyacrylonitrile-based, rayon-based, pitch-based, polyvinyl alcohol-based, regenerated cellulose-based, pitch-based carbon fibers produced from mesophase pitch, etc. Carbon fibers have an advantage in that they have excellent specific strength, in applications where light weight and strength are important, such as for aircraft.

[0048] The carbon fiber may be a general-purpose fiber or a high-strength fiber. The carbon fiber may be a long fiber, a short fiber, a chopped fiber, or a recycled fiber. As a sizing agent for the carbon fiber, any of urethane-based emulsions, epoxy-based emulsions, nylon-based emulsions, and olefin-based emulsions may be used.

[0049] The average length of the carbon fibers, i.e., the average fiber length, is preferably 0.1 mm or more, more preferably 0.3 mm or more, even more preferably 0.5 mm or more, and is preferably 15.0 mm or less, more preferably 13.0 mm or less. When the average fiber length is 0.1 mm or more, the reinforcing effect of the carbon fibers on mechanical properties tends to be sufficiently exhibited. When the average fiber length is 15.0 mm or less, the dispersibility of the carbon fibers in the ethylene polymer composition (A) tends to be good. As a result, the appearance of a molded article obtained by molding the resin composition (X) containing the ethylene polymer composition (A) and the carbon fibers tends to be good.

[0050] The average diameter of the carbon fibers is preferably 3 μm or more, more preferably 5 μm or more, and preferably 30 μm or less, more preferably 21 μm or less, and even more preferably 19 μm or less. When the average diameter of the carbon fibers is 3 μm or more, the carbon fibers are less likely to break during molding, and the impact strength of the resulting molded article tends to be high. When the average diameter of the carbon fibers is 30 μm or less, the appearance of the molded article tends to be good, and the aspect ratio of the carbon fibers does not decrease, and a sufficient reinforcing effect tends to be obtained in the mechanical properties such as rigidity and heat resistance of the molded article obtained from the resin composition (X).

[0051] The carbonaceous filler (B) may be used alone or in combination of two or more.

[0052] <Other Components> The resin composition (X) may contain other thermoplastic resins such as polyolefin resins, or resin additives (e.g., stabilizers such as heat stabilizers and weather stabilizers, crosslinking agents, crosslinking aids, antistatic agents, slip agents, antiblocking agents, antifogging agents, lubricants, dyes, pigments, fillers, mineral oil-based softeners, petroleum resins, waxes other than the ethylene polymer (a2)), etc., as long as the object of the present invention is not impaired. When the other components are contained, the total amount of the other components in the resin composition (X) is usually 5% by mass or less, preferably 2% by mass or less, and more preferably 1% by mass or less. In other words, the proportion of the total mass of the ultra-high molecular weight ethylene polymer (a1), the ethylene polymer (a2), and the carbon-based filler (B) in the resin composition (X) to the mass of the resin composition (X) is usually 95% by mass or more, preferably 98% by mass or more, and more preferably 99% by mass or more.

[0053] <Ethylene-Based Resin Composition (X)> The resin composition (X) satisfies the requirements (X-a) and (X-b). Preferably, the resin composition (X) satisfies the requirements (X-a) and (X-b) and one or more of the requirements (X-c) to (X-f).

[0054] [Requirement (X-a)] The resin composition (X) contains 100 parts by mass of the ethylene polymer composition (A) and 1 to 30 parts by mass of a carbon-based filler (B). The amount of the carbon-based filler (B) blended per 100 parts by mass of the ethylene polymer composition (A) is preferably 5 to 25 parts by mass, more preferably 5 to 15 parts by mass.

[0055] Since the resin composition (X) contains the carbon-based filler (B) in the above range, it has high electrical conductivity, and a molded article obtained from the resin composition (X) also has high electrical conductivity. Furthermore, since the resin composition (X) contains the ethylene polymer composition (A) in the above range, it has high sliding properties, abrasion resistance, rigidity, and chemical resistance, and a molded article obtained from the resin composition (X) also has sliding properties, abrasion resistance, rigidity, and chemical resistance.

[0056] [Requirement (X-b)] The resin composition (X) is heated at a temperature of 250°C and a shear rate of 1330 s -1 Shear viscosity η measured at 1330 and resin composition (X) at a temperature of 250°C and a shear rate of 13.3 s -1 Shear viscosity η measured at 13.3 The ratio of 1330 / η 13.3 ) is less than 0.027. 1330 / η 13.3 ) is preferably 0.005 to 0.0265, more preferably 0.005 to 0.026, and even more preferably 0.010 to 0.0255. 1330 / η 13.3 ) is within the above range, the resin composition (X) is likely to have both good abrasion resistance and good injection moldability.

[0057] [Requirement (X-c)] Resin composition (X) is heated at a temperature of 250°C and a shear rate of 1330 s -1 Shear viscosity η measured at 1330 is preferably 100 to 300 Pa·s, more preferably 120 to 280 Pa·s, and even more preferably 150 to 250 Pa·s. The shear rate applied to the molten resin during injection molding is 1330 s -1 Since the shear viscosity η 1330It can be said that the shear viscosity η of the resin composition (X) is an index of the injection moldability of the resin composition (X) in a temperature range around 250° C. 1330 When the temperature is within the above range, the resin composition (X) tends to be easily injection molded in a temperature range around 250°C.

