Thiol compound
The novel multifunctional thiol compound addresses the adhesion issue in epoxy resin curing by providing high elongation, low elasticity, and tack-free performance, enhancing the curing efficiency and properties of the resin for diverse applications.
Patent Information
- Application Number
- PCT/JP2024/011676
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Existing thiol compounds used for curing epoxy resins often result in cured products that are prone to adhesion, lacking tack-free performance and exhibiting low elongation and high elasticity, which is undesirable for practical applications.
A novel multifunctional thiol compound with a specific structural formula, featuring phenyl or naphthalene rings and multiple thiol groups, is developed to provide high elongation, low elasticity, and tack-free performance as a curing agent for epoxy resins, addressing the adhesion issue and enhancing the properties of the cured resin.
The novel thiol compound enables rapid curing of epoxy resins with excellent tack-free performance, high impact resistance, and improved hydrolysis resistance, making it suitable for various applications including adhesives and coatings.
Smart Images

Figure JPOXMLDOC01-APPB-I000001 
Figure JPOXMLDOC01-APPB-I000002 
Figure JPOXMLDOC01-APPB-I000003
Abstract
Description
thiol compounds
[0001] The present invention relates to a novel thiol compound used for curing epoxy resins, etc. More specifically, the novel thiol compound can be used as a curing agent for epoxy resins.
[0002] Compositions using compounds containing thiol groups (also known as sulfanyl groups or mercapto groups, or -SH groups) as curing agents for epoxy resins have been extensively studied due to their excellent low-temperature curing properties. In particular, various studies have been conducted on compounds containing multiple thiol groups in the molecule (Patent Documents 1 to 3).
[0003] JP 2012-153794 A JP 2016-164134 A International Publication No. 2014 / 084292 Pamphlet
[0004] Generally, when curing an epoxy resin, the use of a bifunctional thiol compound with a long molecular chain can produce a cured product with high elongation, low elasticity, and excellent impact resistance. However, when a finger or other object touches the surface of a cured product after curing has progressed, uncured cured material may adhere to the finger or other object, affecting the surface condition of the cured product. Therefore, there has been a demand for a thiol compound that does not adhere to fingers or other objects, that is, has so-called tack-free properties, and can exhibit high elongation and low elasticity.
[0005] The present inventors have conducted extensive research to solve the above-mentioned problems. As a result, the present inventors have discovered that a compound having a specific thiol group is a polyfunctional thiol compound that exhibits high elongation and low elasticity, yet is effective as a curing agent that gives a cured resin product with good tack-free properties, and have arrived at the present invention. That is, the present invention can include the following aspects.
[0006] [1] General formula (I): (In formula (I), each ring P is independently a phenyl group or a naphthalene group; when ring P is a phenyl group, 1 to 5 As are present for each ring P; when ring P is a naphthalene group, 1 to 7 As are present for each ring P; each As is independently -R1-SH; each R1 is independently a C1 to C6 alkylene group optionally substituted with one or more Ys; B is a substituent on ring P other than A, and each is independently a hydrogen atom, a C1 to C6 alkyl group optionally substituted with one or more Ys, or a C1 to C6 alkoxy group optionally substituted with one or more Ys; when ring P is a phenyl group, A and B are independently at the ortho-position, meta-position, or para-position relative to the position where ring P is bonded to the main chain. each R2 is independently a hydrogen atom, a C1 to C6 alkyl group optionally substituted with one or more Y's, or a C1 to C6 alkoxy group optionally substituted with one or more Y's; each Y is independently a hydrogen atom, a C1 to C6 alkyl group, or a C1 to C6 alkoxy group; each Z is independently a direct bond, -CH2-, -O-, or -S-; and n is an integer of 1 to 20. [2] The compound according to the above [1], wherein ring P is a phenyl group, one A is present in each ring P, and each A is independently bonded to the ortho-position or para-position relative to the position where ring P is bonded to the main chain. [3] The compound according to the above [1], wherein ring P is a phenyl group, one A is present in each ring P, R1 is a linear C2-C3 alkylene group, all B's are hydrogen atoms, X is -O-, Y is a hydrogen atom, Z is a direct bond or -O-, and n is an integer of 2 to 5. [4] The compound according to the above [1], wherein ring P is a phenyl group, R1 is a linear C2-C3 alkylene group, one A is present for each ring P, one of B present in each ring P is a methyl group, a methoxy group, or a phenyl group, all other B present in each ring P are hydrogen atoms, X is -O-, Y is a hydrogen atom, Z is a direct bond or -O-, and n is an integer of 2 to 5.[5] The compound shown below. , , , , or [6] An epoxy resin composition containing an epoxy resin and the compound described in any one of [1] to [5]. [7] An epoxy resin curing agent containing the compound described in any one of [1] to [5]. [8] A cured epoxy resin obtained by thermally curing an epoxy resin and the compound described in any one of [1] to [5].
[0007] The present invention provides an epoxy resin curing agent that can exhibit high elongation and low elasticity while providing a cured product with good tack-free properties. By using the compound having a thiol group of the present invention, the curing of the epoxy resin proceeds rapidly, and a cured epoxy resin with good tack-free properties can be provided.
[0008] NMR data of thiol compound (1) prepared in Example 1. NMR data of thiol compound (3) prepared in Example 3.
[0009] Here, the embodiments for carrying out the invention will be described in detail, but the preferred and more preferred embodiments exemplified below can be used in appropriate combination with each other regardless of expressions such as "preferable" or "more preferred." Furthermore, the descriptions of numerical ranges are merely examples, and ranges obtained by appropriately combining the upper and lower limits of each range and the numerical values of the examples can also be preferably used. Furthermore, terms such as "contain" or "comprise" may be read as "essentially consisting of" or "consisting only of."
[0010] [Thiol Compound] One embodiment of the present invention is a thiol compound represented by the following general formula (I).
[0011] In formula (I), each ring P is independently a phenyl group or a naphthalene group, preferably a phenyl group. When ring P is a phenyl group, there are 1 to 5, preferably 1 to 3, more preferably 1 to 2, and even more preferably 1 As for each ring P. When ring P is a naphthalene group, there are 1 to 7, preferably 1 to 5, more preferably 1 to 3, and even more preferably 1 to 2 As for each ring P. Each As is independently -R1-SH, and each R1 is independently a C1 to C6 alkylene group optionally substituted with one or more Ys. R1 is preferably an unsubstituted C2-C5 alkylene group, more preferably an unsubstituted C2-C3 alkylene group. The alkylene group may be linear or branched, saturated or unsaturated, and may or may not be further substituted with Y. The definition of Y is as described below.
[0012] B is a substituent other than A on ring P. Therefore, the total number of substituents A and B on one ring P is 5 when ring P is a phenyl group, and 7 when ring P is a naphthalene group. The number of substituents A and B on one ring P is, for example, 1 to 2 A for each ring P and 0 to 2 B other than hydrogen atoms, more preferably 1 A for each ring P and 0 to 1 B other than hydrogen atoms. Each B is independently a hydrogen atom, a C1 to C6 alkyl group optionally substituted with one or more Y, or a C1 to C6 alkoxy group optionally substituted with one or more Y. The definition of Y is as described below. Preferably, each B is independently a hydrogen atom, an unsubstituted C1 to C3 alkyl group, or an unsubstituted C1 to C3 alkoxy group, more preferably, each B is independently a hydrogen atom, a methyl group, or a methoxy group, and even more preferably, B is a hydrogen atom. In another embodiment, one or two of B present in each ring P may be a methyl group, a methoxy group, or a phenyl group, and all other B present in each ring P may be hydrogen atoms. When ring P is a phenyl group, 0 to 4, preferably 0 to 3, more preferably 1 to 2 B for each ring P may be other than a hydrogen atom. When ring P is a naphthalene group, 0 to 6, preferably 0 to 5, more preferably 1 to 3, even more preferably 1 to 2 B for each ring P may be other than a hydrogen atom.
