Composite compound for low dielectric loss resin compositions, low dielectric loss resin composition, molded body for high frequency devices, and high frequency device

The use of inorganic fluoride with thermally fused PTFE particles in a composite compound addresses the high dielectric loss issues in high-frequency equipment, enhancing signal transmission and chemical resistance within high-frequency bands.

WO2024204090A1PCT designated stage expired Publication Date: 2024-10-03STELLA CHEMIFA CORP

Patent Information

Application Number
PCT/JP2024/011750
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional resin compositions for high-frequency equipment exhibit high dielectric constants and dielectric loss tangents in high-frequency bands, leading to signal attenuation and reduced transmission reliability, and they often have poor affinity with polymer resins and chemical resistance.

Method used

A composite compound is developed using inorganic fluoride as a base material with fluororesin particles thermally fused to its surface, specifically using polytetrafluoroethylene (PTFE) particles, to reduce dielectric constants and tangents, and incorporating these particles into a polymer resin to enhance affinity and chemical resistance.

Benefits of technology

The solution effectively reduces dielectric loss and signal attenuation in high-frequency bands, improving signal transmission speed and reliability while maintaining good affinity with polymer resins and chemical resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011750_03102024_PF_FP_ABST
    Figure JP2024011750_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: a novel composite compound for low dielectric loss resin compositions, the composite compound suppressing the loss coefficient in a high frequency band and having a good dielectric loss; a low dielectric loss resin composition; a molded body for high frequency devices; and a high frequency device. A composite compound for low dielectric loss resin compositions according to the present invention is for use in a low dielectric loss resin composition, and is characterized by containing a base material that is composed of an inorganic fluoride, and fluororesin particles that are held on at least a part of the surface of the base material. This composite compound for low dielectric loss resin compositions is also characterized in that the dielectric loss tangent of the fluororesin particles is 0.002 or less at a frequency of 1 GHz or more and a temperature of 25°C.
Need to check novelty before this filing date? Find Prior Art

Description

Composite compound for low dielectric loss resin composition, low dielectric loss resin composition, molded article for high frequency device, and high frequency device

[0001] The present invention relates to a composite compound for a low dielectric loss resin composition that can be used in electronic components such as circuit boards, information and communication devices, etc., a low dielectric loss resin composition, a molded article for high-frequency devices, and a high-frequency device.

[0002] BACKGROUND ART In recent years, in electronic components such as printed wiring boards, flexible circuit boards and high frequency boards, as well as in information and communication devices, the frequency of electrical signals used has been increasing in order to achieve high speed and large capacity data communication.

[0003] In particular, in electronic components for high-frequency applications, the attenuation of electrical signals increases due to transmission loss in the transmission path as the frequency increases, which can lead to a decrease in transmission reliability. Therefore, materials with a small loss factor are required for high-frequency devices and their components. Here, the loss factor is calculated by dividing the dielectric constant (ε r ) and the dielectric loss tangent (tan δ).

[0004] For example, Patent Document 1 discloses a thermosetting resin composition containing, as essential components, (A) a polyimide resin having a carboxyl group or an acid anhydride group and a linear hydrocarbon structure with a number average molecular weight of 300 to 6,000, (B) an epoxy resin, (C) an organic solvent with a boiling point of 100°C or higher, and spherical silica, with the aim of achieving a low relative dielectric constant and low dielectric loss tangent for a multilayer printed circuit board. According to Patent Document 1, it is possible to form an interlayer insulating resin layer that has sufficient adhesion to a conductor and has high heat resistance, flame retardancy, a low dielectric constant, a low dielectric loss tangent, and a low water absorption.

[0005] Patent Document 2 discloses an inorganic filler whose surface has been modified by sequentially introducing an alkyl group and an amine group, which has excellent compatibility and reactivity with epoxy resins. According to Patent Document 2, by producing an epoxy resin composition using this surface-modified inorganic filler such as silica, it is possible to impart the property of a low dielectric loss factor.

[0006] Furthermore, Patent Document 3 discloses a surface-treated metal oxide particulate material having a metal oxide particulate material such as silica and a polyorganosiloxane compound that surface-treats the metal oxide particulate material. According to Patent Document 3, by incorporating the surface-treated metal oxide particulate material into a resin material, it is possible to suppress the viscosity of the resulting resin composition and also to suppress the relative dielectric constant and dielectric loss tangent of the resin composition.

[0007] However, the resin compositions disclosed in Patent Documents 1 to 3 still have large relative permittivity and dielectric loss tangent in the high frequency band, and therefore, further reduction in dielectric loss is desired.

[0008] Japanese Patent No. 5564012 Japanese Patent Application Laid-Open No. 2015-67534 Japanese Patent Application Laid-Open No. 2020-66678

[0009] The present invention aims to provide a novel composite compound for a low dielectric loss resin composition, which reduces the relative dielectric constant and dielectric loss tangent in the high frequency band and is excellent in reducing dielectric loss, a low dielectric loss resin composition, a molded article for high frequency devices, and a high frequency device.

[0010] In order to solve the above-mentioned problems, the composite compound for a low dielectric loss resin composition of the present invention is a composite compound for a low dielectric loss resin composition, which comprises a base material made of an inorganic fluoride and fluororesin particles held on at least a portion of the surface of the base material, and is characterized in that the dielectric loss tangent of the fluororesin particles is 0.002 or less at a frequency of 1 GHz or more and a temperature of 25°C.

[0011] In the above-mentioned configuration, it is preferable that the fluororesin particles are held on the surface of the inorganic fluoride matrix by thermal fusion.

[0012] In the above-mentioned configuration, the fluororesin is preferably polytetrafluoroethylene.

[0013] In the above-mentioned structure, the inorganic fluoride is MFn (wherein M is at least one selected from the group consisting of Li, Na, K, Mg, Al, Ca, Sc, Mn, Fe, Ga, Rb, Sr, Y, Zr, Sn, Ba, La, Ce, Yb, Hf and Bi, and n is an integer of 1 to 4) or K 2 SiF 6 It is preferable that:

[0014] Furthermore, in the above-mentioned structure, the inorganic fluoride is AlF 3 It is preferable that:

[0015] In the above-mentioned composition, it is preferable that the base material made of the inorganic fluoride has an average particle diameter D50 of 0.05 μm or more and 75 μm or less.

[0016] In the above-mentioned configuration, the content of the fluororesin particles is preferably 0.5% by mass or more and less than 26% by mass with respect to the total mass of the base material made of the inorganic fluoride.

[0017] In order to solve the above-mentioned problems, the low dielectric loss resin composition of the present invention is characterized by containing at least a polymer resin and the composite compound for the low dielectric loss resin composition.

[0018] In the above-mentioned composition, the content of the composite compound is preferably 1% by mass or more and 85% by mass or less with respect to the total mass of the low dielectric loss resin composition.

[0019] In the above-mentioned configuration, it is preferable that the polymer resin contains at least one kind of thermoplastic resin and / or at least one kind of thermosetting resin.

[0020] Furthermore, in the above-mentioned configuration, it is preferable that the polymer resin is at least one selected from the group consisting of olefin resins, styrene resins, polyvinyl resins, methacrylic resins, thermoplastic elastomer resins, thermoplastic polyurethane resins, polyacrylonitrile resins, polylactic acid resins, polyamide polyacetal resins, polycarbonate resins, polyphenylene ether resins, polyethylene terephthalate resins, polysulfone resins, polyether sulfone resins, polyphenylene sulfide resins, polyether ether ketone resins, liquid crystal polymer resins, polyimide resins, fluororesins, phenolic resins, amine resins, furan resins, unsaturated polyester resins, epoxy resins, diallyl phthalate resins, guanamine resins, ketone resins, silicone resins, thermosetting elastomer resins, natural rubber, synthetic rubber, and modified products thereof.

[0021] In order to solve the above-mentioned problems, the molded article for high-frequency devices of the present invention is a molded article for high-frequency devices used in a frequency band of 1 GHz or more, and is characterized in that it is a molded article containing the low dielectric loss resin composition.

[0022] In order to solve the above-mentioned problems, the high-frequency device of the present invention is a high-frequency device used in a frequency band of 1 GHz or more, and is characterized by containing the low dielectric loss resin composition described above.

