Multilayer ceramic capacitor

The multilayer ceramic capacitor design addresses the limitations of existing capacitors by controlling crystal orientation and layer structure, achieving enhanced mechanical strength and dielectric performance.

WO2024204018A1PCT designated stage expired Publication Date: 2024-10-03MURATA MFG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011609
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing multilayer ceramic capacitors do not adequately improve electrical characteristics and reliability, particularly in terms of mechanical strength and dielectric constant.

Method used

A multilayer ceramic capacitor design with a laminate structure featuring stacked dielectric and internal electrode layers, where the crystal orientation of dielectric layers is controlled to have adjacent grains with a crystal orientation difference of within 5 degrees, and an external electrode layer connected to internal electrode layers, enhancing mechanical strength and dielectric properties.

Benefits of technology

The design results in improved mechanical strength and higher dielectric constant, as demonstrated by reduced crack occurrence and increased dielectric constant values, respectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011609_03102024_PF_FP_ABST
    Figure JP2024011609_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a multilayer ceramic capacitor having further improved mechanical strength. A multilayer ceramic capacitor 1 includes: a plurality of laminated dielectric layers; and a plurality of laminated internal electrode layers. The multilayer ceramic capacitor 1 comprises: a laminate 2 that includes a first main surface M1 and a second main surface M2 facing each other in the height direction T, a first side surface S1 and a second side surface S2 facing each other in a width direction W orthogonal to the height direction T, and a first end surface E1 and a second end surface E2 facing each other in a length direction L orthogonal to the height direction T and the width direction W; and an external electrode layer provided on the laminate 2 and connected to a portion of the internal electrode layers. If a crystal orientation of crystal particles C of the dielectric layers is measured by an electron beam backscatter diffraction method, two or more sets of crystal particles are found in which a difference between crystal orientations of two adjacent crystal particles C in an observation range of 2μ square is within 5 degrees on the basis of a given direction.
Need to check novelty before this filing date? Find Prior Art

Description

Multilayer ceramic capacitors

[0001] The present invention relates to a multilayer ceramic capacitor.

[0002] In recent years, multilayer ceramic capacitors have been increasingly applied to electronic devices that require high dielectric constants and high reliability, such as small in-vehicle devices. Patent Document 1 describes a technique for improving the performance of multilayer ceramic capacitors by adjusting the distribution of nickel near the grain boundaries.

[0003] Japanese Patent Application Laid-Open No. 2017-228590

[0004] However, the technology described in Patent Document 1 may not sufficiently improve electrical characteristics or reliability in some cases. Therefore, an object of the present invention is to provide a multilayer ceramic capacitor with improved mechanical strength.

[0005] The multilayer ceramic capacitor of the present invention comprises a laminate including a plurality of laminated dielectric layers and a plurality of laminated internal electrode layers, the laminate having first and second main surfaces opposing each other in a height direction, first and second side surfaces opposing each other in a width direction perpendicular to the height direction, and first and second end faces opposing each other in a length direction perpendicular to the height and width directions, and external electrode layers provided on the laminate and connected to some of the internal electrode layers, wherein, when the crystal orientation of the crystal grains of the dielectric layers is measured by electron backscatter diffraction, there are two or more pairs of crystal grains in an observation area of ​​2 μm square, in which the difference in crystal orientation between two adjacent crystal grains is within 5 degrees based on an arbitrary direction.

[0006] According to the present invention, it is possible to provide a multilayer ceramic capacitor with improved mechanical strength.

[0007] 1 is a perspective view of a multilayer ceramic capacitor according to embodiment 1. FIG. 1 is a cross-sectional view taken along line II of FIG. 1. FIG. 1 is a cross-sectional view taken along line II-II of FIG. 1. FIG. 2 is an image quality map showing crystal grains observed in an example of embodiment 1. FIG. 4A is a crystal orientation map created based on FIG. 4A. FIG. 5A is an image quality map showing crystal grains observed in a comparative example of embodiment 1. FIG. 5A is a crystal orientation map created based on FIG. 5A. FIG. 6 is a diagram showing peak diffraction angles for an example of embodiment 2. FIG. 7 is a diagram showing peak diffraction angles for a comparative example of embodiment 2. FIG. 8 is a diagram showing a case where a crystal orientation (100) plane is observed in observation using high-angle scattering dark-field scanning transmission electron microscopy. FIG. 9 is a diagram showing a case where a crystal orientation (100) plane is observed in observation using high-angle scattering dark-field scanning transmission electron microscopy. FIG. 10 is a diagram showing a case where a crystal orientation (100) plane is observed in observation using high-angle scattering dark-field scanning transmission electron microscopy. FIG. 11 is a diagram showing a case where a crystal orientation (100) plane is observed in observation using high-angle scattering dark-field scanning transmission electron microscopy.

[0023] FIG. 1 is a diagram showing a case where a crystal orientation (100) plane is observed in observation using a high-angle scattering dark-field scanning transmission electron microscope.

[0024] FIG. 2 is a diagram showing a case where a crystal orientation (100) plane is observed in observation using a high-angle scattering dark-field scanning transmission electron microscope.

[0025] FIG. 3 is a diagram showing a case where a crystal orientation (100) plane is not observed in observation using a high-angle scattering dark-field scanning transmission electron microscope.

[0026] FIG. 4 is a diagram showing the state of observation using a high-angle scattering dark-field scanning transmission electron microscope.

[0008] (Embodiment 1) An embodiment of the present invention will be described with reference to Fig. 1. Fig. 1 is a perspective view of a multilayer ceramic capacitor 1 according to embodiment 1 of the present invention. Note that Fig. 1 shows a so-called two-terminal multilayer ceramic capacitor. However, the multilayer ceramic capacitor 1 of the present invention is not limited to a two-terminal multilayer ceramic capacitor. The multilayer ceramic capacitor 1 of the present invention may also be a multi-terminal multilayer ceramic capacitor, such as a three-terminal multilayer ceramic capacitor.

[0009] (Laminate) The laminate 2 includes a plurality of dielectric layers and a plurality of internal electrode layers that are stacked together. The shape of the laminate 2 is approximately a rectangular parallelepiped.

[0010] In the laminate 2, the direction in which the dielectric layers and internal electrode layers are stacked is defined as a height direction T. The direction perpendicular to the height direction T is defined as a width direction W. The direction perpendicular to the height direction T and the width direction W is defined as a length direction L.

[0011] Of the two surfaces of the laminate 2 that face each other in the height direction T, one surface is designated as the first main surface M1. The remaining surface is designated as the second main surface M2. Of the two surfaces of the laminate 2 that face each other in the width direction W, one surface is designated as the first side surface S1. The remaining surface is designated as the second side surface S2. Of the two surfaces of the laminate 2 that face each other in the length direction L, one surface is designated as the first end surface E1. The remaining surface is designated as the second end surface E2.

