Method for manufacturing circuit board, and resin composition
The method of thermal curing and polishing a ferrite-containing resin composition for circuit boards enables effective wet plating without permeability loss, addressing the challenge of forming conductor layers on magnetic cured materials and maintaining magnetic properties.
Patent Information
- Application Number
- PCT/JP2024/011714
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
The challenge in manufacturing circuit boards with integrated inductors is the difficulty in forming a conductor layer on a magnetic cured material layer containing magnetic powder without causing a decrease in relative magnetic permeability, as conventional methods like wet plating with oxidizing agents lead to elution of the resin and magnetic powder, making it brittle and affecting adhesion.
A method involving thermal curing of a resin composition containing ferrite with manganese and zinc, followed by polishing and wet plating on the magnetic cured product, which maintains the magnetic properties and prevents permeability decrease even after acid treatment.
This method allows for the formation of a conductor layer on circuit boards with minimal loss in relative magnetic permeability, ensuring effective plating adhesion and maintaining magnetic properties, thus enhancing the performance of inductor components.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure 00000067_0000 
Figure 00000067_0001
Abstract
Description
Circuit board manufacturing method and resin composition
[0001] The present invention relates to a method for producing a circuit board using a resin composition containing magnetic powder; and to the resin composition.
[0002] Inductors, which are sometimes called power inductors, high-frequency band inductors, or common mode choke coils, are mounted in large numbers in information terminals such as mobile phones and smartphones. Traditionally, independent inductor components were mounted on circuit boards, but in recent years, a method has emerged in which coils are formed using the conductor patterns of the circuit board and the inductor is mounted inside the circuit board.
[0003] For example, Patent Document 1 discloses a multilayer circuit board with a built-in inductor, in which a spiral conductor pattern is formed on multiple layers of the multilayer board, and the ends of the conductor pattern on each layer are connected to the upper and lower layers to form a spiral coil as a whole. Patent Document 2 also discloses that an inductor component is built into a core substrate of a circuit board in order to make the circuit board thinner.
[0004] When manufacturing an inductor component in which an inductor is formed by a plurality of conductor patterns formed on an insulating layer, it is possible to use a resin composition containing magnetic powder as a material for forming the insulating layer. Using an insulating layer (magnetic cured material layer) containing magnetic powder can increase the inductance value and also suppress leakage of magnetic field lines outside the inductor. For example, Patent Document 2 discloses that a resin composition constituting a resin composition layer of a resin sheet with a support contains magnetic powder, and the resulting insulating layer is made of a magnetic material.
[0005] Furthermore, for example, Patent Document 3 discloses an inductor component that is small and achieves high inductance by filling a through hole in a circuit board for the inductor component with a resin composition containing magnetic powder to form a magnetic core, and then arranging the magnetic core at the center of a coil formed on a wiring layer of the circuit board.
[0006] JP 2009-16504 A JP 2012-186440 A JP 2016-197624 A
[0007] In the manufacture of these inductor components (circuit boards), a conductive layer may be formed on a magnetic hardened material layer containing magnetic powder, and it is desirable to form the conductive layer by wet plating, which is advantageous in terms of cost.
[0008] When forming a conductor layer on an insulating layer that does not contain magnetic powder, it is common to form the conductor layer after treating the surface of the insulating layer with an oxidizing agent. However, the present inventors have previously found that when forming a conductor layer on a magnetic hardened material layer that contains magnetic powder, treating the surface of the magnetic hardened material layer with an oxidizing agent causes the resin and magnetic powder to elute, making the magnetic hardened material layer brittle, making it difficult to achieve good plating adhesion.
[0009] Therefore, the present inventors have investigated a method of forming a conductor layer on a magnetic cured material layer by polishing the surface of the magnetic cured material layer without using an oxidizing agent. However, when the conductor layer is formed on the magnetic cured material layer by wet plating after polishing the surface of the magnetic cured material layer, the conductor dissolves in an acidic treatment solution such as a reducing agent in the wet plating process, resulting in a decrease in the relative permeability after the formation of the conductor layer.
[0010] The present invention has been made in view of the above circumstances, and aims to provide a method for manufacturing a circuit board in which a conductor layer is formed by wet plating on a magnetic cured material layer containing magnetic powder, and a resin composition that can suppress a decrease in relative permeability even after acid treatment.
[0011] In order to achieve the above object, the inventors conducted extensive research and discovered that by selecting and using a specific ferrite containing manganese and zinc as the magnetic powder to be contained in a resin composition, it is possible to suppress a decrease in relative permeability even after acid treatment in the production of circuit boards in which a conductor layer is formed by wet plating, and thus completed the present invention.
[0012] That is, the present invention includes the following: [1] A method for producing a circuit board, comprising the steps of: (1) thermally curing a resin composition to obtain a magnetically cured product, (2) polishing at least a portion of the surface of the magnetically cured product, and (3) forming a conductor layer by wet plating on at least a portion of the polished surface of the magnetically cured product, in this order, wherein the resin composition comprises (A) a magnetic powder, (B) an epoxy resin, and (C) a curing agent, the component (A) comprises (A-1) a ferrite containing manganese and zinc, the content of iron contained in the component (A-1) is 56% by mass or more and 63% by mass or less, the content of manganese contained in the component (A-1) is 7% by mass or more and 13% by mass or less, and the content of zinc contained in the component (A-1) is 1% by mass or more and 3% by mass or less. [2] The method for producing a circuit board according to [1], wherein a cured product obtained by heating the resin composition at 190°C for 90 minutes has a decrease in relative magnetic permeability of 10% or less after being immersed in hydrochloric acid. [3] The method for producing a circuit board according to [1] or [2], wherein the resin composition is in a paste form. [4] The method for producing a circuit board according to any of [1] to [3], wherein the resin composition forms a resin composition layer. [5] A resin composition comprising: (A) a magnetic powder; (B) an epoxy resin; and (C) a curing agent; wherein the component (A) comprises (A-1) a ferrite containing manganese and zinc; the content of iron contained in the component (A-1) is 56% by mass or more and 63% by mass or less; the content of manganese contained in the component (A-1) is 7% by mass or more and 13% by mass or less; and the content of zinc contained in the component (A-1) is 1% by mass or more and 3% by mass or less. [6] The resin composition according to [5], which is a resin composition for use in a method for producing a circuit board, comprising, in this order: (1) a step of thermally curing the resin composition to obtain a magnetically cured product; (2) a step of polishing at least a part of the surface of the magnetically cured product; and (3) a step of forming a conductor layer by wet plating on at least a part of the polished surface of the magnetically cured product.
[0013] According to the present invention, in the manufacture of a circuit board in which a conductor layer is formed by wet plating on a magnetic cured material containing magnetic powder, a method for manufacturing a board and a resin composition can be provided that can suppress a decrease in relative permeability even after acid treatment.
[0014] FIG. 1 is a schematic cross-sectional view of a core substrate as an example of a first embodiment of the method for manufacturing a circuit board. FIG. 2 is a schematic cross-sectional view of a core substrate with through holes formed therein as an example of the first embodiment of the method for manufacturing a circuit board. FIG. 3 is a schematic cross-sectional view showing a state in which a plating layer has been formed in a through hole as an example of the first embodiment of the method for manufacturing a circuit board. FIG. 4 is a schematic cross-sectional view showing a state in which a through hole has been filled with a through hole filling paste as an example of the first embodiment of the method for manufacturing a circuit board. FIG. 5 is a schematic cross-sectional view showing a magnetic cured material obtained by thermally curing the filled through hole filling paste as an example of the first embodiment of the method for manufacturing a circuit board. FIG. 6 is a schematic cross-sectional view showing a state after polishing the magnetic cured material as an example of the first embodiment of the method for manufacturing a circuit board. FIG. 7 is a schematic cross-sectional view showing a state in which a conductor layer has been formed on the polished surface as an example of the first embodiment of the method for manufacturing a circuit board. FIG. 8 is a schematic cross-sectional view showing a state in which a patterned conductor layer has been formed as an example of the first embodiment of the method for manufacturing a circuit board. FIG. 9 is a schematic cross-sectional view for explaining step (α) as an example of a second embodiment of the method for manufacturing a circuit board. FIG. 10 is a schematic cross-sectional view illustrating step (α) as an example of a second embodiment of the method for manufacturing a circuit board. FIG. 11 is a schematic cross-sectional view illustrating step (β) as an example of a second embodiment of the method for manufacturing a circuit board. FIG. 12 is a schematic cross-sectional view illustrating a state in which a patterned conductor layer is formed as an example of the second embodiment of the method for manufacturing a circuit board. FIG. 13 is a schematic plan view of an inductor component including a circuit board obtained by the second embodiment of the method for manufacturing a circuit board, as an example, viewed from one side in the thickness direction. FIG. 14 is a schematic view illustrating a cut end surface of an inductor component including a circuit board obtained by the second embodiment of the method for manufacturing a circuit board, cut at the position indicated by the dashed line II-II. FIG. 15 is a schematic plan view illustrating the configuration of a first conductor layer of an inductor component including a circuit board obtained by the second embodiment of the method for manufacturing a circuit board, as an example.
[0015] Hereinafter, embodiments of the present invention will be described with reference to the drawings. Note that each drawing merely shows the shape, size, and arrangement of components in a schematic manner to the extent that the invention can be understood. The present invention is not limited by the following description, and each component can be modified as appropriate. In the drawings used in the following description, similar components are denoted by the same reference numerals, and redundant explanations may be omitted. Furthermore, the configuration according to the embodiments of the present invention may not necessarily be manufactured or used in the arrangement shown in the drawings.
[0016] [Circuit Board] A circuit board refers to a substrate having a conductor layer (circuit). The circuit board can be used as a wiring board for mounting electronic components such as semiconductor chips, and can also be used as a (multilayer) printed wiring board using such a wiring board as an inner layer substrate.
[0017] The method for manufacturing the circuit board will be described below.
[0018] [Method for manufacturing circuit board] The method for manufacturing a circuit board of the present invention includes, in this order: (1) a step of thermally curing a resin composition to obtain a magnetic cured product; (2) a step of polishing at least a portion of the surface of the magnetic cured product; and (3) a step of forming a conductor layer by wet plating on at least a portion of the polished surface of the magnetic cured product.
[0019] The resin composition includes (A) a magnetic powder, (B) an epoxy resin, and (C) a curing agent. The component (A) includes (A-1) a ferrite containing manganese and zinc, wherein the iron content in the component (A-1) is 56% by mass or more and 63% by mass or less, the manganese content in the component (A-1) is 7% by mass or more and 13% by mass or less, and the zinc content in the component (A-1) is 1% by mass or more and 3% by mass or less. Thus, the resin composition of the present invention uses the acid-resistant component (A-1) as the magnetic powder (A). Therefore, by using the magnetic cured material in the manufacture of a circuit board, even when a polishing treatment is performed instead of treating the surface of the magnetic cured material layer with an oxidizing agent, a decrease in the relative permeability of the magnetic cured material is suppressed in a wet plating process. Furthermore, an increase in the loss factor of the magnetic cured material is usually suppressed.
[0020] -Step (1)- Step (1) is a step of thermally curing the resin composition to obtain a magnetic cured product. The shape of the magnetic cured product is not particularly limited and is set appropriately depending on the mode of use, etc. Performing step (1) may include a step of preparing a resin composition. The resin composition may be a paste-like resin composition (magnetic paste). The resin composition may also form a resin composition layer. In other words, the resin composition may be prepared as a resin composition layer formed from the resin composition. The resin composition layer can be obtained from a magnetic sheet described below.
[0021] The curing temperature of the resin composition in step (1) varies depending on the composition and type of the resin composition, but is preferably 120° C. or higher, more preferably 130° C. or higher, even more preferably 150° C. or higher, and preferably 240° C. or lower, more preferably 220° C. or lower, and even more preferably 200° C. or lower. The curing time of the resin composition is preferably 5 minutes or longer, more preferably 10 minutes or longer, even more preferably 15 minutes or longer, and preferably 120 minutes or shorter, more preferably 100 minutes or shorter, and even more preferably 90 minutes or shorter.
[0022] Before thermally curing the resin composition, the resin composition may be subjected to a preheating treatment in which the resin composition is heated at a temperature lower than the curing temperature. For example, prior to thermally curing the resin composition, the resin composition may be preheated at a temperature of typically 50°C or higher and lower than 120°C (preferably 60°C or higher and 110°C or lower, more preferably 70°C or higher and 100°C or lower) for typically 5 minutes or longer (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes).
[0023] The degree of cure of the magnetic cured product obtained in step (1) is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. The degree of cure can be measured, for example, using a differential scanning calorimeter.
[0024] -Step (2)- Step (2) is a step of polishing the surface of the magnetic cured product. The surface to be polished may be at least a part of the surface of the magnetic cured product. Examples of the polishing method include buff polishing and belt polishing. Examples of commercially available buff polishing devices include "NT-700IM" manufactured by Ishii Hyoki Co., Ltd., and examples of commercially available ceramic roll polishing devices include "#1500" manufactured by Ishii Hyoki Co., Ltd.
[0025] The arithmetic mean roughness (Ra) of the polished surface of the magnetic cured material is preferably 300 nm or more, more preferably 350 nm or more, and even more preferably 400 nm or more, from the viewpoint of improving plating adhesion with the conductor layer. The upper limit is preferably 1000 nm or less, more preferably 900 nm or less, and even more preferably 800 nm or less. The surface roughness (Ra) can be measured, for example, using a non-contact surface roughness meter.
