Integrated molding and method for manufacturing integrated molding
The integration of fiber-reinforced thermosetting resin and metal members with controlled expansion coefficients and heat welding through a thermoplastic resin region addresses the challenges of strength, weight, and productivity in joining complex shapes, achieving a stable and lightweight bonded state with high bonding strength and accuracy.
Patent Information
- Application Number
- PCT/JP2024/011577
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Existing methods for joining fiber-reinforced thermosetting resin and metal members often result in reduced strength, increased weight, and productivity issues due to bolt processing, adhesive voids, and inadequate bonding control, particularly in complex shapes.
An integrated molded product is formed by joining a fiber-reinforced thermosetting resin structural member with a metal member, where the metal member overlaps and contacts the structural member in a joint area, with a linear expansion coefficient ratio between 1.0 to 50, allowing for stable bonding and lightweight construction through heat welding via a thermoplastic resin region.
This approach achieves a lightweight, stable bonded state with high bonding strength and improved productivity by controlling pressure and expansion differences, reducing voids and stress concentration, and ensuring high dimensional accuracy.
Smart Images

Figure JP2024011577_03102024_PF_FP_ABST
Abstract
Description
Integral molded product and manufacturing method of integrally molded product
[0001] The present invention relates to an integrally molded product formed by joining a structural member essentially made of a fiber-reinforced thermosetting resin and a metal member.
[0002] Fiber-reinforced composite materials are materials with excellent mechanical properties and light weight, and are widely used in components for aircraft, automobiles, industrial equipment, etc. In such applications, frame structures with fiber-reinforced composite materials as the main skeleton are sometimes adopted.
[0003] In this case, it is necessary to form a connectable or detachable member on a part of a frame material made of a fiber-reinforced composite material. However, because such a member has a relatively complex shape, it has generally been manufactured separately by injection molding or metal processing, and then fixed to the frame material using adhesives or bolts. For example, Patent Document 1 discloses a method of mechanically joining a fiber-reinforced resin pipe by bolting the joint. Patent Document 2 discloses a structure in which a carbon fiber-reinforced resin pipe and a metal part are joined with an adhesive. Furthermore, Patent Document 3 discloses a method of joining a carbon fiber-reinforced resin member having a flat or curved surface to a metal part using a hot-melt adhesive.
[0004] Japanese Patent Laid-Open No. 11-350592 Japanese Patent Laid-Open No. 2016-221784 Japanese Patent Laid-Open No. 2013-244725
[0005] However, the method described in Patent Document 1 raises concerns about a decrease in strength due to bolt processing of the pipe, and also has issues such as increased weight due to the bolts themselves. Furthermore, the method described in Patent Document 2 can eliminate voids inside the adhesive and improve joint strength, but requires the adhesive surface to have a tapered shape or surface irregularities, resulting in reduced productivity. Furthermore, Patent Document 3 can improve joint strength and productivity by using a hot melt adhesive made of a thermoplastic resin, but this is a joining technology for structures where pressure can be sufficiently controlled, making it difficult to apply to joining structures between cylindrical bodies and fittings.
[0006] An object of the present invention is to obtain a lightweight, stably joined, integrally molded product of a cylindrical body made of thermosetting resin and a metal member.
[0007] The present invention, which solves the above-mentioned problems, is as follows.
[0008] An integrally molded product formed by joining a structural member (a) essentially made of a fiber-reinforced thermosetting resin and a metal member (b), wherein the metal member (b) has an overlap region that overlaps the structural member (a), and at least a portion of the overlap region has a joint that contacts the structural member (a), and the joint has a linear expansion coefficient α of the joint periphery of the structural member (a) in a measurement temperature range of 60°C to 150°C. ta and the linear expansion coefficient α of the joining periphery of the metal member (b) tb The ratio of (α tb / α ta ) is 1.0 to 50.
[0009] According to the present invention, it is possible to obtain a lightweight, stably joined integrally molded product of a structural member essentially made of a fiber-reinforced thermosetting resin and a metal member.
[0010] FIG. 1 is a schematic diagram showing an example of a joint as a metal member (b). FIG. 2 is a schematic diagram showing an example of an integrally molded product in which the joint shown in FIG. 1 is joined with a structural member (a). FIG. 3 is a schematic diagram showing an example of a base as a metal member (b). FIG. 4 is a schematic diagram showing an example of an integrally molded product in which the base shown in FIG. 3 is joined with a structural member (a). FIG. 5 is a schematic diagram showing an example of a second cylindrical body as a metal member (b). FIG. 6 is a schematic diagram showing an example of an integrally molded product in which the second cylindrical body shown in FIG. 5 is joined with a structural member (a). FIG. 7 is a cross-sectional view showing an example of a joint between a structural member (a) and a metal member (b).
[0011] Preferred embodiments of the present invention will be described below.