[0023] In order to solve the above-mentioned problems, the high-frequency device of the present invention is a high-frequency device used in a frequency band of 1 GHz or more, and is characterized by including the above-mentioned molded article for high-frequency devices.

[0024] According to the present invention, a composite compound having fluororesin particles supported on at least a portion of the surface of an inorganic fluoride matrix can be incorporated into a low dielectric loss resin composition in place of conventional inorganic fillers such as silica. This reduces the loss factor in the high frequency band, thereby reducing dielectric loss. Furthermore, by using a low dielectric loss resin composition containing this composite compound in a molded article for high frequency devices or in high frequency devices, attenuation of electrical signals due to transmission loss can be suppressed even when used in the high frequency band of 1 GHz or higher, enabling high-speed, high-frequency transmission.

[0025] FIG. 1(a) shows the α-AlF 3 and PTFE particles, and Fig. 1(b) shows the SEM image of α-AlF 3 2(a) is an SEM image of a composite compound in which PTFE particles are thermally fused to the surface of α-AlF 3 and PTFE particles, and Fig. 2(b) shows the SEM image of α-AlF 3 3(a) is an SEM image of a composite compound in which PTFE particles are thermally fused to the surface of α-AlF 3 and PTFE particles, and Fig. 3(b) shows the SEM image of α-AlF 3 4(a) is an SEM image of a composite compound in which PTFE particles are thermally fused to the surface of CaF 2 and PTFE particles, and Fig. 4(b) shows the SEM image of CaF 2 5(a) is an SEM image of a composite compound in which PTFE particles are thermally fused to the surface of α-AlF 3 and PTFE particles, and Fig. 5(b) shows the SEM image of α-AlF 3 6(a) is an SEM image of a composite compound in which PTFE particles are heat-fused to the surface of silica according to Comparative Example 4. FIG. 6(b) is an SEM image of a composite composed of silica and PTFE particles. FIG. 7(a) is a reference photograph showing the state in which the slurry composition falls smoothly, and FIG. 7(b) is a reference photograph showing the state in which the slurry composition falls in clumps.

[0026] (Composite Compound for Low Dielectric Loss Resin Composition) First, the composite compound for the low dielectric loss resin composition according to this embodiment (hereinafter referred to as the "composite compound") will be described below.

[0027] The composite compound of this embodiment includes a base material (hereinafter sometimes referred to as "base material") made of an inorganic fluoride and fluororesin particles (hereinafter sometimes referred to as "fluororesin particles") held on at least a portion of the surface of the base material. Herein, the phrase "held" on at least a portion of the surface of the base material refers to the case where the fluororesin particles are held (immobilized) by chemical bonding to the surface of the base material, as well as the case where the fluororesin particles are thermally fused to the surface of the base material and physically held (immobilized). In this embodiment, the composite compound is preferably a case where the fluororesin particles are held on the surface of the base material by thermal fusion. Furthermore, in this specification, "thermal fusion" refers to a state in which fluororesin particles, at least the surface of which has been thermally fused by heating, come into contact with the base material made of an inorganic fluoride, and the fluororesin particles are fixed to the base material at the contact surface. The melting point of the fluororesin is usually lower than that of the inorganic fluoride.

[0028] In the present invention, by supporting fluororesin particles on the surface of an inorganic fluoride matrix, the dielectric constant and dielectric dissipation factor can be reduced in the high frequency range, thereby reducing dielectric loss, compared to when only inorganic fluorides are included in the low dielectric loss resin composition. Generally, inorganic fluorides have higher dielectric constants and dielectric dissipation factors in the high frequency range than silica. Therefore, it is conceivable to support fluororesin on the surface of silica matrix. However, it has been found that, although the dielectric constant can be reduced, the dielectric dissipation factor cannot be reduced. Furthermore, it has been found that poor affinity with polymer resins makes it difficult to obtain a low dielectric loss resin composition in which the fluororesin particles are uniformly dispersed in the polymer resin. Furthermore, when such low dielectric loss resin compositions are used as materials for electronic components, for example, they exhibit poor chemical (alkali) resistance, e.g., silica elution upon contact with alkaline solutions during alkaline etching.

[0029] On the other hand, in the present invention, an inorganic fluoride is selected from among many inorganic fillers as the base material, and a fluororesin is further selected from among many polymer resins as the polymer resin to be attached to the surface of the base material. It has been found that this allows the relative dielectric constant and dielectric loss tangent in the high frequency band to be reduced compared to silica alone or when a fluororesin is attached to the surface of the silica. Furthermore, it has been found that the affinity with the polymer resin is good, making it possible to obtain a resin composition in which the composite compound is uniformly dispersed, and that the composition also has excellent chemical resistance.

[0030] Dielectric constant ε of composite compound r0 The upper limit of [-] is preferably 6 or less, more preferably 4 or less, and particularly preferably 3 or less, at a frequency of 1 GHz or more and a temperature of 25°C. r0 When the loss factor is 6 or less, the loss factor can be reduced, and the dielectric loss can be reduced.

[0031] In addition, the dielectric loss tangent tanδ of the composite compound 0 The upper limit of [-] is preferably 0.01 or less, more preferably 0.005 or less, even more preferably 0.002 or less, and particularly preferably 0.001 or less, at a frequency of 1 GHz or more and a temperature of 25°C. 0 When the loss factor is 0.01 or less, the loss factor can be reduced, and the dielectric loss can be reduced.

[0032] The upper limit of the loss factor of the composite compound is preferably less than 6, more preferably not more than 4, and particularly preferably not more than 3. When the loss factor is less than 6, the loss factor of the composite compound can be reduced, and the dielectric loss can be reduced.

[0033] The relative permittivity ε used to quantify the dielectric properties and dielectric loss r0 and dielectric tangent tanδ 0 The numerical values ​​of the above are based on the values ​​obtained by measuring the composite compound. The measurement method can be selected appropriately. Specifically, for example, each of the values ​​can be measured by the method described in the Examples below.

[0034] The loss factor is the relative permittivity ε of the composite compound. r0 and dielectric tangent tanδ 0 The loss coefficient can be calculated using the measured values ​​of (loss coefficient) = (ε r0 ) 1/2 ×tan δ 0 x10 3 (In the formula, ε r0 [-] represents the relative dielectric constant of the composite compound obtained by measurement, and tan δ 0 [-] represents the dielectric tangent.)

[0035] Relative permittivity ε r0 is a parameter that indicates the degree of polarization of the composite compound obtained by measurement, and the higher the relative dielectric constant, the greater the delay in the propagation of the electrical signal. Therefore, in order to increase the signal propagation speed, a lower relative dielectric constant is preferable. 0 is a parameter obtained by measurement that indicates the amount of signal transmitted through the composite compound that is lost due to conversion to heat. Therefore, the lower the dielectric tangent, the less signal loss there is, and the better the signal transmission rate.

[0036] <Inorganic Fluoride> Next, the base material made of an inorganic fluoride of this embodiment will be described. The base material of this embodiment is preferably a powdery solid particle. Examples of the inorganic fluoride include MFn (wherein M is at least one selected from the group consisting of Li, Na, K, Mg, Al, Ca, Sc, Mn, Fe, Ga, Rb, Sr, Y, Zr, Sn, Ba, La, Ce, Yb, Hf, and Bi, and n is an integer of 1 to 4) and K 2 SiF 6 More specifically, examples of inorganic fluorides include LiF (lithium fluoride), NaF (sodium fluoride), KF (potassium fluoride), and MgF 2 (magnesium fluoride), AlF 3 (aluminum fluoride), CaF 2 (Calcium fluoride), ScF 3 (Scandium fluoride), MnF 2 (manganese fluoride), FeF 3(iron fluoride), GaF 3 (gallium fluoride), RbF (rubidium fluoride), SrF 2 (strontium fluoride), YF 3 (yttrium fluoride), ZrF 4 (zirconium fluoride), SnF 2 (Tin Fluoride), BaF 2 (barium fluoride), LaF 3 (lanthanum fluoride), CeF 3 (cerium fluoride), YbF 2 (ytterbium difluoride), YbF 3 (ytterbium trifluoride), HfF 4 (Hafnium fluoride) and BiF 3 (bismuth fluoride), etc.