[0012] Regarding the cross section of the laminate 2, the cross section taken along line II in Fig. 1 is defined as the LT cross section, and the cross section taken along line II-II in Fig. 1 is defined as the WT cross section.

[0013] The intersections of three surfaces of the laminate 2 are defined as corners of the laminate 2, and the intersections of two surfaces of the laminate 2 are defined as ridges of the laminate 2. The corners and ridges are preferably rounded.

[0014] (Dielectric Layers) The total number of dielectric layers stacked in the laminate 2 is preferably 15 or more and 2000 or less. The main material of the dielectric layers is a ceramic material. Examples of ceramic materials are dielectric ceramics containing barium titanate, calcium titanate, strontium titanate, calcium zirconate, or the like as main components. The ceramic material may also be a dielectric ceramic in which a secondary component such as a manganese compound, an iron compound, a chromium compound, a cobalt compound, or a nickel compound is added to these main components.

[0015] The dielectric layer contains crystal grains. These crystal grains are the main component of the dielectric layer and are made of perovskite oxides containing A-site elements and B-site elements. Perovskite oxides are represented by the general formula: ABO 3The perovskite structure has a composition represented by the formula: Atoms of the A-site element and atoms of the B-site element are ionized and occupy the A-site and B-site, respectively. Examples of the A-site element include elements with a relatively large ion size, such as barium, calcium, and strontium. Examples of the B-site element include elements with a relatively small ion size, such as titanium, zirconium, and hafnium.

[0016] The combination of A-site elements and B-site elements is not particularly limited as long as the perovskite structure is maintained. Each of the A-site elements and B-site elements may contain only one element or a combination of multiple elements.

[0017] Preferably, the A-site element includes barium and the B-site element includes titanium, i.e., the perovskite oxide is preferably a barium titanate-based compound.

[0018] The thickness of each dielectric layer is preferably 0.3 μm or more and 10 μm or less.

[0019] (Division of Laminate) The division of the laminate 2 in the length direction L will be described with reference to Figure 2. Figure 2 is a cross-sectional view taken along line II in Figure 1. The laminate 2 can be divided into a first main surface side outer layer portion OL1, an inner layer area IL, and a second main surface side outer layer portion OL2 in the height direction T. The first main surface side outer layer portion OL1, the inner layer area IL, and the second main surface side outer layer portion OL2 are arranged in this order in the height direction T from the first main surface M1 to the second main surface M2.

[0020] The first outer layer portion OL1 is a portion between the first main surface M1 and the internal electrode layer closest to the first main surface M1. The internal layer range IL is a range where internal electrode layers face each other. The second outer layer portion OL2 is a portion between the second main surface M2 and the internal electrode layer closest to the second main surface M2.

[0021] The first main surface side outer layer portion OL1 is located on the first main surface M1 side of the laminate 2. The first main surface side outer layer portion OL1 is formed by an assembly of multiple dielectric layers located between the first main surface M1 and the internal electrode layer closest to the first main surface M1. The first main surface side outer layer portion OL1 is formed by multiple dielectric layers located between the first main surface M1 and the outermost surface of the inner layer range IL on the first main surface M1 side and an extension of that outermost surface.

[0022] The second main surface side outer layer portion OL2 is located on the second main surface M2 side of the laminate 2. The second main surface side outer layer portion OL2 is formed by an assembly of multiple dielectric layers located between the second main surface M2 and the internal electrode layer closest to the second main surface M2. The second main surface side outer layer portion OL2 is formed by multiple dielectric layers located between the second main surface M2 and the outermost surface of the inner layer range IL on the second main surface M2 side and an extension of that outermost surface.

[0023] The inner layer area IL is an area sandwiched between the first outer layer portion OL1 on the main surface side and the second outer layer portion OL2 on the main surface side.

[0024] Of the dielectric layers, the dielectric layers arranged in the first main surface side outer layer portion OL1 and the second main surface side outer layer portion OL2 are referred to as outer dielectric layers 3. Of the dielectric layers, the dielectric layers arranged in the inner layer range IL are referred to as inner dielectric layers 4.

[0025] The following terms may be used in describing lengths and positions:

[0026] The length in the length direction L is defined as the length direction length, the length in the width direction W is defined as the width direction length, and the length in the height direction T is defined as the height direction length.

[0027] The position that is half the length in the longitudinal direction is defined as the center position in the longitudinal direction L. The center position in the longitudinal direction L is defined as the longitudinal center position.

[0028] The position that is half the length in the width direction is defined as the center position in the width direction W. The center position in the width direction W is defined as the width direction center position.

[0029] The position that is half the length in the height direction is defined as the center position in the height direction T. The center position in the height direction T is defined as the height direction center position.

[0030] The ends in the length direction L are defined as length-direction ends, the ends in the width direction W are defined as width-direction ends, and the ends in the height direction T are defined as height-direction ends.

[0031] The size of the laminate 2 is not particularly limited. The length of the laminate in the longitudinal direction is preferably 0.2 mm or more and 10 mm or less. The length of the laminate 2 in the width direction is preferably 0.1 mm or more and 5 mm or less. The length of the laminate 2 in the height direction is preferably 0.1 mm or more and 5 mm or less.

[0032] (L Gap) The division of the laminate 2 in the longitudinal direction L will be described. The laminate 2 can be divided into a first end surface side outer layer portion LG1, a longitudinally facing portion LF, and a second end surface side outer layer portion LG2 in the longitudinal direction L. The first end surface side outer layer portion LG1, the longitudinally facing portion LF, and the second end surface side outer layer portion LG2 are arranged in this order in the longitudinal direction L from the first end surface E1 to the second end surface E2.

[0033] The longitudinal facing portion LF is a portion where the internal electrode layers face each other in the height direction T. The first end face side outer layer portion LG1 is a portion between the longitudinal facing portion LF and the first end face E1. The second end face side outer layer portion LG2 is a portion between the longitudinal facing portion LF and the second end face E2. The longitudinal facing portion LF is a portion corresponding to the facing electrode portion of the internal electrode layer. The first end face side outer layer portion LG1 and the second end face side outer layer portion LG2 are portions corresponding to the lead electrode portions of the internal electrode layer. The first end face side outer layer portion LG1 and the second end face side outer layer portion LG2 are also referred to as L gaps.

[0034] The counter electrode portion includes a first counter electrode portion 7 a and a second counter electrode portion 7 b. The lead-out electrode portion includes a first lead-out electrode portion 8 a and a second lead-out electrode portion 8 b. The counter electrode portion and the lead-out electrode portion will be described later.

[0035] The first end face side outer layer portion LG1 is located on the first end face E1 side, between the first end face E1 and the end of the second internal electrode layer 6b on the first end face E1 side.