[0012] The integrally molded product according to the present invention is an integrally molded product formed by joining a structural member (a) essentially made of a fiber-reinforced thermosetting resin and a metal member (b). In the present invention, "essentially made of a certain material" means that the structural member contains the material as a major component and is typically made of only the material, but may contain other components as long as the effects of the invention are not lost. Specifically, as described below, the structural member (a) may have a thermoplastic resin region on its surface. However, as long as the majority of the structural member (a) that ensures its strength as a component is made of the fiber-reinforced thermosetting resin, the structural member (a) is described as essentially made of the fiber-reinforced thermosetting resin. Preferably, the structural member (a) has a volume of, for example, 90% or more made of the fiber-reinforced thermosetting resin.
[0013] The fibers contained in the fiber-reinforced thermosetting resin of the structural member (a) of the present invention may be those generally used as reinforcing fibers. Examples include glass fibers, polyacrylonitrile-based, rayon-based, lignin-based, and pitch-based carbon fibers (including graphite fibers), potassium titanate whiskers, zinc oxide whiskers, calcium carbonate whiskers, wollastonite whiskers, aluminum borate whiskers, aramid fibers, alumina fibers, silicon carbide fibers, ceramic fibers, asbestos fibers, gypsum fibers, and metal fibers. Among these, glass fibers, polyacrylonitrile-based, and pitch-based carbon fibers are preferred, and polyacrylonitrile-based and pitch-based carbon fibers are more preferred from the viewpoint of light weight and mechanical properties, with polyacrylonitrile-based carbon fibers being particularly preferred.
[0014] From the viewpoint of improving mechanical properties, it is preferable that the fibers contained in the structural member (a) are surface-treated with a sizing agent. Examples of sizing agents include polyfunctional epoxy resins, acrylic acid-based polymers, polyhydric alcohols, and polyethyleneimines. Specific examples include polyglycidyl ethers of aliphatic polyhydric alcohols such as glycerol triglycidyl ether, diglycerol polyglycidyl ether, polyglycerol polyglycidyl ether, sorbitol polyglycidyl ether, arabitol polyglycidyl ether, trimethylolpropane triglycidyl ether, and pentaerythritol polyglycidyl ether; polyacrylic acid; copolymers of acrylic acid and methacrylic acid; and copolymers of acrylic acid and methacrylic acid. Examples of suitable sizing agents include copolymers with leic acid, or mixtures of two or more of these, polyvinyl alcohol, glycerol, diglycerol, polyglycerol, sorbitol, arabitol, trimethylolpropane, pentaerythritol, and polyethyleneimine containing a large number of amino groups per molecule. Among these, glycerol triglycidyl ether, diglycerol polyglycidyl ether, and polyglycerol polyglycidyl ether are preferably used in the present invention because they contain a large number of highly reactive epoxy groups per molecule, are highly water-soluble, and are easy to apply to fibers. The sizing agent is preferably contained in an amount of 0.01 to 5 parts by mass, and more preferably 0.1 to 2 parts by mass, per 100 parts by mass of fibers.
[0015] The fibers contained in the structural member (a) are preferably continuous fibers. In this specification, "continuous fibers" refers to fibers having a length of 10 mm or more. As long as they have this length, they do not necessarily need to be continuous throughout the entire member, and may be interrupted along the way. Examples of the form of continuous fibers include cross-woven fabrics woven with fiber bundles, and forms in which filaments, braids, filament bundles, spun yarns, etc. are aligned in one direction. Furthermore, the structural member (a) can be formed by combining two or more of these reinforcing fiber forms.
[0016] The structural member (a) is preferably a molded body having a laminated structure formed by laminating prepreg sheets made of fiber-reinforced thermosetting resin. When the prepreg sheets have reinforcing fibers aligned in one direction, it is preferable to use a laminated structure in which the reinforcing fibers are aligned in an angle of approximately 0°, approximately ±45°, approximately 90°, etc., and layer structures with angles other than those mentioned above may also be included.
[0017] The mass content of the fibers present in 100% by mass of the structural member (a) is preferably 20 to 70% by mass, more preferably 25 to 70% by mass, and particularly preferably 30 to 65% by mass. By setting the mass content of the fibers within the above range, a structural member (a) with high rigidity and good dimensional accuracy can be obtained.
[0018] The type of thermosetting resin constituting the fiber-reinforced thermosetting resin of the structural member (a) is not particularly limited, and examples include unsaturated polyester resin, vinyl ester resin, epoxy resin, phenol (resol type) resin, urea-melamine resin, polyimide resin, etc., as well as copolymers and modified products thereof, and resins obtained by blending at least two of these. Among these, thermosetting resins primarily composed of epoxy resin are more preferred from the viewpoint of the mechanical properties of molded products, due to their excellent rigidity and strength. The term "major component" in a thermosetting resin refers to a component ratio in the thermosetting resin of 60% by mass or more.
[0019] The fiber-reinforced thermosetting resin may also contain other fillers or additives depending on the application, etc. Examples include elastomer or rubber components, inorganic fillers, flame retardants, conductivity imparting agents, antibacterial agents, insect repellents, deodorizing agents, coloring inhibitors, mold release agents, antistatic agents, plasticizers, colorants, pigments, dyes, foaming agents, antifoaming agents, and coupling agents.