[0013] When ring P is a phenyl group, A and B may each independently be bonded at the ortho, meta, or para position relative to the position where ring P is bonded to the main chain. Preferably, A and B may each independently be bonded at the ortho or para position relative to the position where ring P is bonded to the main chain. In a more preferred embodiment, there is one A on ring P, and one or no B other than a hydrogen atom is present on ring P, and A is bonded at the ortho or para position relative to the position where ring P is bonded to the main chain, and when a B other than a hydrogen atom is present, B is suitably bonded at the ortho position relative to the position where ring P is bonded to the main chain. On the other hand, when ring P is a naphthalene group, A and B may each independently be bonded at the ortho, meta, para, ana, epi, cata, peri, pros, amphi, or 2,7 position relative to the position where ring P is bonded to the main chain. Preferably, A and B may each independently be bonded to the ana-position, epi-position, cata-position, peri-position, amphi-position, or 2,7-position relative to the position where ring P is bonded to the main chain. In a more preferred embodiment, there is one A on ring P, and one or no B other than a hydrogen atom is present on ring P, and A is bonded to the amphi-position or 2,7-position relative to the position where ring P is bonded to the main chain. Furthermore, when a B other than a hydrogen atom is present, B is bonded to the amphi-position or 2,7-position relative to the position where ring P is bonded to the main chain. Each X is independently -CH2-, -O-, -N(-R2)-, or -S-. Here, each R2 is independently a hydrogen atom, a C1-C6 alkyl group optionally substituted with one or more Ys, or a C1-C6 alkoxy group optionally substituted with one or more Ys. R2 is preferably an unsubstituted C2-C5 alkylene group, more preferably an unsubstituted C2-C3 alkylene group. The alkylene group may be linear or branched, saturated or unsaturated, and may be substituted or unsubstituted with Y. The definition of Y is as described below. X is preferably -CH2- or -O-, more preferably -O-. Each Y is independently a hydrogen atom, a C1-C6 alkyl group, or a C1-C6 alkoxy group. Y is preferably a hydrogen atom, a methyl group, or an ethyl group, more preferably a hydrogen atom.Each Z is independently a direct bond, -CH-, -C2H4-, -C3H6-, -C4H8-, -O-, or -S-. Z is preferably a direct bond or -O-, more preferably a direct bond. n is, for example, an integer of 1 to 20, preferably an integer of 1 to 10, more preferably an integer of 2 to 5 or 1 to 3.
[0014] More specific embodiments of the thiol compound of the present invention include the following thiol compounds (1) to (5) and (5)'. Thiol Compound (1)
[0015] Thiol Compound (2)
[0016] Thiol Compound (3)
[0017] Thiol Compound (4)
[0018] Thiol Compound (5) Thiol compound (5)'
[0019] [Method for Preparing Thiol Compound] The thiol compound can be produced by known methods, but can also be prepared, for example, as follows. The following describes the thiol compound (1) as an example. First, 2-allylphenol and 1,4-dibromobutane are used as starting materials, and tetra-n-butylammonium bromide as a phase transfer catalyst and methyl isobutyl ketone (MIBK) as a reaction solvent are added. Dissolution is carried out, for example, at 50 to 200°C, preferably 60 to 150°C, and more preferably 100°C ± 10 to 20°C, for example, for 1 minute to 12 hours, preferably 10 minutes to 5 hours, and more preferably 30 minutes ± 10 to 20 minutes. A base such as an aqueous KOH solution is added to the resulting solution, and the reaction is continued for 1 to 24 hours, preferably 2 to 10 hours, and more preferably 6 hours ± 1 hour, while only MIBK is returned to the system and water is distilled off at a temperature in the range of 100 to 150°C, preferably 110 to 120°C. The temperature is then lowered to about 60°C, distilled water is added, the mixture is allowed to stand, and the lower by-product brine layer is discarded. Further distilled water and a base (such as sodium dihydrogen phosphate in an amount appropriate for neutralization) are added, and the mixture is allowed to stand and separated, and the lower by-product brine layer is discarded. The mixture is then washed and purified with an equal amount of distilled water 1 to 5 times, preferably 2 to 3 times, and then heated to, for example, 50 to 200°C, preferably 60 to 150°C, and more preferably 120°C ± 10 to 20°C for azeotropic dehydration. The resulting solution is microfiltered to remove impurities, and the MIBK and unreacted 2-allylphenol are distilled under reduced pressure to obtain a liquid resin. The resulting liquid resin, thioacetic acid, toluene, and azobisisobutyronitrile (AIBN) are mixed and reacted, for example, at 50 to 200°C, preferably 60 to 150°C, and more preferably 80°C ± 10 to 20°C, for 30 minutes to 24 hours, preferably 1 to 10 hours, and more preferably 4 hours ± 1 to 2 hours. After removing the toluene from the resulting reaction product, crystallization is carried out using methanol, and the crystallized product is dried and recovered. The recovered dried crystallized product is mixed with a base such as NaOH and reacted, for example, at 50 to 200°C, preferably 60 to 150°C, and more preferably 80°C ± 10 to 20°C, for 30 minutes to 12 hours, preferably 1 to 5 hours, and more preferably 2 hours ± 1 hour. The reaction product is neutralized with an acid such as hydrochloric acid, and the organic layer is separated and washed with water. The toluene is removed from the washed organic layer to obtain the desired thiol compound.
[0020] [Uses of Thiol Compounds] The thiol compounds described above are polyfunctional thiol compounds with long molecular chains and two or more thiol groups. When used as curing agents for epoxy resins, they can produce cured products with high elongation, low elasticity, and excellent impact resistance. Furthermore, these thiol compounds are useful as curing agents for epoxy resins because they exhibit excellent low-temperature curing properties and superior hydrolysis resistance compared to other thiol compounds containing ester groups. Furthermore, these thiol compounds can also be used as crosslinkers or curing aids for compounds containing carbon-carbon double bonds (ene compounds). The reaction between a thiol compound and a carbon-carbon double bond is known as the thiol-ene reaction, and these thiol compounds can be used in the reaction (thiol-ene reaction) between the thiol compound and resins containing carbon-carbon double bonds, such as (meth)acrylate compounds, allyl compounds, vinyl compounds, unsaturated polyesters, and polybutadiene. By using the thiol compound as a crosslinking agent or curing aid, the thiol compound is less susceptible to oxygen inhibition during the reaction and has excellent reactivity with compounds having a carbon-carbon double bond, allowing the crosslinking of compounds having a carbon-carbon double bond to proceed quickly. Note that, in each application, the thiol compound of the present invention may be used alone or in combination of multiple types.
[0021] [Epoxy Resin Composition] One aspect of the present invention is an epoxy resin composition containing an epoxy resin and the above-described thiol compound. Examples of epoxy resins include epoxy resin compounds having, on average, two or more epoxy groups per molecule. Examples of epoxy resins include polyglycidyl ethers obtained by reacting epichlorohydrin with polyhydric phenols such as bisphenol A, bisphenol F, bisphenol AD, catechol, and resorcinol, or polyhydric alcohols such as glycerin and polyethylene glycol; polyglycidyl ether esters obtained by reacting epichlorohydrin with hydroxy acids such as p-hydroxybenzoic acid and β-hydroxynaphthoic acid; polyglycidyl esters obtained by reacting epichlorohydrin with polycarboxylic acids such as phthalic acid and terephthalic acid; and epoxidized phenol novolac resins, epoxidized cresol novolac resins, epoxidized polyolefins, alicyclic epoxy resins, and other urethane-modified epoxy resins. From the viewpoint of maintaining high heat resistance and low moisture permeability, preferred epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, phenol novolac type epoxy resins, biphenyl aralkyl type epoxy resins, phenol aralkyl type epoxy resins, aromatic glycidylamine type epoxy resins, and epoxy resins having a dicyclopentadiene structure, with bisphenol A type epoxy resins and bisphenol F type epoxy resins being more preferred, and bisphenol A type epoxy resins being even more preferred.