[0036] The second end face side outer layer portion LG2 is located on the second end face E2 side, between the second end face E2 and the end of the first internal electrode layer 6 a on the second end face E2 side.

[0037] (W Gap) The division of the laminate 2 in the width direction W will be described with reference to Figure 3. Figure 3 is a cross-sectional view taken along line II-II in Figure 1. The laminate 2 can be divided into a first side surface outer layer portion WG1, a widthwise opposing portion WF, and a second side surface outer layer portion WG2 in the width direction W. The first side surface outer layer portion WG1, the widthwise opposing portion WF, and the second side surface outer layer portion WG2 are arranged in this order in the width direction W from the first side surface S1 to the second side surface S2.

[0038] The widthwise facing portion WF is a portion where internal electrode layers face each other in the height direction T. The first side surface side outer layer portion WG1 is a portion between the widthwise facing portion WF and the first side surface S1. The second side surface side outer layer portion WG2 is a portion between the widthwise facing portion WF and the second side surface S2. The first side surface side outer layer portion WG1 and the second side surface side outer layer portion WG2 are also referred to as W gaps.

[0039] The first side surface side outer layer portion WG1 and the second side surface side outer layer portion WG2 are portions where no internal electrode layers exist in the height direction T. The first side surface side outer layer portion WG1 is located on the first side surface S1 side.

[0040] The second side surface outer layer portion WG2 is located on the second side surface S2 side and is formed of a plurality of dielectric layers located between the second side surface S2 and the outermost surface of the widthwise facing portion WF on the second side surface S2 side.

[0041] (Internal Electrode Layers) The internal electrode layers include a plurality of first internal electrode layers 6 a and a plurality of second internal electrode layers 6 b. The first internal electrode layers 6 a are internal electrode layers exposed at the first end face E1. The second internal electrode layers 6 b are internal electrode layers exposed at the second end face E2.

[0042] The first internal electrode layer 6a can be divided into a first opposing electrode portion 7a and a first lead electrode portion 8a. The first opposing electrode portion 7a is a portion facing the second internal electrode layer 6b. The first lead electrode portion 8a is a portion led from the first opposing electrode portion 7a to the first end face E1 of the laminate 2.

[0043] The end of the first extension electrode 8a on the first end face E1 side is extended to the surface of the first end face E1 of the laminate 2. The end of the first extension electrode 8a extended to the first end face E1 is exposed at the first end face E1.

[0044] The second internal electrode layer 6b can be divided into a second opposing electrode portion 7b and a second lead electrode portion 8b. The second opposing electrode portion 7b is a portion facing the first internal electrode layer 6a. The second lead electrode portion 8b is a portion led from the second opposing electrode portion 7b to the second end face E2 of the laminate 2.

[0045] The end of the second extraction electrode 8b on the second end face E2 side is extracted to the surface of the second end face E2 of the laminate 2. The end of the second extraction electrode 8b extracted to the second end face E2 is exposed at the second end face E2.

[0046] The material of the first internal electrode layer 6a and the second internal electrode layer 6b can be, for example, a metal such as nickel, copper, silver, palladium, gold, etc. The material of the first internal electrode layer 6a and the second internal electrode layer 6b can be an alloy containing at least one of the above-mentioned metals, such as a silver-palladium alloy.

[0047] In the multilayer ceramic capacitor 1, capacitance is formed by the first opposing electrode portion 7a and the second opposing electrode portion 7b facing each other via the inner dielectric layer 4. This allows the multilayer ceramic capacitor 1 to exhibit capacitor characteristics.

[0048] The thickness of the first internal electrode layers 6a and the second internal electrode layers 6b is preferably, for example, about 0.2 μm or more and 2.0 μm or less. The total number of the first internal electrode layers 6a and the second internal electrode layers 6b is preferably 15 or more and 2000 or less.

[0049] (Inner layer portion) The portion where the first internal electrode layer 6a and the second internal electrode layer 6b face each other is referred to as the inner layer portion 10. The inner layer portion 10 is the portion where the lengthwise facing portion LF shown in FIG. 2 and the widthwise facing portion WF shown in FIG. 3 intersect with the inner layer range IL. The shape of the inner layer portion 10 is approximately a rectangular parallelepiped. In FIG. 2, the portion where the lengthwise facing portion LF and the inner layer range IL intersect is shown as the inner layer portion 10. In addition, in FIG. 3, the portion where the widthwise facing portion WF and the inner layer range IL intersect is shown as the inner layer portion 10.

[0050] (External Electrodes) The external electrodes will now be described. The external electrodes include a first external electrode 20a and a second external electrode 20b. The first external electrode 20a is an external electrode connected to the first internal electrode layer 6a. The second external electrode 20b is an external electrode connected to the second internal electrode layer 6b.

[0051] The first external electrode 20a is disposed on the first end face E1, part of the first main face M1, part of the second main face M2, part of the first side face S1, and part of the second side face S2. The second external electrode 20b is disposed on the second end face E2, part of the first main face M1, part of the second main face M2, part of the first side face S1, and part of the second side face S2.

[0052] The external electrodes include a base electrode layer and a plating layer. The plating layer includes a Ni plating layer and a Sn plating layer. These layers are arranged in this order from the end surface of the laminate 2: base electrode layer, Ni plating layer, Sn plating layer.

[0053] The first external electrode 20a includes a first base electrode layer 22a, a first Ni-plated layer 23a, and a first Sn-plated layer 24a, and the second external electrode 20b includes a second base electrode layer 22b, a second Ni-plated layer 23b, and a second Sn-plated layer 24b.

[0054] (Base Electrode Layer) The first base electrode layer 22a is disposed on and covers the first end face E1 of the laminate 2. The first base electrode layer 22a extends from the first end face E1 to a portion of the first main surface M1, a portion of the second main surface M2, a portion of the first side surface S1, and a portion of the second side surface S2.

[0055] The second base electrode layer 22b is disposed on and covers the second end face E2 of the laminate 2. The second base electrode layer 22b extends from the second end face E2 to a portion of the first main surface M1, a portion of the second main surface M2, a portion of the first side surface S1, and a portion of the second side surface S2.

[0056] The base electrode layer includes a glass component and a metal. The glass component includes at least one selected from B, Si, Ba, Mg, Al, Li, etc. The metal includes at least one selected from Cu, Ni, Ag, Pd, an Ag—Pd alloy, Au, etc.

[0057] (Ni Plated Layer and Sn Plated Layer) The first Ni plated layer 23a is disposed so as to cover the first base electrode layer 22a. The first Sn plated layer 24a is disposed so as to cover the first Ni plated layer 23a.

[0058] The second Ni-plated layer 23b is disposed so as to cover the second base electrode layer 22b, and the second Sn-plated layer 24b is disposed so as to cover the second Ni-plated layer 23b.