[0058] [Requirement (X-d)] Resin composition (X) is heated at a temperature of 250°C and a shear rate of 13.3 s -1 Shear viscosity η measured at 13.3 is preferably 5,000 to 20,000 Pa·s, more preferably 5,500 to 18,000 Pa·s, and even more preferably 6,000 to 17,000 Pa·s. When measuring the MFR of the resin composition (X) according to one embodiment of the present invention, the shear rate applied to the molten resin is 13.3 s -1 Therefore, the shear viscosity η 13.3 can be used as an index of the MFR of the resin composition (X). 13.3 The higher the shear viscosity η, the smaller the MFR of the resin composition (X). 13.3 When the value of the MFR falls within the above range, the resin composition (X) is likely to have a small MFR to such an extent that the resin composition (X) has excellent abrasion resistance.

[0059] [Requirement (X-e)] The resin composition (X) has an MFR, measured in accordance with JIS K 7210-1:2014 at 190°C under a load of 10 kg, of preferably 0.1 g / 10 min or less, more preferably less than 0.1 g / 10 min, even more preferably 0.001 g / 10 min or more and less than 0.1 g / 10 min, and particularly preferably in the range of 0.005 to 0.09 g / 10 min. When the MFR of the resin composition (X) is in the above range, the abrasion resistance of the resin composition (X) tends to be good.

[0060] [Requirement (X-f)] The density of the resin composition (X) is preferably 990 to 1020 kg / m 3 and more preferably 995 to 1015 kg / m 3 The density of the resin composition (X) is 990 kg / m 3When the density of the resin composition (X) is 1020 kg / m or more, a molded article having excellent abrasion resistance can be obtained. 3 When the density of the resin composition (X) is not more than 1000 kJ / g, a molded article having excellent lightness can be obtained. The density of the resin composition (X) can be measured by the method described in the Examples.

[0061] <<Production Method of Ethylene-Based Resin Composition (X)>> The resin composition (X) can be obtained by a conventionally known production method, for example, by dry-blending the ethylene-based polymer composition (A), the carbon-based filler (B), and, if necessary, the other components. After dry-blending, the mixture may be melt-kneaded in a single-screw or twin-screw extruder, extruded into a strand, and granulated into pellets to obtain pellets of the resin composition (X). The carbon-based filler (B) and the other components may be pre-mixed with a polymer component such as the ethylene-based polymer composition (A) to form a masterbatch, which may then be added to the ethylene-based polymer composition (A).

[0062] <<Molded Article>> A molded article according to one embodiment of the present invention comprises the resin composition (X). Specific examples of the method for producing a molded article (i.e., a method for molding the resin composition (X)) include conventionally known polyolefin molding methods, such as extrusion molding, injection molding, film molding, inflation molding, blow molding, extrusion blow molding, injection blow molding, press molding, vacuum molding, powder slush molding, calendar molding, and foam molding. A molded article comprising the resin composition (X) is obtained by molding the resin composition (X) preferably by injection molding. A molded article comprising a resin composition (X) containing carbon nanotubes as the carbon-based filler (B) is preferred.

[0063] The molded article may be a molded article formed from the resin composition (X), or may be a molded article having a portion, such as a surface layer, formed from the resin composition (X).

[0064] Generally, injection-molded articles tend to have lower electrical conductivity (higher volume resistivity) than press-molded articles, but molded articles obtained by injection molding resin composition (X) tend to exhibit high electrical conductivity. That is, resin composition (X) can form molded articles having excellent electrical conductivity regardless of the molding method.

[0065] For example, when an electrical conductivity test (test temperature 23°C, humidity 50%, voltage application time 10 seconds, applied current 0.1 to 1.0 mA) is performed on an injection-molded article obtained by injection molding resin composition (X) under conditions of a processing temperature of 250°C and a mold temperature of 50°C, the volume resistivity is preferably 1×10 8 Ω cm or less, more preferably 1×10 6 The smaller the volume resistivity, the better, but the lower limit is usually 1×10 1 It is Ω·cm.

[0066] Furthermore, the molded article made of the resin composition (X) also has excellent mechanical properties.

[0067] When a wear test (test temperature 23°C, mating material S45C, speed 50 cm / sec, sliding distance 3 km, load 15 kg) was conducted on a molded article obtained from resin composition (X), the specific wear rate (unit: 10 -3 mm 3 / (kgf km). The specific wear rate is preferably 200 or less, more preferably 160 or less, even more preferably 150 or less, and particularly preferably 140 or less. The smaller the specific wear rate, the better, but the lower limit is usually 20 × 10 -3 mm 3 When the specific abrasion rate in the abrasion test under the above conditions is within the above range, the abrasion resistance of the molded article obtained from the resin composition (X) is sufficient in the use environment, which is preferable.

[0068] <<Uses of Molded Articles>> Specific examples of molded articles include a wide range of uses, from household goods such as daily necessities and recreational uses to general industrial and industrial products, such as home appliance material parts, communication device parts, electrical parts, electronic parts, automobile parts, other vehicle parts, ship and aircraft materials, machine mechanism parts, building materials, civil engineering materials, agricultural materials, power tool parts, food containers, films, sheets, and fibers.

[0069] Furthermore, the molded article according to an embodiment of the present invention can be widely used for conventionally known polyethylene applications, and since it has an excellent balance of properties such as wear resistance, self-lubrication, impact strength, and thin-wall molding, it can be used for applications requiring these properties, such as metal coating materials (laminates) for steel pipes, electric wires, and automobile sliding door rails, pressure-resistant rubber hoses, automobile door gaskets, clean room door gaskets, automobile glass run channels, and various rubber coating materials (laminates) for automobile weather strips, linings for hoppers and chutes, and sliding materials such as gears, bearings, rollers, tape reels, various guide rails and elevator rail guides, and various protective liner materials.