[0022] The epoxy resin may be liquid or solid. The epoxy resin used herein may be a mixture of liquid and solid epoxy resins. Here, "liquid" and "solid" refer to the state of the epoxy resin at room temperature (25°C). Specific examples of liquid epoxy resins include liquid bisphenol A epoxy resins ("jER (registered trademark) Epoxy Resin 828" and "jER (registered trademark) Epoxy Resin 827" manufactured by Mitsubishi Chemical Corporation), liquid bisphenol F epoxy resins ("jER (registered trademark) Epoxy Resin 807" manufactured by Mitsubishi Chemical Corporation), naphthalene-type bifunctional epoxy resins ("HP4032" and "HP4032D" manufactured by DIC Corporation), liquid bisphenol AF epoxy resins ("ZX1 O59" manufactured by Nippon Steel Epoxy Manufacturing Co., Ltd.), and hydrogenated epoxy resins ("jER (registered trademark) Epoxy Resin YX8000" manufactured by Mitsubishi Chemical Corporation). Among these, "jER (registered trademark) Epoxy Resin 828," "jER (registered trademark) Epoxy Resin 827," and "jER (registered trademark) Epoxy Resin 807," manufactured by Mitsubishi Chemical Corporation, which have high heat resistance and low viscosity, are preferred, with "jER (registered trademark) Epoxy Resin 828" being more preferred. Specific examples of solid epoxy resins include naphthalene-type tetrafunctional epoxy resins ("HP4700" manufactured by DIC Corporation), dicyclopentadiene-type multifunctional epoxy resins ("HP7200" manufactured by DIC Corporation), naphthol-type epoxy resins ("ESN-475V" manufactured by Nippon Steel Epoxy Manufacturing Co., Ltd. (Tohto Kasei Co., Ltd.)), epoxy resins having a butadiene structure ("PB-3600" manufactured by Daicel Corporation), and epoxy resins having a biphenyl structure ("NC3000H" and "NC3000L" manufactured by Nippon Kayaku Co., Ltd., and "YX4000" manufactured by Mitsubishi Chemical Corporation).
[0023] From the viewpoints of coatability, processability, and adhesion, it is preferable that at least 10% by mass of the total epoxy resin used be a liquid epoxy resin, more preferably 30% by mass or more, and even more preferably 50% by mass or more. In the epoxy resin composition of the present invention, the content of the thiol compound of the present invention per 100 parts by mass of epoxy resin varies depending on the number of thiol groups. For example, when the thiol compound of the present invention is a bifunctional thiol compound having two thiol groups (thiol equivalent = 2), it is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, even more preferably 20 parts by mass or more, even more preferably 30 parts by mass or more, particularly preferably 40 parts by mass or more, and especially preferably 50 parts by mass or more. Furthermore, the content of the thiol compound of the present invention per 100 parts by mass of the epoxy resin of the present invention is preferably 300 parts by mass or less, more preferably 250 parts by mass or less, even more preferably 225 parts by mass or less, even more preferably 200 parts by mass or less, especially preferably 180 parts by mass or less, and especially preferably 170 parts by mass or less. The preferred content of the thiol compound of the present invention may be within a range selected from the upper limit, the lower limit, and any of the values in the examples. When the number of thiol groups contained in the thiol compound of the present invention is greater than 2, the content may be proportional to the above content or the thiol equivalent. That is, for example, when the number of thiol groups is 4 (thiol equivalent = 4), the above "preferably 5 parts by mass or more" may be read as "preferably 2.5 parts by mass or more," and "preferably 300 parts by mass or less" may be read as "preferably 150 parts by mass or less."
[0024] Other components that can be added to the epoxy resin composition of the present invention include curing accelerators, solvents, storage stabilizers, other curing agents, thixotropy-imparting agents, fillers, diluents, dispersants, flexibility-imparting agents, coupling agents, antioxidants, etc. Examples of curing accelerators include latent curing accelerators. A latent curing accelerator is a compound that is insoluble in epoxy resins at room temperature (25°C) but becomes soluble upon heating and functions as a curing accelerator for the epoxy resin. Examples include, but are not limited to, imidazole compounds that are solid at room temperature (25°C) and amine adduct latent curing accelerators. Of these, amine adduct latent curing accelerators are preferred. Examples of amine adduct latent curing accelerators include reaction products of amine compounds and epoxy compounds (amine-epoxy adduct latent curing accelerators) and reaction products of amine compounds and isocyanate compounds (amine-isocyanate latent curing accelerators).
[0025] Examples of the imidazole compound that is solid at room temperature (25° C.) include 2-heptadecylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-undecylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-phenyl-4-benzyl-5-hydroxymethylimidazole, 2,4-diamino-6-(2-methylimidazolyl-(1))-ethyl-S-triazine, 2,4-diamino-6- Examples include (2'-methylimidazolyl-(1)')-ethyl-S-triazine isocyanuric acid adduct, 2-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazole trimellitate, and N-(2-methylimidazolyl-1-ethyl)-urea.
[0026] Examples of epoxy compounds used as one of the raw materials for producing the amine-epoxy adduct latent curing accelerator include polyglycidyl ethers obtained by reacting epichlorohydrin with polyhydric phenols such as bisphenol A, bisphenol F, catechol, and resorcinol, or polyhydric alcohols such as glycerin and polyethylene glycol; glycidyl ether esters obtained by reacting epichlorohydrin with hydroxy acids such as p-hydroxybenzoic acid and β-hydroxynaphthoic acid; polyglycidyl esters obtained by reacting epichlorohydrin with polycarboxylic acids such as phthalic acid and terephthalic acid; glycidyl amine compounds obtained by reacting epichlorohydrin with 4,4'-diaminodiphenylmethane or m-aminophenol; and polyfunctional epoxy compounds such as epoxidized phenol novolac resins, epoxidized cresol novolac resins, and epoxidized polyolefins; and monofunctional epoxy compounds such as butyl glycidyl ether, phenyl glycidyl ether, and glycidyl methacrylate.
[0027] The amine compound used as a raw material for producing the amine adduct latent curing accelerator may be any compound having one or more active hydrogen atoms in the molecule capable of addition reacting with an epoxy group or an isocyanate group (also known as an isocyanato group) and one or more amino groups (at least one of a primary amino group, a secondary amino group, and a tertiary amino group) in the molecule. Examples of such amine compounds include aliphatic amine compounds such as diethylenetriamine, triethylenetetramine, propylamine, 2-hydroxyethylaminopropylamine, cyclohexylamine, and 4,4'-diamino-dicyclohexylmethane; aromatic amine compounds such as 4,4'-diaminodiphenylmethane and 2-methylaniline; and nitrogen-containing heterocyclic compounds such as 2-ethyl-4-methylimidazole, 2-ethyl-4-methylimidazoline, 2,4-dimethylimidazoline, piperidine, and piperazine.