[0026] After step (2) and before step (3), a heat treatment step may be carried out as necessary for the purpose of further increasing the degree of hardening of the magnetic cured material. The temperature in the heat treatment step may be in accordance with the above-mentioned hardening temperature, and is preferably 120° C. or higher, more preferably 130° C. or higher, even more preferably 150° C. or higher, and preferably 240° C. or lower, more preferably 220° C. or lower, even more preferably 200° C. or lower. The heat treatment time is preferably 5 minutes or longer, more preferably 10 minutes or longer, even more preferably 15 minutes or longer, and preferably 90 minutes or shorter, more preferably 70 minutes or shorter, even more preferably 60 minutes or shorter.
[0027] In step (2), by polishing the surface of the magnetic cured material, a conductor layer can be formed on the magnetic cured material without treating the surface with an oxidizing agent, thereby preventing the magnetic cured material from becoming brittle and achieving good plating adhesion.
[0028] Furthermore, the component (A-1) may be partially exposed on the polished surface of the magnetic cured product obtained in this manner. However, since the component (A-1) is resistant to acid, even if a conductor layer is formed by wet plating, a decrease in the relative permeability and loss factor is suppressed.
[0029] -Step (3)- Step (3) is a step of forming a conductor layer by wet plating on at least a portion of the polished surface of the magnetic cured product. Although component (A-1) may be present on the polished surface of the magnetic cured product, component (A-1) is unlikely to dissolve in the plating solution, and therefore a decrease in the relative permeability of the magnetic cured product can be suppressed. Examples of materials for the conductor layer include simple metals such as gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin, and indium; and alloys of two or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin, and indium. Among these, from the viewpoints of versatility, cost, ease of patterning, and the like, it is preferable to use chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or a nickel-chromium alloy, a copper-nickel alloy, or a copper-titanium alloy, it is more preferable to use chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or a nickel-chromium alloy, and it is even more preferable to use copper.
[0030] In a preferred embodiment of step (3), it is preferable to perform electroless plating as a wet plating process to form a conductor layer, and it is more preferable to perform electroless plating and then further perform electrolytic plating to form a conductor layer. Therefore, step (3) preferably involves plating the surface of the magnetic cured material by a semi-additive method, a subtractive method, a full-additive method, or the like to form a conductor layer. From the viewpoint of ease of manufacturing the conductor layer, it is preferable to form the conductor layer by a semi-additive method or a subtractive method in step (3).
[0031] In detail, the semi-additive method involves first forming a plating seed layer on the surface of the magnetic cured material by electroless plating. Next, a mask pattern is formed on the formed plating seed layer, exposing a portion of the plating seed layer corresponding to the desired wiring pattern. After forming a conductor layer on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by etching or the like, thereby forming a conductor layer having the desired wiring pattern.
[0032] The electroless plating treatment is carried out by immersing the magnetic cured product in an electroless plating solution. Examples of electroless plating treatment include electroless copper plating, electroless nickel plating, electroless nickel-tungsten plating, electroless tin plating, and electroless gold plating, with electroless copper plating being preferred.
[0033] The electroless plating solution used in the electroless plating process may contain, for example, copper, nickel, tungsten, tin, gold, palladium, PdCl 2 Examples of suitable electroless plating solutions include solutions containing metal ions such as those mentioned above. The electroless plating solution may also contain other additives such as a reducing agent. Commercially available electroless plating solutions can be used. Examples of commercially available electroless plating solutions include "Thrucup PEA" manufactured by Uemura Kogyosho Co., Ltd. and "S-KPD" manufactured by Nippon Kangen Co., Ltd.
[0034] From the viewpoint of activating the catalyst, the treatment time for the electroless plating treatment is preferably 10 minutes or more, more preferably 20 minutes or more, and even more preferably 30 minutes or more, and is preferably 60 minutes or less, more preferably 50 minutes or less, and even more preferably 40 minutes or less.
[0035] From the viewpoint of efficient formation of the conductor layer, the processing temperature for the electroless plating process is preferably 10°C or higher, more preferably 20°C or higher, even more preferably 30°C or higher, and is preferably 60°C or lower, more preferably 55°C or lower, even more preferably 50°C or lower.
[0036] After forming a plating seed layer by electroless plating, a dry film is laminated on the plating seed layer. Then, exposure and development are performed under predetermined conditions using a photomask so that a portion of the plating seed layer is exposed corresponding to the desired wiring pattern, thereby forming a mask pattern. The exposure and development conditions can be those already known.
[0037] The dry film may be a photosensitive dry film made of a photoresist composition, such as a novolac resin or an acrylic resin.
[0038] The mask pattern is used as a plating mask in the electrolytic copper plating process, and is removed after the electrolytic plating process.
[0039] The electrolytic plating treatment is carried out by immersing the magnetic cured product after electroless plating treatment in a plating bath. At this time, an electric current is passed through the plating bath. Examples of the electrolytic plating treatment include electrolytic copper plating, electrolytic nickel plating, electrolytic tin plating, and electrolytic gold plating, with electrolytic copper plating being preferred.
[0040] Examples of plating baths used in electrolytic plating include baths containing copper sulfate, copper pyrophosphate, copper cyanide, and the like.
[0041] From the viewpoint of activating the catalyst, the treatment time for the electrolytic plating treatment is preferably 30 minutes or more, more preferably 40 minutes or more, and even more preferably 50 minutes or more, and is preferably 90 minutes or less, more preferably 80 minutes or less, and even more preferably 70 minutes or less.
[0042] From the viewpoint of efficient formation of the conductor layer, the processing temperature for the electrolytic plating process is preferably 10°C or higher, more preferably 15°C or higher, and even more preferably 20°C or higher, and is preferably 50°C or lower, more preferably 40°C or lower, and even more preferably 30°C or lower.
[0043] The current density of the electrolytic plating treatment is preferably 1.0 A / dm from the viewpoint of efficient formation of the conductor layer. 2 More preferably, 1.5 A / dm 2 More preferably, 2.0 A / dm 2 or more, preferably 4.0 A / dm 2 Less than or equal to 3.5 A / dm 2 or less, more preferably 3.0 A / dm 2 The following is the result.
[0044] The formation of a conductor layer by the subtractive method involves first providing a plating seed layer on the surface of the magnetic cured material by electroless plating, and then providing a metal layer on the plating seed layer by electrolytic plating to form a conductor layer before patterning. A dry film is then provided on the surface of the conductor layer before patterning, and the dry film is exposed and developed to form a pattern. The exposed conductor layer is then removed by etching, and the dry film is also removed, thereby forming a conductor layer with a desired wiring pattern.
[0045] After the formation of the conductor layer, an annealing treatment may be carried out if necessary, for example, by heating the substrate at 150 to 200° C. for 20 to 90 minutes.
[0046] From the viewpoint of thinning, the thickness of the conductor layer is preferably 70 μm or less, more preferably 60 μm or less, even more preferably 50 μm or less, still more preferably 40 μm or less, particularly preferably 30 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less. The lower limit is preferably 1 μm or more, more preferably 3 μm or more, and even more preferably 5 μm or more.
[0047] Hereinafter, first and second embodiments will be described as more specific examples of the method for manufacturing a circuit board. Of course, the method for manufacturing a circuit board according to the present invention is not limited to the first and second embodiments exemplified below.
[0048] First Embodiment A circuit board in the first embodiment includes a substrate having through holes formed therein and a magnetic cured material filling the through holes. Accordingly, a method for manufacturing a circuit board in the first embodiment includes, in this order, the steps of: (1A) filling the through holes of the substrate with a resin composition and thermally curing the resin composition to form a magnetic cured material; (2A) polishing at least a portion of the surface of the magnetic cured material; and (3A) forming a conductor layer by wet plating on at least a portion of the polished surface of the magnetic cured material.
[0049] The method for producing a circuit board in the first embodiment preferably further includes, in this order, after step (2A) and before step (3A), (2A-1) a conditioning step of treating the surface of the cured magnetic material with a solution containing a surfactant, and (2A-2) a catalysis step of applying a catalyst to the surface of the cured magnetic material, and more preferably further includes, after step (2A-2) and before step (3A), (2A-3) a catalyst activation step of activating the catalyst. When steps (2A-1) to (2A-3) are performed after step (2A) is completed, it is possible to suppress the generation of insoluble matter, etc., that occurs particularly in steps (2A-2) and (2A-3).
[0050] Furthermore, after the step (2A-1) and before the step (2A-2), a micro-etching step (2A-1-1) of removing the surfactant from areas where the surfactant is not required may be included.
[0051] Step (1A) Step (1A) is a step of filling through-holes in a substrate with a resin composition and thermally curing the resin composition to form a magnetically cured product. In step (1A), it is preferable to form the magnetically cured product using a magnetic paste. Furthermore, step (1A) may include a step of preparing a core substrate 10 including a support substrate 11 and a first metal layer 12 and a second metal layer 13 made of a metal such as copper foil provided on both surfaces of the support substrate 11, as shown in FIG. 1 . Examples of materials for the support substrate 11 include insulating substrates such as a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate.
[0052] 2, the method may also include a step of forming through holes 14 in the core substrate 10. The through holes 14 can be formed, for example, by drilling, laser irradiation, plasma irradiation, etc. Specifically, the through holes 14 can be formed by forming through holes in the core substrate 10 using a drill or the like.
[0053] The through holes 14 can be formed using a commercially available drilling device, such as the "ND-1S211" manufactured by Hitachi Via Mechanics Co., Ltd.
[0054] After forming the through holes 14 in the core substrate 10, the process may include a step of roughening the core substrate 10 and forming a plating layer 20 within the through holes 14, on the surface of the first metal layer 12, and on the surface of the second metal layer 13, as shown in an example in Figure 3.
[0055] The roughening treatment may be either a dry or wet roughening treatment. An example of the dry roughening treatment is plasma treatment. An example of the wet roughening treatment is a method in which a swelling treatment using a swelling liquid, a roughening treatment using an oxidizing agent, and a neutralization treatment using a neutralizing liquid are performed in this order.
[0056] The plating layer 20 is formed by a plating method, and the procedure for forming the plating layer 20 by a plating method is the same as that for forming the conductor layer in step (3A) described below.
[0057] After preparing the core substrate 10 with the plating layer 20 formed in the through-holes 14, the resin composition 30a is filled into the through-holes 14, as shown in an example in Fig. 4. Examples of filling methods include a method of filling the through-holes 14 with the resin composition 30a using a squeegee, a method of filling the through-holes 14 with the resin composition 30a using a cartridge, a method of filling the through-holes 14 with the resin composition 30a by mask printing, a roll coating method, an inkjet method, etc. The resin composition 30a is preferably a magnetic paste.
[0058] In one embodiment of a method for filling the resin composition 30a into the through-holes 14, a mask having openings formed therein as hollow holes is placed so as to communicate with the through-holes of the core substrate. The resin composition is supplied to the surface of the mask opposite the support substrate, and the resin composition is swept across the openings of the mask using a squeegee.
[0059] After the through-holes 14 are filled with the resin composition 30a, the resin composition 30a is thermally cured to form a magnetic cured material 30 in the through-holes 14, as shown in Fig. 5. The thermal curing conditions for the resin composition 30a and the degree of curing of the magnetic cured material 30 in step (1A) are the same as those shown in step (1) above.
[0060] If necessary, after forming the magnetic cured material in the through-hole, a resin composition may be applied to the core substrate using a die coater or the like, followed by thermal curing to further form a magnetic cured material on the core substrate. This makes it possible to suppress depressions at the through-holes after the magnetic cured material is formed in the through-holes. The thermal curing conditions for forming the magnetic cured material on the core substrate and the degree of curing of the magnetic cured material are the same as those shown in step (1) above.
[0061] - Step (2A) - In step (2A), as shown in an example in Fig. 6, the excess magnetic cured material 30 protruding from or adhering to the core substrate 10 is removed by polishing, and the surface is flattened. As the polishing method, any method that can polish the excess magnetic cured material 30 protruding from or adhering to the core substrate 10 can be used. Such a polishing method is the same as that shown in step (2) above.
[0062] The arithmetic mean roughness (Ra) of the polished surface of the magnetic cured product after step (2A) is preferably 300 nm or more, more preferably 350 nm or more, and even more preferably 400 nm or more, from the viewpoint of improving plating adhesion with the conductor layer. The upper limit is preferably 1000 nm or less, more preferably 900 nm or less, and even more preferably 800 nm or less. The surface roughness (Ra) can be measured, for example, using a non-contact surface roughness meter.
[0063] In step (2A), by polishing the surface of the magnetic cured material, a conductor layer can be formed on the magnetic cured material without treating the surface with an oxidizing agent, thereby preventing the magnetic cured material from becoming brittle and achieving good plating adhesion.
[0064] After step (2A) and before step (3A), a heat treatment step may be performed as necessary to further increase the degree of hardening of the magnetic cured material, as in the case of after step (2) and before step (3) above. Furthermore, when the magnetic cured material is formed on a core substrate, drilling may be performed on the magnetic cured material after step (2A) and before step (3A). The drilling can be performed in the same manner as the formation of through holes described in step (1).
[0065] - Step (2A-1) - Step (2A-1) is a conditioning step in which the surface of the cured magnetic material is treated with a solution containing a surfactant. In step (2A-1), the surface of the cured magnetic material is usually brought into contact with the solution containing a surfactant, thereby cleaning the surface of the cured magnetic material and adjusting the surface charge so as to facilitate adsorption of a catalyst in step (2A-2).