[0070] The molded article according to an embodiment of the present invention has excellent electrical conductivity, and therefore can suppress the electrostatic charge of various machine parts and sliding members, and can be suitably used in applications where anti-electrostatic charge is required.

[0071] Hereinafter, one embodiment of the present invention will be described in more detail based on examples, but the present invention is not limited to these examples.

[0072] <Conditions for measuring physical properties of polymer and polymer composition> The conditions for measuring each physical property are as follows.

[0073] [Intrinsic viscosity [η]] The ethylene polymer composition (A) was dissolved in decalin, and the intrinsic viscosity measured at 135° C. was defined as [η]. Similarly, the intrinsic viscosity of each of the ultrahigh molecular weight ethylene polymer (a1) and the ethylene polymer (a2) measured in decalin at 135° C. was defined as [η].

[0074] [Method for measuring density] The density of the ethylene polymer composition (A) before adding the carbon-based filler was measured by a density gradient method in accordance with ASTM D 1505. The density of the ethylene polymer (a2) was also measured by the same method.

[0075] Catalyst Preparation Example 1: Preparation of a Solid Titanium Catalyst Component: 4.0 L of purified hexane and 95 g of anhydrous magnesium chloride were added to a 10 L reactor equipped with a stirrer, which had been thoroughly purged with nitrogen. 350 ml of ethanol was added dropwise at room temperature over 2 hours with stirring, followed by mixing at room temperature for approximately 1 hour. Next, 330 ml of diethylaluminum chloride was added dropwise over 2 hours. After the addition, the mixture was mixed at room temperature for approximately 1 hour. 1.3 L of titanium tetrachloride was then added dropwise over 1 hour, and the reaction was carried out at 80°C for 1 hour. After the reaction was completed, the solid portion was separated using a filter and washed twice with purified hexane to obtain a solid titanium catalyst component. The titanium content of the solid titanium catalyst component was 6.8 wt %, the magnesium content was 15 wt %, and the chlorine content was 60 wt %.

[0076] Example 1 Production Example 1 Production of Ethylene-Based Polymer Composition (A-1) (First-Stage Polymerization: Polymerization of Ultra-High Molecular Weight Ethylene-Based Polymer (a1-1)) 12 L of purified n-decane was added to a 24 L autoclave that had been thoroughly purged with nitrogen, and the temperature was then raised to 50°C. To the autoclave at 50°C, 12 mmol of triethylaluminum and the solid titanium catalyst component (0.12 mmol in terms of titanium atom) prepared in Catalyst Preparation Example 1 were added. The catalyst charging port was then closed, and the internal pressure of the autoclave was increased to 4.3 kg / cm. 2 Ethylene was introduced so that the viscosity became G, and the first-stage polymerization was carried out at 45 to 46°C. After 45 minutes of ethylene introduction, the pressure was released and the temperature was lowered to room temperature. A portion of the solid white polymer produced was separated and dried, and the intrinsic viscosity [η] was measured, which was found to be 28.0 dl / g. This value is the intrinsic viscosity [η] (135°C, in decalin) of the ultra-high molecular weight ethylene polymer (a1-1) contained in the ethylene polymer (A-1).

[0077] (Second-stage polymerization: polymerization of ethylene polymer (a2-1)) Next, hydrogen was introduced into the autoclave at 5.0 kg / cm 2 G was introduced, and ethylene was further introduced at 3.0 kg / cm 2 The total pressure was 8.0 kg / cm 2 The polymerization temperature was increased to 80°C, and the second stage polymerization (i.e., polymerization of an ethylene polymer (a2-1)) was carried out for 490 minutes. After the temperature was decreased to room temperature, the solid white polymer produced was separated and dried. The weight of the obtained ethylene polymer composition (A-1) was 3,460 g, and the intrinsic viscosity [η] (135°C, in decalin) of the ethylene polymer composition (A-1) was 7.4 dl / g and the density was 966 kg / m 3 It was.

[0078] (Measurement of Physical Properties of Ethylene-Based Polymer (a2-1)) Separately, polymerization was carried out under the second-stage conditions, and the resulting solid white polymer was separated and dried. The weight of the resulting ethylene-based polymer (a2-1') was 2,162 g, the intrinsic viscosity [η] (135°C, in decalin) was 1.1 dl / g, and the density was 970 kg / m 3 Here, the ethylene polymer (a2-1′) corresponds to the polymer produced in the second-stage polymerization of the ethylene polymer composition (A-1), and therefore the intrinsic viscosity, density and production amount of the ethylene polymer (a2-1′) are the same as those of the ethylene polymer (a2-1).

[0079] (Content of Ultra-High Molecular Weight Ethylene Polymer (a1-1)) The difference between the amount of the resulting ethylene polymer composition (A-1) and the amount of the ethylene polymer (a2-1′) produced was defined as the amount of the ultra-high molecular weight ethylene polymer (a1-1). Furthermore, from the mass ratio of the polymers, the content of the ultra-high molecular weight ethylene polymer (a1-1) in the ethylene polymer composition (A-1) was calculated to be 38 mass%.