[0037] Among the exemplified inorganic fluorides, aluminum fluoride, calcium fluoride, and magnesium fluoride are preferred, with aluminum fluoride being more preferred, from the viewpoint of reducing the dielectric loss of the composite compound. Furthermore, aluminum fluoride containing crystalline aluminum fluoride having an α-phase as a main component is preferred. Crystalline aluminum fluoride having an α-phase exhibits excellent low dielectric loss characteristics in the high frequency band of 1 GHz or higher. Therefore, by using a base material containing aluminum fluoride as a main component as a constituent material of a low dielectric loss resin composition, a remarkable effect of reducing the dielectric loss of the low dielectric loss resin composition can be achieved.

[0038] The half-width of the peak at the (012) plane of the α phase in the X-ray diffraction pattern of aluminum fluoride is 0.3° or less, preferably 0.25° or less, and more preferably 0.2°. Generally, as the average particle size of inorganic compound particles decreases, the proportion of the surface layer in the entire particle increases. Because the energy state of the particle surface is higher than that of the interior, structural order is easily disrupted, resulting in reduced crystallinity. As a result, the physical and chemical properties derived from the bulk change, and the dielectric loss tangent at the particle surface tends to increase. Therefore, regardless of the average particle size of the inorganic compound, high crystallinity is desirable. Here, in this embodiment, the degree of crystallinity can be evaluated by the half-width of the X-ray diffraction peak at the (012) plane derived from aluminum fluoride. Generally, the smaller the half-width, the higher the crystallinity and the smaller the fluctuation of the crystal structure, resulting in a smaller dielectric loss tangent. Therefore, in the case of aluminum fluoride, its crystallinity can be improved by reducing the half-width of the peak at the (012) plane in the X-ray diffraction pattern. From this viewpoint, in the present embodiment, the upper limit of the half-width is set to 0.3° or less, thereby preventing the crystallinity of aluminum fluoride from becoming too high and suppressing an increase in the dielectric loss tangent, thereby reducing the loss factor and enabling a reduction in the dielectric loss.

[0039] Furthermore, the lower limit of the half-value width is preferably 0.12° or more, more preferably 0.15° or more. By setting the lower limit of the half-value width to 0.12° or more, excessive grain growth and excessive grain size can be prevented during crystallization or crystal growth of amorphous aluminum fluoride. This prevents the average particle diameter D50 of aluminum fluoride from increasing, and suppresses excessive crystallinity of aluminum fluoride. As a result, when the composite compound of this embodiment is applied to a low dielectric loss resin composition and formed into a film- or sheet-shaped molded product, even when used in electronic components such as thin-layered printed wiring boards, flexible circuit boards, and high-frequency boards, surface irregularities can be reduced or suppressed, preventing deterioration of electrical properties. Furthermore, film- or sheet-shaped molded products with sufficiently suppressed film thickness can be produced.

[0040] Here, in this specification, "half width" means full width at half maximum. Furthermore, "X-ray diffraction pattern" refers to a plot line of diffraction intensity measured at each incident angle in a two-dimensional graph in which the horizontal axis represents the incident angle and the vertical axis represents the diffraction intensity when a sample is measured by (powder) X-ray diffraction. The "(012) plane of the α-phase in the X-ray diffraction pattern of aluminum fluoride" refers to the oriented plane of the aluminum fluoride crystal, and refers to the (012) plane of the α-phase in the X-ray diffraction pattern. The peak of the diffraction intensity due to the (012) plane of the α-phase of aluminum fluoride is located at a 2θ of approximately 25.3°.

[0041] Relative permittivity ε of inorganic fluoride particles r1 The upper limit of [-] is preferably 6 or less, more preferably 4 or less, and even more preferably 3 or less, at a frequency of 1 GHz or more and a temperature of 25°C. r1 When the loss factor is 6 or less, the loss factor can be reduced, and the dielectric loss can be reduced.

[0042] In addition, the dielectric loss tangent tanδ of the inorganic fluoride particles 1 The upper limit of [-] is preferably 0.008 or less, more preferably 0.005 or less, even more preferably 0.002 or less, and particularly preferably 0.001 or less, at a frequency of 1 GHz or more and a temperature of 25°C. 1 When the loss factor is 0.008 or less, the loss factor can be reduced, and the dielectric loss can be reduced.

[0043] The upper limit of the loss factor of the inorganic fluoride particles is preferably less than 6, more preferably not more than 4, and even more preferably not more than 3. When the loss factor is less than 6, the loss factor of the low dielectric loss resin composition can be reduced, and the dielectric loss can be reduced.

[0044] The relative permittivity ε used to quantify the dielectric properties and dielectric loss r1 and dielectric tangent tanδ 1The numerical values ​​of the above are based on the values ​​obtained by measuring inorganic fluoride particles made of powder. The measurement method can be selected appropriately. Specifically, for example, each of the values ​​can be measured by the method described in the Examples below.

[0045] The loss factor is the relative permittivity ε of the inorganic fluoride particles made of powder. r1 and dielectric tangent tanδ 1 The loss coefficient can be calculated using the measured values ​​of (loss coefficient) = (ε r1 ) 1/2 ×tan δ 1 x10 3 (In the formula, ε r1 [-] represents the relative dielectric constant of the inorganic fluoride particles made of powder obtained by measurement, and tan δ 1 [-] represents the dielectric tangent.)

[0046] Relative permittivity ε r1 is a parameter that indicates the degree of polarization of inorganic fluoride particles obtained by measurement, and the higher the relative dielectric constant, the greater the delay in the propagation of electrical signals. Therefore, in order to increase the signal propagation speed, a lower relative dielectric constant is preferable. 1 is a parameter obtained by measurement that indicates the amount of signal transmitted through the inorganic fluoride particle that is lost due to conversion to heat. Therefore, the lower the dielectric loss tangent, the less signal loss there is, and the better the signal transmission rate.

[0047] The average particle diameter D50 of the inorganic fluoride particles (particle diameter at 50% of the cumulative particle size in the volume-based cumulative particle size distribution) is not particularly limited and can be appropriately set depending on, for example, the shape (size, thickness, etc.) of the molded article containing the low dielectric loss resin composition, and the adjustment of the flowability of the material containing the inorganic fluoride particles in the preparation of the low dielectric loss resin composition. Generally, the upper limit of the average particle diameter D50 of the inorganic fluoride particles is preferably 75 μm or less, more preferably 50 μm or less, even more preferably 10 μm or less, and particularly preferably 1 μm or less. On the other hand, the lower limit of the average particle diameter D50 of the inorganic fluoride particles is preferably 0.05 μm or more, more preferably 0.075 μm or more, and even more preferably 0.1 μm or more. If the average particle diameter D50 of the inorganic fluoride particles is too large, it becomes difficult to obtain a flat surface when the inorganic fluoride particles are applied to a film- or sheet-shaped molded article. As a result, for example, when forming a laminate, the electrical properties of the laminate may be impaired due to the unevenness of the surface of the molded article. On the other hand, if the average particle diameter D50 of the inorganic fluoride particles is too small, it may become difficult to mix the composite compound uniformly with the polymer resin, and the viscosity of the mixture may increase to such an extent that molding of the low dielectric loss resin composition becomes difficult.

[0048] Furthermore, when the low dielectric loss resin composition of this embodiment is formed into a film- or sheet-shaped molded product, the average particle diameter D50 of the inorganic fluoride particles is preferably set to 1 / 5 or less, more preferably 1 / 10 or less, of the thickness of the molded product within the above-mentioned numerical range. For example, when the molded product of the low dielectric loss resin composition is a film or sheet-shaped product with a thickness of approximately 20 μm, the average particle diameter D50 of the inorganic fluoride particles is preferably 10 μm or less, more preferably 2 μm or less, and even more preferably 1 μm or less. This allows a film- or sheet-shaped molded product to be formed with the composite compound containing the inorganic fluoride particles aligned in a single layer. As a result, a molded product with reduced or prevented surface irregularities can be obtained. Furthermore, in a pre-cured slurry composition in which a composite compound containing inorganic fluoride particles is dispersed in a solvent, sedimentation of the composite compound can be suppressed, allowing a film- or sheet-shaped molded product in which the composite compound is uniformly filled.

[0049] The average particle diameter D50 of the inorganic fluoride particles is a value obtained by measurement by a laser diffraction / scattering method using, for example, Microtrac MT3300EXII (trade name: manufactured by Nikkiso Co., Ltd.).