[0066] The surfactant-containing solution used in step (2A-1) can be a solution that not only cleans the surface of the magnetic cured product but also adjusts the surface charge to facilitate catalyst adsorption in step (2A-2). Examples of such solutions include alkaline solutions containing a surfactant and acid solutions containing a surfactant, with alkaline solutions containing a surfactant being preferred from the viewpoint of suppressing insoluble matter, etc. Examples of alkaline solutions include sodium hydroxide solution and potassium hydroxide solution.
[0067] The pH of the alkaline solution containing a surfactant is preferably greater than 7, more preferably 8 or higher, and even more preferably 10 or higher. There is no particular upper limit, but it may be preferably 14 or lower, 13 or lower, or the like. The pH of the acid solution containing a surfactant is preferably 1 or higher, more preferably 2 or higher, and even more preferably 3 or higher. There is no particular upper limit, but it may be preferably less than 7, 6 or lower, or the like.
[0068] Examples of surfactants include cationic surfactants such as alkylamine salts, alkyltrimethylammonium salts, and alkyldimethylbenzylammonium salts; anionic surfactants such as fatty acid salts such as sodium oleate, alkyl sulfate ester salts, alkylbenzenesulfonates, alkyl sulfosuccinates, naphthalenesulfonates, polyoxyethylene alkyl sulfates, sodium alkanesulfonates, and sodium alkyldiphenyl ether sulfonates; and nonionic surfactants such as polyoxyethylene nonylphenyl ether, polyoxyethylene lauryl ether, polyoxyethylene styrylphenyl ether, polyoxyethylene octyphenyl ether, polyoxyethylene sorbitol tetraoleate, and polyoxyethylene-polyoxypropylene copolymers.
[0069] Commercially available surfactants can be used, such as "Securigand 902" manufactured by Atotech Japan and "PED-104" manufactured by Uemura Industries Co., Ltd.
[0070] The treatment time for step (2A-1) is, from the viewpoint of facilitating catalyst adsorption, preferably 1 minute or more, more preferably 2 minutes or more, even more preferably 3 minutes or more, and is preferably 20 minutes or less, more preferably 15 minutes or less, even more preferably 10 minutes or less.
[0071] From the viewpoint of facilitating catalyst adsorption, the temperature of the solution containing the surfactant is preferably 30°C or higher, more preferably 40°C or higher, and even more preferably 50°C or higher, and is preferably 90°C or lower, more preferably 80°C or lower, and even more preferably 70°C or lower.
[0072] After the step (2A-1) is completed, a water washing treatment may be carried out as necessary.
[0073] -Step (2A-1-1)- Step (2A-1-1) is a micro-etching step for removing the surfactant from areas where it is not required. In Step (2A-1-1), the surfactant is usually removed from areas where it is not required by bringing a micro-etching liquid into contact with the surface of the magnetic cured material. Examples of areas where it is not required include the first metal layer 12 and the second metal layer 13.
[0074] Examples of microetching solutions include hydrochloric acid, sulfuric acid, hydrogen peroxide, sodium persulfate, ammonium persulfate, and solutions made of combinations of these.
[0075] The concentration of the microetching solution is, in terms of normality, usually 2N or less, preferably 1.5N or less, and more preferably 1N or less, from the viewpoint of removing the surfactant only from unnecessary portions, and is preferably 0.1N or more, more preferably 0.2N or more, and even more preferably 0.5N or more, from the viewpoint of facilitating removal of the surfactant.
[0076] From the viewpoint of facilitating removal of the surfactant, the temperature of the microetching solution is preferably 10°C or higher, more preferably 15°C or higher, and even more preferably 20°C or higher, and is preferably 50°C or lower, more preferably 40°C or lower, and even more preferably 30°C or lower.
[0077] The treatment time for step (2A-1-1) is preferably 10 seconds or more, more preferably 15 seconds or more, even more preferably 30 seconds or more, from the viewpoint of facilitating removal of the surfactant, and is preferably 60 seconds or less, more preferably 50 seconds or less, even more preferably 40 seconds or less.
[0078] After the step (2A-1-1) is completed, a water washing treatment may be carried out as necessary.
[0079] - Step (2A-2) - Step (2A-2) is a catalysis step in which a catalyst is applied to the surface of the magnetic cured material. In step (2A-2), by applying a catalyst to the surface of the magnetic cured material, it is possible to improve the adhesion between the magnetic cured material and the conductor layer. Usually, in step (2A-2), the magnetic cured material is immersed in a solution containing a catalyst, and the catalyst is adsorbed onto the surface of the magnetic cured material.
[0080] Examples of the catalyst include palladium salts, palladium complex compounds, tin-palladium complex salts, and tin-palladium colloids.
[0081] The solution containing the catalyst is usually an alkaline solution. This can significantly suppress the generation of insoluble matter, etc. The pH of this alkaline solution is preferably greater than 7, more preferably 8 or more, and even more preferably 10 or more. There is no particular upper limit, but it can be preferably 14 or less, 13 or less, etc.
[0082] Furthermore, from the viewpoint of allowing the catalyst to be adsorbed throughout the magnetic cured material, the concentration of the solution containing the catalyst is, in terms of normality, preferably 1 mmol / L or more, more preferably 5 mmol / L or more, even more preferably 10 mmol / L or more, and is preferably 500 mmol / L or less, more preferably 300 mmol / L or less, even more preferably 100 mmol / L or less.
[0083] The solution containing the catalyst may be a commercially available product, such as "Activator Neogund 834" manufactured by Atotech Japan, or "Brown Shumer" manufactured by Nippon Kangen Co., Ltd.
[0084] The treatment time for step (2A-2) is preferably 1 minute or more, more preferably 2 minutes or more, and even more preferably 3 minutes or more, from the viewpoint of allowing the catalyst to be adsorbed on the entire magnetic cured material, and is preferably 20 minutes or less, more preferably 15 minutes or less, and even more preferably 10 minutes or less.
[0085] From the viewpoint of adsorbing the catalyst to the entire magnetic cured material, the temperature of the solution containing the catalyst is preferably 10°C or higher, more preferably 20°C or higher, and even more preferably 30°C or higher, and is preferably 60°C or lower, more preferably 50°C or lower, and even more preferably 40°C or lower.
[0086] After the step (2A-2) is completed, a water washing treatment may be carried out as necessary.
[0087] - Step (2A-3) - Step (2A-3) is a catalyst activation step for activating a catalyst. In step (2A-3), the adhesion between the magnetic cured material and the conductor layer can be improved by activating the catalyst. Usually, in step (2A-3), the magnetic cured material to which the catalyst has been applied is immersed in a reducing agent solution to generate catalyst nuclei, thereby activating the catalyst applied to the surface of the magnetic cured material.
[0088] Conventional magnetic powders (such as component (A-2) described below) tend to dissolve easily in reducing agent solutions. Furthermore, some or all of the dissolved magnetic powder components tend to precipitate upon reduction with a reducing agent, resulting in a decrease in the relative permeability and an increase in the loss factor of the cured magnetic material. However, component (A-1) used in the present invention is resistant to acid and therefore does not readily dissolve in a reducing agent solution, thereby preventing a decrease in the relative permeability and an increase in the loss factor of the cured magnetic material.
[0089] The reducing agent used in the step (2A-3) may be, for example, a hypophosphite, or a mixture of dimethylamine borane and a potassium salt of an organic acid.
[0090] An acidic solution is usually used as the reducing agent solution. While such an acidic solution easily dissolves general magnetic powders, component (A-1) is resistant to acids and therefore does not easily dissolve in the acidic solution. This makes it possible to suppress a decrease in the relative permeability of the magnetic cured product. The pH of this acidic solution is preferably 1 or higher, more preferably 2 or higher, and even more preferably 3 or higher. There is no particular upper limit, but it can be preferably less than 7, 6 or lower, etc.
[0091] Furthermore, from the viewpoint of activating the catalyst applied to the surface of the magnetic cured material, the concentration of the reducing agent in the reducing agent solution is, in terms of normality, preferably 0.3 N or more, more preferably 0.4 N or more, even more preferably 0.5 N or more, and is preferably 3 N or less, more preferably 2 N or less, even more preferably 1 N or less.
[0092] The reducing agent solution may be a commercially available product, such as "Reducer Accelerator 810 mod." or "Reducer Neogant WA" manufactured by Atotech Japan, or "K-PVD" manufactured by Nippon Kangen Co., Ltd.
[0093] The treatment time for Step (2A-3) is, from the viewpoint of activating the catalyst, preferably 1 minute or more, more preferably 2 minutes or more, even more preferably 3 minutes or more, and is preferably 20 minutes or less, more preferably 15 minutes or less, even more preferably 10 minutes or less.
[0094] From the viewpoint of activating the catalyst, the temperature of the reducing agent solution is preferably 10°C or higher, more preferably 20°C or higher, and even more preferably 30°C or higher, and is preferably 60°C or lower, more preferably 50°C or lower, and even more preferably 40°C or lower.
[0095] After the step (2A-3) is completed, a water washing treatment may be carried out as necessary.
[0096] -Step (3A)- Step (3A) is a step of forming a conductor layer by wet plating on at least a portion of the polished surface of the magnetic cured material. In step (3A), as shown in an example in Fig. 7, a conductor layer 40 is formed by wet plating on the polished magnetic cured material 30. After forming the conductor layer 40, as shown in an example in Fig. 8, a patterned conductor layer 41 may be formed by removing parts of the conductor layer 40, the first metal layer 12, the second metal layer 13, and the plating layer 20 by a process such as etching. The materials, formation methods, etc. of the conductor layer 40 and the patterned conductor layer 41 in step (3A) can be the same as those shown above for the conductor layer in step (3).
[0097] Second Embodiment A circuit board in a second embodiment includes a substrate including wiring and a magnetic cured material that seals and protects the wiring. For example, the circuit board has a layered magnetic cured material. A method for manufacturing a circuit board in the second embodiment includes, in this order: (1B) a step of laminating a magnetic sheet on a substrate so that a resin composition layer is bonded to the substrate, and thermally curing the resin composition layer to form a magnetic cured material; (2B) a step of polishing at least a portion of the surface of the magnetic cured material; and (3B) a step of forming a conductor layer by wet plating on at least a portion of the polished surface of the magnetic cured material.
[0098] The method for producing a circuit board in the second embodiment preferably further includes a step (1B-1) of drilling holes in the magnetic cured material after the step (1B) and before the step (2B).
[0099] It is more preferable that the method further comprises, in this order, (2B-1) a conditioning step of treating the surface of the cured magnetic material with a solution containing a surfactant and (2B-2) a catalysis step of applying a catalyst to the surface of the cured magnetic material after the step (2B) and before the step (3B), and it is even more preferable that the method further comprises (2B-3) a catalyst activation step of activating the catalyst after the step (2B-2) and before the step (3B).
[0100] Furthermore, after the step (2B-1) and before the step (2B-2), a micro-etching step (2B-1-1) of removing the surfactant from areas where the surfactant is not required may be included.
[0101] Step (1B) is a step of laminating a magnetic sheet on a substrate so that the resin composition layer is bonded to the substrate, and thermally curing the resin composition layer to form a magnetic cured product. Step (1B) may include a step of preparing a magnetic sheet.
[0102] In step (1B), as shown in an example in Figure 9, a magnetic sheet 310 including a support 330 and a resin composition layer 320a provided on the support 330 is laminated on the inner layer substrate 200 so that the resin composition layer 320a is bonded to the inner layer substrate 200.
[0103] The inner substrate 200 is an insulating substrate. Examples of materials for the inner substrate 200 include insulating base materials such as a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate. The inner substrate 200 may be an inner circuit board having wiring and the like formed within its thickness.
[0104] As shown in an example in Figure 9, the inner layer substrate 200 has a first conductor layer 420 provided on the first main surface 200a and an external terminal 240 provided on the second main surface 200b. The first conductor layer 420 includes a plurality of wirings. In the illustrated example, only the wirings constituting the coil-shaped conductive structure 400 of the inductor element are shown. The external terminal 240 is a terminal for electrically connecting to an external device or the like (not shown). The external terminal 240 can be configured as a part of the conductor layer provided on the second main surface 200b.
[0105] The conductive materials that can be used to form the first conductive layer 420, the external terminals 240, and other conductive layers are the same as the materials for the conductive layers described in step (3).
[0106] The first conductor layer 420, the external terminals 240, and other conductor layers may have a single-layer structure or a multi-layer structure in which two or more single-metal layers or alloy layers made of different types of metals or alloys are stacked. The thicknesses of the first conductor layer 420, the external terminals 240, and other conductor layers are the same as those of the patterned conductor layers in the first embodiment.
[0107] The line (L) / space (S) ratio of the first conductor layer 420 and the external terminal 240 is not particularly limited, but from the viewpoint of reducing surface irregularities and obtaining a magnetic cured product with excellent smoothness, it is usually 900 / 900 μm or less, preferably 700 / 700 μm or less, more preferably 500 / 500 μm or less, even more preferably 300 / 300 μm or less, and still more preferably 200 / 200 μm or less. The lower limit of the line / space ratio is not particularly limited, but from the viewpoint of improving the embedding of the resin composition layer in the spaces, it is preferably 1 / 1 μm or more.
[0108] The inner substrate 200 has a plurality of through holes 220 that penetrate the inner substrate 200 from the first main surface 200a to the second main surface 200b. Wiring 220a is provided in the through holes 220. The wiring 220a electrically connects the first conductor layer 420 and the external terminals 240.