[0020] In the present invention, the structural member (a) may have at least a cylindrical or columnar portion. Here, columnar means a solid shape with no hollow space in the cylindrical portion. Typically, the structural member (a) can have a columnar or cylindrical shape as a whole. Alternatively, the structural member (a) may have a form that combines a cylindrical or columnar portion with other shaped portions. Furthermore, when the structural member (a) has a cylindrical portion, the cylindrical portion may have an uneven thickness, where the wall thickness varies. The cylindrical or columnar portion of the structural member (a) may be curved.
[0021] When the structural member (a) has a cylindrical portion, it is preferable that the structural member (a) be tubular, with the length in the direction perpendicular to the opening surface being longer than the diameter of the cylindrical form, from the viewpoint of light weight and high rigidity. A structural member (a) that is a cylindrical body having a cylindrical shape as a whole is a preferred embodiment of the present invention, and a member that is a tubular member as a whole, i.e., a pipe-shaped member, is a particularly preferred embodiment of the present invention, because the integrally molded product can be easily applied to frame structures, etc.
[0022] The shape of the radial cross section of the cylindrical or columnar portion of the structural member (a) is not particularly limited, but is preferably circular or rectangular. 2 More preferably, 50 mm or more 2 That's all. Also, 300mm 2 Preferably less than 200 mm 2 When the radial cross-sectional area of the structural member (a) is within this range, a highly rigid integrally molded product can be obtained with good productivity.
[0023] The structural member (a) is essentially composed of a thermosetting resin, and if it has a thermoplastic resin region exposed on its surface, particularly at the portion where it joins with the metal member (b), it can be easily joined by thermal welding to the metal member (b) via the thermoplastic resin region, particularly to the surface of the structural member (a) located on the structural member (a) side of the joining interface, as described below. Such a thermoplastic resin region is typically provided thinly on the surface of the structural member (a), and its thickness is usually 1 to 300 μm, and more preferably 50 to 150 μm.
[0024] The form of such a thermoplastic resin region is not particularly limited as long as it forms a region in which the thermoplastic resin is exposed on the surface of the structural member (a), but examples thereof include layer-like, spot-like, mesh-like, and lattice-like forms.
[0025] Furthermore, preferred thermoplastic resins constituting such thermoplastic resin regions include polyolefin resins, polyester resins, polyamide resins, polycarbonate resins, polyphenylene sulfide resins, polyimide resins, polyamideimide resins, polyetherimide resins, polyether ketone resins, polyether ether ketone resins, polyether ketone ketone resins, and polyarylate resins.
[0026] When a thermoplastic resin region is present in the structural member (a), it is preferable that the interface between the thermosetting resin and the thermoplastic resin region of the structural member (a) has an uneven shape, from the viewpoint of obtaining high bonding strength. Here, "an uneven interface" means that the boundary surface between the thermosetting resin and the thermoplastic resin region is not flat, but forms an interface in which a shape recessed toward the thermosetting resin region and a shape recessed toward the thermoplastic resin region are mixed. In this case, the depth of the recess is preferably 1 to 200 μm, more preferably 10 to 100 μm.
[0027] In the present invention, the manufacturing method of the structural member (a) is not particularly limited. When the structural member (a) is a cylindrical body, examples of the manufacturing method include a method in which a prepreg or the like, in which reinforcing fibers impregnated with a thermosetting resin are aligned, is wound around a mandrel under a predetermined tension by a filament winding method or a sheet winding method, and then cured to form a shape, or a method in which the prepreg is shaped by internal pressure molding using a shaping mold or press molding, and then cured. As a method for forming a thermoplastic resin region on at least a portion of the outer or inner surface of the structural member (a), a method in which at least one layer of a film made of a thermoplastic resin is wound at the beginning or end of the above method, and then integrated with the thermosetting resin and cured can be mentioned.
[0028] The metal member (b) in the present invention is a member essentially composed of a metal. There are no particular limitations on the metal, and examples thereof include aluminum, copper, nickel, tin, gold, silver, iron, magnesium, chromium, tungsten, zinc, lead, and alloys thereof. The metal member (b) may be composed of one type of metal or a combination of two or more types of metal. Among these, aluminum alloys and titanium alloys, which have high specific strengths, are preferred, and aluminum alloys are most preferred.
[0029] The metal member (b) is preferably either a joint or a base. Typically, a joint is a member for connecting two cylindrical or columnar portions, changing their direction, connecting cylindrical or columnar portions of different thicknesses, or merging or branching three or more cylindrical or columnar portions. A base is a member for receiving and mounting a cylindrical or columnar portion. In the present invention, at least one of these cylindrical portions is the structural member (a) having the aforementioned cylindrical portion, and in a preferred embodiment, all of them are the aforementioned cylindrical portions. Figures 1A to 1D show a typical joint, Figures 2A to 2D show an integrally molded product in which the structural member (a) (cylindrical body) and the joint are integrated, Figures 3A to 3B show a typical base, and Figures 4A to 4B show an integrally molded product in which the structural member (a) (cylindrical body) and the base are integrated, but the structures of each are not limited to these.
[0030] The metal member (b) may also be a cylindrical body. Typically, the cylindrical body is a cylindrical body that differs in length, diameter, thickness, etc. from the cylindrical or columnar portion of the structural member (a). Fig. 5 shows a typical cylindrical body, and Fig. 6 shows a schematic diagram of an integrated molded product in which the structural member (a) (first cylindrical body) 1 and the metal member (b) (second cylindrical body) 2 are integrated, but the structures of each are not limited to these.