[0059] The Ni plating layer can prevent the base electrode layer from being eroded by solder when mounting the multilayer ceramic capacitor 1. The Sn plating layer can improve the wettability of the solder when mounting the multilayer ceramic capacitor 1, making mounting easier.

[0060] A conductive resin layer may be disposed between the base electrode layer and the Ni plating layer. The conductive resin layer may contain epoxy resin, metal filler, and the like.

[0061] The size of the multilayer ceramic capacitor 1 is not particularly limited. The length in the longitudinal direction of the multilayer ceramic capacitor 1 including the laminate 2 and the external electrodes is preferably 0.2 mm or more and 10 mm or less. The length in the height direction of the multilayer ceramic capacitor 1 including the laminate 2 and the external electrodes is preferably 0.1 mm or more and 5 mm or less. The length in the width direction of the multilayer ceramic capacitor 1 including the laminate 2 and the external electrodes is preferably 0.1 mm or more and 10 mm or less.

[0062] (Method for manufacturing a multilayer ceramic capacitor) A method for manufacturing the multilayer ceramic capacitor 1 will be described. (1) A conductive paste for the dielectric sheets and the internal electrode layers is prepared. The conductive paste for the dielectric sheets and the internal electrode layers contains a binder and a solvent. The binder and the solvent may be a known organic binder and organic solvent, etc.

[0063] (2) A conductive paste for the internal electrode layers is printed on the dielectric sheet in a predetermined pattern. The internal electrode layer pattern is formed by printing the conductive paste. The printing can be performed by, for example, screen printing or gravure printing.

[0064] (3) A predetermined number of dielectric sheets for the outer layer portion are stacked. No internal electrode layer pattern is printed on the dielectric sheets for the outer layer portion. Dielectric sheets on which internal electrode layer patterns are printed are stacked in order on the stacked dielectric sheets. Furthermore, a predetermined number of dielectric sheets for the outer layer portion are stacked on top of those. A laminated sheet is produced by stacking these sheets.

[0065] (4) The laminated sheet is pressed in the height direction to produce a laminated block. The pressing method can be isostatic pressing.

[0066] (5) The laminated block is cut to a predetermined size. This cutting process cuts out laminated chips. When cutting, the corners and ridges of the laminated chips may be rounded. The rounding process may be performed by barrel polishing.

[0067] (6) The laminated chip is fired. This firing produces a laminate. The firing temperature is preferably 900° C. or higher and 1200° C. or lower. The firing temperature can be changed depending on the materials of the dielectric and internal electrode layers.

[0068] Cooling after heating to the firing temperature is faster than natural cooling. For example, cooling is performed from the firing temperature of 900°C to 1200°C to a temperature of 100°C to 300°C within 10 minutes. Preferably, cooling is performed from 1000°C to 200°C within 7 minutes. More preferably, cooling is performed from 1000°C to 200°C within 5 minutes. Even more preferably, cooling is performed from 1000°C to 200°C within 1 minute.

[0069] By cooling in this manner, productivity can be improved compared to when the material is simply left to cool naturally.

[0070] Here, "cooling" does not simply mean placing the stacked chips in gas at a predetermined temperature. "Cooling" means more actively cooling the stacked chips. For example, gas at a predetermined temperature can be blown onto the stacked chips. Alternatively, a solid or liquid at a predetermined temperature can be brought into contact with the stacked chips.

[0071] (External Electrodes) Next, the external electrodes are formed. First, a conductive paste that will become the base electrode layer is applied to the two end faces of the laminate 2. The conductive paste contains a glass component, a metal component, etc. The conductive paste can be applied by a method such as dipping. After application, a baking process is performed to form the base electrode layer. The baking temperature is preferably 500°C or higher and 900°C or lower. The baking time is preferably 30 minutes or higher and 2 hours or lower.

[0072] Next, a Ni plating layer is formed on the surface of the base electrode layer. Furthermore, a Sn plating layer is formed on the surface of the Ni plating layer. The Ni plating layer and the Sn plating layer can be formed by a barrel plating method or the like. In this manner, the multilayer ceramic capacitor 1 is obtained.

[0073] The crystal orientation of the crystal grains in the dielectric layer of the multilayer ceramic capacitor 1 of embodiment 1 will be described. (Crystal Orientation) In the dielectric layer of the multilayer ceramic capacitor 1 of embodiment 1, there are many pairs of adjacent crystal grains whose crystal orientations are close to each other. Hereinafter, the crystal orientation determined by electron backscatter diffraction (EBSD) will be described.

[0074] Figures 4A and 4B show an example of embodiment 1, and Figures 5A and 5B show a comparative example of embodiment 1. Figures 4A and 5B are image quality maps showing the appearance of crystal particles C observed in the ND direction by electron backscatter diffraction.

[0075] Fig. 4B is a crystal orientation map created based on the image quality map shown in Fig. 4A. Similarly, Fig. 5B is a crystal orientation map created based on the image quality map shown in Fig. 5A. A crystal orientation map is also called an inverse pole figure orientation map (IPF map).

[0076] For the examples and comparative examples of embodiment 1 shown in Figures 4A and 4B and Figures 5A and 5B, measurements were performed using electron backscatter diffraction on the following samples. The multilayer ceramic capacitor was polished to expose the surface of the sample. The polishing was performed by scraping and advancing along the plane parallel to the width direction W and the height direction T. The surface of the sample was taken as the WT cross section at the center position in the length direction T.

[0077] The crystal orientation was measured in the outer layer because the crystal orientation is highly correlated with cracks that occur in the outer layer.

[0078] The measurement by electron backscatter diffraction method was performed using a thin specimen. The WT cross section at the midpoint in the longitudinal direction T of the multilayer ceramic capacitor was processed into a thin specimen and then measured. Specifically, the surface opposite to the measurement surface was polished to a thickness of 100 nm, and the WT cross section was then measured.

[0079] The area for measuring the crystal orientation in the outer layer is 2 μm square. The number of crystal grains observed within this observation area is usually 50 to 250.

[0080] In the crystal orientation maps shown in Figures 4B and 5B, a dashed line A is drawn at the grain boundary between two adjacent crystal grains whose crystal orientations differ by within 5 degrees from an arbitrary direction.

[0081] As shown in Figure 4B, in the example of embodiment 1, within the measurement range shown in Figure 4B, there are 24 pairs of crystal grains in which the difference in crystal orientation between two adjacent crystal grains is within 5 degrees based on an arbitrary direction.

[0082] In contrast, in the comparative example of the first embodiment, there is one set, as shown in FIG. 5B.

[0083] Furthermore, in the example of embodiment 1, there are four sets of three crystal grains, each of which includes one crystal grain and two crystal grains adjacent to the crystal grain and whose crystal orientations are misaligned by an angle of 5 degrees or less from the crystal grain in question. In contrast, there are zero sets of three crystal grains in the comparative example of embodiment 1.