[0028] Furthermore, among the above-mentioned raw materials, if a compound having a tertiary amino group in the molecule is used, a latent curing accelerator having excellent curing acceleration ability can be produced. Examples of the compound having a tertiary amino group in the molecule include amines having a tertiary amino group in the molecule, such as dimethylaminopropylamine, diethylaminopropylamine, dipropylaminopropylamine, dibutylaminopropylamine, dimethylaminoethylamine, diethylaminoethylamine, N-methylpiperazine, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, and 2-phenylimidazole; 2-dimethylaminoethanol, 1-methyl-2-dimethylaminoethanol, 1-phenoxymethyl-2-dimethylaminoethanol, 2-diethylaminoethanol, 1-butoxymethyl-2-dimethylaminoethanol, 1-(2-hydroxy-3-phenoxypropyl)-2-methylimidazole, 1-(2-hydroxy-3-phenoxypropyl)-2-ethyl-4-methylimidazole, 1-(2-hydroxy-3-butoxypropyl)-2 ... 1-(2-hydroxy-3-phenoxypropyl)-2-phenylimidazoline, 1-(2-hydroxy-3-butoxypropyl)-2-methylimidazoline, 2-(dimethylaminomethyl)phenol, 2,4,6-tris(dimethylaminomethyl)phenol, N-β-hydroxyethylmorpholine, 2-dimethylaminoethanethiol, 2-mercaptopyridine, 2-benzimidazole, 2-methyl and alcohols, phenols, thiols, carboxylic acids and hydrazides having a tertiary amino group in the molecule such as mercaptobenzimidazole, 2-mercaptobenzothiazole, 4-mercaptopyridine, N,N-dimethylaminobenzoic acid, N,N-dimethylglycine, nicotinic acid, isonicotinic acid, picolinic acid, N,N-dimethylglycine hydrazide, N,N-dimethylpropionic acid hydrazide, nicotinic acid hydrazide and isonicotinic acid hydrazide.
[0029] When the epoxy compound and the amine compound are subjected to an addition reaction to produce the amine adduct-based latent curing accelerator, an active hydrogen compound having two or more active hydrogen atoms in the molecule can also be added. Examples of such active hydrogen compounds include polyhydric phenols such as bisphenol A, bisphenol F, bisphenol S, hydroquinone, catechol, resorcinol, pyrogallol, and phenol novolac resin, polyhydric alcohols such as trimethylolpropane, polycarboxylic acids such as adipic acid and phthalic acid, 1,2-dimercaptoethane, 2-mercaptoethanol, 1-mercapto-3-phenoxy-2-propanol, mercaptoacetic acid, anthranilic acid, and lactic acid.
[0030] Examples of the isocyanate compound used as a raw material for producing the amine adduct-based latent curing accelerator include monofunctional isocyanate compounds such as butyl isocyanate, isopropyl isocyanate, phenyl isocyanate, and benzyl isocyanate; polyfunctional isocyanate compounds such as hexamethylene diisocyanate, tolylene diisocyanate (e.g., 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate), 1,5-naphthalene diisocyanate, diphenylmethane-4,4'-diisocyanate, isophorone diisocyanate, xylylene diisocyanate, paraphenylene diisocyanate, 1,3,6-hexamethylene triisocyanate, and bicycloheptane triisocyanate; and terminal isocyanate group-containing compounds obtained by reacting these polyfunctional isocyanate compounds with active hydrogen compounds. Examples of such a terminal isocyanate group-containing compound include an addition compound having a terminal isocyanate group obtained by reacting tolylene diisocyanate with trimethylolpropane, and an addition compound having a terminal isocyanate group obtained by reacting tolylene diisocyanate with pentaerythritol.
[0031] The curing accelerator can be easily obtained, for example, by appropriately mixing the above-mentioned production raw materials, reacting them at room temperature (25°C) to 200°C, cooling them to solidify them, and then pulverizing them; or by reacting the above-mentioned production raw materials in a solvent such as methyl ethyl ketone, dioxane, or tetrahydrofuran, removing the solvent, and then pulverizing the solid content.
[0032] The curing accelerator may be a commercially available product. Examples of amine-epoxy adduct latent curing accelerators include "Amicure (registered trademark) PN-23" (Ajinomoto Fine-Techno Co., Ltd.), "Amicure (registered trademark) PN-H" (Ajinomoto Fine-Techno Co., Ltd.), "Amicure (registered trademark) PN-40" (Ajinomoto Fine-Techno Co., Ltd.), "Hardener X-3661S" (ACR Corporation), "Hardener X-3670S" (ACR Corporation), "Novacure (registered trademark) HX-3742" (Asahi Kasei Corporation), and "Novacure (registered trademark) HX-3721" (Asahi Kasei Corporation). Examples of amine-isocyanate latent curing accelerators include "Fujicure FXE-1000" (Fuji Kasei Co., Ltd.), and "Fujicure FXR-1030" (Fuji Kasei Co., Ltd.).
[0033] In the epoxy resin composition of the present invention, the content of the curing accelerator per 100 parts by mass of the epoxy resin is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, even more preferably 1.5 parts by mass or more, and especially preferably 2 parts by mass or more. Furthermore, the content of the curing accelerator per 100 parts by mass of the epoxy resin of the present invention is preferably 40 parts by mass or less, more preferably 35 parts by mass or less, even more preferably 30 parts by mass or less, even more preferably 25 parts by mass or less, and especially preferably 20 parts by mass or less. A preferred content of the curing accelerator may be within a range selected from the upper limit, lower limit, and values in the examples.
[0034] Examples of the solvent include water and organic solvents that are commonly used in the art. Examples of the organic solvent include toluene, tetrahydrofuran, methyl ethyl ketone, methyl isobutyl ketone, and dioxane. Although the solvent may be present, it is preferably finally removed from the epoxy resin composition.
[0035] The storage stabilizer is used to impart excellent storage stability to the epoxy resin composition, and preferably further contains at least one storage stabilizer selected from, for example, borate compounds, titanate compounds, aluminate compounds, zirconate compounds, isocyanate compounds, carboxylic acids, acid anhydrides, and mercapto organic acids. Examples of the borate compound include trimethyl borate, triethyl borate, tripropyl borate, triisopropyl borate, tributyl borate, tripentyl borate, triallyl borate, trihexyl borate, tricyclohexyl borate, trioctyl borate, trinonyl borate, tridecyl borate, tridodecyl borate, trihexadecyl borate, trioctadecyl borate, tris(2-ethylhexyloxy)borane, bis(1,4,7,10-tetraoxaundecyl)(1,4,7,10,13-pentaoxatetradecyl)(1,4,7-trioxaundecyl)borane, tribenzyl borate, triphenyl borate, tri-o-tolyl borate, tri-m-tolyl borate, and triethanolamine borate.
[0036] Examples of the titanate compounds include tetraethyl titanate, tetrapropyl titanate, tetraisopropyl titanate, tetrabutyl titanate, and tetraoctyl titanate. Examples of the aluminate compounds include triethyl aluminate, tripropyl aluminate, triisopropyl aluminate, tributyl aluminate, and trioctyl aluminate. Examples of the zirconate compounds include tetraethyl zirconate, tetrapropyl zirconate, tetraisopropyl zirconate, and tetrabutyl zirconate. Examples of the isocyanate compound include butyl isocyanate, isopropyl isocyanate, 2-chloroethyl isocyanate, phenyl isocyanate, p-chlorophenyl isocyanate, benzyl isocyanate, hexamethylene diisocyanate, 2-ethylphenyl isocyanate, 2,6-dimethylphenyl isocyanate, tolylene diisocyanate (e.g., 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate), 1,5-naphthalene diisocyanate, diphenylmethane-4,4′-diisocyanate, tolidine diisocyanate, isophorone diisocyanate, xylylene diisocyanate, paraphenylene diisocyanate, and bicycloheptane triisocyanate.