[0109] The resin composition layer 320a and the inner substrate 200 can be bonded, for example, by thermocompression bonding the magnetic sheet 310 to the inner substrate 200 from the support 330 side. Examples of a member for thermocompression bonding the magnetic sheet 310 to the inner substrate 200 (hereinafter also referred to as a "thermocompression bonding member") include a heated metal plate (such as a stainless steel (SUS) plate) or a metal roll (SUS roll). Note that rather than pressing the magnetic sheet 310 by directly contacting it with the thermocompression bonding member, it is preferable to press the magnetic sheet 310 via a sheet made of an elastic material such as heat-resistant rubber so that the magnetic sheet 310 can sufficiently conform to the irregularities on the surface of the inner substrate 200.
[0110] The temperature during thermocompression bonding is preferably in the range of 80°C to 160°C, more preferably 90°C to 140°C, and even more preferably 100°C to 120°C, the pressure during thermocompression bonding is preferably in the range of 0.098 MPa to 1.77 MPa, more preferably 0.29 MPa to 1.47 MPa, and the time during thermocompression bonding is preferably in the range of 20 seconds to 400 seconds, more preferably 30 seconds to 300 seconds. The bonding of the magnetic sheet and the inner layer substrate is preferably carried out under reduced pressure conditions of 26.7 hPa or less.
[0111] The resin composition layer 320a of the magnetic sheet 310 can be bonded to the inner layer substrate 200 using a commercially available vacuum laminator. Examples of commercially available vacuum laminators include a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd. and a vacuum applicator manufactured by Nikko Materials Co., Ltd.
[0112] After bonding the magnetic sheet 310 and the inner layer substrate 200, the laminated magnetic sheet 31 may be smoothed under normal pressure (atmospheric pressure), for example, by pressing from the support side with a thermocompression member. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. Note that the lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.
[0113] After the magnetic sheet is laminated on the inner layer substrate, the resin composition layer is thermally cured to form a magnetic cured material. As shown in an example in Figure 10, the resin composition layer 320a bonded to the inner layer substrate 200 is thermally cured to form the first magnetic cured material layer 320. The thermal curing conditions for the resin composition layer 320a and the degree of curing of the first magnetic cured material layer 320 are the same as those described in step (1).
[0114] The support 330 may be removed between the end of the thermal curing in step (1B) and step (2B), or may be peeled off after step (2B).
[0115] Furthermore, step (1B) may be performed by directly applying or printing a paste-like resin composition (magnetic paste) onto the inner layer substrate, instead of laminating a magnetic sheet onto the inner layer substrate.
[0116] - Step (1B-1) - Step (1B-1) is a step of drilling holes in the magnetic cured material. In step (1B-1), as shown in an example in Fig. 11, holes are drilled in the first magnetic cured material layer 320 to form via holes 360. The via holes 360 serve as paths for electrically connecting the first conductor layer 420 and the second conductor layer 440, which will be described later. The via holes 360 can be formed by the same method as that for forming the through holes described in step (1).
[0117] Step (2B) is a step of polishing at least a part of the surface of the magnetic cured material. The polishing method in step (2B) can be the same as that described in step (2A) of the first embodiment.
[0118] The arithmetic mean roughness (Ra) of the polished surface of the magnetic cured product after step (2B) is preferably 300 nm or more, more preferably 350 nm or more, and even more preferably 400 nm or more, from the viewpoint of improving plating adhesion with the conductor layer. The upper limit is preferably 1000 nm or less, more preferably 900 nm or less, and even more preferably 800 nm or less. The surface roughness (Ra) can be measured, for example, using a non-contact surface roughness meter.
[0119] In step (2B), by polishing the surface of the magnetic cured material, a conductor layer can be formed on the magnetic cured material without treating the surface with an oxidizing agent, thereby preventing the magnetic cured material from becoming brittle and achieving good plating adhesion.
[0120] Steps (2B-1) to (2B-3) are the same as those described in steps (2A-1) to (2A-3) of the first embodiment.
[0121] - Step (3B) - Step (3B) is a step of forming a conductor layer by wet plating on at least a portion of the polished surface of the magnetic cured material. In step (3B), as shown in an example in FIG. 12, a second conductor layer 440 is partially formed on the polished surface of the first magnetic cured material layer 320. The method of forming the second conductor layer 440 is as described in the first embodiment. Note that this step also forms via-hole wiring 360a in the via hole 360. The conductor layer 400 is formed by forming the second conductor layer 440. The second conductor layer 440 includes a plurality of wirings.
[0122] The conductive material that can constitute the second conductor layer 440 is the same as that of the first conductor layer 420. The second conductor layer 440 may have a single-layer structure or a multi-layer structure in which two or more single-metal layers or alloy layers made of different types of metals or alloys are stacked. When the second conductor layer 440 has a multi-layer structure, the layer in contact with the magnetic cured material is preferably a single-metal layer of chromium, zinc, or titanium, or an alloy layer of a nickel-chromium alloy. The thickness of the second conductor layer 440 is the same as that of the first conductor layer 420.
[0123] The first conductor layer 420 and the second conductor layer 440 may be provided in a spiral shape, for example, as shown in Figures 13 to 15 (described later). In one example, one central end of the spiral wiring portion of the second conductor layer 440 is electrically connected to one central end of the spiral wiring portion of the first conductor layer 420 by via-hole wiring 360a. The other outer peripheral end of the spiral wiring portion of the second conductor layer 440 is electrically connected to land 420a of the first conductor layer 42 by via-hole wiring 360a. Therefore, the other outer peripheral end of the spiral wiring portion of the second conductor layer 440 is electrically connected to external terminal 240 via via-hole wiring 360a, land 420a, and through-hole wiring 220a.
[0124] The coil-shaped conductive structure 400 is composed of a spiral wiring portion that is part of the first conductor layer 420, a spiral wiring portion that is part of the second conductor layer 440, and via-hole wiring 360a that electrically connects the spiral wiring portion of the first conductor layer 420 and the spiral wiring portion of the second conductor layer 440.
[0125] After step (3B), a step of forming a magnetic cured material on the conductor layer may be performed. In detail, as shown in an example in Fig. 14, a second magnetic cured material is formed on the first magnetic cured material layer 320 on which the second conductor layer 440 and the via-hole wiring 360a are formed. The second magnetic cured material may be formed by the same steps as those already described.
[0126] [Magnetic Paste] The resin composition of the present invention can be made into a magnetic paste in paste form without containing an organic solvent by using a liquid thermosetting resin such as a liquid epoxy resin. When the magnetic paste contains an organic solvent, the content is preferably less than 1.0 mass%, more preferably 0.8 mass% or less, even more preferably 0.5 mass% or less, and particularly preferably 0.1 mass% or less, based on the total mass of the magnetic paste. There is no particular lower limit, but the content is 0.001 mass% or more, or no organic solvent is contained. By using a magnetic paste with a low content of organic solvent or without an organic solvent, the generation of voids due to the evaporation of the organic solvent can be suppressed, and the magnetic paste can also be made easier to handle and work with.
[0127] The viscosity of the magnetic paste at 25° C. is preferably 20 Pa·s or more, more preferably 25 Pa·s or more, even more preferably 30 Pa·s or more, or 50 Pa·s or more, and is usually less than 200 Pa·s, preferably 180 Pa·s or less, more preferably 160 Pa·s or less. The viscosity can be measured using an E-type viscometer while maintaining the temperature of the magnetic paste at 25±2° C.
[0128] Such a magnetic paste is useful for filling through-holes in a substrate.
[0129] [Magnetic Sheet] The magnetic sheet includes a support and a resin composition layer formed on the support and made of the resin composition of the present invention.
[0130] From the viewpoint of thinning, the thickness of the resin composition layer is preferably 250 μm or less, more preferably 200 μm or less, and even more preferably 150 μm or less, or 100 μm or less. The lower limit of the thickness of the resin composition layer is not particularly limited, but can usually be 5 μm or more.
[0131] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.
[0132] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, with inexpensive polyethylene terephthalate being particularly preferred.
[0133] When a metal foil is used as the support, examples of the metal foil include copper foil and aluminum foil, with copper foil being preferred. The copper foil may be a foil made of a single metal, such as copper, or a foil made of an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.).
[0134] The surface of the support that is to be bonded to the resin composition layer may be subjected to a matte treatment or a corona treatment.
[0135] Furthermore, as the support, a support with a release layer, which has a release layer on the surface that bonds with the resin composition layer, may be used. Examples of the release agent used in the release layer of the support with a release layer include one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. Commercially available products may be used as the support with a release layer, and examples include "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Uni-Peel" manufactured by Unitika Ltd., which are PET films having a release layer mainly composed of an alkyd resin-based release agent.
[0136] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the thickness of the entire support with a release layer is in the above range.
[0137] The magnetic sheet can be produced, for example, by preparing a magnetic paste by dissolving a resin composition in an organic solvent, applying this magnetic paste to a support using a die coater or the like, and then drying it to form a resin composition layer. When the resin composition is in a paste form, the magnetic sheet can be produced by applying the resin composition directly to a support using a die coater or the like to form a resin composition layer.
[0138] Examples of organic solvents include ketones such as acetone, methyl ethyl ketone (MEK), and cyclohexanone, acetate esters such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate, carbitols such as cellosolve and butyl carbitol, aromatic hydrocarbons such as toluene and xylene, and amide solvents such as dimethylformamide, dimethylacetamide (DMAc), and N-methylpyrrolidone. The organic solvents may be used alone or in combination of two or more.
[0139] Drying may be carried out by known methods such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is carried out so that the content of organic solvent in the resin composition layer is 10% by mass or less, preferably 5% by mass or less. Although this varies depending on the boiling point of the organic solvent in the magnetic paste, for example, when using a magnetic paste containing 30% by mass to 60% by mass of organic solvent, the resin composition layer can be formed by drying at 50°C to 150°C for 3 to 10 minutes.
[0140] In the magnetic sheet, a protective film similar to that of the support can be further laminated on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, it is possible to prevent the adhesion of dust and the like to the surface of the resin composition layer and to prevent scratches. The magnetic sheet can be wound up into a roll and stored. When the magnetic sheet has a protective film, it can be used by peeling off the protective film.
[0141] [Inductor Component] The circuit board in the present invention is preferably an inductor component having an inductor element formed by a patterned conductor layer.
[0142] The inductor component includes a circuit board obtained by the circuit board manufacturing method of the present invention. When such an inductor component includes a circuit board obtained by the first embodiment of the circuit board manufacturing method, the inductor component has an inductor element formed of a conductor around at least a portion of the periphery of the magnetic cured product of the resin composition. For example, the inductor component described in JP 2016-197624 A can be used.
[0143] Furthermore, when the circuit board includes a circuit board obtained by the second embodiment of the circuit board manufacturing method, the inductor component has a magnetic cured product of a resin composition (resin composition layer) and a conductive structure at least partially embedded in the magnetic cured product, and includes an inductor element formed by the conductive structure and a portion of the magnetic cured product extending in the thickness direction of the magnetic cured product and surrounded by the conductive structure. Here, Fig. 13 is a schematic plan view of an inductor component incorporating an inductor element, as viewed from one side in the thickness direction. Fig. 14 is a schematic view showing a cut end surface of the inductor component cut at the position indicated by the dashed line II-II in Fig. 13. Fig. 15 is a schematic plan view illustrating the configuration of a first conductor layer of the inductor component.
[0144] 13 and 14, the inductor component 100 may be a build-up wiring board having a plurality of magnetic cured materials (a first magnetic cured material layer 320, a second magnetic cured material layer 340) and a plurality of conductor layers (a first conductor layer 420, a second conductor layer 440), i.e., a build-up magnetic cured material layer and a build-up conductor layer. The inductor component 100 also includes an inner layer substrate 200.
[0145] 14 , the first magnetic cured material layer 320 and the second magnetic cured material layer 340 constitute the magnetic part 300, which can be seen as an integrated magnetic cured material. Therefore, the coiled conductive structure 400 is provided so that at least a portion thereof is embedded in the magnetic part 300. That is, in the inductor component 100 of this embodiment, the inductor element is constituted by the coiled conductive structure 400 and a core portion which is a portion of the magnetic part 300 that extends in the thickness direction of the magnetic part 300 and is surrounded by the coiled conductive structure 400.
[0146] 15, the first conductor layer 420 includes a spiral wiring portion for constituting the coil-shaped conductive structure 400 and a rectangular land 420a electrically connected to the through-hole wiring 220a. In the illustrated example, the spiral wiring portion includes a straight portion, a bent portion bent at a right angle, and a detour portion that detours around the land 420a. In the illustrated example, the spiral wiring portion of the first conductor layer 420 has an overall outline that is approximately rectangular and has a shape that winds counterclockwise from the center toward the outside.
[0147] Similarly, a second conductor layer 440 is provided on the first magnetic cured material layer 320. The second conductor layer 440 includes a spiral wiring portion for configuring the coil-shaped conductive structure 400. In Fig. 13 or 14, the spiral wiring portion includes a straight portion and a bent portion bent at a right angle. In Fig. 13 or 14, the spiral wiring portion of the second conductor layer 44 has an overall outline that is approximately rectangular, and has a shape that is wound clockwise from the center toward the outside.
[0148] Such an inductor component can be used as a wiring board for mounting electronic components such as semiconductor chips, or as a (multilayer) printed wiring board using such a wiring board as an inner layer substrate.Furthermore, such a wiring board can be singulated and used as a chip inductor component, or as a surface-mounted printed wiring board.
[0149] Furthermore, such a wiring board can be used to manufacture various types of semiconductor devices. Semiconductor devices including such wiring boards can be suitably used in electrical products (e.g., computers, mobile phones, digital cameras, televisions, etc.) and vehicles (e.g., motorcycles, automobiles, trains, ships, aircraft, etc.).