[0050] The oxygen content of the inorganic fluoride particles is preferably 2% by mass or less, more preferably 1.5% by mass or less, and even more preferably 1% by mass or less, based on the total mass of the inorganic fluoride particles. The content of oxygen-containing components (e.g., surface hydroxyl groups, adsorbed moisture, and oxides and oxyfluorides as impurities) contained in the inorganic fluoride particles can be reduced, thereby suppressing the influence on dielectric properties. More specifically, by reducing the content of oxygen-containing components as impurities, the crystallinity of the inorganic fluoride particles can be improved. Furthermore, by reducing the content of oxyfluorides as oxygen-containing components, the insulating properties of the inorganic fluoride particles can be improved. Furthermore, by reducing hydroxyl groups and adsorbed moisture, which have high polarizability as oxygen-containing components, the deterioration of dielectric properties can also be suppressed.

[0051] The oxygen content of the inorganic fluoride particles can be measured, for example, by using an X-ray fluorescence analyzer (trade name: ZSX Primus II, manufactured by Rigaku Corporation).

[0052] The shape of the inorganic fluoride particles is not particularly limited and may be appropriately selected in consideration of, for example, the fluidity of the mixture when mixed with fluororesin particles in producing a composite compound, or the fluidity of the mixture when the composite compound is mixed with a polymer resin. The shape may also be appropriately selected depending on the purpose, such as controlling the mechanical strength, thermal conductivity, gas diffusivity, etc. of a molded article containing the low dielectric loss resin composition.

[0053] The shape of the inorganic fluoride particles can be, for example, any shape such as spherical, approximately spherical, elliptical, rod-like, needle-like, spindle-like, or plate-like. The inorganic fluoride particles may have any of these shapes and may be hollow with an internal space. Furthermore, the inorganic fluoride particles of the present embodiment may contain inorganic fluoride particles of the same type of shape, or may contain inorganic fluoride particles of two or more different shapes.

[0054] Furthermore, in the inorganic fluoride particles of this embodiment, for example, the mass loss after heat treatment at 400°C or higher is preferably 2% by mass or less, more preferably 1.5% by mass or less, and even more preferably 1% by mass or less, relative to the mass of the inorganic fluoride particles before heat treatment. By using inorganic fluoride particles with a mass loss of 2% by mass or less after heat treatment, it is possible to prevent a decrease in the low dielectric loss characteristics and mechanical strength of the low dielectric loss resin composition due to heat generation during polymerization of the monomers that form the polymer resin, degassing of impurities during heat treatment, and thermal decomposition of the main component of the polymer resin. There are no particular limitations on the method for reducing the mass loss of inorganic fluoride particles after heat treatment to 2% by mass or less. For example, materials with high thermal decomposition temperatures, materials that do not undergo phase change upon heating, and impurities that cause mass loss during the synthesis of the inorganic fluoride particles may be removed or reduced by prior heat treatment or chemical treatment.

[0055] <Fluororesin Particles> The fluororesin particles of this embodiment may be held on at least a portion of the surface of the base material. In an embodiment in which the fluororesin particles are held on a portion of the surface of the base material, Lewis acid sites are exposed on the surface of the base material where the fluororesin particles are not held. Generally, fluororesins are not compatible with polymer resins. However, by preventing a portion of the surface of the base material from being covered with fluororesin particles, the affinity of the composite compound for the polymer resin (details of which will be described later) in the low dielectric loss resin composition is well maintained, and a decrease in dispersibility in the polymer resin can be suppressed. On the other hand, in an embodiment in which a large amount of fluororesin particles are held, for example, on the entire surface of the base material, the dielectric loss can be further reduced.

[0056] The fluororesin particles are not particularly limited, and examples thereof include those made of polytetrafluoroethylene (PTFE), tetrafluoroethylene perfluorovinyl ether copolymer (PFA), and tetrafluoroethylene hexafluoropropylene copolymer (FEP). Of these fluororesins, PTFE is preferred from the viewpoint of reducing dielectric loss.

[0057] The average particle diameter d50 of the fluororesin particles (particle diameter at 50% of the cumulative particle size in the volume-based cumulative particle size distribution) is preferably in the range of 1 / 10 to 1 / 2 of the average particle diameter D50 of the inorganic fluoride particles. By making the average particle diameter d50 of the fluororesin particles 1 / 10 or more of the average particle diameter D50 of the inorganic fluoride particles, it is possible to entirely coat the base material. On the other hand, by making the average particle diameter d50 of the fluororesin particles 1 / 2 or less of the average particle diameter D50 of the inorganic fluoride particles, it is possible to prevent self-fusion.

[0058] The average particle diameter d50 of the fluororesin particles is a value obtained by measurement by a laser diffraction / scattering method using, for example, Microtrac MT3300EXII (trade name: manufactured by Nikkiso Co., Ltd.).

[0059] The shape of the fluororesin particles before being held in the base material is not particularly limited, and any shape can be used, for example, spherical, approximately spherical, elliptical, rod-like, needle-like, spindle-like, plate-like, etc. Furthermore, fluororesin particles of the same type of shape may be contained, or fluororesin particles of two or more different shapes may be contained.

[0060] The content of the fluororesin particles is preferably in the range of 0.5% by mass or more and less than 26% by mass, more preferably in the range of 1% by mass or more and 25% by mass or less, even more preferably in the range of 1% by mass or more and 15% by mass or less, and particularly preferably in the range of 1% by mass or more and 10% by mass or less, relative to the total mass of the base material. By making the content of the fluororesin particles 0.5% by mass or more, the excellent low dielectric loss characteristics of the composite compound can be maintained. On the other hand, by making the content of the fluororesin particles less than 26% by mass, the affinity of the composite compound for the polymer resin can be well maintained, and a decrease in dispersibility in the polymer resin can be suppressed.

[0061] Fluororesin particle relative permittivity ε r2 The upper limit of [-] is preferably 3.5 or less, more preferably 3.0 or less, and even more preferably 2.9 or less, at a frequency of 1 GHz or more and a temperature of 25°C. r2 When the value is 3.5 or less, the loss factor of the composite compound and the low dielectric loss resin composition containing the composite compound can be reduced, and the dielectric loss can be reduced.

[0062] In addition, the fluororesin particles have a dielectric loss tangent tanδ 2 The dielectric loss tangent tanδ of the fluororesin particles is 0.002 or less, preferably 0.001 or less, at a frequency of 1 GHz or more and a temperature of 25°C. 2 When the value is 0.002 or less, the dielectric loss tangent of the composite compound and the low dielectric loss resin composition containing the composite compound can be reduced, and the dielectric loss can be further reduced.

[0063] The upper limit of the loss factor of the fluororesin particles is preferably not more than 6, more preferably not more than 4, and even more preferably not more than 3. When the loss factor is not more than 6, the loss factor of the composite compound and the low dielectric loss resin composition can be reduced, and the dielectric loss can be further reduced.

[0064] The relative permittivity ε used to quantify the dielectric properties and dielectric loss r2 and dielectric tangent tanδ 2 The numerical values ​​of the above are based on the values ​​obtained by measuring the fluororesin particles. The measurement method can be selected appropriately. Specifically, for example, each of the values ​​can be measured by the method described in the Examples below.

[0065] The loss factor is the relative dielectric constant ε of the fluororesin particles. r2 and dielectric tangent tanδ 2 The loss coefficient can be calculated using the measured values ​​of (loss coefficient) = (ε r2 ) 1/2 ×tan δ 2 x10 3 (In the formula, ε r2 [-] represents the relative dielectric constant of the fluororesin particles obtained by measurement, and tan δ 2 [-] represents the dielectric tangent.)

[0066] Relative permittivity ε r2 is a parameter that indicates the degree of polarization of the fluororesin particles obtained by measurement, and the higher the relative dielectric constant, the greater the delay in the propagation of electrical signals. Therefore, in order to increase the signal propagation speed, a lower relative dielectric constant is preferable. 2 is a parameter obtained by measurement that indicates the amount of signal transmitted inside the fluororesin particle that is lost due to conversion to heat. Therefore, the lower the dielectric loss tangent, the less signal loss there is, and the better the signal transmission rate.