[0037] Examples of the carboxylic acid include saturated aliphatic monobasic acids such as formic acid, acetic acid, propionic acid, butyric acid, caproic acid, and caprylic acid; unsaturated aliphatic monobasic acids such as acrylic acid, methacrylic acid, and crotonic acid; halogenated fatty acids such as monochloroacetic acid and dichloroacetic acid; monobasic hydroxy acids such as glycolic acid, lactic acid, and acetic acid; aliphatic aldehyde acids and ketone acids such as glyoxylic acid; aliphatic polybasic acids such as oxalic acid, malonic acid, succinic acid, and maleic acid; aromatic monobasic acids such as benzoic acid, halogenated benzoic acids, toluic acid, phenylacetic acid, cinnamic acid, and mandelic acid; and aromatic polybasic acids such as phthalic acid and trimesic acid. Examples of the acid anhydride include aliphatic polybasic acid anhydrides such as succinic anhydride, dodecynylsuccinic anhydride, maleic anhydride, an adduct of methylcyclopentadiene and maleic anhydride, hexahydrophthalic anhydride, and methyltetrahydrophthalic anhydride; and aromatic polybasic acid anhydrides such as phthalic anhydride, trimellitic anhydride, and pyrrolimellitic anhydride. Examples of the mercapto organic acid include mercaptoaliphatic monocarboxylic acids such as mercaptoacetic acid, mercaptopropionic acid (e.g., 3-mercaptopropionic acid), and mercaptobutyric acid (e.g., 3-mercaptobutyric acid, 4-mercaptobutyric acid); esters containing a thiol group and a carboxy group obtained by an esterification reaction between a hydroxy acid and a mercapto organic acid; mercaptoaliphatic dicarboxylic acids such as mercaptosuccinic acid and dimercaptosuccinic acid (e.g., 2,3-dimercaptosuccinic acid); and mercaptoaromatic monocarboxylic acids such as mercaptobenzoic acid (e.g., 4-mercaptobenzoic acid).
[0038] As the storage stabilizer, from the viewpoints of versatility, high safety, and improving storage stability, borate compounds are preferred, triethyl borate, tripropyl borate, triisopropyl borate, and tributyl borate are more preferred, and triethyl borate is even more preferred. The content of the storage stabilizer in the epoxy resin composition of the present invention is not particularly limited as long as the storage stability of the composition is improved, but the content is preferably 0.001 to 50 parts by mass, more preferably 0.05 to 30 parts by mass, and even more preferably 0.1 to 10 parts by mass of the storage stabilizer per 100 parts by mass of the epoxy resin.
[0039] The other curing agent may be any compound other than the thiol compound of the present invention, as long as it can be used as a curing agent for epoxy resins. Examples of other curing agents include complete esters of polyols and mercapto organic acids. Here, complete esters refer to esters of polyols and carboxylic acids, in which all of the hydroxyl groups of the polyol form ester bonds. Examples of the polyols include ethylene glycol, trimethylolpropane, pentaerythritol, and dipentaerythritol. Examples of the mercapto organic acid include mercaptoaliphatic monocarboxylic acids such as mercaptoacetic acid, mercaptopropionic acid (e.g., 3-mercaptopropionic acid), and mercaptobutyric acid (e.g., 3-mercaptobutyric acid, 4-mercaptobutyric acid); esters containing a thiol group and a carboxy group obtained by an esterification reaction between a hydroxy acid and a mercapto organic acid; mercaptoaliphatic dicarboxylic acids such as mercaptosuccinic acid and dimercaptosuccinic acid (e.g., 2,3-dimercaptosuccinic acid); and mercaptoaromatic monocarboxylic acids such as mercaptobenzoic acid (e.g., 4-mercaptobenzoic acid). The number of carbon atoms in the mercaptoaliphatic monocarboxylic acid is preferably 2 to 8, more preferably 2 to 6, even more preferably 2 to 4, and particularly preferably 3. Among the mercapto organic acids, mercapto aliphatic monocarboxylic acids having 2 to 8 carbon atoms are preferred, with mercaptoacetic acid, 3-mercaptopropionic acid, 3-mercaptobutyric acid, and 4-mercaptobutyric acid being more preferred, and 3-mercaptopropionic acid being even more preferred.
[0040] Specific examples of complete esters of polyols and mercapto organic acids include ethylene glycol bis(mercaptoacetate), ethylene glycol bis(3-mercaptopropionate), ethylene glycol bis(3-mercaptobutyrate), ethylene glycol bis(4-mercaptobutyrate), trimethylolpropane tris(mercaptoacetate), trimethylolpropane tris(3-mercaptopropionate), trimethylolpropane tris(3-mercaptobutyrate), trimethylolpropane tris(4-mercaptobutyrate), pentaerythritol tetrakis(mercaptoacetate), pentaerythritol tetrakis(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), pentaerythritol tetrakis(4-mercaptobutyrate), and dipentaerythritol Examples of the complete ester include hexakis(mercaptoacetate), dipentaerythritol hexakis(3-mercaptopropionate), dipentaerythritol hexakis(3-mercaptobutyrate), and dipentaerythritol hexakis(4-mercaptobutyrate). From the viewpoint of storage stability, the complete ester preferably has as little basic impurity content as possible, and more preferably does not require the use of a basic substance in its production.
[0041] Other curing agents that can be used include polythiol compounds produced using a basic substance as a reaction catalyst in the production process, such as alkyl polythiol compounds such as 1,4-butanedithiol, 1,6-hexaneedithiol, and 1,10-decanedithiol; terminal thiol group-containing polyethers; terminal thiol group-containing polythioethers; polythiol compounds obtained by reacting an epoxy compound with hydrogen sulfide; and polythiol compounds having terminal thiol groups obtained by reacting a polythiol compound with an epoxy compound. Polythiol compounds produced using a basic substance are preferably subjected to a dealkalization treatment to reduce the alkali metal ion concentration to 50 ppm by weight or less before use. Examples of dealkalization treatments for polythiol compounds produced using a basic substance include dissolving the polythiol compound in an organic solvent such as acetone or methanol, neutralizing it by adding an acid such as dilute hydrochloric acid or dilute sulfuric acid, and then desalting it by extraction and washing, etc.; adsorption using an ion exchange resin; and purification by distillation.
[0042] Other curing agents that can be used include, for example, tris[(3-mercaptopropionyloxy)-ethyl]-isocyanurate and 1,3,5-tris(3-mercaptobutyloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione. Preferably, it is one or more complete esters of ethylene glycol, trimethylolpropane, pentaerythritol, or dipentaerythritol with a mercaptoaliphatic monocarboxylic acid having 2 to 8 carbon atoms; more preferably, ethylene glycol bis(mercaptoacetate), ethylene glycol bis(3-mercaptopropionate), ethylene glycol bis(3-mercaptobutyrate), ethylene glycol bis(4-mercaptobutyrate), trimethylolpropane tris(mercaptoacetate), trimethylolpropane tris(3-mercaptopropionate), trimethylolpropane tris(3-mercaptobutyrate), trimethylolpropane tris(4-mercaptobutyrate), pentaerythritol tetrakis(mercaptoacetate), pentaerythritol tetrakis(3-mercaptopropionate), and pentaerythritol At least one selected from tetrakis(3-mercaptobutyrate), pentaerythritol tetrakis(4-mercaptobutyrate), dipentaerythritol hexakis(mercaptoacetate), dipentaerythritol hexakis(3-mercaptopropionate), dipentaerythritol hexakis(3-mercaptobutyrate), and dipentaerythritol hexakis(4-mercaptobutyrate); more preferably at least one selected from trimethylolpropane tris(mercaptoacetate), trimethylolpropane tris(3-mercaptopropionate), trimethylolpropane tris(3-mercaptobutyrate), and trimethylolpropane tris(4-mercaptobutyrate); particularly preferably trimethylolpropane tris(3-mercaptopropionate).