[0084] As described above, in the dielectric layers of the multilayer ceramic capacitor 1 of the first embodiment, there are many pairs of crystal grains whose crystal orientations are close to each other.

[0085] Furthermore, the multilayer ceramic capacitor 1 of embodiment 1 also has a higher ratio of crystal grains in contact with other crystal grains whose crystal orientations differ by within 5 degrees from the arbitrary direction relative to all crystal grains than conventional multilayer ceramic capacitors. In the multilayer ceramic capacitor 1 of embodiment 1 shown in FIG. 4B , 45 of the 166 total crystal grains were in contact with other crystal grains whose crystal orientations differ by within 5 degrees from the arbitrary direction relative to all crystal grains. This ratio was 27.1%. In contrast, in the comparative example of embodiment 1 shown in FIG. 5B , 2 of the 113 total crystal grains were in contact with other crystal grains whose crystal orientations differ by within 5 degrees from the arbitrary direction relative to all crystal grains. This ratio was 1.8%.

[0086] The multilayer ceramic capacitors of the examples of the first embodiment and the comparative examples of the first embodiment were evaluated for crack occurrence in the outer layer portions.

[0087] The evaluation method and criteria for crack occurrence were as follows: Ten multilayer ceramic capacitors were subjected to a deflection test according to the method of JIS C 6484, and the presence or absence of crack occurrence in the dielectric layer was evaluated when the deflection amount was fixed at 5 mm.

[0088] In the multilayer ceramic capacitor of the example of embodiment 1, no cracks occurred, whereas in the multilayer ceramic capacitor of the comparative example of embodiment 1, cracks occurred.

[0089] (Measurement Method) The length and thickness of each part can be measured as follows: The multilayer ceramic capacitor 1 is polished to the center position in the width direction. Then, the cross section exposed by polishing is observed using an optical microscope or the like. Measurements can be made from the observed cross section.

[0090] (Embodiment 2) A multilayer ceramic capacitor 1 according to embodiment 2 will be described. In the following description, differences from embodiment 1 will be mainly described. Items not specifically described can be the same as embodiment 1.

[0091] The technology described in Patent Document 1 may not be sufficient in improving electrical characteristics or reliability. Therefore, an object of the second embodiment is to provide a multilayer ceramic capacitor having a larger relative dielectric constant.

[0092] The multilayer ceramic capacitor of the second embodiment is a multilayer ceramic capacitor including a laminate including a plurality of laminated dielectric layers and a plurality of laminated internal electrode layers, the laminate having first and second main surfaces opposing each other in a height direction, first and second side surfaces opposing each other in a width direction perpendicular to the height direction, and first and second end faces opposing each other in a length direction perpendicular to the height direction and the width direction, and external electrode layers provided on the laminate and connected to some of the internal electrode layers, and the X-ray diffraction intensity of the dielectric layer is measured in the width direction and the height direction. When a cross section of the parallel laminate is measured by X-ray stress measurement, the width direction is defined as an azimuth angle of 0 degrees, the counterclockwise direction is defined as a positive azimuth angle, and the angle of incidence of X-rays from the sample at an azimuth angle of 30 degrees is changed in the direction of the normal to the sample, the diffraction angle at which the X-ray diffraction intensity is maximized is defined as a first peak diffraction angle, and the angle of incidence of X-rays from the sample at an azimuth angle of 90 degrees is changed in the direction of the normal to the sample, the diffraction angle at which the X-ray diffraction intensity is maximized is defined as a second peak diffraction angle, and the difference between the first peak diffraction angle and the second peak diffraction angle is 0.023 degrees or more.

[0093] According to the multilayer ceramic capacitor of the second embodiment, it is possible to provide a multilayer ceramic capacitor having a larger relative dielectric constant.

[0094] The characteristics of the dielectric layer in the multilayer ceramic capacitor 1 of embodiment 2 will be described. (Peak Diffraction Angle) The peak diffraction angle will be described. In the dielectric layer in the multilayer ceramic capacitor 1 of embodiment 2, the peak diffraction angle varies depending on the azimuth angle at which measurement is performed. The peak diffraction angle refers to the diffraction angle at which the X-ray diffraction intensity is maximum.

[0095] The peak diffraction angle can be measured by X-ray stress measurement, as described in Vol. 47, No. 11, pp. 1188-1194, November 1998, of the magazine "Materials" (J. Soc. Mat. Sci., Japan).

[0096] In X-ray stress measurement, a sample is irradiated with X-rays and the diffracted X-rays from the sample are detected. The angle between the direction of the X-rays irradiating the sample and the direction of the diffracted X-rays emerging from the sample is the diffraction angle. The diffraction angle is equivalent to twice the size of the Bragg angle.

[0097] Diffracted X-rays are detected by changing the irradiation angle of the X-rays on the sample. The irradiation angle of the X-rays on the sample can be changed by changing the irradiation direction from the direction normal to the sample surface to a direction parallel to the sample surface. Alternatively, the irradiation angle of the X-rays on the sample can be changed by changing the irradiation direction from the direction parallel to the sample surface to the direction normal to the sample surface.

[0098] While changing the irradiation angle of the X-ray to the sample, BaTiO 3 The irradiation angle at which the intensity of the diffracted X-rays from the (222) crystal plane is maximum is determined. This irradiation angle is the peak diffraction angle.

[0099] The peak diffraction angle can be measured by changing the azimuthal angle. The azimuthal angle is the direction in which the X-ray irradiation angle is changed. In other words, the azimuthal angle is the direction in which the irradiation direction is tilted when changing from the direction normal to the sample surface to a direction parallel to the sample surface.

[0100] The sample used for measuring the peak diffraction angle will now be described. A multilayer ceramic capacitor is polished to expose the surface of the sample. Polishing is performed by scraping the surface parallel to the width direction W and the height direction T. The surface of the sample is the WT cross section at the center position in the length direction T.

[0101] The X-ray irradiation range was a circular area with a diameter of 500 μm in the center of the WT cross section. The inner layer area IL of the laminate 2 was the measurement range.

[0102] The width direction W in the WT cross section is defined as an azimuth angle of 0 degrees. The counterclockwise direction from the width direction W is defined as the positive azimuth angle direction.

[0103] The diffraction angle at which the X-ray diffraction intensity is maximized when the angle of incidence of the X-ray from the sample surface is changed in the direction normal to the sample surface at an azimuth angle of 30 degrees is defined as the first peak diffraction angle, and the diffraction angle at which the X-ray diffraction intensity is maximized when the angle of incidence of the X-ray from the sample surface is changed in the direction normal to the sample surface at an azimuth angle of 90 degrees is defined as the second peak diffraction angle.