[0080] [Preparation of Masterbatch (C1) Containing Carbon-Based Filler (B-1)] Carbon nanotubes (manufactured by Nanosil Co., Ltd., product name: Carbon Nanotube NC7000, average diameter: 9.5 nm, average length: 1.5 μm) were used as the carbon-based filler (B-1). 15% by mass of the carbon-based filler (B-1) and 85% by mass of the ethylene polymer composition (A-1) obtained in Production Example 1 were kneaded in a twin-screw extruder to prepare a masterbatch (C1). The kneading conditions were a temperature of 250°C, an extruder bore of 30 mm, and L / D = 30.

[0081] Preparation Example 1: Production of Ethylene-Based Resin Composition (X-1) 40% by mass of the ethylene-based polymer composition (A-1) obtained in Preparation Example 1 and 60% by mass of the masterbatch (C1) were mixed and kneaded in a twin-screw extruder to produce an ethylene-based resin composition (X-1). The kneading conditions were a temperature of 250°C, an extruder diameter of 30 mm, and L / D = 30. After the kneading treatment, the ethylene-based resin composition (X-1) was extruded into a strand shape and granulated into pellets. Furthermore, various physical properties of the obtained pellets were measured.

[0082] [Measurement of MFR (Melt Flow Rate)] The MFR of the ethylene-based resin composition (X-1) was measured at a measurement temperature of 190°C and a load of 10 kg in accordance with JIS K7210-1:2014. The results are shown in Table 1-1. In the following description, Table 1-1 and Table 1-2 are collectively referred to as Table 1.

[0083] [Measurement of Density of Ethylene-Based Resin Composition (X-1)] The density of the ethylene-based resin composition (X-1) was measured by the density gradient method in accordance with ASTM D 1505, as in the case of the ethylene-based resin composition (A). The results are shown in Table 1.

[0084] [Measurement of Shear Viscosity] The shear viscosity of the ethylene-based resin composition (X-1) was measured using a capillary rheometer: Capillograph 1D manufactured by Toyo Seiki Seisakusho, Ltd. The conditions were a resin temperature of 250°C, a preheating time of 6 minutes, a barrel diameter of 10 mm, and a shear rate of 13.3 sec. -1 , 1330sec -1 The shear viscosity was measured at 100°C. The results are shown in Table 1.

[0085] [Preparation of Injection-Molded Article] Pellets of the ethylene-based resin composition (X-1) were injection-molded using a fully automatic injection molding machine EC75SX-III manufactured by Shibaura Machine Co., Ltd. under conditions of a processing temperature of 250°C and a mold temperature of 50°C to obtain a square plate of 120 × 130 × 3 mm.

[0086] [Measurement of Volume Resistivity] An injection-molded article (120 × 130 × 3 mm) of the ethylene-based resin composition (X-1) was measured in accordance with JIS K7194; 1994 using a Loresta GX-MCP-T700 low resistivity meter manufactured by Nitto Seiko Analytech Co., Ltd. under conditions of an application time of 10 seconds, a temperature of 23°C, a humidity of 50%, and an applied current of 0.1 to 1.0 mA. The results obtained are shown in Table 1.

[0087] [Measurement of specific wear rate] An injection-molded article (120 x 130 x 3 mm) of the ethylene-based resin composition (X-1) was punched out to 30 x 30 x 3 mm using a Shopper sample punching machine manufactured by Ueshima Seisakusho Co., Ltd. The 30 x 30 x 3 mm punched pieces were measured in accordance with JIS K7218 using a friction and wear tester EFM-3 manufactured by A&D Co., Ltd. The conditions were as follows: mating material S45C, speed 50 cm / sec, distance 3 km, load 15 kg, and temperature 23°C. The obtained results are shown in Table 1.

[0088] Example 2 Production Example 2: Production of ethylene polymer composition (A-2) The internal pressure of the first autoclave was set to 4.6 kg / cm 2 The first and second polymerization stages and measurements were carried out under the same conditions as in Production Example 1, except that the ethylene polymer composition (A-2) was changed to ethylene polymer G, and the resulting solid white polymer was separated and dried. The weight of the resulting ethylene polymer composition (A-2) was 3,550 g, and the intrinsic viscosity [η] (135°C, in decalin) of the ethylene polymer composition (A-2) was 8.3 dl / g and the density of the resulting ethylene polymer composition (A-2) was 966 kg / m 3The intrinsic viscosity [η] of the solid white polymer produced in the first stage (i.e., the intrinsic viscosity of the ultra-high molecular weight ethylene polymer (a1-2), 135°C in decalin) was 28.0 dl / g. Separately, polymerization was carried out under the second stage conditions, and the solid white polymer produced was separated and dried. The weight of the obtained ethylene polymer (a2-2') was 2156 g, the intrinsic viscosity [η] (135°C in decalin) was 1.1 dl / g, and the density was 970 kg / m 3 The intrinsic viscosity, density, and production amount of the ethylene polymer (a2-2') were the same as those of the ethylene polymer (a2-2) contained in the ethylene polymer composition (A-2). From the mass ratio of the polymers, the content of the ultra-high molecular weight ethylene polymer (a1-2) in the ethylene polymer composition (A-2) was calculated to be 39 mass%.

[0089] [Preparation of Masterbatch (C2) Containing Carbon-Based Filler (B-1)] A masterbatch (C2) was prepared in the same manner as in the preparation of the masterbatch (C1), except that the ethylene polymer composition (A-2) was used instead of the ethylene polymer composition (A-1).