[0150] [Resin Composition] The resin composition of the present invention contains (A) magnetic powder, (B) epoxy resin, and (C) curing agent. The resin composition may further contain (D) dispersant, (E) reactive diluent, and (F) other additives, as necessary.
[0151] Such a resin composition is not easily dissolved in a treatment solution such as a reducing agent in a wet plating process, and therefore, even if a conductor layer is formed by wet plating, it is possible to suppress a decrease in the relative permeability and loss factor of the magnetic cured product. Each component of the resin composition in the present invention will be described below.
[0152] <(A) Magnetic Powder> The resin composition of the present invention contains (A) magnetic powder. In the resin composition according to this embodiment, the (A) magnetic powder includes (A-1) ferrite containing manganese and zinc. The (A) magnetic powder may include (A-2) a magnetic powder other than the component (A-1) in combination with the component (A-1). In this specification, the components (A-1) and (A-2) may be collectively referred to as the component (A).
[0153] - (A-1) Ferrite Containing Manganese and Zinc - The ferrite containing manganese and zinc (Mn-Zn ferrite) as the component (A-1) is a ferrite containing iron, manganese, and zinc, in which the content of iron contained in the component (A-1) is 56% by mass or more and 63% by mass or less, the content of manganese contained in the component (A-1) is 7% by mass or more and 13% by mass or less, and the content of zinc contained in the component (A-1) is 1% by mass or more and 3% by mass or less.
[0154] The resin composition of the present invention uses, as the magnetic powder, an Mn-Zn ferrite having iron, manganese, and zinc contents within the above-mentioned ranges. As a result of extensive research, the inventors have found that such an Mn-Zn ferrite has excellent acid resistance. Therefore, even when a magnetic cured product containing component (A-1) is immersed in a treatment solution in a wet plating process, it is possible to suppress a decrease in the relative permeability of the magnetic cured product. Furthermore, it is usually possible to suppress an increase in the loss factor of the magnetic cured product.
[0155] The iron content (mass%) in component (A-1) is 56 mass% or more, preferably 56.5 mass% or more, more preferably 57 mass% or more, and even more preferably 58.5 mass% or more. The upper limit is 63 mass% or less, preferably 62.5 mass% or less, more preferably 62 mass% or less, and even more preferably 61.5 mass% or less. The iron content in component (A-1) represents the iron content when component (A-1) is taken as 100 mass%.
[0156] The manganese content (mass %) in component (A-1) is 7 mass % or more, preferably 7.5 mass % or more, more preferably 7.7 mass % or more, and even more preferably 8 mass % or more. The upper limit is 13 mass % or less, preferably 12.5 mass % or less, more preferably 12 mass % or less, and even more preferably 11.5 mass % or less. The manganese content in component (A-1) is expressed as the manganese content when component (A-1) is taken as 100 mass %.
[0157] The zinc content (mass %) in component (A-1) is 1 mass % or more, preferably 1.5 mass % or more, more preferably 1.8 mass % or more, and even more preferably 2.0 mass % or more. The upper limit is 3 mass % or less, preferably 2.8 mass % or less, more preferably 2.6 mass % or less, and even more preferably 2.4 mass % or less. The zinc content in component (A-1) represents the zinc content when component (A-1) is taken as 100 mass %.
[0158] Component (A-1) may contain elements other than oxygen, iron, manganese, and zinc, such as Si, Cr, B, Ni, Al, Mo, Cu, and Co.
[0159] The content (mass %) of elements other than manganese and zinc in component (A-1) is preferably at least 23 mass %, more preferably at least 24 mass %, and even more preferably at least 25 mass %, with the upper limit being preferably at most 32 mass %, more preferably at most 31 mass %, and even more preferably at most 30 mass %.
[0160] As the component (A-1), a commercially available magnetic powder can be used. Specific examples of commercially available magnetic powders that can be used include "MZ05SIP" and "MZ05SMC" manufactured by Powder Tech Co., Ltd. The component (A-1) can be used alone or in combination of two or more types.
[0161] The component (A-1) is preferably spherical. The aspect ratio (the value obtained by dividing the length of the major axis of the magnetic powder by the length of the minor axis) is preferably 2 or less, more preferably 1.5 or less, and even more preferably 1.2 or less. In general, magnetic powders that are flat rather than spherical tend to improve the relative magnetic permeability. However, the use of spherical magnetic powders is particularly preferred from the viewpoint of reducing magnetic loss and obtaining a paste with a desirable viscosity.
[0162] From the viewpoint of improving the relative magnetic permeability, the average particle size of component (A-1) is preferably 0.01 μm or more, more preferably 0.5 μm or more, and even more preferably 1 μm or more, and is preferably 30 μm or less, more preferably 20 μm or less, and even more preferably 10 μm or less.
[0163] The average particle size of component (A-1) can be measured by a laser diffraction / scattering method based on Mie scattering theory. Specifically, the particle size distribution of the magnetic powder is created on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is used as the average particle size. A preferable measurement sample is one in which the magnetic powder is dispersed in water using ultrasonic waves. Examples of laser diffraction / scattering particle size distribution measuring devices that can be used include the "LA-500" manufactured by Horiba, Ltd. and the "SALD-2200" manufactured by Shimadzu Corporation.
[0164] The specific surface area of the component (A-1) is preferably 0.05 m from the viewpoint of improving the relative permeability. 2 / g or more, more preferably 0.1 m 2 / g or more, more preferably 0.3m 2 / g or more. 2 / g or less, more preferably 8m 2 / g or less, more preferably 5m 2The specific surface area of the component (A-1) can be measured by the BET method.
[0165] From the viewpoint of suppressing a decrease in the relative magnetic permeability of the magnetic cured product and suppressing an increase in the loss factor even after acid treatment, the content (volume %) of component (A-1) is preferably 30% by volume or more, more preferably 40% by volume or more, and even more preferably 50% by volume or more, based on 100% by volume of the nonvolatile components in the resin composition, and is also preferably 85% by volume or less, more preferably 80% by volume or less, and even more preferably 75% by volume or less.
[0166] From the viewpoint of suppressing a decrease in the relative magnetic permeability of the magnetic cured product and suppressing an increase in the loss factor even after acid treatment, the content (mass %) of component (A-1) is preferably 70 mass % or more, more preferably 75 mass % or more, and even more preferably 78 mass % or more, based on 100 mass % of the nonvolatile components in the resin composition. Also, it is preferably 98 mass % or less, more preferably 95 mass % or less, and even more preferably 90 mass % or less.
[0167] - (A-2) Magnetic Powder Other Than Component (A-1) - The resin composition may contain, as an optional component, magnetic powder other than components (A-2) and (A-1), as long as the effects of the present invention are not impaired. Component (A-2) may be used alone, or two or more types may be used in combination.
[0168] (A-2) may be either a soft magnetic powder or a hard magnetic powder, but from the viewpoint of suppressing uneven distribution of the magnetic powder, a soft magnetic powder is preferred.
[0169] Examples of the component (A-2) include Mn-Zn ferrites (excluding those corresponding to the component (A-1)), Fe-Mn ferrites, Mg-Zn ferrites, Mn-Mg ferrites, Cu-Zn ferrites, Mg-Mn-Sr ferrites, Ni-Zn ferrites, Ba-Zn ferrites, Ba-Mg ferrites, Ba-Ni ferrites, Ba-Co ferrites, Ba-Ni-Co ferrites, Y ferrites, iron oxide powder (III), and tetrafluoroethylene (TEO) compounds. Examples of the iron alloy include iron oxide powder such as triiron oxide; pure iron powder; iron alloy metal powders such as Fe-Si alloy powder, Fe-Si-Al alloy powder, Fe-Cr alloy powder, Fe-Cr-Si alloy powder, Fe-Ni-Cr alloy powder, Fe-Cr-Al alloy powder, Fe-Ni alloy powder, Fe-Ni-Mo alloy powder, Fe-Ni-Mo-Cu alloy powder, Fe-Co alloy powder, and Fe-Ni-Co alloy powder; and amorphous alloys such as Co-based amorphous alloys.
[0170] Among these, iron oxide powder is preferred as component (A-2) from the viewpoint of significantly achieving the effects of the present invention. The iron oxide powder is preferably a ferrite containing at least one element selected from Ni, Cu, Mn, and Zn, and more preferably an Fe-Mn ferrite. The Fe-Mn ferrite preferably has a Mn content of preferably 0.5% by mass or more, more preferably 3.0% by mass or more, and even more preferably 5.0% by mass or more, and preferably 25% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, based on 100% by mass of the Fe-Mn ferrite.
[0171] As the component (A-2), commercially available magnetic powders can be used. Specific examples of commercially available magnetic powders that can be used include "M03S", "M05S", "MZ03S", "M001", and "MZ05S" manufactured by Powdertech Co., Ltd.; "MA-RCO-24" manufactured by Dowa Electronics Co., Ltd.; "PST-S" manufactured by Sanyo Special Steel Co., Ltd.; "AW2-08", "AW2-08PF20F", "AW2-08PF10F", "AW2-08PF3F", "Fe-3.5Si-4.5CrPF20F", "Fe-50NiPF20F", and "Fe-80Ni-4MoPF20F" manufactured by Epson Atmix Corporation; and "LD-M", "LD-MH", "KNI-106", and "KNI- "KNI-106GSM", "KNI-106GS", "KNI-109", "KNI-109GSM", "KNI-109GS"; Toda Kogyo Co., Ltd.'s "KNS-415", "BSF-547", "BSF-029", "BSN-125", "BSN-125", "BSN-714", "BSN-828", "S-1281", "S-1641", "S-1651", "S-1470", "S-1511", "S-2430"; Japan Metals and Chemical Industries, Ltd.'s "JR09P2"; CIK Nanotech Co., Ltd.'s "Nanotek"; Kinsei Mater Tech Co., Ltd.'s "JEMK-S", "JEMK-H"; ALDRICH's "Yttrium iron oxide" and the like.
[0172] The component (A-2) is preferably spherical. The aspect ratio, calculated by dividing the length of the major axis of the magnetic powder by the length of the minor axis, is preferably 2 or less, more preferably 1.5 or less, and even more preferably 1.2 or less.
[0173] From the viewpoint of improving the relative magnetic permeability, the average particle size of component (A-2) is preferably 0.01 μm or more, more preferably 0.5 μm or more, and even more preferably 1 μm or more. It is also preferably 30 μm or less, more preferably 20 μm or less, and even more preferably 10 μm or less. The average particle size of component (A-2) can be measured in the same manner as for the average particle size of component (A-1).
[0174] The specific surface area of the component (A-2) is preferably 0.05 m from the viewpoint of improving the relative magnetic permeability. 2 / g or more, more preferably 0.1 m2 / g or more, more preferably 0.3m 2 / g or more. 2 / g or less, more preferably 8m 2 / g or less, more preferably 5m 2 The specific surface area of the component (A-2) can be measured in the same manner as for the component (A-1).
[0175] From the viewpoint of improving the relative permeability and reducing the loss factor, the content (volume %) of component (A-2) is preferably 0.5% by volume or more, more preferably 1% by volume or more, and even more preferably 1.5% by volume or more, based on 100% by volume of the nonvolatile components in the resin composition, and is preferably 15% by volume or less, more preferably 13% by volume or less, and even more preferably 10% by volume or less.
[0176] From the viewpoint of improving the relative permeability and reducing the loss factor, the content (mass %) of component (A-2) is preferably 1 mass % or more, more preferably 2 mass % or more, and even more preferably 3 mass % or more, based on 100 mass % of the nonvolatile components in the resin composition, and is preferably 30 mass % or less, more preferably 25 mass % or less, and even more preferably 20 mass % or less.
[0177] In the present invention, unless otherwise specified, the content of each component in the resin composition is a value when the non-volatile components in the resin composition are taken as 100 mass%, and the non-volatile components mean all non-volatile components in the resin composition excluding the solvent.
[0178] <(B) Epoxy Resin> The resin composition of the present invention usually contains (B) an epoxy resin.
[0179] Examples of (B) epoxy resins include bixylenol-type epoxy resins, bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, bisphenol S-type epoxy resins, bisphenol AF-type epoxy resins, dicyclopentadiene-type epoxy resins, trisphenol-type epoxy resins, naphthol novolac-type epoxy resins, phenol novolac-type epoxy resins, tert-butyl-catechol-type epoxy resins, naphthalene-type epoxy resins, naphthol-type epoxy resins, anthracene-type epoxy resins, glycidylamine-type epoxy resins, glycidyl ester-type epoxy resins, cresol novolac-type epoxy resins, biphenyl-type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane-type epoxy resins, cyclohexane dimethanol-type epoxy resins, naphthylene ether-type epoxy resins, trimethylol-type epoxy resins, and tetraphenylethane-type epoxy resins. These epoxy resins may be used alone or in combination of two or more.
[0180] The resin composition preferably contains, as the epoxy resin (B), an epoxy resin having two or more epoxy groups per molecule. From the viewpoint of significantly achieving the desired effects of the present invention, the proportion of the epoxy resin having two or more epoxy groups per molecule is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more, relative to 100% by mass of the non-volatile components of the epoxy resin (B).
[0181] Epoxy resins include epoxy resins that are liquid at a temperature of 25°C (hereinafter may be referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 25°C (hereinafter may be referred to as "solid epoxy resins"). In one embodiment, the resin composition of the present invention contains a liquid epoxy resin as the epoxy resin. In one embodiment, the resin composition of the present invention contains a solid epoxy resin as the epoxy resin. The resin composition of the present invention may contain only a liquid epoxy resin, or only a solid epoxy resin, or a combination of a liquid epoxy resin and a solid epoxy resin, but in a preferred embodiment, it contains only a liquid epoxy resin.