[0031] The metal member (b) may be subjected to a surface treatment on at least a part of its surface, such as a roughening treatment, an adhesion enhancing treatment, an antistatic treatment, a sandblasting treatment (sand matting), a corona discharge treatment, a plasma treatment, an excimer treatment, a chemical etching treatment, a water matting treatment, a flame treatment, an acid treatment, an alkali treatment, an oxidation treatment, an ultraviolet irradiation treatment, or a silane coupling agent treatment.
[0032] In the present invention, the metal member (b) may have a thermoplastic resin region on at least a portion of its surface. This allows the structural member (a) and the metal member (b) to be joined by thermal welding via the thermoplastic resin region. In a more preferred embodiment, both the structural member (a) and the metal member (b) have such thermoplastic resin regions, and the thermoplastic resin region of the structural member (a) and the thermoplastic resin region of the metal member (b) are joined by thermal welding. When both the structural member (a) and the metal member (b) have thermoplastic resin regions, it is preferable that the thermoplastic resin types constituting the thermoplastic resin regions of both the structural member (a) and the metal member (b) are the same, from the viewpoint of the joining strength between them.
[0033] Such a thermoplastic resin region is typically provided thinly by a method such as applying a thermoplastic resin to the surface of the metal member (b), and its thickness is usually 10 to 300 μm, more preferably 50 to 150 μm. The shape of the thermoplastic resin region can be, for example, a layer, a spot, a mesh, a lattice, or the like.
[0034] Furthermore, from the viewpoint of the bonding strength between the structural member (a) and the metal member (b), when both the structural member (a) and the metal member (b) have thermoplastic resin regions on their surfaces, it is preferable that the thermoplastic resins constituting the thermoplastic resin regions of both members are of the same type.
[0035] In the integrally molded product of the present invention, the metal member (b) has an overlap region that overlaps with the structural member (a), and at least a portion of the overlap region has a joint that contacts the structural member (a). "The metal member (b) overlaps the structural member (a)" means that the structural member (a) and at least a portion of the metal member (b) are in surface contact with each other. The overlap region refers to the contact region.
[0036] 7A and 7B show an embodiment in which a metal member (b) (joint 2) is joined to the outer peripheral surface of a structural member (a) 1. In this embodiment, the inner peripheral surface of the tubular metal member (b) is in contact with the outer peripheral surface of the structural member (a) via a thermoplastic resin layer 3, surrounding the entire outer peripheral surface of the structural member (a). That is, the metal member (b) overlaps the structural member (a) over its entire circumference. The metal member (b) may be in contact only partially with the outer or inner peripheral surface of the structural member (a), rather than the entire circumference. However, to achieve strong joint strength, it is preferable that the metal member (b) be joined over a range of 50% or more of the circumferential length of the cylindrical or columnar portion of the structural member (a) in the overlap region. It is particularly preferable that the metal member (b) be joined over a range of 100% (the entire circumference), i.e., the overlap region has a closed cross section. In particular, FIG. 7B shows an embodiment in which a thermoplastic resin is present on the surface of the structural member (a) located closer to the structural member (a) than the joint interface, which is a more preferred embodiment.
[0037] In addition, when joining to the tubular portion of the structural member (a), whether the metal member (b) is joined by overlapping with the outer peripheral surface or the inner peripheral surface is a matter to be decided depending on the target member, but from the viewpoint of productivity, it is preferable to join by overlapping with the outer peripheral surface of the tubular portion of the structural member (a). Furthermore, the integrally molded product can have both the metal member (b) joined by overlapping with the outer peripheral surface and the metal member (b) joined by overlapping with the inner peripheral surface.
[0038] In the present invention, by designing the clearance between the structural member (a) and the metal member (b) to be within the range of −0.1 to 0.1 mm, sufficient pressure due to the difference in expansion coefficients can be applied and damage to the structural member (a) or the metal member (b) due to the application of excessive pressure can be prevented. The clearance between the structural member (a) and the metal member (b) is preferably −0.075 to 0.075 mm, more preferably −0.05 to 0.05 mm. The clearance between the structural member (a) and the metal member (b) refers to the shortest distance from the outer surface of the member located on the inner side of the overlap region to the inner surface of the member located on the outer side. For example, if the cross-sectional shapes of the structural member (a) and the metal member (b) are elliptical and the metal member (b) is located on the inner side of the structural member (a), the clearance is measured as the shortest distance from the outer surface of the metal member (b) to the structural member (a) at 0°, 90°, 180°, or 270°. From the viewpoint of stress concentration, it is preferable that the coefficient of variation of the clearance between the structural member (a) and the metal member (b) in any radial cross section of the cylindrical or columnar portion of the structural member (a) in the overlap region is 2.0% or less, and more preferably 0.5% or less.