[0090] Preparation Example 2: Production of ethylene-based resin composition (X-2) Except for using 40% by mass of the ethylene-based polymer composition (A-2) and 60% by mass of the masterbatch (C2), a composition was produced in the same manner as in Example 1, and an injection-molded article was produced and various physical properties were measured. The results are shown in Table 1.

[0091] Example 3 Production Example 3: Production of ethylene polymer composition (A-3) The internal pressure of the first autoclave was set to 4.1 kg / cm 2 The first and second polymerization stages and measurements were carried out under the same conditions as in Production Example 1, except that the polymerization temperature was changed to 100°C, and the resulting solid white polymer was separated and dried. The weight of the resulting ethylene polymer composition (A-3) was 3,650 g, and the intrinsic viscosity [η] (135°C, in decalin) of the ethylene polymer composition (A-3) was 6.9 dl / g and the density was 966 kg / m 3The intrinsic viscosity [η] of the solid white polymer produced in the first stage (i.e., the intrinsic viscosity of the ultra-high molecular weight ethylene polymer (a1-3) at 135°C in decalin) was 28.0 dl / g. Separately, polymerization was carried out under the second stage conditions, and the solid white polymer produced was separated and dried. The weight of the obtained ethylene polymer (a2-3') was 2,313 g, the intrinsic viscosity [η] (at 135°C in decalin) was 1.1 dl / g, and the density was 970 kg / m 3 The intrinsic viscosity, density, and production amount of the ethylene polymer (a2-3') were the same as those of the ethylene polymer (a2-3) contained in the ethylene polymer composition (A-3). From the mass ratio of the polymers, the content of the ultra-high molecular weight ethylene polymer (a1-3) in the ethylene polymer composition (A-3) was calculated to be 37 mass%.

[0092] [Preparation of Masterbatch (C3) Containing Carbon-Based Filler (B-1)] A masterbatch (C3) was prepared in the same manner as in the preparation of the masterbatch (C1), except that the ethylene polymer composition (A-3) was used instead of the ethylene polymer composition (A-1).

[0093] Preparation Example 3: Production of ethylene-based resin composition (X-3) Except for using 40% by mass of the ethylene-based polymer composition (A-3) and 60% by mass of the masterbatch (C3), a composition was produced in the same manner as in Example 1, and an injection-molded article was produced and various physical properties were measured. The results are shown in Table 1.

[0094] Example 4 Production Example 4: Production of ethylene polymer composition (A-4) The internal pressure of the first autoclave was set to 3.6 kg / cm 2 The first and second polymerization stages and measurements were carried out under the same conditions as in Production Example 1, except that the ethylene polymer composition (A-4) was changed to ethylene polymer G, and the resulting solid white polymer was separated and dried. The weight of the resulting ethylene polymer composition (A-4) was 3,170 g, and the intrinsic viscosity [η] (135°C, in decalin) of the ethylene polymer composition (A-4) was 5.2 dl / g and the density of the resulting ethylene polymer composition (A-4) was 967 kg / m 3The intrinsic viscosity [η] of the solid white polymer produced in the first stage (i.e., the intrinsic viscosity of the ultra-high molecular weight ethylene polymer (a1-4) at 135°C in decalin) was 28.0 dl / g. Separately, polymerization was carried out under the second stage conditions, and the solid white polymer produced was separated and dried. The weight of the obtained ethylene polymer (a2-4') was 2148 g, the intrinsic viscosity [η] (at 135°C in decalin) was 1.1 dl / g, and the density was 970 kg / m 3 The intrinsic viscosity, density, and production amount of the ethylene polymer (a2-4') were the same as those of the ethylene polymer (a2-4) contained in the ethylene polymer composition (A-4). From the mass ratio of the polymers, the content of the ultra-high molecular weight ethylene polymer (a1-4) in the ethylene polymer composition (A-4) was calculated to be 32 mass%.

[0095] [Preparation of Masterbatch (C4) Containing Carbon-Based Filler (B-1)] A masterbatch (C4) was prepared in the same manner as in the preparation of the masterbatch (C1), except that the ethylene polymer composition (A-4) was used instead of the ethylene polymer composition (A-1).

[0096] Preparation Example 4: Production of ethylene-based resin composition (X-4) Except for using 40% by mass of the ethylene-based polymer composition (A-4) and 60% by mass of the masterbatch (C4), a composition was produced in the same manner as in Example 1, and an injection-molded article was produced and various physical properties were measured. The results are shown in Table 1.

[0097] Example 5 Production Example 5: Production of ethylene polymer composition (A-5) The internal pressure of the first autoclave was set to 5.0 kg / cm 2 The first and second polymerization stages and measurements were carried out under the same conditions as in Production Example 1, except that the ethylene polymer composition (A-5) was changed to ethylene polymer G, and the resulting solid white polymer was separated and dried. The weight of the resulting ethylene polymer composition (A-5) was 3,660 g, and the intrinsic viscosity [η] (135°C, in decalin) of the ethylene polymer composition (A-5) was 9.3 dl / g and the density of the resulting ethylene polymer composition (A-5) was 965 kg / m 3The intrinsic viscosity [η] of the solid white polymer produced in the first stage (i.e., the intrinsic viscosity of the ultra-high molecular weight ethylene polymer (a1-5) at 135°C in decalin) was 28.0 dl / g. Separately, polymerization was carried out under the second stage conditions, and the solid white polymer produced was separated and dried. The weight of the obtained ethylene polymer (a2-5') was 2158 g, the intrinsic viscosity [η] (at 135°C in decalin) was 1.1 dl / g, and the density was 970 kg / m 3 The intrinsic viscosity, density, and production amount of the ethylene polymer (a2-5') were the same as those of the ethylene polymer (a2-5) contained in the ethylene polymer composition (A-5). From the mass ratio of the polymers, the content of the ultra-high molecular weight ethylene polymer (a1-5) in the ethylene polymer composition (A-5) was calculated to be 41 mass%.