[0043] When another curing agent is used in the epoxy resin composition, it is preferably used in an amount that does not affect the curing of the thiol compound of the present invention. Preferably, the amount of the other curing agent is 0.001 to 50 parts by mass, more preferably 0.05 to 30 parts by mass, and even more preferably 0.1 to 10 parts by mass per 100 parts by mass of the epoxy resin. The ratio of the thiol compound of the present invention to the other curing agent, [mass of the thiol compound of the present invention] / [total mass of the thiol compound of the present invention and the other curing agent], is preferably, for example, 0.001 to 0.8. The lower limit of this ratio is more preferably 0.01, even more preferably 0.03, and particularly preferably 0.1. The upper limit of this ratio is not particularly limited, but is more preferably 0.6, even more preferably 0.4, and particularly preferably 0.2.
[0044] The ratio of the total equivalent of thiol groups contained in the thiol compound of the present invention and / or other curing agents to the equivalent of epoxy groups contained in the epoxy resin, i.e., [total number of thiol groups contained in the thiol compound of the present invention and / or other curing agents] / [number of epoxy groups contained in the epoxy resin], is preferably 0.2 to 2.0, more preferably 0.6 to 1.2.
[0045] Examples of the thixotropy-imparting agent include precipitated silica, calcined silica, and fumed silica, and among these, fumed silica is preferred. The specific surface area of the thixotropy-imparting agent measured by the BET method (hereinafter referred to as the BET specific surface area) is preferably 50 m 2 / g or more, more preferably 50 to 600m 2 / g, more preferably 100 to 400m 2 When a thixotropy-imparting agent is used, the content of the thixotropy-imparting agent in the epoxy resin composition is preferably 5 to 200 parts by mass, more preferably 10 to 100 parts by mass, per 100 parts by mass of the epoxy resin.
[0046] The epoxy resin composition may be a one-component epoxy resin composition or a two-component epoxy resin composition. In the case of a two-component epoxy resin composition, for example, an epoxy resin may be component A, and a thiol compound and other additives may be component B, and the two components may be used as a kit. The epoxy resin composition may contain one or more of the above-mentioned components such as the thiol compound.
[0047] [Cured Epoxy Resin Product] One embodiment of the present invention may be a cured epoxy resin product obtained by curing the above-described epoxy resin in the presence of the above-described thiol compound. The curing method may be a thermal curing method typically used for epoxy resins. For example, an epoxy resin, a thiol compound, and other optional additives may be mixed to prepare an epoxy resin composition, and the epoxy resin composition may be maintained at a temperature of, for example, 50 to 250°C, preferably 80 to 200°C, and more preferably 120°C ± 10 to 20°C, for, for example, 10 minutes to 3 hours, preferably 30 minutes to 2 hours, and more preferably 1 hour ± 10 to 20 minutes, to obtain a cured product. When preparing the epoxy resin composition, it is preferable to degas the components using a defoamer or the like.
[0048] The epoxy resin cured product of the present invention can be used for applications such as adhesives, casting agents, sealing agents, encapsulants, fiber-reinforcing resins, coating agents, and paints.
[0049] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to the following examples. [Method for measuring high-performance liquid chromatography and mass spectrometry (LC / MS measurement)] (Measurement conditions for high-performance liquid chromatography and mass spectrometry) A sample was diluted to 1 mg / mL with tetrahydrofuran (THF), and measurement by high-performance liquid chromatography and mass spectrometry (LC / MS) was performed under the following conditions. High-performance liquid chromatography (HPLC): ACQUITY UPLC (Nihon Waters) Mass spectrum (MS): SQ Detector 2 (Nihon Waters) Column: ACQUITY UPLC BEH C8 1.7 μm, 2.1 mm × 50 mm (Nihon Waters) Mobile phase A: 2 mmol ammonium acetate aqueous solution Mobile phase B: 2-propanol / acetonitrile (50:50) Mobile phase mixing time and mixing ratio (A%): 0-0.5 min (95%) → 1 min-8.5 min (75%) → 9-11 min (5%) → 11.1 min (95%) → 13 min (95%) Flow rate: 0.30 mL / min Analysis time: 13 min Column temperature: 40°C, ion mode: ESI (electrospray ionization) positive Ion polarity: Positive detection mode Desolvation gas flow rate: 700 L / hr, 250°C Cone gas: 70 L / hr Ion source heater: 150°C
[0050] [NMR Measurement Method] NMR data for each thiol compound prepared in the Examples was collected using a JEOL LA-500 (manufactured by JEOL Corporation).
[0051] Example 1 Synthesis of Thiol Compound (1) (1) Synthesis of Aliphatic Skeleton Diallyl Compound (1) A 2-L four-necked round flask equipped with a stirrer, thermometer, condenser, dropping funnel, and Dean-Stark trap was charged with 140.9 g (1.05 mol) of 2-allylphenol (reagent), 108.0 g (0.5 mol) of 1,4-dibromobutane (reagent), 3.1 g of tetra-n-butylammonium bromide as a phase transfer catalyst, and 300 g of methyl isobutyl ketone (MIBK) as a reaction solvent. The mixture was heated to 100°C and maintained for 30 minutes to achieve complete dissolution. To the resulting solution, 175 g (1.5 mol) of a 48% aqueous solution of KOH was added dropwise over 1 hour. The water and MIBK azeotropically distilled by the added aqueous KOH solution were separated into water and MIBK in the Dean-Stark trap, and the reaction continued while only the MIBK was returned to the reaction system. The reaction was continued for 6 hours while the MIBK alone was returned to the system at 118°C and the water was distilled off. The temperature was then lowered to 60°C, 100 g of distilled water was added, and the mixture was allowed to stand. The lower by-product brine layer was discarded. Next, 100 g of distilled water and an appropriate amount of sodium dihydrogen phosphate for neutralization were added, and the mixture was allowed to stand. The lower by-product brine layer was discarded. The same amount of distilled water was added and the mixture was washed and purified twice, after which it was heated to 118°C and azeotropically dehydrated. The resulting solution was microfiltered using filter paper No. 5C (manufactured by Kiriyama Seisakusho Co., Ltd.) and a Kiriyama funnel (manufactured by Kiriyama Seisakusho Co., Ltd.) to remove impurities. The MIBK and unreacted 2-allylphenol were then distilled under reduced pressure at a maximum temperature of 180°C to obtain 145 g of a liquid resin. The obtained liquid resin was analyzed according to the above-mentioned LC / MS measurement method, and a spectral peak corresponding to a proton adduct at m / z = 323 and an ammonium adduct at m / z = 340 was detected. From the analytical data, the obtained liquid resin was confirmed to be the diallyl compound (1) having the following structure:
[0052] Diallyl Compound (1)
[0053] (2) Synthesis of Thiol Compound (1) Diallyl compound (1) (100 g, 0.31 mol, 1.0 eq) obtained in (1) above, thioacetic acid (51.9 g, 0.682 mol, 2.2 eq), toluene (360 mL), and azobisisobutyronitrile (AIBN, 5.09 g, 0.031 mol, 0.1 eq) were added to a 1 L four-neck flask and reacted at 80 ° C for 4 hours. The resulting reaction product was concentrated under reduced pressure to remove toluene, and then crystallized from methanol (500 g). The crystallized product was vacuum dried to recover 110.36 g of dried crystallized product. The recovered dried crystallized product (110.36 g) and 32 mass% NaOH (550 g) were added to a 3 L four-neck flask and reacted at 80 ° C for 2 hours. The reaction mixture was neutralized by adding 1N HCl (380 mL), and the organic layer was separated and washed with water. Toluene was removed from the washed organic layer by vacuum concentration, yielding 89.0 g of the target thiol compound (74% yield). The resulting thiol compound was analyzed according to the LC / MS method described above, and spectral peaks at m / z = 391, corresponding to a proton adduct, and m / z = 408, corresponding to an ammonium adduct, were detected. From these analytical data and the NMR spectrum shown in FIG. 1, the resulting thiol compound was confirmed to have the structure of thiol compound (1) shown below.