[0039] Furthermore, since the metal member (b) is essentially composed of metal, the shape change of each member due to heat input during joining is extremely small, resulting in an integrated molded product with high dimensional accuracy. When joined to the cylindrical portion of the structural member (a), i.e., when there is an overlap region in contact with the cylindrical portion, the concentricity, which indicates the center deviation of the cross sections of the structural member (a) and the metal member (b) in the overlap region, is preferably 0.25 mm or less. The concentricity can be measured by comparing the geometric center positions of the structural member (a) and the metal member (b) using a CNC coordinate measuring machine.
[0040] In the present invention, the linear expansion coefficient α of the joint periphery of the structural member (a) in the measurement temperature range of 60°C to 150°C is ta and the linear expansion coefficient α of the joining periphery of the metal member (b) tb The ratio (α tb / α ta By designing the ratio α to be within the range of 1.0 to 50, sufficient pressure can be applied without generating voids due to differences in the expansion coefficient, and the flow of the thermoplastic resin layer to the outside due to the application of excessive pressure can be suppressed. tb / α tais preferably 1.5 to 20, more preferably 2.0 to 10. In this specification, the term "joint perimeter" refers to a curve along the joint surface in a cross section perpendicular to the joint of the integrally molded product, and the linear expansion coefficient of the joint perimeter of a member refers to the ease of expansion of the joint perimeter of the member due to heating. The linear expansion coefficient of the joint perimeter of a member can be calculated by heating the member from 30°C to 180°C at a heating rate of 5°C / min and dividing the expansion amount of the joint perimeter from 60°C to 150°C by the joint perimeter at 60°C and the temperature change. For example, if the structural member (a) is a structural member having a cylindrical or columnar portion, and the metal member (b) has an overlap region that overlaps the outer peripheral surface and / or inner peripheral surface of the cylindrical or columnar portion of the structural member (a), and has a joint in contact with the structural member (a) at the overlap region, the joint perimeter of the structural member (a) in any cross section of the integrally molded product refers to the outer peripheral and / or inner peripheral of the cylindrical or columnar portion. For example, in the case of an elliptical pipe in which a structural member (a) is located on the inner periphery of a metal member (b), the linear expansion coefficient of the joint periphery of the members can be calculated by measuring the amount of expansion of the outer periphery at any cross section of the structural member (a). The amount of expansion of the members can be measured by placing the members on a hot plate, measuring the length of the joint periphery before and after heating from images taken with a camera or microscope, etc., and calculating the amount of change.
[0041] In addition, in the measurement temperature range of 60°C to 150°C, the linear expansion coefficient α of the joint periphery of the structural member (a) at the joint ta and the linear expansion coefficient α of the thermoplastic resin layer at the joining periphery tc The ratio (α tc / α ta When the ratio (R) is designed to be in the range of 1.5 to 10, the generation of voids inside the thermoplastic resin layer during integral molding can be suppressed, and high bonding strength can be obtained. The ratio is preferably 1.5 to 7.5, and more preferably 2.0 to 5.0.
[0042] Linear expansion coefficient α of the thermoplastic resin layer at the joint periphery in the measurement temperature range from 60°C to 150°C tcFrom the viewpoint of obtaining high bonding strength, the surface tension is preferably 60 ppm / °C or more, more preferably 70 ppm / °C or more, and is preferably 200 ppm / °C or less, more preferably 150 ppm / °C or less.
[0043] At the joint between the structural member (a) and the metal member (b), a thermoplastic resin layer is preferably present on the surface of the structural member (a) located closer to the structural member (a) than the joint boundary. Here, the state in which a thermoplastic resin layer is present on the surface of the structural member (a) located closer to the structural member (a) than the joint boundary refers to a state in which, in the cross section of the joint, the line forming the outer periphery of the structural member (a) is the joint boundary, and the thermoplastic resin layer is present closer to the structural member (a) than that.
[0044] At the joint between the structural member (a) and the metal member (b), it is preferable that some of the fibers contained in the structural member (a) straddle the thermosetting resin and thermoplastic resin layers constituting the structural member (a), i.e., be in contact with both the thermosetting resin and the thermoplastic resin layers of the structural member (a). By forming such a structure, a strong bond can be formed due to the fiber reinforcement effect. This effect is particularly pronounced when the fibers contained in the structural member (a) are continuous fibers.
[0045] The bonding strength between the structural member (a) and the metal member (b) is preferably 7 MPa or more, more preferably 10 MPa or more. There is no particular upper limit to the bonding strength, but from the viewpoint of obtaining the integrally molded product of the present invention with good productivity, it is preferably 100 MPa or less.
[0046] For example, the integrally molded product of the present invention can be produced by preparing a structural member (a) having a thermoplastic resin region on at least a portion of the outer and / or inner surface of a cylindrical or columnar portion, and a metal member (b) optionally having a thermoplastic resin region on at least a portion of its surface, and then contacting the structural member (a) and / or the metal member (b) in a heated state so that the structural member (a) and the metal member (b) overlap in a region including the heated thermoplastic resin region. The heat welding method is not particularly limited, and includes hot plate welding, vibration welding, ultrasonic welding, far-infrared heating welding, dielectric heating welding, laser welding, and the like. In this case, the structural member (a) or the metal member (b) is preferably heated to a temperature above the softening temperature of the thermoplastic resin constituting the thermoplastic resin region, and more preferably above the melting temperature.