[0182] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.
[0183] Preferred liquid epoxy resins are bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AF type epoxy resins, naphthalene type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, phenol novolac type epoxy resins, alicyclic epoxy resins having an ester skeleton, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, glycidyl amine type epoxy resins, and epoxy resins having a butadiene structure.
[0184] Specific examples of liquid epoxy resins include "HP4032," "HP4032D," and "HP4032SS" (naphthalene-type epoxy resins) manufactured by DIC Corporation; "828US," "jER828EL" (bisphenol A-type epoxy resin), "jER807" (bisphenol F-type epoxy resin), and "jER152" (phenol novolac-type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630" and "630LSD" (glycidylamine-type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "ZX1059" (a mixture of bisphenol A-type epoxy resin and bisphenol F-type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "EX-721" (glycidyl ester-type epoxy resin) manufactured by Nagase ChemteX Corporation; "PB-3600" (epoxy resin having a butadiene structure); and "MX-153" (bisphenol A-type epoxy resin containing an organic filler having a core-shell structure) manufactured by Kaneka Corporation. These may be used alone or in combination of two or more.
[0185] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferred, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferred.
[0186] Preferred solid epoxy resins include bixylenol-type epoxy resins, naphthalene-type epoxy resins, naphthalene-type tetrafunctional epoxy resins, cresol novolac-type epoxy resins, dicyclopentadiene-type epoxy resins, trisphenol-type epoxy resins, naphthol-type epoxy resins, biphenyl-type epoxy resins, naphthylene ether-type epoxy resins, anthracene-type epoxy resins, bisphenol A-type epoxy resins, bisphenol AF-type epoxy resins, and tetraphenylethane-type epoxy resins.
[0187] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP-7200" (dicyclopentadiene type epoxy resin) manufactured by DIC Corporation; "HP-7200HH" and "HP-7200HH" manufactured by DIC Corporation. HP-7200H, EXA-7311, EXA-7311-G3, EXA-7311-G4, EXA-7311-G4S, and HP6000 (naphthylene ether type epoxy resins); EPPN-502H (trisphenol type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; NC7000L (naphthol novolac type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; NC3000H, NC3000, NC3000L, and NC3100 (biphenyl type epoxy resins) manufactured by Nippon Kayaku Co., Ltd. "ESN475V" (naphthol-type epoxy resin) manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.; "ESN485" (naphthol novolac-type epoxy resin) manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.; "YX4000H", "YX4000", and "YL6121" (biphenyl-type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "YX4000HK" (bixylenol-type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "YX8800" (anthracene-type epoxy resin) manufactured by Mitsubishi Chemical Corporation; " Examples of epoxy resins include "YX7700" (xylene structure-containing novolac type epoxy resin); "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals Co., Ltd.; "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "jER1010" (solid bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical Corporation; and "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical Corporation. These may be used alone or in combination of two or more.
[0188] When a liquid epoxy resin and a solid epoxy resin are used in combination as the epoxy resin (B), the mass ratio of the liquid epoxy resin to the solid epoxy resin (liquid epoxy resin / solid epoxy resin) is preferably 1 or more, more preferably 10 or more, and particularly preferably 50 or more.
[0189] The epoxy equivalent of the (B) epoxy resin is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., even more preferably 80 g / eq. to 2000 g / eq., and even more preferably 110 g / eq. to 1000 g / eq. By being within this range, the crosslink density of the magnetic cured material of the magnetic sheet is sufficient, resulting in a magnetic cured material layer with low surface roughness. The epoxy equivalent is the mass of the resin containing one equivalent of epoxy groups. This epoxy equivalent can be measured in accordance with JIS K7236.
[0190] From the viewpoint of significantly achieving the desired effects of the present invention, the weight average molecular weight (Mw) of the epoxy resin (B) is preferably 100 to 5000, more preferably 250 to 3000, and even more preferably 400 to 1500. The weight average molecular weight of the resin can be measured by gel permeation chromatography (GPC) as a polystyrene-equivalent value.
[0191] The content of the (B) epoxy resin is not particularly limited, but from the viewpoint of significantly achieving the desired effects of the present invention, it is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, based on 100% by mass of the non-volatile components in the resin composition. The upper limit is preferably 50% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, and particularly preferably 10% by mass or less, based on 100% by mass of the non-volatile components in the resin composition.
[0192] The viscosity of the epoxy resin (B) is preferably 0.5 Pa s or more, and preferably 1,000 Pa s or less, more preferably 500 Pa s or less, and even more preferably 100 Pa s or less. The viscosity of the epoxy resin is measured at 25±2°C using an E-type viscometer.
[0193] <(C) Curing Agent> The resin composition of the present invention typically contains a (C) curing agent. This (C) curing agent as component (C) does not include those corresponding to the above-mentioned components (A) and (B). The (C) curing agent includes an epoxy resin curing agent having the function of curing the (B) epoxy resin, and a curing accelerator having the function of accelerating the curing rate of the (B) epoxy resin. The curing accelerator is typically used in combination with an epoxy resin curing agent. The resin composition preferably contains either an epoxy resin curing agent or a curing accelerator as the (C) curing agent, and more preferably contains a curing accelerator. The (C) curing agent may be used alone or in combination of two or more types.
[0194] -Epoxy Resin Curing Agent- The epoxy resin curing agent typically reacts with the (B) epoxy resin to cure the resin composition. Examples of epoxy resin curing agents include phenol-based epoxy resin curing agents, naphthol-based epoxy resin curing agents, active ester-based epoxy resin curing agents, acid anhydride-based epoxy resin curing agents, benzoxazine-based epoxy resin curing agents, cyanate ester-based epoxy resin curing agents, and imidazole-based epoxy resin curing agents. From the viewpoint of significantly achieving the effects of the present invention, the epoxy resin curing agent is preferably one or more selected from phenol-based epoxy resin curing agents and naphthol-based epoxy resin curing agents. One epoxy resin curing agent may be used alone, or two or more may be used in combination.
[0195] As the phenolic epoxy resin curing agent and naphthol epoxy resin curing agent, from the viewpoint of heat resistance and water resistance, a phenolic epoxy resin curing agent having a novolac structure or a naphthol epoxy resin curing agent having a novolac structure is preferred. As the phenolic epoxy resin curing agent, a nitrogen-containing phenolic epoxy resin curing agent is preferred, a triazine skeleton-containing phenolic epoxy resin curing agent is more preferred, and a triazine skeleton-containing phenolic novolac epoxy resin curing agent is even more preferred.
[0196] Specific examples of phenol-based epoxy resin curing agents and naphthol-based epoxy resin curing agents include "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Chemical Industry Co., Ltd., "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd., "SN170", "SN180", "SN190", "SN475", "SN485", and "SN495V" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd. Examples include "SN375", "SN395", "TD-2090", "LA-7052", "LA-7054", "LA-1356", "LA-3018-50P", "EXB-9500", "HPC-9500", "KA-1160", "KA-1163", and "KA-1165" manufactured by DIC Corporation, and "GDP-6115L" and "GDP-6115H" manufactured by Gun-ei Chemical Co., Ltd.
[0197] The active ester-based epoxy resin curing agent is not particularly limited, but compounds having two or more highly reactive ester groups per molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, are generally preferred. The active ester-based epoxy resin curing agent is preferably one obtained by the condensation reaction of a carboxylic acid compound and / or a thiocarboxylic acid compound with a hydroxy compound and / or a thiol compound. From the perspective of improving heat resistance, active ester-based epoxy resin curing agents obtained from a carboxylic acid compound and a hydroxy compound are preferred, and active ester-based epoxy resin curing agents obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound are more preferred. Examples of carboxylic acid compounds include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcinol, bisphenol A, bisphenol F, bisphenol S, phenolphthalene, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolak, etc. Here, "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one dicyclopentadiene molecule with two phenol molecules.
[0198] Specifically, an active ester-based epoxy resin curing agent containing a dicyclopentadiene-type diphenol structure, an active ester-based epoxy resin curing agent containing a naphthalene structure, an active ester-based epoxy resin curing agent containing an acetylated product of phenol novolac, and an active ester-based epoxy resin curing agent containing a benzoylated product of phenol novolac are preferred. The "dicyclopentadiene-type diphenol structure" refers to a divalent structure consisting of phenylene-dicyclopentylene-phenylene.
[0199] Commercially available active ester epoxy resin curing agents include "EXB9451," "EXB9460," "EXB9460S," "HPC-8000-65T," "HPC-8000H-65TM," and "EXB-8000L-65TM" manufactured by DIC Corporation as active ester epoxy resin curing agents containing a dicyclopentadiene-type diphenol structure; "EXB9416-70BK" manufactured by DIC Corporation as an active ester compound containing a naphthalene structure; "DC808" manufactured by Mitsubishi Chemical Corporation as an active ester epoxy resin curing agent containing an acetylated product of phenol novolac; "YLH1026," "YLH1030," and "YLH1048" manufactured by Mitsubishi Chemical Corporation as active ester epoxy resin curing agents containing a benzoylated product of phenol novolac; and "DC808" manufactured by Mitsubishi Chemical Corporation as an active ester epoxy resin curing agent which is an acetylated product of phenol novolac.
[0200] Acid anhydride-based epoxy resin curing agents include epoxy resin curing agents having one or more acid anhydride groups in one molecule. Specific examples of acid anhydride-based epoxy resin curing agents include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenone tetracarbo Examples of suitable acid anhydrides include carboxylic acid dianhydride, biphenyltetracarboxylic acid dianhydride, naphthalenetetracarboxylic acid dianhydride, oxydiphthalic acid dianhydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic acid dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), and polymeric acid anhydrides such as styrene-maleic acid resins in which styrene and maleic acid are copolymerized.
[0201] Commercially available acid anhydride epoxy resin curing agents include "HNA-100" and "MH-700" manufactured by New Japan Chemical Co., Ltd.
[0202] Specific examples of benzoxazine-based epoxy resin curing agents include "HFB2006M" manufactured by Showa Highpolymer Co., Ltd., and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.
[0203] Examples of cyanate ester-based epoxy resin curing agents include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanatephenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanatephenyl-1-(methylethylidene))benzene, bis(4-cyanatephenyl)thioether, and bis(4-cyanatephenyl)ether; polyfunctional cyanate resins derived from phenol novolac, cresol novolac, etc.; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based epoxy resin curing agents include "PT30" and "PT60" (both of which are phenol novolac-type polyfunctional cyanate ester resins), "BA230" and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been triazinated to form a trimer), all of which are manufactured by Lonza Japan Co., Ltd.
[0204] Examples of imidazole-based epoxy resin curing agents include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, and 1-benzyl-2-phenylimidazoline. 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2- Examples thereof include imidazole compounds such as phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds with epoxy resins, with 2-ethyl-4-methylimidazole and 1-benzyl-2-phenylimidazole being preferred.
[0205] As the imidazole-based epoxy resin curing agent, commercially available products may be used, such as "2MZA-PW" and "2PHZ-PW" manufactured by Shikoku Chemical Industry Co., Ltd., and "P200-H50" manufactured by Mitsubishi Chemical Corporation.
[0206] The quantitative ratio of epoxy resin to epoxy resin curing agent, expressed as the ratio of [total number of epoxy groups in the epoxy resin] to [total number of reactive groups in the epoxy resin curing agent], is preferably in the range of 1:0.2 to 1:2, more preferably in the range of 1:0.3 to 1:1.5, and even more preferably in the range of 1:0.4 to 1:1. Here, the reactive groups in the epoxy resin curing agent are active hydroxyl groups, active ester groups, etc., and vary depending on the type of epoxy resin curing agent. Furthermore, the total number of epoxy groups in the epoxy resin is the sum of the values obtained by dividing the mass of the nonvolatile components of each epoxy resin by the epoxy equivalent weight for all epoxy resins, and the total number of reactive groups in the epoxy resin curing agent is the sum of the values obtained by dividing the mass of the nonvolatile components of each epoxy resin curing agent by the reactive group equivalent weight for all epoxy resin curing agents. By maintaining the quantitative ratio of epoxy resin to epoxy resin curing agent within this range, the heat resistance of the cured product is further improved.
[0207] From the viewpoint of significantly obtaining the effects of the present invention, the content of the epoxy resin curing agent is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more, based on 100% by mass of the non-volatile components in the resin composition, and the upper limit is preferably 1.5% by mass or less, more preferably 1% by mass or less, and even more preferably 0.8% by mass or less.
[0208] -Curing Accelerator- The curing accelerator typically acts as a catalyst in the curing reaction of the epoxy resin (B) and can accelerate the curing reaction. Examples of curing accelerators include amine-based curing accelerators, imidazole-based curing accelerators, phosphorus-based curing accelerators, guanidine-based curing accelerators, and metal-based curing accelerators. As the curing accelerator, from the viewpoint of reducing the viscosity of the resin composition, amine-based curing accelerators, imidazole-based curing accelerators, and guanidine-based curing accelerators are preferred, and from the viewpoint of improving the mechanical strength of the obtained cured product, imidazole-based curing accelerators are more preferred. One type of curing accelerator may be used alone, or two or more types may be used in combination. The curing accelerator is generally used in combination with an epoxy resin curing agent.
[0209] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene, with 4-dimethylaminopyridine and 1,8-diazabicyclo(5,4,0)-undecene being preferred.
[0210] As the amine-based curing accelerator, commercially available products may be used, such as "PN-50", "PN-23", and "MY-25" manufactured by Ajinomoto Fine-Techno Co., Ltd.