[0067] <Method for producing composite compound> Next, a method for producing the composite compound will be described below. The method for producing the composite compound of this embodiment is not particularly limited, and known methods can be used. For example, when producing a composite compound in which fluororesin particles are thermally fused to the surface of a base material, the method may be a method (composite treatment) that includes at least a mixing step of mixing the fluororesin particles with an inorganic fluoride base material, a heating step of heating the mixture of the fluororesin particles and the inorganic fluoride base material, and a cooling step of cooling the mixture after heating.

[0068] The heating method in the heating step is not particularly limited, and known methods can be used. The heating temperature is not particularly limited as long as it is equal to or higher than the melting point and lower than the boiling point of the fluororesin particles, and can be appropriately set depending on the type of fluororesin, etc. The heating time is also not particularly limited, and can be appropriately set depending on the heating temperature and the type of material of the fluororesin particles, etc. The cooling method in the cooling step is not particularly limited, and can be, for example, natural cooling or rapid cooling.

[0069] <Others> The surface of the inorganic fluoride base material of this embodiment may be chemically modified by introducing functional groups such as hydroxyl groups, epoxy groups, carboxyl groups, carbonyl groups, amino groups, perfluoroalkane groups, ether groups, and ester groups, within the scope of not impairing the effects of the present invention. Furthermore, the surface of the fluororesin particles of this embodiment may also be chemically modified by introducing functional groups such as hydroxyl groups, epoxy groups, carboxyl groups, carbonyl groups, amino groups, perfluoroalkane groups, ether groups, and ester groups, within the scope of not impairing the effects of the present invention.

[0070] In this embodiment, the inorganic fluoride and the fluororesin particles can be any combination of the materials exemplified above, but it is preferable to use fluororesin particles that have a smaller relative permittivity, dielectric loss tangent, or loss factor than the inorganic fluoride, thereby further reducing the dielectric loss compared to when only inorganic filler consisting of inorganic fluoride particles is used in the low dielectric loss resin composition.

[0071] (Slurry Composition for Low Dielectric Loss Resin Composition) Next, the slurry composition for the low dielectric loss resin composition (hereinafter referred to as "slurry composition") of this embodiment will be described below.

[0072] The slurry composition of this embodiment contains at least the above-described composite compound and a solvent. The slurry composition is a dispersion in which the composite compound is dispersed (including floating and suspended) in a solvent. In this specification, the term "dispersion" refers to a state in which the composite compound is dispersed as a dispersoid in a solvent that is a dispersion medium. However, the term "dispersion" does not include a solid colloid (organogel) in which a dispersoid is dispersed in a solid dispersion medium and fluidity is lost.

[0073] The lower limit of the content of the complex compound is preferably 1% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, relative to the total mass of the slurry composition. On the other hand, the upper limit of the content of the complex compound is preferably 85% by mass or less, more preferably 82% by mass or less, and even more preferably 79% by mass or less, relative to the total mass of the slurry composition. When the lower limit of the content of the complex compound is 1% by mass or more, the loss factor of the slurry composition decreases, and the dielectric loss is reduced.

[0074] As the solvent, a linear alkane is preferred, and a linear alkane having 10 to 16 carbon atoms is more preferred. More specifically, linear alkanes include n-decane, n-tetradecane, and n-hexadecane. These solvents can be used alone or in combination. Among these linear alkanes, n-hexadecane is particularly preferred because it can exist as a liquid at room temperature (e.g., 5°C to 35°C), has low polarity among linear alkanes, and is suitable for dielectric property evaluation. Linear alkanes having 10 or more carbon atoms have low dielectric constants and dielectric dissipation factors due to their low polarity, and are poorly soluble in water. Furthermore, because they have high boiling points, they can suppress concentration changes due to volatilization, unlike hexane, which has a low boiling point. On the other hand, linear alkanes having 16 or fewer carbon atoms can suppress the melting point to 20°C or below, thereby preventing the deterioration of handleability caused by their existence as a solid at room temperature. Herein, when a range of carbon numbers is expressed, the range means that all integer carbon numbers within that range are included. Therefore, for example, a linear alkane having "10 to 16 carbon atoms" means all linear alkanes having 10, 11, 12, 13, 14, 15, and 16 carbon atoms.

[0075] The lower limit of the solvent content is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 15% by mass or more, relative to the total mass of the slurry composition, while the upper limit of the solvent content is preferably 99% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less, relative to the total mass of the slurry composition.

[0076] Relative dielectric constant ε of the slurry composition r3 The upper limit of [-] is preferably 6 or less, more preferably 4 or less, and even more preferably 3 or less, at a frequency of 1 GHz or more and a temperature of 25°C. r3 When the loss factor is 6 or less, the loss factor can be reduced, and the dielectric loss can be reduced.

[0077] The dielectric loss tangent tanδ of the slurry composition 3 The upper limit of [-] is preferably 0.005 or less, more preferably 0.002 or less, and particularly preferably 0.001 or less, at a frequency of 1 GHz or more and a temperature of 25°C. 3 When the loss factor is 0.005 or less, the loss factor can be reduced, and the dielectric loss can be reduced.

[0078] The upper limit of the loss factor of the slurry composition is preferably less than 6, more preferably not more than 4, and even more preferably not more than 3. When the loss factor is less than 6, the loss factor of the slurry composition can be reduced, and the dielectric loss can be reduced.

[0079] The relative permittivity ε used to quantify the dielectric properties and dielectric loss r3 and dielectric tangent tanδ 3 The numerical values ​​are based on the values ​​obtained by measuring the slurry composition. The measurement method can be selected appropriately. Specifically, for example, each can be measured by the method described in the Examples below.

[0080] The loss factor is calculated by multiplying the relative dielectric constant ε of the slurry composition by r3 and dielectric tangent tanδ 3 The loss coefficient can be calculated using the measured values ​​of (loss coefficient) = (ε r3 ) 1/2 ×tan δ 3 x10 3 (In the formula, ε r3 [-] represents the relative dielectric constant of the slurry composition obtained by measurement, and tan δ 3 [-] represents the dielectric tangent.)

[0081] Relative permittivity ε r3 is a parameter that indicates the degree of polarization of the slurry composition obtained by measurement, and the higher the relative dielectric constant, the greater the delay in the propagation of electrical signals. Therefore, in order to increase the signal propagation speed, a lower relative dielectric constant is preferable. 3is a parameter obtained by measurement that indicates the amount of signal transmitted through the slurry composition that is lost due to conversion to heat. Therefore, the lower the dielectric loss tangent, the less signal loss there is, and the better the signal transmission rate.

[0082] The slurry composition of the present embodiment may contain other additives as long as they do not interfere with the object of the present invention. The other additives are not particularly limited, and examples thereof include ultraviolet inhibitors, colorants, flame retardants, stabilizers, and dispersants. The content of the other additives is not particularly limited, and can be appropriately determined depending on the application, purpose, etc.

[0083] The method for producing the slurry composition of this embodiment is not particularly limited, and the slurry composition of this embodiment can be produced by adding a predetermined amount of a complex compound to a solvent and stirring for a predetermined period of time.

[0084] (Low dielectric loss resin composition) Next, the low dielectric loss resin composition of this embodiment will be described below. The low dielectric loss resin composition of this embodiment contains at least the above-described composite compound and a polymer resin.

[0085] With regard to the content of the complex compound, the lower limit is preferably 1% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, relative to the total mass of the low dielectric loss resin composition. On the other hand, the upper limit of the content of the complex compound is preferably 85% by mass or less, more preferably 82% by mass or less, and even more preferably 79% by mass or less, relative to the total mass of the low dielectric loss resin composition. When the lower limit of the content of the complex compound is 1% by mass or more, the loss factor of the low dielectric loss resin composition decreases, thereby reducing the dielectric loss. On the other hand, when the upper limit of the content of the complex compound is 85% by mass or less, deterioration of physical strength such as brittleness can be prevented, and it is possible to improve hardness, reduce the thermal expansion coefficient, and improve weather resistance.

[0086] The polymeric resin preferably comprises at least one thermoplastic resin and / or at least one thermosetting resin.