[0047] The integrally molded product of the present invention is preferably used as a member for forming a frame structure because it comprises a lightweight, highly rigid structural member (a) and a metal member (b) that can be connected, merged, branched, or placed on a fixed position. Examples of such structures include the bodies and arms of industrial robots, the bodies and arms of automobiles, motorcycles, bicycles, aircraft, helicopters, drones, ships, submarines, and the like, and construction materials. In particular, from the viewpoints of rigidity and light weight, it is preferably used as a structural member for flying objects such as aircraft, helicopters, and drones.
[0048] Furthermore, because the arm component including the integrally molded product of the present invention is lightweight, it is suitable for use in a multi-rotor flying vehicle equipped with three or more rotors, preferably six or more rotors, and more preferably eight or more rotors, in order to maximize the effect of weight reduction.
[0049] The weight of an arm part including the integrally molded product of the present invention is preferably within the range of 300 g or less. While there is no particular lower limit on the weight, it is preferably 50 g or more from the viewpoint of handling the flying object. Furthermore, from the viewpoint of determining the center of gravity of the flying object, the weight variation coefficient of the arm part including the integrally molded product of the present invention is preferably within the range of 0.1 to 1.0%.
[0050] Since the integrally molded product of the present invention is lightweight, a projectile using the integrally molded product of the present invention can be loaded with goods, and the loaded weight can account for 20 to 60% of the total weight of the projectile.
[0051] The present invention will be explained in more detail below by showing examples, but the present invention is not limited to the descriptions of the examples in any way.
[0052] Example 1: Pellets of copolymer polyamide resin (CM4000, manufactured by Toray Industries, Inc., polyamide 6 / 66 / 610, melting point 150°C) were hot-pressed to obtain a polyamide film. The polyamide film, adjusted to a thickness of 70 μm, was wrapped around a release-treated stainless steel mandrel with a tip outer diameter of 30 mm, a taper of 6.0 / 1000, and a length of 700 mm as a thermoplastic resin layer. Then, using "TORAYCA PREPREG" P3051S-30 and P3052S-12 manufactured by Toray Industries, Inc., P3051S-30 was laminated at a material angle of 0 degrees, and P3052S-12 was laminated at a material angle of 60 degrees, assuming the longitudinal direction of the mandrel as the 0-degree axis. Furthermore, wrapping tape (heat-resistant film tape, width 10 mm) was wrapped around the outside of the mandrel with a tension of 3 kg, and the film was heat-molded in a curing oven at 150°C for 30 minutes. Thereafter, the mandrel was removed, the wrapping tape was removed, and the pipe 1 was cut to obtain a pipe 1 having a thickness of 0.5 mm and a length of 500 mm.
[0053] The cross section of the pipe 1 was observed using a digital microscope (Keyence Corporation, VHX-5000), and it was confirmed that there were reinforcing fibers straddling the boundary surface between the thermoplastic layer and the thermosetting layer. When the pipe 1 was heated to 150°C, the inner diameter expanded by 36 μm, and the calculated linear expansion coefficient α ta The linear expansion coefficient of the thermoplastic resin layer at the periphery of the bond was 9.6 ppm / °C.
[0054] Next, a ring-shaped A2000 series aluminum molded body having an outer diameter of 28 mm and a length of 30 mm was prepared. When the aluminum molded body was heated to 150° C., the outer diameter expanded by 59 μm, and the calculated linear expansion coefficient α tb was 23.4 ppm / °C.
[0055] That is, in this embodiment, α tb / α ta = 2.44.
[0056] The aluminum molded body was then fitted onto the pipe so that the outer surface of the aluminum molded body was in contact with the inner surface of the pipe 30 mm from the end and fixed in a vice, and the aluminum molded body was heated to 200°C using a far-infrared heater and then cooled to produce an integrated molded product.
[0057] The joints of the obtained integrally molded product were observed using a digital microscope (Keyence Corporation, VHX-5000) and the thickness of the thermoplastic resin layer was measured at any four points. The average value was 69.3 μm, and the coefficient of variation was 0.2%.
[0058] For the five integrally molded products thus obtained, the pipe 1 and the aluminum molded body were fixed together using a special jig, and a tensile test was carried out. As a result, all five products showed a bonding strength of 15 MPa or more.
[0059] Example 2: A mandrel made of SS400 material with an outer diameter of 28 mm and a length of 1.5 m was subjected to a release treatment. The release-treated mandrel was laminated using "TORAYCA PREPREG" P3051S-30 manufactured by Toray Industries, Inc., with the longitudinal direction of the mandrel as the 0° axis at angles of ±45°, 90°, and 0°. The same polyamide film as in Example 1 was then adjusted to a thickness of 100 μm and wrapped around once as a thermoplastic resin layer. A wrapping tape (heat-resistant film tape, width 10 mm) was then wrapped around the outside of the mandrel with a tension of 3 kg, and the resulting product was subjected to heat molding in a curing oven at 150°C for 30 minutes. The mandrel was then removed, the wrapping tape was removed, and the resulting product was cut to obtain a pipe 2 with a thickness of 0.5 mm and a length of 500 mm. The cross section of the pipe 2 was observed using a digital microscope (Keyence Corporation, VHX-5000), and it was confirmed that reinforcing fibers were present across the boundary between the thermoplastic layer and the thermosetting layer.