[0054] Thiol Compound (1)
[0055] Example 2 Synthesis of Thiol Compound (2) (1) Synthesis of Aliphatic Skeleton Diallyl Compound (2) 142 g of liquid resin was obtained in the same manner as in Example 1, except that 201.0 g (1.05 mol) of 2-allylphenol (reagent) in Example 1 was replaced with 201.0 g (1.05 mol) of 4-allylphenol (reagent). The obtained liquid resin was measured according to the LC / MS measurement method described above, and a spectral peak of m / z = 323 corresponding to a proton adduct and a spectral peak of m / z = 340 corresponding to an ammonium adduct were detected. From the analytical data, it was confirmed that the obtained liquid resin was diallyl compound (2) having the following structure:
[0056] Diallyl Compound (2)
[0057] (2) Synthesis of Thiol Compound (2) 91 g of the target thiol compound was obtained in the same manner as in Example 1(2), except that 100 g (0.31 mol) of the diallyl compound (1) in Example 1(2) was replaced with 100 g (0.31 mol) of the diallyl compound (2) synthesized in Example 2(1). The obtained thiol compound was measured according to the LC / MS measurement method described above, and a spectral peak of m / z = 391 corresponding to a proton adduct and a spectral peak of m / z = 408 corresponding to an ammonium adduct were detected. From the results of the analytical data, it was confirmed that the obtained thiol compound had the structure of thiol compound (2) according to the following structure.
[0058] Thiol Compound (2)
[0059] Example 3 Synthesis of Thiol Compound (3) (1) Synthesis of Aliphatic Skeleton Diallyl Compound (3) 165 g of liquid resin was obtained in the same manner as in Example 1, except that 108.0 g (0.5 mol) of 1,4-dibromobutane (reagent) in Example 1 was replaced with 150.0 g (0.5 mol) of 1,10-dibromodecane. The obtained liquid resin was measured according to the LC / MS measurement method described above, and a spectral peak of m / z = 407 corresponding to a proton adduct and a spectral peak of m / z = 424 corresponding to an ammonium adduct were detected. From the analytical data, it was confirmed that the obtained liquid resin was diallyl compound (3) having the following structure:
[0060] Diallyl Compound (3)
[0061] (2) Synthesis of Thiol Compound (3) 109 g of the target thiol compound was obtained in the same manner as in Example 1(2), except that 100 g (0.31 mol) of the diallyl compound (1) in Example 1(2) was replaced with 125.9 g (0.31 mol) of the diallyl compound (3) synthesized in Example 3(1). The obtained thiol compound was measured according to the LC / MS measurement method described above, and a spectral peak of m / z = 475 corresponding to a proton adduct and a spectral peak of m / z = 492 corresponding to an ammonium adduct were detected. From the analytical data and the NMR spectrum results shown in Figure 2, it was confirmed that the obtained thiol compound had the structure of thiol compound (3) shown below.
[0062] Thiol Compound (3)
[0063] Example 4 Synthesis of Thiol Compound (4) (1) Synthesis of Aliphatic Skeleton Diallyl Compound (4) 161 g of liquid resin was obtained in the same manner as in Example 1, except that 201.0 g (1.05 mol) of 2-allylphenol (reagent) in Example 1 was changed to 172.4 g of eugenol. The obtained liquid resin was measured according to the LC / MS measurement method described above, and a spectral peak of m / z = 383 corresponding to a proton adduct and a spectral peak of m / z = 400 corresponding to an ammonium adduct were detected. From the analytical data, it was confirmed that the obtained liquid resin was diallyl compound (4) having the following structure:
[0064] Diallyl Compound (4)
[0065] (2) Synthesis of Thiol Compound (4) 107 g of the target thiol compound was obtained in the same manner as in Synthesis Example 1(2), except that 100 g (0.31 mol) of the diallyl compound (1) in Example 1(2) was replaced with 118.6 g (0.31 mol) of the diallyl compound (4) synthesized in Example 4(1). The obtained thiol compound was measured according to the LC / MS measurement method described above, and a spectral peak of m / z = 451 corresponding to a proton adduct and a spectral peak of m / z = 468 corresponding to an ammonium adduct were detected. From the results of the analytical data, it was confirmed that the obtained thiol compound had the structure of thiol compound (4) shown below.
[0066] Thiol Compound (4)
[0067] Example 5 Synthesis of Thiol Compound (5) (1) Synthesis of Diallyl Compound (5) A 2-L four-necked round flask equipped with a stirrer, thermometer, condenser, dropping funnel, and Dean-Stark trap was charged with 155.6 g (1.05 mol) of 2-allyl-6-methylphenol (reagent), 150.0 g (0.5 mol) of 1,10-dibromodecane, 3.1 g of tetra-n-butylammonium bromide as a phase transfer catalyst, and 300 g of methyl isobutyl ketone (MIBK) as a reaction solvent, and the mixture was heated to 100°C to achieve complete dissolution. To the resulting solution, 175 g (1.5 mol) of a 48% aqueous solution of KOH was added dropwise over 1 hour. The water and MIBK azeotropically distilled by the added aqueous KOH solution were separated into water and MIBK in the Dean-Stark trap, and the reaction continued while only the MIBK was returned to the reaction system. The reaction was continued for 6 hours while the MIBK alone was returned to the system at 118°C and the water was distilled off. The temperature was then lowered to 60°C, 100 g of distilled water was added, and the mixture was allowed to stand. The lower by-product brine layer was discarded. Next, 100 g of distilled water and an appropriate amount of sodium dihydrogen phosphate for neutralization were added, and the mixture was allowed to stand. The lower by-product brine layer was discarded. The same amount of distilled water was added and the mixture was washed and purified twice, after which it was heated to 118°C and azeotropically dehydrated. The resulting solution was microfiltered using filter paper No. 5C (manufactured by Kiriyama Seisakusho Co., Ltd.) and a Kiriyama funnel (manufactured by Kiriyama Seisakusho Co., Ltd.) to remove impurities. Then, MIBK and unreacted 2-allyl-6-methylphenol were distilled under reduced pressure at a maximum temperature of 180°C to obtain 176 g of a liquid resin. The obtained liquid resin was analyzed according to the above-mentioned LC / MS measurement method, and a spectral peak corresponding to a proton adduct at m / z=435 and an ammonium adduct at m / z=452 was detected. From the analytical data, the obtained liquid resin was confirmed to be the diallyl compound (5) having the following structure:
[0068] Diallyl Compound (5)
[0069] (2) Synthesis of Thiol Compound (5) 110 g of the target thiol compound was obtained in the same manner as in Example 1 (2), except that 100 g (0.31 mol) of the diallyl compound (1) obtained in Example 1 (2) was replaced with 134.7 g (0.31 mol) of the aliphatic skeleton diallyl compound (5) synthesized in Example 5 (1). The obtained thiol compound was measured according to the LC / MS measurement method described above, and a spectral peak of m / z = 475 corresponding to a proton adduct and a spectral peak of m / z = 492 corresponding to an ammonium adduct were detected. From the results of the analytical data, it was confirmed that the obtained thiol compound had the structure of thiol compound (5) shown below.