[0098] [Preparation of Masterbatch (C5) Containing Carbon-Based Filler (B-1)] A masterbatch (C5) was prepared in the same manner as in the preparation of the masterbatch (C1), except that the ethylene polymer composition (A-5) was used instead of the ethylene polymer composition (A-1).

[0099] Preparation Example 5: Production of ethylene-based resin composition (X-5) Except for using 40% by mass of the ethylene-based polymer composition (A-5) and 60% by mass of the masterbatch (C5), a composition was produced in the same manner as in Example 1, and an injection-molded article was produced and various physical properties were measured. The results are shown in Table 1.

[0100] Comparative Example 1 Production Example 6: Production of ethylene polymer composition (A-6) The internal pressure of the first autoclave was set to 3.2 kg / cm 2 The first and second polymerization stages and measurements were carried out under the same conditions as in Production Example 1, except that the ethylene polymer composition (A-6) was changed to ethylene polymer G, and the resulting solid white polymer was separated and dried. The weight of the resulting ethylene polymer composition (A-6) was 3,380 g, and the intrinsic viscosity [η] (135°C, in decalin) of the ethylene polymer composition (A-6) was 4.3 dl / g and the density of the resulting ethylene polymer composition (A-6) was 969 kg / m 3The intrinsic viscosity [η] of the solid white polymer produced in the first stage (i.e., the intrinsic viscosity of the ultra-high molecular weight ethylene polymer (a1-6) at 135°C in decalin) was 28.0 dl / g. Separately, polymerization was carried out under the second stage conditions, and the solid white polymer produced was separated and dried. The weight of the obtained ethylene polymer (a2-6') was 2468 g, the intrinsic viscosity [η] (at 135°C in decalin) was 1.1 dl / g, and the density was 970 kg / m 3 The intrinsic viscosity, density, and production amount of the ethylene polymer (a2-6') were the same as those of the ethylene polymer (a2-6) contained in the ethylene polymer composition (A-6). From the mass ratio of the polymers, the content of the ultra-high molecular weight ethylene polymer (a1-6) in the ethylene polymer composition (A-6) was calculated to be 27 mass%.

[0101] [Preparation of Masterbatch (C6) Containing Carbon-Based Filler (B-1)] A masterbatch (C6) was prepared in the same manner as in the preparation of the masterbatch (C1), except that the ethylene polymer composition (A-6) was used instead of the ethylene polymer composition (A-1).

[0102] Preparation Example 6: Production of ethylene-based resin composition (CX-6) Except for using 40% by mass of the ethylene-based polymer composition (A-6) and 60% by mass of the masterbatch (C6), a composition was produced in the same manner as in Example 1, and an injection-molded article was produced and various physical properties were measured. The results are shown in Table 1.

[0103] Comparative Example 2 Production Example 7 Production of Ethylene-Based Polymer Composition (A-7) The internal pressure of the first-stage autoclave was set to 2.9 kg / cm 2 The first and second polymerization stages and measurements were carried out under the same conditions as in Production Example 1, except that the ethylene polymer composition (A-7) was changed to ethylene polymer G, and the resulting solid white polymer was separated and dried. The weight of the resulting ethylene polymer composition (A-7) was 3,220 g, and the intrinsic viscosity [η] (135°C, in decalin) of the ethylene polymer composition (A-7) was 3.5 dl / g and the density of the resulting ethylene polymer composition (A-7) was 969 kg / m 3The intrinsic viscosity [η] of the solid white polymer produced in the first stage (i.e., the intrinsic viscosity of the ultra-high molecular weight ethylene polymer (a1-7) at 135°C in decalin) was 28.0 dl / g. Separately, polymerization was carried out under the second stage conditions, and the solid white polymer produced was separated and dried. The weight of the obtained ethylene polymer (a2-7') was 2394 g, the intrinsic viscosity [η] (at 135°C in decalin) was 1.1 dl / g, and the density was 970 kg / m 3 The intrinsic viscosity, density, and production amount of the ethylene polymer (a2-7') were the same as those of the ethylene polymer (a2-7) contained in the ethylene polymer composition (A-7). From the mass ratio of the polymers, the content of the ultra-high molecular weight ethylene polymer (a1-7) in the ethylene polymer composition (A-7) was calculated to be 26 mass%.

[0104] [Preparation of Masterbatch (C7) Containing Carbon-Based Filler (B-1)] A masterbatch (C7) was prepared in the same manner as in the preparation of the masterbatch (C1), except that the ethylene polymer composition (A-7) was used instead of the ethylene polymer composition (A-1).

[0105] Preparation Example 7 Production of Ethylene-Based Resin Composition (CX-7) Except for using 40% by mass of the ethylene-based polymer composition (A-7) and 60% by mass of the masterbatch (C7), a composition was produced in the same manner as in Example 1, and an injection-molded article was produced and various physical properties were measured. The results are shown in Table 1.