[0104] 6A and 6B are diagrams showing the peak diffraction angles of an example of embodiment 2 and a comparative example of embodiment 2. Fig. 6A shows the peak diffraction angle of the example of embodiment 2, and Fig. 6B shows the peak diffraction angle of the comparative example of embodiment 2. Fig. 6A and Fig. 6B show the peak diffraction angle when the azimuth angle is 30 degrees and the peak diffraction angle when the azimuth angle is 90 degrees, respectively.

[0105] 6A and 6B , in the example of embodiment 2, the difference between the first peak diffraction angle and the second peak diffraction angle is 0.023 degrees or more, whereas in the comparative example of embodiment 2, the difference between the first peak diffraction angle and the second peak diffraction angle is less than 0.023 degrees.

[0106] Tables 1 and 2 show the relative dielectric constants of examples of embodiment 2 and comparative examples of embodiment 2. Table 1 shows the case where the number of laminated sheets is 300 and the dielectric layer thickness is 1.0 μm, while Table 2 shows the case where the number of laminated sheets is 410 and the dielectric layer thickness is 0.6 μm. In both cases, the examples of embodiment 2 show high relative dielectric constants exceeding 3800. On the other hand, the comparative examples of embodiment 2 do not have relative dielectric constants exceeding 3800.

[0107] In this way, by making the difference between the first peak diffraction angle and the second peak diffraction angle 0.023 degrees or more, a high relative dielectric constant can be realized.

[0108] The size of the multilayer ceramic capacitors of the example and comparative example of embodiment 2 is 1.0 mm in the length direction L, and 0.5 mm in the width direction W and height direction T. The number of laminated internal electrode layers is 300 or 410, and the thickness of the dielectric layer is 0.60 μm or 1 μm. The thickness of the internal electrode layer is 0.5 μm.

[0109] (Measurement Method) The length and thickness of each part can be measured as follows: The multilayer ceramic capacitor 1 is polished to the center position in the width direction. Then, the cross section exposed by polishing is observed using an optical microscope or the like. Measurements can be made from the observed cross section.

[0110] (1) A multilayer ceramic capacitor comprising: a laminate including a plurality of laminated dielectric layers and a plurality of laminated internal electrode layers, the laminate having first and second main surfaces opposing each other in a height direction, first and second side surfaces opposing each other in a width direction perpendicular to the height direction, and first and second end surfaces opposing each other in a length direction perpendicular to the height and width directions; and external electrode layers provided on the laminate and connected to some of the internal electrode layers, wherein when the X-ray diffraction intensity of the dielectric layer is measured by X-ray stress measurement in a cross section of the laminate parallel to the width and height directions, the width direction is defined as an azimuth angle of 0 degrees, the counterclockwise direction is defined as a positive azimuth angle, and when the angle of incidence of X-rays from a sample is changed in a direction normal to the sample at an azimuth angle of 30 degrees, the diffraction angle at which the X-ray diffraction intensity becomes maximum is defined as a first peak diffraction angle, A multilayer ceramic capacitor in which, when the angle of incidence of an X-ray from a sample is changed in a direction normal to the sample at an azimuth angle of 90 degrees, the diffraction angle at which the X-ray diffraction intensity is maximized is defined as a second peak diffraction angle, and the difference between the first peak diffraction angle and the second peak diffraction angle is 0.023 degrees or more.

[0111] (Embodiment 3) A multilayer ceramic capacitor 1 according to embodiment 3 will be described. In the following description, differences from embodiment 1 will be mainly described. Items that are not specifically described can be the same as embodiment 1.

[0112] The technology described in Patent Document 1 may not sufficiently improve electrical characteristics or reliability. Therefore, an object of the third embodiment is to provide a multilayer ceramic capacitor having a larger relative dielectric constant.

[0113] The multilayer ceramic capacitor of embodiment 3 is a multilayer ceramic capacitor comprising: a laminate including a plurality of laminated dielectric layers and a plurality of laminated internal electrode layers, the laminate having first and second main surfaces opposing each other in a height direction, first side surfaces and second side surfaces opposing each other in a width direction perpendicular to the height direction, and first end surfaces and second end surfaces opposing each other in a length direction perpendicular to the height direction and the width direction; and external electrode layers provided on the laminate and connected to some of the internal electrode layers, wherein when the dielectric layers are observed by high-angle scattering dark-field scanning transmission electron microscopy, a plurality of 100-plane crystal orientations are observed by arranging the optical axis of the microscope in a direction perpendicular to the observation surface and tilting the observation surface by an angle between −20 degrees and +20 degrees from a plane perpendicular to the optical axis.

[0114] According to the multilayer ceramic capacitor of the third embodiment, it is possible to provide a multilayer ceramic capacitor having a larger relative dielectric constant.

[0115] Detection of the (100) crystal orientation plane of the crystal grains in the dielectric layer in the multilayer ceramic capacitor 1 of embodiment 3 will be described. (Crystal orientation (100) plane) In the dielectric layer in the multilayer ceramic capacitor 1 of embodiment 3, the probability of the presence of the (100) crystal orientation plane is high. Hereinafter, the description will be based on observations using high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM).

[0116] 7A to 7G show the cases where the (100) crystal orientation plane was observed by high-angle scattering dark-field scanning transmission electron microscopy, and Fig. 7H shows the case where the (100) crystal orientation plane was not observed. Observation of the observation surface by high-angle scattering dark-field scanning transmission electron microscopy is performed while tilting the observation surface.

[0117] Fig. 8 is a diagram showing the state of observation of an observation surface by high-angle scattering dark-field scanning transmission electron microscopy. In the XYZ orthogonal coordinate system shown in Fig. 8, when the observation surface is arranged on the YZ plane, the electron beam in high-angle scattering dark-field scanning transmission electron microscopy is irradiated from the positive side of the X axis toward the negative side of the X axis, as indicated by the arrow EB.

[0118] The observation surface arranged on the YZ plane can rotate around the Z axis and the Y axis. In Figure 8, rotation around the Z axis is indicated by arrow A, and rotation around the Y axis is indicated by arrow B.

[0119] When rotating around the Z axis, the angle of rotation is defined as angle α. Rotation in the positive direction of the X axis is defined as the positive direction of angle α. When rotating around the Y axis, the angle of rotation is defined as angle β. Rotation in the positive direction of the X axis is defined as the positive direction of angle β.

[0120] Observation using high-angle scattering dark-field scanning transmission electron microscopy was performed on the WT cross section of the multilayer ceramic capacitor at the midpoint in the length direction T. The multilayer ceramic capacitor was polished to expose the WT cross section. Polishing was performed by scraping along the surface parallel to the width direction W and the height direction T.