[0087] More specifically, the polymer resin may be, for example, an olefin-based resin such as polyethylene resin or polypropylene resin; a styrene-based resin such as polystyrene resin or acrylonitrile butadiene styrene resin (ABS resin); a polyvinyl resin such as polyvinyl acetate resin, polyvinyl chloride resin, polyvinyl alcohol resin, or polyvinylidene chloride resin; a methacrylic resin; a thermoplastic elastomer resin; a thermoplastic polyurethane resin; a polyacrylonitrile resin; a polylactic acid resin; a polyamide polyacetal resin; a polycarbonate resin; a polyphenylene ether resin; a polyethylene terephthalate resin; a polysulfone resin; a polyether sulfone resin; a polyphenylene sulfide resin; a polyether ether ketone resin; a liquid crystal polymer resin; or a polyimide. Resins include fluororesins such as polytetrafluoroethylene resin (PTFE), polytetrafluoroethylene and perfluoroalkoxyethylene copolymer (PFA), polychlorotrifluoroethylene resin (PCTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), and tetrafluoroethylene-ethylene copolymer (ETFE); phenolic resins; amine resins such as urea resins and melamine resins; furan resins; unsaturated polyester resins; epoxy resins; diallyl phthalate resins; guanamine resins; ketone resins; silicone resins; thermosetting elastomer resins; natural rubber; synthetic rubbers such as neoprene rubber, styrene-butadiene rubber, isoprene rubber, butyl rubber, and urethane rubber; and modified versions thereof. These polymer resins can be used alone or in combination of two or more, depending on the processability and application of the low dielectric loss resin composition. For example, when using a polymer resin obtained by mixing a polyphenylene ether resin with an epoxy resin, the processability can be improved by increasing the fluidity. The degree of polymerization of the polymer resin is not particularly limited, and can be appropriately selected depending on the application of the low dielectric loss resin composition.

[0088] The content of the polymer resin is preferably 15% by mass or more and 99% by mass or less, more preferably 18% by mass or more and 90% by mass or less, and even more preferably 21% by mass or more and 80% by mass or less, based on the total mass of the low dielectric loss resin composition. By making the content of the polymer resin 15% by mass or more, the properties of the polymer resin, such as adhesion and water resistance, can be fully exhibited. On the other hand, by making the content of the polymer resin 99% by mass or less, the dielectric loss of the resin composition can be reduced by adding a composite compound while maintaining the properties of the polymer resin.

[0089] Relative dielectric constant ε of low dielectric loss resin composition r4 The upper limit of [-] is preferably 6 or less, more preferably 4 or less, and particularly preferably 3 or less, at a frequency of 1 GHz or more and a temperature of 25°C. r4 When the loss factor is 6 or less, the loss factor can be reduced, and the dielectric loss can be reduced.

[0090] In addition, the dielectric loss tangent tanδ of the low dielectric loss resin composition 4 The upper limit of [-] is preferably 0.02 or less, more preferably 0.005 or less, even more preferably 0.002 or less, and particularly preferably 0.001 or less, at a frequency of 1 GHz or more and a temperature of 25°C. 4 When the loss factor is 0.02 or less, the loss factor can be reduced, and the dielectric loss can be reduced.

[0091] The upper limit of the loss factor of the low dielectric loss resin composition is preferably less than 6, more preferably not more than 4, and particularly preferably not more than 3. When the loss factor is less than 6, the loss factor of the low dielectric loss resin composition can be reduced, and the dielectric loss can be reduced.

[0092] The relative permittivity ε used to quantify the dielectric properties and dielectric loss r4 and dielectric tangent tanδ 4The numerical values ​​of the low dielectric loss resin composition are based on the values ​​obtained by the measurement. The measurement method can be selected appropriately. Specifically, for example, each of the values ​​can be measured by the method described in the Examples below.

[0093] The loss factor is the relative dielectric constant ε of the low dielectric loss resin composition r4 and dielectric tangent tanδ 4 The loss coefficient can be calculated using the measured values ​​of (loss coefficient) = (ε r4 ) 1/2 ×tan δ 4 x10 3 (In the formula, ε r4 [-] represents the relative dielectric constant of the low dielectric loss resin composition obtained by measurement, and tan δ 4 [-] represents the dielectric tangent.)

[0094] Relative permittivity ε r4 is a parameter that indicates the degree of polarization of a low dielectric loss resin composition obtained by measurement, and the higher the relative dielectric constant, the greater the delay in the propagation of an electric signal. Therefore, in order to increase the signal propagation speed, a lower relative dielectric constant is preferable. Dielectric loss tangent tanδ 4 is a parameter obtained by measurement that indicates the amount of signal transmitted through the low dielectric loss resin composition that is lost due to conversion to heat. Therefore, the lower the dielectric loss tangent, the less signal loss there is, and the better the signal transmission rate.

[0095] Next, a method for producing the low dielectric loss resin composition according to this embodiment will be described below. The low dielectric loss resin composition according to this embodiment can be produced by adding a composite compound and any other additives to a polymer resin and uniformly mixing or kneading the mixture. Alternatively, the low dielectric loss resin composition can be produced by adding and dispersing the composite compound and any other additives to a solution (e.g., a varnish or dispersion) in which the polymer resin or a monomer that forms the polymer resin is dissolved or dispersed in an organic solvent.

[0096] The low dielectric loss resin composition of this embodiment may contain impurities to the extent that it does not contradict the object of the present invention. Examples of such impurities include metal impurities containing elements other than those constituting the inorganic fluoride, and metal oxides. The content of impurities is preferably 100 ppm or less, more preferably 10 ppm or less, based on the total mass of the low dielectric loss resin composition.

[0097] The low dielectric loss resin composition of the present embodiment may contain other additives as long as they do not interfere with the object of the present invention. The other additives are not particularly limited, and examples thereof include curing agents, lubricants, crystal nucleating agents, ultraviolet protection agents, colorants, flame retardants, stabilizers, plasticizers, reinforcing agents, and dispersants. The content of the other additives is not particularly limited, and can be appropriately determined depending on the application, purpose, etc.

[0098] The low dielectric loss resin composition of the present embodiment can be used as a resin composition for insulating films (solder resist), a resin composition for semiconductor encapsulation, an adhesive, a paint, a coating material for wiring for power supplies, communications, etc.

[0099] (Molded Article for High-Frequency Device and Manufacturing Method Thereof) The molded article for high-frequency device of this embodiment (hereinafter referred to as "molded article") is made of a molded article containing a low dielectric loss resin composition.

[0100] The molded body can be produced, for example, by using a known kneader and extruder. Examples of kneaders that can be used include an internal pressure kneader and an open roll. A sheet-shaped low dielectric loss resin composition material can be produced using these kneaders, and then a molded body can be produced using the low dielectric loss resin composition material. Alternatively, a pellet-shaped low dielectric loss resin composition material can be produced using an extruder, and then a molded body can be produced using an injection molding machine. When a molding machine such as an extruder is used to mix a polymer resin with a composite compound and other additives, the number of steps can be reduced, and production efficiency can be improved. Furthermore, the composite compound may be appropriately subjected to a drying treatment or the like before mixing with the polymer resin.

[0101] Furthermore, a sheet-like molded product can be produced by a known method. For example, a composite compound and any other additives are added to a varnish tank filled with a solution (resin varnish) containing a polymer resin, and the mixture is uniformly dispersed. The dispersion is then heated at a predetermined temperature. The cured product produced by heating is stretched into a sheet, thereby producing a sheet-like molded product.

[0102] Alternatively, a sheet-like substrate such as glass cloth or a bonding sheet may be immersed in a bath of a dispersion containing a polymer resin, a composite compound, and any other additives, and passed through the bath to impregnate the sheet-like substrate with the dispersion. The sheet impregnated with the dispersion is then dried to produce an impregnated sheet impregnated with the low dielectric loss resin composition. By passing the sheet-like substrate through the bath of the dispersion multiple times, it is also possible to produce a laminate in which multiple low dielectric loss resin composition layers are stacked.

[0103] (High-Frequency Device) The high-frequency device according to this embodiment contains a low dielectric loss resin composition or includes a molded article of a low dielectric loss resin composition.

[0104] The high-frequency device of this embodiment is used for information processing and information communication performed by electronically exchanging signals. In particular, the high-frequency device of this embodiment is used in a high-frequency band in which the frequency band of radio waves and signals used during communication is 1 GHz or higher, more preferably 10 GHz or higher. The high-frequency device of this embodiment also includes high-frequency electronic components used in such high-frequency bands.