[0106] Comparative Example 3 Production Example 8 Production of Ethylene-Based Polymer Composition (A-8) The internal pressure of the first-stage autoclave was set to 2.5 kg / cm 2 The first and second polymerization stages and measurements were carried out under the same conditions as in Production Example 1, except that the ethylene polymer composition (A-8) was changed to ethylene polymer G, and the resulting solid white polymer was separated and dried. The weight of the resulting ethylene polymer composition (A-8) was 3,300 g, and the intrinsic viscosity [η] (135°C, in decalin) of the ethylene polymer composition (A-8) was 2.4 dl / g and the density of the resulting ethylene polymer composition (A-8) was 969 kg / m 3The intrinsic viscosity [η] of the solid white polymer produced in the first stage (i.e., the intrinsic viscosity of the ultra-high molecular weight ethylene polymer (a1-8), 135°C in decalin) was 28.0 dl / g. Separately, polymerization was carried out under the second stage conditions, and the solid white polymer produced was separated and dried. The weight of the obtained ethylene polymer (a2-8') was 2526 g, the intrinsic viscosity [η] (135°C in decalin) was 1.1 dl / g, and the density was 970 kg / m 3 The intrinsic viscosity, density, and production amount of the ethylene polymer (a2-8') were the same as those of the ethylene polymer (a2-8) contained in the ethylene polymer composition (A-8). From the mass ratio of the polymers, the content of the ultra-high molecular weight ethylene polymer (a1-8) in the ethylene polymer composition (A-8) was calculated to be 23 mass%.

[0107] [Preparation of Masterbatch (C8) Containing Carbon-Based Filler (B-1)] A masterbatch (C8) was prepared in the same manner as in the preparation of the masterbatch (C1), except that the ethylene-based polymer composition (A-8) was used instead of the ethylene-based polymer composition (A-1).

[0108] Preparation Example 8: Production of ethylene-based resin composition (CX-8) Except for using 40% by mass of the ethylene-based polymer composition (A-8) and 60% by mass of the masterbatch (C8), a composition was produced in the same manner as in Example 1, and an injection-molded article was produced and various physical properties were measured. The results are shown in Table 1.

[0109] Comparative Example 4 Production Example 9 Production of Ethylene-Based Polymer Composition (A-9) The internal pressure of the first-stage autoclave was set to 3.4 kg / cm 2 The first-stage polymerization, the second-stage polymerization, and measurements were carried out under the same conditions as in Production Example 1, except that the ethylene polymer composition (A-9) was changed to ethylene polymer G, and the resulting solid white polymer was separated and dried. The weight of the resulting ethylene polymer composition (A-9) was 3,160 g, and the intrinsic viscosity [η] (135°C, in decalin) of the ethylene polymer composition (A-9) was 4.8 dl / g and the density of the resulting ethylene polymer composition (A-9) was 968 kg / m 3The intrinsic viscosity [η] of the solid white polymer produced in the first stage (i.e., the intrinsic viscosity of the ultra-high molecular weight ethylene polymer (a1-9) at 135°C in decalin) was 28.0 dl / g. Separately, polymerization was carried out under the second stage conditions, and the solid white polymer produced was separated and dried. The weight of the obtained ethylene polymer (a2-9') was 2224 g, the intrinsic viscosity [η] (at 135°C in decalin) was 1.1 dl / g, and the density was 970 kg / m 3 The intrinsic viscosity, density, and production amount of the ethylene polymer (a2-9') were the same as those of the ethylene polymer (a2-9) contained in the ethylene polymer composition (A-9). From the mass ratio of the polymers, the content of the ultra-high molecular weight ethylene polymer (a1-9) in the ethylene polymer composition (A-9) was calculated to be 30 mass%.

[0110] [Preparation of Masterbatch (C9) Containing Carbon-Based Filler (B-1)] A masterbatch (C9) was prepared in the same manner as in the preparation of the masterbatch (C1), except that the ethylene polymer composition (A-9) was used instead of the ethylene polymer composition (A-1) and the kneading temperature was set to 270°C.

[0111] Preparation Example 9: Production of ethylene-based resin composition (CX-9) Except for using 40% by mass of the ethylene-based polymer composition (A-2) and 60% by mass of the masterbatch (C9), a composition was produced in the same manner as in Example 1, and an injection-molded article was produced and various physical properties were measured. The results are shown in Table 1.

[0112] Comparative Example 5 Production Example 10: Production of ethylene polymer composition (A-10) The internal pressure of the first-stage autoclave was set to 3.3 kg / cm 2 The first-stage polymerization, the second-stage polymerization, and measurements were carried out under the same conditions as in Production Example 1, except that the ethylene polymer composition (A-10) was changed to ethylene polymer G, and the resulting solid white polymer was separated and dried. The weight of the resulting ethylene polymer composition (A-10) was 3,400 g, and the intrinsic viscosity [η] (135°C, in decalin) of the ethylene polymer composition (A-10) was 4.7 dl / g and the density of the resulting ethylene polymer composition (A-10) was 968 kg / m 3The intrinsic viscosity [η] of the solid white polymer produced in the first stage (i.e., the intrinsic viscosity of the ultra-high molecular weight ethylene polymer (a1-10) at 135°C in decalin) was 28.0 dl / g. Separately, polymerization was carried out under the second stage conditions, and the solid white polymer produced was separated and dried. The weight of the obtained ethylene polymer (a2-10') was 2438 g, the intrinsic viscosity [η] (at 135°C in decalin) was 1.1 dl / g, and the density was 970 kg / m 3 The intrinsic viscosity, density, and production amount of the ethylene polymer (a2-10') were the same as those of the ethylene polymer (a2-10) contained in the ethylene polymer composition (A-10). From the mass ratio of the polymers, the content of the ultra-high molecular weight ethylene polymer (a1-10) in the ethylene polymer composition (A-10) was calculated to be 28 mass%.