[0211] The imidazole-based curing accelerator is the same as the imidazole-based epoxy resin curing agent described above. When used in combination with other epoxy resin curing agents, the imidazole-based epoxy resin curing agent may function as a curing accelerator.
[0212] Examples of the phosphorus-based curing accelerator include triphenylphosphine, phosphonium borate compounds, tetraphenylphosphonium tetraphenylborate, n-butylphosphonium tetraphenylborate, tetrabutylphosphonium decanoate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate, with triphenylphosphine and tetrabutylphosphonium decanoate being preferred.
[0213] Examples of guanidine curing accelerators include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene. Examples of suitable biguanide include 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide. Of these, dicyandiamide and 1,5,7-triazabicyclo[4.4.0]dec-5-ene are preferred.
[0214] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organic cobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organic copper complexes such as copper(II) acetylacetonate, organic zinc complexes such as zinc(II) acetylacetonate, organic iron complexes such as iron(III) acetylacetonate, organic nickel complexes such as nickel(II) acetylacetonate, and organic manganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octoate, tin octoate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.
[0215] From the viewpoint of significantly obtaining the effects of the present invention, the content of the curing accelerator is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more, where the total amount of non-volatile components in the resin composition is 100% by mass, and the upper limit is preferably 1.5% by mass or less, more preferably 1% by mass or less, and even more preferably 0.8% by mass or less.
[0216] From the viewpoint of significantly obtaining the effects of the present invention, the content of the (C) curing agent is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more, based on 100% by mass of the non-volatile components in the resin composition, and the upper limit is preferably 1.5% by mass or less, more preferably 1% by mass or less, and even more preferably 0.8% by mass or less.
[0217] <(D) Dispersant> The resin composition may further contain a (D) dispersant as an optional component. The (D) dispersant as this (D) component does not include those corresponding to the above-mentioned (A) to (C) components. The (D) dispersant can effectively increase the dispersibility of the (A) magnetic powder, thereby effectively reducing the viscosity of the resin composition. One type of (D) dispersant may be used alone, or two or more types may be used in combination.
[0218] There are no limitations on the type of (D) dispersant. For example, the (D) dispersant may contain a functional group capable of adsorbing to the (A) magnetic powder, and when adsorbed to the (A) magnetic powder, disperse the (A) magnetic powder due to repulsion between the (D) dispersants (e.g., electrostatic repulsion, steric repulsion, etc.). Examples of such (D) dispersants include acidic dispersants and basic dispersants.
[0219] Acidic dispersants usually contain a carboxyl group, a sulfo group (-SO 3 H), sulfate group (-OSO 3 H), phosphono group (-PO(OH) 2 ), a phosphonooxy group (—OPO(OH) 2The acidic dispersant contains an acidic functional group such as a hydroxyphosphoryl group (-PO(OH)-), a sulfanyl group (-SH), or the like. The acidic functional group usually has a dissociable proton, and may be neutralized with a base such as an amine or hydroxide ion. Preferred examples of the acidic dispersant include acidic polymer dispersants containing a polymer chain such as a polyoxyalkylene chain or a polyether chain. Preferred examples of acidic dispersants include "C-2093I" and "SC-1015F (a polyfunctional comb-type functional polymer having an ionic group in the main chain and a polyoxyalkylene chain in the graft chain)" manufactured by NOF Corporation; "DA-375 (a polyether phosphate ester compound-based dispersant)" manufactured by Kusumoto Chemicals Co., Ltd.; "RS-410," "RS-610," and "RS-710" (pH 1.9) (phosphate ester-based dispersant) from the "Phosphanol" series manufactured by Toho Chemical Industry Co., Ltd.; and "AKM-0531," "AFB-1521," "SC-0505K," and "SC-0708A" from the "Marialim" series manufactured by NOF Corporation.
[0220] The basic dispersant typically contains basic functional groups such as primary, secondary, and tertiary amino groups; ammonium groups; imino groups; and nitrogen-containing heterocyclic groups such as pyridine, pyrimidine, pyrazine, imidazole, and triazole. The basic functional group may be neutralized with an acid such as an organic acid or an inorganic acid. Preferred examples of the basic dispersant include basic polymer dispersants containing polymer chains such as polyester chains. Preferred examples of the basic dispersant include "Ajisper PB881" (a polyamine-based dispersant containing polyester chains) manufactured by Ajinomoto Fine-Techno Co., Ltd.
[0221] From the viewpoint of significantly obtaining the effects of the present invention, the content of the (D) dispersant is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more, based on 100% by mass of the non-volatile components in the resin composition, and the upper limit is preferably 2.0% by mass or less, more preferably 1.5% by mass or less, and even more preferably 1.0% by mass or less.
[0222] <(E) Reactive Diluent> The resin composition may contain a (E) reactive diluent as an optional component. The (E) reactive diluent as component (E) does not include any of the above-mentioned components (A) to (D). In general, when a resin composition contains a large amount of component (A), the viscosity of the resin composition increases. However, by including component (E) in the resin composition, it is possible to reduce the viscosity of the resin composition.
[0223] From the viewpoint of reducing the viscosity of the resin composition, the viscosity of the (E) reactive diluent is preferably 0.001 Pa s or more, more preferably 0.005 Pa s or more, and even more preferably 0.01 Pa s or more. The upper limit is preferably less than 0.5 Pa s. The viscosity of the reactive diluent can be measured in the same manner as the viscosity of the (B) epoxy resin.
[0224] The reactive diluent (E) preferably has a reactive group from the viewpoint of improving mechanical strength. Examples of the reactive group include an epoxy group, an acrylic group, a methacrylic group, and an oxetane group. Among these, the reactive group is preferably an epoxy group from the viewpoint of further reducing the viscosity of the resin composition.
[0225] Commercially available products can be used as the (E) reactive diluent. Specific examples of commercially available (C) reactive diluents that can be used include "EX-201" (alicyclic glycidyl ether), EX-830, EX-821 (ethylene glycol-type epoxy resins), and EX-212 (hexanediol-type epoxy resin), all manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane); "EP-3980S" (glycidylamine-type epoxy resin), "EP-4088S," and "EP-4088L" (dicyclopentadiene-type epoxy resin), and ED-509S (tert-butylphenyl glycidyl ether), all manufactured by ADEKA Corporation; and X-22-163 (siloxane-type epoxy resin), all manufactured by Shin-Etsu Chemical Co., Ltd. These may be used alone or in combination of two or more.
[0226] When the (E) reactive diluent has a glycidyl group or an epoxy group, the epoxy equivalent of the (E) reactive diluent is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., even more preferably 60 g / eq. to 2000 g / eq., and still more preferably 70 g / eq. to 1000 g / eq. When the epoxy equivalent is within this range, a cured product having sufficient crosslink density can be obtained.
[0227] From the viewpoint of obtaining a resin composition having a suitable viscosity, the content of the (E) reactive diluent is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more, and is preferably 15% by mass or less, more preferably 13% by mass or less, and even more preferably 10% by mass or less, based on 100% by mass of the non-volatile components in the resin composition.
[0228] <(F) Other Additives> The resin composition may further contain (F) other additives as an optional component in combination with the above-described (A) to (E) components. The (F) other additives as the (F) component do not include those corresponding to the above-described (A) to (E) components.
[0229] (F) Other additives include, for example, thermoplastic resins such as phenoxy resins, polyimide resins, polyvinyl acetal resins, polyolefin resins, polybutadiene resins, polyamideimide resins, polyetherimide resins, polysulfone resins, polyethersulfone resins, polyphenylene ether resins, polycarbonate resins, polyetheretherketone resins, and polyester resins; radical polymerizable compounds such as maleimide-based radical polymerizable compounds, vinylphenyl-based radical polymerizable compounds, (meth)acrylic-based radical polymerizable compounds, allyl-based radical polymerizable compounds, and polybutadiene-based radical polymerizable compounds; radical polymerization initiators such as peroxide-based radical polymerization initiators and azo-based radical polymerization initiators; inorganic particles (inorganic fillers) such as silica particles; organic fillers such as rubber particles; organometallic compounds such as organocopper compounds and organozinc compounds; polymerizable compounds such as hydroquinone, catechol, pyrogallol, and phenothiazine. antifoaming agents such as silicone-based leveling agents and acrylic polymer-based leveling agents; thickeners such as bentone and montmorillonite; antifoaming agents such as silicone-based defoaming agents, acrylic-based defoaming agents, fluorine-based defoaming agents, and vinyl resin-based defoaming agents; ultraviolet absorbers such as benzotriazole-based ultraviolet absorbers; adhesion improvers such as urea silanes; adhesion imparting agents such as triazole-based adhesion imparting agents, tetrazole-based adhesion imparting agents, and triazine-based adhesion imparting agents; antioxidants such as hindered phenol-based antioxidants; flame retardants such as phosphorus-based flame retardants (e.g., phosphate ester compounds, phosphazene compounds, phosphinic acid compounds, and red phosphorus), nitrogen-based flame retardants (e.g., melamine sulfate), halogen-based flame retardants, and inorganic flame retardants (e.g., antimony trioxide); and stabilizers such as borate-based stabilizers, titanate-based stabilizers, aluminate-based stabilizers, zirconate-based stabilizers, isocyanate-based stabilizers, carboxylic acid-based stabilizers, and carboxylic anhydride-based stabilizers. (F) Other additives may be used alone or in combination of two or more.
[0230] <Characteristics of Resin Composition> The resin composition of the present invention uses component (A-1) as a magnetic powder, and therefore is not easily dissolved in a treatment solution used in a wet plating process in manufacturing a substrate. Therefore, even if a conductor layer is formed by wet plating, a decrease in the relative permeability of the magnetic cured product can be suppressed.
[0231] The cured product obtained by heating the resin composition at 190°C for 90 minutes is resistant to acid, and exhibits the characteristic of a high relative magnetic permeability after impregnation with 5 mol / L hydrochloric acid. For example, the relative magnetic permeability of the cured product of the resin composition after impregnation with hydrochloric acid, measured under measurement conditions of a measurement frequency of 50 MHz and a measurement temperature of 23°C, is preferably 4 or more, more preferably 6 or more, and even more preferably 8 or more. There is no particular upper limit, and it can be, for example, 50 or less. The relative magnetic permeability after impregnation with hydrochloric acid can be measured using the method described in the Examples below.
[0232] The cured product obtained by heating the resin composition at 190°C for 90 minutes is resistant to acid and exhibits a low loss factor after impregnation with 5 mol / L hydrochloric acid. For example, the loss factor of the cured product of the resin composition measured under measurement conditions of a measurement frequency of 50 MHz and a measurement temperature of 23°C is preferably 0.1 or less, more preferably 0.05 or less, and even more preferably 0.03 or less. There is no particular restriction on the lower limit, and it can be, for example, 0.001 or more. The loss factor after impregnation with hydrochloric acid can be measured using the method described in the Examples below.
[0233] The cured product obtained by heating the resin composition at 190°C for 90 minutes is resistant to acid and exhibits a low weight loss rate after impregnation in 5 mol / L hydrochloric acid. The weight loss rate is preferably 7% or less, more preferably 6% or less, and even more preferably 5% or less. There is no particular restriction on the lower limit, and it can be, for example, 0% or more, 0.1% or more, etc. The weight loss rate can be measured by the method described in the examples below.
[0234] A cured product obtained by heating a resin composition at 190°C for 90 minutes exhibits the characteristic of having a high relative magnetic permeability before impregnation with hydrochloric acid. For example, the relative magnetic permeability of a cured product of the resin composition measured under measurement conditions of a measurement frequency of 50 MHz and a measurement temperature of 23°C is preferably 4 or more, more preferably 6 or more, and even more preferably 8 or more. There is no particular upper limit, and it can be, for example, 50 or less. The relative magnetic permeability before impregnation with hydrochloric acid can be measured using the method described in the Examples below.
[0235] A cured product obtained by heating a resin composition at 190°C for 90 minutes exhibits the characteristic of a low loss factor before impregnation with hydrochloric acid. For example, the loss factor of a cured product of the resin composition measured under measurement conditions of a measurement frequency of 50 MHz and a measurement temperature of 23°C is preferably 0.1 or less, more preferably 0.05 or less, and even more preferably 0.03 or less. There is no particular restriction on the lower limit, and it can be, for example, 0.001 or more. The loss factor before impregnation with hydrochloric acid can be measured using the method described in the Examples below.
[0236] The cured product obtained by heating the resin composition at 190°C for 90 minutes is resistant to acid, and exhibits the characteristic of a low rate of decrease in relative permeability after impregnation with hydrochloric acid. The rate of decrease in relative permeability is preferably 10% or less, more preferably 9% or less, and even more preferably 8% or less, 7% or less, 6% or less, or 5% or less. There is no particular restriction on the lower limit, and it can be, for example, 0% or more, 0.1% or more, etc. The rate of decrease in relative permeability can be measured by the method described in the examples below.
[0237] <Method for Producing Resin Composition> The resin composition can be produced, for example, by stirring the blending components using a stirring device such as a three-roll mill, a rotary mixer, or a high-speed rotary mixer. The resin composition may be defoamed after production, etc. Examples of defoaming methods include defoaming by leaving the composition to stand, defoaming by centrifugation, vacuum defoaming, defoaming by stirring, and combinations of these.
[0238] When forming a magnetic cured product for a circuit board, the resin composition may be used in the form of a paste-like resin composition (magnetic paste), or in the form of a magnetic sheet including a layer of the resin composition.
[0239] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following description, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified.