[0060] When the pipe 2 was heated to 150°C, the outer diameter expanded by 36 μm, and the calculated linear expansion coefficient α ta The linear expansion coefficient of the thermoplastic resin layer at the periphery of the bond was 10.2 ppm / °C.
[0061] Next, a ring-shaped A2000 series aluminum molded body having an inner diameter of 28.3 mm, an outer diameter of 40 mm, and a length of 30 mm was prepared. When the aluminum molded body was heated to 150°C, the inner diameter expanded by 59 μm, and the calculated linear expansion coefficient α tb was 22.5 ppm / °C.
[0062] That is, in this embodiment, α tb / α ta = 2.21.
[0063] The aluminum molded body was then heated to 200°C using a far-infrared heater, and then fitted onto the pipe so that the outer surface of the aluminum molded body was in contact with the inner surface of the pipe 30 mm from the end, fixed in place with a vise, and cooled to produce an integrated molded product.
[0064] The thickness of the thermoplastic resin layer was measured in the same manner as in Example 1, and the average value was 98.7 μm, and the coefficient of variation of the bonded circumference was 0.4%.
[0065] When a tensile test similar to that in Example 1 was carried out, all five pieces showed a bonding strength of 17 MPa or more.
[0066] (Example 3) The same experimental procedure as in Example 2 was carried out, except that a polyamide film having a thickness of 300 μm was used. When the thickness of the thermoplastic resin layer was measured in the same manner as in Example 1, the average value was 298.7 μm, and the coefficient of variation was 1.5%.
[0067] When a tensile test similar to that in Example 1 was carried out, all five pieces showed a bonding strength of 9 MPa or more.
[0068] (Example 4) A female mold with a concave shape was prepared, and a polyamide film adjusted to 100 μm was placed therein. Then, ten sheets of "TORAYCA PREPREG" P3051S-12 manufactured by Toray Industries, Inc. were laminated onto the female mold so that the angle was [0° / 90°] 5s when the longitudinal direction of the molded product was 0°. A male mold was then set in place, and the mold was press-molded at 150°C for 30 minutes under a pressure of 5 MPa to produce member 1. Member 1 had a U-shaped cross section corresponding to the concave shape of the female mold, and was 1.2 mm thick and had each side of 10 cm.
[0069] Cross-sectional observation of the member 1 using a digital microscope (Keyence Corporation, VHX-5000) confirmed the presence of reinforcing fibers across the boundary between the thermoplastic layer and the thermosetting layer. When the member 1 was heated to 150°C, the three sides expanded by a total of 202 μm, and the calculated linear expansion coefficient α of the joint circumference was ta The linear expansion coefficient of the thermoplastic resin layer at the periphery of the bond was 7.5 ppm / °C. Similarly, the linear expansion coefficient of the thermoplastic resin layer at the periphery of the bond was 86 ppm / °C.
[0070] Next, a U-shaped A2000 series aluminum molded body was prepared, each of whose inner sides was 10 cm long and whose thickness was 10 mm. When the aluminum molded body was heated to 150°C, the three sides expanded by a total of 653 μm, and the calculated linear expansion coefficient α tb was 24.2 ppm / °C.
[0071] That is, in this embodiment, α tb / α ta = 3.23.
[0072] The aluminum molded body was heated to 300°C using a far-infrared heater, and then fixed in place with the outer surface of member 1 and the inner surface of the aluminum molded body in contact with each other, followed by cooling to produce an integrated molded product.
[0073] A drop test was conducted on the five integrally molded products obtained, dropping them from a height of 1.5 m with the joint facing downwards, and visually inspecting the bonded state. As a result, no changes were observed in the joints of any of the five products, and a good bonded state was maintained.
[0074] Comparative Example 1 The same operation as in Example 2 was carried out, except that an annular tungsten molded body having an inner diameter of 28.4 mm, an outer diameter of 40 mm, and a length of 30 mm was prepared instead of the aluminum molded body. When the tungsten molded body was heated to 150°C, the inner diameter expanded by 14.6 μm, and the calculated linear expansion coefficient was 4.1 ppm / °C.
[0075] That is, in this comparative example, α tb / α ta = 0.40.
[0076] When the integrally molded product was pulled by hand, the pipe 2 and the tungsten molded body were easily separated, indicating that the joint strength was not sufficient.
[0077] 1 Structural member (a) (first cylindrical body) 2 Metal member (b) (joint, base or second cylindrical body) 3 Thermoplastic resin
Claims
1. An integrally molded product in which a structural member (a) essentially made of a fiber-reinforced thermosetting resin and a metal member (b) are joined together, the metal member (b) having an overlap region that overlaps the structural member (a), at least a portion of the overlap region having a joint in contact with the structural member (a), and the linear expansion coefficient α of the joint periphery of the structural member (a) in the measurement temperature range of 60°C to 150°C is ta and the linear expansion coefficient α of the joint periphery of the metal member (b) tb Ratio to (α tb / α ta ) is 1.0 to 50.