[0070] Thiol Compound (5)
[0071] [Evaluation Test] The state of curing of epoxy resins using each of the thiol compounds obtained in the above examples was evaluated. Specifically, the epoxy resin, thiol compound, and curing accelerator (Amicure (registered trademark) PN-H, manufactured by Ajinomoto Fine-Techno Co., Ltd.) were weighed and mixed in the amounts shown in Table 1 below (component amounts in Table 1 are in parts by mass). The mixture was then degassed in a revolution-type agitator / defoamer (HM-200W, manufactured by Kyoritsu Seiki Co., Ltd.) at 900 rpm for 2 minutes under vacuum to obtain the desired resin composition. The resulting resin composition was cured in a heat circulation oven at 120°C for 1 hour to obtain a cured product. The surface of the resulting cured product was touched with a finger to confirm whether any residue remained on the finger. jER (registered trademark) 828 (manufactured by Mitsubishi Chemical Corporation) was used as the epoxy resin. In Comparative Example 1, BD-1 (1,4-bis(3-mercaptobutyryloxy)butane, manufactured by Resonac Co., Ltd.) was used as the thiol curing agent.
[0072] BD-1 (1,4-bis(3-mercaptobutyryloxy)butane)
[0073] Table 1
[0074] As shown in Table 1, tack-free cured products were obtained in Examples 1 and 2. On the other hand, in Comparative Example 1, part of the cured product adhered to the finger, and tackiness was observed, and it was visually confirmed that at least a part of the product was in an uncured state.
[0075] [Synthesis Application Examples] By substituting other compounds as starting materials in the synthesis of the various thiol compounds in the above examples, various types of compounds represented by general formula (I) can be synthesized. Specific synthesis application examples for the synthesis example of the aliphatic skeleton diallyl compound (1) in Example 1 are shown below. <Synthesis Application Example 1> Substituted raw material in Example 1: 2-allylphenol Substituted raw material used: 1-(2-propen-1-yl)-2-naphthalenol Examples of the compound represented by general formula (I) obtained include thiol compound (1b) having the following structure (in general formula (I), ring P is a naphthalene group). (1b)
[0076] <Synthesis Application Example 2> Substituted raw material for Example 1: 2-allylphenol Substituted raw material used: 4-ethyl-2-(2-propen-1-yl)phenol An example of the compound represented by general formula (I) obtained is a thiol compound (1c) having the following structure (in general formula (I), B is an ethyl group). (1c) <Synthesis Application Example 3> Substituted raw material of Example 1: 2-allylphenol Substituted raw material used: 4-ethoxy-2-(2-propen-1-yl)phenol An example of the compound represented by general formula (I) obtained is a thiol compound (1d) having the following structure (in general formula (I), B is an ethoxy group). (1d)
[0077] <Synthesis Application Example 4> Substituted raw material in Example 1: 2-allylphenol Substituted raw material used: 2-vinylphenol An example of the compound represented by general formula (I) obtained is a thiol compound (1e) having the following structure (in general formula (I), R1 is a C2-alkylene group). (1e) <Synthesis Application Example 5> Substituted raw material for Example 1: 2-allylphenol Substituted raw material used: N-methyl-2-(2-propen-1-yl)benzeneamine An example of the compound represented by general formula (I) obtained is a thiol compound (1f) having the following structure (in general formula (I), X is —N(CH)—). (1f)
[0078] <Synthesis Application Example 6> Substituted raw material for Example 1: 2-allylphenol Substituted raw material used: 2-(2-propen-1-yl)menzenthiol An example of the compound represented by general formula (I) obtained is a thiol compound (1g) having the following structure (in general formula (I), X is -S-). (1g) <Synthesis Application Example 7> Substituted raw material in Example 1: 1,4-dibromobutane Substituted raw material used: 2-bromoethyl ether Examples of the compound represented by general formula (I) that can be obtained include thiol compounds (1h) having the following structure (in general formula (I), Z is —O—). (1h)
[0079] <Synthesis Application Example 8> Substituted raw material in Example 1: 1,4-dibromobutane Substituted raw material used: 1,1'-thiobis[2-bromoethane] Examples of the compound represented by general formula (I) that can be obtained include thiol compounds (1i) having the following structure (in general formula (I), Z is -S-). (1i) <Synthesis Application Example 9> Substituted raw material in Example 1: 1,4-dibromobutane Substituted raw material used: 1,6-dibromo-2,5-dimethylhexane An example of the compound represented by general formula (I) obtained is a thiol compound (1j) having the following structure (wherein Y is a methyl group in general formula (I)). (1j)
Claims
1. General formula (I): (In formula (I), each ring P is independently a phenyl group or a naphthalene group; when ring P is a phenyl group, 1 to 5 A's are present for each ring P; when ring P is a naphthalene group, 1 to 7 A's are present for each ring P; each A's are independently -R1-SH; each R1's are independently a C1-C6 alkylene group optionally substituted with one or more Y's; each B's are substituents other than A on ring P, and each B's are independently substituted with a hydrogen atom or one or more Y's. A and B are each independently bonded to the ortho-, meta-, or para-position relative to the position where ring P is bonded to the main chain when ring P is a phenyl group, and bonded to the ortho-, meta-, para-, ana-, epi-, cata-, peri-, pros-, amphi-, or 2,7-position relative to the position where ring P is bonded to the main chain when ring P is a naphthalene group, and X are each independently bonded to -CH 2 -, -O-, -N(-R2)-, or -S-, each R2 is independently a hydrogen atom, a C1-C6 alkyl group which may be substituted with one or more Y, or a C1-C6 alkoxy group which may be substituted with one or more Y, each Y is independently a hydrogen atom, a C1-C6 alkyl group, or a C1-C6 alkoxy group, each Z is independently a direct bond, -CH 2 -, -O-, or -S-, and n is an integer of 1 to 20.
2. The compound according to claim 1, wherein ring P is a phenyl group, A is present in each ring P, and each A is independently bonded at the ortho or para position relative to the position where ring P is bonded to the main chain.
3. The compound according to claim 1, wherein ring P is a phenyl group, A is present once in each ring P, R1 is a linear C2-C3 alkylene group, all B are hydrogen atoms, X is -O-, Y is a hydrogen atom, Z is a direct bond or -O-, and n is an integer from 2 to 5.
4. The compound according to claim 1, wherein ring P is a phenyl group, A is present in each ring P once, R1 is a linear C2-C3 alkylene group, one of B present in each ring P is a methyl group, a methoxy group, or a phenyl group, all other B present in each ring P are hydrogen atoms, X is -O-, Y is a hydrogen atom, Z is a direct bond or -O-, and n is an integer from 2 to 5.
5. The compound shown below. , , , or 6. An epoxy resin composition comprising an epoxy resin and a compound according to any one of claims 1 to 5.
7. A curing agent for epoxy resins, comprising the compound according to any one of claims 1 to 5.
8. An epoxy resin cured product obtained by thermally curing an epoxy resin and a compound according to any one of claims 1 to 5.
Citation Information
Patent Citations
Resin composition, resin cured material, and resin molded product
JP2012153794A
Novel glycoluril having thioether linkage and mercapto group and use thereof
JP2016164134A
Resin curing agent and one-pack type epoxy resin composition
WO2014084292A1
UV light-cured resin composition as well as preparation method and application thereof
CN113943420A
Photocurable adhesive composition for optical use
JP2004035857A
Cited By
Biphenyl type polythiol compound as well as preparation method and application thereof
CN119528781A
A biphenyl-type polysulfydryl compound, a preparation method and application thereof
CN119528781B