[0113] [Preparation of Masterbatch (C10) Containing Carbon-Based Filler (B-1)] A masterbatch (C10) was prepared in the same manner as in the preparation of the masterbatch (C1), except that the ethylene polymer composition (A-10) was used instead of the ethylene polymer composition (A-1).

[0114] Preparation Example 10: Production of ethylene-based resin composition (CX-10) Except for using 40% by mass of the ethylene-based polymer composition (A-10) and 60% by mass of the masterbatch (C10), a composition was produced in the same manner as in Example 1, and an injection-molded article was produced and various physical properties were measured. The results are shown in Table 1.

[0115] Comparative Example 6 Production Example 11: Production of Ethylene-Based Polymer Composition (A-11) An ultra-high molecular weight ethylene polymer (a1-11) having an intrinsic viscosity [η] of 30 dl / g (135°C, in decalin) and an ethylene polymer (a2-11-1) having an intrinsic viscosity [η] of 1.5 dl / g (135°C, in decalin) were polymerized in a mass ratio of 41 / 59 by two-stage polymerization to obtain an ethylene polymer composition (A-11') having an intrinsic viscosity [η] of 4.4 dl / g (135°C, in decalin). Next, using a PCM twin-screw extruder manufactured by Ikegai Iron Works, Ltd., an ethylene polymer composition (A-11') having an intrinsic viscosity [η] of 1.1 dl / g (135°C, in decalin) and a density of 965 kg / m 3 (manufactured by Prime Polymer Co., Ltd., trade name Hi-Zex 1700JP) (a2-11-2) were melt-blended in a ratio of 49 / 51 to obtain pellets of an ethylene polymer composition (A-11).

[0116] [Preparation of Masterbatch (C11) Containing Carbon-Based Filler (B-1)] A masterbatch (C11) was prepared in the same manner as in the preparation of the masterbatch (C1), except that 75 mass% of the ethylene polymer composition (A-11) was used instead of the ethylene polymer composition (A-1), and 10 mass% of a wax (polyethylene wax, corresponding to the ethylene polymer (a2)) was additionally used.

[0117] Preparation Example 11: Production of ethylene-based resin composition (CX-11) Except for using 40% by mass of the ethylene-based polymer composition (A-11) and 60% by mass of the masterbatch (C11), a composition was produced in the same manner as in Example 1, and an injection-molded article was produced and various physical properties were measured. The results are shown in Table 1.

[0118]

[0119]

Claims

1. A composition comprising 100 parts by mass of an ethylene-based polymer composition (A) and 1 to 30 parts by mass of a carbon-based filler (B), at a temperature of 250°C and a shear rate of 1330 s -1 Shear viscosity η measured at 1330 Temperature: 250°C, shear rate: 13.3 s -1 Shear viscosity η measured at 13.3 Ratio to η 1330 / 13.3 The ethylene-based resin composition (X), wherein the molar ratio is less than 0.

027.

2. The ethylene-based resin composition (X) according to claim 1, wherein the carbon-based filler (B) is a carbon nanotube.

3. The ethylene-based resin composition (X) according to claim 1, wherein the ethylene-based polymer composition (A) comprises, per 100 parts by mass of a total amount of an ultra-high molecular weight ethylene polymer (a1) having an intrinsic viscosity [η] of 10 to 40 dl / g measured in decalin at 135°C and a low- to high-molecular weight ethylene polymer (a2) having an intrinsic viscosity [η] of 0.1 to 9 dl / g measured in decalin at 135°C, the content of the ultra-high molecular weight ethylene polymer (a1) is 20 to 60 parts by mass and the content of the low- to high-molecular weight ethylene polymer (a2) is 40 to 80 parts by mass.

4. The ethylene-based resin composition (X) according to claim 1, having a melt flow rate of 0.1 g / 10 min or less at 190° C. under a load of 10 kg.

5. The ethylene polymer composition (A) has an intrinsic viscosity [η] of 3.0 to 15 dl / g measured in decalin at 135° C., and a density of 930 to 980 kg / m 3 The ethylene-based resin composition (X) according to claim 1, 6. A molded article comprising the ethylene-based resin composition (X) according to any one of claims 1 to 5.

7. The molded article according to claim 6, which is an injection molded article.

8. The molded article according to claim 6, which is a coating material or a sliding material.

Citation Information

Patent Citations

  • Ram extruding machine for manufacturing plastic pipe

    JP1980028896A

  • Resin composition containing cellulose fiber, method of manufacturing the same, and molded article

    JP2019035005A

  • Ethylene polymer particle, method for producing the same, and molded article using the same

    WO2008013144A1

  • Ethylene polymer composition, manufacturing method therefor, and molded article obtained using same

    WO2010074073A1

  • Carbon fiber composite material and preparation method thereof, enhanced ultra-high molecular weight polyethylene composition containing carbon fiber composite material and preparation method of enhanced ultra-high molecular weight polyethylene composition

    CN112080101A