[0121] In addition, observations using high-angle scattering dark-field scanning transmission electron microscopy were performed using thin-film samples. That is, thin-film samples including a WT cross section at the midpoint of the multilayer ceramic capacitor in the longitudinal direction T were prepared, and the WT cross section of the thin-film sample was observed. The surface of the thin-film sample opposite to the WT cross section to be observed was polished, and the sample was formed to a thickness of 70 μm.

[0122] The observation was carried out on the central part of the crystal grain. In the case of barium titanate, which has a core-shell structure, the core part was the object of observation.

[0123] Figure 7A shows the (100) crystal orientation plane observed by tilting the observation plane by α=1.95° and β=0.27°. Similarly, Figure 7B shows the (100) crystal orientation plane observed by tilting the observation plane by α=9.84° and β=1.87°, Figure 7C shows the (100) crystal orientation plane observed by tilting the observation plane by α=9.06° and β=2.35°, Figure 7D shows the (100) crystal orientation plane observed by tilting the observation plane by α=0.96° and β=−13.75°, Figure 7E shows the (100) crystal orientation plane observed by tilting the observation plane by α=9.21° and β=11.38°, Figure 7F shows the (100) crystal orientation plane observed by tilting the observation plane by α=17.59° and β=10.94°, and Figure 7G shows the (100) crystal orientation plane observed by tilting the observation plane by α=17.59° and β=6.38°.

[0124] In the dielectric layer of the multilayer ceramic capacitor 1 of embodiment 3, by tilting the observation surface at an angle α of −20 degrees or more and +20 degrees or less, and at an angle β of −20 degrees or more and +20 degrees or less, it is possible to observe multiple crystal orientation (100) planes.

[0125] On the other hand, in a conventional multilayer ceramic capacitor, the (100) crystal orientation plane cannot be observed by tilting the observation surface by an angle α of −20 degrees to +20 degrees and an angle β of −20 degrees to +20 degrees. The observation result when the (100) crystal orientation plane is not observed is shown in FIG. 7H.

[0126] In the multilayer ceramic capacitor 1 of embodiment 3, in which the crystal orientation (100) plane can be observed by tilting the observation surface at an angle α of −20 degrees or more and +20 degrees or less, and at an angle β of −20 degrees or more and +20 degrees or less, a higher dielectric constant was achieved than in conventional multilayer ceramic capacitors.

[0127] 7A to 7G show the results of observation of the central portion of the crystal grains. In the multilayer ceramic capacitor 1 of embodiment 3, the crystal orientation (100) plane was observed in the central portion of the crystal grain where the crystal orientation (100) plane is difficult to observe.

[0128] Furthermore, in the multilayer ceramic capacitor 1 of embodiment 3, the above-described crystal orientation (100) planes are observed in both of two adjacent crystal grains. As described above, in the multilayer ceramic capacitor 1 of embodiment 3, the crystal orientation (100) planes are present accurately without distortion and with a high probability.

[0129] (Measurement Method) The length and thickness of each part can be measured as follows: The multilayer ceramic capacitor 1 is polished to the center position in the width direction. Then, the cross section exposed by polishing is observed using an optical microscope or the like. Measurements can be made from the observed cross section.

[0130] (1) A multilayer ceramic capacitor comprising: a laminate including a plurality of laminated dielectric layers and a plurality of laminated internal electrode layers, the laminate having first and second main surfaces opposing each other in a height direction, first and second side surfaces opposing each other in a width direction perpendicular to the height direction, and first and second end faces opposing each other in a length direction perpendicular to the height direction and the width direction; and external electrode layers provided on the laminate and connected to some of the internal electrode layers, wherein, when the dielectric layers are observed by high-angle scattering dark-field scanning transmission electron microscopy, a plurality of 100-plane crystal orientations are observed by arranging the optical axis of the microscope in a direction perpendicular to the observation surface and tilting the observation surface by an angle between -20 degrees and +20 degrees from a plane perpendicular to the optical axis.

[0131] (2) The multilayer ceramic capacitor according to (1), wherein the observation is performed by observing the center of a crystal grain contained in the dielectric layer.

[0132] (3) The multilayer ceramic capacitor according to (2), wherein the (100) plane is observed in both adjacent crystal grains.

[0133] (Embodiment 4) A multilayer ceramic capacitor 1 according to embodiment 4 will be described. In the following description, differences from embodiment 1 will be mainly described. Items that are not specifically described can be the same as embodiment 1.

[0134] The technology described in Patent Document 1 may not sufficiently improve electrical characteristics or reliability. Therefore, an object of the fourth embodiment is to provide a multilayer ceramic capacitor having a larger relative dielectric constant.

[0135] A multilayer ceramic capacitor according to a fourth embodiment is a multilayer ceramic capacitor comprising: a laminate including a plurality of laminated dielectric layers and a plurality of laminated internal electrode layers, the laminate having first and second main surfaces opposing each other in a height direction, first and second side surfaces opposing each other in a width direction perpendicular to the height direction, and first and second end surfaces opposing each other in a length direction perpendicular to the height direction and the width direction; and external electrode layers provided on the laminate and connected to some of the internal electrode layers, wherein the first average grain size is a median diameter of crystal grains in the dielectric layers determined by observation with a scanning transmission electron microscope, the crystal orientations of the crystal grains in the dielectric layers are measured by electron backscatter diffraction, and a value of the second average grain size / the first average grain size is 1.0 or more.

[0136] According to the multilayer ceramic capacitor of the fourth embodiment, it is possible to provide a multilayer ceramic capacitor having a larger relative dielectric constant.

[0137] (Grain size) A description will be given of the grain size of the crystal grains in the dielectric layer of the multilayer ceramic capacitor 1 of embodiment 4. In the dielectric layer of the multilayer ceramic capacitor 1 of embodiment 4, when the grain size determined based on observation with a scanning transmission electron microscope is compared with the grain size determined based on a crystal orientation map of transmission EBSD, the grain size is either the same or larger.

[0138] Here, the particle size of the crystal particles refers to the median diameter in the area particle size distribution. The median diameter is also called d50.

[0139] When determining the grain size based on the crystal orientation map of transmission EBSD, the crystal orientation of the crystal grains of the dielectric layer is first measured by electron backscatter diffraction. Two adjacent crystal grains are considered to be a single grain if the difference between their crystal orientations is within 5 degrees of an arbitrary direction. Therefore, the more adjacent crystal grains there are that have a difference between their crystal orientations within 5 degrees of an arbitrary direction, the larger the grain size determined based on the crystal orientation map of transmission EBSD.

[0140] Table 3 shows the cooling time after firing of the multilayer ceramic capacitor, as well as the grain size and dielectric constant. The median diameter of the crystal grains in the dielectric layer determined based on observation with a scanning transmission electron microscope is defined as the first average grain size. The crystal orientation is measured by electron backscatter diffraction, and the median diameter of the crystal grains when the deviation angle between the crystal orientations of two adjacent grains is within 5 degrees relative to an arbitrary direction is considered to be one crystal grain is defined as the second average grain size.