[0105] Examples of high-frequency devices include housings for information processing and information communication devices, circuit boards, printed wiring boards, transmission lines, high-frequency electronic components such as capacitors and inductors, and ceiling and wall materials for rooms in which high-frequency devices are installed.Furthermore, high-frequency devices including insulating films and semiconductor sealing resins formed from the low dielectric loss resin composition, and wiring coated with the low dielectric loss resin composition as a coating material are also included in the high-frequency devices of the present embodiment.

[0106] Preferred examples of the present invention are described in detail below. However, unless otherwise specified, the materials and blending amounts described in the examples are not intended to limit the scope of the present invention.

[0107] Example 1 <Inorganic Fluoride> First, α-AlF 3 (manufactured by Stella Chemifa Corporation) was prepared, and this powdered α-AlF 3 The half-width of the peak at the (012) plane in the X-ray diffraction pattern was measured for each sample. An X-ray diffractometer (product name: RINT-ULTIMA, manufactured by Rigaku Corporation) was used for the measurement. The measurement conditions were as follows: X-ray tube: Cu; tube voltage: 40 kV; tube current: 40 mA; step size (width): 0.02°; measurement range (scanning range of diffraction angle): 2θ = 10° to 70°

[0108] α-AlF appears near 2θ = 25.3° 3 The half-width was calculated from the diffraction intensity peak corresponding to the (012) plane of α-AlF 3 The half width of the peak was 0.17°.

[0109] Next, α-AlF 3 First, powdered α-AlF was added to 200 mL of circulating solvent (water) flowing in a particle size distribution measuring device (trade name: Microtrac MT3300EXII, manufactured by Nikkiso Co., Ltd.). 3 was added in the range of 0.1 to 0.3 g. 3 An aqueous dispersion was prepared in which the concentration of α-AlF was in the range of 0.05 to 0.15% by mass relative to the total mass, and this aqueous dispersion was measured by a laser diffraction / scattering method. In the obtained particle size distribution, the average particle size at which the cumulative volume reached 50% was calculated as D50. As a result, α-AlF 3 The average particle diameter D50 was 2 μm.

[0110] Next, α-AlF 3The powder was filled into a quartz tube, and the relative permittivity and dielectric loss tangent were measured in a 10 GHz frequency range by a cavity resonator method under an environmental atmosphere at a temperature of 25°C and a relative humidity of 40%. A vector network analyzer (manufactured by Anritsu Corporation, product name: MS46122B) was used for the measurements. 3 The measured values ​​of the relative permittivity and dielectric loss tangent of the quartz tube filled with α-AlF 3 Bulk density and true density of α-AlF 3 The void portion is corrected using the filling amount of α-AlF 3 The relative permittivity ε r1 [-] and dielectric tangent tanδ 1 [-] was calculated. As a result, the relative dielectric constant ε r1 is 3.2 [-], and the dielectric loss tangent tanδ 1 was 0.0027 [-].

[0111] <Fluororesin Particles> The fluororesin particles have an average particle diameter d50 in the range of 200 nm or more and 500 nm or less, and a relative dielectric constant ε r2 is 3.0 [-] or less, and the dielectric loss tangent tanδ 2 The PTFE particles used were those having a viscosity of 0.002 [-] or less.

[0112] <Preparation of Composite Compound> 99 parts by mass of α-AlF 3 and 1 part by mass of PTFE particles are mixed, and then the PTFE particles are heated to a temperature equal to or higher than the melting point of the PTFE particles to form α-AlF 3 The mixture was then cooled to room temperature to prepare the composite compound according to this example.

[0113] Example 2 In this example, α-AlF 3 The content of the PTFE particles was changed to 90 parts by mass, and the content of the PTFE particles was changed to 10 parts by mass. Except for these, the composite compound according to this example was produced in the same manner as in Example 1.

[0114] Comparative Example 1 In this comparative example, α-AlF was used instead of the composite compound. 3 100 parts by mass of an inorganic filler consisting of the above was used.

[0115] (Example 3) In this example, α-AlF 3 α-AlF 3 Other than that, the composite compound according to this example was produced in the same manner as in Example 1.

[0116] Example 4 In this example, α-AlF 3 α-AlF 3 Other than that, the composite compound according to this example was produced in the same manner as in Example 2.

[0117] Example 5 In this example, α-AlF 3 The content of the PTFE particles was changed to 20 parts by mass. Except for these, the composite compound according to this example was produced in the same manner as in Example 3.

[0118] Example 6 In this example, α-AlF 3 Instead, CaF having an average particle diameter D50 of 40 μm 2 The composite compound of this example was prepared in the same manner as in Example 1 except for the above.

[0119] Example 7 In this example, α-AlF 3 Instead, K having an average particle diameter D50 of 3 μm 2 SiF 6 95 parts by mass of Stella Chemifa Co., Ltd. was used. The content of the PTFE particles was changed to 5 parts by mass. Other than these, the composite compound according to this example was produced in the same manner as in Example 1.

[0120] Comparative Example 2 In this comparative example, α-AlF 200 having an average particle size D50 of 10 μm was used instead of the composite compound. 3 100 parts by mass of an inorganic filler consisting of the above was used.

[0121] Comparative Example 3 In this comparative example, 100 parts by mass of an inorganic filler made of silica having an average particle size D50 of 1 μm was used in place of the composite compound.

[0122] Comparative Example 4 In this comparative example, α-AlF 3 Instead of the silica particles, 95 parts by mass of silica having an average particle diameter D50 of 1 μm was used. The content of the PTFE particles was changed to 5 parts by mass. Other than these, a composite according to this comparative example was produced in the same manner as in Example 1.

[0123] Comparative Example 5 In this comparative example, instead of the composite compound, CaF 2 100 parts by mass of an inorganic filler consisting of the above was used.

[0124] (Comparative Example 6) In this comparative example, K 100 having an average particle size D50 of 3 μm was used instead of the composite compound. 2 SiF 6 100 parts by mass of an inorganic filler consisting of the above was used.

[0125] Example 8 In this example, α-AlF 3 The content of the PTFE particles was changed to 5 parts by mass. Except for these, the composite compound according to this example was produced in the same manner as in Example 1.

[0126] (SEM Images) SEM images were taken using an electron microscope (product name: SU1510, manufactured by Hitachi High-Technologies Corporation) for the composite compounds of Examples 1, 2, 5, 6, and 8, and the composite of Comparative Example 4. The respective SEM images are shown in Figures 1 to 6.

[0127] As can be seen from FIGS. 1 to 3 and 5, in Examples 1, 2, 5 and 8, α-AlF 3 By subjecting the mixture of α-AlF and PTFE particles to a composite treatment, 3 It was confirmed that a composite compound was obtained in which PTFE particles were thermally fused to a part of the surface of the CaF 2 The mixture of CaF and PTFE particles is subjected to a composite treatment. 2 On the other hand, in Comparative Example 4, as can be seen from Figure 6, even when the mixture of silica and PTFE particles was subjected to the composite treatment, a composite compound like that in Example 1 was not obtained.

[0128] (Measurement of Relative Dielectric Constant and Dielectric Loss Tangent) The relative dielectric constant and dielectric loss tangent of each sample of the composite compounds according to Examples 1 to 7, the inorganic fillers according to Comparative Examples 1 to 3, 5, and 6, and the composite according to Comparative Example 4 were measured. That is, each sample was filled into a quartz tube, and the relative dielectric constant and dielectric loss tangent were measured in a 10 GHz frequency range by a cavity resonator method in an ambient atmosphere at a temperature of 25°C and a relative humidity of 40%. A vector network analyzer (manufactured by Anritsu Corporation, product name: MS46122B) was used for the measurements. Furthermore, the measured values ​​of the relative dielectric constant and dielectric loss tangent of the quartz tube filled with each sample were corrected for voids using the bulk density and true density of each sample and the amount of each sample filled relative to the filling volume, and the relative dielectric constant ε r0 [-] and dielectric tangent tanδ 0 The results are shown in Table 1.