[0240] Example 1 Preparation of Magnetic Paste 1 15 parts by mass of epoxy resin ("ZX-1059", a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin, manufactured by Nippon Steel Chemical & Material Co., Ltd., viscosity at 25°C of 2000 mPa·s), 5 parts by mass of reactive diluent ("ZX-1658GS", a cyclic aliphatic diglycidyl ether, manufactured by Nippon Steel Chemical & Material Co., Ltd., viscosity at 25°C of 34 mPa·s), 1 part by mass of acidic dispersant ("C-209 Magnetic paste 1 was prepared by mixing 1.1 parts by mass of "3I", an acidic dispersant for nanoparticles, manufactured by NOF Corporation), 1 part by mass of a curing agent ("2MZA-PW", an imidazole-based epoxy resin curing agent, manufactured by Shikoku Chemicals Corporation), and 150 parts by mass of magnetic powder ("MZ05SIP", an Mn-Zn ferrite, Fe content 62.9% by mass, Mn content 7.9% by mass, Zn content 1.0% by mass, average particle size 3 μm, manufactured by Powder Tech Co., Ltd.).
[0241] Example 2 Preparation of Magnetic Paste 2 In Example 1, 1) 150 parts by mass of magnetic powder ("MZ05SIP", Mn-Zn ferrite, Fe content 62.9% by mass, Mn content 7.9% by mass, Zn content 1.0% by mass, average particle size 3 μm, manufactured by Powder Tech Co., Ltd.) was changed to 150 parts by mass of magnetic powder ("MZ05SMC", Fe content 58.4% by mass, Mn content 10.7% by mass, Zn content 3.0% by mass, average particle size 3 μm, manufactured by Powder Tech Co., Ltd.), and 2) 1.1 parts by mass of dispersant ("PB881", polyamine-based dispersant, manufactured by Ajinomoto Fine-Techno Co., Ltd.) was further used. Magnetic paste 2 was prepared in the same manner as in Example 1 except for the above.
[0242] Example 3 Preparation of Magnetic Paste 3 In Example 2, 1.1 parts by mass of dispersant ("PB881", polyamine-based dispersant, manufactured by Ajinomoto Fine-Techno Co., Inc.) was changed to 1.1 parts by mass of dispersant ("SC-1015F", acidic dispersant for nanoparticles, manufactured by NOF Corporation). Magnetic paste 3 was prepared in the same manner as in Example 1, except for the above.
[0243] Example 4 Preparation of Magnetic Paste 4 In Example 3, 1) the amount of magnetic powder ("MZ05SMC", Fe-Mn ferrite, Fe content 56.7% by mass, Mn content 12.3% by mass, Zn content 2.9% by mass, average particle size 3 μm, manufactured by Powder Tech Co., Ltd.) was changed from 150 parts by mass to 140 parts by mass, 2) further, magnetic powder ("M03S", Fe-Mn ferrite, Fe content 62.2% by mass, Mn content 8.1% by mass, average particle size 0.5 μm, specific gravity 5.1 m) manufactured by Powder Tech Co., Ltd. 2 Magnetic paste 4 was prepared in the same manner as in Example 3 except for the above points.
[0244] <Comparative Example 1> In Example 1, 1) 150 parts by mass of magnetic powder ("MZ05SIP", Mn-Zn ferrite, Fe content 62.9% by mass, Mn content 7.9% by mass, Zn content 1.0% by mass, average particle size 3 μm, manufactured by Powder Tech Co., Ltd.) was added to magnetic powder ("MZ05S", Fe-Mn ferrite, Fe content 54.8% by mass, Mn content 13.5% by mass, Zn content 3.57% by mass, average particle size 3.0 μm, specific surface area 0.68 m 2 / g, specific gravity 5.1g / cm 3 1) The magnetic paste 5 was prepared in the same manner as in Example 1, except for the above points.
[0245] <Comparative Example 2> In Example 2, 150 parts by mass of magnetic powder ("MZ05SMC", Fe content 58.4 mass%, Mn content 10.7 mass%, Zn content 3.0 mass%, average particle size 3 μm, manufactured by Powder Tech Co., Ltd.) was mixed with magnetic powder ("AW2-08 PF3F", Fe-Cr-Si alloy (amorphous), average particle size 3.0 μm, specific surface area 0.66 m) 2 / g, specific gravity 7.11g / cm 3 Magnetic paste 6 was prepared in the same manner as in Example 2, except for the above points.
[0246] Comparative Example 3 In Example 1, 1) 150 parts by mass of magnetic powder ("MZ05SIP", Mn-Zn ferrite, Fe content 62.9% by mass, Mn content 7.9% by mass, Zn content 1.0% by mass, average particle size 3 μm, manufactured by Powder Tech Co., Ltd.) was mixed with magnetic powder ("MA-RCO-5", Fe-Ni alloy, average particle size 3.0 μm, specific surface area 0.45 m) 2 / g, specific gravity 8.0g / cm 3 1) The magnetic paste 7 was prepared in the same manner as in Example 1, except for the above points.
[0247] <Measurement of relative magnetic permeability and loss factor before hydrochloric acid impregnation> A polyethylene terephthalate (PET) film ("PET501010" manufactured by Lintec Corporation, thickness 50 μm) treated with a silicone-based release agent was prepared as a support. Each of the magnetic pastes 1 to 7 was uniformly applied to the release surface of the PET film using a doctor blade so that the thickness of the resin composition layer after drying was 100 to 110 μm, thereby obtaining a magnetic sheet. The obtained magnetic sheet was heated at 190°C for 90 minutes to thermally cure the resin composition layer, and the support was peeled off to obtain a sheet-like cured product. Both sides of the obtained cured product were polished with sandpaper #320. The polished cured product was cut into a toroidal test piece with an outer diameter of 19 mm and an inner diameter of 9 mm, which was used as an evaluation sample.
[0248] Six of these evaluation samples were stacked, and the relative permeability (μ') and magnetic loss (μ'') were measured using Keysight Technologies (manufactured by Keysight Technologies, Inc., "16454A E4991B") at a measurement frequency of 50 MHz and room temperature of 23°C. The loss factor was calculated from μ'' / μ'.
[0249] <Measurement of relative magnetic permeability and loss factor after hydrochloric acid impregnation> Six evaluation samples were immersed in a sample vial containing 100 mL of 5 mol / L hydrochloric acid, placed in an ultrasonicator, and exposed to ultrasonic waves for 1 hour. The six evaluation samples were removed, washed with water, and dried in a desiccator for 24 hours or more. After drying, the relative magnetic permeability was measured and the loss factor was calculated using the same method as before the hydrochloric acid impregnation.
[0250] <Reduction Rate of Relative Permeability> The relative permeability after impregnation with hydrochloric acid was divided by the relative permeability before impregnation with hydrochloric acid, and the result was subtracted from 1 to obtain the reduction rate (%) of relative permeability.
[0251] <Calculation of Weight Reduction Rate> (Measurement of Weight Before Impregnation with Hydrochloric Acid) The weights of the six evaluation samples before impregnation with hydrochloric acid were measured using a precision balance.
[0252] (Measurement of Weight After Impregnation with Hydrochloric Acid) The weight of each of the six evaluation samples after impregnation with hydrochloric acid was measured using a precision balance.
[0253] (Calculation of Weight Loss Rate) The weight loss rate was calculated as follows: Weight loss rate %=1−(weight after hydrochloric acid impregnation / weight before hydrochloric acid impregnation).
[0254] <Evaluation of Acid Resistance> Acid resistance was evaluated as follows. Acid resistance was judged from the rate of decrease in relative permeability, and was evaluated according to the following criteria from the viewpoint of the performance stability of the inductor. Note that a lower rate of decrease in relative permeability means better acid resistance. ○: Rate of decrease in relative permeability is less than 5% ×: Rate of decrease in relative permeability is 5% or more
[0255]
[0256] Example A: Fabrication of Circuit Board (Preparation of Support Substrate) A glass cloth epoxy resin double-sided copper-clad laminate (copper foil thickness 18 μm, substrate thickness 1.0 mm, R1515A manufactured by Matsushita Electric Works, Ltd.) with a plurality of uniformly formed through-holes was prepared as a support substrate. The through-holes were cylindrical holes with a diameter of 450 μm and a spacing of 100 μm between the through-holes.
[0257] (Preparation of Mask) A metal mask was prepared as a mask, which was a 100 μm thick metal plate having an opening formed therein as a hollow hole. The planar shape of the opening was a square with a side of 20 mm.
[0258] (Printing of Magnetic Paste) Using the above mask, magnetic paste 1 was printed on the support substrate in the following manner. The printing was performed using a vacuum high-precision screen printer ("LS-100VC" manufactured by Newlong Precision Industry Co., Ltd.).
[0259] A mask was placed on one side of the support substrate such that each opening in the mask communicated with a plurality of through-holes in the support substrate.
[0260] Thereafter, magnetic paste 1 was applied to the surface of the mask opposite to the support substrate.
[0261] Then, a rubber squeegee (manufactured by Newlong Precision Industry Co., Ltd., "SVFSQ", thickness 9 mm, rubber hardness 90 degrees) made of rubber as an elastic material was moved along the surface of the mask to print magnetic paste 1. The squeegee attack angle was 5°, the printing pressure was 4.4 MPa, and the printing speed was 5 mm / sec. The squeegee moved across the opening of the mask while maintaining a pool of magnetic paste ahead of the squeegee's movement direction. This operation swept the magnetic paste with the squeegee, filling the through-holes with magnetic paste 1.
[0262] The prepared magnetic paste 1 was uniformly applied with a doctor blade onto a support substrate filled with magnetic paste 1 to form a paste layer approximately 120 μm thick. The paste layer was heated at 130° C. for 30 minutes and then at 145° C. for 30 minutes to be thermally cured, forming a magnetically cured product.
[0263] (Polishing) The surface of the formed magnetic cured product was polished with a ceramic roll (Ishii Hyoki Co., Ltd., #1500), then washed with high-pressure water (3.0 MPa, 15 seconds), and heat-treated by heating at 180°C for 30 minutes.
[0264] (Drilling) Through holes were drilled in the magnetic cured material using a drill (trade name "NEU 108-W150" (φ150 μm, length 2 mm) manufactured by Union Tool Co., Ltd. Specifically, while rotating the drill at 80,000 rpm, holes were drilled at a feed rate of 0.5 m / min with a pitch of 550 μm.
[0265] (Plating Treatment) The support substrate on which the magnetic cured material was formed was subjected to electroless copper plating and electroplating to form a conductor layer having a thickness of 25 μm on the surface of the substrate and inside the through-holes formed with a drill.
[0266] (Patterning) A dry film was laminated on the conductor layer, exposed to light, developed, and patterned. Next, a patterned conductor layer was formed by a subtractive method using an iron chloride etching solution, and then the dry film was peeled off to produce an inductor-embedded substrate.
[0267] REFERENCE SIGNS LIST 10 Core substrate 11 Support substrate 12 First metal layer 13 Second metal layer 14 Through hole 20 Plating layer 30a Resin composition 30 Magnetic cured material 40 Conductor layer 41 Patterned conductor layer 100 Inductor component 200 Inner layer substrate 200a First main surface 200b Second main surface 220 Through hole 220a Wiring inside through hole 240 External terminal 300 Magnetic part 310 Magnetic sheet 320a Resin composition layer 320 First magnetic cured material layer 330 Support 340 Second magnetic cured material layer 360 Via hole 360a Wiring inside via hole 400 Coil-shaped conductive structure 420 First conductor layer 420a Land 440 Second conductor layer
Claims
1. A method for producing a circuit board comprising the steps of: (1) thermally curing a resin composition to obtain a magnetic cured product; (2) polishing at least a portion of the surface of the magnetic cured product; and (3) forming a conductor layer by wet plating on at least a portion of the polished surface of the magnetic cured product, in this order; wherein the resin composition comprises (A) a magnetic powder, (B) an epoxy resin, and (C) a curing agent; the (A) component comprises (A-1) a ferrite containing manganese and zinc; the iron content in the (A-1) component is 56% by mass or more and 63% by mass or less; the manganese content in the (A-1) component is 7% by mass or more and 13% by mass or less; and the zinc content in the (A-1) component is 1% by mass or more and 3% by mass or less.
2. A method for producing a circuit board as described in claim 1, in which the cured product obtained by heating the resin composition at 190°C for 90 minutes has a relative magnetic permeability reduction rate of 10% or less after being immersed in hydrochloric acid.
3. The method for producing a circuit board according to claim 1, wherein the resin composition is in a paste form.
4. The method for producing a circuit board according to claim 1, wherein the resin composition forms a resin composition layer.
5. A resin composition comprising: (A) a magnetic powder; (B) an epoxy resin; and (C) a curing agent; the (A) component comprises (A-1) a ferrite containing manganese and zinc; the iron content in the (A-1) component is 56% by mass or more and 63% by mass or less; the manganese content in the (A-1) component is 7% by mass or more and 13% by mass or less; and the zinc content in the (A-1) component is 1% by mass or more and 3% by mass or less.
6. The resin composition according to claim 5, which is a resin composition for use in a method for manufacturing a circuit board, comprising the steps of: (1) thermally curing the resin composition to obtain a magnetic cured product; (2) polishing at least a portion of the surface of the magnetic cured product; and (3) forming a conductor layer by wet plating on at least a portion of the polished surface of the magnetic cured product, in that order.
Citation Information
Patent Citations
Magnetic paste
JP2021097110A
Resin composition
JP2021141295A
Resin composition
JP2022064640A
Mn-zn ferrite particles, resin molded body, soft magnetic mixed powder, and magnetic core
WO2019065923A1
Ferrite powder, ferrite resin composite material, and electromagnetic shielding material, electronic material, or electronic component
WO2022209640A1