[0141] Table 3 shows the first average particle size and the second average particle size, as well as the value of the dielectric constant / first average particle size. The value of the dielectric constant / first average particle size indicates the dielectric constant per particle size, and the larger this value, the more preferable the electrical properties. In samples in which the ratio of the second average particle size / first average particle size is 1 or more, the value of the dielectric constant / first average particle size is 13 or more. In other words, these samples exhibited preferable electrical properties.

[0142] The measurements shown in Table 3 were performed on the WT cross section at the midpoint of the length direction T of the multilayer ceramic capacitor. The multilayer ceramic capacitor was polished to expose the WT cross section. The polishing was performed by scraping the surface parallel to the width direction W and the height direction T.

[0143] Measurements using electron backscatter diffraction to obtain a crystal orientation map of the transmission EBSD were performed using a thin specimen. The WT cross section of the multilayer ceramic capacitor at the midpoint in the longitudinal direction T was processed into a thin specimen and then measured. Specifically, the surface opposite to the measurement surface was polished to a thickness of 100 nm, and the WT cross section was then measured.

[0144] The grain size was evaluated in the central part of this WT cross section. The size of the evaluation object was set to 2 μm square. With electron backscatter diffraction, accurate values ​​may not be obtained in areas where multiple crystal grains overlap in the direction perpendicular to the measurement surface. If a high proportion of such areas where accurate values ​​cannot be obtained are included within the range of the evaluation object, accurate evaluation becomes difficult. Therefore, the size of the evaluation object was set to 2 μm square.

[0145] (Measurement Method) The length and thickness of each part can be measured as follows: The multilayer ceramic capacitor 1 is polished to the center position in the width direction. Then, the cross section exposed by polishing is observed using an optical microscope or the like. Measurements can be made from the observed cross section.

[0146] (1) A multilayer ceramic capacitor comprising: a laminate including a plurality of laminated dielectric layers and a plurality of laminated internal electrode layers, the laminate having first and second main surfaces opposing each other in a height direction, first and second side surfaces opposing each other in a width direction perpendicular to the height direction, and first and second end surfaces opposing each other in a length direction perpendicular to the height direction and the width direction; and external electrode layers provided on the laminate and connected to some of the internal electrode layers, wherein a first average grain size is defined as a median diameter of crystal grains in the dielectric layers determined by observation with a scanning transmission electron microscope, and a second average grain size is defined as a median diameter of crystal grains when the crystal orientations of the crystal grains in the dielectric layers are measured by electron backscatter diffraction, and a crystal grain whose deviation angle between the crystal orientations of two adjacent crystal grains is within 5 degrees relative to an arbitrary direction is considered to be one crystal grain, and the value of the second average grain size / the first average grain size is 1.0 or more.

[0147] Although the embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments and various changes and modifications are possible.

[0148] REFERENCE SIGNS LIST 1 Multilayer ceramic capacitor 2 Laminate 3 Outer dielectric layer 4 Inner dielectric layer 5a First dielectric layer 5b Second dielectric layer 6a First internal electrode layer 6b Second internal electrode layer 20a First external electrode 20b Second external electrode C Crystal grain

Claims

1. A multilayer ceramic capacitor comprising: a laminate including a plurality of laminated dielectric layers and a plurality of laminated internal electrode layers, the laminate having a first main surface and a second main surface opposing each other in a height direction, a first side surface and a second side surface opposing each other in a width direction perpendicular to the height direction, and a first end surface and a second end surface opposing each other in a length direction perpendicular to the height direction and the width direction; and an external electrode layer provided on the laminate and connected to some of the internal electrode layers, wherein, when the crystal orientation of the crystal grains of the dielectric layer is measured by electron backscatter diffraction method, within an observation area of ​​2 μm square, there are two or more pairs of crystal grains in which the difference in crystal orientation between two adjacent crystal grains is within 5 degrees based on any direction.

2. The multilayer ceramic capacitor according to claim 1, wherein there are 20 or more pairs of crystal grains in which the difference in crystal orientation between two adjacent crystal grains is within 5 degrees relative to an arbitrary direction.

3. A multilayer ceramic capacitor according to claim 1 or 2, comprising at least one group of three crystal grains, each group including one crystal grain and two crystal grains adjacent to the crystal grain and having a deviation angle of 5 degrees or less between the crystal grain and the crystal grain.

4. The multilayer ceramic capacitor according to claim 1 or 2, wherein 50 to 250 crystal grains are observed within the observation area.

5. A multilayer ceramic capacitor comprising: a laminate including a plurality of laminated dielectric layers and a plurality of laminated internal electrode layers, the laminate having a first main surface and a second main surface opposing each other in a height direction, a first side surface and a second side surface opposing each other in a width direction perpendicular to the height direction, and a first end surface and a second end surface opposing each other in a length direction perpendicular to the height direction and the width direction; and an external electrode layer provided on the laminate and connected to some of the internal electrode layers, wherein, when the crystal orientation of the crystal grains of the dielectric layers is measured by electron backscatter diffraction method, crystal grains in contact with other crystal grains whose crystal orientation difference is within 5 degrees based on an arbitrary direction account for 2% or more of all crystal grains.

6. The multilayer ceramic capacitor according to claim 5, wherein crystal grains in contact with other crystal grains, the difference in crystal orientation being within 5 degrees of any direction as the reference, account for 20% or more of all crystal grains.

7. A multilayer ceramic capacitor comprising: a laminate including a plurality of laminated dielectric layers and a plurality of laminated internal electrode layers, the laminate having a first main surface and a second main surface opposing each other in a height direction, a first side surface and a second side surface opposing each other in a width direction perpendicular to the height direction, and a first end surface and a second end surface opposing each other in a length direction perpendicular to the height direction and the width direction; and an external electrode layer provided on the laminate and connected to some of the internal electrode layers, wherein a first average grain size is a median diameter of crystal grains in the dielectric layers determined by observation with a scanning transmission electron microscope, and a second average grain size is a median diameter of crystal grains when the crystal orientations of the crystal grains in the dielectric layers are measured by electron backscatter diffraction method, and a crystal grain in which the deviation angle between the crystal orientations of two adjacent crystal grains is within 5 degrees with respect to an arbitrary direction is regarded as one crystal grain, and the value of the second average grain size / the first average grain size is 1.0 or more.

Citation Information

Patent Citations

  • Capacitive element and resonant circuit

    JP2014045008A

  • Multilayer ceramic capacitor

    JP2017228590A

  • Dielectric ceramic composition, multilayer ceramic capacitor containing the same, and manufacturing method of multilayer ceramic capacitor

    JP2021169404A

  • Multilayer ceramic capacitor

    JP2022143403A