[0129] As can be seen from Table 1, the composite compounds according to Examples 1 and 2 have the same or similar properties as the α-AlF 3 It was confirmed that the dielectric loss tangent was lower than that of the inorganic filler consisting of α-AlF in Comparative Example 2, and that the dielectric loss was reduced. 3 Furthermore, it was confirmed that the dielectric loss tangent value was lower than that of the inorganic filler composed of CaF 2 The dielectric loss tangent value was lowered compared to the inorganic filler consisting of 2 SiF 6 It was confirmed that the dielectric loss tangent was lower than that of the inorganic filler consisting of PTFE particles, and that the dielectric loss was reduced in both cases. This is thought to be because the PTFE particles were thermally fused to the surface of the base material consisting of each inorganic fluoride to form a composite, and the dielectric loss of the PTFE particles was expressed as a synergistic effect.

[0130] In the case of the inorganic filler made of silica according to Comparative Example 3, the dielectric constant was 2.8 and the dielectric loss tangent was 0.0016. In Comparative Example 4, in which a composite treatment was performed on a mixture of silica and PTFE particles, the dielectric constant value was reduced compared to the silica according to Comparative Example 3, but the dielectric loss tangent value increased (worsened), and no synergistic effect was observed due to the combined use of PTFE particles. The decrease in the dielectric constant value of the composite according to Comparative Example 4 is presumed to be due to the formation of air layers in the silica during the composite treatment with PTFE particles.

[0131] (Evaluation of Dispersibility and Fluidity) Next, the dispersibility in polymer resins was evaluated for each sample of the composite compounds according to Examples 1 to 7, the inorganic fillers according to Comparative Examples 1 to 3, 5 and 6, and the composite according to Comparative Example 4. That is, each sample and an epoxy resin (trade name: jER (registered trademark) 828, jER (registered trademark) Cure, manufactured by Mitsubishi Chemical Corporation) were placed in a container cup so that the concentration of each sample was 50 mass % relative to the total mass of the resulting composition, and the mixture was kneaded with a defoaming mixer to prepare a composition.

[0132] The dispersibility and fluidity of each obtained composition were evaluated based on the following criteria. The results are shown in Table 1. ◯: The slurry composition fell smoothly, as shown in Figure 7(a). Δ: The slurry composition fell but lacked smoothness. ×: No slurry composition was obtained, or the slurry composition fell in clumps, as shown in Figure 7(b).

[0133] As can be seen from Table 1, in all of Examples 1 to 7, slurry compositions were obtained in which the composite compound was well dispersed (suspended) in the epoxy resin. In particular, the composite compounds of Examples 1 to 4, 6, and 7 exhibited excellent dispersibility in the epoxy resin, and all of them produced slurry compositions with good fluidity. Generally, PTFE does not have good compatibility with polymer resins. However, in the composite compounds of Examples 1 to 4, 6, and 7, the surface of the respective inorganic fluoride matrix is ​​not completely covered with PTFE particles, presumably exposing the Lewis acid sites on the matrix surface. Therefore, these composite compounds are believed to maintain their affinity with the epoxy resin, resulting in uniform dispersion in the epoxy resin. On the other hand, the composite compound of Example 5 contained a high content of PTFE particles, which resulted in more PTFE particles being thermally fused to the matrix surface compared to the composite compounds of Examples 1 to 4, 6, and 7, presumably resulting in a decrease in affinity with the epoxy resin and a slight decrease in fluidity.

[0134] In Comparative Examples 3 and 4, silica does not inherently have a good affinity for epoxy resins, so phase separation occurred with the epoxy resin, and no slurry composition was obtained.

[0135]

[0136] (Evaluation of Chemical Resistance) Either the composite compound according to Example 8, the silica according to Comparative Example 3, or the composite according to Comparative Example 4 was added to a 1N NaOH aqueous solution so that the concentration was 10% by mass. After addition, the samples were stored in a static state for 3 days in an environment at a temperature of 80°C. After the storage period, the amounts of Al element and Si element eluted were measured using an ICP-AES analyzer (product name: ULTIMA 2, manufactured by HORIBA, Ltd.) (Al detection wavelengths: 396 nm and 152 nm, Si detection wavelengths: 611 nm and 251 nm). The results are shown in Table 2.

[0137]

[0138] As can be seen from Table 2, the composite compound of Example 8 was confirmed to have excellent chemical resistance, with aluminum elution being suppressed to 100 ppm or less even when immersed in an aqueous sodium hydroxide solution at 80° C. for 3 days. On the other hand, the silica of Comparative Example 3 and the composite of Comparative Example 4 both eluted silicon in an amount of 3 mass % or more relative to the total mass of each, confirming that they had poor chemical resistance.

Claims

1. A composite compound for a low dielectric loss resin composition, comprising: a base material made of an inorganic fluoride; and fluororesin particles held on at least a portion of the surface of the base material, wherein the dielectric tangent of the fluororesin particles is 0.002 or less at a frequency of 1 GHz or more and a temperature of 25°C.

2. A composite compound for use in a low dielectric loss resin composition according to claim 1, wherein the fluororesin particles are held on the surface of the base material made of the inorganic fluoride by thermal fusion.

3. The composite compound for a low dielectric loss resin composition according to claim 1, wherein the fluororesin is polytetrafluoroethylene.

4. The inorganic fluoride is MFn (wherein M is at least one selected from the group consisting of Li, Na, K, Mg, Al, Ca, Sc, Mn, Fe, Ga, Rb, Sr, Y, Zr, Sn, Ba, La, Ce, Yb, Hf and Bi, and n is an integer of 1 to 4) or K 2 SiF 6 2. The composite compound for use in a low dielectric loss resin composition according to claim 1, which is 5. The inorganic fluoride is AlF 3 5. The composite compound for use in a low dielectric loss resin composition according to claim 4, which is 6. A composite compound for use in a low dielectric loss resin composition according to claim 1, wherein the average particle diameter D50 of the base material made of the inorganic fluoride is 0.05 μm or more and 75 μm or less.

7. A composite compound for a low dielectric loss resin composition according to claim 1, wherein the content of the fluororesin particles is 0.5 mass % or more and less than 26 mass % based on the total mass of the base material made of the inorganic fluoride.

8. A low dielectric loss resin composition comprising at least a polymer resin and the composite compound for a low dielectric loss resin composition according to any one of claims 1 to 7.

9. The low dielectric loss resin composition according to claim 8, wherein the content of the complex compound is 1 mass % or more and 85 mass % or less based on the total mass of the low dielectric loss resin composition.

10. The low dielectric loss resin composition according to claim 8, wherein the polymeric resin comprises at least one thermoplastic resin and / or at least one thermosetting resin.

11. The low dielectric loss resin composition according to claim 10, wherein the polymer resin is at least one selected from the group consisting of olefin resins, styrene resins, polyvinyl resins, methacrylic resins, thermoplastic elastomer resins, thermoplastic polyurethane resins, polyacrylonitrile resins, polylactic acid resins, polyamide polyacetal resins, polycarbonate resins, polyphenylene ether resins, polyethylene terephthalate resins, polysulfone resins, polyether sulfone resins, polyphenylene sulfide resins, polyether ether ketone resins, liquid crystal polymer resins, polyimide resins, fluororesins, phenol resins, amine resins, furan resins, unsaturated polyester resins, epoxy resins, diallyl phthalate resins, guanamine resins, ketone resins, silicone resins, thermosetting elastomer resins, natural rubber, synthetic rubber, and modified versions thereof.

12. A molded article for use in high-frequency devices used in a frequency band of 1 GHz or more, comprising a molded article containing the low dielectric loss resin composition according to claim 8.

13. A high-frequency device used in a frequency band of 1 GHz or more, comprising the low dielectric loss resin composition according to claim 8.

14. A high-frequency device used in a frequency band of 1 GHz or more, comprising the molded article for high-frequency devices according to claim 12.

Citation Information

Patent Citations

  • Optical thin film and its production

    JP1996101301A

  • Composite particle material, production method therefor, composite particle material slurry, and resin composition

    WO2018212279A1

  • PTFE composite powder, preparation method, and composite material containing PTFE composite powder

    WO2022246892A1

  • Low dielectric loss resin composition, method for producing same, molded body for high frequency devices, and high frequency device

    WO2022254960A1

Cited By

  • Filler for low dielectric loss resin compositions, low dielectric loss resin composition, molded body for high frequency device, and high frequency device

    WO2026075045A1