2. The integrally molded product according to claim 1, wherein the structural member (a) is a structural member having a cylindrical portion or a columnar portion, and the metal member (b) has an overlap region that overlaps with the outer peripheral surface and / or the inner peripheral surface of the cylindrical portion or columnar portion of the structural member (a), and has a joint that contacts the structural member (a) over at least a portion of the overlap region.
3. The integrally molded product according to claim 1 or 2, wherein the structural member (a) has a thermoplastic resin region exposed on the surface, and the metal member (b) has an overlap region that overlaps the structural member (a), and at least a portion of the overlap region has a joint that is joined to the structural member (a) via a thermoplastic resin layer.
4. The linear expansion coefficient α of the joint periphery of the structural member (a) at the joint ta and the linear expansion coefficient α of the thermoplastic resin layer at the joining periphery tc The ratio of (α tc / α ta 4. The integrally molded product according to claim 3, wherein the ratio of the molecular weight of the polymer to the molecular weight of the solid polymer is 1.5 to 10.
5. Linear expansion coefficient α of the thermoplastic resin layer at the joint periphery tc The integrally molded product according to claim 3, wherein the viscosity is 60 ppm / °C or more and 200 ppm / °C or less.
6. The integrally molded product according to claim 3, wherein the thickness of the thermoplastic resin layer is 10 to 300 μm.
7. The integrally molded product according to claim 2, wherein the clearance between the structural member (a) and the metal member (b) is -0.1 to 0.1 mm in any radial cross section of the cylindrical or columnar portion of the structural member (a) in the overlap region.
8. The integrally molded product according to claim 7, wherein the coefficient of variation Cv of the clearance is 2.0% or less.
9. An integrally molded product formed by joining a structural member (a) having a cylindrical or columnar portion, which is essentially made of a fiber-reinforced thermosetting resin, to a metal member (b), wherein the structural member (a) has a thermoplastic resin region exposed on the outer peripheral surface and / or inner peripheral surface of the cylindrical or columnar portion, the metal member (b) has an overlap region overlapping the outer peripheral surface and / or inner peripheral surface of the cylindrical or columnar portion of the structural member (a), and at least a part of the overlap region has a joint portion joined to the structural member (a) via a thermoplastic resin layer, and wherein the linear expansion coefficient α of the joint periphery of the structural member (a) in the measurement temperature range of 60°C to 150°C is less than 0.05%. ta and the linear expansion coefficient α of the joint periphery of the metal member (b) tb Ratio to (α tb / α ta 3. The integrally molded product according to claim 2, wherein the ratio of the molecular weight of the polymer to the molecular weight of the solid polymer is 1.0 to 50.
10. An integrally molded product according to claim 2 or 9, wherein the fibers contained in the structural member (a) are continuous fibers, and the continuous fibers are in contact with both the thermosetting resin and the thermoplastic resin layer constituting the structural member (a).
11. The integrally molded product according to claim 1 or 2, wherein the bonding strength between the structural member (a) and the metal member (b) is 7 MPa or more and 100 MPa or less.
12. The integrally molded product according to claim 2 or 9, wherein the metal member (b) has a cylindrical portion, the cylindrical portion has the overlap region, and in the overlap region, the concentricity between the cylindrical or columnar portion of the structural member (a) and the cylindrical portion of the metal member (b) is 0.25 mm or less.
13. The integrally molded product according to claim 2 or 9, wherein the structural member (a) is a member having a generally tubular shape.
14. The integrally molded product according to claim 2 or 9, wherein the metal member (b) is a joint or a base.
15. A frame structure comprising the integrally molded product according to claim 2 or 9.
16. A flying object made using the integrally molded product according to claim 1, 2 or 9.
17. A multi-rotor flying vehicle equipped with three or more arm parts including the integrally molded product according to claim 2 or 9.
18. The flying object according to claim 17, wherein the weight of the arm part is 50 to 300 g.
19. The flying object according to claim 17, wherein the weight variation coefficient Cv of the arm parts is 0.1 to 1.0%.
20. The flying object according to claim 16 or 17, which is capable of carrying cargo, and the load weight is 20 to 60% of the total weight of the flying object.
21. A method for producing an integrally molded product in which a structural member (a) essentially consisting of a fiber-reinforced thermosetting resin and a metal member (b) are joined by thermal welding via a thermoplastic resin layer, comprising the steps of: preparing a structural member (a) having a thermoplastic resin region on at least a portion of a surface layer; and optionally preparing a metal member (b) having a thermoplastic resin region on at least a portion of a surface; and, while the structural member (a) and / or the metal member (b) are heated, bringing the structural member (a) and the metal member (b) into contact with each other in a region of the structural member (a) that includes the thermoplastic resin region, so that the structural member (a) and the metal member (b) overlap each other.
Citation Information
Patent Citations
Joining structure of truss member
JP1999350592A
Method for producing joint body of thermoplastic composite material and metal member
JP2013244725A
Integrally assembled product of CFRP pipe and metal part, and bonding method therefor
JP2016221784A
Manufacture of composite material
JP1998016072A
Composite structure
JP2011213108A
Cited By
Frame structure, flying object, and method for producing frame structure
WO2026071057A1